Welded assembly of molybdenum and molybdenum alloy
A molybdenum assembly with specific compositions and microstructures addresses weld zone embrittlement by enhancing strength and ductility, enabling high-stress applications.
Patent Information
- Application Number
- PCT/EP2026/055203
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-02-26
- Publication Date
- 2026-11-19
AI Technical Summary
Molybdenum and molybdenum alloys suffer from grain coarsening and embrittlement in weld zones, leading to reduced mechanical strength and increased brittle-ductile transition temperatures, making welded assemblies unsuitable for high-stress applications.
An assembly comprising a first component with >99.93 wt.% molybdenum and 15-50 ppmw boron and carbon, and a second component with >50 wt.% molybdenum-based alloy, welded together without a filler material, forming a weld zone with distinct microstructures that enhance strength.
The assembly exhibits higher strength in the weld zone, allowing for fracture outside the weld zone during tensile testing, with an elongation at break of >14%, suitable for high-stress applications.
Smart Images

Figure EP2026055203_19112026_PF_FP_ABST
Abstract
Description
[0001] 1155 EP, 2026-02-26
[0002] Welded assembly made of molybdenum and molybdenum alloy
[0003] The present invention relates to an assembly comprising at least two components, wherein the components are welded together by forming a weld zone. A first component is made of a molybdenum (Mo) material with a molybdenum content of > 99.93 wt.% and a boron and carbon content of > 3 ppmw each, wherein the total boron and carbon content in the Mo material is between 15 and 50 ppmw. A second component is made of a Mo-based alloy with a Mo content of > 50 wt.% and < 99.7 wt.%.
[0004] In principle, molybdenum and molybdenum alloys can only be modified to a limited extent by
[0005] Ten welding processes (e.g., fusion welding processes such as arc welding, laser or electron beam welding) can be used to join components together. The heat input in the weld zone causes grain coarsening, negatively impacting the strength and ductility properties of the assembly compared to the unaffected base materials of the individual components, e.g., a titanium-zirconium-molybdenum (TZM) component. Within the weld zone, these materials become embrittled, meaning they lose toughness and are more prone to fracture or cracking. Consequently, the welded assembly made from these materials has limited mechanical strength. Furthermore, welding induces stresses that can only be partially mitigated by heat treatment before, during, or after the welding process.In particular, embrittlement occurs within the weld zone, with a significant increase in the brittle-ductile transition temperature.
[0006] For example, the tensile strength of a welded assembly in which the individual components are made of pure molybdenum decreases by approximately 50%. For individual components made of a molybdenum alloy, such as titanium-zirconium-molybdenum, the decrease is approximately 25%. The elongation at break is reduced by about 90% in both cases due to laser welding. Such welded joints are unsuitable for applications where the weld seam is subjected to high mechanical cyclic stresses, as stresses cannot be relieved through plastic deformation. Instead, if the maximum stress is exceeded, the component fails immediately due to brittle fracture along the weld seam.
[0007] A molybdenum sintered part with a composition according to the first component of the present invention is known from publication EP 3 688200 Al. The patent application shows,
[0008] Public1155 EP, 2026-02-26
[0009] 2
[0010] that two molybdenum sintered parts with identical composition according to the invention can be welded together well. However, the publication does not provide any information on whether the molybdenum sintered part according to this invention can also be welded with other molybdenum-based alloys that have a different composition. It is generally stated that molybdenum cannot be welded.
[0011] Document WO2014 / 134642 Al discloses an arrangement of two component sections made of Mo or a Mo-based material. The component sections are joined together by fusion welding. A welding filler material (which differs from the base materials, e.g., V, Ti, Cr) 10 is used.
[0012] The object of the present invention is to provide an assembly in which components made of Mo materials with different compositions are welded together, wherein the assembly has high strength so that high compressive stress or tensile stress is possible.
[0013] The technical problem of the present invention is solved by the assembly according to claim 1 and a method for manufacturing the assembly according to claim 12. Advantageous embodiments of the invention can be found in the dependent claims, which are freely combinable with one another. Features and details described in connection with the assembly according to the invention naturally also apply in connection with the method according to the invention, and vice versa, so that the disclosure of the individual aspects of the invention always refers to, or can refer to, each other.
[0014] According to the present invention, an assembly is provided comprising at least two components, characterized in that a first component is made of a molybdenum-25 material with a molybdenum content of > 99.93 wt.% and a boron and carbon content of > 3 ppmw (3 pg / g) each, wherein the total boron and carbon content in the molybdenum material is between 15 and 50 ppmw, and a second component is made of a molybdenum-based alloy with a molybdenum content of > 50 wt.% and < 99.7 wt.%, and wherein the components are welded together in a metallurgical bond 30, forming a weld zone.
[0015] Public1155 EP, 2026-02-26
[0016] 3
[0017] The assembly according to the invention exhibits higher strength in the weld zone than the first component, resulting in fracture outside the weld zone during tensile testing. The first component has a total molybdenum content of > 99.93 wt.%, preferably > 99.97 wt.%. The maximum molybdenum content is 99.99 wt.%. The boron and carbon content of the first component is each > 3 ppmw (3 pg / g), preferably each > 5 ppmw. In a preferred embodiment, the boron content can be between 5 and 45 ppmw, preferably between 10 and 40 ppmw. The carbon content can be between 5 and 30 ppmw, more preferably between 15 and 20 ppmw. The total boron and carbon content in the first component is between 15 and 50 ppmw, preferably between 25 and 40 ppmw.
[0018] 10. The combination of boron and carbon in these areas leads to a significantly increased grain boundary strength of the component.
[0019] The first component can have an oxygen content of < 20 ppmw, preferably between 5 and 15 ppmw, a tungsten content of max. 330 ppmw, and a content of unavoidable impurities of max. 300 ppmw. All elements add up to 100% of the composition. The tungsten content of max. 330 ppmw is typically already determined by the molybdenum extraction and powder production.
[0020] The second component is made of a molybdenum-based alloy. A molybdenum-based alloy is defined as an alloy in which molybdenum is the main constituent, i.e., present in a higher proportion (measured in wt.%) than any of the other elements it contains. Preferably, the molybdenum-based alloy contains more than 50 wt.% molybdenum.
[0021] Preferably, the molybdenum-based alloy can contain > 59 wt.% molybdenum. In a further embodiment, the molybdenum-based alloy can contain at least 70 wt.% molybdenum and up to a maximum of 99.7 wt.% molybdenum. This alloy may also contain unavoidable impurities of up to 1000 ppmw, preferably less than 700 ppmw.
[0022] The term "unavoidable impurities" refers to manufacturing-related impurities in gases or accompanying elements that originate from the raw materials used. A distinction can be made between metallic and non-metallic impurities. Metallic impurities include, for example, zirconium (Zr), hafnium (Hf), titanium (Ti), vandium (V), aluminum (Al), chromium (Cr), iron (Fe), silicon (Si), rhenium (Re), potassium (K), etc. The proportion of such impurities in the first Public1155 EP, 2026-02-26
[0023] 4
[0024] The concentration of such impurities in the first component is preferably below 300 pg / g (corresponding to 300 ppmw), preferably below 200 pg / g, more preferably below 150 pg / g, and particularly preferably below 50 pg / g. In the second component, the concentration of such impurities is below 500 pg / g, preferably below 350 pg / g. Non-metallic impurities can be elements such as O, C, N, H, S, etc. Here, the preferred range for the first component is below 20 pg / g, preferably below 10 pg / g. For the second component, the preferred range is below 400 pg / g, preferably below 300 pg / g. Suitable methods for chemical elemental analysis are known to depend on the chemical element to be analyzed.For the chemical analysis of the unavoidable impurities according to the invention, hot extraction analysis for the elements N and O (see ASTM E 10 1019:2018) or combustion analysis for the elements C and S (see ASTM E 1019:2018) or ICP-MS (inductively coupled plasma mass spectrometry) or ICP-OES (inductively coupled plasma optical emission spectrometry) was used. The notation "ppmw" represents the weight fraction multiplied by 10. -6 out of.
[0025] A chemically bonded connection is characterized by the fact that the joined parts are held together by atomic or molecular bonds. Such connections are insoluble and can only be separated by destruction.
[0026] The weld zone is the area where both components are joined by welding. It encompasses the fusion zone and the adjacent heat-affected zone, which is influenced by the heat of the welding process. Microscopically, the fusion zone is clearly distinguishable from the microstructure of the individual components. The grains are noticeably enlarged compared to the grain structure of the individual components and exhibit a solidification structure (without pores) with columnar grains. The grain diameter (within the interdecile range, i.e., between 10% and 90%) ranges from 10 to 124 pm. The diameter is determined via the maximum Feret diameter. This is measured as the distance between two parallel tangents drawn to the outer edge of a grain. Furthermore, the columnar grains exhibit an aspect ratio or grain size ratio (within the interdecile range) of 1:1.5 to 1:4.The aspect ratio is determined via an ellipse, which is adapted to the contour of the respective grain.
[0027] 30 According to further training, both components are manufactured using powder metallurgy via pressing and sintering. Powder metallurgy allows for the production of complex geometries with
[0028] Public1155 EP, 2026-02-26
[0029] 5
[0030] They are manufactured with minimal material input, exhibiting a homogeneous composition as well as controlled porosity and density. The powder metallurgy components are produced by pressing raw powders into a compact and then sintering the compact.
[0031] 5. The manufacturing process may include additional steps such as mixing and homogenizing the powders (e.g. in a plowshare mixer).
[0032] According to further training, the first component exhibits a sintered structure, and the second component exhibits a formed structure. The first component shows a typical sintered structure, which is readily recognizable to a person skilled in the art. This microstructure is characterized by its
[0033] 10. Fine grain structure (typical rounded grains, with the grain diameter (within the interdecile range, 10%-90%) between 10 and 64 pm, measured over the maximum Feret diameter). Furthermore, pores are uniformly distributed throughout the entire cross-section of the sintered part. In the case of "good" or "complete" sintering (the density is then > 93% of the theoretical density and there is no open porosity), these pores appear at the grain boundaries as well as rounded cavities inside the resulting sintered grains. The second component exhibits a formed microstructure. For this, the component is formed after sintering, for example, uniaxially by forging or rolling. Preferably, the formed microstructure is a rolled microstructure. The microstructure of the second component therefore exhibits an anisotropic elongated grain elongation perpendicular to the forming direction. The 20 textured structure exhibits, firstly, grain elongation with a grain elongation ratio, i.e.An aspect ratio (within the interdecile range) of at least 1:2, preferably at least 1:7, is required. The aspect ratio can also be larger, for example 1:20. The diameter of the Mo alloy grains, measured over the maximum Feret diameter, lies (within the interdecile range, 10%–90%) between 10 and 129 pm.
[0034] In a preferred embodiment, the density of the first component is > 93%, preferably > 94%, of the theoretical density. The maximum upper limit of the theoretical density may, in one embodiment, be < 98%. The second component has a density of > 99% of the theoretical density. The maximum upper limit of the theoretical density is < 99.99%. The theoretical density is the maximum achievable density of the respective component, provided that no pores, internal cavities, or impurities are present.
[0035] A higher density is achieved by reshaping the second component. The theoretical
[0036] Public1155 EP, 2026-02-26
[0037] 6
[0038] The density of molybdenum alloys can be calculated from the densities of the individual metals and their weight fractions. The density can be determined, for example, using the Archimedes method by measuring the weight of the component in air and in water. Increased density leads to increased strength and hardness, making the components more resistant to mechanical stress.
[0039] The assembly is preferably characterized in that it is welded without a welding filler material. A welding filler material is a material that is used in addition to the components to be joined during welding. It is melted and, together with the molten base material 10, forms the weld metal during the joining process. Such welding filler materials, such as Mo, Ti, Zr, V, Re, Nb, Ta, Ni, Ru, Cr, and alloys thereof, are known from the prior art. In contrast, the assembly according to the invention does not require a welding filler material, which is advantageous with regard to material purity, cost savings, reduced susceptibility to defects, and simpler handling.
[0040] According to the present invention, the components are in a metallically bare state before welding. This means that neither component undergoes any pretreatment that creates optimal conditions for the welding process of Mo components with other Mo components, e.g., coating or carburizing the components. Thus, neither component undergoes any welding-process-supporting pretreatment. The prior art describes improved weldability of Mo or a Mo alloy with Mo or a Mo alloy by nitriding or carburizing the components beforehand.
[0041] In a preferred embodiment, the fusion zone has a higher hardness value HV 0.1 according to DIN 50159-1 (as of 2015-01) than the first component. The fusion zone during welding is the area in which the first and second components are joined together by the action of the welding heat source through a physical change of state (solid-molten-solid).
[0042] The DIN 50159 (2015-01) method describes a procedure for hardness testing of metallic materials using the UCI (Ultrasonic Contact Impedance) method. Similar to the Vickers method, an indentation is created in the component under test with a defined 30 kJ / cm test load. A Vickers diamond is used, located at the end of a vibrating rod. The vibrating rod is induced by a piezoelectric crystal.
[0043] Public1155 EP, 2026-02-26
[0044] 7
[0045] Longitudinal vibrations are excited. The resonant frequency of the vibrating rod changes during the penetration process, which is used to determine the hardness. The method is particularly suitable for measurements on welds. A test force of 98 N is used for the hardness test of the weld zone and the first component. The standard DIN 50159-1
[0046] Section 5 describes the specific requirements and procedures for this type of hardness test.
[0047] As already explained above, the weld zone of the assembly according to the invention comprises a melt zone and a heat-affected zone. These zones are microscopically distinguishable. The assembly is characterized in that a heat-affected zone and a melt zone form on the side of the second component, while only a melt zone forms on the side of the first component. Thus, a formed microstructure, a heat-affected zone, and a melt zone can be observed microscopically on the side of the second component. The heat-affected zone is an area around the melt zone that has been affected by the heat of the welding process but has not melted. The formed microstructure is the unaffected material that has not been affected by the welding process. The melt zone is the area in which the base materials of the first and second components are completely melted and mixed together.
[0048] On the side of the first component, the sintered structure transitions directly into the melting zone without forming a heat-affected zone.
[0049] In the heat-affected zone, the formed structure, e.g. the rolled structure, undergoes a structural change due to the heat of the welding process, without the material completely melting.
[0050] The heat-affected zone can lead to changes in mechanical properties.
[0051] In the heat-affected zone of the second component, the grain size diameter, measured across the maximum Feret diameter, ranges from 11 to 86 pm (within the 10%–90% range). The elongated grain structure obtained through rolling changes to a more rounded grain structure during welding, with the grains also increasing in diameter. The aspect ratio of at least 1:7 (or greater) in the formed microstructure changes to an aspect ratio of 1:1.5 to 1:4 (within the 10%–90% range).
[0052] These characteristic features are examined in cross-section.
[0053] 30 light microscopic or electron microscopic images.
[0054] Public1155 EP, 2026-02-26
[0055] 8
[0056] The second component preferably consists of a molybdenum-based alloy selected from the group consisting of titanium zirconium molybdenum (TZM), molybdenum hafnium carbon (MHC), molybdenum rhenium (MoRe), or molybdenum lanthanum oxide (ML).
[0057] TZM refers to a molybdenum alloy with a titanium content of 0.40 to 0.55 wt.%, a zirconium content of 0.06 to 0.08 wt.%, a carbon content of 0.005-0.04 wt.%, an oxygen content of less than 0.03 wt.% and the remaining content (apart from any impurities) molybdenum.
[0058] In this context, MHC refers to a molybdenum alloy that has a hafnium content of 1.0 to 1.3 wt.%, a carbon content of 0.05 to 0.12 wt.%, an oxygen content of less than 0.06 wt.% and the remaining content (apart from any impurities) is molybdenum.
[0059] ML refers to a molybdenum alloy with 0.3 to 0.7 wt.% La2Ü3 and the remaining molybdenum (apart from any impurities).
[0060] MoRe refers, on the one hand, to a molybdenum alloy with a rhenium content between 40.15 and 50 wt.%, preferably between 41 and 47.5 wt.% rhenium (and any impurities). In an alternative embodiment, however, the rhenium content can deviate significantly from this and, for example, be only 5 wt.%.
[0061] According to a further development of the present invention, the weld zone is formed by laser beam welding or electron beam welding. These welding processes are advantageous compared to TIG welding processes because the laser or electron beam can be focused on a small area, which allows for precise control of the welding process.
[0062] The elongation at break of such an assembly is more than 14% according to DIN ISO 4136:2012. This standard refers to the destructive testing of welded joints in metallic materials, in particular the transverse tensile test. In this test, the specimen is clamped in a testing machine and subjected to a tensile load acting perpendicular to the weld. The machine pulls the specimen apart until it breaks. This provides two important pieces of information: firstly, the maximum tensile force the specimen can withstand before breaking, and secondly, the precise point at which the specimen breaks, allowing conclusions to be drawn about the quality of the weld and the material. An elongation at break of more than 14% represents the
[0063] Public1155 EP, 2026-02-26
[0064] 9
[0065] This represents the critical limit at which welded structures can be used in pressure vessel construction without requiring additional structural safety measures. The maximum upper limit of elongation at break is 40%.
[0066] The assembly according to the invention thus enables the realization of structures 5 which, on the one hand, connect areas with high stresses made of a high-strength material (second component) and, on the other hand, areas with lower stresses (first component). The inventive method for manufacturing an assembly is characterized by the following steps:
[0067] Manufacturing a first component from a molybdenum material with a molybdenum content of > 99.93 wt.%, a boron and carbon content of > 3 ppm each, wherein the total boron and carbon content in the molybdenum material is between 15 and 50 ppm, by pressing and sintering;
[0068] Manufacturing a second component from a molybdenum-based alloy with a molybdenum content of > 50 wt.% and < 99.7 wt.%, by pressing and sintering;
[0069] Material-bonded joining of the first and second components, forming a weld zone.
[0070] To produce the first component, a powder mixture is blended and then predominantly cold isostatically pressed into a green compact / pressed compact. The green compact is then sintered at temperatures around 2,000 °C.
[0071] 20 The second component is manufactured in a similar manner, whereby a powder mixture of molybdenum-based alloy is pressed into a green compact. In a preferred embodiment, the sintered molded body is compacted by forming, preferably rolling.
[0072] Both components are then welded together by forming a weld zone, creating a material bond 25. Preferably, no welding filler material is used.
[0073] As already stated above, both components can be in their bare metallic state and are not subjected to any pretreatment.
[0074] Public1155 EP, 2026-02-26
[0075] 10
[0076] In a preferred embodiment, the fusion welding process is carried out by arc welding or beam welding (laser welding, electron beam welding). Preferably, friction welding, diffusion welding, or explosion welding is not used. Further advantages and expediencies of the invention will become apparent from the following description of an exemplary embodiment with reference to the accompanying figures.
[0077] The figures show
[0078] Fig. 1: schematic cross-section of an exemplary assembly;
[0079] Fig. 2: schematic cross-section of an embodiment of the present invention, wherein two components (here two sheets) are butted together;
[0080] 10 Fig. 3A Micrograph of the weld zone in the area of the joint (magnification 500X);
[0081] Fig. 3B Hardness scan over the polished section 3A (magnification 500X);
[0082] Fig. 4 Micrograph of the weld zone in the area of the joint (magnification 200X),
[0083] Enlarged image of Fig. 3A;
[0084] Fig. 5 Micrograph of the weld zone in the area of the second component (magnification 200X), enlarged image of Fig. 4;
[0085] Fig. 6 Micrograph of the weld zone in the area of the first component (magnification 200X), enlarged image of Fig. 4;
[0086] Fig. 7 Components after tensile test according to DIN EN ISO 4136.
[0087] Figure 1 schematically shows a cross-sectional view of an assembly of the present invention, wherein the first component 1 is, for example, a pressure vessel and the second component 2 is, for example, a pipeline. Both components are made of molybdenum alloys with different molybdenum contents (see claim 1). Both components are welded together to form a weld zone 3.
[0088] Fig. 2 schematically shows a cross-section of two components. The first component differs from the second component in the molybdenum content of the respective Mo material. The components are butted together and welded without the addition of filler metals. The weld zone 3 forms between the two components during welding.
[0089] 30
[0090] Public1155 EP, 2026-02-26
[0091] 11
[0092]
[0093] Manufacturing the first and second components
[0094] Both components were provided by the company Plansee. The first component is a pressed and sintered molybdenum part containing 22 ppmw boron, 12 ppmw carbon, and 7 ppmw oxygen; the remainder is molybdenum and unavoidable impurities.
[0095] The second component was selected such that, apart from impurities, it would have a composition of 0.5 wt.% Ti, 0.08 wt.% Zr, 0.005-0.04 wt.% C, less than 0.03 wt.% oxygen, and the remainder molybdenum (after completion of all processes within the scope of the
[0096] The component undergoes 10 processes and heat treatments carried out in powder metallurgy manufacturing (i.e., TZM). It was formed into a shaped structure by rolling.
[0097] Welding the first component to the second component:
[0098] The first component, with its sintered structure, was butted against the second component, with its formed structure, and welded together using laser beam welding on a laser welding system (Trumpf TruDisk 8000 disk laser). The following welding parameters were used:
[0099] Welding power: 3000 W (watts)
[0100] Focus diameter: 150 pm (micrometers)
[0101] 20 Welding speed: 60 mm / sec (millimeters per second)
[0102] Shielding gas: 100% Argon
[0103] Thus, an assembly according to the invention is obtained.
[0104] For microstructure analysis, the component segment to be examined is cut out by wire EDM in the area of the weld zone and the adjacent, unaffected base material. This segment is then heat-embedded in a plastic granulate perpendicular to the weld seam. After the embedding material has hardened, the surface is ground, polished, and optionally etched to improve the visibility of the grain structure. To measure the grain size, the polished sample is imaged under a light microscope at 25x magnification and then analyzed with the
[0105] 30. Image editing program FiJi-l mageJ converted into a binary image. With the same
[0106] Public1155 EP, 2026-02-26
[0107] 12
[0108] The program then proceeds with the measurement of the individual grains in the selected areas of the welding zone and the unaffected base materials.
[0109] Fig. 3A shows a stereomicroscopic image of the cross-section across the weld zone of the assembly, i.e., the second component made of TZM and the first component made of Mo with 34 ppmw B5 and C. The different microstructures are clearly visible. On the left of the image is the rolled TZM component, and on the right, the sintered first component. The rounded grains and the pores resulting from sintering are clearly visible in the first component. In the second component, the elongated grains of the rolled structure are visible. The weld zone is visible in the middle. The solidification structure with large, partially elongated grains is discernible. The black dots in the image are pores that formed during the welding process.
[0110] Fig. 3B shows the hardness scan over Fig. 3A. The hardness scan was performed using a BAQ UT200 UCI hardness scanner with a dot pattern of 0.15 mm x 0.15 mm. A test force of 0.98 N or 0.1 kgf (kilogram force) is used to determine the hardness of the materials. It can be seen that the HV0,l value (hardness according to the Vickers method) is lowest in the area of the first component (right in the image) (light gray) and increases in the weld zone (light gray and dark gray). The HV0,l value is highest in the dark gray areas (second component and weld zone).
[0111] Fig. 4 is an enlargement of Fig. 3A and clearly shows the different
[0112] 20 Microstructures. Fig. 4 shows that, starting from the melt zone C, the weld zone of the first component exhibits only a melt zone C (without a discernible heat-affected zone). Area D identifies the microstructure of the sintered first component. In contrast, a melt zone C and a heat-affected zone B are discernible for the second TZM component. Area A identifies the microstructure of the second rolled TZM component.
[0113] Fig. 5 is an enlargement of Fig. 4 and shows the rolling structure A of the second component, as well as the heat-affected zone B and the melting zone C.
[0114] Fig. 6 is an enlargement of Fig. 4 and clearly shows the sintered structure D of the first component, as well as the melting zone C. Here, no heat-affected zone forms between the 30 sintered structure and the melting zone.
[0115] Public1155 EP, 2026-02-26
[0116] 13
[0117] Fig. 7 shows an assembly according to the invention after a tensile test according to DIN EN ISO 4136, which was loaded until fracture. The tensile specimen exhibits a pronounced yield strength and a necking zone before failure occurs. At the same time, an elongation at break of > 14% is achieved according to DIN ISO 4136 (2012), which represents the critical limit 5 for use as a welded structure, i.e., as an assembly in pressure vessel construction without further additional structural safety measures. The arrows indicate the weld zone, making it clear that the fracture occurs in the first component. The welded molybdenum sintered parts can therefore be used for applications in which the welded joint is subjected to cyclic loading, since
[0118] Ten stresses can be relieved by plastic deformation of the assembly before the assembly fails, thus following the principle of pressure vessel construction "deformation before fracture".
[0119] 15
[0120] Public
Claims
1155 EP, 2026-02-26 14 REQUIREMENTS 1. Assembly comprising at least two components, characterized in that a first component is made of a molybdenum material with a molybdenum content of > 99.93 wt.%, a boron and carbon content of > 3 ppmw each, wherein the total boron and carbon content in the molybdenum material is between 15 and 50 ppmw, and a second component is made of a molybdenum-based alloy with a molybdenum content of > 50 wt.% and < 99.7 wt.%, and wherein the components are welded together by forming a weld zone.
2. Assembly according to claim 1, characterized in that both components are manufactured using powder metallurgy by pressing and sintering.
3. Assembly according to claim 1 or claim 2, characterized in that the first component has a sintered structure and the second component has a formed structure.
4. Assembly according to any one of the preceding claims, characterized in that the density of the first component is > 93% of the theoretical density and the density of the second component is > 99% of the theoretical density.
5. Assembly according to one of the preceding claims, characterized in that the components are welded without a welding filler material.
6. Assembly according to one of the preceding claims, characterized in that the components are metallically bright before welding.
7. Assembly according to one of the preceding claims, characterized in that the melt zone has a higher hardness value HV 0.1 according to DIN 50159-1 (2015-01) than the first component.
8. Assembly according to one of the preceding claims, characterized in that in the cross-section perpendicular to the weld seam the weld zone on the side of the second component has a heat-affected zone and a melting zone and on the side of the first component has only a melting zone.
9. Assembly according to one of the preceding claims, characterized in that the second component is made from the group consisting of titanium-zirconium-molybdenum, molybdenum-hafnium-carbon, molybdenum-rhenium, or molybdenum-lanthanum oxide. 1155 EP, 2026-02-26 15 10. Assembly according to any one of the preceding claims, characterized in that the weld zone is formed by laser beam welding or electron beam welding.
11. Assembly according to any one of the preceding claims, characterized in that the elongation at break according to DIN ISO 4136 (2012) of the assembly is more than 14%.
12. Method for manufacturing an assembly, characterized by the following steps: Manufacturing a first component from a molybdenum material with a molybdenum content of > 99.93 wt.%, a boron and carbon content of > 3 ppm each, wherein the total boron and carbon content in the molybdenum material is between 15 and 50 ppm, by pressing and sintering; Manufacturing a second component from a molybdenum-based alloy with a molybdenum content of > 50 wt.% and < 99.7 wt.%, by pressing and sintering; Material-bonded joining of the first and second components, forming a weld zone.
13. Method according to claim 12, characterized in that the second component is reshaped after sintering and before the joining step.
14. Method according to claim 12 or 13, characterized in that the joining is carried out without welding filler material.
15. Method according to any one of the preceding claims 12 to 14, wherein the joining is carried out by a fusion welding process.