A method of manufacturing a spar cap with steps of consolidation for use in wind turbine rotor blades

The method addresses wrinkle issues in spar cap manufacturing by using non-crimp fabrics with binder material and consolidation, enhancing mechanical properties and reducing costs and weight in wind turbine rotor blades.

WO2026238210A1PCT designated stage Publication Date: 2026-11-19DENCAM COMPOSITE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/DK2026/060062
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Manufacturing spar caps for wind turbine rotor blades using non-crimp fabrics is hindered by issues with wrinkles, which degrade mechanical properties and necessitate additional fabrication material, increasing costs and weight.

Method used

A method involving the use of non-crimp fabrics with a binder material, followed by consolidation and infusion steps, including layup, consolidation, and curing, to form a multilayered lamellar structure that reduces wrinkles and enhances structural integrity.

Benefits of technology

The method reduces wrinkles, optimizes mechanical properties, decreases material usage, and lowers manufacturing costs while maintaining structural rigidity, resulting in lighter and more durable spar caps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DK2026060062_19112026_PF_FP_ABST
    Figure DK2026060062_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A method for manufacturing a spar cap for a wind turbine rotor blade, the method comprises steps of: - layup (1000) of non-crimp fabric layers (110) including a binder material in a spar cap mould (120), thereby forming a multilayered lamellar structure (140); - infusion (1100) of resin into the multilayered lamellar structure (140); and - curing (1200) the multilayered lamellar structure (140), thereby manufacturing a spar cap.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] A method of manufacturing a spar cap with steps of consolidation for use in wind turbine rotor blades

[0002] Field of the Invention

[0003] The present invention relates to a manufacturing method for fabricating a spar cap for wind turbine rotor blades, wherein a multilayered lamellar structure comprising noncrimp fabrics including a binder material are cured in a spar cap mould into a spar cap.

[0004] The present method further comprises a step wherein the multilayered structure is consolidated after layup, followed by a step of infusion.

[0005] The present method additionally comprises a step of passing that can be performed before the layup, to fabricate semi-rigid structures comprising layers of non-crimp fabrics.

[0006] Background of the Invention

[0007] Spar caps are an essential part of wind turbine rotor blades, due to their reinforcing properties that ensures the rotor blades ability to withstand the harsh environment during operation of the wind turbine. The spar caps thus serve an important role, and manufacturing spar caps with a high quality with a minimal number of defects is vital.

[0008] One method that can be used to manufacture spar caps is by using non-crimp fabrics. However, one of the major shortcomings of manufacturing with non-crimp fabrics are issues with wrinkles. Wrinkles in spar caps are known to have a huge impact on the mechanical properties of the spar caps which then translates to the mechanical properties of the wind turbine rotor blade.

[0009] To compensate for the reduced mechanical properties due to wrinkles in the spar cap, additional fabrication material is added during the manufacturing. The act of adding extra fabrication material is called safety factor. Based on the technique used for manufacturing, the designer knows the average amount of defects appearing in the spar cap and adds additional fabrication material accordingly. However, adding additional fabrication material increases costs and the weight of the spar cap.To overcome the issue of wrinkling of non-crimp fabrics used in the manufacturing of wind turbine rotor blade spar caps, new methods or technologies must be developed.

[0010] Object of the Invention

[0011] One objective of the present disclosure is to achieve a method to overcome the above-mentioned problems of the prior art.

[0012] One objective of the present method is achieved by using non-crimp fabrics including binder material to form a multilayered lamellar structure, which is infused and cured to manufacture a spar cap for wind turbine rotor blades.

[0013] One objective of the present method is achieved by consolidating the multilayered structure after the step of layup, followed by a step of waiting before the step of infusion.

[0014] One objective of the present method is achieved by a step of passing before the step of layup, to consolidate two or more layers of non-crimp fabrics including binder material with a heated die into semi-rigid structures.

[0015] Description of the Invention

[0016] One objective of the invention is achieved by a method for manufacturing a spar cap for a wind turbine rotor blade, the method comprises steps of:

[0017] layup of non-crimp fabric layers including a binder material in a spar cap mould, thereby forming a multilayered lamellar structure;

[0018] infusion of resin into the multilayered lamellar structure; and

[0019] curing the multilayered lamellar structure, thereby manufacturing a spar cap.

[0020] The main purpose of the method is for manufacturing a spar cap for a wind turbine rotor blade. The method starts by a step of layup, where the non-crimp fabric layers including a binder material are placed in the spar cap mould in a specific designed order of direction of the non-crimp fabric.In one aspect of the method, the non-crimp fabric layers used may have unidirectional fibre direction. The non-crimp fabric layers with unidirectional fibre direction are defined as having 95% or more, such as 95% to 99% of the fibres being in a common direction. The remaining 5% of fibres, such as the remaining 1% to 5% of fibres, may be substantially perpendicular to the common direction. The remaining 5% of fibres, such as the remaining 1% to 5% of fibres, may be arranged in an angle or angles between 80 to 90 degrees to the common direction.

[0021] Furthermore, for spar caps, all of the unidirectional non-crimp fabric layers may be in the same direction in the spar cap mould, with the common direction being substantially parallel to the long side of the mould.

[0022] Throughout the description the word spar cap mould and mould will be used interchangeably. Additionally, the use of non-crimp fabric layers and layers will also be used interchangeably. Furthermore, the use of spar cap, spar cap for wind turbine rotor blade and wind turbine rotor blade spar cap will be used interchangeably.

[0023] The step of layup is the repeating of adding a layer or layers of non-crimp fabrics including a binder material to the spar cap mould. The repeating of adding non-crimp fabrics layers including a binder material to the mould forms the multilayered lamellar structure.

[0024] Throughout the description the wording non-crimp fabric layers including a binder material can mean off-the-shelf non-crimp fabrics supplied with a binder material comprised in or on the fabric. It also covers non-crimp fabric layers having been applied a binder material in a subsequent step of applying prior to layup step.

[0025] The binder material may be applied to and distributed over the entire surface of the non-crimp fabric layers, over the entire width of the non-crimp fabric layers, or at specific locations on the surface of the non-crimp fabric layers, for example along a midsection or edge-section of the non-crimp fabric layer.

[0026] In the step of infusion, the multilayered lamellar structure infused with resin during the infusion step, where resin is introduced into the multilayered lamellar structureensuring wetting of fibres in resin and uniform distribution of the resin throughout the multilayered lamellar structure.

[0027] In the last step, the resin infused multilayered structure is cured during the curing step. In the curing step the resin is solidified and creates a composite matrix, where the noncrimp fabrics fibres are bound together and can transfer stress between the fibres and provide structural support. Curing may be done at room temperature and / or by heating, depending on the resin.

[0028] In one aspect, the resin infused during the infusion step may be polyester resin, vi-nylester resin, or epoxy resin. The polyester resin and the vinylester resin are curable at room temperature, while epoxy resin requires heating, generally to above 80 degrees Celsius.

[0029] The infusion and curing steps may be done by a technique such as resin transfer moulding (RTM) or vacuum infusion also called vacuum assisted resin transfer moulding (VARTM).

[0030] In resin transfer moulding, the multilayered lamellar structure arranged in the spar cap mould, which is sealed before a resin is injected into the spar cap mould and cured to form a spar cap. The resin transfer moulding has a higher manufacturing cost compared to vacuum infusion. However, this process provides a better control over interfaces to neighbouring components, final Fiber Volume Fraction (FVF), and surface finish of the spar cap.

[0031] In vacuum assisted resin transfer moulding, next in the layup process, the multilayered lamellar structure is covered by a vacuum bag. The vacuum bag ensures that the multilayered lamellar structure on the mould is in a closed environment, as the last part of the layup process vacuum is now applied to the multilayered structure through a port or valve. The multilayered lamellar structure is now ready to be infused with resin during the infusion step. In the infusion step, resin is introduced into the multilayered lamellar structure where the vacuum ensures wetting of fibres in resin and uniform distribution.One advantage of this method is that the method is based on using binder material to produce wind turbine spar caps. The binder material within each layer of the noncrimp fabrics in the multilayer lamellar structure will stabilize the structure before and during the cure temperature. The stabilization will ensure that the multilayered structure holds a consistent shape while also preventing fibre movement, thereby reducing wrinkles. Furthermore, vacuum infusion is a more cost-effective process compared to resin transfer moulding and, thus, provides a lower manufacturing cost.

[0032] The present method of using non-crimp fabrics including binder material reduces wrinkles in the final spar cap, thereby fully utilizing the characteristics of non-crimp fabrics regarding reinforcement, lightweight design, improved processability, cost efficiency, and durability.

[0033] In a further embodiment of the method following the step of layup, the method may comprise:

[0034] - a step of consolidating the multilayered lamellar structure and the binder material by heating and pressure.

[0035] The step of consolidating is performed after the application of the vacuum bag or sealing of the spar cap mould in the layup process, just before the infusion step. In the consolidation step, pressure and heat is applied to the multilayered lamellar structure causing the binder material to melt or soften, leading to spreading of the binder material across the fibres in the non-crimp fabrics bonding and stabilizing the structure. In addition, the pressure ensures that the multilayered lamellar structure is bonded and stabilized at minimum thickness, causing a high fibre volume fraction. Having the step of consolidating before the step of curing provides the multilayered lamellar structure with more rigid structural properties. The more rigid structure makes the multilayered lamellar structure less susceptible to wrinkling during the curing of the material.

[0036] The pressure needed during the consolidation step is generally applied with a vacuum pressure, wherein the vacuum pressure is created by the removing air from the mould sealed by the vacuum bag or by other means, such as lid or cover. Removal of air further removes entrapped air or bubbles between each of the non-crimp fabrics layers with binder material in the multilayered lamellar structure.The binder material may comprise:

[0037] - a powder material,

[0038] - comprising of thermoplastics and / or thermosets,

[0039] - being one or two component mixes,

[0040] - being compatible with epoxy, polyester and / or vinylester.

[0041] Furthermore, the binder material may be in a ratio between 1 to 5%.

[0042] In a further embodiment of the method the step of consolidation may be followed by a step of:

[0043] - waiting until the multilayered lamellar structure reaches a threshold temperature before performing the step of infusion.

[0044] After the multilayered lamellar structure has been consolidated, the multilayered lamellar structure needs to be resin infused during the infusion step. However, if the temperature of the multilayered lamellar structure is not within a threshold temperature, it could affect the infusion of resin. By having a step of waiting after the consolidation and before infusion, a suitable temperature of the multilayered lamellar structure can be reached.

[0045] Having a step of waiting after consolidation further ensures that the consolidated binder material in the multilayered lamellar structure can set properly. The setting of the consolidated binder material also allows the binder material to bind together the fabrics within the multilayered lamellar structure. The waiting thus produces a more stable multilayered lamellar structure before the next step of infusion.

[0046] The threshold temperature could be at or below 50 degrees Celsius, ideally 40 degrees Celsius.

[0047] In a further embodiment of the method the non-crimp fabric layers may comprise materials chosen amongst carbon, glass, and / or a hybrid or a combination thereof.The hybrid composite may be a combination of carbon fibre and glass fibre. By combining carbon fibre and glass fibre, it is possible to obtain hybrid materials that merge the properties of both materials. Depending on the ratio between carbon and glass fibre the hybrid can be more carbon or glass-like. As carbon fibre is generally more expensive than glass fibre, a hybrid can reduce costs if only some specific properties of carbon are needed. The hybrid material could be in the range of a mix of four-part carbon fibre and one-part glass fibre to a mix of one-part carbon fibre and one-part glass fibre, or anything in between. In one example the mix could be of two-part carbon fibre and one-part glass fibre.

[0048] In a further embodiment of the method wherein preceding the step of layup, the method may comprise a step of:

[0049] - passing two or more non-crimp fabric layers including binder material through a heated die, wherein the heat and pressure from the heated die consolidates the two or more non-crimp fabric layers including binder material into a semi-rigid composite of non-crimp fabric layers; or the method comprises steps of:

[0050] - applying binder material to two or more non-crimp fabric layers and

[0051] - passing the two or more non-crimp fabric layers applied binder material through the heated die, wherein the heat and pressure from the heated die consolidates the two or more non-crimp fabrics layers and binder material into a semi-rigid composite of non-crimp fabric layers.

[0052] The steps of passing describe how to consolidate the binder material within or applied to the non-crimp fabrics using a heated die. In this method, two or more non-crimp fabric layers including binder material or applied binder material are lead through a heated die. The heat from the heated die melts or soften the binder material causing the binder material to spread across the fibres within or applied to the non-crimp fabrics bonding and stabilize the two or more non-crimp fabrics. Furthermore, the heated die also applies pressure to the two or more non-crimp fabrics. The pressure compresses the two or more non-crimp fabrics and the melted or softened binder material thereby stabilizes non-crimp fabrics and binder material to a thin semi-rigid composite with a high fibre volume fraction.The semi-rigid composite comprises two or more non-crimp fabric layers including or applied binder material and can be laid up in the spar cap mould similar to singular layers. However, since the semi-rigid structure is more rigid than singular layers, the semi-rigid structure is less likely to be impacted by wrinkles during the layup and curing process.

[0053] In another aspect of the passing step, where the non-crimp fabrics does not include a binder material, the passing step must include adding binder material to the non-crimp fabrics before passing through the heated die. By including a process of adding binder to the non-crimp fabrics in the passing step, the need for buying expensive non-crimp fabrics including a binder from a supplier is eliminated. The additional process of adding binder thus reduces manufacturing costs and is more economically feasible.

[0054] Furthermore, the step of adding the binder onto the non-crimp fabrics and consolidating the two or more layers in the heated die could potentially create higher interlayer bonding between non-crimp fabric layers, as the binder material is at the very surface of the fabric. In the standard process of adding the powder binder to non-crimp fabrics, each layer is heated under pressure and therefore binder materials are pushed into the fabric. The heated die can be a pultrusion die.

[0055] The binder material may be applied to and distributed over the entire surface of the non-crimp fabric layers, over the entire width of the non-crimp fabric layers, or at specific locations on the surface of the non-crimp fabric layers, for example along a midsection or edge-section of the non-crimp fabric layer. By applying the binder material to specific locations, the two or more non-crimp fabric layers can be connected to one another, when consolidated in the heated die, thereby easing the lay up in the spar cap mould and preventing displacement of the con-crimp fabric layer, while minimizing the amount of binder material needed and reducing manufacturing cost. By applying the binder material to the entire surface or entire width of the non-crimp fabric layer the two or more non-crimp fabric layers can be consolidated to form a semi-rigid structure, which is less likely to be impacted by wrinkles during the layup and curing process.In a further embodiment of the method the step of passing may be performed by pultrusion.

[0056] Pultrusion is a continuous manufacturing process known for its ability to produce composites with high strength-to-weight ratio and being cost-effective for producing long straight composite profiles. Thus, an ideal process for the step of passing.

[0057] In a further embodiment of the method the semi-rigid composite may comprise 2-40 non-crimp fabric layers, such as 5-30 non-crimp fabric layers, or preferably 10-20 non-crimp fabric layers.

[0058] The rigidity of the semi-rigid composite fabricated during the step of passing, can be customized to suit the need of the end product and / or layup process. The versatility of the step of passing comes from its ability to consolidate a variety number of non-crimp fabric layers including a binder material into a semi-rigid structure, depending on a predetermined passing process setup.

[0059] The optimal semi-rigid structure properties are obtained by consolidating 10-20 non-crimp fabrics including a binder material into a semi-rigid structure, and obtaining a semi-rigid structure thickness typically in the range of 1 to 7 mm. The semi-rigid structure may have a thickness in the range of 2 to 6 mm. The main impact on the rigidity of the semi-rigid structure may be the non-crimp fabric construction and the amount / type of binder material used.

[0060] The level of rigidity must be carefully designed according to the spar cap geometry and size. Higher rigidity reduces the risk of the formation of wrinkles during the layup and curing but could, on the other hand, create challenges with the layup and conforming the geometry of the spar cap mould. Moreover, higher rigidity, which is mostly due to high powder binder content, will negatively impact the resin infusion process by blocking the resin flow passages. Hence, the level of rigidity must be tuned for each and every spar cap.

[0061] Additionally, the number of layers contained within a semi-rigid structure also effects the time needed for the layup step. A complete spar cap may comprise on averageabout 100 layers. If the semi-rigid structure comprises many layers, for example 20 non-crimp fabric layers, only 5 semi-rigid structures is needed during layup. While, if the semi-rigid structure comprises less layers, for example 5 non-crimp fabric layers, 20 semi-rigid structures would be needed during layup.

[0062] The fabrication time of the semi-rigid structure substantially does not depend on number of non-crimp fabric layers used in passing through the heated die. Depending on the number of non-crimp fabric layers in the semi-rigid structure the size and / or temperature of the heated die can be adjusted to keep the same fabrication time. Thereby, having many layers in the semi-rigid structure decreases both time needed to fabricate semi-rigid structures and the number of steps during layup, thus decreasing costs and time during fabrication of a spar cap.

[0063] In a further embodiment of the method the heated die may have a width between 300 millimetres and 1000 millimetres, and a thickness between 1 millimetre and 7 millimetres.

[0064] During the passing step, the layers of non-crimp fabrics including a binder material are passed through a heated die. The dimension of the heated die defines the maximum width, height, and overall shape of the semi-rigid structure profile. Accordingly, the size of the heated die depends on the size of the wanted semi-rigid structure, and the thickness of the heated die depends on the amount of non-crimp fabric layers needed in the semi-rigid structure.

[0065] In a further embodiment of the method wherein each layer of the fabric layers may have an area weight between 500 grams per square meter and 1200 grams per square meter.

[0066] The spar cap can be produced by a variety of different non-crimp fabrics with different area weight. The area weight of the non-crimp fabric layers effects the mechanical properties, resin consumption, permeability, drapeability, and cost, of the non-crimp fabric layer.The spar cap may have a substantially rectangular cross-section. The cross-section of the spar cap may be rectangular along the entire length of the spar cap or it may have a chord-wise taper along the edges if the spar cap. Here chord-wise refers to a direction, running along an airfoil's chord, specifically from the leading edge to the trailing edge.

[0067] The spar cap may furthermore be a curved spar cap, such that a first side of the spar cap configured for engaging the wind turbine blade mould is convex and a second side opposite and parallel to the first side is optionally concave. Thereby, the spar cap better conforms to the wind turbine blade layup, that is the concave shape of the wind turbine blade mould. This is advantageous as it prevents the formation of a profile bridge across the surface in the transverse direction of the blade mould, leaving a gab beneath the spar cap for race tracing and large resin pool, which is detrimental to the mechanical properties of the wind turbine blade. The curved spar cap may be manufactured with a pultrusion process.

[0068] A wind turbine rotor blade comprising spar cap produced by the method according to any of claims 1 to 9.

[0069] During general production of spar caps, the designer knows how many wrinkles are expected in an average spar cap manufactured by a certain technology. Knowing the average amount of wrinkles, the designer must compensate for the reduced mechanical properties due to wrinkles, which is done by adding additional carbon material. The method according to the invention utilizes non-crimp fabrics including binder material combined with new production steps to reduce the number of wrinkles in the spar cap. Thereby, the designer will require less additional carbon material to compensate for the wrinkles in the spar cap, and thus reducing safety factor.

[0070] Due to the fewer materials used, wind turbine rotor blades comprising a spar cap produced by the method according to the invention has reduced weight. The reduced weight of wind turbine rotor blades reduces the wind turbines rotational inertia and lowers stress on central components.

[0071] Description of the Drawing

[0072] Embodiments of the invention will be described in the figures, whereon:Fig. 1 illustrates the method for manufacturing a spar cap for wind turbine rotor blade

[0073] Fig. 2 illustrates a front and side view of the layers of non-crimp fabric in the spar cap mould and a cross-section of the cured multilayered lamellar structure. Fig. 3 illustrates the fabrication of the semi-rigid structure by passing non-crimp fabrics including binder through a heated die.

[0074] Detailed Description of the Invention

[0075] Item No

[0076] 110 Non-crimp fabric layers

[0077] 120 Spar cap mould

[0078] 130 Vacuum bag or other sealing means

[0079] 140 Multilayered lamellar structure

[0080] 150 Matrix

[0081] 160 Non-crimp fabric fibres

[0082] 200 Passing setup

[0083] 220 Heated die

[0084] 230 Heating elements

[0085] 240 Semi-rigid structure

[0086] 900 Passing

[0087] 1000 Layup

[0088] 1030 Consolidating

[0089] 1060 Waiting

[0090] 1100 Infusion

[0091] 1200 Curing

[0092]

[0093] Fig. 1 illustrates the method for manufacturing a spar cap for a wind turbine rotor blade. The first step of the process is the layup 1000 of non-crimp fabric layers 110 including a binder material (not shown in Fig. 1) in a spar cap mould 120 (not shown in Fig. 1). In the spar cap mould 120 (not shown in Fig. 1) repeated actions of adding and draping non-crimp fabrics layers including a binder material in the spar cap mould forms a multilayered lamellar structure 140 (not shown in Fig. 1). The last action in the layup 1000 step is to cover the multilayered lamellar structure 140 (not shown inFig. 1) in the spar cap mould 120 (not shown in Fig. 1) with a vacuum bag or other sealing means 130 (not shown in Fig. 1).

[0094] After the vacuum bag 130 (not shown in Fig. 1) has been properly sealed or the spar cap mould 120 have been sealed by other sealing mean 130 such as a lid or cover, the multilayered lamellar structure 140 (not shown in Fig. 1) is exposed to a step of infusion 1100, where a resin is infused into the multilayered lamellar structure 140 (not shown in Fig. 1). Here the resin flows through the non-crimp fabric layers and saturates the fibres within the non-crimp fabrics. Proper resin saturation is vital to the mechanical properties of the cured spar cap, as the resin binds together the non-crimp fabric fibres 160 (not shown in Fig. 1) in the final spar cap and creates the matrix 150 (not shown in Fig. 1).

[0095] When the multilayered lamellar structure 140 (not shown in Fig. 1) in the spar cap mould 120 (not shown in Fig. 1) has been properly saturated with resin during the infusion 1100 step, the multilayered lamellar structure 140 (not shown in Fig. 1) is followed by curing 1200. During curing, the binder material is first activated to stabilize the multilayered lamellar structure 140 (not shown in Fig. 1) before solidification of the infused resin. In a vacuum assisted resin transfer moulding, curing 1200 of the multilayered lamellar structure 140 (not shown in Fig. 1) is under vacuum and can be performed at room temperature. However, the process is typically accelerated by elevated temperatures. In resin transfer moulding, curing 1200 of the multilayered structure 140 is under high pressure as a consequence of the resin injection and can be performed at room temperature. However, the process is typically accelerated by elevated temperatures.

[0096] In a second approach to reduce the risk of wrinkles in the layers non-crimp fabrics, the multilayered lamellar structure 140 (not shown in Fig. 1) is consolidated by a step of consolidating 1030 after layup 1000 and before infusion 1100. The consolidating 1030 of the multilayered lamellar structure 140 (not shown in Fig. 1) is performed by activating the binder material, typically by heating and pressure. After activating the binder material, the binder material will provide stability and cohesion of the multilayered lamellar structure 140 (not shown in Fig. 1). This makes the multilayered la-mellar structure 140 (not shown in Fig. 1) more rigid and thus presents better resistance towards wrinkles.

[0097] After consolidating 1030 the multilayered lamellar structure 140 (not shown in Fig. 1), a step of waiting 1060 is performed to wait for the multilayered lamellar structure 140 (not shown in Fig. 1) to reach a threshold temperature. In the case where the binder material is activated by heat, the multilayered lamellar structure 140 (not shown in Fig. 1) may be at a too high temperature to start the infusion 1100. Furthermore, the waiting will also allow the binder material to set properly in the multilayered lamellar structure 140 (not shown in Fig. 1) before continuing with infusion.

[0098] In a third approach, the non-crimp fabrics undergoes a passing 900 step before layup to create a semi-rigid structure 240 (not shown in Fig. 1) comprising layers of noncrimp fabrics. In the process, two or more non-crimp fabric layers 110 including or applied binder material (not shown in Fig. 1) passes through a heated die 220 (not shown in Fig. 1). The heat and pressure from the heated die 220 (not shown in Fig. 1) activates the binder material, which melts or softens to bind the non-crimp fabrics together, forming a semi-rigid structure 240 (not shown in Fig. 1) comprising two or more layers of non-crim fabrics 110 including or applied binder material (not shown in Fig. 1). The semi-rigid structure 240 (not shown in Fig. 1) can then be used in the layup 1000 process. The semi-rigid structure 240 (not shown in Fig. 1) can thus either follow the layup 1000, infuse 1100, and curing 1200 method or the layup 1000, consolidate 1030, waiting 1060, infuse 1100, and curing 1200 method.

[0099] Fig. 2 illustrates a front and side view of the layers of non-crimp fabric layers 110 including binder material in the spar cap mould 120 and a cross-section of the cured multilayered lamellar structure 140.

[0100] Fig. 2a illustrates a front view of the non-crimp fabric layers 110 including binder material laid up in the spar cap mould 120, forming a multilayered lamellar structure 140. Fig. 2 further illustrates a vacuum bag 130 or other sealing means 130 as a dashed line. During layup 1000 (not shown in Fig. 2) one or multiple non-crimp fabric layers including 110 binder material is laid up and draped on to the spar cap mould 120, which is then repeated and thus fabricates the multilayered lamellar structure140. As a last step in the layup 1000 (not shown in Fig. 2) process, the multilayered lamellar structure 140 is sealed with a vacuum bag 130 or other sealing means 130.

[0101] The cured multilayered lamellar structure 140 and, thus, the spar cap may have a substantially rectangular cross-section as illustrated in fig. 2a. The cross-section of the spar cap may be rectangular along the entire length of the spar cap or it may have a chord-wise taper along the edges of the spar cap.

[0102] The spar cap may furthermore be a curved spar cap, such that a first side of the spar cap configured for engaging the wind turbine blade mould is convex and a second side opposite and parallel to the first side is optionally concave. Thereby, the spar cap better conforms to the wind turbine blade layup, that is the concave shape of the wind turbine blade mould. The curved spar cap may be manufactured with a pultrusion process, as described below for fig. 3.

[0103] Fig. 2b illustrates a side view of the non-crimp fabric layers 110 including binder material as it would look when laid up in the spar cap mould 120. The stepwise size of the non-crimp fabric layers 110 including binder material is a method to ensure proper shape of the final product, in this case the spar cap. The stepwise size of the non-crimp fabric layers 110 may be both in the length direction and / or width direction of the non-crimp fabric layers 110. When the stepwise size is arranged in the length direction, the two or more non-crimp fabric layers 110 are arranged such that a first end of the non-crimp fabric layers 110 align and then stepwise decrease in size from the first (bottom layer) to the last (top layer) at a second end of the non-crimp fabric layers 110, thereby providing a chordwise taper of the resulting spar cap. When the stepwise size is arranged in the width direction, the two or more non-crimp fabric layers 110 are arranged such that centre area, e.g. a centreline, of the non-crimp fabric layers 110 align and then stepwise decrease in size from the first (bottom layer) to the last (top layer) at a second end of the non-crimp fabric layers 110, thereby providing a spar cap with tapered side-edges.

[0104] Fig. 2c illustrates a cross-section of the cured multilayered structure 140. The crosssection illustrates unidirectional non-crimp fabric fibres 160, and how the resin sur-rounds and binds all the fibres together in the matrix 150 after curing 1200 (not shown in Fig. 2).

[0105] Fig. 3 illustrates the fabrication of the semi-rigid structure 240 by either passing 900 non-crimp fabric layers 110 including binder through a heated die 220 or applying binder material to non-crimp fabric layers 110 prior to passing 900 the non-crimp fabric layers 110 applied binder through a heated die 220. In Fig. 3 multiple non-crimp fabric layers 110 including or applied binder is passed through the heated die 220. In this embodiment, 4 non-crimp fabric layers 110 including or applied binder is consolidated to a semi-rigid structure, however it could just as well be two or more non-crimp fabric layers 110 including or applied binder material. The heated die 220 is heated by a plurality of heating elements 230. Inside the heated die 220 the multiple non-crimp fabric layers 110 including or applied binder material is exposed to heat and pressure, which activates the binder material and consolidates the multiple non-crimp fabric layers 110 including or applied binder material into a semi-rigid structure 240. The semi-rigid structure 240 comprises non-crimp fabric layers 110 including or applied binder material and can be used during the layup 1000 (not shown in Fig. 3) to lay up multiple non-crimp fabric layers 110 including or applied binder material at the same time, thereby saving time while the semi-rigid structure 240 prevents wrinkle formation.

Claims

CLAIMS1. A method for manufacturing a spar cap for a wind turbine rotor blade, the method comprises steps of:layup (1000) of non-crimp fabric layers (110) including a binder material in a spar cap mould (120), thereby forming a multilayered lamellar structure (140); infusion (1100) of resin into the multilayered lamellar structure (140); and curing (1200) the multilayered lamellar structure (140), thereby manufacturing a spar cap.

2. A method according to claim 1, wherein following the step of layup (1000) the method comprises:- a step of consolidating (1030) the multilayered lamellar structure (140) and the binder material by heating and pressure.

3. A method according to claim 2, wherein the step of consolidation (1030) is followed by a step of:- waiting (1060) until the multilayered lamellar structure (140) reaches a threshold temperature before performing the step of infusion (1100).

4. A method according to any of claims 1 to 3, wherein the non-crimp fabric layers comprise materials chosen amongst carbon, glass, and / or a hybrid or a combination thereof.

5. A method according to any of the preceding claims, wherein preceding the step of layup (1000), the method comprises a step of:- passing (900) two or more non-crimp fabric layers (110) including binder material through a heated die (220), wherein the heat and pressure from the heated die (220) consolidates the two or more non-crimp fabrics layers (110) including binder material into a semi-rigid composite (240) of non-crimp fabric layers; or the method comprises steps of:- applying binder material to two or more non-crimp fabric layers (110) and- passing (900) the two or more non-crimp fabric layers (110) applied binder material through the heated die (220), wherein the heat and pressure from the heated die (220)consolidates the two or more non-crimp fabrics layers (110) and binder material into a semi-rigid composite (240) of non-crimp fabric layers.6 A. method according to claim 5, wherein the step of passing (900) is performed by pultrusion.

7. A method according to any of claim 5 or 6, wherein the semi-rigid composite (240) comprises 2-40 non-crimp fabric layers (110), such as 5-30 non-crimp fabric layers (110), or preferably 10-20 non-crimp fabric layers (110).

8. A method according to any of claims 6 to 8, wherein the heated die has a width between 300 millimetres and 1000 millimetres, and a thickness between 1 millimetre and 7 millimetres.

9. A method according to any of the preceding claims, wherein each layer of the fabric layers has an area weight between 500 grams per square meter and 1200 grams per square meter.

10. A wind turbine rotor blade comprising spar cap produced by the method according to any of claims 1 to 9.