Ternary positive electrode material compositely modified by means of surface gradient doping and coating and preparation method therefor, and sulfide-based all-solid-state battery
By modifying ternary cathode materials through surface gradient doping and coating, the space charge layer problem between ternary cathode materials and sulfide solid electrolytes was solved, improving interfacial compatibility and lithium-ion migration rate, and enhancing the electrochemical performance of all-solid-state batteries.
Patent Information
- Application Number
- PCT/CN2026/095092
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
The space charge layer between ternary cathode materials and sulfide solid electrolytes leads to poor interfacial compatibility, hinders lithium-ion transport, and affects the electrochemical performance of all-solid-state batteries.
A ternary cathode material modified by surface gradient doping and coating is used. Through the synergistic effect of gradient doping elements, transition metal elements and oxygen in the ternary cathode material lattice, the chemical potential of lithium ions on both sides of the interface is balanced. The space charge layer effect is suppressed by the surface coating, thereby improving the interface stability and lithium ion migration rate.
It effectively suppressed the space charge layer effect between the ternary cathode material and the sulfide solid electrolyte, improved the interfacial compatibility and lithium-ion migration performance, and enhanced the electrochemical performance of the all-solid-state battery.
Smart Images

Figure CN2026095092_19112026_PF_FP_ABST
Abstract
Description
Surface gradient doping and coating composite modification of ternary cathode materials, their preparation methods and sulfide all-solid-state batteries Technical Field
[0001] This invention relates to the field of power battery technology, and in particular to a ternary cathode material for use in all-solid-state batteries and its preparation method. Background Technology
[0002] With the development of new energy vehicles, the market has placed higher demands on the energy density, charging speed, and safety of power batteries. All-solid-state batteries use a solid electrolyte to transfer lithium ions between the positive and negative electrodes, replacing flammable and volatile liquid organic electrolytes and improving battery safety. Furthermore, solid electrolytes possess superior mechanical properties, inhibiting lithium dendrite growth and potentially enabling the use of lithium metal anodes in the future, significantly increasing battery energy density.
[0003] Sulfide solid electrolytes possess ionic conductivity comparable to that of electrolytes, making them one of the most promising solid electrolytes. However, sulfide solid electrolytes and ternary cathode materials suffer from problems such as space charge layers, chemical / electrochemical side reactions, and contact failure.
[0004] The space charge layer, also known as the lithium-ion space layer, occurs when a sulfide solid electrolyte comes into contact with a ternary cathode material. Due to the difference in lithium-ion chemical potentials between the two, some lithium ions migrate from the electrolyte surface to the oxide cathode material side, creating a lithium-ion concentration difference between the electrolyte bulk phase and the interface, thus hindering lithium-ion transport. Since the ternary cathode material is an ion-electron composite conductor, its electronic conductivity can balance the lithium-ion concentration gradient on the cathode material side, causing more lithium ions to migrate towards the cathode material side. This forms a lithium-ion "loss zone" at the interface, significantly reducing the migration rate of lithium ions at the electrolyte-cathode material interface, thereby reducing the electrochemical performance of the material. Therefore, the poor interfacial compatibility between ternary cathode materials and sulfide solid electrolytes, coupled with the unique space charge layer effect, severely hinders lithium-ion transport at the interface, limiting the electrochemical performance of the cathode material in all-solid-state batteries.
[0005] Patent application CN113745497A describes a process where soluble X and Y metal salts are co-precipitated with nickel, cobalt, and manganese salts to prepare X and Y-doped precursors. These precursors are then mixed with lithium salts and calcined to obtain a single-crystal high-nickel cathode material with X bulk doping and Y in-situ gradient doping. Patent application CN118173763A describes a process where a cobalt-containing compound and a metal compound are mixed and sintered to obtain a cobalt-doped material. This cobalt-doped material is then mixed with a precursor and lithium salt and sintered again, followed by a second sintering coating to obtain a cobalt-gradient-doped modified ternary cathode material. While these techniques can improve the performance of ternary cathode materials in electrolyte systems to some extent, they fail to effectively address the interface problems faced by ternary cathode materials in all-solid-state battery systems. Summary of the Invention
[0006] To address the inherent space charge layer problem between ternary cathode materials and sulfide solid electrolytes, this invention provides a ternary cathode material and its preparation method that are modified by surface gradient doping and coating. Through the synergistic effect of gradient doping elements, transition metal elements within the ternary cathode material lattice, and oxygen, the chemical potential of lithium ions on both sides of the interface is balanced. Furthermore, the introduction of a new interface through surface coating avoids direct contact, suppressing the space charge layer effect between the electrode material and the solid electrolyte, improving interface stability and lithium ion migration rate, and enhancing the performance of the ternary cathode material in all-solid-state batteries.
[0007] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows:
[0008] A ternary cathode material with surface gradient doping and coating composite modification, comprising a gradient doped region of element M1 on the surface of a ternary cathode material matrix, and a coating containing element M2 on the surface of the gradient doped region; wherein the ionic radius R of element M1 is... M1 With respect to the nickel ion radius R Ni3+ The relationship between R Ni3+ <R M1 ≤1.3R Ni3+ The ionic radius R of the M2 element M2 With respect to the nickel ion radius R Ni3+ The relationship between R M2 ≥1.3R Ni3+ ,and
[0009] The depth of the gradient doping region is within 1000 nm. Within the gradient doping region, the content of doped M1 element gradually decreases from the outside to the inside, and the proportion of M1 element content within 100 nm of the surface of the gradient doping region to the total amount of M1 element is Wt. surface % meets 30wt% <Wt surface % <70wt%.
[0010] In the above ternary cathode material modified by surface gradient doping and coating composite, preferably, the mass proportion of the M1 element in the ternary cathode material is 0.01 to 2 wt%, and the mass proportion of the M2 element in the ternary cathode material is 0.01 to 1 wt%.
[0011] Preferably, the M1 element includes one or more of Mg, Ti, Co, Ga, Zr, Nb, Mo, Sn, Sb, Ta, W, and the M2 element includes one or more of Na, K, Ca, Zn, Sr, Y, Ba, La, Ce.
[0012] Preferably, the nickel ion radius R Ni3+ is
[0013] Preferably, the ternary cathode material has a single crystal morphology, and the particle D 50 is 2 to 7 μm.
[0014] Preferably, the coating substance is island-shaped coated particles, and the particle size of the coated particles is 50 to 500 nm. The coated particles are the coating substance with lithium ion conductivity formed by the reaction of the M2 element with the residual lithium on the surface.
[0015] Preferably, the chemical formula of the ternary cathode material matrix is LiNi 1-x-y-z Co x Mn y Z z O2, where 0.5≤1-x-y-z<1, 0<x≤0.3, 0<y≤0.3, 0<z≤0.01, and the Z element includes one or more of Mg, Al, Ca, Ti, Sr, Zr, Ba, La, W.
[0016] Preferably, the doping depth and content of the M1 element and the content of the M2 element are obtained by EPMA analysis.
[0017] Based on a general inventive concept, the present invention further provides a preparation method of the ternary cathode material modified by surface gradient doping and coating composite, comprising the following steps:
[0018] 1) Weigh the ternary cathode material matrix, and mix it with additives containing M1 and M2 elements to obtain a mixture;
[0019] 2) Subject the mixture to a staged calcination treatment to obtain a calcined product;
[0020] 3) The calcined product is crushed and sieved to obtain the ternary cathode material modified by surface gradient doping and coating composite.
[0021] In the above preparation method, preferably, in step 1), the additive containing elements M1 and M2 is one or more of oxides, hydroxides, carbonates, nitrates, acids and ammonium salts; the mixing machine is used at a speed of 500-2000 rpm and the mixing time is 10-60 min.
[0022] Preferably, in step 2), the segmented calcination includes a first stage and a second stage, wherein the calcination temperature T1 of the first stage and the ionic radius R of element M1 are... M1 satisfy The calcination time is 1–5 h; the calcination temperature T2 in the second stage and the ionic radius R of element M1 are also considered. M1 satisfy The calcination time is 1–8 h, the heating / cooling rate is 1–10 °C / min, and the calcination atmosphere is oxygen or air. The purpose of this segmented calcination process is to first calcine at a higher temperature T1 to promote the thermal diffusion of the M1 element with a small ionic radius into the material lattice, forming a surface gradient doping; then cool down to a lower temperature T2 to prevent excessive diffusion of the M1 element and the formation of uniform bulk doping, while allowing the M2 element with a larger ionic radius to continue reacting with residual lithium to form a surface coating.
[0023] The technical principle of this invention is as follows:
[0024] This invention utilizes the different thermal diffusion rates of metal ions with different radii and employs a segmented calcination process to control the diffusion process of elements from the particle surface to the interior, achieving one-step synthesis of composite modified cathode materials with gradient doping and surface coating:
[0025] Among them, the ionic radius of element M1 is greater than that of element Ni. 3+ Slightly larger, it is easier for M1 to enter the ternary material lattice through thermal diffusion during the calcination process, forming surface gradient doping. If the ionic radius of element M1 is larger than that of Ni... 3+ If the doping density is too low, the M1 element will diffuse entirely into the particle interior during calcination, forming uniform doping. This prevents the M1 from accumulating on the surface and forming a surface gradient doping, thus hindering targeted improvement of the material's surface structure. Therefore, this invention selects gradient-doped M1 elements to precisely regulate the chemical potential of lithium ions on the surface of the ternary material particles, balancing the lithium ion concentration on both sides of the interface, suppressing the space charge layer effect, improving near-surface lattice stability, reducing oxygen vacancies, decreasing near-surface volume changes, and suppressing contact failure between the cathode material and the solid electrolyte.
[0026] Meanwhile, the ionic radius of element M2 is greater than that of element Ni. 3+Much larger, these lithium-ion conductors are difficult to diffuse into the crystal lattice during calcination and tend to react with residual lithium on the particle surface to form a lithium-ion conductive coating. Introducing a lithium-ion conductive coating at the interface between the cathode material particles and the sulfide solid electrolyte transforms the original cathode / electrolyte interface into a cathode / coating and coating / electrolyte interface. The formation of this new interface not only hinders direct contact between the cathode material and the solid electrolyte, thereby reducing side reactions, but also balances the chemical potentials on both sides, suppresses the formation of a space charge layer, improves the migration rate of lithium ions at the interface, and enhances the performance of ternary cathode materials in all-solid-state batteries.
[0027] In summary, this invention, based on the differences in diffusion properties of elements with different ionic radii in the crystal lattice during calcination, combines modifying elements with different ionic radii and controls the calcination temperature according to the ionic radius. It adopts a segmented calcination process to control the diffusion process of elements from the particle surface to the interior. Surface gradient doping and surface coating composite modification can be achieved simultaneously in one calcination step, which has the advantages of simple process, low cost and easy control.
[0028] Based on a general inventive concept, the present invention also provides a sulfide all-solid-state battery, which includes the ternary cathode material that has been surface-gradient doped and coated with composite modification. In addition, the sulfide all-solid-state battery also includes a sulfide solid electrolyte and a negative electrode active material.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0030] 1. The ternary cathode material of this invention is modified by gradient doping and coating of the substrate surface with modifying elements of different ionic radii. Surface gradient doping focuses on adjusting the chemical potential of lithium ions on the surface of the ternary material particles, balancing the lithium ion concentration on both sides of the interface, suppressing the space charge layer effect, and improving the stability of the near-surface lattice, reducing the generation of oxygen vacancies, reducing the volume change of the near-surface, and suppressing contact failure between the cathode material and the solid electrolyte. Synergistic surface coating can suppress the space charge layer effect and interfacial side reactions at the cathode material / sulfide solid electrolyte interface, thereby improving interfacial compatibility and lithium ion migration rate. Developing a composite modified cathode material suitable for all-solid-state battery systems and easy for large-scale industrial production is of great significance.
[0031] 2. The preparation method of the present invention simplifies the process and reduces production costs through a one-step synthesis method, simultaneously achieving surface gradient doping and surface coating composite modification, improving the interfacial compatibility between ternary materials and sulfide solid electrolytes, suppressing the space charge layer effect, and improving the interfacial lithium-ion conductivity. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0033] Figure 1 is a schematic diagram of the structure of the ternary cathode material of the present invention.
[0034] Figure 2 is a SEM image of the ternary cathode material of Embodiment 1 of the present invention.
[0035] Figure 3 shows the EPMA mapping and line scan of the ternary cathode material in Embodiment 1 of the present invention (the horizontal axis is in mm; the vertical axis is the signal intensity).
[0036] Figure 4 is a SEM image of the ternary cathode material of Example 2 of the present invention.
[0037] Figure 5 shows the EPMA mapping and line scan of the ternary cathode material in Embodiment 2 of the present invention (the horizontal axis is in mm; the vertical axis is the signal strength).
[0038] Figure 6 is a SEM image of the ternary cathode material of Comparative Example 1 of the present invention.
[0039] Figure 7 shows the EPMA mapping and line scan of the ternary cathode material of Comparative Example 1 of the present invention (the horizontal axis is in mm; the vertical axis is the signal strength).
[0040] Figure 8 is a SEM image of the ternary cathode material of Comparative Example 2 of the present invention.
[0041] Figure 9 is an EPMA mapping diagram of the ternary cathode material of Comparative Example 2 of the present invention.
[0042] Figure 10 is a SEM image of the ternary cathode material of Comparative Example 3 of the present invention.
[0043] Figure 11 shows the EPMA mapping and line scan of the ternary cathode material of Comparative Example 3 of the present invention (the horizontal axis is in mm; the vertical axis is the signal strength).
[0044] Figure 12 is a SEM image of the ternary cathode material of Comparative Example 4 of the present invention.
[0045] Figure 13 shows the EPMA mapping and line scan of the ternary cathode material of Comparative Example 4 of the present invention (the horizontal axis is in mm; the vertical axis is the signal strength).
[0046] Figure 14 shows the first charge-discharge curves of the ternary cathode materials of Example 1 and Comparative Example 1 of the present invention.
[0047] Figure 15 shows the cycle performance of solid-state mold batteries in various embodiments and comparative examples of the present invention. Detailed Implementation
[0048] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the accompanying drawings and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0049] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0050] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0051] The ternary cathode material modified by surface gradient doping and coating of the present invention, as shown in Figure 1, has a gradient doping region of M1 element on the surface of the ternary cathode material (NCM) matrix. The content of M1 element in this region gradually decreases from the outside to the inside. The surface of the gradient doping region has a coating containing M2 element.
[0052] In the following examples, the nickel ion radius R Ni3+ for
[0053] Example 1:
[0054] A method for preparing a ternary cathode material with surface gradient doping and coating composite modification according to the present invention includes the following steps:
[0055] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.85 Co 0.10 Mn 0.045 Al 0.005 O2, with 1 wt% TiO2 (based on Ti content, ) and 0.3 wt% La2O3 (based on La content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1200 rpm for 45 minutes.
[0056] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 5℃ / min, and the calcination temperature T1 was 750℃. The calcination time was 4 hours; subsequently, the temperature was reduced at a rate of 3℃ / min, with the calcination temperature T2 being 470℃. The calcination time was 5 hours, and the atmosphere was oxygen, to obtain the calcined product;
[0057] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with Ti gradient doping and La coating composite modification.
[0058] As shown in Figure 2, the ternary cathode material modified by Ti surface gradient doping and La coating has a single crystal morphology, with particle D... 50 The particle size is about 4μm, and the surface is covered with nanoscale island-like coatings formed by the metal element La, with the coating particle size being 150nm.
[0059] As shown in Figure 3, EPMA analysis revealed that the surface Ti gradient doping depth is 810 nm. The Ti content within the doped region gradually decreases from the outside to the inside. The proportion of Ti content (Wt) within a 100 nm depth range on the particle surface relative to the total Ti content is [not specified]. surface % = 56%.
[0060] Example 2:
[0061] A method for preparing a ternary cathode material with surface gradient doping and coating composite modification according to the present invention includes the following steps:
[0062] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.90 Co 0.05 Mn 0.04 Al 0.01 O2, with 0.8 wt% ZrO2 (based on Zr content, ) and 0.2 wt% Nb₂O₅ (based on Nb content, ) and 0.2 wt% Sr(NO3)2 (based on Sr content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1500 rpm for 35 minutes.
[0063] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 2℃ / min, and the calcination temperature T1 was 640℃. The calcination time was 5 hours; subsequently, the temperature was reduced at a rate of 2℃ / min, with the calcination temperature T2 being 450℃. The calcination time was 8 hours, and the atmosphere was oxygen, to obtain the calcined product;
[0064] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with surface Zr / Nb gradient doping and Sr coating composite modification.
[0065] As shown in Figure 4, the ternary cathode material modified by Nb surface gradient doping and Sr coating has a single crystal morphology, with particle D 50The particle size is about 3.5 μm, and the surface is covered with nanoscale island-like coatings formed by the metal element Sr, with the coating particle size being about 290 nm.
[0066] As shown in Figure 5, EPMA analysis revealed that the surface Zr gradient doping depth was 530 nm, and the surface Nb gradient doping depth was 620 nm. The content of Zr and Nb elements in the doped region gradually decreased from the outside to the inside. The proportion of Zr element in the particle surface depth within 100 nm to the total Zr element content was Wt. surface % = 67%, the proportion of Nb element in the particle surface depth range of 100 nm to the total Nb element content (Wt) surface % = 45%.
[0067] Example 3:
[0068] A method for preparing a ternary cathode material with surface gradient doping and coating composite modification according to the present invention includes the following steps:
[0069] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.75 Co 0.20 Mn 0.04 Sr 0.01 O2, with 0.35 wt% SnO2 (based on Sn content, ) and 0.25 wt% Sb₂O₅ (based on Sb content, ) and 0.6 wt% BaCO3 (based on Ba content, ) and 0.4 wt% Ca(OH)2 (based on Ca content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1100 rpm for 50 min.
[0070] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 5℃ / min, and the calcination temperature T1 was 760℃. The calcination time was 3 hours; subsequently, the temperature was reduced at a rate of 4℃ / min, with the calcination temperature T2 being 420℃. The calcination time was 6 hours, and the atmosphere was oxygen, to obtain the calcined product;
[0071] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with surface Sn / Sb gradient doping and Ba / Ca coating composite modification.
[0072] The ternary cathode material modified by Sn / Sb surface gradient doping and Ba coating has a single-crystal morphology, with particle D 50The particle size is about 4.2 μm, and the surface is covered with metal elements Ba and Ca to form nanoscale island-like coatings, with the coating particle sizes being 370 nm and 280 nm, respectively.
[0073] EPMA analysis revealed that the surface Sn gradient doping depth was 440 nm, and the surface Sb gradient doping depth was 720 nm. The content of Sn and Sb elements in the doped region gradually decreased from the outside to the inside. The proportion of Sn element content (Wt) within a 100 nm depth range on the particle surface relative to the total Sn content was... surface % = 64%, the proportion of Sb element in the particle surface depth range of 100 nm to the total Sb element content (Wt) surface % = 39%.
[0074] Example 4:
[0075] A method for preparing a ternary cathode material with surface gradient doping and coating composite modification according to the present invention includes the following steps:
[0076] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.65 Co 0.07 Mn 0.277 W 0.003 O2, with 0.75 wt% Ta2O5 (based on Ta content, ) and 0.45 wt% K2CO3 (based on K content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1800 rpm for 30 minutes.
[0077] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 6℃ / min, and the calcination temperature T1 was 780℃. The calcination time was 2 hours, followed by a cooling rate of 3℃ / min, with a calcination temperature T2 of 500℃. The calcination time was 7 hours, and the atmosphere was air, to obtain the calcined product;
[0078] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with surface Ta gradient doping and K coating composite modification.
[0079] The ternary cathode material modified by Ta surface gradient doping and K coating has a single crystal morphology, with particles D 50 The particle size is about 4.3 μm, and the surface is covered with nanoscale island-like coatings formed by the metal element K, with the coating particle size being 310 nm.
[0080] EPMA analysis revealed a surface Ta gradient doping depth of 500 nm. The Ta content within the doped region gradually decreased from the outside to the inside. The proportion of Ta within a 100 nm depth on the particle surface (Wt) was the highest among all Ta elements. surface % = 42%.
[0081] Example 5:
[0082] A method for preparing a ternary cathode material with surface gradient doping and coating composite modification according to the present invention includes the following steps:
[0083] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.93 Co 0.4 Mn 0.025 Mg 0.005 O2, and 0.4 wt% (NH4)2MoO4 (based on Mo content, ) and 0.55 wt% SrCO3 (based on Sr content, The mixture is obtained by mixing in a high-speed mixer at a speed of 900 rpm for 60 minutes.
[0084] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 4℃ / min, and the calcination temperature T1 was 580℃. The calcination time was 3 hours, followed by a cooling rate of 2℃ / min, with a calcination temperature T2 of 390℃. The calcination time was 8 hours, and the atmosphere was oxygen, to obtain the calcined product;
[0085] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with surface Mo gradient doping and Sr coating composite modification.
[0086] The ternary cathode material modified by Mo surface gradient doping and Sr coating has a single crystal morphology and particle D 50 The particle size is about 3.1 μm, and the surface is covered with nanoscale island-like coatings formed by the metal element Sr, with the coating particle size being 260 nm.
[0087] EPMA analysis revealed a surface Mo gradient doping depth of 350 nm. The Mo content within the doped region gradually decreased from the outside to the inside. The proportion of Mo in the total Mo content (Wt) within a 100 nm depth region on the particle surface was [not specified]. surface % = 51%.
[0088] Comparative Example 1:
[0089] A method for preparing a ternary cathode material includes the following steps:
[0090] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.85 Co 0.10 Mn 0.045 Al 0.005 O2, with 1 wt% TiO2 (based on Ti content, ) and 0.3 wt% La2O3 (based on La content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1200 rpm for 45 minutes.
[0091] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 5℃ / min, and the calcination temperature T1 was 750℃. The calcination time was 10 hours, and the calcined product was obtained.
[0092] 3) The calcined product is crushed and sieved to obtain a Ti bulk doped and La coated composite modified ternary cathode material.
[0093] As shown in Figure 6, the ternary cathode material modified by Ti bulk doping and La coating has a single crystal morphology, with particle D... 50 The particle size is about 4μm, and the surface is covered with nanoscale island-like coatings formed by the metal element La, with the coating particle size being 170nm.
[0094] As shown in Figure 7, EPMA analysis shows that after sintering at high temperature, Ti elements diffuse into the bulk lattice through thermal diffusion and are uniformly distributed inside the particles.
[0095] Comparative Example 2:
[0096] A method for preparing a ternary cathode material includes the following steps:
[0097] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.85 Co 0.10 Mn 0.045 Al 0.005 O2, and 1 wt% ZnO2 (based on Zn content, ) and 0.3 wt% La2O3 (based on La content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1200 rpm for 45 minutes.
[0098] 2) The mixture was placed in a box furnace for calcination at a temperature of 750℃ for 10 hours, with a heating rate of 5℃ / min and an oxygen atmosphere, to obtain the calcined product.
[0099] 3) The calcined product is crushed and sieved to obtain a ternary cathode material with Zn / La coating modification on the surface.
[0100] As shown in Figure 8, the ternary cathode material modified by Zn and La coating has a single-crystal morphology, and the particle size is D. 50 The particle size is about 4μm, and the surface is covered with nanoscale island-like coatings formed by the metal elements Zn and La, with particle sizes of 430nm and 300nm, respectively.
[0101] As shown in Figure 9, EPMA analysis revealed that Zn elements were distributed on the surface of the material particles in an island-like pattern, with no bulk doping.
[0102] Comparative Example 3:
[0103] A method for preparing a ternary cathode material includes the following steps:
[0104] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.85 Co 0.10 Mn 0.045 Al 0.005 O2, with 1 wt% TiO2 (based on Ti content, ) and 0.3 wt% La2O3 (based on La content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1200 rpm for 45 minutes.
[0105] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 5℃ / min, and the calcination temperature T1 was 750℃. The calcination time was 4 hours, followed by a cooling rate of 3℃ / min, with a calcination temperature T2 of 650℃. The calcination time was 5 hours, and the calcined product was obtained.
[0106] 3) The calcined product is crushed and sieved to obtain a Ti bulk doped and La coated composite modified ternary cathode material.
[0107] As shown in Figure 10, the ternary cathode material modified by Ti surface gradient doping and La coating has a single crystal morphology, with particles D... 50 The particle size is about 4μm, and the surface is covered with nanoscale island-like coatings formed by the metal element La, with the coating particle size being 170nm.
[0108] As shown in Figure 11, EPMA analysis revealed a Ti gradient doping depth of 1740 nm on the surface. The proportion of Ti element within a 100 nm depth range on the particle surface (Wt) is also shown. surface % = 17%.
[0109] Comparative Example 4:
[0110] A method for preparing a ternary cathode material includes the following steps:
[0111] 1) Weigh 10 kg of ternary cathode material matrix LiNi 0.85 Co 0.10 Mn 0.045 Al 0.005 O2, with 1 wt% TiO2 (based on Ti content, ) and 0.3 wt% La2O3 (based on La content, The mixture is obtained by mixing in a high-speed mixer at a speed of 1200 rpm for 45 minutes.
[0112] 2) The mixture was placed in a box furnace for calcination, with the temperature increased at a rate of 5℃ / min, and the calcination temperature T1 was 460℃. The calcination time was 4 hours, followed by a cooling rate of 3℃ / min, with a calcination temperature T2 of 400℃. The calcination time was 5 hours, and the calcined product was obtained.
[0113] 3) The calcined product is crushed and sieved to obtain a Ti bulk doped and La coated composite modified ternary cathode material.
[0114] As shown in Figure 12, the ternary cathode material modified by Ti surface gradient doping and La coating has a single crystal morphology, with particles D... 50 The particle size is about 4μm, and the surface is covered with nanoscale island-like coatings formed by the metal element La, with the coating particle size being 140nm.
[0115] As shown in Figure 13, EPMA analysis revealed a Ti gradient doping depth of 670 nm on the surface. The proportion of Ti element within a 100 nm depth range on the particle surface (Wt) is also shown. surface % = 78%.
[0116] The assembly method for all-solid-state molded batteries is as follows:
[0117] The steps for assembling an all-solid-state mold battery in a glove box protected by an argon atmosphere are as follows: 1) Place the sulfide solid electrolyte Li6PS5Cl powder in a mold and press it into a sheet under pressure; 2) Take the composite-coated ternary cathode material obtained in the above example or the single-coated ternary cathode material obtained in the comparative example, mix it with the solid electrolyte Li6PS5Cl and the conductive agent VGCF in a mass ratio of 70:29:1 to obtain a composite cathode, and then pour the composite cathode into one side of the electrolyte sheet and press it under pressure; 3) Attach the indium sheet and lithium sheet to the other side of the electrolyte sheet in sequence, and then apply pressure; 4) Assemble the mold battery and apply a constant pressure of 50MPa to test its electrochemical performance.
[0118] Electrochemical testing methods:
[0119] The assembled mold battery was placed in a 30°C constant temperature chamber, and the test voltage range was 2.1–3.7V. The first four charge-discharge cycles were 0.1C, 0.2C, 0.33C, and 0.5C, respectively, followed by 50 charge-discharge cycles at a rate of 0.33C. The initial charge-discharge specific capacity, initial coulombic efficiency, and 50-cycle capacity retention of the examples and comparative examples are shown in Table 1 and Figures 14-15.
[0120] Table 1: Test Results of Examples and Comparative Examples
[0121] The results show that the ternary cathode materials prepared in Examples 1-5 of this invention have higher initial charge-discharge efficiency, capacity utilization, and cycle stability compared to Comparative Examples 1-4. This indicates that the surface gradient doping and surface coating composite modification strategy provided by this invention can effectively suppress the space charge layer effect and interfacial side reactions between the ternary cathode material and the sulfide solid electrolyte interface, thereby improving interfacial compatibility.
Claims
1. A ternary cathode material with surface gradient doping and coating composite modification, characterized in that, The surface of the ternary cathode material matrix has a gradient doped region containing element M1, and the surface of the gradient doped region has a coating containing element M2; the ionic radius R of element M1 is... M1 With respect to the nickel ion radius R Ni3+ The relationship between R Ni3+ <R M1 ≤1.3R Ni3+ The ionic radius R of the M2 element M2 With respect to the nickel ion radius R Ni3+ The relationship between R M2 ≥1.3R Ni3+ ,and The depth of the gradient-doped region is within 1000 nm, in the gradient-doped region, the content of the doped M1 element gradually decreases from outside to inside, and the proportion of the content of the M1 element within 100 nm from the surface of the gradient-doped region to the total content of the M1 element is Wt surface % satisfies 30wt% < Wt surface % < 70wt%.
2. The surface gradient doped and coated composite modified ternary cathode material of claim 1, wherein, The mass percentage of element M1 in the ternary cathode material is 0.01–2 wt%, and the mass percentage of element M2 in the ternary cathode material is 0.01–1 wt%.
3. The ternary cathode material with surface gradient doping and coating composite modification according to claim 1, characterized in that, The M1 element includes one or more of Mg, Ti, Co, Ga, Zr, Nb, Mo, Sn, Sb, Ta, and W, and the M2 element includes one or more of Na, K, Ca, Zn, Sr, Y, Ba, La, and Ce.
4. The ternary cathode material with surface gradient doping and coating composite modification according to claim 1, characterized in that, The ternary positive electrode material is single crystal morphology, and the particle D 50 is 2-7 μm.
5. The ternary cathode material with surface gradient doping and coating composite modification according to claim 1, characterized in that, The coating material is island-shaped coated particles with a particle size of 50–500 nm.
6. The ternary cathode material with surface gradient doping and coating composite modification according to any one of claims 1 to 5, characterized in that, The ternary positive electrode material matrix has a chemical formula of LiNi 1-x-y-z Co x Mn y Z z O2, wherein 0.5≤1-x-y-z<1, 0 x≤0.3, 0 y≤0.3, 0 z≤0.01, wherein the Z element comprises one or more of Mg, Al, Ca, Ti, Sr, Zr, Ba, La, W.
7. A method for preparing a ternary cathode material with surface gradient doping and coating composite modification as described in any one of claims 1 to 6, characterized in that, Includes the following steps: 1) Weigh out the ternary cathode material matrix and mix it with an additive containing elements M1 and M2 to obtain a mixture; 2) The mixture is subjected to segmented calcination to obtain the calcined product; 3) The calcined product is crushed and sieved to obtain a ternary cathode material with surface gradient doping and coating composite modification.
8. The method for preparing the ternary cathode material with surface gradient doping and coating composite modification according to claim 7, characterized in that, In step 1), the additive containing elements M1 and M2 is one or more of oxides, hydroxides, carbonates, nitrates, acids and ammonium salts; the mixing machine is used at a speed of 500 to 2000 rpm and the mixing time is 10 to 60 min.
9. The method for preparing the ternary cathode material with surface gradient doping and coating composite modification according to claim 7, characterized in that, In step 2), the segmented calcination includes a first stage and a second stage, wherein the calcination temperature T1 of the first stage and the ionic radius R of element M1 are... M1 satisfy The calcination time is 1–5 h; the calcination temperature T2 in the second stage and the ionic radius R of element M1 are also considered. M1 satisfy The calcination time is 1–8 hours, the heating / cooling rate is 1–10 °C / min, and the calcination atmosphere is oxygen or air.
10. A sulfide all-solid-state battery, characterized in that, It includes the ternary cathode material with surface gradient doping and coating composite modification as described in any one of claims 1 to 6, or the ternary cathode material with surface gradient doping and coating composite modification prepared by the preparation method described in any one of claims 7 to 9.