Multi-layer copper current collector, preparation method therefor and use thereof

By introducing a multilayer copper current collector with a nanotwin structure into the current collector of lithium batteries, the problems of insufficient strength and ductility of traditional copper layers are solved, the extrusion resistance and safety performance of the battery are improved, and the manufacturing process is simplified and the cost is reduced.

WO2026237856A1PCT designated stage Publication Date: 2026-11-19YANGZHOU NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/095945
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing lithium battery current collectors have shortcomings in terms of extrusion resistance and safety performance. Traditional copper layers lack strength and ductility, and the presence of polymer layers in composite current collectors limits the improvement of battery safety performance. Furthermore, the carbon-copper layer preparation process is complex and costly.

Method used

A multilayer copper current collector with a nanotwin structure is used to improve the strength and ductility of the copper layer by controlling the microstructure parameters of the copper layer, including the preferred orientation of a specific (111) crystal plane and the width of the twin layer. The copper layer is deposited on the base film by electroplating or magnetron sputtering.

Benefits of technology

This achieves a balance between the strength and ductility of the copper layer, improves the battery's resistance to extrusion and electrochemical performance, simplifies the manufacturing process, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026095945_19112026_PF_FP_ABST
    Figure CN2026095945_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a multi-layer copper current collector, a preparation method therefor and a use thereof. The multi-layer copper current collector comprises a base film and a copper layer located on at least one side of the base film; the copper layer comprises a nanotwinned structure; and in the copper layer, x represents the ratio of the XRD relative peak intensity of a crystal plane (111) to the XRD relative peak intensity of a crystal plane (200), y represents the ratio of the XRD relative peak intensity of the crystal plane (111) to the XRD relative peak intensity of a crystal plane (220), and D1 represents the width of a twin lamella in the nanotwinned structure, wherein x≥1, y≥1, and D1=4-150 nm.
Need to check novelty before this filing date? Find Prior Art

Description

A multilayer copper current collector, its preparation method, and its application. Technical Field

[0001] This application belongs to the field of current collector and battery technology, specifically relating to a multilayer copper current collector and its preparation method and application. Background Technology

[0002] Lithium-ion batteries are widely used in consumer electronics, power batteries, and energy storage due to their stable cycle performance and high energy density. Meanwhile, the rapid development of electric vehicles has placed higher demands on the safety, stability, and energy density of lithium-ion batteries. Composite current collectors are a new type of power battery current collector material, generally possessing a "metal-polymer material-metal" sandwich structure. They use polymer insulating materials such as PET / PP / PI as the "core" layer, with aluminum or copper deposited on both the top and bottom surfaces. Composite copper foil mainly consists of three parts: a middle layer of organic PET, PP, PI, or other base film, with copper layers approximately 1 μm thick on both sides.

[0003] In lithium battery cell safety testing, cells are required to have high resistance to compression. Traditional current collectors cannot adequately meet the compression resistance test requirements. Composite current collectors have high ductility due to the presence of polymer layers, but they can only improve the safety performance of cells by 10-30%. Since the copper layer on the surface of the base film in composite current collectors has low hardness, it cannot guarantee the safety performance of the battery. Therefore, it is necessary to design a metal layer structure with higher strength to meet the growing safety requirements. Summary of the Invention

[0004] To address the problems and shortcomings of existing technologies, this application provides a multilayer copper current collector, its preparation method, and its application. The copper layer of this multilayer copper current collector has a nanotwinned structure, which effectively improves its strength, even exhibiting higher strength than C-Cu (carbon-copper), thus effectively optimizing battery safety performance. Furthermore, the pure copper layer exhibits higher conductivity, which is beneficial for further improving the battery's rate performance and cycle performance.

[0005] According to a first aspect of this application, a multilayer copper current collector is provided, including a base film and a copper layer located on at least one side of the base film, the copper layer including a nanotwin structure; in the copper layer, x represents the ratio of the relative peak XRD intensity of the (111) crystal plane to the (200) crystal plane, y represents the ratio of the relative peak XRD intensity of the (111) crystal plane to the (220) crystal plane, D1 represents the width of the twin crystal layer in the nanotwin structure, x≥1, y≥1, D1=4~150nm.

[0006] In the fabrication of functional or composite current collectors, copper layers are typically used as the metal layer. Currently, pure copper layers are mainly used as the conductive layer. However, in current applications, the strength and ductility of pure copper layers formed on the base film are still somewhat lacking, easily leading to poor extrusion resistance in the fabricated cells, thus reducing the safety performance of the cells and failing to meet the increasingly stringent requirements for current cell specifications. In addition, carbon-copper layers are also used as the conductive layer for current collectors, but carbon-copper layers have even lower strength, further compromising cell safety. Moreover, the fabrication of carbon-copper layers usually requires the composite of carbon materials and copper, involving multiple process steps such as carbon material dispersion, coating, or deposition. These processes are relatively complex, requiring high levels of equipment and process control, increasing production costs and difficulty. Therefore, using carbon-copper layers is not conducive to actual production.

[0007] To further improve the strength and ductility of the pure copper layer, this application starts from the microstructure of the copper layer, controlling the copper layer to have a nanotwin structure with a specific (111) preferred crystal plane orientation and twin sheet width, effectively improving the strength and ductility of the copper layer. It should be noted that a twin refers to two crystals (or two parts of a single crystal) forming a mirror-symmetric orientation relationship along a common crystal plane (i.e., a specific orientation relationship). These two crystals are called "twins," and this common crystal plane is called the twin plane. The width of the twin sheet refers to the distance between the crystal layers on both sides of the twin boundary.

[0008] Regarding strength and ductility, strength refers to a material's ability to resist permanent deformation and fracture; that is, its ability to maintain its shape and dimensions when subjected to external forces. Ductility refers to a material's ability to change shape in various directions before cracking occurs. This ability primarily measures whether a material can be effectively reshaped after deformation. Materials with good ductility can undergo significant deformation without breaking under external forces, and there is a certain balance between strength and ductility. Generally speaking, high-strength materials tend to have poor ductility, while materials with good ductility tend to have lower strength. This is because high strength usually means that the material is difficult to deform under external forces, while good ductility means that the material is easy to deform but not easy to break under external forces. Therefore, in practical applications, it is necessary to weigh strength and ductility according to specific requirements.

[0009] Therefore, this application controls the relevant parameters of the microstructure in the aforementioned copper layer within a specific range, enabling multilayer copper current collectors to simultaneously achieve good strength and ductility. This results in a better balance between strength and ductility compared to conventional copper or carbon-copper current collectors, without affecting the original conductivity of the copper layer. Specifically, in the twinned structure, the twin boundaries effectively hinder dislocation movement, achieving metal strengthening. Furthermore, when the width of the twinned wafers is refined to the nanometer scale (4~150nm), the strength of copper is significantly improved, with a tensile strength reaching 1GPa and tensile plasticity exceeding 10%. This is because, according to the traditional Hall-Petch relation, dislocations are difficult to transfer from one grain to another through incoherent internal grain boundary barriers, causing their strength to be inversely proportional to the square root of the grain size. Unlike high-interface-energy incoherent interfaces, low-interface-energy coherent grain boundaries (TBs) such as twins not only effectively block dislocation movement but also relax local stresses. When the twin spacing is in the micrometer range, coherent grain boundaries (TB) exhibit strength comparable to conventional grain boundaries (GB), and both conform to the Hall-Petch (hp) relationship. Furthermore, coherent twin boundaries can impede dislocation movement and store dislocations, thus improving the mechanical strength and plasticity of the thin film. Moreover, controlling the preferred orientation of the Cu(111) crystal plane according to the above relationship can also enhance the strength of the copper layer and effectively improve its ductility. Therefore, under the control of various microscopic parameters of the copper layer, both the strength and ductility of the copper layer can be effectively improved simultaneously, further enhancing the balance between strength and ductility. This improves the strength and ductility of multilayer copper current collectors, resulting in battery cells with excellent extrusion resistance.

[0010] It should also be noted that the copper layer with a twinned structure in this application differs from ordinary copper layers in the following ways: First, the grain arrangement of ordinary copper layers is relatively disordered, with large and unevenly distributed grains; while in the copper layer with a twinned structure, there are a large number of parallel twin lamellae. These twin lamellae are part of the crystal, and their atomic arrangement has a specific symmetry relationship with the matrix crystal, making the crystal structure more regular and ordered. Second, the grain boundaries of ordinary copper layers are mostly large-angle grain boundaries with high grain boundary energy and irregular atomic arrangement; the twinned grain boundaries in the copper layer with a twinned structure are a special type of grain boundary with a certain periodicity and symmetry in atomic arrangement and lower grain boundary energy.

[0011] Preferably, x ≥ 2; or, x ≥ 3; or, x ≥ 4; or, x ≥ 5; or, x ≥ 6; or, x ≥ 7; or, x ≥ 8; or, x ≥ 9; or, x ≥ 10; or, x ≥ 11; or, x ≥ 12; or, x ≥ 13; or, x ≥ 14; or, x ≥ 15; or, x ≥ 16; or, x ≥ 17; or, x ≥ 18; or, x ≥ 19; or, x ≥ 20; or, x ≥ 21; or, x ≥ 22; or, x ≥ 23; or, x ≥ 24; or, x ≥ 25; or x≥26; or x≥27; or x≥28; or x≥29; or x≥30; or x≥31; or x≥32; or x≥33; or x≥34; or x≥35; or x≥36; or x≥37; or x≥38; or x≥39; or x≥40; or x≥41; or x≥42; or x≥43; or x≥44; or x≥45; or x≥46; or x≥47; or x≥48; or x≥ 49; or, x≥50; or, x≥51; or, x≥52; or, x≥53; or, x≥54; or, x≥55; or, x≥56; or, x≥57; or, x≥58; or, x≥59; or, x≥60; or, x≥61; or, x≥62; or, x≥63; or, x≥64; or, x≥65; or, x≥66; or, x≥67; or, x≥68; or, x≥69; or, x≥70; or, x≥71; or, x≥72 ; or, x≥73; or, x≥74; or, x≥75; or, x≥76; or, x≥77; or, x≥78; or, x≥79; or, x≥80; or, x≥81; or, x≥82; or, x≥83; or, x≥84; or, x≥85; or, x≥86; or, x≥87; or, x≥88; or, x≥89; or, x≥90; and the lower limit of x is not limited to the data listed above, and other unlisted values ​​within the numerical range also apply.

[0012] Preferably, x=2; or, x=3; or, x=4; or, x=5; or, x=6; or, x=7; or, x=8; or, x=9; or, x=10; or, x=11; or, x=12; or, x=13; or, x=14; or, x=15; or, x=16; or, x=17; or, x=18; or, x=19; or, x=20; or, x=21; or, x=22; or, x=23; or, x=24; or, x=25; or x=26; or x=27; or x=28; or x=29; or x=30; or x=31; or x=32; or x=33; or x=34; or x=35; or x=36; or x=37; or x=39; or x=38; or x=40; or x=41; or x=42; or x=43; or x=44; or x=45; or x=46; or x=47; or x=48; or x= 49; or, x=50; or, x=51; or, x=52; or, x=53; or, x=54; or, x=55; or, x=56; or, x=57; or, x=58; or, x=59; or, x=60; or, x=61; or, x=62; or, x=63; or, x=64; or, x=65; or, x=66; or, x=67; or, x=68; or, x=69; or, x=70; or, x=71; or, x=72 ; or, x=73; or, x=74; or, x=75; or, x=76; or, x=77; or, x=78; or, x=79; or, x=80; or, x=81; or, x=82; or, x=83; or, x=84; or, x=85; or, x=86; or, x=87; or, x=88; or, x=89; or, x=90; and the value of x is not limited to the data listed above, other unlisted values ​​within the numerical range also apply.

[0013] Preferably, y≥2; or y≥3; or y≥4; or y≥5; or y≥6; or y≥7; or y≥8; or y≥9; or y≥10; or y≥11; or y≥12; or y≥13; or y≥14; or y≥15; or y≥16; or y≥17; or y≥18; or y≥19; or y≥20; or y≥21; or y≥22; or y≥23; or y≥24; or y≥25; or y≥26; or y≥27; or y≥28; or y≥29; or y≥30; or y≥31; or y≥32; or y≥33; or y≥34; or y≥35; or y≥36; or y≥37; or y≥38; or y≥39; or y≥40; or y≥41; or y≥42; or y≥43; or y≥44; or y≥45; or y≥46; or y≥47; or y≥48; or y≥ 49; or, y≥50; or, y≥51; or, y≥52; or, y≥53; or, y≥54; or, y≥55; or, y≥56; or, y≥57; or, y≥58; or, y≥59; or, y≥60; or, y≥61; or, y≥62; or, y≥63; or, y≥64; or, y≥65; or, y≥66; or, y≥67; or, y≥68; or, y≥69; or, y≥70; or, y≥71; or, y≥72 ; or, y≥73; or, y≥74; or, y≥75; or, y≥76; or, y≥77; or, y≥78; or, y≥79; or, y≥80; or, y≥81; or, y≥82; or, y≥83; or, y≥84; or, y≥85; or, y≥86; or, y≥87; or, y≥88; or, y≥89; or, y≥90; and the lower limit of y is not limited to the data listed above, but also applies to other unlisted values ​​within the numerical range.

[0014] Preferably, y=2; or y=3; or y=4; or y=5; or y=6; or y=7; or y=8; or y=9; or y=10; or y=11; or y=12; or y=13; or y=14; or y=15; or y=16; or y=17; or y=18; or y=19; or y=20; or y=21; or y=22; or y=23; or y=24; or y=25; or y=26; or y=27; or y=28; or y=29; or y=30; or y=31; or y=32; or y=33; or y=34; or y=35; or y=36; or y=37; or y=38; or y=39; or y=40; or y=41; or y=42; or y=43; or y=44; or y=45; or y=46; or y=47; or y=48; or y= 49; or y=50; or y=51; or y=52; or y=53; or y=54; or y=55; or y=56; or y=57; or y=58; or y=59; or y=60; or y=61; or y=62; or y=63; or y=64; or y=65; or y=66; or y=67; or y=68; or y=69; or y=70; or y=71; or y=72 ; or, y = 73; or, y = 74; or, y = 75; or, y = 76; or, y = 77; or, y = 78; or, y = 79; or, y = 80; or, y = 81; or, y = 82; or, y = 83; or, y = 84; or, y = 85; or, y = 86; or, y = 87; or, y = 88; or, y = 89; or, y = 90; and the value of y is not limited to the data listed above, other unlisted values ​​within the numerical range also apply.

[0015] Preferably, D1 = 4nm; or, D1 = 5nm; or, D1 = 6nm; or, D1 = 7nm; or, D1 = 8nm; or, D1 = 9nm; or, D1 = 10nm; or, D1 = 11nm; or, D1 = 12nm; or, D1 = 13nm; or, D1 = 14nm; or, D1 = 15nm; or, D1 = 16nm; or, D1 = 17nm; or, D1 = 18nm; or, D1 = 19nm; or, D1 = 20nm; or, D1 = 23nm; or, D1 = 25nm; or, D1 = 30nm; or, D1 = 35nm; or, D1 = 40nm; or, D1 = 45nm; or, D1 =50nm; or, D1=55; or, D1=60nm; or, D1=65nm; or, D1=70nm; or, D1=75nm; or, D1=80nm; or, D1=85nm; or, D1=90nm; or, D1=95nm; or, D1=100nm; or, D1=105nm; or, D1=110nm; or, D1=105nm; or, D1=120nm; or, D1=125nm; or, D1=130nm; or, D1=135nm; or, D1=140nm; and the value of D1 is not limited to the data listed above, other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the copper layer is disposed on both sides of the base film.

[0017] Preferably, 1.61≤x≤46.5; 1.04≤y≤18.6. Controlling the upper and lower limits of x and y is more conducive to balancing the regulation of the copper deposition process conditions and the overall performance of the copper layer. Therefore, it is beneficial to ensure the multi-faceted performance of the obtained multi-layer copper current collector and its performance in the battery cell.

[0018] Preferably, in the copper layer, z represents the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes, and z ≥ 1. Furthermore, by controlling the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes in the copper layer to ≥ 1, the preferred orientation of the (111) crystal plane in the copper layer is higher. Under such parameter control, it is more conducive to taking into account both the conductivity and mechanical properties of the copper layer, and therefore more conducive to taking into account the safety performance, cycle performance and rate performance of the battery cell prepared from it.

[0019] Preferably, z≥2; or, z≥3; or, z≥4; or, z≥5; or, z≥6; or, z≥7; or, z≥8; or, z≥9; or, z≥10; or, z≥11; or, z≥12; or, z≥13; or, z≥14; or, z≥15; or, z≥16; or, z≥17; or, z≥18; or, z≥19; or, z≥20; or, z≥21; or, z≥22; or, z≥23; or, z≥24; or, z≥25; or, z≥26; or, z≥27; or, z≥28; or, z≥ 29; or, z≥30; or, z≥31; or, z≥32; or, z≥33; or, z≥34; or, z≥35; or, z≥36; or, z≥37; or, z≥38; or, z≥39; or, z≥40; or, z≥41; or, z≥42; or, z≥43; or, z≥44; or, z≥45; or, z≥46; or, z≥47; or, z≥48; or, z≥49; or, z≥50; and regarding the lower limit of z, it is not limited to the data listed above, and other unlisted values ​​within the numerical range also apply.

[0020] Preferably, z=2; or, z=3; or, z=4; or, z=5; or, z=6; or, z=7; or, z=8; or, z=9; or, z=10; or, z=11; or, z=12; or, z=13; or, z=14; or, z=15; or, z=16; or, z=17; or, z=18; or, z=19; or, z=20; or, z=21; or, z=22; or, z=23; or, z=24; or, z=25; or, z=26; or, z=27; or, z=28; or, z= 29; or z=30; or z=31; or z=32; or z=33; or z=34; or z=35; or z=36; or z=37; or z=38; or z=39; or z=40; or z=41; or z=42; or z=43; or z=44; or z=45; or z=46; or z=47; or z=48; or z=49; or z=50; and the value of z is not limited to the data listed above, other unlisted values ​​within the numerical range also apply.

[0021] In some implementations, 1 ≤ z ≤ 20.

[0022] In some implementations, D1 = 8~30nm. Furthermore, controlling the width of the twin wafer layer within this range is beneficial for obtaining a copper layer with a higher (111) crystal plane orientation, which is more conducive to improving the strength and ductility of the copper layer, thereby optimizing the overall strength and ductility of the multilayer copper current collector, improving the cell's resistance to compression, and enabling it to maintain a safe state without gas leakage, fire, or explosion under more complex external force conditions.

[0023] In some embodiments, the copper layer satisfies at least one of the following conditions: (1) the thickness of the copper layer is represented by D2, where D2 = 500~2000 nm; (2) the copper content in the copper layer is not less than 99 wt%. On the one hand, the deposited copper layer needs to maintain a certain thickness. Too small a thickness is not conducive to improving its conductivity and mechanical properties (such as strength and ductility), while too large a thickness is not conducive to forming a uniform copper layer, and also not conducive to the overall performance of the copper layer. On the other hand, ensuring that the copper layer is approximately composed of pure copper can help ensure its excellent conductivity.

[0024] In some embodiments, the base film satisfies at least one of the following conditions: (1) the thickness of the base film is represented by D3, where D3 = 1~10 μm; (2) the material of the base film includes one or more of insulating polymer materials, metal materials, organic fiber materials, carbon materials, and inorganic materials.

[0025] In some embodiments, the insulating polymer material includes one or more of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene ether, polystyrene, polyimide, and polyimide urea; the metallic material includes one or more of aluminum, copper, nickel, iron, titanium, silver, gold, cobalt, chromium, molybdenum, or tungsten; the organic fiber material includes one or more of polyacrylonitrile fiber, poly(p-phenylenebenzobisoxazole) fiber, polybenzimidazole fiber, and polyimide fiber; the carbon material includes one or more of conductive carbon black, acetylene black, natural graphite, artificial graphite, mesophase carbon microspheres, mesophase carbon fiber, vapor-grown carbon fiber, hard carbon, soft carbon, petroleum coke, graphene, fullerene, carbon nanotubes, and glassy carbon; and the inorganic material includes one or more of oxides, carbides, silicides, and nitrides.

[0026] In some embodiments, the substrate material includes one or more of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene ether, polystyrene, polyimide, and polyimide urea.

[0027] According to a second aspect of this application, a method for preparing the aforementioned multilayer copper current collector is provided, specifically by depositing a copper layer on at least one side of a base film using electroplating; wherein the electroplating solution used in the electroplating process includes Cu 2+ 0.2~5mol / L, plating solution additives 2~800ppm, H +The ion concentration is 0.2~0.75mol / L; the current density is 3~40 ASD; the plating solution additives include one or more of gelatin, sodium 3-mercapto-1-propanesulfonate (MPS), polyethylene glycol (PEG), and Janus Green (JGB).

[0028] By controlling the above electroplating conditions, a uniform copper layer can be deposited on the base film, and the deposited copper layer has a preferred orientation of (111). The ratio of the relative peak intensity of XRD of the (111) crystal plane to that of the (200) crystal plane and the (220) crystal plane is ≥1. Therefore, under this preparation process condition, the multilayer copper current collector has higher strength and ductility, which is more conducive to meeting the performance requirements of high strength and high conductivity.

[0029] In some embodiments, Cu in the electroplating solution 2+ The concentration can be 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, or 5 mol / L; however, it is not limited to the data listed above, and other unlisted values ​​within the range are also applicable.

[0030] In some embodiments, the concentration of the plating solution additive in the electroplating solution can be 2 ppm, 4 ppm, 6 ppm, 8 ppm, 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm, 100 ppm, 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, or 800 ppm; however, it is not limited to the data listed above, and other unlisted values ​​within the numerical range are also applicable.

[0031] In some embodiments, H in the electroplating solution + The concentration can be 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, 0.7 mol / L, or 0.75 mol / L; however, it is not limited to the data listed above, and other unlisted values ​​within the range are also applicable.

[0032] In some embodiments, the current density during electroplating can be 3 ASD, 4 ASD, 5 ASD, 6 ASD, 7 ASD, 8 ASD, 9 ASD, 10 ASD, 13 ASD, 15 ASD, 17 ASD, 20 ASD, 22 ASD, 25 ASD, 28 ASD, 30 ASD, 33 ASD, 35 ASD, 37 ASD, or 40 ASD; but is not limited to the data listed above, other unlisted values ​​within the range are also applicable.

[0033] In some embodiments, the plating solution additives include gelatin and Janus Green (JGB); and the concentration ratio of gelatin to Janus Green (JGB) is 20~800ppm:1~40ppm. Using these two plating solution additives in a specific molar ratio is beneficial for electroplating and depositing a more uniform copper layer on the base film, while ensuring that the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the (200) crystal plane and the (220) crystal plane in the copper layer is ≥1, so that the copper layer has a high preferred orientation of the (111) crystal plane, thereby making the copper layer exhibit higher mechanical and electrical properties, which is more conducive to optimizing the safety and cycle performance of the battery cell.

[0034] In some embodiments, Cu in the electroplating solution 2+ The source of copper is the dissolution of copper salts, including but not limited to the following compounds: copper sulfate (CuSO4·5H2O), copper chloride (CuCl2), copper nitrate (Cu(NO3)2), basic copper carbonate (Cu2(OH)2CO3), and copper acetate (Cu(CH3COO)2); or Cu²⁺ in the electroplating solution. + Derived from the chemical dissolution of copper powder or copper oxide, including but not limited to: copper powder (Cu), copper oxide (CuO), and cuprous oxide (Cu2O).

[0035] In some embodiments, H in the electroplating solution + The acidic electrolytes are derived from the addition of acidic electrolytes, including but not limited to the following compounds: sulfuric acid (H2SO4), hydrochloric acid (HCl), nitric acid (HNO3), phosphoric acid (H3PO4), and acetic acid (CH3COOH); or H2O from the electroplating solution. + It originates from the hydrolysis of acidic copper salts, including but not limited to: copper sulfate (CuSO4), copper chloride (CuCl2), and copper nitrate (Cu(NO3)2).

[0036] In some embodiments, the electroplating solution includes copper sulfate (CuSO4·5H2O), sulfuric acid (H2SO4), gelatin, polyethylene glycol (PEG), and sodium 3-mercapto-1-propanesulfonate (MPS); or, the electroplating solution includes copper sulfate (CuSO4·5H2O), sulfuric acid (H2SO4), JGB, polyethylene glycol (PEG), and sodium 3-mercapto-1-propanesulfonate (MPS); or, the electroplating solution includes copper sulfate (CuSO4·5H2O), sulfuric acid (H2SO4), JGB, gelatin, and sodium 3-mercapto-1-propanesulfonate (MPS).

[0037] According to a second aspect of this application, a method for preparing the above-mentioned multilayer copper current collector is provided, specifically, a copper layer is deposited on at least one side of a base film by magnetron sputtering; during the magnetron sputtering process, a copper target is used as the target material, the target power is 10~15kW, the inert gas flow rate is 40~70mL / min, the coating vacuum degree is 0.05~0.1Pa, and the coating time is 4~6s.

[0038] Under the above magnetron sputtering preparation process conditions, a copper layer can be uniformly deposited on the base film surface. At the same time, the ratio of the relative peak intensity of XRD of the (111) crystal plane to that of the (200) crystal plane and the (220) crystal plane in the copper layer is ≥1. This results in the copper layer having a high preferred orientation of the (111) crystal plane, which is beneficial to make the copper layer exhibit higher mechanical and electrical properties, and thus more beneficial to optimize the safety and cycle performance of the battery cell.

[0039] In some embodiments, during magnetron sputtering, the purity of copper in the copper target is not less than 99%.

[0040] In some implementations, the inert gas used in magnetron sputtering includes argon.

[0041] In some implementations, during magnetron sputtering, the target power is 12kW, the argon flow rate is 50mL / min, the coating vacuum is 0.08Pa, and the coating time is 5s.

[0042] In some implementations, the temperature of the main roller during the magnetron sputtering process is 20°C.

[0043] According to a third aspect of this application, an electrode is provided, comprising the multilayer copper current collector described above or the multilayer copper current collector prepared by the above method, and an electrode active material located on the multilayer copper current collector.

[0044] According to a fourth aspect of this application, a lithium battery cell is provided, comprising the aforementioned electrode.

[0045] According to a fifth aspect of this application, a battery pack is provided, comprising the aforementioned lithium battery cell.

[0046] According to a sixth aspect of this application, an electrical device is provided, comprising the aforementioned lithium battery cell or the aforementioned battery pack.

[0047] Compared with the prior art, the beneficial effects of this application are as follows:

[0048] This application improves the strength and ductility of a copper layer by controlling its microstructure, including a nanotwinned structure, a preferred orientation of the (111) crystal plane, and the width of the twin wafers. Specifically, by controlling the relevant parameters of the microstructure within a specific range, this application enables multilayer copper current collectors to simultaneously achieve good strength and ductility. Compared to conventional copper or carbon-copper current collectors, this provides a better balance between strength and ductility without affecting the original conductivity of the copper layer. Therefore, the resulting battery cells exhibit excellent extrusion resistance and electrochemical performance. Attached Figure Description

[0049] Figure 1 shows the XRD pattern of the copper layer in Example 1.

[0050] Figures 2(a) to 2(c) show the EBSD patterns of the copper layer in Example 1.

[0051] Figure 3 shows the XRD pattern of the copper layer in Example 2.

[0052] Figures 4(a) to 4(c) show the EBSD patterns of the copper layer in Example 2.

[0053] Figure 5 shows the XRD pattern of the copper layer in Comparative Example 1.

[0054] Figure 6 shows the XRD pattern of the copper layer in Comparative Example 2.

[0055] Figure 7 shows a schematic diagram of the X, Y, and Z directions when the battery cell is subjected to a compression test. Embodiments of the present invention

[0056] Example 1

[0057] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0058] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 0.2 mol / L, plating solution additive 40 ppm, H + Ion concentration: 0.4 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0059] The base film material is PP (polypropylene); Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0060] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 46.5, i.e., x = 46.5 (x = 1). (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 18.6, i.e., y = 18.6 (y = I). (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 13.3, i.e., z = 13.3 (z = I (111) / (I (200) +I (220) ));

[0061] The XRD (X-ray diffraction) and EBSD (electron backscattering diffraction) data obtained are shown in Figures 1 and 2. The blue part corresponds to the Cu(111) crystal plane. The results in Figures 1 and 2(a) to 2(c) show that the (111) crystal plane has a significantly larger proportion, indicating that the material has a preferred orientation of the (111) crystal plane, and the degree of preferred orientation is high. At this time, the twin lamellae width of the copper layer was measured to be 15 nm, i.e., D1 = 15 nm. The twin lamellae width of the copper layer was measured by TEM, mainly based on electron diffraction and high-resolution imaging technology. Selected area electron diffraction (SAED) technology was used to measure the distance from the diffraction spot to the center, and the interplanar spacing of the twin lamellae, i.e., the twin lamellae width, was obtained by calculation using reciprocal space. The twin lamellae width of the copper layer in other embodiments and comparative examples were also measured by the same method as in Example 1.

[0062] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0063] Example 2

[0064] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0065] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+4mol / L, plating solution additive 80ppm, H + Ion concentration: 0.2 mol / L; Current density: 20 ASD; Electroplating time: 60 s;

[0066] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0067] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 1.61, i.e., x = 1.61 (x = 1). (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 1.04, i.e., y = 1.04 (y = I). (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.6, i.e., z = 0.6 (z = I (111) / (I (200) +I (220) ));

[0068] The XRD (X-ray diffraction) and EBSD (electron backscattering diffraction) data obtained are shown in Figures 3 and 4. The blue part corresponds to the Cu(111) crystal plane. The results in Figures 3 and 4(a) to 4(c) show that the (111) crystal plane has a significantly larger proportion, indicating that the material has a preferred orientation of the (111) crystal plane, and the degree of preferred orientation is high. At this time, the width of the twin layer of the copper layer was measured to be 10 nm, that is, D1 = 10 nm.

[0069] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0070] Example 3

[0071] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0072] Copper layers were deposited on both sides of the base film using magnetron sputtering, forming a multilayer copper current collector. The thickness of the copper layer, D2, was 1 μm (single layer), and the thickness of the base film, D3, was 4.5 μm. During the magnetron sputtering process, a copper target (purity: 99.99%) was used as the target material, the target power was 12 kW, the argon flow rate was 50 mL / min, the coating vacuum degree was 0.08 Pa, the coating time was 5 s, and the temperature of the main roller during the coating process was 20 °C.

[0073] The base film material is PP;

[0074] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 40.4, i.e., x = 40.4. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 15.2, i.e., y = 15.2. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 11.2, i.e., z = 11.02 (z = I (111) / (I (200) +I (220) ));

[0075] Furthermore, the width of the copper twin layer was measured to be 18nm, i.e., D1=18nm.

[0076] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0077] Example 4

[0078] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0079] Copper layers were deposited on both sides of the base film using magnetron sputtering, forming a multilayer copper current collector. The thickness of the copper layer, D2, was 1 μm (single layer), and the thickness of the base film, D3, was 4.5 μm. During the magnetron sputtering process, a copper target (purity: 99.99%) was used as the target material, the target power was 12 kW, the argon flow rate was 50 mL / min, the coating vacuum degree was 0.1 Pa, the coating time was 6 s, and the temperature of the main roller during the coating process was 20 °C.

[0080] The base film material is PP;

[0081] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 14.6, i.e., x = 14.6. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 17.5, i.e., y = 17.5. (y = I) (111) / I (220)); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 7.95, i.e., z = 7.95 (z = I (111) / (I (200) +I (220) ));

[0082] Furthermore, the width of the copper twin layer was measured to be 24 nm, i.e., D1 = 24 nm.

[0083] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0084] Example 5

[0085] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0086] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 0.2 mol / L, plating solution additive 40 ppm, H + Ion concentration: 0.75 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0087] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0088] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 3.25, i.e., x = 3.25. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 7.47, i.e., y = 7.47. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 2.26, i.e., z = 2.26 (z = I (111) / (I (200) +I (220) ));

[0089] Furthermore, the width of the copper twin layer was measured to be 6nm, i.e., D1=6nm.

[0090] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0091] Example 6

[0092] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0093] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 2 mol / L, plating solution additive 40 ppm, H + Ion concentration: 0.2 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0094] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0095] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 6.73, i.e., x = 6.73. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 1.16, i.e., y = 1.16. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.99, i.e., z = 0.99 (z = I (111) / (I (200) +I (220) ));

[0096] Furthermore, the width of the copper twin layer was measured to be 40nm, i.e., D1=40nm.

[0097] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0098] Example 7

[0099] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0100] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 4 mol / L, plating solution additive 10 ppm, H + Ion concentration: 0.2 mol / L; Current density: 20 ASD; Electroplating time: 60 s;

[0101] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is Janus Green (JGB).

[0102] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 11.4, i.e., x = 11.4. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 6.72, i.e., y = 6.72. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 4.23, i.e., z = 4.23 (z = I (111) / (I (200) +I (220) ));

[0103] Furthermore, the width of the copper twin layer was measured to be 60nm, i.e., D1=60nm.

[0104] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0105] Example 8

[0106] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0107] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 5 mol / L, plating solution additive 80 ppm, H + Ion concentration: 0.2 mol / L; Current density: 20 ASD; Electroplating time: 60 s;

[0108] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is polyethylene glycol (PEG).

[0109] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 1.88, i.e., x = 1.88. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 2.15, i.e., y = 2.15. (y = I) (111) / I (220) Furthermore, the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 1.01, i.e., z = 1.01 (z = I). (111) / (I (200) +I (220) ));

[0110] Furthermore, the width of the copper twin layer was measured to be 100nm, i.e., D1=100nm.

[0111] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0112] Example 9

[0113] The multilayer copper current collector of this embodiment was prepared according to the following steps:

[0114] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 0.2 mol / L, plating solution additive 30 ppm, H + Ion concentration: 0.4 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0115] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the plating solution additives are gelatin and Janus Green (JGB), and the concentration ratio of gelatin to Janus Green (JGB) is 20ppm:10ppm.

[0116] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 31.5, i.e., x = 31.5. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 12.8, i.e., y = 12.8. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 9.1, i.e., z = 9.1 (z = I (111) / (I (200) +I (220) ));

[0117] Furthermore, the width of the copper twin layer was measured to be 13nm, i.e., D1=13nm.

[0118] Under the aforementioned parameter conditions, such as specific x, y, and / or z, D1, the copper layer can be considered to have excellent strength and ductility. At the same time, under the aforementioned specific parameters, the copper layer also has excellent electrical conductivity.

[0119] Comparative Example 1

[0120] The multilayer copper current collector of this comparative example was prepared according to the following steps:

[0121] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 8 mol / L, plating solution additive 100 ppm, H + Ion concentration: 0.5 mol / L; Current density: 15 ASD; Electroplating time: 60 s;

[0122] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0123] XRD characterization of the copper layer of the multilayer copper current collector prepared in this comparative example showed that the ratio of the relative peak intensities of the (111) crystal plane to the (200) crystal plane in the copper layer was 0.61, i.e., x = 0.61. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 6.77, i.e., y = 6.77. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.58, i.e., z = 0.58 (z = I (111) / (I (200) +I (220) The XRD (X-ray diffraction) data obtained are shown in Figure 5. The above results indicate that the copper layer does not have a preferred orientation of the (111) crystal plane, but has a higher preferred orientation of the (200) crystal plane. At this time, the twin layer width of the copper layer was measured to be 35 nm, that is, D1=35 nm.

[0124] Among the above-mentioned parameters, the x and y values ​​are not both ≥1 and the (200) crystal plane has a high preferred orientation. In this case, the copper layer has poor strength and ductility.

[0125] Comparative Example 2

[0126] The multilayer copper current collector of this comparative example was prepared according to the following steps:

[0127] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 2 mol / L, plating solution additive 100 ppm, H + Ion concentration: 0.8 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0128] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0129] XRD characterization of the copper layer of the multilayer copper current collector prepared in this comparative example showed that the ratio of the relative peak intensities of the (111) crystal plane to the (200) crystal plane in the copper layer was 1.09, i.e., x = 1.09. (x = I) (111) / I (200) The ratio of the relative peak XRD intensities of the (111) crystal plane to that of the (220) crystal plane is 0.05, i.e., y = 0.05. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.05, i.e., z = 0.05 (z = I (111) / (I (200) +I (220)The XRD (X-ray diffraction) data obtained are shown in Figure 6. The above results indicate that the copper layer does not have a preferred orientation of the (111) crystal plane, but has a higher preferred orientation of the (220) crystal plane. At this time, the width of the twin layer of the copper layer was measured to be 96 nm, that is, D1=96 nm.

[0130] Among the above-mentioned parameters, the following conditions are not met: x and y values ​​are both ≥1, the (220) crystal plane has a high preferred orientation, and D1 is large. In this case, the copper layer has poor strength and ductility.

[0131] Comparative Example 3

[0132] The multilayer copper current collector of this comparative example was prepared according to the following steps:

[0133] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 10mol / L, plating solution additive 400ppm, H + Ion concentration: 0.8 mol / L; Current density: 40 ASD; Electroplating time: 60 s;

[0134] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0135] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 0.53, i.e., x = 0.53. (x = I) (111) / I (200) The ratio of the relative peak XRD intensities of the (111) crystal plane to that of the (220) crystal plane is 0.11, i.e., y = 0.11. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.09, i.e., z = 0.09 (z = I (111) / (I (200) +I (220) ));

[0136] Furthermore, the measured width of the copper twin layer was 121 nm, i.e., D1 = 121 nm.

[0137] If the x and y values ​​do not both satisfy ≥1, the copper layer will have poor strength and ductility.

[0138] Comparative Example 4

[0139] The multilayer copper current collector of this comparative example was prepared according to the following steps:

[0140] Copper layers are deposited on both sides of the base film using electroplating, forming a multilayer copper current collector. The thickness of the copper layer, D2, is 1 μm (single layer), and the thickness of the base film, D3, is 4.5 μm. The electroplating solution used in the electroplating process includes Cu... 2+ 8 mol / L, plating solution additive 400 ppm, H + Ion concentration: 0.5 mol / L; Current density: 60 ASD; Electroplating time: 60 s;

[0141] The base film material is PP; Cu 2+ The source is copper sulfate (CuSO4·5H2O); H + The source of the solution is sulfuric acid (H2SO4); the additive in the plating solution is gelatin.

[0142] The copper layer of the multilayer copper current collector prepared in this embodiment was characterized by XRD. The ratio of the relative peak intensity of the (111) crystal plane to the (200) crystal plane in the copper layer was measured to be 0.27, i.e., x = 0.27. (x = I) (111) / I (200) The ratio of the relative peak XRD intensity of the (111) crystal plane to that of the (220) crystal plane is 0.86, i.e., y = 0.86. (y = I) (111) / I (220) ); and the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes is 0.21, i.e., z = 0.21 (z = I (111) / (I (200) +I (220) ));

[0143] Furthermore, the measured width of the copper twin layer was 165nm, i.e., D1=165nm.

[0144] Among the parameters mentioned above, if D1 is too large, the copper layer will have poor strength and ductility.

[0145] Test case

[0146] 1. Experimental Construction Method

[0147] (1) The tensile strength and elongation at break of the multilayer copper current collectors obtained in Examples 1-9 and Comparative Examples 1-4 were tested. The specific test methods are as follows:

[0148] Tensile tests were performed on the samples using a universal tensile testing machine. The test conditions were: tensile rate of 100 mm / min, test temperature of 22℃, and relative humidity of 20%. The tensile strength and elongation at break of the samples were measured according to ASTM D638 (or ISO 527) standards.

[0149] (2) The multilayer copper current collectors obtained in Examples 1-9 and Comparative Examples 1-4 were used to prepare the battery cell. The specific preparation method is as follows: For the positive electrode, the positive electrode current collector is a traditional aluminum foil (thickness is 13μm), and the positive electrode material is LiNi. 0.6 Mn 0.2 Co 0.2 O2 (NCM622); For the negative electrode: the negative electrode current collector is the composite current collector prepared in this application, and the negative electrode material is artificial graphite; For the separator, an alumina ceramic-coated polyethylene separator (25 μm thick) is used; For the electrolyte, 1 mol·L⁻¹ is used. -1 A carbonate solution of LiPF6, wherein the carbonate comprises propylene carbonate, ethylene carbonate and ethyl methyl carbonate in a mass ratio of 1:1:1; lithium-ion batteries are assembled using the above materials according to relevant procedures.

[0150] The battery cell prepared above was subjected to a compression test. Certain pressures were applied in the X, Y, and Z directions, and the deformation under these pressures was measured. Deformation was calculated as (size before pressure application - size after pressure application) / size before pressure application. The state of the battery cell after applying pressure in the X, Y, and Z directions was also recorded.

[0151] For the X, Y, and Z directions, please refer to Figure 7.

[0152] 2. Experimental Results

[0153] The relevant parameters of the multilayer copper current collector prepared above, as well as its tensile strength and elongation at break properties, are recorded in Table 1. Meanwhile, the results of the extrusion test on the battery cell prepared using the multilayer copper current collector are shown in Table 2.

[0154] Table 1. Relevant parameters of multilayer copper current collectors, including tensile strength and elongation at break.

[0155]

[0156] Table 2. Results of the cell extrusion test

[0157]

[0158] As shown in Tables 1 and 2, the multilayer copper current collector provided in this application has good tensile strength and elongation at break, that is, it has good mechanical properties, which further enables the battery cell made from it to have good anti-extrusion performance, thus effectively improving the safety performance of the battery cell. See Examples 1 to 9 for reference.

[0159] In Comparative Examples 1-4, the conditions of x ≥ 1 and y ≥ 1 are not met. Specifically, x < 1 in Comparative Example 1, y < 1 in Comparative Example 2, and x < 1 and y < 1 in Comparative Examples 3 and 4. Furthermore, the twin wafer width D1 in Comparative Example 4 is too large. These variables result in an unbalanced tensile strength and elongation at break (ductility) of the multilayer copper current collectors in Comparative Examples 1-4. Consequently, even with relatively low pressure in the three different directions, the deformation is large, leading to gas leakage and / or fire and explosion, significantly reducing the safety performance of the battery cell. This indicates that ensuring x > 1 and y > 1, while simultaneously ensuring D1 is within a specific range, is more conducive to obtaining a multilayer copper current collector with a balance between tensile strength and elongation at break. This can further optimize the extrusion resistance of the battery cell and improve its safety performance.

[0160] Furthermore, comparing Example 1 and Example 2, in Example 2, z<1, the crystal orientation degree is relatively lower, which cannot better balance the tensile strength and elongation at break of the multilayer copper current collector. As a result, in Example 2, there is a large deformation under lower pressure in three different directions, which is not conducive to further improving the extrusion resistance of the cell and reduces the safety performance of the cell.

[0161] Observing Examples 3 and 4, it can be found that in addition to electroplating, magnetron sputtering can also be used to prepare the multilayer copper current collector in this application. This means that as long as the relevant process conditions in the preparation process of the multilayer copper current collector are reasonably controlled, multilayer copper current collectors with x, y, z, and D1 all within a suitable range can be obtained, thereby effectively improving the tensile strength and elongation at break of the multilayer copper current collector, thereby improving the extrusion resistance of the battery cell and optimizing the safety performance of the battery cell.

[0162] Comparing Examples 1 and Examples 5, 6, 7, and 8, where D1 in Examples 5, 6, 7, and 8 are 6nm, 40nm, 60nm, and 100nm respectively, it can be seen that when D1 is not in the range of 8~30nm, the tensile strength and elongation at break (ductility) of the multilayer copper current collector are not well balanced. This results in a large deformation under lower pressure in three different directions in Example 2, which is not conducive to further improving the extrusion resistance of the cell and reduces the safety performance of the cell.

[0163] Comparing Examples 1 and 9, the plating solution additive in Example 9 was gelatin + Janus Green (JGB). The resulting multilayer copper current collector better balanced tensile strength and elongation at break, thus further improving the cell's resistance to compression. Specifically, under high pressure in three different directions, it maintained a similar deformation to Example 1, optimizing the cell's safety performance. This demonstrates that with specific plating solution additive compositions, the performance of the electroplated multilayer copper current collector can be further optimized, thereby further improving the cell's safety performance.

[0164] In summary, when x ≥ 1 and y ≥ 1, the copper layer exhibits a high preferred orientation, and the multilayer copper current collector can effectively balance tensile strength and elongation at break, resulting in relatively good strength and ductility, while also demonstrating good cell compression resistance. Furthermore, a larger z-value indicates a better preferred orientation, further balancing tensile strength and elongation at break, and further enhancing cell compression resistance. The twin layer width D1 has a non-linear effect on compression resistance. When x < 1 and / or y < 1 and / or D1 is not within the range of 4–150 nm, the copper layer lacks a preferred orientation or cannot effectively block dislocation movement, causing the multilayer copper current collector to fail to effectively balance high tensile strength and / or elongation at break, resulting in poor strength and / or ductility, and consequently, poor cell compression resistance.

Claims

1. A multilayer copper current collector, comprising a base film and a copper layer located on at least one side of the base film, the copper layer comprising a nanotwin structure; In the copper layer, x represents the ratio of the relative peak intensity of XRD of the (111) crystal plane to that of the (200) crystal plane, y represents the ratio of the relative peak intensity of XRD of the (111) crystal plane to that of the (220) crystal plane, and D1 represents the width of the twin crystal layer in the nanotwin structure, x≥1, y≥1, D1=4~150nm.

2. The multilayer copper current collector as described in claim 1, wherein: 1.61≤x≤46.5; 1.04≤y≤18.

6.

3. The multilayer copper current collector as described in claim 1, wherein: In the copper layer, z represents the ratio of the relative peak intensity of the XRD of the (111) crystal plane to the sum of the (200) and (220) crystal planes, and z≥1.

4. The multilayer copper current collector as described in claim 1, wherein: D1 = 8~30nm.

5. The multilayer copper current collector as described in claim 1, wherein: The copper layer satisfies at least one of the following conditions: (1) Let D2 represent the thickness of the copper layer, where D2 = 500~2000 nm; (2) The copper content in the copper layer is not less than 99 wt%.

6. The multilayer copper current collector as described in claim 1, wherein: The base film satisfies at least one of the following conditions: (1) Let D3 represent the thickness of the base film, where D3 = 1~10 μm; (2) The material of the base film includes one or more of the following: insulating polymer materials, metal materials, organic fiber materials, carbon materials, and inorganic materials; The insulating polymer material includes one or more of the following: polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene ether, polystyrene, polyimide, and polyimide urea. The metallic material includes one or more of aluminum, copper, nickel, iron, titanium, silver, gold, cobalt, chromium, molybdenum, or tungsten; The organic fiber material includes one or more of polyacrylonitrile fiber, poly(p-phenylenebenzobisoxazole) fiber, polybenzimidazole fiber, and polyimide fiber. The carbon materials include one or more of the following: conductive carbon black, acetylene black, natural graphite, artificial graphite, mesophase carbon microspheres, mesophase carbon fibers, vapor-grown carbon fibers, hard carbon, soft carbon, petroleum coke, graphene, fullerene, carbon nanotubes, and glassy carbon. The inorganic material includes one or more of oxides, carbides, silicides, and nitrides.

7. A method for preparing the multilayer copper current collector as described in claim 1, comprising the following steps: The copper layer is deposited on at least one side of the base film using electroplating. The electroplating solution used in the electroplating process includes Cu 2+ 0.2~5mol / L, plating solution additives 2~800ppm, H + Ion concentration: 0.2–0.75 mol / L; Current density: 3–40 ASD; The plating solution additives include one or more of gelatin, sodium 3-mercapto-1-propanesulfonate, polyethylene glycol, and Janus Green.

8. The method for a multilayer copper current collector as described in claim 7, wherein: The plating solution additives include the gelatin and the Janus Green; The concentration ratio of the gelatin to the phenazine is 20-800 ppm: 1-40 ppm.

9. A method for preparing the multilayer copper current collector as described in claim 1, wherein: The copper layer is deposited on at least one side of the base film using magnetron sputtering. During the magnetron sputtering process, a copper target is used as the target material, the target power is 10~15kW, the inert gas flow rate is 40~70mL / min, the coating vacuum degree is 0.05~0.1Pa, and the coating time is 4~6s.

10. A lithium battery cell, wherein: The electrode includes an electrode sheet comprising a multilayer copper current collector as described in any one of claims 1 to 7 or a multilayer copper current collector prepared by the method described in any one of claims 8 to 9, and an electrode active material located on the multilayer copper current collector.