Catalyst for trans-stereospecific polymerization of dienes, and preparation method therefor and use thereof
Magnesium chloride alcohol support precursors were prepared by chemically activating magnesium chloride, and the loading structure of transition metals on the support was controlled, which solved the problems of low catalytic efficiency and insufficient trans structure content of diene polymerization catalysts, and realized efficient diene polymerization.
Patent Information
- Application Number
- PCT/CN2026/096435
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing diene polymerization catalysts have low catalytic efficiency and insufficient trans structure content, making it difficult to meet industrial requirements.
Magnesium chloride ethanolate precursors were prepared by chemically activating magnesium chloride. Catalysts with different structures and components were prepared by controlling the loading structure of transition metals titanium and vanadium compounds on the support, restricting the spatial insertion sites of monomers, and increasing the content of trans structures.
The catalytic activity for diene polymerization reached 50–500 kg polymer/g transition metal/hour, with a trans structure content of over 95 mol%, even 99 mol%, and a weight-average molecular weight of 0.05–200 × 10⁴.
Smart Images

Figure CN2026096435_19112026_PF_FP_ABST
Abstract
Description
A catalyst for trans-directional polymerization of dienes, its preparation method and uses Technical Field
[0001] This invention belongs to the field of catalysts, specifically relating to catalysts for diene polymerization, and more specifically to a catalyst for the trans-directional polymerization of dienes, its preparation method, and its uses. The catalyst can improve the catalytic efficiency of diene polymerization and the content of the trans structure in the polymer. Background Technology
[0002] Anhydrous magnesium chloride (α-MgCl2) has a cubic close-packed layered structure, characterized by high crystallinity, low specific surface area, and lacks reactive groups with substances such as TiCl4. Therefore, to use it as a support for supported Ziegler-Natta catalysts, it must be activated, i.e., its crystal structure must be disrupted, its grain size reduced, and highly disordered δ-MgCl2 formed. MgCl2 support activation mainly employs two methods: physical grinding and chemical methods.
[0003] Titanium-supported Ziegler-Natta catalysts used for diene polymerization mostly employ a simple physical (grinding) activation method. This involves grinding the support (usually anhydrous MgCl2) and the active material (usually TiCl4) in a planetary ball mill, activating the support and simultaneously complexing the active material onto it. However, this method yields catalysts with low activity and uncontrollable particle morphology. Examples previously reported include: CN 105623001A (activity > 500 g polymer / g Ti / h, trans content > 97%), CN 108690156A (activity 523.6 g polymer / g Ti / h, trans content > 98%), and CN 113773426A (highest activity 3872 g polymer / g Ti / h, highest trans content 97.8%).
[0004] Therefore, in order to better meet the requirements of industrialization and reduce production costs, it is necessary to prepare a supported Ziegler-Natta catalyst with high efficiency and high orientation.
[0005] Compared to catalysts obtained by physical grinding activation, chemical activation can produce catalyst particles with good particle morphology and high specific surface area, resulting in higher polymerization activity. These catalysts are now widely used in the industrial production of α-olefins such as ethylene and propylene. However, there are few reports on supported Ziegler-Natta catalysts for diene polymerization prepared by chemical activation. CN 105504113A reports a dual-supported Ziegler-Natta catalyst prepared by adding SiO2 during chemical activation for isoprene polymerization, with a polymerization activity of 9.2 g polymer / g Cat / h and a trans content of 98.2%. CN 117467039A reports the preparation of an active MgCl2 support using Mg powder as raw material, supported on TiCl4, and used to catalyze isoprene polymerization, achieving a polymerization activity of 14740.35 g polymer / g Ti, but with a low trans content (93.2 mol%). Summary of the Invention
[0006] Based on the problems of low catalytic efficiency or low trans structure content of existing catalysts for diene polymerization, this invention discloses a special catalyst that uses a chemical method to activate magnesium chloride to obtain a magnesium chloride alcohol support precursor and uses it to prepare a catalyst, so as to achieve higher catalytic efficiency and polymer trans structure content for diene polymerization.
[0007] One objective of this invention is to provide a dedicated catalyst for improving the catalytic efficiency and trans-structure content in diene polymerization. Through the design of the main catalyst support and the construction of the catalyst system, the catalytic activity for diene polymerization reaches 50–500 kg polymer / g transition metal / hour, and the trans-structure content in diene polymerization reaches over 95 mol%, even reaching 99 mol%, with a weight-average molecular weight of 0.05–200 × 10⁻⁶. 4 .
[0008] Another object of the present invention is to provide a method for preparing such a catalyst.
[0009] Another object of the present invention is to provide the use of the catalyst for the polymerization of dienes, which enables the preparation of polyolefins with a high trans structure content.
[0010] To achieve the above objectives, this invention aims to enable the catalyst to efficiently catalyze diene polymerization to obtain polydiolefins with high trans-structure content. The novelty of this invention lies in the use of a novel process in the preparation of the main catalyst to prepare magnesium chloride alcoholic compound support precursors with different structures and alcohol contents, thereby preparing catalysts with different structures and compositions. Simultaneously, the spatial structure of transition metal titanium and / or vanadium compounds loaded on the support is controlled, thereby restricting the spatial insertion sites of monomers during diene polymerization and increasing the trans-structure content of the polydiolefin.
[0011] According to one aspect of the present invention, a catalyst for trans-directional polymerization of dienes is provided, wherein the catalyst comprises a transition metal compound, magnesium chloride (MgCl2), optional alkyl aluminum compound, optional electron donor, and other organic compounds, wherein, based on the total mass of the catalyst, the content of the transition metal element is 0.1–8.0 wt%, the content of MgCl2 is 15–30 wt%, the content of aluminum element is 0–10 wt%, the content of electron donor is 0–20 wt%, and the content of other organic compounds is 0–10 wt%.
[0012] In some embodiments, the catalyst is prepared by chemical reaction and complexation reaction in a solvent and dispersion medium from a transition metal compound, magnesium chloride MgCl2, optional alkyl aluminum, optional electron donor, and other organic compound.
[0013] In some embodiments, the transition metal compound is one or more compounds selected from titanium and vanadium, specifically one or more (e.g., two) selected from TiCl4, TiBr4, TiI4, VCl3, VBr3, VOCl3, VOBr3, VCl4, VBr4, and V2O5; the alkylaluminum compound is an alkylaluminum complexed on the catalyst surface, wherein the alkylaluminum is one or more (e.g., two) selected from triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, diisobutylaluminum chloride, dihexylaluminum chloride, and dioctylaluminum chloride; The organic compound is selected from one or more (e.g., two) of the following: n-hexane, cyclohexane, n-heptane, cycloheptane, n-octane, isooctane, toluene, xylene, low molecular weight trans-1,4-polyisoprene, low molecular weight trans-1,4-polybutadiene, low molecular weight trans-1,4-butadiene-isoprene copolymer, low molecular weight trans-1,4-im-pentadiene, and low molecular weight trans-1,4-butadiene-im-pentadiene copolymer, wherein the molecular weight of the low molecular weight polymer is less than 1000; the electron donor is selected from one or more (e.g., two) of the following: ester compounds, ether compounds, and siloxane compounds.
[0014] In some embodiments, the transition metal comprises V and Ti, wherein the molar ratio of V to Ti is 0 to 1:1.
[0015] In some embodiments, the catalyst is a solid particle with an average BET specific surface area of 30–70 m². 2 / g (e.g., 35, 40, 45, 50, 55, 60, 65m) 2 / g), with an average pore size of 40–1000 nm (e.g., 100, 200, 300, 400, 600, 800, 900 nm) and an average porosity of 30–80% (e.g., 35%, 45%, 55%, 65%, 75%).
[0016] According to the present invention, in the catalyst, transition metals, magnesium chloride (MgCl2), alkyl aluminum, electron donors, and other organic compounds may exist in complex form.
[0017] In some embodiments, the catalyst exhibits a catalytic activity of 50–500 kg polymer / g transition metal / hour for diene polymerization.
[0018] According to another aspect of the present invention, a method for preparing the catalyst is provided, comprising the following steps:
[0019] S1, Preparation of the carrier precursor, including:
[0020] S1-1, Preparation of metal chloride solution
[0021] Add anhydrous MgCl2 and dispersion medium to an anhydrous and oxygen-free reactor, stir and disperse, then heat to 40-100℃, add alcohol, heat again to 60-150℃, and stir at a constant temperature until MgCl2 is completely dissolved.
[0022] S1-2, Preparation of carrier particles
[0023] The system was then transferred to a low-temperature medium of 0℃ to -80℃ (e.g., -30℃, -50℃) to cool down, stirred, and an inert solvent at the same temperature as the system was added to the reactor. The stirring was continued until a large number of solid particles precipitated out. The mixture was then filtered and washed with an inert solvent to obtain the solid particles.
[0024] S1-3, Formation of the carrier precursor
[0025] Solid particles are gradually heated from 30°C to 40–250°C (e.g., 80°C, 100°C, 120°C, 150°C, 200°C) at a heating rate of 1–50°C / min (e.g., 10°C, 20°C, 30°C), with each gradient interval of 5–50°C (e.g., 10°C, 30°C, 45°C). Each gradient is held at a constant temperature for 30–600 min, while maintaining a vacuum of -0.01–-0.5 MPa (e.g., -0.02 MPa, -0.05 MPa, -0.1 MPa) during the heating process. At the final temperature of 40–250°C, the temperature and pressure are then held at -0.01–-0.5 MPa for 30–600 min to obtain the carrier precursor.
[0026] S2, the preparation of solid catalyst particles, includes:
[0027] S2-1: The carrier precursor prepared in S1 was added to an inert solvent under anhydrous and oxygen-free conditions at room temperature and dispersed by stirring at room temperature to obtain a suspension.
[0028] S2-2, the suspension obtained in S2-1 is cooled to -80 to 0°C (e.g., -50°C, -30°C, or -20°C), and a transition metal compound is added dropwise to the suspension at this temperature, wherein the mass ratio of the transition metal compound to the carrier precursor is 2:1 to 100:1; then the temperature is raised to 110 to 180°C (e.g., 110°C, 130°C) and the reaction is held at this temperature, followed by filtration; if necessary, an electron donor is added at 55 to 120°C (e.g., 70°C) during the heating process and the reaction is held at this temperature, followed by raising the temperature again to 110 to 180°C and holding the reaction at this temperature, followed by filtration;
[0029] S2-3: Add the same amount of transition metal compound as in S2-2 to the reactor, heat the reactor to 110-180℃ (e.g., 110℃, 130℃), and filter after reaction.
[0030] S2-4, add an inert solvent to the reactor, stir at -20 to 80°C, filter and wash, and dry the obtained powder solid under vacuum to obtain solid catalyst particles;
[0031] S3, Pretreatment of solid catalyst particles:
[0032] The solid catalyst particles obtained in step S2 are added to an inert solvent at room temperature, stirred and dispersed at room temperature to obtain a suspension, filtered and vacuum dried to obtain pretreated catalyst particles; if necessary, the above suspension is cooled to -10 to 20°C (e.g., 0°C, 10°C), alkyl aluminum is added, and optionally a single or mixed diene monomer is introduced, reacted at a constant temperature of -10 to 20°C (e.g., 0°C, 10°C), filtered and vacuum dried to obtain the pretreated catalyst.
[0033] In some embodiments, in the preparation of the carrier precursor S1, in S1-1, the mixture is stirred and dispersed at a speed of 10 to 1000 rpm (e.g., 300 to 800 rpm, especially 400, 500, or 600 rpm) for 5 to 100 min, and heated at a rate of 1 to 50 °C per minute.
[0034] In some embodiments, in step S1-1, the mass ratio of anhydrous MgCl2 to dispersion medium is 1:1 to 1:100 (e.g., 1:10, 1:20, 1:50, 1:80), and the dispersion medium is one or more (e.g., two) selected from n-nonane, n-decane, undecane, dodecane, white oil, paraffin oil, and kerosene.
[0035] In some embodiments, in step S1-1, the alcohol used is one or more (e.g., two) of saturated or unsaturated alcohols containing 1 to 20 carbon atoms, such as C2, C4, C6, and C8 alkyl alcohols, and the mass ratio of anhydrous MgCl2 to alcohol is 1:1 to 1:100 (e.g., 1:5).
[0036] In some embodiments, in step S1-1, anhydrous MgCl2 is added alone to the anhydrous and oxygen-free reactor or anhydrous MgCl2 is added to the reactor together with a portion of a transition metal (e.g., vanadium) compound.
[0037] In some embodiments, during the preparation of the carrier precursor S1, in S1-2, the mixture is stirred at a speed of 50 to 10,000 rpm (e.g., 2,000, 4,000, 6,000, 8,000 rpm), wherein the mass ratio of anhydrous MgCl2 to inert solvent is 1:1 to 1:100 (e.g., 1:10, 1:25, 1:50).
[0038] In some embodiments, in steps S1-2 of S1, the inert solvent used is one or more (e.g., two) selected from n-hexane, cyclohexane, n-heptane, cycloheptane, n-octane, isooctane, toluene, and xylene.
[0039] According to the present invention, in steps S1-3 of S1, the carrier precursor obtained is a magnesium chloride alkoxide with the structure MgCl2·nROH, wherein R is a C1-C20 alkyl group (e.g., C2, C4, C6, C8 alkyl group), and n is 0.01-6. Specifically, the magnesium chloride alkoxide has an average specific surface area of 20-70 m². 2 / g, with an average pore size of 40–1000 nm and an average porosity of 30–80%.
[0040] In some embodiments, the preparation S1 of the carrier precursor includes:
[0041] S1-1, Add anhydrous MgCl2 or a combination of it and vanadium compounds and a dispersion medium to an anhydrous and oxygen-free reactor, stir and disperse at a speed of 10-1000 rpm (e.g., 300-800 rpm, especially 400, 500, 600 rpm) for 5-100 min, heat to 40-100 °C at a heating rate of 1-50 °C / min, add alcohol, and heat again to 60-150 °C at a heating rate of 1-50 °C / min, and stir at a constant temperature for 0.5-5 h until MgCl2 is completely dissolved;
[0042] S1-2, then transfer the system to a low-temperature medium of 0℃ to -80℃ (e.g., -30℃, -50℃) to cool it down, and stir it at a speed of 50 to 10000 rpm (e.g., 2000, 4000, 6000, 8000 rpm) for 0.5 to 30 min. Then add an inert solvent at the same temperature as the system (0℃ to -80℃) into the reactor, wherein the mass ratio of anhydrous MgCl2 to inert solvent is 1:1 to 1:100 (e.g., 1:10, 1:25, 1:50). Continue stirring until a large number of solid particles precipitate out, filter to obtain solid particles, and wash the solid particles 1 to 3 times with excess inert solvent.
[0043] S1-3, then, the solid particles are heated from 30°C to 40-250°C (e.g., 100°C, 120°C, 150°C, 200°C) at a heating rate of 1-50°C / min (e.g., 10°C, 20°C, 30°C) with a gradient (each gradient interval is 5-50°C) and held at each gradient for 30-600 min. During the heating process, the vacuum degree is maintained at -0.01--0.5 MPa (e.g., -0.02 MPa, -0.05 MPa, -0.1 MPa). The temperature and pressure are then held at 40-250°C and -0.01--0.5 MPa for 30-600 min to obtain the carrier precursor.
[0044] In some embodiments, in the preparation of solid catalyst particles S2, in S2-1, the mass ratio of the support precursor to the inert solvent is 1:1 to 1:100 (e.g., 1:20, 1:40, 1:60).
[0045] In some embodiments, in step S2-2, the drop rate of the transition metal is 1 to 50 ml / min, and the mass ratio of the transition metal compound to the magnesium chloride alcohol carrier precursor is 10:1 to 50:1 (e.g., 20:1, 30:1, 40:1).
[0046] In some embodiments, in step S2-2, the electron donor is one or more selected from ester compounds, ether compounds, and siloxane compounds, with ethyl benzoate being an exemplary embodiment.
[0047] In some embodiments, during the preparation of solid catalyst particles S2, in S2-2 and S2-3, the temperature is increased at a rate of 0.1 to 50 °C / min (e.g., 2 °C / min, 5 °C / min, 10 °C / min), respectively.
[0048] In some embodiments, in the preparation of solid catalyst particles S2, in S2-4, the mass ratio of the support precursor to the inert solvent is 1:1 to 1:100 (e.g., 1:20, 1:40, 1:60), and / or the resulting powder solid is vacuum dried at 40 to 80°C (e.g., 50°C, 80°C) for 0.1 to 5 h.
[0049] In some embodiments, the preparation S2 of the solid catalyst particles includes:
[0050] S2-1, Under anhydrous and oxygen-free conditions at room temperature, the carrier precursor prepared above is added to an inert solvent, wherein the mass ratio of the carrier precursor to the inert solvent is 1:1 to 1:100 (e.g., 1:20, 1:40, 1:60), and the carrier precursor suspension is dispersed at room temperature with a stirring speed of 50 to 10000 rpm for 5 to 30 minutes.
[0051] S2-2: Cool the suspension obtained in S2-1 to -80 to 0°C (e.g., -50°C, -30°C, or -20°C). At this temperature, add a transition metal compound dropwise to the suspension at a rate of 1 to 50 ml / min. After the addition is complete, heat the reactor to 110 to 180°C (e.g., 110°C, 130°C) at a rate of 0.1 to 50°C / min (e.g., 2°C / min, 5°C / min, 10°C / min) and hold the temperature for 0.01 to 10 hours. Filter the solution. If necessary, an electron donor can be added at 55 to 120°C (e.g., 70°C) during the heating process and held at the temperature for 5 to 60 minutes. Then, heat the solution to 110 to 180°C (e.g., 110°C, 130°C) at a rate of 0.1 to 50°C / min and hold the temperature for 0.01 to 10 hours. Filter the solution.
[0052] S2-3, add the same amount of transition metal compound as in S2-2 to the reactor, heat the reactor to 110-180°C (e.g., 110°C, 130°C) at a heating rate of 0.1-50°C / min (e.g., 2°C / min, 5°C / min, 10°C / min), react for 0.01-10 hours, and then filter.
[0053] S2-4, add an inert solvent to the reactor, with a mass ratio of the support precursor to the inert solvent of 1:1 to 1:100 (e.g., 1:20, 1:40, 1:60). Stir at -20 to 80°C (e.g., 50°C) at a speed of 50 to 10000 rpm (e.g., 500 rpm, 1000 rpm, 2000 rpm) for 5 to 60 minutes. Filter and wash, repeat 5 times. The resulting powder solid is vacuum dried at 40 to 80°C (e.g., 50°C, 80°C) for 0.1 to 5 hours to obtain solid catalyst particles with MgCl2 as the support.
[0054] In some embodiments, during the pretreatment S3 of the solid catalyst particles, the molar ratio of aluminum to transition metal is 0.1 to 10:1 (e.g., 2:1, 4:1, 6:1).
[0055] In some embodiments, during the pretreatment S3 of the solid catalyst particles, the molar ratio of monomer to transition metal element is 0.1 to 100:1 (e.g., 5:1, 20:1). If the monomer is a mixture of two monomers, the molar ratio of monomers in the monomer mixture is 0.1:1 to 10:1 (e.g., 0.1:1, 1:1).
[0056] In some embodiments, during the pretreatment S3 of the solid catalyst particles, the diene monomer is butadiene, isoprene, isoprene, butadiene-isoprene mixture, or butadiene-isoprene mixture. In particular, the molar ratio of monomers in the monomer mixture is 0.1:1 to 10:1 (e.g., 0.1:1, 1:1).
[0057] In some embodiments, during the pretreatment S3 of the solid catalyst particles, the pretreated catalyst particles comprise transition metal compounds, magnesium chloride (MgCl2), alkyl aluminum compounds, electron donors, and other organic compounds.
[0058] In some embodiments, in step S3, the alkylaluminum is selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, diisobutylaluminum chloride, dihexylaluminum chloride, and dioctylaluminum chloride.
[0059] In some embodiments, the pretreatment S3 of the solid catalyst particles includes:
[0060] The solid catalyst particles obtained in step S2 are added to an inert solvent at room temperature, wherein the mass ratio of solid catalyst particles to inert solvent is 1:1 to 1:100 (e.g., 1:1, 1:5). The solid particle suspension is dispersed at room temperature with a stirring speed of 50 to 10,000 rpm (e.g., 500 rpm) for 5 to 30 minutes. The suspension is then filtered and vacuum dried at 40 to 80°C (e.g., 50°C) for 0.1 to 5 hours to obtain pretreated catalyst particles. If necessary, the suspension is cooled to -10 to 20°C (e.g., 0°C, 10°C), and alkyl aluminum is added, wherein the molar ratio of aluminum to transition metal is 0.1 to 10:1 (e.g., 2:1). The reaction mixture is prepared at a constant temperature for 0.1-30 minutes (4:1, 6:1), and optionally, butadiene, isoprene, isoprene, butadiene-isoprene mixture, or butadiene-isoprene mixture is introduced, wherein the molar ratio of monomer to transition metal element is 0.1-100:1 (e.g., 5:1, 20:1). The reaction is carried out at a constant temperature of -10-20℃ (e.g., 0℃, 10℃) for 0.1-30 minutes, filtered, and vacuum dried at 40-80℃ (e.g., 70℃, 80℃) for 0.1-5 hours to obtain pretreated catalyst particles; wherein the pretreated catalyst particles contain transition metal compounds, magnesium chloride (MgCl2), alkyl aluminum compounds, electron donors, and other organic compounds.
[0061] In some embodiments, according to the present invention, the transition metal compound may be one or more compounds selected from titanium and vanadium, specifically one or more selected from TiCl4, TiBr4, TiI4, VCl3, VBr3, VOCl3, VOBr3, VCl4, VBr4, and V2O5.
[0062] According to the present invention, in some embodiments, the pretreated catalyst particles obtained in step S3 are wherein the content of transition metal titanium and / or vanadium in the pretreated catalyst particles is 0.1 to 8.0 wt%, the content of magnesium is 15 to 30 wt%, the content of aluminum is 0 to 10 wt%, the content of electron donor in the solid particles is 0 to 20 wt%, and the content of other organic compounds is 0 to 10 wt%.
[0063] According to another aspect of the present invention, a catalyst prepared by the above method is provided, in particular, the catalyst having the characteristics of the catalyst described above.
[0064] According to another aspect of the invention, the use of the catalyst for the polymerization of dienes is provided to prepare polyolefins having a high trans structure content.
[0065] According to another aspect of the present invention, a method for polymerizing a diene is provided, comprising the following steps:
[0066] A measured amount of monomer, alkylaluminum, the catalyst or a catalyst prepared by the method, and a molecular weight regulator are sequentially added to a reactor that has been pre-treated to be anhydrous and oxygen-free, wherein the molar ratio of transition metal element to monomer in the catalyst is 0.001 to 100 × 10⁻⁶. -5 The molar ratio of alkylaluminum to transition metal elements in the catalyst is 5–800:1, the molar ratio of molecular weight regulator to monomer is 1:10–10000, and the reaction is carried out at 10–70 °C for 1 h. Subsequently, water or alcohol or other terminators are added to the reactor to terminate the polymerization. The polymer is then dried in a vacuum drying oven to constant weight to obtain diene homopolymer or copolymer.
[0067] According to the present invention, the molecular weight regulator is a conventional regulator in the art, such as hydrogen, alkyl zinc, alkoxy zinc, alkyl magnesium, alkyl aluminum, ethylene, propylene, propylene, 1,2-butadiene, cyclooctadiene, or one or more of alcohols, thiols, amines, phenols and their salts.
[0068] According to the polymerization method of the present invention, the content of trans-1,4-structure of diene monomer units in the obtained homopolymer or copolymer is 95 mol% or more, for example 98 mol% or more, or even 99 mol% or more, and the weight average molecular weight is 0.05 to 200 × 10⁻⁶. 4 .
[0069] The catalyst of this invention is applied to diene polymerization, particularly homopolymerization of isoprene, butadiene, and isoprene, copolymerization of butadiene-isoprene, butadiene-isoprene, and isoprene-isoprene, or copolymerization of any of the above diene monomers with styrene, ethylene, propylene, and butene, or more of them.
[0070] The key advantage of this invention's catalyst for diene polymerization is that the polymerization catalytic efficiency of the catalyst prepared using the magnesium chloride alcohol of this invention as a support precursor is significantly improved compared to catalysts using anhydrous magnesium chloride as a support precursor, reaching 50–500 kg polymer / g transition metal / hour. The content of the trans-1,4-structure of the diene monomer units in the homopolymer or copolymer is above 95 mol%, even reaching above 99 mol%, and the weight-average molecular weight is 0.05–200 × 10⁻⁶. 4 . Attached Figure Description
[0071] Figure 1 shows a scanning electron microscope (SEM) image of the magnesium chloride alcohol support precursor prepared in Example 1;
[0072] Figure 2 shows a scanning electron microscope (SEM) image of the solid catalyst particles prepared in Example 1. Detailed Implementation
[0073] The present invention will be further illustrated below with reference to specific embodiments. These embodiments are for illustrative purposes only and do not limit the scope of the invention. Furthermore, after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, which also fall within the scope defined by the appended claims.
[0074] Unless otherwise specified, the methods and apparatus used in this invention are conventional methods and apparatus in the art.
[0075] The test conditions are as follows:
[0076] The titanium content (wt%) in the catalyst was determined using a UV spectrophotometer.
[0077] The vanadium and aluminum content (wt%) in the catalyst was determined by inductively coupled plasma spectrometry (ICP spectrometry).
[0078] The specific surface area, average pore size, and porosity of the magnesium chloride alcohol precursor and catalyst were obtained based on nitrogen adsorption / desorption experiments and high-pressure mercury intrusion porosimetry.
[0079] Catalytic activity is calculated using the following formula:
[0080] CA = W 聚合物 / W 过渡金属 *10 -3 *t -1 kg 聚合物 ·(g 过渡金属 ) -1 ·h -1 Where CA represents the catalytic activity of the catalyst, and W 聚合物 W represents the mass (g) of the polymerization product. 过渡金属 t represents the amount of transition metal in the catalyst (g), and t represents the polymerization time (h).
[0081] Polymer trans-structure content (trans-1,4) and butadiene unit content (F) Bd )Depend on 1 The H-NMR spectrum was obtained through calculation.
[0082] Weight-average molecular weight (M w ) and molecular weight distribution (M w / M n The characteristics were obtained by gel permeation chromatography.
[0083] Example 1
[0084] 1) Preparation of the carrier precursor:
[0085] In a stirred reactor that has been treated to be anhydrous and oxygen-free, anhydrous magnesium chloride and n-decane are added at a mass ratio of 1:20, stirred and dispersed at 500 rpm for 5 min, heated to 60°C at a heating rate of 50°C / min, ethanol is added at a mass ratio of anhydrous MgCl2 to ethanol of 1:5, heated to 120°C at a heating rate of 50°C / min, and reacted at a constant temperature for 2 h, until MgCl2 is completely dissolved into a transparent solution.
[0086] The system was then rapidly transferred to a -30°C cryogenic medium for cooling. During the cooling process, the system was stirred at 2000 rpm. After cooling to -30°C, the system was stirred for 5 minutes. Then, -30°C n-heptane was added to the stirred reactor. The mass ratio of MgCl2 to n-heptane was 1:25. The system was stirred at 2000 rpm for 30 minutes. After a large number of solid particles precipitated, the solid particles were filtered out. The solid particles were then washed and filtered with n-heptane (the mass ratio of MgCl2 to n-heptane was 1:25). The washing and filtration were repeated twice.
[0087] The washed solid particles were heated from 30°C to 120°C at a rate of 10°C / min (with a gradient interval of 30°C between each gradient) and held at each gradient for 120 min. The vacuum degree was maintained at -0.05 MPa during the heating process. The temperature and pressure were then kept constant at 120°C and -0.05 MPa for 120 min to obtain a dried magnesium chloride alcoholic compound support precursor.
[0088] Tests showed that the average specific surface area of the magnesium chloride alcohol precursor was 49 m². 2 / g, with an average pore size of 201nm and a porosity of 62%. A scanning electron microscope (SEM) image of the magnesium chloride alcoholic compound support precursor is shown in Figure 1.
[0089] 2) Preparation of solid catalyst particles:
[0090] In a stirred reactor that has undergone anhydrous and oxygen-free treatment, the above-mentioned magnesium chloride alcohol precursor and n-heptane are added, wherein the mass ratio of magnesium chloride alcohol precursor to n-heptane is 1:20. The precursor suspension is stirred and dispersed at room temperature at a stirring speed of 500 rpm for 10 min. The reactor is then cooled to -20°C, and titanium tetrachloride is slowly added dropwise to the precursor suspension at a dropping rate of 5 ml / min at -20°C, wherein the mass ratio of magnesium chloride alcohol precursor to titanium tetrachloride is 1:20. After the addition is complete, the reactor is heated to 130°C at a heating rate of 2°C / min and reacted for 1 h. The liquid is then removed by filtration.
[0091] Subsequently, the same amount of titanium tetrachloride as above was added to the reactor, and the reactor was heated to 130°C at a heating rate of 2°C / min. The reaction was carried out for 1 hour, and the liquid was removed by filtration.
[0092] Finally, n-heptane (the mass ratio of magnesium chloride alcohol support precursor to n-heptane is 1:20) was added to the reactor, and the mixture was stirred and washed at 500 rpm for 10 min at 50 °C. The washing was repeated 5 times, and the resulting powder solid was vacuum dried at 50 °C for 2 h to obtain solid catalyst particles with MgCl2 as support.
[0093] Tests showed that the average specific surface area of the solid catalyst particles was 52 m². 2 / g, with an average pore size of 235nm and a porosity of 66%. A scanning electron microscope (SEM) image of the solid catalyst particles is shown in Figure 2.
[0094] 3) Pretreatment of solid catalyst particles:
[0095] The above-mentioned solid catalyst particles were added to toluene at room temperature, with a mass ratio of solid catalyst particles to toluene of 1:1. The solid particle suspension was dispersed at room temperature with a stirring speed of 500 rpm for 10 min. The suspension was then cooled to 10 °C, and triethylaluminum was added, with a molar ratio of aluminum to titanium supported on the solid catalyst particles of 2:1. The mixture was reacted at a constant temperature for 10 min. A butadiene-isoprene mixture was then introduced, with a molar ratio of monomer to titanium of 20:1 and a molar ratio of butadiene to isoprene of 0.1:1. The mixture was reacted at a constant temperature of 10 °C for 10 min, filtered, and vacuum dried at 70 °C for 2 h to obtain pretreated catalyst particles. The characterization of the pretreated catalyst particles is shown in Table 1.
[0096] 4) Butadiene-isoprene copolymerization:
[0097] The pretreated catalyst particles were used for butadiene-isoprene copolymerization: Butadiene-isoprene mixed monomers (with a titanium molar ratio of 3 × 10⁻⁶ to monomers) were sequentially added to a reactor that had been pre-treated to be anhydrous and oxygen-free. -5 The polymerization was carried out using butadiene and isoprene monomers in a molar ratio of 6:94, triethylaluminum (molar ratio of triethylaluminum to titanium in the catalyst was 80:1), pretreated catalyst particles, and hydrogen (molar ratio of hydrogen to monomer was 1:400). The reaction was carried out at 30°C for 1 hour. Subsequently, anhydrous ethanol was added to the reactor to terminate the polymerization. The polymer was then dried in a vacuum drying oven to constant weight to obtain the butadiene-isoprene copolymer.
[0098] The catalyst, polymerization parameters, and results are shown in Table 1.
[0099] Example 2
[0100] 1) Preparation of the carrier precursor:
[0101] In a stirred reactor that has been treated to be anhydrous and oxygen-free, anhydrous magnesium chloride and paraffin oil are added in a mass ratio of 1:1. The stirring is started and stirred at 500 rpm for 60 min to disperse the mixture evenly. The temperature is increased to 80°C at a heating rate of 40°C / min. Ethanol is added in a mass ratio of anhydrous MgCl2 to ethanol of 1:20. The temperature is increased again to 150°C at a heating rate of 30°C / min. The reaction is kept at a constant temperature for 0.5 h until the MgCl2 is completely dissolved into a transparent solution.
[0102] The system was then rapidly transferred to a 0°C medium for cooling. After stirring at 8000 rpm for 5 min, 0°C n-hexane was added to the stirred reactor, with a MgCl2 to n-hexane mass ratio of 1:100. The mixture was stirred at 8000 rpm for 10 min. After a large amount of solid particles precipitated, the solid particles were filtered out. The solid particles were then washed with n-hexane (MgCl2 to n-hexane mass ratio of 1:100), filtered, and the washing and filtration were repeated once.
[0103] The washed solid particles were heated from 30°C to 100°C at a rate of 50°C / min (with a gradient interval of 10°C between each gradient) and held at each gradient for 400 min. The vacuum degree was maintained at -0.01 MPa during the heating process. The temperature and pressure were then maintained at 100°C and -0.01 MPa for another 400 min to obtain a dried magnesium chloride alcoholic compound support precursor.
[0104] The average specific surface area of the magnesium chloride alcoholic compound carrier precursor was tested to be 63 m². 2 / g, with an average pore size of 249nm and a porosity of 71%.
[0105] 2) Preparation of solid catalyst particles:
[0106] The mass ratio of magnesium chloride alcoholic polymer carrier precursor to titanium tetrachloride was 1:40, and other aspects were the same as in Example 1.
[0107] Tests showed that the average specific surface area of the solid catalyst particles was 65 m². 2 / g, with an average pore size of 301nm and a porosity of 76%.
[0108] 3) Pretreatment of solid catalyst particles:
[0109] Similar to Example 1, except that triethylaluminum was replaced with triisobutylaluminum. The characterization of the pretreated catalyst particles is shown in Table 1.
[0110] 4) Butadiene-isoprene copolymerization:
[0111] Same as Example 1. Catalyst, polymerization parameters, and results are shown in Table 1.
[0112] Example 3
[0113] 1) Preparation of the carrier precursor:
[0114] Same as Example 2, except that anhydrous magnesium chloride is replaced with a 1:1 mass ratio mixture of anhydrous magnesium chloride and anhydrous vanadium tetrachloride.
[0115] 2) Preparation of solid catalyst particles:
[0116] In a stirred reactor that has undergone anhydrous and oxygen-free treatment, the above-mentioned carrier precursor and xylene are added, wherein the mass ratio of the carrier precursor to xylene is 1:20. The carrier precursor suspension is stirred at 1000 rpm for 20 min at room temperature to disperse it. The reactor is then cooled to -20℃, and titanium tetrachloride is slowly added dropwise to the carrier suspension at -20℃ at a dropwise rate of 5 ml / min, with a mass ratio of carrier precursor to titanium tetrachloride of 1:40. After the addition is complete, the reactor is heated to 70℃ at a heating rate of 2℃ / min. Ethyl benzoate is added and reacted at a constant temperature for 30 min, with a molar ratio of ethyl benzoate to carrier precursor of 0.1. After the reaction is complete, the temperature is further increased to 110℃ at a heating rate of 2℃ / min and reacted for 1 h. The mixture is then filtered.
[0117] Subsequently, the same amount of titanium tetrachloride was added to the reactor, and the reactor was heated to 110°C at a heating rate of 2°C / min. The reaction was carried out for 1 hour, and then filtered.
[0118] Finally, xylene (mass ratio of carrier precursor to xylene is 1:20) was added to the reactor, and the mixture was stirred and washed at 500 rpm for 10 min at 50 °C. The washing was repeated 5 times, and the resulting powder solid was vacuum dried at 80 °C for 2 h to obtain solid particles.
[0119] Tests showed that the average specific surface area of the solid catalyst particles was 70 m². 2 / g, with an average pore size of 291nm and a porosity of 70%.
[0120] 3) Pretreatment of solid catalyst particles:
[0121] The above-mentioned solid catalyst particles were added to toluene at room temperature, with a mass ratio of solid catalyst particles to toluene of 1:1. The solid particle suspension was dispersed at room temperature with a stirring speed of 500 rpm for 10 min. The suspension was then cooled to 0 °C, and monochlorodiisobutylaluminum was added, with a molar ratio of aluminum to transition metal of 6:1. The mixture was reacted at a constant temperature for 10 min. A butadiene-isoprene mixture was then introduced, with a molar ratio of monomer to transition metal of 5:1 and a molar ratio of butadiene to isoprene of 0.5:1. The mixture was reacted at a constant temperature of 0 °C for 10 min, filtered, and vacuum dried at 70 °C for 2 h to obtain pretreated catalyst particles. The characterization of the pretreated catalyst particles is shown in Table 1.
[0122] 4) Butadiene-isoprene copolymerization:
[0123] Same as Example 1. Catalyst, polymerization parameters, and results are shown in Table 1.
[0124] Example 4
[0125] 1) Preparation of the carrier precursor:
[0126] In a stirred reactor that has been treated to be anhydrous and oxygen-free, anhydrous magnesium chloride and n-nonane are added at a mass ratio of 1:50. The stirring is started and dispersed at 500 rpm for 10 min. The temperature is increased to 60°C at a heating rate of 20°C / min. Ethanol is added at a mass ratio of anhydrous MgCl2 to ethanol of 1:2. The temperature is increased again to 150°C at a heating rate of 20°C / min. The reaction is kept at a constant temperature for 1 h until MgCl2 is completely dissolved into a transparent solution.
[0127] The system was then rapidly transferred to a -50°C low-temperature medium for cooling. After stirring at 2000 rpm for 5 min, -50°C n-octane was added to the stirred reactor. The mass ratio of MgCl2 to n-octane was 1:25. The mixture was stirred at 2000 rpm for 10 min. After a large amount of solid particles precipitated, the solid particles were obtained by filtration. The solid particles were washed and filtered with n-octane (mass ratio of MgCl2 to n-octane was 1:25). The washing and filtration were repeated 3 times.
[0128] The washed solid particles were heated from 30°C to 120°C at a rate of 1°C / min (with a gradient interval of 45°C between each gradient) and held at each gradient for 540 min. The vacuum degree was maintained at -0.02 MPa during the heating process. The temperature and pressure were then maintained at 120°C and -0.02 MPa for 540 min to obtain a dried magnesium chloride alcoholic compound support precursor.
[0129] The average specific surface area of the magnesium chloride alcohol precursor was tested to be 39 m². 2 / g, with an average pore size of 850nm and a porosity of 35%.
[0130] 2) Preparation of solid catalyst particles:
[0131] Same as Example 1.
[0132] The average specific surface area of the solid particles was measured to be 34 m². 2 / g, with an average pore size of 883nm and a porosity of 33%.
[0133] 3) Pretreatment of solid catalyst particles:
[0134] The above-mentioned solid catalyst particles were added to xylene at room temperature, wherein the mass ratio of solid catalyst particles to xylene was 1:5. The catalyst particle suspension was dispersed at room temperature with a stirring speed of 500 rpm for 10 min, filtered, and vacuum dried at 80 °C for 2 h to obtain pretreated catalyst particles. The characterization of the pretreated catalyst particles is shown in Table 1.
[0135] 4) Butadiene-isoprene copolymerization:
[0136] Same as Example 1. Catalyst, polymerization parameters, and results are shown in Table 1.
[0137] Comparative Example 1
[0138] 1) Preparation of the carrier precursor:
[0139] The washed solid particles were heated from 30°C to 120°C at a heating rate of 10°C / min (non-gradient heating). During the heating process, the vacuum degree was maintained at -0.05 MPa. The temperature and pressure were kept constant at 120°C and -0.05 MPa for 120 min to obtain a dried magnesium chloride alcoholic compound carrier precursor. The rest of the process was the same as in Example 1.
[0140] Tests showed that the average specific surface area of the magnesium chloride alcoholic compound carrier precursor was 26 m². 2 / g, with an average pore size of 140nm and a porosity of 44%.
[0141] 2) Preparation of solid catalyst particles:
[0142] Same as Example 1.
[0143] Tests showed that the average specific surface area of the solid catalyst particles was 35 m². 2 / g, with an average pore size of 209nm and a porosity of 49%.
[0144] 3) Pretreatment of solid catalyst particles:
[0145] Same as in Example 1. Characterization of the pretreated catalyst particles is shown in Table 1.
[0146] 4) Butadiene-isoprene copolymerization:
[0147] Same as Example 1. Catalyst, polymerization parameters, and results are shown in Table 1.
[0148] Comparative Example 2
[0149] 1) Preparation of solid catalyst particles:
[0150] Referring to Example 2 of patent CN 113773426A (where the magnesium salt used is anhydrous MgCl2, the titanium solution is TiCl4, the liquid alkane is n-heptane, the solid alkane is solid paraffin, and the alkyl aluminum is triethylaluminum), using traditional anhydrous magnesium chloride as a carrier precursor, TiCl4 was loaded onto the surface of MgCl2 by physical grinding to obtain solid catalyst particles.
[0151] Tests showed that the average specific surface area of the solid catalyst particles was 70 m². 2 / g, with an average pore size of 480nm and a porosity of 50%.
[0152] 2) Pretreatment of solid catalyst particles:
[0153] Same as in Example 1. Characterization of the pretreated catalyst particles is shown in Table 1.
[0154] 3) Butadiene-isoprene copolymerization:
[0155] Same as Example 1. Catalyst, polymerization parameters, and results are shown in Table 1.
[0156] Table 1. Example Data
[0157] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A catalyst for the trans-directing polymerization of a diene, wherein, The catalyst comprises a transition metal compound, magnesium chloride (MgCl2), optional alkyl aluminum compound, optional electron donor, and other organic compounds. Based on the total mass of the catalyst, the content of the transition metal element is 0.1–8.0 wt%, the content of MgCl2 is 15–30 wt%, the content of aluminum element is 0–10 wt%, the content of electron donor is 0–20 wt%, and the content of other organic compounds is 0–10 wt%.
2. The catalyst according to claim 1, wherein, The transition metal compound is one or more compounds selected from titanium and vanadium, specifically one or more selected from TiCl4, TiBr4, TiI4, VCl3, VBr3, VOCl3, VOBr3, VCl4, VBr4, and V2O5; The alkylaluminum compound is an alkylaluminum complexed on the catalyst surface, wherein the alkylaluminum is selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, diisobutylaluminum chloride, dihexylaluminum chloride, and dioctylaluminum chloride. The other organic compounds are selected from one or more of the following: n-hexane, cyclohexane, n-heptane, cycloheptane, n-octane, isooctane, toluene, xylene, low molecular weight trans-1,4-polyisoprene, low molecular weight trans-1,4-polybutadiene, low molecular weight trans-1,4-butadiene-isoprene copolymer, low molecular weight trans-1,4-im-pentadiene, and low molecular weight trans-1,4-butadiene-im-pentadiene copolymer, wherein the molecular weight of the low molecular weight polymer is less than 1000. The electron donor is selected from one or more of ester compounds, ether compounds, and siloxane compounds.
3. The catalyst according to claim 1, wherein, The transition metal comprises V and Ti, wherein the molar ratio of V to Ti is 0 to 1:
1.
4. The catalyst according to claim 1, wherein, The catalyst is a solid particle having an average BET specific surface area of 30 to 70 m 2 / g, an average pore diameter of 40 to 1000 nm, and an average porosity of 30 to 80%; and / or The catalyst exhibits a catalytic activity of 50–500 kg polymer / g transition metal / hour for diene polymerization.
5. A method for preparing a catalyst, comprising the following steps: S1, Preparation of the carrier precursor, including: S1-1, Preparation of metal chloride solution Add anhydrous MgCl2 and dispersion medium to an anhydrous and oxygen-free reactor, stir and disperse, then heat to 40-100℃, add alcohol, heat again to 60-150℃, and stir at a constant temperature until MgCl2 is completely dissolved. S1-2, Preparation of carrier particles The system was then transferred to a low-temperature medium of 0℃ to -80℃ to cool down, stirred, and an inert solvent at the same temperature as the system was added to the reactor. The stirring was continued until a large number of solid particles precipitated out. The mixture was then filtered and washed with an inert solvent to obtain the solid particles. S1-3, Formation of the carrier precursor The solid particles were gradually heated from 30°C to 40–250°C at a heating rate of 1–50°C / min, with each gradient interval of 5–50°C. The temperature was held at each gradient for 30–600 min, and the vacuum degree was maintained at -0.01–-0.5 MPa during the heating process. At the final temperature of 40–250°C, the temperature and pressure were held at -0.01–-0.5 MPa for 30–600 min to obtain the carrier precursor. S2, the preparation of solid catalyst particles, includes: S2-1: The carrier precursor prepared in S1 was added to an inert solvent under anhydrous and oxygen-free conditions at room temperature and dispersed by stirring at room temperature to obtain a suspension. S2-2, the suspension obtained in S2-1 is cooled to -80 to 0°C, and a transition metal compound is added dropwise to the suspension at this temperature, wherein the mass ratio of the transition metal compound to the carrier precursor is 2:1 to 100:1; then the temperature is raised to 110 to 180°C and the reaction is held at a constant temperature, followed by filtration; optionally, an electron donor is added at 55 to 120°C during the heating process and the reaction is held at a constant temperature, followed by raising the temperature again to 110 to 180°C and the reaction is held at a constant temperature, followed by filtration; S2-3: Add the same amount of transition metal compound as in S2-2 to the reactor, heat the reactor to 110-180°C, and filter after the reaction. S2-4, add an inert solvent to the reactor, stir at -20 to 80°C, filter and wash, and dry the obtained powder solid under vacuum to obtain solid catalyst particles; S3, Pretreatment of solid catalyst particles: The solid catalyst particles obtained in step S2 are added to an inert solvent at room temperature, stirred and dispersed at room temperature to obtain a suspension, filtered and vacuum dried to obtain pretreated catalyst particles; optionally, the above suspension is cooled to -10 to 20°C, alkyl aluminum is added, and optionally a single or mixed diene monomer is introduced, reacted at a constant temperature of -10 to 20°C, filtered and vacuum dried to obtain a pretreated catalyst.
6. The method according to claim 5, wherein, In the preparation of the carrier precursor S1, In S1-1, stir and disperse at a speed of 10-1000 rpm for 5-100 min, and increase the temperature at a rate of 1-50℃ / min; and / or In S1-1, the alcohol used is one or more saturated or unsaturated alcohols containing 1 to 20 carbon atoms, and the mass ratio of anhydrous MgCl2 to alcohol is 1:1 to 1:100; and / or In S1-1, anhydrous MgCl2 is added alone to the anhydrous and oxygen-free reactor, or anhydrous MgCl2 is added to the reactor together with a portion of a transition metal compound (preferably a vanadium compound, such as vanadium tetrachloride); and / or In S1-2, stirring is performed at a speed of 50–10000 rpm, wherein the mass ratio of anhydrous MgCl2 to inert solvent is 1:1 to 1:100; and / or In S1-2, the inert solvent used is one or more selected from n-hexane, cyclohexane, n-heptane, cycloheptane, n-octane, isooctane, toluene, and xylene; and / or In S1-3, the resulting support precursor is a magnesium chloride alcohol compound with the structure MgCl2·nROH, where R is a C1-C20 alkyl group and n is 0.01-6. Specifically, in the preparation S1 of the carrier precursor, the following steps are included: S1-1, Add anhydrous MgCl2 or a combination of it and vanadium compounds and a dispersion medium to an anhydrous and oxygen-free reactor, stir and disperse at a speed of 10-1000 rpm for 5-100 min, heat to 40-100℃ at a heating rate of 1-50℃ / min, add alcohol, and heat again to 60-150℃ at a heating rate of 1-50℃ / min, and stir at a constant temperature for 0.5-5 h until MgCl2 is completely dissolved; S1-2, transfer the system to a low-temperature medium of 0℃ to -80℃ to cool it down, stir it at a speed of 50 to 10000 rpm for 0.5 to 30 min, add an inert solvent at the same temperature as the system into the reactor, wherein the mass ratio of anhydrous MgCl2 to inert solvent is 1:1 to 1:100, continue stirring until a large number of solid particles precipitate, filter to obtain solid particles, and wash the solid particles 1 to 3 times with excess inert solvent; S1-3, the solid particles are gradually heated from 30℃ to 40-250℃ at a heating rate of 1-50℃ / min, and held at each temperature gradient for 30-600min. During the heating process, the vacuum degree is maintained at -0.01 to -0.5MPa. The temperature and pressure are then kept constant at 40-250℃ and -0.01 to -0.5MPa for 30-600min to obtain the carrier precursor.
7. The method according to claim 5 or 6, wherein, In the preparation of solid catalyst particles S2, In S2-1, the mass ratio of the carrier precursor to the inert solvent is 1:1 to 1:100; and / or In S2-2, the dropping rate of the transition metal is 1–50 ml / min, and the mass ratio of the transition metal compound to the magnesium chloride alkoxide carrier precursor is 10:1–50:1; and / or In S2-2, the electron donor is one or more selected from ester compounds, ether compounds, and siloxane compounds, such as ethyl benzoate; and / or In S2-2 and S2-3, the temperature is increased at a rate of 0.1–50 °C / min, respectively; and / or In S2-4, the mass ratio of the carrier precursor to the inert solvent is 1:1 to 1:100, and / or, In S2-4, the obtained powder solid was vacuum dried at 40–80 °C for 0.1–5 h; Specifically, in the preparation of solid catalyst particles S2, the following steps are included: S2-1, Under anhydrous and oxygen-free conditions at room temperature, the carrier precursor prepared above is added to an inert solvent, wherein the mass ratio of the carrier precursor to the inert solvent is 1:1 to 1:100, and the carrier precursor suspension is dispersed at room temperature with a stirring speed of 50 to 10000 rpm for 5 to 30 minutes. S2-2: Cool the suspension obtained in S2-1 to -80 to 0°C. At this temperature, add a transition metal compound dropwise to the suspension at a rate of 1 to 50 ml / min. After the addition is complete, heat the reactor to 110 to 180°C at a rate of 0.1 to 50°C / min and hold the temperature for 0.01 to 10 hours. Filter the solution. If necessary, add an electron donor at 55 to 120°C during the heating process and hold the temperature for 5 to 60 minutes. Then, heat the solution to 110 to 180°C at a rate of 0.1 to 50°C / min and hold the temperature for 0.01 to 10 hours. Filter the solution. S2-3: Add the same amount of transition metal compound as in S2-2 to the reactor. Heat the reactor to 110-180°C at a heating rate of 0.1-50°C / min. React for 0.01-10 hours and then filter. S2-4, add an inert solvent to the reactor, with a mass ratio of the support precursor to the inert solvent of 1:1 to 1:100, stir at 50 to 10000 rpm for 5 to 60 min at -20 to 80 °C, filter and wash, repeat 5 times, and dry the obtained powder solid under vacuum at 40 to 80 °C for 0.1 to 5 h to obtain solid catalyst particles with MgCl2 as support; Specifically, the transition metal compound is one or more compounds selected from titanium and vanadium, specifically one or more selected from TiCl4, TiBr4, TiI4, VCl3, VBr3, VOCl3, VOBr3, VCl4, VBr4, and V2O5.
8. The method according to any one of claims 5 to 7, wherein, In the pretreatment S3 of the solid catalyst particles, the molar ratio of aluminum to transition metal elements is 0.1–10:1; and / or In the pretreatment S3 of the solid catalyst particles, the molar ratio of monomer to transition metal element is 0.1–100:1; if the monomer is a mixture of two monomers, the molar ratio of monomers in the monomer mixture is 0.1:1–10:1; and / or In the pretreatment S3 of the solid catalyst particles, the diene monomer is butadiene, isoprene, isoprene, a mixture of butadiene and isoprene, or a mixture of butadiene and isoprene; particularly, the molar ratio of monomers in the monomer mixture is 0.1:1 to 10:1; and / or In the pretreatment S3 of the solid catalyst particles, the alkyl aluminum is selected from one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, diisobutylaluminum chloride, dihexylaluminum chloride, and dioctylaluminum chloride. Specifically, the pretreatment S3 of the solid catalyst particles includes: The solid catalyst particles obtained in step S2 are added to an inert solvent at room temperature, wherein the mass ratio of solid catalyst particles to inert solvent is 1:1 to 1:
100. The solid particle suspension is dispersed at room temperature with a stirring speed of 50 to 10,000 rpm for 5 to 30 minutes. After filtration, the suspension is vacuum dried at 40 to 80°C for 0.1 to 5 hours to obtain pretreated catalyst particles. If necessary, the suspension is cooled to -10 to 20°C, and alkyl aluminum is added, wherein the molar ratio of aluminum to transition metal is 0.1 to 10:
1. The mixture is then kept at a constant temperature. The reaction is carried out for 0.1-30 minutes, optionally with the introduction of butadiene, isoprene, isoprene, a mixture of butadiene and isoprene, or a mixture of butadiene and isoprene, wherein the molar ratio of monomer to transition metal element is 0.1-100:1, and the reaction is carried out at a constant temperature of -10-20°C for 0.1-30 minutes. The mixture is then filtered and vacuum dried at 40-80°C for 0.1-5 hours to obtain pretreated catalyst particles; wherein the pretreated catalyst particles contain transition metal compounds, magnesium chloride (MgCl2), alkyl aluminum compounds, electron donors, and other organic compounds.
9. A catalyst prepared by the method of claims 5 to 8, wherein the catalyst contains 0.1 to 8.0 wt% transition metal titanium and / or vanadium, 15 to 30 wt% magnesium chloride, 0 to 10 wt% aluminum, 0 to 20 wt% electron donor in the solid particles, and 0 to 10 wt% other organic compounds.
10. Use of the catalyst according to any one of claims 1 to 4 or the catalyst according to claim 9 for the polymerization of dienes to prepare polyolefins having a high trans-structure content; or A method for polymerizing a diene, comprising the following steps: A monomer, alkylaluminum, a catalyst according to any one of claims 1 to 4 or a catalyst according to claim 9, and a molecular weight regulator are sequentially added to a reactor that has undergone pre-treatment to be anhydrous and oxygen-free. The molar ratio of the transition metal element to the monomer in the catalyst is 0.001 to 100 × 10⁻⁶. -5 The molar ratio of alkylaluminum to transition metal elements in the catalyst is 5–800:1, the molar ratio of molecular weight regulator to monomer is 1:10–10000, and the reaction is carried out at 10–70 °C for 1 h. Subsequently, water or alcohol terminator is added to the reactor to terminate the polymerization. The polymer is dried in a vacuum drying oven to constant weight to obtain diene homopolymer or copolymer. In particular, the content of trans-1,4-structures in the diene monomer units in the resulting homo- or copolymer is 95 mol-% or more, such as 98 mol-% or more, even up to 99 mol-% or more, and the weight average molecular weight is in the range of 0.05 to 200 x 10 4 ; Specifically, the polymerization is a homopolymerization of isoprene, butadiene, and isoprene; a copolymerization of butadiene-isoprene, butadiene-isoprene, and isoprene-isoprene; or a copolymerization of any of the above diene monomers with styrene, ethylene, propylene, and butene, or any one or more of them.