Battery pack, energy storage device and electric device

By using a core-shell structured thermal expansion material in the battery pack, with a gas core and a thermoplastic resin coating and adhesive layer, the damage and safety issues during the disassembly of energy storage devices are solved, enabling rapid and non-destructive disassembly.

WO2026237816A1PCT designated stage Publication Date: 2026-11-19CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/095455
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The dismantling of existing energy storage devices can easily cause surface dents, plastic deformation, and localized damage to the main components. Furthermore, dismantling is time-consuming, inefficient, and poses safety hazards. In addition, high-temperature and high-heat treatment can lead to irreversible damage.

Method used

The battery pack uses a core-shell structure with thermal expansion material, where the core is gas and the shell is a thermoplastic resin with a Tg of 90℃-120℃. By setting a thermal expansion coating and an adhesive layer on the surface of the battery pack, rapid and non-destructive disassembly can be achieved.

Benefits of technology

While meeting normal usage requirements, it enables rapid and non-destructive disassembly of battery packs and energy storage devices, avoiding component damage and safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026095455_19112026_PF_FP_ABST
    Figure CN2026095455_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a battery pack, an energy storage device and an electric device. The battery pack comprises a first body component, a first thermal expansion coating, a bonding layer and a second body component, which are sequentially stacked, wherein the first thermal expansion coating comprises a first thermal expansion material having a core-shell structure; the inner core of the first thermal expansion material comprises a first gas; and the shell layer of the first thermal expansion material comprises a thermoplastic resin having a Tg of 90-120°C. The present application can achieve rapid and non-destructive disassembly of the first body component and the second body component on the basis of satisfying the bonding requirements and the use stability.
Need to check novelty before this filing date? Find Prior Art

Description

Battery packs, energy storage devices and electrical appliances

[0001] Related applications

[0002] This application claims priority to Chinese patent application filed on May 16, 2025, with application number 2025106346853 and entitled "Battery Pack, Energy Storage Device and Electrical Device", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of battery technology, and in particular to battery packs, energy storage devices, and electrical devices. Background Technology

[0004] The recycling and dismantling of energy storage devices typically involves cryogenic freezing or immersion in chemical solvents followed by external force removal. This process can easily cause surface dents, plastic deformation, and localized damage to the main components, hindering their reuse. Furthermore, the dismantling process is time-consuming, inefficient, and may even lead to safety accidents. While adhesive strength may be reduced to facilitate dismantling, this can result in insufficient bonding throughout the energy storage device's lifespan, leading to localized or widespread delamination and rendering the device unusable.

[0005] However, disassembling the energy storage device by using thermal expansion coating usually requires processing at high temperatures for a long time. The continuous high temperature and heat can cause irreversible damage to the core components of the energy storage device, making it impossible to achieve rapid and non-destructive disassembly of the energy storage device while meeting normal usage requirements. Summary of the Invention

[0006] This application provides a battery pack, energy storage device, and electrical device that can meet normal usage requirements and can be quickly and non-destructively disassembled.

[0007] In a first aspect, this application provides a battery pack comprising a first body component, a first thermal expansion coating, an adhesive layer, and a second body component stacked sequentially; the first thermal expansion coating comprises a first thermal expansion material with a core-shell structure; the core of the first thermal expansion material comprises a first gas; and the shell of the first thermal expansion material comprises a thermoplastic resin with a Tg of 90°C-120°C.

[0008] The aforementioned battery pack, by sequentially applying a first thermal expansion coating and an adhesive layer to the surface of a first body component, followed by a second body component, and by including a first thermal expansion material with a core-shell structure in the first thermal expansion coating, the core of the first thermal expansion material comprising a first gas, and the shell of the first thermal expansion material comprising a thermoplastic resin with a Tg of 90℃-120℃, ensures that the first thermal expansion material does not affect the adhesive layer. Simultaneously, the shell of the first thermal expansion material can soften within the temperature range that the battery pack can withstand, and the first gas expands rapidly without undergoing decomposition or vaporization. Furthermore, during long-term use or high-temperature testing, the first thermal expansion material will not generate excessive pressure leading to cracks or defects. Therefore, while meeting adhesion requirements and operational stability, the first and second body components can be quickly and non-destructively disassembled.

[0009] In some embodiments, the first gas includes at least one of alkane gas, inert gas, air, and carbon dioxide; optionally, the alkane gas includes at least one of methane, ethane, propane, butane, and isobutane; optionally, the inert gas includes at least one of nitrogen, carbon tetrafluoride, helium, argon, neon, krypton, and xenon.

[0010] The first gas mentioned above is a gas at room temperature and is non-toxic and harmless. At the debinding temperature, it does not need to undergo the process of cracking or gasification to generate gas. Therefore, it can expand rapidly with heating to meet the requirements of rapid debinding.

[0011] In some embodiments, the shell of the first thermal expansion material comprises a thermoplastic resin with a Tg of 90°C-95°C.

[0012] By using the aforementioned thermoplastic resin for the shell layer of the first thermal expansion material, heating it at the battery's safe operating temperature can soften the shell layer of the thermal expansion material. Simultaneously, the gas expands upon heating, enabling disassembly without adversely affecting the performance of the main components.

[0013] In some embodiments, the thermoplastic resin includes a modified acrylic resin; optionally, the modified acrylic resin includes at least one of a silicone-modified acrylic resin and a polyurethane-modified acrylic resin.

[0014] The aforementioned thermoplastic resin has good compatibility with most adhesive resins and can be dispersed well, which is beneficial to improving the uniformity of the thermal expansion coating.

[0015] In some embodiments, the mass percentage of the first thermal expansion material in the first thermal expansion coating is 5%-20%, optionally 9%-17%.

[0016] Controlling the mass percentage of the first thermal expansion material in the thermal expansion coating within the above range is beneficial for balancing adhesion and debonding / disassembly performance.

[0017] In some embodiments, the Dv50 of the first thermal expansion material is 10 μm-50 μm.

[0018] The first thermal expansion material with the above-mentioned particle size is easier to disperse and is conducive to controlling the thickness of the thermal expansion coating, thereby adjusting the debinding and disassembly performance.

[0019] In some embodiments, the thickness of the first thermal expansion coating is 70 μm-300 μm.

[0020] Controlling the thickness of the first thermal expansion coating within the above range is beneficial for achieving a better expansion and debonding effect.

[0021] In some embodiments, the first thermal expansion coating further includes a first adhesive substrate with a curing temperature of <90°C;

[0022] Optionally, the curing temperature of the first adhesive substrate is -20℃ to 80℃.

[0023] The aforementioned adhesive matrix can be cured below the Tg of the first thermal expansion material, without causing the first thermal expansion material to expand or deform, or causing delamination or local damage after curing and cooling, thus affecting normal use.

[0024] In some embodiments, the first adhesive matrix includes at least one of a polyurethane system, an epoxy resin system, an acrylic resin system, a polyurethane-modified acrylic resin system, and a silicone-modified epoxy resin system; optionally, an acrylic resin system.

[0025] The aforementioned adhesive substrate has good compatibility with the first thermal expansion material and good adhesion, which is beneficial to improving the uniformity of the thermal expansion coating and achieving good composite with the main body component and the adhesive layer.

[0026] In some embodiments, the adhesive layer includes an adhesive substrate with a curing temperature of <90°C; optionally -20°C to 80°C.

[0027] The aforementioned adhesive substrate can be cured below the Tg of the first thermal expansion material, which will not cause the first thermal expansion coating to expand or deform during the bonding and curing process, resulting in deformation or local damage and affecting the normal use of the battery pack.

[0028] In some embodiments, the adhesive matrix includes at least one of a silane-modified polyether system, an epoxy resin system, an organosilicon system, and a polyurethane system.

[0029] The aforementioned adhesive matrix has good adhesion and good temperature resistance, which can meet the requirements of bonding and stability in use.

[0030] In some embodiments, a second thermal expansion coating is further disposed between the adhesive layer and the second body component; the second thermal expansion coating includes a core-shell structured second thermal expansion material; the core of the second thermal expansion material includes a second gas; the shell of the second thermal expansion material includes a thermoplastic resin with a Tg of 90°C-120°C.

[0031] By providing a second thermal expansion coating between the adhesive layer and the second body component, and making the second thermal expansion coating include a core-shell structure of the second thermal expansion material; the core of the second thermal expansion material includes a second gas, and the shell of the second thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃, the first body component, the second body component and the adhesive layer can be disassembled simultaneously during heating and disassembly, and the disassembly time can be further shortened.

[0032] In some embodiments, the first body component includes a bottom protective plate, a battery pack housing, a water-cooling plate, a battery cell, or a top cover.

[0033] The first body component and the second body component that are bonded to it have a need for rapid debonding and debonding.

[0034] In some embodiments, the first body component is a battery pack housing, and the second body component is a top cover;

[0035] Alternatively, the first main body component may be a water-cooled plate, and the second main body component may be a single battery cell;

[0036] Alternatively, the first main body component may be a bottom protective plate, and the second main body component may be a battery pack housing.

[0037] The first body component and the second body component mentioned above have the requirement for rapid debonding and debonding.

[0038] In some embodiments, a first thermal expansion coating is disposed on the surface of the first body component facing the second body component, and an adhesive layer is disposed between the surface of the first thermal expansion coating away from the first body component and the surface of the second body component facing the first body component;

[0039] Optionally, a first thermal expansion coating is disposed on the upper surface of the first body component, and an adhesive layer is disposed between the upper surface of the first thermal expansion coating and the lower surface of the second body component.

[0040] The above setup can meet the normal usage requirements of the battery pack, and can also quickly detach the adhesive during heating and disassembly.

[0041] A second aspect of this application provides a method for preparing a battery pack, comprising the following steps:

[0042] The first thermal expansion coating is formed on the surface of the first body component to form a first thermal expansion coating.

[0043] An adhesive is applied between the surface of the first thermal expansion coating and the lower surface of the first body component, and then cured to prepare the battery pack.

[0044] The first thermal expansion coating includes a core-shell structure of a first thermal expansion material; the core of the first thermal expansion material includes a first gas; and the shell of the first thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃.

[0045] A first thermal expansion coating is formed on the surface of a first body component to create a first thermal expansion coating layer. An adhesive is applied between the surface of the first thermal expansion coating layer and the lower surface of the first body component, and then cured to prepare a battery pack. The first thermal expansion coating layer includes a core-shell structure of a first thermal expansion material. The core of the first thermal expansion material includes a first gas, and the shell layer of the first thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃. In this way, the first thermal expansion material will not affect the adhesive layer. At the same time, the shell layer of the first thermal expansion material can soften within the temperature range that the battery pack can withstand. The first gas expands rapidly without undergoing a decomposition or vaporization process. Furthermore, during long-term use or high-temperature testing, the first thermal expansion material will not generate excessive pressure that could lead to cracks or defects. Therefore, while meeting the bonding requirements and the stability of use, the first body component and the second body component can be quickly and non-destructively disassembled.

[0046] In some embodiments, the resin of the first thermal expansion coating includes at least one of polyurethane, epoxy resin, acrylic resin, polyurethane-modified acrylic resin, and silicone-modified epoxy resin; optionally, the raw materials of the acrylic resin include: hard monomers, soft monomers, hydroxyl-containing monomers, functional monomers, and initiators; the hard monomers include at least one of methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, and vinyl acetate; the soft monomers include at least one of n-butyl acrylate, isobutyl acrylate, octyl methacrylate, octyl acrylate, isooctyl acrylate, and lauryl acrylate; the hydroxyl-containing monomers include at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; the functional monomers include at least one of isobornyl methacrylate, glycidyl tert-carbonate, cyclohexyl methacrylate, and benzyl methacrylate;

[0047] Optionally, the raw materials for polyurethane include: diisocyanate, organotin catalyst, polyether polyol, butanediol, and filler; the diisocyanate includes at least one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), naphthalene diisocyanate (NDI), diphenyldimethylbiphenyl diisocyanate (PPDI), and methylcyclohexane diisocyanate; the filler includes at least one of aluminum hydroxide and silica.

[0048] The aforementioned adhesive substrate has good compatibility with the first thermal expansion material and good adhesion, which is beneficial to improving the uniformity of the thermal expansion coating and achieving good composite with the main body component and the adhesive layer.

[0049] In some embodiments, the raw materials of the acrylic resin, by weight, include: 5-30 parts of methyl methacrylate, 10-50 parts of butyl acrylate, 5-30 parts of styrene, 10-30 parts of hydroxyethyl methacrylate, 5-20 parts of acrylic acid, 0.1-4 parts of initiator, and 5-20 parts of isobornyl methacrylate.

[0050] By weight, the raw materials for polyurethane include: 30-80 parts diisocyanate, 0.5-2 parts organotin catalyst, 5-40 parts polyether polyol, 5-30 parts butanediol, and 5-40 parts filler.

[0051] The acrylic resin and polyurethane prepared using the above raw materials have good adhesive properties and strength.

[0052] A third aspect of this application provides an energy storage device, including a battery pack of the first aspect or a battery pack prepared by the preparation method of the second aspect, as well as other functional components or systems.

[0053] The aforementioned energy storage device can meet normal usage requirements and can also be disassembled quickly and without damage.

[0054] A fourth aspect of this application provides an electrical device comprising a battery pack according to the first aspect or a battery pack prepared by the preparation method of the second aspect, or an energy storage device according to the third aspect.

[0055] The aforementioned electrical equipment can meet normal usage requirements and can be quickly and non-destructively disassembled. Attached Figure Description

[0056] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0057] Figure 1 is a schematic diagram of the assembly method of the main body components in the battery pack provided in some embodiments of this application;

[0058] Figure 2 is a schematic diagram of the assembly method of the main body components in the battery pack provided in some other embodiments of this application;

[0059] Figure 3 is a schematic diagram of a battery pack provided in some embodiments of this application;

[0060] Figure 4 is an exploded view of a battery pack provided in some embodiments of this application.

[0061] Explanation of reference numerals in the attached diagram: 1. Battery pack; 2. Top cover; 3. PACK housing; 4. Individual battery cell. Detailed Implementation

[0062] Hereinafter, some embodiments of the battery pack, energy storage device, and power consumption device of this application are described in detail with appropriate reference to the accompanying drawings. However, some unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0063] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0064] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0065] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0066] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0067] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if a method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if a method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0068] In this application, open-ended technical features or solutions described using terms such as "containing," "comprising," or "including" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members." In this application, unless otherwise specified, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0069] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0070] In this application, "gas" refers to a volatile substance that is a gas at room temperature (25 degrees Celsius) and normal pressure (standard atmospheric pressure), and may be a volatile substance with a boiling point below 20°C.

[0071] In this application, "thermally expanding material" refers to thermally expanding microspheres that use thermoplastic resin as the shell and are internally coated with volatile substances. The coating of volatile substances must be complete; otherwise, the uniformity of the thermally expanding material's quality cannot be guaranteed. Therefore, when the internal volatile substance is a gas or liquid, after heating to above the boiling point of the volatile substance, the internal pressure will differ. After the liquid volatile substance completely vaporizes, the amount of gas produced will be far greater than that of the gaseous volatile substance.

[0072] The recycling and dismantling of energy storage devices typically involves cryogenic freezing or immersion in chemical solvents followed by external force removal. This process can easily cause surface dents, plastic deformation, and localized damage to the main components, hindering their reuse. Furthermore, the dismantling process is time-consuming, inefficient, and may even lead to safety accidents. While adhesive strength may be reduced to facilitate dismantling, this can result in insufficient bonding throughout the energy storage device's lifespan, leading to localized or widespread delamination and rendering the device unusable.

[0073] However, disassembling the energy storage device by using thermal expansion coating usually requires processing at high temperatures for a long time. The continuous high temperature and heat can cause irreversible damage to the core components of the energy storage device, making it impossible to achieve rapid and non-destructive disassembly of the energy storage device while meeting normal usage requirements.

[0074] Based on this, this application provides a battery pack, energy storage device, and power consumption device that can meet normal use requirements and enable quick and non-destructive disassembly.

[0075] In a first aspect, some embodiments of this application provide a battery pack, including a first body component, a first thermal expansion coating, an adhesive layer, and a second body component stacked sequentially; the first thermal expansion coating includes a first thermal expansion material with a core-shell structure; the core of the first thermal expansion material includes a first gas; the shell layer of the first thermal expansion material includes a thermoplastic resin with a Tg of 90°C-120°C.

[0076] The aforementioned battery pack, by sequentially applying a first thermal expansion coating and an adhesive layer to the surface of a first body component, followed by a second body component, and by including a first thermal expansion material with a core-shell structure in the first thermal expansion coating, the core of the first thermal expansion material comprising a first gas, and the shell of the first thermal expansion material comprising a thermoplastic resin with a Tg of 90℃-120℃, ensures that the first thermal expansion material does not affect the adhesive layer. Simultaneously, the shell of the first thermal expansion material can soften within the temperature range that the battery pack can withstand, and the first gas expands rapidly without undergoing decomposition or vaporization. Furthermore, during long-term use or high-temperature testing, the first thermal expansion material will not generate excessive pressure leading to cracks or defects. Therefore, while meeting adhesion requirements and operational stability, the first and second body components can be quickly and non-destructively disassembled.

[0077] Understandably, when the core of a thermal expansion material contains liquid volatile substances, it needs to undergo a vaporization process to become gas and expand, requiring a certain reaction time and preventing rapid expansion for debinding. Simultaneously, the vaporization of liquid volatile substances generates a large amount of gas, leading to excessive internal pressure within the thermal expansion material. Furthermore, during high and low temperature tests, the material repeatedly undergoes vaporization and liquefaction (excessive pressure followed by decrease in pressure), which can easily cause cracks or defects, affecting the normal operation of the battery pack. In contrast, a thermal expansion material with a gas core, upon reaching the Tg of the thermoplastic resin in the shell, can rapidly expand as the shell softens, achieving rapid debinding. Moreover, during dual 85°C or high and low temperature cycling tests, the degree of gas expansion is relatively limited, preventing excessive expansion that could cause cracks or defects in the thermal expansion material, thus ensuring the stability of the battery pack.

[0078] In this application, "Tg" refers to the glass transition temperature, which is the characteristic temperature at which the amorphous region in an amorphous or semi-crystalline polymer changes from a hard and brittle "glassy state" to a soft and elastic "rubbery state" (or high-elasticity state). It can be determined by differential scanning calorimetry (DSC), dynamic thermomechanical analysis (DMA), or thermomechanical analysis (TMA).

[0079] In some specific examples, the Tg of the thermoplastic resin in the shell of the first thermal expansion material is 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, etc.; 90℃-95℃ can be selected.

[0080] By using the aforementioned thermoplastic resin for the shell layer of the first thermal expansion material, heating it at the battery's safe operating temperature can soften the shell layer of the thermal expansion material. Simultaneously, the gas expands upon heating, enabling disassembly without adversely affecting the performance of the main components.

[0081] In some embodiments, the first gas includes at least one of alkane gas, inert gas, air, and carbon dioxide; optionally, the alkane gas includes at least one of methane, ethane, propane, butane, and isobutane; optionally, the inert gas includes at least one of nitrogen, carbon tetrafluoride, helium, argon, neon, krypton, and xenon.

[0082] The first gas is a gas at room temperature (25℃) and is non-toxic and harmless. At the debinding temperature, it does not need to undergo the process of cracking or gasification to generate gas. Therefore, it can expand rapidly with heating to meet the requirements of rapid debinding.

[0083] In some embodiments, the thermoplastic resin includes a modified acrylic resin; optionally, the modified acrylic resin includes at least one of a silicone-modified acrylic resin and a polyurethane-modified acrylic resin.

[0084] The aforementioned thermoplastic resin has good compatibility with most adhesive resins and can be dispersed well, which is beneficial to improving the uniformity of the thermal expansion coating.

[0085] In some embodiments, the mass percentage of the first thermal expansion material in the first thermal expansion coating is 5%-20%, optionally 9%-17%, such as 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.

[0086] Controlling the mass percentage of the first thermal expansion material in the thermal expansion coating within the above range is beneficial for balancing adhesion and debonding / disassembly performance.

[0087] In some embodiments, the Dv50 of the first thermal expansion material is 10 micrometers (μm) to 50 μm, such as 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.

[0088] The first thermal expansion material with the above-mentioned particle size is easier to disperse and is conducive to controlling the thickness of the thermal expansion coating, thereby adjusting the debinding and disassembly performance.

[0089] In this application, Dv50 has a meaning known in the art, where Dv50 represents the particle size corresponding to the cumulative percentage of particle volume distribution reaching 50% from the smallest particle size, which can be tested using methods known in the art. For example, it can be determined using a laser particle size analyzer (such as a Malvern Master Size 3000). The particle size distribution can be obtained by the following method: Take a clean beaker, add an appropriate amount of the sample to be tested, and sonicate thoroughly to ensure complete dispersion of the sample. The testing instrument is a Malvern 2000 (USA). After the sample is poured into the injection tower, it circulates with the solution to the test optical path system. Under the irradiation of the laser beam, the particle size distribution characteristics (opause: 8%-12%) can be obtained by receiving and measuring the energy distribution of the scattered light. A particle size distribution map is plotted based on the test data.

[0090] In some embodiments, the thickness of the first thermal expansion coating is 70μm-300μm, such as 70μm, 80μm, 90μm, 100μm, 150μm, 200μm, 250μm, 300μm, etc.

[0091] Controlling the thickness of the first thermal expansion coating within the above range is beneficial for achieving a better expansion and debonding effect.

[0092] In some embodiments, the thickness of the adhesive layer is 1.5 mm to 3.5 mm, such as 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, etc.

[0093] By controlling the thickness of the adhesive layer within the above range, the bonding requirements can be met.

[0094] In some embodiments, the first thermal expansion coating further includes a first adhesive substrate with a curing temperature of <90°C;

[0095] Optionally, the curing temperature of the first adhesive substrate is -20℃ to 80℃, such as -20℃, -10℃, 0℃, 10℃, 20℃, 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, etc.

[0096] The aforementioned adhesive matrix can be cured below the Tg of the first thermal expansion material, without causing the first thermal expansion material to expand or deform, or causing delamination or local damage after curing and cooling, thus affecting normal use.

[0097] In some embodiments, the first adhesive matrix includes at least one of a polyurethane system, an epoxy resin system, an acrylic resin system, a polyurethane-modified acrylic resin system, and a silicone-modified epoxy resin system; optionally, an acrylic resin system.

[0098] The aforementioned adhesive substrate has good compatibility with the first thermal expansion material and good adhesion, which is beneficial to improving the uniformity of the thermal expansion coating and achieving good composite with the main body component and the adhesive layer.

[0099] In some embodiments, the adhesive layer includes an adhesive substrate with a curing temperature of <90°C; the curing temperature can be selected from -20°C to 80°C, for example -20°C, -10°C, 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, etc.

[0100] The aforementioned adhesive substrate can be cured below the Tg of the first thermal expansion material, which will not cause the first thermal expansion coating to expand or deform during the bonding and curing process, resulting in deformation or local damage and affecting the normal use of the battery pack.

[0101] In some embodiments, the adhesive matrix includes at least one of a silane-modified polyether system, an epoxy resin system, an organosilicon system, and a polyurethane system.

[0102] The aforementioned adhesive matrix has good adhesion and good temperature resistance, which can meet the requirements of bonding and stability in use.

[0103] In some embodiments, a second thermal expansion coating is further disposed between the adhesive layer and the second body component; the second thermal expansion coating includes a core-shell structured second thermal expansion material; the core of the second thermal expansion material includes a second gas; the shell of the second thermal expansion material includes a thermoplastic resin with a Tg of 90°C-120°C.

[0104] By providing a second thermal expansion coating between the adhesive layer and the second body component, and making the second thermal expansion coating include a core-shell structure of the second thermal expansion material; the core of the second thermal expansion material includes a second gas, and the shell of the second thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃, the first body component, the second body component and the adhesive layer can be disassembled simultaneously during heating and disassembly, and the disassembly time can be further shortened.

[0105] In some specific examples, the Tg of the thermoplastic resin in the shell of the second thermal expansion material is 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, etc.; 90℃-95℃ can be selected.

[0106] In some specific examples, the second gas includes at least one of alkane gases, inert gases, air, and carbon dioxide; optionally, the alkane gases include at least one of methane, ethane, propane, butane, and isobutane; optionally, the inert gases include at least one of nitrogen, carbon tetrafluoride, helium, argon, neon, krypton, and xenon.

[0107] In some specific examples, the thermoplastic resin in the shell of the second thermal expansion material includes a modified acrylic resin; optionally, the modified acrylic resin includes at least one of a silicone-modified acrylic resin and a polyurethane-modified acrylic resin.

[0108] In some specific examples, the mass percentage of the second thermal expansion material in the second thermal expansion coating is 5%-20%, optionally 9%-17%, such as 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.

[0109] In some specific examples, the Dv50 of the second thermal expansion material is 10μm-50μm, such as 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, etc.

[0110] In some specific examples, the thickness of the first thermal expansion coating is 70μm-300μm, such as 70μm, 80μm, 90μm, 100μm, 150μm, 200μm, 250μm, 300μm, etc.

[0111] In some specific examples, the second thermal expansion coating also includes a second adhesive substrate with a curing temperature of <90°C;

[0112] Optionally, the curing temperature of the first adhesive substrate is -20℃ to 80℃, such as -20℃, -10℃, 0℃, 10℃, 20℃, 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, etc.

[0113] In some specific examples, the second adhesive matrix includes at least one of a polyurethane system, an epoxy resin system, an acrylic resin system, a polyurethane-modified acrylic resin system, and a silicone-modified epoxy resin system; an acrylic resin system may be selected.

[0114] Understandably, there are no limitations on the first and second body components in this application; any two body components that are bonded together in the battery pack can be selected.

[0115] In some embodiments, the first body component includes a bottom protective plate, a battery pack housing (i.e., a PACK housing), a water-cooling plate, a battery cell, or a top cover.

[0116] The first body component and the second body component that are bonded to it have a need for rapid debonding and debonding.

[0117] In some embodiments, the first body component is a battery pack housing, and the second body component is a top cover;

[0118] Alternatively, the first main body component may be a water-cooled plate, and the second main body component may be a single battery cell;

[0119] Alternatively, the first main body component may be a bottom protective plate, and the second main body component may be a battery pack housing.

[0120] The first body component and the second body component mentioned above have the requirement for rapid debonding and debonding.

[0121] In some embodiments, a first thermal expansion coating is disposed on the surface of the first body component facing the second body component, and an adhesive layer is disposed between the surface of the first thermal expansion coating away from the first body component and the surface of the second body component facing the first body component;

[0122] Optionally, a first thermal expansion coating is disposed on the upper surface of the first body component, and an adhesive layer is disposed between the upper surface of the first thermal expansion coating and the lower surface of the second body component.

[0123] The above setup can meet the normal usage requirements of the battery pack, and can also quickly detach the adhesive during heating and disassembly.

[0124] Secondly, in some embodiments of this application, a method for preparing a battery pack is provided, comprising the following steps:

[0125] The first thermal expansion coating is formed on the surface of the first body component to form a first thermal expansion coating.

[0126] An adhesive is applied between the surface of the first thermal expansion coating and the lower surface of the first body component, and then cured to prepare the battery pack.

[0127] The first thermal expansion coating includes a core-shell structure of a first thermal expansion material; the core of the first thermal expansion material includes a first gas; and the shell of the first thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃.

[0128] A first thermal expansion coating is formed on the surface of a first body component to create a first thermal expansion coating layer. An adhesive is applied between the surface of the first thermal expansion coating layer and the lower surface of the first body component, and then cured to prepare a battery pack. The first thermal expansion coating layer includes a core-shell structure of a first thermal expansion material. The core of the first thermal expansion material includes a first gas, and the shell layer of the first thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃. In this way, the first thermal expansion material will not affect the adhesive layer. At the same time, the shell layer of the first thermal expansion material can soften within the temperature range that the battery pack can withstand. The first gas expands rapidly without undergoing a decomposition or vaporization process. Furthermore, during long-term use or high-temperature testing, the first thermal expansion material will not generate excessive pressure that could lead to cracks or defects. Therefore, while meeting the bonding requirements and the stability of use, the first body component and the second body component can be quickly and non-destructively disassembled.

[0129] In some embodiments, the resin of the first thermal expansion coating includes at least one of polyurethane, epoxy resin, acrylic resin, polyurethane-modified acrylic resin, and silicone-modified epoxy resin; optionally, the raw materials of the acrylic resin include: hard monomers, soft monomers, hydroxyl-containing monomers, functional monomers, and initiators; the hard monomers include at least one of methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, and vinyl acetate; the soft monomers include at least one of n-butyl acrylate, isobutyl acrylate, octyl methacrylate, octyl acrylate, isooctyl acrylate, and lauryl acrylate; the hydroxyl-containing monomers include at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; the functional monomers include at least one of isobornyl methacrylate, glycidyl tert-carbonate, cyclohexyl methacrylate, and benzyl methacrylate;

[0130] Optionally, the raw materials for polyurethane include: diisocyanate, organotin catalyst, polyether polyol, butanediol, and filler; the diisocyanate includes at least one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), naphthalene diisocyanate (NDI), diphenyldimethylbiphenyl diisocyanate (PPDI), and methylcyclohexane diisocyanate; the filler includes at least one of aluminum hydroxide and silica.

[0131] The aforementioned adhesive substrate has good compatibility with the first thermal expansion material and good adhesion, which is beneficial to improving the uniformity of the thermal expansion coating and achieving good composite with the main body component and the adhesive layer.

[0132] In some embodiments, the raw materials of the acrylic resin, by weight, include: 5-30 parts of methyl methacrylate, 10-50 parts of butyl acrylate, 5-30 parts of styrene, 10-30 parts of hydroxyethyl methacrylate, 5-20 parts of acrylic acid, 0.1-4 parts of initiator, and 5-20 parts of isobornyl methacrylate.

[0133] By weight, the raw materials for polyurethane include: 30-80 parts diisocyanate, 0.5-2 parts organotin catalyst, 5-40 parts polyether polyol, 5-30 parts butanediol, and 5-40 parts filler.

[0134] The acrylic resin and polyurethane prepared using the above raw materials have good adhesive properties and strength.

[0135] Understandably, the curing conditions of the first and second thermal expansion coatings can be adjusted. For example, curing at room temperature usually requires 20-80 hours; curing at 40-50℃ requires only 3-10 hours.

[0136] Understandably, the curing conditions of the adhesive layer can be adjusted. For example, curing at room temperature usually takes 3 to 10 days; curing at 40℃-50℃ takes 8 to 20 hours; and curing at 70℃-80℃ takes 2 to 6 hours.

[0137] In some specific examples, the second thermal expansion coating is obtained by curing a second thermal expansion coating material; the composition of the second thermal expansion coating material may be the same as or different from that of the first thermal expansion coating material.

[0138] Optionally, the resin of the second thermal expansion coating includes at least one of polyurethane, epoxy resin, acrylic resin, polyurethane-modified acrylic resin, and silicone-modified epoxy resin; optionally, the raw materials of the acrylic resin include: hard monomers, soft monomers, hydroxyl-containing monomers, functional monomers, and initiators; the hard monomers include at least one of methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, and vinyl acetate; the soft monomers include at least one of n-butyl acrylate, isobutyl acrylate, octyl methacrylate, octyl acrylate, isooctyl acrylate, and lauryl acrylate; the hydroxyl-containing monomers include at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate. The functional monomers include at least one of isobornyl methacrylate, glycidyl tert-carbonate, cyclohexyl methacrylate, and benzyl methacrylate; optionally, the raw materials for the polyurethane include: diisocyanate, organotin catalyst, polyether polyol, butanediol, and filler; the diisocyanate includes at least one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), naphthalene diisocyanate (NDI), diphenyl dimethyl biphenyl diisocyanate (PPDI), and methylcyclohexane diisocyanate; the filler includes at least one of aluminum hydroxide and silica.

[0139] Understandably, the raw materials for acrylic resins also include solvents; said solvents include one or more of toluene, xylene, trimethylbenzene, ethyl acetate, butyl acetate, tetrahydrofuran, ethylene glycol methyl ether, and acetone. The solvent accounts for 40 wt% to 70 wt% of the raw materials for acrylic resins by mass.

[0140] Thirdly, in some embodiments of this application, an energy storage device is provided, including a battery pack of the first aspect or a battery pack prepared by the preparation method of the second aspect, as well as other functional components or systems.

[0141] The aforementioned energy storage device can meet normal usage requirements and can also be disassembled quickly and without damage.

[0142] Fourthly, in some embodiments of this application, an electrical device is provided, including a battery pack of the first aspect or a battery pack prepared by the preparation method of the second aspect, or an energy storage device of the third aspect.

[0143] The aforementioned electrical equipment can meet normal usage requirements and can be quickly and non-destructively disassembled.

[0144] As an example, the battery pack includes a first body component, a first thermal expansion coating, an adhesive layer, and a second body component stacked sequentially, as shown in Figure 1. A thermal expansion coating is formed by coating the upper surface of the water-cooling plate with a thermal expansion coating, and then an adhesive is applied to place the battery cells, forming a sequentially stacked structure of water-cooling plate (first body component) - thermal expansion coating (first thermal expansion coating) - adhesive layer - battery cells (second body component); or a thermal expansion coating is formed by coating the upper surface of the PACK housing with a thermal expansion coating, and then an adhesive is applied to attach the top cover, forming a sequentially stacked structure of PACK housing (first body component) - thermal expansion coating (first thermal expansion coating) - adhesive layer - top cover (second body component).

[0145] As an example, the battery pack includes a first body component, a first thermal expansion coating, an adhesive layer, a second thermal expansion coating, and a second body component stacked sequentially, as shown in Figure 2. The first thermal expansion coating is formed by coating the upper surface of the water-cooling plate with the first thermal expansion coating, and the second thermal expansion coating is formed by coating the bottom of the battery cell with the second thermal expansion coating. Then, an adhesive is applied to the surface of the water-cooling plate, and the battery cell is placed there, forming a sequentially stacked structure of water-cooling plate (first body component) - thermal expansion coating (first thermal expansion coating) - adhesive layer - thermal expansion coating (second thermal expansion coating) - battery cell (second body component); or the first thermal expansion coating is applied to the upper surface of the PACK housing to form the first thermal expansion coating, and the second thermal expansion coating is applied to the lower surface of the top cover edge to form the second thermal expansion coating. Then, an adhesive is applied to the upper surface of the PACK housing to attach the top cover, forming a sequentially stacked structure of PACK housing (first body component) - thermal expansion coating (first thermal expansion coating) - adhesive layer - thermal expansion coating (second thermal expansion coating) - top cover (second body component).

[0146] As an example, some embodiments of this application provide a battery pack 1 as shown in Figures 3-4. Referring to Figures 3-4, the battery pack 1 may include a battery box and a plurality of battery cells 4 disposed in the battery box. The battery box includes a top cover 2 and a PACK housing 3. The top cover 2 can cover the PACK housing 3 and form a closed space for accommodating the battery cells 4. The plurality of battery cells 4 can be arranged in any manner in the battery box. A water-cooling plate is also provided at the bottom or a specific location of the PACK housing 3, and the battery cells are disposed above the water-cooling plate; a bottom protective plate may be provided at the bottom of the PACK housing 3.

[0147] As an example, some embodiments of this application provide an energy storage device including one or more battery clusters to increase the voltage and capacity of the energy storage device. The battery cluster may include multiple battery packs 1, which are connected in series via a busbar to increase the voltage of the energy storage device. When the energy storage device includes multiple battery clusters, the multiple battery clusters are connected in parallel to increase the capacity of the energy storage device. The energy storage device can be used in energy storage power stations, wind power generation systems, solar power generation systems, mobile power systems, or temporary power supply systems, etc. The energy storage device can store electrical energy as needed and output electrical energy when appropriate. For example, the energy storage device can store electrical energy during off-peak hours and provide power to relevant users or electrical equipment during peak hours. The energy storage system provided in the embodiments of this application can be any power system that requires the use of an energy storage device. In some embodiments, the energy storage device is an energy storage container or an energy storage cabinet.

[0148] In some embodiments, the energy storage device may include a cabinet and one or more battery clusters housed within the cabinet.

[0149] In some embodiments, the energy storage device may include modules such as a thermal management module, a main control module, a central control module, a power distribution module, and a fire protection module.

[0150] As an example, the thermal management module may include a liquid cooling unit that supplies coolant to each battery pack via piping to regulate the temperature of the individual battery cells.

[0151] As an example, the main control module can serve as the battery management unit for the battery cluster, used to monitor and manage the battery cluster. The main control module can monitor information such as the current, voltage, power, or temperature of the battery cluster. For instance, it can control the charging and discharging current and voltage of the battery cluster. The main control module includes modules such as an auxiliary battery management unit (SBMU) and a fusion switch.

[0152] As an example, the central control module can serve as the battery management unit for an energy storage device, used to monitor and manage the device. The central control module can monitor information such as the energy storage device's current, voltage, power, state of charge, or temperature. For instance, it can control the charging and discharging current and voltage of the energy storage device. As an example, the central control module includes modules such as the Insulation Monitoring Module (IMM), the Master Battery Management Unit (MBMU), the Ethernet (ETH) module, and the fiber optic conversion module.

[0153] As an example, a fire protection system includes control panels, detectors, alarm devices, etc., used to detect, alarm, or extinguish fires in energy storage systems.

[0154] As an example, the power distribution unit can be used to distribute power to the power modules of the energy storage device.

[0155] As an example, some embodiments of this application provide an electrical device, which includes a battery pack or energy storage device provided in this application. The battery pack can be used as a power source for the electrical device or as an energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.

[0156] As an electrical device, battery packs, batteries, and energy storage devices can be selected according to their usage requirements.

[0157] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0158] The following are exemplary descriptions of some of the raw materials used in the embodiments and comparative examples:

[0159] Thermal expansion materials: Shell: polyurethane modified acrylic resin, Tg of 75℃, 90℃, 95℃, 100℃, 110℃, 120℃ or 135℃; or silicone modified epoxy resin, Tg of 95℃; or acrylic resin, Tg of 70℃; Core: n-butane or hexane.

[0160] Adhesive for bonding layer: polyurethane adhesive, component A: 25 parts polyether polyol, 30 parts polyester polyol, 30 parts aluminum hydroxide, 5 parts dibutyltin dilaurate, 10 parts fumed silica; component B: 65 parts diphenylmethane diisocyanate, 35 parts silica powder; mix component A and component B in a volume ratio of 1:1 and cure before use.

[0161] Examples 1-5 and 7-9

[0162] Example of component preparation with thermal expansion coating

[0163] 1. Preparation of thermal expansion coatings

[0164] The formulations of the thermal expansion coatings for Examples 1-5 and 7-9 are shown in Table 1, and the preparation methods are as follows:

[0165] 1) Preparation of acrylic resin: Weigh the raw materials according to the formula, add 50wt% solvent (toluene) to the reaction vessel as the reaction medium, purge the air with nitrogen, start the stirrer, maintain the speed at 100 rpm, and heat to 135℃ using an oil bath device, and stabilize for 10 min. Add the mixed solution of other components to the reaction vessel within 2 hours. After the addition is complete, continue the reaction for 1 hour to end the reaction. Cool to room temperature to obtain acrylic resin.

[0166] 2) Preparation of thermal expansion coating: The acrylic resin prepared in step 1) is mixed with the remaining solvent and thermal expansion microspheres, and dispersed at a high speed of 1000 r / min for 15 minutes (min) and then allowed to stand at room temperature to obtain the thermal expansion coating.

[0167] 2. Assembly of components with thermal expansion coatings

[0168] A thermal expansion coating is applied to the surface of a first aluminum plate (3003 aluminum alloy), and baked at 50°C for 5 hours to form a thermal expansion coating (100μm thick). Then, an adhesive layer (2.5mm thick) is applied to the surface of the thermal expansion coating, and a second aluminum plate (3003 aluminum alloy) is placed on it. The plate is then left to stand at room temperature for 7 days to cure, thus obtaining a component with a thermal expansion coating.

[0169] Example 6

[0170] Except for the use of polyurethane as the adhesive matrix in the thermal expansion coating, the rest is the same as in Example 1. The composition and preparation method of the thermal expansion coating are as follows:

[0171] By weight: 50 parts TDI (toluene diisocyanate), 1 part dibutyltin dilaurate, 20 parts polyether polyol (number average molecular weight, 150,000), 15 parts butanediol, 10 parts aluminum hydroxide (Dv50 is 10μm), and 5 parts silica (Dv50 is 15μm).

[0172] Preparation method: First, TDI and dibutyltin dilaurate are added to a reaction vessel. After purging the air with nitrogen, the stirrer is started and the speed is maintained at 100 r / min. The mixture is heated to 45°C using an oil bath and stabilized for 10 min. A mixed solution of polyether polyol and butanediol is added to the reaction vessel over 1 hour. Then, the temperature is raised to 115°C and maintained at this temperature for 1 hour before being discharged. The mixture is then cooled to room temperature to obtain the matrix resin. Aluminum hydroxide and silica are added, and the mixture is dispersed at a high speed of 1600 r / min for 30 min before being discharged. After standing at room temperature, the polyurethane adhesive matrix is ​​obtained.

[0173] Comparative Example 1

[0174] Except for not adding thermally expandable microspheres, the rest is the same as in Example 1.

[0175] Comparative Example 2

[0176] Except that the core of the thermally expandable microspheres is n-pentane (boiling point of 36.1°C at standard atmospheric pressure, liquid at 25°C), the rest is the same as in Example 1.

[0177] Comparative Example 3

[0178] Except that the shell of the thermally expandable microspheres is made of acrylic resin (Tg is 70℃), the rest is the same as in Example 1.

[0179] Comparative Example 4

[0180] Except for the shell of the thermally expanded microspheres being made of polyurethane-modified acrylic resin (Tg = 135°C), the rest is the same as in Example 1.

[0181] Comparative Example 5

[0182] Except for the shell of the thermally expanded microspheres being made of polyurethane-modified acrylic resin (Tg = 75°C), the rest is the same as in Example 1.

[0183] Test case

[0184] The relevant parameter testing procedures for the components containing thermal expansion coatings in the examples and comparative examples are as follows:

[0185] 1. The shear strength and tensile strength were tested separately at room temperature, after treatment at 100℃ for 10 seconds (100℃@10s), after treatment at 125℃ (or 135℃) for 10 seconds (125℃@10s, or 135℃@10s), after aging at 85℃ (85% humidity) for 1000 hours, and after 1000 cycles of high and low temperatures (low temperature: -40℃, time: 30min; high temperature: 85℃, time: 30min; temperature transition time: 5min; number of cycles: 1000). The samples for each performance test corresponded to components with thermal expansion coatings. The samples varied slightly depending on the test performance (e.g., shape, bonding area), but the assembly method was the same. The specific test methods are as follows:

[0186] 1) Shear strength test:

[0187] The tensile shear strength of adhesives was determined according to the national standard GB / T 7124-2008 (rigid material to rigid material), and the unit is MPa. The test temperature was 25℃±2℃, and the tensile speed was 5mm / min.

[0188] 2) Tensile strength test:

[0189] The tensile strength of adhesive butt joints was determined according to the national standard GB / T 6329-1996, and the unit is MPa. The test temperature was 25℃±2℃, and the tensile speed was 5mm / min.

[0190] 2. High-temperature resistance test of individual battery cells:

[0191] After discharging, the battery cells are placed in a temperature chamber and heated from room temperature to 130±2℃ at a rate of 5℃ / min, and maintained at this temperature for 30 minutes before stopping heating. Then, the cells are observed at the test ambient temperature for 1 hour. If the battery cells do not catch fire, explode, or show any abnormalities in appearance, their performance is considered OK, and they can withstand a high temperature of 130℃ for 30 minutes. The upper limit of the operating temperature for a battery cell is generally 130℃. Its usage temperature or processing temperature should not exceed 130℃, as excessively high temperatures may cause irreversible damage to the battery cells.

[0192] The test results of the examples and comparative examples are shown in Tables 1-2.

[0193] Table 1 Summary of formulations and performance of Examples 1-9

[0194] Table 2 Summary of formulations and performance of Examples 1 and Comparative Examples 1-5 (based on a total of 100 parts of component A)

[0195] As shown in Tables 1-2, within the range of the embodiments, the performance at room temperature is unaffected, and the product performance remains unaffected after undergoing double 85 aging and high and low temperature aging, thus ensuring normal product use. However, the temperature of the thermal expansion material shell has a significant impact on debonding performance, double 85 aging performance, and high and low temperature aging performance. When the Tg of the thermal expansion material shell is 70℃, performance stability after double 85 aging and high and low temperature aging tests cannot be guaranteed. When the shell Tg is 135℃, after treatment at 100℃@10s, the adhesive strength shows no significant change and debonding is impossible; even increasing the treatment temperature to 135℃ does not prevent debonding. When the Tg of the expanded microsphere shell is 90-120℃, normal product use can be guaranteed, and after treatment at 100℃@10s or 125℃@10s, the adhesive strength decreases significantly, allowing for rapid debonding and disassembly. Especially when the Tg is 90-95℃, rapid debonding and disassembly can be achieved at 100℃@10s.

[0196] Analysis example

[0197] The Influence of Thermal Expansion Materials on the Properties of Adhesive Layers

[0198] Thermal expansion materials: Shell: polyurethane modified acrylic resin, Tg value 95℃, core is n-butane.

[0199] The basic adhesive layer formulation is as follows: Component A: 25 parts polyether polyol, 30 parts polyester polyol, 30 parts aluminum hydroxide, 5 parts dibutyltin dilaurate, and 10 parts fumed silica; Component B: 65 parts diphenylmethane diisocyanate and 35 parts silica powder.

[0200] The adhesive formulation for the bonding layer containing thermally expanding materials is as follows: Component A: 25 parts polyether polyol, 30 parts polyester polyol, 15 parts aluminum hydroxide, 15 parts thermally expanding material, 5 parts dibutyltin dilaurate, and 10 parts fumed silica; Component B: 65 parts diphenylmethane diisocyanate, 20 parts silica powder, and 15 parts thermally expanding material. The only difference from the base bonding layer adhesive is that the 15 parts of aluminum hydroxide in Component A of the base bonding layer adhesive are replaced with the thermally expanding material, and the 15 parts of silica powder in Component B of the base bonding layer adhesive are replaced with the thermally expanding material.

[0201] The base adhesive and the adhesive containing the thermal expansion material, components A and B, were mixed at a volume ratio of 1:1, cured, and their performance was tested. The performance testing methods and results are shown in Table 3 below:

[0202] Table 3

[0203] As can be seen from Table 3, if the expanded microspheres are used directly in the adhesive layer, the various properties of the adhesive layer will decrease and fail to meet the application requirements.

[0204] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.

[0205] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery pack, comprising a first body component, a first thermal expansion coating, an adhesive layer, and a second body component stacked sequentially; the first thermal expansion coating comprising a core-shell structure of a first thermal expansion material; the core of the first thermal expansion material comprising a first gas; and the shell of the first thermal expansion material comprising a thermoplastic resin with a Tg of 90°C-120°C.

2. The battery pack of claim 1, wherein, The first gas includes at least one of alkane gases, inert gases, air, and carbon dioxide; Optionally, the alkane gas includes at least one of methane, ethane, propane, butane, and isobutane; Optionally, the inert gas includes at least one of nitrogen, carbon tetrafluoride, helium, argon, neon, krypton, and xenon.

3. The battery pack of any one of claims 1-2, wherein, The shell of the first thermal expansion material comprises a thermoplastic resin with a Tg of 90℃-95℃.

4. The battery pack of claim 3, wherein, The thermoplastic resin includes a modified acrylic resin; Optionally, the modified acrylic resin includes at least one of silicone-modified acrylic resin and polyurethane-modified acrylic resin.

5. The battery pack of any one of claims 1-4, wherein, In the first thermal expansion coating, the mass percentage of the first thermal expansion material is 5%-20%, optionally 9%-17%.

6. The battery pack of any one of claims 1-5, wherein, The Dv50 of the first thermal expansion material is 10μm-50μm.

7. The battery pack of any one of claims 1-6, wherein, The thickness of the first thermal expansion coating is 70μm-300μm.

8. The battery pack of any one of claims 1-7, wherein, The first thermal expansion coating also includes a first adhesive substrate with a curing temperature of <90°C; Optionally, the curing temperature of the first adhesive substrate is -20℃ to 80℃.

9. The battery pack of claim 8, wherein, The first adhesive matrix includes at least one of a polyurethane system, an epoxy resin system, an acrylic resin system, a polyurethane-modified acrylic resin system, and a silicone-modified epoxy resin system; an acrylic resin system may be selected.

10. The battery pack of any one of claims 1-9, wherein, The adhesive layer includes an adhesive substrate with a curing temperature of <90℃; optionally -20℃ to 80℃.

11. The battery pack of claim 10, wherein, The adhesive matrix includes at least one of silane-modified polyether systems, epoxy resin systems, silicone systems, and polyurethane systems.

12. The battery pack of any one of claims 1-11, wherein, A second thermal expansion coating is further provided between the adhesive layer and the second body component; the second thermal expansion coating includes a core-shell structure of a second thermal expansion material; the core of the second thermal expansion material includes a second gas; the shell of the second thermal expansion material includes a thermoplastic resin with a Tg of 90℃-120℃.

13. The battery pack of any one of claims 1-12, wherein, The first main body component includes a bottom protective plate, a battery pack housing, a water-cooling plate, and a battery cell or a top cover.

14. The battery pack of any one of claims 1-12, wherein, The first main body component is the battery pack housing, and the second main body component is the top cover; Alternatively, the first body component may be a water-cooled plate, and the second body component may be a battery cell; Alternatively, the first main body component may be a bottom protective plate, and the second main body component may be a battery pack housing.

15. The battery pack of any one of claims 1-14, wherein, The first thermal expansion coating is disposed on the surface of the first body component facing the second body component, and the adhesive layer is disposed between the surface of the first thermal expansion coating away from the first body component and the surface of the second body component facing the first body component; Optionally, the first thermal expansion coating is disposed on the upper surface of the first body component, and the adhesive layer is disposed between the upper surface of the first thermal expansion coating and the lower surface of the second body component.

16. A method for preparing a battery pack, comprising the following steps: The first thermal expansion coating is formed on the surface of the first body component to form a first thermal expansion coating. An adhesive is applied between the surface of the first thermal expansion coating and the lower surface of the first body component, and then cured to prepare the battery pack. The first thermal expansion coating comprises a core-shell structure of a first thermal expansion material; the core of the first thermal expansion material comprises a first gas; and the shell of the first thermal expansion material comprises a thermoplastic resin with a Tg of 90℃-120℃.

17. The production method according to claim 16, wherein The resin of the first thermal expansion coating includes at least one of polyurethane, epoxy resin, acrylic resin, polyurethane-modified acrylic resin, and silicone-modified epoxy resin. Optionally, the raw materials of the acrylic resin include: hard monomers, soft monomers, hydroxyl-containing monomers, functional monomers, and initiators; the hard monomers include at least one selected from methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, and vinyl acetate; the soft monomers include at least one selected from n-butyl acrylate, isobutyl acrylate, octyl methacrylate, octyl acrylate, isooctyl acrylate, and lauryl acrylate; the hydroxyl-containing monomers include at least one selected from acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; the functional monomers include at least one selected from isobornyl methacrylate, glycidyl tert-carbonate, cyclohexyl methacrylate, and benzyl methacrylate. Optionally, the raw materials for the polyurethane include: diisocyanate, organotin catalyst, polyether polyol, butanediol, and filler; the diisocyanate includes at least one selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, diphenyldimethylbiphenyl diisocyanate, and methylcyclohexane diisocyanate; the filler includes at least one selected from aluminum hydroxide and silica.

18. The production method according to claim 16 or 17, wherein By weight, the raw materials of the acrylic resin include: 5-30 parts methyl methacrylate, 10-50 parts butyl acrylate, 5-30 parts styrene, 10-30 parts hydroxyethyl methacrylate, 5-20 parts acrylic acid, 0.1-4 parts initiator, and 5-20 parts isobornyl methacrylate; and / or, The polyurethane raw materials, by weight, include: 30-80 parts diisocyanate, 0.5-2 parts organotin catalyst, 5-40 parts polyether polyol, 5-30 parts butanediol, and 5-40 parts filler.

19. An energy storage device comprising a battery pack according to any one of claims 1-15 or a battery pack prepared by the preparation method according to any one of claims 16-18.

20. An electrical device comprising a battery pack according to any one of claims 1-15 or a battery pack prepared by the preparation method according to any one of claims 16-18, or an energy storage device according to claim 19.