Negative electrode material, composite negative electrode material, negative electrode sheet, and secondary battery

By sieving and controlling the lattice defect distortion coefficient of carbon-based material particles of different sizes, the synergistic effect between particles is achieved, which solves the shortcomings of lithium-ion battery anode materials in terms of capacity, efficiency and expansion rate, and improves the performance of secondary batteries.

WO2026238064A1PCT designated stage Publication Date: 2026-11-19BTR NEW MATERIAL GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/096999
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials have shortcomings in balancing capacity, initial coulombic efficiency, and electrode expansion rate. In particular, graphite anode materials have limited specific capacity, and silicon-based materials suffer structural damage due to volume expansion during charge and discharge.

Method used

Carbon-based material particles of different sizes are obtained by sieving, and their lattice defect distortion coefficients are controlled so that the lattice defect distortion coefficients of large, medium and small particles meet a specific relationship, thereby optimizing their hardness and toughness, realizing the synergistic effect between particles, buffering stress, avoiding structural damage, and combining them with silicon-based materials.

Benefits of technology

It improves the initial discharge capacity and initial coulombic efficiency of the negative electrode material, reduces the electrode expansion rate, and enhances the cycle stability and electrochemical performance of the secondary battery. In particular, when combined with silicon-based materials, it significantly improves the overall performance of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026096999_19112026_PF_FP_ABST
    Figure CN2026096999_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of secondary batteries, and discloses a negative electrode material, a composite negative electrode material, a negative electrode sheet, and a secondary battery. The negative electrode material comprises a carbon-based material. The negative electrode material is sieved using a 600-mesh sieve, the oversize particles that fail to pass through the 600-mesh sieve are designated as a first fraction, the undersize particles that pass through the 600-mesh sieve are sieved again using a 1000-mesh sieve, the oversize particles that fail to pass through the 1000-mesh sieve are designated as a second fraction, and the undersize particles that pass through the 1000-mesh sieve are designated as a third fraction. The Raman spectra of the negative electrode material, the first fraction, the second fraction, and the third fraction each exhibit a D peak and a G peak. The lattice defect distortion coefficients of the first fraction, the second fraction, and the third fraction are Va, Vb, and Vc, respectively, satisfying: Vb≥Va and Vb>Vc, or Vb >Va and Vb≥Vc. When the negative electrode material is made into a negative electrode sheet for use in a secondary battery, the capacity and initial coulombic efficiency are improved, and the expansion rate of the electrode sheet is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

A negative electrode material, a composite negative electrode material, a negative electrode sheet, and a secondary battery

[0001] This application claims priority to Chinese patent application 202510626008.7, filed on May 14, 2025. The entire contents of the aforementioned Chinese patent application are incorporated herein by reference. Technical Field

[0002] This application relates to the field of secondary battery technology, and more specifically, to a negative electrode material, a composite negative electrode material, a negative electrode sheet, and a secondary battery. Background Technology

[0003] Lithium-ion batteries are widely used in 3C products, power devices, and energy storage equipment due to their advantages such as low self-discharge rate, high charge-discharge efficiency, no memory effect, and long cycle life. Among these, the anode material is a crucial component of lithium-ion batteries, and its performance directly affects the electrochemical performance of the battery. Graphite anode materials have attracted widespread attention due to their low charge-discharge plateau and low cost. However, the limited specific capacity of graphite anode materials results in poor capacity and initial coulombic efficiency in secondary batteries. Silicon-based materials are one option for improving specific capacity and initial coulombic efficiency; however, adding silicon-based materials to graphite causes silicon to expand by approximately 300% during charge-discharge, far exceeding the volume change of graphite. This can lead to cracking or even peeling of the graphite's lamellar structure, accelerating structural damage and performance degradation of the electrode material. Summary of the Invention

[0004] The main objective of this application is to provide a negative electrode material, a composite negative electrode material, a negative electrode sheet, and a secondary battery to solve the problem that existing negative electrode materials cannot simultaneously achieve capacity, initial coulombic efficiency, and electrode expansion rate.

[0005] To achieve the above objectives, according to a first aspect of this application, a negative electrode material is provided, comprising a carbon-based material; the negative electrode material is sieved using a 600-mesh sieve, and the particles that fail to pass through the sieve are the first sieve material; the particles that pass through the 600-mesh sieve are sieved again using a 1000-mesh sieve, and the particles that fail to pass through the sieve are the second sieve material; the particles that pass through the 1000-mesh sieve are the third sieve material.

[0006] The Raman spectra of the negative electrode material, the first sieve material, the second sieve material, and the third sieve material all exhibit D and G peaks.

[0007] The lattice defect distortion coefficients of the first, second, and third sieve materials are respectively V a V b V c Satisfying: V b ≥V a And V b >Vc Or, V b >V a And V b ≥V c ;

[0008] V a V b V c We obtain the following from equations I, II, and III:

[0009] in, The average value of the D / G half-peak width ratio of the first sieve material; This represents the average D / G half-peak width ratio of the second sieve material; W1 is the average D / G half-peak width ratio of the third sieve material; W1 is the average D / G half-peak width ratio of the negative electrode material; ΔF Da ΔF is the difference in peak position between the D peak of the first sieve material and the negative electrode material; Db ΔF is the difference in the peak position of the D peak between the second sieve material and the negative electrode material; Dc It is the difference between the peak position of the D peak of the third sieve material and the negative electrode material.

[0010] A second aspect of this application provides a composite anode material, comprising the anode material of the first aspect and a silicon-based material.

[0011] A third aspect of this application provides a negative electrode sheet, which includes the aforementioned negative electrode material or composite negative electrode material.

[0012] A fourth aspect of this application provides a secondary battery, which includes the aforementioned negative electrode.

[0013] By applying the technical solution of this application, this application ensures that V is controlled by adjusting the lattice defect distortion coefficient V of particles of different sizes in the negative electrode material. b ≥V a And V b >V c Or, V b >V a And V b ≥V cBy controlling the defect distribution of carbon-based material particles and optimizing their hardness and toughness, the material can better buffer stress and avoid structural damage. This helps maintain the stability of the particle structure and the close contact between particles during charging and discharging, thereby improving the overall conductivity. At the same time, it achieves synergistic effects among large, medium, and small particle sizes in the negative electrode material. This avoids cracking or peeling caused by excessive distortion of small particles, and also prevents the problem of large particles being unable to effectively buffer the volume expansion of the negative electrode due to excessively high lattice defect distortion coefficients. This size synergy effect helps reduce the expansion rate of the electrode during charging and discharging, and reduces the formation of the SEI layer. As a result, the negative electrode material has both a low expansion rate, high capacity, and high initial coulombic efficiency. Specifically, it can achieve an initial discharge capacity ≥350mAh / g, an initial coulombic efficiency ≥92%, a capacity retention rate ≥95.3% after 50 cycles, and an electrode expansion rate ≤23.7%. Furthermore, when the anode material of this application is used in combination with silicon-based materials, it can effectively buffer stress during the expansion of the silicon-based material, effectively balancing the hardness and toughness of the anode material and the volume expansion requirements of the silicon-based material. This allows the anode sheet to maintain good particle contact and conductive network, improves the electrode conductivity, and achieves better electrochemical performance and cycle stability. Specifically, the composite anode material can achieve an initial discharge capacity ≥365mAh / g, an initial coulombic efficiency ≥90%, and an electrode conductivity ≥0.8S / cm and an electrode expansion rate ≤84% after 50 cycles. Attached Figure Description

[0014] Figure 1 is a SEM image of the negative electrode material in one embodiment of this application;

[0015] Figure 2 is a schematic diagram of the structure of a secondary battery provided in one embodiment of this application during charging;

[0016] Figure 3 is a schematic diagram of the structure of a secondary battery provided in one embodiment of this application during discharge.

[0017] Explanation of reference numerals in the attached figures: 100 - Electrode assembly; 101 - Positive electrode; 102 - Negative electrode; 103 - Separator. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] As described in the background section of this application, existing anode materials suffer from capacity decay and poor initial coulombic efficiency. To address these issues, in a typical embodiment of this application, an anode material is provided. The anode material is sieved using a 600-mesh sieve; particles that fail to pass through the sieve are designated as the first sieve material. The particles that pass through the 600-mesh sieve are then sieved again using a 1000-mesh sieve; particles that fail to pass through the 600-mesh sieve are designated as the second sieve material, and particles that pass through the 1000-mesh sieve are designated as the third sieve material. The Raman spectra of the anode material, the first sieve material, the second sieve material, and the third sieve material exhibit D and G peaks. The lattice defect distortion coefficients of the first sieve material, the second sieve material, and the third sieve material are V0, V1, V2, V3, V4, V5, V6, V7, V8, V9 ... a V b V c Satisfying: V b ≥V a And V b >V c Or, V b >V a And V b ≥V c V a V b V c We obtain the following from equations I, II, and III:

[0020] in, The average value of the D / G half-peak width ratio of the first sieve material; This represents the average D / G half-peak width ratio of the second sieve material; W1 is the average D / G half-peak width ratio of the third sieve material; W1 is the average D / G half-peak width ratio of the negative electrode material; ΔF Da ΔF is the difference in peak position between the D peak of the first sieve material and the negative electrode material; Db ΔF is the difference in the peak position of the D peak between the second sieve material and the negative electrode material; Dc It is the difference between the peak position of the D peak of the third sieve material and the negative electrode material.

[0021] The negative electrode material is initially screened using a 600-mesh sieve. Larger particles that fail to pass through the 600-mesh sieve are referred to as the first sieve material; these particles represent a relatively large size range within the negative electrode material. Smaller particles that pass through the 600-mesh sieve require further screening using a 1000-mesh sieve. Particles that fail to pass through the 1000-mesh sieve are referred to as the second sieve material; these particles represent a medium size range within the negative electrode material. Particles that pass through the 1000-mesh sieve are referred to as the third sieve material; these particles represent a relatively small size range within the negative electrode material. It should be noted that the 600-mesh and 1000-mesh sieves used in this application are standard sieves, conforming to the national standard GB / T 6003-2017, and are made of 304 stainless steel.

[0022] The lattice defect distortion coefficient is a parameter used to quantitatively characterize the state of lattice defects and the degree of lattice distortion. The lattice defect state refers to the region in the lattice structure where the atomic arrangement deviates from the ideal crystal structure, while the degree of lattice distortion refers to the degree of local or global lattice deformation caused by the deviation of atomic arrangement from ideal periodicity. A larger lattice defect distortion coefficient indicates a wider distribution of lattice defects and a higher degree of lattice deformation in the material, which directly affects the material's physical, chemical, and mechanical properties.

[0023] Particles of different sizes exhibit varying degrees of lattice defect distortion under the same conditions. Smaller particles, with their higher specific surface area and surface energy, are more prone to accumulating defects, but also exhibit greater mechanical flexibility, effectively buffering volume expansion stress. Larger particles, on the other hand, have difficulty releasing internal stress, making them susceptible to localized lattice defects such as cracking or fissures during charge-discharge cycles when used in secondary batteries. This application addresses this by controlling the lattice defect distortion coefficients of particles of different sizes, effectively balancing the requirements for hardness, toughness, and buffering volume expansion stress in the anode material, maintaining structural integrity, and preventing the generation and propagation of cracks, thereby achieving superior electrochemical performance.

[0024] Specifically, Raman spectroscopy is used to analyze the molecular structure and vibrational modes of materials. Carbon-based materials exhibit two key Raman spectral characteristic peaks: the D peak and the G peak. These two characteristic peaks are located at 1345 cm⁻¹. -1 ~1365cm -1 1575cm -1 ~1585cm -1 Within the range. The D peak represents a defect peak, and its appearance is associated with lattice defects in the graphite layer, such as edge defects, boundary defects, or point defects; while the G peak represents a graphite peak, reflecting the ordered stacking of the graphite layers.

[0025] The full width at half maximum (HWHM) in Raman spectroscopy refers to the complete measurement of the width of a peak at half its peak height, i.e., the distance from the left half-maximum to the right half-maximum. The D / G HWHM ratio can be understood as the ratio of the widths at the half-maximum intensity points (half the maximum intensity value) of the D and G peaks, reflecting the degree of disorder and defect distribution in the material. A larger D / G HWHM ratio indicates the presence of more lattice disorder or defect regions in the material.

[0026] In this application, for the first sieve, the second sieve, and the third sieve, the lattice defect distortion coefficient (V) a V b V c It is related to the D / G half-peak width ratio and the degree of peak position shift. W1 is calculated by averaging the half-width ratio of the D peak to the G peak in the Raman spectra of the first sieve material, the second sieve material, the third sieve material, and the negative electrode material. These refer to the differences between the average D / G half-peak width ratio of the first, second, and third sieve materials and the average D / G half-peak width ratio of their respective total negative electrode materials, reflecting the degree of increase in lattice defects. ΔF Da ΔF Db ΔF Dc These refer to the differences in the positions of the D peaks in the first, second, and third sieve materials compared to the total D peak position of their respective negative electrode materials. This is the blue shift of the D peak position (i.e., the phenomenon of the peak position shifting to a higher frequency), reflecting the degree of lattice distortion in the graphite layer structure. Lattice defect distortion coefficient V a V b V c It reflects the lattice defect state and lattice distortion degree of the internal structure of the first, second, and third sieve materials relative to the overall anode material.

[0027] By limiting V b ≥V a , or V b >V a This indicates that the lattice defect distortion coefficient of the first sieve material does not exceed that of the second sieve material. This means that in the anode material, the lattice defect distortion coefficient of large-sized particles (first sieve material) is less than or equal to that of medium-sized particles (second sieve material), which helps to provide better buffering capacity, thereby better buffering volume expansion.

[0028] By limiting V b ≥V c Or V b >V cThis indicates that the lattice defect distortion coefficient of the third sieve material does not exceed that of the second sieve material. This means that in the anode material, the lattice defect distortion coefficient of small-sized particles (third sieve material) is less than or equal to that of medium-sized particles (second sieve material), which can prevent small-sized particles from cracking or even peeling due to excessive defect distortion, thus affecting the structural stability of the anode material.

[0029] When V is satisfied b ≥V a And V b >V c This indicates that in the negative electrode material, the lattice defect distortion coefficient of large-sized particles (first sieve material) is less than or equal to that of medium-sized particles (second sieve material), and the lattice defect distortion coefficient of small-sized particles (third sieve material) is less than that of medium-sized particles (second sieve material); when V... b >V a And V b ≥V c This indicates that in the negative electrode material, the lattice defect distortion coefficient of large-sized particles (first sieve material) is less than or equal to that of medium-sized particles (second sieve material), and the lattice defect distortion coefficient of small-sized particles (third sieve material) is less than that of medium-sized particles (second sieve material).

[0030] In this way, by controlling the degree of lattice defect distortion of particles of different sizes, the first, second, and third sieve materials can achieve optimal synergistic effects in the anode material, helping to maintain the structural integrity of the particles and their stability during cycling, thereby optimizing the overall mechanical and electrochemical properties of the material. Furthermore, by limiting V... b ≥V a And V b >V c Or, V b >V a And V b ≥V c This effectively controls the defects and distortions inside the negative electrode material, which can not only effectively buffer stress during expansion and slow down the growth rate of the solid electrolyte interphase (SEI) layer, making the SEI layer thinner and more stable, but also avoid the excessively thick SEI layer from increasing the internal resistance of the secondary battery and reducing electrochemical activity and capacity, while reducing side reactions, thereby improving the overall performance of the secondary battery.

[0031] This application controls the lattice defect distortion coefficient of particles of different sizes in the anode material, thereby controlling the defect distribution within the anode material. This optimizes the hardness, toughness, and conductivity of the anode material, while also acting as a buffer during volume expansion, reducing the material's expansion rate. This effectively balances the requirements for hardness, toughness, and buffering volume expansion stress in the anode material, reducing the thickness growth of the SEI layer, and thus achieving superior electrochemical performance, including but not limited to improved capacity, first-time coulombic efficiency, and reduced electrode expansion rate. In addition to its excellent electrochemical performance, the anode material of this application, when used in conjunction with silicon-based materials with high expansion rates, can also simultaneously address the impact of silicon expansion on the performance of the secondary battery.

[0032] In some embodiments, after multiplying Formula I by 100%, the lattice defect distortion coefficient V of the first sieve material is obtained. a Satisfy: 8% ≤ V a ≤80%. Large particles generally have higher structural stability, but during lithium-ion insertion and extraction, uneven internal stress release can lead to stress accumulation and structural damage. If the lattice defect distortion coefficient V of the first sieve material... a If the particle size is too large, the internal structure of the particles will be excessively distorted, resulting in excessive residual stress. This will make the first-screen material extremely prone to breakage when the silicon-based material expands, creating new active surfaces, accelerating the consumption of active lithium, and affecting the cycle stability and capacity retention of the secondary battery; if V a If the graphite particles are too small, the degree of lattice defect distortion inside the particles is very low, and the graphite sheet structure is relatively ordered. Although the graphite particles maintain high toughness and strength, due to their high structural order, their resistance to compression during the volume expansion of silicon-based materials is relatively weak. This leads to the graphite particles breaking during the volume expansion of silicon-based materials due to insufficient elastic deformation capacity, thereby impairing the structural stability and electrochemical performance of the anode material. By controlling the lattice defect distortion coefficient of the large-size first sieve material to 8%–80%, it is possible to ensure that it maintains structural stability and lithium storage capacity while buffering the volume expansion of silicon-based materials.

[0033] The lattice defect distortion coefficient V of the first sieve material a It can be a range of 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or any two of these.

[0034] In some embodiments, after multiplying Formula II by 100%, the lattice defect distortion coefficient V of the second sieve material is obtained. b Satisfy: 16% ≤ V b≤90%. A medium-sized second sieve helps the anode material find a balance between hardness and toughness, effectively buffering the stress on the silicon-based material while preventing excessive fragmentation or loss of lithium intercalation capacity during cycling. This maintains the stability of the graphite sheet structure and the continuity of the conductive network, achieving optimal stress buffering and lithium-ion storage capacity. This is achieved by controlling the lattice defect distortion coefficient V of the second sieve. b With a content of 10% to 90%, the second sieve material plays a role in stress buffering and structural stabilization in the composite material formed by carbon-based and silicon-based materials. The second sieve material can effectively disperse the stress generated by silicon-based materials during charging and discharging while maintaining good electrical conductivity, preventing particle breakage and excessive thickening of the SEI layer, thereby maintaining the high energy density and long cycle life of the secondary battery.

[0035] The lattice defect distortion coefficient V of the second sieve material b It can be a range of 16%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, or any two of these.

[0036] In some embodiments, after multiplying Formula III by 100%, the lattice defect distortion coefficient V of the third sieve material is obtained. c Satisfy: 9% ≤ V c ≤60%. Small-sized third-sieve materials have a higher specific surface area, making them prone to lattice defect distortion during high-temperature processing, but they also possess better surface activity and stress dispersion capabilities. If the lattice defect distortion coefficient V of the third-sieve material... c If the value is too small, it means that the structure of the third sieve material is relatively intact with low internal distortion. Although this improves the mechanical strength and deformation resistance of the third sieve material, it is prone to agglomeration when the silicon-based material expands, affecting the overall dispersion of the negative electrode material, thereby increasing the expansion rate of the electrode and reducing electrochemical performance; if V c An excessively large value indicates excessive distortion of the third sieve material, making it prone to crushing by silicon-based materials and increasing the consumption of active lithium. This can be addressed by controlling the lattice defect distortion coefficient V of the third sieve material. c With a content of 9% to 60%, it can prevent the third-screen material from becoming too fragile due to excessive distortion, reduce particle agglomeration or breakage, find the best balance between deformation resistance and avoiding agglomeration, help maintain good particle dispersion, reduce the overall expansion of the electrode, and avoid structural damage and active lithium consumption caused by excessive distortion, thereby further improving the first coulombic efficiency and energy density of the secondary battery.

[0037] The lattice defect distortion coefficient V of the third sieve material cIt can be a range of 9%, 10%, 12%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any two of these.

[0038] In some preferred embodiments, the lattice defect distortion coefficient V of the third sieve material c Satisfy: 15% ≤ V c ≤60%. This is achieved by further controlling the lattice defect distortion coefficient V of the third sieve material. c The ratio of 15% to 60% helps to control the hardness and toughness of the third sieve material within a moderate range, maintain the dispersion of the negative electrode material, and avoid the problem that the third sieve material is too rigid to adapt to volume changes, resulting in the SEI layer thickening too quickly.

[0039] This application controls the lattice defect distortion coefficient (VL) of the first, second, and third sieves of different sizes. a V b V c Within the aforementioned numerical range, synergistic effects between particles are achieved. For example, large-sized first-sieve materials provide structural stability, medium-sized second-sieve materials optimize stress distribution, and small-sized third-sieve materials improve surface activity and lithium storage. Under this synergistic mechanism, the mechanical properties, electrochemical properties, and compatibility with silicon-based materials of the anode material are effectively balanced. This helps reduce the overall expansion rate of the secondary battery during cycling, reduces the formation of the SEI layer, and accelerates the diffusion rate of lithium ions, thereby achieving optimized performance in secondary battery applications. This includes, but is not limited to, improving the capacity, initial coulombic efficiency, and cycle life of the secondary battery. In particular, when used in conjunction with silicon-based materials, it helps to further suppress the volume expansion of silicon-based materials during charge and discharge, reduce the formation of the SEI layer, and improve the cycle stability and energy density of the secondary battery.

[0040] The D / G half-width ratio reflects the number of internal defects in the material. A larger D / G half-width ratio indicates more lattice defects and a more disordered structure within the material. In some embodiments, the average value W1 of the D / G half-width ratio of the anode material satisfies: 2 ≤ W1 ≤ 7. If W1 is less than 2, it indicates that the graphite sheet structure is too ordered and cannot effectively disperse stress, which is not conducive to buffering the volume change of the silicon-based material during charging and discharging. If W1 is too large, there are too many internal defects in the material, which may lead to instability of the graphite sheet structure and affect the mechanical and electrochemical properties of the material. By controlling the average value W1 of the D / G half-width ratio of the anode material to be between 2 and 7, the lattice defects of the graphite component in the anode material are ensured to be within a moderate range, which is beneficial to improving the buffering capacity of the anode material against the expansion of the silicon-based material, while maintaining the lithium storage capacity of the graphite. Specifically, the average value W1 of the D / G half-width ratio of the anode material can be a range of 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, or any combination thereof.

[0041] In the specific implementation of this application, 15 points are selected on the test sample of the negative electrode material. Raman spectroscopy analysis is used to obtain 15 Raman spectra corresponding to these 15 points. Each spectrum corresponds to a D / G half-peak width ratio (HWHM). The HWHM values ​​of the D peak and G peak in these 15 Raman spectra are measured and recorded. The HWHM values ​​of the D peak and G peak in these 15 Raman spectra are added together to obtain the sum. Finally, the sum is divided by 15 to obtain the average value of the D / G HWHM of the negative electrode material.

[0042] In some embodiments, the average D / G half-peak width ratio of the first sieve material satisfy: like If the particles are too small, it means that there are very few defects inside the first sieve material, and the structure is highly ordered. Such particles have weak resistance to compression when facing the expansion of silicon-based materials, and cannot effectively disperse stress, leading to increased electrode expansion and decreased structural stability. If the diameter is too large, numerous lattice defects exist within the first sieve material, resulting in a relatively disordered structure. While this increases the stress buffering effect of graphite on the expansion of silicon-based materials, it limits the lithium intercalation capability between graphite layers, thus reducing its lithium storage capacity. By controlling the average D / G half-width ratio of the first sieve material... A value of 4 to 7 helps improve the stress buffering capacity of the anode material when facing the large volume expansion of silicon-based materials, while maintaining sufficient mechanical strength and electrical conductivity. Specifically, the average D / G half-peak width ratio of the first sieve material... It can be a range consisting of 4, 4.5, 5, 5.5, 6, 6.5, 7, or any two of them.

[0043] In some embodiments, the average D / G half-peak width ratio of the second sieve material satisfy: By controlling the D / G half-width at half-maximum (HWHM) of the medium-sized second sieve within this range, the aim is to find a balance between hardness and toughness to achieve effective stress dispersion and lithium-ion storage. A higher HWHM reflects more lattice defects, which to some extent enhances the material's stress buffering performance, but this also needs to be limited to avoid affecting the stability of the graphite structure and electrochemical performance. The average HWHM of the second sieve is controlled by... With a value of 4.5–8, it can effectively buffer the volume expansion of silicon-based materials while maintaining lithium storage performance. Specifically, the average D / G half-width ratio of the second sieve material is... It can be a range consisting of 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, or any two of them.

[0044] In some embodiments, the average D / G half-peak width ratio of the third sieve material satisfy: Smaller-sized third-screen materials typically have higher specific surface area and surface energy. This can be achieved by controlling the average D / G half-peak width ratio of the third-screen material. A value of 4–8 enhances the interfacial interaction between the third sieve material and the silicon-based material particles, contributing to the uniform dispersion of the silicon-based material and reducing the overall expansion of the electrode, while ensuring structural stability. Specifically, the average D / G half-width ratio of the third sieve material... It can be a range consisting of 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, or any two of them.

[0045] This application optimizes the microstructure of materials by controlling the average D / G half-peak width ratio of the first, second, and third sieve materials respectively, maximizing the synergistic effect between different particles. This synergistic effect effectively buffers the volume expansion of silicon-based materials during charging and discharging, slows down the growth rate of the solid electrolyte interphase (SEI) layer, reduces the internal resistance of the secondary battery, and also improves the diffusion rate and insertion / extraction efficiency of lithium ions. At the same time, it ensures that graphite particles can exert a high capacity, thereby achieving the best balance in terms of the stability, energy density, and cycle life of the secondary battery, including but not limited to improving the capacity, initial coulombic efficiency, and reducing the electrode expansion rate of the secondary battery.

[0046] The position of the D peak is closely related to the lattice defects and disorder within the material. The specific position of the D peak in the Raman spectrum is directly associated with the lattice defects of the carbon-based material. In some embodiments, the peak position F of the D peak in the anode material... D1 Meets the requirement: 1351cm -1 ≤F D1 ≤1353cm -1By controlling the peak position of the D peak of the negative electrode material at 1351 cm⁻¹ -1 ~1353cm -1 Within a certain range, ensuring that the overall lattice defects of the anode material are at an appropriate level and avoiding excessive compaction and disorder, this optimized defect distribution helps to improve the stress buffering capacity of the anode material while maintaining good electrochemical performance.

[0047] In the specific implementation of this application, 15 points are selected on the test sample of the negative electrode material. Raman spectroscopy analysis is used to obtain 15 Raman spectra corresponding to these 15 points. Each spectrum corresponds to the peak position of a D peak. The peak positions of the D peaks in these 15 Raman spectra are measured and recorded. The peak positions of the D peaks in these 15 Raman spectra are added together to obtain the sum. Finally, the sum is divided by 15 to obtain the peak position of the D peak of the negative electrode material.

[0048] A blue shift (shift of the D peak to higher wavenumbers) typically indicates an increase in defect density within the crystal lattice. ΔF Da ΔF Db ΔF Dc The difference in peak position between the D peak of particles of different sizes and the overall anode material. A moderate distribution of lattice defects not only helps the anode material disperse stress and prevent structural damage when the silicon-based material expands, but also ensures that the graphite particles have sufficient lithium storage space to maintain high capacity.

[0049] In some embodiments, the difference ΔF between the peak positions of the first sieve material and the negative electrode material is... Da Satisfying: 10cm -1 ≤ΔF Da ≤30cm -1 It can be understood that in Raman spectroscopy, compared to the negative electrode material, the position of the D peak of the first sieve material shifts towards higher frequencies, also known as a blue shift. The difference in peak position between the first sieve material and the negative electrode material can be understood as the blue shift amount. The blue shift amount reflects the degree of lattice defects and the degree of disorder of the graphite sheets within the material. By controlling the difference in peak position (blue shift amount) between the first sieve material and its corresponding negative electrode material to 10 cm⁻¹... -1 ~30cm -1 This ensures that the lattice defect distribution of graphite in the large-sized first sieve of the anode material can work in synergy with other particles to achieve optimal performance, optimizes the relationship between stress buffering capacity and lithium intercalation depth, and ensures the stability and high capacity of the anode material.

[0050] The difference ΔF between the peak positions of the D peaks of the first sieve material and the negative electrode material Da It can be 10cm -1 15cm -1 20cm -1 25cm -1 30cm-1 or a range consisting of any two of them.

[0051] In some embodiments, the difference ΔF between the peak positions of the second sieve material and the negative electrode material is... Db Meets the requirement of 6.5cm -1 ≤ΔF Db ≤11cm -1 It can be understood that in Raman spectroscopy, compared to the negative electrode material, the D peak of the second sieve material shifts to a higher frequency direction, also known as a blue shift. The difference in peak position between the second sieve material and the negative electrode material can be understood as the blue shift amount. The blue shift amount reflects the degree of lattice defects and the degree of disorder of the graphite sheets within the material. By controlling the difference in peak position (blue shift amount) between the first sieve material and its corresponding negative electrode material to 6.5 cm⁻¹, this method can be achieved. -1 ~11cm -1 This ensures that the lattice defect distribution of graphite in the medium-sized second sieve of the anode material can work in synergy with other particles to achieve optimal performance, optimizes the relationship between stress buffering capacity and lithium intercalation depth, and ensures the stability and high capacity of the anode material.

[0052] The difference ΔF between the peak positions of the D peaks of the second sieve material and the negative electrode material Db It can be 6.5cm. -1 8cm -1 9cm -1 10cm -1 11cm -1 or a range consisting of any two of them.

[0053] In some embodiments, the difference ΔF between the peak positions of the third sieve material and the negative electrode material is... Dc Satisfying: 8cm -1 ≤ΔF Dc ≤20cm -1 It can be understood that in Raman spectroscopy, compared to the anode material, the D peak of the third sieve material shifts to a higher frequency, also known as a blue shift. The difference in peak position between the third sieve material and the anode material can be understood as the blue shift amount. The blue shift amount reflects the degree of lattice defects and the disorder of graphite sheets within the material. By controlling the difference in peak position (blue shift amount) between the third sieve material and its corresponding anode material to 8 cm⁻¹, this method can be achieved. -1 ~20cm -1 This ensures that the lattice defect distribution of graphite in the small-sized third sieve of the anode material can work in synergy with other particles to achieve optimal performance, optimizes the relationship between stress buffering capacity and lithium intercalation depth, and ensures the stability and high capacity of the anode material.

[0054] The difference ΔF between the peak positions of the D peaks of the third sieve material and the negative electrode material Dc It can be 8cm-1 10cm -1 12cm -1 15cm -1 18cm -1 20cm -1 or a range consisting of any two of them.

[0055] This application optimizes the lattice defect distribution of each particle by adjusting the difference between the peak positions of the D peaks of the first, second, and third sieve materials and the overall D peak position of the negative electrode material. This achieves microstructural synergy among particles of different sizes, resulting in the optimal synergistic effect. Consequently, it establishes a structural environment conducive to dispersing expansion stress and ensures that each particle can maintain efficient lithium-ion insertion / extraction capabilities. This helps improve the overall performance of the secondary battery, including extending cycle life, increasing energy density, and ensuring the safety of the secondary battery.

[0056] In the specific implementation of this application, the average value of the D / G half-peak width ratio of the first screen material It can be obtained through equation I-1, which is:

[0057] In Equation I-1, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; The D / G half-width ratio in the i-th Raman spectrum of the first sieve material. This refers to the average D / G half-peak width ratio of the first sieve material. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0058] Specifically, 100 points were selected from the test sample of the first sieve material. Raman spectroscopy analysis was used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to a D / G half-peak width ratio (HWHM). The HWHM values ​​of the D and G peaks in these 100 Raman spectra were measured and recorded. The HWHM values ​​of the D and G peaks in these 100 Raman spectra were added together to obtain a sum. Finally, the sum was divided by 100 to obtain the average HWHM of the first sieve material. That is, the average HWHM of the first sieve material is calculated using Equation I-1.

[0059] In some embodiments, the D / G half-peak width ratio of the first screen material is 1.5 to 13, i.e. satisfy: That is, the D / G half-width ratio in the i-th Raman spectrum of the first sieve material is 1.5 to 13. In the specific implementation of this application, the D / G half-width ratio of the first sieve material can be flexibly adjusted to adjust the internal defect distribution of the carbon-based material, thereby helping to find the optimal balance between the structural stability and lithium intercalation performance of the anode material to meet the performance requirements of secondary batteries.

[0060] The D / G half-peak width ratio of the first sieve material can be a range of 1.5, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or any two of these.

[0061] In the specific implementation of this application, the average value of the D / G half-peak width ratio of the second screen material It can be obtained from Equation II-1, which is:

[0062] In Equation II-1, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; The full width at half maximum (FWHM) ratio of the D peak to the G peak in the i-th Raman spectrum of the second sieve material. This refers to the average D / G half-peak width ratio of the second sieve material. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0063] Specifically, 100 points were selected from the test sample of the second sieve material. Raman spectroscopy analysis was used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to a D / G half-peak width ratio (HWHM). The HWHM values ​​of the D and G peaks in these 100 Raman spectra were measured and recorded. The HWHM values ​​of the D and G peaks in these 100 Raman spectra were added together to obtain a sum. Finally, the sum was divided by 100 to obtain the average HWHM of the second sieve material. That is, the average HWHM of the second sieve material is calculated using Equation II-1.

[0064] In some embodiments, the D / G half-peak width ratio of the second sieve material is 2 to 18, i.e. satisfy That is, the half-width ratio (WHM) of the D peak to the G peak in the i-th Raman spectrum of the second sieve material is 2 to 18. In the specific implementation of this application, the WHM of the second sieve material can be flexibly adjusted to adjust the distribution of internal defects in the carbon-based material, thereby helping to find the optimal balance between the structural stability and lithium intercalation performance of the anode material to meet the performance requirements of secondary batteries.

[0065] The D / G half-peak width ratio of the second sieve material can be a range of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 15, 18 or any two of them.

[0066] In the specific implementation of this application, the average value of the D / G half-peak width ratio of the third sieve material It can be obtained from Equation III-1, which is:

[0067] In Equation III-1, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; The D / G half-width ratio in the i-th Raman spectrum of the third sieve material. This refers to the average D / G half-peak width ratio of the third sieve material. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0068] Specifically, 100 points were selected from the test sample of the third sieve. Raman spectroscopy analysis was used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to a D / G half-peak width ratio (HWHM). The HWHM values ​​of the D and G peaks in these 100 Raman spectra were measured and recorded. The HWHM values ​​of the D and G peaks in these 100 Raman spectra were added together to obtain a sum. Finally, the sum was divided by 100 to obtain the average HWHM of the second sieve. That is, the average HWHM of the second sieve was calculated using Equation III-1.

[0069] In some embodiments, the D / G half-peak width ratio of the third sieve material is 1.2 to 13. satisfy: That is, the D / G half-width ratio in the i-th Raman spectrum of the third sieve material is 1.2 to 13. In the specific implementation of this application, the D / G half-width ratio of the third sieve material can be flexibly adjusted to adjust the internal defect distribution of the carbon-based material, thereby helping to find the optimal balance between the structural stability and lithium intercalation performance of the anode material to meet the performance requirements of secondary batteries.

[0070] The D / G half-peak width ratio of the third sieve material can be a range of 1.2, 2, 3, 4, 5, 8, 10, 12, 13 or any two of these.

[0071] In the specific implementation of this application, the difference ΔF between the peak positions of the D peaks of the first sieve material and the negative electrode material is... Da It can be obtained from equation I-2, which is:

[0072] In Equation I-2, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; F Dai F represents the peak position of peak D in the i-th Raman spectrum of the first sieved material; D1 The peak position of peak D in the Raman spectrum of the negative electrode material is given. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0073] Specifically, 100 points are selected from the test sample of the first sieve material. Raman spectroscopy analysis is used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to the peak position of a D peak. The peak positions of the D peaks in these 100 Raman spectra are measured and recorded. The peak positions of the D peaks in these 100 Raman spectra are added together to obtain a sum. Finally, the sum is divided by 100 to obtain the peak position of the D peak of the first sieve material. That is, the peak position of the D peak of the first sieve material is calculated using Equation I-2.

[0074] In the specific implementation of this application, the difference ΔF between the peak positions of the D peaks of the second sieve material and the negative electrode material is... Db It can be obtained from Equation II-2, which is:

[0075] In Equation II-2, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; F Dbi The peak position of peak D in the i-th Raman spectrum of the second sieve material; F D1 The peak position of peak D in the Raman spectrum of the negative electrode material is given. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0076] Specifically, 100 points are selected from the test sample of the second sieve material. Raman spectroscopy analysis is used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to the peak position of a D peak. The peak positions of the D peaks in these 100 Raman spectra are measured and recorded. The peak positions of the D peaks in these 100 Raman spectra are added together to obtain a sum. Finally, the sum is divided by 100 to obtain the peak position of the D peak of the second sieve material. That is, the peak position of the D peak of the second sieve material is calculated using Equation II-2.

[0077] In the specific implementation of this application, the difference ΔF between the peak positions of the D peak of the third sieve material and the negative electrode material is... Dc It can be obtained from Equation III-2, which is:

[0078] In Equation III-2, n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; FDci The peak position of peak D in the i-th Raman spectrum of the third sieve material; F D1 The peak position of peak D in the Raman spectrum of the negative electrode material is given. Here, n represents the total number of measurements, set to 100 here to ensure the statistical significance and representativeness of the data. i represents the sequence number of the measurement, ranging from 1 to n, all being positive integers.

[0079] Specifically, 100 points were selected from the test sample of the third sieve material. Raman spectroscopy analysis was used to obtain 100 Raman spectra corresponding to these 100 points. Each spectrum corresponds to the peak position of a D peak. The peak positions of the D peaks in these 100 Raman spectra were measured and recorded. The peak positions of the D peaks in these 100 Raman spectra were added together to obtain a sum. Finally, the sum was divided by 100 to obtain the peak position of the D peak of the third sieve material. That is, the peak position of the D peak of the third sieve material is calculated using Equation III-2.

[0080] In some embodiments, the D50 particle size of the first sieve material is 13.5 μm to 16.0 μm. Larger particle sizes in the first sieve material provide higher compaction density, which helps improve the energy density of the secondary battery. By controlling the D50 particle size of the first sieve material within the above range, problems such as conductive network interruption and increased lithium-ion transport paths caused by excessively large particles are avoided, and lattice defect distortion is also easier to control. Specifically, the D50 particle size of the first sieve material can be a range of 13.5 μm, 14 μm, 14.5 μm, 15 μm, 15.5 μm, 16.0 μm, or any combination thereof.

[0081] In some embodiments, the D50 particle size of the second sieve material is 13 μm to 15.0 μm. Medium-sized particles offer a good balance in terms of compaction density, conductivity, and lithium-ion diffusion capability. By controlling the D50 particle size of the second sieve material within this range, a stable and efficient structure can be formed in the anode material, working synergistically with the first and third sieve materials to improve the performance of the anode material. Specifically, the D50 particle size of the second sieve material can be a range of 13 μm, 13.5 μm, 14 μm, 14.5 μm, 15.0 μm, or any combination thereof.

[0082] In some embodiments, the D50 particle size of the third sieve material is 8 μm to 12.8 μm. Smaller particles help form a denser conductive network, shorten the lithium-ion transport path, and improve the kinetic performance of the material. By controlling the D50 particle size of the third sieve material within the above range, the dramatic increase in specific surface area caused by excessively small particles is avoided, which would lead to an increase in surface side reactions. At the same time, the structural stability of the negative electrode material and good lithium-ion insertion / extraction capabilities are ensured. Specifically, the D50 particle size of the third sieve material can be a range of 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.8 μm, or any combination thereof.

[0083] This application improves the compaction density of the negative electrode material by controlling the D50 particle size of the first, second, and third sieve materials within the aforementioned range, thereby increasing the energy density of the secondary battery. Simultaneously, it helps form a dense conductive network, shortens the lithium-ion diffusion path, accelerates lithium-ion transport, and enhances the electrochemical reaction rate of the negative electrode material. Furthermore, it helps strengthen the structural stability of the negative electrode material, reduces particle breakage and surface side reactions during cycling, thereby extending the cycle life of the secondary battery.

[0084] In this application, D50 particle size represents the particle size corresponding to a cumulative particle size distribution volume percentage of 50%, and D90 particle size represents the particle size corresponding to a cumulative particle size distribution volume percentage of 90%.

[0085] In some embodiments, the mass percentage of the first sieve material in the negative electrode material is 30% to 40%. Controlling the mass percentage of the first sieve material within this range is beneficial for improving the mechanical strength and stability of the negative electrode material. The mass percentage of the first sieve material in the negative electrode material can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, or any combination thereof.

[0086] In some embodiments, the mass percentage of the second sieve material in the anode material is 40% to 50%. Controlling the mass percentage of the second sieve material within this range helps to improve the compaction density and lithium-ion insertion / extraction rate of the material, while ensuring a uniform distribution of lattice defects in the anode material, thereby maintaining overall electrochemical performance and structural stability. The mass percentage of the second sieve material in the anode material is a range of 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, or any combination thereof.

[0087] In some embodiments, the mass percentage of the third sieve material in the negative electrode material is 10% to 30%. Controlling the mass percentage of the third sieve material within this range is beneficial for improving the conductive network and lithium-ion transport path of the negative electrode material, thereby enhancing the kinetic performance of the negative electrode material. The mass percentage of the third sieve material in the negative electrode material is a range of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, or any combination thereof.

[0088] This application, by controlling the mass proportion of particles of different sizes, facilitates the comprehensive optimization of anode materials in terms of mechanical strength, kinetic performance, and electrochemical stability. Specifically, while ensuring the mechanical strength of the anode material, it is beneficial to form specific microstructures within the anode material. This allows the anode material to better disperse stress when facing the volume expansion of silicon-based materials, avoiding structural damage, improving its electrochemical reaction rate and lithium-ion diffusion capability, and ensuring efficient lithium-ion storage and release.

[0089] In some embodiments, the negative electrode material includes secondary particles and / or primary particles, and a first coating layer present on at least a portion of the surface of the carbon-based material. The first coating layer includes carbon material and is covered with the coating layer, which is intended to enhance the overall electronic conductivity and mechanical stability of the negative electrode material.

[0090] Among them, carbon materials include at least one of amorphous carbon and graphitized carbon. By controlling the specific type of carbon material, it is helpful to further improve the overall conductivity of the negative electrode material, slow down volume expansion and contraction, and protect the structural integrity of the negative electrode material.

[0091] In some embodiments, the carbon-based material includes at least one of artificial graphite, natural graphite, hard carbon, soft carbon, amorphous carbon, activated carbon, mesophase carbon microspheres, carbon nanotubes, carbon nanofibers, and graphene. Preferably, the carbon-based material is at least one of artificial graphite and natural graphite; for example, the carbon-based material includes at least one of petroleum coke-based graphite, pitch coke-based graphite, and needle coke-based graphite.

[0092] In some embodiments, the anode material includes hydrogen and a metal element, including at least one of Zn, Ba, and Ca. The anode material contains not only carbon but also hydrogen and trace amounts of the metal element. Thus, in the carbon-based material, hydrogen can participate in the formation of functional groups, such as hydroxyl (-OH) or carboxyl (-COOH), at graphite edges or defect sites. These functional groups not only improve the surface properties of the anode material, enhancing its hydrophilicity and dispersibility, but also help provide additional active sites during lithium-ion insertion / extraction, thereby improving the lithium storage performance and cycle stability of the anode material. The metal elements Zn, Ba, and Ca can participate in the lattice of the carbon-based material, altering the graphite interlayer spacing and thus affecting the lithium-ion insertion / extraction behavior. Furthermore, the presence of the metal element in the anode material can be used to further modulate the characteristics of the D peak to control lattice defect distortion.

[0093] This application significantly enhances the lithium-ion storage and transport capabilities of anode materials by introducing hydrogen and metal elements, thereby improving the capacity and energy density of secondary batteries. On the one hand, the presence of hydrogen helps improve the surface properties of anode materials, making them more compatible with other components, such as electrolytes and binders, during the preparation of secondary batteries, thus optimizing the overall performance of the secondary batteries. On the other hand, the addition of trace metal elements helps regulate the distribution of lattice defects, enhances the resistance of anode materials to volume expansion, and thus improves the structural stability and cycle life of anode materials.

[0094] In some embodiments, the mass content of hydrogen in the negative electrode material is ≤0.1%, and the mass content of metal elements in the negative electrode material is 1ppm to 50ppm. Specifically, the mass content of hydrogen in the negative electrode material can be 0 to 0.1%, and the mass content of metal elements in the negative electrode material can be within the range of 1ppm, 2ppm, 5ppm, 10ppm, 15ppm, 20ppm, 25ppm, 30ppm, 35ppm, 40ppm, 45ppm, 50ppm, or any combination thereof. Controlling the mass content of metal elements within the above range means that the metal elements exist in the negative electrode material in the form of trace elements, avoiding the negative impact of metal elements on the conductivity of the negative electrode material, and also reducing potential battery safety risks, such as short circuit events that may be caused by metal impurities.

[0095] In some embodiments, the D50 particle size of the negative electrode material is 10 μm to 15 μm, and the D90 particle size is 19 μm to 24 μm. Controlling the particle size distribution of the negative electrode material within these ranges helps to increase its compaction density, thereby improving the energy density of the secondary battery. This also helps to establish a more efficient lithium-ion transport path, shorten the lithium-ion diffusion distance, and accelerate the lithium-ion insertion / extraction process, thus improving the charge / discharge rate and kinetic performance of the secondary battery. Furthermore, controlling the particle size distribution helps to form a uniform stress distribution in the negative electrode material, reducing mechanical damage between particles, enhancing the structural stability of the negative electrode material and its resistance to volume expansion, thereby extending the cycle life of the secondary battery. Specifically, the D50 particle size of the negative electrode material can be a range of 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, or any combination thereof, and the D90 particle size of the negative electrode material can be a range of 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, or any combination thereof.

[0096] In some embodiments, the oil absorption value of the negative electrode material is 45 mL / 100g to 60 mL / 100g. A higher oil absorption value means that the negative electrode material has higher porosity and specific surface area, which is beneficial to lithium-ion insertion / extraction to some extent. However, it also increases the possibility of surface side reactions, leading to a decrease in battery performance, such as reduced cycle stability and energy density. Negative electrode materials with excessively high oil absorption values ​​often require more conductive agents or binders to fill the pores, which may reduce the conductivity and mechanical strength of the negative electrode material, thereby affecting the charge-discharge efficiency and overall structural stability of the secondary battery. By controlling the oil absorption value of the negative electrode material within the above range, it is ensured that the negative electrode material has reasonable porosity and specific surface area, thereby reducing surface side reactions, improving the cycle stability and energy efficiency of the secondary battery, while maintaining good conductivity and mechanical strength of the negative electrode material, reducing the amount of conductive agents and binders used, thereby increasing the proportion of active materials and further improving the energy density of the secondary battery. In addition, it makes the negative electrode material easier to shape during processing, reduces the moisture absorption and agglomeration of the negative electrode material, and improves the consistency and reliability of secondary battery manufacturing. Specifically, the oil absorption value of the negative electrode material can be a range of 45mL / 100g, 48mL / 100g, 50mL / 100g, 55mL / 100g, 58mL / 100g, 60mL / 100g, or any combination thereof.

[0097] In some embodiments, the powder compaction density of the negative electrode material under a pressure of 5T is 1.6 g / cm³. 3 ~2.1g / cm 3Compaction density directly affects the volumetric energy density and overall structural stability of secondary batteries. Controlling the powder compaction density of the anode material within the aforementioned range at 3T pressure helps increase the filling density of the active material in the secondary battery, increasing the effective active material content per unit volume, and thus improving the volumetric energy density. Simultaneously, it helps maintain sufficient lithium-ion diffusion capacity while increasing energy density, ensuring stable electrochemical performance. Furthermore, it helps avoid excessive particle compression, reducing structural damage to the anode material during cycling, thereby extending the cycle life of the secondary battery. Specifically, the powder compaction density of the anode material at 5T pressure can be 1.6 g / cm³. 3 1.7g / cm 3 1.8g / cm 3 1.9g / cm 3 2.0g / cm 3 2.1g / cm 3 or a range consisting of any two of them.

[0098] In some embodiments, the specific surface area of ​​the negative electrode material is 0.8 m². 2 / g~5m 2 / g. Specific surface area refers to the total surface area per unit mass of negative electrode material, usually measured using the BET method. By controlling the specific surface area of ​​the negative electrode material within the above range, sufficient active sites are ensured to facilitate lithium-ion insertion / extraction, while reducing SEI film formation and mitigating the impact of surface side reactions on secondary battery performance, such as improving initial discharge capacity and cycle stability. Secondly, it helps to form more efficient lithium-ion transport pathways, avoiding increased lithium-ion transport resistance due to excessive porosity, thereby improving the charge / discharge efficiency of the secondary battery. Furthermore, it helps to reduce moisture absorption and agglomeration of the negative electrode material during manufacturing, improving the performance of mixing and coating processes. Specifically, the specific surface area of ​​the negative electrode material can be 0.8m². 2 / g, 1m 2 / g, 1.2m 2 / g, 1.4m 2 / g, 1.6m 2 / g、2m 2 / g, 2.5m 2 / g、3m 2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g or a range consisting of any two of them.

[0099] In some embodiments, the orientation degree of the (004) crystal plane of the negative electrode material is 1.6–5. The negative electrode material is characterized using X-ray diffraction, exhibiting diffraction peaks on both the (004) and (110) crystal planes. The orientation degree refers to the ratio of the peak area C004 of the (004) crystal plane to the peak area C110 of the (110) crystal plane. The orientation degree of the (004) crystal plane of the negative electrode material reflects the degree of directionality of the crystal arrangement within the material. Especially in graphite or similar layered carbon-based materials, the orientation of the crystal layers directly affects the electrochemical and mechanical properties of the negative electrode material. By controlling the orientation degree of the negative electrode material within the aforementioned range, the diversity of lithium-ion insertion paths is increased, and stress concentration in specific directions is reduced. This helps improve the stability of the negative electrode material during charge and discharge, avoids structural collapse or fracture during high-current charge and discharge, thereby extending the cycle life of the secondary battery. Simultaneously, it promotes uniform diffusion of lithium ions in multiple directions, accelerates the lithium-ion insertion / extraction rate, and optimizes the kinetic performance of the secondary battery. Secondly, it improves the overall toughness and crack propagation resistance of the negative electrode material. Especially when the negative electrode material is used in conjunction with silicon-based materials, it can better resist the internal pressure caused by volume changes in the silicon-based material during charge and discharge, avoiding graphite layer fracture due to volume expansion of the silicon-based material during charge and discharge, thus preventing a decrease in secondary battery performance. Furthermore, it helps maintain the structural integrity of the negative electrode material during cycling, reducing performance degradation caused by stress concentration, thereby improving the cycle stability and energy density of the secondary battery. Specifically, the (004) crystal plane orientation degree of the negative electrode material can be a range of 1.6, 2, 2.5, 3, 3.5, 4, 4.5, 5, or any combination thereof.

[0100] In some embodiments, the powder conductivity of the negative electrode material at 4 kN is 80 S / cm to 800 S / cm. Controlling the powder conductivity of the negative electrode material within this range at 4 kN helps to accelerate the insertion and extraction of lithium ions into the negative electrode material, improving the charge-discharge speed and kinetic performance of the secondary battery. Secondly, it reduces the accumulation of charge within the negative electrode material, avoiding material degradation caused by localized hot spots, thereby improving the cycle stability and lifespan of the secondary battery. Furthermore, it reduces the interfacial impedance with the electrolyte, improving the overall energy efficiency and power density of the secondary battery. Specifically, the powder conductivity of the negative electrode material at 4 kN can be within the range of 80 S / cm, 100 S / cm, 200 S / cm, 300 S / cm, 400 S / cm, 500 S / cm, 600 S / cm, 700 S / cm, 800 S / cm, or any combination thereof.

[0101] The negative electrode material of this application can be directly applied to secondary batteries, effectively improving the capacity, initial coulombic efficiency, and reducing electrode expansion rate. In some embodiments, when this negative electrode material is fabricated into a negative electrode sheet and applied to a secondary battery, the initial discharge capacity is ≥350mAh / g, the initial coulombic efficiency is ≥92%, the capacity retention rate after 50 cycles is ≥95.3%, and the electrode expansion rate is ≤23.7%.

[0102] This application does not limit the specific preparation process of the negative electrode material, as long as the above parameters are met. In some embodiments, the preparation method of the above-mentioned negative electrode material includes the following steps:

[0103] S1, the first coke raw material is first crushed to obtain the first crushed material; the first crushed material is mixed with the first carbon source and first carbon coating is performed to obtain the first modified coke raw material;

[0104] S2, the second coke raw material is pulverized a second time to obtain a second pulverized material; the second pulverized material is mixed with a metal dopant and subjected to doping treatment to obtain a second modified coke raw material;

[0105] S3, the third coke raw material is crushed for the third time to obtain the third crushed material; the third crushed material is mixed with the second carbon source and coated with the second carbon to obtain the third modified coke raw material;

[0106] S4, the first modified coke raw material, the second modified coke raw material, and the third modified coke raw material are mixed in a solid phase to obtain the first mixture;

[0107] S5, the first mixture is graphitized to obtain graphite particles; the graphite particles are mixed with a third carbon source to obtain a second mixture; the second mixture is heat-treated to obtain a negative electrode material;

[0108] The D50 particle size of the second pulverized material is greater than that of the first pulverized material and the third pulverized material, and the D50 particle size of the first pulverized material is 6μm to 11μm; the D50 particle size of the second pulverized material is 12μm to 18μm; and the D50 particle size of the third pulverized material is 5μm to 8μm.

[0109] Specifically, in step S1, the first pulverized material undergoes a first carbon coating process, causing the first carbon source to form a first carbon coating layer on the surface of the pulverized material, thus obtaining the first modified coke raw material. The first carbon coating effectively buffers the thermal stress generated during subsequent graphitization, effectively controls the lattice defect distortion coefficient of the particles, prevents particle distortion due to excessive thermal stress, and reduces the lattice defect distortion coefficient of the first modified coke raw material. Furthermore, the first carbon coating layer provides an additional physical barrier, increasing surface stability and protecting the internal carbon-based material from external environmental influences such as oxidation and electrolyte corrosion. Simultaneously, the first carbon coating layer helps establish efficient electron conduction pathways, improving the conductivity of the negative electrode material and thereby enhancing the charge and discharge efficiency of the secondary battery.

[0110] In step S2, during the doping process, the metal elements in the metal dopant are incorporated into the lattice defects of the second pulverized material. On the one hand, this helps to adjust the microstructure orientation of the carbon-based material. Due to the interaction between the metal elements and the carbon skeleton, the crack propagation path is disturbed, making the structure formed in the subsequent graphitization process more stable and less prone to crack propagation, thereby increasing the overall mechanical strength and toughness of the anode material. On the other hand, the metal elements can further penetrate into the lattice of the carbon-based material during the subsequent graphitization process. This not only helps to improve the conductivity of the carbon-based material and enhance its lithium-ion insertion / extraction performance, but also further regulates the lattice defect distortion coefficient of the second modified coke raw material, enabling it to provide sufficient buffering capacity when facing the expansion stress of silicon-based materials and maintain the structural integrity of the anode material.

[0111] In step S3, the third pulverized material is coated with a second carbon layer, which promotes the formation of a second carbon coating layer on the surface of the third pulverized material, resulting in the third modified coke raw material. The second carbon coating effectively buffers the thermal stress generated during subsequent graphitization, effectively controls the lattice defect distortion coefficient of small-sized particles, prevents distortion of small-sized particles due to excessive thermal stress, and reduces the lattice defect distortion coefficient of the third modified coke raw material. Furthermore, the second carbon coating layer provides an additional physical barrier, protecting the internal carbon-based material from external environmental influences such as oxidation and electrolyte corrosion. The second carbon coating layer also improves the electrical conductivity of the carbon-based material, facilitating rapid lithium-ion transport and improving the charge-discharge efficiency of the secondary battery. Thus, in subsequent solid-phase mixing, the first and second carbon coating layers ensure optimal physical barrier protection for particles of different size ranges, while simultaneously constructing a more uniform conductive network and optimizing the electrochemical performance of the secondary battery.

[0112] In step S4, by controlling the mixing of particles of different sizes, the uniform distribution of the first, second, and third modified coke raw materials is ensured, promoting the interaction between the particles of different modified coke raw materials, maximizing the positive synergistic effect, and ensuring the balance of lattice defect distortion in the entire material system, thereby optimizing the electrochemical performance and mechanical stability of the anode material. At the same time, the solid-phase mixing process helps to ensure uniform particle dispersion, avoid agglomeration, improve the uniformity and consistency of the material, help to increase the compaction density of the anode material, and reduce internal stress, so that the anode material maintains better structural integrity and performance stability during cycling. In addition, by performing graphitization treatment after solid-phase mixing, the distribution of lattice defects in the material can be further homogenized, ensuring a more uniform conductive network in the material, improving the lithium-ion transport efficiency and the charge-discharge performance of the secondary battery.

[0113] In step S5, the graphitization process not only transforms the carbon skeleton into a graphite structure, improving the electrochemical activity and stability of the anode material, but also further enhances the conductive network of the anode material and improves its conductivity through heat treatment after mixing with the third carbon source.

[0114] The method for preparing the anode material in this application involves different treatments for pulverized materials of different sizes (particle diameters) to control the characteristics of particles of different sizes in the anode material. In particular, it optimizes the lattice defect distortion coefficient of particles of different sizes in the anode material, thereby reducing the lattice defect distortion coefficient (Vt) of particles of different sizes. a V b V c Satisfy: V b ≥V a And V b >V c Or, V b >V a And V b ≥V cThis process enables particles of different sizes to exhibit a synergistic effect in the final anode material. On one hand, it adjusts the microstructure and orientation of the carbon-based material, allowing the prepared anode material to provide sufficient buffering capacity when facing the expansion stress of the silicon-based material, while reducing the possibility of crack propagation and improving the mechanical properties and structural stability of the anode material. The final anode material has optimized defect distribution, particle size distribution, and conductivity, effectively buffering the volume expansion caused by the silicon-based material, reducing SEI layer thickening, and maintaining structural integrity and stability. On the other hand, through the synergistic effect of multi-step carbon coating and doping treatment, a more uniform and efficient conductive network is constructed, significantly improving the conductivity of the anode material and improving the lithium-ion insertion / extraction rate. The final anode material shows significant improvements in both electrochemical performance and mechanical stability, effectively reducing the expansion rate of the secondary battery during charge and discharge, increasing the initial discharge capacity and initial coulombic efficiency, reducing the SEI layer growth rate, and thus improving the overall performance and lifespan of the secondary battery.

[0115] This application does not limit the specific type of coke feedstock. For example, in some embodiments, the first coke feedstock, the second coke feedstock, and the third coke feedstock include at least one of petroleum coke, pitch coke, and needle coke. By controlling the specific type of coke feedstock and combining it with fine modification and graphitization treatment, it is beneficial to prepare anode materials with optimized lattice defect distortion, good electrical conductivity, and structural stability.

[0116] The first, second, and third crushing processes are used to optimize the particle size distribution of the raw materials, providing ideal particle morphology for subsequent modification and graphitization. This helps improve the effectiveness of carbon coating and doping treatments, ensures uniform modification of particles of different sizes, and achieves precise control over lattice defect distortion. In some embodiments, the first, second, and third crushing processes all include: coarse crushing using a jaw crusher followed by further crushing and shaping. The coarse crushing using a jaw crusher can significantly reduce the size of large raw materials, laying the foundation for subsequent fine crushing and shaping. By precisely controlling the particle size distribution of the coke raw materials, it can meet the specific size requirements of the anode material.

[0117] The first pulverized material has a D50 particle size of 6μm to 11μm, for example, a range of 6μm, 7μm, 8μm, 9μm, 10μm, 11μm or any two of these; the second pulverized material has a D50 particle size of 12μm to 18μm, for example, a range of 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm or any two of these; and the third pulverized material has a D50 particle size of 5μm to 8μm, for example, a range of 5μm, 6μm, 7μm, 8μm or any two of these.

[0118] Both the first and second carbon coatings can be performed using chemical vapor deposition (CVD). For example, in step S1, the first pulverized material is placed in a CVD furnace, a first carbon source is introduced at a first coating temperature, and the first carbon coating is performed at a first coating time, promoting a full reaction between the first carbon source and the first pulverized material to form a stable first carbon coating layer. Similarly, in step S3, the third pulverized material is placed in a CVD furnace, a second carbon source is introduced at a second coating temperature, and the second carbon coating is performed at a second coating time, promoting a full reaction between the second carbon source and the third pulverized material to form a stable second carbon coating layer.

[0119] In some embodiments, the first carbon source and the second carbon source each independently include at least one of alkanes, alkenes, and alkynes, such as methane, ethylene, and acetylene. The first coating temperature is 600°C to 800°C, and the first coating time is 60 min to 100 min. The second coating temperature is 600°C to 800°C, and the second coating time is 60 min to 100 min. The mass ratio of the first pulverized material to the first carbon source is 100:(0.3 to 1), and the mass ratio of the second pulverized material to the second carbon source is 100:(0.3 to 0.8).

[0120] In some embodiments, step S2 includes: placing the second pulverized material in a vacuum furnace, introducing a metal dopant at a vacuum level of less than 200 Pa, performing doping treatment at a first doping temperature and a first doping time, and then performing cooling treatment at a first cooling rate to obtain a third modified coke raw material after cooling to room temperature.

[0121] Among these measures, controlling the vacuum level to within 200 Pa creates a low-pressure environment that helps improve the diffusion efficiency of metal dopants and ensures that metal elements are evenly distributed on the particle surface and inside.

[0122] Metal dopants can be in a gaseous state and include at least one metal element selected from Zn, Ba, and Ca. For example, a metal dopant can be ZnS vapor.

[0123] The initial doping temperature is 1300℃~1500℃, the flow rate of the metal dopant is 3L / min~10L / min, and the initial doping time is 0.5h~3h. This selection of temperature range, flow rate, and time helps promote the effective reaction between the metal element and the carbon framework, while avoiding excessive metal element deposition that could lead to material performance degradation. Furthermore, by controlling the flow rate of the metal dopant and the initial doping time, the concentration and distribution of metal elements in the anode material can be controlled, keeping the lattice defect distortion coefficient of large-sized particles within a reasonable range, thereby improving the mechanical stability and electrochemical performance of the anode material.

[0124] The initial cooling rate is 50℃ / min to 100℃ / min. Rapid cooling, combined with a cooling process to room temperature, helps to fix the state of the metal elements within the carbon framework, reducing volatilization losses during post-processing. It also effectively alleviates residual stress caused by uneven thermal stress, prevents the generation of new lattice defects during cooling, and helps to control the lattice defect distortion coefficient, thereby optimizing the performance of the anode material. Furthermore, precise cooling temperature control improves the controllability of the lattice defect distortion coefficient.

[0125] In some embodiments, in step S4, solid-phase mixing can employ a variety of different mixing techniques, such as VC mixing, triple-eccentric mixing, ball milling, and high-speed mixing, to ensure that the raw materials can be fully and uniformly mixed to form a negative electrode material with synergistic effects.

[0126] The mass ratio of the first modified coke raw material to the second modified coke raw material is 1:(1-8), for example, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, or any combination thereof; the mass ratio of the first modified coke raw material to the third modified coke raw material is 1:(1-8), for example, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, or any combination thereof. By controlling the mass ratio between different modified coke raw materials, the lattice defect distortion coefficients of particles of various sizes can be balanced. This helps to improve the overall hardness and toughness of the anode material, enabling it to better buffer the volume expansion of silicon-based materials, reduce the formation of the SEI layer, and thus reduce the electrode expansion rate; in addition, the optimized mass ratio helps to form a more uniform and stable anode material structure, reducing structural damage caused by uneven particle size and lattice defect distribution, thereby improving the structural stability and energy density of the secondary battery.

[0127] In some embodiments, step S5 includes: graphitizing the first mixture at a first graphitization temperature to obtain graphite particles; mixing the graphite particles with a third carbon source at a first mixing temperature and a first mixing time to obtain a second mixture; and heat-treating the second mixture at a first heat treatment temperature and a second heat treatment time, and then naturally cooling it to room temperature to obtain a negative electrode material.

[0128] In some embodiments, the first mixture is directly graphitized, or the first mixture is mixed with natural graphite and then graphitized. The specific choice can be made according to actual needs, and this application does not impose any restrictions here.

[0129] In some embodiments, the third carbon source includes at least one of liquid asphalt, solid asphalt, and resin. The mass ratio of graphite particles to the third carbon source is 1:(0.01 to 0.1), for example, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, or any combination thereof.

[0130] In some embodiments, the first mixing temperature is 200℃ to 400℃, and the first mixing time is 40 min to 80 min. By mixing the third carbon source with graphite particles at the first mixing temperature and the first mixing time, on the one hand, the adhesive properties of the molten third carbon source can be used to bind the fine powder into secondary particles, reducing the specific surface area and increasing the tap density; on the other hand, it can promote the wetting and spreading of the third carbon source on the surface of the graphite particles, which helps to achieve a more complete coating on the particle surface. In addition, the above mixing conditions eliminate the secondary granulation process, reduce costs, simplify the process, and help with product quality control.

[0131] In some embodiments, the first heat treatment temperature is 1000℃~1300℃, and the first heat treatment time is 3h~8h. By controlling the first heat treatment temperature and time, the reaction between the third carbon source and graphite particles is promoted to form a high-quality carbon coating layer, while ensuring the stability of the anode material structure and the appropriate control of lattice defect distortion.

[0132] This application can precisely control the lattice defect distribution, particle size distribution, and lattice defect distortion coefficient of the anode material by controlling the first mixing temperature, the first mixing time, the first heat treatment temperature, and the first heat treatment time, so as to ensure that the performance of the final anode material meets the above requirements.

[0133] A second aspect of this application provides a composite anode material, comprising the anode material provided in the first aspect and a silicon-based material.

[0134] The negative electrode material of this application is particularly suitable for use in combination with silicon-based materials. In this case, the negative electrode material of this application is combined with silicon-based materials to form a negative electrode active material. When this negative electrode active material is applied to the negative electrode sheet, it can not only improve the capacity, initial coulombic efficiency and reduce the electrode expansion rate of the secondary battery, but also better buffer the expansion stress of the silicon-based material and withstand the volume change generated by the silicon-based material. During the cycling process, the negative electrode material can maintain good electrical contact with the silicon-based material, promote the integrity of the overall electrode structure, and the electrode still maintains a good conductive network after cycling, which helps to improve the electrochemical performance of the secondary battery assembled from the composite negative electrode material.

[0135] Specifically, when the negative electrode material of this application is used in combination with silicon-based materials, the negative electrode material of this application, by controlling the lattice defect distortion coefficient of particles of different sizes, can effectively buffer stress when the silicon-based material expands, effectively balancing the hardness and toughness of the negative electrode material and the volume expansion requirements of the silicon-based material, thus achieving better electrochemical performance and cycle stability. Furthermore, the combination of the high specific capacity of the silicon-based material and the good structural stability and conductivity of the negative electrode material significantly improves the overall specific capacity of the negative electrode material; the structural stability of the negative electrode material can effectively suppress the volume expansion of the silicon-based material during charging and discharging, avoiding pulverization and breakage of the electrode material, and improving the cycle performance of the battery.

[0136] In some embodiments, silicon-based materials can be commercially available and include at least one of silicon, silicon-carbon, silicon-oxygen, silicon oxide, doped silicon oxide, and silicon alloys. The silicon includes at least one of amorphous silicon, crystalline silicon, and composites of crystalline and amorphous silicon. For example, amorphous silicon expands isotropically during lithium intercalation, which can reduce pore collapse, suppress rapid capacity decay of the anode material, and improve the lithium intercalation cycle performance of the anode material. The silicon-carbon in the silicon-based material includes at least one of milled silicon-carbon, deposited silicon-carbon, and doped silicon-carbon. By mixing silicon with carbon, the structural stability and good conductivity of carbon materials are utilized to mitigate the large volume expansion of silicon, improving the cycle stability and electrochemical performance of the composite anode material. Silicon-based materials include those with the general chemical formula SiO. x Silicon oxides with a value of 0 < x ≤ 2 exhibit smaller volume changes and higher cycle stability during charge and discharge, and their lithiation reaction can provide stable capacity output. Doped silicon oxides in silicon-based materials contain doping elements, including at least one of Ca, Mg, Sn, Li, P, Al, and N, for example, forming silicon-based materials containing lithium silicate or magnesium silicate. Introducing doping elements into silicon oxide materials not only modulates the electrochemical performance of the material but also further improves its structural stability and cycle life. Silicon alloys can be lithium silicon alloys, magnesium silicon alloys, etc. In some cases, silicon alloys include elemental silicon particles and alloys. Alloys formed with silicon and other metals not only reduce the volume expansion of silicon but also improve the electronic and lithium-ion conductivity of the material.

[0137] In some embodiments, at least a portion of the surface of the silicon-based material is provided with a second coating layer. The thickness of the second coating layer is 1 nm to 400 nm, for example, a range of 1 nm, 10 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, or any combination thereof. This avoids the second coating layer being too thin to effectively protect the silicon-based material, while also avoiding it being too thick to hinder the rapid diffusion of lithium ions and affect the charge and discharge rate of the battery. Specifically, the second coating layer includes at least one of carbon, nitride, metal oxide, metal fluoride, metal oxyfluoride, and polymer. These materials, when used as a second coating layer, can not only effectively mitigate the volume change of silicon during charge and discharge, but also form a stable SEI layer, reducing side reactions in the electrolyte and enhancing the conductivity of the silicon-based material.

[0138] In some embodiments, the specific surface area of ​​the composite negative electrode material is <8.0 m². 2 / g, by controlling the specific surface area of ​​the composite negative electrode material to be <8.0m². 2 / g helps to further improve the cycle stability of secondary batteries, reduce side reactions, and enhance conductivity and lithium-ion diffusion efficiency.

[0139] In some embodiments, the mass percentage of moisture in the composite anode material is <0.5%. By strictly controlling the mass percentage of moisture in the composite anode material to <0.5%, it helps to ensure the safety performance of the composite anode material.

[0140] In some embodiments, the D10 particle size of the composite negative electrode material is 1μm to 10μm, and the D90 particle size is 15μm to 40μm. By controlling the particle size of the composite negative electrode material to meet the above requirements, it is helpful to reduce the volume expansion during the charging and discharging process, reduce the cracking of the composite negative electrode material, and improve the cycle life.

[0141] In some embodiments, the tap density of the composite negative electrode material is 0.7 g / cm³. 3 ~3.0g / cm 3 By controlling the tap density of the composite anode material to meet the above-mentioned range requirements, it is helpful to enable the composite anode material to be more tightly packed, achieve effective filling of internal particles, and store more lithium ions per unit volume, thereby improving the energy density of the secondary battery. At the same time, it reduces the volume change of the electrode material during charging and discharging, maintains the stability of the electrode structure, and extends the cycle life of the secondary battery.

[0142] In some embodiments, the powder compaction density of the composite negative electrode material under 5T pressure is 0.8 g / cm³. 3 ~5.0g / cm 3This ensures that the composite anode material can fill more tightly under pressure, improving its density and helping to form a denser conductive network, thus improving the conductivity of the composite anode material.

[0143] In some embodiments, the mass ratio of the anode material to the silicon-based material in the composite anode material is (3-97):(3-97), for example, 3:97, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:40, 70:30, 80:20, 90:10, 97:3 or any combination thereof.

[0144] The negative electrode material of this application can be directly used in secondary batteries, or it can be used in combination with silicon-based materials in negative electrode sheets, which can effectively improve the capacity, initial coulombic efficiency, and reduce the electrode expansion rate of secondary batteries. When the composite negative electrode material formed by combining the negative electrode material of this application with silicon-based materials is used as a negative electrode sheet in secondary batteries, it can achieve an initial discharge capacity ≥365mAh / g, an initial coulombic efficiency ≥90%, an electrode conductivity ≥0.8S / cm after 50 cycles, an electrode expansion rate ≤84%, and a capacity retention rate ≥85%.

[0145] In some embodiments, the preparation method of the composite anode material includes the following steps: sequentially adding the anode material and the silicon-based material into a mixer in a certain proportion, and after mixing, obtaining the composite anode material. The mixer can be a conventional mixer in the art, such as a VC mixer, etc., and the mixing speed is 300 rpm to 800 rpm, and the mixing time is 20 min to 60 min, to ensure that the anode material and the silicon-based material are fully and uniformly dispersed and combined.

[0146] A third aspect of this application provides a negative electrode sheet, which includes the negative electrode material provided in the first aspect or the composite negative electrode material provided in the second aspect.

[0147] The negative electrode sheet of this application includes a negative electrode current collector and a negative electrode active layer formed of a negative electrode material disposed on the surface of the negative electrode current collector. Because it includes the aforementioned high-performance negative electrode material or composite negative electrode material, applying this negative electrode sheet to a secondary battery can reduce the expansion rate and help improve capacity and initial coulombic efficiency.

[0148] In the specific preparation of the negative electrode sheet, the negative electrode material or composite negative electrode material can be dispersed with a conductive agent and a binder in an appropriate amount of solvent, and thoroughly stirred to form a uniform negative electrode slurry. The negative electrode slurry is then uniformly coated onto the negative electrode current collector, and after drying, rolling, and slitting, the negative electrode sheet is obtained. In one specific embodiment, the negative electrode active layer comprises, by mass percentage, 70%–99% negative electrode material, 0.5%–15% conductive agent, and 0.5%–15% binder.

[0149] The conductive agent may be selected from at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and graphene; the binder may be selected from at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyvinyl alcohol, and sodium polyacrylate.

[0150] A third aspect of this application provides a secondary battery comprising the negative electrode provided in the second aspect above.

[0151] Due to the inclusion of the aforementioned high-performance negative electrode, this secondary battery exhibits excellent capacity, initial coulombic efficiency, and electrode expansion rate.

[0152] The secondary battery of this application also includes a positive electrode, an electrolyte, and a separator.

[0153] Specifically, the secondary battery includes a casing, an electrode assembly, and an electrolyte. Both the electrode assembly and the electrolyte are located inside the casing.

[0154] The outer casing can be a packaging bag encapsulated with a sealing film (such as aluminum-plastic film), for example, a pouch battery. In other embodiments, it can also be a steel-cased battery, an aluminum-cased battery, etc.

[0155] Referring to Figures 2 and 3, the electrode assembly 100 includes a positive electrode 101, a negative electrode 102, and a separator 103, with the separator 103 disposed between the positive electrode 101 and the negative electrode 102. During charging, as shown in Figure 2, active ions (such as lithium ions) are extracted from the crystal lattice of the positive electrode material (such as a lithium-ion intercalated compound) of the positive electrode 101, pass through the separator 103 via the electrolyte, reach the negative electrode 102, and are inserted into the crystal lattice of the negative electrode material. During discharging, as shown in Figure 3, active ions (such as lithium ions) are extracted from the crystal lattice of the negative electrode material of the negative electrode 102, pass through the separator 103 via the electrolyte, reach the positive electrode 101, and are inserted into the crystal lattice of the positive electrode material (such as a lithium-ion intercalated compound). Electrons are generated and travel from the negative electrode 102 to the positive electrode 101 via an external circuit. The reverse movement of these electrons forms an electric current, which can be used by electrical appliances.

[0156] In some embodiments, the electrode assembly 100 may be a stacked structure, which is formed by alternatingly stacking a positive electrode 101, a separator 103, and a negative electrode 102. In other embodiments, the electrode assembly 100 may also be a wound structure, which is formed by sequentially stacking and then winding the positive electrode 101, the separator 103, and the negative electrode 102.

[0157] The positive electrode 101 includes a positive current collector and a positive electrode material active layer disposed on at least one surface of the positive current collector. The positive current collector can be aluminum foil or nickel foil, or any composite current collector disclosed in the prior art, such as, but not limited to, current collectors formed by combining the aforementioned conductive foil and polymer substrate. The positive electrode material active layer includes a positive electrode active material, which includes a compound that reversibly inserts and extracts lithium ions (i.e., a lithiation intercalation compound). In some embodiments, the positive electrode active material may include a lithium transition metal composite oxide. This lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese, and nickel. In some embodiments, the positive electrode active material may include, but is not limited to, lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary materials (NCM), lithium manganese oxide (LiMn2O4), and lithium nickel manganese oxide (LiNi). 0.5 Mn 1.5 At least one of lithium iron phosphate (LiFePO4) or lithium iron phosphate (LiFePO4).

[0158] The positive electrode material active layer also includes an adhesive for bonding the positive electrode active material particles to facilitate the formation of the film layer, and also to improve the bonding force between the positive electrode material active layer and the positive electrode current collector. In some embodiments, the adhesive may include, but is not limited to, at least one of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon.

[0159] The positive electrode material active layer may further include a conductive material, which includes, but is not limited to, carbon-based materials, metal-based materials, conductive polymers, or any combination thereof. In some embodiments, carbon-based materials may include, but are not limited to, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, metal-based materials may include, but are not limited to, metal powders or metal fibers, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.

[0160] The separator 103 includes a membrane layer with a porous structure, and its material includes, but is not limited to, at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, or aramid. For example, the separator 103 may be a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane, etc.

[0161] The electrolyte serves to conduct ions between the positive electrode 101 and the negative electrode 102. The electrolyte can be in one or more states, including gel, solid, and liquid. In some embodiments, the electrolyte is a liquid electrolyte solution. The liquid electrolyte solution serves to conduct active ions between the positive electrode 101 and the negative electrode 102. In some embodiments, the liquid electrolyte solution includes a lithium salt and an organic solvent. The lithium salt may be selected from, but is not limited to, one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetraphenylborate (LiB(C6H5)4), lithium methanesulfonate (LiCH3SO3), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2), lithium tri(trifluoromethanesulfonyl)methyllithium (LiC(SO2CF3)3), lithium dioxolaneborate (LiBOB), and lithium difluorophosphate (LiPO2F2). For example, LiPF6 is selected as the lithium salt because it provides high ionic conductivity and improves cycling characteristics. The organic solvent may be a carbonate compound, a carboxylic acid ester compound, an ether compound, a nitrile compound, other organic solvents, or combinations thereof. Examples of carbonate compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, or combinations thereof.

[0162] In the preparation of secondary batteries, positive electrode sheets, separators and negative electrode sheets are wound or stacked to obtain battery cells. The battery cells are then encapsulated in pre-stamped aluminum-plastic films. After the encapsulated secondary batteries are dried, electrolyte is injected into the dried secondary batteries. The secondary batteries are then placed, formed and resealed to complete the preparation of the secondary batteries.

[0163] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0164] Example 1

[0165] The preparation method of the negative electrode material in this embodiment includes the following steps:

[0166] S1, the first petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the first crushed material with a D50 particle size of 8.2μm; 1kg of the first crushed material is placed in a CVD furnace, heated to 700℃, and acetylene is introduced at an inlet flow rate of 2L / min. After reacting for 60min, it is naturally cooled to room temperature to obtain the first modified coke raw material;

[0167] S2, the second petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a second crushed material with a D50 particle size of 15.2μm; 5kg of the second crushed material is placed in a vacuum furnace, the vacuum degree is set to 50Pa, the temperature is raised to 1300℃, ZnS steam is introduced and reacted for 40min, and then the temperature is lowered to room temperature at a rate of 80℃ / min to obtain the second modified coke raw material; wherein, the ZnS steam flow rate is 6L / min;

[0168] S3, the needle coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a third crushed material with a D50 particle size of 6.5μm; 1kg of the third crushed material is placed in a CVD furnace, heated to 700℃, and acetylene is introduced at a flow rate of 1.5L / min. The reaction is carried out for 80min and then naturally cooled to room temperature to obtain the third modified coke raw material.

[0169] S4, the first modified coke raw material, the second modified coke raw material, and the third modified coke raw material are put into the VC mixing equipment in a mass ratio of 1:7:2 and mixed at 600 rpm for 60 min to obtain the first mixture;

[0170] S5, the first mixture was graphitized at 3000℃ for 8 days to obtain graphite particles; the graphite particles and phenolic resin were mixed at a mass ratio of 1:0.03 for 40 minutes at a mixing temperature of 280℃ to obtain the second mixture; the second mixture was placed in a box furnace and heat-treated at 1200℃ for 4 hours, and then naturally cooled to room temperature to obtain the negative electrode material. Figure 1 is a SEM image of the negative electrode material in Example 1.

[0171] Example 2

[0172] The difference from Example 1 is that in S2, ZnS vapor is replaced with Ba vapor formed from barium metal particles.

[0173] Example 3

[0174] The difference from Example 1 is that in S2, the flow rate of ZnS steam is 8 L / min.

[0175] Example 4

[0176] The difference from Example 1 is that in S3, acetylene is introduced and reacted for 90 minutes.

[0177] Example 5

[0178] The difference from Example 3 is that in S3, acetylene is introduced and reacted for 100 minutes.

[0179] Example 6

[0180] The difference from Example 1 is that in S2, ZnS steam is introduced and reacted for 60 minutes; in S3, the D50 particle size of the third pulverized material is 5.5 μm.

[0181] Example 7

[0182] The difference from Example 1 is that in S2, ZnS vapor is replaced with Ca vapor formed from CaCO3.

[0183] Example 8

[0184] The difference from Example 3 is that in S3, acetylene is introduced and reacted for 40 minutes.

[0185] Example 9

[0186] The difference from Example 1 is that in S2, the flow rate of ZnS vapor is 3 L / min.

[0187] Example 10

[0188] The difference from Example 1 is that in S1, acetylene is introduced and reacted for 90 min; in S2, the flow rate of ZnS vapor is 3 L / min and the reaction is carried out for 20 min; and in S3, acetylene is introduced and reacted for 60 min.

[0189] Example 11

[0190] The difference from Example 6 is that in S2, the reaction with ZnS vapor was introduced for 30 minutes; and in S3, the reaction with acetylene was introduced for 60 minutes.

[0191] Example 12

[0192] The difference from Example 1 is that in S2, the flow rate of ZnS vapor is 10 L / min and the reaction time is 100 min; in S3, acetylene is introduced and the reaction time is 20 min.

[0193] Example 13

[0194] The difference from Example 12 is that in S1, acetylene is introduced and reacted for 40 minutes.

[0195] Example 14

[0196] The difference from Example 9 is that in S2, ZnS steam is introduced and reacted for 20 minutes.

[0197] Example 15

[0198] The difference from Example 12 is that in S3, acetylene is introduced and reacted for 80 minutes.

[0199] Example 16

[0200] The difference from Example 10 is that in S4, the mass ratio of the first modified coke raw material, the second modified coke raw material, and the third modified coke raw material is 2:6:2.

[0201] Example 17

[0202] The difference from Example 12 is that in S1, acetylene is introduced and reacted for 90 minutes.

[0203] Example 18

[0204] The difference from Example 11 is that in S2, the flow rate of ZnS vapor is 4 L / min.

[0205] Example 19

[0206] The difference from Example 17 is that in S4, the mass ratio of the first modified coke raw material, the second modified coke raw material, and the third modified coke raw material is 2:6:2.

[0207] Example 20

[0208] The difference from Example 17 is that in S4, the mass ratio of the first modified coke raw material, the second modified coke raw material, and the third modified coke raw material is 0.5:7.5:2.

[0209] Example 21

[0210] 850g of the negative electrode material prepared in Example 1 and 150g of silicon-carbon material (from BTR New Materials Group Co., Ltd., commercially available model BDS-L) were weighed and added sequentially into a 2.5L VC mixer. After mixing at 500rpm for 40min, the mixture was removed to obtain the composite negative electrode material of this example. Its specific capacity, initial coulombic efficiency, specific surface area, particle size, electrode conductivity, post-cycle electrode expansion rate, and capacity retention were tested. The results are shown in Table 5.

[0211] Example 22

[0212] Compared with Example 21, the silicon-based material was changed to ordinary silicon oxide (from BTR New Materials Group Co., Ltd. commercially available model BSO-1), while other steps remained unchanged.

[0213] Example 23

[0214] Compared with Example 21, the silicon-based material was changed to lithium-doped silicon oxide (from BTR New Materials Group Co., Ltd. commercially available model BSO-L-1), while other steps remained unchanged.

[0215] Example 24

[0216] Compared to Example 21, the silicon-based material was changed to magnesium-doped silicon oxide (from BTR New Materials Group Co., Ltd., commercially available model BSO-2), while other steps remained unchanged.

[0217] Example 25

[0218] Compared to Example 21, the silicon-based material was changed to nano-silicon (from BTR New Materials Group Co., Ltd., commercially available model BDS-S), while other steps remained unchanged.

[0219] Comparative Example 1

[0220] The preparation method of the comparative negative electrode material includes the following steps: S1, the first petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the first crushed material with a D50 particle size of 8.2μm;

[0221] S2, the second petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a second crushed material with a D50 particle size of 15.2μm; 5kg of the second crushed material is placed in a vacuum furnace, the vacuum degree is set to 50Pa, the temperature is raised to 1300℃, ZnS steam is introduced and reacted for 40min, and then the temperature is lowered to room temperature at a rate of 80℃ / min to obtain the second modified coke raw material; wherein, the ZnS steam flow rate is 6L / min;

[0222] S3, the needle coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the third crushed material with a D50 particle size of 6.5μm;

[0223] S4, the modified first pulverized material, the second modified coke raw material, and the third pulverized material are put into the VC mixing equipment at a mass ratio of 1:7:2 and mixed at 600 rpm for 60 min to obtain the first mixture;

[0224] S5. The first mixture is graphitized at 3000℃ for 8 days to obtain graphite particles; the graphite particles and phenolic resin are mixed at a mass ratio of 1:0.03 for 40 minutes at a mixing temperature of 280℃ to obtain the second mixture; the second mixture is placed in a box furnace and heat-treated at 1200℃ for 4 hours, and then naturally cooled to room temperature to obtain the negative electrode material.

[0225] Comparative Example 2

[0226] The preparation method of the comparative negative electrode material includes the following steps: S1, the first petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the first crushed material with a D50 particle size of 8.2μm;

[0227] S2, the second petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a second crushed material with a D50 particle size of 15.2μm;

[0228] S3. The needle coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a third crushed material with a D50 particle size of 6.5μm. 1kg of the third crushed material is placed in a CVD furnace, heated to 700℃, and then acetylene is introduced at a rate of 1.5L / min. The reaction is carried out for 80min and then naturally cooled to room temperature to obtain the third modified coke raw material.

[0229] S4, the modified first pulverized material, the second pulverized material, and the third modified coke raw material are put into the VC mixing equipment at a mass ratio of 1:7:2 and mixed at 600 rpm for 60 min to obtain the first mixture;

[0230] S5. The first mixture is graphitized at 3000℃ for 8 days to obtain graphite particles; the graphite particles and phenolic resin are mixed at a mass ratio of 1:0.03 for 40 minutes at a mixing temperature of 280℃ to obtain the second mixture; the second mixture is placed in a box furnace and heat-treated at 1200℃ for 4 hours, and then naturally cooled to room temperature to obtain the negative electrode material.

[0231] Comparative Example 3

[0232] The preparation method of the comparative negative electrode material includes the following steps: S1, the first petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the first crushed material with a D50 particle size of 8.2μm; 1kg of the first crushed material is placed in a CVD furnace, heated to 700℃ and then acetylene is introduced at a rate of 2L / min. After reacting for 60min, it is naturally cooled to room temperature to obtain the first modified coke raw material;

[0233] S2, the second petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a second crushed material with a D50 particle size of 15.2μm; 5kg of the second crushed material is placed in a vacuum furnace, the vacuum degree is set to 50Pa, the temperature is raised to 1300℃, ZnS steam is introduced and reacted for 40min, and then the temperature is lowered to room temperature at a rate of 80℃ / min to obtain the second modified coke raw material; wherein, the ZnS steam flow rate is 6L / min;

[0234] S3, the needle coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the third crushed material with a D50 particle size of 6.5μm;

[0235] S4, the first modified coke raw material, the second modified coke raw material, and the third pulverized material are put into the VC mixing equipment in a mass ratio of 1:7:2 and mixed at 600 rpm for 60 min to obtain the first mixture;

[0236] S5. The first mixture is graphitized at 3000℃ for 8 days to obtain graphite particles; the graphite particles and phenolic resin are mixed at a mass ratio of 1:0.03 for 40 minutes at a mixing temperature of 280℃ to obtain the second mixture; the second mixture is placed in a box furnace and heat-treated at 1200℃ for 4 hours, and then naturally cooled to room temperature to obtain the negative electrode material.

[0237] Comparative Example 4

[0238] The preparation method of the comparative negative electrode material includes the following steps: S1, the first petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain the first crushed material with a D50 particle size of 8.2μm;

[0239] S2, the second petroleum coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a second crushed material with a D50 particle size of 15.2μm; 5kg of the second crushed material is placed in a vacuum furnace, the vacuum degree is set to 50Pa, the temperature is raised to 1300℃, ZnS steam is introduced and reacted for 40min, and then the temperature is lowered to room temperature at a rate of 80℃ / min to obtain the second modified coke raw material; wherein, the ZnS steam flow rate is 6L / min;

[0240] S3. The needle coke raw material is crushed by a jaw crusher and then crushed and shaped by a crushing and shaping equipment to obtain a third crushed material with a D50 particle size of 6.5μm. 1kg of the third crushed material is placed in a CVD furnace, heated to 700℃, and then acetylene is introduced at a rate of 1.5L / min. The reaction is carried out for 80min and then naturally cooled to room temperature to obtain the third modified coke raw material.

[0241] S4, the first pulverized material, the second modified coke raw material, and the third modified coke raw material are put into the VC mixing equipment in a mass ratio of 1:7:2 and mixed at 600 rpm for 60 min to obtain the first mixture;

[0242] S5. The first mixture is graphitized at 3000℃ for 8 days to obtain graphite particles; the graphite particles and phenolic resin are mixed at a mass ratio of 1:0.03 for 40 minutes at a mixing temperature of 280℃ to obtain the second mixture; the second mixture is placed in a box furnace and heat-treated at 1200℃ for 4 hours, and then naturally cooled to room temperature to obtain the negative electrode material.

[0243] Comparative Example 5

[0244] Compared with Example 21, the negative electrode material was adjusted to the negative electrode material prepared in Comparative Example 1, while other steps remained unchanged, to obtain the composite negative electrode material of this comparative example.

[0245] Comparative Example 6

[0246] Compared with Comparative Example 5, the silicon-based material was changed to ordinary silicon oxide material (from BTR New Materials Group Co., Ltd. commercially available model BSO-1), while other steps remained unchanged, to obtain the composite anode material of this comparative example.

[0247] Test methods

[0248] Sample preparation: Take 1000g of negative electrode material and manually sieve it using a 600-mesh sieve (standard sieve, sourced from GreenRuo, made of 304 stainless steel). Particles that fail to pass through the sieve are the first sieve material. Use a 1000-mesh sieve (standard sieve sample, meeting national standard GB / T 6003-2017, made of 304 stainless steel) to sieve the particles that pass through the 600-mesh sieve again. Particles that fail to pass through the sieve are the second sieve material, and particles that pass through the 1000-mesh sieve are the third sieve material. The first sieve material, second sieve material, third sieve material, and negative electrode material are the sample to be tested. Special note: When passing through a 1000-mesh sieve, liquid phase sieving is used. The specific operation is as follows: Dissolve the particles that pass through a 600-mesh sieve in 2000 mL of anhydrous ethanol, stir at 80 rpm for 10 min to obtain a suspension, and slowly pour the suspension into a 1000-mesh sieve. Particles that fail to pass through the 1000-mesh sieve are dried at 60℃ for 12 h to become the second sieve material. Particles that pass through the 1000-mesh sieve are filtered and dried (at 60℃ for 12 h) to become the third sieve material.

[0249] 1. Raman spectroscopy test

[0250] The Raman spectra of the anode material were measured using a Renishaw In Via confocal micro-Raman spectrometer (UK). The test parameters were: laser wavelength 532 nm, grating band range 100 cm⁻¹. -1 ~3000cm -1 The power attenuation was 1%, the number of cycles was 2, a ×50L objective lens was selected, and the test method was "Map image acquisition".

[0251] Take the sample to be tested and distribute it evenly on a glass slide using a spatula, ensuring the sample surface is flat and free of obvious agglomeration. Place the glass slide with the sample on the stage of the In Via microconfocal Raman spectrometer and execute the "Map image acquisition" test procedure. The raw data is first preprocessed by the instrument software, including removing cosmic ray background noise, subtracting the baseline, marking the Raman peak positions, fixing the peak positions of secondary peaks, and performing curve fitting. Then, the peak intensities of each peak are obtained, and the Raman peak intensities at each test point are statistically analyzed. If the peak intensity at a certain band exceeds 100, it is determined that there is a significant characteristic peak in this band. When testing the D and G peaks, the peak position and peak intensity are determined by the highest peak within the corresponding peak range.

[0252] Determination of the peak position of the D peak in the negative electrode material: 1) Select 15 points on the test sample of the negative electrode material and obtain 15 Raman spectra corresponding to these 15 points through Raman spectroscopy analysis; 2) Each spectrum corresponds to the peak position of a D peak. Measure and record the peak positions of the D peaks in these 15 Raman spectra; add the peak positions of the D peaks in these 15 Raman spectra to obtain the sum; finally, divide the sum by 15 to obtain the peak position of the D peak of the negative electrode material. The peak position of the D peak in the negative electrode material was determined to be at 1351 cm⁻¹. -1 ~1353cm -1 Within the range; 3) Similarly, each spectrum corresponds to a D / G half-peak width ratio value. Measure and record the half-peak width ratio values ​​of the D peak and G peak in these 15 Raman spectra; add the half-peak width ratio values ​​of the D peak and G peak in these 15 Raman spectra to obtain the sum; finally, divide the sum by 15 to obtain the average value of the D / G half-peak width ratio of the negative electrode material.

[0253] Determination of the average D / G half-peak width ratio of the first, second, and third sieve materials: Taking the first sieve material as an example, 1) 100 points were selected from the test sample of the first sieve material, and 100 Raman spectra corresponding to these 100 points were obtained through Raman spectroscopy analysis; 2) Each spectrum corresponds to a D / G half-peak width ratio value, and the half-peak width ratio values ​​of the D peak and G peak in these 100 Raman spectra were measured and recorded; the half-peak width ratio values ​​of the D peak and G peak in these 100 Raman spectra were then calculated. Add the ratios together to get the total, and finally divide the total by 100. That is, calculate the average value of the D / G half-peak width ratio of the first sieve material using Equation I-1; 3) Similarly, each spectrum corresponds to the peak position of a D peak. Measure and record the peak positions of the D peaks in these 100 Raman spectra; add the peak positions of the D peaks in these 100 Raman spectra together to get the total; finally divide the total by 100. That is, calculate the peak position of the D peak of the first sieve material using Equation I-2.

[0254] Similarly, the average value of the D / G half-peak width ratio of the second sieve material is calculated using Equation II-1, and the peak position of the D peak of the second sieve material is calculated using Equation II-2; the average value of the D / G half-peak width ratio of the third sieve material is calculated using Equation III-1, and the peak position of the D peak of the third sieve material is calculated using Equation III-2.

[0255] The lattice defect distortion coefficient V of the first sieve material is calculated according to Equations I, II, and III. a The lattice defect distortion coefficient V of the second sieve material b The lattice defect distortion coefficient V of the third sieve material c :

[0256] Where n = 100, 1 ≤ i ≤ n, and i and n are both positive integers; This represents the average D / G half-peak width ratio of the first sieve material; This represents the average D / G half-peak width ratio of the second sieve material; ΔF is the average D / G half-peak width ratio of the third sieve material; W1 is the average D / G half-peak width ratio of the negative electrode material; ΔF Da ΔF is the difference in peak position between the D peak of the first sieve material and the negative electrode material; Db ΔF is the difference in peak position between the D peak of the second sieve material and the negative electrode material. Dc This is the difference in the peak position of the D peak between the third sieve material and the negative electrode material; The D / G half-width ratio in the i-th Raman spectrum of the first sieve material; The full width at half maximum (FWHM) ratio of the D peak to the G peak in the i-th Raman spectrum of the second sieve material; F represents the D / G half-width ratio in the i-th Raman spectrum of the third sieve material. Dai F represents the peak position of peak D in the i-th Raman spectrum of the first sieved material; Dbi The peak position of peak D in the i-th Raman spectrum of the second sieve material; F Dci The peak position of peak D in the i-th Raman spectrum of the third sieve material; F D1 The peak position of the D peak in the Raman spectrum of the negative electrode material is shown.

[0257] 2. Particle size test

[0258] The test was conducted using a Malvern 3000 Particle Size Analyzer (from Malvern Panalytical Ltd.): 1) Instrument parameter settings: stirring speed 2500 r / min; ultrasonic power 50%; continuous ultrasonic mode, continuous sonication from the start of sample addition; refractive index 2.42°; absorptivity 1; 2) Sample preparation: place the sample to be tested in a 50 mL beaker, add 1-2 mL of anhydrous ethanol, stir with a glass rod to wet the sample, then add 2-5 mL of pure water to the sample, stir clockwise with a glass rod, then add pure water to the 20-30 mL mark on the beaker, stir until the sample is dispersed, and then perform external ultrasonication on the sample at a frequency of 53 kHz for 1 min; 3) Sample testing: after the sample is stirred evenly, quickly pour it into the test beaker, control the shading degree at 5%-15%, stabilize for 5-6 seconds, and then start the test. D10 represents the particle size corresponding to a cumulative particle size volume distribution percentage of 10%, D50 represents the particle size corresponding to a cumulative particle size volume distribution percentage of 50%, and D90 represents the particle size corresponding to a cumulative particle size volume distribution percentage of 90%.

[0259] 3. Metal element content test

[0260] The metal element content was tested using an ICP spectrometer (Agilent 5800VDVICP-OES). The specific testing method is as follows: 0.100g of the negative electrode material was placed in a clean platinum crucible and then calcined in a muffle furnace under air atmosphere at 750℃ for 4 hours. After cooling, the cooled calcined residue was fully reacted with a mixture of 4mL HNO3 and 6mL HF. The platinum crucible containing the acid and decomposition products was then heated on a 350℃ hot plate until the hydrofluoric acid evaporated and no more white smoke was emitted. 6mL of concentrated HCl was then added, and the mixture was heated until the residue was completely dissolved, forming a transparent solution. After cooling to room temperature, the solution was diluted to 100mL in a plastic volumetric flask to obtain the mother liquor for testing. Finally, the metal element content in the mother liquor was tested using an ICP spectrometer.

[0261] 4. Specific surface area test

[0262] The surface area and pore size analyzer was a TriStar 3020 from the USA, and the gas adsorption BET method was used for testing. A specific surface area tube, after being dried at high temperature, was weighed (M1). A certain amount of negative electrode material sample (1 / 2 to 2 / 3 of the tube's volume) was then added and weighed (M2). The mass of the negative electrode material sample is M2-M1. The tube containing the sample was placed in the degassing station of the TriStar 3020 analyzer, the temperature was set to 300℃ for 1 hour, and the sample was purged with nitrogen (N). Afterward, the sample was cooled to room temperature and then placed in the test station of the analyzer. The sample mass M2-M1 was entered, and the gas adsorption BET test was performed. The specific surface area was calculated by measuring the amount of nitrogen adsorbed under different relative pressures. The sampling range was 0.05 g / cm³. 3 ~0.30g / cm 3 Every 0.05g / cm 3 Collect a single data point to obtain a detailed adsorption isotherm.

[0263] 5. Powder conductivity test

[0264] The volume resistivity of the negative electrode material was determined using the four-probe method. The testing equipment was from Mitsubishi Chemical, Japan, model MCP-PD51, and is a powder conductivity meter. Test parameters: the initial resistance order of magnitude could be selected as 10. -3 The voltage limit can be selected as 10V. The sample mass is compressed to a thickness of 3-5mm under a pressure of 20KN, and then held for 3 seconds at five pressure points: 4KN, 8KN, 12KN, 16KN, and 20KN, and the conductivity is measured. The electrode radius is set to 0.7mm, and the sample radius is set to 10mm.

[0265] 6. Compacted density

[0266] The powder compaction density was tested according to the method specified in GB / T 24533. A Sansi Zongheng UTM7305 testing instrument was used. The diameter of the test mold was 12.83 mm, and the base area was 1.292 cm². 2 The mass of the test sample was controlled within 1g ± 0.005g, the pressurization and holding time was set to 30s, the depressurization and holding time was set to 10s, and the applied pressure was 5T (tons).

[0267] 7. Tapped density

[0268] Referring to GB / T 5162-2006 / ISO 3953:1993 "Determination of tap density of metal powders", the tap density was tested using a Canta DAT-4-220 tap density analyzer manufactured by Anton Paar (Shanghai) Trading Co., Ltd. The tap density T is the value after 1000 vibrations. The feed weight was 60g, and the unit is g / cm³. 3 .

[0269] 8. Oil absorption value

[0270] Using an oil absorption value tester (ASAHI SOUKEN, S-500, Japan), a powder sample was placed in the mixing chamber, and dibutyl phthalate (DBP) was added as oil at a constant rate while simultaneously stirring with a rotating blade at 630 r / min. The oil absorption value (mL / 100g) of the sample was calculated by measuring the amount of oil added when the torque-viscosity change was measured to the endpoint of 70% of the maximum torque obtained from the torque curve generated by the viscosity characteristic change.

[0271] 9. Orientation

[0272] An X'pert PRO X-ray diffractometer from Panaco (Netherlands) was used, and the method in GB / T 24533-2019 "Graphite Anode Materials for Lithium-ion Batteries" was followed. Silicon was used as an internal standard, and 30% was added to the graphite. The sample and silicon powder in the mortar were ground back and forth with a pestle to make them evenly mixed. The grinding time was 3 minutes. After grinding, the sample was scraped with a glass slide and poured into the groove of the glass sample holder. It was then pressed and smoothed with a glass slide (care should be taken not to press too hard to avoid stress orientation of the sample). XRD was then tested with a tube voltage of 40 kV, a tube current of 40 mA, a scan rate of 0.138213° / s, and a step size of 0.0131303° in the range of 10°-35°. The ratio of the peak area C004 of the (004) crystal plane to the peak area C110 of the (110) crystal plane of the anode material particles was determined by X-ray diffraction pattern.

[0273] 10. Moisture

[0274] Moisture content was determined according to the Karl Fischer method. The test was conducted using a Karl Fischer coulometric moisture analyzer with a C30S-Inmotion KF heating furnace autosampler (source: Mettler-Toledo International Inc.).

[0275] 1) Sample dosage: Place a dry, clean sample vial on the analytical balance and zero it. Then, accurately add a certain mass of negative electrode material sample to the vial, accurate to 0.0001g. Weighing rules: If the sample moisture content is <0.10%, weigh 0.3-1.0g of sample; if the sample moisture content is ≥0.10%, weigh 0.1-0.5g of sample. 2) Sample preparation: After weighing the sample vial, remove it from the balance, cover it with a threaded plastic cap (with aluminum foil inside for sealing), and tighten the cap securely. Mark the vial. Gently tap the vial wall to evenly distribute the sample at the bottom. 3) Sample testing: Place the sealed sample vial into a Karl Fischer coulometric moisture analyzer (model C30S-Inmotion KF heating furnace autosampler). (Company: Mettler-Toledo International) Inc.), heat to 200℃ and keep warm for 8 minutes to turn the moisture in the sample into water vapor, which is then carried into the moisture analyzer's analytical cell by the dry carrier gas for testing; 4) Record the results: read the data and record the test results.

[0276] 11. Initial discharge capacity and initial coulombic efficiency tests

[0277] The negative electrode materials of Examples 1-20 and Comparative Examples 1-4, or the composite negative electrode materials of Examples 21-25 and Comparative Examples 5-6, conductive carbon black, and CMC+SBR were dissolved in deionized water at a mass ratio of 95.4:1.2:3.4 to obtain a negative electrode slurry. The negative electrode slurry was coated onto a copper foil current collector, and after vacuum drying at 120°C and rolling, a compacted density of 1.6 g / cm³ was obtained. 3 Negative electrode: A lithium metal sheet is used as the counter electrode, and the cells are assembled into coin cells in an argon-filled glove box. The separator is Celgard C2400, and the electrolyte contains 1.3 mol / L LiPF6 as the solute, and the solutes are ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) in a volume ratio of 3:1:6.

[0278] The coin cell was charged and discharged at a current density of 0.1C within a range of 0.05 to 1.5V to obtain the first reversible specific capacity, the first charge capacity, and the first discharge capacity. The first coulombic efficiency (first efficiency) was calculated according to the formula: first discharge capacity / first charge capacity.

[0279] 12. Capacity retention rate, electrode expansion rate, and electrode conductivity testing.

[0280] The negative electrode materials of Examples 1-20 and Comparative Examples 1-4 were dissolved in deionized water with conductive carbon black, CMC and SBR in a mass percentage of 95.2:1.5:2:1.3, and a negative electrode slurry was prepared by high-speed centrifugation. The slurry preparation equipment was a planetary disperser from Thinking, Japan. The prepared slurry was coated on a 7.5μm copper foil and dried to form a negative electrode sheet. A lithium metal sheet was used as the counter electrode, and a coin cell was assembled in a glove box filled with Ar gas. The coin cell model was 2016.

[0281] The composite negative electrode materials of Examples 21-25 and Comparative Examples 1-2 were dissolved in deionized water with conductive carbon black, CMC and SBR at a mass percentage of 92:4:4, and a negative electrode slurry was prepared by high-speed centrifugation. The slurry preparation equipment was a planetary disperser from Thinking, Japan. The prepared slurry was coated on a 7.5μm copper foil and dried to form a negative electrode sheet. A lithium metal sheet was used as the counter electrode, and a coin cell was assembled in a glove box filled with Ar gas. The coin cell model was 2016.

[0282] The above-mentioned button cells were tested according to the following charge-discharge regime: the battery charge-discharge range was 0.05V to 1.5V, and the equipment used to test the charge-discharge curves was a Lanhe CT3002A. After cycling at current densities of 0.1C, 0.2C, and 0.3C for 3 cycles respectively, the cycle was completed after 47 cycles at a fixed current density of 1C.

[0283] The capacity retention rate of a coin cell after 50 cycles is calculated using the following formula: Capacity retention rate after 50 cycles = Lithium removal capacity in cycle 50 / Lithium removal capacity in cycle 1 × 100%.

[0284] After cycling, the battery is charged to 100% SOC and disassembled in an Ar atmosphere glove box. The thickness of the negative electrode is measured, and the electrode expansion rate is calculated according to the following formula: Electrode expansion rate = (thickness of negative electrode at 100% SOC after 50 cycles - thickness of copper foil) / (thickness of negative electrode after rolling - thickness of copper foil) × 100%.

[0285] The cycled battery was discharged to 0% SOC and disassembled in an Ar atmosphere glove box. The negative electrode was then tested. Resistivity was measured at three random points using an electrode resistance meter, and the average of the three conductivity values ​​was taken as the measured electrode conductivity of the composite negative electrode material. The electrode resistance meter was manufactured by Yuaneng Technology, model BER2500.

[0286] The test results are shown in Tables 1, 2, 3, 4 and 5.

[0287] Table 1

[0288] Table 2

[0289] Table 3

[0290] Table 4

[0291] Table 5

[0292] According to Tables 3 and 4, the negative electrode materials of Examples 1 to 20 all satisfy V b ≥V a And V b >V c Or, V b >V a And V b ≥V c Among them, Examples 1-2, 5-7, and 9-20 all satisfy V. b >V a V b >V c Examples 3 and 8 satisfy V b =V a And V b >V c Example 4 satisfies V b >V a And V b =V c However, neither comparative examples 1 nor 2 satisfies V. b ≥V a And V b >V c Or, V b >V a And V b ≥V c Compared to the anode materials of Comparative Examples 1 and 2, the anode material of this embodiment can significantly reduce the expansion rate, while simultaneously improving capacity, first-cycle coulombic efficiency, and cycle performance. Although Comparative Example 3 satisfies V... b >V a However, it does not satisfy V. b ≥V c Although the comparison example 4 satisfies V b >V c However, it does not satisfy V. b ≥V a Although the expansion rates of Comparative Examples 3 and 4 were reduced, the improvement was limited. Furthermore, the capacity retention, capacity, and initial coulombic efficiency decreased significantly after 50 cycles. Therefore, it can be concluded that this application achieves the desired effect by making the anode material meet the V... b >V a V b >V cIt can significantly improve capacity, initial coulombic efficiency, cycle performance and reduce expansion rate.

[0293] Furthermore, compared to Examples 5-6, 12, 15, and 20, the negative electrode materials of Examples 1-4, 7-9, 11, and 18-19 meet the V... b ≥V a And V b >V c Or, V b >V a And V b ≥V c At the same time, it also meets the following requirements: 10cm -1 ≤ΔF Da ≤30cm -1 6.5cm -1 ≤ΔF Db ≤11cm -1 8cm -1 ≤ΔF Dc ≤20cm -1 Although Example 6 satisfies 8cm -1 ≤ΔF Dc ≤20cm -1 However, it does not meet the 10cm requirement. -1 ≤ΔF Da ≤30cm -1 6.5cm -1 ≤ΔF Db ≤11cm -1 Although the initial discharge capacity, initial coulombic efficiency, and capacity retention after 50 cycles were increased in Example 6, the improvement was limited, and the electrode expansion rate deteriorated; although Examples 12, 15, and 20 met the 10cm requirement... -1 ≤ΔF Da ≤30cm -1 8cm -1 ≤ΔF Dc ≤20cm -1 However, it does not meet the 6.5cm requirement. -1 ≤ΔF Db ≤11cm -1 Although the initial discharge capacity of Examples 12, 15, and 20 increased significantly, the initial coulombic efficiency, capacity retention after 50 cycles, and electrode expansion rate were severely degraded.

[0294] Compared to Examples 5-6, the negative electrode materials of Examples 1-4, 7-9, 11, and 18-19 meet the V... b ≥V a And V b >V c Or, V b >Va And V b ≥V c At the same time, it also satisfies: 2≤W1≤7, although Example 5 satisfies However, it is not satisfied. Although Example 6 satisfies 2≤W1≤7, it does not satisfy the condition 2≤W1≤7. Examples 5 and 6 cannot achieve a simultaneous improvement in performance such as initial discharge capacity, initial coulombic efficiency, capacity retention after 50 cycles, and electrode expansion rate.

[0295] Compared to Examples 16-17, the negative electrode materials of Examples 1-4, 7-9, 11, and 18-19 meet the V... b ≥V a And V b >V c Or, V b >V a And V b ≥V c At the same time, it also satisfies: Although the initial discharge capacity of Examples 16-17 increased and the capacity after 50 cycles remained good, the initial coulombic efficiency and electrode expansion rate after 50 cycles deteriorated significantly.

[0296] Compared to Examples 10, 13-14, and 16, the negative electrode materials of Examples 1-4, 7-9, 11, and 18-19 meet the V... b ≥V a And V b >V c Or, V b >V a And V b ≥V c At the same time, it also satisfies: 8% ≤ V a ≤80%, 16%≤V b ≤90%; Although Example 14 satisfies 16% ≤ V b ≤90%, but does not meet the requirement of 8%≤V a ≤80%, the secondary battery formed by the negative electrode material in Example 14 showed an increase in initial discharge capacity, but performance characteristics such as initial coulombic efficiency, capacity retention after 50 cycles, and electrode expansion rate deteriorated. Although Example 13 met the requirement of 8% ≤ V a ≤80%, but does not meet the requirement: 16%≤V b Although the initial coulombic efficiency of the secondary battery formed by the negative electrode material of Example 13 was maintained relatively well (≤90%), the performance of the initial discharge capacity, capacity retention rate after 50 cycles, and electrode expansion rate deteriorated.

[0297] As shown in Table 5, Examples 21-25 use the method that satisfies V b ≥V a And V b >V c Or, V b >V a And V b ≥V c The negative electrode material is used in combination with different types of silicon-based materials. Comparative examples 5-6 use materials that do not meet the V... b ≥V a And V b >V c Or, V b >V a And V b ≥V c The negative electrode material is used in combination with different types of silicon-based materials. Compared with Comparative Examples 5-6, the batteries assembled with the composite negative electrode materials of Examples 21-25 have higher electrode conductivity, higher initial discharge capacity, and higher initial coulombic efficiency after 50 cycles. In contrast, the batteries assembled with the composite negative electrode materials of Comparative Examples 5-6 have significantly lower electrode conductivity and significantly higher expansion rate after 50 cycles, and their initial discharge capacity and initial coulombic efficiency are lower than those of Examples 21-25. This indicates that the negative electrode material of this application can maintain good electrical contact with the silicon-based material during cycling, promoting the integrity of the overall electrode structure. It is speculated that this is because the negative electrode material with a lattice defect distortion coefficient that meets the requirements can better buffer the expansion stress of the silicon-based material and withstand the volume changes caused by the silicon-based material. After cycling, the electrode still maintains a good conductive network, which helps to improve the electrochemical performance of the secondary battery assembled with this composite negative electrode material.

[0298] In Examples 21-25 and Comparative Examples 5-6, the mass ratio of the negative electrode material to the silicon-based material was 85:15. By controlling the mass ratio of the negative electrode material to the silicon-based material within this range, this application can achieve an initial discharge capacity ≥503 mAh / g, an initial coulombic efficiency ≥90%, an electrode conductivity ≥2 S / cm after 50 cycles, and an electrode expansion rate ≤60%. This demonstrates that the composite negative electrode material formed by combining the negative electrode material and the silicon-based material in this application possesses excellent capacity, initial coulombic efficiency, electrode conductivity, and a low expansion rate.

Claims

1. A negative electrode material, characterized by, The negative electrode material includes carbon-based materials; the negative electrode material is sieved using a 600-mesh sieve, and the particles that fail to pass through the sieve are the first sieve material; the particles that pass through the 600-mesh sieve are sieved again using a 1000-mesh sieve, and the particles that fail to pass through the sieve are the second sieve material; the particles that pass through the 1000-mesh sieve are the third sieve material. The negative electrode material, the first sieve, the second sieve, and the third sieve all exhibit D and G peaks in their Raman spectra. The lattice defect distortion coefficients of the first sieve material, the second sieve material, and the third sieve material are respectively V a V b V c Satisfying: V b ≥V a And V b >V c Or, V b >V a And V b ≥V c ; V a 、V b 、V c by formula I, formula II, formula III: wherein the average of the D / G full width at half maximum ratio for the first sieve fraction; the average of the D / G full width at half maximum ratio of the second sieve fraction; W1 is the average D / G half-peak width ratio of the third sieve material; W1 is the average D / G half-peak width ratio of the negative electrode material; ΔF Da ΔF is the difference in peak position between the D peak of the first sieve material and the negative electrode material; Db ΔF is the difference in the peak position of the D peak between the second sieve material and the negative electrode material; Dc It is the difference between the peak position of the D peak of the third sieve material and the negative electrode material.

2. The negative electrode material according to claim 1, characterized in that, The negative electrode material satisfies at least one of the following characteristics: (1) the first sieve material has a lattice defect distortion coefficient V a satisfies: 8%≤V a ≤80%. (2) the lattice defect distortion coefficient V of the second screening material b satisfies: 16%≤V b ≤90%. (3) the third sieve material has a lattice defect distortion coefficient V c satisfies: 9%≤V c ≤60%.

3. The negative electrode material of claim 1, wherein, The negative electrode material satisfies at least one of the following characteristics: (1) The average value W1 of the D / G half-peak width ratio of the negative electrode material satisfies: 2≤W1≤7; (2) the average of the D / G half-peak width ratios of the first sieve fraction Satisfies: (3) the average of the D / G half-peak width ratios of the second sieve fraction Satisfies: (4) the average of the D / G half-peak width ratios of the third sieve fraction Satisfies:

4. The negative electrode material of claim 1, wherein, The negative electrode material satisfies at least one of the following characteristics: (1) the peak position F of the D peak of the negative electrode material D1 satisfies: 1351 cm -1 ≤ F D1 ≤ 1353 cm -1 ; (2) 10 cm -1 ≤ ΔF Da ≤ 30 cm -1 ; (3) 6.5 cm -1 ≤ ΔF Db ≤ 11 cm -1 ; (4) 8 cm -1 ≤ ΔF Dc ≤ 20 cm -1 .

5. The negative electrode material of claim 1, wherein, The negative electrode material satisfies at least one of the following characteristics: (1) The D50 particle size of the first sieve material is 13.5μm~16.0μm; (2) The D50 particle size of the second sieve material is 13μm~15.0μm; (3) The D50 particle size of the third sieve material is 8μm to 12.8μm; (4) The mass percentage of the first sieve material in the negative electrode material is 30% to 40%; (5) The mass percentage of the second sieve material in the negative electrode material is 40% to 50%; (6) The mass percentage of the third sieve material in the negative electrode material is 10% to 30%.

6. The negative electrode material of claim 1, wherein, The negative electrode material satisfies at least one of the following characteristics: (1) The negative electrode material includes secondary particles and / or primary particles; (2) The negative electrode material includes a first coating layer present on at least a portion of the surface of the carbon-based material; (3) The negative electrode material includes a first coating layer present on at least a portion of the surface of the carbon-based material, the first coating layer comprising carbon material; (4) The negative electrode material includes a first coating layer present on at least a portion of the surface of the carbon-based material, the first coating layer including carbon material, the carbon material including at least one of amorphous carbon and graphitized carbon.

7. The negative electrode material of claim 1, wherein, The negative electrode material satisfies at least one of the following characteristics: (1) The carbon-based material includes at least one of artificial graphite and natural graphite; (2) The negative electrode material includes hydrogen and metal elements, wherein the metal elements include at least one of Zn, Ba and Ca; (3) The negative electrode material includes hydrogen and metal elements, wherein the mass content of hydrogen in the negative electrode material is ≤0.1%, and the mass content of metal elements in the negative electrode material is 1ppm to 50ppm.

8. The negative electrode material according to any one of claims 1 to 7, characterized in that, The negative electrode material satisfies at least one of the following characteristics: (1) The D50 particle size of the negative electrode material is 10μm~15μm, and the D90 particle size is 19μm~24μm; (2) The oil absorption value of the negative electrode material is 45mL / 100g to 60mL / 100g; (3) the powder compaction density of the negative electrode material under 5T pressure is 1.6 g / cm 3 ~ 2.1 g / cm 3 ; (4) the specific surface area of the negative electrode material is 0.8 m 2 / g ~ 5 m 2 / g; (5) The orientation degree of the (004) crystal plane of the negative electrode material is 1.6 to 5; (6) The powder conductivity of the negative electrode material at 4KN is 80S / cm~800S / cm.

9. The negative electrode material according to any one of claims 1 to 7, characterized in that, The negative electrode material satisfies at least one of the following characteristics: (1) The capacity of the negative electrode material is ≥350mAh / g; (2) The initial coulombic efficiency of the negative electrode material is ≥92%; (3) The capacity retention rate of the negative electrode material after 50 cycles is ≥95.3%; (4) The electrode expansion rate of the negative electrode material after 50 cycles is ≤23.7%.

10. A composite negative material, characterized by, Includes the negative electrode material and silicon-based material as described in any one of claims 1 to 9.

11. The composite anode material of claim 10, wherein, The silicon-based material includes at least one of silicon, silicon carbon, silicon oxide, doped silicon oxide, and silicon alloy.

12. The composite anode material of claim 11, wherein, The composite anode material satisfies at least one of the following characteristics: (1) The silicon-based material contains at least one of milled silicon carbon, deposited silicon carbon, and doped silicon carbon; (2) the silicon-based material comprises a silicon oxide of the general formula SiO x 0 < x < 2; (3) The doped silicon oxide in the silicon-based material contains a doping element, which includes at least one of Ca, Mg, Sn, Li, P, Al, and N; (4) At least a portion of the surface of the silicon-based material is provided with a second coating layer; the thickness of the second coating layer is 1 nm to 400 nm; and / or, the second coating layer includes at least one of carbon, nitride, metal oxide, metal fluoride, metal oxyfluoride, and polymer.

13. The composite anode material of claim 10, wherein, The composite anode material satisfies at least one of the following characteristics: (1) the specific surface area of the composite negative electrode material is < 8.0 m 2 / g; (2) The mass percentage of water in the composite negative electrode material is <0.5%; (3) The composite negative electrode material has a D10 particle size of 1μm to 10μm and a D90 particle size of 15μm to 40μm; (4) the tap density of the composite negative electrode material is 0.7 g / cm 3 ~ 3.0 g / cm 3 ; (5) the powder compaction density of the composite negative electrode material under 5T pressure is 0.8 g / cm 3 ~ 5.0 g / cm 3 ; (6) In the composite negative electrode material, the mass ratio of the negative electrode material to the silicon-based material is (3-97):(3-97); (7) The capacity of the composite negative electrode material is ≥365mAh / g; (8) The initial coulombic efficiency of the composite negative electrode material is ≥90%; (9) The electrode conductivity of the composite negative electrode material after 50 cycles is ≥0.8 S / cm; (10) The electrode expansion rate of the composite negative electrode material after 50 cycles is ≤84%.

14. A negative electrode sheet characterized by comprising: The negative electrode sheet comprises the negative electrode material according to any one of claims 1 to 9 or the composite negative electrode material according to any one of claims 10 to 13.

15. A secondary battery characterized by comprising: The secondary battery includes the negative electrode sheet as described in claim 14.