Optical component and method for manufacturing thereof

By laminating a sheet with defined surface roughness onto a mold and curing optical material, the method addresses 3D printing limitations, producing high-quality optical components with integrated coatings.

WO2026238602A1PCT designated stage Publication Date: 2026-11-19NERSESYAN VARSENIK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063528
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-10
Filing Date
2026-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing 3D printing methods for optical lenses result in microscopic surface roughness and lack of thermal and humidity stability, compromising optical quality and requiring additional processing steps and materials.

Method used

A method involving laminating a sheet or film with defined surface roughness onto a mold, casting a curable optical material, and curing it to form an optical component, where the sheet defines the surface quality and can integrate functional coatings, independent of mold quality.

Benefits of technology

The method produces optical-grade surfaces with improved surface quality and integrated coatings, independent of mold quality, enabling efficient, cost-effective, and high-performance optical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063528_19112026_PF_FP_ABST
    Figure EP2026063528_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing an optical component (1). The method comprises the step of providing (11) at least one mold (3). The method further comprises the step of laminating (12) onto said mold (3) a sheet (4), preferably a film. The method further comprises the step of casting (13) a curable material (5) onto the laminated sheet (4). The method further comprises the step of curing (14) said curable material (5) to form a body of said optical component (1). The method further comprises the step of separating (15) the body of said optical component (1) from the mold (3). A surface roughness of the sheet (4) is equal to or lower than a surface roughness of the mold (3).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Optical component and method for manufacturing thereof

[0002] Technical background

[0003] The present invention relates to a method and a system for manufacturing an optical component, and to an optical component.

[0004] Background

[0005] Lenses are commonly manufactured from transparent optical materials in order to provide one or more optically functional surfaces. The optical quality and form accuracy of these surfaces are key factors influencing the performance of the lens.

[0006] 3D printing of optical lenses has gained significant interest due to its potential for streamlining production and enabling customized geometries. However, direct 3D printing of lenses has limitations which may prevent its widespread adoption in high-quality optical applications. In particular, 3D-printed lenses often have a microscopic surface roughness, typically in a range of 1 to 10 micrometres depending on the 3D printing technology used, which may compromise optical quality. Post-treatment methods such as spin-coating of resin layers have been proposed, but such methods may add steps, complexity, and cost.

[0007] Additionally, materials used in direct 3D printing may lack the thermal, ultraviolet, and humidity stability required for long-term optical performance, which may result in defects such as yellowing, haze, or mechanical degradation. Even advanced 3D-printing systems, such as continuous liquid interface production or resin-based photopolymer printers, may not produce optically smooth surfaces without additional processing.

[0008] Because of these problems, there remains a need for improved optical components and cost-effective methods and devices for the manufacturing thereof.

[0009] Summary

[0010] The invention relates to a method for manufacturing an optical component, wherein a sheet or film is laminated onto a mold and a curable optical material is cast and cured against the film. The film defines the surface roughness and geometry of the optical surface and may remain attached to the optical component after demolding. This enables the production of optical-grade surfaces independent of mold quality and allows functional coatings, such as anti-reflective or hardcoat layers, to be integrated during the molding process. It is an object of embodiments of the present invention to provide a method and a device for manufacturing an optical component. This invention offers a new approach for manufacturing an optical component, wherein said approach provides advantages over the known approaches.

[0011] In a first aspect, the invention relates to a method for manufacturing an optical component, the method comprising the steps of:providing at least one mold;

[0012] laminating onto said mold a sheet, said sheet is preferably a film, for example the sheet or film having an optical-grade surface roughness, for example the sheet forms a surface having an optical-grade surface roughness, for example wherein said film comprises at least one layer;

[0013] casting a curable material onto the laminated sheet;

[0014] curing said curable material to form a body of said optical component; and

[0015] separating the body of said optical component from the mold;

[0016] o wherein a surface roughness of the sheet is equal to or lower than a surface roughness of the mold,

[0017] and / or

[0018] o wherein said sheet forms an optical surface of the optical component, wherein a geometry and surface roughness of the surface is defined, at least partially, by said sheet, and wherein the optical component is suitable for optical use.

[0019] It is an advantage that a geometry of said at least one optical surface of the optical component is defined by the mold, while the sheet (e.g. film, for example optical film) interposed between the mold and the curable optical material provides an interface the surface quality of which is substantially independent of the microscopic surface roughness of the mold. In other words, the surface roughness of the sheet is lower (i.e. better) than the surface roughness of the mold. It is a further advantage that the sheet improves a surface quality of the optical component, by compensating irregularities or a microscopic surface roughness of the mold. It is a further advantage that the surface quality of the optical component is substantially independent of the surface quality of the mold, since the curable optical material is cast onto the sheet rather than directly onto the mold. It is a further advantage that the method is compatible with various types of molds, including molds manufactured by different techniques, since the sheet may accommodate the surface characteristics of the mold. It is a further advantage that the method is efficient, since the geometry of the optical surface and an interface between the mold and the curable optical material are provided in a single lamination step. This allows an efficient, fast, and cost-effective method. It is a further advantage that the curable optical material may be selected independently of any constraints imposed by the manufacturing of the mold, such that high-performance optical material may be used for forming the body of the optical component.

[0020] Preferred embodiments of the first aspect of the invention comprise one or a suitable combination of more than one of the following features.

[0021] Preferably, after the step of separating, the sheet remains attached to a surface of the said optical component.

[0022] It is an advantage that the sheet becomes an integral part of the optical component, such that the sheet may provide one or more functional properties to the optical component, such as an optical property, for example an anti-reflective property or a photochromic property, or a mechanical property, for example a scratch resistance,without requiring additional post-processing steps such as the deposition of coatings after the optical component has been formed. It is a further advantage that the sheet defines an outer surface of the optical component, thereby providing a high-quality outer surface that is substantially independent of the surface quality of the mold and that may comprise one or more integrated functional layers.

[0023] Preferably, the method further comprises the step of 3D-printing said mold.

[0024] It is an advantage that 3D-printing enables the manufacturing of molds with customized geometries in a flexible and efficient manner, and may be suitable for low-volume or personalized production of optical components. At the same time, microscopic surface irregularities typically associated with 3D-printed molds may be compensated by the sheet (e.g. film), such that the surface quality of the optical component may be substantially independent of the surface quality of the 3D-printed mold. A preferred embodiment would use volumetric 3D prints to create the mold. For example, volumetric 3d printing machines are Xolo's Xolography 3D print, Readily3D, Manifest 3D tech, lOT's Lightform tech, etc.

[0025] Preferably, said sheet further comprises at least one of the following layers: a hardcoat, an anti-reflective coating, photochromic coating, an anti-smudge coating, a decorative coating, or polarizing characteristics. The layers may cover at least part of the sheet.

[0026] It is an advantage that an anti-reflective coating may be applied to the film and transferred to the optical component as part of the lamination and separation steps, such that the optical component may exhibit reduced reflections without requiring a separate coating step after the optical component has been formed. In other words, this allows efficient transfer of the coating to the optical component as an integrated part of the lamination and separations steps. In other words, the coating is applied to the film in advance, such that it is integrated into the film, and then used in the lamination and separation steps. For example, the film can be off-the-shelf and has already the an AR coating on it. It is a further advantage that the anti-reflective coating may be applied as part of a single film lamination step, thereby simplifying the manufacturing process by avoiding different lamination steps.

[0027] It is an advantage that one or more additional functional coatings may be integrated into the film, such as a hardcoat for improved scratch resistance, or a photochromic coating for enabling the optical component to reversibly darken in response to light. It is further an advantage that said additional functional coatings may be transferred to the optical component as part of the lamination and separation steps, thereby avoiding separate coating steps.

[0028] Preferably, said sheet comprises at least one adhesive layer facing (e.g. and in contact with) the mold, wherein said at least one adhesive layer is at least one of: a pressure-sensitive adhesive layer, a heat-sensitive adhesive layer, and an ultraviolet-curable adhesive layer.It is an advantage that the adhesive layer enables the film to conform to the mold during the step of laminating, such that microscopic irregularities of the mold may be compensated by the adhesive layer. It is a further advantage that different types of adhesive layers may be selected according to the specific application or process conditions, such as a pressure-sensitive adhesive for application without external heating or irradiation, a heatsensitive adhesive for activation by temperature, or an ultraviolet-curable adhesive for activation by ultraviolet light.

[0029] Preferably, said at least one adhesive layer comprises:

[0030] a first adhesive layer facing (e.g. and in contact with) the mold, and

[0031] a second adhesive layer facing (e.g. and in contact with) the cured material,

[0032] wherein said step of separating occurs between said first adhesive layer and said second adhesive layer.

[0033] It is an advantage that two adhesive layers may be used to define two distinct interfaces: a first interface between the film and the mold, and a second interface between the film and the cured optical material. It is a further advantage that, during the step of separating, the film may split between said first adhesive layer and said second adhesive layer, such that a first portion of the film may remain on the mold and a second portion of the film may remain attached to the optical component. It is a further advantage that this arrangement provides flexibility in the design of the film, and enables the use of pre-existing multilayer film configurations. It is a further advantage that the split between the first adhesive layer and the second adhesive layer during the step of separating enables the selection of which layers of the film remain on the mold and which layers remain attached to the optical component. For example, an anti-reflective coating comprised in the film may be configured to remain attached to the optical component, thereby being transferred to the optical component in a single lamination step. As such the adhesive layers are preferably different, to allow differential adhesion (i.e. stronger adhesion to a certain layer and weaker adhesion to another layer), as discussed below.

[0034] Preferably, said separation between the sheet and the mold is performed by a differential adhesion, wherein said differential adhesion between the sheet and the mold is weaker than an adhesion between the sheet and the cured optical material.

[0035] Preferably, the differential adhesion is provided by an adhesion gradient across the sheet-mold-cured material interface. The adhesion between the sheet and the mold is sufficiently high to hold the sheet in a desired position during filling and / or curing, but sufficiently low to allow release during demolding. The adhesion between the sheet and the cured optical material is higher than the adhesion between the sheet and the mold, such that separation occurs at the sheet-mold interface rather than at the sheet-cured material interface.

[0036] Preferably, the adhesion between the sheet and the cured optical material is at least 2 times, preferably 5 times, more preferably 10 times greater than the adhesion between the sheet and the mold.

[0037] In an embodiment, a sheet comprising a triacetyl cellulose (TAC) film having an anti-reflection (AR) coating on a mold-facing surface is temporarily fixed to a mold using a differential pressure-sensitive adhesive. The adhesive is configured such that a first adhesion between the adhesive and the AR-coated surface is lower than a second adhesion between the adhesive and the mold. Suitable adhesives include differential double-sided or transfertapes, for example tesa 62565, Nitto 61390, or 3M 9425, wherein a low-adhesion side is arranged against the AR coating and a high-adhesion side is arranged against the mold.

[0038] Preferably, the adhesion between the adhesive and the AR-coated TAC surface is in the range of 0.01 to 1.0 N / 25 mm, while the adhesion between the adhesive and the mold is 0.5 to 10 N / 25 mm, and the adhesion between the TAC sheet and a subsequently cured optical material, such as a 3D-printed acrylic, is 1 to 20 N / 25 mm, measured under identical peel conditions. The adhesion between the TAC sheet and the cured optical material is thus greater than the adhesion between the TAC sheet and the adhesive, such that upon demolding the sheet separates from the adhesive and remains attached to the cured optical component.

[0039] It is an advantage that the differential adhesion enables a clean separation of the film from the mold, while the film remains attached to the optical component after the step of separating. It is a further advantage that the differential adhesion may be achieved by appropriate selection of materials of the film, and optionally by a surface treatment of the mold.

[0040] Preferably, the method comprises the step of preforming the sheet (e.g. film) prior to the step of laminating, preferably by thermoforming.

[0041] It is an advantage that preforming the film allows the film to better match the geometry of the mold during the step of laminating, which may be particularly advantageous for molds having a high curvature. It is a further advantage that thermoforming may enable preforming of the film without compromising its optical or mechanical properties.

[0042] Preferably, the method further comprises the step of providing two molds, wherein said molds define two, preferably opposite, optical surfaces of said optical component.

[0043] It is an advantage that two molds may be used to define two, preferably opposite, optical surfaces of the optical component, such that both optical surfaces may be shaped at once, and optionally provided with a respective sheet. It is a further advantage that this arrangement enables the manufacturing of optical components in which both optical surfaces are independently customized, for example, for the manufacturing of progressive lenses, which may benefit from independent shaping of the front and back optical surfaces..

[0044] Preferably, the method further comprises the step of providing a preformed optical substrate, wherein said preformed optical substrate has an optical surface, wherein the step of curing is performed while the preformed optical substrate is in contact with the curable material, such that said mold defines a first optical surface of said optical component and said preformed optical substrate defines a second optical surface of said optical component, wherein said second optical surface is preferably opposite to said first optical surface.

[0045] It is an advantage that only one of the optical surfaces is shaped by a mold, such that the volume of curable optical material required is reduced. As a consequence, the curing time may be reduced, and the exothermicheat generated during the step of curing may be reduced, which may reduce the risk of thermal damage and defects in the optical component.

[0046] It is a further advantage that the preformed optical substrate may already comprise one or more functional features. For example, the substrate may include pre-integrated waveguides for augmented reality (AR) applications, electrochromic layers, coatings, or embedded components.

[0047] The subsequent casting or additive manufacturing step may then provide at least part of the optical prescription (e.g., refractive power or freeform correction) without exposing the pre-integrated functional features to the full thermal and volumetric stresses associated with bulk curing of the entire optical element.

[0048] Preferably, said preformed optical substrate comprises at least one functional feature, preferably wherein said preformed optical substrate comprises at least one of: a pre-applied coating, an embedded component, an electrochromic layer, and a waveguide.

[0049] Preferably, the optical component is a lens or other optical elements or optical stacks.

[0050] It is an advantage that the method is suitable for the manufacturing of lenses, such as ophthalmic lenses, including customized ophthalmic lenses which may be manufactured on demand in an easy and quick manner.

[0051] In a second aspect, the invention relates to an optical component, for example obtainable by the method of the first aspect, wherein said optical component comprises:

[0052] a body of cured material,

[0053] a sheet, preferably a film, laminated to the body at an external surface of the optical component, wherein

[0054] the sheet forms an optical surface of the optical component, and

[0055] the geometry and surface roughness of said optical surface being defined by the sheet and being suitable for optical use.

[0056] It is an advantage that the optical component manufactured according to the method of the first aspect exhibits improved characteristics, such as a high surface quality and optionally integrated functional coatings, without requiring post-processing steps after separation from the mold.

[0057] Preferably, the optical component comprises a functional layer, preferably embedded in said body, wherein the functional layer is configured for at least one of: an electrical, a mechanical, and an optical interfacing, preferably at one or more edges of the body.

[0058] It is an advantage that the optical component may be provided with additional functionalities such as variable transmission, light guiding, beam shaping, or user monitoring, by means of a functional layer embedded in thebody, while maintaining the optical quality of the surfaces defined by the sheet. It is a further advantage that the functional layer may be configured for electrical, mechanical, and / or optical interfacing at one or more edges of the body, thereby enabling external connection without compromising the optical surfaces. This makes the optical component particularly suitable for wearable optical devices such as smart glasses, augmented-reality, virtual-reality, or mixed-reality devices, and head-mounted displays.

[0059] Preferably, the sheet comprises a support layer, and preferably one or more further layers, more preferably wherein the sheet comprises at least one of the following layers: anti-reflective coating and a hardcoat.

[0060] Preferably, the support layer is a rigid support layer made of at least one of polycarbonate, triacetyl cellulose (TAC), and cyclic olefin polymer (COP).

[0061] Preferably, the thickness of the support layer is from 20 to 200 micrometres, preferably 40 to 100 micrometers, more preferably 50 to 80 micrometers, most preferably 60 to 75 micrometers.

[0062] Preferably, the optical component comprises two opposite optical surfaces, and wherein each of said optical surfaces is formed by a respective sheet laminated to the body of cured material.

[0063] Preferably, the optical component further comprises a preformed optical substrate, wherein said preformed optical substrate is attached to the optical component, wherein said preformed optical substrate is preferably attached on a side of the optical component opposite to the side at which the sheet is laminated. For example, the optical component comprises, in order across its thickness: the sheet at a first external surface, the body of cured material in the middle, and the preformed optical substrate at a second external surface opposite to the first external surface. This configuration may be obtained, for example, by the method of the first aspect, wherein the mold defines the first optical surface (carrying the sheet) and the preformed optical substrate defines the second optical surface, as illustrated for example in Figure 1 (d). It is an advantage that, when the preformed optical substrate is positioned on the opposite side (see Fig. 1 (d)), the optical component may have two independently customized optical surfaces, suitable for example for progressive ophthalmic lenses or for AR / VR optical components having a corrective surface on one side and an integrated functional feature (e.g., a waveguide) on the other, or other suitable configurations.

[0064] In a third aspect, the invention relates to a device for manufacturing an optical component, wherein said device is configured to perform the method of the first aspect, the device comprising:

[0065] a module configured to provide at least one mold;

[0066] optionally a module configured to clean the mold;

[0067] a lamination module configured to laminate a sheet onto the mold, preferably by vacuum lamination and / or thermo-compression;

[0068] a dispensing module configured to cast a curable material onto the laminated sheet;a curing module configured to cure the curable material; and

[0069] a separation module configured to separate the cured material from the mold.

[0070] It is an advantage that the device integrates the different modules required to perform the method of the first aspect, such that the method may be performed in an automated and efficient manner. It is a further advantage that the device may be compact and suitable for laboratory or in-office production of optical components, including customized optical components.

[0071] Preferably, the device further comprises a cuvette, wherein said cuvette is configured to serve as a molding chamber, a lamination platform, and a curing chamber.

[0072] It is an advantage that the cuvette integrates multiple functions into a single component, thereby simplifying the device and reducing the number of parts required to perform the method. It is a further advantage that the cuvette may provide a controlled environment for the steps of laminating, casting, and curing, and may enable curing through walls of the cuvette, for example when the walls are transparent to a curing wavelength.

[0073] In a fourth aspect, the invention relates to a use of a method according to the first aspect, or a device according to the third aspect, for manufacturing an optical grade component, for example a wearable optical component or a dental appliance, preferably for manufacturing an ophthalmic lens. In another aspect, the invention relates to the use of the optical component in wearable optical components, or dental appliance, or ophthalmic lenses, or contact lenses, or AR / VR / XR glasses, or smart glasses, or other applications requiring a smooth surface.

[0074] It is an advantage that the method and device may be used for a variety of applications involving optical components or appliances requiring a smooth surface and optionally integrated coatings.

[0075] Brief description of the figures

[0076] The disclosure will be further illustrated by means of the following description and the appended non-limiting drawings.

[0077] Figure 1 schematically illustrates cross-sectional views of optical component (1) and mold (3) arrangements, according to embodiments of the present invention.

[0078] Figure 2 schematically illustrates a flowchart of method steps for manufacturing an optical component (1), according to embodiments of the present invention.

[0079] Figure 3 schematically illustrates a cross-sectional view of the smoothing effect of the film (4) when laminated into the mold (3), according to embodiments of the present invention

[0080] Figure 4 schematically illustrates a cross-sectional view of different configurations of the film (4), according to embodiments of the present invention.

[0081] Figure 5 schematically illustrates a cross-sectional view of an embodiment of the method in which the optical component (1) is formed between two molds (3, 3'), according to embodiments of the present invention.Figure 6 schematically illustrates a cross-sectional view of an embodiment of the method in which a first optical surface of the optical component (1) is defined by a mold (3) and a second optical surface of the optical component (1) is defined by a preformed optical substrate, according to embodiments of the present invention. Figure 7 schematically illustrates a cross-sectional view of an embodiment of the method showing successive states of the film (4), the mold (3), and the optical component (1) during the steps of laminating, casting, curing, and separating, according to embodiments of the present invention.

[0082] Any reference signs in the claims shall not be construed as limiting the scope. In the different drawings, the same reference signs refer to the same or analogous elements. The drawings are schematic and not to scale.

[0083] Detailed description

[0084] The present invention relates to a method and a device for manufacturing an optical component.

[0085] The term "optical component" may denote any component comprising at least one optical surface, such as a lens, a window, a prism, a mirror, or any other component in which light is intended to be transmitted, reflected, or refracted. The optical component may be, for example, an ophthalmic lens, a contact lens, a dental appliance, or other kind of optical components, or a dental appliance such as a dental guard or a dental implant. This term is not limited to ophthalmic lenses. For example, optical stack suitable for use in AR / VR / XR devices, for example smart glasses and generally wearable device, might make use of such an optical component.

[0086] The term "optical surface" may denote a surface of the optical component through which light is intended to be transmitted, reflected, or refracted. The optical surface may be a front surface, a back surface, or any other surface of the optical component having an optical function.

[0087] The term 'film' may denote a single-layer or multilayer flexible structure, the at least one layer of which is selected to provide the film with one or more optical and / or mechanical functions. The film may be optical (i.e., providing an interaction with light, as defined herein, for example an optical film), or non-optical (e.g., a substantially transparent carrier film without specific optical function).

[0088] The term 'sheet' may denote any flat or substantially flat structure having a thickness that is small relative to its other dimensions, suitable for being laminated onto a mold and for forming an interface between the mold and the curable optical material. The sheet may be flexible or substantially rigid, single-layer or multilayer, and may be made of any suitable material providing the required mechanical and / or optical functions. Preferably, the sheet is a film, as defined herein, although the term 'sheet' is not so limited. In this description, the use of the word "film" in some parts may be generalized to the word "sheet".

[0089] The term 'mold' may denote any element having a surface that defines a geometry to be transferred to at least one optical surface of the optical component. The mold may be manufactured by any suitable technique, including, but not limited to, 3D printing. The mold may be a pre-fabricated element or may be fabricated as part of the method."

[0090] The term 'cuvette' may denote a container having one or more walls, configured to receive or contain elements used in the method, such as the mold, the film, and the curable optical material. The cuvette may serve as a molding chamber, a lamination platform, and a curing chamber. The cuvette may be made of a material that issubstantially transparent to a curing wavelength, such that the step of curing may be performed at least partially through the walls of the cuvette.

[0091] The term 'preformed optical substrate1may denote a substrate having at least one optical surface, provided prior to the step of casting the curable optical material. The preformed optical substrate may be made of any suitable optical material, including glass or a polymer, and may comprise one or more pre-applied coatings or functional elements, such as a waveguide for augmented-reality applications. It may also have a similar film attached thereto as the optical component.

[0092] The term 'optical', when used as a qualifier of any of the terms 'component', 'surface', 'film', 'material', 'function', or 'property', may denote an interaction with light, including transmission, reflection, refraction, diffraction, absorption, scattering, polarization, or modulation of light, or any combination thereof. Said light may be visible light, ultraviolet light, or infrared light, depending on the intended application of the optical component. The term 'optical' does not imply that transparency is required. For example, an optical component is a component that interacts with light, an optical surface is a surface through which light interacts, etc."

[0093] In a first aspect, the present invention relates to a method for manufacturing an optical component. For example, the optical component comprises at least one optical surface.

[0094] The method comprises the step of providing at least one mold. The mold has a surface that defines the geometry to be transferred to at least one optical surface of the optical component. The mold may be provided as a prefabricated element, or may be fabricated as part of the method itself, for example by (volumetric) 3D-printing. The mold may be made of any suitable material, including a polymer, a glass, a ceramic, or a metal. The material of the mold is preferably selected to be compatible with the curing technique used in the method. For example, when the step of photocuring is performed at least partially through the mold, the mold may be made of a material that is substantially transparent to the curing wavelength, such as a transparent polymer or a transparent glass. When the step of curing is performed by thermal curing, the mold may be made of any material that withstands the curing temperature, including a metal or a ceramic. The material of the mold is further preferably selected to withstand the steps of laminating and curing without substantial deformation or degradation.

[0095] The method further comprises the step of laminating onto said mold a sheet, the sheet is for example a film, wherein said sheet or film comprises at least one layer. For example, the film can be made of one layer, but in some cases it is advantageous to have multiple layers. The film is laminated onto the surface of the mold that defines said geometry. The film may comprise one layer or multiple layers, depending on the functions to be provided by the film. The film may comprise, for example, a support layer, for example a rigid support layer, one or more adhesive layers, and one or more coatings, as will be explained further below. The sheet for example has an optical grade surface roughness. This allows using the optical component for optical use.The film may be produced by any suitable method known in the art, such as extrusion, lamination, or coating processes. The film may optionally be treated, for example by plasma treatment, to enhance compatibility with applied layers. The thickness of the film is preferably selected to balance two competing considerations: a film that is too thick may impair curing efficiency of the curable optical material, while a film that is too thin may not provide sufficient mechanical stability or surface smoothness.

[0096] The method further comprises the step of casting a curable material onto the laminated film. The curable material is preferably a curable optical material, since the resulting cured material is used for optical purposes, as explained below. The curable optical material is a material intended to form a body of the optical component after curing. The curable optical material is preferably a resin, for example an optical liquid resin, which may be, for example, a photo-curable resin, a thermally curable resin, or a resin that is curable by a combination of photocuring and thermal curing. The material may be selected so as to provide the optical component with desired optical properties, such as a refractive index, a transmission, an Abbe number, and a glass transition temperature. For example, the material may be a liquid optical resin having a refractive index greater than 1.56, a transmission greater than 92%, for example between 80% and 100%, preferably between 85% and 98%, more preferably between 90% and 95%, an Abbe number greater than 30, and a glass transition temperature greater than 60 °C. The material may be applied under vacuum, so as to reduce the presence of air bubbles in the material.

[0097] The values disclosed herein represent typical parameters for optically clear lens materials as used in ophthalmic applications and are based on industry-standard material properties. The refractive index of the lens material may vary depending on the intended optical correction and material selection, and is preferably in the range of 1.50 to 1.76, such as about 1.56 for commonly used materials (e.g., MR-8 supplied by Mitsui Chemicals), or higher for high-index materials (e.g., MR-series materials up to about 1.76 supplied by Mitsui Chemicals). The optical transmission is, for example, between 80% and 100%, preferably between 85% and 98%, more preferably between 90% and 95%, such as about 92% or more than 92%. The thermal or processing temperatures are typically in the range of 30°C to 60°C, depending on the specific material system and curing conditions, such as to avoid deformation of the optical component due to thermal effects or the introduction of residual stresses."

[0098] An example of a suitable curable optical material is EPO-TEK 301, a low-viscosity optical-grade epoxy supplied by Epoxy Technology, which exhibits substantially no yellowing during and after curing.

[0099] The method further comprises the step of curing the curable optical material, so as to form a body of the optical component. The conditions of curing, including the dose and duration of a curing light or curing heat, may be adapted to the volume and geometry of the optical component, so as to provide a uniform curing and to reduce the occurrence of defects. For example, for optical components of a larger volume, an initial dose of light may be reduced so as to reduce an exothermic reaction during curing. The mold may be actively or passively cooled during the step of curing, for example by circulation of water, so as to provide a substantially uniform curing and to reduce thermal stress and provide thermal control. In case of photo curing, it is important that the cuvette is configured so that it allows the passage of the light for the curing.The method further comprises the step of separating the body of the optical component from the mold.

[0100] For example, the surface roughness of the sheet is equal to or lower than the surface roughness of the mold, so as to create an optical component having a surface roughness suitable for optical use.

[0101] For example, after the step of separating, the body of the optical component has at least one optical surface. For example, the sheet forms an optical surface of the optical component, wherein the geometry and surface roughness of the surface is defined, at least partially, by the sheet (which conforms defined by the mold). In other words, the surface is defined by the mold via said sheet. The optical component is thereafter suitable for optical use.

[0102] The optical surface preferably has an arithmetic average roughness Ra of 100 or 50 nm or less, preferably 20 nm or less, more preferably 10 nm or less, even more preferably 5 nm or less, measured by atomic force microscopy or optical profilometry over a defined scan area. For example, between 5 and 200 nanometers, preferably between 10 and 100 nanometers.

[0103] It is an advantage that the geometry of the at least one optical surface of the optical component is defined by the mold, while the film interposed between the mold and the curable optical material provides an interface the surface quality of which is independent of the microscopic surface roughness of the mold i.e. providing a substantially smoother surface than the mold itself. It is a further advantage that the film may improve the surface quality of the optical component, by compensating irregularities or a microscopic surface roughness of the mold. It is a further advantage that the method is compatible with various types of molds. It is a further advantage that the optical component may exhibit improved thermal and optical stability, since the body of the optical component is formed from a curable optical material that may be selected for its optical properties, and is not constrained by requirements imposed by e.g. 3D printing. It is a further advantage that the surface quality of the optical component is substantially independent of the surface quality of the mold, since the curable optical material is cast onto the film rather than directly onto the mold. It is a further advantage that the method is efficient, since the geometry of the optical surface and an interface between the mold and the curable optical material are provided in a single lamination step. This allows an efficient, fast, and cost-effective method. It is a further advantage that the curable optical material may be selected independently of any constraints imposed by the manufacturing of the mold, such that high-performance curable optical materials may be used for forming the body of the optical component.

[0104] Preferably, the method further comprises a cleaning step for the mold to remove residual material from a previous process cycle, such as cured or uncured optical material, for example an acrylic-based resin.

[0105] The cleaning may comprise a solvent rinse using a solvent capable of removing the optical material, such as isopropyl alcohol.

[0106] Additionally or alternatively, the cleaning may comprise spinning the mold, for example using a centrifuge or spin device, to remove remaining material by centrifugal force.

[0107] In some embodiments, the cleaning comprises a combination of solvent rinsing and spinning.Preferably, afterthe step of separating, the film remains attached to said at least one optical surface of the optical component. In other words, the film is transferred from the mold to the optical component during the step of separating, such that the film becomes an integral part of the optical component. For example, the adhesion to the mold is weaker than the adhesion to the cured optical material, as will be discussed below. As a result, the film may provide one or more functional properties to the optical component, such as an optical property, for example an anti-reflective property or a photochromic property, or a mechanical property, for example a scratch resistance, without requiring additional post-processing steps, such as the deposition of coatings afterthe optical component has been formed.

[0108] In embodiments, the outer surface of the optical component may be defined by the film, such that the surface quality, e.g. the outer surface quality, of the optical component is substantially independent of the surface quality of the mold. This allows providing a high-quality surface that is substantially independent of the surface quality of the mold and that may comprise one or more integrated functional layers. For example, the film may provide an outer surface of the optical component having a surface roughness that is lower than the surface roughness of the mold. For example, the method enables the production of optical components, such as lenses, with smooth optical surfaces and integrated coatings, without requiring polishing or post-processing. The film may furthermore act as a barrier against contaminants and mechanical damage to the optical component.

[0109] Preferably, the film further comprises at least one of the following: a hardcoat, an anti-reflective coating, a photochromic coating or a anti-smudge coating or a decorative coating, polarizing characteristics, or any other coating typically used in ophthalmic eyeglasses. These and other coatings, such as coatings providing additional optical properties, for example tinting, blue-light filtering, or polarization, may be integrated into to the film. The anti-reflective coating may be, for example, a single-layer or multilayer coating comprising materials having different refractive indices, and arranged so as to reduce reflections at a surface of the optical component, for one or more wavelengths or ranges of wavelengths. A hardcoat may provide increased scratch resistance to the optical component, while a photochromic coating may enable the optical component to reversibly darken in response to light, for example in response to ultraviolet light or to light (e.g. visible) of a specific wavelength range. These and other coatings may be applied to the film, and may be transferred to the optical component as part of the lamination and separation steps, thereby avoiding separate coating steps after manufacturing. Examples of suitable films comprising one or more coatings include the AR200-T081V-JD-HD multilayer film supplied by Dexerials, comprising an anti-reflective coating, a hardcoat, a triacetyl cellulose support layer, and a pressure-sensitive adhesive. Other examples include the Tech-Film AR Regular supplied by Satisloh.

[0110] Preferably, the film is configured to carry one or more functional coatings, including a hardcoat and / or anti-reflective (AR) coating, on at least one surface of said film.

[0111] It is an advantage that the anti-reflective coating is applied to the film and is transferred to the optical component as part of the lamination and separation steps. Accordingly, the optical component may exhibit reducedreflections without requiring a separate coating step after the optical component has been formed. In contrast to approaches in which an anti-reflective coating is applied to the optical component after manufacturing, this approach may enable the anti-reflective coating to be integrated in a single film lamination step.

[0112] Preferably, the film comprises a support layer, preferably rigid. The rigid support layer may be made of any material having a suitable rigidity and optical properties, for example a material that is substantially transparent to visible light. Preferably, the rigid support layer comprises at least one of: polycarbonate, triacetyl cellulose (TAC), and cyclic olefin polymer (COP). Such materials exhibit optical properties suitable for use in optical components, including high optical transmission, low birefringence or controlled birefringence, and a glass transition temperature that permits thermoforming. In addition, these materials are already established within the eyewear industry and its supply chain. The (e.g. rigid) support layer may have a thickness, for example, between 20 and 200 micrometres, preferably about 70 micrometres (e.g. in case of ophthalmic lenses), although other thicknesses are possible depending on the application.. For example, the support layer is provided first, and then the coatings are applied thereto.

[0113] The rigid support layer preferably comprises a thermoformable polymeric material having a glass transition temperature in the range of 140°C to 200°C, suitable for forming into a desired lens geometry while maintaining optical quality, such as, but not limited to, triacetyl cellulose (TAC) or comparable optically clear polymers.

[0114] The rigid support layer provides mechanical stability to the film during the steps of laminating, casting, and curing. Furthermore, the rigid support layer may bridge across microscopic irregularities of the mold, thereby presenting a substantially smooth outer surface towards the curable optical material. As a result, the curable optical material takes the shape of the substantially smooth outer surface of the rigid support layer, rather than the shape of any microscopic irregularities of the mold, which may improve the surface quality of the optical component. For example, the film applies as a Gaussian filter to the surface roughness of the said mold.

[0115] Preferably, the film comprises at least one adhesive layer. The adhesive layer enables the film to conform to the mold during the step of laminating. The adhesive layer may have a thickness of, for example, between 25 and 100 micrometres (e.g. in case of ophthalmic lenses), for example 50 micrometers, although other thicknesses are possible depending on the application. The at least one adhesive layer may be, for example, arranged on a face of the film facing the mold, or on a face of the film facing the cured optical material, or the film may comprise adhesive layers on both faces

[0116] The total thickness of the film stack as supplied is preferably between 100 and 200 micrometres. After removal of the protective liners and the buffer layer (see Fig. 7), the final film portion remaining attached to the optical component, comprising the rigid support layer and the one or more coatings, preferably has a total thickness of less than 50 micrometres.The at least one adhesive layer is at least one of: a pressure-sensitive adhesive layer, a heat-sensitive adhesive layer, and an ultraviolet-curable adhesive layer. A pressure-sensitive adhesive layer may be activated by the application of pressure, without requiring heating or irradiation. A heat-sensitive adhesive layer may be activated by the application of heat, such that the adhesive layer bonds to the mold upon reaching a predetermined temperature. An ultraviolet-curable adhesive layer may be activated by ultraviolet light, such that the adhesive layer bonds to the mold upon exposure to ultraviolet light of a predetermined wavelength range. The type of adhesive layer may be selected according to the specific application and process conditions. In embodiments, the adhesive layer may be an optically clear adhesive.

[0117] The adhesive layer may furthermore compensate microscopic irregularities of the mold, by filling and conforming to said microscopic irregularities during lamination, while the rigid support layer bridges across said microscopic irregularities. In this way, the combination of the adhesive layer and the rigid support layer may provide an outer surface of the film that is substantially smoother than the surface of the mold. The adhesive layer may be configured to compensate surface variations at a nanometric and microscopic scale, to eliminate air bubbles at interfaces, to substantially match a refractive index of adjacent layers, and to provide uniform bonding on curved or irregular surfaces.

[0118] In some embodiments, the adhesive layer facing the mold may be omitted, wherein the contact between the film and the mold may be maintained by the uncured curable optical material itself. For example, the curable material has adhesive properties.

[0119] In some embodiments, the film may further comprise, on a side of the film facing the curable optical material, a surface activation layer configured to strengthen a bond between the film and the cured optical resin. Said surface activation layer may be the same as, or distinct from, an adhesive layer, and may be, for example, a primer layer, a chemically-activated layer, or a plasma-treated surface.

[0120] The film may further comprise a cushion layer (also referred to as a buffer layer) . The cushion layer may serve to distribute pressure uniformly during the step of laminating, thereby improving the uniformity of contact between the film and the mold.

[0121] Preferably, the at least one adhesive layer comprises a first adhesive layer facing and in contact with the mold, and a second adhesive layer facing and in contact with the cured optical material. In this embodiment, the film comprises two distinct adhesive layers, providing two distinct interfaces: a first interface between the film and the mold, and a second interface between the film and the cured optical material.

[0122] The separation occurs between said first adhesive layer and said second adhesive layer. In other words, during the step of separating, the film splits somewhere between the first adhesive layer and the second adhesive layer, such that a first portion of the film remains on the mold, while a second portion of the film remains attached tothe optical component. The second portion of the film may, for example, include the rigid support layer and one or more optical coatings, such that these layers and coatings become part of the final optical component. It is an advantage that this arrangement provides flexibility in the design of the film. In particular, the film may be configured to split at a predetermined interface during the step of separating, and the layers remaining on the optical component may be selected accordingly. This arrangement also enables the use of pre-existing multilayer film configurations. For example, the first adhesive layer may remain on the mold after the step of separating, while the at least one coating (such as an anti-reflective coating), the rigid support layer, and the second adhesive layer may remain attached to the optical component.

[0123] Preferably, the separation between the film and the mold is performed by a differential adhesion, wherein the adhesion between the film and the mold is weaker than an adhesion between the film and the cured optical material. The differential adhesion may be achieved, for example, by an appropriate selection of materials of the film, by a surface treatment of the mold, by the use of a release agent on the mold, or by a combination of these.

[0124] The differential adhesion enables a clean separation of the film from the mold, while the film remains attached to the optical component after the step of separating. In this embodiment, substantially the entire film is transferred to the optical component, since the separation occurs at the interface between the film and the mold rather than within the film itself. Accordingly, the film may be configured to separate at different locations during the step of separating. In embodiments comprising two adhesive layers, as described above, the film may split between the two adhesive layers, such that a first portion of the film remains on the mold and a second portion of the film remains attached to the optical component. In embodiments comprising differential adhesion, the film may separate at the interface between the film and the mold, such that substantially the entire film is transferred to the optical component.

[0125] Preferably, the step of laminating comprises vacuum lamination. Vacuum lamination is a process in which the film is applied to the mold under reduced pressure, so as to enable a uniform contact between the film and the mold and to reduce the presence of air bubbles at the interface between the film and the mold.

[0126] Optionally, the step of laminating further comprises a step of thermo-compression and / or vacuum lamination. In a thermo-compression step, the film and the mold are subjected to an elevated temperature and an elevated pressure for a period of time, so as to further improve the uniformity of the contact and to reduce any residual air bubbles, which may otherwise result in optical defects. Air bubbles at the interface may otherwise cause deformations of the film and optical defects in the optical component, in particular due to the exothermic heat generated during the step of curing. In case both thermos-compression and vacuum lamination are used, the thermo-compression step may be performed after vacuum lamination.

[0127] Preferably, the method comprises the step of preforming the film prior to the step of laminating. Preforming refers to a process in which the film is shaped, prior to lamination, so as to substantially match the curvature ofthe mold. Preforming may be particularly advantageous for molds having a high curvature, which may be difficult to accommodate by the film during lamination without preforming. Preferably, preforming is performed by thermoforming. In thermoforming, the film is heated to a temperature at which the film becomes sufficiently pliable to be shaped, and is then shaped to a desired geometry, for example by the use of a preforming tool. Preforming by thermoforming enables the film to be shaped without substantially compromising its optical or mechanical properties.

[0128] Preferably, the step of curing comprises photo-curing and / or thermal curing the curable optical material. Photocuring refers to a process in which the curable optical material is cured by exposure to light, typically ultraviolet light, of a predetermined wavelength range. Thermal curing refers to a process in which the curable optical material is cured by the application of heat.

[0129] Photo-curing and thermal curing may be used independently or in combination. For example, to only thermally cure the curable optical material, or to only photo cure the curable optical material, or both. For example, the curable optical material may be initially photo-cured to form the body of the optical component, followed by a thermal post-cure to complete the curing. The step of photo-curing may be performed through the mold, through the curable optical material from a side opposite to the mold, or through both, depending on the configuration of the device and the transparency of the mold. For example, if the mold is substantially transparent to the curing wavelength, curing may be performed at least partially through the mold.

[0130] It is an advantage that the step of curing may be adapted to the type of curable optical material used. It is a further advantage that a combination of photo-curing and thermal curing may be used, such that the material e.g. resin may be cured in a controlled manner, for example by initial photo-curing followed by a thermal postcure.

[0131] In embodiments where the step of curing comprises photo-curing, the curable optical material is preferably exposed to radiation in the wavelength range of 365 to 405 nanometres, at an irradiance of 10 to 200 mW / cm2, for a duration of 10 seconds to 10 minutes. The step of curing may optionally comprise an initial partial cure to define the geometry of the optical component, followed by a full cure to achieve final optical and mechanical properties. The step of curing may further be performed under inert atmosphere or at elevated irradiance to reduce oxygen inhibition.

[0132] The curing conditions are preferably selected as a function of the thickness of the curable optical material, wherein increased thickness requires longer exposure times and / or reduced curing intensity to ensure controlled polymerization. In particular, the curing process is adapted to minimize thermal gradients, material expansion, and fluid flow during curing, thereby reducing the formation of internal stresses and optical distortions.

[0133] In some embodiments, the curable optical material is partially cured or gelled prior to full curing, such as to increase its viscosity and reduce fluid mobility, thereby limiting flow, deformation, or damage to the mold surfaces. Following this pre-curing step, a final curing stage is applied to achieve full polymerization and thedesired optical and mechanical properties. As a result, the material does not need to be fully cured in a single step, and the required curing dose, duration, and heat generation due to exothermic reactions can be reduced or more effectively controlled.

[0134] For example, a curable optical material layer having a thickness of about 3 mm may be introduced into the mold cavity. In this example, the curable optical material is first subjected to a pre-curing step using UV radiation at an irradiance of about 20 to 50 mW / cm2for 10 to 30 seconds to achieve partial gelation and increase viscosity. Subsequently, a final curing step is performed at an irradiance of about 50 to 150 mW / cm2for 60 to 300 seconds to complete polymerization.

[0135] For thinner layers, for example <1 mm, the curing may be performed in a single step at higher irradiance and shorter duration. For thicker layers, for example >4 to 5 mm, the curing is preferably performed in multiple stages with reduced irradiance and extended duration to limit thermal gradients, exothermic heat buildup, and fluid flow, thereby improving dimensional stability and optical quality of the resulting optical component.

[0136] Preferably, the method further comprises the step of providing two molds, wherein said molds define two, preferably opposite, optical surfaces of the optical component. In this embodiment, the optical component is formed between two molds, each defining one of the two opposite optical surfaces. Each mold may have a respective film laminated thereon, or, alternatively, only one of the two molds may have a film laminated thereon.

[0137] It is an advantage that two molds may be used to define two, preferably opposite, optical surfaces of the optical component, such that both optical surfaces may be shaped at once, and optionally provided with a respective film. It is a further advantage that this arrangement enables the manufacturing of optical components in which both optical surfaces are independently customized. This arrangement may be particularly advantageous, for example, for the manufacturing of progressive lenses, which may benefit from independent shaping of the front and back optical surfaces.

[0138] Preferably, the method further comprises the step of providing a preformed optical substrate, wherein the preformed optical substrate has an optical surface. The preformed optical substrate may be, for example, a halflens substrate, a preformed optical element, or an optical insert. For example, a preformed lens. The preformed optical substrate may be made of any suitable optical material, including glass or a polymer. The preformed optical substrate may comprise one or more pre-applied coatings or functional features.

[0139] The step of curing is performed while the preformed optical substrate is in contact with the curable optical material, such that the mold defines a first optical surface of the optical component and the preformed optical substrate defines a second optical surface of the optical component, preferably opposite, to the first optical surface. In this way, only one of the optical surfaces of the optical component is shaped by a mold, such that the volume of curable optical material required is reduced. As a consequence, the curing time may be reduced, andthe exothermic heat generated during the step of curing may be reduced, which may reduce the risk of thermal damage and defects in the optical component.

[0140] The preformed optical substrate may comprise one or more pre-applied coatings, embedded components, or functional elements. In particular, the preformed optical substrate may comprise a waveguide for augmented-reality applications, such that the optical component manufactured according to the method may be suitable for use in augmented-reality systems.

[0141] In embodiments, the preformed optical substrate is a semi-finished lens having a predetermined curvature, which defines a surface of the mold cavity and remains attached to the final optical component after curing, thereby forming, for example, the front surface of the optical component. The opposing surface of the optical component may be formed by a mold obtained by additive manufacturing, in particular by 3D-printing, or by machining or other suitable fabrication methods to define the complementary surface.

[0142] The semi-finished lens is preferably formed of an optically transparent polymeric material, such as an injection-molded substrate selected from polycarbonate (PC), polymethyl methacrylate (PMMA), cyclic olefin polymer (COP), cyclic olefin copolymer (COC), or polyurethane-based optical materials (e.g., CR-39 or high-index urethane resins), suitable for ophthalmic or optical applications.

[0143] In some embodiments, the surface of the semi-finished lens facing the curable optical material is configured to enable bonding with the curable optical material, optionally by surface treatment, primer application, or partial curing, such that a monolithic optical element is formed after curing. In alternative embodiments, selected mold surfaces may be provided with a release-promoting coating to facilitate separation where required.

[0144] Preferably, the method further comprises the step of 3D-printing the mold. 3D-printing enables the manufacturing of molds with customized geometries in a flexible and efficient manner, without requiring dedicated tooling for each mold geometry. 3D-printing may be particularly suitable for low-volume or personalized production of optical components, such as customized ophthalmic lenses. Techniques such as stereolithography (SLA) or digital light processing (DLP), or volumetric 3D printing, preferably volumetric 3D printing, may be used to 3D-print the mold with high precision. In preferred embodiments, volumetric 3D printing is used, such as volumetric 3D printing supplied under the brand names Xolography by Xolo, Readily3D, Manifest 3D, or Lightform by IOT. 3D-printed molds may exhibit a microscopic surface roughness, typically in the range of 1 to 10 micrometres. It is a particular advantage of the method of the invention that the film compensates for said microscopic surface roughness, such that the surface quality of the optical component may be substantially independent of the surface quality of the 3D-printed mold. Furthermore, the mold may be 3D-printed using resins that are substantially transparent to ultraviolet light, such that the step of curing may be performed at least partially through the mold.

[0145] Preferably, the method further comprises the step of 3D-printing the mold using a volumetric printing process. Volumetric printing refers to an additive manufacturing method in which the three-dimensional geometry isformed within a volume of photosensitive material by controlled energy deposition, enabling the entire structure to be generated in a substantially continuous manner rather than through sequential layering. This enables the manufacturing of molds with customized geometries in a flexible and efficient manner, without requiring dedicated tooling for each mold geometry, and is particularly suitable for low-volume or personalized production of optical components, such as customized ophthalmic lenses.

[0146] Volumetrically printed molds may exhibit a microscopic surface roughness, typically in the range of 1 to 10 micrometres. It is a particular advantage of the method of the invention that the film compensates for said microscopic surface roughness, such that the surface quality of the optical component may be substantially independent of the surface quality of the printed mold. Furthermore, the mold may be printed using materials that are substantially transparent to ultraviolet light, such that the step of curing may be performed at least partially through the mold.

[0147] After 3D-printing, the mold may be subjected to one or more post-processing steps, such as a washing step to remove residual material e.g. resin, a drying step such as a spin-drying step, and a secondary curing step, such as a secondary ultraviolet or thermal cure, to harden the surface of the mold and to maintain the dimensional integrity of the mold during subsequent steps.

[0148] It is a further advantage that the curable optical material (e.g. liquid optical resins) used for casting is not constrained by the requirements of 3D printing, such that high-performance optical materials optimized for optical clarity, refractive index, Abbe number, or environmental stability may be used, even if such resins are not compatible with 3D printing.

[0149] The material used for 3D-printing the mold is preferably selected so as to withstand the steps of laminating and curing without substantial deformation or degradation. The mold may be 3D-printed from commercially available curable resins, such as curable resins supplied under the brand name Anycubic, or photochromic photoinitiator resins supplied under the brand name Xolo3D. Other examples may be acrylate- or methacrylate-based UV-curable photopolymer resins, for example Formlabs Clear Resin V4 (an acrylate / methacrylate oligomer-and-monomer-based photopolymer with photoinitiators) or Anycubic High Clear Resin (a UV-curable acrylate-based photopolymer), or photochromic photoinitiator resins supplied under the brand name Xolo3D.

[0150] Preferably, the optical component is a lens or other optical elements. For example, an optical stack. The method is particularly well-suited to the manufacturing of lenses, such as ophthalmic lenses, which may be customized to the prescription of an individual user. More generally, the method may be applied to the manufacturing of optical elements with customized geometries in a flexible and efficient manner, without requiring dedicated tooling for each geometry, including, but not limited to, components used in imaging systems or wearable optical devices.In some embodiments, the film may comprise a complete stack of layers including a rigid support layer, one or more adhesive layers, one or more coatings such as a hardcoat or an anti-reflective coating, one or more protective liners, and a buffer layer. In such embodiments, the film may comprise, in order from a mold-facing side to an opposite side: a first protective liner, a first adhesive layer, one or more coatings such as a hardcoat and an anti-reflective coating, a rigid support layer, a buffer layer, a second adhesive layer, and a second protective liner. However, the specific configuration of the stack may vary according to the specific application and the construction of the film, and each of the features described below may be present or omitted independently.

[0151] Preferably, the film further comprises at least one protective liner arranged on a face of the film. More preferably, the film comprises a first protective liner on a mold-facing side of the film and a second protective liner on an opposite side of the film. The protective liner, or each of the protective liners, may be configured to be removed prior to the use of the respective face of the film. In such embodiments, the method may further comprise, prior to the step of laminating, the step of removing the first protective liner from the mold-facing side of the film, thereby exposing the first adhesive layer for contact with the mold.

[0152] Preferably, the film further comprises a buffer layer on a side of the film facing away from the mold. The buffer layer is configured to prevent a transfer of a pattern from a lamination apparatus to underlying layers of the film during the step of laminating. The buffer layer is preferably a temporary layer, removed from the film after the step of laminating and before the step of casting, such that the buffer layer does not form part of the final optical component. Accordingly, in such embodiments, the method further comprises, after the step of laminating and before the step of casting, the step of removing said buffer layer from the film.

[0153] Preferably, the first adhesive layer, facing the mold, is a differential adhesive layer configured such that an adhesion between said first adhesive layer and the mold is stronger than an adhesion between said first adhesive layer and an adjacent layer of the film, for example an adjacent coating. In such embodiments, during the step of separating the body of the optical component from the mold, the first adhesive layer preferably remains on the mold while the adjacent layer, and layers above the adjacent layer, remain attached to the optical component. Accordingly, in such embodiments, the step of separating the body of the optical component from the mold may further comprise removing the first adhesive layer together with the mold, such that the first adhesive layer does not form part of the final optical component.

[0154] Preferably, the second adhesive layer, disposed between the buffer layer and the second protective liner, is configured to have a strong adhesion such that, when the buffer layer is removed from the film after the step of laminating and before the step of casting, the second adhesive layer and the second protective liner are removed together with the buffer layer as a single unit, and such that the second adhesive layer does not separate from the buffer layer or the second protective liner.Preferably, after the step of separating, the optical component comprises the body of cured optical material, the rigid support layer, and the one or more coatings, wherein said rigid support layer and said one or more coatings remain attached to an optical surface of the optical component defined by the mold.

[0155] It is an advantage that such a film stack enables a clean and controlled separation of the film during the respective process steps, such that a first portion of the film comprising the buffer layer, the second adhesive layer and the second protective liner may be removed prior to casting, a second portion of the film comprising the first adhesive layer may remain on the mold and be removed together with the mold during the step of separating, and a third portion of the film, comprising the rigid support layer and the one or more coatings, may remain attached to the optical component. It is a further advantage that the pattern of the lamination apparatus is not transferred to the underlying layers of the film during the step of laminating, due to the presence of the buffer layer. It is a further advantage that the exact configuration of the film stack may be varied according to the specific application.

[0156] It is to be understood that the foregoing describes one specific embodiment of the method, in which the film comprises the full stack of layers as described above. The essential steps of the method are the steps of providing at least one mold, laminating the film onto said mold, casting the curable optical material onto the laminated film, curing the curable optical material, and separating the body of the optical component from the mold, as set out at the beginning of the description of the first aspect. The features described in this embodiment, including the protective liners, the buffer layer, the additional liner-removal and buffer-removal steps, and the specific configuration of the adhesive layers, may be present in any suitable combination, or omitted entirely, depending on the specific application and the construction of the film.

[0157] In a second aspect, the present invention relates to an optical component. This is for example obtainable by the method of the first aspect. But it could be generalized as in the following. The optical component comprises a body of cured material (e.g. cured optical material, e.g. cured optical resin). For example having at least one optical surface. Preferably, the optical component further comprises a sheet (e.g. film) attached to the optical surface, for example the film comprises at least one layer. The sheet is laminated to the body at an external surface of the optical component. The sheet then forms an optical surface of the optical component. The geometry and surface roughness of said optical surface being defined by the sheet. For example, the sheet conforms to the mold, so at least the geometry is defined by the sheet, but the surface roughness is improved because it is influenced by the sheet. Although the sheet here is part of the component because it can provide further functionalities (e.g. optical) to the optical component, the sheet is optional in the optical component as a final product. For example, the sheet is used for obtaining an improved surface roughness, and then removed

[0158] It is an advantage that the optical component manufactured according to the method of the first aspect exhibits improved characteristics, such as a high surface quality and optionally integrated functional coatings, without requiring post-processing steps after separation from the mold.Preferably, the body comprises a functional layer. For example, the functional layer is embedded in the body, but may additionally or alternatively be embedded in the sheet, or in the preformed optical substrate (e.g. preformed lens). The functional layer is exposed at one or more edges of the body for electrical, mechanical, or optical connection. In other words, the functional layer is configured for at least one of: an electrical, a mechanical, and an optical interfacing, preferably at one or more edges of the body.

[0159] In some embodiments, the body comprises a functional layer embedded within the cured material. The functional layer may comprise at least one of, by way of non-limiting examples, an electrochromic film, one or more optical waveguides, a holographic optical element, or a liquid crystal (LC) tunable lens. In further embodiments, the functional layer may include one or more functional components such as sensors, for example eye-tracking sensors, light sensors, or imaging sensors, which may be integrated in or on a film (e.g. the film discussed above) or glass component (e.g. the preformed lens discussed above). Such integration may be achieved using techniques commonly employed in wearable optical devices, including smart glasses or headmounted displays, where functional elements are incorporated within laminated optical stacks, on transparent substrates, or along edge regions to enable electrical, mechanical, and / or optical interfacing. These configurations allow the optical component to provide additional functionalities such as variable transmission, light guiding, beam shaping, or user monitoring while maintaining the optical quality of the surface defined by the sheet.

[0160] As mentioned above, the functional layer may be a waveguide, for example with a thickness between 50 to 500 nanometers. The waveguide may be made for example from glass or glass nano imprinted with polymer, or an airgap, or in any other way known in the art for creating such a structure.

[0161] In a third aspect, the present invention relates to a device for manufacturing an optical component, wherein the device is configured to perform the method of the first aspect. The device comprises a module configured to provide at least one mold. The module configured to provide at least one mold may, for example, comprise a 3D-printing module configured to 3D-print the mold, and / or may comprise a holder configured to receive a prefabricated mold.

[0162] The device further comprises a lamination module configured to laminate a film onto the mold. Preferably, the lamination module is configured to perform vacuum lamination and / or thermo-compression. The device further comprises a dispensing module configured to cast the curable optical material onto the laminated film. The dispensing module (e.g. resin dispensing module) may comprise, for example, a reservoir for the curable optical material, a dispenser, and optionally means for applying the curable optical material under vacuum to reduce the presence of air bubbles. The device further comprises a curing module configured to cure the curable optical material. The curing module may comprise a light source, such as an ultraviolet light source, and / or a heat source, such as a heater, depending on the type of curable optical material used. The curing module may furthercomprise means for actively or passively cooling the mold during curing, for example by circulation of water, so as to reduce thermal effects during curing.

[0163] The device further comprises a separation module configured to separate the cured optical component from the mold. The device may further comprise additional modules, such as a washing module for post-processing the mold, a drying module, a secondary curing module, and / or a finishing module for edging or milling the optical component. It is a further advantage that the method and device may reduce or eliminate the need for final edging, as the mold may define the final geometry of the optical component with high precision.

[0164] The device may further comprise a finishing module, such as an edging or milling module, for precise shaping of the optical component after curing, if further edge refinement is desired.

[0165] It is an advantage that the device integrates the different modules required to perform the method of the first aspect, such that the method may be performed in an automated and efficient manner. The device may be compact, autonomous, and suitable for laboratory or in-office production of optical components, including customized optical components, without requiring a cleanroom environment. The device may also enable fast and precise manufacturing of optical components.

[0166] Preferably, the device comprises a cleaning mechanism. For example, a cleaning module configured to clean the mold. For example, in case the mold was used previously, then it might have excessive resin, which might reduce the quality of the optical component. In such a case, the module is able to clean the mold, for example by spinning or centrifuging the mold or by mechanically scrubbing the mold, in order to remove any residual resin.

[0167] Preferably, the device further comprises a cuvette, wherein the cuvette is configured to serve as a molding chamber, a lamination platform, and a curing chamber. The cuvette may be made of a material that is substantially transparent to ultraviolet light, such as polycarbonate or cyclic olefin polymer, preferably chemically resistant and having low light absorption, such that the step of curing may be performed through the walls of the cuvette. In embodiments, the mold is 3D-printed within the cuvette, and the cuvette remains in place during the subsequent steps of laminating, casting, and curing. A light source for curing, such as a liquid crystal on silicon (LCOS) projector, may be located at a bottom of the cuvette, or at another location depending on the design of the device.

[0168] It is an advantage that the cuvette integrates multiple functions into a single component, thereby simplifying the device and reducing the number of parts. The cuvette may further provide a controlled environment for the steps of laminating, casting, and curing, and may enable curing through walls of the cuvette.

[0169] It is a further advantage that the method and device may reduce or eliminate the need for final edging, as the mold may define the final geometry of the optical component with high precision, including an edge profile that matches the shape of a frame into which the optical component is to be fitted. For example, the optical component may be 3D-printed directly in its final shape, thereby eliminating the need for edging steps. This mayrequire a high-resolution 3D-printing process producing smooth and precise surfaces, optimized design and orientation of the optical component to minimize post-processing, and the addition of an integrated edging or milling module to the device for precise shaping after printing or molding.

[0170] In a fourth aspect, the present invention relates to a use of a method according to the first aspect, or a device according to the third aspect, for manufacturing a wearable optical component or a dental appliance. Said wearable optical component may be, for example, an ophthalmic lens, a contact lens, a camera lens, an augmented-reality (AR) optical component, or a virtual-reality (VR) optical component, or mixed reality (XR) optical component. Therefore, this method is not limited to traditional ophthalmic applications, but also extends to optical components used in AR / VR / XR devices, for example smart glasses and generally wearable device. Said dental appliance may be, for example, a dental guard or a dental implant. The method and the device may be adapted to the specific requirements of each type of optical component or appliance, for example by selecting an appropriate curable optical material, an appropriate film, and appropriate process conditions.

[0171] Any feature of the second aspect (optical component), the third aspect (device), or the fourth aspect (use) may be as correspondingly described in the first aspect (method).

[0172] Further characteristics and advantages of embodiments of the present invention will be described with reference to the figures. It should be noted that the invention is not restricted to the specific embodiments shown in these figures or described in the examples, but is only limited by the claims.

[0173] Figure 1 schematically illustrates cross-sectional views of optical components (1) and mold arrangements according to embodiments of the present invention. Figure 1(a) shows an optical component (1) having an optical surface (2). Figure 1(b) shows a mold (3) having a surface defining the geometry to be transferred to the optical component (1). Figure 1(c) shows the mold (3) with the film (4) laminated thereon, and the curable optical material (5) cast onto the laminated film (4). Figure 1(d) shows an optical component (1) having two opposite optical surfaces (2, 21), according to embodiments in which the optical component (1) is formed between two molds or between a mold and a preformed optical substrate (2').

[0174] Figure 2 schematically illustrates a flowchart of a method of manufacturing an optical component (1) according to embodiments of the present invention. The method comprises the step of providing (11) at least one mold (3). The method further comprises the step of laminating (12) onto the mold (3) a film (4). The method further comprises the step of casting (13) a curable optical material (5) onto the laminated film (4). The method further comprises the step of curing (14) the curable optical material (5) to form a body of the optical component (1). The method further comprises the step of separating (15) the body of the optical component (1) from the mold (3).Figure 3 schematically illustrates a cross-sectional view of the smoothing effect of the film (4) when laminated onto the mold (3). Figure 3(a) shows the mold (3) alone, having a surface with microscopic irregularities, for example due to the mold (3) being 3D-printed. Figure 3(b) shows the film (4) being laminated onto the mold (3), wherein the film (4) conforms to the surface of the mold (3) on a side facing the mold (3), while presenting a substantially smooth outer surface on the other side. Figure 3(c) shows the mold (3) with the laminated film (4), wherein the laminated film (4) providing a substantially smooth outer surface onto which the curable optical material (5) may subsequently be cast.

[0175] Figure 4 schematically illustrates different configurations of the film (4) laminated on the mold (3). Figure 4(a) shows a configuration in which the film (4) comprises, from the mold (3) outwards, an adhesive layer (4b) facing and in contact with the mold (3), a rigid support layer (4a), and at least one coating (4c) on a side of the rigid support layer (4a) opposite to the adhesive layer (4b). Figure 4(b) shows a configuration in which the film (4) comprises, from the mold (3) outwards, at least one coating (4c) facing and in contact with the mold (3), a rigid support layer (4a), and an adhesive layer (4b) on a side of the rigid support layer (4a) opposite to the coating (4c). Figure 4(c) shows a configuration in which the film (4) comprises, from the mold (3) outwards, a first adhesive layer (4b1) facing and in contact with the mold (3), at least one coating (4c), a rigid support layer (4a), and a second adhesive layer (4b") on a side opposite to the first adhesive layer (4b1). In the configuration of Figure 4(c), during the step of separating, the film (4) may split between the first adhesive layer (4b1) and the second adhesive layer (4b"), such that a first portion of the film (4) remains on the mold (3) and a second portion of the film (4) remains attached to the optical component (1). For example, the first adhesive layer (4b1) may remain on the mold (3), while the at least one coating (4c), the rigid support layer (4a), and the second adhesive layer (4b") may remain attached to the optical component (1) after the step of separating. This may be particularly advantageous when the at least one coating (4c) is an anti-reflective coating, such that the anti-reflective coating is transferred to the optical component (1) after the step of separating.

[0176] Figure 5 schematically illustrates a cross-sectional view of an embodiment of the method in which the optical component (1) is formed between two molds (3, 31). Figure 5(a) shows an assembly comprising the mold (3) having the film (4) laminated thereon, a second mold (31) having a second film (41) laminated thereon, and the curable optical material (5) between the mold (3) and the second mold (31). The mold (3) and the second mold (31) may be brought towards each other, optionally under applied pressure, so as to shape the curable optical material (5) between said mold (3) and said second mold (31) during the step of curing. Figure 5(b) shows the optical component (1) obtained after the steps of curing and separating, wherein the optical component (1) comprises a body of cured optical material (5) having two opposite optical surfaces, each defined by a respective one of the mold (3) and the second mold (31), wherein the film (4) and the second film (41) remain attached to said two opposite optical surfaces.

[0177] Figure 6 schematically illustrates a cross-sectional view of an embodiment of the method in which a first optical surface of the optical component (1) is defined by the mold (3) and a second optical surface of the opticalcomponent (1) is defined by a preformed optical substrate (6). Figure 6(a) shows an assembly comprising the mold (3) having the film (4) laminated thereon, the curable optical material (5), and the preformed optical substrate (6) held by a chuck (7) above the mold (3). The preformed optical substrate (6) comprises a coating (6a) on a face of the preformed optical substrate (6) opposite to the curable optical material (5). Pressure may be applied on the chuck (7) so as to bring the preformed optical substrate (6), the curable optical material (5), and the film (4) on the mold (3) into contact with each other, such that said preformed optical substrate (6), said curable optical material (5), and said film (4) form a stack during the step of curing. Figure 6(b) shows the resulting optical component (1) obtained after the steps of curing and separating, the optical component (1) comprising a body of cured optical material (5) having two opposite optical surfaces, the film (4) remaining attached to the first optical surface defined by the mold (3), the preformed optical substrate (6) together with said coating (6a) remaining attached to the second optical surface of the optical component (1), said coating (6a) being arranged on an outer face of the optical component (1).

[0178] Figure 7 schematically illustrates a cross-sectional view of an embodiment of the method, showing successive states of the film (4) during the manufacturing process. Figure 7(a) shows the film (4) prior to use, the film (4) comprising, in order, a first protective liner (4e), a first adhesive layer (4b1), a hardcoat (4c1), an anti-reflective coating (4c"), a rigid support layer (4a), a buffer layer (4d), a second adhesive layer (4b"), and a second protective liner (4e). Figure 7(b) shows the film (4) after the first protective liner (4e) has been removed and the remaining stack has been laminated onto the mold (3). Figure 7(c) shows the film (4) after removal of the second protective liner (4e), the second adhesive layer (4b"), and the buffer layer (4d) as a unit, wherein the rigid support layer (4a) is exposed for the step of casting. Figure 7(d) shows an assembly comprising the curable optical material (5) cast onto the rigid support layer (4a), with the hardcoat (4c1), the anti-reflective coating (4c"), the first adhesive layer (4b1), and the mold (3) below. Figure 7(e) shows the optical component (1) obtained after the steps of curing and separating, wherein the mold (3) and the first adhesive layer (4b1) have been removed together, and wherein the optical component (1) comprises a body of cured optical material (5), the rigid support layer (4a), the anti-reflective coating (4c"), and the hardcoat (4c1), with the hardcoat (4c1) arranged on an outer face of the optical component (1).

[0179] The invention has been described by reference to exemplary embodiments. The skilled person will understand that various modifications and alternatives may be made without departing from the scope of the claims. The use of terms such as "preferably" and "for example" indicates optional features unless explicitly stated otherwise.List of reference signs

[0180] Reference sign Description

[0181] 1 Optical component

[0182] 2 Optical surface

[0183] 3 Mold

[0184] 4 Film

[0185] 4a Rigid support layer

[0186] 4b Adhesive layer

[0187] 4c Coating

[0188] 4d Buffer layer

[0189] 4e Protective liner

[0190] 5 Curable optical material

[0191] 6 Preformed optical substrate

[0192] 6a Coating on the preformed optical substrate

[0193] 7 Chuck

[0194] 11 Step of providing the mold

[0195] 12 Step of laminating the film

[0196] 13 Step of casting the curable optical material

[0197] 14 Step of curing the curable optical material

[0198] 15 Step of separating the body of the optical component from the mold

Claims

Claims1. An optical component (1) comprising:a body of cured material,a sheet (4), preferably a film, laminated to an external surface of the body,whereinthe sheet (4) forms an optical surface of the optical component (1), andthe geometry and surface roughness of said optical surface being defined by the sheet and being suitable for optical use.

2. An optical component (1) according to claim 1, wherein the optical component (1) further comprises a preformed optical substrate, wherein said preformed optical substrate is attached to the optical component, wherein said preformed optical substrate is preferably attached on a side of the optical component (1) opposite to the side at which the sheet (4) is laminated.

3. An optical component (1) according to any one of claims 1 or 2, wherein the optical component (1) comprises a functional layer, preferably embedded in said body, wherein the functional layer is configured for at least one of: an electrical, a mechanical, and an optical interfacing, preferably at one or more edges of the body.

4. An optical component (1) according to any one of claims 1 to 3, wherein the sheet (4) comprises a support layer, and preferably one or more further layers, more preferably wherein the sheet (4) further comprises at least one of the following layers: an anti-reflective coating and a hardcoat.

5. The optical component (1) according to claim 4, wherein the support layer is a rigid support layer made of at least one of polycarbonate, triacetyl cellulose (TAC), and cyclic olefin polymer (COP).

6. The optical component (1) according to any one of claims 4 to 5, wherein the thickness of the support layer is from 20 to 200 micrometres, preferably from 40 to 100 micrometers, more preferably from 50 to 80 micrometers, most preferably from 60 to 75 micrometers.

7. The optical component (1) according to any one of the preceding claims, wherein the optical component comprises two opposite optical surfaces, and wherein each of said optical surfaces is formed by a respective sheet laminated to the body of cured material.

8. A method for manufacturing an optical component (1), the method comprising the steps of:providing (11) at least one mold (3);laminating (12) onto said mold (3) a sheet (4), preferably a film,casting (13) a curable material (5) onto the laminated sheet (4);curing (14) said curable material (5) to form a body of said optical component (1); andseparating (15) the body of said optical component (1) from the mold (3);wherein a surface roughness of the sheet (4) is equal to or lower than a surface roughness of the mold (3).

9. A method according to claim 8, wherein said sheet (4) comprises at least one adhesive layer, wherein said at least one adhesive layer is at least one of: a pressure-sensitive adhesive layer, a heat-sensitive adhesive layer, and an ultraviolet-curable adhesive layer.

10. A method according to claim 9, wherein said at least one adhesive layer comprises:a first adhesive layer facing the mold (3), anda second adhesive layer facing the cured material,wherein said step of separating (15) occurs between said first adhesive layer and said second adhesive layer.

11. A method according to any one of claims 8 to 10, wherein said separation (15) between the sheet (4) and the mold (3) is performed by a differential adhesion, wherein said differential adhesion between the sheet and the mold is weaker than said adhesion between the sheet and the cured material.

12. A method according to any one of claims 8 to 11, wherein the method comprises the step of preforming the sheet (4) prior to the step of laminating (12), preferably by thermoforming.

13. A method according to any one of claims 8 to 12, wherein the method further comprises the step of providing two molds, wherein said molds define two, preferably opposite, optical surfaces of said optical component (1).

14. A method according to any one of claims 8 to 13, wherein the method further comprises the step of providing a preformed optical substrate, wherein said preformed optical substrate has an optical surface, wherein the step of curing is performed while the preformed optical substrate is in contact with the curable material, such that said mold defines a first optical surface of said optical component and said preformed optical substrate defines a second optical surface of said optical component, wherein said second optical surface is preferably opposite to said first optical surface.

15. A method according to claim 14, wherein said preformed optical substrate comprises at least one functional feature, preferably wherein said preformed optical substrate comprises at least one of: a preapplied coating, an embedded component, an electrochromic layer, and a waveguide.