Method for producing a gas diffusion layer for an electrochemical cell, and gas diffusion electrode having a gas diffusion layer

The production of a gas diffusion layer through selective etching of a titanium-based alloy with precious metals addresses corrosion and contact resistance issues, enhancing electrical conductivity and catalytic activity in electrolysis cells.

WO2026238311A1PCT designated stage Publication Date: 2026-11-19SIEMENS ENERGY GLOBAL GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/058904
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-03-27
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing gas diffusion layers in electrochemical cells, particularly in electrolysis cells, suffer from corrosion-induced degradation and inadequate electrical contact, leading to increased contact resistance and ohmic losses, which are not effectively addressed by current methods.

Method used

A method for producing a gas diffusion layer using a titanium-based alloy with catalytically active precious metals, involving selective etching to create an open-pore contact layer with a porous structure, reducing ohmic losses and enhancing electrical conductivity and catalytic activity.

Benefits of technology

The method results in a gas diffusion layer with reduced contact resistance and improved long-term stability, maintaining good transport properties and catalytic activity in oxidative environments, thus extending the operational life of electrochemical cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026058904_19112026_PF_FP_ABST
    Figure EP2026058904_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a gas diffusion layer (9, 17) for an electrochemical cell, wherein a flat component comprising a titanium-based alloy (27) is provided, the alloy having, as an alloy element, at least one catalytically active noble metal which is incorporated into a titanium matrix (33). Etchant is applied onto one surface (35) of the flat component, wherein material of the titanium matrix (33) is removed by a selective etching process, and etchant is introduced into the material up to a penetration depth (h). Material of the alloy element is exposed in such a way that an electrically conductive open-pore contact layer (14) is formed close to the surface, the contact layer having the catalytically active noble metal. By selectively removing titanium from the titanium matrix (33) up to the penetration depth (h) below the open-pore contact layer (14), a catalytically active layer (29) with a porous structure and the layer thickness (h) is formed within the alloy (27). The invention further relates to a gas diffusion electrode (12a, 12b) and to an electrolysis cell (1) having a gas diffusion electrode (12a, 12b).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] 2024PF00645

[0002] Description

[0003] Method for producing a gas diffusion layer for an electrochemical cell and a gas diffusion electrode with a gas diffusion layer

[0004] The invention relates to a method for producing a gas diffusion layer for an electrochemical cell, in particular for an electrolysis cell. The invention further relates to a gas diffusion electrode comprising a correspondingly produced gas diffusion layer.

[0005] Hydrogen can be obtained from deionized water via electrolysis. This involves the electrochemical cell reactions of the hydrogen production reaction (HER) and oxygen production reaction (OER). In the case of acidic electrolysis, these reactions at the anode and cathode can be defined as follows:

[0006] Anode 2 H20 -> 4 H+ + 02+ 4 e~ (I)

[0007] Cathode 2H+ + 2 e~

[0008]

[0009] H2( II )

[0010] For example, in a so-called polymer electrolyte membrane electrolysis (PEM electrolysis), the two partial reactions according to equations (I) and (II) are carried out spatially separated from each other in separate half-cells for OER and HER. The separation of the reaction chambers is achieved by means of a proton-conducting membrane, the polymer electrolyte membrane (PEM), also known as a proton exchange membrane. The PEM ensures a largely complete separation of the product gases hydrogen and oxygen, electrical insulation of the electrodes, and conduction of the hydrogen ions as positively charged particles. A PEM electrolysis system typically comprises a plurality of appropriately designed PEM electrolysis cells, as described, for example, in EP 3 489 394 A1.2024PF00645

[0011] 2

[0012] A PEM electrolysis cell is described, for example, in EP 2 957 659 A1. The PEM electrolysis cell shown there comprises an electrolyte made of a proton-conducting membrane (proton exchange membrane, PEM), on which the electrodes, a cathode and an anode, are located on both sides. The unit consisting of the membrane and electrodes is called a membrane electrode assembly (MEA). A gas diffusion layer is located at each electrode. The gas diffusion layers are contacted by so-called bipolar plates. Each bipolar plate can form or have a channel structure designed for the transport of the reactant and product flows. However, a planar design of a bipolar plate without a channel structure is also possible in principle. At the same time, the bipolar plates separate the individual electrolysis cells from each other, which are stacked to form an electrolysis stack with a large number of electrolysis cells.The PEM electrolysis cell is supplied with deionized water as a reactant, which is electrochemically split at the anode into oxygen product gas and protons (H+). The protons (H+) migrate through the electrolyte membrane towards the cathode. On the cathode side, they recombine to form hydrogen product gas (H2).

[0013] The cell reactions described in equations (I) and (II) are in equilibrium with their reverse reactions at a cell voltage of 1.48 V, taking into account the increase in entropy during the conversion of liquid water to gaseous hydrogen or oxygen. To achieve sufficiently high product flows in a reasonable time (production output) and thus a current flow, a higher voltage, the overvoltage, is necessary, among other reasons. In principle, electrochemical water splitting is possible from 1.23 V if sufficient thermal energy is available in addition to electrical energy. The thermoneutral voltage for water splitting is 1.48 V. However, due to various losses such as activation losses, ohmic losses, mass transport losses, etc., water splitting is generally only possible from approximately 1.7 or 1.8 V. (Degra-2024PF00645)

[0014] During fermentation, the cell voltage gradually rises to 2.1 to 2.3 V and may even increase further depending on operational requirements. In practice, PEM electrolysis is typically carried out at a cell voltage of approximately 1.8 to 2.1 V.

[0015] A PEM electrolysis cell is also described in Kumar, S, et al., Hydrogen production by PEM water electrolysis - A review, Materials Science for Energy Technologies, 2 (3) 2019, 442-454. https: / / doi.org / 10.1016 / j.mset.2019.03.002. From the outside in, the PEM electrolysis cell consists of two bipolar plates or half-plates, gas diffusion layers, catalyst layers, and a proton-conducting membrane. The latter separates the anodic from the cathodic half-cell.

[0016] The oxygen formation reaction at the anode results in very high oxidative potentials. Therefore, high-quality materials with rapid passivation kinetics / oxide layer formation, such as titanium, are generally used at the anode, particularly for the gas diffusion layer or a porous transport layer (PTL). The passivation process aims to minimize the release of metal ions from the component, albeit at the cost of lower electrical conductivity due to the semiconductor properties of titanium oxide. High demands also apply, for example, to the choice of material for the anode-side catalyst and for the bipolar plate that rests against the gas diffusion layer and electrically contacts it. This creates a respective channel structure for the transport of the reactant and product flows involved.The protective oxide layers that form at high potentials lead to increased contact resistances between the individual metallic components and ultimately to increased voltage degradation of the cell. Until now, this problem has been solved by coating corrosion-resistant materials, such as titanium, with a layer of precious metal. These precious metals are stable under the aforementioned oxidative conditions or at least form conductive oxides. Thus, the contact resistance at the interface remains low.

[0017] 4

[0018] before, at least in the case of an intact layer, comparatively low.

[0019] Various approaches to counteract the degradation effects at the anode and cathode described above have been described in the prior art. For example, it has been proposed that a larger quantity of catalytically active species be introduced into the anodic catalyst layer, i.e., that a higher concentration of catalytically active species be maintained. This allows degradation effects at the anode to be compensated for, at least temporarily, with regard to catalytic activity. To reduce degradation effects on the anode side caused by local electrical contact resistances and the associated inhomogeneous current distribution in the gas diffusion layer and catalyst layer system, optimization of the contact pressure of the gas diffusion layer against the catalyst layer has been proposed, among other things.However, this always carries the risk of perforation of the membrane electrode assembly (MEA) due to excessively high contact pressure during assembly and axial stacking of the electrolysis cells into an electrolysis stack, and the resulting mechanical stress under high axial force. This leads to short circuits, rendering the electrolysis cell unusable and significantly jeopardizing or even preventing the operation of the electrolyzer. On the other hand, catalyst materials such as iridium and other platinum group alloying elements are very expensive, so their consumption should be minimized.

[0020] In connection with, for example, the channel structure that spatially confines an electrolysis cell and simultaneously provides electrical contact and substance transport, hardly any measures have been proposed to date with regard to improving corrosion protection and electrical contact with long service lives. There is also considerable potential for improvement in the other metallic components of the electrolysis cell, such as the gas diffusion layer.

[0021] 5

[0022] There is a clear need for improvement in the provision of a corrosion-resistant, electrically conductive contact layer or coating, especially on the anode side of an electrochemical cell.

[0023] The approaches mentioned above do not solve the underlying problems and causes of corrosion-induced degradation and sometimes inadequate electrical contact, particularly at the anode, with sufficient long-term reliability for the operation of the electrolysis cell. At best, they represent temporary measures to partially reduce corrosion-induced degradation effects and extend their duration of operation. At the same time, especially during extended operating periods of an electrolysis cell, the electrical contact properties can be reduced by accompanying oxidation effects. Consequently, despite the use of sometimes expensive metal alloys, the electrical conductivity of the contacts can decrease, leading to increased contact resistance and corresponding ohmic losses.

[0024] The precious metal coating method previously used to reduce contact resistance between corrosion-resistant components has the disadvantage that the layers are very thin and therefore easily damaged during assembly. Furthermore, the coating process is costly and time-consuming, usually carried out under vacuum. Additionally, thin precious metal layers (e.g., platinum) can flake off, oxidize, or be damaged mechanically, chemically, or electrochemically by the high contact pressure during the assembly of the electrolysis stacks or by the electrolysis process itself.

[0025] Against this background, the object of the invention is to provide a method for producing a gas diffusion layer for an electrochemical cell, which is characterized by reduced ohmic losses and good transport properties for the media. The gas diffusion layer thus created is intended to 2024PF00645

[0026] be specially suited for use in a highly oxidative environment of an electrochemical cell, such as an electrolysis cell or a fuel cell.

[0027] This problem is solved according to the invention by a method for producing a gas diffusion layer for an electrochemical cell, in particular for an electrolysis cell, which comprises the following process steps:

[0028] (51) Provision of a planar component comprising a titanium-based alloy which includes as an alloying element at least one catalytically active precious metal embedded in a titanium matrix;

[0029] (52) Applying an etching agent to a surface of the planar component, wherein material of the titanium matrix is ​​removed by selective etching, wherein the etching agent is introduced into the material to a penetration depth; (53) Exposing material of the alloying element such that an electrically conductive open-pore contact layer is formed near the surface, which contains the catalytically active precious metal;

[0030] (54) Selective extraction of titanium from the titanium matrix to the penetration depth below the open-pore contact layer, forming a catalytically active layer with a porous structure and layer thickness within the alloy.

[0031] The process described in the invention enables the production of a titanium-based gas diffusion layer in which targeted material removal is achieved through the proposed solution process. This results in very good electrical contact properties near the surface, i.e., low electrical resistance. An open-pored, electrically conductive contact layer made of the alloying element, which is largely titanium-free, is provided near the surface. Simultaneously, good transport properties for the reactant and product fluids in the gas diffusion layer are achieved by the near-surface structuring and 2024PF00645

[0032] 7

[0033] Material exposure involves deep material dissolution through the application of an etching agent to a desired penetration depth within the titanium matrix. This selective material dissolution to a desired penetration depth of, for example, 100 pm to 300 pm allows for the adjustment of porosity and diffusivity within the material. Titanium is dissolved from the titanium matrix to this penetration depth, exposing the correspondingly catalytically active precious metal. This process forms pores and channels with a catalytically active internal surface. Consequently, a catalytically active transport layer is formed within the alloy material at a depth below the contact layer, maintaining a porous structure and thickness.Near the surface, an electrically conductive, open-pored contact layer is formed, which, like the porous deep layer, contains the catalytically active precious metal due to the etching process.

[0034] Selective etching of the precious metal-rich titanium-based layer creates a porous, transportable structure that simultaneously provides an integrated catalyst within the gas diffusion layer, i.e., an electrically functional layer when used, for example, in an anodic half-cell of an electrolysis cell. Compared to a membrane electrode arrangement with a polymer membrane onto which a catalyst layer is applied as an electrode, the gas diffusion layer of the invention allows for a reduction in catalyst requirements, which is particularly advantageous. Thus, the gas diffusion layer integrates media transport, electrical contact properties, and catalytic activity within the catalytically active layer.

[0035] By selectively exposing material, a precious metal-rich, electrically conductive contact layer is provided, which specifically reduces the contact resistance of the alloy near the surface. The manufacturing process thus makes it possible, in a very advantageous way, to create a metallic 2024PF00645

[0036] 8

[0037] and to provide an electrically conductive component, particularly for use in an electrolysis cell, in which the aforementioned operational degradation problems are significantly reduced and ohmic losses are reduced or completely avoided. The proposed etching process does not limit material removal to the component surface, but also carries it out within the thin contact layer.

[0038] A typical removal or dissolution rate of approximately 0.5 to 1.5 pm per minute is set for the titanium. Depending on the exposure time, titanium as an alloying element is selectively etched out of the titanium matrix, both near the surface and within the volume of the planar component, i.e., dissolved from the alloy. Titanium is dissolved by exposure to the etchant.

[0039] This process causes titanium, for example, as a titanium salt in aqueous solution, to be selectively leached from a layer of the surface and throughout the volume of the component. This leaching of titanium into the volume results in precious metal-containing alloying elements remaining in a locally coherent, porous, and catalytically active structure, which, due to its resistance, is not attacked by the etching agent used. The precious metal-rich porous catalyst layer of a gas diffusion layer produced in this way is corrosion-resistant and remains as oxidation-resistant as the previously untreated titanium-based alloy.

[0040] The process is designed to create an open-pored, precious-metal-containing structure, forming an electrically conductive contact layer, particularly near the surface, depending on the application of the etching process. This open-pored structure, catalytically active due to the precious metals, provides gas diffusion properties through catalytic activity, thus enabling the etching process to function as a gas diffusion electrode. 2024PF00645

[0041] 9

[0042] By selecting this precious metal, the targeted removal of the titanium matrix simultaneously creates an open-pore contact layer with high electrical conductivity and a long service life. This open-pore contact layer allows for longer service lives of the contact layer and thus of the gas diffusion layer during use and operation in an electrolysis cell. The metal dissolution process is designed to ensure deep penetration of the etching agent, rather than just surface contact.

[0043] The application of the etching agent, controlled both on the surface and—for example, via the etching agent's exposure time—within the volume of the flat component, can be achieved, for instance, by partially immersing the component in a bath of liquid etching agent or by spraying the liquid etching agent onto the component's surface. Etching results in the wet-chemical removal of material from the titanium matrix in the form of depressions, channels, and pores on the component's surface through the application of the etching agent. It is also conceivable that specifically selected areas of the component's surface, which are not to be etched or deepened, can be prepared beforehand or selectively masked and protected from the etching process. In principle, it is also possible to protect these local areas with a masking lacquer before exposure to the etching agent.This wet chemical etching process can be repeated multiple times as needed using appropriately adapted etching masks to achieve deep structuring and depth resolution of titanium within the volume of the precious metal-containing titanium matrix, up to the desired penetration depth. It is advantageous to ensure comprehensive porosity within the contact layer as well as within the volume of the catalytically active layer through the process control. 2024PF00645.

[0044] 10

[0045] This process offers the advantage of flexibility and, if required, the ability to etch oxidation-stressed components as so-called "shaped etched parts," even on an industrial scale. This allows for the creation of non-planar surface contours with complex surface geometries. In addition to component outlines, the surface can be structured in a defined manner, or cross-sections (topographies) can be individually created through a specific application of the etching process. Thus, for example, alongside pure depth etching, the finest channels can be etched into the titanium alloy, and titanium can be selectively removed from the titanium matrix near the surface.

[0046] With the gas diffusion layer of the invention, it is now advantageously possible to use a precious metal-containing titanium alloy as the material for a porous transport layer (PTL) in an electrochemical cell, such as an electrolysis or fuel cell. Optionally, either the entire porous transport layer (PTL) can consist of the precious metal-containing titanium alloy, or only the surface or near-surface areas up to the desired layer thickness, which can be easily adjusted via the penetration depth of the etching agent. In sintered structures, which can be powder- or fiber-based and are produced layer by layer, the invention advantageously allows only the uppermost layer(s) to selectively comprise an expensive precious metal-containing alloy with the catalytically active precious metal in a titanium matrix, while the remaining portion, further away from the surface, can consist of nearly pure titanium.

[0047] In a particularly preferred embodiment of the process, the application of the etching agent causes selective dissolution of titanium in the titanium matrix, leaving behind channels and / or pores with a crystalline internal surface containing catalytically active noble metal crystallites. 2024PF00645

[0048] 11

[0049] The application and volume input of the etching agent simultaneously causes selective corrosion of titanium within the titanium matrix on the surface of the planar component, leaving behind a porous and crystalline open-pore structure with precious metal crystallites on the surface, which forms the contact layer. Beneath the contact layer, the porous structure is formed with a layer thickness corresponding to the penetration depth.

[0050] The titanium in the titanium matrix dissolves into aqueous solution upon contact with the etching agent. Dissolved titanium salt can be removed and carried away after the reaction time, revealing or exposing precious metal crystallites. These precious metal crystallites are particularly advantageous with regard to the required contact properties of the component surface, specifically a very low and uniform contact resistance and the mechanical stability of the contact layer. It is advantageous to selectively carry out the etching process such that a precious metal-rich surface layer with a finely porous structure remains, with the pores and channels extending into the volume below the contact layer. This results in the formation of a porous and catalytically active layer within the alloy.

[0051] In conventional contact layers, the operationally negative effect of increased electrical resistance caused by titanium oxide formation is countered by coating the surface of the titanium component with a closed layer of a precious metal, e.g., a thin platinum layer as a corrosion protection layer against oxidative attack. However, these layers are relatively thin and can be damaged during component assembly and operation, thus impairing or limiting their functionality and long-term stability, especially when used in an electrolysis cell. Furthermore, the application of the precious metal coating is disadvantageous.

[0052] 12

[0053] Layering onto the titanium substrate must take place in a separate process step, which implies additional time expenditure and requires special coating equipment.

[0054] In contrast, in a preferred embodiment of the process, a multitude of pores are formed on the surface of the planar component. Due to the open-pore structure, individual islands or island groups of the alloying element can advantageously be formed in the contact layer, which remain after the application of the etching agent.

[0055] The number, size, shape, and distribution of these contact islands across the component surface can be adjusted within certain limits through the etching process and the alloy. For a locally flat component surface, it is advantageous to aim for the most uniform distribution possible of the precious metal-rich contact islands. It is also possible to carry out the etching process in such a way that pairs or groups of connected islands are formed, thus creating clusters of islands.

[0056] In this process, the exposure of the alloying element(s) is carried out in such a way that an electrically conductive, open-pored, precious-metal-rich contact layer is formed near the surface, which continues continuously in the volume below the near-surface contact layer to form a catalytically active layer with a porous structure.

[0057] Initial assessments have shown that a porosity of 50% to 90%, preferably between 70% and 80%, in the catalytically active contact layer is particularly advantageous with regard to the desired electrical contact properties on the one hand and good transport properties for the media on the other. Porosity is defined here as a dimensionless quantity and represents the ratio of void volume to total volume of a material.

[0058] 13

[0059] or material mixture, in this case the porous precious metal layer. It serves as a classifying measure for the actual voids present. This dimension is used in materials science, civil engineering, and geosciences. Porosity has a significant influence on the density of a material and on the resistance to flow through a packed bed according to Darcy's law. In this case, the etching process and the removal of the titanium matrix create a macroporous precious metal structure with an average pore size greater than approximately 50 nm. This results in good fluid conductivity while simultaneously providing a large active internal surface area with the catalytically active precious metal.The gas diffusion layer thus exhibits good diffusion properties with high catalytic activity per surface with reduced precious metal coverage compared to a large-area membrane of a membrane electrode assembly (MEA) coated with a catalyst layer as an electrode.

[0060] Furthermore, the porous and precious-metal-rich support structure provides additional mechanical elasticity. In the installation situation of the oxidation-stressed component, for example in an electrolysis cell of a PEM electrolyzer, this ensures a particularly uniform and, within limits, even spring-like surface pressure and contact.

[0061] The thickness of the precious metal-containing conductive open-pore contact layer produced on the flat component is preferably set between 5 nm and 50 pm. The flat component itself can consist of one or more layers of expanded metal with different mesh geometries. Several layers can be welded together to form a sandwich. Multilayer porous powder- or fiber-based sintered materials are also possible for the flat component to form a gas diffusion layer. In this way, metallic porous transport layers (PTL) or gas diffusion layers (GDL) can be integrally bonded with a titanium-based kataly-2024PF00645.

[0062] 14

[0063] The catalytically active, electrically conductive, and porous transport structure is provided as a "layer-on-top". The total thickness of the catalytically active layer, including the surface-exposed contact layer, is preferably set between approximately 100 pm and 500 pm; for example, a thickness of 250 pm to 300 pm has proven particularly advantageous. Typically, exposure times of several hours for the wet chemical etching agent are required to ensure the dissolution and removal of dissolved titanium from the titanium matrix to the desired penetration depth. The etching process can also be carried out iteratively in several etching and removal steps of the titanium, so that pores and channels are created to the desired depth.

[0064] The layer thickness for layer formation using the etching process is determined to obtain the catalytically active layer with a porous structure up to the desired penetration depth. The pores or channels created in the titanium matrix using wet chemical processes exhibit a wide pore size distribution and have diameters between approximately 10 -2 pm and 10 2 pm, with a relative concentration at a pore size between 1 pm and 10 pm.

[0065] One or more precious metals exhibiting catalytic activity are embedded as alloying elements in the titanium matrix. Alloying elements from the platinum group are preferred.

[0066] This choice of material results in a particularly advantageous high electrical conductivity and the formation of an electrically conductive and at the same time porous and catalytically active layer encompassing the near-surface open-pore contact layer, which is realized on the oxidation-stressed flat component by selective deep etching.

[0067] In a particularly preferred embodiment of the process, a microstructured mask is applied to the surface of the flat-2024PF00645 in a preparation step prior to the application of the etching agent.

[0068] 15

[0069] applied to the component so that selective exposure and targeted penetration of the etchant into the alloy are achieved.

[0070] The microstructured mask is designed to promote pore formation and features numerous uniform micro-openings and channels through which the etching agent is introduced. When the mask is used, the etching agent acts on the titanium-based alloy to be etched, creating a microporous structure by releasing titanium from the matrix material to the desired penetration depth. The etching mask is an auxiliary tool and can be implemented, for example, as a photoresist layer applied to the flat component. Alternatively, a microstructured thin film or perforated mask with numerous through-holes can be temporarily applied to the component surface during the preparation step.In this way, channels and pores can be introduced into the surface and volume of the component using masking technology, and a desired porosity can be set in the layer.

[0071] In a particularly preferred embodiment of the process, a wet chemical etching process is used in which selective removal of titanium from the titanium matrix is ​​effected by the application of an etchant containing hydrofluoric acid (HF).

[0072] Concentrated hydrofluoric acid in aqueous solution is a selective and highly effective etchant for dissolving titanium from the titanium matrix and does not attack the noble metals. Nitric acid (HNO₃) or a mixture of hydrofluoric acid (HF) and nitric acid (HNO₃) can also be used.

[0073] In principle, different solutions can be used as etching agents that can selectively dissolve titanium as a metal in the alloy without dissolving the precious metal as Be-2024PF00645

[0074] 16

[0075] To attack a component of the titanium alloy, e.g., hydrofluoric acid (HF) in an aqueous solution with a concentration of 1%–50%. The etchant can advantageously contain other acids and organic components in a mixture, such as nitric acid (HNO₃) at a concentration of 30–60%, sulfuric acid (H₂SO₄) at a concentration of 10–50%, hydrochloric acid (HCl) at a concentration of 20–50%, glycerin at a concentration of 40–50%, or hydrogen peroxide (H₂O₂) at a concentration of approximately 4%. Furthermore, anhydrous solutions, such as bromoethanol, can also be used. In principle, all known methods for dissolving titanium as a metal can be used as etching processes that selectively target the titanium component in the alloy, for example, immersion, spraying, or electrolytic etching / pickling.Depending on the chosen method, the temperature can be set between -25 °C in anhydrous electrolytes and up to 100 °C in water-based electrolytes. During electrolytic etching, the potential can range from 3 to 75 V. The exposure time can range from a few seconds to several minutes. After etching / pickling, the surface of the component is passivated and dried under defined conditions in a protective atmosphere or in air. This results in the formation of a thin passivation layer of titanium oxide on the surface, from which the porous and electrically conductive precious metal structure protrudes. The precious metal structure exposed in this way forms a porous, electrically conductive, open-pore contact layer that extends into the volume below the contact layer as a catalytically active gas diffusion layer up to the penetration depth of the etching agent.

[0076] An aqueous solution of the aforementioned highly concentrated acids can be easily applied to the titanium alloy component surface to be etched and thus precisely targeted. In principle, it is also possible to etch the titanium alloy both hot and cold. Hot etching is an advantageous and recommended method because it produces a particularly reliable, consistent, and er-2024PF00645

[0077] 17

[0078] This method yields successful results. The etchant is heated before use. Depending on the etchant, it may be necessary to first prepare a solution and activate it accordingly before use, for example, to prepare a titanium etching solution from a crystalline starting material to an aqueous etchant solution. For this, a crystalline starting material is dissolved in distilled water. Sufficient time, heat, and homogeneous stirring are applied to ensure the crystals dissolve completely and become active. The etchant is added to the water, and the aqueous solution is heated and kept warm, for example, between 60°C and 70°C, while being stirred regularly for approximately 30 minutes. Once the etchant is completely dissolved, it is active and ready for use. The etchant can then be used directly for etching, or it can be cooled and stored for later use.In contrast, cold etching advantageously does not require heating equipment, but the results can sometimes be less consistent. The reaction time, i.e., the time the component is exposed to the etchant, ranges from 10 seconds to several minutes.

[0079] In a further preferred embodiment of the process, the selective removal of titanium from the titanium matrix is ​​effected by selective laser-induced etching (SLE), wherein pulsed laser radiation is applied, generating microstructured channels and / or pores.

[0080] Selective laser-induced etching (SLE) has been shown to be a particularly suitable process step for the targeted removal of titanium and the introduction of microchannels and pores in order to incorporate a porous, catalytically active and electrically conductive transport layer into the titanium matrix.

[0081] Selective laser-induced etching (SLE) is a process in which a thin layer of material, namely the titanium matrix, is etched.

[0082] 18

[0083] Materials for planar components, such as titanium expanded metal or titanium micromesh, can be microstructured using focused ultrashort pulsed laser radiation. First, the material is locally illuminated with a femtosecond laser, which increases its etchability. Here, too, masking can be used for targeted and local exposure to the laser pulses. Subsequently, the modified material is removed by wet chemical etching, as described above, to create complex 3D microstructures, microchannels, and pores near the surface and within the bulk. This process therefore particularly advantageously enables the introduction and fabrication of structures such as channels and pores in a gas diffusion layer. The chemical properties of the matrix material are modified and prepared in such a way that the material becomes selectively etchable, allowing for a high degree of geometric freedom.

[0084] The formation of islands rich in precious metals or a continuous layer can be achieved by selectively etching the surface of titanium alloys containing platinum group metals (such as platinum, palladium, rhodium, and ruthenium) as alloying elements. Etching titanium alloys selectively etches only the titanium matrix, leaving behind individual islands or a thin, homogeneous layer of one or more precious metals that exhibits very high corrosion resistance and excellent electrical conductivity. In principle, all components exposed to oxidation in electrochemical cells with Grade 1 or Grade 2 titanium integrated on the anode side are suitable for this etching process. This includes, for example, components of so-called porous transport layers (PTLs) or microporous layers (MPLs), which can be made from fibers or particles of Grade 7 titanium alloys as the base material.

[0085] In a particularly preferred embodiment of the method, at least one alloying element is selected from the elements 2024PF00645

[0086] 19

[0087] the platinum group, comprising ruthenium, rhodium, palladium, osmium, iridium or platinum.

[0088] Particularly preferred for this purpose are alloys such as titanium grade 7 and titanium grade 11 with 0.12–0.25% palladium, but other titanium alloys are also used. Other titanium alloys preferably considered include, for example, titanium-platinum, titanium-ruthenium, or titanium-rhodium alloys, each with a precious metal content of 0.1–10%. Combinations with multiple alloying elements and precious metal components are possible. Iridium is of particular interest as an alloying element in the titanium matrix for creating an anodic gas diffusion layer, for example, to catalyze water splitting at the anode in an electrolysis cell.

[0089] In this process, it is preferably provided that iridium is supplied as an alloying element in a concentration of 0.1 to 0.25% in the titanium matrix.

[0090] In this way, a lower iridium loading per area in the titanium matrix is ​​sufficient to achieve high catalytic efficiency with a large internal surface area in the porous structure after selective titanium dissolution, compared to iridium-coated polymer membranes.

[0091] In a further preferred embodiment of the process, titanium-platinum, titanium-ruthenium, titanium-rhodium or titanium-iridium alloys or mixtures thereof with a precious metal content of 0.1-10% each are provided as titanium-based alloys.

[0092] In a further preferred embodiment of the process, an acidic etchant containing nitric acid (HNOa) or an acid mixture containing hydrofluoric acid (HF) and nitric acid (HNO3) is used as a selective etchant in the etching process. 2024PF00645

[0093] 20

[0094] Another aspect of the invention relates to a gas diffusion electrode for an electrochemical cell, such as an electrolysis cell or a fuel cell, which has a gas diffusion layer produced according to the method.

[0095] By integrating an electrically conductive and catalytically active transport layer of the type PTL or MPL - as described above - into the gas diffusion layer, a gas diffusion electrode can be provided.

[0096] Compared to line-of-sight processes (e.g., PVD sputtering), the material-removing process of the invention, through the application of an etching agent, enables the formation of the precious metal layer even on complex 3D surfaces. A significant advantage over flame spraying is that little to no heat is introduced into the component. This allows a gas diffusion electrode, an essential functional component of an electrochemical cell, to be formed even on thinner titanium components without thermally induced deformation. Furthermore, the bond between the precious metal-rich, catalytically active, and porous electrode layer and the titanium alloy base material is much stronger than with conventional coating processes because the layer is formed from within the base material itself through the etching process.

[0097] According to another aspect of the invention, an electrochemical cell, in particular an electrolysis cell, is specified, comprising a cathodic half-cell and an anodic half-cell, wherein a gas diffusion electrode is inserted into the anodic half-cell.

[0098] To ensure sufficient gas permeability, a gas diffusion electrode of the anodic half-cell manufactured in this way has a gas diffusion layer made of a material with a porous structure. As described, the gas diffusion layer comprises titanium as the base material and embedded alloy (Legie-2024PF00645).

[0099] 21

[0100] The gas diffusion layer can be made of a porous, planar material – such as a titanium-based expanded metal or wire mesh – and provided with the electrically conductive and catalytically active layer, which also leads to a permanent reduction in electrical contact resistance. This increases the service life of such a gas diffusion electrode, reducing the adverse, oxidation-induced degradation effects described above.

[0101] In this system, a gas diffusion electrode, formed from titanium as the base material within a titanium matrix containing a catalytically active precious metal alloy element and another precious metal, is inserted into the anodic half-cell. A fine-mesh titanium material is preferably used as the base material for the gas diffusion layer, for example, titanium fleeces, titanium foams, titanium fabrics, titanium-based expanded metal grids, or combinations thereof. This also increases the local contact points with the electrode and ensures a particularly uniform electrical resistance across the contact area. In this context, the term "grid" refers to a fine-mesh network. The aforementioned substrate materials are characterized by high corrosion resistance. The terms "grid" and "fabric" describe a directional structure, while the term "fleece" describes an undirected structure.

[0102] Another aspect of the invention relates to an electrochemical cell, in particular an electrolysis cell or a fuel cell, which has such a component with a contact layer produced in this way.

[0103] Another aspect of the invention relates to an electrolyzer, in particular a PEM electrolyzer, with a plurality of electrochemical cells designed as electrolysis cells. 2024PF00645

[0104] 22

[0105] Another aspect of the invention relates to a fuel cell assembly with a plurality of electrochemical cells designed in this manner, which are configured as fuel cells.

[0106] The invention is explained below by way of example with reference to the accompanying figures and preferred embodiments, whereby the features shown below can represent an aspect of the invention both individually and in various combinations with one another. The figures show:

[0107] FIG 1 a schematic representation of an electrochemical cell using the example of an electrolysis cell for polymer electrolyte membrane electrolysis;

[0108] FIG 2 schematically shows a sectional view of a gas diffusion layer of an anodic half-cell;

[0109] FIG 3 is a flow diagram illustrating the steps of the production of a gas diffusion layer of an electrochemical cell;

[0110] FIG 4 shows a near-surface sectional view through a planar component as a pre-product before application of the etching agent;

[0111] FIG 5 shows a view of a gas diffusion layer after application of the etching agent to the planar component according to FIG 4.

[0112] FIG 1 shows a schematic cross-sectional view of the basic structure of an electrolysis cell 1 for polymer electrolyte membrane electrolysis (PEM electrolysis). The electrolysis cell 1 serves for the electrolytic production of hydrogen and is one possible application of an electrochemical cell. Another application is shown in ei-2024PF00645.

[0113] 23

[0114] An electrochemical cell is a fuel cell for generating electricity.

[0115] The electrolysis cell 1 has a polymer electrolyte membrane 3. On one side of the polymer electrolyte membrane 3, on the left in the illustration according to Figure 1, is the cathodic half-cell 5 of the electrolysis cell 1, and on the other side of the polymer electrolyte membrane 3, on the right in the illustration according to Figure 1, is the anodic half-cell 7 of the electrolysis cell 1.

[0116] The anodic half-cell 7 comprises an anodic gas diffusion layer 11a arranged directly adjacent to the polymer electrolyte membrane 3. This layer includes an anodic gas diffusion layer 9, which rests on the polymer electrolyte membrane 3. The anodic gas diffusion layer 9 is designed as a porous, electrically conductive, and planar functional component and is directly integrated into the gas diffusion layer 11a and bonded to it. The anodic gas diffusion layer 9 is made of a titanium-based alloy into which an anodic catalyst material 15 made of a precious metal is incorporated. The gas diffusion layer 9, as configured in this way, simultaneously constitutes a gas diffusion electrode 12a within the gas diffusion layer 11a. The gas diffusion electrode 12a lies directly on the polymer electrolyte membrane 3 and exhibits high electrical conductivity and catalytic activity due to the introduced precious metal particles.This is a significant difference compared to a cell structure based on the principle of a membrane electrode assembly, where the electrode is directly applied as a catalytically active electrode layer onto a polymer membrane 3 and connected to it as a component to form a membrane electrode assembly (MEA), e.g., by an electrode-coated polymer membrane 3. In contrast, the gas diffusion electrode 12a inherently provides not only electrical and catalytic properties but also diffusivity and thus the necessary transport properties. The gas diffusion electrode 12a is in operation according to 2024PF00645.

[0117] 24

[0118] This ensures the transport of reactants and products, for example, water as a reactant in PEM water electrolysis and, correspondingly, oxygen or hydrogen as product gases. It is possible that the gas diffusion layer 11a is multilayered and, in addition to the gas diffusion layer 9 forming a gas diffusion electrode 12a, also has several porous and electrically conductive transport layers made of expanded titanium metal or a sintered material, which lie on top of the gas diffusion layer 11a.

[0119] Directly adjacent to the gas diffusion layer 11a, a bipolar plate 21a is arranged in the anodic half-cell 7, thus simultaneously forming a channel structure 13a for fluid transport. The anodic gas diffusion layer 9 contains an anodic catalyst material 15 and catalyzes the anode reaction according to equation (I). Iridium or iridium oxide is chosen as the catalytically active species for the anodic catalyst material 15. It is introduced into the porous gas diffusion layer 9 or was selectively exposed from the titanium base material beforehand as a catalytically active alloying element. This creates pores and / or channels within the gas diffusion layer 9, which contain the catalyst material 15 in fine particles and simultaneously enable effective substance transport, as described above.Iridium oxide exhibits high oxidation and solution stability and is therefore particularly well suited for use as an anodic catalyst material 15. To reduce corrosion, the gas diffusion layer 11a is made of a material on whose surface a passivation layer quickly forms, e.g., titanium. The passivation of the titanium forms titanium dioxide, which, however, has a lower electrical conductivity than metallic titanium. The channel structure 13a is formed by the bipolar plate 21a, thus enabling axial stacking and contacting of a large number of electrolysis cells 1. The comparatively low metal resolution for titanium-based metallic components such as the bipolar plate 21a or the gas diffusion layer 11a is a significant advantage.

[0120] 25

[0121] The oxidative environment during operation of electrolysis cell 1 can be explained by the formation of this near-surface titanium oxide passive layer. However, titanium oxide behaves like a semiconductor, meaning its electrical conductivity is much lower than that of pure titanium. This has the disadvantageous effect that, over extended operating periods, the ohmic losses caused by the formation of titanium oxide significantly affect the conductivity and economic lifespan of electrolysis cell 1. This is counteracted by the gas diffusion electrode 12a with its open-pored and electrically conductive gas diffusion layer 9.

[0122] The cathodic half-cell 5 is constructed in a manner similar to the anodic half-cell 7, but with a material selection adapted to that of the anodic half-cell 7. Here, too, a gas diffusion electrode 12b is incorporated into the cathodic half-cell 5. Accordingly, the cathodic half-cell 5 comprises a porous cathodic gas diffusion layer 17 with a cathodic catalyst material 19, which is arranged directly adjacent to and rests upon the polymer electrolyte membrane 3. The cathodic catalyst material 19 is designed to catalyze the reduction of hydrogen ions (protons), in particular according to equation (II), to molecular hydrogen. Platinum, for example, is used as the cathodic catalyst material 19.Alternatively or additionally to the setup with the gas diffusion electrode 12b, it is possible that in the cathodic half-cell 5 the polymer electrolyte membrane 3 is coated with the cathodic catalyst material 19, so that an electrode layer, e.g., made of platinum, is applied directly to the polymer electrolyte membrane 3. In this alternative embodiment, the design principle of a membrane electrode arrangement (MEA) is therefore retained only in the cathodic half-cell 5, so that, if necessary, only in the anodic half-cell 7 is a gas diffusion electrode 12a, as described above, which rests on the polymer membrane 3 on the anode side. 2024PF00645.

[0123] 26

[0124] The cathodic catalyst material 19 is incorporated into the gas diffusion layer 17. In contrast to the gas diffusion layer 11a of the anodic half-cell 7, the gas diffusion layer 11b of the cathodic half-cell 5 is made of stainless steel as the base material. This choice of material is possible due to the lower oxidation potential in the cathodic half-cell 5 compared to the anodic half-cell 7 and reduces the cost of the electrolysis cell 1. A channel structure 13b is also arranged immediately adjacent to the gas diffusion layer 11b, which, analogous to the anodic half-cell 7, is designed as a bipolar plate 21b. The gas diffusion layers 11a, 11b, in conjunction with the immediately adjacent respective bipolar plates 21a, 21b, functionally form a respective channel structure 13a, 13b, i.e., a fluid-tight flow channel for the transport of the reactants and products during electrolysis.

[0125] Significant operational degradation effects are observed, particularly in the anodic half-cell 7, which limit the service life of the electrolysis cell 1. On the one hand, the high oxygen concentration in the anode-side half-cell 7 and the high oxidative potential during operation lead to damaging corrosion of the materials used. Even the more resistant titanium or a titanium alloy containing a noble metal is subject to oxidative attack. This results in an increase in the local electrical contact resistance during operation. This increase is primarily caused by the rapid oxidation (passivation) of the titanium during operation of the gas diffusion layer 11a or the anodic bipolar plate 21a, which, among other things, serves for electrical contact and current conduction.Oxidation is predominantly observed on the surface of the gas diffusion layer 11a and adjacent current-carrying electrical contact surfaces. These locally poorly conductive contact surfaces, resulting from the oxidation, lead to high ohmic losses in 2024PF00645.

[0126] 27

[0127] of electrolysis cell 1 and a subsequent increase in cell voltage at constant current density. Efficiency losses and degradation, especially of the anodic half-cell 7, are the result of inhomogeneous current distribution with detrimental local current peaks.

[0128] On the side of the cathodic half-cell 5, certain adverse effects can also be observed, especially with regard to acid corrosion promoted by elemental oxygen, but these will not be discussed in more detail here.

[0129] To overcome these disadvantages, at least in the anodic half-cell 7, it is proposed to construct the gas diffusion layer 11a near the surface of the anodic half-cell 7 with a porous, precious-metal-rich gas diffusion layer 9, which has an open-pored, essentially titanium-free or titanium-poor contact layer 14, with a catalytically active and porous structure extending into the volume of the gas diffusion layer 9f. This structure consists of a precious-metal-rich titanium matrix that has been previously treated with an etching process for activation and structuring. This provides a gas diffusion electrode 12a and inhibits, or ideally even largely prevents, the detrimental and ongoing oxidative attack in the anodic half-cell 7 during operation.In the case that a gas diffusion electrode 12b is also implemented in the gas diffusion layer 17 of the cathodic half-cell 5, a corresponding contact layer 14 is provided, which is essentially free of the base material, e.g., stainless steel, and extends into the volume of the gas diffusion layer 19. Platinum is used as the catalyst material 19 on the cathode side, so that a catalytically active and porous structure is provided by the exposure. This structure is previously produced by a selective etching process and catalytically activated by dissolving the base material in the stainless steel matrix. 2024PF00645.

[0130] 28

[0131] FIG. 2 shows a schematic and enlarged sectional view of a section of a gas diffusion layer 9 of an anodic half-cell 7. Here, an electrically conductive and open-pore contact layer 14 of thickness D is formed on a titanium-based alloy. This layer forms part of a porous, catalytically active layer 29, which has a layer thickness h and extends into the metallic base material 27. The near-surface contact layer 14 alone has a layer thickness D of approximately 30 to 50 pm, and the entire catalytically active layer has a layer thickness h of 100 to 300 pm on the base material 27.

[0132] Figure 2 shows an electrically conductive and open-pored contact layer 14 and a corrosion-resistant contact layer 29 formed on a titanium-iridium alloy as the base material 27. Iridium, as a catalytically active precious metal, is embedded as an alloying element in a titanium matrix 33. The illustration demonstrates the mechanism of the surface treatment by etching, whereby a gas diffusion layer 9 was created by dissolving titanium from the titanium matrix 33. In this case, the base body 23 consists, for example, of a titanium-iridium alloy 27 as the base material. Iridium, as a precious metal and alloying element, is embedded or enclosed almost homogeneously in a titanium matrix 33. The individual inclusions of the palladium precious metal are not shown in detail in Figure 3.The surface 35 of the base body 23 is prepared by selectively inducing initial corrosion through the application of an etching agent. An acidic etching agent containing a strong acid, such as nitric acid (HNO₃) or hydrofluoric acid (HF), is applied to the titanium matrix 33, causing titanium from the titanium matrix 33 to be successively dissolved from the surface 35. Due to the targeted near-surface acid action and the local leaching or dissolution of titanium in the area of ​​the surface 35, a porous layer of iridium crystallites 37, initially embedded in the titanium matrix 33, remains.

[0133] 29

[0134] Palladium is deposited on surface 35, with crystallites 37 protruding from the base body 23 near the surface. It is possible that, due to operational factors, an additional thin passivation layer of titanium dioxide (TiO2), not shown in detail, forms on surface 35 through an oxidation reaction with an oxidizing agent. However, this can be largely avoided by selective deep etching of the titanium during continuous metal dissolution, which is desirable in this case. The surface 35 is prepared and adjusted such that the crystallites 37 of the catalytically active noble metal iridium in alloy 27 project above and out of the passivation layer of surface 35 essentially perpendicular to the surface normal. This results in an electrically conductive and open-pored contact layer 14 at the gas diffusion layer 9. Other orientations of the iridium crystallites 37 relative to the surface normal are conceivable.It is also possible that crystallites 37 are optionally formed from other alloying elements of the platinum group or even from mixed crystals and protrude accordingly from the surface 35. This is flexibly adjustable depending on the choice of the precious metal embedded in the titanium matrix 33 as an alloying element and can be adapted to the requirements of a particular component subjected to oxidation. Of particular importance is that the catalytically active layer 29 with a porous structure extends from the surface 35 to a penetration depth h within the alloy 27 even below the open-pore contact layer 14. The deep etching of the titanium matrix 33 creates a gas diffusion layer 9 in which pores and channels with a crystalline internal surface are formed, which contain the catalytically active precious metal crystallites 37.

[0135] The production of a gas diffusion layer 9 or anodic gas diffusion electrode 12b modified and further developed in this way is shown schematically in FIG. 3. A simplified flow diagram is shown, illustrating the process steps for the production of a 2024PF00645

[0136] 30

[0137] Gas diffusion layer 9 – or rather a gas diffusion electrode 12b – of an electrochemical cell is illustrated. References to the embodiments shown in FIGS. 4 and 5, which are discussed further below, are made with respect to the individual elements in the illustration of the manufacturing process.

[0138] In the process for producing a gas diffusion layer 9, a planar component comprising a titanium-based alloy 27 is first provided in step S1. The alloy 27 contains at least one catalytically active noble metal, such as iridium or platinum, embedded in a titanium matrix 33. In a further step S2, an etching agent containing hydrofluoric acid (HF) is applied to the surface 35 of the planar component, whereby material from the titanium matrix 33 is selectively etched away. The etching agent is introduced into the material to a large penetration depth h of more than 100 pm, e.g., 250 pm, and a dwell time is set. For a noble metal-containing titanium matrix, a removal or dissolution rate of the titanium of typically about 0.5 to 1.5 pm per minute is set.Depending on the exposure time, titanium as an alloying element is selectively etched out of the titanium matrix, both near the surface and within the volume of the planar component, i.e., dissolved from the alloy. Accordingly, in step S3, material of the alloying element is successively exposed, and the titanium dissolved by the hydrofluoric acid (HF) is flushed out of the structure. This process forms an electrically conductive and open-pore contact layer 14 near the surface of the planar component, containing the catalytically active precious metal. It is intended that in step S4, by ensuring progressive exposure to and penetration with the etching agent, a selective dissolution of titanium from the titanium matrix 33 is achieved down to the desired penetration depth h below the open-pore contact layer 14. This results in a gas diffusion layer 9 with a catalytically active layer 29 having a porous structure and with the 2024PF00645.

[0139] 31

[0140] A layer thickness h is formed within the alloy 27. It is advantageous to provide a preparation step SO in which a masking element 25, e.g., in the form of a structured mask, an optical grating, or a lacquer layer, is applied to the surface 35 of the planar component to ensure uniform distribution, dosage of the etchant, and exposure of the alloy. This allows for targeted penetration and distribution of the etchant. The process can be advantageously extended to selective laser-induced etching by applying pulsed laser radiation, wherein the masking element 25 then has an optical grating or is designed as an optical grating. In this process, the surface 35 and the deeper volume regions below the surface 35 are pretreated and prepared by intense pulsed laser radiation, creating microstructured channels or pores.A selective etching agent is an acidic etching agent containing nitric acid HNOa or a concentrated acid mixture containing hydrofluoric acid HF and nitric acid HNOa, possibly then in combination with pulsed laser radiation.

[0141] The production or targeted formation of the electrically conductive, open-pore and catalytically active layer 29 on the base body 23 of a gas diffusion layer 11a as an oxidation-stressed component of the electrolysis cell 1, as well as the structure of the open-pore contact layer 14, is illustrated and explained below with reference to FIG 4 and FIG 5.

[0142] Figure 4 shows a near-surface sectional view through an oxidation-stressed, planar component before the application of the etching agent. Figures 4 and 5 also illustrate the process by comparison with the process steps SO, SI, S2, S3, and S4 explained in Figure 3 for preparing a gas diffusion layer 9 on the surface 35. The planar component has a curved surface 35. Inclusions or crystallites of one or more precious metals from the 2024PF00645 are embedded in the titanium matrix 33.

[0143] 32

[0144] Platinum group embedded, for example iridium or platinum as a catalytically active precious metal, so that in a first process step S1 a component made of titanium alloyed with precious metals of the platinum group is provided. As a preparatory step in the process, a masking element 25 can be used in a preceding step SO and a pulsed laser 39, which supports the wet chemical etching with the etchant and prepares the incidence surfaces for the chemical treatment.

[0145] In a further process step S2, the surface 35 is selectively exposed to the etchant, and the titanium matrix 33 is selectively etched. This selectively removes titanium from the titanium matrix 33 near the surface to a depth D. This exposes the material of the embedded alloying element, so that finally, in a process step S3, an electrically conductive and open-pored, low-titanium or titanium-free contact layer 14 with precious metal as the layer material 31 is formed near the surface. The catalytically active layer 29 is designed as a porous layer and has a porosity that can be adjusted via the etching process by selectively exposing the material. This is achieved by successive depth etching, whereby, if necessary, the incidence of pulsed laser radiation via the laser 39 and wet chemical treatment with the etchant are carried out for a period of approximately 200 to 300 minutes.In this way, a porous and catalytically active layer 29 with a layer thickness of approximately 200 pm to 300 pm can be formed, as shown in FIG. 5, whereby the titanium is dissolved, carried away, or washed out. The masking element 25 can have a microstructured mask by means of which the liquid etchant can be metered and applied locally and selectively to the surface in a structured manner. The masking element 25 can also have a microstructured optical grating, so that the pulsed laser beam of the laser 39 optically imprints a structure onto the surface and prepares it for selective etching. This imprinted structure promotes [2024PF00645].

[0146] 33

[0147] The effect of hydrofluoric acid (HF) and / or nitric acid (HNOa) as a liquid etchant is intensified accordingly. The process can be carried out intermittently or continuously, alternating between laser incidence and wet chemical application of the etchant.

[0148] The electrically conductive contact layer 14 shown in FIG. 5 is, in this example, a thin, homogeneous, continuous, and porous layer with a thickness D of crystallites 37. It is also possible for several noble-metal-rich islands to be formed, which may be continuous or separate and extend uniformly and densely across the surface 35. The thickness D of the contact layer 14 resulting from the etching process by dissolving titanium metal is adjustable over a wide range and can be between approximately 5 nm and 50 pm. Typically, a thickness D of approximately 50 nm to 5 pm is used for the electrically conductive, open-pore contact layer 14. Beneath the contact layer 14, the porous and catalytically active layer 29 continues in volume with a total thickness of approximately 200 pm to 300 pm, which is thus many times greater than the thickness D of the near-surface contact layer 29.This creates an integrated gas diffusion layer 9 in the original titanium matrix 33 base material by selective deep etching, which can be used as an anodic gas diffusion electrode 12a .

[0149] Compared to conventional PVD coating processes, the material-removing, wet-chemical process of the invention, through the application of an etching agent, enables the formation of the precious metal layer even on complex 3D surfaces. A significant advantage over flame spraying is that little to no heat is introduced into the component, allowing a contact layer to be formed even on thinner titanium components without thermally induced deformation. Furthermore, the bond between the precious metal-rich contact layer and the base material of the titanium alloy is much better than with conventional coatings.

[0150] 34

[0151] tungsvergänse, because the formation of the layer from the base material takes place through the etching process selectively applied to the surface 35 of the component.

[0152] The thickness D of the contact layer 14 is determined based on the specific component or part and ranges from approximately 5 nm to 50 pm, preferably between 50 nm and 5 pm, allowing it to be relatively thin for many applications. The further penetration depth h is adjusted via the etching depth, which in turn is adjustable via the exposure time of the etching agent applied to the surface of the component. Larger layer thicknesses h are easily achievable for layer 29 with appropriate exposure time and depth etching, optionally with laser assistance, into the titanium matrix 33. This process allows for a greater penetration depth h with mechanical elasticity and, due to the porosity, very good fluid transport properties. This layer 29 is provided with a porous, catalytically active noble metal structure, which also exhibits the necessary fluid transport properties.Thus, for the installation situation and operation in an electrochemical cell, a certain spring elasticity can additionally be ensured by the morphology of the near-surface contact layer 14 and the overall structure of layer 29.

Claims

2024PF00645 Patent claims 1. Method for producing a gas diffusion layer ( 9, 17 ) for an electrochemical cell, in particular an electrolysis cell ( 1 ) comprising the steps: (51) Provision of a planar component comprising a titanium-based alloy (27) which includes as an alloying element at least one catalytically active precious metal embedded in a titanium matrix (33), (52) Applying an etching agent to a surface (35) of the planar component, wherein material of the titanium matrix (33) is removed by selective etching, wherein the etching agent is introduced into the material to a penetration depth (h), (53) Exposure of material of the alloying element such that an electrically conductive open-pore contact layer ( 14 ) is formed near the surface, which contains the catalytically active precious metal . (54) Selective extraction of titanium from the titanium matrix (33) to the penetration depth (h) below the open-pore contact layer (14) is formed, forming a catalytically active layer (29) with a porous structure and layer thickness (h) within the alloy (27).

2. Method according to claim 1, wherein the application of the etching agent causes a selective dissolution of titanium from the titanium matrix (33), leaving channels or pores with a crystalline internal surface containing catalytically active noble metal crystallites (37).

3. A method according to claim 1 or 2, wherein, prior to the application of the etchant in step (S2), a microstructured mask is applied to the surface (35) of the planar component in a preparation step (SO), thereby effecting selective exposure and targeted penetration of the etchant into the alloy (27). 2024PF00645 36 4. Method according to any of the preceding claims, wherein a wet chemical etching process is used, wherein selective removal of titanium from the titanium matrix is ​​effected by the application of an etching agent containing hydrofluoric acid (HF).

5. A method according to any of the preceding claims, wherein selective removal of titanium from the titanium matrix is ​​effected by selective laser-induced etching (SLE), wherein pulsed laser radiation is applied, and microstructured channels or pores are generated.

6. A method according to any of the preceding claims, wherein an alloying element is selected from the elements of the platinum group, comprising ruthenium, rhodium, palladium, osmium, iridium or platinum.

7. Method according to claim 6, wherein iridium is provided as an alloying element in a concentration of 0.1% to 0.25% in the titanium matrix (33).

8. Method according to claim 6 or 7, wherein titanium-platinum, titanium-ruthenium, titanium-rhodium or titanium-iridium or mixtures thereof, each with a precious metal content of 0, 1-10%, is provided as the titanium-based alloy.

9. Method according to one of the preceding claims, wherein an acidic etchant containing nitric acid (HNOa) or an acid mixture containing hydrofluoric acid (HF) and nitric acid (HNOa) is used as the selective etchant.

10. Gas diffusion electrode ( 12a, 12b) with a gas diffusion layer ( 9) produced according to a method according to any one of the preceding claims 2 to 10 .

11. Electrochemical cell, in particular electrolysis cell ( 1 ) , comprising a cathodic half-cell (5) and an anodic half-cell (7 ) , in which the anodic half-cell (7 )2024PF00645 37 a gas diffusion electrode ( 12a) according to claim 10 is inserted.