Edge-isolated cut cell and preparation method therefor
By setting isolation and buffer zones below the emission zone in the sliced cells, combined with a pyramid or tower base structure, the problems of carrier recombination and optical reflection loss are solved, thereby improving cell efficiency and photovoltaic module power.
Patent Information
- Application Number
- PCT/CN2026/087349
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-07-31
- Filing Date
- 2026-03-31
- Publication Date
- 2026-11-19
AI Technical Summary
Existing edge isolation technology cannot effectively suppress carrier recombination in sliced cells, resulting in efficiency loss. Furthermore, the existing passivation layer coverage is uneven, leading to optical reflection loss.
Picosecond laser surface treatment combined with acid etching and alkaline etching processes is used to form an isolation region and a buffer zone on the silicon substrate that are lower than the emission region. The surface of the isolation region is a pyramid or tower base structure, and the buffer zone is a slope structure. The passivation layer is uniformly covered, cutting off the carrier transport channel and optimizing the passivation layer coverage effect.
It effectively reduces carrier recombination, improves cell efficiency, reduces optical reflection loss, is compatible with existing production lines, adapts to multi-segmentation modes, and increases photovoltaic module power.
Smart Images

Figure CN2026087349_19112026_PF_FP_ABST
Abstract
Description
An edge-isolated slicing battery and its preparation method Technical Field
[0001] This invention relates to the field of crystalline silicon solar cell technology, and more specifically, to an edge-isolated sliced solar cell and its fabrication method. Background Technology
[0002] In the battery production process, laser cutting is typically used to slice a completed full-cell battery into half-cells or multiple cells, ultimately forming a battery module based on these sliced cells. This method helps increase the effective area of the cells inside the module, reduces the module current, and increases the module voltage, thereby improving the module's efficiency.
[0003] For sliced solar cells, the edges of cells cut by laser exhibit significant carrier recombination, and this recombination becomes increasingly severe as the perimeter-to-area ratio of small-sized cells increases. This is because the laser thermal ablation and mechanical damage caused by cutting the cells create defects on the surface or edges, leading to edge recombination of charge carriers (electrons and holes) at these defects. The edge recombination rate is typically higher than the bulk recombination rate because the defect density in the damaged area is greater, increasing the probability of carrier recombination.
[0004] For high-efficiency cells, such as those with tunneling oxide passivated contact (TOPCon) slicing, the efficiency impact of edge recombination is more significant, leading to problems such as decreased fill factor and cell leakage. To address the efficiency loss caused by slicing, the industry has proposed using atomic layer deposition (ALD) to deposit a certain thickness (approximately 30 nm) of aluminum oxide (AlO2) at the edge of the silicon substrate after slicing. x Edge passivation is performed. However, this technology has the following drawbacks: aluminum oxide coating affects the appearance of the battery; deposition is time-consuming and gas-intensive, with low capacity and high cost; the equipment is incompatible with existing production lines; the efficiency improvement effect is limited, and the cost-effectiveness for industrial applications is low.
[0005] To address the shortcomings of ALD technology, patent document CN202410971803.5 proposes an edge-isolated sliced solar cell and its fabrication method. This method employs laser etching on the front side of a silicon substrate to form PN junction-free isolation regions on both sides of the laser-etched edge of the cell, ensuring the edge is located within these PN junction-free isolation regions. By introducing these PN junction-free isolation regions, the recombination effect at the edge of the slice can be effectively suppressed, reducing the carrier recombination rate and improving the performance of the sliced solar cell.
[0006] However, research has found that existing edge isolation technologies still have the following problems: the laser etching depth is relatively small, and the surface of the PN junction isolation region is basically flat with the surface of the emitter region, which cannot completely cut off the carrier transport channel; if the etching depth is increased, an almost vertical drop structure will appear at the edge of the isolation region, and gaps are prone to appear in the passivation layer during the process of covering the isolation region. These gaps will form new recombination centers, leading to intensified carrier recombination; in addition, after wet etching removes the damage caused by the nanosecond laser, a planar structure or a large-sized textured structure is formed on the surface of the isolation region, resulting in a large optical reflection loss. The above factors will have an adverse effect on battery efficiency. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the technical problem this invention aims to solve is how to optimize the isolation region structure, improve the edge isolation effect and the passivation layer composite effect, thereby improving battery performance.
[0008] To achieve the above objectives, a first aspect of the present invention provides an edge-isolated sliced battery, comprising a silicon substrate, at least one sidewall of the silicon substrate along its length direction having a cut surface, and one side surface of the silicon substrate along its thickness direction having an emitter region, an isolation region, and a buffer zone. An emitter is provided on the emitter region, and a PN junction is formed between the emitter and the silicon substrate. The isolation region is disposed at the edge of the silicon substrate, and the isolation region is provided at least near the edge of the cut surface in the silicon substrate. The surfaces of the isolation region and the buffer zone have no emitter, and the surface height of the isolation region is lower than that of the emitter region. The isolation region and the emitter region are connected through the buffer zone, which has a sloping structure. The surfaces of the emitter, the isolation region, and the buffer zone are covered with a passivation layer.
[0009] This invention provides a sliced battery with a novel edge isolation structure. By setting an isolation region below the emitter region and without emitters on its surface, and using a buffer zone to connect the emitter region and the isolation region, this unique structure cuts off the transport path of minority carriers from the emitter region to the cut surface, reduces the impact of edge recombination on the battery's working area, and improves battery efficiency. The sloping structure of the buffer zone helps the passivation layer to cover more evenly, reduces void formation, lowers the probability of recombination centers, and further optimizes battery performance.
[0010] Furthermore, the slope angle of the buffer zone is 20° to 60°. This angle range ensures that the passivation layer adheres better when the buffer zone transitions between the emitter and isolation zones. It avoids both an unnatural transition due to an excessively small slope angle affecting the passivation layer coverage and material waste due to an excessively large slope angle, thereby effectively improving the passivation layer composite effect and enhancing battery performance.
[0011] Furthermore, the vertical height of the buffer zone is 1–10 μm. This height range ensures effective edge isolation while providing sufficient transition space between the emission region and the isolation region, allowing for smoother carrier transport and reducing recombination.
[0012] Furthermore, the width of the isolation region is 20–1000 μm. This width range ensures effective isolation between the cut surface and the emitter region, suppresses the influence of minority carrier recombination dark current on the working region at the cut location, and can be flexibly adjusted according to different device batteries and application scenarios, thereby improving device performance while also controlling costs.
[0013] Furthermore, both the surface of the isolation zone and the surface of the emission zone are pyramidal structures, with the pyramidal structure being a square pyramid shape. The pyramidal size of the isolation zone is smaller than that of the emission zone. The use of a small-sized pyramidal structure on the surface of the isolation zone reduces optical reflection loss.
[0014] Furthermore, the pyramid height on the surface of the isolation zone is 0.2–2 μm, and the base side length is 0.5–5 μm. This small-sized pyramid surface structure can significantly increase the light absorption area, improve light capture efficiency, and reduce light reflection loss.
[0015] Furthermore, the pyramidal distribution density on the surface of the isolation zone is 3×10⁻⁶. 5 ~1×10 6 pcs / mm 2 The high density of the pyramid distribution helps to increase the contact area between the passivation layer and the isolation region, further suppressing carrier recombination.
[0016] Furthermore, the surface of the isolation zone has a tower-based structure, which is a frustum shape. Compared to a planar structure, the tower-based structure can reduce optical reflection loss and provide a good adhesion base for the passivation layer.
[0017] Furthermore, the height of the tower base on the surface of the isolation region is less than 0.2 μm, and the side length of the tower base is 10–50 μm. Limiting the tower base size optimizes the device's light utilization efficiency and helps improve device performance.
[0018] Furthermore, the passivation layer is a multilayer film of aluminum oxide and silicon nitride. This composite passivation layer has a good passivation effect, which can reduce surface carrier recombination and improve the photoelectric conversion efficiency of solar cells.
[0019] A second aspect of the present invention provides a method for preparing an edge-isolated sliced battery, comprising the following steps:
[0020] A. Provide a silicon substrate, form an emitter on one side surface of the silicon substrate in the thickness direction, form a PN junction between the emitter and the silicon substrate, and the area on the silicon substrate covering the emitter is the emitter region;
[0021] B. Perform picosecond laser surface treatment on the emitter, perform acid etching and alkaline etching on the laser-treated area to remove the corresponding emitter, and change the surface structure of the silicon substrate to form an isolation area and a buffer area. The surface height of the isolation area is lower than that of the emitter area, and the isolation area and the emitter area are connected by a buffer area with a slope structure.
[0022] C. A passivation layer is deposited on the emitter side of the silicon substrate, and the passivation layer continuously covers the emitter, buffer zone, and isolation zone;
[0023] D. Perform laser non-destructive cutting, with the cutting line located within the isolation zone.
[0024] This invention utilizes picosecond laser surface treatment, combined with acid etching and alkaline etching processes, to precisely remove the corresponding emitter and shape the surface structure of the silicon substrate; it forms an isolation region with a surface height lower than the emitter region, effectively cutting off the carrier transport channel from the emitter region to the cut surface, greatly reducing carrier recombination; and simultaneously forms a buffer zone with a slope structure between the isolation region and the emitter region, which helps the passivation layer to cover the substrate surface more uniformly, reducing the probability of recombination centers and further optimizing battery performance.
[0025] Furthermore, in step B, the laser spot type is a Gaussian spot and / or a flat-top spot. Selecting a picosecond laser and restricting the spot type ensures concentrated laser energy, enabling precise control of the etching depth and forming high-quality isolation and buffer zones.
[0026] Furthermore, in step B, when the laser spot type is a Gaussian spot, the laser frequency is 400–6000 kHz, the power is 10–80 W, and the speed is 1000–40000 mm / s.
[0027] Furthermore, in step B, when the laser spot type is a flat-top spot, the laser frequency is 300–6000 kHz, the power is 10–100 W, and the speed is 2000–40000 mm / s.
[0028] Depending on the type of laser spot, the laser process parameters are restricted to achieve a uniform etching effect and form a buffer zone with a natural transition.
[0029] Furthermore, in step B, the slope angle of the formed buffer zone is 20° to 60°. By adjusting the laser process parameters, the slope angle of the buffer zone can be controlled to ensure better adhesion of the passivation layer. This avoids both an unnatural transition due to an excessively small slope angle affecting the passivation layer coverage and material waste due to an excessively large slope angle, thereby effectively improving the passivation layer composite effect and enhancing battery performance.
[0030] Furthermore, in step B, the vertical height of the formed buffer zone is 1–10 μm. By adjusting the laser process parameters, the size of the buffer zone can be controlled, ensuring both edge isolation and sufficient transition space between the emission and isolation regions, allowing for smoother carrier transport and reducing recombination.
[0031] Furthermore, in step B, an alkaline etching process is performed using an alkaline solution containing a texturing aid to form a pyramid structure on the surface of the isolation area. This pyramid structure is a square pyramid shape. The etching process creates a pyramid structure on the surface of the isolation area, which helps reduce optical reflection loss.
[0032] Furthermore, in step B, the height of the pyramid formed on the surface of the isolation zone is 0.2–2 μm, the side length of the base is 0.5–5 μm, and the pyramid distribution density is 3 × 10⁻⁶. 5 ~1×10 6 pcs / mm 2 Small-sized pyramid surface structures can significantly increase the light absorption area, improve light capture efficiency, and reduce light reflection loss; at the same time, controlling the pyramid distribution density is beneficial to increasing the contact area between the passivation layer and the isolation region, further suppressing carrier recombination.
[0033] Furthermore, in step B, an alkaline etching process is performed using an alkaline solution without texturing aids to form a pyramidal structure on the surface of the isolation region. This pyramidal structure, in the form of a truncated square, results in less optical reflection loss compared to a planar structure and provides a good adhesion base for the passivation layer.
[0034] Furthermore, in step B, the height of the tower base formed on the surface of the isolation zone is less than 0.2 μm, and the side length of the tower base is 10–50 μm. Controlling the tower base size can optimize the battery's light utilization efficiency and help improve battery performance.
[0035] This invention addresses the battery manufacturing process, effectively improving the isolation and passivation layer composite effects, reducing optical reflection loss, and enhancing battery performance. Specific beneficial effects are as follows:
[0036] (1) Improve isolation effect and eliminate edge recombination: An isolation region with the emitter completely removed and lower than the emitter area is set at the edge of the cut surface to cut off the carrier transport channel to the cut surface and suppress carrier recombination caused by the defects of the cut surface. This structure can reduce dark current loss, increase open circuit voltage and fill factor, and improve photoelectric conversion efficiency when applied to batteries.
[0037] (2) Optimize the quality of passivation layer coverage and improve the surface passivation effect: The buffer slope provides a smooth transition basis for the deposition of passivation layer, avoiding coverage gaps and defects; the pyramid structure or base structure on the surface of the isolation zone increases the contact area, closely adheres to the passivation layer, reduces the interface recombination center, and improves the surface passivation effect and electrical performance.
[0038] (3) Reduce optical reflection loss: The surface of the isolation zone is a pyramid structure or a base structure, which can increase the absorption and scattering of light, effectively reduce optical reflection loss, and improve the battery's efficiency in utilizing light energy.
[0039] (4) Adaptable to multiple slab division modes and advanced semiconductor device technologies: The manufacturing process is compatible with existing production lines and can be flexibly adapted to slab division modes such as "slice in two" and "slice in three" to meet the design requirements of different components; it is also compatible with TOPCon, BC battery and other technology routes, and can adapt to different battery structures by adjusting parameters to promote the large-scale application of high-efficiency batteries. Attached Figure Description
[0040] Figure 1 is a structural diagram of the cut portion of the sliced battery in one specific embodiment.
[0041] Figure 2 is a structural diagram of the cut portion of the sliced battery in another specific embodiment.
[0042] Figure 3 is a cross-sectional view of a sliced battery structure according to a specific embodiment.
[0043] Figure 4 is a cross-sectional view of a sliced battery structure according to another specific embodiment.
[0044] Figure 5 is a PL diagram of the sample from Example 1.
[0045] Figure 6 shows the surface morphology of the isolation zone of the sample in Example 2.
[0046] Figure 7 is a side view of the edge of the isolation zone of the sample in Example 2.
[0047] Figure 8 is a frontal feature morphology diagram of the edge of the isolation zone of the sample in Example 3.
[0048] Figure 9 is a side view of the edge of the isolation zone of the sample in Example 3.
[0049] Figure 10 shows the surface morphology of the isolation zone of the sample in Example 5.
[0050] Figure 11 is a frontal feature morphology diagram of the edge of the isolation zone of the sample in Example 5.
[0051] Figure 12 is a frontal feature morphology diagram of the edge of the isolation zone of the sample in Example 6.
[0052] Figure 13 shows a photograph of the edge features of the isolation zone of the sample in Comparative Example 3.
[0053] Figure 14 shows a photograph of the edge features of the isolation zone of the sample in Comparative Example 4.
[0054] Explanation of reference numerals in the attached figures: 1-Silicon substrate, 2-Cut surface, 3-Emitter region, 4-Buffer zone, 5-Isolation region, 6-Emitter, 7-First passivation layer, 8-First electrode, 9-Tunneling oxide layer, 10-Doped polysilicon layer, 11-Second passivation layer, 12-Second electrode. Detailed Implementation
[0055] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be noted that the following embodiments are only used to illustrate the implementation methods and typical parameters of the present invention, and are not intended to limit the parameter range described in the present invention. Reasonable variations derived therefrom are still within the protection scope of the claims of the present invention.
[0056] It should be noted that the endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0057] This invention discloses an edge-isolated sliced solar cell and its fabrication method. Referring to Figure 1, the sliced solar cell includes a silicon substrate 1. One or both sidewalls of the silicon substrate 1 along its length have a cut surface 2 created by laser slicing. One surface of the silicon substrate 1 along its thickness direction has an emitter region 3, an isolation region 5, and a buffer zone 4. An emitter 6 is provided on the emitter region 3, forming a PN junction with the silicon substrate 1. The surface of the emitter region 3 has a pyramidal structure. The isolation region 5 is located near the edge of the cut surface 2. The surface height of the isolation region 5 is lower than that of the emitter region 3, and it has no emitter 6. The surface of the isolation region 5 has a pyramidal structure, and the pyramid size is smaller than that of the emitter region 3. The isolation region 5 can cut off the minority carrier transport channel from the emitter region 3 to the cut surface 2, reducing the impact of edge recombination on the emitter region 3. The small-sized pyramidal structure of the isolation region 5 helps reduce optical reflection losses. The buffer zone 4 is located between the emitter region 3 and the isolation region 5, and it has no emitter 6 on its surface. It has a sloping structure, forming a transition connection. A first passivation layer 7 is provided on the surface of the silicon substrate 1 with an emitter 6. The passivation layer covers the emitter 6, the isolation region 5 and the buffer zone 4. The slope structure of the buffer zone 4 helps the first passivation layer 7 to cover more evenly, avoid gaps, and improve the passivation layer composite effect.
[0058] In some specific embodiments, the size of the buffer zone 4 is optimized, and the slope angle of the buffer zone 4 is controlled to be 20° to 60° and the vertical height is 1 to 10 μm. By limiting the size of the buffer zone 4, the edge isolation effect is ensured, and there is enough transition space between the emission area 3 and the isolation area 5 to ensure the coverage effect of the first passivation layer 7 and avoid gaps.
[0059] In some specific embodiments, the surface of the isolation zone 5 is optimized to have a pyramid structure. The pyramid structure is a square pyramid with a height of 0.2–2 μm, a base side length of 0.5–5 μm, and a pyramid distribution density of 3 × 10⁻⁶. 5 ~1×10 6 pcs / mm 2 This surface structure significantly increases the light absorption area, improves light capture efficiency, and reduces light reflection loss; at the same time, it can increase the contact area between the passivation layer and the isolation region 5, further suppressing carrier recombination.
[0060] In some specific embodiments, the size of the isolation region 5 is optimized, and the width of the isolation region 5 is controlled to be 20 to 1000 μm. Sufficient width can effectively isolate the cutting surface 2 from the emission region 3 and suppress the influence of minority carrier recombination dark current on the emission region 3 at the cutting part.
[0061] In some specific embodiments, the structure of the first passivation layer 7 is optimized, and the first passivation layer 7 is limited to an aluminum oxide and silicon nitride stacked thin film. This composite passivation layer can reduce surface carrier recombination and improve the photoelectric conversion efficiency of solar cells.
[0062] In a specific embodiment, the edge-isolated sliced battery described above is fabricated using the following process: A silicon substrate 1 is provided, and an emitter 6 is formed on one side surface of the silicon substrate 1 in the thickness direction. A PN junction is formed between the emitter 6 and the silicon substrate 1, and the area on the silicon substrate 1 covering the emitter 6 is the emitter region 3. The emitter 6 is subjected to picosecond laser surface treatment, and acid etching and alkaline etching are performed on the laser-treated area to remove the corresponding emitter 6 and modify the surface structure of the silicon substrate 1, forming an isolation region 5 and a buffer zone 4. A first passivation layer 7 is deposited on the side surface of the silicon substrate 1 with the emitter 6, and the first passivation layer 7 continuously covers the emitter 6, the buffer zone 4, and the isolation region 5. Laser non-destructive cutting is performed, with the cutting line located within the isolation region 5.
[0063] In a specific embodiment, to form a high-quality isolation zone 5 and buffer zone 4, the laser spot type is selected as either a Gaussian spot or a flat-top spot, and the laser process parameters are adjusted according to the different spot types. Specifically, when the laser spot type is a Gaussian spot, the laser frequency is controlled at 400–6000 kHz, the power at 10–80 W, and the speed at 1000–40000 mm / s; when the laser spot type is a flat-top spot, the laser frequency is controlled at 300–6000 kHz, the power at 10–100 W, and the speed at 2000–40000 mm / s.
[0064] In some embodiments, flat-top light spots and Gaussian light spots can be used in combination. The main part of the isolation area 5 uses a flat-top light spot to achieve a uniform etching effect, while the edge part uses a Gaussian light spot for etching to form a buffer zone 4 with a natural transition.
[0065] In a specific embodiment, in order to form a pyramid structure on the surface of the isolation region 5, an alkaline etching process is performed using an alkaline solution with added texturing aid. By adjusting the etching process, the isolation region 5 with the ideal surface structure can be obtained.
[0066] As shown in Figure 2, this is another implementation of a sliced battery with edge isolation. The main difference from the above implementation is that the surface of the isolation region 5 is a tower-based structure. The tower-based structure also has the effect of reducing light reflection loss compared to the planar structure.
[0067] In a specific embodiment, the tower base structure is optimized to be a frustum shape with a height of less than 0.2 μm and a base side length of 10–50 μm. This effectively reduces optical reflection loss, optimizes the device's light utilization efficiency, and provides a good adhesion foundation for the passivation layer.
[0068] Furthermore, the fabrication processes for semiconductor devices with tower-based and pyramid-shaped structures on the surface of isolation region 5 are basically the same. The main difference is that alkaline etching is performed using an alkaline solution without texturing aids. By matching the chemical etching process with the laser process, an edge isolation structure with excellent surface quality can be obtained.
[0069] The aforementioned slicing cell technology is applicable to various high-efficiency photovoltaic cells, such as TOPCon cells and BC cells, and can be flexibly adapted to slicing modes such as "slice in two" and "slice in three". The isolation structure is located on the side of the device with the PN junction, which can isolate the recombination loss at the cutting edge to the greatest extent, thereby improving the efficiency of the sliced cells and increasing the overall power of the photovoltaic module.
[0070] Referring to Figure 3, taking a two-segment TOPCon cell as an example, the cell includes a silicon substrate 1. Most of the front surface of the silicon substrate 1 has an emitter 6, and the area covering the emitter 6 is the emitter region 3. The surface of the emitter region 3 has a pyramid structure. A first passivation layer 7 covers the entire front surface of the silicon substrate 1, and a first electrode 8 passes through the first passivation layer 7 to contact the emitter 6. The back surface of the silicon substrate 1 is sequentially covered with a tunneling oxide layer 9, a doped polycrystalline silicon layer 10, and a second passivation layer 11. A second electrode 12 passes through the second passivation layer 11 to contact the doped polycrystalline silicon layer 10. One side of the silicon substrate 1 is a cut surface 2. Near the cut surface 2 on the front surface of the silicon substrate 1, there is an isolation structure. The surface of the isolation structure has no emitter 6 and includes an isolation region 5 and a buffer zone 4. The surface height of the isolation region 5 is lower than that of the emitter region 3, and the surface of the isolation region 5 has a small-sized pyramid structure. The isolation region 5 and the emitter region 3 are connected by a sloped buffer zone 4.
[0071] In some embodiments, isolation regions 5 can also be formed on the silicon substrate 1 at edges not near the cut surface 2. Taking a two-piece TOPCon cell as an example, as shown in Figure 4, isolation regions 5 are formed on the silicon substrate 1 at edges near the cut surface 2, and isolation regions 5 are also formed on other edges. This reduces carrier recombination at non-cut edge locations, further improving cell efficiency. The surrounding isolation regions 5 are connected to corresponding buffer zones 4, and the entire front surface of the silicon substrate 1 is uniformly covered with a first passivation layer 7.
[0072] The technical solution and effects of the present invention will be illustrated by specific embodiments below.
[0073] Example 1
[0074] An n-type silicon substrate was prepared, and the front side was texturized and cleaned using standard RCA. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter. A groove was made in the middle region of the front side of the passivation wafer to remove the corresponding portion of the emitter, forming an isolation region. The edges of the isolation region had a near-vertical structure with a vertical height of 3–5 μm. An aluminum oxide film and a silicon nitride film were deposited on the front side of the passivation wafer to form the front passivation layer, resulting in sample (A).
[0075] An n-type silicon substrate was prepared, and the front side was texturized and cleaned using standard RCA. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter. A groove was created in the central area of the passivation wafer's front side to remove the corresponding emitter portion, forming an isolation region. The edges of the isolation region were designed as a buffer zone with a sloped structure, controlling the slope angle to be 65°–75° and the vertical height to be 3–5 μm. An aluminum oxide film and a silicon nitride film were deposited on the front side of the passivation wafer to form the front passivation layer, yielding sample (B).
[0076] An n-type silicon substrate was prepared, and the front side was texturized and cleaned using standard RCA. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter. A groove was created in the central region of the passivation wafer's front side to remove the corresponding emitter portion, forming an isolation region. The edges of the isolation region were designed as a buffer zone with a sloped structure, controlling the slope angle at 20°–30° and the vertical height at 3–5 μm. An aluminum oxide film and a silicon nitride film were deposited on the front side of the passivation wafer to form the front passivation layer, yielding sample (C).
[0077] Prepare an n-type silicon substrate, perform front-side texturing, and standard RCA cleaning. Boron diffusion is performed on the front side of the silicon substrate to form a boron emitter. A groove is created in the central region of the passivation wafer's front side to remove the corresponding emitter portion, forming an isolation region. The edges of the isolation region are sloped buffer zones, with the slope angle controlled at 50°–60° and the vertical height at 3–5 μm. An aluminum oxide film and a silicon nitride film are deposited on the front side of the passivation wafer to form the front passivation layer, yielding sample (D).
[0078] The four samples prepared were subjected to PL testing, and the results are shown in Figure 5. It can be seen that setting a slope buffer at the edge of the isolation zone is beneficial to improving the passivation layer coverage quality and reducing the interface recombination center. The effect is best when the slope angle of the buffer is 50° to 60°.
[0079] Example 2
[0080] An n-type silicon substrate was prepared, with texturing on the front side and polishing on the back side, followed by standard RCA cleaning. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter. Etching was then performed on the back side to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut lines on the passivation wafer. The laser spot type was a flat-top spot, the laser frequency was 3000kHz, the power was 30W, and the speed was 10000mm / s, removing the emitter at the corresponding position. Acid etching and alkaline etching were then performed sequentially on the laser-treated area to form an isolation region approximately 200μm wide. The surface structure of the isolation region is shown in Figure 6. The base is a truncated pyramid shape with a height of less than 0.1μm and a base side length of approximately 20μm. The two edges of the isolation region form a buffer zone with a sloping structure, as shown in Figure 7. The vertical height of the buffer zone is approximately 3.2μm, and the slope angle is approximately 30°. An aluminum oxide thin film is prepared on the front side of the passivation wafer, followed by the deposition of silicon nitride thin films on both sides. The passivation wafer is then subjected to double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced solar cells.
[0081] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 737.2mV, short-circuit current density (J) sc = 41.13 mA / cm 2 The fill factor (FF) is 86.15% and the efficiency (Eff) is 26.42%.
[0082] Ten 108-cell half-cell battery modules were fabricated using the sliced battery prepared in Example 2. Each battery module measures 9.1cm × 18.2cm. The average power of the modules was tested to be 445.9W.
[0083] Example 3
[0084] An n-type silicon substrate was prepared, and texturing was performed on the front side, followed by polishing on the back side and standard RCA cleaning. Boron diffusion was applied to the front side of the silicon substrate to form a boron emitter. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut line on the passivation wafer. The laser spot type was Gaussian, the laser frequency was 3000 kHz, the power was 30 W, and the speed was 10000 mm / s, removing the emitter at the corresponding position. Backside etching was performed to remove the borosilicate glass. Nano-silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. The laser-treated area was then sequentially etched with acid and alkali to form an isolation region approximately 200 μm wide. The surface of the isolation region formed a tower-based structure with a height of less than 0.1 μm and a base side length of approximately 20 μm. The two sides of the isolation region formed a buffer zone with a sloping structure, the front morphology of which is shown in Figure 8. The edges of the buffer zone and the isolation region were smooth. The side profile is shown in Figure 9. The buffer zone has a vertical height of approximately 3.6 μm and a slope angle of approximately 55°. An aluminum oxide film is prepared on the front side of the passivation sheet, followed by double-sided deposition of silicon nitride films. The passivation sheet undergoes double-sided metallization. Laser cutting is performed along the pre-defined cutting lines to obtain two sliced cells.
[0085] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 738.0mV, short-circuit current density (J) sc = 41.10 mA / cm 2 The fill factor (FF) is 86.64% and the efficiency (Eff) is 26.46%.
[0086] Ten 108-cell half-cell battery modules were fabricated using the sliced battery prepared in Example 3. Each battery module measures 9.1cm × 18.2cm. The average power of the modules was tested to be 446.7W.
[0087] Example 4
[0088] An n-type silicon substrate was prepared, and the front side was texturized, the back side polished, and cleaned using standard RCA. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter. The back side was etched to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut lines on the passivation wafer. The laser spot type was a Gaussian spot, the laser frequency was 2000kHz, the power was 35W, and the speed was 5000mm / s, removing the emitter at the corresponding position. The laser-treated area was then sequentially etched with acid and alkali to form an isolation region approximately 100μm wide. The surface of the isolation region formed a tower-based structure with a height less than 0.2μm and a base side length of approximately 10μm. The two edges of the isolation region formed a buffer zone with a slope structure, a vertical height of approximately 5.0μm, and a slope angle of approximately 60°. An alumina film was prepared on the front side of the passivation wafer, followed by double-sided deposition of silicon nitride films. The passivated sheet is then metallized on both sides. Laser cutting is performed along the pre-defined cutting lines to obtain two sliced cells.
[0089] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 737.8mV, short-circuit current density (J) sc = 41.12 mA / cm 2 The fill factor (FF) is 86.53% and the efficiency (Eff) is 26.45%.
[0090] Example 5
[0091] An n-type silicon substrate was prepared, and texturing was performed on the front side, followed by polishing on the back side and standard RCA cleaning. Boron diffusion was applied to the front side of the silicon substrate to form a boron emitter. Etching was then performed on the back side to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut lines on the passivation wafer. The laser spot type was a flat-top spot, the laser frequency was 4000kHz, the power was 40W, and the speed was 20000mm / s, removing the emitter at the corresponding location. Acid etching and alkaline etching were then performed sequentially on the laser-treated area. A texturing aid was added to the alkaline solution to form an isolation region approximately 200μm wide. The surface of the isolation region had a pyramidal structure, as shown in Figures 10 and 11. The pyramid was a square pyramid with a height of approximately 1μm, a base side length of approximately 2μm, and a distribution density of approximately 6×10⁻⁶. 5 pcs / mm 2The isolation zone has sloping buffer zones on both sides, with a vertical height of approximately 4 μm and a slope angle of approximately 25°. An aluminum oxide film is prepared on the front side of the passivation sheet, followed by double-sided deposition of silicon nitride films. The passivation sheet undergoes double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced cells.
[0092] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 737.5mV, short-circuit current density (J) sc = 41.11 mA / cm 2 The fill factor (FF) is 86.37% and the efficiency (Eff) is 26.43%.
[0093] Ten 108-cell half-cell battery modules were fabricated using the sliced battery prepared in Example 5. Each battery module measures 9.1cm × 18.2cm. The average power of the modules was measured to be 446.2W.
[0094] Example 6
[0095] An n-type silicon substrate was prepared, and texturing was performed on the front side, followed by polishing on the back side and standard RCA cleaning. Boron diffusion was applied to the front side of the silicon substrate to form a boron emitter. Etching was then performed on the back side to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut lines on the passivation wafer. The laser spot type was a Gaussian spot, the laser frequency was 3000kHz, the power was 30W, and the speed was 10000mm / s, removing the emitter at the corresponding location. Acid etching and alkaline etching were then performed sequentially on the laser-treated area. A texturing aid was added to the alkaline solution to form an isolation region approximately 100μm wide. The surface of the isolation region had a pyramidal structure, as shown in Figure 12. The pyramid was a square pyramid with a height of approximately 1μm, a base side length of approximately 2μm, and a distribution density of approximately 6×10⁻⁶. 5 pcs / mm 2 The isolation zone has sloping buffer zones on both sides, with a vertical height of approximately 4 μm and a slope angle of approximately 55°. An alumina film is prepared on the front side of the passivation sheet, followed by double-sided deposition of silicon nitride films. The passivation sheet undergoes double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced cells.
[0096] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 738.3mV, short-circuit current density (J) sc = 41.06 mA / cm 2The fill factor (FF) is 87.02% and the efficiency (Eff) is 26.51%.
[0097] Ten 108-cell half-cell battery modules were fabricated using the sliced battery prepared in Example 6. Each battery module measures 9.1cm × 18.2cm. The average power of the modules was tested to be 447.0W.
[0098] Example 7
[0099] An n-type silicon substrate was prepared, and texturing was performed on the front side, followed by polishing on the back side and standard RCA cleaning. Boron diffusion was applied to the front side of the silicon substrate to form a boron emitter. Etching was then performed on the back side to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut lines on the passivation wafer. The laser spot type was a Gaussian spot, the laser frequency was 3000kHz, the power was 45W, and the speed was 20000mm / s, removing the emitter at the corresponding location. Acid etching and alkaline etching were then performed sequentially on the laser-treated area. A texturing aid was added to the alkaline solution to form an isolation region approximately 200μm wide. The surface of the isolation region had a pyramid structure, approximately 2μm high, with a base side length of approximately 4μm and a distribution density of approximately 2×10⁻⁶. 5 pcs / mm 2 The isolation zone has sloping buffer zones on both sides, with a vertical height of approximately 5 μm and a slope angle of approximately 45°. An aluminum oxide film is prepared on the front side of the passivation sheet, followed by double-sided deposition of silicon nitride films. The passivation sheet undergoes double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced cells.
[0100] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 738.1mV, short-circuit current density (J) sc = 41.08 mA / cm 2 The fill factor (FF) is 86.81% and the efficiency (Eff) is 26.48%.
[0101] Comparative Example 1
[0102] An n-type silicon substrate was prepared, with texturing on the front side and polishing on the back side, followed by standard RCA cleaning. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter; the back side was etched to remove the borosilicate glass. Nanoscale silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. An alumina film was prepared on the front side of the passivation wafer, followed by double-sided deposition of silicon nitride films. The passivation wafer underwent double-sided metallization. Laser cutting was performed along pre-defined cutting lines to obtain two sliced cells. ALD was used to deposit a 30nm thick alumina on the cut surfaces.
[0103] 2000 solar cells were prepared using the above method. The performance of the solar cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V... oc ) = 732.1mV, short-circuit current density (J) sc = 41.80 mA / cm 2 The fill factor (FF) is 85.26% and the efficiency (Eff) is 25.71%.
[0104] Ten 108-cell half-cell modules were fabricated using the sliced cells prepared in Comparative Example 1. Each module measures 9.1cm × 18.2cm. The average power output of the modules was measured to be 439.7W.
[0105] Comparative Example 2
[0106] An n-type silicon substrate was prepared, and the front side was texturized, the back side polished, and cleaned using standard RCA. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter; the back side was etched to remove the borosilicate glass. Nanoscale silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A nanosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut line on the passivation wafer. The laser spot type was a flat-top spot, the laser frequency was 3000kHz, the power was 30W, and the speed was 10000mm / s, removing the emitter at the corresponding position. Acid and alkaline etching were sequentially performed on the laser-treated area to form an isolation region approximately 200μm wide with a planar surface. The edges of the isolation region were nearly vertical, with a vertical height of less than 1μm. An aluminum oxide film was prepared on the front side of the passivation wafer, followed by double-sided deposition of silicon nitride films. The passivation wafer was then double-sided metallized. Laser cutting was performed along the pre-cut line to obtain two sliced cells.
[0107] 2000 solar cells were prepared using the above method. The performance of the solar cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V... oc ) = 734.6mV, short-circuit current density (J) sc = 41.58 mA / cm 2The fill factor (FF) is 85.66% and the efficiency (Eff) is 25.88%.
[0108] Using the sliced cells prepared in Comparative Example 2, ten 108 half-cell battery modules were fabricated, each module measuring 9.1cm × 18.2cm. The average power of the modules was tested to be 441.5W.
[0109] Comparative Example 3
[0110] An n-type silicon substrate was prepared, and texturing was performed on the front side, followed by polishing on the back side and standard RCA cleaning. Boron diffusion was applied to the front side of the silicon substrate to form a boron emitter; etching was performed on the back side to remove the borosilicate glass. Nano-sized silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. A picosecond laser surface treatment was performed on a region of a certain width corresponding to the pre-cut line on the passivation wafer. The laser spot type was a flat-top spot, the laser frequency was 6000kHz, the power was 150W, and the speed was 40000mm / s, removing the emitter at the corresponding position. Acid etching and alkaline etching were performed sequentially on the laser-treated area to form an isolation region with a width of approximately 100μm. The surface of the isolation region has a tower-based structure, with the tower base being a quadrangular frustum shape, less than 0.1μm in height, and the base side length approximately 20μm. The two edges of the isolation region have a nearly vertical structure, and its side morphology is shown in Figure 13, with a vertical height of approximately 5μm. An aluminum oxide thin film is prepared on the front side of the passivation wafer, followed by the deposition of silicon nitride thin films on both sides. The passivation wafer is then subjected to double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced solar cells.
[0111] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 735.4mV, short-circuit current density (J) sc = 41.37 mA / cm 2 The fill factor (FF) is 85.95% and the efficiency (Eff) is 26.14%.
[0112] Using the sliced cells prepared in Comparative Example 3, ten 108 half-cell battery modules were fabricated, each module measuring 9.1cm × 18.2cm. The average power output of the modules was measured to be 442.6W.
[0113] Comparative Example 4
[0114] An n-type silicon substrate was prepared, with texturing on the front side and polishing on the back side, followed by standard RCA cleaning. Boron diffusion was performed on the front side of the silicon substrate to form a boron emitter; the back side was etched to remove the borosilicate glass. A picosecond laser surface treatment was applied to an area of a certain width corresponding to the pre-cut line on the passivation wafer. The laser spot type was a Gaussian spot, the laser frequency was 5000 kHz, the power was 100 W, and the speed was 20000 mm / s, removing the emitter at the corresponding position. The back side was etched to remove the borosilicate glass. Nano-silicon oxide and phosphorus-doped amorphous silicon were sequentially deposited on the back side, followed by annealing at 900℃ for 30 minutes to obtain a TOPCon structure passivation wafer. The laser-treated area was then sequentially etched with acid and alkali to form an isolation region approximately 200 μm wide. The surface of the isolation region formed a tower-based structure with a height less than 0.1 μm and a base side length of approximately 20 μm. The two edges of the isolation region formed a buffer zone with a sloping structure. Its front morphology is shown in Figure 14. The edges of the buffer zone and the isolation region are uneven, exhibiting a zigzag structure. The buffer zone has a vertical height of approximately 4 μm and a slope angle of approximately 60°. An aluminum oxide film is prepared on the front side of the passivation sheet, followed by double-sided deposition of silicon nitride films. The passivation sheet undergoes double-sided metallization. Laser cutting is performed along pre-defined cutting lines to obtain two sliced cells.
[0115] 2000 sliced cells were prepared using the above method. The performance of the sliced cells was tested using Suns-Voc. The average performance test results of the samples are as follows: Open circuit voltage (V oc ) = 736.7mV, short-circuit current density (J) sc = 41.26 mA / cm 2 The fill factor (FF) is 86.05% and the efficiency (Eff) is 26.28%.
[0116] Table 1. Comparison of battery performance between the examples and comparative examples.
[0117] The device performance of Examples 2-7 and Comparative Examples 1-4 is shown in Table 1 above. The test results demonstrate that applying the technology of this invention to batteries can effectively improve the performance of sliced batteries, significantly reduce battery efficiency losses caused by the slicing process, and increase the power of photovoltaic modules.
[0118] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A sliced battery with edge isolation, characterized in that, The device includes a silicon substrate, at least one sidewall along the length direction of the silicon substrate has a diced surface, and one side surface along the thickness direction of the silicon substrate has an emitter region, an isolation region, and a buffer zone. An emitter is provided on the emitter region, and a PN junction is formed between the emitter and the silicon substrate. The isolation region is located at the edge of the silicon substrate, and the isolation region is located at least near the edge of the diced surface. The surfaces of the isolation region and the buffer zone have no emitter. The surface height of the isolation region is lower than that of the emitter region. The isolation region and the emitter region are connected through the buffer zone, which has a sloping structure. The surfaces of the emitter, the isolation region, and the buffer zone are covered with a passivation layer.
2. The edge-isolated sliced battery according to claim 1, characterized in that, The slope angle of the buffer zone is 20° to 60°.
3. The edge-isolated sliced battery according to claim 1, characterized in that, The vertical height of the buffer zone is 1–10 μm.
4. The edge-isolated sliced battery according to claim 1, characterized in that, The width of the isolation zone is 20–1000 μm.
5. The edge-isolated sliced battery according to any one of claims 1-4, characterized in that, The surface of the isolation zone is a pyramid structure, and the surface of the launch zone is a pyramid structure. The pyramid structure is a square pyramid shape, and the pyramid size of the isolation zone is smaller than the pyramid size of the launch zone.
6. The edge-isolated sliced battery according to claim 5, characterized in that, The height of the pyramid on the surface of the isolation zone is 0.2–2 μm, and the side length of the base is 0.5–5 μm.
7. The edge-isolated sliced battery according to claim 6, characterized in that, The pyramid distribution density of the isolation region surface is 3 x 10 5 ~1 x 10 6 mm 2 .
8. The edge-isolated sliced battery according to any one of claims 1-4, characterized in that, The surface of the isolation zone is a tower base structure, which is a truncated quadrangular shape.
9. The edge-isolated sliced battery according to claim 8, characterized in that, The height of the tower base on the surface of the isolation zone is less than 0.2 μm, and the side length of the tower base is 10–50 μm.
10. The edge-isolated sliced battery according to any one of claims 1-4, characterized in that, The passivation layer is a laminated thin film of aluminum oxide and silicon nitride.
11. A method for preparing an edge-isolated sliced battery, characterized in that, Includes the following steps: A. Provide a silicon substrate, form an emitter on one side surface of the silicon substrate in the thickness direction, form a PN junction between the emitter and the silicon substrate, and the area on the silicon substrate covering the emitter is the emitter region; B. Perform picosecond laser surface treatment on the emitter, perform acid etching and alkaline etching on the laser-treated area to remove the corresponding emitter, and change the surface structure of the silicon substrate to form an isolation area and a buffer area. The surface height of the isolation area is lower than that of the emitter area, and the isolation area and the emitter area are connected by a buffer area with a slope structure. C. A passivation layer is deposited on the emitter side of the silicon substrate, and the passivation layer continuously covers the emitter, buffer zone, and isolation zone; D. Perform laser non-destructive cutting, with the cutting line located within the isolation zone.
12. The preparation method according to claim 11, characterized in that, In step B, the laser spot type is a Gaussian spot and / or a flat-top spot.
13. The preparation method according to claim 12, characterized in that, In step B, when the laser spot type is a Gaussian spot, the laser frequency is 400–6000 kHz, the power is 10–80 W, and the speed is 1000–40000 mm / s.
14. The preparation method according to claim 12, characterized in that, In step B, when the laser spot type is a flat-top spot, the laser frequency is 300–6000 kHz, the power is 10–100 W, and the speed is 2000–40000 mm / s.
15. The preparation method according to any one of claims 11-14, characterized in that, In step B, the slope angle of the buffer zone is 20° to 60°.
16. The preparation method according to claim 15, characterized in that, In step B, the vertical height of the buffer zone formed is 1 to 10 μm.
17. The preparation method according to claim 11, characterized in that, In step B, an alkaline solution with added texturing aid is used for alkaline etching to form a pyramid structure on the surface of the isolation area. The pyramid structure is a four-sided pyramid.
18. The preparation method according to claim 17, characterized in that, The pyramid height formed on the surface of the isolation region in step B is 0.2-2 μm, the base length of the pyramid is 0.5-5 μm, and the pyramid distribution density is 3×10 5 -1×10 6 / mm 2 .
19. The preparation method according to claim 11, characterized in that, In step B, an alkaline solution without texturing aids is used for alkaline etching to form a tower base structure on the surface of the isolation area. The tower base structure is a truncated quadrangular shape.
20. The preparation method according to claim 19, characterized in that, In step B, the height of the tower base formed on the surface of the isolation zone is less than 0.2 μm, and the side length of the tower base is 10–50 μm.