Fuel cells and electrolysers containing an anion exchange polymer membrane

A non-crosslinked triblock polymer ionomer with quaternary amine groups, coated from its halogenated precursor, addresses brittleness issues in anion exchange membranes, enhancing ionic conductivity and mechanical properties in electrochemical devices.

WO2026238534A1PCT designated stage Publication Date: 2026-11-19MICHELIN & CO (CIE GEN DES ESTAB MICHELIN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063238
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing electrochemical devices, such as fuel cells and electrolyzers, face challenges in preparing anion exchange polymer membranes that maintain ionic conductivity while avoiding brittleness due to ionic interactions, as membranes prepared from ionomers become brittle after quaternization.

Method used

The use of a non-crosslinked ionomer with a triblock polymer structure, where blocks A and B bear quaternary amine groups, is coated from its halogenated precursor, avoiding direct coating of the ionomer to mitigate brittleness and enhance ionic conductivity.

Benefits of technology

This approach maintains mechanical integrity and improves ionic conductivity, enabling efficient operation of fuel cells and electrolyzers with improved performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000004_0001
    Figure IMGF000004_0001
  • Figure IMGF000005_0001
    Figure IMGF000005_0001
  • Figure IMGF000012_0001
    Figure IMGF000012_0001
Patent Text Reader

Abstract

The invention relates to a fuel cell or electrolyser containing an anion exchange polymer membrane which contains a non-crosslinked ionomer, wherein the ionomer is a triblock polymer of formula (I): A-B-A, the symbol A representing a block of a poly(vinylarene), the symbol B representing a block of a copolymer of a 1,3-diene and a vinylarene monomer, wherein the monomer units of the 1,3-diene are selectively hydrogenated, and wherein all or some of the monomer units of the vinylarene monomers constituting the blocks represented by the symbol A, blocks A, have a quaternary amine group and all or some of the monomer units of the vinylarene monomers constituting the block represented by the symbol B, block B, have a quaternary amine group.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Fuel cells and electrolyzers containing an anion-exchange polymer membrane

[0002] The field of the present invention is that of electrochemical devices such as fuel cells and electrolyzers, which contain an anion exchange polymer membrane as an electrolyte.

[0003] The core of a fuel cell and electrolyzer consists of two electrodes, an anode and a cathode, an electrolytic layer separating them, and a catalyst located at the interfaces between the electrolytic layer and each electrode. Fuel cells and electrolyzers include a membrane that forms the electrolytic layer. One of the membrane's constituents is the ionomer, a polymer bearing ionic or ionizable groups. The presence of these ionic or ionizable groups in the polymer is essential for giving the polymer ionic conductivity, enabling the transfer of anions from the cathode to the anode. In this context, block polymers composed of rigid blocks, such as polystyrenes, and soft blocks, such as hydrogenated 1,3-diene homopolymers, have been modified to incorporate quaternary amine groups into the rigid block.The preparation of these ionomers requires a haloalkylation reaction of the aromatic units of the block polymer to form a halogenated polymer, followed by a reaction with a tertiary amine, known as a quaternization reaction, to form the ionomer. The presence of ionic groups in the modified block polymer makes it very poorly soluble due to ionic interactions, and consequently, the coating process from the ionomer is problematic. Therefore, the preparation of an ionomer film by coating is generally carried out not from the ionomer itself, but from its more soluble halogenated precursor. Once the halogenated precursor is coated into a film, the film is then immersed in an aqueous solution containing a tertiary amine to perform the quaternization reaction.Compared to a membrane obtained by a coating process using the ionomer, the membrane obtained by this process has improved ionic conductivity properties, but it becomes brittle. Therefore, there is a need to develop electrochemical devices such as fuel cells and electrolyzers in which the electrolyte is a membrane that can be prepared by coating from its halogenated precursor without becoming more brittle than a membrane prepared by coating from the ionomer.

[0004] Thus, a first object of the invention is an electrochemical device containing an anion exchange polymer membrane which contains a non-crosslinked ionomer, the ionomer being a triblock polymer of formula (I)

[0005] ABA (I),

[0006] the symbol A representing a block of poly(vinylarene),

[0007] the symbol B representing a block of a copolymer of a 1,3-diene and a vinylarene monomer,

[0008] in which the monomer units of 1,3-diene are selectively hydrogenated, all or part of the monomer units of the vinylarene monomers constituting the blocks represented by the symbol A, blocks A, bear a quaternary amine group, all or part of the monomer units of the vinylarene monomers constituting the block represented

[0009] 2024PAT00290WO, represented by the symbol B, block B, carries a quaternary amine group,

[0010] which electrochemical device is a fuel cell or an electrolyzer.

[0011] Detailed description of the invention

[0012] The polymers mentioned in the description can be of fossil origin or bio-based. In the latter case, they can be derived, partially or entirely, from biomass or obtained from renewable raw materials derived from biomass. Similarly, they can also come from the recycling of previously used materials; that is, they can be derived, partially or entirely, from a recycling process, or even obtained from raw materials themselves derived from a recycling process.

[0013] The terms "membranes" and "films" are well known to those skilled in the technical field. It is well understood that a membrane is a structure as defined by IUPAC in "IUPAC Recommendations 1996." Similarly, and in accordance with the IUPAC definition, the term "film" is understood as defined by IUPAC in "IUPAC Recommendations 1996."

[0014] The ionomer useful to the invention is a block polymer bearing quaternary amine groups of formula ABA, the symbol A representing a block of poly(vinylarene), the symbol B representing a block of a copolymer of 1,3-diene and vinylarene monomer, in which the monomer units of the 1,3-diene are selectively hydrogenated and all or part of the monomer units of the vinylarene monomers constituting both blocks A and block B bear a quaternary amine group. Preferably, the block polymer is a linear polymer.

[0015] In this application, the blocks represented by the symbol A are also referred to as A blocks; the block represented by the symbol B is also called B block.

[0016] In the present invention, the term vinylarene monomer means a monomer of the formula Ar-CH=CH2 or Ar-CR=CH2, where the symbol Ar represents an aryl group and the symbol R an alkyl group such as methyl. The aryl group represented by the symbol Ar is preferably a phenyl group or a phenyl group substituted with an alkyl group having 1 to 4 carbon atoms. Examples of vinylarene monomers useful for the purposes of the invention include styrene, styrene substituted with an alkyl group in the para, meta, ortho, or alpha positions. The alkyl group is preferably an alkyl group having 1 to 4 carbon atoms. The vinylarene monomers, identical or different, of poly(vinylarene) and of the copolymer of a 1,3-diene and a vinylarene monomer are preferentially chosen from styrene and styrenes substituted by an alkyl having 1 to 4 carbon atoms and their mixture, the substituted styrenes being able to be substituted in para, ortho, meta or alpha.

[0017] Poly(vinylarene) can be a homopolymer of a vinylarene monomer or a copolymer of two or more vinylarene monomers; the copolymer can be random, tapered, or block. Poly(vinylarene) is preferentially a homopolymer, more preferably a poly(styrene), in which case the vinylarene monomer of poly(vinylarene) is preferentially styrene.

[0018] According to the invention, block B is a hydrogenated block of a copolymer of a 1,3-diene and a vinylarene monomer in which the monomer units of the 1,3-diene are selectively hydrogenated. By hydrogenated block of a copolymer of a 1,3-diene and a monomer

[0019] 2024PAT00290WOvinylarène refers to a block in which the 1,3-diene monomer units are reduced to more than 95%, preferably more than 98%, and more preferably more than 99% by mole of the 1,3-diene monomer units. The hydrogenation reaction of a copolymer of 1,3-diene and vinylarène monomer is a well-known reaction. Reference can be made, for example, to documents EP 1840993 Bl, US 5239010, US 5468574, and US 20070021569, which describe the selective hydrogenation of a copolymer of 1,3-diene and vinylarène monomer of a block polymer of formula (I). The copolymer of a 1,3-diene and a vinylarene monomer useful for the purposes of the invention may be a random, alternating, or gradient copolymer. "A 1,3-diene" means one or more 1,3-dienes. "Several" means at least two. The 1,3-diene preferably contains 4 to 8 carbon atoms. The 1,3-diene is preferably 1,3-butadiene.The vinylarene monomer of the copolymer of a 1,3-diene and a vinylarene monomer is preferably styrene. In a particular embodiment, the 1,3-diene is 1,3-butadiene and the vinylarene monomers of blocks A and B are styrene.

[0020] Both block A and block B of the ionomer share the essential characteristic of both bearing quaternary amine groups. All or part of the monomeric units of the vinylarene monomers constituting blocks A and B bear a quaternary amine group. The monomeric units of vinylarene monomers bearing a quaternary amine group are preferentially monomeric units in which the aromatic ring is substituted by an alkyl chain itself substituted by a quaternary amine group, also known as a quaternary ammonium function.When the vinylarene monomer is styrene or styrene substituted with an alkyl group having 1 to 4 carbon atoms, the respective monomeric units of styrene and styrene substituted with an alkyl group having 1 to 4 carbon atoms, constituting blocks A and B, are preferably monomeric units in which the aromatic ring is substituted by an alkyl chain itself substituted with a quaternary amine group. This alkyl chain is preferably a chain containing 1 to 10 carbon atoms, more preferably a chain containing 2 to 8 carbon atoms. Preferably, this alkyl chain is a linear chain. Preferably, the quaternary amine group is an N-alkylpiperidinium motif, more preferably an N-methylpiperidinium motif.

[0021] According to any one of the embodiments of the invention, the blocks A are preferably polystyrene blocks in which all or part of the styrene monomer units have the phenyl group substituted by an alkyl chain itself substituted by a quaternary amine group, said alkyl chain substituted by a quaternary amine group being preferably a linear chain containing 1 to 10 carbon atoms, more preferably a linear chain containing 2 to 8 carbon atoms, the quaternary amine group being preferably an N-alkylpiperidinium motif, more preferably the N-methylpiperidinium motif.

[0022] According to any one embodiment of the invention, block B is preferably a hydrogenated block of a 1,3-butadiene-styrene copolymer, in which all or part of the styrene monomer units have the phenyl group substituted by an alkyl chain itself substituted by a quaternary amine group, said alkyl chain substituted by a quaternary amine group preferably being a linear chain containing 1 to 10 carbon atoms, plus

[0023] 2024PAT00290WOpreferably a linear chain containing 2 to 8 carbon atoms, the quaternary amine group being preferentially an N-alkylpiperidinium motif, more preferably the N-methylpiperidinium motif.

[0024] The molar content in block B of vinylarene monomer units, with or without a quaternary amine group, varies preferentially in a range from 1% to 25%, more preferentially from 5% to 20% of the repeat motifs constituting block B.

[0025] In the block polymer ionomer of formula (I), block B preferentially represents 50% to 90% by mass of the total mass of the ionomer, more preferably 60% to 80% by mass of the total mass of the ionomer.

[0026] As is known, a monomer unit of a vinylarene monomer bearing a quaternary amine group is obtained by a two-step modification of the monomer unit: a haloalkylation reaction of the aromatic ring to form a halogenated polymer, followed by a reaction with a tertiary amine to form the ionomer. See, for example, patent application WO 2010010290.

[0027] According to any one of the embodiments of the invention, the quaternary amine group is preferably of formula (II) or (III)

[0028] N + (RI)3(II)

[0029]

[0030] The Ri groups, whether identical or different, are alkyl, with R2 representing a divalent, unbranched hydrocarbon chain, saturated or unsaturated, containing 3 to 5 carbon atoms and potentially interrupted by one or more heteroatoms chosen from oxygen, nitrogen, and sulfur. In formulas (II) and (III), the bond attaching the nitrogen atom to the monomeric units of the ionomer is not shown. Furthermore, the quaternary amine group in formula (III) is preferentially an N-alkylpiperidinium group, and more preferably an N-methylpiperidinium group.

[0031] The proportion of quaternary amine groups in the block polymer of formula (I) can vary widely and is adjusted by those skilled in the art according to the desired performance of the anion exchange membrane, particularly based on the desired trade-off between water uptake and ionic conductivity. It is known that increasing the proportion of quaternary amine groups in an ionomer is beneficial for the ionic conductivity of the membrane containing the ionomer, but also tends to decrease the membrane's stability in highly alkaline environments. Preferably, the proportion of quaternary amine groups in the ionomer is greater than or equal to 0.5 meq / g of ionomer (meq / g, milliequivalents per gram) and less than or equal to 2.5 meq / g of ionomer, the ionomer being the block polymer of formula (I).

[0032] The counterions of quaternary amine groups are preferentially halide anions, more preferentially bromide anions.

[0033] The number-average molar mass of the ionomer, a block polymer of formula (I), can vary widely and is chosen by a person skilled in the art according to performance.

[0034] 2024PAT00290W The desired properties of the anion exchange membrane, particularly with regard to the desired compromise between mechanical properties and its ability to be formed into a film, are specified. Preferably, the number-average molar mass of the block polymer ionomer of formula (I) is greater than 20,000 g / mol and less than 500,000 g / mol in polystyrene equivalent (values ​​determined by steric chromatography (SEC) coupled with a refractometer). The number-average molar mass values ​​of the block polymer ionomer of formula (I) are the number-average molar mass values ​​of the block polymer before the introduction of the quaternary amine groups into the block polymer.

[0035] The block polymer ionomer of formula (I) can be prepared from a starting block polymer. The number-average molar mass of the ionomer can be determined from the number-average molar mass of this starting block polymer, as previously mentioned. The starting block polymer differs from the block polymer of formula (I) in that it does not contain quaternary amine groups, specifically that the aromatic rings are not substituted with groups containing a quaternary amine group, and in that the monomeric units of the 1,3-diene are not reduced.To prepare the ionomer, the 1,3-diene monomer units of the starting block polymer are selectively hydrogenated. Then, the vinylarene monomer units of the starting block polymer are modified by a haloalkylation reaction of the aromatic rings to form a halogenated polymer. The haloalkylation reaction is then followed by a reaction with a tertiary amine, referred to hereafter as the quaternization reaction. The reagent used in the haloalkylation reaction is typically a haloalkene. In the haloalkene, the halogen atom and the double bond are preferentially located at opposite ends of the haloalkene's carbon chain. The haloalkene preferentially contains 2 to 10 carbon atoms, and more preferably 4 to 8 carbon atoms. The constituent carbon chain of the haloalkene is preferentially linear.The tertiary amine used in the quaternization reaction is preferably of formula (IV) or (V).

[0036] N (RI)3(IV)

[0037]

[0038] The Ri atoms, whether identical or different, are alkyl, with R2 representing a divalent, unbranched hydrocarbon chain, saturated or unsaturated, containing 3 to 5 carbon atoms and potentially interrupted by one or more heteroatoms chosen from oxygen, nitrogen, and sulfur. The tertiary amine is preferably of formula (V), more preferably N-alkylpiperidine, and even more preferably N-methylpiperidine.

[0039] Typically, the starting block polymer is a triblock polymer, preferably a thermoplastic elastomer. According to any one of the embodiments of the invention, the starting block polymer is preferably a linear polymer.

[0040] 2024PAT00290WO The starting block polymer may be a commercial product, available for example from Kraton or Kuraray, or may be prepared according to any of the known synthesis processes described below:

[0041] - a) copolymerization of the constituent monomers of block B, in this case 1,3-diene and vinylarene monomer, initiated by a dilithiated compound such as the diisopropenylbenzene and sec-butyllithium adduct described for example in document EP1237941 or 1,1,4,4-tetraphenyl-1,4-dilithiobutane, followed by polymerization of the constituent monomer of block A, vinylarene monomer, to form a triblock polymer;

[0042] - b) anionic polymerization of the vinylarene monomer constituting block A initiated by a monolithic compound such as butyllithium, followed by copolymerization of the monomers constituting block B, then reaction with a coupling agent, for example a dichlorosilane to form a triblock.

[0043] A person skilled in the art understands that the methods of preparing the starting block polymer can lead to mixtures containing the starting block polymer. They understand that the method of preparing the starting block polymer according to process b) can lead to the formation of a mixture containing the starting block polymer, polyvinylarene, and a diblock formed in the third, first, and second steps described in the process, respectively. Similarly, they understand that process a) can lead to a mixture containing the starting block polymer and a copolymer of 1,3-diene and vinylarene monomer formed in the first step.

[0044] For the modification of vinylarene monomer units, one can refer for example to document WO 2010010290; for the hydrogenation reaction, one can refer for example to document WO 03008467.

[0045] Alternatively, the ionomer, a block polymer of formula (I), can be prepared from a commercial product, available for example from Kraton or Kuraray, which commercial product is a block polymer already hydrogenated which differs from the ionomer in that it does not carry quaternary amine groups.

[0046] When one of these methods of preparing the starting block polymer results in a mixture containing the starting block polymer, the hydrogenation and modification reactions of the vinylaromatic monomer units are generally carried out on the mixture containing the starting block polymer. In the case where the hydrogenation and modification reactions of the vinylarene monomer units are carried out on the mixture containing the starting block polymer, the ionomer is obtained as a mixture and is generally used without being isolated from this mixture.

[0047] Since the ionomer is very poorly soluble due to ionic interactions resulting from the presence of quaternary amine groups, the preparation of the film to constitute a membrane for a fuel cell or an electrolyzer is carried out by coating preferably from its precursor, the halogenated polymer.

[0048] The halogenated polymer can be put into the form of a film by depositing a solution of the halogenated polymer onto the surface of a support to cover it, followed by drying, a step of evaporation of the solvent constituting the solution or dispersion.

[0049] Typically, a solution of the halogenated polymer is prepared that can be spread onto a flat surface of a substrate to form a polymer layer by coating the substrate.

[0050] The temperature at which the coating is carried out is chosen by a person skilled in the art, taking into account, in particular, the viscosity of the halogenated polymer solution and the boiling point of the solvent used in the halogenated polymer solution. The coating is preferably carried out at a temperature close to ambient temperature, typically 20°C to 25°C, or at a temperature above ambient temperature and below the boiling point of the solvent used in the halogenated polymer solution. The concentration of the polymer solution is adjusted by a person skilled in the art, taking into account, in particular, the solubility of the halogenated polymer in the solvent and the viscosity of the solution. The solvent used in the halogenated polymer solution is chosen by a person skilled in the art, taking into account, in particular, the solubility of the halogenated polymer in said solvent and its boiling point.The concentration of the halogenated polymer solution generally ranges from 1 to 15% by mass of solids. The solvent for the halogenated polymer solution preferably has a boiling point of 120°C or lower, so that it can be removed from the polymer layer, notably by evaporation under vacuum, air currents, or an inert gas such as nitrogen or argon. Suitable solvents include, for example, hydrocarbon solvents, ethers, mixtures of ethers and alcohols, and halogenated solvents. The solvent is preferably chosen from among toluene, methylcyclohexane, tetrahydrofuran, mixtures of tetrahydrofuran and an alcohol, and chloroform, with ethanol being the preferred alcohol.Drying to remove the solvent from the halogenated polymer solution is generally carried out under vacuum, with a stream of air, or with an inert gas such as nitrogen or argon, preferably at a temperature ranging from ambient temperature (23°C) to the boiling point of the solvent, preferably lowered by 15°C under a stream of air or an inert gas. The thickness of the spread layer after drying is preferably less than or equal to 110 pm, more preferably less than or equal to 90 pm. It is preferably greater than or equal to 10 pm, more preferably greater than or equal to 25 pm.

[0051] Once the halogenated polymer is in film form, it is immersed in a bath of tertiary amine solution to modify the vinylaromatic monomer units and thus form the ionomer in film form. Preferably, the ionomer is then rinsed and dried.

[0052] The ionomer in the form of a film with a thickness ranging preferably from a few tens of microns to a few hundred microns, more preferably from 10 pm to 110 pm, even more preferably from 25 pm to 90 pm, constitutes all or part of a membrane of a fuel cell or an electrolyzer.

[0053] According to a preferred embodiment, the electrochemical device is a fuel cell.

[0054] According to another preferred embodiment, the electrochemical device is an electrolyzer.

[0055] The aforementioned features of the present invention, as well as others, will be better understood upon reading the following description of several examples of embodiments of the invention, given by way of illustration.

[0056] Examples

[0057] 2024PAT00290W The constituent ionomer of a membrane is prepared from a commercial product according to the following sequence of steps:

[0058] 1) Bromoalkylation of the commercial product to prepare a brominated polymer, a polymer in which the vinylaromatic monomer units are substituted by an alkyl group substituted with a bromine atom,

[0059] 2) the formation of a film of the brominated polymer by coating,

[0060] 3) the reaction of a tertiary amine with the brominated polymer which is in the form of a film to form the ionomer which is in the form of a film.

[0061] The commercial product, "Al 536" from Kraton, is a hydrogenated triblock polymer, S-EBS-S, whose central block is a copolymer of 1,3-butadiene and styrene, and whose terminal blocks are polystyrenes, with the hydrogenation of the butadiene units exceeding 99%. Table 1 gives the composition of the commercial product, its macrostructure (number-average molar mass Mn measured by size-exclusion chromatography, PS calibration).

[0062] The commercial product, "G1652" from Kraton, is a hydrogenated triblock polymer, S-EB-S, whose central block is polybutadiene and whose terminal blocks are polystyrenes, with a hydrogenation level of the butadiene units exceeding 99%. Table 1 shows the composition of the commercial product and its macrostructure (number-average molar mass Mn measured by size-exclusion chromatography, PS calibration). Table 1:

[0063] Styrene Ethylene Butylene

[0064] (% mol) (% mol) (% mol)

[0065] S-EBS-S 20 60 20

[0066]

[0067] S-EB-S 12 68 20

[0068] Step 1: Bromoalkylation of the commercial product according to the following procedure:

[0069] Place the polymer and the dichloromethane solvent in a bottle under agitation until completely dissolved (approximately 2 hours at room temperature (23°C)) then place the bottle at 5°C for 12 hours;

[0070] Allow the polymer solution to be bubbled through nitrogen at 5°C for 10 min;

[0071] Cool the solution to 0°C in an ice bath for 30 min;

[0072] With stirring, add trifluoroacetic acid drop by drop (0.6 acid / styrene equivalent) in less than 1 min at 0°C (yellow / orange color);

[0073] Leave under agitation for 30 minutes at 0°C (yellow / orange colouring);

[0074] After the stirring time, allow the solution to return to room temperature;

[0075] Add the 6-bromo-l-hexene alkene drop by drop using a syringe pump for 45 min (the solution turns red), while stirring;

[0076] Leave under agitation for an additional 90 minutes at room temperature (23°C) (colour becomes dark red);

[0077] Add methanol as a reaction stopper (decolorization of the medium);

[0078] Neutralize by fractional addition of a KOH solution in methanol (IM), until pH reaches 7-8 (formation of a little precipitate and decolorization from whitish to mauve);

[0079] Coagulate in methanol (3 times the reaction volume) by pouring the methanol drop by drop into the vortex and then recover the polymer using a filter;

[0080] 2024PAT00290WOLash the polymer by pouring it into a bath of deionized water under agitation for 10 min (to remove the salts) then recover the polymer using a filter;

[0081] Retrieve the polymer and let it dry for 24 hours in an oven at 40°C, 150 mbar.

[0082] The levels of ethylene, butylene, styrene, and substituted styrene motifs in the brominated polymer are measured by NMR analysis and are shown in Table 2. The term "substituted styrene" refers to styrene motifs substituted by an alkyl group substituted by a bromine atom. Table 2:

[0083] Brominated styrene Styrene Ethylene Butylene After bromoalkylation

[0084] (%mol) (%mol) (%mol) (%mol)

[0085] S-EBS-S 6 13 61 20

[0086]

[0087] S-EB-S 4 8 68 20

[0088] Step 2: Formation of a brominated polymer film by coating:

[0089] The films are prepared according to the following procedure:

[0090] a) A solution containing the brominated polymer in toluene is prepared,

[0091] b) The solution is poured onto a flat polytetrafluoroethylene (PTFE) support framed by two shims 2000 µm high to form a 2000 µm thick layer of solution by passing a scraper,

[0092] c) The solvent is evaporated at room temperature for 240 minutes under air sweep to dry the layer,

[0093] d) We retrieve the film from its support and peel the film from its support.

[0094] The films have a thickness of 90 to 110 µm.

[0095] Step 3: Reaction of a tertiary amine with the brominated polymer, which is in the form of a film:

[0096] Prepare a 20%w solution of N-methylpiperidine in deionized water;

[0097] In a glass container (such as a beaker, jar, or other glass container), pour the solution up to the 3 / 4 of the volume;

[0098] Using tweezers, gently immerse the film, avoiding the formation of air bubbles and / or it folding back on itself;

[0099] Place a glass lens over the container to isolate it from the external environment; Leave the film submerged for 65 hours at room temperature;

[0100] Replace the solution with deionized water to wash the film. The water is replaced twice a day for two days;

[0101] Place the film on a PTFE support and place the assembly in an oven at 40°C, 150 mbar overnight.

[0102] Ionic conductivity of membranes:

[0103] Conductivity measurements are performed in a CESH-e cell (Biology). To determine the ionic conductivity of the prepared membrane, its electrochemical impedance is measured across the membrane plane at 30°C, the measurement parameters being a 50 mV amplitude change and an applied potential of 0.

[0104] To measure conductivity, the halide counter-ions are replaced by hydroxide anions according to the following procedure:

[0105] The ionomer, in the form of a film and thus forming a membrane, is immersed for 24 h at room temperature (23°C) in a potassium hydroxide solution in demineralized water to carry out ion exchange between bromide and hydroxide ions. It is then soaked for 15 min in a demineralized water solution to remove excess hydroxide ions.

[0106] The ionic conductivity is then measured.

[0107] Water absorption of the membranes:

[0108] It is determined by the mass difference between the membrane immersed for 24 hours in deionized water (resistivity on the order of MQ.cm'). 1 ) and the membrane dried for 24 hours at 40°C and 100 mb of pressure. The mass percentage of water absorbed by the membrane ("water uptake", WU) is determined using the following calculation:

[0109] %WU=(mi mm ergée _ Hlséchée) / lllséchée X 100.

[0110] Mechanical properties:

[0111] The mechanical properties are determined by tensile testing at 23 °C on a TA Instruments TAHR20 apparatus. A rectangular sample measuring 5 cm x 1 cm is placed between the jaws of the apparatus and is deformed at a speed of 50 mm / min at ambient temperature (between 20 and 25°C) and at ambient humidity of 30 to 60 %RH until the sample breaks.

[0112] Results :

[0113] The results are shown in Table 3.

[0114] Table 3:

[0115] Conductivity, Water uptake, Deformation at failure, Stress at failure (% by mass), (MPa), mS / cm

[0116] S-EBS-S 4 73 452 4.8

[0117]

[0118] S-EB-S 10 87 256 4.8

[0119] The membrane is also prepared by a different process that involves coating with the ionomer. According to this process, the quaternization reaction is carried out in solution, and then the ionomer is deposited as a film according to the following procedures:

[0120] The brominated polymer is dissolved in dichloromethane to form a 2.5% polymer solution by weight. Ten equivalents of N-methylpiperidine per bromine atom grafted onto the polymer are then added. The mixture is stirred for 48 hours at 40°C, then coagulated and washed in methanol. The ionomer is collected using filter paper and then dried in an oven at 40°C for 24 hours.

[0121] a) The quaternized polymer is dissolved in toluene to form a 2% mass solid solution.

[0122] b) the solution is poured onto a flat PTFE support framed by two shims of a height of 2000 pm to form a layer of solution 2000 pm thick by passing a scraper in order to obtain a layer 100 pm thick after drying (after step c described below).

[0123] 2024PAT00290WOc) the solvent is evaporated at room temperature for 4 hours under air sweep to dry the layer.

[0124] The resulting membranes were also evaluated, and the results are shown in Table 4. Table 4:

[0125] Conductivity, Water uptake, Deformation at failure, Stress at failure (% by mass), (MPa), mS / cm

[0126] S-EBS-S 1 38 483 3.9

[0127]

[0128] S-EB-S 7 48 Does not break 3.6

[0129] Unlike membranes prepared from S-EB-S copolymer, membranes prepared by coating with S-EBS-S copolymer exhibit virtually unchanged mechanical properties, regardless of whether the coating process uses the ionomer or the halogenated polymer. It has also been observed that membranes coated with the halogenated polymer of S-EBS-S have improved ionic conductivity properties compared to membranes coated with the ionomer.

[0130] A fuel cell or electrolyzer using a block polymer electrolyte of formula (I) has the advantage of being able to be manufactured by a process that is easily implemented and that gives the best ionic conductivity and mechanical properties.

[0131] 2024PAT00290WO

Claims

Demands 1. Electrochemical device containing an anion exchange polymer membrane which contains a non-crosslinked ionomer, the ionomer being a triblock polymer of formula (I) ABA (I), the symbol A representing a block of poly(vinylarene), the symbol B representing a block of a copolymer of a 1,3-diene and a vinylarene monomer, in which the monomer units of 1,3-diene are selectively hydrogenated, all or part of the monomer units of the vinylarene monomers constituting the blocks represented by the symbol A, block A, bear a quaternary amine group, all or part of the monomer units of the vinylarene monomers constituting the block represented by the symbol B, block B, bear a quaternary amine group, which electrochemical device is a fuel cell or an electrolyzer.

2. Electrochemical device according to claim 1 in which the vinylarene monomers, identical or different, of poly(vinylarene) and of the copolymer of a 1,3-diene and a vinylarene monomer are selected from styrene and styrenes substituted with an alkyl having 1 to 4 carbon atoms and their mixture, the substituted styrenes being able to be substituted in para, ortho, meta or alpha positions.

3. Electrochemical device according to claim 1 or 2 wherein the monomer units of vinylarene monomers bearing a quaternary amine group are monomer units in which the aromatic ring is substituted by an alkyl chain itself substituted by a quaternary amine group.

4. Electrochemical device according to any one of claims 1 to 3 wherein the molar content in block B of vinylarene monomer units bearing or not a quaternary amine group varies in a range from 1% to 25%, preferably from 5% to 20% of the repeating motifs constituting block B.

5. Electrochemical device according to any one of claims 1 to 4 wherein the 1,3-diene is 1,3-butadiene and the vinylarene monomers of blocks A and B are styrene.

6. Electrochemical device according to any one of claims 1 to 5 wherein block B represents from 50% to 90% by mass of the total mass of the ionomer, preferably from 60% to 80% by mass of the total mass of the ionomer.

7. An electrochemical device according to any one of claims 1 to 6, wherein the proportion of quaternary amine groups in the ionomer is greater than or equal to 0.5 meq / g of the ionomer and less than or equal to 2.5 meq / g of the ionomer.

8. An electrochemical device according to any one of claims 1 to 7, wherein the quaternary amine group is of formula (II) or (III). N + (RI)3(II) The Ri, whether identical or different, being alkyl, R2 represents a chain 2024PAT00290WO unbranched divalent hydrocarbon, saturated or unsaturated, containing 3 to 5 carbon atoms and capable of being interrupted by one or more heteroatoms selected from oxygen, nitrogen and sulfur.

9. Electrochemical device according to any one of claims 1 to 8 wherein the quaternary amine group is an N-alkylpiperidinium.

10. Electrochemical device according to any one of claims 1 to 9 wherein the quaternary amine group is N-methylpiperidinium.

11. Electrochemical device according to any one of claims 1 to 10, which electrochemical device is a fuel cell.

12. Electrochemical device according to any one of claims 1 to 10, which electrochemical device is an electrolyzer. 2024PAT00290WO