Three-dimensional porous negative electrode, preparation method therefor, and creep-type all-solid-state lithium metal battery

By using carbon nanotube arrays and silicon deposition layers in a three-dimensional porous anode material, uniform deposition and stripping of lithium metal are achieved, solving the problems of volume change and mechanical stability in solid-state lithium metal batteries and improving the cycle stability and safety of the battery.

WO2026237568A1PCT designated stage Publication Date: 2026-11-19FUJIAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/086857
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-03-28
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Solid-state lithium metal batteries exhibit significant volume changes during lithium deposition and stripping, leading to voids at the electrode-electrolyte interface. The enormous stress generated during cycling may cause the solid electrolyte to fracture, forming lithium dendrite penetration channels, resulting in battery short circuits, and insufficient mechanical and electrochemical stability.

Method used

A three-dimensional porous anode material is used, including a carbon nanotube array and a silicon element deposition layer. The carbon-silicon porous material achieves uniform deposition and stripping of lithium metal through a creep mechanism, forming a 'flowable liquid metal', maintaining good contact between the electrode and the electrolyte interface, and adapting to volume changes through the carbon nanotube array structure.

Benefits of technology

It significantly alleviates stress problems during charging and discharging, improves battery cycle stability and lifespan, enhances the conductivity and adaptability of electrode materials, ensures the integrity of electrode structure, and improves battery performance and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026086857_19112026_PF_FP_ABST
    Figure CN2026086857_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium metal batteries. Specifically disclosed are a three-dimensional porous negative electrode, a preparation method therefor, and a creep-type all-solid-state lithium metal battery. The three-dimensional porous negative electrode material of the present invention combines a carbon nanotube array with a carbon-silicon structure, to achieve uniform deposition and stripping of a lithium metal, reduce stress, maintain interface contact, avoid the formation of a solid electrolyte interface layer, and improve conductivity and volume adaptability, thereby significantly improving the cycle stability, service life, and reliability of a battery. In addition, the present invention further provides a creep-type all-solid-state lithium metal battery. The creep-type all-solid-state lithium metal battery has high energy density and good charge-discharge cycle stability, as well as excellent mechanical stability and safety. These characteristics make the creep-type all-solid-state lithium metal battery have great application potential in future energy storage systems.
Need to check novelty before this filing date? Find Prior Art

Description

A three-dimensional porous anode and its preparation method and a creep-type all-solid-state lithium metal battery Technical Field

[0001] This invention relates to the field of lithium metal battery technology, specifically disclosing a three-dimensional porous anode and its preparation method, and a creep-type all-solid-state lithium metal battery. Background Technology

[0002] With the development of electric vehicles and large-scale grid energy storage technologies, the demand for high-performance batteries continues to grow. Solid-state lithium metal batteries are particularly popular due to the high theoretical capacity of their lithium metal anodes (3860 mAh g⁻¹). -1 Low electrochemical potential (−3.04 V) and low density (0.53 g cm⁻¹) -3 Solid-state lithium metal batteries, along with their safety characteristics and mechanical strength, are considered highly promising energy storage devices. However, in practical applications, solid-state lithium metal batteries face many challenges. For example, significant volume changes during lithium deposition and stripping lead to voids at the electrode-electrolyte interface, resulting in increased polarization; the enormous stress generated during cycling can cause the solid electrolyte to fracture, forming lithium dendrite penetration channels, ultimately causing a short circuit in the battery.

[0003] To address these challenges, researchers have explored various strategies, such as creating artificial SEI films and using three-dimensional electronic or ionic conductors as lithium metal hosts. However, a single material cannot effectively solve all problems. Furthermore, solid-state lithium metal batteries still face difficulties in terms of mechanical and electrochemical stability, particularly in handling the internal stresses of lithium and stability under complex environments. Therefore, there is an urgent need to develop new materials and technologies to overcome these existing problems. Summary of the Invention

[0004] To address the aforementioned problems, this invention provides a three-dimensional porous negative electrode and its preparation method, as well as a creep-type all-solid-state lithium metal battery.

[0005] The first aspect of the present invention provides a three-dimensional porous anode material, comprising a silicon carbide porous material, wherein a lithium metal layer is disposed on the silicon carbide porous material;

[0006] The carbon-silicon porous material includes electronic conductors and ionic conductors, wherein the electronic conductors are carbon nanotube arrays and the ionic conductors are silicon element deposition layers.

[0007] The three-dimensional porous anode material provided by this invention possesses unique structural characteristics, effectively promoting the uniform deposition and stripping of lithium metal within nanotubes via a creep mechanism. This allows lithium metal to form a "flowable liquid metal" at the nanoscale, significantly alleviating stress problems generated during charging and discharging, and maintaining good interfacial contact between the electrode and the electrolyte. Furthermore, the carbon-silicon porous material provided by this invention exhibits extremely high stability against lithium metal, fundamentally eliminating the formation of a solid electrolyte interfacial layer, thereby improving the battery's cycle stability and lifespan.

[0008] Furthermore, the carbon nanotube array structure provided in this invention not only significantly improves the overall conductivity of the electrode material but also possesses excellent adaptability, effectively accommodating the volume changes experienced by the negative electrode material during charge-discharge cycles. This adaptability ensures the integrity of the electrode structure, reduces mechanical damage caused by volume expansion and contraction, thereby further enhancing the battery's performance and reliability.

[0009] Preferably, the method for preparing the silicon carbide porous material includes the following steps:

[0010] Silicon was deposited on the surface of a carbon nanotube array using atomic layer deposition to obtain a carbon-silicon porous material.

[0011] Preferably, the deposition vacuum degree of the atomic layer deposition is (0.5-1.5)×10⁻⁶. -4 Pa, the deposition temperature is 200℃-300℃, and the heating rate to the deposition temperature is 5℃ / min-10℃ / min.

[0012] Preferably, the silicon element is deposited by introducing it into the SiH4 silicon precursor in a pulsed manner, wherein the pulse duration is 0.5s-1.5s and the sweep-blowing time is 15s-25s.

[0013] Preferably, the thickness of the silicon element deposited by chemical vapor deposition is 5nm-50nm.

[0014] Preferably, the method for preparing the carbon nanotube array includes the following steps:

[0015] Carbon elements are deposited on the inner surface of an alumina template by chemical vapor deposition, and then the alumina template is removed to obtain a carbon nanotube array.

[0016] Preferably, the deposition vacuum degree of the chemical vapor deposition is (0.5-1.5)×10⁻¹⁰. -4 Pa, the deposition temperature is 600℃-680℃, and the heating rate to the deposition temperature is 5℃ / min-10℃ / min.

[0017] Preferably, the deposition atmosphere for the chemical vapor deposition is an argon atmosphere.

[0018] Preferably, the carbon element is deposited by introducing acetylene gas.

[0019] Preferably, before removing the alumina template, a platinum support layer is sputtered onto the bottom of the alumina template where carbon elements are deposited.

[0020] Preferably, the sputtering is performed using magnetron sputtering, and the vacuum degree of the magnetron sputtering is (0.5-1.5)×10⁻⁶. -6 Pa, power of 30W-50W, time of 10min-20min.

[0021] Preferably, the magnetron sputtering is performed in an argon atmosphere.

[0022] Preferably, the alumina template is removed by etching with an aqueous sodium hydroxide solution.

[0023] Preferably, the sodium hydroxide aqueous solution has a mass fraction of 10%-15%.

[0024] A second aspect of the present invention provides a method for preparing the three-dimensional porous anode material described in the foregoing scheme, comprising the following steps:

[0025] A three-dimensional porous anode material is obtained by loading a lithium metal layer onto a silicon carbide porous material.

[0026] The lithium metal layer is loaded onto the porous silicon carbon material by electrochemical deposition or melt infusion.

[0027] The method for preparing three-dimensional porous anode materials disclosed in this invention not only boasts advantages such as simple operation and low cost, but also exhibits excellent efficiency. This method can be implemented in a single step, making the preparation process both rapid and convenient, significantly reducing production costs.

[0028] Preferably, the current density of the electrochemical deposition is 0.1 mA cm⁻¹. -2 -0.5mA cm -2 The time ranges from 1 hour to 50 hours.

[0029] Preferably, the infusion volume of the melt infusion is 0.026 mg cm⁻¹. -2 -1.5mg cm -2 .

[0030] Preferably, the thickness of the lithium metal layer is 1μm-30μm.

[0031] A third aspect of the present invention provides a creep-type all-solid-state lithium metal battery, comprising a positive electrode, a solid electrolyte, and a negative electrode;

[0032] The positive electrode includes a positive electrode current collector, a conductive material, a positive electrode solid electrolyte, and a positive electrode active material layer;

[0033] The solid electrolyte is selected from polymers, oxides, or sulfides;

[0034] The negative electrode includes the three-dimensional porous negative electrode material described in the aforementioned scheme.

[0035] The three-dimensional porous anode material proposed in this invention, when applied to solid-state lithium metal batteries, can construct a creep-type all-solid-state lithium metal battery. This creep-type all-solid-state lithium metal battery exhibits high energy density and good charge-discharge cycle stability, as well as excellent mechanical stability and safety. These characteristics make it a promising candidate for future energy storage systems.

[0036] Preferably, the positive electrode active material is selected from lithium iron phosphate, lithium nickel cobalt manganese oxide, or lithium cobalt oxide.

[0037] Preferably, the solid electrolyte is selected from PEO-based polymer solid electrolyte, LLZTO solid electrolyte, or LPSCl solid electrolyte.

[0038] In summary, the present invention includes at least one of the following beneficial technical effects:

[0039] 1. The three-dimensional porous anode material provided by this invention possesses unique structural characteristics, which can effectively promote the uniform deposition and stripping of lithium metal within the nanotubes through a creep mechanism. This allows the lithium metal to form a "flowable liquid metal" at the nanoscale, significantly alleviating stress problems generated during charging and discharging, and maintaining good interfacial contact between the electrode and the electrolyte. Furthermore, the carbon-silicon porous material provided by this invention exhibits extremely high stability against lithium metal, fundamentally eliminating the formation of a solid electrolyte interfacial layer, thereby improving the cycle stability and lifespan of the battery.

[0040] 2. The carbon nanotube array structure provided in this invention not only significantly improves the overall conductivity of the electrode material, but also possesses excellent adaptability, effectively accommodating the volume changes experienced by the negative electrode material during charge-discharge cycles. This adaptability ensures the integrity of the electrode structure, reduces mechanical damage caused by volume expansion and contraction, thereby further improving the battery's performance and reliability.

[0041] 3. The method for preparing the three-dimensional porous anode material involved in this invention not only has the advantages of simple operation and low cost, but also exhibits excellent efficiency. This method can be achieved in a single step, making the preparation process both fast and convenient, significantly reducing production costs.

[0042] 4. The three-dimensional porous anode material proposed in this invention, when applied to solid-state lithium metal batteries, can construct a creep-type all-solid-state lithium metal battery. This creep-type all-solid-state lithium metal battery exhibits high energy density and good charge-discharge cycle stability, as well as excellent mechanical stability and safety. These characteristics make it a promising candidate for future energy storage systems. Attached Figure Description

[0043] Figure 1 is a SEM image of the silicon carbide porous material prepared in Example 1;

[0044] Figure 2 is a mapping diagram of the porous silicon carbide material prepared in Example 1;

[0045] Figure 3 shows the electrochemical performance of the creep-type all-solid-state lithium metal battery in Example 1 and the solid-state lithium metal battery in Comparative Example 1.

[0046] Figure 4 is a performance comparison chart of the half-cells in Example 1 and Comparative Example 1. Detailed Implementation

[0047] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are merely one embodiment of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise specified, the raw materials in the embodiments of the present invention are all purchased through commercial channels. Example 1

[0048] This embodiment provides a three-dimensional porous negative electrode and a creep-type all-solid-state lithium metal battery, specifically including the following solutions:

[0049] A method for preparing a three-dimensional porous negative electrode includes the following steps:

[0050] (1) Place the alumina template on the sample stage of the chemical vapor deposition equipment and evacuate the reaction chamber to 10. -4 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 Torr. The heating system was then turned on, and the reaction chamber was heated at a rate of 5 °C / min until the temperature reached 650 °C. After the temperature and pressure stabilized, acetylene gas was introduced at a flow rate of 100 sccm. The deposition time was 30 min. After the deposition time was completed, the acetylene gas valve was closed, and the carbon nanotube array precursor was obtained after cooling.

[0051] (2) Place the carbon nanotube precursor on the sample stage of the magnetron sputtering equipment, install the platinum target, and evacuate the reaction chamber to a vacuum level of 10. -6Pa, argon gas was introduced to stabilize the pressure in the reaction chamber at 5 mTorr, DC power was turned on at 50W, sputtering time was 10 minutes, the sample was taken out after cooling, then 60g of sodium hydroxide solid was weighed and 500mL of sodium hydroxide aqueous solution was prepared. The sodium hydroxide aqueous solution was used to etch the alumina template to obtain carbon nanotube array.

[0052] (3) Place the carbon nanotube array on the sample stage of the atomic layer deposition equipment and evacuate the reaction chamber to a vacuum level of 10. -4 Pa, turn on the heating system, heat the reaction chamber to 250℃ at a heating rate of 5℃ / min, then open the SiH₄ valve, and introduce the precursor into the reaction chamber in a pulsed manner through the gas flow controller, with a pulse duration of 1s. Close the SiH₄ valve, introduce nitrogen gas, and purge the reaction chamber to remove unreacted precursor molecules and reaction byproducts. The purging time is 20s. Repeat the above deposition cycle until the silicon layer thickness is 10nm, obtaining a porous silicon carbon material;

[0053] (4) The silicon carbide porous material and lithium metal sheet were used as the electrode and counter electrode, respectively, for battery assembly. Lithium metal was deposited on the silicon carbide porous material by electrochemical deposition at a current density of 0.1 mA cm⁻¹. -2 The deposition time was 10 hours, and the thickness of the deposited lithium metal layer was 6.25 μm, resulting in a three-dimensional porous anode.

[0054] A method for preparing a creep-type all-solid-state lithium metal battery includes the following steps:

[0055] Lithium iron phosphate powder, super P, polyethylene oxide, and lithium bis(trifluoromethanesulfonyl)imide were mixed in acetonitrile at a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry. The resulting lithium iron phosphate slurry was then coated onto carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain lithium iron phosphate cathode material.

[0056] By assembling the positive electrode, LPSCl solid electrolyte, and three-dimensional porous negative electrode into a battery, a creep-type all-solid-state lithium metal battery is obtained.

[0057] The carbon-silicon porous material in Example 1 was subjected to SEM and mapping analysis. The results are shown in Figures 1 and 2. Figure 1 is the SEM image of the carbon-silicon porous material prepared in Example 1, and Figure 2 is the mapping image of the carbon-silicon porous material prepared in Example 1. As can be seen from Figure 1, the nanotubes in the carbon-silicon porous material prepared in Example 1 are vertically arranged with a diameter of 100 nm. As can be seen from Figure 2, Si elements are uniformly distributed on the surface of the nanotubes. Example 2

[0058] This embodiment provides a three-dimensional porous negative electrode and a creep-type all-solid-state lithium metal battery, specifically including the following solutions:

[0059] A method for preparing a three-dimensional porous negative electrode includes the following steps:

[0060] (1) Place the alumina template on the sample stage of the chemical vapor deposition equipment and evacuate the reaction chamber to a vacuum level of 1.5 × 10⁻⁶. -4 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 Torr. The heating system was then turned on, and the reaction chamber was heated at a rate of 10 °C / min until the temperature reached 680 °C. After the temperature and pressure stabilized, acetylene gas was introduced at a flow rate of 150 sccm. The deposition time was 35 min. After the deposition time was completed, the acetylene gas valve was closed, and the carbon nanotube array precursor was obtained after cooling.

[0061] (2) Place the carbon nanotube precursor on the sample stage of the magnetron sputtering equipment, install the platinum target, and evacuate the reaction chamber to a vacuum level of 10. -6 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 mTorr. A DC power supply of 60 W was turned on, and the sputtering time was 15 minutes. After cooling, the sample was removed. Then, 60 g of sodium hydroxide solid was weighed and a 500 mL sodium hydroxide aqueous solution was prepared. The sodium hydroxide aqueous solution was used to etch the alumina template to obtain a carbon nanotube array.

[0062] (3) Place the carbon nanotube array on the sample stage of the atomic layer deposition equipment and evacuate the reaction chamber to a vacuum level of 1.5 × 10⁻⁶. -4 At step 1, turn on the heating system and heat the reaction chamber to 300°C at a heating rate of 10°C / min. Then, open the SiH₄ valve and introduce the precursor into the reaction chamber in a pulsed manner through the gas flow controller, with a pulse duration of 1.5 s. Close the SiH₄ valve, introduce nitrogen gas, and purge the reaction chamber to remove unreacted precursor molecules and reaction byproducts. The purging time is 25 s. Repeat the above deposition cycle until the silicon layer thickness is 10 nm, obtaining a porous silicon-carbon material.

[0063] (4) The porous silicon carbon material and lithium metal sheet were used as the electrode and counter electrode, respectively, for battery assembly. Lithium metal was deposited on the porous silicon carbon material using electrochemical deposition at a current density of 0.5 mA cm⁻¹. -2 The deposition time was 4 hours, and the thickness of the deposited lithium metal layer was 12.5 μm, resulting in a three-dimensional porous anode.

[0064] A method for preparing a creep-type all-solid-state lithium metal battery includes the following steps:

[0065] Lithium iron phosphate powder, super P, polyethylene oxide, and lithium bis(trifluoromethanesulfonyl)imide were mixed in acetonitrile at a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry. The resulting lithium iron phosphate slurry was then coated onto carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain lithium iron phosphate cathode material.

[0066] By assembling the positive electrode, LPSCl solid electrolyte, and three-dimensional porous negative electrode into a battery, a creep-type all-solid-state lithium metal battery is obtained. Example 3

[0067] This embodiment provides a three-dimensional porous negative electrode and a creep-type all-solid-state lithium metal battery, specifically including the following solutions:

[0068] A method for preparing a three-dimensional porous negative electrode includes the following steps:

[0069] (1) Place the alumina template on the sample stage of the chemical vapor deposition equipment and evacuate the reaction chamber to a vacuum level of 0.5 × 10⁻⁶. -4 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 Torr. The heating system was then turned on, and the reaction chamber was heated at a rate of 7 °C / min to reach a temperature of 600 °C. After the temperature and pressure stabilized, acetylene gas was introduced at a flow rate of 50 sccm. The deposition time was 25 min. After the deposition time was completed, the acetylene gas valve was closed, and the carbon nanotube array precursor was obtained after cooling.

[0070] (2) Place the carbon nanotube precursor on the sample stage of the magnetron sputtering equipment, install the platinum target, and evacuate the reaction chamber to a vacuum level of 10. -6 Pa, argon gas was introduced to stabilize the pressure in the reaction chamber at 5 mTorr, DC power was turned on at 40W, sputtering time was 15 minutes, the sample was taken out after cooling, then 60g of sodium hydroxide solid was weighed and 500mL of sodium hydroxide aqueous solution was prepared. The sodium hydroxide aqueous solution was used to etch the alumina template to obtain carbon nanotube array.

[0071] (3) Place the carbon nanotube array on the sample stage of the atomic layer deposition equipment and evacuate the reaction chamber to a vacuum level of 0.5 × 10⁻⁶. -4 Pa, turn on the heating system, heat the reaction chamber to 200℃ at a heating rate of 7℃ / min, then open the SiH₄ valve, and introduce the precursor into the reaction chamber in a pulsed manner through the gas flow controller, with a pulse duration of 0.5s. Close the SiH₄ valve, introduce nitrogen gas, and purge the reaction chamber to remove unreacted precursor molecules and reaction byproducts. The purging time is 15s. Repeat the above deposition cycle until the silicon layer thickness is 5nm, obtaining a porous silicon-carbon material;

[0072] (4) The silicon carbide porous material and lithium metal sheet were used as the electrode and counter electrode, respectively, for battery assembly. Lithium metal was deposited on the silicon carbide porous material by electrochemical deposition at a current density of 0.1 mA cm⁻¹. -2 The deposition time was 50 hours, and the thickness of the deposited lithium metal layer was 30 μm, resulting in a three-dimensional porous anode.

[0073] A method for preparing a creep-type all-solid-state lithium metal battery includes the following steps:

[0074] Lithium iron phosphate powder, super P, polyethylene oxide, and lithium bis(trifluoromethanesulfonyl)imide were mixed in acetonitrile at a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry. The resulting lithium iron phosphate slurry was then coated onto carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain lithium iron phosphate cathode material.

[0075] By assembling the positive electrode, LPSCl solid electrolyte, and three-dimensional porous negative electrode into a battery, a creep-type all-solid-state lithium metal battery is obtained. Example 4

[0076] This embodiment provides a three-dimensional porous negative electrode and a creep-type all-solid-state lithium metal battery, specifically including the following solutions:

[0077] A method for preparing a three-dimensional porous negative electrode includes the following steps:

[0078] (1) Place the alumina template on the sample stage of the chemical vapor deposition equipment and evacuate the reaction chamber to a vacuum level of 0.5 × 10⁻⁶. -4 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 Torr. The heating system was then turned on, and the reaction chamber was heated at a rate of 7 °C / min to reach a temperature of 600 °C. After the temperature and pressure stabilized, acetylene gas was introduced at a flow rate of 50 sccm. The deposition time was 25 min. After the deposition time was completed, the acetylene gas valve was closed, and the carbon nanotube array precursor was obtained after cooling.

[0079] (2) Place the carbon nanotube precursor on the sample stage of the magnetron sputtering equipment, install the platinum target, and evacuate the reaction chamber to a vacuum level of 10. -6 Pa, argon gas was introduced to stabilize the pressure in the reaction chamber at 5 mTorr, DC power was turned on at 50W, sputtering time was 10 minutes, the sample was taken out after cooling, then 60g of sodium hydroxide solid was weighed and 500mL of sodium hydroxide aqueous solution was prepared. The sodium hydroxide aqueous solution was used to etch the alumina template to obtain carbon nanotube array.

[0080] (3) Place the carbon nanotube array on the sample stage of the atomic layer deposition equipment and evacuate the reaction chamber to a vacuum level of 0.5 × 10⁻⁶. -4Pa, turn on the heating system, heat the reaction chamber to 200℃ at a heating rate of 7℃ / min, then open the SiH₄ valve, and introduce the precursor into the reaction chamber in a pulsed manner through the gas flow controller, with a pulse duration of 0.5s. Close the SiH₄ valve, introduce nitrogen gas, and purge the reaction chamber to remove unreacted precursor molecules and reaction byproducts. The purging time is 15s. Repeat the above deposition cycle until the silicon layer thickness is 5nm, obtaining a porous silicon-carbon material;

[0081] (4) The porous silicon carbon material and lithium metal sheet are used as electrodes and counter electrodes, respectively, for battery assembly. The molten filling volume is 1 mg cm³. -2 A three-dimensional porous negative electrode was obtained.

[0082] A method for preparing a creep-type all-solid-state lithium metal battery includes the following steps:

[0083] Lithium iron phosphate powder, super P, polyethylene oxide, and lithium bis(trifluoromethanesulfonyl)imide were mixed in acetonitrile at a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry. The resulting lithium iron phosphate slurry was then coated onto carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain lithium iron phosphate cathode material.

[0084] By assembling the positive electrode, LPSCl solid electrolyte, and three-dimensional porous negative electrode into a battery, a creep-type all-solid-state lithium metal battery is obtained. Comparative Example 1

[0085] This comparative example provides a three-dimensional porous anode and a solid-state lithium metal battery, specifically including the following solutions:

[0086] A method for preparing a three-dimensional porous negative electrode includes the following steps:

[0087] (1) Place the alumina template on the sample stage of the chemical vapor deposition equipment and evacuate the reaction chamber to 10. -4 Argon gas was introduced to stabilize the pressure in the reaction chamber at 5 Torr. The heating system was turned on and the reaction chamber was heated at a rate of 5℃ / min to reach 650℃. After the temperature and pressure stabilized, acetylene gas was introduced at a flow rate of 100 sccm. The deposition time was 30 min. After the deposition time was completed, the acetylene gas valve was closed and the carbon nanotube precursor was obtained after cooling.

[0088] (2) Place the carbon nanotube precursor on the sample stage of the magnetron sputtering equipment, install the platinum target, and evacuate the reaction chamber to a vacuum level of 10. -6Pa, argon gas was introduced to stabilize the pressure in the reaction chamber at 5 mTorr, DC power was turned on at 50W, sputtering time was 10 minutes, the sample was taken out after cooling, 60g of sodium hydroxide solid was weighed and 500mL of sodium hydroxide aqueous solution was prepared, and then the alumina template was etched with sodium hydroxide aqueous solution to obtain carbon nanotube array.

[0089] (3) The carbon nanotube array and lithium metal sheet were used as the electrode and counter electrode, respectively, to assemble the battery. Lithium metal was deposited on the carbon nanotube precursor by electrochemical deposition at a current density of 0.1 mA cm⁻¹. -2 The deposition time was 10 hours, and the thickness of the deposited lithium metal layer was 6.25 μm, resulting in a three-dimensional porous anode.

[0090] A method for preparing a solid-state lithium metal battery includes the following steps:

[0091] Lithium iron phosphate powder, super P, polyethylene oxide, and lithium bis(trifluoromethanesulfonyl)imide were mixed in acetonitrile at a weight ratio of 6:1:2:1 to obtain lithium iron phosphate slurry. The resulting lithium iron phosphate slurry was then coated onto carbon-coated aluminum foil and vacuum dried at 70°C for 12 hours to obtain lithium iron phosphate cathode material.

[0092] A solid-state lithium metal battery is obtained by assembling a positive electrode, an LPSCl solid electrolyte, and a three-dimensional porous negative electrode.

[0093] The electrochemical performance of the creep-type all-solid-state lithium metal battery in Example 1 and the solid-state lithium metal battery in Comparative Example 1 was tested, and the results are shown in Figure 3. Figure 3 shows the electrochemical performance of the creep-type all-solid-state lithium metal battery in Example 1 and the solid-state lithium metal battery in Comparative Example 1. As can be seen from Figure 3, the creep-type all-solid-state lithium metal battery provided in Example 1 can stably cycle 200 times at a 1C rate with a capacity decay rate of 0.18%, while the solid-state lithium metal battery in Comparative Example 1 exhibits rapid capacity decay and poor cycle performance.

[0094] Two three-dimensional porous negative electrodes from Example 1 were used as positive and negative electrodes, respectively, and assembled with LPSCl solid electrolyte to form the half-cell of Example 1. Similarly, two three-dimensional porous negative electrodes from Comparative Example 1 were used as positive and negative electrodes, respectively, and assembled with LPSCl solid electrolyte to form the half-cell of Comparative Example 1. The performance of the half-cells in Example 1 and Comparative Example 1 was compared, and the results are shown in Figure 4. Figure 4 is a performance comparison chart of the half-cells in Example 1 and Comparative Example 1. As can be seen from Figure 4, at 0.2 mAh·cm⁻¹... -1 Under the cycling conditions, the half-cell in Example 1 has a cycle performance of 380 h, while the half-cell in Comparative Example 1 has a cycle performance of 100 h.

[0095] The above are all preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape and principle of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A three-dimensional porous negative electrode material, characterized by, The material includes a silicon carbide porous material having a lithium metal layer disposed thereon. The carbon-silicon porous material includes electronic conductors and ionic conductors, wherein the electronic conductors are carbon nanotube arrays and the ionic conductors are silicon element deposition layers.

2. The three-dimensional porous negative material of claim 1, wherein, The method for preparing the porous silicon carbide material includes the following steps: Silicon was deposited on the surface of a carbon nanotube array using atomic layer deposition to obtain a carbon-silicon porous material.

3. The three-dimensional porous anode material of claim 2, wherein, The deposition vacuum degree of the atomic layer deposition is (0.5-1.5) x 10 -4 Pa, the deposition temperature is 200-300℃, and the heating rate for heating to the deposition temperature is 5-10℃ / min.

4. The three-dimensional porous anode material of claim 2, wherein, The silicon element is deposited by introducing it into the SiH4 silicon precursor in a pulsed manner, wherein the pulse duration is 0.5s-1.5s and the sweep-blowing time is 15s-25s; and / or The thickness of the silicon element deposited by chemical vapor deposition is 5nm-50nm.

5. The three-dimensional porous anode material of claim 2, wherein, The method for preparing the carbon nanotube array includes the following steps: Carbon elements are deposited on the inner surface of an alumina template by chemical vapor deposition, and then the alumina template is removed to obtain a carbon nanotube array.

6. The three-dimensional porous anode material of claim 5, wherein, The deposition vacuum degree of the chemical vapor deposition is (0.5-1.5) x 10 -4 Pa, the deposition temperature is 600-680℃, the heating rate for heating to the deposition temperature is 5-10℃ / min; and / or The deposition atmosphere for the chemical vapor deposition is an argon atmosphere; and / or The carbon element is deposited by introducing acetylene gas; and / or The acetylene gas flow rate is 50 sccm-150 sccm, and the time is 25 min-35 min.

7. A method of producing the three-dimensional porous negative electrode material according to any one of claims 1 to 6, characterized by, Includes the following steps: A three-dimensional porous anode material is obtained by loading a lithium metal layer onto a silicon carbide porous material. The lithium metal layer is loaded onto the porous silicon carbon material by electrochemical deposition or melt infusion.

8. The method of producing a three-dimensional porous negative material according to claim 7, wherein The current density of the electrochemical deposition is 0.1 mA cm -2 -0.5 mA cm -2 for a time of 1 h-50 h; and / or The infusion amount of the melt infusion is 0.026 mg cm -2 -1.5 mg cm -2 .

9. The method of claim 7, wherein the three-dimensional porous negative electrode material is prepared by a process comprising: mixing a carbon material and a binder to form a mixture; and coating the mixture on a substrate to form a film. The thickness of the lithium metal layer is 1μm-30μm.

10. A creep-type all-solid-state lithium metal battery, characterized by, Includes positive electrode, solid electrolyte and negative electrode; The positive electrode includes a positive electrode current collector, a conductive material, a positive electrode solid electrolyte, and a positive electrode active material layer; The solid electrolyte is selected from polymers, oxides, or sulfides; The negative electrode includes the three-dimensional porous negative electrode material according to any one of claims 1-6 or the three-dimensional porous negative electrode material prepared by any one of claims 7-9.