Battery cell, battery device, electric device and energy storage device

By optimizing the particle distribution and graphitization degree of the positive electrode film, and combining the use of carbon nanotubes and conductive carbon black as conductive agents, the internal resistance and heat generation of the battery cells are improved. By adopting a porous separator and a dual sealing area design, the balance between energy density and safety performance of lithium-ion batteries is solved, and the improvement of high energy density and safety performance is achieved.

WO2026238156A1PCT designated stage Publication Date: 2026-11-19CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/109828
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-05-12
Filing Date
2026-07-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously improve the energy density and safety performance of lithium-ion batteries, and how to balance the two has become an urgent technical problem to be solved.

Method used

By optimizing the particle distribution and graphitization degree of the positive electrode film, controlling the particle area ratio and particle size concentration, and combining carbon nanotubes and conductive carbon black as conductive agents, the internal resistance and heat generation of the battery cells are improved. Furthermore, the safety performance of the battery is enhanced by adopting a porous separator and a dual-sealing area design.

Benefits of technology

This achieves the goal of increasing battery energy density while reducing internal resistance and heat generation, enhancing battery safety performance, and extending battery cycle life and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026109828_19112026_PF_FP_ABST
    Figure CN2026109828_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A battery cell, a battery device, an electric device and an energy storage device. The battery cell comprises a positive electrode active material that comprises lithium-containing transition metal phosphate particles, the surfaces of which are at least partially provided with a carbon material. On the basis of the total area of particles in a section of a positive electrode film layer along the thickness direction of an electrode sheet, the area of particles having a particle size R1 that satisfies 50 nm≤R1≤400 nm accounts for 20-40%, and the area of particles having a particle size R3 that satisfies 1 μm<R3≤5 μm accounts for less than or equal to 30%. In the cumulative distribution curve of the C value of the graphitization degree of the positive electrode film layer obtained by a laser micro-confocal Raman spectrometer in a surface scanning mode, the median C50 of the graphitization degree is 0.95-1.20.
Need to check novelty before this filing date? Find Prior Art

Description

Battery cells, battery devices, electrical devices, and energy storage devices

[0001] Cross-referencing

[0002] This disclosure incorporates, by reference, PCT / CN2025 / 094369, international patent application filed on May 12, 2025, entitled “Battery cell, battery device, power consumption device and energy storage device”, and PCT / CN2025 / 107786, international patent application filed on July 9, 2025, entitled “Battery cell, battery device, power consumption device and energy storage device”. This publication references and claims priority to Chinese Patent Application No. 2025112111751, filed on August 27, 2025, entitled "Battery Cell, Battery Device, Power Consumption Device and Energy Storage Device", the entire contents of which are incorporated herein by reference. This publication also references PCT / CN2026 / 096520, International Patent Application No. PCT / CN2026 / 096520, filed on May 12, 2026, entitled "Battery Cell, Battery Device, Power Consumption Device and Energy Storage Device", which is incorporated herein by reference. Technical Field

[0003] This disclosure relates to the field of lithium-ion battery technology, and in particular to a battery cell, battery device, power supply device, and energy storage device. Background Technology

[0004] In recent years, battery cells have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.

[0005] As the market demands longer driving range and longer battery life, higher requirements are being placed on battery energy density and safety performance. However, current technologies struggle to simultaneously improve these performance aspects, making it crucial to address this critical technical challenge. Summary of the Invention

[0006] This disclosure is made in view of the above-mentioned issues, and its purpose is to provide a battery cell that combines high energy density and good safety performance.

[0007] A first aspect of the present disclosure provides a battery cell, the battery cell includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium-containing transition metal phosphate particles at least partially provided with a carbon material on the surface; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is 20%-40%; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 30%; in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer in the surface scanning mode of a laser confocal Raman spectrometer, the median C of the graphitization degree 50 is 0.95-1.20, wherein the graphitization degree C value is I G / I D , wherein I G represents the G peak intensity of the Raman spectrum at 1580±100cm -1 , and I D represents the D peak intensity of the Raman spectrum at 1350±100cm -1 .

[0008] The battery cell according to the embodiments of the present disclosure has low internal resistance, which improves the heat generation problem while increasing the energy density of the battery cell, and gives consideration to safety performance.

[0009] The applicant has found that, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, when the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is greater than or equal to 20%, it helps to increase the compaction density of the film layer, thereby improving the energy density of the battery; however, the size of particles with a particle size R1 satisfying 50nm≤R1≤400nm is small, and when the area proportion thereof is greater than 40%, the contact area of particles in the film layer increases significantly, leading to an increase in the ohmic internal resistance of the electrode plate and an increase in heat generation of the battery. At the same time, the size of particles with a particle size R3 satisfying 1μm<R3≤5μm is large, and when the area proportion thereof is greater than 30%, the polarization internal resistance of the positive electrode plate will be significantly increased, thereby aggravating the heat generation problem. In addition, the median C of the graphitization degree of the positive electrode film layer 50 being greater than or equal to 0.95 contributes to the electronic conductivity of the carbon coating layer on the particle surface and reduces the resistance of the electrode plate. When the graphitization degree is higher than 1.2, the concentration of the material will be affected, so in consideration of the uniformity of the material, the graphitization degree of the carbon material layer is usually not higher than 1.2.

[0010] In the embodiments of the present disclosure, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is 20%-40%; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 30%; in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer in the surface scanning mode of a laser confocal Raman spectrometer, the median C of the graphitization degree 50 is 0.95-1.20, which helps reduce the internal resistance of the positive electrode sheet, lower the heat generation of the electrode sheet, and improve the safety performance of the battery cell.

[0011] In some embodiments, in the particle size-area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -D A10 ) / D A50 is less than or equal to 2.3. By making (D A90 -D A10 ) / D A50 less than or equal to 2.3, the medium-sized particles account for a certain proportion in the total particles, and the particle size concentration of the medium-sized particles is within the above range, which helps improve the compaction density of the film layer according to the particle gradation principle, and balance the energy density and safety performance of the battery cell.

[0012] In some embodiments, in the particle size-area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -D A10 ) / D A50 is 0.5-2.3. The medium-sized particles account for a certain proportion in the total particles. By making the particle size concentration of the medium-sized particles within the above range, it helps improve the compaction density of the film layer according to the particle gradation principle, and balance the energy density and safety performance of the battery cell.

[0013] In some embodiments, in the particle size-area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -D A10 ) / D A50is 0.7-1.3. Medium-sized particles account for a certain proportion in the total particles. By setting the particle size concentration of the medium-sized particles within the above range, the particle size difference between the medium-sized particles is small, the particle deformation is relatively synchronous, the internal extrusion between particles is low, and the stress is evenly dispersed, which can reduce the generation of particle cracks. Meanwhile, the design of the particle size concentration will not be too small, and a certain gradation is still retained, thereby taking into account the compaction density of the positive electrode film layer, and further taking into account the energy density and safety performance of the battery cell.

[0014] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm obtained from the cross section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 is 1-2.3, the medium-sized particles account for a relatively high proportion in the total particles, and the particle size concentration of the medium-sized particles is within the above range, which helps to improve the compaction density of the film layer according to the particle gradation principle, and takes into account the energy density and safety performance of the battery cell.

[0015] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm obtained from the cross section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 is 1.5-2.3. Setting the particle size concentration within the above range indicates that the overall particle gradation degree is good, which is beneficial to increasing the compaction density of the pole piece, further increasing the energy density, not deteriorating the ohmic internal resistance, and is beneficial to taking safety into account.

[0016] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the pole piece, the area proportion of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm is greater than or equal to 25%. Accordingly, the medium-sized particles account for a certain proportion in the total particles, which helps to improve the compaction density of the film layer according to the particle gradation principle, and takes into account the energy density and safety performance of the battery cell.

[0017] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the pole piece, the area proportion of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm is 25%-70%. Accordingly, the medium-sized particles account for a relatively high proportion in the total particles, which helps to improve the compaction density of the film layer according to the particle gradation principle, and takes into account the energy density and safety performance of the battery cell.

[0018] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm < R2 ≤ 1μm is 40% - 70%. Accordingly, the proportion of medium-sized particles in the total particles is relatively high, which helps to increase the compaction density of the film layer according to the particle gradation principle, and takes into account both the energy density and safety performance of the battery cell.

[0019] In some embodiments, when the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 70μm - 120μm. This helps to improve the energy density of the lithium-containing transition metal phosphate battery.

[0020] In some embodiments, when the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 90μm - 120μm.

[0021] In some embodiments, when the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 100μm - 120μm.

[0022] The single-side thickness of the positive electrode film layer within the above range helps to further increase the loading amount of the active material on the electrode sheet and improve the energy density of the battery. However, after the loading amount of the active material increases, the heat generation of the electrode sheet intensifies. In the embodiments of the present disclosure, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm ≤ R1 ≤ 400nm is 20% - 40%, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm < R3 ≤ 5μm is less than or equal to 30%, in the cumulative distribution curve of the graphitization degree C value obtained in the surface scanning mode of the laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 0.95 - 1.20, in the cumulative distribution curve of particle size area of particles with a particle size R2 satisfying 0.4μm < R2 ≤ 1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -D A10 ) / D A50 is less than or equal to 2.3, which is especially suitable for battery cells with the single-side thickness of the positive electrode film layer within the above range, and helps to achieve high energy density while taking into account safety performance.

[0023] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm ≤ R1 ≤ 400nm is 25% - 35%.

[0024] The area proportion of particles with a particle size satisfying 50nm≤R1≤400nm falling within the above range helps reduce the contact area between particles, lower the ohmic internal resistance of the electrode sheet, and simultaneously take into account the particle gradation and compaction density in the positive electrode film layer, thereby balancing the energy density and safety performance of the battery.

[0025] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 20%.

[0026] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is 10%-20%.

[0027] The area proportion of particles with a particle size satisfying 1μm<R3≤5μm falling within the above range helps further reduce the polarization internal resistance, lower the heat generation of the electrode sheet, and thus further improve the safety performance of the battery.

[0028] In some embodiments, in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer under the surface scanning mode of a laser micro-confocal Raman spectrometer, the median C of the graphitization degree 50 is 1.01-1.13.

[0029] The median graphitization degree of the positive electrode film layer falling within the above range helps further increase the electronic conductivity on the particle surface, reduce the ohmic internal resistance of the electrode sheet, lower the heat generation of the electrode sheet, and further improve the safety performance of the battery.

[0030] In some embodiments, when the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet is 2.3g / cm 3 -2.6g / cm 3 .

[0031] The compaction density of the positive electrode sheet falling within the above range helps increase the loading amount of the active material per unit volume and improve the energy density of the battery cell.

[0032] In some embodiments, in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the porosity of the positive electrode film layer is 14%-28%.

[0033] The porosity of the positive electrode film layer falling within the above range endows the positive electrode film layer with good electrolyte wettability and tortuosity, facilitates the diffusion of lithium ions in the liquid phase and solid phase, helps reduce the concentration polarization of the thick electrode sheet, lowers the heat generation of the electrode sheet, and improves the safety performance of the battery.

[0034] In some embodiments, in the cumulative distribution curve of the coating value B obtained by the positive electrode film layer under the surface scanning mode of a laser micro-confocal Raman spectrometer, the median B of the coating value50 The value is 0.3-0.6, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0035] Poor coating density of the positive electrode film increases the electron transport path within the coating layer, leading to increased internal resistance and heat generation in the electrode. The median coating value B of the positive electrode film... 50 Within the above range, it is evident that the carbon material layer of the positive electrode active material is relatively dense and uniform, which helps to reduce the internal resistance of the electrode, reduce the heat generation of the electrode, and improve the safety performance of the battery.

[0036] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-2.5% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0037] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomerated region of the conductive agent is within the above range, indicating that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network. This is especially beneficial for improving the electron transport rate of the thick coating film in the thickness direction of the electrode sheet, thereby reducing the internal resistance of the electrode sheet, reducing the heat generation of the electrode sheet, and improving the safety performance of the battery.

[0038] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-1.7% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0039] In this embodiment, the area ratio of the agglomerated region of the conductive agent is further within the above-mentioned range, indicating that the conductive agent is more uniformly distributed in the positive electrode film layer and the content of the conductive agent is low. While reducing the internal resistance of the electrode, the conductive agent content is not excessive, reducing the space occupied by the positive electrode active material, thereby balancing the energy density and safety performance of the battery.

[0040] In some implementations, the range of the area ratio of conductive agent agglomeration regions in a cross section along the thickness direction of the positive electrode sheet is less than or equal to 2%.

[0041] In some implementations, the area ratio of conductive agent agglomeration regions in a cross-section along the thickness direction of the positive electrode sheet varies from 0% to 1%.

[0042] In the cross section along the thickness direction of the positive electrode plate, the range of the area proportion of the conductive agent agglomeration region is within the above range, which indicates that the conductive agent is uniformly dispersed in the positive electrode film layer, and is easy to form a uniform conductive network, which is particularly beneficial to increasing the electron transmission rate of the thickly coated film layer in the thickness direction of the electrode plate, thereby reducing the internal resistance of the electrode plate, reducing heat generation of the electrode plate, and improving the safety performance of the battery.

[0043] In some embodiments, the conductive agent comprises carbon nanotubes, and the carbon nanotubes comprise one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.

[0044] Since carbon nanotubes have a one-dimensional structure, they can form a network structure in the positive electrode film layer. The excellent conductivity of carbon nanotubes makes their network structure an efficient electron transmission channel, which helps to further increase the electron transmission rate of the thickly coated film layer in the thickness direction of the electrode plate, thereby reducing the ohmic internal resistance of the battery, reducing heat generation, and improving the safety performance of the battery.

[0045] In some embodiments, the conductive agent further comprises conductive carbon black.

[0046] Conductive carbon black has a relatively high specific surface area, and thus has good liquid retention capacity. The thick electrode plate has a large expansion force during the cycle process, which makes the electrolyte easy to be squeezed out. The distribution of conductive carbon black in the positive electrode film layer is beneficial to improving the liquid retention capacity of the thick electrode plate, reducing the polarization internal resistance of the battery, reducing heat generation, and improving the safety performance of the battery.

[0047] In some embodiments, the agglomeration region of the conductive agent comprises carbon nanotubes and conductive carbon black.

[0048] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, resulting in uneven dispersion in the positive electrode film layer and failure to form an effective carbon nanotube network structure. Conductive carbon black and carbon nanotubes have relatively close surface energies, and can be adsorbed on the surface of carbon nanotubes to form a physical barrier, which increases the resistance to agglomeration of carbon nanotubes, reduces direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. This helps to further reduce the ohmic internal resistance of the battery, reduce heat generation, and improve the safety performance of the battery.

[0049] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of conductive carbon black satisfies: 0<C2≤2.5%.

[0050] The mass contents of carbon nanotubes and conductive carbon black within the above range can effectively alleviate the agglomeration phenomenon of carbon nanotubes and form a good conductive network structure, reducing the ohmic internal resistance; at the same time, it helps to improve the liquid retention rate of the positive electrode plate during the long cycle process, further reduce the polarization internal resistance, reduce the heat generation of the battery, and improve the safety performance of the battery.

[0051] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector. The undercoat layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.

[0052] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector, and the thickness of the undercoat layer is 0.5 μm-5 μm.

[0053] Compared to the direct contact between the positive electrode current collector and the positive active material layer, the undercoating layer provided in this embodiment has an increased contact area with the positive electrode film layer. This helps to increase the area of ​​electron transport between the current collector and the positive electrode film layer, thereby reducing the internal resistance of the electrode, reducing heat generation, and improving the safety performance of the battery.

[0054] In some implementations, the size of the positive current collector is 12μm-16μm along the thickness direction of the positive electrode sheet.

[0055] The thickness of the positive electrode current collector is within the above range, which helps to increase the cross-sectional area for current transmission within the current collector, thereby reducing the resistance of the current collector, reducing heat generation on the electrode, and helping to improve the safety performance of the battery.

[0056] In some implementations, the size of the positive current collector is 13μm-15μm along the thickness direction of the positive electrode sheet.

[0057] If the positive electrode current collector is too large, it will affect the energy density of the battery. In the embodiments of this disclosure, the thickness of the positive electrode current collector is within the above range, which helps to balance the energy density, toroidal performance and safety performance of the battery.

[0058] In some embodiments, the resistivity of the positive electrode film is 5 Ω·cm - 35 Ω·cm

[0059] If the resistivity of the positive electrode film is within the above range, it indicates that the positive electrode film has low internal resistance, which helps to reduce heat generation on the electrode and improve the safety performance of the battery.

[0060] In some embodiments, the lithium transition metal phosphate particles comprise components represented by the following general formula:

[0061] Li m Fe x P y O j Q q Formula I,

[0062] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.

[0063] In some embodiments, the lithium transition metal phosphate particles include titanium, and the titanium content is 500ppm-8000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0064] In some embodiments, the lithium transition metal phosphate particles include titanium, and the mass content of titanium is 1000ppm-3000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0065] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate raw material reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increasing polarization resistance. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the cathode active material is reduced. This allows the cathode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing the internal resistance of the electrode, reducing heat generation, and improving battery safety performance.

[0066] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and further reducing the internal resistance of the electrode. Furthermore, the uneven diffusion of lithium ions in thick coated films often results in a significant lithium-ion concentration gradient. This disclosure improves the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thereby reducing the polarization resistance of thick electrodes and mitigating the heat generation problem in thick electrode batteries.

[0067] In some embodiments, the lithium transition metal phosphate particles include vanadium, and the vanadium content is 500 ppm to 5000 ppm based on the total mass of the lithium transition metal phosphate particles in the cathode film.

[0068] In some embodiments, the lithium transition metal phosphate particles include vanadium, and the vanadium content is 500ppm-3000ppm based on the total mass of the lithium transition metal phosphate particles in the cathode film.

[0069] Vanadium in the positive electrode film can be in multiple valence states, including +5 vanadium (V5). 5+ Vanadium (V+3) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expand the diffusion channels of lithium ions, thereby improving the ionic conductivity of the positive electrode active material and reducing the internal resistance of the battery; vanadium (V+3) 3+ Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material and reducing the ohmic internal resistance of the battery. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further reduce the internal resistance of the positive electrode film and improve the uniformity of the positive electrode film reaction, thus further enhancing the battery's safety performance.

[0070] Within the aforementioned mass content range, vanadium helps reduce the internal resistance of the positive electrode and decreases heat generation in thick-coated lithium transition metal phosphate batteries. Simultaneously, the synergistic effect of titanium, vanadium, and carbon nanotubes in the positive electrode film helps form a robust three-dimensional network, further enhancing the electronic and ionic conductivity of the positive electrode film, reducing internal resistance, and thus further improving the safety performance of thick-coated lithium transition metal phosphate batteries.

[0071] In some embodiments, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, a ceramic layer disposed on at least one side of the base film, and an adhesive layer disposed on the side of the ceramic layer away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

[0072] Placing ceramic layers on both sides of the base film helps improve the rigidity of the pouch cell.

[0073] In the prior art, the adhesive layer of the separator usually uses aqueous PVDF, which presents an island-like structure in the separator. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing. However, such a separator adhesive layer has a small contact area with the electrode and weak adhesion.

[0074] The separator provided in this embodiment uses a continuous porous layer as the adhesive layer. Compared with the adhesive layer in the prior art, it has a larger bonding area with the electrode, which makes the bonding between the separator and the electrode more firm and uniform. This helps to reduce the spacing between the electrodes, reduce impedance, alleviate heat generation, and improve the safety performance of the battery.

[0075] In some embodiments, the battery cell includes a wound cell, which comprises a positive electrode and a negative electrode formed into an electrode assembly by a winding process.

[0076] In some embodiments, the battery cell includes a stacked cell, which comprises a positive electrode and a negative electrode formed by stacking them to form an electrode assembly.

[0077] Compared to wound cells, stacked cells have less compression between the separator and the electrodes, resulting in a relatively larger gap between the electrodes. This increases the battery's internal resistance and heat generation. Furthermore, it can lead to the positive and negative electrodes bridging each other, increasing the risk of internal short circuits within the cell. Therefore, the separator provided in this disclosure is particularly suitable for stacked cells. The increased adhesion between the porous adhesive layer and the electrodes helps reduce the distance between the positive and negative electrodes, reducing heat generation, and also helps reduce the risk of short circuits caused by electrode bridging, thereby improving battery safety performance.

[0078] In some implementations, the thickness of the base membrane in the diaphragm is 7-9 μm.

[0079] In some embodiments, the thickness of the ceramic layer in the diaphragm is 2-4 μm on one side.

[0080] In some embodiments, the thickness of the adhesive layer on one side of the diaphragm is 1-5 μm.

[0081] If the adhesive layer is too thin, the adhesion between the separator and the electrode is weak. On the one hand, the spacing between the positive and negative electrodes is larger, increasing the battery impedance and heat generation; on the other hand, the probability of a short circuit due to positive-negative electrode overlap increases, thus affecting the battery's safety performance. If the adhesive layer is too thick, it occupies a large amount of battery space, thus affecting the battery's volumetric energy density. In the embodiments of this disclosure, the thickness of the adhesive layer is within the above-mentioned range, which helps to balance the battery's safety performance and volumetric energy density.

[0082] In some embodiments, the battery cell further includes a housing, in which the stacked cells are housed, and the housing includes a pouch material, which includes an aluminum-plastic composite film.

[0083] In some embodiments, the flexible packaging material includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.

[0084] Soft-pack materials have high elongation, resulting in thinner and more flexible casings that improve space utilization of individual battery cells, thereby increasing their energy density. Furthermore, aluminum's high barrier properties effectively reduce the penetration of water and oxygen into the battery, decreasing electrolyte decomposition and electrode material oxidation, thus extending battery life.

[0085] In some embodiments, the housing includes a first receiving portion and a second receiving portion, the first receiving portion and the second receiving portion being integrally connected and disposed opposite to each other, and the stacked battery cell being received within the receiving cavity formed by the first receiving portion and the second receiving portion.

[0086] The increased loading of active material in thickly coated electrodes exacerbates the expansion of the cell during charging and discharging. With the expansion and contraction of the cell, the base of the tabs and the solder joints are subjected to repeated tensile-compressive-shear stresses, which easily lead to fatigue deformation and increased internal resistance. In this embodiment, the battery cell housing includes a first receiving portion and a second receiving portion. Compared to a structure with only one receiving portion, the two receiving portions place the base of the tabs and the solder joints in a more symmetrical stress environment, helping to disperse stress concentration, slowing down the rate of increase in resistance in this area, and thus extending the cycle life of the battery.

[0087] In some embodiments, the shell includes a first sealing area disposed at at least one end of the laminated cell extending along a second direction; the first sealing area includes a folded edge structure extending along a first direction, on which encapsulating adhesive is disposed, and the encapsulating adhesive is continuously disposed along the first direction and fixes the folded edge structure.

[0088] During electrode cycling, the SEI film thickens, leading to significant rebound and gas generation during long cycles. This is especially true in thickly coated electrodes, where increased active material loading results in increased rebound, gas generation, and heat generation. Furthermore, increased gas generation exacerbates side reactions, further increasing gas production. The sealing area of ​​the pouch cell is used to seal the electrode assembly; however, the sealing area has limited strength and is easily breached by large rebounds and high gas generation within the film layer.

[0089] This embodiment further enhances the sealing strength of the first sealing area by including a folded edge structure extending along a first direction. The continuous arrangement of the encapsulating adhesive along the first direction and the fixing of the folded edge structure, compared to a discontinuous arrangement of the encapsulating adhesive along the first direction, further improves the sealing strength, achieving continuous reinforcement of the sealing area in the first direction and reducing the probability of the electrode breaking open the sealing area in the packaging during cycling.

[0090] In some embodiments, the housing includes at least one second sealing area disposed at at least one end of the laminated cell along a first direction of the housing, the second sealing area being disposed on the tab side of the laminated cell.

[0091] The second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the shell material is relatively weak, which makes it easy for gas to escape from the second sealing area. This is conducive to directional pressure relief of the battery, reducing the impact on adjacent cells during thermal runaway, and improving the overall service life of the battery.

[0092] In some embodiments, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in a second direction, and the rubber rings that surround in the second direction are spaced apart in a first direction.

[0093] The rubber rings that surround the cell in the second direction are spaced apart in the first direction, which helps to fix the position between the electrodes in the cell and reduce the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large size in the first direction. It can effectively reduce the mutual displacement between the electrodes in the first direction, thus reducing lithium plating. It helps to maintain the stability of the internal spatial structure of the battery and thus does not affect the normal operation of the battery.

[0094] In some embodiments, the dimension of the casing in the length direction of the battery cell is L1, the dimension of the casing in the width direction of the battery cell is W1, and the dimension of the casing in the thickness direction of the battery cell is H1, wherein 450mm≤L1≤1300mm, 100mm≤W1≤150mm, and 14mm≤H1≤22mm.

[0095] In some embodiments, the dimension of the casing along the length of the battery cell is L1, where 450mm ≤ L1 ≤ 650mm.

[0096] When the length dimension L1 of the casing satisfies 450mm≤L1≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance and the safety performance of the battery.

[0097] In some embodiments, the dimension of the casing along the length of the battery cell is L1, where 900mm ≤ L1 ≤ 1300mm.

[0098] When the length dimension L1 of the casing satisfies 900mm≤L1≤1300mm, the battery cell is relatively long, which helps to reduce the volume ratio of the casing in the battery cell and increase the load ratio of active materials. At the same time, a longer battery cell can reduce the number of batteries required in the battery module, simplify the structural design of the battery module, reduce the number and complexity of structural components in the module, thereby improving the space utilization of the battery pack and thus helping to improve the volumetric energy density of the battery cell.

[0099] In some embodiments, at 25°C, the capacity of the battery cell is 95Ah-300Ah, optionally 150Ah-190Ah.

[0100] A second aspect of this disclosure provides a battery device including the battery cell provided in the first aspect of this disclosure.

[0101] A third aspect of this disclosure provides an electrical device that includes a battery device provided in the second aspect, the battery device being used to provide electrical energy.

[0102] The fourth aspect of this disclosure provides an energy storage device, which includes a battery device provided in the second aspect, the battery device being used to store electrical energy. Attached Figure Description

[0103] Figure 1 is a schematic diagram of a pouch-pack stacked battery disclosed in this invention;

[0104] Figure 2 is a schematic diagram of a diaphragm according to an embodiment of the present disclosure;

[0105] Figure 3 is a schematic diagram of the diaphragm in the prior art;

[0106] Figure 4 is a schematic diagram of the surface morphology of the adhesive layer according to an embodiment of this disclosure;

[0107] Figure 5 is a schematic diagram of an electrical device according to an embodiment of the present disclosure.

[0108] Explanation of reference numerals in the attached drawings: 20 separator; 201 base film; 202 ceramic layer; 203 adhesive layer; 5 battery cell; 50 casing; 51 first sealing area; 52 second sealing area; 53 lead-out component; X length direction; Y width direction; Z thickness direction. Detailed Implementation

[0109] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the battery cell, battery assembly, power consumption device, and energy storage device of this disclosure. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this disclosure and are not intended to limit the subject matter of the claims.

[0110] The "range" disclosed in this disclosure is defined by a lower limit and an upper limit, whereby a given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also expected. Furthermore, if minimum range values ​​1 and 2 are listed, and if maximum range values ​​3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this disclosure, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0111] Unless otherwise specified, all embodiments and optional embodiments of this disclosure may be combined with each other to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.

[0112] Unless otherwise specified, all technical features and optional technical features of this disclosure can be combined to form new technical solutions, and such technical solutions should be considered as included in the disclosure of this disclosure.

[0113] Unless otherwise specified, all steps in this disclosure may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0114] In this disclosure, the terms "multiple" or "a variety" refer to two or more kinds.

[0115] Unless otherwise stated, the terms used in this disclosure have the common meanings as commonly understood by those skilled in the art.

[0116] Unless otherwise stated, the values ​​of the parameters mentioned in this disclosure can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this disclosure. Unless otherwise stated, the test temperature for each parameter is 25°C.

[0117] In embodiments of this disclosure, the battery device may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell units connected in series, parallel, or a combination of these units via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell units; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell units into a single module. As an example, a battery module may be formed by bundling multiple battery cells together with cable ties.

[0118] The battery device can be a battery pack, which includes a housing and one or more individual battery cells housed within the housing. The individual battery cells can be battery modules, which can be housed within the housing by fixing the battery modules to the housing; alternatively, multiple pouch battery cells can be directly fixed to the housing and housed within the housing.

[0119] In embodiments of this disclosure, the housing may include a first housing and a second housing. The first housing and the second housing are fastened together to form a closed space inside the housing for housing individual battery cells. Here, "closed" refers to covering or shutting down; it can be sealed or unsealed. The first housing may be a top cover or a bottom plate. For example, the housing may include a top cover, a frame, and a bottom plate. The top cover and the bottom plate are respectively connected to the frame, forming a closed space inside the housing for housing individual battery cells.

[0120] In embodiments of this disclosure, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.

[0121] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.

[0122] The battery mentioned in the embodiments of this disclosure can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this disclosure can include battery cells, battery modules, or battery packs.

[0123] A single battery cell is the smallest unit that makes up a battery, and it can independently perform the functions of charging and discharging.

[0124] When there are multiple battery cells, they are connected in series, parallel, or mixed via a busbar. In some embodiments, the battery can be a battery module; when there are multiple battery cells, they are arranged and fixed to form a battery module. In some embodiments, the battery can be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed within the housing. In some embodiments, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least part of the vehicle's floor, or a portion of the housing can be at least part of the vehicle's crossbeams and longitudinal beams.

[0125] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.

[0126] In some implementations, individual battery cells can be assembled into a battery module, and the number of individual battery cells contained in the battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module.

[0127] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0128] A "battery cell" refers to the basic unit capable of converting chemical energy into electrical energy. Specifically, it typically includes at least a positive electrode, a separator, a negative electrode, and an electrolyte. During charging and discharging, active ions repeatedly insert and extract between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, provides insulation against electrons, preventing internal short circuits, while allowing active ions to permeate and move between the electrodes. The electrolyte, acting as a conductor for the active ions, lies between the positive and negative electrodes.

[0129] Lithium-containing transition metal phosphates, as positive electrode active materials, offer advantages such as high safety, long cycle life, low cost, and high high-temperature stability. However, their intrinsic specific capacity is significantly lower than that of ternary materials. To compensate for this energy density shortcoming, related technologies employ thick coating strategies to increase the loading of positive electrode active materials, thereby improving battery energy density. However, with the increase in positive electrode active material, the heat generation of the electrode increases significantly, leading to a rise in electrode temperature, which in turn exacerbates side reactions and increases the risk of battery thermal runaway. Therefore, how to improve battery energy density while ensuring safety performance remains a pressing technical problem that needs to be solved.

[0130] A first aspect of the present disclosure provides a battery cell, the battery cell includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium-containing transition metal phosphate particles at least partially provided with a carbon material on the surface; based on the total area of particles in a cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is 20%-40%; based on the total area of particles in a cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 30%; in the cumulative distribution curve of the graphitization degree C value obtained under the surface scanning mode of a laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 0.95-1.20, wherein the graphitization degree C value is I G / I D , wherein I G represents the G peak intensity of the Raman spectrum at 1580±100cm -1 , and I D represents the D peak intensity of the Raman spectrum at 1350±100cm -1 .

[0131] The battery cell according to the embodiments of the present disclosure has low internal resistance, improves the heat generation problem while achieving an increase in the energy density of the battery cell, and gives consideration to safety performance.

[0132] The applicant has found that, based on the total area of particles in a cross section of the positive electrode film layer along the thickness direction of the electrode plate, when the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is greater than or equal to 20%, it helps to increase the compaction density of the film layer, thereby increasing the energy density of the battery; however, the particles with a particle size R1 satisfying 50nm≤R1≤400nm have a relatively small size, and when the area proportion thereof is greater than 40%, the contact area of particles in the film layer increases significantly, leading to an increase in the ohmic internal resistance of the electrode plate and an increase in heat generation of the battery. At the same time, the particles with a particle size R3 satisfying 1μm<R3≤5μm have a relatively large size, and when the area proportion thereof is greater than 30%, the polarization internal resistance of the positive electrode plate will be significantly increased, thereby aggravating the heat generation problem. Therefore, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm being less than or equal to 30% is beneficial to further reducing the heat generation of the electrode plate and improving the safety performance of the battery cell. In addition, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm within the above range can form a good gradation with particles with a particle size R1 satisfying 50nm≤R1≤400nm, thereby further increasing the energy density of the battery cell. Furthermore, the median C of the graphitization degree of the positive electrode film layer 50A value of 0.95 or higher contributes to the electronic conductivity of the carbon coating layer on the particle surface and reduces the resistance of the electrode sheet. When the graphitization degree is higher than 1.2, the material concentration will be affected. Therefore, in consideration of the uniformity of the material, the graphitization degree of the carbon material layer is usually not higher than 1.2.

[0133] Therefore, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm is 20%-40%; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with the particle size R3 satisfying 1μm < R3 ≤ 5μm is less than or equal to 30%; in the cumulative distribution curve of the graphitization degree C value obtained in the surface scanning mode of the laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 0.95-1.20, which helps to improve the energy density of the battery while reducing the internal resistance of the positive electrode sheet, lowering the heat generation of the electrode sheet, and improving the safety performance of the battery cell.

[0134] In some embodiments, in the cumulative distribution curve of particle size area of particles with the particle size R2 satisfying 0.4μm < R2 ≤ 1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -D A10 ) / D A50 is less than or equal to 2.3. By further making (D A90 -D A10 ) / D A50 less than or equal to 2.3, it is helpful to increase the compaction density of the film layer according to the particle gradation principle, and balance the energy density and safety performance of the battery cell.

[0135] In the present disclosure, the laminated cell refers to a cell formed by stacking a positive electrode sheet, a separator and a negative electrode sheet together.

[0136] In the present disclosure, the lithium-containing transition metal phosphate refers to a phosphate material containing lithium element and transition metal element, which can be detected by any known method in the art. For example, it can be detected by the combination of an X-ray diffractometer (XRD), an energy spectrum analyzer and an inductively coupled plasma mass spectrometer.

[0137] In the present disclosure, the carbon coating material disposed on at least part of the surface of the lithium-containing transition metal phosphate particles can be detected by any known method in the art. As an example, the carbon coating material disposed on at least part of the surface of the lithium-containing transition metal phosphate particles can be observed by characterizing the lithium-containing transition metal phosphate particles through the combination of a transmission electron microscope and an energy spectrum analyzer.

[0138] In this disclosure, the fully discharged state refers to the state after placing the battery in a 25°C oven environment, letting it stand for 2 hours, maintaining the battery temperature at 25°C, discharging the battery at a constant current of 1 / 3C to 2.5V, and then discharging it at a constant current of 0.1C to 2.0V.

[0139] In some implementations, the thickness H of the positive electrode film on one side of the battery cell in a fully discharged state is 70 μm-120 μm. This helps to improve the energy density of lithium-containing transition metal phosphate batteries.

[0140] The thickness of the positive electrode film can be measured using any method known in the art. As an example, the thickness of the positive electrode film in a cross-section along the thickness direction of the positive electrode sheet is measured using a scanning electron microscope.

[0141] In some embodiments, when the battery cell is in a fully discharged state, the thickness H of the positive electrode film on one side can be selected as 70μm, 71μm, 72μm, 73μm, 74μm, 75μm, 76μm, 77μm, 78μm, 79μm, 80μm, 81μm, 82μm, 83μm, 84μm, 85μm, 86μm, 87μm, 88μm, 89μm, 90μm, 91μm, 92μm, 93μm, 94μm, 95μm, etc. μm, 96μm, 97μm, 98μm, 99μm, 100μm, 101μm, 102μm, 103μm, 104μm, 105μm, 106μm, 107μm, 108μm, 109 μm, 110μm, 111μm, 112μm, 113μm, 114μm, 115μm, 116μm, 117μm, 118μm, 119μm, 120μm or any numerical range in between.

[0142] In this disclosure, the term "particle" refers to a particle of the positive electrode film layer that has a recognizable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist within the particle, but no complete boundary sufficient to divide the particle can be identified within it. The positive electrode film layer in this disclosure can be a freshly prepared positive electrode film layer or a positive electrode film layer obtained from the disassembly of a battery.

[0143] In this disclosure, the positive electrode film layer includes the positive electrode active material, but the positive electrode film layer does not refer to the positive electrode active material layer alone. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are all collectively referred to as the positive electrode film layer.

[0144] In this disclosure, the particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EMTIC3XCP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) is used to observe the cut surface of the positive electrode film layer along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the scanning electron microscope, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "runcyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the particle's interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.

[0145] It is understood that the particles in the cross-section of the positive electrode film along the thickness direction, especially those larger than 50 nm, mainly originate from the positive electrode active material. Therefore, the embodiments of this disclosure can accurately and objectively reflect the distribution of lithium transition metal phosphate particles in the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode along the thickness direction.

[0146] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained by Malvern laser diffraction based on the principle of laser scattering often only reflect the particle size of the agglomerates, and cannot accurately reflect the particle size of the positive electrode active material, let alone its dispersion state in the film layer. This is because the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film forming rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, and the number of small particles is higher than the actual value. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this disclosure.

[0147] Based on the total area of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the specific test method for the area proportion of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm is as follows: identify the particles in the positive electrode active material layer with reference to the method described above in the present disclosure, import the image after particle judgment and identification is completed into the ImageJ software for analysis, complete the scale setting according to the scanning electron microscope image, and perform statistical analysis on the particle size, area, spheroidicity and roughness of the particles in the cross-section of the positive electrode active material layer along the direction of the battery cell through the analysis functions of "Feret diameter", "Area", "Round" and "Solidity". According to the software manual (ImageJ User Guide IJ1.46r), the "Feret" parameter obtained by analysis represents the maximum distance between all parallel lines in the two-dimensional projection of the particle, which is used to characterize the particle size of the particle; the obtained "Area" parameter represents the pixel area of the particle. Since particles with a particle size of less than 50nm have large errors in the statistical process and are difficult to identify accurately, and the particle size of the conductive agent is generally less than 50nm, which will cause large errors in the statistical results, therefore, in the particle size statistical process of the present disclosure, particles with a particle size of less than 50nm are not counted, and the statistical data of particles corresponding to AR, Round or Solidity displayed as "NaN" are deleted. Calculate the sum of the "Area" parameters of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm and the sum of the "Area" parameters of all particles, which are respectively taken as the area of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm and the total area of the counted particles. The sum of the areas of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm divided by the total area of the counted particles is taken as the area proportion of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm, based on the total area of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece.

[0148] In some embodiments, based on the total area of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the area proportion of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm may optionally be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, or any numerical range between any two of them.

[0149] In some embodiments, based on the total area of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the area proportion of the particles with the particle size R3 satisfying 1μm < R3 ≤ 5μm can be tested with reference to the test method for "the area proportion of the particles with the particle size R1 satisfying 50nm ≤ R1 ≤ 400nm, based on the total area of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece".

[0150] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1 μm < R3 ≤ 5 μm may be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or any numerical range between any two of them.

[0151] In the present disclosure, the cumulative distribution curve of the graphitization degree C value refers to a curve obtained by arranging at least 100 obtained C values in ascending order, with the graphitization degree as the horizontal axis and the cumulative quantity proportion as the vertical axis. C 50 is the C value corresponding to the cumulative quantity proportion of 50% on the vertical axis in the cumulative distribution curve of the graphitization degree C value. The median C of the graphitization degree 50 can reflect the overall graphitization degree of the particles in the positive electrode film layer compared with a point value; compared with the average value, it can reduce the influence of extreme values in the test process and improve the confidence of the test results.

[0152] The graphitization degree C value of the positive electrode film layer can be obtained by the surface scanning mode of a laser micro-confocal Raman spectrometer. As an example, specifically, a laser micro-confocal Raman spectrometer (high-precision Renishaw laser micro-confocal Raman spectrometer) is used, an excitation wavelength of 532 nm is selected, an appropriate amount of the positive electrode film layer is taken for surface scanning on its surface, the scanning area is 45 μm × 45 μm, which is divided into 10×10 grids, the grid vertices are taken as test points, the step length is 5 μm, and the total number of scanning points is 100, thereby obtaining the C values at different sites and the cumulative distribution curve of C values in the surface scanning area. The positive electrode film layer in the present disclosure may be a freshly prepared positive electrode film layer, or a positive electrode film layer obtained by disassembling from a battery.

[0153] The graphitization degree C value of the positive electrode film layer is obtained by the peak intensity ratio of the G band and the D band of Raman spectrum, and the G band position is 1580±100 cm -1 , which characterizes carbon sp 2 hybrid structure; the D band position is 1350±100 cm - 1 , which characterizes a disordered structure, where disorder means that there is no regular arrangement mode between carbon atoms in the structure. In a graphite crystal, carbon atoms in the same layer form covalent bonds by sp 2 hybridization, and van der Waals forces exist between the layers, so that the carbon with a graphite structure is easy to slip. Therefore, the C value can characterize the graphitization degree of the positive electrode film layer. It can be understood that the graphitization degree in the positive electrode film layer mainly comes from the graphitized carbon material in the positive electrode film layer, that is, the carbon material layer of the positive electrode active material. Although rich in sp 2The carbon nanotube conductive agent with a hybrid structure also has a relatively high I G / I D , but due to its low added content and small tube diameter, its addition in the positive electrode film layer appears as an extreme value in the Raman mapping test of the positive electrode film layer, and will not affect the graphitization degree C 50 of the positive electrode film layer. Therefore, the graphitization degree of the positive electrode film layer can also be used to characterize the graphitization degree of the positive electrode active material.

[0154] Those skilled in the art can realize the regulation of the graphitization degree of the active material particles through any known process. As an example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve the adjustment of the graphitization degree of the active material particles.

[0155] In some embodiments, in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer in the mapping mode of the laser confocal Raman spectrometer, the median C of the graphitization degree 50 can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20 or a numerical range between any two of them.

[0156] In the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm, the particle size concentration (D A90 -D A10 ) / D A50 is calculated specifically as follows. The particles in the cross-section of the positive electrode film layer are identified with reference to the method described above in the present disclosure, and the "Feret" and "Area" analysis functions in ImageJ are used to analyze the morphology of the particles in the cross-section of the positive electrode film layer along the thickness direction of the pole piece. To meet the statistically significant number of samples, no less than 10 scanning electron microscope images are collected for each pole piece, and the particle sizes of no less than 5000 particles with a particle size satisfying 0.4μm<R2≤1μm are counted. The obtained particle sizes of at least 5000 particles are arranged in ascending order, with the particle size as the horizontal axis and the cumulative area proportion calculated from the "Area" of the particles as the vertical axis, to obtain the area cumulative distribution curve of the particles in the positive electrode film layer. D A90 , D A50 , D A10 are respectively the corresponding particle size values when the cumulative proportion of the vertical axis in the area cumulative distribution curve is 90%, 50%, and 10%.

[0157] In the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, or a numerical range between any two of them.

[0158] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 can be 0.5-2.3. Medium-sized particles account for a certain proportion in the total particles. By setting the particle size concentration of medium-sized particles within the above range, it is beneficial to increase the compaction density of the film layer according to the particle gradation principle, and balance the energy density and safety performance of the battery cell.

[0159] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 can be 0.7-1.3. Medium-sized particles account for a certain proportion in the total particles. By setting the particle size concentration of medium-sized particles within the above range, the particle size difference between medium-sized particles is small, the particle deformation is relatively synchronous, the internal extrusion between particles is small, the stress is uniformly dispersed, and the generation of particle cracks can be reduced. At the same time, the particle size concentration will not be too small, and a certain gradation is still retained, so that the compaction density of the positive electrode film layer is balanced, and further the energy density and safety performance of the battery cell are balanced.

[0160] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (D A90 -D A10 ) / D A50 can be 1-2.3. Medium-sized particles account for a relatively high proportion in the total particles. Setting the particle size concentration of medium-sized particles within the above range is beneficial to increase the compaction density of the film layer according to the particle gradation principle, and balance the energy density and safety performance of the battery cell.

[0161] In some embodiments, in the particle size area cumulative distribution curve of particles with a particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross-section of the positive electrode film layer along the thickness direction of the pole piece, the particle size concentration (DA90 -D A10 ) / D A50 is 1.5-2.3.

[0162] In the prior art, to improve compaction density, the proportion of large particles is usually increased to serve as the skeleton of the film layer. Studies of the present disclosure show that during the compaction process of the electrode sheet, large particles are the main load-bearing objects, bridging is prone to occur between large particles during the rolling process, voids and stress concentration are formed at the bridging positions, which causes local fracture of the electrode sheet at the stress concentration positions, damages the conductive network inside the electrode sheet, and even generates isolated particles, leading to an increase in the internal resistance of the battery. The lithium-containing transition metal phosphate used in the present disclosure is a ceramic material. During the high-temperature sintering process of this material, grain boundaries melt and grains grow. The sintering of large particles often requires a higher sintering temperature or a longer sintering time, and undergoes more grain boundary melting, so the spheroidicity of the obtained large particles is relatively low. During the rolling process, bridging is more likely to occur between large particles with poor spheroidicity, which is instead not conducive to the improvement of compaction density. For this reason, more small particles need to be introduced to fill the pores formed by the overlapping of large particles with poor spheroidicity, which will further lead to an increase in the internal resistance of the battery. In the present disclosure, by making the particle size concentration within the above range, multi-level gradation is formed between different particle size levels, the overall particle gradation degree is good, which is beneficial to improving the compaction density of the electrode sheet, and further improving the energy density without deteriorating the ohmic internal resistance, which is conducive to balancing the safety performance.

[0163] In some embodiments, when the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 90 μm-120 μm.

[0164] In some embodiments, when the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 100 μm-120 μm.

[0165] The single-side thickness of the positive electrode film layer within the above range helps to further increase the loading amount of the active material on the electrode sheet and improve the energy density of the battery. However, after the loading amount of the active material increases, the heat generation of the electrode sheet intensifies. In the embodiments of the present disclosure, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with the particle size R1 satisfying 50nm≤R1≤400nm is 20%-40%, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with the particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 30%, and in the cumulative distribution curve of the graphitization degree C value obtained in the surface scanning mode of the laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 0.95-1.20, and in the particle size area cumulative distribution curve of particles with the particle size R2 satisfying 0.4μm<R2≤1μm obtained from the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the particle size concentration (D A90 -DA10 ) / D A50 is less than or equal to 2.3, in particular, the particle size concentration degree (D A90 -D A10 ) / D A50 is in the range of 1.5-2.3, which is especially suitable for battery cells with a single-side thickness of the positive electrode film layer within the above range, and helps to achieve high energy density while taking into account safety performance.

[0166] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm may be greater than or equal to 25%. Accordingly, medium-sized particles account for a certain proportion in the total particles, which helps to increase the compaction density of the film layer according to the particle gradation principle, and take into account both the energy density and safety performance of the battery cell.

[0167] Exemplarily, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm may be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 67%, 70% or any numerical range between the two values.

[0168] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm may be 25%-70%. Accordingly, medium-sized particles account for a relatively high proportion in the total particles, which helps to increase the compaction density of the film layer according to the particle gradation principle, and take into account both the energy density and safety performance of the battery cell.

[0169] In some embodiments, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm may be 40%-70%. Accordingly, medium-sized particles account for a relatively high proportion in the total particles, which helps to increase the compaction density of the film layer according to the particle gradation principle, and take into account both the energy density and safety performance of the battery cell.

[0170] In the present disclosure, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm is obtained as follows: there are substantially no particles with a particle size greater than 5μm in the positive electrode film layer, and as mentioned above, particles with a particle size less than 50nm are not counted in the particle size statistics process of the present disclosure. Therefore, the area proportion of particles with a particle size R2 satisfying 0.4μm<R2≤1μm in the present disclosure is calculated by subtracting the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm and the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm.

[0171] In some embodiments, based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is 25%-35%.

[0172] When the area proportion of particles with a particle size satisfying 50nm≤R1≤400nm falls within the above range, it helps reduce the contact area between particles, lower the ohmic internal resistance of the electrode sheet, and at the same time give consideration to the particle gradation in the positive electrode film layer and the compaction density, so as to balance the energy density and safety performance of the battery.

[0173] In some embodiments, based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 20%.

[0174] In some embodiments, based on the total area of particles in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is 10%-20%.

[0175] When the area proportion of particles with a particle size satisfying 1μm<R3≤5μm falls within the above range, it helps further reduce the polarization internal resistance, lower the heat generation of the electrode sheet, so as to further improve the safety performance of the battery.

[0176] In some embodiments, in the cumulative distribution curve of the graphitization degree C value obtained in the surface scanning mode of a laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 1.01-1.13.

[0177] When the median graphitization degree of the positive electrode film layer falls within the above range, it helps further increase the electronic conductivity of the particle surface, reduce the ohmic internal resistance of the electrode sheet, lower the heat generation of the electrode sheet, and further improve the safety performance of the battery.

[0178] In some embodiments, under the fully discharged state of the battery cell, the compaction density of the positive electrode sheet is 2.3g / cm 3 -2.6g / cm 3 .

[0179] In this disclosure, the compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of ​​S. The mass of the circular pieces is obtained as W1, and the thickness T1 of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness T2 of the current collector is measured using a high-precision micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].

[0180] In some embodiments, the compaction density of the positive electrode sheet of the battery cell in its fully discharged state can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.40 g / cm 3 2.41 g / cm 3 2.42 g / cm 3 2.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.50g / cm 3 2.52g / cm 3 2.55g / cm 3 2.6g / cm 3 Or the range of values ​​between any two.

[0181] The compaction density of the positive electrode sheet is within the above range, which helps to increase the loading of active material per unit volume and improve the energy density of the battery cell.

[0182] In some embodiments, the porosity of the positive electrode film layer in a cross-section along the thickness direction of the electrode sheet is 14%-28%.

[0183] In this disclosure, the porosity of the positive electrode film layer can be tested in the following way. Import the cross-sectional scanning electron microscope (SEM) image of the positive electrode film layer along the electrode thickness direction obtained as described above into ImageJ software. Select the line tool and use a line to mark the length of the scale bar in the image. Click "Analyze Set Scale" and set the scale parameters in the software according to the scale bar length in the image. Select the rectangle tool and select the part of the image outside the scale bar area. Use "Image Duplicate" to copy the selected area and use "Image Type 8bit" to adjust the image format. Select "Analyze Set Measurements" and choose the following five options: "Area", "Mean gray value", "Area Fraction", "Limit to threshold", and "Feret's diameter". Select 3 for "Decimal places". Then, select "Image" - "Adjust" - "Threshold" sequentially, and set 0 and 100 to the selected positions in the "Threshold" box. The pore data from the cross-sectional SEM image can then be exported using the Analyze-Measure function. Export using "Image" - "Overlay" - "Flatten" to obtain a pore image; click "Apply" in "Threshold", then click "Analyze" - "Analyze Particles", check the four columns on the left to obtain pore statistics.

[0184] It is understood that in this embodiment of the disclosure, "pores" in the cross-section of the positive electrode film are identified through image color difference and threshold. These "pores" are not the pore data obtained from the degassing test, but are mainly used to characterize the gaps between particles in the cross-section of the positive electrode film. This method is superior to the degassing method because the porosity obtained by the degassing method is related to the pores between particles and the pores in the carbon material layer on the particle surface, and cannot objectively reflect the pores between particles.

[0185] In some embodiments, the porosity of the positive electrode film can be selected as 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or any value range between the two.

[0186] When the porosity of the positive electrode film is within the above range, the positive electrode film has good electrolyte wettability and tortuosity, which helps the diffusion of lithium ions in the liquid and solid phases, helps reduce concentration polarization of thick electrodes, reduces electrode heat generation, and improves battery safety performance.

[0187] In some implementations, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 0.3-0.6, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0188] The cumulative distribution curve of the coating value (B-value) is obtained by arranging at least 100 B-values ​​in ascending order, with the coating value on the horizontal axis and the cumulative percentage on the vertical axis. To reduce the influence of extreme coating values ​​caused by non-particle regions in the positive electrode film on the test results, the median coating value (B-value) is used. 50 Evaluate the density of the carbon material layer on the positive electrode active material. B 50 The B value is the value corresponding to the cumulative number of values ​​on the vertical axis of the cumulative distribution curve of the coverage value B value when the cumulative number accounts for 50%.

[0189] In this disclosure, the coating value (B-value) of the positive electrode film can be obtained by scanning with a laser confocal microscopy (LCM) spectrometer. Specifically, a high-precision Renishaw laser confocal microscopy (LCM) spectrometer is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is scanned across its surface. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. This yields the B-values ​​at different sites and the cumulative distribution curve of the B-values ​​across the scanned area. The positive electrode film in this disclosure can be either freshly prepared or obtained from disassembly of a battery.

[0190] The coating value B of the positive electrode film was obtained by the ratio of the peak intensities of the P-band and D-band in the Raman spectrum, with the P-band located at 948±100 cm⁻¹. -1 Its characterization of phosphate PO4 3- Structure; D peak position is 1350±100cm -1 The characterization of the structure is based on disorder, where disorder refers to the irregular arrangement of carbon atoms within the structure. During the testing process, an excitation wavelength of 532 nm was selected, resulting in a shallow testing depth. Consequently, in the test results obtained using laser microscopy confocal Raman spectroscopy in surface scanning mode, the carbon structure peak exhibited a higher intensity compared to the phosphate structure peak.

[0191] Those skilled in the art can control the coating value of active material particles using any known process. For example, adjusting the carbon source type, carbon source addition amount, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the coating value of the active material particles. The coating value (B-value) reflects the density of the carbon material layer on the surface of lithium transition metal phosphate particles. The denser the carbon material layer, the lower the relative intensity of the phosphate structure detected in the Raman spectrum, and the smaller the coating value (B-value) of the cathode film.

[0192] In some implementations, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, or any value range between the two.

[0193] Poor coating density of the positive electrode film increases the electron transport path within the coating layer, leading to increased internal resistance and heat generation in the electrode. The median coating value B of the positive electrode film... 50 Within the above range, it is evident that the carbon material layer of the positive electrode active material is relatively dense and uniform, which helps to reduce the internal resistance of the electrode, reduce the heat generation of the electrode, and improve the safety performance of the battery.

[0194] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-2.5% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0195] In this disclosure, the area ratio of the conductive agent agglomeration region, based on the total area of ​​the cross-section of the positive electrode film along the electrode thickness direction, can be tested using the following method. A cross-section of the positive electrode film along the electrode thickness direction is observed using a scanning electron microscope (SEM) with a similar method as described above. The area of ​​the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since the conductive agent is generally a carbon-based material, such as conductive carbon black or carbon nanotubes, aggregated conductive agent can be seen under high magnification in the SEM. The conductive agent agglomeration region often appears black and agglomerated compared to other areas in the positive electrode film. Using image analysis software, the conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Specifically, the scanning electron microscope (SEM) images at 3kx magnification are imported into ImageJ. Black conductive agent agglomeration regions with a Feret value greater than or equal to 2μm are selected, and the sum of the areas of these selected regions is recorded as the area of ​​the conductive agent agglomeration region. The area ratio of the conductive agent agglomeration region is the ratio of its area to the total area of ​​the imported SEM images. Three randomly selected, non-overlapping SEM images are used, and the average of these ratios is calculated as the "area ratio of the conductive agent agglomeration region based on the total area of ​​the cross-section along the electrode thickness direction of the positive electrode film."

[0196] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area percentage of the agglomerated region of the conductive agent can be selected from 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two, based on the total area of ​​the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0197] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomerated region of the conductive agent is within the above range, indicating that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network. This is especially beneficial for improving the electron transport rate of the thick coating film in the thickness direction of the electrode sheet, thereby reducing the internal resistance of the electrode sheet, reducing the heat generation of the electrode sheet, and improving the safety performance of the battery.

[0198] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-1.7% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0199] In this embodiment, the area ratio of the agglomerated region of the conductive agent is further within the above-mentioned range, indicating that the conductive agent is more uniformly distributed in the positive electrode film layer and the content of the conductive agent is low. While reducing the internal resistance of the electrode, the conductive agent content is not excessive, reducing the space occupied by the positive electrode active material, thereby balancing the energy density and safety performance of the battery.

[0200] In some implementations, the range of the area ratio of conductive agent agglomeration regions in a cross section along the thickness direction of the positive electrode sheet is less than or equal to 2%.

[0201] In this disclosure, the range of the area ratio of the conductive agent agglomeration region in a cross section along the thickness direction of the positive electrode sheet can be tested by the following method: referring to the above-mentioned test method for the area ratio of the conductive agent agglomeration region based on the total area of ​​the cross section along the thickness direction of the positive electrode film, five non-overlapping scanning electron microscope images are randomly selected, and the area ratio of the conductive agent agglomeration region is calculated for each image. The range of the five values ​​obtained is taken as the "range of the area ratio of the conductive agent agglomeration region in a cross section along the thickness direction of the positive electrode sheet", where the range refers to the difference between the maximum and minimum values ​​in a set of data.

[0202] In some embodiments, the range of the area percentage of the conductive agent agglomeration region in the cross-section along the thickness direction of the positive electrode sheet can be selected as 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any value range between the two.

[0203] In some implementations, the area ratio of conductive agent agglomeration regions in a cross-section along the thickness direction of the positive electrode sheet varies from 0% to 1%.

[0204] If the range of the area ratio of conductive agent agglomeration regions in the cross section along the thickness direction of the positive electrode sheet is within the above range, it indicates that the conductive agent is uniformly dispersed in the positive electrode film layer, which is conducive to forming a uniform conductive network. This is especially beneficial to improving the electron transport rate of the thick coating film layer in the thickness direction of the electrode sheet, thereby reducing the internal resistance of the electrode sheet, reducing the heat generation of the electrode sheet, and improving the battery safety performance.

[0205] In some embodiments, the conductive agent includes carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.

[0206] In this disclosure, the term "carbon nanotube" refers to a structure composed of carbon atoms arranged in sp... 2A nanomaterial consisting of several to dozens of coaxial hollow circular tubes formed by rolling graphene sheets connected by hybrid bonds. Its diameter generally ranges from several nanometers to tens of nanometers, and its length can vary from micrometers to centimeters, presenting a high aspect ratio. According to the number of graphene sheets, it can be divided into: Single-walled Carbon nanotubes (SWCNTs), Few-walled Carbon Nanotubes (FWCNTs) and Multi-walled Carbon nanotubes (MWCNTs). Carbon nanotubes have excellent electrical conductivity and high elastic modulus.

[0207] Due to the one-dimensional structure of carbon nanotubes, they can form a network structure in the positive electrode film layer. The excellent electrical conductivity of carbon nanotubes enables their network structure to become an efficient electron transport channel, which helps to further improve the electron transport rate of the thick coated film layer in the thickness direction of the pole piece, thereby reducing the ohmic internal resistance of the battery, reducing heat generation, and improving the safety performance of the battery.

[0208] In some embodiments, the conductive agent further includes conductive carbon black.

[0209] Conductive carbon black has a high specific surface area, and thus has good liquid retention capacity. The expansion force of the thick pole piece during the cycle process is large, which makes the electrolyte easy to be squeezed out. The distribution of conductive carbon black in the positive electrode film layer is beneficial to improve the liquid retention capacity of the thick pole piece, reduce the polarization internal resistance of the battery, reduce heat generation, and improve the safety performance of the battery.

[0210] In some embodiments, the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0211] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, which leads to uneven dispersion in the positive electrode film layer and fails to form an effective carbon nanotube network structure. The surface energies of conductive carbon black and carbon nanotubes are relatively close, and conductive carbon black can adsorb on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce the direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. This helps to further reduce the ohmic internal resistance of the battery, reduce heat generation, and improve the safety performance of the battery.

[0212] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.

[0213] In some embodiments, based on the mass of the positive electrode film, the mass content C1 of carbon nanotubes can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0214] In some embodiments, based on the mass of the positive electrode film, the mass content C2 of conductive carbon black can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0215] When the mass content of carbon nanotubes and conductive carbon black is within the above range, it can effectively alleviate the agglomeration of carbon nanotubes and form a good conductive network structure, thereby reducing ohmic internal resistance. At the same time, it helps to improve the liquid retention rate of the positive electrode during long-cycle processes, further reduce polarization internal resistance, reduce battery heat generation, and improve battery safety performance.

[0216] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector. The undercoat layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.

[0217] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector, and the thickness of the undercoat layer is 0.5 μm-5 μm.

[0218] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector. The thickness of the undercoat layer can be selected from 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2... 0.5μm, 2.6μm, 2.7μm, 2.8μm, 2.9μm, 3.0μm, 3.1μm, 3.2μm, 3.3μm, 3.4μm, 3.5μm, 3.6μm, 3.7μm, 3.8μm, 3.9μm, 4.0μm, 4.1μm, 4.2μm, 4.3μm, 4.4μm, 4.5μm, 4.6μm, 4.7μm, 4.8μm, 4.9μm, 5μm, or any range of values ​​between two of these.

[0219] Compared to the direct contact between the positive electrode current collector and the positive active material layer, the undercoating layer provided in this embodiment has an increased contact area with the positive electrode film layer. This helps to increase the area of ​​electron transport between the current collector and the positive electrode film layer, thereby reducing the internal resistance of the electrode, reducing heat generation, and improving the safety performance of the battery.

[0220] In some implementations, the size of the positive current collector is 12μm-16μm along the thickness direction of the positive electrode sheet.

[0221] In this disclosure, the dimensions of the positive current collector can be tested using methods and instruments known in the art. As an example, a high-precision micrometer (e.g., a Mitutoyo 293-100 model with an accuracy of 0.1 μm) can be used for testing.

[0222] In some embodiments, the size of the positive electrode current collector along the thickness direction of the positive electrode sheet can be 12 μm, 12.1 μm, 12.2 μm, 12.3 μm, 12.4 μm, 12.5 μm, 12.6 μm, 12.7 μm, 12.8 μm, 12.9 μm, 13 μm, 13.1 μm, 13.2 μm, 13.3 μm, 13.4 μm, 13.5 μm, 13.6 μm, 13.7 μm, 13.8 μm, 13.9μm, 14μm, 14.1μm, 14.2μm, 14.3μm, 14.4μm, 14.5μm, 14.6μm, 14.7μm, 14.8μm, 14.9μm, 15μm, 15.1μm, 15.2μm, 15.3μm, 15.4μm, 15.5μm, 15.6μm, 15.7μm, 15.8μm, 15.9μm, 16μm, or any range between two of these values.

[0223] The thickness of the positive electrode current collector is within the above range, which helps to increase the cross-sectional area for current transmission within the current collector, thereby reducing the resistance of the current collector, reducing heat generation on the electrode, and helping to improve the safety performance of the battery.

[0224] In some implementations, the size of the positive current collector is 13μm-15μm along the thickness direction of the positive electrode sheet.

[0225] If the positive electrode current collector is too large, it will affect the energy density of the battery. In the embodiments of this disclosure, the thickness of the positive electrode current collector is within the above range, which helps to balance the energy density, toroidal performance and safety performance of the battery.

[0226] In some embodiments, the resistivity of the positive electrode film is 5 Ω·cm - 35 Ω·cm

[0227] The resistivity of the positive electrode film can be tested using the following method: A resistance meter (e.g., Suzhou Lidian) is used to test the positive electrode sheet with a single-sided positive electrode film under a standard pressure of 25 MPa. If the positive electrode sheet has a double-sided positive electrode film, one side of the film is wiped off before testing. During the test, eight test points are randomly selected on the film of the positive electrode sheet with a single-sided positive electrode film. Pressure is maintained at each test point for 15 seconds to obtain the resistivity at that test point. The average of the eight resistivities is recorded as ρ1, and the thickness of the positive electrode sheet with a single-sided positive electrode film is measured and recorded as T1. The positive electrode film on the positive current collector is wiped off, and the above test steps are repeated to obtain the resistivity ρ2 of the positive current collector. The thickness of the positive current collector is measured and recorded as T2. The resistivity of the positive electrode film is calculated as: [(ρ1×T1)-(ρ2×T2)] / (T1-T2).

[0228] In some embodiments, the resistivity of the positive electrode film can be selected as 5 Ω·cm, 6 Ω·cm, 7 Ω·cm, 8 Ω·cm, 9 Ω·cm, 10 Ω·cm, 11 Ω·cm, 12 Ω·cm, 13 Ω·cm, 14 Ω·cm, 15 Ω·cm, 16 Ω·cm, 17 Ω·cm, 18 Ω·cm, 19 Ω·cm, 20 Ω·cm, 21 Ω·cm, 22 Ω·cm, 23 Ω·cm, 24 Ω·cm, 25 Ω·cm. m, 26Ω·cm, 27Ω·cm, 28Ω·cm, 29Ω·cm, 29.72Ω·cm, 29.88Ω·cm, 30Ω·cm, 30.55Ω·cm, 30.73Ω·cm, 31Ω·cm, 31.5Ω·cm, 32Ω·cm, 32.2Ω·cm, 33Ω·cm, 33.67Ω·cm, 34Ω·cm, 34.98Ω·cm, 35Ω·cm, or any range of values ​​between two of these.

[0229] If the resistivity of the positive electrode film is within the above range, it indicates that the positive electrode film has low internal resistance, which helps to reduce heat generation on the electrode and improve the safety performance of the battery.

[0230] In some embodiments, the lithium transition metal phosphate particles comprise components represented by the following general formula:

[0231] Li m Fe x P y O j Q q Formula I,

[0232] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.

[0233] In some implementations, m can be selected as 0.8, 0.85, 0.9, 0.95, 0.98, 1.00, 1.03, 1.05, 1.08, 1.10, 1.13, 1.15, or any value range between two of these; x can be selected as 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, or any value range between two of these. y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00 or any value between two of these; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value between two of these; q can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any value between two of these.

[0234] In some embodiments, the lithium-containing transition metal phosphate particles include one or more of lithium iron phosphate, lithium manganese phosphate, lithium fluorinated vanadium phosphate, lithium manganese iron phosphate, and their modified materials.

[0235] In some embodiments, the lithium-containing transition metal phosphate particles include one or more of lithium iron phosphate and its doped and modified materials, and coated and modified materials.

[0236] In some embodiments, the lithium transition metal phosphate particles include titanium, and the titanium content is 500ppm-8000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0237] The types and contents of elements in lithium transition metal phosphate particles can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the elemental composition and content of titanium, referring to Appendix C of GB / T 33822-2017.

[0238] In some embodiments, the lithium transition metal phosphate particles include titanium, and the mass content of titanium, based on the total mass of the lithium transition metal phosphate particles in the positive electrode film, can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, etc. ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, or any range of two.

[0239] In some embodiments, the lithium transition metal phosphate particles include titanium, and the mass content of titanium is 1000ppm-3000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0240] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate raw material reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increasing polarization resistance. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the cathode active material is reduced. This allows the cathode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing the internal resistance of the electrode, reducing heat generation, and improving battery safety performance.

[0241] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and further reducing the internal resistance of the electrode. Furthermore, the uneven diffusion of lithium ions in thick coated films often results in a significant lithium-ion concentration gradient. This disclosure improves the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thereby reducing the polarization resistance of thick electrodes and mitigating the heat generation problem in thick electrode batteries.

[0242] In some embodiments, the lithium transition metal phosphate particles include vanadium, and the vanadium content is 500 ppm to 5000 ppm based on the total mass of the lithium transition metal phosphate particles in the cathode film.

[0243] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) is used to test the vanadium content, referring to Appendix C of GB / T 33822-2017.

[0244] In some embodiments, the lithium transition metal phosphate particles include vanadium. Based on the total mass of the lithium transition metal phosphate particles in the positive electrode film, the mass content of vanadium can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, or 5000ppm.

[0245] In some embodiments, the lithium transition metal phosphate particles include vanadium, and the vanadium content is 500ppm-3000ppm based on the total mass of the lithium transition metal phosphate particles in the cathode film.

[0246] Vanadium in the positive electrode film can be in multiple valence states, including +5 vanadium (V5). 5+ Vanadium (V+3) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expand the diffusion channels of lithium ions, thereby improving the ionic conductivity of the positive electrode active material and reducing the internal resistance of the battery; vanadium (V+3) 3+Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material and reducing the ohmic internal resistance of the battery. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further reduce the internal resistance of the positive electrode film and improve the uniformity of the positive electrode film reaction, thus further enhancing the battery's safety performance.

[0247] Within the aforementioned mass content range, vanadium helps reduce the internal resistance of the positive electrode and decreases heat generation in thick-coated lithium transition metal phosphate batteries. Simultaneously, the synergistic effect of titanium, vanadium, and carbon nanotubes in the positive electrode film helps form a robust three-dimensional network, further enhancing the electronic and ionic conductivity of the positive electrode film, reducing internal resistance, and thus further improving the safety performance of thick-coated lithium transition metal phosphate batteries.

[0248] In some embodiments, the battery cell further includes a separator 20 disposed between the positive electrode and the negative electrode. The separator 20 includes a base film 201, a ceramic layer 202 disposed on at least one side of the base film 201, and an adhesive layer 203 disposed on the side of the ceramic layer 202 away from the base film 201. The adhesive layer 203 is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

[0249] In some embodiments, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film.

[0250] Placing ceramic layers on both sides of the base film helps improve the rigidity of the pouch cell.

[0251] In some embodiments, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on the ceramic layers on the sides away from the base film.

[0252] In some embodiments, the vinylidene fluoride polymer includes one or more of polyvinylidene fluoride (PVDF) and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP).

[0253] In some embodiments, vinylidene fluoride polymers include polyvinylidene fluoride (PVDF).

[0254] In the prior art, the adhesive layer of the separator usually uses aqueous PVDF, which presents an island-like structure in the separator, as shown in Figure 3. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing; however, such a separator adhesive layer has a small contact area with the electrode and weak adhesion.

[0255] The separator provided in this embodiment uses a continuous porous layer as the adhesive layer, as shown in Figures 2 and 4. Compared with the adhesive layer in the prior art, it has a larger bonding area with the electrode, which makes the bonding between the separator and the electrode more firm and uniform. This helps to reduce the spacing between the electrodes, reduce impedance, alleviate heat generation, and improve the safety performance of the battery.

[0256] It is understood that the continuous adhesive layer may break and deform into a blocky structure during electrode manufacturing or cycling due to contact with or compression stress on the positive or negative electrode. The continuous structure referred to in this disclosure means that at the microscopic level, such as under a scanning electron microscope or optical microscope, the adhesive layer of the separator is continuous. To reflect the true morphology of the separator, during sampling, it is preferable to sample in areas of the battery where the separator's adhesive layer is not bonded to the positive or negative electrode. For example, sampling can be performed at locations beyond the positive and negative electrode; or sampling can be performed near the surface of the electrode assembly. This sampling area has less adhesion to the positive or negative electrode, providing a better reflection of the separator's true state.

[0257] In some embodiments, the battery cell includes a stacked cell, which includes the aforementioned positive electrode and negative electrode.

[0258] Compared to wound cells, stacked cells have less compression between the separator and the electrodes, resulting in a relatively larger gap between the electrodes. This increases the battery's internal resistance and heat generation. Furthermore, it can lead to the positive and negative electrodes bridging each other, increasing the risk of internal short circuits within the cell. Therefore, the separator provided in this disclosure is particularly suitable for stacked cells. The increased adhesion between the porous adhesive layer and the electrodes helps reduce the distance between the positive and negative electrodes, reducing heat generation, and also helps reduce the risk of short circuits caused by electrode bridging, thereby improving battery safety performance.

[0259] In some embodiments, the base film may be made of one or more of the following materials, including but not limited to glass fiber, nonwoven fabric, polyethylene (PE), and polypropylene (PP).

[0260] In some embodiments, the ceramic layer includes one or more of alumina (Al2O3), zirconium oxide (ZrO2), titanium oxide (TiO2), silicon oxide (SiO2), and boron nitride (BN).

[0261] Ceramic particles possess flame retardancy and high hardness, making them resistant to deformation under heat and exhibiting excellent dimensional stability. The low thermal conductivity of ceramic materials further prevents certain thermal runaway points in the battery from expanding into overall thermal runaway, thereby improving the safety performance of individual battery cells.

[0262] In some implementations, the thickness of the base membrane in the diaphragm is 7-9 μm.

[0263] In some embodiments, the thickness of the base film in the diaphragm can be selected as 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or any value range between the two.

[0264] In some embodiments, the thickness of the ceramic layer in the diaphragm is 2-4 μm on one side.

[0265] In some embodiments, the thickness of the ceramic layer on one side of the diaphragm can be selected as 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or any value range between the two.

[0266] In some embodiments, the thickness of the adhesive layer on one side of the diaphragm is 1-5 μm.

[0267] In some embodiments, the thickness of the adhesive layer on one side of the diaphragm can be selected as 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value range between the two.

[0268] If the adhesive layer is too thin, the adhesion between the separator and the electrode is weak. On the one hand, the spacing between the positive and negative electrodes is larger, increasing the battery impedance and heat generation; on the other hand, the probability of a short circuit due to positive-negative electrode overlap increases, thus affecting the battery's safety performance. If the adhesive layer is too thick, it occupies a large amount of battery space, thus affecting the battery's volumetric energy density. In the embodiments of this disclosure, the thickness of the adhesive layer is within the above-mentioned range, which helps to balance the battery's safety performance and volumetric energy density.

[0269] In some embodiments, the battery cell further includes a housing, in which the stacked cells are housed, and the housing includes a pouch material, which includes an aluminum-plastic composite film.

[0270] In some embodiments, the flexible packaging material includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.

[0271] Soft-pack materials have high elongation, resulting in thinner and more flexible casings that improve space utilization of individual battery cells, thereby increasing their energy density. Furthermore, aluminum's high barrier properties effectively reduce the penetration of water and oxygen into the battery, decreasing electrolyte decomposition and electrode material oxidation, thus extending battery life.

[0272] In some embodiments, the housing includes a first receiving portion and a second receiving portion, the first receiving portion and the second receiving portion being integrally connected and disposed opposite to each other, and the stacked battery cell being received within the receiving cavity formed by the first receiving portion and the second receiving portion.

[0273] The increased loading of active material in thickly coated electrodes exacerbates the expansion of the cell during charging and discharging. With the expansion and contraction of the cell, the base of the tabs and the solder joints are subjected to repeated tensile-compressive-shear stresses, which easily lead to fatigue deformation and increased internal resistance. In this embodiment, the battery cell housing includes a first receiving portion and a second receiving portion. Compared to a structure with only one receiving portion, the two receiving portions place the base of the tabs and the solder joints in a more symmetrical stress environment, helping to disperse stress concentration, slowing down the rate of increase in resistance in this area, and thus extending the cycle life of the battery.

[0274] In some embodiments, referring to FIG1, the housing 50 includes a first sealing area 51, which is disposed at at least one end of the laminated cell extending along a second direction (Y direction); the first sealing area 51 includes a folded edge structure extending along a first direction (X direction), and encapsulating adhesive is disposed on the folded edge structure, which is continuously disposed along the first direction (X direction) and fixes the folded edge structure.

[0275] A folded edge structure refers to a reinforced structure formed by folding the encapsulation area in half. There is no limit to the number of folds. As an example, it can be a single folded edge structure with one fold or a double folded edge structure with folds on both sides.

[0276] During electrode cycling, the SEI film thickens, leading to significant rebound and gas generation during long cycles. This is especially true in thickly coated electrodes, where increased active material loading results in increased rebound, gas generation, and heat generation. Furthermore, increased gas generation exacerbates side reactions, further increasing gas production. The sealing area of ​​the pouch cell is used to seal the electrode assembly; however, the sealing area has limited strength and is easily breached by large rebounds and high gas generation within the film layer.

[0277] This embodiment further enhances the sealing strength of the first sealing area by including a folded edge structure extending along a first direction. The continuous arrangement of the encapsulating adhesive along the first direction and the fixing of the folded edge structure, compared to a discontinuous arrangement of the encapsulating adhesive along the first direction, further improves the sealing strength, achieving continuous reinforcement of the sealing area in the first direction and reducing the probability of the electrode breaking open the sealing area in the packaging during cycling.

[0278] In some embodiments, the housing 50 includes at least one second sealing region 52, which is disposed at at least one end of the laminated cell along a first direction of the housing, and the second sealing region 52 is disposed on the tab side of the laminated cell.

[0279] It is understandable that the positive and negative electrodes can be located on the same side of the laminated cell, as shown in Figure 1; or they can be located on opposite sides of the laminated cell.

[0280] In some embodiments, the battery cell 5 further includes a lead 53 connected to the tab of the battery cell. For example, the lead 53 can be soldered to the tab. The lead 53 is a conductive element, and at least a portion of the lead 53 is located outside the housing 50. The lead 53 serves as the electrode lead-out end of the battery cell 5 and facilitates electrical connection between the battery cell 5 and other battery cells 5 or other components. For example, the lead 53 can be in the form of a sheet.

[0281] Correspondingly, lead-out element 53 also includes a positive lead-out element and a negative lead-out element, with the positive lead-out element connected to the positive electrode tab and the negative lead-out element connected to the negative electrode tab.

[0282] The second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the shell material is relatively weak, which makes it easy for gas to escape from the second sealing area. This is conducive to directional pressure relief of the battery, reducing the impact on adjacent cells during thermal runaway, and improving the overall service life of the battery.

[0283] In some embodiments, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in a second direction, and the rubber rings that surround in the second direction are spaced apart in a first direction.

[0284] The rubber rings that surround the cell in the second direction are spaced apart in the first direction, which helps to fix the position between the electrodes in the cell and reduce the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large size in the first direction. It can effectively reduce the mutual displacement between the electrodes in the first direction, thus reducing lithium plating. It helps to maintain the stability of the internal spatial structure of the battery and thus does not affect the normal operation of the battery.

[0285] In some embodiments, the dimension of the casing in the length direction of the battery cell is L1, the dimension of the casing in the width direction of the battery cell is W1, and the dimension of the casing in the thickness direction of the battery cell is H1, wherein 450mm≤L1≤1300mm, 100mm≤W1≤150mm, and 14mm≤H1≤22mm.

[0286] In some implementations, L1 can be selected as 450mm, 480mm, 490mm, 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, 1300mm, or any value range between the two.

[0287] In some implementations, W1 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two.

[0288] In some implementations, H1 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two.

[0289] In some embodiments, the dimension of the casing along the length of the battery cell is L1, where 450mm ≤ L1 ≤ 650mm.

[0290] When the length dimension L1 of the casing satisfies 450mm≤L1≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance and the safety performance of the battery.

[0291] In some embodiments, the dimension of the casing along the length of the battery cell is L1, where 900mm ≤ L1 ≤ 1300mm.

[0292] When the length dimension L1 of the casing satisfies 900mm≤L1≤1300mm, the battery cell is relatively long, which helps to reduce the volume ratio of the casing in the battery cell and increase the load ratio of active materials. At the same time, a longer battery cell can reduce the number of batteries required in the battery module, simplify the structural design of the battery module, reduce the number and complexity of structural components in the module, thereby improving the space utilization of the battery pack and thus helping to improve the volumetric energy density of the battery cell.

[0293] In some embodiments, at 25°C, the capacity of the battery cell is 95Ah-300Ah, optionally 150Ah-190Ah.

[0294] In this disclosure, the capacity of a single battery cell has a meaning known in the art and can be tested using methods known in the art. As an example, at 25°C, the battery cell is charged to 3.65V at a charging rate of 0.5C (the nominal capacity of the single cell), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity C during the discharge process is calculated using the formula C = I × t, with the unit being Ah.

[0295] In some embodiments, at 25°C, the capacity of the battery cell can be selected as 95Ah, 100Ah, 125Ah, 130Ah, 135Ah, 140Ah, 145Ah, 150Ah, 155Ah, 160Ah, 165Ah, 170Ah, 175Ah, 180Ah, 185Ah, 190Ah, 300Ah, or any value range between the two.

[0296] A second aspect of this disclosure provides a battery device including the battery cell provided in the first aspect of this disclosure.

[0297] The battery device disclosed in this embodiment can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0298] A third aspect of this disclosure provides an electrical device that uses a battery as a power source, the electrical device including at least one of a battery cell, a battery module, or a battery pack provided in this disclosure. The battery cell, battery module, or battery pack can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The battery cell, battery module, or battery pack can be selected as the electrical device according to its usage requirements.

[0299] Figure 5 illustrates an example electrical device. The electrical device disclosed in this embodiment can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this disclosure, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's drive power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.

[0300] The fourth aspect of this disclosure provides an energy storage device that uses a battery device as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.

[0301] Example

[0302] The following describes embodiments of this disclosure. The embodiments described below are exemplary and are only used to explain this disclosure, and should not be construed as limiting this disclosure. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0303] Example 1

[0304] (1) Preparation of positive electrode active material

[0305] S1: Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, sucrose, glucose and polyethylene glycol are added to deionized water and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate is such that the molar ratio of lithium to iron is 1.02:1.0. Based on the total mass of the mixed raw materials, the mass content of sucrose is 2%, the mass content of glucose is 4%, and the mass content of polyethylene glycol is 5%. After mixing evenly, a mixed raw material with a solid content of 38% is obtained.

[0306] Among them, the particle size D of lithium carbonate V50 The particle size is 6 μm; the morphology of the iron phosphate particles is spherical; both titanium dioxide and vanadium pentoxide are nanoparticles; the purity of sucrose is ≥98%; the moisture content of glucose is <0.5%; and the weight average molecular weight of polyethylene glycol is 1500.

[0307] S2: The mixed raw materials are ground twice in a sand mill, first coarsely for 1 hour and then finely ground. During the grinding process, the slurry temperature is controlled to be less than 40 degrees Celsius to obtain a mixed slurry; the particle size D of the solid particles in the mixed slurry is... V50 The particle size was 0.80 μm. Spray drying was performed to obtain a dried precursor powder. After drying, its particle size D... V50 It is 55.50 μm.

[0308] S3: The precursor powder is subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature is increased from 25℃ to 460℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature is increased from 460℃ to 780℃ at a heating rate of 5℃ / min (second heating stage), and held for 12 hours; the air volume in the heating stage is greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air volume is 1350 cm³. 3 / h, after which cooling is completed; particle size D is obtained by airflow pulverization. V50 The positive electrode active material of lithium iron phosphate has a carbon material on its surface of 1.6 μm. The total mass of the positive electrode active material has a Ti element content of 1050 ppm and a V element content of 950 ppm.

[0309] The above D V50 This refers to data obtained through the Malvern laser scattering method.

[0310] (2) Preparation of positive electrode sheet

[0311] The above-mentioned positive electrode active material (95.3% by mass), conductive agent (0.6% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone. Then, dispersant HNBR (1.1% by mass) was added, and the mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (0.4% by mass) and carbon nanotubes (0.2% by mass), and the specific surface area of ​​the conductive carbon black was 85 m². 2 / g, oil absorption value of 200ml / 100g, average length of carbon nanotubes of 25μm, specific surface area of ​​300m² 2 / g, the mass content of metal impurities in carbon nanotubes is <1wt%.

[0312] The positive electrode slurry was coated onto an aluminum foil with a thickness of 13 μm by extrusion, dried, and then cold-pressed to obtain the positive electrode sheet.

[0313] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0314] In the cross-section along the thickness direction of the positive electrode sheet, the area ratio of the conductive agent agglomeration region is 1.47%, and the range of the area ratio of the conductive agent agglomeration region is 1.5%. In the cumulative distribution curve of the coating value B obtained by laser microscopy confocal Raman spectroscopy under surface scanning mode, the median coating value B... 50 The density of the positive electrode film is 0.51; the single-sided density is 0.4 g / 1540.25 mm. 2 When the battery cell is fully discharged, the thickness of the positive electrode film on one side is 106.1 μm, and the compaction density is 2.46 g / cm³. 3 .

[0315] (3) Preparation of negative electrode sheet

[0316] Natural graphite, conductive carbon black, styrene-butadiene rubber (SBR) binder, and sodium carboxymethyl cellulose (CMC) thickener are mixed evenly in a weight ratio of 95:1:2:2 and deionized water is added. After stirring and dispersing, a negative electrode slurry is obtained. The negative electrode slurry is coated on a copper foil substrate, and after drying, cold pressing, slitting, and sheet forming, a negative electrode sheet is obtained.

[0317] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0318] (4) Diaphragm

[0319] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to a base film with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the film was immersed in deionized water to dissolve the PEG, resulting in a membrane with a porous adhesive layer on both sides. The base film thickness was 8 μm, the ceramic layer thickness on one side was 3 μm, and the adhesive layer thickness on one side was 1 μm.

[0320] (5) Electrolyte

[0321] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), organic solvents dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) are mixed evenly in a mass ratio of 30:50:20.

[0322] Lithium hexafluorophosphate was then added and dissolved in an organic solvent to make the electrolyte concentration 1.05 mol / L. The mixture was stirred until homogeneous to obtain the electrolyte of Example 1.

[0323] (6) Battery fabrication:

[0324] The positive electrode, separator, and negative electrode are stacked sequentially using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight containment. The coated stacked battery cell is placed in an outer packaging material, an aluminum-plastic composite film, which consists of an inner polypropylene layer, a middle aluminum foil layer, and an outer nylon layer. The aluminum-plastic film outer packaging is double-sided perforated and trimmed using a perforation forming machine to obtain the target shape and size. The aluminum-plastic film is then heat-sealed to meet a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking, settling, electrolyte injection, and sealing. Finally, the soft-pack battery is subjected to hot and cold pressing operations. The hot pressing temperature is 45℃, the time is 2 minutes, and the pressure is 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 After processes such as formation, vacuum degassing, and edge trimming, the battery cell is obtained. The battery cell has a length of 600mm, a width of 125mm, a thickness (H1) of 20mm, and a capacity of 159Ah.

[0325] Example 2

[0326] The preparation method of Example 2 is basically the same as that of Example 1, except that:

[0327] Adjust the addition amounts of sucrose, glucose, and polyethylene glycol in step S1 of the preparation of positive electrode active material: based on the total mass of the mixed raw materials, the mass content of sucrose is 1.8%, the mass content of glucose is 3.6%, and the mass content of polyethylene glycol is 4.5%. After mixing evenly, a mixed raw material with a solid content of 38% is obtained.

[0328] Adjust the grinding process in step S2 of the positive electrode active material preparation: Grind the mixed raw materials twice in a sand mill, coarsely grinding for 2 hours followed by fine grinding. Control the slurry temperature to below 40 degrees Celsius during the grinding process to obtain a mixed slurry; the particle size D of the solid particles in the mixed slurry... V50 The particle size was 0.80 μm. Spray drying was performed to obtain a dried precursor powder. After drying, its particle size D... V50 It is 62.50 μm.

[0329] Example 3

[0330] The preparation method of Example 3 is basically the same as that of Example 1, except that:

[0331] The sintering process in step S3 of the positive electrode active material preparation was adjusted as follows: the precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 460℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature was then increased from 460℃ to 785℃ at a heating rate of 5℃ / min (second heating stage), and held for 13 hours; the air flow rate in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air flow rate was 1350 cm³. 3 / h, after which cooling is completed; particle size D is obtained by airflow pulverization. V50 The active material for lithium iron phosphate cathodes has a carbon material on its surface with a thickness of 1.6 μm.

[0332] Example 4

[0333] The preparation method of Example 4 is basically the same as that of Example 1, except that:

[0334] Adjust the single-sided thickness H of the positive electrode film according to Table 1 below.

[0335] Example 5

[0336] The preparation method of Example 5 is basically the same as that of Example 1, except that:

[0337] In S2; the particle size D of the solid particles in the mixed slurry V50 It is 0.70μm.

[0338] Example 6

[0339] The preparation method of Example 6 is basically the same as that of Example 1, except that:

[0340] In S2; the particle size D of the solid particles in the mixed slurry V50 It is 1.20 μm;

[0341] In S3: the temperature is increased from 460℃ to 790℃ at a heating rate of 5℃ / min (second heating stage).

[0342] Example 7

[0343] The preparation method of Example 7 is basically the same as that of Example 1, except that:

[0344] In S2; the particle size D of the solid particles in the mixed slurry V50 It is 1.10 μm. Example 8

[0345] The preparation method of Example 8 is basically the same as that of Example 1, except that:

[0346] In S1: Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, glucose, and polyethylene glycol are added to deionized water and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate is such that the molar ratio of lithium to iron is 1.02:1.0. Based on the total mass of the mixed raw materials, the mass content of glucose is 4% and the mass content of polyethylene glycol is 8%. After uniform mixing, a mixed raw material with a solid content of 38% is obtained.

[0347] Among them, the particle size D of lithium carbonate V50 The particle size is 6 μm; the morphology of the iron phosphate particles is spherical; both titanium dioxide and vanadium pentoxide are nanoparticles; the moisture content of glucose is <0.5% by mass; and the weight average molecular weight of polyethylene glycol is 1500.

[0348] In S3: the temperature is increased from 460℃ to 790℃ at a heating rate of 5℃ / min (second heating stage).

[0349] Example 9

[0350] The preparation method of Example 9 is basically the same as that of Example 1, except that:

[0351] In S3, the temperature was increased from 460℃ to 780℃ (second heating stage) at a heating rate of 7.5℃ / min, and held for 12 hours. The ventilation volume in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total ventilation volume was 1000 cm³. 3 / h, after which cooling is completed; particle size D is obtained by airflow pulverization. V50 The active material for lithium iron phosphate cathodes has a carbon material on its surface with a thickness of 1.6 μm.

[0352] Comparative Example 1

[0353] The preparation methods of Comparative Example 1 and Example 1 are basically the same, except that:

[0354] Adjusting step S2 of the preparation of the positive electrode active material: Divide the mixed raw materials into two parts at a 1:1 ratio, and then ball mill them separately to obtain a first grinding material and a second grinding material; grind the first grinding material in a sand mill for 10 hours at a frequency of 24 Hz; control the slurry temperature to be less than 40°C during the grinding process to obtain the first grinding slurry, wherein the particle size D of the solid particles in the first grinding slurry is... V50 The particle size is 0.5 μm; the second abrasive is ground in a sand mill for 8 hours at a frequency of 22 Hz; the slurry temperature is controlled below 40℃ during the grinding process to obtain the second grinding slurry, and the particle size D of the solid particles in the second grinding slurry is... V50 The particle size is 2.5 μm; the first grinding slurry and the second grinding slurry are mixed at a mass ratio of 85:15 and then spray-dried to obtain a mixed precursor powder;

[0355] Adjusting step S3 of the preparation of the positive electrode active material: The mixed slurry is spray-dried to obtain precursor powder, and the precursor powder is sintered to obtain lithium iron phosphate positive electrode material. The sintering process includes: the precursor powder is subjected to two-stage heating sintering in a nitrogen atmosphere to obtain the positive electrode active material: heating from 25°C to 500°C at a heating rate of 3°C / min (first heating stage), holding for 3 hours; heating from 500°C to 780°C at a heating rate of 5°C / min (second heating stage), holding for 10 hours; wherein, the air flow rate in the heating stage is greater than that in the isothermal stage, with a ratio of 1.3:1, and the total air flow rate is 1500 cm³. 3 / h, then cool down after completion.

[0356] Comparative Example 2

[0357] The preparation methods of Comparative Example 2 and Comparative Example 1 are basically the same, the difference being:

[0358] Adjust the grinding process of the second grinding slurry in step S2 of the positive electrode active material preparation to make the particle size D of the solid particles in the second grinding slurry... V50 The particle size is 1.8 μm. The first grinding slurry and the second grinding slurry are mixed at a mass ratio of 90:10 and then spray-dried to obtain a mixed precursor powder.

[0359] Comparative Example 3

[0360] The preparation method of Comparative Example 3 is basically the same as that of Example 1, except that:

[0361] Adjust the amount of sucrose, glucose and polyethylene glycol added in step S1 of the preparation of positive electrode active material: based on the total mass of the mixed raw materials, the mass content of sucrose is 7%, the mass content of glucose is 4%, and polyethylene glycol is not added.

[0362] Comparative Example 4

[0363] The preparation method of Comparative Example 3 is basically the same as that of Example 1, except that:

[0364] In S2; the particle size D of the solid particles in the mixed slurry V50 It is 0.70 μm;

[0365] In S3: the temperature is increased from 460℃ to 775℃ at a heating rate of 5℃ / min (second heating stage).

[0366] Test methods

[0367] 1. DCIR growth rate after 300 cycles at 60℃

[0368] S1: Charge the battery cell at 25°C with a constant current of 0.5C to 3.65V, then perform constant voltage charging at 3.65V until the current reaches 0.05C, and let it stand for 10 min; then discharge at 0.5C to 20% SOC, let it stand for 5 min, then perform 3C pulse discharge for 30 s, record the voltages before and after the pulse discharge, the calculation formula is DCIR = (voltage before pulse discharge after standing - voltage after pulse discharge before standing) / pulse current, to obtain DCIR1.

[0369] S2: Place the battery cell in an environment of 60°C for 300 cycles, where one cycle refers to: charge the battery cell at a constant current of 0.5C to 3.65V, then perform constant voltage charging at 3.65V until the current reaches 0.05C, let it stand for 10 min; then discharge at a 1C discharge rate to 2.5V.

[0370] S3: After the battery cell is cycled 300 times at 60°C, place it in an environment of 25°C for 24 h, charge it at a constant current of 0.5C to 3.65V, then perform constant voltage charging at 3.65V until the current reaches 0.05C, and let it stand for 10 min; then discharge at 0.5C to 20% SOC, let it stand for 5 min, then perform 3C pulse discharge for 30 s, record the voltages before and after the pulse discharge, and calculate to obtain DCIR2.

[0371] DCIR growth rate after 300 cycles at 60°C = (DCIR2 - DCIR1) / DCIR1 × 100%.

[0372] Test Results

[0373] The test results of the above examples and comparative examples are shown in Table 1.

[0374] Table 1

[0375] It can be seen from the comparison between the examples and the comparative examples that the battery cell includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium-containing transition metal phosphate particles at least part of the surface of which is provided with a carbon material; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying 50 nm ≤ R1 ≤ 400 nm is 20%-40%; based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R3 satisfying 1 μm < R3 ≤ 5 μm is less than or equal to 30%; in the cumulative distribution curve of the graphitization degree C value obtained in the surface scanning mode of the laser confocal Raman spectrometer for the positive electrode film layer, the median C of the graphitization degree 50 is 0.95-1.20, wherein the graphitization degree C value is I G / I D , wherein IG represents the G peak intensity of the Raman spectrum at 1580±100cm -1 , and I D represents the D peak intensity of the Raman spectrum at 1350±100cm -1 , which helps to improve the energy density of the battery cell while taking into account the DCIR growth rate of the battery, ameliorate the heat generation problem, and give consideration to the safety performance of the battery cell.

[0376] As can be seen from the comparison between the Examples and Comparative Example 1, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is less than or equal to 30%, which helps to reduce the growth rate of DCIR, ameliorate the heat generation problem of the battery cell, and improve the safety performance.

[0377] As can be seen from the comparison between the Examples, Comparative Example 2 and Comparative Example 4, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is 20%-40%, which helps to improve the energy density of the battery cell, reduce the growth rate of DCIR, ameliorate the heat generation problem of the battery cell, and take safety performance into consideration.

[0378] As can be seen from the comparison between the Examples and Comparative Example 3, in the cumulative distribution curve of the graphitization degree C value obtained by the positive electrode film layer in the surface scanning mode of a laser confocal Raman spectrometer, the median C of the graphitization degree 50 is 0.95-1.20, which helps to reduce the growth rate of DCIR, ameliorate the heat generation problem of the battery cell, and improve the safety performance. As can be seen from the comparison among Example 1, Example 3 and Example 2, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R1 satisfying 50nm≤R1≤400nm is further in the range of 25%-35%, which helps to reduce the contact area between particles, lower the ohmic internal resistance of the electrode sheet, and simultaneously take into account the particle gradation in the positive electrode film layer and the compaction density, so as to give consideration to both the energy density and safety performance of the battery.

[0379] As can be seen from the comparison among Example 1, Example 2 and Example 3, based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode sheet, the area proportion of particles with a particle size R3 satisfying 1μm<R3≤5μm is further in the range of 10%-20%, which helps to further reduce the polarization internal resistance, lower the heat generation of the electrode sheet, and thus further improve the safety performance of the battery.

[0380] Compared with Examples 1-8, Example 9 makes the particle size concentration (D A90 -D A10 ) / D A50The ratio is 1.5-2.3, and the area ratio of large and small particles is kept within an appropriate range, so that excellent energy density can be obtained while taking into account safety performance.

[0381] It should be noted that this disclosure is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same essential structure and achieving the same effect as the technical concept within the scope of this disclosure are included in the technical scope of this disclosure. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, are also included in the scope of this disclosure without departing from the spirit of this disclosure.

Claims

1. A battery cell, wherein, The battery cell includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer includes a positive active material, and the positive active material includes lithium-containing transition metal phosphate particles at least partially coated with a carbon coating material on the surface; Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying 50 nm ≤ R1 ≤ 400 nm is 20%-40%; Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R3 satisfying 1 μm < R3 ≤ 5 μm is less than or equal to 30%; In the cumulative distribution curve of the graphitization degree C value of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode, the median C of the graphitization degree is... 50 The value ranges from 0.95 to 1.20, where the degree of graphitization C is I. G / I D , where I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

2. The battery cell of claim 1, wherein, The particle size R2 obtained from the section of the positive electrode film layer along the thickness direction of the electrode sheet satisfies 0.4 μm < R2 ≤ 1 μm in the particle size area cumulative distribution curve of the particles, and the particle size concentration degree (D A90 -D A10 ) / D A50 is less than or equal to 2.

3.

3. The battery cell of claim 1 or 2, wherein, The particle size R2 obtained from the section of the positive electrode film layer along the thickness direction of the electrode sheet satisfies 0.4 μm < R2 ≤ 1 μm in the particle size area cumulative distribution curve of the particles, and the particle size concentration degree (D A90 - A10 ) / D A50 is 0.5-2.

3.

4. The battery cell of any one of claims 1-3, wherein, The particle size R2 obtained from the section of the positive electrode film layer along the thickness direction of the electrode sheet satisfies 0.4 μm < R2 ≤ 1 μm in the particle size area cumulative distribution curve of the particles, and the particle size concentration degree (D A90 -D A10 ) / D A50 is 0.7-1.

3.

5. The battery cell of any one of claims 1-3, wherein, The particle size R2 obtained from the section of the positive electrode film layer along the thickness direction of the electrode tab satisfies 0.4 μm < R2 ≤ 1 μm in the particle size area cumulative distribution curve, and the particle size concentration degree (D A90 -D A10 ) / D A50 is 1-2.

3.

6. The battery cell of any one of claims 1-3, wherein, The particle size R2 obtained from the section of the positive electrode film layer along the thickness direction of the electrode sheet satisfies 0.4 μm < R2 ≤ 1 μm in the particle size area cumulative distribution curve of the particles, and the particle size concentration degree (D A90 -D A10 ) / D A50 is 1.5-2.

3.

7. The battery cell of any one of claims 1-6, wherein, Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm is greater than or equal to 25%.

8. The battery cell of any one of claims 1-7, wherein, Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm is 25%-70%.

9. The battery cell of any one of claims 1-8, wherein, Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R2 satisfying 0.4 μm < R2 ≤ 1 μm is 40%-70%.

10. The battery cell of any one of claims 1-9, wherein, When the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 70 μm-120 μm.

11. The battery cell of any one of claims 1-10, wherein, When the battery cell is in a fully discharged state, the single-side thickness H of the positive electrode film layer is 90 μm-120 μm, optionally 100 μm-120 μm.

12. The battery cell of any one of claims 1-11, wherein, Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying 50 nm ≤ R1 ≤ 400 nm is 25%-35%.

13. The battery cell of any one of claims 1-12, wherein, Based on the total area of particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R3 satisfying 1 μm < R3 ≤ 5 μm is less than or equal to 20%, optionally 10%-20%.

14. The battery cell of any one of claims 1-13, wherein, The graphitization degree C value cumulative distribution curve of the positive electrode film layer obtained under the laser microscope confocal Raman spectrometer surface scanning mode, the median number C of the graphitization degree is 1.01-1.

13. 50 1.01-1.

13.

15. The battery cell of any one of claims 1-14, wherein, The battery cell in full discharge state, the compaction density of the positive pole piece is 2.3g / cm 3 -2.6g / cm 3 .

16. The battery cell of any one of claims 1-15, wherein, In the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the porosity of the positive electrode film layer is 14%-28%.

17. The battery cell of any one of claims 1-16, wherein, In the cumulative distribution curve of the coating value B obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median B of the coating value is... 50 The value is 0.3-0.6, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

18. The battery cell of any one of claims 1-17, wherein, The positive electrode film layer further includes a conductive agent, and based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of the agglomerated region of the conductive agent is 0.5%-2.5%, optionally 0.5%-1.7%.

19. The battery cell of claim 18, wherein, In the cross section along the thickness direction of the positive electrode plate, the range of the area proportion of the conductive agent agglomerated region is less than or equal to 2%, optionally 0%-1%.

20. The battery cell of claim 18 or 19, wherein, The conductive agent includes carbon nanotubes, and the carbon nanotubes include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes; optionally, the conductive agent further includes conductive carbon black.

21. The battery cell of any one of claims 18-20, wherein, The agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

22. The battery cell of claim 21, wherein, Based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes satisfies: 0 < C1 ≤ 2.5%, and the mass content C2 of conductive carbon black satisfies: 0 < C2 ≤ 2.5%.

23. The battery cell of any one of claims 1-22, wherein, A bottom coating layer is disposed in the bottom region of the positive electrode film layer adjacent to the positive current collector, and the bottom coating layer meets at least one of the following conditions: (1) The base coating includes a conductive agent and a binder, wherein the conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer; (2) The thickness of the base coating is 0.5μm-5μm.

24. The battery cell of any one of claims 1-23, wherein, Along the thickness direction of the positive electrode sheet, the size of the positive current collector is 12μm-16μm, and can be selected as 13μm-15μm.

25. The battery cell of any one of claims 1-24, wherein, The resistivity of the positive electrode film is 5 Ω·cm-35 Ω·cm.

26. The battery cell of any one of claims 1-25, wherein, The lithium-containing transition metal phosphate particles include components represented by the general formula: Li m Fe x P y O j Q q Formula I, Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.

1.

27. The battery cell of any one of claims 1-26, wherein, The lithium-containing transition metal phosphate particles include titanium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of titanium is 500ppm-8000ppm, and can be selected as 1000ppm-3000ppm.

28. The battery cell of any one of claims 1-27, wherein, The lithium-containing transition metal phosphate particles include vanadium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of vanadium is 500ppm-5000ppm, and can be selected as 500ppm-3000ppm.

29. The battery cell of any one of claims 1-28, wherein, The battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

30. The battery cell of claim 29, wherein, The diaphragm satisfies at least one of the following conditions: (1) The thickness of the base film is 7-9 μm; (2) The thickness of the ceramic layer on one side is 2-4 μm; (3) The thickness of the adhesive layer on one side is 1-5 μm.

31. The battery cell of any one of claims 1-30, wherein, The battery cell includes a stacked cell, and the stacked cell includes a positive electrode and a negative electrode.

32. The battery cell of claim 31, wherein, The battery cell also includes a housing, and the stacked cells are housed within the housing. The housing includes a soft-pack material, which includes an aluminum-plastic composite film. Optionally, the soft-pack material includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.

33. The battery cell of claim 32, wherein, The housing includes a first receiving portion and a second receiving portion, the first receiving portion and the second receiving portion are integrally connected and disposed opposite to each other, and the stacked battery cell is received in the receiving cavity formed by the first receiving portion and the second receiving portion.

34. The battery cell of claim 32 or 33, wherein, The housing includes a first sealing area, which is disposed at at least one end of the laminated cell extending along a second direction; the first sealing area includes a double-folded edge structure extending along a first direction, and encapsulating adhesive is disposed on the double-folded edge structure, which is continuously disposed along the length direction and fixes the double-folded edge structure.

35. The battery cell of any one of claims 32-34, wherein, The housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell extending along a first direction, and is disposed on the tab side of the laminated cell.

36. The battery cell of any one of claims 31-35, wherein, The outer periphery of the laminated cell is provided with a plurality of rubber rings that surround along the second direction, and the surrounding rubber rings are spaced apart along the first direction.

37. The battery cell of any one of claims 32-36, wherein, The housing has a length dimension L1, a width dimension W1, and a thickness dimension H1 in the battery cell, where 450mm≤L1≤1300mm, 100mm≤W1≤150mm, and 14mm≤H1≤22mm.

38. The battery cell of claim 37, wherein, The dimension of the casing along the length of the battery cell is L1, where 450mm ≤ L1 ≤ 650mm.

39. The battery cell of claim 37, wherein, The dimension of the casing along the length of the battery cell is L1, where 900mm ≤ L1 ≤ 1300mm.

40. The battery cell of any one of claims 1-39, wherein, At 25°C, the capacity of the battery cell is 95Ah-300Ah, and can be selected as 150Ah-190Ah.

41. A battery device comprising a battery cell as claimed in any one of claims 1-40.

42. An electrical device comprising a battery device as described in claim 41, the battery device being used to provide electrical energy.