Copper powder and preparation method therefor, conductive copper paste, and use
By coating the surface of copper particles with a copper oxide layer and an organic coating layer, the storage stability and conductivity issues of copper conductive paste in solar cells were solved, achieving high conductivity and stability.
Patent Information
- Application Number
- PCT/CN2026/093649
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-04-22
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-19
AI Technical Summary
Existing conductive silver pastes are expensive, and copper conductive pastes have a short shelf life at room temperature, resulting in a gradual deterioration in conductivity, making them difficult to widely apply to solar cells.
By sequentially coating the surface of copper particles with a copper oxide layer and an organic coating layer, the interaction between copper ions in the copper oxide layer and nitrogen or sulfur in the organic coating layer is utilized to improve the bonding strength, forming copper powder and preparing conductive copper paste.
It enhances the conductivity, hygrothermal stability, and light stability of copper powder, reduces contact resistance, and improves the overall performance of copper electrodes.
Smart Images

Figure CN2026093649_19112026_PF_FP_ABST
Abstract
Description
Copper powder and its preparation methods, conductive copper paste and its applications
[0001] This application claims priority to Chinese invention patent applications filed on May 16, 2025, with application number 202510637341.8 and entitled "Copper Powder and Preparation Method Thereof, Conductive Copper Paste and Its Application", and filed on April 22, 2026, with application number 202610542353.7 and entitled "Copper Powder and Preparation Method Thereof, Conductive Copper Paste and Its Application". Technical Field
[0002] This application relates to the field of conductive materials technology. Specifically, this application relates to a copper powder and its preparation method, a conductive copper paste and its application. More specifically, this application relates to a copper powder and its preparation method, a conductive copper paste, a copper electrode and a solar cell. Background Technology
[0003] As problems such as energy shortages, environmental pollution, and climate change caused by non-renewable energy sources become increasingly serious, people are paying more attention to the use of renewable energy. Solar energy is one of the important renewable energy sources, characterized by being pollution-free, renewable, and having huge reserves.
[0004] Photovoltaic power generation is an environmentally friendly renewable energy technology that converts light energy into electrical energy through solar cells. Conductive silver paste is widely used in solar cells to collect and transport photogenerated carriers. However, as the cost of metallic silver continues to rise, attempts are being made to use other metals to replace it. Copper, as a base metal with conductivity comparable to silver, has a lower cost; however, copper itself is highly reactive, and conductive copper paste has a short storage time at room temperature, causing its conductivity to gradually deteriorate, making it difficult to widely promote and apply. Summary of the Invention
[0005] In view of this, in order to at least partially solve the aforementioned technical problems, this application provides a copper powder and its preparation method, a conductive copper paste and its application.
[0006] According to one embodiment of this application, a copper powder is provided, comprising: copper particles, a copper oxide layer at least partially coating the outer side of the copper particles, and an organic coating layer coating the outer side of the copper oxide layer; the organic coating layer contains nitrogen or sulfur, wherein the mass content of nitrogen is 50 to 800 ppm based on the total mass of the copper powder, or the mass content of sulfur is 30 to 1000 ppm.
[0007] According to another embodiment of this application, a method for preparing the above-mentioned copper powder is provided, comprising: acid washing copper particles to obtain acid-washed copper particles; mixing the acid-washed copper particles with an organic coating agent solution in air to sequentially coat the surface of the copper particles with a copper oxide layer and an organic coating layer to obtain the above-mentioned copper powder; wherein the organic coating agent has nitrogen-containing groups or sulfur-containing groups.
[0008] According to another embodiment of this application, a conductive copper paste is provided, comprising copper powder and a dispersion medium, wherein the copper powder is as described above, and preferably, the conductive copper paste comprises 80-92% copper powder and 8-20% dispersion medium by weight.
[0009] According to another embodiment of this application, a copper electrode is provided, which is formed from the above-described conductive copper paste.
[0010] According to another embodiment of this application, a solar cell is provided, comprising a copper electrode as described above.
[0011] According to embodiments of this application, the copper oxide layer serves as a connector to the organic coating layer, depending on the copper ions (Cu) in the copper oxide layer. 2+ and / or Cu + The interaction between the organic coating and nitrogen or sulfur in the organic coating, such as complexation, significantly improves the bonding strength between the organic coating and copper particles, reducing the likelihood of organic coating detachment, ensuring the overall thermal and photodynamic stability of the copper powder material structure, and reducing and stabilizing the contact resistance of the copper electrode on the solar cell. Furthermore, by adjusting the nitrogen or sulfur content in the organic coating to a suitable range, and through the binding effect of the copper oxide layer, the organic coating is applied to the surface of the copper particles in an appropriate amount, enabling the copper powder to exhibit high conductivity and stable contact resistance. Attached Figure Description
[0012] The above and other objects, features and advantages of this application will become clearer from the following description of embodiments with reference to the accompanying drawings, in which:
[0013] Figure 1 shows a schematic diagram of the structure of copper powder according to an embodiment of this application;
[0014] Figure 2 shows a flowchart of a method for preparing copper powder according to an embodiment of this application;
[0015] Figure 3 shows a transmission electron microscope image of copper powder from Example 1 of this application, where (a) is copper particles, and (b) and (c) are copper oxides.
[0016] Figure 4 shows a partial magnified view and elemental analysis diagram of the copper powder in Figure 3. Specifically, 4-1 shows a partial magnified view and elemental analysis diagram of (a) of the copper powder in Figure 3; 4-2 shows a partial magnified view and elemental analysis diagram of (b) of the copper powder in Figure 3; and 4-3 shows a partial magnified view and elemental analysis diagram of (c) of the copper powder in Figure 3.
[0017] In the accompanying drawings, the reference numerals have the following specific meanings: 1-copper powder; 11-copper particles; 12-copper oxide layer; 13-organic coating layer. Detailed Implementation
[0018] The embodiments of this application will now be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of this application. In the following detailed description, numerous specific details are set forth to provide a thorough understanding of the embodiments of this application for ease of explanation. However, it will be apparent that one or more embodiments may be implemented without these specific details. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of this application.
[0019] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. The term "comprising" as used herein indicates the presence of features, steps, or operations, but does not exclude the presence or addition of one or more other features.
[0020] When using expressions such as "at least one of A, B, and C," the expression should generally be interpreted in accordance with the meaning commonly understood by a person skilled in the art (e.g., "a system having at least one of A, B, and C" should include, but is not limited to, systems having A alone, having B alone, having C alone, having A and B, having A and C, having B and C, and / or having A, B, and C, etc.). Similarly, when using expressions such as "at least one of A, B, or C," the expression should generally be interpreted in accordance with the meaning commonly understood by a person skilled in the art (e.g., "a system having at least one of A, B, or C" should include, but is not limited to, systems having A alone, having B alone, having C alone, having A and B, having A and C, having B and C, and / or having A, B, and C, etc.).
[0021] In cases where numerical ranges are provided, such as concentration ranges, percentage ranges, or ratio ranges, it should be understood that, unless the context explicitly specifies otherwise, all intermediate values between the upper and lower limits of the range, up to one-tenth of the lower limit unit, and any other values or intermediate values within the range are included in the subject matter. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges, and such embodiments are also included in the subject matter, limited by any specific excluded limit values within the range. Where the range includes one or two limit values, the range excluding any one or both of those included limit values is also included in the subject matter.
[0022] In the context of this invention, unless otherwise expressly stated or the context in which the reference is made explicitly implies the contrary, the indefinite articles (“a”, “an”) and definite articles (“the”) in the singular form include the plural form.
[0023] Solar cells are widely used due to their mature technology and high photoelectric conversion efficiency. Currently, the electrodes in solar cells are typically made using conductive silver paste. However, the high cost of silver contributes to the overall high cost of solar cells. Therefore, it is necessary to find a way to reduce the cost of solar cells while maintaining high conductivity.
[0024] In realizing the concept of this application, it was discovered that when copper particles are sequentially coated with a copper oxide layer and an organic coating layer, the organic coating layer can be coated on the surface of copper particles in an appropriate amount through the binding effect of the copper oxide layer, thereby improving the conductivity, hygrothermal stability and light stability of the copper powder, and thus improving the conductivity of the copper electrode, and reducing and stabilizing the contact resistance of the copper electrode.
[0025] Specifically, according to one aspect of the present application, a copper powder is provided. FIG1 shows a schematic diagram of the structure of the copper powder according to an embodiment of the present application. As shown in FIG1, the copper powder 1 includes: copper particles 11, a copper oxide layer 12 at least partially covering the outside of the copper particles 11, and an organic coating layer 13 covering the outside of the copper oxide layer 12.
[0026] According to the embodiments of this application, without being bound by theory, a copper oxide layer 12 is formed in situ on at least a portion of the surface of the copper particles 11. By means of the strong interaction between the copper ions in the copper oxide layer 12 and the nitrogen or sulfur in the organic coating layer 13, such as complexation, active sites are provided, and the interfacial bonding force between the copper oxide layer 12 and the organic coating layer 13 is improved. Thus, the organic coating layer 13 is tightly connected to the copper particles 11 through the copper oxide layer 12. The stable organic coating layer 13 is used to improve the overall conductivity, hygrothermal stability and light stability of the copper powder.
[0027] It should be noted that copper particles 11 refer to particles whose main component is zero-valent copper.
[0028] In this embodiment, the term "at least partially" can be understood as meaning that the copper oxide layer 12 can completely cover the copper particles 11, such that the organic coating layer 13 is entirely connected to the copper particles 11 through the copper oxide layer 12; or that the copper oxide layer 12 partially covers the copper particles 11, such that part of the organic coating layer 13 is connected to the copper particles 11 through the copper oxide layer 12, and the other part of the organic coating layer 13 is directly connected to the copper particles 11. Regardless of the coverage ratio of the copper oxide layer 12, from the perspective of suppressing the oxidation of the copper particles 11, the organic coating layer 13 needs to have a coverage rate of more than 98% on the outermost surface relative to the surface area of the outermost surface of the copper particles 11, which can be determined by transmission electron microscopy.
[0029] It is understood that this application does not require all copper particles 11 in copper powder 1 to be coated with a copper oxide layer 12; partial coating with a copper oxide layer 12 is sufficient to enhance the bonding between the organic coating layer 13 and the copper particles 11. In actual testing, several copper powders 1 can be randomly selected and examined using an electron microscope to determine whether they are coated with a copper oxide layer 12.
[0030] Because copper particles 11 and copper oxide layer 12 have different crystal states, interplanar spacings, and positional distributions, they can be distinguished by an electron microscope.
[0031] Furthermore, the organic coating layer 13 contains nitrogen or sulfur. Based on the total mass of the copper powder 1, the nitrogen content is 50-800 ppm, or the sulfur content is 30-1000 ppm. This configuration ensures that the organic coating layer 13 coats the surface of the copper particles 11 in a suitable amount and with strong adhesion, providing a better passivation effect, improving oxidation resistance, extending storage time, improving hygrothermal stability and light stability, while also improving the electrical conductivity of the copper particles 11. If there is too much nitrogen or sulfur, the amount of organic coating layer 13 formed will be excessive, resulting in an overly thick organic coating layer 13. This reduces the conductivity of the copper powder 1 and the storage stability of the conductive paste prepared from the copper powder 1, and also reduces the printability of the conductive paste. If there is too little nitrogen or sulfur, the amount of organic coating layer 13 formed will be insufficient, resulting in an overly thin organic coating layer 13. This reduces the insulating effect on the surface of the copper powder 1, causing the copper particles 11 to be exposed to oxygen in the air and oxidized, thus degrading the conductivity. Furthermore, insufficient nitrogen or sulfur content will also reduce the number of adhesion sites of the organic coating layer 13 on the copper oxide layer 12 and / or the copper particles 1, reducing the adhesion of the organic coating layer 13 on the copper oxide layer 12 and / or the copper particles 1.
[0032] It should be noted that the above-mentioned nitrogen or sulfur content data can be obtained by elemental analysis. Specifically, to measure the nitrogen content: weigh a certain amount of copper powder 1, place it in a fluxing nickel foil, wrap it, and then place it in an oxygen-nitrogen analyzer, such as an ONH5500 analyzer, for elemental analysis. The mass content of nitrogen is obtained based on the total mass of the measured copper powder. To measure the sulfur content: weigh a certain amount of copper powder 1, place it in a fluxing nickel foil, wrap it, and then place it in a carbon-sulfur analyzer, such as a CS3500 analyzer, for elemental analysis. The mass content of sulfur is obtained based on the total mass of the measured copper powder.
[0033] The organic coating layer 13 contains nitrogen or sulfur, which can be understood as having nitrogen-containing groups or sulfur-containing groups in the organic coating layer 13.
[0034] For example, based on the total mass of copper powder, the mass content of nitrogen element can be, for example, 50ppm, 55ppm, 100ppm, 150ppm, 198ppm, 200ppm, 250ppm, 300ppm, 311ppm, 350ppm, 400ppm, 450ppm, 500ppm, 550ppm, 600ppm, 650ppm, 700ppm, 750ppm, 780ppm or 800ppm, or a range consisting of any two of the above values. Based on the total mass of copper powder, the mass content of sulfur can be, for example, 30ppm, 40ppm, 50ppm, 100ppm, 150ppm, 200ppm, 245ppm, 250ppm, 300ppm, 350ppm, 400ppm, 450ppm, 500ppm, 537ppm, 550ppm, 600ppm, 650ppm, 700ppm, 750ppm, 800ppm, 850ppm, 900ppm, 950ppm, or 1000ppm, or a range consisting of any two of the above values.
[0035] It should be noted that ppm represents one part per million. A nitrogen content of 50 ppm means that in every million parts of copper powder 1, the mass of nitrogen is 50 parts.
[0036] In some embodiments, the organic coating layer 13 is amorphous and can be detected by an electron microscope. Of course, it is not limited to electron microscopy. Other methods known in the art can also be used to distinguish it, or a combination of multiple detection and testing methods can be used to distinguish it, such as X-ray photoelectron spectroscopy (XPS), infrared spectroscopy, X-ray emission spectroscopy (XES), etc.
[0037] In some embodiments, the nitrogen content is 100–600 ppm, or the sulfur content is 200–600 ppm. This configuration helps improve the oxidation and corrosion resistance of the copper powder 1 through the interaction between nitrogen or sulfur and copper ions in the copper oxide layer 12. It also results in a more uniform surface organic coating layer 13 with less adverse effects, further improving the overall conductivity, hygrothermal stability, and light stability of the copper powder 1. Too low a nitrogen and sulfur content will lead to uneven coating of copper particles in the copper powder 1, while too high a nitrogen and sulfur content will result in a thicker organic coating layer after the copper powder 1 is prepared into a copper slurry, affecting the viscosity and dispersibility of the slurry during storage and use, and consequently, its stability.
[0038] In some embodiments, the thickness of the organic coating layer 13 is 2–15 nm. If the thickness is too thin, it is difficult to achieve a uniform and continuous coverage of the copper particles 11 by the organic coating layer 13, potentially leading to missing organic coating layers on the surface. This makes the copper powder 1 more susceptible to oxidation, reducing the stability of the subsequently prepared electrode. If the thickness of the organic coating layer 13 is too thick, the passivation degree of the copper powder is too high, resulting in high resistance and reduced conductivity when used as an electrode. Furthermore, during the preparation of the conductive paste, some of the organic coating agent in the organic coating layer 13 on the copper powder surface dissolves into the paste. Excessive organic coating layer thickness affects the viscosity of the paste, reducing its printability. Setting the thickness of the organic coating layer 13 within the aforementioned range ensures both uniform and continuous coverage and a tight bond between the copper oxide layer 12 and the copper particles 11. This allows for a thinner organic coating layer 13 while maintaining high conductivity and stability when used as a copper electrode.
[0039] It is understandable that the thickness of the organic coating layer 13 can be obtained by image analysis and measurement using transmission electron microscopy.
[0040] For example, the thickness of the organic coating layer 13 can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm or 15nm, or a range consisting of any two of the above values.
[0041] Optionally, the thickness of the organic coating layer 13 is 5–10 nm. This setting allows for a better passivation effect while further reducing the thickness of the organic coating layer 13, resulting in higher conductivity of the copper powder 1 when it is subsequently used as a conductive copper paste.
[0042] In some embodiments, the copper oxide layer 12 comprises copper oxide and / or cuprous oxide. The presence of the copper oxide layer 12 forms a dense protective layer on the surface of the copper particles 11, preventing direct contact between the copper particles 11 and external oxygen, moisture, and corrosive media, further inhibiting the oxidation or corrosion of the copper powder 1. The surface of the copper oxide layer 12 is rich in hydroxyl groups and unsaturated copper active sites, which can chemically bond with nitrogen-containing or sulfur-containing groups in the organic coating layer 13. For example, sulfur atoms form strong coordination bonds with copper ions; nitrogen-containing groups, such as amino groups, are connected to the hydroxyl groups on the surface of the copper oxide layer 12 via hydrogen bonds or covalent bonds.
[0043] Furthermore, the surface of the copper oxide layer 12 is a rough surface with micro-nano morphology formed by the oxidation of copper in a weak oxidizing environment, which helps to increase the physical adhesion of the organic coating layer 13, further enhance the adhesion effect of the organic coating layer 13, and reduce peeling.
[0044] It is understood that the copper oxide layer 12 can be composed of a single copper oxide, a single cuprous oxide, or a mixture of both. The combination of these two materials complements each other to form a protective layer with wider environmental adaptability, further enhancing stability and durability under complex operating conditions.
[0045] In some embodiments, the copper oxide layer 12 may be crystalline or amorphous (e.g., an amorphous structure refers to a structure that does not show a crystal lattice in transmission electron microscopy (TEM) analysis). In some embodiments, the copper oxide layer 12 is copper oxide, which is a monoclinic crystal phase with a (111) crystal plane orientation. And / or, the copper oxide layer 12 is cuprous oxide, which is a cubic crystal phase with a (111) crystal plane orientation. Its (111) crystal plane has a high surface energy and is rich in unsaturated copper atoms, which helps to interact with nitrogen-containing or sulfur-containing groups in the organic coating layer 13, thereby strengthening the tight connection between the organic coating layer 13 and the copper particles 11.
[0046] In some embodiments, the thickness of the copper oxide layer 12 is 2–8 nm. This configuration helps to form a dense covering layer on at least a portion of the surface of the copper particles 11, effectively isolating the copper particles 11 from direct contact with oxygen, moisture, and corrosive media, thus enhancing the antioxidant effect. The surface of the copper oxide layer 12 of the aforementioned thickness has abundant hydroxyl groups and metal active sites, which helps to form chemical bonds with the nitrogen-containing or sulfur-containing groups of the organic coating layer 13, further strengthening the interfacial bonding strength between the organic coating layer 13 and the copper particles 11. If the thickness of the copper oxide layer 12 is too thin, it is difficult to form a continuous oxide layer, resulting in limited improvement in the antioxidant capacity of the copper particles 11; if the thickness of the copper oxide layer 12 is too thick, stress mismatch may occur, leading to cracking, which limits the antioxidant effect and hinders electron conduction between the copper particles 11.
[0047] The thickness of the copper oxide layer 12 can be obtained by image analysis using transmission electron microscopy.
[0048] For example, the thickness of the copper oxide layer 12 can be 2nm, 3nm, 4nm, 5nm, 6nm, 7nm or 8nm, or a range consisting of any two of the above values.
[0049] Optionally, the thickness of the copper oxide layer 12 can be 2-3 nm. This configuration allows for good oxidation resistance while forming an ultrathin copper oxide layer 12, and also enables it to connect with the organic coating layer 13, fixing the organic coating layer 13 through chemical bonding, without significantly affecting the conductivity of the copper powder 1.
[0050] In some embodiments, the organic coating layer 13 includes at least one of organic amine compounds and thiol compounds. This configuration, using such compounds as organic coating agents, helps to isolate the copper particles 11 from external oxygen and moisture, thereby inhibiting oxidation reactions and improving the stability of the copper powder 1 in humid and hot environments. The organic coating agent in the organic coating layer 13 forms a dense molecular layer through chemisorption, reducing the resistivity of the conductive pathway.
[0051] It should be noted that the organic amine and thiol compounds used here can be long-chain organic coating agents. The steric hindrance effect of long carbon chains helps reduce the agglomeration of copper particles 11, maintaining good rheological properties during subsequent copper paste preparation. Simultaneously, long-chain organic coating agents can withstand the effects of high-temperature sintering during subsequent processing, avoiding performance degradation caused by thermal decomposition. The amine groups in the organic amine compounds form a chemisorbed organic coating layer 13 with the surface of copper particles 11 and / or copper oxide layer 12 through coordination bonds, significantly increasing the bonding strength between the organic coating layer 13 and the copper particles 11. The thiol groups in the thiol compounds form covalent bonds with the surface of copper particles 11 and / or copper oxide layer 12, and the empty orbitals of sulfur atoms undergo charge transfer with the d electrons of copper, which helps to inhibit chemical corrosion and optimize electrochemical performance.
[0052] Optionally, the organic coating layer 13 includes C6 to C6. 22 Aliphatic amine compounds, C6-C 22 At least one of aliphatic thiols. Long carbon chain, C6–C6. 22 Aliphatic amine compounds self-assemble into molecular membranes via van der Waals forces, further blocking water molecule permeation. With this configuration, C6–C6… 22 Aliphatic amine compounds help to further enhance the adhesion between the organic coating layer 13 and the copper particles 11, C6~C 22 Aliphatic thiol compounds were used to further optimize electrochemical performance.
[0053] Further optionally, C6~C 22 The aliphatic amine compound is selected from at least one of n-octylamine, n-hexylamine, dodecylamine, tetradecylamine, hexadecylamine, stearylamine, oleylamine, and tetrahydroxyethylethylenediamine, wherein C6-C6 are present in the aliphatic amine. 12 Short-chain amines, such as n-hexylamine and n-octylamine, have lower molecular weights and suitable high-temperature volatility, making them more suitable for low-temperature slurry curing processes. Among them, C... 14 ~C 22 Long-chain amines, such as hexadecylamine and stearylamine, have longer carbon chains, which help to provide stronger steric hindrance and inhibit the sintering and agglomeration of composite copper particles. (C6~C) 22 The aliphatic thiol compound is selected from at least one of hexathiol, octylthiol, dodecylthiol, and octadecylthiol. Among them, short-chain thiols such as hexathiol or octylthiol have a faster molecular diffusion rate, which can achieve the formation of the organic coating layer 13 in a shorter time and improve the passivation efficiency. Among them, long-chain thiols such as octadecylthiol form an organic coating layer 13 with a thicker thickness and higher wear resistance, which helps to provide effective passivation protection for copper particles 11.
[0054] It is understood that the organic coating layer 13 can be a single-layer membrane structure of the above-mentioned materials, or a multilayer membrane structure of different above-mentioned materials, without any particular limitation.
[0055] In some embodiments, the copper particles 11 are flake-shaped copper particles or spherical copper particles.
[0056] Flaky copper particles can be understood as having a two-dimensional planar structure, exhibiting a two-dimensional planar extension morphology. Flaky copper particles have a relatively small thickness and a large aspect ratio, which can be understood as the ratio between the shortest diameter and the thickness along the two-dimensional planar extension direction. Specifically, flaky copper particles can be understood as copper particles with an aspect ratio greater than or equal to 2. Because flaky copper particles form a relatively flat surface and achieve surface-to-surface contact, their effective contact area is high, significantly reducing contact resistance. Furthermore, the organic coating layer 13 provides a relatively continuous and uniform coverage, resulting in good oxidation resistance. Spherical copper particles, compared to flaky copper particles, have better fluidity and are more densely packed, contributing to higher mechanical stability during subsequent copper electrode formation. Specifically, spherical copper particles can be understood as copper particles with an aspect ratio less than 2. During the preparation of copper powder 1 or during the subsequent mixing to form copper slurry, flake copper particles and spherical copper particles can be compounded as needed. The spherical copper particles provide a supporting framework, while the flake copper particles dispersed between the spherical copper particles construct a lower resistance path. The compounding ratio of the two can be adjusted according to actual needs, and this application does not impose any special limitations on this.
[0057] It is understandable that when copper particles 11 are flake-shaped copper particles, the D of copper powder 1... 50 Particle size can be understood as the cumulative particle size by volume, which is the median particle size (D) in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measuring device for copper powder 1. 50 ) as the cumulative particle size. Similarly, when the copper particles 11 are spherical copper particles, the D of the copper powder 1 50 Particle size can be understood as the cumulative particle size by volume, which is the median particle size (D) in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measuring device for copper powder 1. 50 ) is used as the cumulative particle size.
[0058] It should be noted that copper powder 1 was mixed into ethanol and dispersed by ultrasonic irradiation, and the resulting product was used as the test sample.
[0059] Considering the need for better oxidation resistance and good adhesion to the substrate during subsequent preparation of conductive metal pastes, when copper particles 11 are flake-shaped copper particles, the D of the copper powder is... 50The particle size is 1–10 μm, for example, it can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, or 10 μm, or a range consisting of any two of these values; when the copper particles 11 are spherical copper particles, the D of the copper powder 50 The particle size is 0.1 to 1 μm, for example, it can be 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm or 1 μm, or a range consisting of any two of these values.
[0060] Optionally, when the copper particles 11 are spherical copper particles, the D of the copper powder... 50 The particle size is 100–800 nm, for example, it can be 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, or 800 nm, or a range consisting of any two of these values. This setting further maintains the good stability and low resistivity of the copper powder.
[0061] In some implementations, the median thickness of the sheet copper particles is 100 to 500 nm. The median thickness can be understood as the midpoint of the distribution of sheet copper particles in the thickness dimension. For example, a median thickness of 100 nm means that 50% of the sheet copper particles have a thickness of less than or equal to 100 nm, and 50% of the sheet copper particles have a thickness greater than 100 nm.
[0062] The median thickness can be measured using SEM (scanning electron microscopy image analysis). For example, take pictures of 10 different areas of the test sample, then measure the size of 10 sheet-like copper particles observed in each picture along the vertical plane, and then calculate the median value, which is the median thickness.
[0063] The median thickness of the sheet-like copper particles is 100–500 nm, for example, it can be 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 220 nm, 250 nm, 280 nm, 300 nm, 320 nm, 350 nm, 380 nm, 400 nm, 420 nm, 450 nm, 480 nm, or 500 nm, or a range consisting of any two of these values. This setting makes it easier to form a surface-to-surface contact network structure during the formation of copper particles 11, thereby reducing contact resistance. If the median thickness is too high, the aspect ratio (the ratio between diameter and thickness) of the sheet-like copper particles decreases, resulting in a reduced contact area and increased resistivity; if the median thickness is too low, the mechanical strength of the sheet-like copper particles decreases, making them prone to breakage during processing and impairing the continuity of the conductive path.
[0064] Optionally, the ratio of the longest diameter to the shortest diameter of the sheet-like copper particles along the two-dimensional plane extension direction is 1 to 10, for example, it can be 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10.
[0065] In some embodiments, when the copper particles 11 are flake-shaped copper particles, the specific surface area of the copper powder 1 is 0.1–0.9 m². 2 / g, when copper particles 11 are spherical copper particles, the specific surface area of copper powder 1 is 0.8~9m². 2 / g. Specific surface area can be understood as the surface area per unit mass of copper powder 1, and can be measured by conventional methods, such as the determination of specific surface area of metal powders according to GB / T 13390-2008. This setting allows the flake-shaped and / or spherical copper particles to have good oxidation resistance. If the specific surface area is too large, the surface activity of copper particles 11 is higher, making them easier to oxidize; if the specific surface area is too small, the particle size of copper particles 11 is larger, affecting the low-temperature sintering performance of the copper conductive paste prepared by copper particles 11, resulting in difficulty in fully sintering at low temperatures, or poor contact between the copper particles 11 and the substrate after sintering.
[0066] For example, when the copper particles 11 are flake-shaped copper particles, the specific surface area of the copper powder can be, for example, 0.1 m². 2 / g, 0.2m 2 / g, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g or 0.9m 2 / g, or a range consisting of any two of these values. When the copper particles 11 are spherical copper particles, the specific surface area of the copper powder can be, for example, 0.8m². 2 / g, 0.9m 2 / g、1m 2 / g、2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g or 9m 2 / g, or a range consisting of any two of these values. This setting helps provide sufficient surface energy, thereby improving sintering activity during the sintering of the copper paste, increasing the contact area between copper particles, reducing contact resistance, and ultimately enhancing the conductivity of the copper powder. If the specific surface area is too small, for example, below the lower limit of the specific surface area of copper powder in the case of sheet-like and / or spherical copper particles, the provided sintering activity is limited, resulting in insufficient sintering, high contact resistance between copper particles 11, and poor conductivity. If the specific surface area is too large, for example, above the upper limit of the specific surface area of copper powder in the case of sheet-like and / or spherical copper particles, the provided sintering activity is too high, making the copper particles 11 easily oxidized.
[0067] In some preferred embodiments, when the copper particles 11 are spherical copper particles, the specific surface area of the copper powder is 0.8–3.5 m². 2 / g. This helps to provide moderate sintering activity, forming a strong contact surface between copper particles 11 or promoting the fusion of copper particles 11, which helps to further reduce contact resistance and thus improve the conductivity of copper powder.
[0068] In some embodiments, the tap density of copper powder 1 is 3.5–5 g / mL, for example, it can be 3.5 g / mL, 3.6 g / mL, 3.7 g / mL, 3.8 g / mL, 3.9 g / mL, 4.0 g / mL, 4.1 g / mL, 4.2 g / mL, 4.3 g / mL, 4.4 g / mL, 4.5 g / mL, 4.6 g / mL, 4.7 g / mL, 4.8 g / mL, 4.9 g / mL, or 5.0 g / mL, or a range consisting of any two of the above values. This configuration significantly reduces the volume of the same mass of copper particles 11 when used in conductive pastes, thereby reducing the viscosity of the conductive paste and consequently reducing the possibility of incomplete or broken copper grid lines.
[0069] Tap density can be understood as the mass of copper powder contained in a unit volume after copper powder is compacted through mechanical vibration or tapping.
[0070] In some preferred embodiments, the tap density of copper powder 1 is 4.0–5 g / mL. This allows copper powder 1 to form a good, continuous copper particle network in copper slurry, enabling better surface contact or fusion between copper particles 11 during sintering, further reducing contact resistance and improving the conductivity of the copper powder.
[0071] According to another aspect of this application, a method for preparing the aforementioned copper powder 1 is provided. FIG2 shows a flowchart of the method for preparing copper powder according to an embodiment of this application. As shown in FIG2, the preparation method includes operations S201 to S202.
[0072] In operation S201, copper particles 11 are acid-washed to obtain acid-washed copper particles 11.
[0073] In this embodiment, acid washing of the initial copper particles 11 helps to remove the original oxides and impurities attached to the copper particles 11, thereby improving the surface activity of the copper particles 11 in subsequent processing. It can be understood that acid washing here can be interpreted as removing all or part of the original oxides attached to the surface of the copper particles 11, preferably removing all of the original oxides.
[0074] In operation S202, the pickled copper particles 11 are mixed with an organic coating agent solution in air so that the surface of the copper particles 11 is sequentially coated with a copper oxide layer 12 and an organic coating layer 13, thus obtaining copper powder 1.
[0075] In this embodiment, by mixing in the air, a micro-oxidation environment is provided for the copper particles 11, which helps to form a copper oxide layer 12 before forming an organic coating layer 13, and then interact with the organic coating agent solution to form an organic coating layer 13. The copper oxide layer 12 enhances the bonding effect between the organic coating layer 13 and the copper particles 11.
[0076] It should be noted that the copper oxide layer 12 formed here is the same as described above, which can completely cover the surface of the copper particles 11 or partially cover the surface of the copper particles 11.
[0077] According to the embodiments of this application, the surface of copper particles 11 is controlled to oxidize by mixing in air, and the reaction process is shown in the following formula (I): 4Cu + O2 + 2H2O → 2Cu(OH)2 → CuO / C u Formula 2O (I).
[0078] By mixing in air, the copper oxide layer 12 is at least partially covered on the surface of the copper particles 11. The copper oxide layer 12 further strengthens the bond between the copper particles 11 and the organic coating layer 13. When subsequently applied to a copper electrode, the synergistic effect between the copper oxide layer 12 and the organic coating layer 13 enhances the anti-oxidation and anti-corrosion effect of the copper powder 1. This allows the copper electrode to continuously and stably provide good conductivity, preventing the copper electrode from losing conductivity and increasing the contact resistance between the copper electrode and the solar cell due to the peeling or decomposition of the organic coating layer 13 under humid, hot, or light conditions.
[0079] It is understood that the shape of the copper particles 11, the material of the copper oxide layer 12, the particle size and tap density of the copper powder 1, and the material and thickness of the organic coating layer 13 are the same as those mentioned above, and will not be repeated here.
[0080] In this embodiment, the organic coating agent solution includes at least one of an organic amine solution and a thiol solution. The organic coating agent solution can be understood as a solution formed by dissolving an organic coating agent in an organic solvent. The type of organic coating agent is the same as the material of the aforementioned organic coating layer 13, and will not be described again here. The organic solvent can be an alcohol solvent, such as methanol or ethanol. The addition of the organic solvent helps to fully dissolve the organic coating agent.
[0081] In some embodiments, pickling includes: adding copper particles 11 to an acid solution and stirring; the pickling further removes the original oxide layer and organic contaminants present on the initial copper particles 11, while retaining some active sites to promote subsequent oxidative bonding. The acid solution includes at least one of hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, perchloric acid, sulfurous acid, phosphoric acid, hydrofluoric acid, acetic acid, carbonic acid, hydrosulfuric acid, and hypochlorous acid. It is understood that the acid solution can be of a lower concentration as needed, for example, by mixing concentrated sulfuric acid with water in a certain proportion to obtain a dilute sulfuric acid solution of a certain concentration. The concentration of the acid solution can be adjusted according to the thickness of the original oxide layer.
[0082] Optionally, the temperature of the acid solution is 25–35°C, for example, 25°C, 30°C, or 35°C, and the pickling time is 40–60 minutes, for example, 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes. This setting helps to fully remove impurities and the original oxide layer attached to the surface of the copper particles 11.
[0083] In some embodiments, the temperature of the organic coating agent solution is 35–45°C, for example, 35°C, 40°C, or 45°C, or a range consisting of any two of the above values. The mixing time is 0.5–1.5 h, for example, 0.5 h, 1 h, or 1.5 h, or a range consisting of any two of the above values. This setting allows for appropriate temperature increase, which helps promote the diffusion of organic coating agent molecules to the surface of the copper oxide layer 12, shortens the reaction time, and helps activate the coordination reaction between the organic coating agent molecules and copper ions in the copper oxide (e.g., copper oxide or cuprous oxide), improving the chemical bond strength. This further strengthens the tight bond between the organic coating layer 13 and the copper particles 11, preventing the organic coating layer 13 from detaching, thus giving the copper powder 1 better antioxidant properties and electrical conductivity stability. Setting an appropriate mixing time can control the thickness of the copper oxide layer, preventing it from being too thin or too thick, exceeding the range of 2–8 nm.
[0084] In some embodiments, the molar concentration of the organic coating agent solution is 0.0001-0.05 mol / L, for example, it can be 0.0001 mol / L, 0.0003 mol / L, 0.0005 mol / L, 0.0007 mol / L, 0.0009 mol / L, 0.001 mol / L, 0.002 mol / L, 0.003 mol / L, 0.004 mol / L, 0.005 mol / L, 0.006 mol / L, 0.007 mol / L, 0.008 mol / L, 0.009 mol / L, 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, or 0.05 mol / L, or a range consisting of any two of the above values. With this setup, by controlling or selecting the concentration of the organic coating agent solution, the thickness and density of the organic coating layer 13 can be adjusted, thereby adjusting the content of nitrogen or sulfur elements in the organic coating layer.
[0085] According to another aspect of this application, a conductive copper paste is provided, comprising: copper powder as described above and a dispersion medium.
[0086] According to the embodiments of this application, the synergistic effect of the copper oxide layer 12 and the organic coating layer 13 enables the conductive copper paste to have better anti-oxidation properties and storage stability, reduces the resistance of the conductive paste, and provides a new approach for replacing silver with copper.
[0087] Optionally, the conductive copper paste comprises 80-92% copper powder 1 and 8-20% dispersion medium by mass. If the mass content of copper powder 1 is too high, although it can provide more conductive particles, it may result in poor dispersion, affecting the uniformity of conductivity; if the mass content of copper powder 1 is too low, it is difficult to provide sufficient conductivity, resulting in higher resistance and lower conductivity efficiency. Adjusting the mass content of copper powder 1 within the above range helps to form a sufficient conductive network, reducing resistance while ensuring the uniformity of the conductive network. If the mass content of the dispersion medium is too high, the copper powder 1 content is too low, resulting in higher resistance; if the mass content of the dispersion medium is too low, the conductive copper paste becomes too viscous, making subsequent printing or coating processes difficult. Adjusting the mass content of the dispersion medium within the above range helps to balance the fluidity and conductivity of the conductive copper paste.
[0088] In some embodiments, the resistivity of the conductive copper paste is 10–15 μΩ·cm, for example, it can be 10 μΩ·cm, 10.3 μΩ·cm, 11 μΩ·cm, 11.1 μΩ·cm, 11.5 μΩ·cm, 12 μΩ·cm, 12.1 μΩ·cm, 12.5 μΩ·cm, 13 μΩ·cm, 13.5 μΩ·cm, 14 μΩ·cm, 14.5 μΩ·cm, or 15 μΩ·cm. Based on the synergistic effect between the organic coating layer 13 and the copper oxide layer 12, the layered structure on the surface of the copper powder 1 can achieve a more superior oxygen-isolation and oxidation-resistant effect even with thinning. Correspondingly, the thinning of the surface coating layer results in a lower resistivity and better conductivity in the conductive copper paste.
[0089] In some embodiments, the dispersion medium includes a resin, a curing agent, a dispersant, and a solvent. The addition of the resin and curing agent provides better low-temperature curing, while the addition of the dispersant and solvent reduces the viscosity of the conductive copper paste, making it suitable for finer copper grid line printing processes.
[0090] From the perspective of obtaining better low-temperature curing effect, the resin is selected from at least one of epoxy resin, phenolic resin, phenoxy resin, acrylic resin, aldehyde-ketone resin, polyurethane, and polyester.
[0091] Optionally, the epoxy resin can be a thermosetting resin, specifically selected from one or more of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, polyurethane modified epoxy resin, dimer acid modified epoxy resin, siloxane modified epoxy resin, phenolic type epoxy resin, polyol glycidyl ether type epoxy resin, and polyacid glycidyl ester type epoxy resin. Of course, other resins known in the art that can be used in this application may also be selected, but since this is not the focus of this application, further limitations are not made here.
[0092] The curing agent is selected from at least one of dicyandiamide curing agents, tertiary amine curing agents, isocyanate curing agents, blocked isocyanate curing agents, imidazole curing agents, and acid anhydride curing agents.
[0093] Optionally, the curing agent may be selected from one or more of the following: triethanolamine, blocked isocyanate, 1-butyl-3-methylimidazolium dibutyl phosphate, Baxington 7982, Trixene BI 7982 (blocked isocyanate based on HDI), MF-K60X (blocked polyisocyanate HDI curing agent), ketoxime-terminated isocyanate, hexamethylene hexamethylene diisocyanate-terminated, and dodecyl mercaptan-terminated diphenyl diisocyanate. Of course, other curing agents known in the art that can be used in this application may also be selected, but since this is not the focus of this application, further limitations are not made here.
[0094] From the perspective of reducing the viscosity of conductive copper paste, the dispersant is selected from C. 16 ~C 22 Ether dispersants, C 16 ~C 22 Amine dispersants, C 16 ~C 22 At least one of carboxylic acid dispersants, wherein the end group of the dispersant is a polar group such as an amino group or a hydroxyl group.
[0095] Optionally, the dispersant may be selected from at least one of Tween-type dispersants, oleic acid, and Span-type dispersants. Of course, other dispersants known in the art that can be used in this application may also be selected, but since this is not the focus of this application, no further limitation is made here.
[0096] From the perspective of improving the solubility of various dispersion media, the solvent can be selected from at least one of ester solvents, ether solvents, ketone solvents or alcohol solvents.
[0097] Optionally, the solvent may be selected from sec-amyl acetate, cyclohexanone, amyl propionate, isopropyl lactate, divalent esters, amyl acetate, diethylene glycol acetate, diethylene glycol butyl ether acetate, ethylene glycol carbonate, propylene glycol carbonate, tributyl borate, triphenyl phosphate, tricresyl phosphate, butyl acetate, diethyl carbonate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, γ-butyrolactone, butyl carbitol acetate, ethyl carbitol acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate. Ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol butyl ether, ethylene glycol diethyl ether, diethylene glycol butyl ether, ethylene glycol monoisopropyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol propyl ether, dipropylene glycol butyl ether, dipropylene glycol ether, ethylene glycol dimethyl ether, tripropylene glycol methyl ether, tripropylene glycol dimethyl ether, diethylene glycol monobutyl ether, 4-heptanone, sec-pentanol, ethylene glycol, propylene glycol, pentanol, hexanol, heptanol, octanol, methylpentanol, butyl carbitol, terpineol, dihydroterpineol.
[0098] It is understandable that conductive copper paste may also include other additives such as accelerators as needed, which will not be elaborated here.
[0099] According to another aspect of this application, a copper electrode is provided, which is formed from the above-described conductive copper paste.
[0100] According to the embodiments of this application, as described above, since the connection between the organic coating layer 13 and the copper particles 11 is strengthened by the copper oxide layer 12, better isolation effect against oxygen, moisture and the like can be provided even when the organic coating layer 13 and the copper oxide layer 12 are relatively thin, thereby reducing the resistivity of the copper electrode, making it have higher conductivity and improving the stability of the copper electrode in use.
[0101] This application also provides a method for preparing the aforementioned copper electrode, comprising the following steps: pre-prepared conductive copper paste is screen-printed onto a solar cell (e.g., HJT / HBC), with the grid line width set to 40-120 μm; then, it is heated and cured in a nitrogen oven. The curing temperature is generally 100-220℃, for example, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, 210℃, 220℃, etc., and the curing time is 10 min-60 min, for example, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc., thereby forming the electrode grid lines.
[0102] According to another embodiment of this application, a solar cell is provided, including the copper electrode described above.
[0103] According to the embodiments of this application, as described above, the copper electrode configured in this way, based on the synergistic effect of the copper oxide layer 12 and the organic coating layer 13, provides an effective approach and solution for the base metallization of the grid line material when applied in solar cells.
[0104] In some embodiments, the solar cell is selected from any one of a back contact cell, a heterojunction cell, or a perovskite-crystalline silicon tandem cell.
[0105] It is understood that the electrodes of the back contact battery are located on the back side of the battery. The copper electrodes mentioned above are applied to the electrode material of the back grid lines. For example, the electrodes can be formed by screen printing. The copper powder 1 formed by copper particles 11 sequentially coated by the copper oxide layer 12 and the organic coating layer 13 helps to provide the back contact battery with better anti-oxidation effect, reduces the possibility of the organic coating layer 13 falling off, improves the stability of electrode use, and can improve the conductivity efficiency to a certain extent. Since it replaces the silver electrode, it is beneficial to reduce costs.
[0106] It is understood that heterojunction solar cells are bifacial cells. Copper electrodes are formed on the substrate surface, for example, grid electrodes can be prepared by screen printing, and a transparent conductive layer can be prepared by electrochemical deposition using the copper powder 1 of this application, as needed. Similarly, since silver electrodes are replaced, better current collection and transmission efficiency and stability of electrode use can be provided while reducing costs.
[0107] It is understandable that in perovskite-crystalline silicon tandem solar cells, copper electrodes can be used as the intermediate connecting layer to replace the traditional ITO / Ag, or as the electrode of the top cell. Since it replaces silver, similar to the above, it can reduce costs while providing better current collection and transmission efficiency and maintaining the stability of electrode use.
[0108] The present application is further illustrated below through embodiments, accompanying drawings, and related test experiments and results. In the following detailed description, numerous specific details are set forth for ease of explanation to provide a comprehensive understanding of the embodiments of the present application. However, it is apparent that one or more embodiments may be implemented without these specific details. Moreover, the details in the following embodiments can be arbitrarily combined to form other feasible embodiments without conflict.
[0109] It should be noted that the specific embodiments described below are merely illustrative examples, and the scope of protection of this application is not limited thereto. The chemicals and raw materials used in the following embodiments are all commercially available or prepared using recognized processing methods.
[0110] Example 1:
[0111] Take 50g of raw copper particles (spherical, D)50 =200nm), add 200mL of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish acid washing, remove the anti-oxidation layer, oxides and impurities on the surface of the original copper particles, and separate the acid-washed spherical copper particles.
[0112] Dissolve 0.5 g of tetrahydroxyethyl ethylenediamine in 500 mL of ethanol to obtain a nitrogen organic coating agent solution.
[0113] 50g of acid-washed spherical copper particles were mixed with a nitrogen-based organic coating agent solution in air at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0114] 30 mg of copper powder was placed in a fluxing nickel foil, wrapped up, and then placed in an oxygen and nitrogen analyzer. The mass content of nitrogen was measured to be 311 ppm.
[0115] Figure 3 shows a transmission electron microscope (TEM) image of the copper powder of Example 1 of this application; Figure 4 shows a partial magnified view of the copper powder in Figure 3, wherein 4-1 shows a partial magnified view and elemental analysis diagram of (a) of the copper powder in Figure 3; 4-2 shows a partial magnified view and elemental analysis diagram of (b) of the copper powder in Figure 3; and 4-3 shows a partial magnified view and elemental analysis diagram of (c) of the copper powder in Figure 3. As can be seen from Figures 3 and 4, a copper oxide layer exists between the organic coating layer and the copper particles. Measurements of the copper oxide layer indicate that its thickness is 2–3 nm. Lattice calculations from the TEM images show that (a) in Figure 4-1 represents copper particles, primarily copper (200) crystal planes with a spacing of 1.82 Å. (b) in Figure 4-2 represents copper oxide, primarily CuO (111) crystal planes with a spacing of 2.31 Å. In Figure 4-3, (c) represents copper oxide, mainly Cu2O(111) crystal planes with a spacing of 2.42 angstroms.
[0116] Example 2:
[0117] The preparation process of Example 2 is largely the same as that of Example 1, except that the spherical copper particles are replaced with plate-shaped copper particles, and the D of the plate-shaped copper particles is... 50 =3.5μm, the specific surface area of the prepared copper powder is 0.5m². 2 / g.
[0118] 30 mg of copper powder was placed in a nickel foil flux, wrapped up, and then placed in an oxygen and nitrogen analyzer. The nitrogen content was measured to be 198 ppm.
[0119] Examples 3-4:
[0120] The preparation process of Examples 3 and 4 is largely the same as that of Example 1, except that the amount of tetrahydroxyethyl ethylenediamine used is different. In Example 3, 0.1 g of tetrahydroxyethyl ethylenediamine was used, and in Example 4, 1.0 g of tetrahydroxyethyl ethylenediamine was used. The nitrogen content of the prepared samples is shown in Table 1 below.
[0121] Example 5:
[0122] Take 50g of raw copper particles (spherical, D) 50 =200nm), add 200mL of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish acid washing, remove the anti-oxidation layer, oxides and impurities on the surface of the original copper particles, and separate the acid-washed spherical copper particles.
[0123] Dissolve 1 mL of octadecyl mercaptan in 500 mL of ethanol to obtain a sulfur organic coating solution.
[0124] 50g of pickled spherical copper particles were mixed with a sulfur organic coating agent solution in air at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0125] 1g of copper powder was placed in a fluxing nickel foil, wrapped up, and then placed in a carbon-sulfur analyzer. The sulfur content was measured to be 537ppm.
[0126] Example 6:
[0127] The preparation process of Example 6 is largely the same as that of Example 5, except that the spherical copper particles are replaced with plate-shaped copper particles, and the D of the plate-shaped copper particles is... 50 =3.5μm, the specific surface area of the prepared copper powder is 0.5m². 2 / g.
[0128] 1g of copper powder was placed in a flux nickel foil, wrapped up, and then placed in a carbon-sulfur analyzer. The sulfur content was measured to be 245ppm.
[0129] Examples 7-8:
[0130] The preparation process of Examples 7 and 8 is largely the same as that of Example 5, the difference being the amount of octadecyl mercaptan used. In Example 7, 0.07 mL of octadecyl mercaptan was used, while in Example 8, 2 mL of octadecyl mercaptan was used. The sulfur content of the prepared samples is shown in Table 1 below.
[0131] Example 9:
[0132] Take 50g of raw copper powder particles (spherical, D) 50=300nm), add 200mL of pre-diluted 3mol / L dilute sulfuric acid, stir at 40℃ for 90min to finish acid washing, remove the anti-oxidation layer, oxides and impurities on the surface of the original copper powder particles, and separate the acid-washed copper powder particles.
[0133] Dissolve 1 mL of dodecyl mercaptan in 500 mL of ethanol to obtain a sulfur organic coating solution.
[0134] 50g of pickled copper powder particles were mixed with a sulfur organic coating agent solution in air at 50°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0135] 1g of copper powder was placed in a fluxing nickel foil, wrapped up, and then placed in a carbon-sulfur analyzer. The sulfur content was measured to be 260ppm.
[0136] Comparative Example 1:
[0137] Take 50g of raw copper particles (spherical, D) 50 =200nm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish pickling, remove the surface antioxidant layer, oxides and impurities, and separate the pickled spherical copper particles.
[0138] Dissolve 0.5 g of tetrahydroxyethyl ethylenediamine in 500 mL of ethanol to obtain a nitrogen organic coating agent solution.
[0139] 50g of acid-washed spherical copper particles were mixed with a nitrogen-based organic coating agent solution under vacuum at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0140] 30 mg of copper powder was placed in a nickel foil flux, wrapped up, and then placed in an oxygen and nitrogen analyzer. The nitrogen content was measured to be 200 ppm.
[0141] Comparative Example 2:
[0142] Take 50g of raw copper granules (flakes, D) 50 =3.5μm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish pickling, remove the surface antioxidant layer, oxides and impurities, and separate the pickled flake copper particles.
[0143] Dissolve 0.5 g of tetrahydroxyethyl ethylenediamine in 500 mL of ethanol to obtain a nitrogen organic coating agent solution.
[0144] 50g of acid-washed flake copper particles were mixed with a nitrogen-based organic coating agent solution under vacuum at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0145] 30 mg of copper powder was placed in a nickel foil flux, wrapped up, and then placed in an oxygen and nitrogen analyzer. The nitrogen content was measured to be 101 ppm.
[0146] Comparative Example 3:
[0147] Take 50g of raw copper particles (spherical, D) 50 =200nm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish pickling, remove the surface antioxidant layer, oxides and impurities, and separate the pickled spherical copper particles.
[0148] Dissolve 1 mL of octadecyl mercaptan in 500 mL of ethanol to obtain a sulfur organic coating solution.
[0149] 50g of acid-washed spherical copper particles were mixed with a sulfur organic coating agent solution under vacuum at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and then dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0150] 1g of copper powder was placed in a fluxing nickel foil, wrapped up, and then placed in a carbon-sulfur analyzer. The sulfur content was measured to be 235ppm.
[0151] Comparative Example 4:
[0152] Take 50g of raw copper granules (flakes, D) 50 =3.5μm), add 200ml of pre-diluted 3mol / L dilute sulfuric acid, stir at 30℃ for 50min to finish pickling, remove the surface antioxidant layer, oxides and impurities, and separate the pickled flake copper particles.
[0153] Dissolve 1 mL of octadecyl mercaptan in 500 mL of ethanol to obtain a sulfur organic coating solution.
[0154] 50g of acid-washed flake copper particles were mixed with a sulfur organic coating agent solution under vacuum at 40°C for 1 hour to obtain passivated copper powder. The passivated copper powder was washed with ethanol and dried in an oven under a nitrogen atmosphere to obtain copper powder.
[0155] 1g of copper powder was placed in a fluxing nickel foil, wrapped up, and then placed in a carbon-sulfur analyzer. The sulfur content was measured to be 116ppm.
[0156] The relevant parameters of the copper powder in the above embodiments and comparative examples are shown in Table 1 below.
[0157] Table 1
[0158] The copper powders prepared in Examples 1-9 and Comparative Examples 1-4 were subjected to electrical performance tests.
[0159] The copper powders obtained after passivation in Examples 1-9 and Comparative Examples 1-4 were respectively formulated into conductive copper pastes. Specifically, 0.4g of hydrogenated bisphenol A epoxy resin, 0.15g of blocked isocyanate as curing agent, 0.15g of imidazole dibutyl phosphate as curing accelerator, 0.05g of oleylamine as dispersant, and 0.3g of diethylene glycol butyl ether acetate as solvent were mixed and stirred evenly to obtain a slurry mother liquor. 8g of the copper powder obtained after passivation in Examples 1-8 or Comparative Examples 1-4 was poured into the slurry mother liquor, stirred, and then poured into a three-roll mill for rolling and grinding to obtain a homogeneous conductive copper paste.
[0160] The copper grid lines are screen-printed onto the solar cell with a width of 70 μm. They are then heated and cured in a nitrogen oven at a temperature of 100–200 °C for 30 minutes to form copper electrode blocks and copper grid lines. The electrical properties of the paste can be obtained through a series of tests.
[0161] The copper electrode block and copper grid lines were tested. The resistivity of the copper electrode block was measured using the four-probe method, and the resistivity was calculated. The grid line contact resistance was tested using transmission line mode (TLM). DH5 represents the contact resistance of the cured battery after being placed at 85% humidity and 85°C for 5 hours. Table 2 below shows the relevant performance parameters of the copper electrodes in Examples 1-9 and Comparative Examples 1-4.
[0162] Table 2
[0163] As shown in Table 2, it can be seen that Examples 1 and 3-4 have relatively lower resistivity compared to Comparative Example 1, Example 2 has relatively lower resistivity compared to Comparative Example 2, Examples 5 and 7-9 have relatively lower resistivity compared to Comparative Example 3, and Example 6 has relatively lower resistivity compared to Comparative Example 4. This indicates that the copper powder of this application improves the conductivity of the copper electrode. Examples 1-9 and Comparative Examples 1-4 all have good initial contact at the start of the electrochemical reaction, while the copper electrodes of Examples 1-9 still maintain low contact resistance under high temperature and high humidity conditions. Based on the DH5 test, it is confirmed that Examples 1-9 of this application still have good hydrothermal stability after multiple cycles. Further comparisons were made between Examples 1 and Examples 3-4, and between Examples 5 and Examples 7-9. Example 1 has better hydrothermal stability than Examples 3-4, and Example 5 has better hydrothermal stability than Examples 7-9.
[0164] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A copper powder comprising: Copper particles, a copper oxide layer at least partially covering the outside of the copper particles, and an organic coating layer covering the outside of the copper oxide layer; The organic coating layer contains nitrogen or sulfur, and the nitrogen content is 50-800 ppm or the sulfur content is 30-1000 ppm based on the total mass of the copper powder.
2. The copper powder of claim 1, wherein, The mass content of nitrogen is 100–600 ppm, or the mass content of sulfur is 200–600 ppm.
3. The copper powder of claim 1, wherein, The thickness of the organic coating layer is 2–15 nm.
4. The copper powder of claim 1, wherein, The copper oxide layer includes copper oxide and / or cuprous oxide, and / or the thickness of the copper oxide layer is 2-8 nm.
5. The copper powder according to any one of claims 1 to 4, wherein The organic coating layer includes at least one of organic amine compounds and thiol compounds; Preferably, the organic coating layer comprises at least one of a C6-C 22 aliphatic amine compound, a C6-C 22 aliphatic thiol compound; More preferably, C6~C 22 The aliphatic amine compound is selected from at least one of n-octylamine, n-hexylamine, dodecylamine, tetradecylamine, hexadecylamine, stearylamine, oleylamine, and tetrahydroxyethylethylenediamine, wherein C6-C 22 The aliphatic thiol compound is selected from at least one of the following: thiol, octylthiol, dodecylthiol, and octadecylthiol.
6. The copper powder according to any one of claims 1 to 4, wherein The copper particles are either flake-shaped or spherical.
7. The copper powder of claim 6, wherein, When the copper particles are flaky copper particles, the D50 of the copper powder is 1-10 μm 50 When the copper particles are flaky copper particles, the D50 of the copper powder is 1-10 μm 50 When the copper particles are spherical copper particles, the D50 of the copper powder is 0.1-1 μm.
8. The copper powder of claim 6, wherein, when the copper particles are flaky copper particles, the specific surface area of the copper powder is 0.1-0.9 m 2 / g; when the copper particles are spherical copper particles, the specific surface area of the copper powder is 0.8-9 m 2 / g; and / or the tap density of the copper powder is 3.5-5 g / mL.
9. A method for preparing the copper powder according to any one of claims 1-8, comprising: The copper particles are acid-washed to obtain acid-washed copper particles; The pickled copper particles are mixed with an organic coating agent solution in air so that the surface of the copper particles is sequentially coated with a copper oxide layer and an organic coating layer to obtain the copper powder. Among them, organic coating agents have nitrogen-containing groups or sulfur-containing groups.
10. The production method according to claim 9, wherein The organic coating agent solution includes at least one of the following: an organic amine solution and a thiol solution.
11. The production method according to claim 9, wherein The temperature of the organic coating agent solution is 35–45°C, and the mixing time is 0.5–1.5 h.
12. The production method according to claim 9, wherein, The molar concentration of the organic coating agent solution is 0.0001–0.05 mol / L.
13. An electrically conductive copper paste comprising: Copper powder and dispersion medium, wherein the copper powder is the copper powder as described in any one of claims 1 to 8 or the copper powder prepared by the method described in any one of claims 9 to 12; Preferably, the conductive copper paste comprises 80-92% copper powder and 8-20% dispersion medium by weight.
14. A copper electrode, formed from the conductive copper paste described in claim 13.
15. A solar cell comprising the copper electrode as claimed in claim 14.