A mega tensile steel wire for rubber reinforcement
A lower carbon content and optimized heat treatment process for mega tensile steel wires address brittleness and breakage issues, achieving enhanced ductility and cost-effectiveness in production.
Patent Information
- Application Number
- PCT/EP2026/063370
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-19
AI Technical Summary
The production of mega tensile steel wires is hindered by high brittleness and breakage risks during processing, leading to high production costs due to the use of high carbon content steel wire rods, which are difficult to produce and costly.
A method involving a steel wire with a lower carbon content (0.86%-0.95%) and improved ductility, achieved through a specific heat treatment and reduced area reduction rates in the wet wire drawing process, resulting in a steel wire with enhanced torsion ductility and reduced wire fracture risk.
The method produces a mega tensile steel wire with improved ductility and reduced production costs, minimizing wire breakage during processing and maintaining desired tensile strength.
Smart Images

Figure EP2026063370_19112026_PF_FP_ABST
Abstract
Description
A mega tensile steel wire for rubber reinforcement DescriptionTechnical Field
[0001] The invention relates to a mega tensile steel wire for rubber reinforcement.The invention also relates to a method for making the steel wire, and a steel cord comprising two or more steel wires.Background Art
[0002] Steel wire is widely used as a reinforcement for rubber articles, such as tire, hose, conveyor belt and etc. The steel wire can be used solely as a reinforcement for rubber articles or can be used to make a steel cord for reinforcing rubber articles.
[0003] A trend in rubber tire field is a lighter tire which has advantages such as lower rolling resistance and energy saving for carbon emissions reduction. Steel wires or steel cords, as the reinforcement of the tire, are developed to be finer and lighter accordingly. One solution is to increase the tensile strength of the steel wire, and due to the use of steel wires with higher tensile strength, the finer steel wires can provide sufficient cord breaking load, as thus the diameter and the weight of the steel cord can be reduced. The use of the finer and lighter steel cords or steel wires makes the tire being thinner and lighter. The tensile strength of the steel wire is developed from normal tensile (NT) or high tensile (HT) to super high tensile (ST), even ultra-high tensile (UT) and now mega tensile (MT).
[0004] One problem of the production of a mega tensile steel wire is the steel wire is very brittle and easier to break either during the processing of drawing to make a steel wire from wire rod until a desired fine diameter or during the processing of twisting to make a steel cord by twisting two or more steel wires together. JP6724400 discloses a steel wire for tire, the steel wire has a carbon content of 0.8-1.2% such as 0.88% or 0.90%, the steel wire has a tensile strength of at least 4620MPa, the steel wire has a diameter of 0.04-0.4mm, the steel wire has a torsion performance of 23-26 turns (100D test). It discloses a method for making the steel wire including the steps of: the use of norean elliptical die having an elliptical hole, and an elliptical die having a hole rotated by 90 degrees with respect to the 1 MIE25B0004PCT Classification: Confidential Informationhole of the first elliptical die, a skin pass step with an area reduction rate of 1 %-5%, a short peening step after the final drawing step, and heating the wire after final drawing step. However, the ductility performance of the steel wire is still not very good, to meet the expectation. This leads to high filament fracture during the cord making process, low productivity, and high production cost.
[0005] Another problem of the production of a mega tensile steel wire is the use of high carbon content steel wire rod as raw material to make the mega tensile steel wire, this is very costly. CN103785704 discloses a steel wire with a carbon content of 0.97%, the steel wire has a diameter of 0.35mm, and it has a tensile strength of 3920MPa, which is corresponding to 4620- 2000d MPa, the steel wire has a torsion performance of 33 turns (100D). However, with the higher carbon content of the steel, the cost becomes higher, and the steel wire rod with high carbon content, as the raw material of steel wire, i.e. , 0.97% C%, is very difficult to produce, and brings the risk of unstable raw material supply and high cost.
[0006] It is desired to develop a mega tensile steel wire with reduced wire fracture / breaking risk and lower production cost.Disclosure of Invention
[0007] The primary object of the invention is to provide a mega tensile steel wire for rubber reinforcement with reduced wire fracture / breaking risk and lower production cost.
[0008] The second object of the invention is to provide a method for making the mega tensile steel wire with better torsion ductility.
[0009] The second object of the invention is to provide a method for making the mega tensile steel wire with better torsion ductility.
[0010] The third object of the invention is to provide a steel cord comprising two or more mega tensile steel wires mentioned above.
[0011] According to the first aspect of the invention, a steel wire is provided, the steel wire comprises a steel substrate and a metallic coating covering on the steel substrate, the steel wire having a tensile strength in a range of 4600-2000xd - 5000-2000xd MPa, d being the steel wire diameter expressed in mm and in a range of 0.15-0.55 mm, the steel wire has a2 MIE25B0004PCT Classification: Confidential Informationcarbon content of 0.86%-0.95% in weight percentage, the steel wire has a ductility torsion value, measured by a 100D torsion test method, being more than 30 turns.
[0012] The invention provides a mega tensile steel wire with relatively lower carbon content and better ductility performance. The invention mega tensile steel wire has an improved ductility performance particular the torsion ductility performance, i.e. , ductility torsion value of the invention mega tensile steel wire is more than 30 turns, and thus the wire fracture / breaking risk during the cord making process is reduced relative to the prior arts. And, the invention mega tensile steel wire has a relatively lower carbon content of 0.86%-0.95%, which leads to a lower production cost of a mega tensile steel wire. In theory, to make the steel wire with mega tensile from a relatively lower carbon content steel wire rod for example 0.86%-0.95% or about 90%, this requires a higher total area reduction rate of wet wire drawing (‘WWD’) process to realize a mega tensile steel wire with such relatively lower carbon content, for example, higher than 100% or even higher total area reduction rate of WWD, ‘the total area reduction rate of WWD’ means the total area reduction rate of the steel wire during the whole WWD process. Higher total area reduction rate of WWD brings two risks, one is lower ductility performance of the steel wire, another is wire breaking during WWD process. Oppositely, if the total area reduction rate of WWD is not high enough, it is impossible to reach desired tensile strength, i.e., mega tensile. The invention overcomes the abovementioned drawbacks and realizes a mega tensile steel wire with a relatively lower carbon content and an improved ductility performance.
[0013] Preferably, the carbon content of the steel wire is in a range of 0.88%- 0.94%. More preferably, the carbon content of the steel wire is in a range of 0.89%-0.93%.
[0014] Preferably, the steel wire diameter is in a range of 0.16-0.40 mm, or in a range of 0.16-0.30mm .
[0015] Preferably, the ductility torsion value of the steel wire is more than 35 turns, or in a range of 40-80 turns. Ductility performance of the steel wire is3 MIE25B0004PCT Classification: Confidential Informationvery critical for the making processes of steel cord, i.e. , the process of twisting the steel wires together for forming a steel cord. If the ductility performance of the steel wire is poor, the loss of the tensile strength of the steel wire caused by twisting operation during the cord making process is big, and the steel wire fracture or breaking is more likely to occur during the twisting. The ductility torsion value of the steel wire is one of the features for charactering the ductility performance of the steel wire. The higher the ductility torsion value of the steel wire, the lower the loss of the tensile strength of the steel wire caused by twisting operation during the cord making process, and the lower the wire fracture risk during the cord making process.
[0016] Preferably, the steel wire has a delamination torsion value, measured by a delamination torsion test method, being more than 160 turns. The delamination torsion value of the steel wire is another feature for charactering the ductility performance of the steel wire. The delamination torsion value of the steel wire is the torsion value until the steel wire delamination occurs (but not until the steel wire breaking). Delamination torsion value of the steel wire is more meaningful for the production of steel cord, because if the steel wire delamination occurs during the cord making process, this quality of the final steel cord will not meet the requirements. The higher the delamination torsion value of the steel wire, the lower the loss of the tensile strength of the steel wire caused by twisting operation during the cord making process, and the lower the wire fracture risk during the cord making process.
[0017] Preferably, the delamination torsion value of the steel wire is more than 170 turns, or in a range of 170-500 turns.
[0018] The metallic coating could be any one of the existing coating for steel wire known in the field of rubber reinforcement, to provide adhesion with the rubber compound and corrosion resistance. Preferably, the metallic coating of the steel wire is zinc coating, zinc alloy coating such as zincsilver coating, copper alloy coating such as brass coating or bronze coating, ternary or quaternary coating comprising three or four metals selected from the group consisting of copper, zinc, cobalt, nickel, tin,4 MIE25B0004PCT Classification: Confidential Informationindium, titanium, manganese, iron, silver, bismuth and molybdenum, such as Zn-Cu-Co, Zn-Cu-Fe, Zn-Cu-Ni ternary coating.
[0019] The steel wire can be made from a wire rod that is made from pure fresh steel which doesn’t contain any recycled steel such as direct reduced iron, hot briquetted iron or pig iron, or a wire rod made from steel containing recycled steel or steel containing recycled steel. Preferably, the steel wire is made from a wire rod which is made from steel with a recycled steel content of at least 15%.
[0020] According to the second aspect of the invention, a method for making a steel wire as recited in the first aspect of the invention is provided. The method comprises the steps of:1) providing an intermediate wire with an intermediate diameter ranging from 1.0 mm to 2.5 mm, the intermediate wire comprises a steel substrate, 2) subjecting the intermediate wire to a heat treatment, the heat treatment comprising firstly heating the intermediate wire at a temperature of 900- 1000°C and thereafter cooling the intermediate wire at a temperature of 550-590°C,3) subjecting the intermediate wire to a coating process to apply a metallic coating covering on said steel substrate,4) subjecting the intermediate wire to a wet wire drawing operation thereby obtaining a steel wire, the wet wire drawing operation comprises a series of drawing passes for area reduction, the total area reduction rate of wet wire drawing operation is 97.0%-98.2% and the area reduction rate of each of last six drawing passes is 2.5%-7%.
[0021] In theory, to make the steel wire with mega tensile from a relatively lower carbon content steel wire rod for example 0.86%-0.95% or 90% of C%, this requires a higher total area reduction rate of wet wire drawing (‘WWD’) process to realize a mega tensile steel wire with relatively lower carbon content, for example, higher than 100% or even higher total area reduction rate of WWD, ‘the total area reduction rate of WWD’ means the total area reduction rate of the steel wire during the whole WWD process. Higher total area reduction rate of WWD brings two risks, one is lower ductility performance of the steel wire, another is wire breaking during WWD5 MIE25B0004PCT Classification: Confidential Informationprocess. Oppositely, if the total area reduction rate of WWD is not high enough, it is not possible to reach desired tensile strength, i.e. , mega tensile. The invention method overcomes the abovementioned drawbacks and realizes a mega tensile steel wire with a relatively lower carbon content, higher ductility performance and reduced wire breaking risk during wet wire drawing process. The invention slightly reduces the total area reduction rate of WWD, this ensures that the steel wire has mega tensile; and the invention reduces the area reduction rate of each of last six drawing passes, as thus the heat inside the steel wire caused by drawing of last six drawing passes is reduced, the dynamic aging of the steel wire is less, the brittleness of the steel wire is reduced, as thus the ductility performance particular the torsion ductility performance of the steel wire is improved, while the tensile strength of the steel wire is as expected, i.e., mega tensile level.
[0022] As a result of lower cooling temperature in step 2), the intermediate wire, after heat treatment in step 2), has a pearlite structure with an average lamellar spacing of the pearlite of no more than 60 nm. A pearlite structure with such a fine lamellar spacing may be obtained by known methods, for example by increasing the undercooling, which is defined as the difference between the equilibrium phase-transition temperature and the actual temperature at which the phase transition starts, while suppressing the formation of bainite.
[0023] According to the third aspect of the invention, a steel cord for rubber reinforcement is provided. The steel cord comprises two or more steel wires as recited in the first aspect of the invention, the steel cord has a cord twist pitch of 4 mm to 40 mm, preferably 6mm-38mm, wherein at least one of the two or more steel wires has a ductility torsion value, measured by a 100D torsion test method on the steel wire unravelled out of the steel cord, of more than 24 turns.
[0024] Preferably, at least one of the two or more steel wire has a ductility torsion value, measured by a 100D torsion test method on the steel wire unravelled out of the steel cord, of more than 27 turns, or in a range of SO- 72 turns.6 MIE25B0004PCT Classification: Confidential Information
[0025] Preferably, at least one of the two or more steel wire has a delamination torsion value, measured by a delamination torsion test method on the steel wire unravelled out of the steel cord, of more than 145 turns, or in a range of 150-450 turns.
[0026] Preferably, at least one of the two or more steel wires is measured with a surface twisting angle in a range of 1.5-5 degree when it is unravelled out of the steel cord. Depending on the steel cord construction and the cord making method, the steel wire of the steel cord may have a relatively big surface twisting angle, i.e. , in a range of 1.5-5 degree, or the steel wire of the steel cord may have a relatively small surface twisting angle, i.e., 0-0.5 degree, which is measured on the steel wire that is unravelled out of the steel cord.
[0027] The invention steel wire and the invention steel cord can be used to reinforce any rubber article known in the field, such as tire, hose, conveyor belt and etc.
[0028] The tire comprises at least one belt layer, at least one carcass layer, at least one tread layer and a pair of bead portions, wherein the belt layer, the carcass layer, the tread layer and / or the bead portions comprises at least one steel wire as recited in the first aspect of the invention or at least one steel cord as recited in the third aspect of the invention.Brief Description of the Figures in the Drawings
[0029] Figure 1 illustrates cross-sectional views of 1x2 steel cord.
[0030] Figures 2a-2b illustrate surface drawing lines on a steel wire from cabled cord and an enlarged view, respectively.
[0031] Figures 3a-3b illustrate surface drawing lines on a steel wire from bunched cord and an enlarged view, respectively.Mode(s) for Carrying Out the Invention
[0032] The steel wire is made from a wire rod with a carbon content of 0.86%- 0.95% in wt%. The wire rod may contain at least 15% recycled steel. The invention mega tensile steel wire improves ductility performance and thus reduces wire fracture / breaking risk during cord making process relative to the prior arts. And, the invention mega tensile steel wire has a carbon 7 MIE25B0004PCT Classification: Confidential Informationcontent of 0.86%-0.95% in wt%, which leads to a lower production cost of a mega tensile steel wire. According to one embodiment of the invention, a steel wire for rubber reinforcement is provided, the steel wire comprises a steel substrate and a metallic coating covering on the steel substrate and has a tensile strength in a range of 4600-2000xd - 5000-2000xd MPa, d being the steel wire diameter expressed in mm and in a range of 0.15-0.55 mm, the steel wire has a carbon content of 0.86%-0.95% in wt%, the steel wire has a ductility torsion value, measured by a 100D torsion test method, being more than 30 turns.
[0033] The steel wire diameter d is preferably in a range of 0.16-0.40 mm or more preferably in a range of 0.16-0.30 mm. The carbon content of the steel wire is preferably in a range of 0.88%-0.94% in wt%, more preferably in a range of 0.89%-0.93% in wt%.
[0034] 100D torsion test method is according to GB / T 239.1 -2012 - Metallic material - Wire- Part 1 : Simple torsion test, with one specific setting on the gauge length L between two chucks (nominal value) being 100xD, D is the steel wire diameter in mm. Preferably, the invention steel wire has a ductility torsion value, measured by the 100D torsion test method, being more than 35 turns, or even in a range of 40-80 turns.
[0035] 100D torsion test method and delamination torsion test method are two methods of measuring the torsion ductility performance of the steel wire. Delamination torsion test method is:1 ) Prepare a steel wire specimen with a length of 50 cm;2) Place the steel wire specimen between the two chucks;3) Mark a line on one side of the steel wire specimen with a marker to monitor the applied torsions on the steel wire specimen;4) Start with the sequence of rotations and monitor the torsion stability of the steel wire specimen; the sequence of rotations is according to the following:i. Rotate the steel wire in the first direction (for example, S direction) with a number of rotations of 30 times,ii. Rotate the steel wire in the second direction which is opposite to the first direction (for example, Z direction) with a number of8 MIE25B0004PCT Classification: Confidential Informationrotations according to the steel wire diameter as defined in table below,Steel wire diameter D (mm) Number of rotations (turns)50.15<D<0.18 680.18<D<0.23 600.23<D<0.30 52100.30<D<0.40 460.40<D<0.55 42iii. Rotate the steel wire in the first direction (for example, S direction) until the wire delamination occurs and continue until wire fracture.5) Register torsion when the wire delamination occurs, as thedelamination torsion; if no wire delamination occurs, the torsion when the wire fracture occurs is registered as the delamination torsion.
[0036] The invention steel wire has a delamination torsion value, measured bythe delamination torsion test method, being more than 160 turns, or more than 170 turns, for example, in a range of 170-500 turns.
[0037] Table 1 shows the comparison between the invention steel wires and the reference steel wire in terms of wire diameter, carbon content, tensile strength, delamination torsion value and 100D torsion value (i.e., ductility torsion value).
[0038] Table 1Sample Wire Carbon Tensile Delamination 100D Total area Area reduction rate Cooling diameter content strength Torsion Torsion reduction of last 6 drawing temperature at (mm) (%) (MPa) (turns) (turns) rate of passes heat treatment WWDInvention 0.301 0.90 4182 217 33 97.66% 5.08%;4.57%;4.67%; 570°C 1 4.79%;5.59%;3.59%Invention 0.240 0.90 4263 255 39 97.91% 5.44%;4.79%;4.92%; 570°C 2 4.21%;5.15%;3.54%9 MIE25B0004PCT Classification: Confidential InformationInvention 0.200 0.91 4313 324 43 98.07% 6.06%;5.48%;6.43%; 585°C 3 5.00%;5.97%;3.67% Reference 0.300 0.90 4156 76 18 98.30% 7.36%;7.02%;7.27%; 650°C 1 6.54%;4.15%;3.84%
[0039] The above table shows that on the premise of substantially equivalent wire diameter and carbon content, the invention steel wires reach desired tensile strength, i.e. , mega tensile, the invention steel wires also have obviously improved torsion ductility performance, as measured by the delamination torsion test method and the 100D torsion test method, relative to the reference steel wire. Since ductility performance is very critical for the processes, such as the process of twisting the steel wires together for forming a steel cord, the poor ductility performance of the reference steel wire is more likely to lead to wire fracture or breaking and loss of the wire tensile strength during the wire twisting, while the obviously high ductility performance of the invention steel wires leads to lower fracture or breaking risk and less loss of the wire tensile strength during the steel cord making process.
[0040] The tensile strength of the steel wire is measured according to the standard ISO6892-1 :2019.
[0041] In order to make a mega tensile steel wire with an improved ductility performance by avoiding the use of high total reduction rate of WWD, a method for making the mega tensile steel wire with better torsion ductility is provided.
[0042] An intermediate wire with an intermediate diameter ranging from 1.0 mm to 2.5 mm is provided for making the mega tensile steel wire. The intermediate wire comprises a steel substrate, and it is made by the known process, i.e., drawing a wire rod with a big diameter, i.e., 5-5.5mm, until a fine diameter, i.e., 1.0-2.5mm.
[0043] The wire rod has a carbon content of 0.86%-0.95% wt%, preferably in the range of 0.88%-0.94% wt% or 0.89%-0.93% wt%, one example is about 0.90% wt%. The wire rod comprises other components like 0.05%-0.50% Si, 0.15%-0.60% Mn, 0.05%-0.60% Cr, no more than 0.10% Cu, no more than 0.01% Al, no more than 0.10% Ni, no more than 0.10% S, no moreio MIE25B0004PCT Classification: Confidential Informationthan 0.10% P, no more than 0.05% Mo, no more than 0.01% Sn, no more than 0.01% N, while the rest is iron and the unavoidable impurities. All the above contents are in weight percentage. The content value is average of measurements of six specimens of one steel wire.
[0044] The wire rod is firstly cleaned by mechanical descaling and / or by chemical pickling in a H2SO4 or HCI solution in order to remove the oxides present on the surface. The wire rod is then rinsed in water and is dried. The dried wire rod is then subjected to a first series area reduction operations of dry drawing operations in order to reduce the diameter until a first diameter.
[0045] At this first diameter, e.g. at about 3.0 to 3.5 mm, the dry drawn steel wire is subjected to a first heat treatment, called patenting. Patenting means first austenitizing until a temperature of about 1000°C followed by a transformation phase from austenite to pearlite at a temperature of about 600 - 650°C. The steel wire is then ready for further mechanical deformation.
[0046] Thereafter the steel wire is further dry drawn from the first diameter until a second diameter in a second number of diameter reduction steps. The second diameter typically ranges from 1.0 mm to 2.5 mm. An intermediate wire with an intermediate diameter ranging from 1.0mm to 2.5mm is thereafter provided.
[0047] The intermediate wire is then subjected to a heat treatment, i.e. , firstly heating the intermediate wire at a temperature of 900-1000°C and thereafter cooling the intermediate wire at a temperature of no more than 600°C, for example 500 - 590°C, to allow for transformation to much finer pearlite, for example with an average lamellar spacing of the pearlite of no more than 60 nm, the finer pearlite structure gives the steel wire a higher tensile after heat treatment.
[0048] After heat treatment, the steel wire is provided with a metallic coating for adhesion performance with rubber compound and corrosion resistance performance, for example brass coating: copper is plated on the steel filament and zinc is plated on the copper, and a thermos-diffusion treatment is applied to form the brass coating. Alternatively, the steel filament can be provided with a zinc coating, zinc alloy coating such as11 MIE25B0004PCT Classification: Confidential Informationzinc-silver coating, copper alloy coating such as bronze coating, ternary or quaternary coating comprising three or four metals selected from the group consisting of copper, zinc, cobalt, nickel, tin, indium, titanium, manganese, iron, silver, bismuth and molybdenum or other known metal.
[0049] The metallic coating coated steel filament is then subjected to a wet wire drawing operation. Wet drawing operation includes a series of drawing passes, for example 23-28 drawing passes according to the invention, the drawing passes are the area reduction operations done by various drawing dies. According to the invention, to reach mega tensile level and improved torsion ductility performance, the total area reduction rate of wet wire drawing operation is set to be 97.0% - 98.2% to reach mega tensile for a steel wire with a relative lower carbon content of 86%-95% in wt%, and the area reduction rate of each of last six passes is reduced to be 2.5%-7% (much smaller than the existing area reduction rate of 13%- 14%). Firstly, the slightly reduced total area reduction rate of wet wire drawing operation ensures that the steel wire has mega tensile; secondly, due to the smaller area reduction in the last six drawing passes, the heat inside the steel wire caused by drawing is reduced, the dynamic aging of the steel wire is less, the brittleness of the steel wire is reduced, as thus the ductility performance particular the torsion ductility performance of the steel wire is improved. The steel filament after wet drawing has a final diameter d of 0.10 to 0.55 mm.
[0050] According to the invention, the method for making the mega tensile steel wire with improved ductility performance comprises two key steps: firstly, lowering the phase transformation temperature to be less than 600°C to have finer pearlite structure, the finer pearlite structure gives the steel wire a higher tensile after heat treatment;secondly, reducing the WWD area reduction rate, particular the area reduction rate of each of last six drawing passes is reduced to be 2.5%- 7%, and the total area reduction rate of WWD is slightly reduced to be 97.0%-98.2%.
[0051] Area reduction rate is calculated: (A1 -A2) / A1 , A1 is the area of the steel wire before one drawing pass, A2 is the area of the steel wire after that12 MIE25B0004PCT Classification: Confidential Informationdrawing pass, area is the cross section area of the steel wire nr2, r is the semidiameter of the steel wire. One drawing pass refers to a drawing step carried out between two capstans, using one or two or more drawing dies.
[0052] The steel wire can be used solely in rubber articles, such as monofilament for belt layer of tire, bead wire for tire, alternatively, the steel wire can be used to be twisted with one or more steel wires to make a steel cord for reinforcing rubber articles. Figure 1 illustrates cross sectional view of exemplary construction of 1x2 steel cord.
[0053] Compared to before twisting, the torsion ductility performance of the steel wire after twisting are slightly reduced, due to the twisting operation on the steel wire. The reduction rate is smaller than 10%, calculated by (torsion value before twisting - torsion value after twisting) / torsion value before twisting, for both 100D torsion value and delamination torsion value. For the steel wire unravelled out of the steel cord, it has a ductility torsion value, measured by a 100D torsion test method, of more than 24 turns, preferably of more than 27 turns, or more preferably in a range of 30-72 turns. And for the steel wire unravelled out of the steel cord, it has a delamination torsion value, measured by a delamination torsion test method on the steel wire unravelled out of the steel cord, of more than 145 turns, or in a range of 150-450 turns.
[0054] The steel cord can be made by any of existing methods, either by the cabling machine or by the bunching machine, preferably by the bunching machine to have a higher production efficiency.
[0055] The difference between the steel cord made by the cabling machine and the steel cord made by bunching machine is: the steel wire of the steel cord made by cabling machine rotates around the axis of the steel cord, while the steel wire of the steel cord made by bunching machine rotates around the axis of the steel cord and as well as the axis of its own. Such difference can be characterized by the surface twisting angle of the drawing lines of the steel wire, and the drawing lines of the steel wire are in the form of thin grooves on the surface of the steel substrate of the steel wire, which are caused by the wet wire drawing operation.13 MIE25B0004PCT Classification: Confidential Information
[0056] For the steel cord made by cabling machine, when the steel wire was unravelled out of the steel cord, it was measured with a surface twisting angle of no more than 0.5 degree, even zero degree. Figures 2a and 2b are the illustration of surface drawing lines of the steel wire from cabled cord. They show the surface drawing lines are substantially parallel with the axis of the steel wire.
[0057] For the steel cord made by bunching machine, when the steel wire was unravelled out of the steel cord, it was measured with a surface twisting angle of more than 1.5 degree, even in the range of 2-5 degree. Figures 3a and 3b are the illustration of surface drawing lines of the steel wire from bunched cord, having the same steel cord construction as the cabled cord comprising the steel wire shown in Figures 2a and 2b. They show the surface drawing lines are inclined to the axis of the steel wire. The above is only available to the steel wire with a twist pitch of 4-40mm due to the steel wire itself being twisted. For the steel wire has no twist pitch or has an infinite twist pitch, since the steel wire itself is not twisted, such steel wire is not the case; for example, the 2 core steel wires for the steel cord having a construction of 2+2, or the 1 core steel wire for the steel cord having a construction of 1 +6.
[0058] The measurement of surface twisting angle of the steel wire is:1 ) Prepare a specimen of steel wire, that is unravelled out from a steel cord and then straightened, with a length approximately 50 mm; 2) Take the photo of the specimen by Scanning-Electro-Microscope with 500x magnification ratio, and then analyse the photo of the specimen to measure the surface twisting angle of the drawing lines relative to the axial direction of said steel wire, the maximum of the surface twisting angle of the drawing lines of the steel wire in the photo is the surface twisting angle of the steel wire.
[0059] The unravelling operation of the steel wire is to take the steel wire out of the steel cord without causing any damage to the steel wire, neither to its shape nor to its mechanical properties, and nor removing or adding twists to the steel wire. The unravelling operation of the steel wire is done manually.14 MIE25B0004PCT Classification: Confidential Information
[0060] The invention is appliable to any of the known steel cords in the field. The steel cord can be made by any of known methods. In the steel cord field, the steel cord is classified to be:1 ) Multi-strands steel cord with a construction of nxm, n being the number of the strand and being at least two, m being the number of the steel wire of each strand and being at least two, examples are 3x3, 3x4, 7x7;2) Single strand steel cord with a construction of 1xn, such steel cord has at least two steel wires which have been twisted together, examples are 1x2, 1x3, 1x4, 1x5, 1x6, 1x7, 1x8;3) Steel cord with a construction of n+m, such steel cord comprising two groups of steel wires. The two groups are twisted around each other and form helicoids of a same pitch, the first group has n steel wires, n being at least two, the n steel wires being substantially untwisted and parallel to each other; the second group has m steel wires, m being at least one, examples are 2+2, 2+3, 3+2, 3+3, 4+3, 4+6;4) Layered constructions l+m(+n), such steel cord comprises a core having I steel wires, a first layer having m steel wires, and possibly a second layer having n steel wires. The whole may or may not be surrounded with a wrapping wire, examples are 1+3, 1+4, 1+5, 1+6, 2+5, 2+5cc, 2+6, 2+7, 2+7cc, 2+8, 3+6, 3+8, 3+8cc, 3+9, 3+9cc 1+3+8, 1+4+8cc, 1+4+9, 1+5+10, 1+5+10cc, 1+6+11, 1+6+12, 1 +6+12cc, 2+5+10, 2+6+12, 3+8+13, 3+9+15 or 4+10+16.15 MIE25B0004PCT Classification: Confidential Information
Claims
Claims1. A steel wire for rubber reinforcement, said steel wire comprising a steel substrate and a metallic coating covering on said steel substrate, said steel wire having a tensile strength in a range of 4600-2000xd - 5000-2000xd MPa, d being the steel wire diameter expressed in mm and in a range of 0.15-0.55 mm, the steel wire has a carbon content of 0.86%-0.95% in weight percentage, characterized in that the steel wire has a ductility torsion value, measured by a 100D torsion test method, being more than 30 turns.
2. A steel wire as claimed in claim 1 , characterized in that the carbon content of the steel wire is in a range of 0.88%-0.94% in weight percentage.
3. A steel wire as claimed in claim 1 , characterized in that the steel wire diameter is in a range of 0.16-0.40 mm, or in a range of 0.16-0.30mm.
4. A steel wire as claimed in claim 1 , characterized in that the ductility torsion value of the steel wire is more than 35 turns, or in a range of 40-80 turns.
5. A steel wire as claimed in claim 1 , characterized in that said steel wire has a delamination torsion value, measured by a delamination torsion test method, being more than 160 turns.
6. A steel wire as claimed in claim 5, characterized in that the delamination torsion value of the steel wire is more than 170 turns, or in a range of 170-500 turns.
7. A steel wire as claimed in any one of claims 1 to 6, characterized in that said metallic coating of said steel wire is zinc coating, brass coating, bronze coating, ternary or quaternary coating comprising three or four metals selected from the group consisting of copper, zinc, cobalt, nickel, tin, indium, manganese, iron, bismuth and molybdenum.
8. A method for making the steel wire as claimed in any one of claims 1 -7, characterized in that comprising the steps of:1) providing an intermediate wire with an intermediate diameter ranging from 1.0 mm to 2.5 mm, said intermediate wire comprises a steel substrate,2) subjecting the intermediate wire to a heat treatment, the heat treatment comprising firstly heating the intermediate wire at a temperature of 900-1000°C and thereafter cooling the intermediate wire at a temperature of 550-590°C,16 MIE25B0004PCT Classification: Confidential Information3) subjecting the intermediate wire to a coating process to apply a metallic coating covering on said steel substrate,4) subjecting the intermediate wire to a wet wire drawing operation thereby obtaining a steel wire, the wet wire drawing operation comprises a series of drawing passes for area reducion, the total area reduction rate of wet wire drawing operation is 97.0% - 98.2% and the area reduction rate of each of last 6 drawing passes is 2.5% - 7%.
9. A method for making the steel wire as claimed in claim 8, characterized in that the intermediate wire, after heat treatment in step 2), has a pearlite structure with an average lamellar spacing of the pearlite of no more than 60 nm.
10. A steel cord for rubber reinforcement, said steel cord comprising two or more steel wires as claimed in any one of claims 1-7, said steel cord having a cord twist pitch of 4 mm to 40 mm, characterized in that at least one of said two or more steel wires has a ductility torsion value, measured by a 100D torsion test method on the steel wire unravelled out of the steel cord, of more than 24 turns.11.A steel cord as claimed in claim 10, characterized in that at least one of said two or more steel wire has a ductility torsion value, measured by a 100D torsion test method on the steel wire unravelled out of the steel cord, of more than 27 turns, or in a range of 30-72 turns.
12. A steel cord as claimed in claim 10 or 11 , characterized in that at least one of said two or more steel wire has a delamination torsion value, measured by a delamination torsion test method on the steel wire unravelled out of the steel cord, of more than 145 turns, or in a range of 150-450 turns.
13. A steel cord as claimed in any one of claims 10-12, characterized in that at least one of said two or more steel wires is measured with a surface twisting angle in a range of 1.5-5 degree when it is unravelled out of the steel cord.
14. A steel cord as claimed in any one of claims 10-13, characterized in that said steel cord has a construction of 1x2, 1x3, 1x4, 1x5, 1+4, 1+5, 1+6, 2+2, 2+3, 3+2, 3+3, 3+4, 2x2, 2x3, 3x2, 3x3.17 MIE25B0004PCT Classification: Confidential Information