Polyolefin separator having high heat resistance and high ionic conductivity and preparation method therefor

By combining high-melting-point polyolefin raw materials with antioxidants and nucleating agents, a polyolefin separator with high heat resistance and ionic conductivity is prepared, which solves the problems of thermal shrinkage and insufficient fast-charging performance of lithium-ion batteries at high temperatures, and improves the safety and fast-charging capability of the battery.

WO2026237793A1PCT designated stage Publication Date: 2026-11-19SHANGHAI ENERGY NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/095126
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

When lithium-ion batteries are charged and discharged at high rates and in high-temperature environments, the insufficient heat resistance of the separator can lead to thermal shrinkage, pore blockage, or membrane rupture, increasing the risk of short circuits, failing to interrupt current in time, and causing safety accidents. At the same time, the performance of the separator affects the fast charging performance of the battery.

Method used

Polyolefin membranes are prepared by combining high-melting-point polyolefin raw materials with antioxidants and nucleating agents. The heat resistance and ionic conductivity of the membranes are improved through processes such as premixing, melt extrusion, stretching and heat setting.

Benefits of technology

It improves the heat resistance and ionic conductivity of lithium-ion battery separators, reduces thermal shrinkage, and enhances battery safety and fast-charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2026095126-FTAPPB-I100001
    Figure PCTCN2026095126-FTAPPB-I100001
Patent Text Reader

Abstract

A polyolefin separator and a preparation method therefor, wherein the polyolefin separator is a wet-process separator and comprises: a polyolefin raw material, an antioxidant, and a nucleating agent. The polyolefin resin has a high melting point, and the wet-process separator prepared using same as the main material exhibits a good heat resistance. Moreover, during processing, the antioxidant can substantially reduce the degree of molecular weight of the system, resulting in the melt system exhibiting a good viscoelasticity, thereby substantially improving the processability of the material. In addition, the nucleating agent capable of enhancing the crystallization ability can promote the crystallization of the polyolefin, improve the formation of the pore structure, and reduce the tortuosity of the pores, thereby enabling the separator to have a relatively high ionic conductivity. Therefore, the use of the separator significantly improves the ionic conductivity of a lithium-ion battery separator while providing a good heat resistance thereto.
Need to check novelty before this filing date? Find Prior Art

Description

High heat resistance and high ionic conductivity polyolefin membrane and its preparation method Technical Field

[0001] This invention relates to the field of battery separator technology, and in particular to a polyolefin separator with high heat resistance and high ionic conductivity and its preparation method. Background Technology

[0002] During use, lithium-ion batteries generate heat due to electrochemical reactions, especially during high-rate charging and discharging, high-current operation, and high-temperature environments, where the battery temperature rises significantly. If the separator has poor heat resistance, problems such as thermal shrinkage, pore blockage, or even membrane rupture may occur at high temperatures. Thermal shrinkage may reduce the distance between the positive and negative electrodes, increasing the risk of short circuits; if the pore blockage temperature is too high or the membrane rupture temperature is too low, the current cannot be blocked in time when the battery temperature rises abnormally, leading to thermal runaway and serious safety accidents such as fires and explosions. Therefore, good heat resistance is one of the keys to ensuring the safe and stable operation of lithium-ion batteries.

[0003] Furthermore, with the rapid development of mobile electronic devices and new energy vehicles, the demand for fast-charging performance of lithium-ion batteries is increasing daily. Fast charging can significantly shorten charging time, improve the convenience of device use, and enhance the practicality of electric vehicles. As a key component of the battery, the performance of the separator directly affects the lithium-ion transport rate, and thus the battery's fast-charging performance. Summary of the Invention

[0004] This invention is mainly aimed at wet-process base films used in lithium-ion batteries. By using a high-melting-point main material in combination with auxiliary materials that improve crystallization ability, the wet-process base film can be made to have both good heat resistance and high ionic conductivity.

[0005] The present invention is implemented as follows:

[0006] A polyolefin separator, which is a wet-process separator, comprises: a polyolefin raw material, an antioxidant, and a nucleating agent, wherein the antioxidant is one or more of hindered phenols, phosphites, and thioesters, and the nucleating agent is one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium salt.

[0007] In one embodiment of the present invention, the polyolefin raw material is polypropylene and meets one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm.

[0008] In one embodiment of the present invention, the mass ratio of the antioxidant, the nucleating agent, and the polyolefin raw material is 1:(1 to 3):(30 to 60).

[0009] In one embodiment of the present invention, the antioxidant includes one or more of the following: (1) hindered phenols and (2) phosphites and thioesters.

[0010] In one embodiment of the present invention, when the antioxidant comprises: (1) hindered phenols and (2) phosphites, the mass ratio of the hindered phenols to the phosphites is 1:(1 to 3); when the antioxidant comprises: (1) hindered phenols and (2) thioesters, the mass ratio of the hindered phenols to the thioesters is 1:(1 to 3); when the antioxidant comprises: (1) hindered phenols and (2) phosphites and thioesters, the mass ratio of the hindered phenols to all of the phosphites and thioesters is 1:(1 to 3).

[0011] This invention is also implemented in the same way:

[0012] A method for preparing a polyolefin separator includes: premixing a portion of polyolefin raw materials with an antioxidant to obtain a first premix; premixing a nucleating agent with the first premix to obtain a second premix; premixing another portion of polyolefin raw materials with the second premix to obtain a third premix, and then melt-extruding it with a pore-forming agent to obtain a melt; cooling the melt to obtain a cast sheet, preheating the cast sheet, then stretching the cast sheet longitudinally, and then stretching the cast sheet laterally; extracting the cast sheet, then stretching the cast sheet laterally at a small ratio, and then shrinking the cast sheet laterally at a small ratio; and heat-setting the cast sheet to obtain a polyolefin separator.

[0013] In one embodiment of the present invention, one portion of the polyolefin raw material is polypropylene and satisfies one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm; the other portion of the polyolefin raw material is polypropylene and satisfies one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm.

[0014] In one embodiment of the present invention, the antioxidant is one or more of hindered phenols, phosphites, and thioesters.

[0015] In one embodiment of the present invention, the antioxidant includes one or more of the following: (1) hindered phenols and (2) phosphites and thioesters.

[0016] In one embodiment of the present invention, the nucleating agent is one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium salt.

[0017] In one embodiment of the present invention, the pore-forming agent is one or more of paraffin oil and dioctyl phthalate.

[0018] In one embodiment of the present invention, the mass ratio of the antioxidant, the nucleating agent, the portion of the polyolefin raw material and the entire portion of the polyolefin raw material, to the pore-forming agent is 1:(1 to 3):(30 to 60):(68 to 136).

[0019] In one embodiment of the present invention, the mass ratio of the antioxidant, the nucleating agent, the portion of the polyolefin raw material, the other portion of the polyolefin raw material, and the pore-forming agent is 1:(1 to 3):(10 to 20):(20 to 40):(68 to 136).

[0020] In one embodiment of the present invention, the premixing step of the first premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 4 min to 10 min; the premixing step of the second premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 1 min to 4 min; the premixing step of the third premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 2 min to 5 min.

[0021] In one embodiment of the present invention, the melt extrusion step includes the following conditions: screw temperature of 145°C to 235°C, melt pipe temperature of 190°C to 220°C, and screw speed of 40 rpm to 70 rpm.

[0022] In one embodiment of the present invention, the cooling step includes the following conditions: the cooling temperature is 5°C to 30°C.

[0023] In one embodiment of the present invention, the thickness of the cast sheet is controlled to be between 0.5 mm and 1.5 mm.

[0024] In one embodiment of the present invention, the temperature of the preheating step is ≤ the temperature of the longitudinal stretching step ≤ the temperature of the transverse stretching step ≤ the temperature of the transverse small-ratio stretching step ≤ the temperature of the transverse small-ratio retraction step.

[0025] In one embodiment of the present invention, the stretching ratio of the transverse stretching step is greater than or equal to the stretching ratio of the transverse small-ratio stretching step.

[0026] In one embodiment of the present invention, the temperature of the preheating step is 110°C to 130°C, the temperature of the longitudinal stretching step is 120°C to 140°C, the temperature of the transverse stretching step is 140°C to 160°C, the temperature of the transverse small-ratio stretching step is 145°C to 165°C, and the temperature of the transverse small-ratio retraction step is 145°C to 165°C.

[0027] In one embodiment of the present invention, the stretching ratio of the longitudinal stretching step is 1 to 20 times, the stretching ratio of the transverse stretching step is 1 to 20 times, the stretching ratio of the transverse small-ratio stretching step is 1 to 5 times, and the shrinking ratio of the transverse small-ratio retraction step is 1 to 3 times.

[0028] In one embodiment of the present invention, the temperature of the heat setting step is 140°C to 160°C.

[0029] This invention is implemented in the following way:

[0030] A polyolefin separator that satisfies one or more of the following conditions: porosity ≥ 47.5%, unit needle penetration strength ≥ 48 gf / μm, MD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1 h, TD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1 h, and ionic conductivity ≥ 1.2 mS / cm at 25℃.

[0031] In one embodiment of the present invention, the polyolefin separator is a polypropylene wet-process separator prepared using the polyolefin separator preparation method described above.

[0032] According to the disclosure of this invention, wet-process separators made primarily from high-melting-point polyolefin resins (such as polypropylene resin) exhibit excellent heat resistance. Furthermore, during processing, antioxidants significantly reduce the decrease in molecular weight, resulting in a good viscoelastic state in the melt system and greatly improving the material's processability. Additionally, nucleating agents that enhance crystallization ability promote polyolefin crystallization, improve pore structure formation, reduce pore tortuosity, and thus give the separator higher ionic conductivity. Therefore, the separator using this invention significantly improves the ionic conductivity of lithium-ion battery separators while maintaining excellent heat resistance. Detailed Implementation

[0033] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0034] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0035] The first embodiment of the present invention provides a polyolefin separator, which is a wet-process separator and includes: polyolefin raw material, antioxidant, and nucleating agent.

[0036] The polyolefin membrane preferably meets one or more of the following conditions: porosity ≥ 47.5%, unit needle penetration strength ≥ 48 gf / μm, MD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1 h, TD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1 h, and ionic conductivity ≥ 1.2 mS / cm at 25℃. The porosity is preferably among 47.5%, 47.6%, 47.7%, 47.8%, 47.9%, 48%, 48.1%, 48.2%, 48.3%, 48.4%, 48.5%, 48.6%, 48.7%, 48.8%, 48.9%, 49%, 49.1%, 49.2%, 49.3%, 49.4%, 49.5%, 49.6%, 49.7%, 49.8%, 49.9%, and 50%. The range of any value or any two values; preferably, the needle penetration intensity is 48 gf / μm, 48.2 gf / μm, 48.4 gf / μm, 48.5 gf / μm, 48.6 gf / μm, 48.8 gf / μm, 49 gf / μm, 49.2 gf / μm, 49.4 gf / μm, 49.5 gf / μm, 49.6 gf / μm, 49.8 gf / μm, 50 gf / μm, 50.2 gf / μm, 50 The MD heat shrinkage rate after holding at 130°C for 1 hour is preferably any value or a range between any two values ​​of 0.4 gf / μm, 50.5 gf / μm, 50.6 gf / μm, 50.8 gf / μm, and 51 gf / μm; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, and 0.8%; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0. The concentration is 1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, or a range between any two of these values; the ionic conductivity at 25°C is preferably 1.2 mS / cm, 1.3 mS / cm, 1.4 mS / cm, 1.5 mS / cm, 1.6 mS / cm, 1.7 mS / cm, 1.8 mS / cm, 1.9 mS / cm, 2 mS / cm, or a range between any two of these values. Furthermore, the thickness of the polyolefin membrane is preferably ≤15 μm, more preferably ≤10 μm, and even more preferably 9 μm, 9.1 μm, 9.2 μm, 9.3 μm, 9.4 μm, 9.5 μm, 9.6 μm, 9.7 μm, 9.8 μm, 9.9 μm, 10 μm, or a range between any two of these values.

[0037] In terms of type, polyolefin raw materials are preferably one or more of polyethylene and polypropylene, and more preferably ultra-high molecular weight polypropylene. In terms of properties, polyolefin raw materials preferably meet one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥99.5%, and particle size: D50≤150μm, D90≤200μm. The molecular weight is preferably any value or a range between any two of the following: 1.5 million, 1.55 million, 1.6 million, 1.65 million, 1.7 million, 1.75 million, 1.8 million, 1.85 million, 1.9 million, 1.95 million, 2 million, 2.05 million, 2.1 million, 2.15 million, 2.2 million, 2.25 million, 2.3 million, 2.35 million, 2.4 million, 2.45 million, and 2.5 million; the melt index is preferably any value or a range between any two of the following: 1.0 g / 10 min, 1.1 g / 10 min, 1.2 g / 10 min, 1.3 g / 10 min, 1.4 g / 10 min, 1.5 g / 10 min, 1.6 g / 10 min, 1.7 g / 10 min, 1.8 g / 10 min, 1.9 g / 10 min, and 2.0 g / 10 min; and the isotacticity is preferably 99. 5%, 99.6%, 99.7%, 99.8%, 99.9% or a range between any two of these values; Particle size: D50 is preferably any value or a range between 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm. The range between two values, D90 is preferably any one of 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm, or the range between any two values.

[0038] The antioxidant is preferably one or more of hindered phenols, phosphites, and thioesters, and more preferably includes: (1) hindered phenols and (2) one or more of phosphites and thioesters. Furthermore, hindered phenols include, for example, one or more of antioxidant 1010 and antioxidant 1076; and phosphites include, for example, one or more of antioxidant 168 and antioxidant 626. Furthermore, when the antioxidants include: (1) hindered phenols and (2) phosphites, the mass ratio between hindered phenols and phosphites is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) thioesters, the mass ratio between hindered phenols and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) phosphites and thioesters, the mass ratio between hindered phenols and all of phosphites and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values).

[0039] The nucleating agent is preferably one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium.

[0040] The preferred mass ratio of antioxidant, nucleating agent, and polyolefin raw material is 1:(1 to 3):(30 to 60), more preferably 1:(any value or range between any two of 1, 1.25, 1.5, 1.75, 2, 2.25, 2.5, 2.75, 3):(any value or range between any two of 30, 31.25, 32.5, 35, 37.5, 40, 41.25, 42.5, 45, 47.5, 50, 51.25, 52.5, 55, 57.5, 60).

[0041] In this embodiment, high-melting-point polyolefin is used as the main material, resulting in a wet-process membrane with excellent heat resistance. Furthermore, the antioxidant significantly reduces the decrease in molecular weight, resulting in a good viscoelastic state in the melt system and greatly improving the material's processability. Additionally, the nucleating agent, which enhances crystallization ability, promotes the crystallization of polyolefin, improves pore structure formation, reduces pore tortuosity, and consequently gives the membrane high ionic conductivity.

[0042] The second embodiment of the present invention provides a polyolefin separator that satisfies one or more of the following conditions: porosity ≥ 47.5%, unit needle penetration strength ≥ 48 gf / μm, MD heat shrinkage rate ≤ 0.8% after holding at 130°C for 1 h, TD heat shrinkage rate ≤ 0.8% after holding at 130°C for 1 h, and ionic conductivity ≥ 1.2 mS / cm at 25°C. The porosity is preferably among 47.5%, 47.6%, 47.7%, 47.8%, 47.9%, 48%, 48.1%, 48.2%, 48.3%, 48.4%, 48.5%, 48.6%, 48.7%, 48.8%, 48.9%, 49%, 49.1%, 49.2%, 49.3%, 49.4%, 49.5%, 49.6%, 49.7%, 49.8%, 49.9%, and 50%. The range of any value or any two values; preferably, the needle penetration intensity is 48 gf / μm, 48.2 gf / μm, 48.4 gf / μm, 48.5 gf / μm, 48.6 gf / μm, 48.8 gf / μm, 49 gf / μm, 49.2 gf / μm, 49.4 gf / μm, 49.5 gf / μm, 49.6 gf / μm, 49.8 gf / μm, 50 gf / μm, 50.2 gf / μm, 50 The MD heat shrinkage rate after holding at 130°C for 1 hour is preferably any value or a range between any two values ​​of 0.4 gf / μm, 50.5 gf / μm, 50.6 gf / μm, 50.8 gf / μm, and 51 gf / μm; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, and 0.8%; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0. The concentration is 1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, or a range between any two of these values; the ionic conductivity at 25°C is preferably 1.2 mS / cm, 1.3 mS / cm, 1.4 mS / cm, 1.5 mS / cm, 1.6 mS / cm, 1.7 mS / cm, 1.8 mS / cm, 1.9 mS / cm, 2 mS / cm, or a range between any two of these values. Furthermore, the thickness of the polyolefin membrane is preferably ≤15 μm, more preferably ≤10 μm, and even more preferably 9 μm, 9.1 μm, 9.2 μm, 9.3 μm, 9.4 μm, 9.5 μm, 9.6 μm, 9.7 μm, 9.8 μm, 9.9 μm, 10 μm, or a range between any two of these values.

[0043] The polyolefin membrane is preferably a wet-process membrane and comprises: a polyolefin raw material, an antioxidant, and a nucleating agent. In terms of type, the polyolefin raw material is preferably one or more of polyethylene and polypropylene, more preferably ultra-high molecular weight polypropylene. When the polyolefin raw material is polyethylene, the polyolefin membrane is preferably a polyethylene wet-process membrane; when the polyolefin raw material is polypropylene, the polyolefin membrane is preferably a polypropylene wet-process membrane. In terms of properties, the polyolefin raw material preferably meets one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm. The molecular weight is preferably any value or a range between any two of the following: 1.5 million, 1.55 million, 1.6 million, 1.65 million, 1.7 million, 1.75 million, 1.8 million, 1.85 million, 1.9 million, 1.95 million, 2 million, 2.05 million, 2.1 million, 2.15 million, 2.2 million, 2.25 million, 2.3 million, 2.35 million, 2.4 million, 2.45 million, and 2.5 million; the melt index is preferably any value or a range between any two of the following: 1.0 g / 10 min, 1.1 g / 10 min, 1.2 g / 10 min, 1.3 g / 10 min, 1.4 g / 10 min, 1.5 g / 10 min, 1.6 g / 10 min, 1.7 g / 10 min, 1.8 g / 10 min, 1.9 g / 10 min, and 2.0 g / 10 min; and the isotacticity is preferably 99. 5%, 99.6%, 99.7%, 99.8%, 99.9% or a range between any two of these values; Particle size: D50 is preferably any value or a range between 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm. The range between two values, D90 is preferably any one of 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm, or the range between any two values.

[0044] The antioxidant is preferably one or more of hindered phenols, phosphites, and thioesters, and more preferably includes: (1) hindered phenols and (2) one or more of phosphites and thioesters. Furthermore, hindered phenols include, for example, one or more of antioxidant 1010 and antioxidant 1076; and phosphites include, for example, one or more of antioxidant 168 and antioxidant 626. Furthermore, when the antioxidants include: (1) hindered phenols and (2) phosphites, the mass ratio between hindered phenols and phosphites is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) thioesters, the mass ratio between hindered phenols and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) phosphites and thioesters, the mass ratio between hindered phenols and all of phosphites and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values).

[0045] The nucleating agent is preferably one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium.

[0046] The preferred mass ratio of antioxidant, nucleating agent, and polyolefin raw material is 1:(1 to 3):(30 to 60), more preferably 1:(any value or range between any two of 1, 1.25, 1.5, 1.75, 2, 2.25, 2.5, 2.75, 3):(any value or range between any two of 30, 31.25, 32.5, 35, 37.5, 40, 41.25, 42.5, 45, 47.5, 50, 51.25, 52.5, 55, 57.5, 60).

[0047] The third embodiment of the present invention provides a method for preparing a polyolefin separator. This method can be used to prepare the polyolefin separators proposed in the first and second embodiments, but should not be used to limit this method.

[0048] First, a portion of the polyolefin raw material is premixed with an antioxidant to obtain a first premix. In terms of type, the polyolefin raw material used here is preferably one or more of polyethylene and polypropylene, more preferably ultra-high molecular weight polypropylene. In terms of properties, the polyolefin raw material used here preferably meets one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm. The molecular weight is preferably any value or a range between any two of the following: 1.5 million, 1.55 million, 1.6 million, 1.65 million, 1.7 million, 1.75 million, 1.8 million, 1.85 million, 1.9 million, 1.95 million, 2 million, 2.05 million, 2.1 million, 2.15 million, 2.2 million, 2.25 million, 2.3 million, 2.35 million, 2.4 million, 2.45 million, and 2.5 million; the melt index is preferably any value or a range between any two of the following: 1.0 g / 10 min, 1.1 g / 10 min, 1.2 g / 10 min, 1.3 g / 10 min, 1.4 g / 10 min, 1.5 g / 10 min, 1.6 g / 10 min, 1.7 g / 10 min, 1.8 g / 10 min, 1.9 g / 10 min, and 2.0 g / 10 min; and the isotacticity is preferably 99. 5%, 99.6%, 99.7%, 99.8%, 99.9% or a range between any two of these values; Particle size: D50 is preferably any value or a range between 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm. The range between the two values, D90 is preferably any value or a range between any two values ​​selected from 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, and 200 μm. The antioxidant is preferably one or more of hindered phenols, phosphites, and thioesters, more preferably including: (1) hindered phenols and (2) one or more of phosphites and thioesters. Furthermore, hindered phenols include, for example, one or more of antioxidant 1010 and antioxidant 1076; and phosphites include, for example, one or more of antioxidant 168 and antioxidant 626.Furthermore, when the antioxidants include: (1) hindered phenols and (2) phosphites, the mass ratio between hindered phenols and phosphites is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) thioesters, the mass ratio between hindered phenols and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values); when the antioxidants include: (1) hindered phenols and (2) phosphites and thioesters, the mass ratio between hindered phenols and all of phosphites and thioesters is preferably 1:(1 to 3), more preferably 1:(any value of 1, 1.5, 2, 2.5, 3 or a range between any two values). The premixing process here is preferably carried out under one or more of the following conditions: a mixing temperature of 30°C to 70°C, a mixing speed of 30 rpm to 40 rpm, and a mixing time of 4 min to 10 min. More preferably, the mixing temperature is any value or a range between any two of the following: 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, and 70°C; more preferably, the mixing speed is any value or a range between any two of the following: 30 rpm, 32.5 rpm, 35 rpm, 37.5 rpm, 40 rpm, 42.5 rpm, 45 rpm, 47.5 rpm, and 50 rpm; and more preferably, the mixing time is any value or a range between any two of the following: 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, and 10 min.

[0049] Next, the nucleating agent is premixed with the first premix to obtain a second premix. The nucleating agent is preferably one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and sodium 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate. The premixing process is preferably carried out under one or more of the following conditions: a mixing temperature of 30°C to 70°C, a mixing speed of 30 rpm to 40 rpm, and a mixing time of 1 min to 4 min. The mixing temperature is preferably any one of 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, or a range between any two of these values; the mixing speed is preferably any one of 30rpm, 32.5rpm, 35rpm, 37.5rpm, 38rpm, 40rpm, 42.5rpm, 45rpm, 47.5rpm, 48rpm, 50rpm, or a range between any two of these values; and the mixing time is preferably any one of 1min, 1.5min, 2min, 2.5min, 3min, 3.5min, 4min, or a range between any two of these values.

[0050] Next, another portion of the polyolefin raw material is premixed with the second premix to obtain a third premix, which is then melt-extruded with a pore-forming agent to obtain a melt. In terms of type, the polyolefin raw material used here is preferably one or more of polyethylene and polypropylene, more preferably ultra-high molecular weight polypropylene. In terms of properties, the polyolefin raw material used here preferably meets one or more of the following conditions: molecular weight of 1.5 million to 2.5 million, melt index of 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm. The molecular weight is preferably any value or a range between any two of the following: 1.5 million, 1.55 million, 1.6 million, 1.65 million, 1.7 million, 1.75 million, 1.8 million, 1.85 million, 1.9 million, 1.95 million, 2 million, 2.05 million, 2.1 million, 2.15 million, 2.2 million, 2.25 million, 2.3 million, 2.35 million, 2.4 million, 2.45 million, and 2.5 million; the melt index is preferably any value or a range between any two of the following: 1.0 g / 10 min, 1.1 g / 10 min, 1.2 g / 10 min, 1.3 g / 10 min, 1.4 g / 10 min, 1.5 g / 10 min, 1.6 g / 10 min, 1.7 g / 10 min, 1.8 g / 10 min, 1.9 g / 10 min, and 2.0 g / 10 min; and the isotacticity is preferably 99. 5%, 99.6%, 99.7%, 99.8%, 99.9% or a range between any two of these values; Particle size: D50 is preferably any value or a range between 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm. The range between the two values, D90 is preferably any one of 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, and 200μm, or a range between any two values. The premixing process is preferably carried out under one or more of the following conditions: a mixing temperature of 30°C to 70°C, a mixing speed of 30 rpm to 40 rpm, and a mixing time of 2 min to 5 min.The mixing temperature is preferably any one of 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, or a range between any two of these values; the mixing speed is preferably any one of 30rpm, 32.5rpm, 35rpm, 37.5rpm, 40rpm, 42.5rpm, 45rpm, 47.5rpm, 50rpm, or a range between any two of these values; and the mixing time is preferably any one of 2min, 2.5min, 3min, 3.5min, 4min, 4.5min, 5min, or a range between any two of these values.

[0051] In terms of type, the pore-forming agent is preferably one or more of paraffin oil and dioctyl phthalate. In terms of properties, the kinematic viscosity of the pore-forming agent at 40°C is preferably between 40 cSt and 80 cSt, more preferably within any value or a range between any two of 40 cSt, 45 cSt, 50 cSt, 55 cSt, 60 cSt, 65 cSt, 70 cSt, 75 cSt, and 80 cSt. The melt extrusion process is preferably carried out under one or more of the following conditions: screw temperature of 145°C to 235°C, melt pipe temperature of 190°C to 220°C, and screw speed of 40 rpm to 70 rpm. The screw temperature is preferably any value or a range between any two of the following: 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 225°C, 230°C, and 235°C; the melt pipe temperature is preferably any value or a range between any two of the following: 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, and 220°C; and the screw speed is preferably any value or a range between any two of the following: 40 rpm, 45 rpm, 50 rpm, 55 rpm, 60 rpm, 65 rpm, and 70 rpm. Furthermore, the melt extrusion process is preferably carried out in a twin-screw extruder.

[0052] The mass ratio of antioxidant, nucleating agent, total of pre-added and post-added polyolefin raw materials, and pore-forming agent is preferably 1:(1 to 3):(30 to 60):(68 to 136), more preferably 1:(any value or range between any two of 1, 1.25, 1.5, 1.75, 2, 2.25, 2.5, 2.75, 3):(any value or range between any two of 30, 31.25, 32.5, 35, 37.5, 40, 41.25, 42.5, 45, 47.5, 50, 51.25, 52.5, 55, 57.5, 60). (Any value or a range between any two values ​​from 68, 70, 71.25, 72, 74, 75, 76, 78, 80, 81.25, 82, 84, 85, 86, 88, 90, 91.25, 92, 94, 95, 96, 98, 100, 101.25, 102, 104, 105, 106, 108, 110, 111.25, 112, 114, 115, 116, 118, 120, 121.25, 122, 124, 125, 126, 128, 130, 131.25, 132, 134, 135, 136). Furthermore, the preferred mass ratio of antioxidant, nucleating agent, pre-added polyolefin raw material, post-added polyolefin raw material, and pore-forming agent is 1:(1 to 3):(10 to 20):(20 to 40):(68 to 136), more preferably 1:(any value or range between any two of 1, 1.25, 1.5, 1.75, 2, 2.25, 2.5, 2.75, 3):(any value or range between any two of 10, 12.5, 15, 17.5, 18.75, 20, 22.5, 25, 27.5, 28.75, 30):(20, 22.5, 25, 27.5, 30, 32.5, 35, 37.5) (Any value or any two values ​​between any two of the following: 68, 70, 71.25, 72, 74, 75, 76, 78, 80, 81.25, 82, 84, 85, 86, 88, 90, 91.25, 92, 94, 95, 96, 98, 100, 101.25, 102, 104, 105, 106, 108, 110, 111.25, 112, 114, 115, 116, 118, 120, 121.25, 122, 124, 125, 126, 128, 130, 131.25, 132, 134, 135, 136).

[0053] Then, after cooling the melt to obtain a cast sheet, the cast sheet is first preheated, then stretched longitudinally, and then stretched transversely. The cooling process is preferably carried out under the following conditions: a cooling temperature of 5°C to 30°C; more preferably, a cooling temperature within the range of any two of the following values: 5°C, 7.5°C, 10°C, 12.5°C, 15°C, 17.5°C, 20°C, 22.5°C, 25°C, 27.5°C, 30°C. The cast sheet thickness is preferably controlled between 0.5 mm and 1.5 mm, more preferably within the range of any two of the following values: 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm. From the perspective of relative temperature relationships, the following conditions are preferably met: preheating temperature ≤ longitudinal stretching temperature ≤ transverse stretching temperature; more preferably, preheating temperature = longitudinal stretching temperature < transverse stretching temperature. From the perspective of absolute temperature relationships, the preheating temperature is preferably between 110℃ and 130℃, more preferably any value or a range between any two of 110℃, 115℃, 120℃, 125℃, and 130℃; the longitudinal stretching temperature is preferably between 120℃ and 140℃, more preferably any value or a range between any two of 120℃, 125℃, 130℃, 135℃, and 140℃; the transverse stretching temperature... The temperature during the stretching process is preferably between 140°C and 160°C, and more preferably any value or a range between any two of the following: 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, 151°C, 152°C, 153°C, 154°C, 155°C, 156°C, 157°C, 158°C, 159°C, and 160°C. Furthermore, the stretching ratio during the longitudinal stretching process is preferably between 1 and 20 times, more preferably between any two of the following values: 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20 times. The stretching ratio during the transverse stretching process is preferably between 1 and 20 times, more preferably between any two of the following values: 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, and 20 times.

[0054] Furthermore, after extraction and casting, the cast sheet is first stretched laterally at a small magnification, and then retracted laterally at a small magnification. Dichloromethane is preferably used in the extraction process. From a relative temperature perspective, the following conditions are preferably met: the temperature of the laterally stretched sheet at a small magnification ≤ the temperature of the laterally retracted sheet at a small magnification; more preferably, the temperature of the laterally stretched sheet at a small magnification < the temperature of the laterally retracted sheet at a small magnification. Again, from a relative temperature perspective, the following conditions are preferably met: the temperature of the preheating process ≤ the temperature of the longitudinal stretching process ≤ the temperature of the transverse stretching process ≤ the temperature of the laterally stretched sheet at a small magnification ≤ the temperature of the laterally retracted sheet at a small magnification; more preferably, the temperature of the preheating process = the temperature of the longitudinal stretching process < the temperature of the transverse stretching process = the temperature of the laterally stretched sheet at a small magnification < the temperature of the laterally retracted sheet at a small magnification. From the perspective of absolute temperature relationships, the optimal temperature range for the transverse small-ratio stretching process is 145℃ to 165℃, more preferably any value or a range between any two of the following: 145℃, 147℃, 149℃, 151℃, 153℃, 155℃, 157℃, 159℃, 161℃, 163℃, and 165℃. Similarly, the optimal temperature range for the transverse small-ratio shrinkage process is 145℃ to 165℃, more preferably any value or a range between any two of the following: 145℃, 150℃, 155℃, and 160℃. Furthermore, from the perspective of relative stretching ratios, the optimal condition is that the stretching ratio of the transverse stretching process is ≥ the stretching ratio of the transverse small-ratio stretching process, and more preferably, the stretching ratio of the transverse stretching process is > the stretching ratio of the transverse small-ratio stretching process. From the perspective of the absolute relationship of stretching ratio, the stretching ratio in the transverse low-ratio stretching process is preferably 1 to 5 times, and more preferably any value or any two values ​​among 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, and 5 times. The range of the horizontal small-scale retraction process is preferably 1 to 3 times, more preferably any value or any two values ​​between 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, and 3 times.

[0055] Finally, the heat-set casting yields a polyolefin separator. The temperature during the heat-setting process is preferably between 140°C and 160°C, more preferably any value or a range between any two of the following: 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C, and 160°C. The polyolefin separator preferably satisfies one or more of the following conditions: porosity ≥ 47.5%, unit needle penetration strength ≥ 48 gf / μm, MD heat shrinkage rate ≤ 0.8% after holding at 130°C for 1 hour, TD heat shrinkage rate ≤ 0.8% after holding at 130°C for 1 hour, and ionic conductivity ≥ 1.2 mS / cm at 25°C. The porosity is preferably among 47.5%, 47.6%, 47.7%, 47.8%, 47.9%, 48%, 48.1%, 48.2%, 48.3%, 48.4%, 48.5%, 48.6%, 48.7%, 48.8%, 48.9%, 49%, 49.1%, 49.2%, 49.3%, 49.4%, 49.5%, 49.6%, 49.7%, 49.8%, 49.9%, and 50%. The range of any value or any two values; preferably, the needle penetration intensity is 48 gf / μm, 48.2 gf / μm, 48.4 gf / μm, 48.5 gf / μm, 48.6 gf / μm, 48.8 gf / μm, 49 gf / μm, 49.2 gf / μm, 49.4 gf / μm, 49.5 gf / μm, 49.6 gf / μm, 49.8 gf / μm, 50 gf / μm, 50.2 gf / μm, 50 The MD heat shrinkage rate after holding at 130°C for 1 hour is preferably any value or a range between any two values ​​of 0.4 gf / μm, 50.5 gf / μm, 50.6 gf / μm, 50.8 gf / μm, and 51 gf / μm; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, and 0.8%; the TD heat shrinkage rate after holding at 130°C for 1 hour is preferably 0. The concentration is 1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, or a range between any two of these values; the ionic conductivity at 25°C is preferably 1.2 mS / cm, 1.3 mS / cm, 1.4 mS / cm, 1.5 mS / cm, 1.6 mS / cm, 1.7 mS / cm, 1.8 mS / cm, 1.9 mS / cm, 2 mS / cm, or a range between any two of these values. Furthermore, the thickness of the polyolefin membrane is preferably ≤15 μm, more preferably ≤10 μm, and even more preferably 9 μm, 9.1 μm, 9.2 μm, 9.3 μm, 9.4 μm, 9.5 μm, 9.6 μm, 9.7 μm, 9.8 μm, 9.9 μm, 10 μm, or a range between any two of these values.

[0056] In this embodiment, a wet-process membrane is prepared using polyolefin resin (e.g., ultra-high molecular weight polypropylene) and a pore-forming agent as the main components, combined with a nucleating agent and an antioxidant. After staged premixing, the membrane is extruded using a twin-screw extruder, cast, stretched, extracted, and heat-treated. The resulting membrane exhibits good heat resistance and high ionic conductivity. Specifically, the high melting point of ultra-high molecular weight polyolefin resin contributes to the excellent heat resistance of the wet-process membrane. The nucleating agent, acting as a heterogeneous nucleation point, significantly enhances the crystallization rate and density of the polyolefin, inducing the ordered arrangement of polyolefin molecular chains to form a finer spherulite structure. This refined crystal structure reduces light scattering, improving membrane uniformity and thermal stability. The small particle size of the polyolefin allows for more uniform dispersion in the solvent, resulting in a microporous structure with smaller pore size and narrower distribution through the wet process. The small-particle-size polyolefin, combined with the nucleating agent, significantly increases the melting point and heat distortion temperature of the membrane by improving crystallinity. For example, the melting point of polypropylene can be increased from 160°C in pure polypropylene to over 165°C, suppressing high-temperature shrinkage. Furthermore, it forms a dense and uniform pore structure to reduce the tortuosity of ion transport paths, improve electrolyte wettability, thereby reducing internal resistance and increasing ionic conductivity.

[0057] In addition, during the processing of the main polyolefin material, hindered phenols are used as the primary antioxidants, and phosphites or thioesters as secondary antioxidants. The hindered phenolic primary antioxidant interrupts the oxidation chain reaction by capturing free radicals, while the phosphites or thioesters further block the oxidation reaction by decomposing hydrogen peroxide. The combination of these two antioxidants creates a synergistic effect, covering different stages of oxidative degradation, thereby significantly improving overall antioxidant efficiency. High-temperature processing may cause fluctuations in the viscosity of the polyolefin melt. The combined use of antioxidants can maintain stable melt flowability by inhibiting oxidation reactions and reducing processing defects (such as bubbles and crystal points). Thioester secondary antioxidants exhibit excellent hydrolytic stability in wet processes and are suitable for processing environments containing solvents (such as paraffin oil), reducing the risk of antioxidant extraction by solvents or hydrolytic failure. Wet-processed membranes require solvent extraction and biaxial stretching steps; the combined antioxidants can balance solvent resistance and thermal stability.

[0058] The process employs a staged premixing approach. By initially mixing a small amount of polyolefin with antioxidants, the anchoring effect of the antioxidants in the matrix is ​​preferentially established, preventing migration or agglomeration of the antioxidants due to insufficient molecular chain entanglement during the subsequent high-temperature melting stage. When nucleating agents are added later, the network framework formed by the premixed polyolefin system facilitates the uniform distribution of the nucleating agents within the matrix. The staged addition of different components allows for gradual adjustment of the melt rheological properties. The antioxidants introduced first (such as hindered phenols) form a hydrogen bond network with the polyolefin molecular chains during the premixing stage. This not only inhibits thermal degradation but also serves as an auxiliary nucleation site, increasing the crystallization temperature by 5°C to 8°C and enhancing the high-temperature dimensional stability of the membrane. The nucleating agent added later preferentially contacts the high-purity polyolefin matrix, avoiding competitive adsorption with the subsequent pore-forming agent. This ensures an ordered crystal structure control mechanism and effectively improves the orientation consistency of the microporous structure in the subsequent stretching process. The pore-forming agent is added in the final stage, which can utilize the shear field established by the preceding premixing system to achieve more uniform liquid-solid phase dispersion and reduce the closed-cell defect rate during the subsequent phase separation process.

[0059] The invention is illustrated by way of example using the following embodiments:

[0060] Example 1

[0061] Polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) accounting for 10% of the mass percentage of the subsequently obtained melt and antioxidant (a mixture of antioxidants 1010 and 626 at a mass ratio of 1:2) were premixed in a ribbon mixer (50 °C, 35 rpm, 5 min).

[0062] Subsequently, nucleating agent 2,2'-methylene-bis(4,6-di-tert-butylphenylphosphine) basic aluminum, accounting for 1.2% of the mass of the resulting melt, was added and premixed in a ribbon mixer (50°C, 35 rpm, 2 min).

[0063] Then, 20% of the mass percentage of the subsequently obtained melt is added to polypropylene powder (molecular weight of 1.5 million, melt index of 1.0 g / 10 min, isotacticity of 99.8%, particle size: D50 of 150 μm, D90 of 180 μm) for premixing (50℃, 35 rpm, 3 min). Subsequently, it is melt-extruded with 68% of the mass percentage of the subsequently obtained melt to obtain a melt. The melt extrusion is carried out by twin-screw extrusion, with the screw temperature at 220℃, the melt pipe temperature at 210℃, and the screw speed at 45 rpm.

[0064] After the melt flows out of the die, it immediately contacts the cooling roller to cool and obtain a casting sheet, wherein the cooling temperature is 10℃ and the thickness of the casting sheet is controlled to be 1mm.

[0065] After preheating the cast sheet to 130℃, it is first stretched longitudinally at 130℃ with a stretching ratio of 7x. Then, it is stretched transversely at 147℃ with a stretching ratio of 7x. After extracting the cast sheet with dichloromethane, it is first stretched transversely at a small ratio of 1.2x at 147℃. Next, it is retracted transversely at a small ratio of 1.1x at 150℃.

[0066] A polypropylene diaphragm is obtained by heat-setting a casting sheet, wherein the heat-setting temperature is 140℃.

[0067] Example 2

[0068] Similar to Example 1, except that "10% by mass of the subsequently obtained melt polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) and 0.8% by mass of antioxidant (a mixture of antioxidants 1010 and 626, in a mass ratio of 1:2) were premixed in a ribbon mixer (50°C, 35 rpm, 5 min)" is replaced with "10% by mass of the subsequently obtained melt polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm)" The phrase “90 (180 μm) and 1% by mass of antioxidant (a mixture of antioxidant 1010 and 626 at a mass ratio of 1:1.5) were premixed in a ribbon mixer (50°C, 35 rpm, 6 min),” and “subsequently, 1.2% by mass of nucleating agent 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum was added and premixed in a ribbon mixer (50°C, 35 rpm, 2 min)” is replaced with “subsequently, 1% by mass of nucleating agent (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt was added and premixed in a ribbon mixer (50°C, 38 rpm, 1.5 min)”.

[0069] Example 3

[0070] Similar to Example 1, except that "10% by mass of the subsequently obtained melt polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) and 0.8% by mass of antioxidant (a mixture of antioxidants 1010 and 626, in a mass ratio of 1:2) were premixed in a ribbon mixer (50°C, 35 rpm, 5 min)" is replaced with "10% by mass of the subsequently obtained melt polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm)" The phrase “90 (180 μm) and 0.5% by mass of antioxidant (a mixture of antioxidants 1010 and 626 in a mass ratio of 1:3) were premixed in a ribbon mixer (50°C, 35 rpm, 4 min), and “then 1.2% by mass of nucleating agent 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum was added and premixed in a ribbon mixer (50°C, 35 rpm, 2 min)” is replaced with “then 1.5% by mass of nucleating agent 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium was added and premixed in a ribbon mixer (55°C, 40 rpm, 3 min).”

[0071] Example 4

[0072] Similar to Example 1, except that "10% by mass of the resulting melt polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) and 0.8% by mass of antioxidant (a mixture of antioxidants 1010 and 626, mass ratio 1:2) were mixed in a ribbon mixer (50°C, 35 rpm, 5 min)". "Premix" is replaced by "premixing polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) at 10% by mass of the subsequently obtained melt with antioxidant (a mixture of antioxidants 1010 and 168 at a mass ratio of 1:2) in a ribbon mixer (50°C, 35 rpm, 5 min)".

[0073] Example 5

[0074] Similar to Example 1, except that "premixing 10% by mass of polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm) and 0.8% by mass of antioxidant (a mixture of antioxidants 1010 and 626, mass ratio 1:2) in a ribbon mixer (50°C, 35 rpm, 5 min)" is replaced with "premixing 10% by mass of the subsequently obtained melt..." "15% polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 140 μm, D90 200 μm) and 0.8% antioxidant (a mixture of antioxidants 1010 and 626, mass ratio 1:2) were premixed in a ribbon mixer (50℃, 35 rpm, 5 min), and then 20% polypropylene powder (molecular weight 1.5 million) was added as the mass percentage of the subsequently obtained melt." The mixture (with a melt index of 1.0 g / 10 min, isotacticity of 99.8%, and particle size of D50 of 150 μm and D90 of 180 μm) was premixed (50℃, 35 rpm, 3 min). Then, it was melt-extruded with 68% (by mass) of pore-forming agent 68# white oil to obtain the melt. The melt extrusion was performed using a twin-screw extruder with a screw temperature of 220℃, a melt pipe temperature of 210℃, and a screw speed of 45 rpm. The mixture was then replaced with a further percentage (by mass) of pore-forming agent 68# white oil. 18% polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 140 μm, D90 200 μm) was premixed (50℃, 40 rpm, 5 min), and then melt-extruded with 65% of the pore-forming agent 68# white oil, which accounted for 65% of the mass of the resulting melt, to obtain a melt. The melt extrusion was carried out using a twin-screw extruder with a screw temperature of 220℃, a melt pipe temperature of 210℃, and a screw speed of 45 rpm.

[0075] Comparative Example 1

[0076] The melt was obtained by melt extrusion of 30% polypropylene powder (molecular weight 1.5 million, melt index 1.0 g / 10 min, isotacticity 99.8%, particle size: D50 150 μm, D90 180 μm), 0.8% antioxidant (a mixture of antioxidants 1010 and 626 in a mass ratio of 1:2), 1.2% nucleating agent 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 68% pore-forming agent 68# white oil. The melt extrusion was carried out using a twin-screw extruder with a screw temperature of 220°C, a melt pipe temperature of 210°C, and a screw speed of 45 rpm.

[0077] After the melt flows out of the die, it immediately contacts the cooling roller to cool and obtain a casting sheet, wherein the cooling temperature is 10℃ and the thickness of the casting sheet is controlled to be 1mm.

[0078] After preheating the cast sheet to 130℃, it is first stretched longitudinally at 130℃ with a stretching ratio of 7x. Then, it is stretched transversely at 147℃ with a stretching ratio of 7x. After extracting the cast sheet with dichloromethane, it is first stretched transversely at a small ratio of 1.2x at 147℃. Next, it is retracted transversely at a small ratio of 1.1x at 150℃.

[0079] A polypropylene diaphragm is obtained by heat-setting a casting sheet, wherein the heat-setting temperature is 140℃.

[0080] Comparative Example 2

[0081] Similar to Example 1, except that the main material added before and after the experiment was replaced with polyethylene instead of polypropylene.

[0082] Comparative Example 3

[0083] Similar to Example 2, except that the main material added before and after the experiment was replaced with polyethylene instead of polypropylene.

[0084] Comparative Example 4

[0085] Similar to Example 3, except that the main material added before and after the experiment was replaced with polyethylene instead of polypropylene.

[0086] Thickness test

[0087] Standard: GB / T 6672-2001 Mechanical Measurement Method for Determination of Thickness of Plastic Films and Sheets.

[0088] Test method:

[0089] Using a high-precision thickness gauge, perform at least three sets of tests at equal intervals along the transverse direction and one set of tests every 200 mm along the longitudinal direction, for a total of five sets of tests. Calculate the average value as the thickness of the diaphragm.

[0090] Porosity test

[0091] Standard: GB / T 36363-2018 "Polyolefin separators for lithium-ion batteries".

[0092] Unit needle penetration intensity test

[0093] Standard: GB / T 36363-2018.

[0094] Test method:

[0095] The lithium battery separator is laid flat in the tensile testing machine fixture and clamped. Puncture is performed at a rate of (100±10) mm / min. After completion, the sample is removed and the thickness is tested at 4 points around the needle hole according to the provisions of GB / T 6672-2001. The average value is taken and the puncture strength is calculated according to the formula.

[0096] Heat shrinkage test

[0097] Standard: GB / T 36363-2018.

[0098] Test method:

[0099] Three 100mm×100mm square diaphragms are cut from the longitudinal direction of the membrane roll. If the diaphragm width is less than 100mm, the sample size is 100mm×diaphragm width.

[0100] Place the sample flat between two frames embedded with metal mesh, ensuring that the distance between the two metal meshes is maintained between 1 mm and 3 mm.

[0101] According to the test requirements, set the test temperature and time (e.g., 130℃, 1h), and ensure that there is an appropriate amount of heat transfer medium (e.g., glycerin) in the heating tank and that the temperature reaches the set value and remains stable.

[0102] Quickly immerse the frame containing the sample into the isothermal medium at the set temperature and start timing. Allow the sample to contract freely in the isothermal medium for a period of time (e.g., 20 seconds), then remove it.

[0103] Ion conductivity test

[0104] Standard: GB / T 36363-2018 "Polyolefin Separators for Lithium-ion Batteries"

[0105] Test method:

[0106] During testing, a diaphragm sample matching the resistance testing mold is cut, and the diaphragm is placed in an electrolyte with a concentration of 1 mol / L and tested according to the conditions specified in the standard.

[0107] As shown in Table 1, the graded premixing method can improve the porosity, unit needle penetration strength, heat shrinkage rate, and ionic conductivity of the polyolefin membrane (comparative Examples 1 to 5 with Comparative Example 1). Furthermore, compared to polyethylene membranes, the graded premixing method can improve the porosity, heat shrinkage rate, and ionic conductivity of polypropylene membranes (comparative Examples 1 and 2, 2 and 3, 3 and 4).

[0108] Further analysis of the experimental data in Table 1 shows that the polyolefin wet-process separator prepared based on the process of this invention achieves synergistic optimization of the micropore structure by controlling phase separation kinetics and crystallization behavior. The resulting polyolefin exhibits high ionic conductivity (25℃) while maintaining thermal dimensional stability at 130℃, which is higher than that of traditional wet-process polyolefin separators. This synergistic enhancement effect of heat resistance and high ionic conductivity not only effectively suppresses the risk of thermal runaway caused by lithium dendrite penetration, but its optimized three-dimensional interconnected pore structure also shortens the electrolyte wetting time, providing a key solution for charge transport kinetics under high-rate charge and discharge conditions. This technological breakthrough marks a significant advancement in the unification of high safety and fast-charging performance in lithium-ion batteries.

[0109] Table 1

[0110] The above content involving common knowledge will not be described in detail, as those skilled in the art will understand.

[0111] The above descriptions are merely some specific embodiments of the present invention and are not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A polyolefin separator characterized by, The membrane is a wet-process membrane and includes: a polyolefin raw material, an antioxidant, and a nucleating agent. The antioxidant is one or more of hindered phenols, phosphites, and thioesters. The nucleating agent is one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium salt.

2. The polyolefin separator according to claim 1, characterized by, The polyolefin raw material is polypropylene and meets one or more of the following conditions: molecular weight below 2.5 million, melt index from 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm.

3. The polyolefin separator according to claim 1, characterized by, The mass ratio of the antioxidant, the nucleating agent, and the polyolefin raw material is 1:(1 to 3):(30 to 60).

4. The polyolefin separator according to claim 3, characterized by, The antioxidants include one or more of the following: (1) hindered phenols and (2) phosphites and thioesters.

5. The polyolefin separator according to claim 4, characterized by When the antioxidant comprises (1) hindered phenols and (2) phosphites, the mass ratio of the hindered phenols to the phosphites is 1:(1 to 3); when the antioxidant comprises (1) hindered phenols and (2) thioesters, the mass ratio of the hindered phenols to the thioesters is 1:(1 to 3); when the antioxidant comprises (1) hindered phenols and (2) phosphites and thioesters, the mass ratio of the hindered phenols to all of the phosphites and thioesters is 1:(1 to 3).

6. A method for producing a polyolefin separator, characterized by, include: A portion of the polyolefin raw materials are premixed with an antioxidant to obtain the first premix; The nucleating agent is premixed with the first premix to obtain a second premix; Another portion of the polyolefin raw material is premixed with the second premix to obtain a third premix, which is then melt-extruded with a pore-forming agent to obtain a melt. After cooling the melt to obtain a casting, the casting is first preheated, then stretched longitudinally, and then stretched laterally. After extraction of the cast sheet, the cast sheet is first stretched laterally at a small magnification, and then retracted laterally at a small magnification; and The heat-set casting yields a polyolefin membrane.

7. The method of producing a polyolefin separator according to claim 6, characterized by, One portion of the polyolefin raw material is polypropylene and meets one or more of the following conditions: molecular weight below 2.5 million, melt index from 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm; the other portion of the polyolefin raw material is polypropylene and meets one or more of the following conditions: molecular weight below 2.5 million, melt index from 1.0 g / 10 min to 2.0 g / 10 min, isotacticity ≥ 99.5%, and particle size: D50 ≤ 150 μm, D90 ≤ 200 μm.

8. The method of producing a polyolefin separator according to claim 6, characterized by, The mass ratio of the antioxidant, the nucleating agent, the entire portion of the polyolefin raw material and the other portion of the polyolefin raw material to the pore-forming agent is 1:(1 to 3):(30 to 60):(68 to 136).

9. The method of producing a polyolefin separator according to claim 6, characterized by, The mass ratio of the antioxidant, the nucleating agent, one portion of the polyolefin raw material, the other portion of the polyolefin raw material, and the pore-forming agent is 1:(1 to 3):(10 to 20):(20 to 40):(68 to 136).

10. The method of producing a polyolefin separator according to claim 8 or 9, characterized by, The antioxidant is one or more of hindered phenols, phosphites, and thioesters.

11. The method of producing a polyolefin separator according to claim 10, characterized by, The antioxidants include one or more of the following: (1) hindered phenols and (2) phosphites and thioesters.

12. The method of producing a polyolefin separator according to claim 8 or 9, characterized by, The nucleating agent is one or more of (1R,2S)-REL-1,2-cyclohexanedicarboxylate calcium salt, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, and 2,2'-methylene-bis(4,6-di-tert-butylphenyl) phosphate sodium salt.

13. The method of producing a polyolefin separator according to claim 8 or 9, characterized by, The pore-forming agent is one or more of paraffin oil and dioctyl phthalate.

14. The method of producing a polyolefin separator according to claim 6, characterized by, The premixing step of the first premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 4 min to 10 min; the premixing step of the second premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 1 min to 4 min; the premixing step of the third premix includes the following conditions: mixing temperature of 30°C to 70°C, mixing speed of 30 rpm to 40 rpm, and mixing time of 2 min to 5 min.

15. The method of producing a polyolefin separator according to claim 6, characterized by, The melt extrusion step includes the following conditions: screw temperature of 145°C to 235°C, melt pipe temperature of 190°C to 220°C, and screw speed of 40 rpm to 70 rpm.

16. The method of producing a polyolefin separator according to claim 6, characterized by, The cooling step includes the following conditions: the cooling temperature is 5°C to 30°C.

17. The method of producing a polyolefin separator according to claim 6, characterized by, The thickness of the cast sheet is controlled between 0.5 mm and 1.5 mm.

18. The method of producing a polyolefin separator according to claim 6, characterized by, The temperature of the preheating step is less than or equal to the temperature of the longitudinal stretching step, which is less than or equal to the temperature of the transverse stretching step, which is less than or equal to the temperature of the transverse small-ratio stretching step, which is less than or equal to the temperature of the transverse small-ratio retraction step.

19. The method of producing a polyolefin separator according to claim 6, characterized by, The stretching ratio of the transverse stretching step is greater than or equal to the stretching ratio of the transverse small-ratio stretching step.

20. The method of producing a polyolefin separator according to claim 18 or 19, characterized in that, The temperature of the preheating step is 110°C to 130°C, the temperature of the longitudinal stretching step is 120°C to 140°C, the temperature of the transverse stretching step is 140°C to 160°C, the temperature of the transverse small-ratio stretching step is 145°C to 165°C, and the temperature of the transverse small-ratio retraction step is 145°C to 165°C.

21. The method of producing a polyolefin separator according to claim 18 or 19, characterized in that, The stretching ratio of the longitudinal stretching step is 1 to 20 times, the stretching ratio of the transverse stretching step is 1 to 20 times, the stretching ratio of the transverse small-ratio stretching step is 1 to 5 times, and the shrinking ratio of the transverse small-ratio retraction step is 1 to 3 times.

22. The method of producing a polyolefin separator according to claim 6, characterized by, The temperature for the heat setting step is 140°C to 160°C.

23. A polyolefin separator, characterized by, It meets one or more of the following conditions: unit needle penetration intensity ≥ 48 gf / μm, MD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1h, TD heat shrinkage rate ≤ 0.8% after holding at 130℃ for 1h, and ionic conductivity ≥ 1.2 mS / cm at 25℃.