Multi-layer printed circuit board and manufacturing method for multi-layer printed circuit board
By exposing the conductive layer, insulating layer, and resin layer in the through-hole of a multilayer printed circuit board and forming an insulating opening on the back side, the problem of residual copper plating is solved by using the resin layer to remove excess copper plating, thus improving the signal transmission quality.
Patent Information
- Application Number
- PCT/CN2026/090950
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-19
AI Technical Summary
Existing multilayer printed circuit boards suffer from stub effect during signal transmission, which affects signal quality and is particularly difficult to solve effectively in high-performance devices such as AI servers.
A multilayer printed circuit board with a specific structure achieves zero residual solder joints by exposing the surfaces of conductive, insulating, and resin layers formed in through-holes and forming insulating openings on the back side. Only a small amount of copper plating adheres to the resin layer, and excess copper plating is removed by back drilling.
It significantly improved signal transmission quality, reduced the impact of residual stakes on signal transmission, achieved a zero-residual-stake effect, and improved signal integrity.
Smart Images

Figure CN2026090950_19112026_PF_FP_ABST
Abstract
Description
Multilayer printed circuit boards and their manufacturing methods Technical Field
[0001] This invention relates to multilayer printed circuit boards, and more particularly to multilayer printed circuit boards suitable for use in high-performance devices (e.g., substrates for artificial intelligence (AI) servers). Background Technology
[0002] In printed circuit boards (PCBs), conductor patterns used to connect components are formed on or within an insulating substrate through printing, according to the circuit design. Electronic components are then positioned and soldered. In recent years, the miniaturization of electronic products such as mobile phones, portable electronic terminals, and personal computers has demanded higher density PCBs used within these products. Especially with the rapid development of AI technology in recent years, the performance requirements for servers are increasing daily, placing higher demands on both the speed and quality of signal transmission.
[0003] Regarding multilayer printed circuit boards (PCBs), to cope with the increasing component mounting density and the complexity of circuit wiring, a multilayer PCB is formed by alternating layers of insulating resin and conductive layers (circuit wiring) printed with circuit patterns. Multiple conductive layers are connected using through-holes (TH), which penetrate between layers (referred to as through-holes in this invention) and are plated with a conductive material (see "Platement Process" below). These through-holes are formed by plating after stacking insulating and conductive layers and drilling (one-time drilling), and the entire through-hole is plated with a conductive material through this plating process.
[0004] When plating a through-hole as a whole, if there are sections where the conductive layer connection is undesirable, back drilling (also known as reverse drilling) is performed from the reverse side to remove excess hole wall (secondary drilling). However, due to limitations in back drilling process precision, it is difficult to completely remove excess hole wall. Typically, a short section of copper-plated hole wall is left, known as a stub. The presence of this stub can cause signal reflection, scattering, and delay, thus affecting the integrity of signal transmission; this is called the "stub effect" or "stub effect." This is especially problematic for high-performance devices such as AI servers, where minimizing or eliminating these effects is desirable. Some literature has proposed using non-platable electrical isolation layers to achieve electrical separation of the through-hole structure; however, it is currently difficult to achieve non-platable electrical isolation layers, and therefore, this approach has not been adopted in actual production.
[0005] For example, Patent Document 1 discloses a multilayer printed circuit board in which one or more gaps are systematically created within the via structure by an electroplated protective layer, thereby preventing the placement of conductive material. As a result, the placement of conductive material within the via structure can be limited to areas where electrical signal transmission is required. Furthermore, according to a specific embodiment, by dividing the via structure into physically isolated portions, the pattern winding performance or wiring density of the printed circuit board design can be significantly improved. By using the physically isolated portions of the divided vias, signals from multiple layers associated with that specific portion can be electrically connected.
[0006] Furthermore, the electroplated protective layer used in the formation of the multilayer printed circuit board in Patent Document 1 can be made of hydrophobic insulating materials such as silicone resin, polyethylene resin, fluorocarbon resin, polyurethane resin, and acrylic resin. The hydrophobicity of such an electroplated protective layer is used to prevent the accumulation of catalyst nuclei (seed crystals).
[0007] Existing technical documents
[0008] Patent documents
[0009] Patent Document 1: CN100587921C Publication Summary of the Invention
[0010] The problem the invention aims to solve
[0011] Patent document 1 describes how, although the hydrophobicity of the electroplated protective layer prevents the accumulation of catalyst nuclei (seed crystals), it cannot completely prevent accumulation. When a small amount of accumulation occurs, post-processing is required to remove the residual deposits. Therefore, this multilayer printed circuit board has room for further improvement in terms of its structure and process.
[0012] The purpose of this invention is to provide a multilayer printed circuit board, which has a conductive layer, an insulating layer, and a resin layer as an inner layer. This multilayer printed circuit board can achieve zero stubs, thereby significantly improving the quality of signal transmission and achieving unexpected technical effects. Furthermore, the purpose of this invention is to provide a method for manufacturing the above-mentioned multilayer printed circuit board.
[0013] Solution for solving the problem
[0014] In order to solve the above-mentioned problems, the inventors conducted in-depth research and found that the above-mentioned problems could be solved by using the following multilayer printed circuit board with a specific structure, thereby completing the present invention.
[0015] That is, the present invention is a multilayer printed circuit board as follows.
[0016] [1]. A multilayer printed circuit board, comprising a conductive layer, an insulating layer, and a resin layer as an inner layer, characterized in that...
[0017] The multilayer printed circuit board has through holes, exposing the surfaces of the conductive layer, the insulating layer, and the resin layer.
[0018] The front side of the multilayer printed circuit board in the thickness direction has a through hole formed by plating a conductive material onto the surface of the conductive layer and the insulating layer of the through hole.
[0019] The back side of the multilayer printed circuit board in the thickness direction has an insulating opening formed by reverse drilling to the back side of the resin layer in the thickness direction and cutting out from the back side surface of the through hole.
[0020] [2]. The multilayer printed circuit board according to [1], wherein the resin layer as the inner layer is located inside the insulating layer.
[0021] [3]. The multilayer printed circuit board according to [1] or [2], wherein the resin layer is directly stacked with a conductive layer that is closer to the front side of the multilayer printed circuit board than the resin layer.
[0022] [4]. The multilayer printed circuit board according to [1] or [2], wherein the resin layer is formed from a cured resin composition.
[0023] [5]. The multilayer printed circuit board according to [1] or [2], wherein the conductive material is plated with copper.
[0024] [6]. The multilayer printed circuit board according to [1] or [2], wherein the vias and the insulating openings are filled with a cured material, the cured material being formed from a resin composition for filling vias.
[0025] [7]. The multilayer printed circuit board according to [1] or [2], wherein, from the perspective of a side view, the resin layer extends through the diameter of the through hole.
[0026] [8]. The multilayer printed circuit board according to [1] or [2], wherein, from a top view perspective, the resin layer has an area that allows it to completely cover the entire through-hole.
[0027] [9]. An electronic device, characterized in that it comprises any one of [1] to [8] a multilayer printed circuit board.
[0028]
[0010] . A method for manufacturing a multilayer printed circuit board, characterized in that the manufacturing method includes:
[0029] The process of forming a multilayered laminate, wherein the laminate comprises a conductive layer, an insulating layer, and a resin layer as an inner layer.
[0030] A process of pressing a laminate comprising the conductive layer, the insulating layer and the resin layer;
[0031] For the pressed laminate, a process of forming through holes in a manner that penetrates the laminate, thereby exposing the surfaces of the conductive layer, the insulating layer and the resin layer.
[0032] The process of plating through holes;
[0033] The reverse drilling process involves removing a portion of the resin layer to form a through hole and an insulating opening in the following manner.
[0034] The via is formed on the front side of the multilayer printed circuit board in the thickness direction. The via is formed by depositing conductive material onto the surfaces of the conductive layer and the insulating layer of the via.
[0035] The insulating opening is formed on the back side in the thickness direction of the multilayer printed circuit board. The insulating opening is formed by reverse drilling to the back side in the thickness direction of the resin layer and cutting it out from the back side surface of the through hole.
[0036]
[0011] . The method for manufacturing a multilayer printed circuit board according to
[0010] further includes a step of filling the vias and the insulating openings with a cured material formed of a via-filling resin composition.
[0037] The effects of the invention
[0038] Regarding the multilayer printed circuit board of the present invention, after copper plating of the through holes, since the copper plating is only a small amount and not tightly attached to the resin layer, the copper plating attached to the unremoved resin layer will be removed due to the following reasons during back drilling, thereby achieving zero residual holes, significantly improving the quality of signal transmission, and achieving unexpected technical effects. Attached Figure Description
[0039] Figure 1 is a cross-sectional schematic diagram of a multilayer printed circuit board before the formation of through holes, illustrating one embodiment of the present invention.
[0040] Figure 2 is a cross-sectional schematic diagram showing a multilayer printed circuit board with through holes formed according to an embodiment of the present invention.
[0041] Figure 3 is a cross-sectional schematic diagram showing a multilayer printed circuit board after copper plating following the formation of through holes according to one embodiment of the present invention.
[0042] Figure 4 is a cross-sectional schematic diagram showing a multilayer printed circuit board of one embodiment of the present invention after back drilling after copper plating of through holes.
[0043] Figure 5 is a cross-sectional schematic diagram showing a multilayer printed circuit board of one embodiment of the present invention being filled with a resin composition for filling holes after back drilling. Detailed Implementation
[0044] In a multilayer printed circuit board, conductive and insulating layers in a circuit pattern are alternately stacked, and through-holes are formed to facilitate conduction between the conductive layers. In the multilayer printed circuit board of the present invention, the through-holes expose the surfaces of the conductive layer, the insulating layer, and the resin layer. The front side of the multilayer printed circuit board in the thickness direction has a conductive hole formed by plating a conductive material onto the surfaces of the conductive layer and the insulating layer of the through-hole (i.e., the exposed surfaces of the conductive layer and the insulating layer on the side of the through-hole). The back side of the multilayer printed circuit board in the thickness direction has an insulating opening formed by reverse drilling to the back side of the resin layer in the thickness direction and cutting out from the back side surface of the through-hole.
[0045] Here, "front side" refers to the surface of a multilayer circuit board (e.g., a stack with N layers) containing the first layer (Layer 1), which is also the surface the drill bit enters during a single drilling operation. Correspondingly, "back side" refers to the surface of the multilayer circuit board containing the Nth layer (Layer N), which is also the surface the drill bit enters during back drilling.
[0046] The term "inner layer" refers to the resin layer located inside the multilayer circuit board, specifically within the space sandwiched between the front and back sides. This resin layer is directly laminated to a conductive layer that is closer to the front side of the multilayer printed circuit board than the resin layer itself; this structure is preferred due to its simpler manufacturing process. Furthermore, the resin layer is formed from a cured resin composition that allows only trace amounts of copper plating to adhere. This structure can be obtained using any known method. For example, the resin layer can be formed on a conductive layer using a resin composition, and a prepreg of an insulating layer can be formed on another conductive layer. The two layers can then be laminated together with the resin layer facing the insulating layer and subjected to hot pressing.
[0047] Furthermore, the multilayer circuit board of the present invention is preferably formed such that the through-hole extends entirely through the resin layer. That is, from the perspective of a side view (as shown in Figures 2-5), the resin layer extends through the entire diameter of the through-hole. From the perspective of a top view (not shown in the figures), the resin layer has an area that is at least large enough to completely cover the entire through-hole. Thus, the excess copper plating that adheres to, for example, the surface of an insulating layer in the prior art is adhered to the surface of the resin layer in the present invention. Since the copper plating on the resin layer is only a small amount and not tightly adhered, when the lower part of the resin layer is removed during the back-drilling process, the copper plating attached to the unremoved resin layer will be removed due to collateral damage, thereby minimizing copper residue and reducing the impact on signal transmission to a minimum. Thus, the amount of copper adhering to the exposed surface of the resin layer can be minimized as much as possible, thereby minimizing or even eliminating the aforementioned residual pile effect.
[0048] It should be noted that in this invention, "zero residual stake" does not mean that there is no copper attached to the resin layer at all. Rather, it means that most of the copper has been removed compared to the residual stake portion in the prior art, thereby reducing the impact of the residual stake on signal transmission to a negligible level.
[0049] Furthermore, the resin composition for the resin layer of the present invention comprises a thermosetting resin, a fluororesin, and an inorganic filler. An example of an embodiment of the multilayer printed circuit board of the present invention is illustrated with Figures 1 to 5. These figures show cross-sections of portions formed by alternating layers of conductive layers (i.e., wiring portions) and insulating layers in a circuit pattern.
[0050] As shown in Figure 1, a multilayer printed circuit board is fabricated by hot-pressing a prepreg 4 sandwiching an insulating layer between substrates 3A and 3B. Substrate 3A has a conductive layer 1B with a circuit pattern and an insulating layer 2A. Substrate 3B has a conductive layer 1C with a circuit pattern and an insulating layer 2B. A resin layer 5, formed by coating and curing a resin composition, is disposed above the prepreg 4 and below the conductive layer 1B. The prepreg 4 of the insulating layer functions to insulate the conductive layer and therefore also corresponds to the insulating layer of this invention. The multilayer printed circuit board shown in Figure 1 is fabricated by hot-pressing a prepreg 4 sandwiching an insulating layer between substrates 3A and 3B.
[0051] Next, as shown in Figure 2, a drill bit is used to drill through the entire multilayer printed circuit board (one-time drilling) to form a through-hole 6. The inner wall of the through-hole 6 includes the exposed surface of the conductive layer, the exposed surface of the resin layer, and the exposed surface of the insulating layer.
[0052] Then, after performing, for example, desmearing treatment, chemical plating and / or electroplating of copper are performed to form copper-plated through holes 6A, conductive layer 1A, and conductive layer 1D as shown in FIG3, with substrate 3A becoming substrate 3A' and substrate 3B becoming substrate 3B'.
[0053] Next, as shown in Figure 4, a secondary drilling (back drilling) is performed on the back side of the multilayer printed circuit board using drill bit 7 to remove unwanted conductor portions, i.e., to remove excess copper plating. Figure 4 shows back drilling performed on the portion of the original copper-plated through-hole 6A (see Figure 3) located below the resin layer to block the signal from the unwanted conductor portions present in the through-hole. After the back drilling process, corresponding to the drill bit 7 used for back drilling, a portion of the copper-plated surface of the original copper-plated through-hole 6A is removed, thereby forming an insulating opening 8. The original copper-plated through-hole 6A located above the resin layer forms a via 6B. A small amount of copper plating adheres to the exposed surface 5A of the resin layer 5, and due to factors such as (drill bit) adhesion, this portion of copper plating is also removed. Therefore, it can be considered that the exposed surface 5A of the resin layer 5 does not actually contain copper plating. The phrase "in essence" here does not mean that the exposed surface 5A of the resin layer 5 is completely free of copper plating, but rather that, compared to the residual stud portion of the prior art, most of the copper has been removed, thereby reducing the impact of the residual stud on signal transmission to a negligible level.
[0054] Then, as shown in Figure 5, the via 6B and the insulating opening 8 are filled with a via-filling resin composition. After the via-filling resin composition is cured by heating, a cured via-filling resin composition 9 is formed. The unwanted portions of the cured via-filling resin composition exposed on the surface of the printed circuit board are removed by a known polishing method to achieve planarization. After that, the wiring layer on the surface is patterned into a specified pattern to form a specified circuit pattern.
[0055] As described above, since the resin layer of the present invention has only a small amount of copper plating attached and is not tightly attached, the copper plating attached to the unremoved resin layer will be removed due to collateral damage or other reasons during back drilling, thereby achieving zero residual piles and significantly suppressing the adverse effects of residual piles in the through hole on the signal.
[0056] The following is a detailed explanation of each component.
[0057] <Resin Composition for Resin Layers>
[0058] The resin composition for the resin layer of the present invention is a resin composition comprising a thermosetting resin, a fluoropolymer, and an inorganic filler. The detailed mechanism is not necessarily clear, but it can be assumed that the fluoropolymer hinders the adhesion of catalyst nuclei such as palladium required during plating, thereby enabling the resin layer to function.
[0059] The resin composition for the resin layer must include a thermosetting resin and a fluororesin. Epoxy resins are particularly preferred as thermosetting resins. Commonly known multifunctional epoxy resins having at least two epoxy groups per molecule can be used as epoxy resins. Epoxy resins can be liquids, solids, or semi-solids. Here, liquid, solid, and semi-solid refer to the state of the epoxy resin at 30°C.
[0060] Examples include cresol varnish-type resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol varnish-type epoxy resins, alkylphenol varnish-type epoxy resins, biphenol type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, epoxides of condensates of phenols and aromatic aldehydes with phenolic hydroxyl groups, triglycidyl isocyanurate, and alicyclic epoxy resins. Examples of epoxy resins include: jER828, jER834, jER1001, jER1004 manufactured by Mitsubishi Chemical Corporation; EPICLON 840, 850, 850-S, 1050, 2055 manufactured by DIC Corporation; Epototo YD-011, YD-013, YD-127, YD-128 manufactured by NIPPON STEEL & SUMIKIN TEXENG.CO.,LTD; DER317, DER331, DER661, DER664 manufactured by Dow Chemical Company; and SUMI-EPOXY ESA-011, ESA-014, ELA-115, ELA-128 manufactured by Sumitomo Chemical Corporation (all trade names) bisphenol A type epoxy resins; Mitsubishi Chemical Brominated epoxy resins include: jERYL903 manufactured by Mitsubishi Chemical Corporation; EPICLON 152 and 165 manufactured by DIC Corporation; Epototo YDB-400 and YDB-500 manufactured by NIPPON STEEL & SUMIKIN TEXENG.CO.,LTD; DER542 manufactured by Dow Chemical Company; and SUMI-EPOXY ESB-400 and ESB-700 manufactured by Sumitomo Chemical Corporation (all trade names); and brominated epoxy resins including jER152 and jER154 manufactured by Mitsubishi Chemical Corporation; DEN431 and DEN438 manufactured by Dow Chemical Company; and EPICLON manufactured by DIC Corporation. N-730, N-770, N-865; EPPN-201, EOCN-1025, EOCN-1020, EOCN-104S, RE-306, NC-3000 manufactured by Nippon Kayaku Co., Ltd.; SUMI-EPOXY ESCN-195X, ESCN-220 manufactured by Sumitomo Chemical Co., Ltd.; NIPPON STEEL & SUMIKIN TEXENG.CO.Phenolic varnish-type epoxy resins such as YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-701, YDCN-704, YDCN-704A manufactured by DIC Corporation; EPICLON N-680, N-690, N-695 (all trade names) manufactured by DIC Corporation; bisphenol F type epoxy resins such as EPICLON 830 manufactured by DIC Corporation; JER807 manufactured by Mitsubishi Chemical Corporation; and Epototo YDF-170, YDF-175, YDF-2004 (all trade names) manufactured by NIPPON STEEL & SUMIKIN TEXENG.CO.,LTD; and Epototo... Hydrogenated bisphenol A type epoxy resins such as ST-2004, ST-2007, ST-3000 (trade names), and YX8034 manufactured by Mitsubishi Chemical Corporation; jER604 manufactured by Mitsubishi Chemical Corporation; NIPPON STEEL & SUMIKIN TEXENG.CO.Epototo YH-434 manufactured by MIT Technology Ltd., SUMI-EPOXY ELM-120 manufactured by Sumitomo Chemical Co., Ltd., etc. (all trade names) are glycidylamine type epoxy resins; hydantoin type epoxy resins; CELLOXIDE 2021 manufactured by Daicel Co., Ltd., etc. (all trade names) are alicyclic epoxy resins; YL-933 manufactured by Mitsubishi Chemical Corporation, EPPN-501 and EPPN-502 manufactured by Nippon Kayaku Co., Ltd., etc. (all trade names) are trihydroxyphenylmethane type epoxy resins; Mitsubishi Chemical The following epoxy resins are listed: YL-6056, YX-4000, YL-6121 (trade names) and other bixylenol or biphenol type epoxy resins or mixtures thereof manufactured by Nippon Kayaku Co., Ltd.; EBPS-200 manufactured by Nippon Kayaku Co., Ltd.; EPX-30 manufactured by ADEKA Co., Ltd.; EXA-1514 (trade name) manufactured by DIC Co., Ltd. and other bisphenol S type epoxy resins; jER157S (trade name) manufactured by Mitsubishi Chemical Corporation and other bisphenol A phenolic varnish type epoxy resins; jERYL-931 (trade name) manufactured by Mitsubishi Chemical Corporation and other tetrahydroxyphenyl ethane type epoxy resins; TEPIC (trade name) manufactured by Nissan Chemical Co., Ltd. and other heterocyclic epoxy resins; Blemmer DGT (trade name) phthalate diglycidyl ester resins manufactured by Nippon Yu Co., Ltd.; NIPPON STEEL & SUMIKIN TEXENG.CO.,LTD manufactures tetraglycidyl dimethylbenzene ethane resins such as ZX-1063; NIPPON STEEL & SUMIKIN TEXENG.CO.,LTD manufactures naphthyl-containing epoxy resins such as ESN-190 and ESN-360; DIC Corporation manufactures HP-4032, EXA-4750, and EXA-4700; DIC Corporation manufactures HP-7200 and HP-7200H epoxy resins with a dicyclopentadiene backbone; Nippon Oil Corporation manufactures CP-50S and CP-50M glycidyl methacrylate copolymer epoxy resins; further, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resins; CTBN modified epoxy resins (e.g., NIPPON STEEL & SUMIKIN). TEXENG.CO.,LTD manufactures YR-102, YR-450, etc., but is not limited to these.
[0061] Among these, commercially available products are preferably ZX-1059 (low-chlorinated) manufactured by NIPPON STEEL Chemical & Material Co., Ltd. (a mixed epoxy resin of bisphenol A and bisphenol F types), and JER-630 (low-chlorinated) manufactured by Mitsubishi Chemical Corporation (triglycidyl-p-aminophenol). As a fluoropolymer, polytetrafluoroethylene (PTFE) or a copolymer of tetrafluoroethylene with an ethylene unsaturated compound represented by the following general formula (1) can be used.
[0062] In general formula (1), R1 to R4 are each independently a hydrogen atom, a fluorine atom, an alkyl group, or -ORf, wherein Rf is an alkyl group containing at least a fluorine atom. The case where all R1 to R4 are fluorine atoms is excluded. As the fluoropolymer, any known and commonly used product may be used, such as commercially available products such as LUBRON L-2, L-5, L-5F, LDW-410 manufactured by Daikin Industries, Ltd., AS-201, 202, 210, 230, 210AS (copolymers of tetrafluoroethylene and perfluoroalkyl vinyl ethers) manufactured by NEOFLON PFA, and EP506, 526, 610 (copolymers of tetrafluoroethylene and ethylene) manufactured by NEOFLON ETFE.
[0063] Teflon fine powder (such as 6-J, 62-J, 6C-J, 640-J, TLP10F-1, MP1300-J manufactured by Mitsui-DuPont) can also be micronized to an average particle size of several μm using an airflow micronizer such as a jet mill.
[0064] The resin composition used in the resin layer of the present invention may further include fluoropolymers such as NP101, 102, NP20, NP30 (polytetrafluoroethylene with a fluoromethyl structure) manufactured by NEOFLON FEP or VP825 (polyvinylidene fluoride polymer with a linear structure having cross-bonded CF2 and CH2) manufactured by NEOFLON PVDF.
[0065] In the above general formula (1), the alkyl group of R1 to R4 is preferably an alkyl group with 1 to 10 carbon atoms.
[0066] In the above general formula (1), the alkyl group containing at least a fluorine atom represented by Rf, which can be R1 to R4, is preferably an alkyl group containing fluorine atoms with 1 to 10 carbon atoms.
[0067] As copolymers of the aforementioned tetrafluoroethylene and the ethylene-unsaturated compounds represented by the above general formula (1), examples include copolymers of tetrafluoroethylene and ethylene (in the above general formula (1), R1 to R4 are hydrogen atoms), and copolymers of tetrafluoroethylene and perfluoroalkyl vinyl ethers (in the above general formula (1), any one of R1 to R4 is -ORf, and the remaining three are fluorine atoms). Commercially available products such as ETFE manufactured by Asahi Glass Co., Ltd. and NEOFLON AP230 manufactured by Daikin Industries, Ltd. can also be used.
[0068] Among the fluororesins, polytetrafluoroethylene, copolymers of tetrafluoroethylene and ethylene, and copolymers of tetrafluoroethylene and perfluoroalkyl vinyl ethers are preferred. Furthermore, copolymers of tetrafluoroethylene and ethylene and copolymers of tetrafluoroethylene and perfluoroalkyl vinyl ethers are more preferred due to their good compatibility with epoxy resin components and curing agent components, excellent crack resistance, and excellent low CTE. Copolymers of tetrafluoroethylene and ethylene are even more preferred.
[0069] In addition, since it has good compatibility with epoxy resin components and curing agent components, excellent crack resistance, and excellent low CTE, the fluororesin preferably includes tetrafluoroethylene and vinyl.
[0070] In the copolymer of tetrafluoroethylene and the ethylene-unsaturated compound represented by the above general formula (1), the structural units derived from tetrafluoroethylene are preferably 20 to 80 mol%, more preferably 30 to 70 mol%. In the copolymer of tetrafluoroethylene and ethylene, the molar ratio of structural units derived from tetrafluoroethylene to structural units derived from ethylene is preferably 20 / 80 to 80 / 20, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40.
[0071] The average particle size of the fluororesin is preferably 1 to 5 μm.
[0072] The fluororesin can be coated with silica. The coating method is not particularly limited; a method involving treatment with silica and a silane coupling agent is suitable. The method of coating with silica is not particularly limited; it can be achieved by simply mixing while applying stress, or by mixing followed by vibration. Furthermore, after coating with silica, a surface treatment can be performed. This surface treatment can be performed using a silane coupling agent or an organosilazane. Additionally, a pretreatment step can be applied to the silica; the pretreatment step preferably includes a surface treatment step and a step of removing the liquid medium (solidification step). The surface treatment step is a step of surface treatment in a liquid medium containing water (water, or alcohols other than water) using a silane coupling agent and an organosilazane. The silane coupling agent is preferably a silane coupling agent having three alkoxy groups and at least one group selected from the group consisting of phenyl, vinyl, epoxy, methacryl, amino, urea, mercapto, isocyanate, and acryloyl groups. The fluororesin can be used alone or in combination of two or more. The amount of the fluororesin mixed is preferably 25 to 55 parts by weight relative to 100 parts by weight of the resin composition for the resin layer, based on the solid content.
[0073] Without impairing the effects of the present invention, the resin composition for the resin layer may contain other organic fillers besides the fluororesin. Also, without impairing the effects of the present invention, the resin composition for the resin layer may optionally contain an isocyanate compound.
[0074] Furthermore, when using thermosetting resins such as epoxy resins, it is preferable to include a curing agent. As a curing agent, imidazole-based curing agents such as 2-methylimidazolium (2MZ-AP), 2-ethyl-4-methylimidazolium (2E4MZ), 2-phenylimidazolium (2PZ), and 2-phenyl-4-methyl-5-hydroxymethylimidazolium (2P4MHZ), amine-based curing agents such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, m-phenylenediamine, isophorone diamine, norbornene diamine, 1,3-diaminomethylcyclohexane, and N-aminoethylpiperazine, and polyamides can be used. Phenolic curing agents such as amines, vinylphenol, aralkyl phenolic resins, phenol phenyl aralkyl resins, and phenol biphenyl aralkyl resins; and anhydride curing agents such as phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyl nadic anhydride, dodecyl succinic anhydride, chloric anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bis(triphenylamine), and methylcyclohexene tetracarboxylic anhydride, are all known curing agents. Commercially available products include, for example, 2MZ-AP (2-methyl-imidazole) manufactured by Shikoku Chemical Industry Co., Ltd.
[0075] Furthermore, the content of the curing agent is preferably 0.5 to 20 parts by weight relative to 100 parts by weight of the thermosetting resin component. When the amount of curing agent is less than 0.5 parts by weight, the resin composition may not cure sufficiently; even when the amount exceeds 20 parts by weight, the desired effect may not be achieved. The filler material can be either inorganic or organic, but inorganic materials are typically used. Examples of inorganic fillers include silica, amorphous silica, talc, clay, mica powder, barium sulfate, calcium carbonate, magnesium carbonate, barium titanate, alumina, aluminum hydroxide, and titanium dioxide.
[0076] Examples of organic fillers include organosilicon powder and nylon powder.
[0077] Furthermore, spherical fillers can achieve high filling without impairing the ink's flowability, making them a preferred choice.
[0078] As spherical fillers, spherical silica (also known as spherical silica), spherical alumina (also known as spherical bauxite), or spherical titanium dioxide are preferred. By using a combination of spherical silica and spherical titanium dioxide, plating resistance is improved.
[0079] The spherical silica can be any shape, as long as it is used as a filler for electronic materials. It can also be spherical silica whose surface has been treated with a silane coupling agent. Examples of silane coupling agents include those having at least one group selected from the group consisting of vinyl, amino, epoxy, and mercapto groups. Specifically, examples include: vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinepropyltrimethoxysilane, 3-epoxypropoxypropyltrimethoxysilane, 3-epoxypropoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, etc., which can be used alone or in combination.
[0080] Spherical fillers only need to be spherical, and are not limited to perfect spheres. Suitable spherical fillers include, for example, fillers with a sphericity of 0.8 or higher as measured below, but are not limited to this. Sphericity is measured as follows: SEM images are taken, and the area and perimeter of the observed particles are calculated using the formula (sphericity) = {4π × (area) ÷ (perimeter)}. 2 The value is calculated using an image processing device. Specifically, the average value is obtained by measuring 100 particles.
[0081] There are no particular limitations on the manufacturing methods for spherical silica particles and spherical alumina; methods known to those skilled in the art can be applied. For example, they can be manufactured by burning silicon or aluminum powder using the VMC (vaporized metal combustion) method. The VMC method refers to a method in which a chemical flame is formed using a burner in an oxygen-containing atmosphere, and metal powder constituting part of the target oxide particles is introduced into the chemical flame in an amount sufficient to form a dust cloud, causing deflagration to obtain oxide particles.
[0082] Commercially available spherical silica includes the SO series manufactured by Admatechs Company Limited and the HPS series (HPS-0500, HPS-1000, HPS3500, etc.) manufactured by Toa Gosei Co., Ltd.
[0083] The aforementioned spherical alumina can be any type of spherical alumina used as a filler for electronic material applications.
[0084] Commercially available spherical alumina includes the AO series manufactured by Admatechs Company Limited, the TC-975c manufactured by Admatechs Company Limited, and the ALUNABEADS / CB series manufactured by Resonac Co., Ltd.
[0085] Ideally, the average particle size of the filler should be 25 μm or less, more preferably 10 μm or less, and even more preferably 3 μm or less. The content of inorganic filler is preferably 15 to 75 parts by weight relative to 100 parts by weight of the solids in the resin composition for the resin layer of the present invention. Particularly preferred is 15 to 50 parts by weight. When the filler content exceeds the upper limit mentioned above, the folding resistance of the cured coating decreases; when it is below the lower limit, there is a tendency for insufficient coating resistance.
[0086] The above-mentioned resin composition may also contain solvents, diluents, curing accelerators, thickeners, defoamers, leveling agents, coupling agents, flame retardants, photopolymerization initiators, etc., as needed.
[0087] <Through holes, through holes, and insulating openings>
[0088] In the multilayer printed circuit board of the present invention, the through-hole before plating is formed by penetrating the conductive layer, the insulating layer, and the resin layer. The resin layer is formed inside the multilayer circuit board, that is, within the space sandwiched between the front and back sides of the multilayer circuit board. By plating and back-drilling the through-hole, the portion of the through-hole near the front side of the multilayer printed circuit board forms a conductive hole, and the portion of the through-hole near the back side of the multilayer printed circuit board forms an insulating opening.
[0089] <Resin Composition for Filling Holes>
[0090] The via-filling resin composition of the present invention can use any known resin composition for filling various through-holes of printed circuit boards. The via-filling resin composition is generally a resin composition comprising at least a photocurable and / or thermocurable resin that is liquid at room temperature (20-25°C), a curing agent, and a filler material. Without any limitation, examples of via-filling resin compositions described in patent documents CN119439622A, CN113126430A, CN111937501A, and CN111748078A can be cited.
[0091] <Circuit patterned conductive layer>
[0092] The conductive layer in the multilayer printed circuit board of the present invention is a circuit pattern formed using a conductor such as copper, nickel, tin, gold, or their alloys. The method for forming the circuit pattern can be any known method, for example, the subtraction method and the addition method.
[0093] <Insulating layer>
[0094] The insulating layer in the multilayer printed circuit board of the present invention can be made of any material as long as it is used as the insulating layer of the multilayer printed circuit board, and is preferably an insulating layer formed by curing a resin composition (in the present invention, the resin composition is sometimes also referred to as "resin composition for insulating layer"). The resin composition for insulating layer can be liquid, semi-solid or solid.
[0095] Examples of materials that can be used as insulating layers include FR-4, epoxy glass, polyimide glass, ceramic hydrocarbons, polyimide films, resin-impregnated glass fibers, resin films, resin-impregnated pad materials, KEVLAR, paper, and resin layers with dispersed nanoparticles.
[0096] In addition, as mentioned above, the prepreg also has the function of insulating the conductive layer, and is therefore included within the insulating layer of the present invention.
[0097] Prepregs are typically sheets made by impregnating a substrate such as glass cloth with a varnish such as an epoxy resin composition, a bismaleimide triazine resin composition, or a polyimide resin composition, and then heating and drying it to achieve semi-curing. Examples include Panasonic Electric Works Co., Ltd.'s R-1410A, R-5670(K), R-1650D, and R-1551, Mitsubishi Gas Chemical Co., Ltd.'s GEPL-190 and GHPL-830, and Resonac Co., Ltd.'s CCL-EL190T and MCL-E-679 series.
[0098] <Resin Layer>
[0099] The composition of the resin layer is as described in the "Resin Composition for Resin Layers" section above. The method for forming the resin layer as an inner layer within a multilayer printed circuit board can be any known method. For example, a composition film can be formed on a conductive layer by coating or printing with a resin composition for resin layers at predetermined locations. The same applies to the insulating layer. The resin layer is then laminated against the insulating layer and hot-pressed to form the layer. As a coating method, roller coating, spray coating, etc., can be used; as a printing method, screen printing, gravure printing, etc., can be used. Heating is typically performed at 80–200°C, preferably 100–170°C, for 5–60 minutes, preferably 10–60 minutes.
[0100] <Substrate>
[0101] The multilayer printed circuit board of the present invention may have a core substrate. The core substrate is a substrate in the multilayer printed circuit board that serves as a base for forming conductive and insulating layers in the form of circuit patterns; it is the substrate that serves as the core material. Examples of materials used as the substrate for the core substrate include glass epoxy materials, ceramics, and metal core substrates, which are formed by impregnating a thermosetting resin such as epoxy resin into glass cloth and then curing it.
[0102] The multilayer printed circuit board of the present invention is particularly suitable for use in high-end devices such as substrates for artificial intelligence (AI) servers. That is, it is particularly suitable for devices requiring printed circuit boards with high layer count, high aspect ratio, high density, and high transmission speed.
[0103] <Manufacturing Methods of Multilayer Printed Circuit Boards>
[0104] The manufacturing method of the multilayer printed circuit board of the present invention is characterized in that the manufacturing method includes:
[0105] The process of forming a multilayered laminate, wherein the laminate comprises a conductive layer, an insulating layer, and a resin layer as an inner layer.
[0106] The laminate comprising the conductive layer, the insulating layer, and the resin layer is pressed;
[0107] For the pressed laminate, a process of forming through holes in a manner that penetrates the laminate, thereby exposing the surfaces of the conductive layer, the insulating layer, and the resin layer;
[0108] The process of plating through holes;
[0109] The reverse drilling process involves removing a portion of the resin layer to form a through hole and an insulating opening in the following manner.
[0110] The via is formed on the front side of the multilayer printed circuit board in the thickness direction. The via is formed by depositing a conductive material onto the surfaces of the conductive layer and the insulating layer of the via.
[0111] The insulating opening is formed on the back side in the thickness direction of the multilayer printed circuit board. The insulating opening is formed by reverse drilling to the back side in the thickness direction of the resin layer and cutting it out from the back side surface of the through hole.
[0112] The manufacturing method further includes a step of filling the through hole and the insulating opening with a cured material formed from a filling resin composition.
[0113] In addition, depending on the different performance and design requirements of different products, only a portion of the conductive layer, insulating layer and resin layer can be penetrated, exposing each surface of the penetrated conductive layer, insulating layer and resin layer.
[0114] When a multilayer printed circuit board has multiple through-holes, it is preferable to apply a resin layer to all through-holes and perform back drilling. For example, when there is a through-hole A that connects to layers 1-3 and a through-hole B that connects to layers 1-5 (not shown in the attached figures, Figure 3 can be understood as the state of the through-hole connecting to layer 3), in the multilayering process, resin layers are stacked below layers 3 and 5 respectively. After plating, back drilling is performed on through-holes A and B respectively. As a result, most of the residual stubs in through-holes A and B are removed, and a multilayer printed circuit board with significantly improved signal transmission quality can be obtained.
[0115] The pressing process is preferably performed by hot pressing. For example, it is a process of multilayering wiring substrates by hot pressing, for example, with an epoxy prepreg (insulating layer) sandwiched between them.
[0116] (Multi-layered process)
[0117] The multilayering process is a process of forming a laminate comprising a conductive layer, an insulating layer, and a resin layer. A preferred method is to form a resin film on a substrate having a conductive layer using a resin composition by coating or printing at predetermined locations (i.e., locations where primary drilling and back drilling are to be performed). Similarly, an insulating resin composition is formed on a substrate having a conductive layer by coating or printing. The two layers are then laminated with the resin layer facing the insulating layer to form the laminate.
[0118] (Pressing process)
[0119] The above-mentioned laminate is hot-pressed to form a pressed laminate. That is, a laminate is formed by fixing the conductive layer, the insulating layer, and the resin layer. Hot pressing can be performed using known methods. The preferred pressing conditions are 150–200°C and 20–60 kg / cm³. 2 .
[0120] (The process of forming a through hole)
[0121] A through hole is formed by drilling through the pressed laminate (one-time drilling). The inner wall of the through hole includes exposed surfaces of the conductive layer, resin layer, and insulating layer.
[0122] (Drilling sludge removal process)
[0123] Descaling can be performed using known methods. For example, oxidants formed from aqueous solutions of chromic acid, permanganate, etc., can be used. Alternatively, oxygen plasma, mixed plasma of CF4 and oxygen, corona discharge, etc., can be employed for treatment.
[0124] (Plating process)
[0125] For the multilayer printed circuit board of the present invention, the surface of the through-hole formed by a single drilling is covered with a conductive material by plating. The plating process is performed by electroless plating, and electroplating may be performed thereafter as desired. Examples of catalyst nuclei for electroless plating include palladium, tin, silver, gold, platinum, copper, and nickel, or combinations thereof, with palladium being preferred. Examples of electroless plating include electroless copper plating, electroless nickel plating, electroless nickel-tungsten alloy plating, electroless tin plating, and electroless gold plating, with electroless copper plating being preferred. The film thickness of the electroless plating is preferably 0.1 to 5 μm.
[0126] (Back drilling process)
[0127] The length of the residual pile formed by the back-drilling process is determined by both the error and the drill bit. In this invention, the length of the exposed surface 5A of the resin layer after the back-drilling process is equivalent to the length of the residual pile (see Figures 4 and 5). Due to the accuracy issues of the back-drilling equipment, an error of no more than 150 μm is usually generated. Therefore, the length of the exposed surface 5A of the resin layer after the back-drilling process is roughly the same as that of conventional residual piles, which is typically 80–200 μm.
[0128] As mentioned earlier, even after the copper plating process, only a trace amount of copper plating adheres to the exposed surface of the resin layer, and due to factors such as (drill bit) adhesion, this trace amount of copper plating is removed after back drilling. That is, the copper plating portion (= residual stake) originally present at position 5A is mostly removed in this invention, thereby reducing the impact of the residual stake on signal transmission to a negligible level.
[0129] The back-drilling process involves drilling to a depth close to but not touching the last conductive layer to which the connection is desired (see Figure 4). To control the drilling depth, the back-drilling process is performed using conventional equipment, such as various types of drilling equipment with known drilling depth control functions.
[0130] It should be noted that Figures 1-5 are schematic diagrams and not to scale for actual structures. For example, in actual substrates, because back drilling may remove most of the resin layer, the length of the exposed resin layer surface 5A after the back drilling process is only on the order of tens to hundreds of micrometers. That is, the actual length of the exposed resin layer surface 5A after the back drilling process may be very small compared to the original thickness of the resin layer 5. Due to space and equipment limitations, it is very difficult to accurately measure the amount of residual copper plating. Therefore, in this invention, the residual copper plating is evaluated by observing the cross-section of the substrate under a microscope (see the embodiments section below for details).
[0131] (Filling process)
[0132] The vias and insulating openings of a multilayer printed circuit board, such as those described in the above embodiment, are filled using a known patterning method such as screen printing, roller coating, die coating, or vacuum printing. The vias and insulating openings are then completely filled, leaving only slight exposure. The multilayer printed circuit board with the vias and insulating openings filled with the via-holes and insulating openings is then heated at 80°C to 160°C for approximately 30 to 180 minutes to cure the via-holes and form a cured product. From the perspective of easily removing unwanted portions exposed on the substrate surface by physical grinding after via filling, the curing of the via-holes and resin composition can be performed in two stages. That is, the via-holes and resin composition can be pre-cured at a lower temperature, followed by final curing (final curing). Pre-curing conditions preferably involve heating at 80°C to 130°C for approximately 30 to 180 minutes. The hardness of the pre-cured product is relatively low; therefore, unwanted portions exposed on the substrate surface can be easily removed by physical grinding, resulting in a flat surface. Afterwards, heating is applied to achieve formal curing. Preferred conditions for formal curing are heating at 130°C to 160°C for approximately 30 to 180 minutes. In either pre-curing or formal curing, curing can be performed using a hot air circulating drying oven, an IR oven, a heating plate, a convection oven, etc. (using a heat source equipped with steam heating to create a counter-current flow of hot air within the dryer, or by spraying hot air from a nozzle onto the object to be cured). A hot air circulating drying oven is particularly preferred. In this case, due to low expansion, the cured material exhibits virtually no expansion or contraction, resulting in a final cured product with excellent dimensional stability, low moisture absorption, good adhesion, and electrical insulation. It should be noted that the hardness of the pre-cured material can be controlled by adjusting the pre-curing heating time and temperature.
[0133] After the via-filling resin composition is cured as described above, the unwanted portions of the cured material exposed on the surface of the printed circuit board are removed by a known physical polishing method to achieve planarization. Then, the wiring layer on the surface is patterned into a predetermined pattern to form a predetermined circuit pattern. It should be noted that, as needed, the surface of the cured material can also be roughened using an aqueous solution of potassium permanganate, etc., and then a wiring layer can be formed on the cured material by electroless plating or the like.
[0134] Example
[0135] The present invention will now be described in more detail using examples. The present invention is not limited to the following examples. (Preparation of the resin composition for the resin layer)
[0136] According to Table 1 below, the components were mixed using a three-roll mill to obtain the resin composition of Example 1. The numbers in the table represent parts by mass of solids.
[0137] (Evaluation of substrate fabrication)
[0138] Patterns were printed on the FR-4 substrate of the copper foil laminate using the resin composition of Example 1, with the dried coating thickness approximately 50 μm, via screen printing. The substrate was then cured by drying at 170°C for 60 minutes using a hot air circulating dryer. Next, the dried substrate and the FR-4 substrate of the copper foil laminate were sandwiched together with epoxy prepreg (R-1650D manufactured by Panasonic Electric Works Co., Ltd.) and subjected to a curing process at 170°C for 60 minutes and a pressure of 20 kg / cm². 2 After hot pressing, the drill bit is used to process the hole, forming a through hole with a diameter of 0.7 mm.
[0139] (Drilling fouling removal process)
[0140] For the test substrate of Example 1, it was immersed in a mixture of CIRCUPOSIT MLB Conditioner 211 (manufactured by Rohm and Haas Company, 200 ml / l) and CIRCUPOSIT Z (manufactured by Rohm and Haas Company, 100 ml / l) as swelling solution at 80°C for 5 minutes. Then, it was immersed in a mixture of CIRCUPOSIT MLB Promoter 213A (manufactured by Rohm and Haas Company, 100 ml / l) and CIRCUPOSIT MLB Promoter 213B (manufactured by Rohm and Haas Company, 150 ml / l) as roughening solution at 80°C for 10 minutes. Finally, it was immersed in CIRCUPOSIT MLB Neutralizer 216-2 (manufactured by Rohm and Haas Company, 200 ml / l) as neutralizing solution at 50°C for 5 minutes.
[0141] (Chemical copper plating process)
[0142] After descaling, as a cleaning and conditioner process, the sample is immersed in Cleaner Security Gantt P500 (manufactured by Atotech Company, 40 ml / l) at 50°C for 5 minutes. Next, as a pre-dip process, it is immersed in a mixture of Pre-dip Neogant B (manufactured by Atotech Company, 20 ml / l) and sulfuric acid (1 ml / l) at 25°C for 1 minute. Then, as a catalyst-adding process, it is immersed in a mixture of Activator Neogant 834Conch (manufactured by Atotech Company, 40 ml / l), sodium hydroxide (4 g / l), and boric acid (5 g / l) at 35°C for 5 minutes. Following this, as a reduction process, it is immersed in a mixture of Reducer Neogant WA (manufactured by Atotech Company, 5 ml / l) and boric acid (25 g / l) at 25°C for 1 minute. Finally, as a chemical copper plating process, it is immersed in Basic Solution Printgant MSK (manufactured by Atotech Company). The sample was immersed in a mixture of Copper Solution Printgant MSK (manufactured by Atotech Company, 80 ml / l), Reducer Cu (manufactured by Atotech Company, 40 ml / l), Stabilizer Printgant MSK (manufactured by Atotech Company, 14 ml / l), and Stabilizer Printgant MSK (manufactured by Atotech Company, 3 ml / l) at 35°C for 10 minutes, and then dried at 100°C for 30 minutes using a hot air circulating dryer.
[0143] (Electroplated copper process)
[0144] Following the electroless copper plating process, the sample is immersed for 1 minute at 30°C in a mixture of pickling cleaner FR (manufactured by Atotech Company, 100 ml / l) and sulfuric acid (100 ml / l) as an acid pickling process. Next, as an acid immersion process, it is immersed for 1 minute at 25°C in sulfuric acid (100 ml / l). Finally, as a copper sulfate electroplating process, the sample is immersed for 60 minutes at 23°C in a mixture of copper(II) pentahydrate (80 ml / l), sulfuric acid (200 ml / l), chlorine (50 mg / l), additive Cupracid HL (manufactured by Atotech Company, 10 ml / l), and corrective agent Cupracid GS (manufactured by Atotech Company, 0.1 ml / l) (current density 1 A / dm³). 2Then, dry it at 150°C for 60 minutes using a hot air circulating dryer.
[0145] (Back drilling process)
[0146] Back-drilling is performed from the back of the multilayer printed circuit board using a 600μm diameter drill bit to remove excess copper plating from the inner wall and back-drill to the bottom of the resin layer (the back side in the resin layer thickness direction).
[0147] (Hole filling process)
[0148] The through holes and insulating openings of the substrate that has undergone back drilling are filled with a through-hole resin composition under atmospheric pressure by screen printing. After filling, the substrate is placed in a hot air circulating dryer and dried at 150°C for 60 minutes to cure the through-hole resin composition. Next, the entire surface of the printed circuit board is polished with a polishing wheel to make it planar, thus obtaining the evaluation substrate of the embodiment.
[0149] <Printing conditions>
[0150] Scraper: 20mm thick, 70° hardness, 23° angled grinding.
[0151] Version: PET 100 mesh offset version
[0152] Printing pressure: 50kg, squeegee speed: 30mm / second
[0153] Scraper angle: 80°.
[0154] (Evaluation Method)
[0155] After copper electroplating, the surface of the resin layer located on the inner wall of the through hole was observed under a microscope to confirm whether the copper plating adhered to the resin layer of Example 1, and the evaluation was carried out according to the following criteria. The results are shown in Table 1 below.
[0156] (Electroplating resistance evaluation criteria)
[0157] ○: No conductive material (copper) was observed to be plated in the resin layer of the through hole.
[0158] △: The resin layer in the through hole is partially coated with a conductive material (copper).
[0159] ×: The resin layer in the through hole is plated with a conductive material (copper).
[0160] (Viscosity performance evaluation criteria)
[0161] Viscosity at 25°C:
[0162] A 0.2 ml sample was collected, and the viscosity was determined using a cone-plate viscometer (TV-33 manufactured by Toki Sangyo Co., Ltd.) at 25°C and 5 rpm for 30 seconds.
[0163] The evaluation criteria are as follows:
[0164] ○: Viscosity below 600 dPa·s
[0165] ×: Viscosity exceeding 600 dPa·s
[0166] Table 1
[0167] Remark:
[0168] *1: ZX-1059 (Low Chloride) is manufactured by NIPPON STEEL Chemical & Material Co., Ltd., a mixed epoxy resin of bisphenol A and bisphenol F types.
[0169] *2: JER-630 (Low Chloride) manufactured by Mitsubishi Chemical Corporation, contains triglycidyl-p-aminophenol.
[0170] *3: 2MZ-AP, imidazole thermosetting catalyst, manufactured by Shikoku Chemical Industry Co., Ltd.
[0171] *4: Surface-treated silica, spherical silica, average particle size (D50) = 4.3 μm ethylene surface treatment
[0172] *5: Surface-treated silica, spherical silica, average particle size (D50) = 4.3μm epoxy-based surface treatment
[0173] *6: Made by Admatechs, nano-silica coated PTFE, average particle size (D50) = 3μm
[0174] *7: PTFE-104S, untreated PTFE, Nanjing Tianshi New Material Technology Co., Ltd., PTFE micro powder, average particle size (D50) = 5.0μm
[0175] (Method for evaluating copper coverage)
[0176] After back drilling and before hole filling, the resin layer or the corresponding area on the inner wall of the through hole is observed under a microscope to confirm the amount of copper on each surface, and the evaluation is based on the following criteria. The results are shown in Table 2 below.
[0177] (Criteria for determining copper coverage)
[0178] ○: No coating of conductive material (copper) was observed.
[0179] △: A small amount of conductive material (copper) is plated on it.
[0180] ×: Plated with a conductive material (copper).
[0181] Table 2
[0182] As shown in Table 2, Comparative Examples 1 and 2 were conducted based on the above embodiments, with or without the formation of a resin layer or the back-drilling process. In Example 1, after back-drilling, the amount of copper plating on the surface of the resin layer located on the inner wall of the through-hole was observed under a microscope; no conductive material plating was observed. In Comparative Example 1, no resin layer was provided. After back-drilling, the amount of copper plating on the surface of the resin layer corresponding to the resin layer in Example 1 located on the inner wall of the through-hole was observed; the amount of copper plating was equivalent to the level of the prior art with residual pins. In Comparative Example 2, after copper plating, the amount of copper plating on the surface of the resin layer located on the inner wall of the through-hole was observed. Although a resin layer was provided, no back-drilling process was performed; the resin layer was not partially removed, and the copper plating on the resin layer was not further removed due to cascading or other reasons; therefore, a small amount of copper was plated on the resin layer. Since the residual pin effect is caused by excess copper plating, it can be expected that Example 1 has better signal loss resistance performance compared to Comparative Examples 1 and 2.
[0183] Industrial availability
[0184] This invention provides a multilayer printed circuit board with zero residual stubs, which significantly improves the quality of signal transmission. The multilayer printed circuit board of this invention is particularly suitable for electronic devices with higher requirements for substrate performance, such as multilayer substrates for AI servers.
[0185] Figure reference numerals: 1A, 1B, 1C, 1D: Conductive layer; 2A, 2B: Insulating layer; 3A, 3A', 3B, 3B': Substrate; 4: Insulating layer (prepreg); 5: Resin layer; 5A: Resin layer exposed after back drilling; 6: Through hole; 6A: Through hole with copper plating; 6B: Conductive hole; 7: Back drill bit; 8: Insulating opening; 9: Cured resin composition for filling holes.
Claims
1. A multilayer printed circuit board, comprising a conductive layer, an insulating layer, and a resin layer as an inner layer, characterized in that, The multilayer printed circuit board has through holes, exposing the surfaces of the conductive layer, the insulating layer, and the resin layer. The front side of the multilayer printed circuit board in the thickness direction has a through hole formed by plating a conductive material onto the surface of the conductive layer and the insulating layer of the through hole. The back side of the multilayer printed circuit board in the thickness direction has an insulating opening formed by reverse drilling to the back side of the resin layer in the thickness direction and cutting out from the back side surface of the through hole.
2. The multilayer printed circuit board of claim 1, wherein, The resin layer, which serves as the inner layer, is located inside the insulating layer.
3. The multilayer printed circuit board according to claim 1 or 2, wherein, The resin layer is directly stacked with a conductive layer that is closer to the front side of the multilayer printed circuit board than the resin layer.
4. The multilayer printed circuit board according to claim 1 or 2, wherein, The resin layer is formed from the cured resin composition.
5. The multilayer printed circuit board of claim 1 or 2, wherein, The conductive material is plated with copper.
6. The multilayer printed circuit board of claim 1 or 2, wherein, The through-hole and the insulating opening are filled with a cured material, which is formed from a filling resin composition.
7. The multilayer printed circuit board of claim 1 or 2, wherein, From the perspective of a side view, the resin layer extends through the diameter of the through hole.
8. The multilayer printed circuit board of claim 1 or 2, wherein, From a top view perspective, the resin layer has an area that allows it to completely cover the entire through-hole.
9. An electronic device, characterized by A multilayer printed circuit board comprising any one of claims 1 to 8.
10. A method of manufacturing a multilayer printed circuit board, characterized by, The manufacturing method includes: The process of forming a multilayered laminate, wherein the laminate comprises a conductive layer, an insulating layer, and a resin layer as an inner layer. A process of pressing a laminate comprising the conductive layer, the insulating layer and the resin layer; For the pressed laminate, a process of forming through holes in a manner that penetrates the laminate, thereby exposing the surfaces of the conductive layer, the insulating layer and the resin layer. The process of plating through holes; The reverse drilling process involves removing a portion of the resin layer to form a through hole and an insulating opening in the following manner. The via is formed on the front side of the multilayer printed circuit board in the thickness direction. The via is formed by depositing conductive material onto the surfaces of the conductive layer and the insulating layer of the via. The insulating opening is formed on the back side in the thickness direction of the multilayer printed circuit board. The insulating opening is formed by reverse drilling to the back side in the thickness direction of the resin layer and cutting it out from the back side surface of the through hole.
11. The method of manufacturing a multilayer printed circuit board according to claim 10, wherein, It also includes the step of filling the through hole and the insulating opening with a cured material formed from a filling resin composition.