Wafer backside metallization method and semiconductor process device

By forming a dense layer on the back of the wafer and then forming a metal layer on it by magnetron sputtering, the problem of insufficient adhesion between the wafer and the metal layer is solved, resulting in higher adhesion and a shorter production cycle, and reduced production costs.

WO2026237671A1PCT designated stage Publication Date: 2026-11-19BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/092181
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-04-22
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

In existing technologies, the interfacial bonding force between the wafer and the metal layer is low, which makes the metal layer easy to peel off, affecting heat dissipation and production efficiency.

Method used

A dense layer is formed on the back side of the wafer, and a metal layer is formed on the side of the dense layer away from the wafer by magnetron sputtering. The dense layer is used to prevent metal atoms from entering the wafer, and the bonding force between the metal atoms and the dense layer is greater than the bonding force between the metal atoms and the wafer. The metal atoms do not contain Al.

Benefits of technology

The elimination of the need to form an Al layer enhances the adhesion between the metal layer on the back of the wafer and the wafer, reduces the risk of peeling, shortens the production cycle, improves production efficiency, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026092181_19112026_PF_FP_ABST
    Figure CN2026092181_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a wafer backside metallization method and a semiconductor process device. The method comprises: forming a dense layer on the backside of a wafer; and by means of magnetron sputtering, forming a metal layer on the side of the dense layer that is away from the backside of the wafer, wherein the dense layer is used for preventing metal atoms from entering the wafer during the magnetron sputtering, the bonding strength between the metal atoms and the dense layer is greater than the bonding strength between the metal atoms and the material of the wafer, and the metal atoms do not contain Al. The wafer backside metallization method and the semiconductor process device provided in the present application can solve the problem in the prior art of metal being peeled off of a wafer due to a poor interfacial bonding strength.
Need to check novelty before this filing date? Find Prior Art

Description

Methods and semiconductor process equipment for back-side metallization of wafers Technical Field

[0001] This application relates to the field of semiconductor manufacturing, and more specifically, to a method for metallizing the back side of a wafer and semiconductor process equipment. Background Technology

[0002] Chips generate a significant amount of heat during operation. If this heat cannot be dissipated effectively and promptly, the chip temperature will become excessively high, impacting its performance and lifespan. With the development of advanced packaging, the heat dissipation requirements for wafers are gradually increasing. Directly conducting heat from the wafer to the thermally conductive layer is currently the primary heat dissipation method. Specifically, as shown in Figure 1, the application of wafer backside metallization for chip 104 involves plating metal on the backside of the wafer. The metal layer 103 is soldered to the substrate 101 via solder pads 102. This serves to protect chip 104 while simultaneously dissipating heat, reducing temperature fluctuations, and ensuring the normal operation of chip 104.

[0003] The metallization process on the back side of a wafer mainly uses physical vapor deposition (PVD) to deposit metal materials on the back side of the wafer. However, due to the low interfacial adhesion between the wafer and the metal material, most metal layers cannot effectively adhere to the wafer surface and are prone to peeling. Summary of the Invention

[0004] This application aims to solve at least one of the technical problems existing in the prior art, and proposes a method and semiconductor process equipment for back-side metallization of wafers, which can solve the problem of peeling between wafers and metals due to low interfacial adhesion in the prior art.

[0005] To achieve the objectives of this application, a method for metallizing the back side of a wafer is provided, comprising:

[0006] A dense layer is formed on the back side of the wafer;

[0007] On the side of the dense layer away from the back of the wafer, a metal layer is formed by magnetron sputtering. The dense layer is used to prevent metal atoms from entering the wafer during the magnetron sputtering process, and the bonding force between the metal atoms and the dense layer is greater than the bonding force between the metal atoms and the material of the wafer. The metal atoms do not contain Al.

[0008] As another technical solution, this application also provides a semiconductor process apparatus, including a pre-cleaning chamber, an inlet assembly, an upper electrode assembly, a lower electrode assembly, a deposition chamber, and a controller. The controller includes at least one processor and at least one memory, in which a computer program is stored. When the computer program is executed by the processor, it implements the wafer backside metallization method provided in this application.

[0009] This application has the following beneficial effects:

[0010] The method and semiconductor process equipment for wafer backside metallization provided in this application involve forming a dense layer on the backside of the wafer; a metal layer is then formed on the side of the dense layer away from the backside of the wafer by magnetron sputtering. This dense layer serves to prevent metal atoms from entering the wafer during magnetron sputtering, and the bonding force between the metal atoms and the dense layer is greater than the bonding force between the metal atoms and the wafer material. The metal atoms do not contain Al. Unlike related technologies that completely remove impurities from the backside of the wafer through acid washing and pre-cleaning, requiring the pre-plating of an Al layer before subsequent wafer backside metallization, this application, on the one hand, prevents magnetron sputtered metal atoms from entering the wafer material layer, avoiding the formation of a double-layer structure that reduces bonding force; on the other hand, the bonding force between the dense layer and the metal atoms is greater than the bonding force between the metal atoms and the wafer material. Therefore, the wafer backside metallization method of this application embodiment can enhance the bonding force between the metal layer on the backside of the wafer and the wafer without forming an Al layer, reducing the risk of peeling. Moreover, eliminating the Al layer not only reduces one deposition step and the corresponding chamber occupation, but also eliminates the temperature control and chamber switching time before and after Al layer deposition, thereby significantly shortening the production cycle, improving production efficiency and reducing production costs. Attached Figure Description

[0011] The accompanying drawings used in the description of the embodiments or prior art are briefly introduced below with reference to the accompanying drawings. Obviously, the drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0012] Figure 1 is a schematic diagram of the bonding between the metal on the back of the wafer and the substrate;

[0013] Figure 2a is a flowchart of the wafer backside metallization method used in the related technology;

[0014] Figure 2b is a scanning electron microscope image of the Ti-Si interface in the related technology;

[0015] Figure 3 is a flowchart of a wafer backside metallization method provided in an embodiment of this application;

[0016] Figure 4 is a flowchart of a specific embodiment of step S11 used in this application;

[0017] Figure 5 is a chamber layout diagram of the semiconductor process equipment used in the embodiments of this application;

[0018] Figure 6 is a flowchart of a specific embodiment of step S1 used in this application;

[0019] Figure 7 is a flowchart of a specific embodiment of step S11' used in this application;

[0020] Figure 8 is a schematic diagram of the pre-cleaning chamber used in the embodiments of this application. Detailed Implementation

[0021] To enable those skilled in the art to better understand the technical solutions of this application, the method for wafer backside metallization and the semiconductor process equipment provided in this application will be described in detail below with reference to the accompanying drawings.

[0022] In related technologies, such as for Insulated Gate Bipolar Transistors (IGBTs), the back side of the wafer needs to be metallized during the fabrication process, as shown in Figure 2a. The specific steps of the wafer back side metallization method used in related technologies include:

[0023] S01. The wafer (e.g., a silicon wafer) is acid-washed (e.g., using an HF acid solution) to completely remove the natural oxides on the back side of the wafer;

[0024] S02. The back side of the wafer after step S01 is pre-cleaned in the pre-cleaning chamber to remove impurities (including contaminants and residues) from the back side of the wafer.

[0025] S03. Sequentially deposit Al layer, Ti layer, NiV layer and Ag layer on the back side of the wafer after step S02;

[0026] S04. Perform high-temperature annealing on the wafer after completing step S03 to form a good ohmic contact between the wafer and the Al layer, thereby reducing the contact resistance.

[0027] Because silicon wafers and Al layers have good bonding strength, depositing an Al layer before depositing Ti, NiV, and Ag layers on the back of the wafer to achieve back-side metallization can improve the bonding strength of the metal layers on the back of the wafer and prevent peeling.

[0028] However, the back-side metallization process does not require the formation of an Al layer to create an ohmic contact with the wafer. In related technologies, to improve the adhesion of the back-side metal layer, semiconductor process equipment needs to include a process chamber for depositing the Al layer, which increases production costs and reduces production efficiency. Theoretically, eliminating this Al layer would simplify the process and reduce costs.

[0029] The inventors of this application discovered through research that if the Al layer formation step is omitted and the Ti layer is deposited directly on the back side of the wafer, the interfacial adhesion between the wafer and the Ti layer decreases, leading to delamination. Specifically, for the back-side metallization process, after the back-side thinning and stress-relief cleaning steps, an amorphous silicon layer is formed on the surface of the back side of the wafer due to etching damage. This amorphous silicon layer contains a small number of Ar atoms and its material is relatively porous. When the Ti layer is deposited directly by magnetron sputtering, Ti will interdiffuse with the Si atoms on the surface of the back side of the wafer, as shown in Figure 2b. This results in a two-layer structure of amorphous silicon and amorphous TiSi at the Ti-Si interface. As Ti diffuses into the amorphous silicon layer, the Ar atoms are squeezed to the lower layer and aggregate, leading to a decrease in the interfacial adhesion between the wafer and the Ti layer, making delamination more likely.

[0030] To address the aforementioned problems, this application provides a method for metallizing the back side of a wafer, as shown in Figure 3. The method includes:

[0031] S1. A dense layer is formed on the back side of the wafer;

[0032] S2. A metal layer is formed on the side of the dense layer away from the back of the wafer by magnetron sputtering.

[0033] The aforementioned dense layer is used to prevent metal atoms from entering the wafer during magnetron sputtering, and the bonding force between the metal atoms and the dense layer is greater than the bonding force between the metal atoms and the wafer material. The metal atoms do not contain Al.

[0034] Unlike related technologies that completely remove impurities from the back side of the wafer through acid pickling and pre-cleaning, requiring the pre-plating of an Al layer before subsequent back-side metallization, the back-side metallization method of this application first forms a dense layer on the back side of the wafer. On one hand, the dense layer can prevent magnetron sputtered metal atoms from entering the wafer material layer, avoiding the formation of a double-layer structure that reduces adhesion. On the other hand, the adhesion between the dense layer and the metal atoms is greater than the adhesion between the metal atoms and the wafer material. Therefore, the back-side metallization method of this application can enhance the adhesion between the metal layer on the back side of the wafer and the wafer without forming an Al layer, reducing the risk of peeling. Moreover, eliminating the Al layer not only reduces one deposition step and the corresponding chamber occupancy but also eliminates the temperature control and chamber switching time before and after Al layer deposition, thereby significantly shortening the production cycle, improving production efficiency, and reducing production costs.

[0035] For the wafer backside metallization process, if the Al layer formation step is omitted, the aforementioned metal layer does not contain Al. In this case, the metal atoms formed during magnetron sputtering in step S2 do not contain Al. In other words, the metal layer is formed from an Al-free metallic material, for example, it may include a single-layer or multi-layer structure composed of one or more metallic elements selected from Ti, Ni, V, and Ag.

[0036] In some embodiments, the metal layer described above is used as a thermally conductive layer, for example, in a semiconductor chip.

[0037] In some embodiments, the wafer material includes Si; the metal layer includes a Ti layer, a NiV layer, and an Ag layer formed sequentially away from the dense layer. The Ag layer serves a heat dissipation function; the Ti layer acts as a seed layer to improve the adhesion between the Ag layer and the wafer; the NiV layer acts as an intermediate layer between the Ti and Ag layers, also improving the adhesion between the Ag layer and the wafer. The aforementioned metal layer does not contain an Al layer. As mentioned above, if the Ti layer is deposited directly on the back side of the wafer, the interfacial bonding between the wafer and the Ti layer will decrease, leading to peeling. To address this, this embodiment forms a dense layer on the back side of the wafer. On the one hand, the dense layer can prevent magnetron sputtered metal atoms (i.e., Ti) from entering the wafer, avoiding the formation of a double-layer structure that reduces bonding strength. On the other hand, the bonding strength between the dense layer and the metal atoms (i.e., Ti) is greater than the bonding strength between the metal atoms (i.e., Ti) and the wafer material (i.e., Si). Therefore, it is unnecessary to form an Al layer, and the bonding strength between the metal layer on the back side of the wafer and the wafer can be enhanced, reducing the risk of peeling.

[0038] In some embodiments, the dense layer is an oxide layer.

[0039] When the wafer material includes Si, the dense layer formed in step S1 above is a silicon dioxide (SiO2) layer. Taking the metal layer including the Ti layer as an example, SiO2 can block Ti atoms sputtered by magnetron sputtering from entering the Si layer of the wafer, avoiding the formation of a double-layer structure that reduces the bonding force. Moreover, since the bonding force between SiO2 and Ti is greater than that between Si and Ti, the interfacial bonding force between SiO2 and the Ti layer is better. Therefore, there is no need to form an Al layer. This can also enhance the bonding force between the metal layer on the back side of the wafer and the wafer, reducing the risk of peeling.

[0040] The high bonding force between the oxide layer (such as SiO2) and the Ti layer is due to the fact that the surface of SiO2 is rich in dangling bonds or polar functional groups, which can form strong chemical adsorption or interfacial reaction with Ti atoms. In particular, the oxygen atoms in it are more likely to combine with Ti atoms. Therefore, the interfacial bonding energy between SiO2 and Ti is significantly higher than that between Si and Ti.

[0041] It should be noted that the embodiments of this application are not limited to the embodiments where the wafer material includes Si and the oxide layer formed is a silicon dioxide (SiO2) layer. For wafers of other materials, if the interfacial adhesion between the oxide layer and the metal layer is better than that of wafers of that material, the wafer backside metallization method provided in the embodiments of this application is applicable, and can achieve the effect of improving the interfacial adhesion between the wafer and the Ti layer without forming an Al layer, thereby reducing the risk of peeling. The metal layer included in this application is not limited to Ti, NiV, and Ag layers. In practical applications, the film layers can be replaced or added according to specific needs.

[0042] It should also be noted that the dense layer formed can also be any film layer other than the oxide layer, which has a better interfacial bonding strength with the metal layer than the interfacial bonding strength between the wafer and the metal layer.

[0043] In some embodiments, the thickness of the dense layer is greater than or equal to and less than or equal to If the thickness of the dense layer is less than It is difficult to form a continuous and dense barrier layer, which cannot effectively prevent the diffusion of metal atoms; if the thickness of the dense layer is greater than... While the blocking effect could be further improved, it might introduce excessive interfacial stress and adversely affect the thermal conductivity of the wafer's back side. Controlling the thickness to within... It can achieve the best balance between diffusion barrier, interfacial bonding force and thermal conductivity.

[0044] Specifically, the inventors of this application discovered that a natural oxide layer is typically formed on the back side of a wafer, and the thickness of this natural oxide layer is generally 10 angstroms. In this case, the natural oxide layer can be used as the aforementioned dense layer to improve the interfacial adhesion between the wafer and the metal layer. Specifically, step S1 includes:

[0045] S11. Partially etch the natural oxide layer on the back side of the wafer, and use the remaining natural oxide layer as a dense layer.

[0046] In step S11 above, etching the natural oxide layer on the back side of the wafer not only allows for obtaining a natural oxide layer of the desired thickness as a dense layer to improve the interfacial bonding between the wafer and the metal layer, but also removes impurities (including contaminants and residues) on the back side of the wafer by etching part of the natural oxide layer, thereby improving the surface cleanliness of the back side of the wafer.

[0047] When the wafer material includes Si, the natural oxide layer is a silicon dioxide (SiO2) layer.

[0048] In some embodiments, in order to effectively improve the surface cleanliness of the wafer back side while retaining a portion of the natural oxide layer as an oxide layer, the etching thickness in step S11 (i.e., the thickness of the natural oxide layer etched away) is greater than or equal to 1 angstrom. And less than or equal to 10 angstroms. Preferably greater than or equal to 5 angstroms and less than or equal to 10 angstroms. Since the thickness of the natural oxide layer is generally greater than 10 angstroms, the above-mentioned etching thickness range can ensure that a portion of the natural oxide layer can be retained as an oxide layer.

[0049] In some embodiments, after the wafer backside thinning and stress-relief cleaning steps, and before transferring the wafer into the process chamber for metal layer (e.g., Ti layer) deposition, the wafer is transferred to a pre-clean chamber for a pre-cleaning process to remove impurities (including contaminants and residues) from the wafer backside. This avoids contamination during metal layer (e.g., Ti layer) deposition. Based on this, the wafer backside metallization method provided in this application embodiment can perform step S11 simultaneously with the pre-cleaning process to obtain an oxide layer. This not only avoids contamination during metal layer deposition and reduces the risk of wafer scrap, but also saves process steps, improves production efficiency, and reduces production costs.

[0050] Specifically, as shown in Figure 4, step S11 above includes:

[0051] S111. Place the wafer in the pre-cleaning chamber;

[0052] S112. A pre-cleaning process is performed on the back side of the wafer using etching gas to remove impurities on the back side of the wafer, while partially etching the natural oxide layer.

[0053] The etching gas mentioned above includes, for example, Ar. The plasma formed by Ar gas can physically bombard the back side of the wafer to remove impurities on the back side of the wafer and simultaneously etch the natural oxide layer. In some embodiments, after completing the above step S112, the surface roughness of the oxide layer is less than 5 nm, and the number of particles on the back side of the wafer is less than 50 ea @ 0.2 μm. In other words, after completing the above step S112, the total number of particulate contaminants with a diameter greater than or equal to 0.2 μm on the surface of the back side of the wafer is controlled to be less than 50.

[0054] In one specific embodiment, this application provides a method for backside metallization of a wafer, which, for example, employs a semiconductor process apparatus 1000 as shown in FIG. 5. The semiconductor process apparatus 1000 may include, for example, an Equipment front end module (EFEM) 100, a load lock chamber 200, a degassing chamber 500, a preclean chamber 400a, three process chambers (400b, 400c, 400d) for depositing Ti, NiV, and Ag layers respectively, and a transfer chamber 300 connected to these chambers. The preclean chamber 400a may, for example, be an inductively coupled plasma (ICP) chamber, such as the preclean chamber 20 shown in FIG. 8. Specifically, the precleaning process mainly includes the following steps: introducing etching gas into the preclean chamber and turning on the upper electrode power supply to apply upper electrode power to the upper electrode (e.g., a coil) to excite the etching gas in the preclean chamber to form plasma. The upper electrode power supply is, for example, a radio frequency (RF) power supply, specifically a high-frequency RF power supply with a frequency of, for example, 2 MHz. A high-frequency RF power supply is beneficial for increasing electron concentration and generating high-density plasma. Furthermore, by turning on the lower electrode power supply, lower electrode power is applied to the lower electrode (located on the support device for holding the wafer) to attract plasma towards the wafer surface, enabling bombardment of the wafer surface. Additionally, the aforementioned pre-cleaning chamber also has an exhaust port connected to a vacuum pump (e.g., a molecular pump) to expel gas from the pre-cleaning chamber, thereby controlling the chamber pressure.

[0055] In some embodiments, the process parameters used in step S112 are, for example, as follows: the etching gas includes Ar, the flow rate of the etching gas is greater than or equal to 5 sccm and less than or equal to 20 sccm; the upper electrode power is greater than or equal to 100W and less than or equal to 1000W; the lower electrode power is greater than or equal to 50W and less than or equal to 800W; and the process duration is greater than or equal to 1s and less than or equal to 10s.

[0056] Step S112, by employing the aforementioned process parameters, removes impurities from the back side of the wafer, thereby improving the surface cleanliness of the back side. Simultaneously, it partially etches the natural oxide layer, retaining it as an oxide layer with a thickness greater than or equal to 1 angstrom and less than or equal to 10 angstroms. This oxide layer enhances the interfacial adhesion between the wafer and the metal layer.

[0057] In the above embodiments, the retained natural oxide layer is used as a dense layer. However, the etching thickness of this method is relatively small, which is suitable for scenarios with high surface cleanliness on the back side of the wafer. For example, if the number of particles on the back side of the wafer is small (e.g., @0.06μm < 10ea, that is, fewer than 10 particles with a size greater than 0.06μm), the above step S112 can be used to form an oxide layer to ensure that a portion of the natural oxide layer is retained while removing impurities on the back side of the wafer.

[0058] For scenarios with low surface cleanliness on the back side of the wafer, such as a large number of particles on the back side (e.g., @0.06μm > 10ea), the above method may not be effective in removing impurities on the back side of the wafer. In this case, the etching thickness can be increased to completely remove the natural oxide layer on the back side of the wafer, and then an additional oxide layer can be formed on the back side of the wafer as a dense layer. This ensures that the surface cleanliness of the back side of the wafer meets the requirements. Specifically, in another embodiment, as shown in Figure 6, step S1 includes:

[0059] S11': Complete etching of the natural oxide layer on the back side of the wafer;

[0060] S12. Oxidize the back side of the wafer to form an oxide layer as a dense layer.

[0061] In step S11' above, by completely etching the natural oxide layer on the back side of the wafer, impurities (including contaminants and residues) on the back side of the wafer can be effectively removed, thereby improving the surface cleanliness of the back side of the wafer. It should be noted that, depending on the etching thickness, step S11' above can be either completely etching the natural oxide layer without etching the wafer, or etching the wafer after completely etching the natural oxide layer.

[0062] In some embodiments, in order to effectively etch away impurities (including contaminants and residues) on the back side of the wafer, the etching thickness is greater than or equal to 50 angstroms and less than or equal to 1000 angstroms.

[0063] Similar to the above embodiments, step S11' can be performed simultaneously with the pre-cleaning process. This not only avoids contamination during metal layer deposition and reduces the risk of wafer scrap, but also saves process steps, improves production efficiency, and reduces production costs.

[0064] Specifically, as shown in Figure 7, step S11' above includes:

[0065] S111' Place the wafer in the pre-cleaning chamber;

[0066] S112': Use etching gas to pre-clean the back side of the wafer to remove impurities on the back side of the wafer, and at the same time etch the natural oxide layer completely.

[0067] The pre-cleaning process used in step S112' is similar to step S112 in the above embodiment, except that the etching thickness (or process time) is different. Specifically, in order to achieve complete etching of the natural oxide layer, step S112' requires a relatively long process time.

[0068] In some embodiments, the process parameters used in step S112' are, for example, as follows: the etching gas includes Ar, the flow rate of the etching gas is greater than or equal to 5 sccm and less than or equal to 20 sccm; the upper electrode power is greater than or equal to 100W and less than or equal to 1000W; the lower electrode power is greater than or equal to 50W and less than or equal to 800W; and the process duration is greater than or equal to 10s and less than or equal to 100s.

[0069] After completing step S112', step S12 is executed. Specifically, step S12 may include:

[0070] S121. After the pre-cleaning process is completed, oxygen-containing gas is introduced into the pre-cleaning chamber to oxidize the back side of the wafer to form an oxide layer.

[0071] The pre-cleaning process ends when both the upper and lower electrode power supplies are turned off, and the etching gas is stopped being introduced into the pre-cleaning chamber. At the start of step S121, the exhaust port of the pre-cleaning chamber is closed, and oxygen-containing gas is introduced into the pre-cleaning chamber. The thickness of the oxide layer can be adjusted by regulating the flow rate and / or the duration of oxygen-containing gas introduction to obtain the desired thickness. In some embodiments, the oxygen-containing gas is oxygen, and the oxygen flow rate is greater than or equal to 10 sccm and less than or equal to 100 sccm; or, the duration of oxygen introduction into the pre-cleaning chamber is greater than or equal to 5 s and less than or equal to 10 s. In some embodiments, the thickness of the oxide layer is greater than or equal to 1 angstrom and less than or equal to 10 angstroms.

[0072] The inventors discovered through experiments that if the oxygen flow rate is below 10 sccm or the inlet time is less than 5 seconds, the resulting oxide layer thickness is difficult to achieve. The above applies; if the oxygen flow rate exceeds 100 sccm or the inlet time exceeds 10 s, the oxide layer thickness is likely to exceed [the specified value]. Furthermore, it may introduce oxidative damage. By controlling the flow rate and duration within the above range, the oxide layer thickness can be stably controlled. between.

[0073] As can be seen from the above, step S11 can be applied to scenarios with high surface cleanliness on the back side of the wafer, and step S11' can be applied to scenarios with low surface cleanliness on the back side of the wafer (e.g., @0.06μm>10ea). In this case, before performing step S1, the wafer back side metallization method provided in this application embodiment further includes:

[0074] S00. Determine whether the surface cleanliness of the wafer is greater than or equal to a preset threshold. For example, the semiconductor process equipment 1000 may further include a detection module (not shown), which can be located inside the pre-cleaning chamber 400a or in the transfer chamber 300, for detecting the surface cleanliness of the back side of the wafer before or after it is transferred into the pre-cleaning chamber 400a. This detection module can, for example, employ a light-scattering particle counter, which scans the wafer surface with a laser to obtain the number of particles and their size distribution on the back side of the wafer in real time, thereby determining whether the surface cleanliness of the back side of the wafer reaches the preset value.

[0075] When the wafer surface cleanliness is high, there are fewer impurities, and partial etching can remove impurities while preserving the dense layer. When the cleanliness is low, impurities may have penetrated or contaminated the natural oxide layer. In this case, it is necessary to completely remove the contaminated oxide layer and regrow it to ensure the purity of the dense layer and the interface quality.

[0076] If the surface cleanliness of the wafer is greater than or equal to a preset threshold, perform the above step S11;

[0077] If the surface cleanliness of the wafer is less than a preset threshold, perform the above step S11'.

[0078] In one specific embodiment, the surface cleanliness of the wafer backside includes, for example, the number of particles on the wafer backside. The preset threshold is a preset threshold for the number of particles. This preset threshold is, for example, 50ea@0.2μm.

[0079] After completing step S1, the wafer with the oxide layer is transferred to the corresponding deposition chamber for step S2. Specifically, the deposition chamber is, for example, a physical vapor deposition (PVD) chamber. Taking the semiconductor process equipment 1000 shown in Figure 5 as an example, three deposition chambers (400b, 400c, and 400d) are used to deposit Ti, NiV, and Ag layers, respectively. Since the method of depositing the above metal layers using PVD technology is a well-known technique, it will not be described in detail here.

[0080] In some embodiments, the upper electrode power used in step S2 is greater than or equal to 1 kW and less than or equal to 20 kW, preferably 8 kW. This range is larger than the range of upper electrode power used when depositing Ti directly on the back side of the wafer. In other words, since Ti is deposited after forming an oxide layer on the back side of the wafer, the increased oxide layer can relax the Ti deposition conditions.

[0081] In some embodiments, during step S2, the lower electrode power supply is kept off, i.e., the lower electrode power is not applied. This can prevent Ti or Ar from bombarding the film during the Ti deposition process, which would increase the film stress and thus improve the process quality.

[0082] In some embodiments, the thickness of the Ti layer is 50 nm to 500 nm; the thickness of the NiV layer is 100 nm to 800 nm; and the thickness of the Ag layer is 500 nm to 1500 nm.

[0083] In summary, the wafer backside metallization method provided in this application involves forming a dense layer on the backside of the wafer; and then forming a metal layer on the side of the dense layer away from the backside of the wafer via magnetron sputtering. This dense layer serves to prevent metal atoms from entering the wafer during magnetron sputtering, and the bonding force between the metal atoms and the dense layer is greater than the bonding force between the metal atoms and the wafer material. The metal atoms do not contain Al. Unlike related technologies that completely remove impurities from the backside of the wafer through acid washing and pre-cleaning, requiring the pre-plating of an Al layer before subsequent wafer backside metallization, this application, on the one hand, prevents metal atoms from magnetron sputtering from entering the wafer material layer, avoiding the formation of a double-layer structure that reduces bonding force; on the other hand, the bonding force between the dense layer and the metal atoms is greater than the bonding force between the metal atoms and the wafer material. Therefore, the wafer backside metallization method of this application can enhance the bonding force between the metal layer on the backside of the wafer and the wafer without forming an Al layer, reducing the risk of peeling, improving production efficiency, and reducing production costs.

[0084] Figure 8 shows a schematic diagram of the pre-cleaning chamber structure of an embodiment disclosed in this application. As shown in Figure 8, the semiconductor process apparatus includes a pre-cleaning chamber 20, a deposition chamber (not shown in Figure 8), an inlet assembly 20A, an upper electrode assembly 20B, a lower electrode assembly 20C, and a controller (not shown in Figure 8). The controller includes at least one processor and at least one memory, the memory storing a computer program that, when executed by the processor, implements the method of any of the above embodiments.

[0085] For example, the controller can be a host computer or a slave computer. The controller can open the valve of the air intake assembly 20A to introduce the corresponding etching gas into the pre-cleaning chamber 20; the controller can also control the flow rate of the etching gas by controlling the opening and closing degree of the valve of the air intake assembly 20A. The controller can also control the air extraction assembly to evacuate the interior of the pre-cleaning chamber 20, thereby controlling the pressure inside the pre-cleaning chamber 20 and removing etching byproducts.

[0086] In addition, the controller is communicatively connected to a detection module for detecting wafer surface cleanliness, and its memory stores etching process recipes corresponding to different cleanliness thresholds. Based on the cleanliness signal sent by the detection module, the controller calls the corresponding etching process recipe and generates corresponding control commands to control the air intake and / or air extraction components to perform partial or complete etching processes that match the current wafer cleanliness.

[0087] The upper electrode assembly 20B includes an RF coil 21, an upper RF power supply 23, and an upper matching unit 25. The controller further controls the upper RF power supply 23 to provide upper electrode power to the RF coil 21 through the upper matching unit 25, so that the RF coil 21 excites the etching gas inside the pre-cleaning chamber 20 to generate plasma. The upper RF power supply 23 is, for example, a high-frequency RF power supply with a frequency of, for example, 2 MHz.

[0088] The lower electrode assembly 20C includes a wafer carrier 22, a lower RF power supply 24, and a lower matching unit 26. The controller is also used to control the lower RF power supply 24 to provide lower electrode power to the lower electrode of the wafer carrier 22 through the lower matching unit 26, so that the lower electrode of the wafer carrier 22 is provided with RF bias voltage to attract plasma above the wafer W to bombard the wafer W.

[0089] The aforementioned deposition chambers are, for example, physical vapor deposition (PVD) chambers. There are, for example, three deposition chambers, used to deposit Ti, NiV, and Ag layers respectively. Since the method for depositing these metal layers using PVD is a well-known technique, it will not be described in detail here.

[0090] It is understood that the above embodiments are merely exemplary implementations used to illustrate the principles of this application, and this application is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and substance of this application, and these modifications and improvements are also considered to be within the scope of protection of this application.

Claims

1. A method of wafer backside metallization, characterized by, include: A dense layer is formed on the back side of the wafer; On the side of the dense layer away from the back side of the wafer, a metal layer is formed by magnetron sputtering. The dense layer is configured to prevent metal atoms from entering the wafer during magnetron sputtering, and the bonding force between the metal atoms and the material of the dense layer is greater than the bonding force between the metal atoms and the material of the wafer. The metal atoms do not contain Al.

2. The method for metallizing the back side of a wafer according to claim 1, characterized in that, The dense layer is an oxide layer; and / or, The thickness of the compact layer is greater than or equal to and less than or equal to 3. The method for metallizing the back side of a wafer according to claim 1, characterized in that, The metal atom includes at least one of Ti, Ni, V, and Ag.

4. The method for metallizing the back side of a wafer according to any one of claims 1 to 3, characterized in that, The formation of a dense layer on the back side of the wafer includes: Partial etching is performed on the natural oxide layer on the back side of the wafer, leaving the preserved natural oxide layer as the dense layer; or The natural oxide layer on the back side of the wafer is completely etched; the back side of the wafer is oxidized to form an oxide layer, which serves as the dense layer.

5. The method for metallizing the back side of a wafer according to claim 1, characterized in that, Prior to forming the oxide layer on the back side of the wafer, the method further includes: Determine whether the surface cleanliness of the wafer is greater than or equal to a preset threshold; When the surface cleanliness of the wafer is greater than or equal to the preset threshold, the process of forming a dense layer on the back side of the wafer includes: Partial etching is performed on the natural oxide layer on the back side of the wafer, and the remaining natural oxide layer is used as the dense layer; When the surface cleanliness of the wafer is less than the preset threshold, the process of forming a dense layer on the back side of the wafer includes: The natural oxide layer on the back side of the wafer is completely etched; the back side of the wafer is oxidized to form an oxide layer, which serves as the dense layer.

6. The method for metallizing the back side of a wafer according to claim 4, characterized in that, The partial etching of the natural oxide layer on the back side of the wafer includes: The wafer is placed in a pre-cleaning chamber; The back side of the wafer is pre-cleaned using an etching gas to remove impurities and partially etch the natural oxide layer.

7. The method for metallizing the back side of a wafer according to claim 4, characterized in that, The etching of the entire natural oxide layer on the back side of the wafer includes: The wafer is placed in a pre-cleaning chamber; The back side of the wafer is pre-cleaned using etching gas to remove impurities and simultaneously etch the natural oxide layer. The oxidation of the back side of the wafer to form an oxide layer includes: After the pre-cleaning process is completed, oxygen-containing gas is introduced into the pre-cleaning chamber to oxidize the back side of the wafer to form the oxide layer.

8. The method for metallizing the back side of a wafer according to claim 7, characterized in that, The oxygen-containing gas is oxygen, and the flow rate of the oxygen is greater than or equal to 10 sccm and less than or equal to 100 sccm; or, The oxygen is introduced into the pre-cleaning chamber for a duration greater than or equal to 5 seconds and less than or equal to 10 seconds.

9. The method for metallizing the back side of a wafer according to claim 1, characterized in that, The wafer is made of Si; The metal layer includes a Ti layer, a NiV layer, and an Ag layer formed sequentially away from the dense layer.

10. A semiconductor process apparatus, comprising a pre-cleaning chamber, an inlet assembly, an upper electrode assembly, a lower electrode assembly, a deposition chamber, and a controller, characterized in that, The controller includes at least one processor and at least one memory, the memory storing a computer program that, when executed by the processor, implements the method of wafer backside metallization as described in any one of claims 1 to 9.