Continuous casting with high thickness reduction

The continuous casting process addresses center segregation and porosity issues by employing dynamic hard reduction and controlled cooling, achieving high-quality thick sheets through adjustable strand guide rollers and intentional bulging, improving productivity and quality.

WO2026238449A1PCT designated stage Publication Date: 2026-11-19PRIMETALS TECH AUSTRIA GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/062584
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-04-30
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing continuous casting methods struggle to effectively reduce center segregation and porosity in metallic strands, particularly for thick sheets, due to limitations in dynamic adjustment to changing process parameters and the inability to apply high reduction forces without causing defects.

Method used

Implementing a continuous casting process with hard reduction segments that dynamically adjust to process changes, using adjustable strand guide rollers to achieve high reduction rates, combined with intentional bulging and controlled cooling to manage strand thickness and temperature, ensuring high-quality product production.

Benefits of technology

Significantly reduces center segregation and porosity by applying high reduction forces where needed, allowing for thicker sheets to be produced with less deformation, enhancing productivity and quality while adapting to varying casting conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026062584_19112026_PF_FP_ABST
    Figure EP2026062584_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method and system for continuously casting metal strands with high thickness reduction. The aim of the invention is to significantly reduce center segregation and center porosities that can impair the quality of flat products. The method comprises the production of an initially bulged strand of variable thickness and the use of hard reduction, in which the thickness of the strand is greatly reduced by strand guide rollers. The hard reduction is carried out immediately before final solidification and can be dynamically adapted to the casting conditions. The continuous casting system comprises a mold, a casting arc and a horizontal region with strand guide segments which adjust the casting gap and allow for the thickness reduction. The combination of intentional bulging, hard reduction and other reduction methods achieves improved center quality and more economical production of thick sheets.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] 202400296

[0002] 1

[0003] Description

[0004] Title of the invention

[0005] Continuous casting with high thickness reduction

[0006] field of technology

[0007] The present invention is in the field of continuous casting technology and describes a method for casting a metallic strand on a continuous casting plant. The method comprises the following steps:

[0008] -Producing a strand which has a thickness in a casting-width-related central area that is at least 5-20 mm, preferably at least 7-14 mm greater than in an edge area,

[0009] -Hard reduction of the strand within a hard reduction region.

[0010] Furthermore, a continuous casting plant for casting a metallic strand, comprising a mold, a subsequent casting arc, and a subsequent horizontal area, is described.

[0011] The casting arc comprises at least one strand guide segment with first actuators with casting gap adjustment and the horizontal area comprises at least one strand guide segment with second actuators with single roller adjustment, wherein the second actuators are designed to reduce the thickness of a metallic strand to be cast by at least 3 mm.

[0012] State of the art

[0013] Center segregation and center porosity are detrimental effects on quality in continuous casting, but these can at least be reduced by known process engineering measures such as soft reduction.

[0014] Excessive center segregation or center porosity can lead to problems or defects in the final product, especially during rolling, and must therefore be avoided or at least limited. Rolled slabs with unacceptably severe center defects are detected and rejected by ultrasonic testing. The better the center quality of the slabs, the less deformation is required during rolling for certain end products. The greater the porosity in the center of the slab, the greater the deformation required to remove or close it. (Improvement-202400296)

[0015] 2

[0016] Improving the center quality can therefore lead to the production of thicker sheets with the same initial slab thickness, thus reducing the required degree of forming. This can result in a significant economic advantage. For example, sheets that would otherwise only be produced from ingot-cast slabs can be manufactured via a much more economical continuous casting route.

[0017] US2017 / 0050239A1 describes a process for producing slabs with high internal quality. A significant thickness reduction of the strand is achieved by two reduction rollers at two specific positions in the continuous casting plant.

[0018] Since these are individual rollers in fixed positions, dynamic adjustment to changing process parameters, such as casting speed, cooling, overheating of the steel to be cast, steel grade or casting thickness, is not possible.

[0019] EP2881196A1 describes a continuous casting process in which a strand is intentionally bulged and then compressed by soft reduction to reduce center segregation in the strand.

[0020] The strand is guided by strand guide rollers, with a constant pouring gap from just below a mold until the thickness of the solidified strand shell reaches 15 mm. The pouring gap is then gradually increased, causing the strand to bulge by 3 to 20 mm. The pouring gap then remains constant for a short time. Finally, with a solids content between 0.2 and 0.9, the strand is compressed such that the product of the compression rate and pouring speed is 0.3 to 1.0 mm / min * m / min.

[0021] Summary of the invention

[0022] The object of the present invention is to provide a continuous casting process or a continuous casting plant which avoids, or at least significantly reduces, center segregation and center porosity in the continuous casting of flat products. This is particularly important for the production of thick sheets.

[0023] Simulations have shown that the so-called hard reduction rate, i.e., the reduction of strand thickness per strand length, is an advantageous parameter for influencing the internal quality of the cast product. This applies in particular to the reduction or complete elimination of center segregation and / or center porosity. Hard reduction rates of at least 6 mm / m, preferably at least 8 mm / m, are required. These values ​​result in a significantly higher product quality.

[0024] 3

[0025] Compression rate and casting speed as specified, for example, in EP2881196A1. Assuming a casting speed of 0.6 m / min, this product yields 2.16, preferably 2.88 mm / min * m / min. Conventional continuous casting segments designed for soft reduction with casting gap adjustment are typically unable to achieve such high values.

[0026] Methods for preventing such defects offer a decisive advantage, especially when they can dynamically respond to changes in process parameters, such as changes in steel grade, casting speed, or steel overheating. By significantly reducing the thickness of the cast strand over a much shorter length (compared to soft reduction) immediately before solidification, center segregation and porosity can be greatly reduced. This process is known as hard reduction or heavy reduction. In hard reduction, a very high total reduction of at least 5 mm, preferably at least 7 mm, is applied immediately before final solidification, distributed across a few rolls (at least one, preferably two to three). The required total thickness reduction depends on the casting thickness and the number of rolls involved.A minimum thickness reduction of 3 mm per roll is required to achieve the desired effect. Typically, the thickness reduction per roll is in the range of 5 mm or more. While soft reduction is applied in the range of a solids content of approximately 10–100%, hard reduction operates in a solids content range of approximately 70–100%, preferably approximately 80–95%. With soft reduction, the strand thickness is reduced by 1–2.5%. The thickness reduction in hard reduction is always greater than 2.5% and is typically 3% or higher. Hard reduction can only be performed using suitable hard reduction segments. These segments must be capable of generating significantly higher forces per roll to achieve the required thickness reductions. Such a segment must be sufficiently rigid to ensure that certain deformation limits are not exceeded.The required reduction forces depend on the amount of stripping, the thickness of the strand shell, the steel grade, and the strand temperature. A hard reduction segment comprises several rollers. Multiple hard reduction segments are installed in the strand guide in the area of ​​expected solidification. Because multiple hard reduction segments are used, it is possible to apply hard reduction over a larger area to accommodate varying production conditions, such as casting speed, steel grade, superheating of the liquid steel introduced into the mold, and cooling of the strand. The hard reduction can be dynamically adapted to the casting conditions, particularly to the point of final solidification. This is therefore referred to as dynamic hard reduction. 202400296.

[0027] 4

[0028] Calculations have shown that for larger casting thicknesses, roller forces on the order of 10 MN can occur during hard reduction. A segment capable of generating these high forces is too large for integration into a conventional continuous casting plant. Very large roller diameters would be required to accommodate bearings with the necessary load-bearing capacity. Large roller diameters would lead to large roller spacings, resulting in unacceptably severe bulging of the strand shell. A segment with such large roller spacings would also preclude the use of dynamic hard reduction. Due to the large distance between the rollers and the relatively small number of rollers, a finely graduated spatial resolution of the hard reduction zone could not be achieved.

[0029] Furthermore, such a segment would involve high manufacturing costs and be disadvantageous in operation due to its high mass. To keep the forces required for thickness reduction within manageable limits when dealing with large casting thicknesses, the following measures, for example, can be taken individually or in combination:

[0030] -Intentional-Bulging

[0031] - Maintaining a high strand temperature for longer periods, for example by reducing spray cooling and using special, peripherally cooled strand guide rollers - Casting of bulging strands

[0032] -Casting strands with chamfers

[0033] -Use of strand guide rollers with a diameter that varies across the casting width

[0034] -Heating and / or insulating the narrow sides of the strand to be cast.

[0035] The problem is solved by a process for casting a metallic strand on a continuous casting plant, comprising the process steps carried out sequentially.

[0036] -Producing a strand which has a thickness in a casting-width-related central area that is at least 5-20 mm, preferably at least 7-14 mm greater than in an edge area,

[0037] -Hard reduction of the strand within a hard reduction region,

[0038] wherein the hard reduction zone extends over a casting length of 2.5 m before to 2.5 m after, preferably 1.5 m before to 0.75 m after, a solidification point, and the hard reduction is effected by at least one adjustable strand guide roller, preferably by at least two adjustable strand guide rollers, particularly preferably by three adjustable strand guide rollers, wherein a thickness reduction in the hard reduction zone in the central region is between 5 and 25 mm, preferably between 7 and 20 mm, wherein a hard reduction rate in the hard reduction zone is at least-202400296

[0039] 5

[0040] tens 6 mm / m, preferably at least 8 mm / m, wherein the strand after hard reduction has a substantially the same predetermined thickness in the middle region as in the edge region.

[0041] The hard reduction takes place in an area of ​​the strand where the solidification is 0.7 - 1.0, preferably 0.8 - 0.95.

[0042] Due to the high dip rate in a section of the strand where there is already a very high degree of solidification and a correspondingly thin liquid bottom layer, this bottom layer, enriched with alloying elements, can be effectively displaced upstream and thus removed. In the process, the upper and lower halves of the strand are compressed and joined together. This largely or completely prevents macrosegregation.

[0043] To facilitate the deformation of the strand in the area of ​​the narrow sides that occurs during hard reduction, or to reduce the formation of cracks, a temperature of the strand that is as high as possible, especially in the area near the edges, is advantageous.

[0044] These areas can be heated for this purpose. Heating can be achieved, for example, using a burner and / or an induction heater.

[0045] Furthermore, thermal insulation of the narrow sides can also lead to less cooling and thus a higher temperature during hard reduction. This insulation can be applied after the bending process, thereby effectively reducing the cooling of the narrow sides.

[0046] A concomitant reduction in the strand's strength also leads to a reduction in the required rolling forces. This is all the more significant the thicker and / or colder the cast strand is.

[0047] When designing the drives for the hard reduction segments, increased pull-out forces must be taken into account in order to be able to apply the additional rolling moments that occur due to the thickness reduction.

[0048] The pull-out force of the entire continuous casting plant is taken into account. If the pull-out force of the hard reduction segment(s) is insufficient to overcome the locally occurring rolling torques, the remaining segments must absorb the additional pull-out forces. Preferably, these forces are distributed among all remaining driven rollers by means of a load balancing control system for the drives.

[0049] Typically, each strand guide segment has at least one driven roller on both the inner and outer arc. This applies particularly to the hard reduction segments.

[0050] Driven rollers arranged on the inner arc are typically designed to be positioned against the strand being cast with a force sufficient to transmit pull-out forces. An increased force is called an adjustment-202400296

[0051] 6

[0052] Force that exceeds the force required to support the forces generated by hydrostatic pressure in the strand. In particular, so-called hard reduction segments are suitable for transmitting increased tension forces. These are strand guide segments with individual roller adjustment.

[0053] Furthermore, it is advantageous that, viewed in the casting direction, after the hard reduction segments, additional segments with increased actuation force and thus a large pull-out force reserve are arranged. After the hard reduction, the strand is completely solidified, which is why the driven rollers on the inner bend can be actuated with increased force if necessary, without causing undesirable defects in the strand. This allows the pull-out force to be increased without slippage of the drives. For this to work, the driven rollers must be actuated with increased force, for example, by using larger hydraulic cylinders. At a minimum, however, the last segment, and preferably also the penultimate segment, is equipped with an increased pull-out force reserve.

[0054] Furthermore, additional pull-out rollers, so-called pinch rollers, can be installed after the strand guide, which can achieve an increased starting force and consequently a high pull-out force.

[0055] By equipping a sufficiently long section with hard-reduction-capable segments, hard reduction can be applied over a wider operating range. This range encompasses various parameters such as casting speed, steel grade, casting thickness, superheating of the steel being cast, and / or cooling of the strand. Thus, unlike conventional methods, hard reduction is not limited to a fixed position in the strand guide and therefore to a fixed operating point. When the position of the solidification point changes, the hard reduction can dynamically adjust over a wide range, enabling higher productivity with correspondingly high product quality.

[0056] In a preferred embodiment, at least one of the following process steps is carried out:

[0057] -The area-related cooling water supply to the strand is less than 8 l / (min m²) between a casting length of 4 m, preferably 9 m and one end of the hard reduction section. 2 ), preferably less than 4 l / (min m 2 )

[0058] -The thickness of the strand is reduced in the hard reduction area by adjusting the respective adjustable strand guide rollers relative to a strand guide roller immediately preceding it in the middle area along the casting length by at least 3 mm, preferably at least 4 mm.

[0059] -a casting thickness of 250 - 500 mm is set.

[0060] - A pouring speed of 0.35 - 1.5 m / min is set. 202400296

[0061] 7

[0062] In a further preferred embodiment, the application of cooling water to the strand is suitable to limit the length of solidification tongues in the direction of the casting length to less than 500 mm, preferably less than 300 mm, particularly preferably less than 200 mm.

[0063] A homogeneous solidification front, or the avoidance of pronounced solidification tongues, can be achieved by cooling as uniformly as possible across the casting width. In the case of pronounced solidification tongues, the solidification point of the strand varies across the strand width, which can reduce the achievable quality, especially good center quality across the entire casting width.

[0064] Simulations have shown it to be advantageous if the temperature profile of the strand surface in the direction of the casting width varies by less than 35 K in the area of ​​a casting length of at least 5 m before the hard reduction area to the end of the hard reduction area.

[0065] Since the edges are significantly colder than the rest of the strand surface, edge strips of at least 150 mm, preferably at least 200 mm, width are excluded for this consideration.

[0066] The distribution of the surface temperature can be influenced by an arrangement of cooling nozzles with a corresponding spray pattern.

[0067] In a further preferred embodiment, a soft reduction of the strand within a soft reduction area of ​​a casting length is carried out by strand guide rollers, wherein the soft reduction area extends along the casting length in the area between 12 m, preferably 2 m, before the start of the hard reduction area and the start of the hard reduction area, wherein the thickness reduction in the soft reduction area in the middle area is between 2 and 10 mm, preferably between 3 and 8 mm.

[0068] In a further preferred embodiment, the strand is bulged within an intentional bulging area by positioning strand guide rollers, wherein the intentional bulging area extends along the casting length in the range between 4 m, preferably 9 m, from a bath level of a mold and the beginning of the hard reduction area of ​​the strand.

[0069] Typically, the intentional bulging area features essentially cylindrical strand guide rollers.

[0070] Another way to create a bulge in the strand is to use strand guide rollers with a diameter that varies across the casting width. 202400296

[0071] 8

[0072] In a further preferred embodiment, the production of the strand, which has a greater thickness in the central area in terms of casting width than in the outer area, is carried out at least partially by shaping in a mold.

[0073] In a further preferred embodiment, at least one of the following process steps is carried out:

[0074] - Liquid core reduction of the strand takes place within a liquid core reduction area, wherein the liquid core reduction area extends along the casting length in the region between a lower end of a mold and a distance of 10 m from a bath level of the mold, wherein in the liquid core reduction area the thickness of the strand is reduced by 2-20 mm, preferably by 7-14 mm, by strand guide rollers arranged on broad sides of the strand, wherein the strand in the liquid core reduction area has a substantially the same thickness in a casting-width-related central region as in an edge region

[0075] -at least the beginning and end of one of the following areas are movable: -Liquid Core Reduction Area (1)

[0076] -Intentional bulging area (2)

[0077] -Soft reduction area (3a)

[0078] -Hard reduction area (3b),

[0079] wherein the respective positions are preferably controlled / regulated by a higher-level plant control system depending on a simulated position of a solidification point.

[0080] Liquid core reduction allows for greater flexibility in achieving a desired thickness of the cast product at the end of the continuous casting process.

[0081] Depending on whether intentional bulging is applied or not, a different final thickness results. Without liquid core reduction, for example, the mold would have to be changed to achieve a thickness difference of approximately 10 mm to reach the desired final thickness. By reducing the strand thickness using liquid core reduction and subsequent intentional bulging, the force required for thickness reduction during a later hard reduction process can be reduced. This is possible because the strand edges no longer need to be compressed to the same extent during hard reduction as they would without prior liquid core reduction.

[0082] Especially with large casting thicknesses, significant thickness reductions are only possible in combination with intentional bulging or by casting a bulged strand. This applies particularly to casting thicknesses greater than 250 mm, preferably greater than 300 mm, and most preferably greater than 350 mm. 202400296

[0083] 9

[0084] Dynamic hard reduction requires a sufficient number of hard-reduction-capable rollers or segments. This ensures that hard reduction can be maintained even with varying casting parameters, such as steel grade, casting speed, or overheating of the steel entering the mold.

[0085] Along the direction of pouring, the length of a hard reduction-capable area is at least 2 m, i.e., one segment length, but preferably 4 - 8 m, which corresponds to two to four segment lengths.

[0086] The strand guide segments in the hard-reduction-capable strand length range are single-roll positioning segments, i.e., so-called SRD segments (Single-Roll Dynagap).

[0087] This allows for precise and flexible sampling based on the location of the solidification point. This requires, on the one hand, dynamic control of the segments or the sampling of the segment rollers. On the other hand, a precise calculation model is needed to determine the solidification process and calculate the solidification point, or to determine the solids content along a casting thickness or within a casting cross-section.

[0088] This allows for an automatic and safe switch between soft reduction and hard reduction.

[0089] This can be the case, for example, if the

[0090] The solidification point is reached when a significant change in pouring speed occurs, causing the hard reduction to leave the solidification range. Such changes can occur, for example, at the beginning or end of the pouring process.

[0091] Therefore, if the solidification point leaves the hard reduction range, a switch to soft reduction can be made automatically, which allows certain quality standards of the cast product to still be maintained.

[0092] Furthermore, the problem is solved by a continuous casting plant, wherein the second actuators can be controlled by a control device such that a hard reduction zone can be defined in a section of the strand guide segments with individual roller adjustment, wherein each of the rollers located in the hard reduction zone can be individually adjusted by the second actuators to reduce the thickness relative to a preceding roller, wherein the casting gap in the hard reduction zone is reduced by 5–25 mm, preferably 7–20 mm, wherein a hard reduction rate of at least 6 mm / m, preferably at least 8 mm / m, can be set in the hard reduction zone, wherein the continuous casting plant has at least one of the following bulging devices: 202400296

[0093] 10

[0094] -In the control unit, an intentional bulging area can be defined in the area of ​​the strand guide segments with first actuators for adjusting the casting gap or in the area of ​​the strand guide segments with second actuators with individual roller adjustment, wherein the first actuators and / or second actuators of the strand guide segments in the intentional bulging area can be controlled by the control unit in such a way that the casting gap within the intentional bulging area is increased by 5 - 20 mm, preferably 7 - 14 mm.

[0095] -the mold comprises two broad-sided copper plates,

[0096] wherein the broad-sided copper plates are designed such that they have a casting gap at the lower ends in a casting-width-related central area which is 5 - 20 mm, preferably 7 - 14 mm larger than in the two edge areas.

[0097] In a preferred embodiment, a soft reduction area can be defined in the control device in the area of ​​the strand guide segments with first actuators with casting gap adjustment and in the area of ​​the strand guide segments with second actuators with individual roller adjustment such that, viewed in the casting direction,

[0098] starting 2 - 12 m before the hard reduction area and ending at the beginning of a hard reduction area, wherein the first actuators and / or the second actuators can be controlled by the control device in such a way that the casting gap in the soft reduction area is reduced by 2 - 10 mm, preferably by 3 - 8 mm.

[0099] In a further preferred embodiment, in the control device, in the area of ​​the strand guide segments with first actuators with casting gap adjustment and in the area of ​​the strand guide segments with second actuators with single roller adjustment, the intentional bulging area can be defined such that, viewed in the casting direction, it begins 3 - 10 m after one end of the mold and ends 0 - 15 m before the start of the hard reduction area or a soft reduction area.

[0100] In a further preferred embodiment, a liquid core reduction area can be defined in the control device in the area of ​​the strand guide segments with first actuators with casting gap adjustment such that, viewed in the casting direction, it ends at the beginning of an intentional bulging area, wherein the first actuators can be controlled by the control device in such a way that the casting gap in the liquid core reduction area is reduced by 2 - 20 mm, preferably by 7 - 14 mm.

[0101] In a further preferred embodiment, the strand guide segments with single-roll adjustment, comprising second actuators, are designed such that they can be adjusted via 202400296

[0102] 11

[0103] The respective strand guide rollers transmit a force of at least 3000 kN, preferably at least 4000 kN, and particularly preferably at least 5000 kN to the strand.

[0104] Since relatively high forces occur per roller or segment during hard reduction, sufficient stiffness of the segments and roller supports must be provided through design measures to prevent excessive deformation or deflection under these high forces. A roller deflection of less than 1.5 mm is targeted in this context.

[0105] In a further preferred embodiment, the area with strand guide segments with second actuators with single-roll adjustment has a length of 2 - 12 m, preferably 4 - 9 m, and is located in a horizontal area.

[0106] In a further preferred embodiment, the continuous casting plant has at least one of the following features:

[0107] -The strand guide segments with individual roller adjustment comprise second actuators designed such that a force of at least 3000 kN, preferably at least 4000 kN, and particularly preferably at least 5000 kN can be transmitted to the strand via at least one strand guide roller, preferably all strand guide rollers. -At least one strand guide roller, preferably all strand guide rollers, have a diameter of at least 350 mm, preferably at least 400 mm.

[0108] -The roller axis-related distances of rollers of strand guide segments with individual roller adjustment that are immediately adjacent along the casting length are each less than 600 mm, preferably less than 520 mm.

[0109] Furthermore, the task is solved by a computer program product comprising commands that cause the continuous casting plant with control device according to one of claims 8 - 13 to perform the process steps according to one of claims 1 - 7, by the control device individually controlling the adjustable strand guide rollers by means of the actuators for thickness reduction.

[0110] Furthermore, the problem is solved by a computer-readable medium on which the computer program according to claim 14 is stored.

[0111] Brief description of the drawings

[0112] The properties, features and advantages of this invention described above, as well as the manner in which they are achieved, will be explained more clearly and understandably in section 202400296.

[0113] 12

[0114] This relates to the following description of an exemplary embodiment, which is explained in more detail in conjunction with the drawings. These show:

[0115] Fig. 1 shows a sectional view of a continuous casting plant, comprising a strand, a mold, strand guide segments, and strand guide rollers.

[0116] Figs. 2-4 Cross-sectional views of strand cross-sections at different positions in a continuous casting plant and

[0117] Fig. 5 shows a profile of a casting thickness over a casting length in a casting-width-based central area of ​​a strand to be cast.

[0118] Description of the embodiments

[0119] Fig. 1 shows an embodiment of the invention in the form of a sectional view of a continuous casting plant, comprising a strand 4, a mold 20, strand guide segments 8 and 9, and strand guide rollers 7. After exiting the mold 20, the strand 4 passes through a liquid core reduction section 1. This is followed by the intentional bulging section 2 and the soft reduction section 3a. These sections include strand guide segments with casting gap adjustment 8. Furthermore, these sections can include strand guide segments with individual roller adjustment 9.

[0120] The hard reduction section 3b follows, located in the horizontal area hz. The hard reduction section 3b is formed by strand guide segments with individual roller adjustment 9.

[0121] Fig. 2 shows sectional views of a strand 4 with the solid and liquid sections at different positions in the continuous casting plant. Here, it shows

[0122] a) a strand cross-section with straight broadsides 6 before entering an intentional bulging area 2,

[0123] b) a strand cross-section with bulged broad sides 6 after the intentional bulging area 2,

[0124] c) a strand cross-section before entering a soft reduction area 3a or a strand cross-section during passage through this area and

[0125] d) a strand cross-section in a hard reduction region 3b at the moment of solidification.

[0126] Fig. 3 shows sectional views of a strand 4 with the solid and liquid sections at different positions in the continuous casting plant. Figure 202400296 shows...

[0127] 13

[0128] a) a strand cross-section with bulging broad sides 6 after exiting a mold with bulging broad sides copper plates,

[0129] b) a strand cross-section with bulging broad sides 6 after growth of the strand shell,

[0130] c) a strand cross-section before entering a soft reduction area 3a or a strand cross-section during passage through this area and

[0131] d) a strand cross-section in a hard reduction region 3b at the moment of solidification.

[0132] Fig. 4 shows sectional views of a strand 4 with the solid and liquid sections at different positions in the continuous casting plant. Here, it shows

[0133] a) a strand cross-section with chamfers after exiting a mold,

[0134] b) a strand cross-section with chamfers after growth of the strand shell during or after a liquid core reduction,

[0135] c) a strand cross-section before entering a hard reduction region 3b or a strand cross-section during passage through this region and d) a strand cross-section in the hard reduction region 3b at the moment of solidification.

[0136] Fig. 5 shows the thickness profile of a strand 4 over a casting length 5. The thickness in a central region 12b is shown. After exiting a mold 20, the strand 4 passes through a liquid core reduction section 1, where an initial thickness reduction occurs.

[0137] Afterwards, strand 4 passes through an intentional bulging area 2, where a bulging of the broadsides 6 occurs.

[0138] The strand 4 then passes through a soft reduction area 3a, where a further thickness reduction takes place.

[0139] Finally, strand 4 passes through a hard reduction area 3b, where a strong reduction in thickness and complete solidification take place.

[0140] Further thickness reduction of the strand is achieved primarily through thermal shrinkage.

[0141] Although the invention has been further illustrated and described by the preferred embodiments, the invention is not limited by the disclosed examples and other variations can be derived from them by a person skilled in the art without departing from the scope of protection of the invention. 202400296

[0142] Reference symbol list

[0143] 1 Liquid Core Reduction Area

[0144] 2. Intentional Bulging Area

[0145] 3a Soft-Reduction Area

[0146] 3b Hard Reduction Area

[0147] 4 strand

[0148] 5 Casting length

[0149] 6 broadsides

[0150] 7 strand guide rollers

[0151] 8 strand guide segments with casting gap adjustment 9 strand guide segment with individual roller adjustment 10 center area

[0152] 11 Edge area

[0153] 12a Thickness in the edge area

[0154] 12b thickness in the middle area

[0155] 13 width

[0156] 15 narrow pages

[0157] 20 molds

[0158] 21 Solidification point

[0159] 25 Pouring gap

[0160] 26 Lower end of the mold

[0161] Hz Horizontal Range

Claims

202400296 15 Claims 1. Method for casting a metallic strand (4) on a continuous casting plant, comprising the process steps carried out sequentially: -Producing a strand (4) which has a thickness (12) in a casting-width central region (10) that is at least 5-20 mm, preferably at least 7-14 mm greater than in an edge region (11), -Hard reduction of the strand (4) within a hard reduction region (3b), characterized by that the hard reduction zone extends over a casting length (5) of 2.5 m before to 2.5 m after, preferably 1.5 m before to 0.75 m after a solidification point (21), and the hard reduction is carried out by at least one adjustable strand guide roller (7), preferably by at least two adjustable strand guide rollers (7), particularly preferably by three adjustable strand guide rollers (7), wherein a thickness reduction in the hard reduction area (3b) in the central area is between 5 and 25 mm, preferably between 7 and 20 mm, wherein a hard reduction rate in the hard reduction area (3b) is at least 6 mm / m, preferably at least 8 mm / m, wherein the strand (4) after hard reduction has a substantially the same predetermined thickness (12) in the middle region (10) as in the edge region (11).

2. The method of claim 1, wherein at least one of the following method steps is performed: -The area-related cooling water supply of the strand (4) is less than 8 l / (min m) between a casting length of 4 m, preferably 9 m and an end of the hard reduction area (3b). 2 ), preferably less than 4 l / (min m 2 ) -The thickness of the strand is reduced in the hard reduction area (3b) by adjusting the respective adjustable strand guide rollers (7) with respect to a strand guide roller (7) immediately preceding it in the central area (10) along the casting length (5) by at least 3 mm, preferably at least 4 mm. -a casting thickness of the strand of 250 - 500 mm is set202400296 16 -A pouring speed of 0.35 - 1.5 m / min is set.

3. Method according to claim 2, wherein the cooling water supply to the strand (4) is suitable to limit the length of solidification tongues in the direction of the casting length (5) to less than 500 mm, preferably less than 300 mm, particularly preferably less than 200 mm.

4. Method according to one of the preceding claims, wherein a soft reduction of the strand (4) within a soft reduction area (3a) of a casting length (5) is carried out by strand guide rollers (7), wherein the soft reduction area (3a) extends along the casting length (5) in the area between 12 m, preferably 2 m, before the start of the hard reduction area (3b) and the start of the hard reduction area (3b), wherein the thickness reduction in the soft reduction area (3a) in the middle area is between 2 and 10 mm, preferably between 3 and 8 mm.

5. Method according to one of the preceding claims, wherein bulging of the strand (4) within an intentional bulging area (2) is carried out by positioning strand guide rollers (7), wherein the intentional bulging area (2) extends along the casting length (5) in the range between 4 m, preferably 9 m, after a bath level of a mold (20) and the beginning of the hard reduction area (3b) of the strand (4).

6. Method according to one of the preceding claims, wherein the production of the strand (4) which has a greater thickness (12b) in the casting width-related central area (10) than in the edge area (12a), at least partially by shaping in a mold (20).

7. A method according to any of the preceding claims, wherein at least one of the following method steps is carried out: -a liquid core reduction of the strand (4) takes place within a liquid core reduction area (1), wherein the liquid core reduction area (1) extends along the casting length (5) in the area between a lower end of a mold (20) and a distance of 10 m from a bath level of the mold (20), wherein in the liquid core reduction area (1) the thickness (12) of the strand (4) is reduced by strand guide rollers (7) which are attached to broad sides (6) of the strand (4)202400296 17 are arranged the thickness is reduced by 2 - 20 mm, preferably by 7 - 14 mm, wherein the strand (4) in the liquid core reduction area (1) has a substantially the same thickness (12) in a casting width-related central area (10) as in an edge area (11). -at least the beginning and end of one of the following areas can be moved: -Liquid core reduction area (1) -Intentional bulging area (2) -Soft reduction area (3a) -Hard reduction area (3b), wherein the respective positions are preferably controlled / regulated by a higher-level plant control system depending on a simulated position of a solidification point (21).

8. Continuous casting plant for casting a metallic strand (4) comprising a mold (20), a subsequent casting arc, and a subsequent horizontal section (hz), wherein the casting arc includes at least one strand guide segment with first actuators with casting gap adjustment (8), and the horizontal area (hz) includes at least one strand guide segment with second actuators with single-roll adjustment (9), wherein the second actuators are designed to reduce the thickness of a metallic strand to be cast by at least 3 mm, characterized in that that the second actuators can be controlled / regulated by a control device in such a way, that in a partial area of ​​the strand guide segments with single roller adjustment (9), a hard reduction area (3b) can be defined, wherein the casting gap in the hard reduction area (3b) is reduced by 5-25 mm, preferably 7-20 mm, wherein each of the rollers located in the hard reduction area (3b) can be individually adjusted by the second actuators to reduce the thickness relative to a preceding roller, wherein in the hard reduction area (3b) a hard reduction rate of at least 6 mm / m, preferably at least 8 mm / m, is adjustable, wherein the continuous casting plant has at least one of the following bulging devices: 202400296 18 -In the control unit, an intentional bulging area (2) can be defined in the area of ​​the strand guide segments with first actuators for adjusting the casting gap or in the area of ​​the strand guide segments with second actuators with individual roller adjustment (9), wherein the first actuators and / or second actuators of the strand guide segments in the intentional bulging area (2) can be controlled by the control unit in such a way that that the casting gap (25) within the intentional bulging area is enlarged by 5-20 mm, preferably 7-14 mm -the mold (20) comprises two broad-sided copper plates, wherein the broad-sided copper plates are designed such that they have a casting gap at the lower ends in a casting-width-related central area which is 5 - 20 mm, preferably 7 - 14 mm larger than in the two edge areas.

9. Continuous casting plant according to claim 8, wherein in the control device in the area of ​​the strand guide segments with first actuators with casting gap adjustment (8) and in the area of ​​the strand guide segments with second actuators with single roller adjustment (9) a soft reduction area (3a) can be defined such that that, viewed in the direction of casting (5), it begins 2 - 12 m before the hard reduction area and ends at the beginning of a hard reduction area, whereby the first actuators and / or the second actuators can be controlled by the control device in such a way, that the casting gap in the soft reduction area (3a) is reduced by 2 - 10 mm, preferably by 3 - 8 mm.

10. Continuous casting plant according to claim 8 or 9, wherein in the control device in the area of ​​the strand guide segments with first actuators with casting gap adjustment (8) and in the area of ​​the strand guide segments with second actuators with single roller adjustment (9) the intentional bulging area (2) can be defined in such a way that that this seen in the direction of pouring (5), 3 - 10 m after one end of the mold (26) begins and 0 - 15 m before the start of the hard reduction zone or a soft reduction zone ends. 202400296 19 11. Continuous casting plant according to one of claims 8 - 10, wherein in the control device in the area of ​​the strand guide segments with first actuators with casting gap adjustment (8) a liquid core reduction area (1) can be defined in such a way, that this seen in the direction of pouring (5), 0.2 - 5 m after one end of the mold (26) begins and 6 - 12 m after one end of the mold (26) or at the beginning of an intentional bulging phase, wherein the first actuators can be controlled by the control unit in such a way, that in the liquid core reduction area (1) the casting gap is reduced by 2 - 20 mm, preferably by 7 - 14 mm.

12. Continuous casting plant according to one of claims 8 - 11, wherein the area with strand guide segments with second actuators with single roller adjustment (9) has a length of 2 - 12 m, preferably 4 - 9 m, and is located in a horizontal area (hz).

13. Continuous casting plant according to one of claims 8 - 12, which has at least one of the following features -The strand guide segments with individual roller adjustment (9) comprise second actuators designed such that a force of at least 3000 kN, preferably at least 4000 kN, and particularly preferably at least 5000 kN can be transmitted to the strand (4) via at least one strand guide roller (7), preferably via all strand guide rollers (7). -at least one strand guide roller (7), preferably all strand guide rollers (7) have a diameter of at least 350 mm, preferably at least 400 mm -The roller axis-related distances of rollers of strand guide segments with single roller adjustment (9) immediately adjacent along the casting length (5) are each less than 600 mm, preferably less than 520 mm.

14. Computer program product comprising commands that cause the continuous casting plant with control device according to one of claims 8-13 to execute the process steps according to one of claims 1-7, by the control device adjusting the adjustable strand guide rollers (7) by means of 202400296 20 the actuators (9) are individually controlled for thickness reduction.

15. Computer-readable medium on which the computer program according to claim 14 is stored.