Electromagnetic-interference shielding packaging structure and manufacturing method therefor, and electronic device
By combining insulating and conductive adhesive layers, the problem of large metal shielding cover size is solved, achieving electromagnetic shielding effect and structural stability, and supporting the miniaturization and weight reduction of electronic devices.
Patent Information
- Application Number
- PCT/CN2026/092187
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-22
- Publication Date
- 2026-11-19
AI Technical Summary
Existing metal shielding covers are bulky, hindering the miniaturization, thinning, and high-density development of electronic devices.
The device employs a combination of insulating and conductive adhesive layers. The insulating adhesive layer covers the outer wall of the electronic device, while the conductive adhesive layer covers the surface of the insulating adhesive layer and is electrically connected to the grounding point of the circuit board. The ratio of the coefficients of thermal expansion is 1 < n ≤ 4. Combined with a metal shielding cover, it forms an electromagnetic shielding structure.
It achieves the reduction of space occupation and weight while maintaining good electromagnetic shielding effect, adapts to electronic devices of different shapes, improves structural stability and reliability, and supports the miniaturization, thinning and lightening of equipment and high density.
Smart Images

Figure CN2026092187_19112026_PF_FP_ABST
Abstract
Description
Electromagnetic shielding packaging structure and its preparation method, electronic equipment
[0001] This application claims priority to Chinese Patent Application No. 202510619405.1, filed on May 13, 2025, entitled "Electromagnetic Shielding Packaging Structure and Preparation Method Thereof, Electronic Device", the entire contents of which are incorporated herein by reference. Technical Field
[0002] This disclosure relates to the field of electronic equipment technology, and in particular to electromagnetic shielding packaging structures and their preparation methods, as well as electronic equipment. Background Technology
[0003] Electronic components (such as chips) in electronic devices are not only susceptible to electromagnetic interference from other electronic components on the same circuit board, but also from electromagnetic interference from other external electronic devices. In order to protect electronic components from electromagnetic interference and prevent excessive electromagnetic radiation, metal shielding covers are usually installed on the outside of electronic components.
[0004] In related technologies, a metal shield is fixedly connected to a circuit board and grounded, and electronic components are housed inside the metal shield. There is a clear space gap between the inner wall of the metal shield and the electronic components to achieve a good electromagnetic shielding effect.
[0005] However, the aforementioned metal shielding covers have the disadvantage of being large in size, which is not conducive to the miniaturization, thinning, and high-density development of electronic devices. Summary of the Invention
[0006] This disclosure provides an electromagnetic shielding packaging structure and its preparation method, as well as an electronic device, which can solve the technical problem of large volume of metal shielding covers in related technologies. Specifically, the technical solution is as follows.
[0007] On one hand, an electromagnetic shielding encapsulation structure is provided, comprising a circuit board, electronic components, an insulating adhesive layer, and a conductive adhesive layer. The electronic components are fixed to the circuit board, and the insulating adhesive layer covers at least a portion of the outer wall of the electronic components. The conductive adhesive layer covers at least a portion of the surface of the insulating adhesive layer and is electrically connected to a grounding point provided on the circuit board. The ratio of the coefficients of thermal expansion of the insulating adhesive layer and the conductive adhesive layer at the same temperature is n, where 1 < n ≤ 4.
[0008] The electromagnetic shielding encapsulation structure provided in this disclosure enables the conductive adhesive layer to be electrically connected to the grounding point on the circuit board, thereby achieving electromagnetic shielding of electronic devices based on the conductive adhesive layer in the form of an adhesive layer. An insulating adhesive layer is provided between the conductive adhesive layer and the electronic device to isolate the electronic device from other electronic devices and to prevent short circuits by isolating the conductive adhesive layer from the electronic device. The insulating adhesive layer covers at least a portion of the outer wall of the electronic device, and the conductive adhesive layer covers at least a portion of the surface of the insulating adhesive layer. This allows both the insulating and conductive adhesive layers to be adapted to the shape of the electronic device, reducing or eliminating the need for clearance height, reducing the space occupied by the electromagnetic shielding structure, and the adhesive material also helps to reduce the weight of the electromagnetic shielding structure. Therefore, the electromagnetic shielding encapsulation structure provided in this disclosure, while maintaining good electromagnetic shielding effect, also has the advantages of miniaturization and lightweight, which is beneficial to the miniaturization, thinning, and high-density development of electronic devices.
[0009] By limiting the ratio of the thermal expansion coefficients of the insulating and conductive adhesive layers as described above, on the one hand, a high degree of matching in their thermal expansion coefficients is ensured. This effectively prevents excessive internal stress caused by the difference in expansion and contraction between the two materials during temperature changes, which could lead to delamination, cracking, or other phenomena between the adhesive layers, affecting the integrity and stability of the electromagnetic shielding encapsulation structure. On the other hand, the thermal expansion coefficient of the insulating adhesive layer is greater than that of the conductive adhesive layer. This difference in thermal expansion coefficients makes the insulating adhesive layer more flexible than the conductive adhesive layer, ensuring that the insulating adhesive layer always maintains effective isolation from the conductive adhesive layer, preventing insulation damage caused by thermal stress, and ensuring the reliability of insulation performance. Tests showed that, with the ratio of the thermal expansion coefficients of the insulating and conductive adhesive layers meeting the above requirements, no cracks or separation of the adhesive layers were observed after low-temperature-high-temperature cyclic aging.
[0010] In some possible implementations, the low-temperature coefficient of thermal expansion of the insulating adhesive layer is greater than 10 ppm / ℃ and less than 200 ppm / ℃, and the high-temperature coefficient of thermal expansion of the insulating adhesive layer is greater than or equal to 200 ppm / ℃ and less than 1000 ppm / ℃; the low-temperature coefficient of thermal expansion of the conductive adhesive layer is greater than or equal to 10 ppm / ℃ and less than 100 ppm / ℃, and the high-temperature coefficient of thermal expansion is greater than or equal to 100 ppm / ℃ and less than 500 ppm / ℃. Herein, the low-temperature coefficient of thermal expansion is the coefficient of thermal expansion of the adhesive layer under conditions below the glass transition temperature, and the high-temperature coefficient of thermal expansion is the coefficient of thermal expansion of the adhesive layer under conditions above the glass transition temperature.
[0011] At temperatures less than T gIn low-temperature environments, both the insulating and conductive adhesive layers have low coefficients of thermal expansion. This ensures that the adhesive layers will not crack or delaminate due to excessive thermal shrinkage at low temperatures, maintaining the integrity and stability of the electromagnetic shielding encapsulation structure and ensuring good electromagnetic shielding and insulation performance even at low temperatures. On the other hand, at temperatures greater than T... g In high-temperature environments, both the insulating adhesive layer and the conductive adhesive layer have high coefficients of thermal expansion. The insulating adhesive layer can better adapt to the thermal deformation of the structure at high temperatures, fill any gaps that may occur, and further enhance the insulation effect. Meanwhile, the conductive adhesive layer can maintain good ductility and conductivity at high temperatures, avoid interruption of the conductive path due to excessive expansion, and maintain electromagnetic shielding performance.
[0012] In some possible implementations, the electromagnetic shielding encapsulation structure further includes a metal shielding cover surrounding the electronic device and electrically connected to the grounding point of the circuit board. The metal shielding cover has an opening on the side facing away from the circuit board, and the side of the electronic device facing away from the circuit board is located outside the opening or flush with the opening. An insulating adhesive layer covers at least a portion of the outer wall of the electronic device, and the insulating adhesive layer is at least partially located inside the metal shielding cover. A conductive adhesive layer is in contact with the insulating adhesive layer and is also electrically connected to the metal shielding cover.
[0013] The height of the metal shielding cover is equal to or less than the height of the electronic device. While ensuring the excellent electromagnetic shielding effect provided by the metal shielding cover, it also ensures the advantages of small size and low weight of the electromagnetic shielding packaging structure. In addition, the metal shielding cover surrounds the outside of the electronic device and is electrically connected to the grounding point of the circuit board, which can also serve as a support and protection structure, thereby improving the structural stability and reliability of the electromagnetic shielding packaging structure.
[0014] In some possible implementations, the side of the electronic device facing away from the circuit board has a metal encapsulation layer, the metal encapsulation layer being at least partially located outside the opening, the insulating adhesive layer covering the outer wall of the electronic device without the metal encapsulation layer, and the conductive adhesive layer being electrically connected to the metal shield and the metal encapsulation layer, respectively.
[0015] For electronic devices with metal encapsulation layers, the embodiments of this disclosure make reasonable use of the metal encapsulation layer, which, together with the conductive adhesive layer and the metal shielding cover, constitutes an electromagnetic encapsulation structure. This not only achieves excellent electromagnetic shielding effect, but also has the advantages of small size and low weight.
[0016] In some possible implementations, the insulating adhesive layer covers all the outer walls of the electronic device that are not shielded by the circuit board and partially covers the circuit board, while the insulating adhesive layer avoids the grounding point of the circuit board; the conductive adhesive layer covers the surface of the insulating adhesive layer and is electrically connected to the grounding point of the circuit board.
[0017] In this implementation scheme, the shape of the portion of the insulating adhesive layer covering the electronic device is adapted to the shape of the electronic device, and the shape of the conductive adhesive layer is adapted to the shape of the insulating adhesive layer. Thus, it can adapt to the packaging of electronic devices of different sizes and shapes, which is conducive to the miniaturization of electromagnetic shielding packaging structures. At the same time, it also has the advantages of strong electromagnetic shielding reliability and simple manufacturing process.
[0018] In some possible implementations, the conductive adhesive layer satisfies at least one of the following physical properties: the thickness of the conductive adhesive layer is 30μm-150μm, the conductivity of the conductive adhesive layer is greater than 1E+5S / m, the Young's modulus of the conductive adhesive layer is greater than or equal to 150MPa, and the elongation at break of the conductive adhesive layer is greater than or equal to 2%.
[0019] The conductive adhesive layer has a thickness of 30μm-150μm, ensuring both reliable electromagnetic shielding and a thin profile. Its conductivity is greater than 1E+5S / m to guarantee that it meets electromagnetic shielding requirements. The Young's modulus is greater than or equal to 30MPa to ensure good shape and dimensional stability, thus maintaining stable electromagnetic shielding and electrical connection performance. The elongation at break is greater than or equal to 2%, improving the fatigue resistance and reliability of the electromagnetic shielding encapsulation structure and ensuring its integrity and stability under different temperature conditions.
[0020] In some possible implementations, the conductive adhesive layer comprises a polyurethane matrix and metal conductive particles dispersed in the polyurethane matrix, wherein the mass percentage of the metal conductive particles in the conductive adhesive layer is greater than or equal to 70% and less than or equal to 90%. Using polyurethane as the matrix of the conductive adhesive layer allows for a tight bond between the conductive adhesive layer and insulating layers, PCB solder mask, etc., ensuring no delamination, while the metal conductive particles impart good conductivity to the conductive adhesive layer.
[0021] In some possible implementations, the polyurethane matrix comprises polyurethane and a modifier, wherein the modifier comprises at least one selected from alkyd resin, acrylic resin, and epoxy resin. The modifier increases the adhesion between the conductive adhesive layer and other interfaces, while also increasing the waterproof capability of the conductive adhesive layer, thereby improving the structural stability of the electromagnetic shielding encapsulation structure.
[0022] In some possible implementations, the conductive metal particles satisfy at least one of the following conditions: the conductive metal particles include at least two of the following: spherical or near-spherical particles, sheet-like particles, dendritic particles, and fibrous particles; and the particle size D50 of the conductive metal particles is 0.5 μm-50 μm. By using a combination of two or more particle shapes, it is beneficial for the conductive metal particles to form a continuous conductive network in the polyurethane matrix, thereby improving the conductivity of the conductive adhesive layer and also enhancing its mechanical properties.
[0023] In some possible implementations, the conductive metal particles include spherical or near-spherical particles and sheet-like particles, wherein the mass percentage of the sheet-like particles in the conductive metal particles is greater than or equal to 50%, and the mass percentage of the spherical or near-spherical particles in the conductive metal particles is less than or equal to 50%. The combination of conductive metal particles of different sizes also helps the conductive adhesive layer to possess both good Young's modulus and elongation at break.
[0024] In some possible implementations, the sheet-like particles include a first sheet-like particle and a second sheet-like particle, wherein the first sheet-like particle has a particle size D50 of 5 μm-20 μm, and the second sheet-like particle has a particle size D50 of 1 μm-5 μm. This configuration allows the two particle sizes to work together to form a multi-level conductive network, improving conductivity and also contributing to a conductive adhesive layer with good Young's modulus and elongation at break.
[0025] In some possible implementations, the conductive adhesive layer comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of conductive metal particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of dispersant. Based on the above formulation of the conductive adhesive layer, excellent adhesion is achieved between the conductive adhesive layer and the PCB solder mask, epoxy molding compound, and metal encapsulation layer, with an adhesion strength greater than 4B in the cross-cut adhesion test.
[0026] In some possible implementations, the insulating adhesive layer satisfies at least one of the following physical properties: the thickness of the insulating adhesive layer is 20μm-200μm, the Young's modulus of the insulating adhesive layer is greater than or equal to 200MPa, and the elongation at break of the insulating adhesive layer is greater than or equal to 5%.
[0027] The thickness of the insulating adhesive layer ranges from 20μm to 200μm, ensuring both reliable insulation and a relatively thin profile. The Young's modulus of the insulating adhesive layer is greater than or equal to 200MPa to ensure good shape and dimensional stability, thereby maintaining stable electromagnetic shielding and electrical connection performance. The elongation at break of the insulating adhesive layer is greater than or equal to 5%, improving the fatigue resistance and reliability of the electromagnetic shielding encapsulation structure, and ensuring its integrity and stability under different temperature conditions.
[0028] In some possible implementations, the insulating adhesive layer comprises a polyurethane matrix and insulating filler particles dispersed in the polyurethane matrix, wherein the mass percentage of the insulating filler particles in the insulating adhesive layer is greater than or equal to 20% and less than or equal to 90%. Using polyurethane as the matrix of the insulating adhesive layer, and making it use the same matrix resin as the conductive adhesive layer, helps to improve interfacial adhesion and prevent aging and cracking of the insulating and conductive adhesive layers. The insulating filler particles not only improve the insulation performance of the insulating adhesive layer but also enhance its mechanical properties, heat resistance, and chemical stability.
[0029] In some possible implementations, the insulating filler particles satisfy at least one of the following conditions: the insulating filler particles include at least one of titanium dioxide particles, silicon dioxide particles, aluminum oxide particles, magnesium oxide particles, zinc oxide particles, aluminum nitride particles, boron nitride particles, silicon carbide particles, calcium sulfate particles, calcium carbonate particles, barium sulfate particles, barium titanate particles, sulfate particles, carbonate particles, and titanate particles; the particle size D50 of the insulating filler particles is 0.1 μm-20 μm. When the particle size D50 of the insulating filler particles is greater than or equal to 0.1 μm, its dispersibility in the insulating coating is better, which is beneficial to improving storage stability. When the particle size D50 of the insulating filler particles is less than or equal to 20 μm, it reduces the valve clogging problem caused by excessively large particle size during coating, such as during dispensing.
[0030] In some possible implementations, the insulating adhesive layer comprises the following components in parts by weight: 10-50 parts of polyurethane or modified polyurethane adhesive, 20-90 parts of insulating filler particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of thixotropic agent. Based on the above formulation of the insulating adhesive layer, excellent adhesion is achieved between the insulating adhesive layer and PCB solder mask, optional epoxy molding compound, and optional metal encapsulation layer, with an adhesion strength greater than 4B in the cross-cut adhesion test.
[0031] On the other hand, a method for preparing an electromagnetic shielding encapsulation structure is provided. The electromagnetic shielding encapsulation structure is as described in any of the above descriptions. The preparation method includes: mounting electronic devices on a circuit board, applying an insulating coating and curing it to form an insulating adhesive layer, applying a conductive coating and curing it to form a conductive adhesive layer, thereby preparing the electromagnetic shielding encapsulation structure.
[0032] The fabrication steps are adapted to the specific structure of the electromagnetic shielding package. For example, for an electromagnetic shielding package with an open metal shield, the fabrication method further includes mounting the open metal shield onto the circuit board. Additionally, the application positions of the insulating and conductive coatings are also adapted to the specific structure of the electromagnetic shielding package.
[0033] In some possible implementations, the insulating coating comprises the following components in parts by weight: 10-50 parts of polyurethane or modified polyurethane adhesive, 20-90 parts of insulating filler particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, 0-5 parts of thixotropic agent, and 10-60 parts of solvent; the conductive coating comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of metallic conductive particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, 0-5 parts of dispersant, and 5-30 parts of solvent. Both the insulating and conductive coatings can be applied to the corresponding positions by dispensing, spraying, or other methods, offering advantages such as ease of operation, high operational reliability, easy control of adhesive layer thickness, improved production efficiency, and increased material utilization.
[0034] In some possible implementations, the conductive coating satisfies at least one of the following physical properties: viscosity of 5000 mPa·s-50000 mPa·s, thixotropic index ≥1.3; the insulating coating satisfies at least one of the following physical properties: viscosity of 10000 mPa·s-50000 mPa·s or 4000 mPa·s-50000 mPa·s, thixotropic index ≥1.2. This allows the coating to be suitable for coating scenarios with different shapes, for example, to achieve sufficient and reliable coverage of uneven electronic components on circuit boards, while ensuring that the edges of the components to be covered, such as the edges of electronic components, are completely covered, and that the thickness of the adhesive layer is relatively uniform.
[0035] In another aspect, an electronic device is provided, the electronic device including a housing and an electromagnetic shielding encapsulation structure housed inside the housing, the electromagnetic shielding encapsulation structure being as described in any of the above descriptions.
[0036] For example, the electronic device may be a mobile phone, tablet, computer, watch, headphones, or smart wearable device (such as AR glasses, VR glasses, etc.). Attached Figure Description
[0037] Figure 1 is a schematic diagram of an exemplary electromagnetic shielding packaging structure provided in an embodiment of this disclosure;
[0038] Figure 2 is a schematic diagram of another exemplary electromagnetic shielding packaging structure provided in an embodiment of this disclosure;
[0039] Figure 3 is a schematic diagram of another exemplary electromagnetic shielding packaging structure provided in the embodiments of this disclosure.
[0040] The reference numerals in the attached figures represent: 100, circuit board; 101, grounding point; 200, electronic device; 201, metal encapsulation layer; 300, insulating adhesive layer; 400, conductive adhesive layer; 500, metal shielding cover. Detailed Implementation
[0041] To address the disadvantage of large size in existing electromagnetic shielding covers for electronic devices, which hinders the miniaturization, thinning, and high-density development of electronic equipment, this disclosure provides a novel electromagnetic shielding packaging structure, as shown in Figures 1-3. This electromagnetic shielding packaging structure includes a circuit board 100, an electronic device 200, an insulating adhesive layer 300, and a conductive adhesive layer 400. The electronic device 200 is fixed to the circuit board 100, and the insulating adhesive layer 300 covers at least a portion of the outer wall of the electronic device 200. The conductive adhesive layer 400 covers at least a portion of the surface of the insulating adhesive layer 300 and is electrically connected to a grounding point 101 on the circuit board 100. The ratio of the thermal expansion coefficients of the insulating adhesive layer and the conductive adhesive layer at the same temperature is n, where 1 < n ≤ 4.
[0042] The electromagnetic shielding packaging structure provided in this embodiment enables the conductive adhesive layer 400 to be electrically connected to the grounding point 101 provided on the circuit board 100, thereby achieving electromagnetic shielding of the electronic device 200 based on the conductive adhesive layer 400 in the form of an adhesive layer. By providing an insulating adhesive layer 300 between the conductive adhesive layer 400 and the electronic device 200, the electronic device 200 is isolated from other electronic devices 200, and short circuits are avoided by isolating the conductive adhesive layer 400 from the electronic device 200. The insulating adhesive layer 300 covers at least a portion of the outer wall of the electronic device 200, and the conductive adhesive layer 400 covers at least a portion of the surface of the insulating adhesive layer 300. This allows both the insulating adhesive layer 300 and the conductive adhesive layer 400 to be adapted to the shape of the electronic device 200, reducing or avoiding the need for clearance height, reducing the space occupied by the electromagnetic shielding structure, and the adhesive layer material also helps to reduce the weight of the electromagnetic shielding structure. Thus, the electromagnetic shielding encapsulation structure provided in this embodiment of the present disclosure has the advantages of miniaturization and light weight while maintaining good electromagnetic shielding effect, which is conducive to the miniaturization, thinning and high density development of electronic devices.
[0043] To prevent interfacial delamination and microcracks from forming between the insulating adhesive layer 300 and the conductive adhesive layer 400 after aging, which could lead to shielding failure, the embodiments of this disclosure ensure that the coefficients of thermal expansion (CTE) of the insulating adhesive layer 300 and the conductive adhesive layer 400 satisfy the following relationship: the ratio of the coefficients of thermal expansion of the insulating adhesive layer 300 and the conductive adhesive layer 400 at the same temperature is n, where 1 < n ≤ 4, and further, 1 < n ≤ 3. For example, the value of n includes, but is not limited to, the following point values or the numerical range formed by any two point values: 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, etc.
[0044] It should be noted that the coefficient of thermal expansion involved in the embodiments of this disclosure can be a linear coefficient of thermal expansion, such as the linear coefficient of thermal expansion along the stacking arrangement direction of the insulating adhesive layer 300 and the conductive adhesive layer 400. The coefficient of thermal expansion can be tested by thermomechanical analysis (TMA) with a test temperature range of -60℃ to 200℃ and a heating rate that can be set to 5℃ / min.
[0045] By limiting the ratio of the thermal expansion coefficients of the insulating adhesive layer 300 to the conductive adhesive layer 400 as described above, on the one hand, a high degree of matching in their thermal expansion coefficients is ensured. This effectively avoids excessive internal stress caused by the difference in expansion and contraction between the two materials during temperature changes, which could lead to delamination, cracking, or other phenomena between the adhesive layers, affecting the integrity and stability of the electromagnetic shielding encapsulation structure. On the other hand, the thermal expansion coefficient of the insulating adhesive layer 300 is greater than that of the conductive adhesive layer 400. This difference in thermal expansion coefficients makes the insulating adhesive layer 300 more flexible than the conductive adhesive layer 400, ensuring that the insulating adhesive layer 300 always maintains effective isolation from the conductive adhesive layer 400, preventing insulation damage caused by thermal stress, and ensuring the reliability of insulation performance. Testing showed that, with the ratio of the thermal expansion coefficients of the insulating adhesive layer 300 to the conductive adhesive layer 400 meeting the above requirements, after low-temperature-high-temperature cyclic aging, there were no cracks or separation between the insulating adhesive layer and the conductive adhesive layer 400.
[0046] As mentioned above, the insulating adhesive layer 300 covers at least a portion of the outer wall of the electronic device 200. This means that for the outer wall of the electronic device 200 that is not shielded by the circuit board 100, a portion or all of the outer wall can be covered by the insulating adhesive layer 300, thereby achieving an insulating isolation effect. Specifically, the insulating adhesive layer 300 covers at least the circuit board 100 located around the electronic device 200 to ensure the insulating isolation effect on the electronic device 200. The conductive adhesive layer 400 covers at least a portion of the surface of the insulating adhesive layer 300. The area covered by the conductive adhesive layer 400 is sufficient to achieve a sufficiently reliable electromagnetic shielding effect for the electronic device 200. The specific arrangement of the insulating adhesive layer 300 and the conductive adhesive layer 400 can be determined according to the actual scenario. The following examples illustrate this.
[0047] In some embodiments (1), as shown in Figures 1-2, the electromagnetic shielding encapsulation structure further includes a metal shield 500, which surrounds the outside of the electronic device 200 and is electrically connected to the grounding point 101 of the circuit board 100. The side of the metal shield 500 facing away from the circuit board 100 has an opening, and the side of the electronic device 200 facing away from the circuit board 100 is located outside the opening or flush with the opening. An insulating adhesive layer 300 covers at least a portion of the outer wall of the electronic device 200, and the insulating adhesive layer 300 is at least partially located inside the metal shield 500. A conductive adhesive layer 400 is in contact with the insulating adhesive layer 300 and is also electrically connected to the metal shield 500.
[0048] This example retains a portion of the metal shield 500, with an opening on the side of the metal shield 500 facing away from the circuit board 100. For example, the opening's position corresponds to the position of the electronic device 200, allowing the electronic device 200 to be exposed through the opening. The side of the electronic device 200 facing away from the circuit board 100 is located outside the opening or flush with it. Therefore, the height of the metal shield 500 is equal to or less than the height of the electronic device 200, preventing the metal shield 500 from exceeding the height of the electronic device 200. This ensures excellent electromagnetic shielding performance while maintaining the advantages of a small size and low weight in the electromagnetic shielding packaging structure. Furthermore, the metal shield 500, surrounding the electronic device 200 and electrically connected to the grounding point 101 of the circuit board 100, also serves as a support and protective structure, enhancing the structural stability and reliability of the electromagnetic shielding packaging structure.
[0049] In related technologies, the metal shielding cover has no openings and is positioned above the electronic device. Furthermore, the metal shielding cover typically uses a high-density metal material (e.g., density 8.93 g / cm³). 3 The use of nickel silver (a type of copper alloy) necessitates a gap between the top wall of the metal shield and the top wall of the electronic device as a clearance height, thereby increasing the volume of the metal shield and consequently its weight.
[0050] This embodiment of the invention uses a conductive adhesive layer 400 to replace part of the metal shielding cover, thereby reducing the volume and weight of the metal shielding cover 500 while still achieving electromagnetic shielding. The metal shielding cover 500 in this embodiment can be made of any known metal shielding cover material. Testing has shown that, compared to related technologies that use only metal shielding covers, this embodiment combines the conductive adhesive layer 400 with an open metal shielding cover 500, achieving both thinning and weight reduction. For example, the thickness can be reduced by at least 0.1 mm, and the weight by at least 50%.
[0051] In this example, the insulating adhesive layer 300 covers at least a portion of the outer wall of the electronic device 200, and the insulating adhesive layer 300 is at least partially located inside the metal shield 500. For example, the insulating adhesive layer 300 covers at least the portion of the electronic device 200 inside the outer metal shield 500, and the insulating adhesive layer 300 covers the outer wall of the electronic device 200 located inside the metal shield 500, thereby achieving a surrounding effect on the current electronic device 200, so that the current electronic device 200 is insulated from other electronic devices 200 in its vicinity. The conductive adhesive layer 400 is in contact with the insulating adhesive layer 300, and the conductive adhesive layer is also electrically connected to the metal shield 500, which is in turn electrically connected to the grounding point 101 on the circuit board 100. That is, the conductive adhesive layer is indirectly electrically connected to the grounding point 101 through the metal shield 500, creating a Faraday cage to achieve a shielding effect.
[0052] As an example, referring to Figure 1, the side of the electronic device 200 facing away from the circuit board 100 has a metal encapsulation layer 201, which is at least partially located outside the opening. An insulating adhesive layer 300 covers the outer wall of the electronic device 200 where the metal encapsulation layer 201 is not provided. A conductive adhesive layer 400 is electrically connected to the metal shield 500 and the metal encapsulation layer 201, respectively.
[0053] In this example, the metal encapsulation layer 201 can be located outside the opening of the metal shield 500, or it can penetrate through the opening of the metal shield 500. That is, part of the metal encapsulation layer 201 is located outside the opening of the metal shield 500, and another part of the metal encapsulation layer 201 is located inside the opening of the metal shield 500. The arrangement position of the conductive adhesive layer 400 is set according to the different situations described above. For example, when the metal encapsulation layer 201 penetrates through the opening of the metal shield 500, the conductive adhesive layer 400 can be set to block the opening of the metal shield 500.
[0054] In this case, the side of the electronic device 200 facing away from the circuit board 100 has a metal encapsulation layer 201 (also known as a metal sputtering layer). Considering that the metal encapsulation layer 201 can also provide electromagnetic shielding for the electronic device 200, in this embodiment, the insulating adhesive layer 300 covers the outer wall of the electronic device 200 without the metal encapsulation layer 201 for isolation, while the conductive adhesive layer 400 is electrically connected to the metal shield 500 and the metal encapsulation layer 201 respectively. Thus, the grounding point 101-metal shield 500-conductive adhesive layer 400-metal encapsulation layer 201 are electrically connected. The metal shield 500, conductive adhesive layer 400, and metal encapsulation layer 201 work together to form a Faraday cage to achieve electromagnetic shielding.
[0055] As can be seen, for the electronic device 200 with the metal encapsulation layer 201, the embodiments of this disclosure make reasonable use of the metal encapsulation layer 201, so that it, together with the conductive adhesive layer 400 and the metal shielding cover 500, forms an electromagnetic encapsulation structure, which not only achieves excellent electromagnetic shielding effect, but also has the advantages of small size and low weight.
[0056] It is not excluded that, referring to Figure 2, for electronic devices 200 without a metal encapsulation layer 201, the insulating adhesive layer 300 can cover all the outer walls of the electronic device 200 that are not shielded by the circuit board 100, especially the outer walls of the electronic device 200 located outside the opening. The conductive adhesive layer 400 covers the surface of the insulating adhesive layer 300 and is connected to the metal shielding cover 500, which can also achieve excellent electromagnetic shielding effect and has the advantages of small size and low weight.
[0057] In some implementation schemes (2), as shown in Figure 3, the insulating adhesive layer 300 covers all the outer walls of the electronic device 200 that are not covered by the circuit board 100 and covers part of the circuit board 100, and the insulating adhesive layer 300 avoids the grounding point 101 of the circuit board 100; the conductive adhesive layer 400 covers the surface of the insulating adhesive layer 300, and the conductive adhesive layer 400 is electrically connected to the grounding point 101 of the circuit board 100.
[0058] In this implementation scheme, the shape of the portion of the insulating adhesive layer 300 covering the electronic device 200 is adapted to the shape of the electronic device 200, and the shape of the conductive adhesive layer 400 is adapted to the shape of the insulating adhesive layer 300. Thus, it can adapt to the packaging of electronic devices 200 of different sizes and shapes, which is conducive to the miniaturization of electromagnetic shielding packaging structures. At the same time, it also has the advantages of strong electromagnetic shielding reliability and simple manufacturing process.
[0059] As an example, the circuit board 100 may have multiple electronic devices 200, each covered by a continuously arranged insulating adhesive layer 300. This insulating adhesive layer 300 also covers the circuit board 100 between any two adjacent electronic devices 200. A conductive adhesive layer 400 is continuously arranged and covers the surface of the insulating adhesive layer 300. Thus, any two adjacent electronic devices 200 can be isolated by the insulating adhesive layer 300 and achieve reliable electromagnetic shielding through the conductive adhesive layer 400. This solution demonstrates high adaptability to situations where multiple electronic devices 200 are mounted on the circuit board 100, and where the types and sizes of the electronic devices 200 vary, significantly simplifying the manufacturing process.
[0060] The insulating and conductive adhesive layers have different coefficients of thermal expansion at different temperatures. Building upon the above requirements, the insulating adhesive layer's low-temperature thermal expansion coefficient is greater than 10 ppm / ℃ and less than 200 ppm / ℃ (e.g., 80 ppm / ℃ - 150 ppm / ℃), and its high-temperature thermal expansion coefficient is greater than or equal to 200 ppm / ℃ and less than 1000 ppm / ℃ (e.g., 300 ppm / ℃ - 500 ppm / ℃). Similarly, the conductive adhesive layer's low-temperature thermal expansion coefficient is greater than or equal to 10 ppm / ℃ and less than 100 ppm / ℃ (e.g., 40 ppm / ℃ - 100 ppm / ℃), and its high-temperature thermal expansion coefficient is greater than or equal to 100 ppm / ℃ and less than 500 ppm / ℃ (e.g., 150 ppm / ℃ - 300 ppm / ℃).
[0061] Among them, the low-temperature thermal expansion coefficient is the coefficient of thermal expansion of the adhesive layer when it is below the glass transition temperature (T). g The coefficient of thermal expansion under certain conditions is the coefficient of thermal expansion of the adhesive layer under conditions greater than the glass transition temperature.
[0062] It should be noted that the low-temperature thermal expansion coefficient of the insulating adhesive layer is greater than that of the conductive adhesive layer, and the high-temperature thermal expansion coefficient of the insulating adhesive layer is greater than that of the conductive adhesive layer.
[0063] Through the above scheme, on the one hand, at temperatures less than T g In low-temperature environments, both the insulating and conductive adhesive layers have low coefficients of thermal expansion. This ensures that the adhesive layers will not crack or delaminate due to excessive thermal shrinkage at low temperatures, maintaining the integrity and stability of the electromagnetic shielding encapsulation structure and ensuring good electromagnetic shielding and insulation performance even at low temperatures. On the other hand, at temperatures greater than T... g In high-temperature environments, both the insulating adhesive layer and the conductive adhesive layer have high coefficients of thermal expansion. The insulating adhesive layer can better adapt to the thermal deformation of the structure at high temperatures, fill any gaps that may occur, and further enhance the insulation effect. Meanwhile, the conductive adhesive layer can maintain good ductility and conductivity at high temperatures, avoid interruption of the conductive path due to excessive expansion, and maintain electromagnetic shielding performance.
[0064] Furthermore, in some examples, the difference between the high-temperature thermal expansion coefficient and the low-temperature thermal expansion coefficient of the conductive adhesive layer can be greater than or equal to 50 ppm / ℃ and less than or equal to 150 ppm / ℃, which is beneficial for the conductive adhesive layer to have both good Young's modulus and elongation at break.
[0065] For any of the electromagnetic shielding encapsulation structures mentioned above, the conductive adhesive layer can be further made to meet at least one of the following physical properties: the thickness of the conductive adhesive layer is 30μm-150μm, the conductivity of the conductive adhesive layer is greater than 1E+5S / m, the Young's modulus of the conductive adhesive layer is greater than or equal to 30MPa, and the elongation at break of the conductive adhesive layer is greater than or equal to 2% (and may be greater than or equal to 5%). For example, the conductive adhesive layer can simultaneously meet all of the above physical properties.
[0066] The thickness of the conductive adhesive layer is 30μm-150μm. Tests have shown that the electromagnetic shielding effectiveness of a 100-micron thick conductive adhesive layer can reach 30dB@0.7-5GHz, ensuring that the conductive adhesive layer has both reliable electromagnetic shielding effect and the advantage of thinness.
[0067] The conductivity of the conductive adhesive layer is greater than 1E+5S / m, that is, 1×10⁻⁵S / m. 5 The conductivity of the conductive adhesive layer is measured to ensure that its conductivity meets electromagnetic shielding requirements. Furthermore, the conductivity of the conductive adhesive layer is 3.5 × 10⁻⁶ S / m. 5 S / m-5×10 5 The conductivity (S / m) not only meets the electromagnetic shielding requirements but also simplifies the formulation of the conductive adhesive layer. Testing in this embodiment shows that the conductive adhesive layer meeting the above conductivity requirement achieves an electromagnetic shielding effectiveness (SE) greater than or equal to 20 dB. The SE is tested using the flange coaxial method at a frequency of 1.5 GHz.
[0068] When the Young's modulus of the conductive adhesive layer is greater than or equal to 30 MPa, it can ensure that the conductive adhesive layer can provide a certain rigid support for the electromagnetic shielding encapsulation structure, so that it can maintain good shape and dimensional stability when subjected to external forces, thereby maintaining the performance stability of electromagnetic shielding and electrical connection.
[0069] The conductive adhesive layer has an elongation at break greater than or equal to 2%. This not only allows the conductive adhesive layer to adapt to changes such as vibration, impact, or thermal expansion and contraction when electronic devices are subjected to these factors, but also prevents it from easily breaking, thus improving the fatigue resistance and reliability of the electromagnetic shielding packaging structure. Furthermore, the high elongation at break allows the conductive adhesive layer to relieve stress through its own deformation, avoiding cracking or debonding between the conductive adhesive layer and other materials due to thermal stress concentration. This ensures the integrity and stability of the electromagnetic shielding packaging structure under different temperature conditions.
[0070] The above-described performance arrangement applicable to the conductive adhesive layer can make the conductive adhesive layer include: a polyurethane matrix and metal conductive particles dispersed in the polyurethane matrix, wherein the mass percentage of the metal conductive particles in the conductive adhesive layer is greater than or equal to 70% and less than or equal to 90%.
[0071] Using polyurethane as the substrate for conductive adhesive layers offers at least the following advantages: good adhesion, excellent flexibility and elasticity, good insulation properties, good chemical stability, and good processability. These advantages are highly beneficial for imparting these properties to the conductive adhesive layer. Therefore, using polyurethane as the substrate for conductive adhesive layers allows for a tight bond between the conductive adhesive layer and insulating layers, PCB solder mask, etc., ensuring no delamination.
[0072] Metal conductive particles impart good conductivity to the conductive adhesive layer. The mass percentage of metal conductive particles in the conductive adhesive layer is greater than or equal to 70% and less than or equal to 90%, including but not limited to the following point values or numerical ranges formed by any two point values: 70%, 75%, 80%, 85%, 90%, etc.
[0073] In some examples, the polyurethane matrix contains 100% polyurethane resin by mass. In other examples, the polyurethane matrix includes polyurethane and a modifier (in which case the polyurethane matrix can be referred to as a modified polyurethane matrix). The modifier includes at least one of alkyd resin, acrylic resin, and epoxy resin. The above-mentioned modifier is used to increase the adhesion between the conductive adhesive layer and other interfaces, while increasing the waterproof capability of the conductive adhesive layer and improving the structural stability of the electromagnetic shielding encapsulation structure.
[0074] For schemes containing modifiers, the mass percentage of the modifier in the polyurethane matrix can be 50%-90%, or more specifically 60%-90%, which can be the following point values or a numerical range consisting of any two point values: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.
[0075] In some examples, the modifier is an alkyd resin, which is obtained by polycondensation reaction of a polyol, a polyacid (e.g., a dicarboxylic acid), and a fatty acid or fatty oil (e.g., a triglyceride ester). For example, the polyol may be glycerol or pentaerythritol, the polyacid may be at least one of terephthalic acid, isophthalic acid, and adipic acid, the fatty oil may be vegetable oil such as linseed oil, tung oil, soybean oil, or tall oil, and the fatty acid may be synthetic fatty acid.
[0076] For a polyurethane matrix including a modifier, the modifier can be chemically grafted onto the polyurethane resin to form a modifier-modified polyurethane resin, or the modifier can be independent of the polyurethane resin, and the two can be blended in proportion and then film-formed to obtain a polyurethane matrix with a modifier.
[0077] In some examples, the modifier is an alkyd resin, which is beneficial for enhancing the adhesion of the adhesive layer. The alkyd resin can be chemically grafted onto the polyurethane resin to prepare an alkyd-modified polyurethane resin. The preparation method can be as follows:
[0078] The preparation of isocyanate-terminated polyurethane prepolymers includes: adding polyether polyol, polyester polyol (e.g., polyethylene adipate) and polyisocyanate (e.g., toluene diisocyanate TDI) in proportion to a reaction vessel, and reacting them under suitable temperature and stirring conditions to generate isocyanate-terminated polyurethane prepolymers.
[0079] Alkyd resin (which can be considered as an alkyd resin prepolymer containing hydroxyl groups) is prepared by mixing and stirring a polyurethane prepolymer in a specific ratio to obtain an alkyd-modified polyurethane resin. During this process, the hydroxyl groups (-OH) in the alkyd resin react with the isocyanate groups (-NCO) in the polyurethane prepolymer to form urethane bonds (-NHCOO-), thereby introducing the alkyd resin into the polyurethane molecular chain and achieving the modification of polyurethane by the alkyd resin.
[0080] The mass ratio of alkyd resin to polyurethane resin can be adjusted according to the properties of the polyurethane resin to be modified with alkyd resin. The structure of alkyd resin and polyurethane resin can also be adapted by selecting appropriate polyacids, polyols and polyisocyanates based on performance.
[0081] Considering the coatability of conductive coatings, such as the feasibility of dispensing or spraying, polyurethane materials or modified polyurethane materials can be liquid or solid at room temperature. During application, the polyurethane material or modified polyurethane material is dissolved in a solvent to improve its coatability. The solvent can be, for example, an environmentally friendly solvent, such as D30, D40, D50, D60, D70, D80, or D90 solvent oil.
[0082] The conductive particles involved in the conductive adhesive layer can be silver particles, copper particles, nickel particles, and alloy particles (such as silver-coated copper particles, silver-coated nickel particles), etc., to obtain good conductivity. For example, the conductive particles can be silver particles.
[0083] In some examples, the conductive metal particles in the conductive adhesive layer satisfy at least one of the following conditions: the conductive metal particles include at least two of the following: spherical or near-spherical particles, sheet-like particles, dendritic particles (e.g., tree-like), and fibrous particles; the particle size D50 of the conductive metal particles is 0.5 μm-50 μm; for example, the conductive metal particles satisfy both of the above conditions simultaneously. It should be noted that for particles with irregular shapes such as sheet-like particles, dendritic particles, and fibrous particles, the particle size can differ in different directions. The largest dimension among multiple dimensions along different directions can be used as the particle size. For example, the particle size of sheet-like particles can be the length dimension of the sheet-like particle.
[0084] By combining metal conductive particles with two or more different shapes, it is beneficial for the metal conductive particles to form a through conductive network in the polyurethane matrix, thereby improving the conductivity of the conductive adhesive layer and also improving the mechanical properties of the conductive adhesive layer.
[0085] The particle size D50 of the conductive metal particles is set to 0.5 μm-50 μm, and further to 5 μm-20 μm. This is because when the particle size D50 of the conductive metal particles is greater than or equal to 0.5 μm, and especially greater than or equal to 1 μm, their dispersibility in conductive coatings is better, they are more resistant to oxidation, and this is beneficial for improving storage stability. The conductive coating is the same coating used to prepare the conductive adhesive layer. Simultaneously, when the particle size D50 of the conductive metal particles is greater than or equal to 1 μm, the conductive metal particles are more likely to overlap and form conductive pathways, improving the conductivity and shielding efficiency of the conductive adhesive layer. Furthermore, it is desirable for the particle size D50 of the conductive metal particles to be less than or equal to 50 μm to reduce valve blockage problems caused by excessively large particle sizes during coating application, such as during dispensing.
[0086] For example, the conductive metal particles can include conductive metal particles with a particle size D50 of 5-20 μm and conductive metal particles with a particle size D50 of 1-5 μm. The combination of conductive metal particles with different particle sizes also helps the conductive adhesive layer to have both good Young's modulus and elongation at break.
[0087] For example, the conductive metal particles may include spherical or near-spherical particles and sheet-like particles, wherein the mass percentage of sheet-like particles in the conductive metal particles is greater than or equal to 50%, and the mass percentage of spherical or near-spherical particles in the conductive metal particles is less than or equal to 50%.
[0088] Plate-like particles possess a larger specific surface area and superior two-dimensional planar conductive pathways. By ensuring that the mass percentage of plate-like particles in the metallic conductive particles is greater than or equal to 50%, it is beneficial to form a wider and more continuous conductive network, thereby improving conductivity. In addition, plate-like particles can also act as a supporting "skeleton," enhancing the strength and other mechanical properties of the conductive adhesive layer.
[0089] An appropriate amount of spherical or near-spherical particles facilitates the flow and shaping of conductive coatings during processing, improving processing efficiency and film quality while reducing energy consumption and equipment wear. Considering the tendency for spherical or near-spherical particles to settle in conductive coatings, to improve the storage stability of the conductive coating, the mass percentage of spherical or near-spherical particles in the metallic conductive particles should be controlled to be less than or equal to 50%.
[0090] While a higher content of large-diameter flake particles improves the conductivity of the conductive adhesive layer, it also leads to an increase in the modulus and a decrease in the elongation at break. To balance the conductivity and toughness of the conductive adhesive layer, the mass percentage of metallic conductive particles in the layer is controlled to be greater than or equal to 70% and less than or equal to 90%. Furthermore, the D50 particle size of the flake particles is expected to be 1μm-20μm. This is because excessively large particle sizes result in a decrease in the elongation at break of the conductive adhesive layer, which is detrimental to its mechanical reliability.
[0091] Furthermore, the sheet-like particles can be composed of a first sheet-like particle and a second sheet-like particle, where the first sheet-like particle has a particle size D50 of 5μm-20μm and the second sheet-like particle has a particle size D50 of 1μm-5μm. This configuration allows the two particle sizes to work together to form a multi-level conductive network, improving conductivity and also contributing to a conductive adhesive layer with good Young's modulus and elongation at break.
[0092] The ratio of the first sheet particles to the second sheet particles can be selected according to actual needs. The content of the first sheet particles can be greater than that of the second sheet particles, or the content of the first sheet particles can be less than that of the second sheet particles. For example, increasing the proportion of the first sheet particles is beneficial to increasing the conductivity of the conductive adhesive layer and improving its mechanical properties, while increasing the proportion of the second sheet particles can refine the conductive network and improve the conductivity uniformity of the conductive adhesive layer.
[0093] Regarding the conductive adhesive layer mentioned above, an exemplary formulation of the conductive adhesive layer is as follows: the conductive adhesive layer comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of metal conductive particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of dispersant.
[0094] For example, the weight parts of polyurethane or modified polyurethane can include, but are not limited to, the following values or a range of values formed by any two points: 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc. Modified polyurethane refers to polyurethane that has been modified by a modifier. Within a suitable dosage range, polyurethane or modified polyurethane helps the conductive adhesive layer to possess both good Young's modulus and elongation at break, improving its application reliability.
[0095] The weight percentages of the conductive metal particles can include, but are not limited to, the following values or any range of two values: 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts, etc. Within a suitable dosage range, the conductive metal particles ensure that the conductive adhesive layer has good conductivity.
[0096] The weight parts of the coupling agent can be, but are not limited to, the following values or a range of values formed by any two points: 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.
[0097] The coupling agent can be a silane coupling agent. By adding a certain amount of coupling agent by weight, at least the following advantages can be achieved: improving the interfacial bonding force between the conductive adhesive layer and other interfaces, improving the dispersibility of metal conductive particles, and enhancing the water resistance and chemical resistance of the conductive adhesive layer.
[0098] For example, some suitable coupling agents can be silane coupling agents, such as γ-glycidoxypropyltrimethoxysilane (KAH560 for short).
[0099] Antioxidants are optional ingredients. The weight parts of antioxidants may include, but are not limited to, the following values or a range of values formed by any two points: 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, etc.
[0100] Antioxidants can prevent conductive adhesive layers from aging due to oxidation, such as discoloration, brittleness, chalking, and cracking, and can also improve the stability of conductive coatings. For example, antioxidants can be phenolic antioxidants, such as 2,6-di-tert-butyl-4-methylphenol (BHT), butylated hydroxyanisole (BHA), and tert-butylhydroquinone (TBHQ).
[0101] The dispersant is an optional component. The weight parts of the dispersant can be, but are not limited to, the following values or a range of values formed by any two points: 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.
[0102] Dispersants can promote the uniform dispersion of conductive metal particles in conductive adhesive layers and improve the conductivity uniformity of conductive adhesive layers in various regions. For example, dispersants can be oleic acid, citric acid, tributyl citrate, etc.
[0103] It should be noted that by adjusting the formulation of the conductive adhesive layer, various physical properties of the conductive adhesive layer, including the coefficient of thermal expansion, can be adjusted to ensure that these properties meet the aforementioned ranges. Furthermore, based on this conductive adhesive layer formulation, excellent adhesion is achieved between the conductive adhesive layer and the PCB solder mask, epoxy molding compound, and metal encapsulation layer, with an adhesion strength greater than 4B in the cross-cut adhesion test.
[0104] The above provides an exemplary description of the arrangement scheme for the conductive adhesive layer. For the arrangement scheme of the insulating adhesive layer, please refer to the following. In some examples, the insulating adhesive layer satisfies at least one of the following physical properties: the thickness of the insulating adhesive layer is 20μm-200μm, the Young's modulus of the insulating adhesive layer is greater than or equal to 200MPa, and the elongation at break of the insulating adhesive layer is greater than or equal to 5%.
[0105] The thickness of the insulating adhesive layer ranges from 20μm to 200μm, ensuring both reliable insulation and a relatively thin profile. The Young's modulus of the insulating adhesive layer is greater than or equal to 200MPa, ensuring it provides rigid support for the electromagnetic shielding encapsulation structure. This allows it to maintain good shape and dimensional stability under external forces, thus maintaining stable performance of electromagnetic shielding and electrical connections. The elongation at break of the insulating adhesive layer is greater than or equal to 5%. This not only allows the insulating adhesive layer to adapt to changes caused by vibration, impact, or thermal expansion and contraction in electronic equipment through its own tensile deformation, preventing easy breakage and improving the fatigue resistance and reliability of the electromagnetic shielding encapsulation structure, but also allows the conductive adhesive layer to relieve stress through its own deformation. This prevents cracking or debonding between the conductive adhesive layer and other materials due to thermal stress concentration, ensuring the integrity and stability of the electromagnetic shielding encapsulation structure under different temperature conditions.
[0106] The above-described performance arrangement applicable to the insulating adhesive layer allows the insulating adhesive layer to include: a polyurethane matrix and insulating filler particles dispersed in the polyurethane matrix, wherein the mass percentage of the insulating filler particles in the insulating adhesive layer is greater than or equal to 20% and less than or equal to 90%.
[0107] Using polyurethane as the matrix for the insulating adhesive layer, and making it the same matrix resin as the conductive adhesive layer, helps to improve the interfacial bonding force and prevent the insulating adhesive layer and the conductive adhesive layer from aging and cracking.
[0108] Insulating filler particles can not only improve the insulation performance of insulating adhesive layers, but also enhance the mechanical properties, heat resistance and chemical stability of insulating adhesive layers. The mass percentage of insulating filler particles in insulating adhesive layers is greater than or equal to 20% and less than or equal to 90%, including but not limited to the following point values or numerical ranges formed by any two point values: 20%, 30%, 40%, 50%, 60%, 70%, 75%, 80%, 85%, 90%, etc.
[0109] In some examples, the polyurethane matrix in the insulating adhesive layer contains 100% polyurethane resin by mass. In other examples, the polyurethane matrix in the insulating adhesive layer includes polyurethane and a modifier, which includes at least one of alkyd resin, acrylic resin, and epoxy resin. The modifier increases the adhesion between the insulating adhesive layer and other interfaces, while also increasing the waterproof capability of the conductive adhesive layer and improving the structural stability of the electromagnetic shielding encapsulation structure. Exemplarily, the mass percentage of the modifier in the polyurethane matrix can be 5%-50%, which can be any of the following values or a range of any two values: 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.
[0110] In this embodiment of the disclosure, the insulating filler particles satisfy at least one of the following conditions: the insulating filler particles include at least one of titanium dioxide particles, silicon dioxide particles, aluminum oxide particles, magnesium oxide particles, zinc oxide particles, aluminum nitride particles, boron nitride particles, silicon carbide particles, calcium sulfate particles, calcium carbonate particles, barium sulfate particles, barium titanate particles, sulfate particles, carbonate particles, and titanate particles, and the particle size D50 of the insulating filler particles is 0.1 μm-20 μm. For example, the insulating filler particles simultaneously satisfy both of the above conditions.
[0111] The insulating filler particles can be spherical or near-spherical, with a particle size D50 of 0.1 μm-20 μm. More specifically, it can be 0.5 μm-10 μm. This is because when the particle size D50 of the insulating filler particles is greater than or equal to 0.1 μm, especially greater than or equal to 0.5 μm, its dispersibility in the insulating coating is better, which is beneficial for improving storage stability. The insulating coating is the coating used to prepare the insulating adhesive layer. At the same time, a particle size D50 of less than or equal to 20 μm reduces the risk of valve blockage during coating application, such as during dispensing, caused by excessively large particle sizes.
[0112] Regarding the aforementioned insulating adhesive layer, an exemplary formulation of the insulating adhesive layer is as follows: the insulating adhesive layer comprises the following components in parts by weight: 10-50 parts of polyurethane or modified polyurethane adhesive, 20-90 parts of insulating filler particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of thixotropic agent.
[0113] For example, the weight parts of polyurethane or modified polyurethane can include, but are not limited to, the following values or any range of two values: 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, etc. Modified polyurethane refers to polyurethane that has been modified by a modifier.
[0114] The weight percentage of insulating filler particles can be, but is not limited to, the following values or a range of values consisting of any two points: 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, etc.
[0115] The weight parts of the coupling agent can be, but are not limited to, the following values or a range of values formed by any two points: 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.
[0116] The coupling agent can be a silane coupling agent. By adding a certain amount of coupling agent by weight, at least the following advantages are achieved: improving the interfacial bonding force between the insulating adhesive layer and other interfaces, improving the dispersibility of insulating filler particles, and enhancing the water resistance and chemical resistance of the insulating adhesive layer.
[0117] For example, some suitable coupling agents can be silane coupling agents, such as γ-glycidoxypropyltrimethoxysilane (KAH560 for short).
[0118] Antioxidants are optional ingredients. The weight parts of antioxidants may include, but are not limited to, the following values or a range of values formed by any two points: 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, etc.
[0119] Antioxidants can prevent the insulating adhesive layer from aging phenomena such as discoloration, brittleness, powdering, and cracking due to oxidation, and can also improve the stability of the insulating coating.
[0120] The weight parts of the thixotropic agent can be, but are not limited to, the following values or a range of values consisting of any two points: 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.
[0121] Thixotropic agents enable insulating coatings to rapidly decrease in viscosity when subjected to shear forces (such as those applied during brushing or spraying), making them easier to flow and apply, facilitating construction and ensuring uniform coverage of the object's surface. After application, the viscosity of the coating quickly returns to normal once the shear force disappears, preventing sagging and dripping, and maintaining a good appearance and uniform texture of the insulating layer. For example, some suitable thixotropic agents are polyamide waxes.
[0122] It should be noted that by adjusting the formulation of the insulating adhesive layer, various physical properties of the insulating adhesive layer, including the coefficient of thermal expansion, can be adjusted to ensure that these properties meet the aforementioned ranges. Furthermore, based on this formulation, excellent adhesion is achieved between the insulating adhesive layer and the PCB solder mask, optional epoxy molding compound, and optional metal encapsulation layer, with an adhesion strength greater than 4B in the cross-cut adhesion test.
[0123] On the other hand, this disclosure also provides a method for preparing an electromagnetic shielding encapsulation structure, which is as described in any of the above descriptions. The preparation method includes: mounting electronic devices on a circuit board, applying an insulating coating and curing it to form an insulating adhesive layer, applying a conductive coating and curing it to form a conductive adhesive layer, thereby preparing an electromagnetic shielding encapsulation structure.
[0124] The fabrication steps are adapted to the specific structure of the electromagnetic shielding package. For example, for an electromagnetic shielding package with an open metal shield, the fabrication method further includes mounting the open metal shield onto the circuit board. Additionally, the application positions of the insulating and conductive coatings are also adapted to the specific structure of the electromagnetic shielding package.
[0125] Some suitable insulating coatings include the following components in parts by weight: 10-50 parts polyurethane or modified polyurethane adhesive, 20-90 parts insulating filler particles, 0.1-5 parts coupling agent, 0-2 parts antioxidant, 0-5 parts thixotropic agent, and 10-60 parts solvent.
[0126] The conductive coating comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of conductive metal particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, 0-5 parts of dispersant, and 5-30 parts of solvent.
[0127] The formulations of conductive and insulating coatings can be found in the formulations of the conductive adhesive layer and insulating coating mentioned above, and will not be repeated here. Furthermore, the solvent can be an environmentally friendly solvent, such as isoparaffinic solvent oils (D30, D40, D50, D60, D70, D80, D90 solvent oils, etc.). After the conductive and insulating coatings are applied to form a liquid film, they undergo a curing process. The liquid film solidifies to form the corresponding adhesive layer, and the solvent evaporates during this process.
[0128] Insulating coatings can be applied to the corresponding positions by means of dispensing, spraying, etc., which has the advantages of simple operation, high reliability, easy control of adhesive layer thickness, and improved production efficiency and material utilization. After the insulating coating is applied, it is heated and cured, for example, heated to 100℃-130℃ and held for 10 minutes-20 minutes to cure it into an insulating adhesive layer. Then, conductive coatings are applied on it.
[0129] Conductive coatings can be applied to the corresponding positions by means of dispensing, spraying, etc., which has the advantages of simple operation, high reliability, easy control of adhesive layer thickness, and improved production efficiency and material utilization. After the conductive coating is applied, it is heated and cured, for example, heated to 100℃-130℃ and held for 10-20 minutes to cure it.
[0130] To make the coating suitable for coating scenarios with different shapes, such as to achieve sufficient and reliable coverage of uneven electronic components on circuit boards, the viscosity of both the insulating and conductive coatings needs to be controlled within a suitable range, and both need to have a certain degree of thixotropy to ensure that the edges of the components to be coated, such as the edges of electronic components, can be completely covered, and that the thickness of the adhesive layer is relatively uniform. In embodiments of this disclosure, the conductive coating satisfies at least one of the following physical properties: a viscosity of 5000 mPa·s-50000 mPa·s and a thixotropic index ≥1.3; and the insulating coating satisfies at least one of the following physical properties: a viscosity of 10000 mPa·s-50000 mPa·s or 4000 mPa·s-50000 mPa·s and a thixotropic index ≥1.2.
[0131] For example, conductive coatings simultaneously meet the following physical properties: viscosity of 5000 mPa·s-50000 mPa·s and thixotropic index ≥1.3; and insulating coatings simultaneously meet the following physical properties: viscosity of 10000 mPa·s-50000 mPa·s or 4000 mPa·s-50000 mPa·s and thixotropic index ≥1.2. This approach is more advantageous for the coatability and stackability of the coatings, thereby achieving stackable coatings, stable adhesive layer structure, and reliable interface sealing.
[0132] For the electromagnetic shielding encapsulation structure involved in implementation scheme (1), the viscosity of the insulating coating can be 10000 mPa·s-50000 mPa·s. For the electromagnetic shielding encapsulation structure involved in implementation scheme (2), the viscosity of the insulating coating can be 4000 mPa·s-50000 mPa·s. For different scenarios, to ensure that the insulating coating has stacking properties and acts as a dam, it prevents the conductive coating from overflowing and flowing to surrounding electronic devices, causing short circuits.
[0133] In this embodiment of the disclosure, the viscosity and thixotropic index of the insulating coating and the conductive coating are both measured using a rheometer at a test temperature of 25°C. The test rotor is a CP25 rotor with a measurement gap of 0.1 mm. The shear rate during the viscosity test is 1 / s, and the shear rates during the thixotropic index test are 1 / s and 10 / s. The thixotropic index is the ratio of the viscosity at a shear rate of 1 / s to the viscosity at a shear rate of 10 / s.
[0134] In another aspect, embodiments of this disclosure provide an electronic device, which includes a housing and an electromagnetic shielding encapsulation structure housed within the housing, the electromagnetic shielding encapsulation structure being as described above.
[0135] The electronic device provided in this disclosure has all the advantages of the electromagnetic shielding packaging structure mentioned above, and will not be repeated here.
[0136] For example, the electronic device may be a mobile phone, tablet, computer, watch, headphones, or smart wearable device (such as AR glasses, VR glasses, etc.).
[0137] Exemplary embodiments of this disclosure will now be described in more detail. While exemplary embodiments of this disclosure are described below, it should be understood that this disclosure can be implemented in various forms and should not be limited to the embodiments set forth herein. Where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with techniques or conditions described in the literature in the art or according to product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0138] The alkyd-modified polyurethane resins used in the following examples and comparative examples were prepared by the following method: Alkyd resin was prepared by reacting terephthalic acid, adipic acid, tall oil, and glycerol; the alkyd resin and polyurethane prepolymer were mixed and stirred in a mass ratio of 1:6 to obtain the alkyd-modified polyurethane resin. The polyurethane prepolymer (i.e., the unmodified polyurethane resin) was prepared by reacting toluene diisocyanate (TDI), polyether polyol, and polyethylene adipate.
[0139] Examples 1-6
[0140] Examples 1-6 each provide a conductive coating and the conductive adhesive layer prepared therefrom. The formulations of the conductive coatings are shown in Table 1. The content of each component in the conductive coating is calculated in parts by mass. Furthermore, the polyurethane matrix in Examples 1-4 and Example 6 is an alkyd-modified polyurethane resin, while the polyurethane matrix in Example 5 is an unmodified polyurethane resin. Comparative examples, designated Comparative Examples 1-2, are also provided. The polyurethane matrix in these examples is an alkyd-modified polyurethane resin, and the formulations of their conductive coatings are shown in Table 1.
[0141] The conductive coatings described above were prepared by the following method: Alkyd-modified polyurethane resin was dissolved in D60 solvent oil according to the conductive coating formulation, and stirred at room temperature until the alkyd-modified polyurethane resin was completely dissolved. Then, conductive metal particles, coupling agent KAH560, and antioxidant BHT were added, and the mixture was homogenized using a homogenizer, followed by further mixing using a three-roll mill to obtain the conductive coating.
[0142] The viscosity of the conductive coating was determined using a rheometer at a test temperature of 25℃. A CP25 rotor was used, with a measurement gap of 0.1 mm. The shear rate during the viscosity test was 1 / s. Simultaneously, the viscosity at a shear rate of 10 / s was also measured. Based on the ratio of the viscosity at a shear rate of 1 / s to that at a shear rate of 10 / s, the thixotropic index of the conductive coating was calculated. All test results are listed in Table 2.
[0143] The conductive coating is scraped onto the surface of the release film to form a liquid film. The liquid film is then heated at 120°C for 15 minutes to solidify. The release film is then peeled off to obtain a conductive adhesive layer with a thickness of 100µm.
[0144] The conductivity of the conductive adhesive layer was tested using a four-probe method. The test results are listed in Table 2. It is expected that the conductivity of the conductive adhesive layer will be ≥1.0E+5S / m. At this point, the conductive adhesive layer can be used as an electromagnetic shielding material and achieve the electromagnetic shielding effect.
[0145] The low-temperature and high-temperature thermal expansion coefficients of the conductive adhesive layer were tested using thermomechanical analysis. The test temperature range was -60℃ to 200℃, and the heating rate was set to 5℃ / min. The test results are listed in Table 2.
[0146] The Young's modulus and elongation at break of each conductive adhesive layer were tested, and the test results are listed in Table 2.
[0147] Table 1
[0148] Table 2
[0149] As can be seen from the above embodiments and comparative examples, flake-shaped silver particles have better conductivity than spherical silver particles. Furthermore, the conductivity is even better when the particle size of flake-shaped silver particles is larger. Therefore, the mass percentage of spherical silver particles in the conductive metal particles is controlled to be less than 20%. The higher the amount of silver particles added, the higher the conductivity. To ensure the conductivity of the conductive adhesive layer, the mass percentage of silver particles in the conductive adhesive layer is controlled to be greater than 50%.
[0150] The conductive adhesive layers involved in Examples 1-5 not only meet the electromagnetic shielding requirements in terms of conductivity, but also possess the desired Young's modulus and elongation at break. They can be applied to the electromagnetic shielding encapsulation structures provided in Scheme (1) and Scheme (2) of this disclosure, giving them a stable and reliable electromagnetic shielding effect. The conductive adhesive layer provided in Example 6 meets the electromagnetic shielding requirements in terms of conductivity. However, Example 6 uses a relatively large amount of sheet-like silver particles with a D50 of 20-50 micrometers. Although this increases the Young's modulus of the conductive adhesive layer, it degrades its elongation at break to some extent. Although it can still be applied to the electromagnetic shielding encapsulation structure, and the electromagnetic shielding effect is considerable in a short time, its durability is relatively weak.
[0151] In Comparative Example 1, the excessive content of polyurethane matrix resulted in a correspondingly low content of conductive metal particles, significantly degrading the conductivity of the conductive adhesive layer. In Comparative Example 2, the insufficient content of polyurethane matrix, while improving conductivity, resulted in extremely poor elongation at break, failing to achieve both the desired Young's modulus and elongation at break. This led to poor reliability of this type of conductive adhesive layer in electromagnetic shielding encapsulation structures.
[0152] Examples 7-11
[0153] Examples 7-11 provide an insulating coating and the insulating adhesive layer prepared therefrom. The formulation of the insulating coating is shown in Table 3. The content of each component in the insulating coating is calculated in parts by mass. In addition, the polyurethane matrix in Examples 7-10 is alkyd modified polyurethane resin, while the polyurethane matrix in Example 11 is unmodified polyurethane resin.
[0154] The above-mentioned insulating coatings were prepared by the following method: Alkyd-modified polyurethane resin was dissolved in D60 solvent oil according to the coating formulation, and stirred at room temperature until the resin was completely dissolved. Then, insulating filler particles, coupling agent KAH560, antioxidant BHT, and thixotropic agent polyamide wax were added, and the mixture was homogenized using a homogenizer, followed by further mixing using a three-roll mill to obtain the insulating coating. Comparative examples, designated Comparative Examples 3-4, were also provided, and their insulating coating formulations are shown in Table 3.
[0155] The viscosity of the insulating coating was determined using a rheometer at a test temperature of 25℃. A CP25 rotor was used, with a measurement gap of 0.1 mm. The shear rate during the viscosity test was 1 / s. Simultaneously, the viscosity at a shear rate of 10 / s was also measured. Based on the ratio of the viscosity at a shear rate of 1 / s to that at a shear rate of 10 / s, the thixotropic index of the insulating coating was calculated. All test results are listed in Table 4.
[0156] The insulating coating is scraped onto the surface of the release film to form a liquid film. The liquid film is then heated at 120°C for 15 minutes to solidify. The release film is then peeled off to obtain an insulating adhesive layer with a thickness of 100 μm.
[0157] The thermal expansion coefficients at low and high temperatures of the insulating adhesive layer were tested using thermomechanical analysis. The test temperature range was -60℃ to 200℃, and the heating rate was set to 5℃ / min. The test results are listed in Table 4.
[0158] The Young's modulus and elongation at break of each insulating layer were tested, and the test results are listed in Table 4.
[0159] Table 3
[0160] Table 4
[0161] It is evident that when the formulation of the insulating adhesive layer meets the requirements of the embodiments of this disclosure, the obtained insulating adhesive layer possesses both the desired thermal expansion characteristics and a high Young's modulus and elongation at break.
[0162] Application examples
[0163] The insulating and conductive adhesive layers involved in the above embodiments are combined and applied to randomly prepare electromagnetic shielding encapsulation structures as described in embodiment (1) of this disclosure (see Figure 1) and embodiment (2) (see Figure 3). The combination methods and thicknesses of the insulating coating and conductive adhesive layer are listed in Table 5.
[0164] The relevant performance of the electromagnetic shielding packaging structure was tested, and the test results are also listed in Table 5. The unit of electromagnetic shielding effectiveness is dB@1.5GHz. In addition, insulating adhesive layers were stacked on the surface of the circuit board, and corresponding conductive adhesive layers were stacked on the surface of the insulating adhesive layers to form test samples. Temperature shock aging tests were conducted on each test sample, and the test method is as follows: the test samples were subjected to -40℃ and +85℃ for 5 minutes each, with a maximum transition time between high and low temperatures of less than 20 seconds, for 500 cycles. Then, the insulating adhesive layer and conductive adhesive layer were observed under an optical microscope before and after aging to evaluate the environmental aging reliability of the prepared electromagnetic shielding packaging structure.
[0165] Table 5
[0166] As shown in Table 5, the higher the conductivity of the conductive adhesive layer, the higher its electromagnetic shielding efficiency. For the same conductive coating, the thicker the conductive adhesive layer, the higher the electromagnetic shielding efficiency.
[0167] When the CTE ratio of the insulating adhesive layer to the conductive adhesive layer is ≤3, the adhesive layer shows no microcracks after curing and temperature shock aging. Furthermore, the adhesion test results using the cross-cut adhesion method are both >4B before and after temperature shock aging, demonstrating excellent anti-aging performance. It is evident that the electromagnetic shielding encapsulation structure prepared based on the conductive and insulating adhesive layers provided in the above embodiments possesses both excellent electromagnetic shielding effect and mechanical properties, exhibiting operational reliability under different temperature environments.
[0168] The above description is only for the purpose of enabling those skilled in the art to understand the technical solutions disclosed herein, and is not intended to limit the scope of this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.
Claims
1. An electromagnetic shielded package structure, wherein, The electromagnetic shielding packaging structure includes a circuit board, electronic components, an insulating adhesive layer, and a conductive adhesive layer. The electronic device is fixed to the circuit board, and the insulating adhesive layer covers at least a portion of the outer wall of the electronic device; The conductive adhesive layer covers at least a portion of the surface of the insulating adhesive layer, and the conductive adhesive layer is also electrically connected to a grounding point provided on the circuit board; The ratio of the coefficients of thermal expansion of the insulating adhesive layer and the conductive adhesive layer at the same temperature is n, where 1 < n ≤ 4.
2. The electromagnetic shield package structure of claim 1, wherein, The low-temperature thermal expansion coefficient of the insulating adhesive layer is greater than 10ppm / ℃ and less than 200ppm / ℃, and the high-temperature thermal expansion coefficient of the insulating adhesive layer is greater than or equal to 200ppm / ℃ and less than 1000ppm / ℃. The low-temperature thermal expansion coefficient of the conductive adhesive layer is greater than or equal to 10ppm / ℃ and less than 100ppm / ℃, and the high-temperature thermal expansion coefficient is greater than or equal to 100ppm / ℃ and less than 500ppm / ℃. Wherein, the low-temperature thermal expansion coefficient is the thermal expansion coefficient of the adhesive layer under conditions below the glass transition temperature, and the high-temperature thermal expansion coefficient is the thermal expansion coefficient of the adhesive layer under conditions above the glass transition temperature.
3. The electromagnetic shielded package structure of any of claims 1-2, wherein, The electromagnetic shielding encapsulation structure also includes a metal shielding cover, which surrounds the outside of the electronic device and is electrically connected to the grounding point of the circuit board. The side of the metal shielding cover facing away from the circuit board has an opening, and the side of the electronic device facing away from the circuit board is located outside the opening or flush with the opening. The insulating adhesive layer covers at least a portion of the outer wall of the electronic device, and the insulating adhesive layer is at least partially located inside the metal shielding cover; The conductive adhesive layer is in contact with the insulating adhesive layer, and the conductive adhesive layer is also electrically connected to the metal shield.
4. The electromagnetic shield package structure of claim 3, wherein, The electronic device has a metal encapsulation layer on the side opposite to the circuit board. The metal encapsulation layer is at least partially located outside the opening. The insulating adhesive layer covers the outer wall of the electronic device without the metal encapsulation layer. The conductive adhesive layer is electrically connected to the metal shield and the metal encapsulation layer, respectively.
5. The electromagnetic shielded package structure of any of claims 1-2, wherein, The insulating adhesive layer covers all the outer walls of the electronic device that are not shielded by the circuit board and partially covers the circuit board, while the insulating adhesive layer avoids the grounding point of the circuit board; The conductive adhesive layer covers the surface of the insulating adhesive layer, and the conductive adhesive layer is electrically connected to the grounding point of the circuit board.
6. The electromagnetic shielded package structure of any of claims 1-5, wherein, The conductive adhesive layer satisfies at least one of the following physical properties: the thickness of the conductive adhesive layer is 30μm-150μm, the conductivity of the conductive adhesive layer is greater than 1E+5S / m, the Young's modulus of the conductive adhesive layer is greater than or equal to 30MPa, and the elongation at break of the conductive adhesive layer is greater than or equal to 2%.
7. The electromagnetic shield package structure of claim 6, wherein, The conductive adhesive layer comprises: a polyurethane matrix and metal conductive particles dispersed in the polyurethane matrix, wherein the mass percentage of the metal conductive particles in the conductive adhesive layer is greater than or equal to 70% and less than or equal to 90%.
8. The electromagnetic shield package structure of claim 7, wherein, The polyurethane matrix comprises polyurethane and a modifier, wherein the modifier comprises at least one of alkyd resin, acrylic resin, and epoxy resin.
9. The electromagnetic shield package structure of claim 7, wherein, The conductive metal particles satisfy at least one of the following conditions: the conductive metal particles include at least two of the following: spherical or near-spherical particles, sheet-like particles, dendritic particles, and fibrous particles; and the particle size D50 of the conductive metal particles is 0.5 μm to 50 μm.
10. The electromagnetic shield package structure of claim 9, wherein, The conductive metal particles include spherical or near-spherical particles and sheet-like particles, wherein the mass percentage of the sheet-like particles in the conductive metal particles is greater than or equal to 50%, and the mass percentage of the spherical or near-spherical particles in the conductive metal particles is less than or equal to 50%.
11. The electromagnetic shield package structure of claim 10, wherein, The sheet-like particles include a first sheet-like particle and a second sheet-like particle, wherein the particle size D50 of the first sheet-like particle is 5μm-20μm and the particle size D50 of the second sheet-like particle is 1μm-5μm.
12. The electromagnetic shielded encapsulation structure according to any one of claims 7-11, wherein, The conductive adhesive layer comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of conductive metal particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of dispersant.
13. The electromagnetic shielded encapsulation structure according to any one of claims 1-12, wherein, The insulating adhesive layer satisfies at least one of the following physical properties: the thickness of the insulating adhesive layer is 20μm-200μm, the Young's modulus of the insulating adhesive layer is greater than or equal to 200MPa, and the elongation at break of the insulating adhesive layer is greater than or equal to 5%.
14. The electromagnetic shield package structure of claim 13, wherein, The insulating adhesive layer comprises: a polyurethane matrix and insulating filler particles dispersed in the polyurethane matrix, wherein the mass percentage of the insulating filler particles in the insulating adhesive layer is greater than or equal to 20% and less than or equal to 90%.
15. The electromagnetic shield package structure of claim 14, wherein, The insulating filler particles satisfy at least one of the following conditions: the insulating filler particles include at least one of titanium dioxide particles, silicon dioxide particles, aluminum oxide particles, magnesium oxide particles, zinc oxide particles, aluminum nitride particles, boron nitride particles, silicon carbide particles, calcium sulfate particles, calcium carbonate particles, barium sulfate particles, barium titanate particles, sulfate particles, carbonate particles, and titanate particles. The particle size D50 of the insulating filler particles is 0.1μm-20μm.
16. The electromagnetic shielded encapsulation structure according to any of claims 14-15, wherein, The insulating adhesive layer comprises the following components in parts by weight: 10-50 parts of polyurethane or modified polyurethane adhesive, 20-90 parts of insulating filler particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, and 0-5 parts of thixotropic agent.
17. A method of producing an electromagnetic shielded package structure, wherein, The electromagnetic shielding encapsulation structure is as described in any one of claims 1-16, and the preparation method includes: Electronic components are mounted on a circuit board, an insulating coating is applied and cured to form an insulating adhesive layer, and a conductive coating is applied and cured to form a conductive adhesive layer, thus preparing the electromagnetic shielding encapsulation structure.
18. The method of making according to claim 17, wherein, The insulating coating comprises the following components in parts by weight: 10-50 parts of polyurethane or modified polyurethane adhesive, 20-90 parts of insulating filler particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, 0-5 parts of thixotropic agent, and 10-60 parts of solvent. The conductive coating comprises the following components in parts by weight: 10-20 parts of polyurethane or modified polyurethane, 50-95 parts of conductive metal particles, 0.1-5 parts of coupling agent, 0-2 parts of antioxidant, 0-5 parts of dispersant, and 5-30 parts of solvent.
19. The method of making according to claim 17, wherein, The conductive coating satisfies at least one of the following physical properties: viscosity of 5000 mPa·s-50000 mPa·s, and thixotropic index ≥1.3; The insulating coating satisfies at least one of the following physical properties: viscosity of 10000mPa·s-50000mPa·s or 4000mPa·s-50000mPa·s, and thixotropic index ≥1.
2.
20. An electronic device, comprising: The electronic device includes a housing and an electromagnetic shielding encapsulation structure housed within the housing, the electromagnetic shielding encapsulation structure being as described in any one of claims 1-16.