Composite lithium supplementation material and preparation method therefor, positive electrode sheet, battery and electronic device

WO2026238046A1PCT designated stage Publication Date: 2026-11-19BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/096968
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-14
Publication Date
2026-11-19

Smart Images

  • Figure CN2026096968_19112026_PF_FP_ABST
    Figure CN2026096968_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A composite lithium supplementation material and a preparation method therefor, a positive electrode sheet, a battery and an electronic device. The composite lithium supplementation material comprises a lithium-rich compound core and a coating layer coated on at least a portion of the surface of the lithium-rich compound core. The coating layer comprises LiyAlzPO4-xF1+x, where 0≤x<4, y>0 and z>0. The composite lithium supplementation material of the present application comprises the lithium-rich compound core and the coating layer, such that a battery manufactured by using the composite lithium supplementation material has higher charge specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Composite lithium supplementation materials and their preparation methods, cathode sheets, batteries, and electronic devices.

[0001] This application claims priority to Chinese Patent Application No. 202510625980.2, filed on May 14, 2025, entitled "Composite Lithium Supplementation Material and Preparation Method Thereof, Positive Electrode Sheet, Battery, Electronic Device", the entire contents of which are incorporated herein by reference.

[0002] This application claims priority to Chinese Patent Application No. 202510633944.0, filed on May 15, 2025, entitled "Lithium Supplement Agent and Preparation Method Thereof, Positive Electrode Sheet, Battery, Battery Pack and Electrical Equipment", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of battery technology, and in particular to a composite lithium replenishment material and its preparation method, a positive electrode, a battery, and electronic equipment. Background Technology

[0004] Lithium-rich compounds possess high theoretical specific capacity and can be used as positive electrode lithium replenishment materials in lithium-ion batteries to compensate for irreversible capacity loss during the first cycle and improve battery cycle life. However, lithium-rich compounds readily react with H2O and CO2 in the air, which not only reduces their electrochemical activity but also generates residual alkali that can lead to gas production in the battery, posing a safety hazard.

[0005] To address these issues, existing technologies employ methods such as coating and doping to modify lithium-rich compounds, with TiO2 and Li3PO4 being common modifying materials. However, the modified lithium-rich compound materials have not achieved the expected improvement in battery specific capacity. Summary of the Invention

[0006] The first aspect of this application provides a composite lithium replenishment material with a stable structure, which is beneficial to improving the charging capacity of the battery.

[0007] The second aspect of this application provides a method for preparing a composite lithium replenishment material. The composite lithium replenishment material prepared by this method has a stable structure, which is beneficial to improving the charging capacity of the battery.

[0008] A third aspect of this application provides a positive electrode sheet, which, since it is made from the aforementioned composite lithium-filling material, is beneficial for improving the charging capacity of the battery.

[0009] The fourth aspect of this application provides a battery that, since it is made from the aforementioned positive electrode sheet, has a high charge capacity.

[0010] The fifth aspect of this application provides an electronic device that, since it is made from the aforementioned battery, has a long standby time.

[0011] The first aspect of this application provides a composite lithium supplement material, comprising:

[0012] A lithium-rich compound core and a coating layer covering at least a portion of the surface of the lithium-rich compound core, the coating layer comprising Li y Al z PO 4- x F 1+x Where 0 ≤ x < 4, y > 0, z > 0.

[0013] The composite lithium replenishment material as described above, wherein the lithium-rich compound core comprises a core layer and a transition layer covering at least a portion of the surface of the core layer, the core layer comprising a lithium-rich compound, and the transition layer comprising an element-doped lithium-rich compound, wherein the element comprises at least one of P, Al, and F.

[0014] The composite lithium supplementation material described above, wherein y:z = 1-10:1.

[0015] The composite lithium supplementation material as described above, wherein 0.02≤x≤0.1; and / or 0.5≤y≤3; and / or 0.1≤z≤1.

[0016] In the composite lithium-supplementing material described above, the mass of the coating layer accounts for 0.1-2% of the mass of the lithium-rich compound core; and / or, the thickness of the coating layer is 1-500 nm.

[0017] The composite lithium supplementation material as described above, wherein the Li y Al z PO 4-x F 1+x The particle size Dn50 satisfies: 1nm≤Dn50≤50nm.

[0018] The composite lithium-rich material described above, wherein the element-doped lithium-rich compound has at least one of a layered structure, a rock-salt-like structure, and a spinel-like structure.

[0019] In the composite lithium supplementation material described above, the mass percentage of P element in the transition layer is 0.1-20.8% of the mass of the transition layer; and / or, the mass percentage of Al element in the transition layer is 0.1-18.2% of the mass of the transition layer; and / or, the mass percentage of F element in the transition layer is 0.1-12.8% of the mass of the transition layer.

[0020] In the composite lithium replenishment material described above, the thickness of the transition layer is 2-499 nm.

[0021] The composite lithium-rich material as described above, wherein the lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0022] In the composite lithium supplementation material described above, the particle size Dn50 of the lithium-rich compound satisfies: 500nm≤Dn50≤15μm.

[0023] A second aspect of this application provides a method for preparing a composite lithium supplement material, comprising:

[0024] In an oxygen atmosphere, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mixture is calcined to obtain the composite lithium supplement material.

[0025] In the preparation method described above, the lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1-2.

[0026] In the preparation method described above, the calcination temperature is 200-800℃ and the calcination time is 0.5-6h.

[0027] In the preparation method described above, the calcination temperature is 300-600℃ and the calcination time is 2-6h.

[0028] The composite lithium-supplementing material described above, wherein, prior to calcination, further includes: reacting the lithium-rich compound with Li... y Al z PO 4-x F 1+x The solvent is mixed and then spray-dried to obtain the mixture; the spray-drying conditions include:

[0029] The pressure is 0.2-1 MPa; and / or the inlet temperature is 100-300℃; and / or the outlet temperature is 80-100℃; and / or the feed rate is 0.5-2 L / h.

[0030] A third aspect of this application provides a positive electrode sheet comprising the aforementioned composite lithium-replenishing material, or the composite lithium-replenishing material prepared by the aforementioned method.

[0031] A fourth aspect of this application provides a battery including the aforementioned positive electrode.

[0032] The fifth aspect of this application provides an electronic device including the battery described above.

[0033] The composite lithium-rich material of this application includes a lithium-rich compound core and a coating layer (Li). y Al z PO 4-x F 1+x The coating layer not only acts as a physical barrier to isolate water and carbon dioxide from the lithium-rich compound core, but also provides structural stability, suppressing side reactions and ensuring the structural stability of the core. Furthermore, the coating layer enables efficient lithium-ion conduction. Therefore, the composite lithium replenishment material of this application can effectively improve the specific charging capacity of the battery.

[0034] The main objective of this application is to provide a lithium replenishing agent that has high stability and excellent kinetic performance, which is beneficial to the utilization of the charging capacity of the lithium replenishing agent, improves the lithium replenishing effect of the lithium replenishing agent, and enhances the cycle performance of the battery.

[0035] This application also provides a method for preparing a lithium replenishing agent, which is capable of preparing the above-mentioned lithium replenishing agent and has a simple process and low cost.

[0036] This application also provides a positive electrode sheet comprising the above-mentioned lithium replenishing agent or a lithium replenishing agent prepared by the above-mentioned lithium replenishing agent preparation method. Therefore, when this positive electrode sheet is applied to a battery, the cycle performance of the battery can be improved.

[0037] This application also provides a battery comprising the above-described lithium replenishing agent, or a lithium replenishing agent prepared according to the above-described method for preparing the lithium replenishing agent, or the above-described positive electrode sheet; therefore, the battery has excellent cycle performance.

[0038] This application also provides a battery pack comprising the above-mentioned lithium replenishing agent, or a lithium replenishing agent prepared according to the above-mentioned lithium replenishing agent preparation method, or the above-mentioned positive electrode sheet, or the above-mentioned battery, and therefore, the battery pack has excellent cycle performance.

[0039] This application also provides an electrical device, including the above-mentioned lithium replenishing agent, or a lithium replenishing agent prepared according to the above-mentioned lithium replenishing agent preparation method, or the above-mentioned positive electrode sheet, or the above-mentioned battery, or the above-mentioned battery pack. Therefore, the battery performance of the electrical device is superior.

[0040] In a sixth aspect, this application provides a lithium replenishing agent, including a lithium replenishing material and a coating layer present on the surface of the lithium replenishing material, the coating layer including a lithium-containing fluoride.

[0041] The lithium supplement described above, wherein the lithium-containing fluoride has the chemical formula Li. x M y F zWhere 0 < x ≤ 3, 0 < y ≤ 1, 0 < z ≤ 6, and M is selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga.

[0042] The lithium supplement agent as described above, wherein the lithium-containing fluoride includes at least one of LiAlF4, Li3AlF6, Li2ZrF6, Li2TiF6, Li2SiF6, LiSbF6, LiBiF4, LiInF4 and LiGaF4, preferably LiAlF4 and / or Li3AlF6.

[0043] In the lithium replenishing agent described above, the lithium-containing fluoride accounts for 0.1%-10% of the lithium replenishing agent by mass, preferably 0.5%-2%;

[0044] And / or, the thickness of the coating layer is 1nm-500nm.

[0045] The lithium replenishing agent as described above includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4;

[0046] And / or, the particle size Dn50 of the lithium replenishment material is 500nm-15μm.

[0047] The lithium replenishing agent as described above, wherein the lithium replenishing material comprises a core and a transition layer, the transition layer being present between the core and the coating layer, the core comprising at least one of Li2NiO2, Li6CoO4, and Li5FeO4, and the transition layer comprising at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0048] The lithium replenishing agent described above, wherein the transition layer comprises at least one of rock salt phase, rock salt-like phase, spinel-like structure, and layered structure;

[0049] And / or, the thickness of the transition layer is 2nm-200nm;

[0050] And / or, the transition layer contains an element X, the element X being selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga, and the mass percentage of the element X in the transition layer is 0.1%-20%;

[0051] And / or, the transition layer contains F element, wherein the mass percentage of F element in the transition layer is 0.1%-70%.

[0052] Seventhly, this application provides a method for preparing the lithium supplement agent as described above, comprising the following steps:

[0053] The lithium replenishing material and the coating agent are mixed and then sintered to obtain the lithium replenishing agent; wherein the coating agent includes lithium-containing fluorides.

[0054] In the lithium supplement preparation method described above, the sintering temperature is 300℃-600℃ and the time is 0.5h-6h.

[0055] Eighthly, this application provides a positive electrode sheet comprising the lithium replenishing agent as described above or the lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above.

[0056] Ninthly, this application provides a battery comprising the lithium replenishing agent as described above, or the lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above, or the positive electrode sheet as described above.

[0057] In a tenth aspect, this application provides a battery pack comprising the lithium replenishing agent as described above, or the lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above, or the positive electrode sheet as described above, or the battery as described above.

[0058] Eleventhly, this application provides an electrical device, including the lithium replenisher as described above, or the lithium replenisher prepared according to the lithium replenisher preparation method described above, or the positive electrode sheet as described above, or the battery as described above, or the battery pack as described above.

[0059] The lithium replenishing agent provided in this application has a coating layer comprising lithium-containing fluoride. The lithium-containing fluoride has excellent chemical stability and good lithium-ion conductivity, which can effectively prevent adverse reactions between the lithium replenishing material and the electrolyte or other active substances, inhibit the formation of residual alkali, and promote the rapid migration of lithium ions, thereby improving the stability and kinetic performance of the lithium replenishing agent, which is conducive to the utilization of the charging capacity of the lithium replenishing agent, improving the lithium replenishing effect of the lithium replenishing agent, and improving the cycle performance of the battery. Attached Figure Description

[0060] Figure 1-1 is a schematic diagram of the composite lithium replenishment material provided in Embodiment 1 of this application;

[0061] Figure 2-1 is a schematic diagram of the structure of a lithium replenishing agent provided in this application;

[0062] Figure 2-2 is a schematic diagram of another lithium replenishing agent provided in this application.

[0063] Figure label:

[0064] 1-Core layer; 2-Transition layer; 3-Covering layer; 1B-Lithium replenishment material; 2B-Covering layer; 11-Core; 12-Transition layer. Detailed Implementation

[0065] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0066] Lithium-rich compounds, such as Li₂NiO₂, are suitable as cathode materials for lithium-ion batteries due to their high theoretical capacity ratio. However, Li₂NiO₂ readily reacts with H₂O and CO₂ in the air, reducing its activity. To address this issue, those skilled in the art have modified Li₂NiO₂ using TiO₂ or ZrO₂ through coating or doping. However, test results show that the battery structure made from this modified Li₂NiO₂ material has unsatisfactory stability, and the improvement in battery specific capacity has not met expectations.

[0067] The inventors analyzed that the above reasons are as follows: the Ti and Zr elements in TiO2 or ZrO2 have a high valence state of +4, making it difficult to achieve deep and uniform doping, thus reducing the doping effect. Furthermore, after calcination, TiO2 oxide may have oxygen vacancies, causing Ti to appear in the coating layer. 3+ / Ti 4+ Electron pair oxidation of the electrolyte reduces the stability of the battery system, thus preventing it from achieving the expected results.

[0068] Based on this, the first aspect of this application provides a composite lithium supplement material, as shown in Figure 1-1, comprising:

[0069] The lithium-rich compound core and the coating layer 3 covering at least a portion of the surface of the lithium-rich compound core, the coating layer 3 comprising Li y Al z PO 4- x F 1+x Where 0 ≤ x < 4, y > 0, z > 0.

[0070] It should be explained that in the composite lithium replenishment material of this application, the lithium-rich compound core provides active lithium ions to replenish the lithium ions consumed during battery charging and discharging, which are formed during the formation of the SEI film or lithium dendrites. This application does not limit the choice of the lithium-rich compound core, as long as it can release lithium ions during the first charge.

[0071] The composite lithium replenishment material of this application can significantly improve the charging capacity of batteries. Besides the coating layer acting as a physical barrier to isolate water and carbon dioxide to a certain extent, the inventors believe the main reason is: firstly, the Li in the coating layer... y Al z PO4- x F 1+x Lithium has high ionic and electronic conductivity, and can act as a "dual conductor" to improve the interfacial dynamics of lithium-rich transition metal oxides, thereby enhancing lithium-ion transport efficiency and diffusion performance, and thus increasing the battery's charge capacity. On the other hand, Li... y Al z PO 4-x F 1+x Li exhibits strong chemical stability and a low probability of side reactions with water and carbon dioxide, significantly reducing the formation of residual alkali and avoiding electrolyte side reactions. This lowers the lithium requirement for SEI film reconstruction, allowing more lithium ions to participate in the insertion / extraction of the positive and negative electrodes. Furthermore, the suitable ionic radii of P, Al, and F elements in the coating layer, with strong bond energies between P, Al, and O elements enhancing structural stability, and the high electronegativity of F doping to partially replace oxygen, further contribute to structural stability. Therefore, Li... y Al z PO 4-x F 1+x It is easier to coat the surface of lithium-rich transition metal oxides, thus making the connection between the lithium-rich transition metal oxides and the coating layer more stable, extending the lifespan of the coating structure, and thus enabling a more long-lasting and significant coating effect. This further improves the stability and electronic and ionic conductivity of the composite lithium replenishment material. Therefore, this composite lithium replenishment material has both good structural stability and electronic and ionic conductivity, thereby further improving the battery's charging capacity and stability.

[0072] In one specific embodiment, as shown in FIG1-1, the lithium-rich compound core includes a core layer 1 and a transition layer 2 covering at least a portion of the surface of the core layer 1. The core layer 1 includes a lithium-rich compound, and the transition layer 2 includes an element-doped lithium-rich compound, wherein the element includes at least one of P, Al, and F.

[0073] As shown in Figure 1-1, the composite lithium supplement material comprises, from the inside out, a core layer 1, a transition layer 2, and a coating layer 3. The core layer is a lithium-rich compound; the coating layer is Li. y Al z PO 4-x F 1+x The transition layer is formed when at least one of the P, Al, and F elements provided in the coating layer enters the lithium-rich compound. Because the P, Al, and F elements in the coating layer have suitable ionic radii and strong structural stability, they are more easily incorporated into the bulk phase of the lithium-rich compound core, resulting in a higher and more uniform doping depth. The resulting transition layer exhibits good structural stability and has minimal impact on the theoretical capacity of the lithium-rich compound, further enhancing the structural stability and lithium replenishment performance of the composite lithium replenishment material.

[0074] In one specific embodiment, y:z = 1-10:1. At this ratio, the doping effect of P, Al, and F elements is better, the transition layer is more stable, and the composite lithium replenishment material has stronger chemical stability and better ionic and electronic conductivity, thereby further improving the specific charging capacity of the battery.

[0075] For example, y:z = 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, or a range consisting of any two of these values.

[0076] In one specific implementation, 0.02 ≤ x ≤ 0.1. By controlling the range of values ​​for x, the amount of F element replacing O element can be controlled, thereby allowing Li... y Al z PO 4-x F 1+x It has a stronger ability to conduct electrons and ions.

[0077] For example, x is 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, or a range of any two of these values.

[0078] In one specific implementation, 0.5 ≤ y ≤ 3. Within this range, Li... y Al z PO 4-x F 1+x The structure is more stable.

[0079] For example, y can be 0.5, 1, 1.5, 2, 2.5 or 3, or a range of any two of these values.

[0080] In one specific implementation, 0.1 ≤ z ≤ 1. Within this range, Li y Al z PO 4-x F 1+x The structure is more stable.

[0081] For example, z can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1, or a range of any two of these values.

[0082] When the following conditions are met simultaneously: 0.02≤x≤0.1, 0.5≤y≤3, and 0.1≤z≤1, Li y Al z PO 4-x F 1+x It has the best electron-ion conduction ability.

[0083] In one specific embodiment, as shown in Figure 1-1, the mass of the coating layer 3 accounts for 0.1-2% of the mass of the lithium-rich compound core. Within this range, it is more conducive to the efficient transport of lithium ions in the lithium-rich compound.

[0084] For example, the mass of the coating layer accounts for 0.1%, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.7%, 1.9% or 2% of the mass of the lithium-rich compound core, or a range of any two of these values.

[0085] In one specific embodiment, as shown in Figure 1-1, the thickness of the coating layer 3 is 1-500 nm. Within this range, the impedance is lower and the lithium-ion transport efficiency is higher.

[0086] For example, the thickness of the coating layer is 1 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, or a range of any two of these values.

[0087] In one specific implementation, Li y Al z PO 4-x F 1+x The particle size Dn50 satisfies: 1nm ≤ Dn50 ≤ 50nm. Within this range, the coating layer can more uniformly and completely coat the core layer.

[0088] For example, Li y Al z PO 4-x F 1+x The particle size Dn50 is 1nm, 2nm, 5nm, 10nm, 20nm, 30nm, 40nm or 50nm, or a range of any two of these values.

[0089] In one specific embodiment, the transition layer 2, i.e., the element-doped lithium-rich compound, has at least one of a layered structure, a rock-salt-like structure, and a spinel-like structure. The rock-salt-like structure includes a disordered rock-salt-like structure. The structure of the transition layer is determined by the specific structure of the core layer; different core layers (lithium-rich compounds) result in different transition layer structures. The crystal phase structure described above is more stable, less prone to collapse, and more conducive to lithium-ion conduction, thus having a more significant effect on improving the battery's specific capacity.

[0090] In one specific embodiment, the mass of the P element in the transition layer 2 accounts for 0.1-20.8% of the mass of the transition layer 2. For example, the mass of the P element in the transition layer accounts for 0.1%, 0.5%, 0.8%, 12.5%, 14.6%, 15.8%, or 20.8% of the mass of the transition layer, or a range consisting of any two of these values.

[0091] In one specific embodiment, the mass of Al element in transition layer 2 accounts for 0.1-18.2% of the mass of transition layer 2. Exemplarily, the mass of Al element in transition layer accounts for 0.1%, 4.2%, 9.3%, 13.6%, 15.5%, 17.3% or 18.2% of the mass of transition layer, or a range consisting of any two of these values.

[0092] In one specific embodiment, the mass of element F in transition layer 2 accounts for 0.1-12.8% of the mass of transition layer 2. Exemplarily, the mass of element F in the transition layer accounts for 0.1%, 0.4%, 0.7%, 1.8%, 3.2%, 6.4%, 9.3%, or 12.8% of the mass of the transition layer, or a range consisting of any two of these values.

[0093] When the mass contents of P, Al, and F elements in the transition layer are all within the above ranges, the stability of the transition layer is better.

[0094] In one specific embodiment, as shown in Figure 1-1, the thickness of the transition layer 2 is 2-499 nm. Within this range, the thickness of the transition layer can further reduce interfacial impedance, ensure higher utilization of lithium ions released from the core layer, and have minimal impact on the theoretical capacity of the lithium-rich compound.

[0095] For example, the thickness of the transition layer is 2nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or 499nm, or a range of any two of these values.

[0096] In one specific embodiment, the lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0097] Specifically, when the core layer is Li2NiO2, Li5FeO4, or a mixture of Li2NiO2 and Li5FeO4, it is conducive to the formation of a disordered rock-salt-like phase structure doped with P, Al, and F in the transition layer; when the core layer is Li6CoO4, it is conducive to the formation of a mixed disordered structure of layered structure, rock-salt-like structure, and spinel-like structure doped with P, Al, and F in the transition layer.

[0098] In one specific embodiment, the particle size Dn50 of the lithium-rich compound satisfies: 500 nm ≤ Dn50 ≤ 15 μm. Within this range, the diffusion path of lithium ions is shortened, the diffusion efficiency is improved, thereby improving the specific charge capacity of the battery.

[0099] For example, the particle size Dn50 of the lithium-rich compound is 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 3 μm, 6 μm, 9 μm, 12 μm or 15 μm, or a range of any two of these values.

[0100] In this embodiment of the application, particle size Dn50 (or Dn50) is the median particle size of the material, that is, in the particle sample, 50% of the particles have a particle size less than or equal to this value, and the other 50% of the particles have a particle size greater than this value.

[0101] The second aspect of this application provides a method for preparing the composite lithium-supplementing material of the first aspect, comprising:

[0102] In an oxygen atmosphere, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mixture is calcined to obtain a composite lithium supplement material.

[0103] It should be noted that the oxygen atmosphere in this application refers to a pure oxygen atmosphere. This application uses an oxygen atmosphere for calcination to avoid the formation of oxygen vacancies, thereby improving the performance of the composite lithium supplementation material. After calcining the above mixture, Li... y Al z PO 4-x F 1+x By coating the surface of lithium-rich compounds, a composite lithium supplement material is obtained.

[0104] This application does not specify the calcination temperature and time, as long as it can calcine Li... y Al z PO 4-x F 1+x It can be coated onto the surface of lithium-rich compounds.

[0105] This application relates to lithium-rich compounds, Li y Al z PO 4-x F 1+x The source is not specifically limited; any product prepared using commercially available products or conventional preparation methods known to those skilled in the art is acceptable.

[0106] This application does not specifically limit the equipment used for calcination; in one embodiment, a sintering furnace is used.

[0107] In one specific embodiment, lithium-rich compounds, Li y Al z PO 4-x F 1+xThe mass ratio is 100:0.1-2. Within this mass ratio range, lithium-ion transport in lithium-rich compounds becomes more efficient.

[0108] The resulting composite lithium supplement material exhibits better structural stability and ionic and electronic conductivity.

[0109] For example, lithium-rich compounds, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1, 100:0.5, 100:1, 100:1.5 or 100:2, or a range of any two of these values.

[0110] To improve the stability of the resulting composite lithium supplement material, the calcination temperature and time were further controlled.

[0111] In one specific embodiment, the calcination temperature is 200-800℃, and the calcination time is 0.5-6 hours. Within this calcination temperature and time range, the obtained composite lithium-supplementing material exhibits better stability.

[0112] For example, the calcination temperature is 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, or 800°C, or a range of any two of these values.

[0113] For example, the calcination time is 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, or a range of any two of these values.

[0114] Preferably, the calcination temperature is 300-600℃, and the calcination time is 2-6 hours. Within this calcination time and temperature range, the prepared composite lithium replenishment material exhibits good structural stability and electronic and ionic conductivity, thereby further improving the specific charging capacity of the battery.

[0115] In one specific embodiment, prior to calcination, the process further includes: reacting a lithium-rich compound with Li... y Al z PO 4-x F 1+x After mixing with solvent, the mixture is spray-dried to obtain a mixture; the spray-drying conditions include at least one of the following:

[0116] In one embodiment, the spray drying pressure is 0.2-1 MPa. Within this pressure range, a uniform pre-coating layer can be achieved.

[0117] In one embodiment, the inlet air temperature for spray drying is 100-300°C. Within this temperature range, the drying rate of each raw material is increased.

[0118] In one embodiment, the outlet temperature of the spray dryer is 80-100°C. This outlet temperature range further ensures more thorough drying of the raw materials.

[0119] In one embodiment, the feed rate for spray drying is 0.5-2 L / h. Within this range, the efficiency of spray drying is higher.

[0120] When the above-mentioned spray drying pressure, inlet air temperature, outlet air temperature, and feed rate are simultaneously satisfied, the spray drying method is as follows:

[0121] In a protective atmosphere, lithium-rich compounds and Li y Al z PO 4-x F 1+x The mixture is dispersed in a solvent and spray-dried; the protective atmosphere pressure is 0.2-1 MPa, the inlet temperature is 100-300℃, the outlet temperature is 80-100℃, and the feed rate is 0.5-2 L / h. First, lithium-rich compounds and Li... y Al z PO 4-x F 1+x Spray drying is performed to ensure that the coating layer covers the core layer more evenly and completely after calcination.

[0122] For example, the protective atmosphere pressure is 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.9 MPa, or 1 MPa, or a range of any two of these values.

[0123] For example, the intake temperature is 100°C, 130°C, 160°C, 190°C, 210°C, 240°C, 270°C, or 300°C, or a range of any two of these values.

[0124] For example, the outlet temperature is 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C or 100°C, or a range of any two of these values.

[0125] For example, the feed rate is 0.5L / h, 0.7L / h, 0.9L / h, 1.1L / h, 1.3L / h, 1.5L / h, 1.7L / h, 1.9L / h or 2L / h, or a range of any two of these values.

[0126] This application does not specifically limit the type of protective atmosphere; for example, it can be an inert atmosphere.

[0127] This application addresses the dispersion of lithium-rich compounds, Li y Al z PO 4-x F 1+x The solvent is not specifically limited. In one embodiment, the solvent includes at least one of N-methylpyrrolidone (NMP), ethanol, isopropanol, and ethylene glycol dimethyl ether.

[0128] This application does not specifically limit the equipment used for spray drying. In one embodiment, a spray dryer is used.

[0129] A third aspect of this application provides a positive electrode sheet comprising the composite lithium-supplementing material of the first aspect, or the composite lithium-supplementing material prepared by the preparation method of the second aspect.

[0130] The positive electrode sheet of this application specifically includes a positive current collector and a positive active layer formed of a positive active material (the composite lithium supplementation material of this application) disposed on the surface of the positive current collector.

[0131] In the specific preparation of the positive electrode sheet, for example, the composite lithium-supplementing material of this application can be dispersed with a conductive agent and a binder in an appropriate amount of N-methylpyrrolidone (NMP) solvent, and thoroughly stirred to form a uniform positive electrode slurry; the positive electrode slurry is uniformly coated on the positive electrode current collector, and after drying, rolling and slitting, the positive electrode sheet is obtained. In one specific embodiment, the positive electrode active layer comprises, by weight percentage, 70-99 wt% of positive electrode active material, 0.5-15 wt% of conductive agent, and 0.5-15 wt% of binder, and more specifically, 80-98 wt% of positive electrode active material, 1-10 wt% of conductive agent, and 1-10 wt% of binder.

[0132] The positive electrode current collector can be made of at least one of aluminum foil and nickel foil; the conductive agent can be made of at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber; and the binder can be made of at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinylpyrrolidone, and polyurethane.

[0133] A fourth aspect of this application provides a battery including the aforementioned positive electrode.

[0134] In addition to the aforementioned positive electrode, the battery of this application also includes a negative electrode, a separator, and an electrolyte. The following example illustrates the fabrication method of a lithium-ion battery:

[0135] This application does not strictly limit the negative electrode active material in the negative electrode sheet. It can be at least one of the negative electrode active materials commonly used in lithium-ion batteries, such as graphite, hard carbon, soft carbon, mesophase carbon microspheres, silicon-based negative electrode materials (mainly including silicon suboxide and silicon-carbon negative electrode), and tin-based negative electrode materials (mainly including tin and tin alloy).

[0136] This application does not strictly limit the choice of electrolyte, which may include one or more of the solvents commonly used in lithium-ion battery electrolytes, as well as the electrolyte lithium salts commonly used in lithium-ion electrolytes. For example, the solvent may be one or more of ethylene carbonate, propylene carbonate, butene carbonate, fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), difluoroethylene carbonate (DFEC), dipropyl carbonate, methyl ethyl carbonate (EMC), ethyl acetate, ethyl propionate, propyl acetate, propyl propionate, sulfolane, and γ-butyrolactone; the lithium salt may be one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0137] This application does not strictly limit the choice of separator material. It can be one of the separator materials commonly used in lithium-ion batteries, such as polypropylene separator (PP), polyethylene separator (PE), polypropylene / polyethylene double-layer composite membrane (PP / PE), polyimide electrospun separator (PI), polypropylene / polyethylene / polypropylene triple-layer composite membrane (PP / PE / PP), cellulose nonwoven separator, and separator with ceramic coating.

[0138] In the preparation of lithium-ion batteries, the positive electrode, separator, and negative electrode are wound or stacked to obtain a bare cell, which is then packaged into a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dried battery. The battery undergoes resting, formation, and secondary sealing to complete the preparation of the lithium-ion battery.

[0139] The battery of this application may be in the form of a battery cell, a battery module, or a battery pack. In some embodiments, battery cells may be assembled into a battery module, and the number of battery cells contained in a battery module may be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery module. In some embodiments, battery modules may also be assembled into a battery pack, and the number of battery modules contained in a battery pack may be one or more, the specific number of which can be selected by those skilled in the art based on the application and capacity of the battery pack.

[0140] The specific type of battery described in this application is not particularly limited. For example, from a shape perspective, the battery includes, but is not limited to, prismatic batteries, pouch batteries, and cylindrical batteries, etc., and this application does not impose any particular restrictions. From the perspective of the core structure, the battery core can be a wound core (i.e., a core formed by stacking positive electrode sheets, negative electrode sheets, and separators and then winding them) or a stacked core (i.e., multiple positive electrode sheets, negative electrode sheets, and separators are stacked to form a core). The outer casing can be a hard casing (such as a steel casing, a hard plastic casing, etc.) or a soft casing (such as an aluminum-plastic film casing, a pouch-type soft casing, etc.), etc., and this application does not impose any particular restrictions.

[0141] This application provides a fifth aspect of an electronic device, including the battery described in the fourth aspect above. This electronic device has the advantage of a long standby time. The electronic device provided in this application can be any conventional electrical device in the art, such as power equipment (e.g., electric vehicles), electrical devices (e.g., mobile phones, tablets, laptops, digital cameras, etc.), wearable devices (e.g., watches, bracelets, VR glasses, etc.), energy storage power stations, etc., without particular limitation.

[0142] The present application will be further described below through specific embodiments.

[0143] Example 1A

[0144] The preparation method of the composite lithium supplementation material in this embodiment includes the following steps:

[0145] 1) Fluorinated phosphate LiAlPO 3.94 F 1.06 High-energy ball milling was performed to control the particle size Dn50 to 10 nm; the grinding balls were zirconia grinding balls with a diameter of 1–8 mm; LiAlPO4 was used. 3.94 F 1.06 The mass ratio of grinding balls to the ball mill is 1:30; the inert atmosphere is nitrogen and / or argon; the ball milling jar speed is 1200 rpm; the ball milling time is 24 hours.

[0146] 2) Under an argon atmosphere, the ball-milled LiAlPO4 was processed. 3.94 F 1.06 A solid material was obtained by mixing lithium-rich compound Li2NiO2 at a mass ratio of 100:1. The solid material was then added to an NMP solution and stirred until homogeneous to obtain a mixture. The volume ratio of the solid material to the NMP solution was 1:1.1.

[0147] 3) Under an argon atmosphere, the mixture is fed into a spray dryer for spray drying to obtain a pretreated mixture; the heating argon pressure is 0.6 MPa, the inlet temperature is 250℃, the outlet temperature is 95℃, and the feed rate is 1.6 L / h.

[0148] 4) The pretreated mixture was fed into a sintering furnace and calcined at 600°C for 2 hours in an oxygen atmosphere to obtain LiAlPO4. 3.94 F 1.06 The coated Li2NiO2 material is a composite lithium supplement material.

[0149] The coating layer of the composite lithium-rich material accounts for 0.9% of the mass of the lithium-rich compound core.

[0150] Example 2A

[0151] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination temperature of the sintering furnace is 200℃.

[0152] Example 3A

[0153] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination temperature of the sintering furnace is 150°C.

[0154] Example 4A

[0155] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination temperature of the sintering furnace is 300℃.

[0156] Example 5A

[0157] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination temperature of the sintering furnace is 800℃.

[0158] Example 6A

[0159] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination temperature of the sintering furnace is 900℃.

[0160] Example 7A

[0161] This embodiment is basically the same as Example 1A, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:2.

[0162] Example 8A

[0163] This embodiment is basically the same as Example 1A, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.1.

[0164] Example 9A

[0165] This embodiment is basically the same as Example 1A, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:0.08.

[0166] Example 10A

[0167] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination time in the sintering furnace is 4 hours.

[0168] Example 11A

[0169] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination time in the sintering furnace is 6 hours.

[0170] Example 12A

[0171] This embodiment is basically the same as embodiment 1A, except that in step 4), the calcination time in the sintering furnace is 0.5h.

[0172] Example 13A

[0173] This embodiment is basically the same as Embodiment 1A, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.9 F 1.1 .

[0174] Example 14A

[0175] This embodiment is basically the same as Embodiment 1A, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.92 F 1.08 .

[0176] Example 15A

[0177] This embodiment is basically the same as Embodiment 1A, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.96 F 1.04 .

[0178] Example 16A

[0179] This embodiment is basically the same as Embodiment 1A, except that in step 1), the fluorinated phosphate is LiAlPO4. 3.98 F 1.02 .

[0180] Example 17A

[0181] This embodiment is basically the same as that of Embodiment 1A, except that in step 1), the fluorinated phosphate is LiAlPO4F.

[0182] Example 18A

[0183] This embodiment is basically the same as embodiment 1A, except that in step 2), Li2NiO2 is replaced with Li5FeO4.

[0184] Example 19A

[0185] This embodiment is basically the same as embodiment 1A, except that in step 2), Li2NiO2 is replaced with Li6CoO4.

[0186] Example 20A

[0187] This embodiment is basically the same as Embodiment 1A, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 60 nm.

[0188] Example 21A

[0189] This embodiment is basically the same as Embodiment 1A, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 50 nm.

[0190] Example 22A

[0191] This embodiment is basically the same as Embodiment 1A, except that: LiAlPO 3.94 F 1.06 The particle size Dn50 is 1 nm.

[0192] Example 23A

[0193] This embodiment is basically the same as that of Example 1A, except that the particle size Dn50 of the lithium-rich compound is 17 μm.

[0194] Example 24A

[0195] This embodiment is basically the same as Example 1A, except that: lithium-rich compound, Li y Al z PO 4-x F 1+x The mass ratio is 100:2.5.

[0196] Example 25A

[0197] This embodiment is basically the same as Example 1A, except that: lithium-rich compound, Li y Alz PO 4-x F 1+x The mass ratio is 100:0.4.

[0198] Example 26A

[0199] This embodiment is basically the same as Embodiment 1A, except that: x = 0.01, that is, the coating layer is LiAlPO 3.99 F 1.01 .

[0200] Example 27A

[0201] This embodiment is basically the same as Embodiment 1A, except that: x = 0.11, that is, the coating layer is LiAlPO 3.89 F 1.11 .

[0202] Comparative Example 1A

[0203] This embodiment is basically the same as Embodiment 1A, except that: the core layer lithium-rich compound Li2NiO2 is not modified, that is, Li2NiO2 is directly used as the lithium supplement material.

[0204] Comparative Example 2A

[0205] This embodiment is basically the same as embodiment 1A, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with Al2O3, that is, modify Li2NiO2 with Al2O3.

[0206] Comparative Example 3A

[0207] This embodiment is basically the same as embodiment 1A, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with TiO2, that is, modify Li2NiO2 with TiO2.

[0208] Comparative Example 4A

[0209] This embodiment is basically the same as embodiment 1A, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06 Replace with Li3PO4, that is, modify Li2NiO2 with Li3PO4.

[0210] Comparative Example 5A

[0211] This embodiment is basically the same as embodiment 1A, except that: the LiAlPO4 in step 1) is removed. 3.94 F 1.06Replace it with Al-doped ZnO, that is, modify Li2NiO2 with Al-doped ZnO.

[0212] Comparative Example 6A

[0213] This embodiment is basically the same as Embodiment 18A, except that: the core layer lithium-rich compound Li5FeO4 is not modified, that is, Li5FeO4 is directly used as the lithium supplement material.

[0214] Comparative Example 7A

[0215] This embodiment is basically the same as Embodiment 19A, except that: the core layer lithium-rich compound Li6CoO4 is not modified, that is, Li6CoO4 is directly used as the lithium supplement material.

[0216] The implementation conditions for different embodiments and comparative examples are shown in Table 1A.

[0217] Test method:

[0218] The percentage of the mass of the coating layer relative to the mass of the lithium-rich compound core (abbreviated as coating amount).

[0219] Table 1A

[0220] Test case

[0221] (1) The composite lithium replenishing materials prepared in the above embodiments and comparative examples were subjected to the following tests. The thickness of the transition layer of the composite lithium replenishing materials and the percentage of P, Al and F elements in the transition layer by mass are shown in Table 2A.

[0222] Test method:

[0223] 1) Transition layer thickness

[0224] The FIB is used to process the target particles to obtain a cross-section, which is then characterized by STEM to observe the surface crystal structure of the particle cross-section. The thickness of the transition layer and the surface fluorinated phosphate modified layer can be measured.

[0225] 2) The mass ratio of P, Al, and F elements in the transition layer

[0226] By using the EELS equipped with STEM for statistical characterization of surface element distribution, the mass ratios of P, Al, and F in the transition layer can be measured.

[0227] Table 2A

[0228] (2) Battery manufacturing

[0229] The modified Li2NiO2 materials and the unmodified Li2NiO2 materials in the examples and comparative examples were exposed to air at a temperature of 25°C and a humidity of 40% for 24 hours.

[0230] The materials that were not placed in a humid environment and the materials that were placed in a humid environment were used as positive electrode materials to make button cells.

[0231] In the fabrication of coin cells, positive electrode material, conductive carbon black, and PVDF are dispersed in NMP at a mass ratio of 8:1:1. The positive electrode is obtained through slurry preparation, coating, drying, and rolling. A lithium metal sheet is used as the negative electrode, a Celgard 2400 polypropylene membrane as the separator, and a mixed solution of EC and DMC containing 1 mol / L lithium hexafluorophosphate (volume ratio 1:1) is used as the electrolyte. The battery is assembled with the aforementioned positive electrode in an argon-filled glove box.

[0232] Using the LAND battery testing system, the batteries were charged to 4.2V at constant current rates of 0.05C and 0.33C, respectively, and then charged at constant voltage at 4.2V until the current equals 0.03C. The charge capacity at 0.05C and the charge capacity at 0.33C were recorded respectively.

[0233] After the lithium replenishing agent powder is left to stand for 24 hours at 25°C and 40% humidity, the battery is made according to the above steps and charged at a constant current rate of 0.05C to 4.2V. Then, it is charged at a constant voltage rate of 4.2V to a current of 0.03C. The charging capacity at this time is recorded as the gram capacity of the powder after standing for 24 hours and charging at 0.05C.

[0234] The test results are shown in Table 3A.

[0235] Table 3A

[0236] As can be seen from Table 3A, compared with the comparative example, the battery made from the composite lithium replenishment material of the present application has a higher charging capacity.

[0237] The sixth aspect of this application provides a lithium replenishing agent, including a lithium replenishing material and a coating layer present on the surface of the lithium replenishing material, the coating layer including a lithium-containing fluoride.

[0238] The chemical formula of lithium fluoride is Li x M y F z Where 0 < x ≤ 3, 0 < y ≤ 1, 0 < z ≤ 6, and M is selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga.

[0239] The lithium-containing fluoride includes at least one of LiAlF4, Li3AlF6, Li2ZrF6, Li2TiF6, Li2SiF6, LiSbF6, LiBiF4, LiInF4 and LiGaF4, preferably LiAlF4 and / or Li3AlF6.

[0240] The lithium fluoride content in the lithium supplement is 0.1%-10% by mass, preferably 0.5%-2%;

[0241] And / or, the thickness of the coating layer is 1nm-500nm.

[0242] Lithium supplementation materials include at least one of Li2NiO2, Li6CoO4, and Li5FeO4;

[0243] And / or, the particle size Dn50 of the lithium replenishment material is 500nm-15μm.

[0244] The lithium supplement material includes a core and a transition layer, with the transition layer existing between the core and the coating layer. The core includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4, and the transition layer includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0245] The transition layer includes at least one of the following: rock salt phase, rock salt-like phase, spinel-like structure, and layered structure;

[0246] And / or, the thickness of the transition layer is 2nm-200nm;

[0247] And / or, the transition layer contains an element X, which is selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga, and the mass percentage of the element X in the transition layer is 0.1%-20%.

[0248] And / or, the transition layer contains F element, and the mass percentage of F element in the transition layer is 0.1%-70%.

[0249] Seventhly, this application provides a method for preparing the above-mentioned lithium supplement, comprising the following steps:

[0250] The lithium replenishing material and the coating agent are mixed and then sintered to obtain the lithium replenishing agent; wherein the coating agent includes lithium-containing fluorides.

[0251] The sintering temperature is 300℃-600℃, and the time is 0.5h-6h.

[0252] Eighthly, this application provides a positive electrode sheet comprising the lithium replenishing agent as described above or a lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above.

[0253] Ninthly, this application provides a battery comprising the lithium replenishing agent as described above, or a lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above, or a positive electrode sheet as described above.

[0254] In a tenth aspect, this application provides a battery pack comprising the above-described lithium replenishing agent, or a lithium replenishing agent prepared according to the above-described method for preparing the lithium replenishing agent, or the above-described positive electrode sheet, or the above-described battery.

[0255] In one aspect, this application provides an electrical device, including the lithium replenishing agent as described above, or a lithium replenishing agent prepared according to the lithium replenishing agent preparation method described above, or a positive electrode sheet as described above, or a battery as described above, or a battery pack as described above.

[0256] The performance of lithium-ion batteries largely depends on the chemical stability and electrochemical activity of their electrode materials. With the increasing demand for high energy density and long lifespan batteries, the introduction of lithium replenishers has become an effective strategy to address irreversible capacity loss during the first cycle. Lithium replenishers, such as Li₂NiO₂, have attracted considerable attention due to their high theoretical specific capacity and their ability to improve initial coulombic efficiency. However, these materials readily react with water and carbon dioxide in air, leading to decreased electrochemical activity and increased safety risks.

[0257] To address these challenges, existing technologies typically employ surface coating methods, such as carbon coating, which prevents direct contact between the lithium supplement and the environment by forming a protective layer on the surface of the supplement.

[0258] However, the inventors of this application have discovered that traditional coating materials often exhibit insufficient stability and kinetic performance in practical applications. This deficiency not only limits the effectiveness of lithium replenishers but may also affect their specific charging capacity, resulting in poor lithium replenishment and decreased battery cycle performance. Using lithium-containing fluorides as coating agents can significantly improve the stability and kinetic performance of lithium replenishers, facilitating the realization of their specific charging capacity, improving their lithium replenishment effect, and enhancing battery cycle performance.

[0259] Based on this, in a sixth aspect, as shown in FIG2-1, this application provides a lithium replenishing agent, including a lithium replenishing material 1B and a coating layer 2B present on the surface of the lithium replenishing material 1B, the coating layer 2B including a lithium-containing fluoride.

[0260] The lithium replenishing agent provided in this application has a coating layer 2B on the surface of the lithium replenishing material 1B. The coating layer 2B includes lithium-containing fluoride, which can improve the stability and kinetic performance of the lithium replenishing agent, facilitate the utilization of the charging capacity of the lithium replenishing agent, improve the lithium replenishing effect of the lithium replenishing agent, and improve the cycle performance of the battery when applied to the battery.

[0261] The reasons for this are as follows: lithium-containing fluorides possess excellent chemical stability. As the coating layer 2B, they effectively prevent adverse reactions between the lithium replenishment material 1B and the electrolyte or other active substances, inhibiting residual alkali formation, thus extending the lifespan of the lithium replenishment agent and reducing side reactions. Furthermore, they form a stable interface between the lithium replenishment material 1B and the electrolyte, reducing interfacial impedance and facilitating smooth lithium ion transport, thereby improving the battery's charge and discharge efficiency. Additionally, lithium-containing fluorides have good lithium-ion conductivity, promoting rapid lithium ion migration and improving the kinetic performance of the lithium replenishment agent, which is particularly important for rapid charge and discharge processes. Simultaneously, the coating layer 2B also provides some mechanical protection, preventing the lithium replenishment material 1B from pulverizing or cracking due to volume changes or other mechanical stresses during cycling. This maintains the material's structural integrity, improves its stability and kinetic performance, and is beneficial for maximizing the charging capacity of the lithium replenishment material, improving its lithium replenishment effect, and ultimately enhancing the battery's cycle performance.

[0262] Therefore, the lithium replenishing agent provided in this application has a coating layer 2B comprising lithium-containing fluoride. The lithium-containing fluoride has excellent chemical stability and good lithium-ion conductivity, which can effectively prevent the lithium replenishing material 1B from reacting adversely with the electrolyte or other active substances, inhibit the formation of residual alkali, and promote the rapid migration of lithium ions, thereby improving the stability and kinetic performance of the lithium replenishing agent, which is conducive to the utilization of the charging capacity of the lithium replenishing agent, improving the lithium replenishing effect of the lithium replenishing agent, and improving the cycle performance of the battery.

[0263] In some embodiments of this application, the chemical formula of the lithium fluoride is Li. x M y F z Where 0 < x ≤ 3, 0 < y ≤ 1, 0 < z ≤ 6, and M is selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga.

[0264] For example, x can be a range of 0.01, 0.5, 1, 1.5, 2, 3 or any two of them; y can be a range of 0.01, 0.3, 0.5, 0.7, 0.9, 1 or any two of them; z can be a range of 0.01, 1, 2, 3, 4, 5, 6 or any two of them.

[0265] The lithium-containing fluoride of this application can further improve the stability of the lithium replenishing agent, thereby improving the lithium replenishment effect of the lithium replenishing agent and improving the cycle performance of the battery.

[0266] In some embodiments of this application, the lithium fluoride includes at least one of LiAlF4, Li3AlF6, Li2ZrF6, Li2TiF6, Li2SiF6, LiSbF6, LiBiF4, LiInF4 and LiGaF4, preferably LiAlF4 and / or Li3AlF6.

[0267] It should be noted that when lithium-containing fluorides include LiAlF4 and / or Li3AlF6, Al and F elements can achieve a deeper doping depth, which can further improve the structural stability of the lithium replenishing agent, thereby improving the lithium replenishing effect of the lithium replenishing agent and improving the cycle performance of the battery.

[0268] In some embodiments of this application, the lithium fluoride content in the lithium supplement is 0.1%-10% by mass, for example, it can be a range of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any two of these, preferably 0.5%-2%.

[0269] In this application, the lithium-containing fluoride accounts for a percentage of the lithium replenishing agent within the aforementioned range. On the one hand, this effectively forms a stable coating layer 2B, reducing side reactions between the electrolyte and electrode materials, and thus improving the overall electrochemical stability of the battery. On the other hand, the lithium-containing fluoride has good lithium-ion conductivity, which promotes rapid lithium-ion transport. An appropriate amount of lithium-containing fluoride can improve the charge-discharge efficiency of the battery without significantly increasing the interfacial impedance.

[0270] When the mass percentage of lithium fluoride in the lithium replenisher is 0.5%-2%, the overall electrochemical stability of the battery can be further improved, and the charge and discharge efficiency of the battery can be enhanced.

[0271] In some embodiments of this application, the thickness of the cladding layer 2B is 1nm-500nm, for example, it can be a range of 1nm, 10nm, 20nm, 50nm, 100nm, 200nm, 300nm, 400nm, 500nm or any two of these.

[0272] The thickness of the coating layer 2B in this application is within the aforementioned range, enabling the formation of a stable interface between the lithium replenishment material 1B and the electrolyte, reducing interfacial impedance, and thus improving lithium-ion transport efficiency and the overall electrochemical performance of the battery. It also effectively isolates the lithium replenishment material 1B from direct contact with the electrolyte, preventing adverse chemical reactions and improving the chemical stability of the lithium replenisher, thereby enhancing its lithium replenishment effect and increasing the battery's cycle life. Furthermore, the thickness of the coating layer 2B is sufficient to provide mechanical protection, preventing the lithium replenishment material 1B from pulverizing or cracking due to volume changes or other mechanical stresses during charging and discharging, thus maintaining the structural integrity of the material. Simultaneously, the thickness of the coating layer 2B does not significantly increase the lithium-ion diffusion path, thereby maintaining or even enhancing the kinetic performance of the lithium replenisher and supporting rapid charging and discharging.

[0273] The thickness of the coating layer 2B in this application can be obtained by cutting the lithium supplement agent, testing the thickness of the coating layer 2B in the cross section using a transmission electron microscope (TEM), and taking the average thickness of 20 particles.

[0274] In some embodiments of this application, the lithium supplement material 1B includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0275] In this application, the lithium replenishment material 1B includes the aforementioned materials, which can provide a greater number of lithium ions for the battery's charging and discharging process, thereby facilitating the utilization of the lithium replenishment material's charging capacity. Furthermore, the aforementioned lithium replenishment material 1B exhibits good cycle stability during charging and discharging, effectively reducing capacity decay and extending battery life.

[0276] The lithium replenishment material 1B of this application can be commercially available or prepared in-house using conventional methods in the art.

[0277] In some embodiments of this application, the particle size Dn50 of the lithium replenishment material 1B is 500 nm to 15 μm, for example, it can be a range of 500 nm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm or any two of these.

[0278] In this application, the particle size Dn50 of the lithium replenishing material 1B is within the above-mentioned range, which is beneficial for the coating layer 2B to coat the lithium replenishing material 1B, so that the lithium replenishing agent formed after coating has better stability and kinetic performance, thereby improving the lithium replenishing effect of the lithium replenishing agent and improving the cycle performance of the battery.

[0279] The particle size Dn50 of the lithium replenishment material 1B in this application refers to the particle size corresponding to a cumulative distribution percentage of 50%.

[0280] The particle size Dn50 of the lithium supplement material 1B of this application can be obtained by testing with a laser particle size analyzer.

[0281] In some embodiments of this application, as shown in FIG2-2, the lithium replenishment material includes a core 11 and a transition layer 12, the transition layer 12 being present between the core 11 and the coating layer 2B. The core 11 includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4, and the transition layer 12 includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

[0282] The presence of the transition layer 12 serves two main purposes. First, it effectively buffers the interfacial stress between the core 11 and the coating layer 2B, reducing interfacial reactions and impedance, and improving overall interfacial stability. Second, the transition layer 12 prevents direct contact between the electrolyte and the core 11, reducing side reactions and helping to maintain the integrity of the electrode material and the amount of active lithium, thereby increasing the battery's energy density. Furthermore, the transition layer 12 acts as a buffer layer, absorbing and dispersing mechanical stress caused by volume changes, reducing material pulverization and structural damage, thus improving the battery's cycle life.

[0283] The materials in the core 11 and transition layer 12 have high chemical and structural stability, which can improve the structural integrity of the lithium replenishment agent during the charging and discharging process and reduce the expansion and contraction of the material.

[0284] In some embodiments of this application, the transition layer 12 includes at least one of the following: rock salt phase, rock salt-like phase, spinel-like structure, and layered structure.

[0285] It should be noted that when the lithium replenishing material 1B is Li2NiO2, the transition layer 12 is a rock salt phase. When the lithium replenishing material 1B is Li5FeO4, the transition layer 12 is a rock salt-like phase. When the lithium replenishing material 1B is Li6CoO4, the transition layer 12 is a mixed disordered phase consisting of layered, rock salt-like, and spinel-like phases. Furthermore, the stability of the aforementioned transition layers 12 is superior to that of the uncoated lithium replenishing material 1B, and they can serve as a passivation layer.

[0286] The rock salt and rock salt-like phases in the transition layer 12 of this application exhibit good ionic conductivity and chemical stability, which can promote lithium-ion transport and improve the cycle performance of the battery. The spinel-like structure provides three-dimensional lithium-ion channels, which helps to improve the migration rate of lithium ions. The layered structure can provide rapid lithium-ion insertion and extraction pathways, improving kinetic performance.

[0287] In some embodiments, the thickness of the transition layer 12 is 2nm-200nm, for example, it can be a range of 2nm, 10nm, 50nm, 100nm, 200nm or any two of them.

[0288] The thickness of the transition layer 12 in this application is within the above-mentioned range, which can further improve the structural stability of the lithium replenishing agent, facilitate the utilization of the charging capacity of the lithium replenishing agent, improve the lithium replenishing effect of the lithium replenishing agent, and improve the cycle performance of the battery.

[0289] In the lithium-containing fluoride of this application, the M and F elements are relatively easy to dop into the bulk phase of the lithium material 1B due to their suitable ionic radius and low valence state, thereby obtaining a certain doping depth and forming a transition layer 12 including the X and F elements on the surface of the coated particles.

[0290] In some embodiments, the transition layer 12 has an element X, which is selected from at least one of Al, Zr, Ti, Si, Sb, Bi, In, and Ga. The mass percentage of the element X in the transition layer 12 is 0.1%-20%, for example, it can be a range of 0.1%, 0.5%, 1%, 5%, 10%, 15%, 20%, or any combination thereof.

[0291] In some embodiments, the transition layer 12 contains an element F, and the mass percentage of the element F in the transition layer 12 is 0.1%-70%, for example, it can be a range of 0.1%, 0.5%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 65%, 70%, or any combination thereof.

[0292] In this application, the mass percentage content of elements X and F is within the above range, which can further improve the mechanical properties and chemical stability of the transition layer 12, prevent adverse reactions from occurring, and improve the chemical stability of the lithium supplement.

[0293] In this application, the thickness of the transition layer 12 can be obtained by cutting the lithium supplement agent, testing the thickness of the transition layer 12 cross section using a transmission electron microscope (TEM), and taking the average thickness of 20 particles.

[0294] The mass percentages of X and F elements in the transition layer 12 of this application can be obtained by aberration transmission electron microscopy and electron energy loss spectroscopy (EELS).

[0295] In a seventh aspect, this application provides a method for preparing the above-mentioned lithium replenishing agent, comprising the following steps: mixing the lithium replenishing material and the coating agent, and then performing a sintering treatment to obtain the lithium replenishing agent; wherein the coating agent includes a lithium-containing fluoride.

[0296] In this application, sintering the mixture formed by mixing the lithium replenishment material and the coating agent can make the resulting coating layer structure more stable and form a transition layer.

[0297] Specifically, the mixture of lithium replenishing material and coating agent can be spray-dried under an inert atmosphere. This process uniformly disperses the mixture, including lithium replenishing material 1B and coating agent, into fine particles, achieving pre-coating and facilitating the formation of a uniform coating layer 2B. The spray-drying pressure can be 0.2 MPa-1 MPa, the inlet temperature can be 100℃-300℃, the outlet temperature can be 80℃-100℃, and the feed rate can be 0.5 L / h-2 L / h.

[0298] Sintering under an oxygen atmosphere helps repair oxygen defects in the lithium replenisher, prevents the formation of oxygen vacancies, and improves the electrochemical performance and cycle stability of the lithium replenisher. Furthermore, sintering promotes the doping of M and F elements into the bulk phase of the lithium replenisher material 1B, forming a transition layer 12.

[0299] The method for preparing the lithium replenishing agent provided in this application can prepare the lithium replenishing agent provided in the first aspect of this application. The lithium replenishing agent has excellent structural stability and kinetic performance, which is conducive to the utilization of the charging capacity of the lithium replenishing agent, improves the lithium replenishing effect of the lithium replenishing agent, and improves the cycle performance of the battery.

[0300] In some embodiments of this application, the sintering temperature is 300℃-600℃, for example, it can be a range of 300℃, 350℃, 400℃, 450℃, 500℃, 550℃, 600℃ or any two of these. The time is 0.5h-6h, for example, it can be a range of 0.5h, 1h, 2h, 3h, 4h, 5h, 6h or any two of these.

[0301] The sintering temperature in this application is within the aforementioned range, which allows the lithium supplement to achieve good crystallization, contributing to the formation of a stable phase structure and improving the electrochemical performance of the lithium supplement. It also prevents excessive sintering or phase transformation of the lithium supplement at excessively high temperatures, maintaining the structural integrity of the lithium supplement.

[0302] The sintering time in this application is within the aforementioned range, which allows the internal reaction of the lithium supplement to proceed fully, improving its mechanical and chemical stability. Furthermore, appropriate time control can prevent excessive particle growth, maintain particle size, and thus optimize specific surface area and kinetic properties.

[0303] In addition, the temperature and time of sintering in this application will also affect the thickness of the transition layer 12 and the content of X and F elements in the transition layer 12.

[0304] In some embodiments, the mass ratio of lithium supplement material 1B to coating agent is 1:(0.001-0.05), for example, it can be a range of 1:0.001, 1:0.005, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05 or any two of these.

[0305] In this application, the mass ratio of lithium replenishing material 1B to coating agent is within the above-mentioned range, which can form a coating layer 2B of suitable thickness. This effectively isolates the lithium replenishing material 1B from direct contact with the electrolyte, prevents adverse chemical reactions from occurring, thereby improving the chemical stability of the lithium replenishing agent, and further improving the lithium replenishing effect of the lithium replenishing agent and improving the cycle performance of the battery.

[0306] Eighthly, this application provides a positive electrode sheet comprising the lithium replenishing agent as described above or a lithium replenishing agent prepared according to the preparation method described above.

[0307] The positive electrode sheet of this application can be prepared using conventional techniques in the art. Specifically, the above-mentioned lithium supplement, positive electrode active material, conductive agent and binder can be uniformly dispersed in a solvent to obtain a positive electrode active layer slurry. Then, the positive electrode active layer slurry is coated on at least one functional surface of the positive electrode current collector, and after drying, the positive electrode sheet of this application can be obtained.

[0308] This application does not specifically limit the categories of conductive agents and adhesives. The conductive agents, adhesives and other components can be selected from conventional substances in the field. For example, the conductive agent can be selected from one or more of conductive carbon black, carbon nanotubes, conductive graphite and graphene, and the adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), acrylic modified PVDF, polyacrylate polymers, polyimide, styrene-butadiene rubber and styrene-acrylic rubber.

[0309] This application does not specify the coating method; any coating method such as gravure coating, extrusion coating, spraying, or screen printing can be used to achieve the coating of the positive electrode active layer slurry.

[0310] The positive electrode sheet provided in this application includes the aforementioned lithium replenishing agent. Therefore, when this positive electrode sheet is applied to a battery, it can improve the battery's cycle performance.

[0311] Ninthly, this application provides a battery comprising the above-mentioned lithium replenishing agent, or a lithium replenishing agent prepared according to the above-mentioned preparation method, or a positive electrode sheet as described above. This battery has advantages corresponding to the above-mentioned positive electrode sheet, which will not be elaborated further.

[0312] In addition to the positive electrode, the battery of this application also includes a separator, a negative electrode, and an electrolyte. The composition of the negative electrode can refer to conventional negative electrode sheets in the art, and the separator can also be a separator commonly used in the art, such as PP film, PE film, etc.

[0313] The battery of this application can be prepared using conventional methods in the art. Specifically, the positive electrode, separator and negative electrode can be stacked in sequence, and the cell can be obtained by stacking or winding. Then, the battery can be obtained by baking, liquid injection, formation and packaging.

[0314] In a tenth aspect, this application provides a battery pack comprising the above-mentioned lithium replenishing agent, or a lithium replenishing agent prepared according to the above-mentioned preparation method, or the above-mentioned positive electrode sheet, or the above-mentioned battery, wherein the battery pack has advantages corresponding to the above-mentioned positive electrode sheet, which will not be elaborated further.

[0315] The battery pack of this application includes at least two batteries as described above. These batteries can be electrically connected by conventional methods in the art, such as series connection, parallel connection, or a hybrid connection including both of these connection methods, without any particular limitation.

[0316] Eleventhly, this application provides an electrical device including the lithium replenishing agent as described above, or the lithium replenishing agent prepared according to the preparation method described above, or the positive electrode sheet as described above, or the battery as described above, or the battery pack as described above. The electrical device has advantages corresponding to the positive electrode sheet described above, which will not be elaborated further.

[0317] The electrical equipment used in this application can be conventional electrical equipment in the field, such as power equipment (e.g., electric vehicles), electronic equipment (e.g., computers, mobile phones, digital cameras, printers, fax machines, etc.), wearable devices (e.g., watches, wristbands, VR glasses, etc.), and household appliances (e.g., air conditioners, refrigerators, washing machines, microwave ovens, etc.), etc., without any particular limitation.

[0318] The technical solution of this application will be further described below with reference to specific embodiments.

[0319] Example 1B

[0320] The preparation method of the lithium supplement in this embodiment includes the following steps:

[0321] 1) Take an appropriate amount of lithium-containing fluoride LiAlF4 as a coating agent. Under an argon atmosphere, add the above coating agent LiAlF4 and lithium-supplementing material Li2NiO2 to N-methylpyrrolidone (NMP) and stir to mix evenly to obtain a mixture. The mass ratio of lithium-supplementing material to coating agent is 1:0.001.

[0322] 2) Under an argon atmosphere, the above mixture is fed into a spray dryer for spray drying to obtain a lithium supplement precursor; the pressure is controlled at 0.5 MPa, the inlet temperature at 210℃, the outlet temperature at 95℃, and the feed rate at 0.8 L / h.

[0323] 3) The above-mentioned lithium replenishing agent precursor is fed into a sintering furnace and sintered in an oxygen atmosphere for 2 hours at a sintering temperature of 600℃. After sintering, the lithium replenishing agent is obtained by sieving. The particle size Dn50 of the lithium replenishing material is 10000nm.

[0324] The lithium replenishing agent includes the lithium replenishing material Li2NiO2 and the coating layer LiAlF4 on the surface of the lithium replenishing material. The lithium replenishing material also includes a transition layer, which is a rock salt phase.

[0325] Example 2B

[0326] The preparation method of the lithium replenishing agent in Example 2B is basically the same as that in Example 1B, except that the mass ratio of lithium replenishing material to coating agent is changed to 1:0.005, so that the mass percentage of lithium fluoride in the lithium replenishing agent is 0.5%, the coating layer thickness is 10 nm, the content of X element in the transition layer is 1.3%, the content of F element in the transition layer is 2.8%, and the thickness of the transition layer is 10 nm.

[0327] Example 3B

[0328] The preparation method of the lithium replenishing agent in Example 3B is basically the same as that in Example 1B. The difference is that the mass ratio of lithium replenishing material and coating agent is changed to 1:0.01, so that the mass percentage of lithium fluoride in the lithium replenishing agent is 1%, the coating layer thickness is 45nm, the content of X element in the transition layer is 3.3%, the content of F element in the transition layer is 6.9%, and the thickness of the transition layer is 25nm.

[0329] Example 4B

[0330] The preparation method of the lithium replenishing agent in Example 4B is basically the same as that in Example 1B, except that the mass ratio of lithium replenishing material to coating agent is changed to 1:0.02, so that the mass percentage of lithium fluoride in the lithium replenishing agent is 2%, the coating layer thickness is 88nm, the content of X element in the transition layer is 5.4%, the content of F element in the transition layer is 11.7%, and the thickness of the transition layer is 44nm.

[0331] Example 5B

[0332] The preparation method of the lithium replenishing agent in Example 5B is basically the same as that in Example 1B, except that the mass ratio of lithium replenishing material to coating agent is changed to 1:0.1, so that the mass percentage of lithium fluoride in the lithium replenishing agent is 10%, the coating layer thickness is 497 nm, the content of X element in the transition layer is 7.2%, the content of F element in the transition layer is 15.7%, and the thickness of the transition layer is 197 nm.

[0333] Example 6B

[0334] The preparation method of the lithium replenishing agent in Example 6B is basically the same as that in Example 1B, except that the mass ratio of lithium replenishing material to coating agent is changed to 1:0.12, so that the mass percentage of lithium fluoride in the lithium replenishing agent is 12%, the coating layer thickness is 545 nm, the content of X element in the transition layer is 8.1%, the content of F element in the transition layer is 17.3%, and the thickness of the transition layer is 214 nm.

[0335] Example 7B

[0336] The preparation methods of the lithium replenishing agent in Example 7B and Example 3B are basically the same, except that the particle size Dn50 of the lithium replenishing material Li2NiO2 is changed to 500nm, so that the coating layer thickness is 65nm, the content of X element in the transition layer is 4.2%, the content of F element in the transition layer is 7.4%, and the thickness of the transition layer is 32nm.

[0337] Example 8B

[0338] The preparation methods of the lithium replenishing agent in Example 8B and Example 3B are basically the same, except that the particle size Dn50 of the lithium replenishing material Li2NiO2 is changed to 15000nm, so that the coating layer thickness is 37nm, the content of X element in the transition layer is 2.9%, the content of F element in the transition layer is 6.1%, and the thickness of the transition layer is 22nm.

[0339] Example 9B

[0340] The preparation methods of the lithium supplement in Example 9B and Example 3B are basically the same, except that the sintering temperature is changed to 300°C and the sintering time is changed to 0.5h, so that the coating layer thickness is 47nm, the content of X element in the transition layer is 0.1%, the content of F element in the transition layer is 0.2%, and the thickness of the transition layer is 2nm.

[0341] Example 10B

[0342] The preparation methods of the lithium supplement in Example 10B and Example 3B are basically the same, except that the sintering temperature is changed to 600°C and the sintering time is changed to 6h, so that the coating layer thickness is 24nm, the content of X element in the transition layer is 20%, the content of F element in the transition layer is 68%, and the thickness of the transition layer is 56nm.

[0343] Example 11B

[0344] The preparation methods of the lithium replenishing agent in Example 11B and Example 3B are basically the same, except that the coating agent is changed to Li3AlF6, so that the coating layer thickness is 47nm, the content of X element in the transition layer is 3.5%, the content of F element in the transition layer is 7.4%, and the thickness of the transition layer is 27nm.

[0345] Example 12B

[0346] The preparation methods of the lithium replenishing agent in Example 12B and Example 3B are basically the same, except that the coating agent is changed to Li3AlF6 and the lithium replenishing material is Li6CoO4, so that the coating layer thickness is 55nm, the F element content in the transition layer is 6.7%, and the transition layer thickness is 20nm.

[0347] Example 13B

[0348] The preparation methods of the lithium replenishing agent in Example 13B are basically the same as those in Example 3B. The difference is that the coating agent is changed to Li3AlF6 and the lithium replenishing material is Li5FeO4, so that the coating layer thickness is 40nm, the content of X element in the transition layer is 4.1%, the content of F element in the transition layer is 11.3%, and the thickness of the transition layer is 82nm.

[0349] Example 14B

[0350] The preparation methods of the lithium replenishing agent in Example 14B and Example 3B are basically the same, except that the coating agent is changed to Li2ZrF6, so that the coating layer thickness is 42nm, the content of X element in the transition layer is 3.2%, the content of F element in the transition layer is 6.8%, and the thickness of the transition layer is 31nm.

[0351] Example 15B

[0352] The preparation methods of the lithium replenishing agent in Example 15B and Example 3B are basically the same, except that the coating agent is changed to Li2TiF6, so that the coating layer thickness is 52nm, the content of X element in the transition layer is 2.9%, the content of F element in the transition layer is 6.4%, and the thickness of the transition layer is 20nm.

[0353] Example 16B

[0354] The preparation methods of the lithium replenishing agent in Example 16B and Example 3B are basically the same, except that the coating agent is changed to Li2SiF6, so that the coating layer thickness is 46nm, the content of X element in the transition layer is 2.8%, the content of F element in the transition layer is 5.9%, and the thickness of the transition layer is 23nm.

[0355] Example 17B

[0356] The preparation methods of the lithium replenishing agent in Example 17B are basically the same as those in Example 3B, except that the coating agent is changed to LiSbF6, so that the content of X element in the transition layer is 3.4%, the content of F element in the transition layer is 7.1%, and the thickness of the transition layer is 21 nm.

[0357] Example 18B

[0358] The preparation methods of the lithium replenishing agent in Example 18B and Example 3B are basically the same, except that the coating agent is changed to LiBiF4, so that the coating layer thickness is 41nm, the content of X element in the transition layer is 3.3%, the content of F element in the transition layer is 6.9%, and the thickness of the transition layer is 32nm.

[0359] Example 19B

[0360] The preparation methods of the lithium replenishing agent in Example 19B and Example 3B are basically the same, except that the coating agent is changed to LiInF4, so that the content of X element in the transition layer is 3.2%, the content of F element in the transition layer is 6.9%, and the thickness of the transition layer is 23nm.

[0361] Example 20B

[0362] The preparation methods of the lithium replenishing agent in Example 20B and Example 3B are basically the same, except that the coating agent is changed to LiGaF4, so that the coating layer thickness is 44nm, the content of X element in the transition layer is 3.5%, the content of F element in the transition layer is 7.6%, and the thickness of the transition layer is 26nm.

[0363] Comparative Example 1B

[0364] The lithium supplement agent in Comparative Example 1B was Li2NiO2, which was not surface coated.

[0365] Comparative Example 2B

[0366] The preparation methods of the lithium supplement in Comparative Example 2B and Example 1B are basically the same, except that Al2O3 is used as the coating agent.

[0367] Comparative Example 3B

[0368] The preparation methods of the lithium supplement in Comparative Example 3B and Example 1B are basically the same, except that TiO2 is used as a coating agent.

[0369] Comparative Example 4B

[0370] The preparation methods of the lithium supplement in Comparative Example 4B and Example 1B are basically the same, except that LiNi is used. 0.33 Co 0.33 Mn 0.33 O2 was used as a coating agent.

[0371] Comparative Example 5B

[0372] The lithium supplementer for Comparative Example 5B was Li5FeO4, which was not surface coated.

[0373] Comparative Example 6B

[0374] The lithium supplementer for Comparative Example 6B was Li6CoO4, which was not surface coated.

[0375] Experimental example:

[0376] The lithium supplement, conductive carbon black, and PVDF from the examples and comparative examples were dispersed in NMP at a mass ratio of 8:1:1. The positive electrode was obtained by slurry preparation, coating, drying, and rolling. A lithium metal sheet was used as the negative electrode, a Celgard 2400 polypropylene membrane as the separator, and a mixed solution of EC and DMC containing 1 mol / L lithium hexafluorophosphate (volume ratio 1:1) as the electrolyte. The battery was assembled with the positive electrode in an argon-filled glove box.

[0377] 1. Dn50: The particle size Dn50 of the lithium replenishment material was tested using a laser particle size analyzer.

[0378] 2. Coating layer thickness and transition layer thickness: The thickness of the coating layer or transition layer in this application can be obtained by cutting the lithium supplement agent and testing the cross-section using a transmission electron microscope (TEM), and taking the average thickness of 20 particles.

[0379] 3. X element content and F element content in the transition layer: These were determined using aberration-corrected transmission electron microscopy (TEM) and electron energy loss spectroscopy (EELS). Specifically, the positions of the particles to be observed were calibrated using TEM, and then the particles were scanned and analyzed using EELS to obtain the surface distribution map and specific content of the elements.

[0380] 4. Charging capacity test: Using the LAND battery testing system, charge at a constant current rate of 1C to 4.2V, and then charge at a constant voltage of 4.2V until the current is equal to 0.03C. The charging capacity at this time is recorded as the 1C charging capacity.

[0381] 5. After the lithium replenishing agent powder is left to stand for 24 hours at a temperature of 25℃ and an ambient humidity of 40%, the battery is made according to the above steps and charged at a constant current rate of 1C to 4.2V. Then, it is charged at a constant voltage of 4.2V until the current is equal to 0.03C. The charging capacity at this time is recorded as the 1C charging capacity after the powder has stood for 24 hours.

[0382] 6. Cycle Performance: The positive electrode active material NCM333, lithium supplement, conductive carbon black, and PVDF of the examples and comparative examples were dispersed in NMP at a mass ratio of 7.8:0.2:1:1. The positive electrode sheet was obtained by slurry preparation, coating, drying, and rolling. A lithium metal sheet was used as the negative electrode sheet, a Celgard 2400 polypropylene membrane as the separator, and a mixed solution of EC and DMC containing 1 mol / L lithium hexafluorophosphate (volume ratio 1:1) as the electrolyte. The battery was assembled with the above positive electrode sheet in an argon-filled glove box.

[0383] At 25°C, the capacitor was charged at a constant current rate of 1C to 4.2V, then charged at a constant voltage of 4.2V to a current rate of 0.5C, and finally discharged at a discharge rate of 1C to 2.5V. This charge-discharge cycle was repeated 300 times. The discharge capacity Q1 at the first cycle and the discharge capacity Q at the 300th cycle were measured. 300 The capacity retention rate after 300 cycles is Q = Q 300 / Q1*100%.

[0384] Table 1B

[0385] As shown in Table 1B, compared with Comparative Examples 1B-6B, the lithium replenishing agent provided in this application has a coating layer containing lithium fluoride. The lithium fluoride has excellent chemical stability and good lithium-ion conductivity, which can effectively prevent adverse reactions between the lithium replenishing material and the electrolyte or other active substances, inhibit the formation of residual alkali, and promote the rapid migration of lithium ions, thereby improving the stability and kinetic performance of the lithium replenishing agent, which is conducive to the utilization of the charging capacity of the lithium replenishing agent, improving the lithium replenishing effect of the lithium replenishing agent, and improving the cycle performance of the battery.

[0386] Comparative studies of Examples 1B-6B show that when the mass percentage of lithium fluoride in the lithium replenishing agent is 0.1%-10%, the coating layer thickness is 1nm-500nm, and the transition layer thickness is 2nm-200nm, the lithium replenishment effect of the lithium replenishing agent can be further improved, thus enhancing the battery's cycle performance. In particular, when the mass percentage of lithium fluoride in the lithium replenishing agent is 0.5%-2%, the lithium replenishment effect can be further improved, further enhancing the battery's cycle performance.

[0387] Comparing Examples 3B, 11B, and 14B-20B, it can be seen that when the lithium-containing fluoride is LiAlF4 and / or Li3AlF6, the lithium replenishment effect of the lithium replenishing agent can be further improved, thereby improving the cycle performance of the battery.

[0388] Finally, it should be noted that other embodiments of this application will readily conceive of by those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and alterations may be made without departing from its scope. The scope of this application is limited only by the appended claims.

Claims

1. A composite lithium supplement material, wherein, comprising a lithium-rich compound core and a coating layer coated on at least part of a surface of the lithium-rich compound core, the coating layer comprising Li y Al z PO 4-x F 1+x ; wherein 0≤x<4, y>0, z>0.

2. The lithium-lithiated composite material of claim 1, wherein, The lithium-rich compound core includes a core layer and a transition layer covering at least a portion of the surface of the core layer. The core layer includes a lithium-rich compound, and the transition layer includes an element-doped lithium-rich compound, wherein the element includes at least one of P, Al, and F.

3. The lithium-lithiating material composite according to claim 1 or 2, wherein, y:z = 1-10:

1.

4. The lithium supplement material according to any one of claims 1-3, wherein, 0.02≤x≤0.1; and / or, 0.5≤y≤3; and / or, 0.1≤z≤1.

5. The lithium supplement material according to any one of claims 1-4, wherein, The mass of the coating layer accounts for 0.1-2% of the mass of the lithium-rich compound core; and / or, the thickness of the coating layer is 1-500 nm.

6. The lithium-lithiating material composite according to any one of claims 1 to 5, wherein, The Li y Al z PO 4-x F 1+x The particle size Dn50 of the LiPOF satisfies: 1 nm ≤ Dn50 ≤ 50 nm.

7. The lithium-lithiated composite material of claim 2, wherein, The element-doped lithium-rich compound has at least one of the following structures: layered structure, rock salt-like structure, and spinel-like structure.

8. The lithium-lithiated composite material of claim 7, wherein, The mass of P element in the transition layer accounts for 0.1-20.8% of the mass of the transition layer; and / or, the mass of Al element in the transition layer accounts for 0.1-18.2% of the mass of the transition layer; and / or, the mass of F element in the transition layer accounts for 0.1-12.8% of the mass of the transition layer.

9. The lithium-lithiating material composite according to claim 7 or 8, wherein, The thickness of the transition layer is 2-499 nm.

10. The lithium-lithiating material composite according to any one of claims 7-9, wherein, The lithium-rich compound includes at least one of Li2NiO2, Li6CoO4, and Li5FeO4.

11. The lithium-lithiating material composite according to any one of claims 7-10, wherein, The particle size Dn50 of the lithium-rich compound satisfies: 500nm≤Dn50≤15μm.

12. A method of preparing the composite lithium supplement material according to any one of claims 1-11, wherein, include: The mixture including a lithium-rich compound, Li y Al z PO 4-x F 1+x is subjected to calcination treatment to obtain the composite lithium supplement material.

13. The production method according to claim 12, wherein said lithium-rich compound, Li y Al z PO 4-x F 1+x mass ratio of 100:0.1-2.

14. The production method according to claim 12 or 13, wherein, The calcination treatment temperature is 200-800℃, and the calcination treatment time is 0.5-6h.

15. The method of making according to any one of claims 12-14, wherein, The calcination temperature is 300-600℃, and the calcination time is 2-6 hours.

16. The method of making according to any one of claims 12-15, wherein, The method further comprises, before the calcining, mixing the lithium-rich compound, Li y Al z PO 4-x F 1+x After the mixing of the solvent, spray drying is performed to obtain the mixture; the spray drying conditions comprise: The pressure is 0.2-1 MPa; and / or the inlet temperature is 100-300℃; and / or the outlet temperature is 80-100℃; and / or the feed rate is 0.5-2 L / h.

17. A positive electrode sheet, wherein Includes the composite lithium replenishing material according to any one of claims 1-11, or the composite lithium replenishing material prepared by the preparation method according to any one of claims 12-16.

18. A battery, wherein, Includes the positive electrode sheet as described in claim 17.

19. An electronic device, comprising: Includes the battery as described in claim 18.