Separator for lead-acid battery and high-performance power-type lead-acid battery
By using benzidine-modified polyethylene terephthalate fiber as the separator material for lead-acid batteries, the problems of insufficient high-rate discharge, cycle life and vibration resistance of traditional lead-acid batteries have been solved, and the stability and safety of high-performance power lead-acid batteries have been improved.
Patent Information
- Application Number
- PCT/CN2026/083706
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-03-16
- Publication Date
- 2026-11-19
AI Technical Summary
Traditional lead-acid batteries are inadequate in terms of high-rate discharge, cycle life, and vibration resistance, and cannot meet the needs of vehicle starting or short-term high-power output. In addition, they have poor structural stability and pose safety hazards.
Benzidine-modified polyethylene terephthalate fiber was used as the battery separator material. Modified fiber was prepared by acylation and further reaction. It was then combined with glass fiber to prepare a high-performance lead-acid battery separator. The plate grid alloy formulation and assembly process were optimized.
It improves the battery's high-rate discharge capability, extends cycle life, enhances vibration resistance and structural stability, reduces the risk of thermal runaway, and improves battery safety and consistency.
Smart Images

Figure PCTCN2026083706-FTAPPB-I100001
Abstract
Description
A separator for lead-acid batteries and a high-performance power lead-acid battery Technical Field
[0001] This invention belongs to the field of lead-acid battery technology, specifically relating to a separator for lead-acid batteries and a high-performance power lead-acid battery. Background Technology
[0002] Lead-acid batteries are still widely used in the field of power batteries due to their mature technology, low cost, high reliability and easy recycling.
[0003] However, traditional lead-acid battery technology has certain limitations in terms of high-rate discharge, deep cycling, and vibration resistance, which are mainly reflected in the following aspects:
[0004] 1) Insufficient high-rate discharge capability
[0005] Existing lead-acid batteries exhibit low utilization of active materials within the plates during high-rate discharge, resulting in high internal resistance and a significant drop in output voltage. This makes them unable to meet the demands of vehicle starting or short-term high-power output. Battery performance deteriorates even more rapidly under extreme temperature conditions and frequent start-stop cycles.
[0006] 2) Limited cycle life
[0007] Traditional lead-acid batteries experience a gradual decrease in capacity and a shortened lifespan due to the accumulation of sulfation on the plates during long-term cyclic use. This is particularly pronounced under deep discharge and high-rate operating conditions, where problems such as active material stripping, mesh corrosion, and lead dendrite growth become more prominent, directly impacting the battery's durability and safety.
[0008] 3) Vibration resistance and structural stability issues
[0009] In automotive and other power applications, batteries often need to withstand significant vibration and impact. Traditional manufacturing processes for electrode plates and assembly have certain shortcomings, which can easily lead to safety hazards such as loosening of internal structures, electrolyte leakage, or partial short circuits. Therefore, improving the vibration resistance and overall structural stability of lead-acid batteries has become a crucial technical problem that urgently needs to be solved.
[0010] The battery separator is a crucial component of lead-acid batteries, and its performance directly impacts the battery's overall performance. Currently, numerous studies both domestically and internationally have focused on improving battery performance through separator modification.
[0011] For example, patent application CN1398008A discloses a modification method for ultrafine glass fiber separators used in lead-acid batteries. This method utilizes a hydrophobic organic polymer, polytetrafluoroethylene (PTFE) emulsion, to modify the ultrafine glass fiber separator to be hydrophobic. The treated ultrafine glass fiber separator provides a separate lateral channel for gas, improving its permeability, effectively increasing the gas recombination efficiency of VRLA batteries, reducing internal pressure, decreasing the frequency of valve opening, preventing battery drying, extending battery life, and at a lower cost.
[0012] For example, patent application CN114497885A discloses a manufacturing process for an ultrafine glass fiber battery separator: S001, preparation of phenolic resin adhesive; S002, preparation of ultrafine glass fiber felt; S003, preparation of the battery separator. This application modifies the phenolic resin adhesive using phenol, formaldehyde, and graphene oxide as raw materials to obtain a modified phenolic resin adhesive. The phenolic resin adhesive is then sprayed onto the secondary ultrafine glass fiber filaments, effectively improving the strength, tensile properties, and high-temperature resistance of the battery separator. Furthermore, the ultrafine glass fiber felt is homogenized multiple times to improve the uniformity of the battery separator, thereby extending the lifespan of the lead-acid battery.
[0013] However, there is still room for improvement in the high-rate discharge capability, cycle life, vibration resistance, and structural stability of lead-acid batteries, and finding new methods for modifying battery separators remains of great significance. Summary of the Invention
[0014] To address the aforementioned technical problems in the prior art, the present invention provides a separator for lead-acid batteries and a high-performance power lead-acid battery.
[0015] This invention first provides a method for preparing benzidine-modified polyethylene terephthalate fiber, comprising the following steps, wherein the parts are parts by weight:
[0016] (1) Place 100-140 parts of polyester fiber in 1000-1300 parts of dichloroethane, stir evenly, then add 10-20 parts of maleic anhydride and 5-10 parts of aluminum chloride to carry out acylation reaction.
[0017] (2) Add 11-22 parts of diaminobenzidine, 0.04-0.5 parts of triethylboron-diethylenetriamine, and 2-5 parts of potassium hydroxide to the above reaction system, mix well, and react.
[0018] (3) After the reaction is complete, the fiber obtained by the reaction is filtered and separated, unreacted substances are washed to remove the unreacted substances, and dried to obtain benzidine-modified polyethylene terephthalate fiber.
[0019] Preferably, in step (1), the reaction temperature is 35-45℃ and the reaction time is 10-15 hours.
[0020] Preferably, in step (2), the reaction temperature is 65-70℃ and the reaction time is 5-10 hours.
[0021] This invention provides benzidine-modified polyethylene terephthalate fibers prepared by the above preparation method.
[0022] The present invention also provides a separator for lead-acid batteries, comprising glass fiber and the above-mentioned benzidine-modified polyethylene terephthalate fiber, wherein the benzidine-modified polyethylene terephthalate fiber is added at a mass percentage of 7%-9%.
[0023] Preferably, the benzidine-modified polyethylene terephthalate fiber is added at a mass percentage of 9%.
[0024] The present invention also provides a high-performance power lead-acid battery, comprising an electrode group, the electrode group including a positive electrode plate, a negative electrode plate and a separator for the lead-acid battery described above.
[0025] Preferably, the positive electrode plate includes a positive electrode grid and a positive electrode lead paste, and the negative electrode plate includes a negative electrode grid and a negative electrode lead paste. By mass parts, the positive electrode grid comprises: 0.10-2.0 parts tin, 0.05-0.10 parts antimony, 0.005-0.02 parts bismuth, 0.005-0.05 parts selenium, with the balance being lead; by mass parts, the negative electrode grid comprises: 0.10-0.15 parts calcium, 0.10-0.80 parts tin, 0.02-0.03 parts aluminum, with the balance being lead.
[0026] Preferably, both the positive and negative electrode grids are prepared by continuous rolling and stamping, wherein the lead strip thickness of the rolled positive electrode grid is 0.70±0.01mm; the lead strip thickness of the rolled negative electrode grid is 0.55±0.01mm; during the rolling process of the positive and negative electrode grids, the temperature is controlled at 80-120℃, the rolling speed is controlled at 0.5-2.0m / s, and the rolling pressure is controlled at 50-150MPa.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1) Improve battery performance and stability
[0029] Benzidine-modified polyethylene terephthalate (PET) fibers are used to manufacture lead-acid battery separators, enhancing the fiber's chemical stability and mechanical properties. Improved chemical stability allows for better resistance to sulfuric acid electrolyte corrosion, extending separator life and improving overall battery stability and reliability; good mechanical properties ensure the integrity of the separator structure, preventing short circuits between the positive and negative electrodes and guaranteeing safe battery operation.
[0030] 2) Optimize battery performance
[0031] The fiber's unique structure and modified components optimize the internal ion transport pathways of lead-acid batteries, altering the surface charge distribution and pore structure to facilitate the migration of sulfate ions, thereby improving charge-discharge efficiency, reducing energy loss, and enhancing battery power performance, particularly under high-current charge-discharge conditions. Simultaneously, during battery charge-discharge cycles, it inhibits the shedding of electrode active materials and the growth of lead sulfate crystals, maintaining electrode activity and stability, extending cycle life, and reducing capacity decay.
[0032] 3) Enhance battery safety and consistency
[0033] Fiber materials may possess flame retardancy and thermal stability. When abnormalities such as overcharging or over-discharging cause internal temperature rise in batteries, they can prevent heat diffusion and spread, reduce the risk of thermal runaway, and decrease safety accidents such as fires. Furthermore, using this fiber to make components such as separators can improve the consistency of lead-acid battery production, making the performance of different batches of batteries more similar, which is beneficial for battery pack assembly and improves the overall performance and lifespan of the battery pack. Detailed Implementation
[0034] Example 1
[0035] Preparation method of high-performance power lead-acid battery
[0036] (1) Formulation of positive and negative electrode grid alloys
[0037] Under vacuum melting conditions, positive plate alloy and negative plate alloy are obtained by melting according to the following mass ratio, with each of the positive plate alloy and negative plate alloy weighing a total of 100 kg:
[0038] Positive plate alloy:
[0039] Tin (Sn): 0.50 kg; Antimony (Sb): 0.06 kg; Bismuth (Bi): 0.01 kg; Selenium (Se): 0.01 kg; Balance: Lead (Pb).
[0040] Negative plate alloy:
[0041] Calcium (Ca): 0.12 kg; Tin (Sn): 0.60 kg; Aluminum (Al): 0.025 kg; Balance: Lead (Pb).
[0042] The melting temperature is controlled at 700℃ and the melting time is 1.5 hours.
[0043] (2) Strip rolling
[0044] The positive lead strip is rolled from a calcium-free alloy with a thickness controlled at 0.70 mm; the negative lead strip is rolled from a high-calcium, low-tin alloy with a thickness controlled at 0.55 mm. During the rolling process, the temperature is set at 100℃, the rolling speed at 1.0 m / s, and the rolling pressure at 100 MPa.
[0045] (3) Strip stamping of plate grid
[0046] Positive lead strips are directly processed into the coating process after punching; negative lead strips are placed in a 90℃ oven for aging treatment for 10 hours after punching.
[0047] (4) Curing of coating
[0048] The positive lead paste consists of 92 wt% lead oxide, 5 wt% binder (polyvinyl alcohol), and 3 wt% dispersant (polyvinylpyrrolidone), with an apparent density controlled at 4.400 g / cm³. 3 The coating thickness is 0.35 mm. The negative board lead paste consists of 0.2 wt% lignin, 1.5 wt% barium sulfate, 5 wt% binder (polyvinyl alcohol), and 3 wt% dispersant (polyvinylpyrrolidone), with an apparent density controlled at 4.450 g / cm³. 3 The coating thickness is 0.25mm.
[0049] (5) Electrode assembly and assembly
[0050] The ratio of positive to negative electrode plates is 6:7. The positive electrode plate is wrapped with AGM separator (glass fiber separator) containing 7wt% benzidine-modified polyethylene terephthalate fiber. After casting and welding in the lower tank, it is assembled into a 2V-12Ah semi-finished battery.
[0051] The preparation method of the benzidine-modified polyethylene terephthalate fiber:
[0052] Acylation reaction stage: 120g of polyester fiber was placed in 1150g of dichloroethane and mechanically stirred to ensure uniform dispersion. Then, 15g of maleic anhydride and 7.5g of aluminum chloride were added, and the temperature was slowly raised to 40°C. The mixture was stirred at this temperature and reacted for 12 hours.
[0053] Further reaction stage: 16.5 g of diaminobenzidine, 0.2 g of triethylboron-diethylenetriamine, and 3.5 g of potassium hydroxide were added to the above reaction system. After initial mixing at room temperature, the temperature was gradually increased to 68 °C and maintained at this temperature for 7 hours.
[0054] Post-processing stage: After the reaction is complete, the modified fibers are collected by filtration. The fibers are washed repeatedly with deionized water until no obvious unreacted substances remain in the washing solution. Finally, the fibers are dried in an oven at a suitable temperature to obtain benzidine-modified polyethylene terephthalate fibers.
[0055] (6) Semi-finished batteries are acidified
[0056] The semi-finished battery was acidified in 36wt% dilute sulfuric acid at a controlled temperature of 25℃ for 36 hours.
[0057] Example 2
[0058] Preparation method of high-performance power lead-acid battery
[0059] (1) Preparation of positive and negative grid alloys, with the positive and negative alloys each calculated in a total of 100 kg:
[0060] Positive plate alloy:
[0061] Tin (Sn): 1.5 kg; Antimony (Sb): 0.1 kg; Bismuth (Bi): 0.02 kg; Selenium (Se): 0.05 kg; Balance: Lead (Pb).
[0062] Negative plate alloy:
[0063] Calcium (Ca): 0.15 kg; Tin (Sn): 0.8 kg; Aluminum (Al): 0.03 kg; Balance: Lead (Pb).
[0064] Melting temperature 650℃, melting time 2 hours.
[0065] (2) Strip rolling
[0066] The thickness of the positive lead strip is 0.69 mm, and the thickness of the negative lead strip is 0.56 mm. The rolling temperature is 120℃, the speed is 2.0 m / s, and the pressure is 150 MPa.
[0067] (3) Strip stamping of plate grid
[0068] Positive lead strips go directly into the coating process; negative lead strips undergo aging treatment in a 95℃ oven for 8 hours.
[0069] (4) Curing of coating
[0070] The positive lead paste contains 95 wt% lead oxide, 5 wt% polyvinyl alcohol and polyvinylpyrrolidone, with an apparent density of 4.40 g / cm³. 3 The coating thickness is 0.40 mm. The negative plate lead paste consists of 0.2 wt% lignin, 1.5 wt% barium sulfate, 5 wt% binder (polyvinyl alcohol), and 3 wt% dispersant (polyvinylpyrrolidone), with an apparent density of 4.450 g / cm³. 3 The coating thickness is 0.30mm.
[0071] (5) Electrode assembly and assembly
[0072] The positive and negative plates are in a 6:7 ratio. The positive plate uses an AGM separator containing 8wt% benzidine-modified fiber. After being cast and welded in the lower tank, they are assembled into a 2V-12Ah semi-finished battery.
[0073] The preparation method of the benzidine-modified polyethylene terephthalate fiber:
[0074] Acylation reaction stage: Take 100g of polyester fiber and disperse it in 1000g of dichloroethane, ensuring that the fiber is fully impregnated. Add 10g of maleic anhydride and 5g of aluminum chloride, heat to 35℃, maintain constant temperature and stir for 15 hours.
[0075] Further reaction stage: 11g of diaminobenzidine, 0.04g of triethylboron-diethylenetriamine, and 2g of potassium hydroxide were added to the reaction system. After mixing thoroughly at room temperature, the temperature was raised to 65℃ and the reaction was maintained for 10 hours.
[0076] Post-treatment stage: filtration, washing (using deionized water), and drying are the same as in Example 1.
[0077] (6) Semi-finished batteries are acidified
[0078] 38wt% dilute sulfuric acid, temperature 20℃, reaction time 48 hours.
[0079] Example 3
[0080] Preparation method of high-performance power lead-acid battery
[0081] (1) Preparation of positive and negative grid alloys, with the positive and negative alloys each calculated in a total of 100 kg:
[0082] Positive plate alloy:
[0083] Tin (Sn): 1.0 kg; Antimony (Sb): 0.08 kg; Bismuth (Bi): 0.005 kg; Selenium (Se): 0.005 kg; Balance: Lead (Pb).
[0084] Negative plate alloy:
[0085] Calcium (Ca): 0.10 kg; Tin (Sn): 0.10 kg; Aluminum (Al): 0.02 kg; Balance: Lead (Pb).
[0086] Melting temperature 800℃, melting time 1 hour.
[0087] (2) Strip rolling
[0088] The thickness of the positive lead strip is 0.71 mm, and the thickness of the negative lead strip is 0.54 mm. The rolling temperature is 80℃, the speed is 0.5 m / s, and the pressure is 50 MPa.
[0089] (3) Strip stamping of plate grid
[0090] Positive plates are directly coated; negative plates undergo aging treatment in an 85℃ oven for 12 hours.
[0091] (4) Curing of coating
[0092] The positive lead paste contains 90 wt% lead oxide, 10 wt% polyacrylate and polyvinylpyrrolidone, with an apparent density of 4.40 g / cm³. 3 The coating thickness is 0.30 mm. The negative board lead paste consists of 0.2 wt% lignin, 1.5 wt% barium sulfate, 5 wt% binder (polyvinyl alcohol), and 3 wt% dispersant (polyvinylpyrrolidone), with an apparent density of 4.450 g / cm³. 3 The coating thickness is 0.20mm.
[0093] (5) Electrode assembly and assembly
[0094] The positive and negative plates are in a 6:7 ratio. The positive plate uses an AGM separator containing 8wt% benzidine-modified fiber. After being cast and welded in the lower tank, they are assembled into a 2V-12Ah semi-finished battery.
[0095] The preparation method of the benzidine-modified polyethylene terephthalate fiber:
[0096] Acylation reaction stage: 140g of polyester fiber was placed in 1300g of dichloroethane solvent. 20g of maleic anhydride and 10g of aluminum chloride were added, and the temperature was raised to 45℃. The mixture was stirred and reacted for 10 hours under these conditions.
[0097] Further reaction stage: Add 22g of diaminobenzidine, 0.5g of triethylboron-diethylenetriamine, and 5g of potassium hydroxide to the reaction system. After mixing at room temperature, heat to 70℃ and continue the reaction for 5 hours.
[0098] Post-treatment stage: filtration, washing, and drying operations follow the method of Example 1.
[0099] (6) Semi-finished batteries are acidified
[0100] 34wt% dilute sulfuric acid, temperature 30℃, reaction time 24 hours.
[0101] Example 4
[0102] Preparation method of high-performance power lead-acid battery
[0103] (1) Preparation of positive and negative grid alloys, with the positive and negative alloys each calculated in a total of 100 kg:
[0104] Positive plate alloy:
[0105] Tin (Sn): 2.0 kg; Antimony (Sb): 0.05 kg; Bismuth (Bi): 0.015 kg; Selenium (Se): 0.02 kg; Balance: Lead (Pb).
[0106] Negative plate alloy:
[0107] Calcium (Ca): 0.13 kg; Tin (Sn): 0.50 kg; Aluminum (Al): 0.025 kg; Balance: Lead (Pb).
[0108] The melting temperature is 750℃ and the melting time is 1.5 hours.
[0109] (2) Strip rolling
[0110] The thickness of the positive lead strip is 0.70 mm, and the thickness of the negative lead strip is 0.55 mm. The rolling temperature is 110℃, the speed is 1.5 m / s, and the pressure is 120 MPa.
[0111] (3) Strip stamping of plate grid
[0112] Positive plates are directly coated; negative plates undergo aging treatment in a 90℃ oven for 10 hours.
[0113] (4) Curing of coating
[0114] The positive lead paste contains 93% lead oxide, 7% polyvinyl alcohol, and polyvinylpyrrolidone, with an apparent density of 4.40 g / cm³. 3 The coating thickness is 0.38 mm. The negative board lead paste consists of 0.2% lignin, 1.5% barium sulfate, 5% binder (polyvinyl alcohol), and 3% dispersant (polyvinylpyrrolidone), with an apparent density of 4.450 g / cm³. 3 The coating thickness is 0.28mm.
[0115] (5) Electrode assembly and assembly
[0116] The positive and negative plates are in a 6:7 ratio. The positive plate uses AGM separators containing 9wt% benzidine-modified fiber. After being cast and welded in the lower tank, they are assembled into a 2V-12Ah semi-finished battery.
[0117] The preparation method of the benzidine-modified polyethylene terephthalate fiber:
[0118] Acylation reaction stage: 130g of polyester fiber was uniformly dispersed in 1200g of dichloroethane. 17.5g of maleic anhydride and 8.75g of aluminum chloride were added, the temperature was raised to 42.5℃, and the reaction was carried out with stirring for 12.5 hours.
[0119] Further reaction stage: 16g of diaminobenzidine, 0.3g of triethylboron-diethylenetriamine, and 4g of potassium hydroxide were added to the system. The mixture was thoroughly mixed at room temperature, then heated to 67.5℃ and reacted for another 7.5 hours.
[0120] Post-processing stage: The fibers are collected by filtration, thoroughly washed with deionized water to remove all unreacted substances, and then dried to obtain benzidine-modified polyethylene terephthalate fibers.
[0121] (6) Semi-finished batteries are acidified
[0122] 37wt% dilute sulfuric acid, temperature 28℃, reaction time 36 hours.
[0123] Comparative Example 1
[0124] The difference between this example and Example 1 is that in this example, polyester fiber is used to replace benzidine-modified polyethylene terephthalate fiber in an equal amount during the electrode assembly and combination.
[0125] Comparative Example 2
[0126] The difference between this example and Example 1 is that diaminobenzidine is not added during the preparation of the benzidine-modified polyethylene terephthalate fiber in this example.
[0127] Comparative Example 3
[0128] The difference between this example and Example 1 is that triethylboron-diethylenetriamine is not added during the preparation of the benzidine-modified polyethylene terephthalate fiber in this example.
[0129] Detection Example 1
[0130] The lead-acid batteries prepared in Examples 1-4 and Comparative Examples 1-3 were subjected to the following tests:
[0131] 1. High-rate discharge test
[0132] Testing equipment: Digital battery testing system with constant current discharge function and real-time data acquisition.
[0133] Test conditions: Temperature controlled at 25±2℃; test magnification set at 0.2C (low magnification) and 0.5C (higher magnification).
[0134] Test steps:
[0135] Charge the battery to 100%.
[0136] At 25°C, discharge at a rate of 0.2C to the termination voltage of 1.80V, and then record the discharge capacity.
[0137] After charging to 100% state of charge, a discharge test was conducted at a rate of 0.5C. The discharge was continued until the termination voltage of 1.75V, at which point the voltages during the discharge process and the battery discharge capacity at the discharge cutoff were recorded.
[0138] Calculate the capacity retention rate of the battery under 0.5C discharge conditions (the ratio of the test results under 0.2C conditions).
[0139] 2. Cyclic life test
[0140] Testing equipment: Cycle life tester, which automatically records data during the charge and discharge process.
[0141] Test conditions:
[0142] Temperature is controlled at 25±2℃; standard charge and discharge protocol is adopted.
[0143] Test steps:
[0144] After charging the battery to 100%, perform a charge-discharge cycle:
[0145] (1) Circuit discharge: Discharge 6A until the voltage is 1.75V;
[0146] (2) Constant voltage and current limiting charging: control the charging voltage at 2.47V, the charging current at 6A, and the charging time at 4h;
[0147] (3) Let stand for 30 minutes;
[0148] The discharge capacity is recorded once per cycle, and the cumulative number of cycles reaches 500.
[0149] Analyze the remaining percentage of battery capacity after the cycle ends and calculate the capacity decay rate.
[0150] 3. Vibration resistance test
[0151] Test equipment: vibration table with sinusoidal and random vibration functions; dynamic monitoring data acquisition system.
[0152] Test conditions: Test frequency: 10-200Hz sinusoidal vibration; acceleration: 5-10g; during random vibration testing, the total acceleration range is 5-8g, and the duration is 30 minutes.
[0153] Test steps:
[0154] Install the battery on the vibration table and perform sinusoidal vibration test according to the specified vibration parameters;
[0155] After vibration, check the battery's appearance, structure, and electrolyte for any leakage.
[0156] After conducting random vibration tests, repeat the checks and record any abnormalities.
[0157] At the same time, the same test was performed on the comparison sample to observe whether there was any loosening of the electrode plate or damage to the internal components.
[0158] After the vibration test, the battery's open voltage and 0.5C discharge capacity were tested.
[0159] Table 1 Test Results
[0160] The test results are shown in Table 1, which demonstrates the significant improvements of the preparation method of the present invention in key performance aspects such as high-rate discharge, long cycle life and excellent vibration resistance, providing strong technical support for the efficient and stable application of power lead-acid batteries.
Claims
1. A method for producing a benzidine-modified polyethylene terephthalate fiber, characterized by, Includes the following steps, where the number of parts refers to the number of parts by weight: (1) Place 100-140 parts of polyester fiber in 1000-1300 parts of dichloroethane, stir evenly, then add 10-20 parts of maleic anhydride and 5-10 parts of aluminum chloride to carry out acylation reaction. (2) Add 11-22 parts of diaminobenzidine, 0.04-0.5 parts of triethylboron-diethylenetriamine, and 2-5 parts of potassium hydroxide to the above reaction system, mix well, and react. (3) After the reaction is complete, the fiber obtained by the reaction is filtered and separated, unreacted substances are washed to remove the unreacted substances, and dried to obtain benzidine-modified polyethylene terephthalate fiber.
2. The method for preparing benzidine-modified polyethylene terephthalate fiber according to claim 1, characterized in that, In step (1), the reaction temperature is 35-45℃ and the reaction time is 10-15 hours.
3. The method for preparing benzidine-modified polyethylene terephthalate fiber according to claim 1, characterized in that, In step (2), the reaction temperature is 65-70℃ and the reaction time is 5-10 hours.
4. Benzidine-modified polyethylene terephthalate fiber prepared by the preparation method according to any one of claims 1-3.
5. A separator for lead storage batteries, characterized by The composition includes glass fiber and benzidine-modified polyethylene terephthalate fiber as described in claim 4, wherein the benzidine-modified polyethylene terephthalate fiber is added at a mass percentage of 7%-9%.
6. A high performance power lead-acid battery comprising a group of plates, the group of plates comprising positive plates, negative plates and separators, characterised in that, The separator is the separator used in the lead-acid battery as described in claim 5.
7. A high performance power lead-acid battery according to claim 6, wherein The positive electrode plate includes a positive electrode grid and positive lead paste, and the negative electrode plate includes a negative electrode grid and negative lead paste. The positive electrode grid composition, by weight, comprises: 0.50-2.0 parts tin, 0.05-0.10 parts antimony, 0.005-0.02 parts bismuth, 0.005-0.05 parts selenium, with the balance being lead; The negative electrode grid composition, by mass, comprises: 0.10-0.15 parts calcium, 0.10-0.80 parts tin, 0.02-0.03 parts aluminum, with the balance being lead.
8. The high-power, power-type lead-acid storage battery of claim 7 wherein, Both the positive and negative electrode grids are prepared by continuous rolling and stamping. The lead strip thickness of the rolled positive electrode grid is 0.70±0.01mm, and the lead strip thickness of the rolled negative electrode grid is 0.55±0.01mm. During the rolling process of the positive and negative electrode grids, the temperature is controlled at 80-120℃, the rolling speed is controlled at 0.5-2.0m / s, and the rolling pressure is controlled at 50-150MPa.