Polishing compositions with tunable copper removal rates in barrier polishing
Alkaline barrier CMP compositions with copper ion complexing agents like triazole derivatives enhance copper removal rates and selectivity, addressing the limitations of existing technologies in semiconductor wafer planarization.
Patent Information
- Application Number
- PCT/EP2026/063361
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing barrier CMP compositions fail to achieve tunable copper removal rates and selectivity for copper to TEOS and copper to TaN polishing, as azole compounds used as corrosion inhibitors have high solubility in water and form complexes that hinder copper removal.
Alkaline barrier CMP polishing compositions using copper ion complexing agents, such as triazole derivatives, in combination with inorganic oxide abrasive particles, oxidizers, and pH adjusters, to enhance copper removal rates and selectivity.
The compositions provide boosted copper removal rates and tunable selectivity for copper to TEOS and copper to TaN polishing, essential for achieving global flatness in semiconductor wafer planarization.
Smart Images

Figure IMGF000003_0001 
Figure IMGF000004_0001 
Figure IMGF000004_0002
Abstract
Description
Attorney Docket No. P25-209-SEC-W001TITLE OF THE INVENTION:POLISHING COMPOSITIONS WITH TUNABLE COPPER REMOVAL RATES IN BARRIER POLISHINGCROSS REFERENCE TO RELATED PATENT APPLICATIONS
[0001] The application claims the benefit of U.S. Application No. 63 / 804,317 filed on May 12, 2025, the disclosure of which is hereby incorporated by reference as if fully set forth.BACKGROUND OF THE INVENTION
[0002] This invention relates to the Chemical Mechanical Planarization (CMP) polishing compositions, methods, and systems to be used for barrier layer Chemical Mechanical Planarization polishing in semiconductor manufacture.
[0003] Specifically, the Chemical Mechanical Planarization (CMP) polishing composition (interchangeable with polishing slurry, polishing formulation) provides high copper removal rates and tunable removal rate ratio of copper polishing vs TECS or TaN polishing at alkaline pH conditions.
[0004] An important step in the fabrication processes to manufacture microelectronic devices is the chemical mechanical planarization polishing process to planarize the patterned wafer surface with multi-type of films to achieve global flatness through well-designed chemical mechanical planarization polishing compositions which provide the tunable film removal rates and optimized selectivity among various types of the films via polishing process.
[0005] Usually, a barrier layer covers the patterned dielectric layer, and a metal layer covers the barrier layer. The metal layer has at least sufficient thickness to fill the patterned trenches with metal to form circuit interconnects.
[0006] A barrier typically is a metal, metal alloy, or intermetallic compound, such as tantalum or tantalum nitride. The barrier forms a layer that prevents electron migration or diffusion between layers within a wafer. For example, barriers prevent the diffusion of interconnect metal such as copper or silver into an adjacent dielectric. Barrier materials must be resistant to corrosion by most acids, and thereby, resist dissolution in a fluid polishing composition for CMP. Furthermore, these barrier materials may exhibit a toughness that resists removal by abrasion abrasive particles in a CMP slurry and from fixed abrasive pads.
[0007] In relation to CMP, the current state of this technology involves the use of a multi-step, such as, a two-step process to achieve local and global planarization.
[0008] During step 1 of a CMP process, metal layer such as the overburden copper is removed, while leaving a smooth planar surface on the wafer with metal-filled lines,Attorney Docket No. P25-209-SEC-W001vias and trenches that provide circuit interconnects planar to the polished surface. First step of polishing steps tends to remove excess interconnect metals, such as copper. Then step 2 of the CMP process, frequently referred to as a barrier CMP process, follows to remove the barrier layer and excess metal layers and other films on the surface of the patterned wafers to achieve both local and global planarization surface on the dielectric layer.
[0009] Barrier slurry compositions need to meet several stringent requirements including high barrier removal rates, very low post-polish topography, no corrosion defects and very low scratches or residue defects. Therefore, there are significant needs for barrier CMP compositions, CMP process(es), or methods when these requirements become more stringent as the semiconductor industry continues to move towards smaller feature sizes.
[0010] The chemical mechanical planarization process using barrier chemical mechanical planarization polishing compositions involves polishing multi-type films on a patterned wafer surface, such as metal, oxide, dielectric, barrier films.
[0011] U.S. Pat. No. 8,404,146 discloses the acidic barrier CMP polishing compositions which contain colloidal silica particles as abrasives, organic surfactant, especially anionic organic surfactants, a corrosion inhibitor including benzotriazole or its derivatives, an organic acid, and a quaternary ammonium cation.
[0012] U.S. Pat. No. 10,988,635 discloses the barrier CMP polishing compositions which contain cationic colloidal silica particles as abrasives, and a corrosion inhibitor including triazole compound or its derivatives, mainly a triazole pyridine compound.
[0013] U.S. Pat. No. 9,505,951 discloses the barrier CMP polishing compositions which contain colloidal silica particles as abrasives, pH adjusting agent, and a copper corrosion inhibitor including an azole compound or its derivatives.
[0014] As the afore listed prior arts, the known prior works teach that azole compounds are commonly used as corrosion inhibitors in metal polishing, particularly for yellow metals like copper and its alloys. Azoles form a protective coating or passivation layer on the metal surface, thus hinder corrosion.
[0015] However, the afore listed prior arts failed to teach barrier chemical mechanical planarization polishing compositions fortuning copper removal rates in barrier layer polishing using certain types of azole compounds which have higher solubility in deionized water and have functions as copper ion chelating agents to form more easily removal copper ion-some azole molecule complexes through polishing process.
[0016] Thus, there is a significant need for barrier Chemical Mechanical Planarization polishing compositions fortuning copper removal rates.Attorney Docket No. P25-209-SEC-W001SUMMARY OF THE INVENTION
[0017] The present invention satisfies the need by providing alkaline barrier CMP polishing compositions using a new type of copper ion complexing agents, methods, and systems for achieving boosted copper removal rates and enhanced tunable copper to TEOS and copper to TaN polishing selectivity.
[0018] In one aspect (Aspect 1), there is provided an alkaline barrier CMP polishing composition comprising:inorganic oxide abrasive particles;copper corrosion inhibitor;copper ion complexing agent;oxidizer;aqueous solvent; andoptionally at least one ofsalts of silicate;pH adjusting agent;biocide;wherein the polishing composition has a pH of 8 to 12, preferably 9 to 11.5, and more preferably 10 to 11.
[0019] The inorganic oxide abrasive particles include but are not limited to colloidal silica, high purity colloidal silica, fumed silica, alumina, titania, and combinations thereof.
[0020] The oxidizer includes but is not limited to hydrogen peroxide, ammonium persulfate, potassium persulfate, peroxy sulfonic acid, peroxy acetic acid, periodic acid, and combinations thereof. Hydrogen peroxide is preferred.
[0021] The copper corrosion inhibitor includes but is not limited to benzotriazole or its derivatives, and has the general molecular structure (1):
[0022] In general molecular structure (1), Ri can be hydrogen, amino, alkyl, amide or alkoxy groups, R2 can be hydrogen, alkyl, alkoxy or other organic functional groups which can be connected to the -4, -5, -6 or -7 position of the aromatic 6-Attorney Docket No. P25-209-SEC-W001member ring; wherein in alkyl group -(CH2)nCH3, n is ranged from 1 to 11 , and in alkoxy group -O(CH2)mCH3having m is ranged from 1 to 11.
[0023] Example of molecular structures are: benzotriazole (i) when both Ri and R2are hydrogen atoms; tolyltriazole (ii) when R1 is a hydrogen atom and R2is a methyl group connected to the 6-member ring at position -5; benzotriazole-1 -methanol (iii) when R1 is methanol and R2 is a hydrogen atom; and benzotriazole-1 -carboxamide (iv) when R1 is an amide group, and R2 is a hydrogen atom.(iii):
[0024] The copper ion complexing agent is a triazole compound and its derivatives and has general molecular structure (2) and (3):and
[0025] In the general molecular structures of (2) and (3), R3, R4, R5, R6, R7 or R8 can be hydrogen atom, amino group, alkyl group, alkoxy group, carboxylic acid group, amide group, and / or other organic functional groups do not contain any aromatic ring. R3, R4 and R5 can be the same functional groups or different functional groups in general molecular structure (2), R6, R7 and R8 can be the same functional groups or different functional groups in general molecular structure (3).
[0026] Some examples of copper ion complexing agents include but are not limited to 1,2,4-triazole(a), 1,2,3-triazole(b), 3,5-diamino-1 ,2,4-triazole(c), 1,2,3-triazole-1-Attorney Docket No. P25-209-SEC-W001ethanol(d), 3-amino-1,2,4-triazole(e), amino-triazole(f), and 1 ,2,3-triazole-5-carboxylic acid(g), and the molecular structures are shown below:(a), (b),N.HO.\ — I (d)1and (g).
[0027] The salts of silicate include but are not limited to potassium silicate, and ammonium silicate.
[0028] The aqueous solvent includes, but is not limited to, deionized (DI) water, distilled water, and organic alcohols.
[0029] In another aspect (Aspect 2), there is provided a Chemical Mechanical Planarization polishing method for chemical mechanical planarization of a patterned wafer comprising at least one surface containing copper; comprising, consisting essentially of, or consisting of the steps of:Attorney Docket No. P25-209-SEC-W001providing the chemical mechanical planarization polishing compositions in Aspect 1, providing a polishing pad;contacting the at least one surface containing copper with the polishing pad and the chemical mechanical planarization polishing composition;polishing the at least one surface containing copper.
[0030] In yet another aspect (Aspect 3), there is provided a system of chemical mechanical planarization (CMP) polishing a patterned wafer having at least one surface containing copper; the system comprising:a. the semiconductor substrate;b. the chemical mechanical planarization polishing composition in Aspect 1; c. a polishing pad,wherein the at least one surface containing copper is in contact with the polishing pad and the chemical mechanical planarization polishing composition.
[0031] The semiconductor substrate comprising at least one surface containing copper further comprises TaN and TEOS.
[0032] Other aspects, features, and embodiments of the invention will be more fully apparent from the ensuing disclosure and appended claims. The embodiments of the invention can be used alone or in combinations with each other.DETAILED DESCRIPTION OF THE INVENTION
[0033] In the global planarization of using barrier chemical mechanical polishing compositions to polish the patterned wafers, enhancing copper film removal rates and tuning copper to silicon dioxide and copper to tantalum nitride polishing selectivity are very important to achieve global flatness of the polished patterned wafers.
[0034] The present invention provides CMP polishing compositions used for Chemical Mechanical Polishing or Planarization (CMP) polishing of semiconductor devices, particularly as alkaline barrier slurries.
[0035] The CMP polishing compositions using a new type of copper ion complexing agents for achieving boosted copper removal rates and copper to oxide and copper to tantalum nitride polishing selectivity.
[0036] In one aspect (Aspect 1), there is provided an alkaline barrier CMP polishing composition comprising:inorganic oxide abrasive particles;Attorney Docket No. P25-209-SEC-W001copper corrosion inhibitor;copper ion complexing agent;oxidizer;aqueous solvent; andoptionally at least one ofsalts of silicate;pH adjusting agent;biocide;wherein the polishing composition has a pH of 8 to 12, preferably 9 to 11.5, and more preferably 10 to 11.
[0037] The inorganic oxide abrasive particles include but are not limited to colloidal silica, high purity colloidal silica, fumed silica, alumina, titania, and combinations thereof.
[0038] Colloidal silica particles are preferred. The colloidal silica particles include, but are not limited to, the standard colloidal silica particles, the high purity colloidal silica particles made from the precursor of tetramethyl orthosilicate (TMOS) or tetraethyl orthosilicate (TEOS).
[0039] The more preferred colloidal silica particles are the high purity colloidal silica particles made from TMOS or TEOS.
[0040] The inorganic oxide abrasive particles may have any shape, spherical or cocoon shapes are preferred.
[0041] The inorganic oxide abrasive particles may have surface been modified to have a positive or negative zeta potential at a given pH.
[0042] The mean particle size (MPS) or a primary particle size of abrasive particles, such as colloidal silica particles or high purity colloidal silica particles, are ranged from 10 nm to 1 ,000nm, 15 nm to 500 nm, 20 to 400 nm, 30 nm to 250 nm, or 40 nm to 100 nm. MPS refers to the diameter of the particles and is measured using dynamic light scattering (DLS) technology.
[0043] The CMP polishing compositions comprise from 0.1 wt.% to 20.0 wt.%, from 1.0 wt.% to 15.0 wt.%, and from 2.0 wt.% to 10.0 wt.% of abrasive particles.
[0044] The oxidizer includes but is not limited to hydrogen peroxide, ammonium persulfate, potassium persulfate, peroxy sulfonic acid, peroxy acetic acid, periodic acid, and combinations thereof. Hydrogen peroxide is preferred.Attorney Docket No. P25-209-SEC-W001
[0045] The CMP polishing compositions comprise from 0.01 wt.% to 5.0 wt.%, the from 0.1 wt.% to 3.0 wt.%, or from 0.5 wt.% to 2.0 wt.% of oxidizer.
[0046] The copper corrosion inhibitor includes but is not limited to benzotriazole or its derivatives, and has the general molecular structure (1):(1)
[0047] In general molecular structure (1), Ri can be hydrogen, amino, alkyl, amide or alkoxy groups, R2 can be hydrogen, alkyl, alkoxy or other organic functional groups which can be connected to the -4, -5, -6 or -7 position of the aromatic 6-member ring; wherein in alkyl group -(CH2)nCH3, n is ranged from 1 to 11 , and in alkoxy group -O(CH2)mCH3having m is ranged from 1 to 11.
[0048] Example of molecular structures are: benzotriazole (i) when both R1 and R2are hydrogen atoms; tolyltriazole (ii) when R1 is a hydrogen atom and R2is a methyl group connected to the 6-member ring at position -5; benzotriazole-1 -methanol (iii) when R1 is methanol and R2 is a hydrogen atom; and benzotriazole-1 -carboxamide (iv) when R1 is an amide group, and R2 is a hydrogen atom.
[0049] The CMP polishing compositions comprise from 0.0005 wt.% to 0.5 wt.%, 0.001 wt.% to 0.25 wt.%, or 0.0025 wt.% to 0.1 wt.% of a copper corrosion inhibitor.
[0050] The copper ion complexing agent is triazole compounds and their derivatives and has general molecular structure (2) and (3):Attorney Docket No. P25-209-SEC-W001
[0051] In the general molecular structures of (2) and (3), R3, R4, R5, R6, R7 or R8 can be hydrogen atom, amino group, alkyl group, alkoxy group, carboxylic acid group, amide group, and / or other organic functional groups that do not contain any aromatic ring. R3, R4 and R5 can be the same functional groups or different functional groups in general molecular structure (2), R6, R7 and R8 can be the same functional groups or different functional groups in general molecular structure (3).
[0052] Some examples of copper ion complexing agents include but are not limited to 1,2,4-triazole(a), 1,2,3-triazole(b), 3,5-diamino-1 ,2,4-triazole(c), 1,2,3-triazole-1- ethanol(d), 3-amino-1,2,4-triazole(e), amino-triazole(f), and 1 ,2,3-triazole-5-carboxylic acid(g), and the molecular structures are shown below:Attorney Docket No. P25-209-SEC-W001(e), (f).and (g).
[0053] The CMP polishing compositions comprise from 0.0005 wt.% to 1.0 wt.%, 0.001 wt.% to 0.5 wt.%, or 0.0025 wt.% to 0.25 wt.% of copper ion complexing agents.
[0054] Please note that, the copper ion complexing agents are different than the copper corrosion inhibitors in the CMP polishing compositions.
[0055] The afore listed prior arts teach that azole compounds are commonly used as corrosion inhibitors in metal polishing, particularly for yellow metals like copper and its alloys. Those azoles form a protective coating or passivation layer on the metal surface, thus hinder corrosion but typically reduce the Cu removal rate.
[0056] Without being bound by any theory, the disclosed new type of copper ion complexing agents comprise triazoles having structures (2) and (3) are more soluble in deionized water to react with various copper ions having different oxidation states in the presence of an oxidizing agent to form complexes which are more easily to be removed, thus, lead to the enhanced copper removal rates. Thus, the disclosed triazoles work as complexing agents, more specifically, copper ion complexing agents, not as copper corrosion inhibitors in current application.
[0057] The salts of silicate include but are not limited to potassium silicate, and ammonium silicate.
[0058] The CMP polishing compositions may contain from 0.1 wt.% to 5.0 wt.%, from 0.5 wt.% to 4.0 wt.%, and from 1.0 wt.% to 3.0 wt.% of salts of silicate.
[0059] The optional pH adjuster has acidic pH adjuster used to adjust pH towards the more acidic direction, and alkaline pH adjuster used to adjust pH towards the more alkaline direction.
[0060] The chemical mechanical planarization polishing composition comprises a pH adjuster selected from the group consisting of (a) nitric acid, hydrochloric acid, sulfuric acid, tartaric acid, succinic acid, citric acid, malic acid, malonic acid, various fatty acids, various polycarboxylic acids, and mixtures thereof to lower the pH; and (b) potassium hydroxide(KOH), sodium hydroxide, ammonium hydroxide,Attorney Docket No. P25-209-SEC-W001tetraethylammonium hydroxide, ethylenediamine, piperazine, polyethyleneimine, modified polyethyleneimine, and mixtures thereof to raise the pH.
[0061] The alkaline barrier CMP polishing compositions may contain from 0 .0 wt.% to 1.0 wt.%, 0.01 wt.% to 0.50 wt.%, or 0.05 wt.% to 0.25 wt.% pH adjuster.
[0062] The optional biocide can be any biocide which provides active ingredients to prevent biological growth and thus provides more stable shelf time of the CMP polishing compositions.
[0063] The optional biocide includes but is not limited to NeoIone™ M10, a methyl isothiazolinone-based biocide from DuPont; Kathon™, Kathon™ CG / ICP II, from Dow Chemical Co. They have active ingredients of 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-4-isothiazolin-3-one.
[0064] The CMP polishing composition may contain 0.0000 wt.% to 0.05 wt.%; 0.0002 wt.% to 0.025 wt.%; or 0.002 wt.% to 0.01 wt.% biocide.
[0065] The aqueous solvent includes, but is not limited to, deionized (DI) water, distilled water, and organic alcohols.
[0066] The benzotriazole or its derivatives disclosed as copper corrosion inhibitors are excluded from the use as the disclosed copper ion complexing agent due to their low solubility in water which makes them unsuitable as a complexing agent.
[0067] In another aspect (Aspect 2), there is provided a Chemical Mechanical Planarization polishing method for chemical mechanical planarization of a patterned wafer comprising at least one surface containing copper; comprising, consisting essentially of, or consisting of the steps of:providing the chemical mechanical planarization polishing compositions in Aspect 1, providing a polishing pad;contacting the at least one surface containing copper with the polishing pad and the chemical mechanical planarization polishing composition;polishing the at least one surface containing copper.
[0068] In yet another aspect (Aspect 3), there is provided a system of chemical mechanical planarization (CMP) polishing a patterned wafer comprising at least one surface containing copper; the system comprising:a. the semiconductor substrate;b. the chemical mechanical planarization polishing composition in Aspect 1;c. a polishing pad,wherein the at least one surface containing copper is in contact with the polishing pad and the chemical mechanical planarization polishing composition.
[0069] The patterned wafer comprising at least one surface containing copper may further comprise TaN, TEOS, and other barrier films.Attorney Docket No. P25-209-SEC-W001EXAMPLES CMP Methodology
[0070] In the examples presented below, CMP experiments were run using the procedures and experimental conditions given below.GLOSSARY / COMPONENTS
[0071] The high purity colloidal silica particles were supplied by Fuso Chemical Co., LTD. in Japan and were used as abrasives having a mean particle size or primary particle size of approximately 20 nanometers (nm) to 100 nanometers (nm) range.
[0072] The chemical additives: salts of potassium silicate, triazole compounds or derivatives, benzotriazoles or derivatives, hydrogen peroxide, pH adjusting agents, were supplied by Sigma-Aldrich, St. Louis, MO.
[0073] TEOS: tetraethyl orthosilicate
[0074] Polishing Pad: VP6000, or any other pads were used during CMP, supplied by DuPont Electronics & Industrial.
[0075] PARAMETERS
[0076] General
[0077] A: angstrom(s) - a unit of length
[0078] BP: back pressure, in psi units
[0079] CMP: chemical mechanical planarization
[0080] CS: carrier speed
[0081] DF: Down force: pressure applied during CMP, unit: psi
[0082] min: minute(s)
[0083] ml: milliliter(s)
[0084] mV: millivolt(s)
[0085] psi: pounds per square inch
[0086] PS: platen rotational speed of polishing tool, in rpm (revolution (s) per minute)
[0087] SF: composition flow, ml / min.
[0088] Wt. %: weight percentage (of a listed component) based on the total weight of the CMP polishing composition is100%.
[0089] Copper: Cu Film
[0090] TEOS: SiO2film
[0091] TaN: TaN FilmAttorney Docket No. P25-209-SEC-W001
[0092] Cu, TEOS or TaN Removal Rates: Measured Cu, TEOS or TaN removal rate at a given down pressure. The down pressure of the CMP tool was 2.0 psi in the examples listed below.
[0093] Cu Removal Rates: Measured Cu removal rate at a given down pressure. The down pressure of the CMP tool was 2.0 psi in the examples listed below.
[0094] TEOS Removal Rates: Measured TEOS removal rate at a given down pressure. The down pressure of the CMP tool was 2.0 psi in the examples listed below.
[0095] TaN Removal Rates: Measured TaN removal rate at a given down pressure. The down pressure of the CMP tool was 2.0psi in the examples listed below.
[0096] Metrology
[0097] Film removal rates were measured with a ResMap CDE, model 168, manufactured by Creative Design Engineering, Inc, 20565 Alves Dr., Cupertino, CA, 95014. The ResMap tool is a four-point probe sheet resistance tool. Forty-nine-point diameter scan at 5mm edge exclusion for film was taken.CMP Tool
[0098] The CMP tool that was used is a 300mm AMAT LK polisher manufactured by Applied Materials, 3050 Boweres Avenue, Santa Clara, California, 95054. A VP6000 pad supplied by DuPont Electronics & Industrial, 451 Bellevue Rd., Newark, DE 19713 was used on platen 1 for blanket wafer studies.
[0099] The VP6000 pad was broken in by conditioning the pad through polishing 25 TEOS dummy wafers using a commercial barrier CMP slurry supplied by Versum Materials Inc. at baseline conditions.
[0100] Polishing experiments were conducted using PECVD or LECVD or HDP TEOS wafers, PECVD TaN wafers, and electroless plating Cu wafers. These blanket wafers were purchased from Silicon Valley Microelectronics, 2985 Kifer Rd., Santa Clara, CA 95051.Polishing Experiments
[0101] In blanket wafer studies, oxide blanket wafers, TaN blanket wafers, and Cu blanket wafers were polished at baseline conditions. The tool baseline conditions were: table speed; 93 rpm, head speed: 87 rpm, membrane pressure; 2.0 psi DF, slurry flow rate: 300 ml / min.Example 1
[0102] Reference sample (Ref.) was made with 7.47 wt.% high purity colloidal silica, 2.44 wt.% potassium silicate, 0.026 wt.% benzotriazole (BTA), and 1.5 wt.% hydrogen peroxide with pH adjusted to 10.3 by using alkaline pH adjusting agent.Attorney Docket No. P25-209-SEC-W001
[0103] Working sample (#1) was made with 7.47 wt.% high purity colloidal silica, 2.44 wt.% potassium silicate, 0.026 wt.% benzotriazole (BTA), 0.005 wt.% 1,2,4-triazole, and 1.5 wt.% hydrogen peroxide with pH adjusted to 10.3 by using alkaline pH adjusting agent.
[0104] Working sample (#2) was made with 7.47 wt.% high purity colloidal silica, 2.44 wt.% potassium silicate, 0.026 wt.% benzotriazole (BTA), 0.020 wt.% 1,2,4-triazole, and 1.5 wt.% hydrogen peroxide with pH adjusted to 10.3 by using alkaline pH adjusting agent.
[0105] Working sample (#3) was made with 7.47 wt.% high purity colloidal silica, 2.44 wt.% potassium silicate, 0.026 wt.% benzotriazole (BTA), 0.040 wt.% 1,2,4-triazole, and 1.5 wt.% hydrogen peroxide with pH adjusted to 10.3 by using alkaline pH adjusting agent.
[0106] The effects of copper ion complexing agents, 1,2,4-Triazole, an azole compound on copper, TEOS and TAN removal rates (RR at A / min.) were evaluated.
[0107] The change of Cu RR vs the concentration of 1 ,2,4-T riazole was also calculated.
[0108] The results were listed in Table 1.Table 1. 1,2,4-triazole on Cu RR and Cu RR change (%) Cu RR TEOS RR TaN RR Cu RR Composition(A / min.) (A / min.) (A / min.) Change%Ref. 249 458 780 0.0% Sample# 1 309 468 762 24.1% Sample# 2 407 462 710 63.5%Sample# 3 647 435 750 159.8%
[0109] As shown in Table 1, the use of copper ion complexing agent, 1,2,4-triazole at three different concentrations, there were no obvious impacts on removal rates for silicon dioxide and TaN film polishing. However, significantly enhanced copper film removal rates were observed. Cu removal rate was enhanced by 24.1 %, 63.5%, and 159.8% when 0.005 wt.%, 0.020 wt.% or 0.040 wt.% of 1 ,2,4-triazole were added to the reference composition, respectively.
[0110] The enhanced copper film removal rates by using 1,2,4-triazole also led to the increased Cu to oxide film and Cu to TaN polishing selectivities which are some key factors to be considered in barrier CMP polishing compositions to be used for barrier CMP applications.
[0111] The effects of 1,2,4-triaozle as copper ion complexing agent on copper to TEOS and copper to TaN polishing selectivity (Cu RR: TEOS RR and Cu RR: TaN RR) were listed in Table 2.Attorney Docket No. P25-209-SEC-W001Table 2. 1 ,2,4-triazole on Cu:TEOS and Cu:TaN Selectivity Cu:TEOSComposition Cu RR (A / min.) Cu:TaN Selectivity SelectivityRef. 249 0.54 0.32 Sample# 1 309 0.66 0.41 Sample# 2 407 0.88 0.57Sample# 3 647 1.49 0.86
[0112] As the results shown in Table 2, the use of 1 ,2,4-triazole as copper ion complexing agent at different concentrations, there are no obvious impacts on TEOS RR or TaN RR; thus, the increasing of Cu RR led to the increasing of Cu:TEOS and Cu:TaN polishing selectivity respectively.Example 2
[0113] Reference sample (Ref.) was the same as used in Example 1.
[0114] Working sample #4, #5 and #6 were the same as #1 , #2 and #3 in Example 1 except 3-amino-1,2,4-triazole (amitrole) replaced 1,2,4-triazole.
[0115] The effects of 3-amino-1,2,4-triazole on copper removal rates (RR at A / min) were evaluated. The results of the film removal rate and copper removal rate changes were listed in Table 3.Table 3. 3-amino-1 ,2,4-triazole on Cu RR and Cu RR change (%)Cu RR TEOS RR TaN RR Cu RR Composition (A / min.) (A / min.) (A / min.) Change%Ref. 249 458 780 0.0%Sample# 4 284 491 735 14.1%Sample# 5 344 444 752 38.2%Sample# 6 379 485 752 52.2%
[0116] As the results shown in Table 3, like the results shown in Table 1, there were no obvious impacts on removal rates for silicon dioxide and TaN film polishing when 3-amino-1 ,2,4-triazole was added to the ref. composition; again, enhanced copper film removal rates were observed. Cu removal rate was enhanced by 14.1%, 38.1%, and 52.2% when 0.005 wt.%, 0.020 wt.% or 0.040 wt.% of 3-amino-1 ,2,4-triazole was added to the reference composition, respectively.
[0117] Copper to TEOS and Copper to TaN polishing selectivity were listed in Table 4.Attorney Docket No. P25-209-SEC-W001Table 4. 3-amino-1 ,2,4-triazole on Cu:TEOS and Cu:TaN Selectivity Cu RR Cu:TEOSComposition Cu:TaN(A / min.) Selectivity SelectivityRef. 249 0.54 0.32 Sample# 4 284 0.58 0.39Sample# 5 344 0.77 0.46Sample# 6 379 0.78 0.50
[0118] As the results shown in Table 4, like the results shown in Table 2, there are no obvious impacts on TEOS RR or TaN RR from the use of 3-amino-1,2,4-triazole as copper ion complexing agent as difference concentrations; thus the increase of Cu RR led to the increase of Cu:TEOS and Cu:TaN polishing selectivity respectively.Example 3
[0119] In this Example, 3, 5-diamino-1 ,2,4-triazole was used to replace 1,2,4-triazole in Example 1 for working sample #7, #8, and #9.
[0120] The effects of 3, 5-diamino-1 ,2,4-triazole on copper removal rates (RR at A / min) were evaluated. The results of the film removal rate and copper removal rate changes were listed in Table 5.Table 5. 3, 5-diamino-1 ,2,4-triazole on Cu RR (A / min.) & Cu RR% Change Cu RR TEOS RR TaN RR Cu RR Composition(A / min.) (A / min.) (A / min.) Change% Ref. 249 458 780 0.0% Sample# 7 273 459 784 9.6% Sample# 8 336 449 786 34.9%Sample# 9 366 444 770 47.0%
[0121] As the results shown in Table 5, like the results shown in Table 1, there were no obvious impacts on removal rates for silicon dioxide and TaN film polishing when 3,5-diamino-1,2,4-triazole was added to the ref. composition; again, enhanced copper film removal rates were observed. Cu removal rate was enhanced by 9.6%, 34.9%, and 47.0% when 0.005 wt.%, 0.020 wt.% and 0.040 wt.% of 3,5-diamino-1 ,2,4-triazole was added to the reference composition, respectively.
[0122] The effects of 3, 5-diamino-1 ,2,4-triazole on Cu to TEOS and Cu to TaN polishing selectivity were listed in Table 6.Attorney Docket No. P25-209-SEC-W001Table 6. 3,5-diamino-1 ,2,4-triazole on Cu:TEOS and Cu:TaN Selectivity Cu RR Cu:TEOSComposition Cu:TaN(A / min.) Selectivity SelectivityRef. 249 0.54 0.32 Sample# 7 273 0.59 0.35Sample# 8 336 0.75 0.43Sample# 9 366 0.82 0.48
[0123] As the results shown in Table 6, like the results shown in Table 2, there are no obvious impacts on TEOS RR or TaN RR from the use of 3, 5-diamino-1 ,2,4-triazole as copper ion complexing agent at difference concentrations; thus the increase of Cu RR led to the increase of Cu:TEOS and Cu: TaN polishing selectivity respectively.
[0124] The working examples have demonstrated that triazoles having the general molecular structures of (2) and (3) used in the disclosed alkaline barrier CMP polishing compositions boost copper removal rates but have minimal effects on the dielectric films such as TEOS and barrier layer films such as TaN removal rates. Thus, the disclosed triazoles work as complexing agents, more specifically, copper ion complexing agents in polishing copper in the present invention.
[0125] Furthermore, the use of triazoles in the polishing compositions have provided tunable selectivity ranges of Cu:TEOS and Cu:TaN : >0.3 to< 1.5.
[0126] The embodiments of this invention listed above, including the working examples, are exemplary of numerous embodiments that may be made of this invention. It is contemplated that numerous other configurations of the process may be used, and the materials used in the process may be elected from numerous materials other than those specifically disclosed.
Claims
Attorney Docket No. P25-209-SEC-W001CLAIMS1. A Chemical Mechanical Planarization (CMP) polishing composition for Cu barrier CMP polishing process and application comprising:inorganic oxide abrasive particles;copper corrosion inhibitors;copper ion complexing agents;at least one per-oxy compound;aqueous solvent;optionally at least onesalt of silicate;a biocide; anda pH adjuster.
2. The Chemical Mechanical Planarization (CMP) polishing composition according to claim 1 , wherein the inorganic oxide abrasive particles are selected from the group consisting of colloidal silica, high purity colloidal silica, fumed silica, alumina, titania, and combinations thereof.
3. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1-2, wherein the inorganic oxide abrasive particles are silica based abrasives selected from the group consisting of colloidal silica, silica particles doped by other inorganic oxide within lattice of the colloidal silica; high purity colloidal silica particles; and combinations thereof.
4. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1-3, wherein the inorganic oxide abrasive particles are the high purity colloidal silica particles.
5. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1-4, wherein the inorganic oxide abrasive particles have a mean particle size or a primary particle size ranging from 10 nm to 1 ,000 nm, from 25 nm to 250 nm, or from 30 nm to 100 nm.
6. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 5, wherein the inorganic oxide abrasive particles are present in the CMP composition at a concentration ranging from 0.1 wt.% to 20.0 wt.%, from 1.0 wt.% to 15.0 wt.%, or from 2.0 wt.% to 10.0 wt.%.
7. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 6, wherein the copper corrosion inhibitor has a general molecular structure (1):Attorney Docket No. P25-209-SEC-W001wherein Ri is selected from the group consisting of hydrogen, amino, alkyl, amide, and alkoxy groups; R2 is selected from the group consisting of hydrogen, alkyl, alkoxy, and other organic functional groups which can be connected to the - 4, -5, -6 or -7 position of the aromatic 6-member ring; wherein alkyl group - (CH2)nCH3 has n from 1 to 11 , and alkoxy group -O(CH2)mCH3 has m from 1 to 11.
8. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 7, wherein the copper corrosion inhibitor is selected from the group consisting of benzotriazole, totyltriazole, benzotriazole- 1- methanol, benzotriazole- 1 -carboxamide, and combinations thereof.
9. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 8, wherein the copper corrosion inhibitor is present in the CMP composition at a concentration ranging from 0.0005 wt.% to 0.5 wt.%, 0.001 wt.% to 0.25 wt.%, or 0.0025 wt.% to 0.1 wt.%.
10. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 9, wherein the copper ion complexing agent has a general molecular structure selected from the group consisting of (2), (3) and combinations thereof;Attorney Docket No. P25-209-SEC-W001wherein R3, R4, R5, R6, R7 or R8 can be hydrogen atom, amino group, alkyl group, alkoxy group, carboxylic acid group, amide group, or other organic functional groups that do not contain any aromatic ring;R3, R4 and R5 can be the same functional groups or different functional groups; andR6, R7 and R8 can be the same functional groups or different functional groups.
11. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 10, wherein the copper ion complexing agent is selected from the group consisting of 1 ,2,4-triazole, 1 ,2,3-triazole, 3,5-diamino-1 ,2,4- triazole, 1,2,3-triazole-1-ethanol, 3-amino-1,2,4-triazole, amino-triazole, and 1,2,3-triazole-5-carboxylic acid, and combinations thereof.
12. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 11 , wherein the copper ion complexing agent is presented in the CMP composition at a concentration ranging from 0.0005 wt.% to -1.0 wt.%, 0.001 wt.% to -0.5 wt.%, or 0.0025 wt.% to 0.25 wt.%.
13. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 12, wherein the oxidizer is selected from the group consisting of ammonium persulfate, potassium persulfate, peroxy sulfonic acid, peroxy acetic acid, periodic acid, hydrogen peroxide, and combinations thereof.
14. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 13, wherein the oxidizer is present in the chemical mechanical planarization polishing composition at a concentration ranging from 0.01 wt.% to 5.0 wt.%, the from 0.1 wt.% to 3.0 wt.%, or from 0.5 wt.% to 2.0 wt.%.
15. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 14, wherein the optional salt of silicate is selected from potassium silicate, ammonium silicate, and combinations thereof.
16. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 15, wherein the salt of silicate is present in the CMP composition at a concentration ranging from 0.1 wt.% to 5.0 wt.%, from 0.5 wt.% to 4.0 wt.%, or from 1.0 wt.% to 3.0 wt.%.Attorney Docket No. P25-209-SEC-W00117. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 16, wherein the Chemical Mechanical Planarization (CMP) polishing composition comprises a pH adjuster selected from the group consisting of (a) nitric acid, sulfuric acid, tartaric acid, succinic acid, citric acid, malic acid, malonic acid, various fatty acids, various polycarboxylic acids, and mixtures thereof to lower the pH; and (b) potassium hydroxide(KOH), sodium hydroxide, ammonia, tetraethylammonium hydroxide, ethylenediamine, piperazine, polyethyleneimine, modified polyethyleneimine, and mixtures thereof to raise the pH.
18. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 17, wherein the Chemical Mechanical Planarization (CMP) polishing composition comprises 0.0 wt.% to 1.0 wt.%, 0.01 wt.% to 0.50 wt.%, or 0.05 wt.% to 0.25 wt.% of a pH adjuster.
19. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 18, wherein the Chemical Mechanical Planarization (CMP) polishing composition has a pH of from 8 to12, 9 to 11.5, or 10 to 11.
20. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 19, wherein the chemical mechanical planarization polishing composition comprises a biocide having active ingredient of 5-chloro-2- methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, or combinations thereof.
21. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 20, wherein the Chemical Mechanical Planarization (CMP) polishing composition comprises 0.0000 wt.% to 0.05 wt.%; 0.0002 wt.% to 0.025 wt.%; or 0.002 wt.% to 0.01 wt.% of a biocide.
22. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 21, wherein the chemical mechanical planarization polishing composition comprises:the inorganic oxide abrasive particles selected from the group consisting of colloidal silica, high purity colloidal silica, fumed silica, and combinations thereof;Attorney Docket No. P25-209-SEC-W001the copper corrosion inhibitors selected from the group consisting of benzotriazole, totyltriazole, benzotriazole- 1 -methanol, benzotriazole- 1- carboxamide, and combinations thereof;the copper ion complexing agents selected from the group consisting of 1 ,2,4- triazole, 1,2,3-triazole, 3,5-diamino-1,2,4-triazole, 1, 2, 3-triazole-1 -ethanol, 3- amino-1,2,4-triazole, amino-triazole, and 1,2,3-triazole-5-carboxylic acid, and combinations thereof; andthe at least one per-oxy compound selected from the group consisting of ammonium persulfate, potassium persulfate, peroxy sulfonic acid, peroxy acetic acid, periodic acid, hydrogen peroxide, and combinations thereof.
23. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 22, wherein the chemical mechanical planarization polishing composition comprises:the inorganic oxide abrasive particles selected from the group consisting of colloidal silica, high purity colloidal silica, and combinations thereof;the copper corrosion inhibitors selected from the group consisting of benzotriazole, benzotriazole-1-methanol, and combinations thereof;the copper ion complexing agents selected from the group consisting of 1 ,2,4- triazole, 3,5-diamino-1,2,4-triazole, 3-amino-1,2,4-triazole, and combinations thereof; andthe at least one per-oxy compound selected from the group consisting of ammonium persulfate, peroxy sulfonic acid, periodic acid, hydrogen peroxide, and combinations thereof.
24. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 23, wherein the chemical mechanical planarization polishing composition comprises:high purity colloidal silica;benzotriazole;the copper ion complexing agents selected from the group consisting of 1 ,2,4- triazole, 3,5-diamino-1,2,4-triazole, 3-amino-1,2,4-triazole, and combinations thereof; andhydrogen peroxide;wherein the Chemical Mechanical Planarization (CMP) polishing composition has a pH of from 8 to12 or 9 to 11.5.Attorney Docket No. P25-209-SEC-W00125. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 24, wherein the chemical mechanical planarization polishing composition comprises:the inorganic oxide abrasive particles selected from the group consisting of colloidal silica, high purity colloidal silica, and combinations thereof;the copper corrosion inhibitors selected from the group consisting of benzotriazole, benzotriazole-1-methanol, and combinations thereof;the copper ion complexing agents selected from the group consisting of 1 ,2,4- triazole, 3,5-diamino-1,2,4-triazole, 3-amino-1,2,4-triazole, and combinations thereof;potassium silicate, ammonium silicate, or combinations thereof;andthe at least one per-oxy compound selected from the group consisting of ammonium persulfate, peroxy sulfonic acid, periodic acid, hydrogen peroxide, and combinations thereof.
26. The Chemical Mechanical Planarization (CMP) polishing composition according to any one of claims 1 to 24, wherein the chemical mechanical planarization polishing composition comprises:high purity colloidal silica;benzotriazole;the copper ion complexing agents selected from the group consisting of 1 ,2,4- triazole, 3,5-diamino-1,2,4-triazole, 3-amino-1,2,4-triazole, and combinations thereof;potassium silicate; andhydrogen peroxide;wherein the Chemical Mechanical Planarization (CMP) polishing composition has a pH of from 8 to12 or 9 to 11.5.
27. A method of Chemical Mechanical Planarization (CMP) polishing, the method comprises steps of:providing a patterned wafer having at least one surface containing at least one first material and at least one second material;providing a polishing pad;providing the Chemical Mechanical Polishing (CMP) composition according to any one of claims 1 to 26;Attorney Docket No. P25-209-SEC-W001contacting at least one surface of the patterned wafer with the polishing pad and the chemical mechanical polishing composition; andpolishing the at least one surface;wherein the at least one first material comprises metal, and the at least one second material comprises dielectric materials, materials in a barrier layer other than metal, or combinations thereof.
28. The method of Chemical Mechanical Planarization (CMP) polishing according to claim 27, wherein the at least one first material comprises copper, and at least one second material comprises silicon dioxide (TECS) film, tantalum nitride (TaN) film, or combinations thereof.
29. The method of Chemical Mechanical Planarization (CMP) polishing according to claim 28, wherein removal rate (RR) selectivity of Cu RR vs TECS RR, or Cu RR vs TaN RR is >0.3 and < 1.5.
30. A system of Chemical Mechanical Planarization (CMP) polishing comprising a patterned wafer having at least one surface containing at least one first material and at least one second material;the chemical mechanical polishing (CMP) composition according to any one of claims 1 to 26; anda polishing pad;wherein the at least one first material comprises metal, and the at least one second material comprises dielectric materials, materials in a barrier layer other than metal or combinations thereof; and the at least one first material and the at least one second material are in contact with the chemical mechanical planarization polishing composition and the polishing pad.
31. The system of Chemical Mechanical Planarization (CMP) polishing according to claim 30, wherein the at least one first material comprises copper, and at least one second material comprises silicon dioxide (TECS) film, tantalum nitride (TaN) film, or combinations thereof.
32. The system of Chemical Mechanical Planarization (CMP) polishing according to claim 31 , wherein removal rate (RR) selectivity of Cu RR vs TECS RR, or Cu RR vs TaN RR is >0.3 and < 1.5.