Conversion element, method for producing a plurality of conversion elements, and optoelectronic device
A substrate-free conversion element with a polysiloxane matrix and phosphor particles addresses thermal stress and environmental hazards, achieving efficient wavelength conversion and cost savings in amber LED production.
Patent Information
- Application Number
- PCT/EP2026/060262
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-04-09
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional phosphor-in-matrix-on-substrate converters face issues such as thermal stress, high surface roughness, and environmental hazards due to the use of toxic materials, along with high production costs and complex processing requirements, particularly in amber LED applications.
A conversion element comprising a polysiloxane matrix with incorporated phosphor particles and filler particles, free from a substrate, which allows for improved thermal stability, reduced surface roughness, and cost-effective production, using a method that avoids toxic materials and reduces processing complexity.
The solution provides a conversion element with low surface roughness, improved mechanical properties, and efficient wavelength conversion, suitable for high-power applications like automotive LEDs, while eliminating toxic materials and reducing production costs.
Smart Images

Figure EP2026060262_19112026_PF_FP_ABST
Abstract
Description
[0001] 2024PF01861 April 9, 2026
[0002] P2025, 0059 WO N
[0003] 1
[0004] Description
[0005] CONVERSION ELEMENT, METHOD FOR PRODUCING A PLURALITY OF CONVERSION ELEMENTS, AND OPTOELECTRONIC DEVICE
[0006] A conversion element, a method for producing a plurality of conversion elements, and an optoelectronic device are specified.
[0007] It is an obj ect to provide a conversion element with improved properties. Furthermore, it is an obj ect to provide a method for producing a plurality of conversion elements with improved efficiency. It is also an obj ect to provide an optoelectronic device with improved performance.
[0008] According to at least one embodiment, a conversion element is provided. In particular, the conversion element is configured to convert electromagnetic radiation of a first wavelength range into electromagnetic radiation of a second wavelength range, in particular from higher energy to lower energy, such as from blue light to green light. For example, the electromagnetic radiation of the first wavelength range is provided by a light-emitting semiconductor chip on which the conversion element can be arranged.
[0009] According to at least one embodiment, the conversion element comprises a polysiloxane. A polysiloxane can comprise or consist of M-units (R3SiO-), D-units (-OR2SiO-), and / or
[0010] T-units (-ORSiO2-). Furthermore, Q-units (-OSiO3-) may be present in a polysiloxane, or a polysiloxane may be free of Q-units. In contrast to a silicone, the polysiloxane can comprise T-units. For example, a polysiloxane can be formed2024PF01861 April 9, 2026
[0011] P2025, 0059 WO N
[0012] - 2 -
[0013] from a polysiloxane precursor which comprises the M-units, D-units, and / or T-units.
[0014] The polysiloxane can create a 3D-network and, thus, form a matrix phase in which, for example, phosphor particles and / or other fillers may be incorporated into the matrix phase, thus forming a composite structure. If phosphor particles are present, the conversion element can also be called a phosphor-in-matrix (PiM) conversion element, or a phosphor-in-polysiloxane (PiX) conversion element.
[0015] According to at least one embodiment, the conversion element comprises first phosphor particles and second phosphor particles. In particular, the first phosphor particles are different from the second phosphor particles. Together they form a mixture or blend of phosphor particles, which is incorporated into the matrix phase.
[0016] In particular, the first phosphor particles and the second phosphor particles convert the electromagnetic radiation of the first wavelength range (primary radiation) into electromagnetic radiation of a second wavelength range (secondary radiation). The second wavelength range is composed of the radiation converted by the first phosphor particles and the radiation converted by the second phosphor particles. In other words, wavelength converting properties of the conversion element arise from the first and second phosphor particles. For example, the first phosphor particles and the second phosphor particles may be independently chosen from any phosphor that is known to absorb light for example in the near UV to blue region of the electromagnetic spectrum and emit electromagnetic radiation for example in the visible region of the electromagnetic spectrum. Any combination of2024PF01861 April 9, 2026
[0017] P2025, 0059 WO N
[0018] 3
[0019] the first and second phosphor particles with additional known phosphors is applicable as well.
[0020] The first and second phosphor particles may be independently chosen from inorganic compounds, for example, from ceramic phosphors and quantum dot phosphors. A ceramic phosphor comprises, for instance, a material selected from the group consisting of a garnet, a nitride, an oxynitride, SiAlONs, an oxynitridosilicate, a perovskite, a silicate, and combinations thereof, each doped with at least one appropriate element.
[0021] For example, the first and second phosphor particles are independently selected from the following group: (RE1-xCex)3(Al1-yA'y)5O12with 0 < x < 0.1 and 0 < y < 1, (RE1-xCex)3(Al5-2yMgySiy)O12with 0 < x < 0.1 and 0 < y < 2, (RE1-xCex)3Al5-ySiyO12-yNywith 0 < x < 0.1 and 0 < y < 0.5, (RE1-xCex)2CaMg2Si3O12:Ce3+with 0 < x < 0.1, (AE1-xEux)2Si5N8with 0 < x < 0.1, (AE1-xEux)AlSiN3with 0 < x < 0.1, (AE1-xEux)2Al2Si2N6with 0 < x < 0.1, (Sr1-xEux)LiAl3N4with 0 < x < 0.1, (AE1-xEux)3Ga3N5with 0 < x < 0.1, (AE1-xEux)Si2O2N2with 0 < x < 0.1, (AExEuy)Si12-2x-3yAl2x+3yOyN16-ywith 0.2 < x < 2.2 and 0 < y < 0.1, (AE1-xEux)2SiO4with 0 < x < 0.1, (AE1-xEux)3Si2O5with 0 < x < 0.1, K2(Si1-x-yTiyMnx)F6with 0 < x < 0.2 and 0 < y < 1-x, (AE1-xEux)5(PO4)3Cl with 0 < x < 0.2, (AE1-xEux)Al10O17with 0 < x < 0.2, wherein RE is one or more of Y, Lu, Tb and Gd, AE is one or more of Mg, Ca, Sr, Ba, A' is one or more of Sc and Ga, wherein the phosphors optionally include one or more of halides.
[0022] In particular, the first phosphor particles comprise or consist of a garnet, and the second phosphor particles comprise or consist of a nitride.
[0023] 2024PF01861 April 9, 2026
[0024] P2025, 0059 WO N
[0025] According to at least one embodiment, the conversion element comprises fumed silica. In particular, fumed silica comprises or consists of silica nanoparticles. The addition of fumed silica may alter the rheology of the slurry during the production of the conversion element. Increasing the fumed silica content can increase the viscosity and thixotropy of such a slurry.
[0026] According to at least one embodiment, the conversion element comprises filler particles. By adding filler particles to a formulation or composition of a conversion element, the solids content is increased, while the polysiloxane content may be decreased. Various properties of the conversion element may be altered and adapted by adding filler particles. The filler particles are, in particular, chosen from high purity fillers, i. e., from filler particles with only traces of impurities or even no impurities. Thus, an impact on absorption and / or emission properties of the conversion element through the filler particles is reduced or avoided.
[0027] According to at least one embodiment, the filler particles comprise a total content being chosen from the range between and including 20 vol% and 40 vol%, in particular between and including 25 vol% and 36 vol%, for example between and including 27 vol% and 34 vol%. Such a total content of filler particles increases the solids content in the conversion element and allows for decreasing the content of polysiloxane. Additionally, such a total content of filler particles allows for a content of first and second phosphor particles that is high enough for achieving full conversion of the primary radiation into a secondary radiation. Thus,2024PF01861 April 9, 2026
[0028] P2025, 0059 WO N
[0029] 5
[0030] for example, an amber light emitting device can be realized with a conversion element as described here.
[0031] According to at least one embodiment, a conversion element is provided, the conversion element comprising:
[0032] - a polysiloxane,
[0033] - first phosphor particles and second phosphor particles,
[0034] - fumed silica, and
[0035] - filler particles,
[0036] wherein a total content of the filler particles is chosen from a range between and including 20 vol% and 40 vol%.
[0037] The conversion element is a PiM or, respectively, PiX conversion element, i. e., a free-standing conversion element. Compared to conventional phosphor-in-matrix-on-substrate (PiMoS) converters, the free-standing conversion element is not bonded to a substrate, i. e., is free of any substrate.
[0038] Limitations that are known for conventional phosphor-in-matrix-on-substrate (PiMoS) converters, like phosphor-in-polysiloxane-on-glass (PiXoG) converters, can be minimized or avoided with the conversion element as described here. For example, as the conversion element is free of a substrate it can shrink during curing without creating stresses and, thus, camber, as there is no thermal expansion mismatch between the conversion layer and a substrate. Lower stress allows for improving other properties such as the surface roughness, which may be very low. Conversion elements with lower surface roughness improve device performance when being used in devices, such as light emitting diodes (LED). Furthermore, the thickness of the conversion element can be varied over a wide range by adjusting the phosphor concentration. Moreover, when producing the conversion element, a good thickness
[0039] 2024PF01861 April 9, 2026
[0040] P2025, 0059 WO N
[0041] 6
[0042] control can be realized which allow for thickness tolerances that are lower than in conventional PiXoG converters.
[0043] Additionally, due to its composition, the conversion element as described here may offer several advantages over conventional converters, in particular conventional fullconversion converters. The blend of at least the first and second phosphor particles is incorporated in a matrix phase containing polysiloxane. The polysiloxane forms a thermal stable resin which may be applied in high temperature applications, like for example in the automotive field.
[0044] Furthermore, the first and second phosphor particles may be chosen and blended in a ratio to modify the emitted color and / or the performance of the conversion element.
[0045] Furthermore, the conversion element may be produced with a method, which does not require extensive processing and that has cost saving opportunities.
[0046] Additionally, due to the composition of the components of the conversion element as described here, it can be produced with an optimized process, such that a conversion element with low camber, low surface roughness, low edge chipping, and mechanical properties adequate for subsequent processing into LED devices results. The conversion element as described here may, thus, achieve the performance and reliability for automotive LED applications, for example for amber automotive LED applications.
[0047] Conventional phosphor-converted amber LEDs contain phosphor powder or phosphor ceramic. Phosphor-converted amber LEDs using phosphor powder is normally made by mixing phosphors2024PF01861 April 9, 2026
[0048] P2025, 0059 WO N
[0049] 7
[0050] with silicone first, and then cast the slurry of phosphors and silicone around a blue LED chip in LED packages, also known as volume converter. Due to a high organic content of silicone, the phosphor powder in the silicone cannot withstand high power and high temperature applications.
[0051] Conventional amber phosphor ceramics are prepared using
[0052] (Ba, Sr )2Si5N8: Eu powders and a high temperature spark plasma sintering (SPS) process (up to about 1650°C) which results in a sintered amber ceramic cylinder. Since the conventional amber full conversion ceramics process needs high temperature ceramic sintering, and multiple mechanical singulation steps, it requires expensive capital equipment investment and is also labor intense. Another major disadvantage for amber full conversion ceramic is that it contains toxic Ba in its starting powder, which is a not environmentally friendly material.
[0053] In contrast, the conversion element as described here has a flexibility for phosphor particles that can be used to modify the color and / or the performance of the conversion element and that are incorporated in a thermally stable polysiloxane matrix phase. In particular, it allows the use of Ba-free first and second phosphor particles. Thus, toxic Ba waste stream can be eliminated which additionally offers cost savings.
[0054] According to at least one embodiment, the first phosphor particles differ from the second phosphor particles in at least one of composition, shape, size, and emission color.
[0055] The first and second phosphor particles may comprise a range of particle sizes, for example chosen from a range between2024PF01861 April 9, 2026
[0056] P2025, 0059 WO N
[0057] - 8 -
[0058] and including 10 µm and 30 µm. Here and in the following sizes are specified by d50-values of the respective particles. According to at least one embodiment, the first phosphor particles have a different size than the second phosphor particles.
[0059] Additionally, or alternatively, the first and / or second phosphor particles may be surface treated. Surface treatment of phosphor particles may be used to promote improved bonding of the first and / or second phosphor particles in the conversion element, i. e. in the matrix phase formed by the polysiloxane. Surface treatment of phosphor particles may also be used to improve resistance to environmental factors, such as moisture, of the first and / or second phosphor particles in the conversion element.
[0060] Additionally, or alternatively, the first and second phosphor particles may comprise a range of shapes. Exemplary shapes are sphere-like or boulder-like shapes or shapes comprising corners, like a brick-like shape. The shapes of the first and / or second phosphor particles may comprise an aspect ratio, i. e. a variable ratio between a width and a height of the respective particles. As an example, the first phosphor particles comprise a sphere-like or boulder-like shape and the second phosphor particles comprise a shape with an aspect ratio.
[0061] Additionally, or alternatively, the compound for the first and second phosphor particles may be chosen such that their mixture leads to a total emission having a desired emission color, for example amber light. For example, the first phosphor particles are chosen from garnets, and the second phosphor particles are chosen from nitrides.
[0062] 2024PF01861 April 9, 2026
[0063] P2025, 0059 WO N
[0064] According to at least one embodiment, a total emission of the first phosphor particles and the second phosphor particles is chosen from the amber range of the electromagnetic spectrum. The total emission is the mixture of emissions of both, the first phosphor particles and the second phosphor particles. The amber range of the electromagnetic spectrum can be chosen from a wavelength range between and including 570 nm and 640 nm.
[0065] According to at least one embodiment, the conversion element comprises at least one surface having an average surface roughness (Sa) of less than 0.2 pm, in particular less than 0.15 pm. An average surface roughness (Sa) is to be understood as an arithmetical mean height and is defined in the ISO 25178 standard. It is defined as the average deviation of individual heights and depths from a mean height plane. The at least one surface of the conversion element is in particular the surface which will be applied on a semiconductor chip in an optoelectronic device, which can be also called bottom surface. Such a low average surface roughness contributes to an improved device performance of an optoelectronic device comprising the conversion element.
[0066] According to at least one embodiment, the conversion element comprises at least one surface having a maximum peak height (Sp) of less than 1 pm, in particular of less than 0.75 pm. The maximum peak height describes the peak height of the highest peak, i. e. the highest height above the average surface height. The maximum peak height is also defined in the ISO 25178 standard. The at least one surface of the conversion element is in particular the surface which will be applied on a semiconductor chip in an optoelectronic device.2024PF01861 April 9, 2026
[0067] P2025, 0059 WO N
[0068] - 10 -
[0069] A low average surface roughness Sa and / or a low maximum peak height Sp at the surface of the conversion element to be applied on and bonded to a semiconductor chip of an optoelectronic device, impacts the performance of an optoelectronic device such as an LED device. In general, a low surface roughness allows for decreasing a bondline thickness, i. e., the thickness of an adhesive layer required to bond the conversion element to the chip, resulting in increased brightness of optoelectronic device. The low surface roughness may be realized, for example, by the increased thickness and, thus, decreased phosphor particle content of the conversion element.
[0070] According to at least one embodiment, the polysiloxane has a content being chosen from a range between and including 15 vol% and 45 vol%, in particular between and including 28 vol% and 38 vol%, for example between and including
[0071] 30 vol% and 35 vol%. The content of polysiloxane means the total content, irrespective of different kinds of polysiloxanes, if present. Here and in the following, values of volume percent refer to the respective component in the cured conversion element.
[0072] According to at least one embodiment, the polysiloxane comprises T-units and D-units, wherein a content of D-units is within a range between and including 0 vol% and 10 vol%, in particular between and including 0 vol% and 8 vol%, for example between and including 3 vol% and 6 vol%. Thus, the conversion element comprises or consists of T-units or comprises or consists of T-units and D-units, wherein the content of D-units is within the above-mentioned range. By adding a certain content of D-units, the content of T-units2024PF01861 April 9, 2026
[0073] P2025, 0059 WO N
[0074] - 11 -
[0075] ls decreased. While the T-unit polysiloxane can create a 3D-network, the D-unit polysiloxane can be used to modify the matrix phase by breaking up the 3D-network of the T-unit polysiloxane, thus decreasing the stiffness, i. e., the storage modulus, of the matrix phase. Generally, it is possible to add 30 vol% or more of a D-unit polysiloxane to a T-unit polysiloxane. In other words, D-unit polysiloxanes and T-unit polysiloxanes show good compatibility.
[0076] A polysiloxane comprising T-units comprises or consists of, for example, a polymethylsiloxane. A D-unit polysiloxane comprises or consists of, for example, a hydroxyl-terminated polydimethylsiloxane. An exemplary polydimethylsiloxane is shown in formular la. Formula lb shows the corresponding D-unit, i. e. the dimethylsiloxane unit:
[0077]
[0078] Ia Ib
[0079] According to at least one embodiment, the D-unit polysiloxane comprises a molecular weight in a range between and including 400g / mol and 2000 g / mol, in particular in a range between and including 700 g / mol and 1500 g / mol. Thus, a low molecular weight D-unit polysiloxane is used for the conversion element.
[0080] According to at least one embodiment, the fumed silica comprises a content being chosen from a range between and including 0.5 vol% and 7 vol%, in particular between and including 1 vol% and 5 vol%, for example between and including 2 vol% and 4 vol%.
[0081] 2024PF01861 April 9, 2026
[0082] P2025, 0059 WO N
[0083] 12
[0084] According to at least one embodiment, the fumed silica comprises a surface area in a range between and including 50 m2 / g and 600 m2 / g. The presence of fumed silica can alter the rheology of a slurry during the preparation of the conversion element. Increasing the content of fumed silica in a slurry increases the viscosity and thixotropy thereof.
[0085] According to at least one embodiment, the conversion layer has a thickness being chosen from a range between and including 90 pm to 150 pm. In particular, the thickness of the conversion element is chosen from a range between and including 115 pm and 135 pm. Here and in the following, with the thickness the spatial extent perpendicular to a main extension area of the conversion element is meant. The thickness of the conversion element can impact the performance and the mechanical robustness of the conversion element during its subsequent processing.
[0086] According to at least one embodiment, the filler particles comprise at least one of silica powder, siloxane powder, and modified siloxane powder. According to at least one embodiment, the silica powder comprises at least one of fused silica powder and crystalline silica powder. According to at least one embodiment, the filler particles comprise or consist of at least one of fused silica powder and modified siloxane powder.
[0087] Generally, by adding filler particles to the formulation or composition of a conversion element, the solids content is increased, while the polysiloxane content may be decreased. Various properties of the conversion element may be altered and adapted by adding filler particles. The filler particles are, in particular, chosen from high purity fillers, i. e.,2024PF01861 April 9, 2026
[0088] P2025, 0059 WO N
[0089] 13
[0090] from filler particles with only traces of impurities or even no impurities. Thus, an impact on absorption and / or emission properties of the conversion element through the filler particles is reduced or avoided.
[0091] According to at least one embodiment, the filler particles have a spherical shape. According to at least one embodiment, the filler particles have a narrow particle size distribution. In particular, the filler particles have a spherical shape and a narrow particle size distribution.
[0092] According to at least one embodiment, the filler particles comprise a size chosen from the range between and including 0.3 pm to 20 pm, in particular between and including 0.5 pm to 8 pm, for example between and including 0.8 pm and 5 pm. Here and in the following, the particle sizes are to be understood as d50 values.
[0093] According to at least one embodiment, the filler particles comprise at least first filler particles of a first size and second filler particles of a second size, wherein the first size is chosen from a first sub-range within the range between and including 0.3 µm and 20 µm and the second size is chosen from a second sub-range within the range between and including 0.3 µm and 20 µm. " At least" means, that more filler particles, for example third filler particles of a third size and / or fourth filler particles of a fourth size, may also be present, wherein the third size is chosen from a third sub-range within the range between and including 0.3 pm and 20 pm and / or the fourth size is chosen from a fourth subrange within the range between and including 0.3 pm and
[0094] 20 pm. In particular, all sub-ranges are different from each other. Thus, a blend of filler particles of different sizes2024PF01861 April 9, 2026
[0095] P2025, 0059 WO N
[0096] - 14 -
[0097] may be present in the conversion element. For example, the first sub-range comprises between and including 0.8 pm and 1 pm, the second sub-range comprises between and including 1.5 pm and 2 pm, and, if third filler particles are present, the third sub-range comprises between and including 3.5 pm and 4.5 pm, for example 4 pm. Blending filler particles with different sizes can improve and optimize the particle packing in the matrix phase and further reduce the surface roughness of the conversion element.
[0098] According to at least one embodiment, the modified siloxane powder comprises a reduced silanol content and optionally a reduced CH3-group content with respect to the siloxane powder. According to at least one embodiment the modified siloxane powder comprises a reduced silanol content while maintaining the CH3-group content with respect to the siloxane powder. According to at least one embodiment, the modified siloxane powder comprises a particle size in the range of between and including 0.3 pm and 5 pm, in particular 0. 8 pm and 4 pm.
[0099] According to at least one embodiment, the conversion element is free of a substrate. Thus, the conversion element is a free-standing conversion platelet.
[0100] Furthermore, a method for producing a plurality of conversion elements is specified. In particular, the method is used to produce the conversion element described herein. Thus, features, embodiments and advantages described in combination with the conversion element also apply to the method and vice versa.
[0101] 2024PF01861 April 9, 2026
[0102] P2025, 0059 WO N
[0103] 15
[0104] According to at least one embodiment, the method comprises the step of preparing a slurry comprising a polysiloxane precursor, first phosphor particles, second phosphor particles, fumed silica, and filler particles. During the method, from the polysiloxane precursor the polysiloxane is formed. In particular, the slurry comprises high purity polysiloxane precursor, high purity first phosphor particles, high purity second phosphor particles, high purity fumed silica, and high purity filler particles.
[0105] For example, the polysiloxane precursor, the first phosphor particles, the second phosphor particles, the fumed silica, and the filler particles are blended to form the slurry. In particular, the components of the slurry are mixed to be blended and milled to ensure a good dispersion of the first and second phosphor particles, the filler particles, and the fumed silica in the polysiloxane.
[0106] Furthermore, a hardener may be added to the slurry. The choice of hardener depends on the polysiloxane resin being used. The hardener may be selected from titanium alkoxides (e. g., titanium n-butoxide), zirconium alkoxides, aluminum alkoxides, organo-tin compounds, amines (e. g., tetra methyl guanidine), or combinations thereof. The hardener might be present in an amount between and including 0.1 wt% and 5 wt% based on the polysiloxane content. A hardener may be chosen that is compatible with the slurry, such that no precipitants, no gelation, and no significant thickening of the slurry occurs before further processing, for example before a curing step.
[0107] Additionally or alternatively, a solvent may be added to the slurry. A solvent may be chosen such that the viscosity of2024PF01861 April 9, 2026
[0108] P2025, 0059 WO N
[0109] - 16 -
[0110] the slurry is adjusted to optimize, for example, the slurry tape casting process. The solvent may be removed during, for example, a curing step. A typical solvent for a methyl methoxy polysiloxane resin containing slurry is butyl acetate.
[0111] According to at least one embodiment, a total content of the filler particles is chosen from a range between and including 20 vol% and 40 vol%. The content range refers to the cured conversion element, thus, the slurry may comprise a slightly different total content of filler particles. Such a total content of filler particles enables a phosphor particles content which is necessary for full conversion of primary radiation into secondary radiation.
[0112] According to at least one embodiment, a conversion sheet is produced from the slurry. According to at least one embodiment, the conversion sheet comprises a thickness, in particular a casting thickness, chosen from a range between and including 150 pm and 300 pm, in particular between and including 180 pm and 270 pm. A length of the conversion sheet may be variable depending on the quantity of the slurry. The conversion sheet length comprises, for example, 0.5 meter to 5 meters. The conversion sheet can be trimmed into smaller sheets comprising, for example, a lateral dimension of 10.16 cm x 15.24 cm (4" x 6") for ease of handling.
[0113] According to at least one embodiment, the conversion sheet is cured. In this step, the polysiloxane precursor transforms to the polysiloxane forming the matrix phase in which the phosphor particles, the filler particles and the fumed silica are incorporated into the matrix phase. Thus, a cured conversion sheet is formed.
[0114] 2024PF01861 April 9, 2026
[0115] P2025, 0059 WO N
[0116] 17
[0117] According to at least one embodiment, the method comprises the step of singulating the cured conversion sheet into conversion elements. In this step, a plurality of conversion elements is formed which have desired length, width, and thickness dimensions. Depending on the dimensions of each conversion element, a certain number of conversion elements is produced when singulating the cured conversion sheet.
[0118] According to at least one embodiment, a method for producing a plurality of conversion elements is provided, the method comprising the steps of:
[0119] - preparing a slurry comprising a polysiloxane precursor, first phosphor particles, second phosphor particles, fumed silica, and filler particles, wherein a total content of the filler particles is chosen from a range between and including 20 vol% and 40 vol%,
[0120] - producing a conversion sheet from the slurry,
[0121] - curing the conversion sheet, and
[0122] - singulating the cured conversion sheet into conversion elements.
[0123] With this method, conversion elements with good performance and high reliability can be produced. Additionally, this method can be performed with reduced costs compared to methods for producing conventional converters.
[0124] In particular, materials can be saved, as no substrate, for example no glass substrate, is necessary. The material saving also contributes to a simplification of some method steps, for example of the production of the conversion sheet and of the singulation of the cured conversion sheet.
[0125] 2024PF01861 April 9, 2026
[0126] P2025, 0059 WO N
[0127] 18
[0128] The absence of a substrate also minimizes or avoids additional stresses during curing and thereby shrinking of the PiX layer. Thus, conversion elements without curl or camber can be achieved with this method. Lower stress during curing improves also other properties of the produced conversion element, such as the surface roughness. As with this method conversion elements of a high thickness can be produced, the phosphor content in the conversion layer may be decreased, which reduces surface roughness even more.
[0129] Additionally, the conversion sheet may be produced on a very smooth and flat surface, for example on a tape casting film. This provides also an exceptionally smooth surface on the surface of the conversion sheet being in contact with the smooth surface. A lower surface roughness can lead to improved performance of a device comprising the conversion element.
[0130] Furthermore, the singulation can be performed while producing edges and corners of the conversion elements of high quality. This means, after singulation the conversion elements comprise very smooth edges and corners without or with only a few phosphor particle pullouts and having low chipping. A tight dimensional control during singulation is possible as well.
[0131] Additionally, with this method first and second phosphor particles can be chosen and processed that are free of Ba and, thus, less harmful for health and environment.
[0132] According to at least one embodiment, producing the conversion sheet comprises tape casting the slurry onto a tape casting film. Alternatively, the production of a
[0133] 2024PF01861 April 9, 2026
[0134] P2025, 0059 WO N
[0135] 19
[0136] conversion sheet can also be achieved using methods known in industry, for example slot die casting, spray coating and spin coating. With tape casting an excellent thickness control is possible which can decrease the color distribution and improve the thickness inspection yields of the produced conversion elements. Furthermore, the conversion sheet is provided with a smooth surface facing the tape casting film.
[0137] According to at least one embodiment, curing comprises a first curing step being performed at room temperature and a second curing step being performed at an elevated temperature. During curing the polysiloxane precursor forms the polysiloxane. Due to a shrinkage of the polysiloxane precursor or the polysiloxane during curing, the thickness of the final conversion element, for example being in a range chosen from between and including 90 pm and 150 pm, can be achieved.
[0138] According to at least one embodiment, the first curing step is performed for a time chosen from a range between and including 1 day and 7 days. According to at least one embodiment, the first curing step is performed at room temperature and a relative humidity (RH) of between and including 40% to 60%, for example of 50%.
[0139] According to at least one embodiment, the second curing step is performed at a temperature chosen of a range between and including 200°C and 300°C. In particular, the second curing step is performed in an oxygen containing environment. Thus, first and second curing step are low temperature steps saving costs and allowing for more variability of the components of the conversion element.
[0140] 2024PF01861 April 9, 2026
[0141] P2025, 0059 WO N
[0142] - 20 -
[0143] According to at least one embodiment, singulating comprises a method chosen from saw dicing, laser dicing, plasma dicing, and punching. In particular, singulating comprises saw dicing. The conversion sheet, which is free of a substrate, is easy to saw dice without producing chipping of glass edges and yield losses. In particular, saw dicing is conducted with a blade of between and including 25 pm to 100 pm blade thickness. With saw dicing, in particular with saw dicing with a 25 pm blade, smooth diced surfaces and edges of the conversion elements can be realized. At the same time, the dicing speed may be increased (e. g., dicing speeds ranging from and including 8 mm to 50 mm per second). An increased dicing speed can save time and costs of this method while increasing throughput.
[0144] The method as described here, thus, opens numerous opportunities for cost savings due to the low temperature processing and reduced processing required to obtain singulated conversion elements.
[0145] Furthermore, an optoelectronic device is specified. The optoelectronic device comprises a conversion element as described herein. Thus, features, embodiments, and advantages described in combination with the conversion element and the method for producing a plurality of conversion elements also apply to the optoelectronic device and vice versa.
[0146] According to at least one embodiment, the optoelectronic device comprises a semiconductor chip that emits electromagnetic radiation of a first wavelength range. For example, the semiconductor chip is a light-emitting diode (LED).
[0147] 2024PF01861 April 9, 2026
[0148] P2025, 0059 WO N
[0149] 21
[0150] For example, the semiconductor chip comprises a semiconductor layer sequence formed from a semiconductor material. The semiconductor layer sequence comprises an active layer which is configured to generate the electromagnetic radiation of the first wavelength range. The generated electromagnetic radiation can be emitted through a radiation exit surface of the electromagnetic radiation emitting semiconductor chip. The generated electromagnetic radiation can comprise blue or UV light.
[0151] According to at least one embodiment, the optoelectronic device comprises the conversion element as described herein. In particular, the optoelectronic device comprises the conversion element on the semiconductor chip that converts at least partially, in particular fully, the electromagnetic radiation of the first wavelength range (primary radiation) into electromagnetic radiation of a second wavelength range (secondary radiation). For example, the conversion element is arranged on the radiation exit surface of the semiconductor chip.
[0152] The optoelectronic device can emit, for example, a total emission that corresponds mainly or fully to the secondary radiation. In this case, the conversion element fully or mainly converts the primary radiation into secondary radiation. The total emission has, for example, an emission color chosen from the amber range of the electromagnetic spectrum.
[0153] According to at least one embodiment, an optoelectronic device is specified comprising:
[0154] - a semiconductor chip that emits electromagnetic radiation of a first wavelength range, and
[0155] 2024PF01861 April 9, 2026
[0156] P2025, 0059 WO N
[0157] 22
[0158] - a conversion element as described herein on the semiconductor chip that converts at least partially the electromagnetic radiation of the first wavelength range into electromagnetic radiation of a second wavelength range.
[0159] Due to the properties as mentioned with respect to the conversion element, the optoelectronic device has an improved efficiency.
[0160] According to at least one embodiment, the conversion element is applied on the semiconductor chip with the surface that was arranged on the tape casting film during its production. This surface is also called bottom surface of the conversion element. According to at least one embodiment, the conversion element is fixed on the semiconductor chip with an adhesive layer. In other words, an adhesive layer is present between the semiconductor chip and the conversion element, in particular its bottom surface. In particular, the bottom surface comprises a very low surface roughness. Thus, only a low thickness of the adhesive layer is necessary resulting in an increased brightness of the optoelectronic device.
[0161] According to at least one embodiment, the optoelectronic device emits amber light. For example, such a device can be used in automotive indicator lighting or automotive daytime running lights.
[0162] Advantageous embodiments and developments of the conversion element, the optoelectronic device, and the method for producing a conversion element will become apparent from the exemplary embodiments described below in conjunction with the figures.
[0163] 2024PF01861 April 9, 2026
[0164] P2025, 0059 WO N
[0165] 23
[0166] Figure 1 shows a schematic cross section of a conversion element according to an exemplary embodiment.
[0167] Figures 2a and 2b show SEM images of conversion elements according to comparative examples.
[0168] Figures 3a and 3b show SEM images of conversion elements according to exemplary embodiments.
[0169] Figure 4a shows a schematic cross section of the conversion sheet before and after curing according to a comparative example.
[0170] Figure 4b shows a schematic cross section of the conversion sheet before and after curing according to an exemplary embodiment.
[0171] Figure 5 shows a side-view image of a cured conversion sheet according to an exemplary embodiment.
[0172] Figure 6 shows a SEM image of a cross section of a conversion element according to an exemplary embodiment.
[0173] Figure 7 shows an optical image of a plurality of conversion elements according to an exemplary embodiment.
[0174] Figure 8 shows an optical image of an optoelectronic device according to an exemplary embodiment.
[0175] Figure 9 shows a schematic cross section of an optoelectronic device according to an exemplary embodiment.
[0176] 2024PF01861 April 9, 2026
[0177] P2025, 0059 WO N
[0178] - 24 -
[0179] In the exemplary embodiments and figures, similar or similarly acting constituent parts are provided with the same reference signs. The elements illustrated in the figures and their size relationships among one another should not be regarded as true to scale. Rather, individual elements may be represented with an exaggerated size for the sake of better representability and / or for the sake of better understanding.
[0180] Figure 1 shows a schematic cross section of a conversion element 10 according to an exemplary embodiment. The conversion element 10 contain first phosphor particles 14-1 and second phosphor particles 14-2. The first phosphor particles 14-1 differ from the second phosphor particles 14-2 at least in their shape. First phosphor particles 14-1 are sphere-like or boulder-like, while second phosphor particles 14-2 have an aspect ratio.
[0181] Principally, the kind and content of phosphor particles can be varied to achieve the desired color coordinates and performance requirements. As first and second phosphor particles 14-1, 14-2 phosphors are chosen that can absorb light in the near UV to blue region of the electromagnetic spectrum and emit light in the visible region of the electromagnetic spectrum. The blend of first phosphor particles 14-1 and second phosphor particles 14-2 can be composed to emit light in the amber region of the electromagnetic spectrum, for example. Exemplary phosphors are garnets, SrCaSiAlN, oxynitridosilicates, perovskites, silicates, any phosphor mentioned above, or combinations thereof, each doped with at least one appropriate element.
[0182] Additionally, the conversion element 10 contains a matrix phase formed from a polysiloxane 11. The polysiloxane 11
[0183] 2024PF01861 April 9, 2026
[0184] P2025, 0059 WO N
[0185] 25
[0186] comprises T-units and optionally D-units. For example, while the total content of polysiloxane in the conversion element 10 is between and including 28 vol% and 38 vol%, the content of D-unit polysiloxane is in the range of 0 vol% to including 8 vol%.
[0187] Apart from the first phosphor particles 14-1 and second phosphor particles 14-2, that are dispersed in the matrix phase, there is additionally fumed silica 12 and filler particles 13 incorporated in the polysiloxane 11. The material of the filler particles 13 is chosen from silica powder ( fused and crystalline silica powder), siloxane powder, modified siloxane powder, and combinations thereof. The total content of filler particles 13 ranges from between and including 20 vol% and 45 vol%, for example between and including 25 vol% and 36 vol%. The particle size of the filler particles can be in the range of between and including 0.3 pm and 20 pm, in particular between and including 0.5 pm and 8 pm. There may be a particle size blending with a first size of the range between and including 0.8 pm and 1 pm, a second size of the range between and including 1.5 pm and 2 pm and a third size of, for example, 4 pm.
[0188] The thickness of conversion element 10 is in the range between and including 90 pm and 150 pm, in particular between and including 115 pm and 135 pm which serves for a mechanical robustness during subsequent processing.
[0189] Also indicated in figure 1 are the bottom surface 16 and the top surface 17 of the conversion element 10 which both have a low average surface roughness. In particular, the bottom surface 16 has a very low average surface roughness.
[0190] 2024PF01861 April 9, 2026
[0191] P2025, 0059 WO N
[0192] 26
[0193] A conversion element 10 can be produced as follows: First, a slurry is prepared by providing and blending the constituents of a conversion element 10. For example, a polysiloxane precursor, first phosphor particles 14-1, second phosphor particles 14-2, fumed silica 12 and filler particles 13 are mixed, for example by planetary centrifugal mixing. All materials should be high purity materials for an optimized composition of the conversion element 10. After mixing, 3-roll milling is used to ensure excellent dispersion of the first phosphor particles 14-1, the second phosphor particles 14-2, the fumed silica 12, and the filler particles 13 in the polysiloxane precursor. A further mixing step by planetary centrifugal mixing can be used to further mix and homogenize the slurry. Defoaming or vacuum treatment may be used during planetary centrifugal mixing to ensure wetting of all particles and to minimize air in the slurry. If needed, a solvent can be added to the slurry to adjust its viscosity. Furthermore, a hardener can be added to the slurry prior to producing a conversion sheet 15.
[0194] A conversion sheet 15 is produced from the slurry by tape casting. In this step, the slurry is coated on a tape casting film, e. g. Mylar, at a specified thickness, for example in the casting thickness range of 150 pm to 300 pm.
[0195] The final conversion sheet 15 can have a dimension of 10.16 cm x 15.24 cm (4" x 6") and be cured at room temperature at about 50% relative humidity for about 1 day to 7 days. After this, a thermal curing at a temperature between and including 200°C and 300°C in an oxygen containing environment is conducted. The cured conversion sheets 15 are singulated into specific sizes using saw dicing with a 25 pm blade.
[0196] 2024PF01861 April 9, 2026
[0197] P2025, 0059 WO N
[0198] - 27 -
[0199] An exemplary embodiment for a composition of a conversion element 10 is shown in table 1. The composition is shown as vol% of a cured conversion element 10. The thickness of conversion element 10 is about 135 pm.
[0200] The formulation, especially the total phosphor particle content, is, for example, suitable for conversion elements 10 that are about 135 pm thick. With this optimized formulation following criteria are met: low to no camber, no large-scale cracking in the conversion element 10, low surface roughness at least at the bottom surface 16 of the conversion element 10 (Sa < 0.2 pm), and mechanical robustness to withstand subsequent processes without damage. The exemplary embodiment of table 1 meets all criteria, for example due to a decreased T-unit polysiloxane content, an addition of a D-unit polysiloxane, and an increased total filler particle content.
[0201]
[0202] Table 1
[0203] In the exemplary embodiment, the first phosphor particles 14-1 are garnet phosphors, more specifically a YAG: Ce phosphor. The measured particle size d50 of the first phosphor particles 14-1 ranges from 14 pm to 21 pm, and in2024PF01861 April 9, 2026
[0204] P2025, 0059 WO N
[0205] 28
[0206] general they have a sphere-like or boulder-like shape as indicated in figures 1 and figure 6. The YAG: Ce phosphor has a yellow emission. The second phosphor particles 14-2 are a red nitride phosphor, more specifically a SrCaSi2Al2N6: Eu. The measured particle size d50 of the second phosphor particles 14-2 is 19.7 pm, where the particle shape can vary. As indicated in figures 1 and figure 6, particle shape can vary in aspect ratio (i. e., variable ratio between the width and height of the second phosphor particles 14-2 ). The SrCaSi2Al2N6: Eu phosphor has a red emission.
[0207] Figures 2a and 2b show scanning electron microscope (SEM) images ( 1000 x magnification) of a comparative PiXoG converter, i. e. comparative conversion element 30, comprising a substrate 36 and a conversion layer 37. The thickness of the conversion layer is about 90 pm, the thickness of the substrate 37 is about 175 pm, that is, a total thickness is about 265 pm. The substrate 36 is a glass substrate. Saw dicing was done with a 100 pm blade. Figure 2a shows in particular the edge, figure 2b shows in particular the corner. A rough edge quality, and an amount of phosphor grain pullouts which can result in debris can be observed.
[0208] The saw diced PiXoG edge ( figure 2a) shows some chipping, cracking, and particle pull-out in the conversion layer due to the dicing process. In addition, the glass substrate 36 also shows chipping on the edge which can result in yield losses due to chipping defects. Figure 2b provides a glancing view of the PiX surface, where the high concentration of phosphor in the formulation results is a rough surface.
[0209] Surface roughness is correlated with the amount of glue required to attach the platelet to the LED surface. In
[0210] 2024PF01861 April 9, 2026
[0211] P2025, 0059 WO N
[0212] 29
[0213] general, higher glue requirements results in decreasing brightness of the LED device.
[0214] Figures 3a and 3b show scanning electron microscope (SEM) images ( 1000 x magnification) of the PiX conversion element, i. e. conversion element 10 according to the exemplary embodiment, in particular the edge ( figure 3a) and a corner ( figure 3b). Due to the absence of a (glass) substrate, saw dicing was performed with a 25 pm dicing blade at a high dicing speed. The saw diced edge of the conversion element 10 shows minimal chipping and particle pull-out compared to the comparative conversion element shown in figures 2a and 2b. The saw diced edges and corners of the conversion element 10 are sharp and there appears to be minimal debris. Figure 3b shows a glancing view of the bottom surface 16 of the conversion element 10, where the surface is very smooth. The smooth bottom surface 16 requires minimal glue to bond to a semiconductor chip of an LED, thus maximizing the brightness of the device.
[0215] The surface roughness characteristics of the conversion element 10 according to the exemplary embodiment were measured using a coherence scanning interferometry technique (Zygo NewView 9000). The arithmetical mean height, i. e. the average surface roughness (Sa) and the maximum peak height (Sp) were measured for the exemplary embodiment. Table 2 shows the surface roughness data for the bottom surface 16 being cast on the Mylar tape casting film.
[0216]
[0217] Table 2
[0218] 2024PF01861 April 9, 2026
[0219] P2025, 0059 WO N
[0220] - 30 -
[0221] Figure 4a shows a schematic cross section of a conversion sheet 35 according to a comparative example. On the left side the as-cast PiXoG conversion sheet 35 is shown, where the slurry for the conversion layer 37 has been cast on the glass substrate 36. As the conversion sheet 35 dries and cures in the first curing step Cl and the second curing step 02, i. e. at room temperature and at elevated temperatures, the conversion layer 37, in particular the polysiloxane shrinks, resulting in stress in the conversion sheet 35. This stress is typically observed by a curl or camber in the cured conversion sheet 35 as shown on the right side.
[0222] In contrast, as shown in figure 4b, a conversion sheet 15 which is free of a substrate 36 and comprises the slurry as described above is shown after tape casting (left side). Due to the absence of a substrate 36 and due to the composition of the slurry, shrinkage during curing steps Cl and C2 can appear without additional stress. Thus, low to no curl or camber is achieved after curing steps Cl and C2 (right side).
[0223] Figure 5 shows a side-view image of a cured conversion sheet 15 according to the exemplary embodiment showing extremely low camber. The conversion sheet 15 was cured at 200°C and has a thickness of about 135 pm. Flatness, i. e. low camber of a conversion sheet 15 is essential for optimized bonding to the semiconductor chip, for example the LED, and subsequent LED device performance.
[0224] Figure 6 shows a SEM image (3, 000 x magnification) of a polished cross-section of conversion element 10 according to the exemplary embodiment, where in particular the microstructure of the conversion elements 10 can be observed.2024PF01861 April 9, 2026
[0225] P2025, 0059 WO N
[0226] 31
[0227] The large bright particles are the first phosphor particles 14-1 and second phosphor particles 14-2. The grey connected phase is the polysiloxane 11 forming the matrix phase that contains a variety of filler particles 13 and fumed silica 12. The filler particles can comprise first filler particles of a first size, second filler particles of a second size and third filler particles of a third size, for example. First, second and third size are different from each other and all within the filler particle size d50 ranging from 0.8 pm to 4 pm. The filler particles 13 include modified siloxane particles, fused or crystalline silica particles or combinations thereof.
[0228] The microstructure of the conversion elements 10 shown in figure 6 has a dense matrix phase formed of polysiloxane 11, there is no cracking observed, but an excellent bonding of the first and second phosphor particles 14-1, 14-2 in the matrix phase (i. e., there is no sign of delamination at the first and second phosphor particles 14-1, 14-2 to polysiloxane 11 interfaces). Small defects on the surface are observed due to "pull-out" of small filler particles during the mechanical polishing process.
[0229] Mechanical robustness of the conversion elements 10 is essential for producing LED devices. Conversion elements 10 are subjected to various mechanical stressors during the inspection and package building process. The absence of a glass substrate results in mechanical stressors applied directly to the conversion element 10. However, due to the formulation of conversion elements 10, they have the required mechanical robustness for subsequent processing into optoelectronic devices like LED devices.
[0230] 2024PF01861 April 9, 2026
[0231] P2025, 0059 WO N
[0232] 32
[0233] Figure 7 shows an optical image of conversion elements 10 according to the exemplary embodiment. The conversion elements 10 are arranged on a thermal release tape following rigorous inspection of each conversion element 10 using a turret-based semiconductor test handler. Each conversion element 10 goes through more than ten inspection stations where parameters such as length, width, thickness, camber, optical properties, and defect inspection occur. The conversion elements 10 are then placed on a thermal release film to proceed to the next stage of the process.
[0234] Figure 8 shows an optical image of an optoelectronic device 100 comprising the conversion element 10 according to the exemplary embodiment. No defects like cracking or chipping can be observed.
[0235] Figure 9 shows a schematic cross section of an optoelectronic device 100 according to an exemplary embodiment. The optoelectronic device 100 comprises a semiconductor chip 20 and a conversion element 10 as described herein on the semiconductor chip 20. In particular, the conversion element 10 is arranged on the semiconductor chip 20 with its bottom surface 16, i. e. the surface that was tape cast on the tape cast film and, thus, has a very low surface roughness.
[0236] The conversion element 10 can be fixed on the semiconductor chip 20 via an adhesive layer (not shown here). Due to the low surface roughness of the conversion element 10, the thickness of the adhesive layer, i. e. the bondline thickness, is decreased resulting in an increased brightness of the optoelectronic device 100.
[0237] 2024PF01861 April 9, 2026
[0238] P2025, 0059 WO N
[0239] 33
[0240] The semiconductor chip 20 comprises a semiconductor layer sequence comprising an active layer which is configured to generate primary radiation via a radiation exit surface. The conversion element 10 is applied on the radiation exit surface of the semiconductor chip 20.
[0241] The conversion element 10 converts the primary radiation into a secondary radiation. Thus, the optoelectronic device 100 can emit the secondary radiation, for example amber light.
[0242] Conversion elements 10 are provided that show the necessary mechanical robustness for subsequent processing into LED devices. They can, thus substitute conventional converters (phosphor-in-matrix-on-glass, phosphor-in-glass, or ceramic) and offer improved processing, more consistent properties, and lower cost options.
[0243] The features and exemplary embodiments described in connection with the figures can be combined with each other according to further exemplary embodiments, even if not all combinations are explicitly described. Furthermore, the exemplary embodiments described in connection with the figures may have alternative or additional features as described in the general part.
[0244] The invention is not restricted to the exemplary embodiments by the description on the basis of said exemplary embodiments. Rather, the invention encompasses any new feature and also any combination of features, which in particular comprises any combination of features in the patent claims and any combination of features in the exemplary embodiments, even if this feature or this
[0245] 2024PF01861 April 9, 2026
[0246] P2025, 0059 WO N
[0247] - 34 -
[0248] combination itself is not explicitly specified in the patent claims or exemplary embodiments.
[0249] This patent application claims the priority of US patent application 63 / 806,548, the disclosure content of which is hereby incorporated by reference.
[0250] 2024PF01861 April 9, 2026
[0251] P2025, 0059 WO N
[0252] 35
[0253] References
[0254] 10 conversion element
[0255] 11 polysiloxane
[0256] 12 fumed silica
[0257] 13 filler particles
[0258] 14-1 first phosphor particles
[0259] 14-2 second phosphor particles
[0260] 15 conversion sheet
[0261] 16 bottom surface
[0262] 17 top surface
[0263] 100 optoelectronic device
[0264] 20 semiconductor chip
[0265] 30 conversion element according to a comparative example
[0266] 35 conversion sheet according to a comparative example
[0267] 36 substrate according to a comparative example
[0268] 37 conversion layer according to a comparative example
[0269] Cl first curing step
[0270] C2 second curing step
Claims
2024PF01861 April 9, 2026P2025, 0059 WO N- 36 -Claims1. A conversion element ( 10 ), comprising:- a polysiloxane ( 11 ),- first phosphor particles ( 14- 1 ) and second phosphor particles ( 14-2 ),- fumed silica ( 12 ), and- filler particles ( 13 ),wherein a total content of the filler particles ( 13 ) is chosen from a range between and including 20 vol% and 40 vol%.
2. The conversion element ( 10 ) according to the preceding claim, wherein the first phosphor particles ( 14- 1 ) differ from the second phosphor particles ( 14-2 ) in at least one of composition, shape, size, and emission color.
3. The conversion element ( 10 ) according to any of the preceding claims, wherein a total emission of the first phosphor particles and the second phosphor particles is chosen from the amber range of the electromagnetic spectrum.
4. The conversion element ( 10 ) according to any of the preceding claims, wherein the polysiloxane ( 11 ) has a content being chosen from a range between and including 15 vol% and 45 vol%.
5. The conversion element ( 10 ) according to any of the preceding claims, wherein the polysiloxane ( 11 ) comprises T-units and D-units, wherein a content of D-units is within a range between and including 0 vol% and 10 vol%.2024PF01861 April 9, 2026P2025, 0059 WO N376. The conversion element ( 10) according to any of the preceding claims, wherein the fumed silica ( 12 ) comprises a content being chosen from a range between and including 0.5 vol% and 7 vol%.
7. The conversion element ( 10) according to any of the preceding claims, wherein the fumed silica ( 12 ) comprises a surface area in a range between and including 50 m2 / g and 600 m2 / g.
8. The conversion element ( 10) according to any of the preceding claims, having a thickness being chosen from a range between and including 90 pm to 150 pm.
9. The conversion element ( 10) according to any of the preceding claims, wherein the filler particles ( 13) comprise at least one of silica powder, siloxane powder, and modified siloxane powder.
10. The conversion element ( 10) according to the preceding claim, wherein the silica powder comprises at least one of fused silica powder and crystalline silica powder.
11. The conversion element ( 10) according to any of the preceding claims, wherein the filler particles ( 13) comprise a size chosen from the range between and including 0.3 pm and 20 pm.
12. The conversion element ( 10) according to the preceding claim, wherein the filler particles ( 13) comprise at least first filler particles of a first size and second filler particles of a second size, wherein the first size is chosen from a first sub-range within the range between and including2024PF01861 April 9, 2026P2025, 0059 WO N380.3 µm and 20 µm and the second size is chosen from a second sub-range within the range between and including 0.3 µm and 20 µm.
13. The conversion element ( 10 ) according to any of claims 9 to 12, wherein the modified siloxane powder comprises a reduced silanol content and optionally a reduced CH3-group content with respect to the siloxane powder.
14. The conversion element ( 10 ) according to any of the preceding claims, wherein the conversion element ( 10 ) is free of a substrate.
15. A method for producing a plurality of conversion elements ( 10 ), comprising the steps of:- preparing a slurry comprising a polysiloxane precursor, first phosphor particles ( 14- 1 ), second phosphor particles ( 14-2 ), fumed silica ( 12 ), and filler particles ( 13 ), wherein a total content of the filler particles ( 13 ) is chosen from a range between and including 20 vol% and 40 vol%,- producing a conversion sheet ( 15 ) from the slurry, the conversion sheet ( 15 ),- curing the conversion sheet ( 15 ), and- singulating the cured conversion sheet ( 15 ) into conversion elements ( 10 ).
16. The method according to the preceding claim, wherein producing the conversion sheet ( 15 ) comprises tape casting the slurry onto a tape casting film.
17. The method according to any of claim 15 and 16, wherein curing comprises a first curing step being performed at room2024PF01861 April 9, 2026P2025, 0059 WO N- 39 -temperature and a second curing step being performed at an elevated temperature.
18. The method according to any of claims 15 to 17, wherein singulating comprises a method chosen from saw dicing, laser dicing, plasma dicing, and punching.
19. An optoelectronic device ( 100) comprising- a semiconductor chip (20) that emits electromagnetic radiation of a first wavelength range, and- a conversion element ( 10) according to any of claims 1 to14 on the semiconductor chip (20) that converts the electromagnetic radiation of the first wavelength range into electromagnetic radiation of a second wavelength range.