A method for preparing glass microspheres
The method of grinding and granulating mining tailings into glass microspheres addresses the inefficiencies of traditional glass production by utilizing waste materials, reducing energy consumption and environmental risks, and producing high-quality glass microspheres.
Patent Information
- Application Number
- PCT/EP2026/063616
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing glass microspheres are energy-intensive and do not effectively utilize waste materials, particularly mining tailings, which are often contaminated and require significant disposal efforts.
A method involving grinding and granulating mining tailings with a binder to directly convert them into glass microspheres, bypassing energy-demanding steps like melting and fritting, thereby utilizing waste materials and reducing environmental risks.
This method produces glass microspheres efficiently from mining tailings, reducing waste and environmental contamination while providing a valuable product with controlled density and composition.
Smart Images

Figure IMGF000016_0001_TABLE 
Figure IMGF000017_0001_TABLE 
Figure IMGF000017_0002_TABLE
Abstract
Description
A method for preparing glass microspheresTECHNICAL FIELD
[0001] The present invention relates to a method of preparing glass microspheres using mining tailings. The present invention further relates to glass microspheres as such, like solid glass microspheres or hollow glass microspheres.BACKGROUND
[0002] Glass microspheres are typically used as additives and / or fillers in coatings, paints or sealants for various applications. For example, glass microspheres can be used to provide road paints with a specific retro reflectivity. Polymer composite materials including glass microspheres are also known in the art. In general, solid glass microspheres have a comparatively high compressive strength which can increase the mechanical properties of a composite material. Hollow glass microspheres have a comparatively low density which can reduce the average density of a composite material.
[0003] Known processes for making glass microspheres typically require melting and homogenizing a glass, fritting the glass, grinding the glass to a desired particle size, and then converting the ground glass into spheres by heating.
[0004] There is a continuing need in the art to provide more sustainable ways of making glass microspheres and to provide glass microspheres which are based on waste materials or recycled materials.SUMMARY OF INVENTION
[0005] In one aspect, the present invention provides a method for preparing glass microspheres, the method comprising:- providing mining tailings;- grinding the mining tailings to obtain ground mining tailings;- granulating the ground mining tailings with a binder to obtain a granulate;- converting the granulate into glass microspheres.
[0006] Another aspect of the present invention provides glass microspheres which are composed of a material which is at least partially made from mining tailings. In another aspect, the present invention provides glass microspheres which are obtainable by the method according to the present invention. In yet another aspect, the present invention provides a product comprising the glass microspheres according to the present invention.
[0007] It has been found that the method as defined herein allows to make glass microspheres, like solid glass microspheres or hollow glass microspheres, from mining tailings. In particular, it has been found that, by grinding and granulating the mining tailings, the tailings can be converted directly into glass microspheres. Mining tailings are typically a heterogenous blend of crystalline mineral particles. By the method of the present invention, the mining tailings can be converted into glass microspheres without the need of energy-demanding intermediate steps of melting, fritting, and grinding a glass. Mining tailings is an industrial waste material which can occur in significant amounts during mining operations. The appropriate treatment and / or disposal of mining tailings can require much effort andcosts. Additionally, mining tailings may be contaminated, e.g., with heavy metals, and may thus be associated with a risk of leaching into the environment. Recycling mining tailings for making glass microspheres has the potential to reduce a mining waste stream, while at the same time providing a valuable product, thereby increasing circularity of the related industries. Furthermore, potential contaminants can be incorporated into a glass matrix which eliminates, or at least significantly reduces, the risk that such contaminants may leach to its surroundings.
[0008] In one embodiment, the mining tailings are calcium carbonate mining tailings or copper mining tailings.
[0009] In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 40 to 70 wt.% of SiC>2; 19 to 55 wt.% of a combined amount of Me1O and Me22O, wherein Me1O is selected from MgO, CaO, SrO and BaO, and Me22O is selected from IJ2O, Na2O, K2O and Rb2O; 3 to 25 wt.% of Me32C>3, wherein Me32C>3 is selected from AI2O3 and Fe2Os.
[0010] In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 40 to 70 wt.% of SiC>2; 15 to 50 wt.% of CaO; 1 to 20 wt.% of AI2O3; and 0.1 to 15 wt.% of a combined amount of Na2O and K2O.
[0011] In one embodiment, the ground mining tailings have a median particle size d50 in a range of 0.2 to 15 pm.
[0012] In one embodiment, the mining tailings have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(6) poise at a temperature of less than 1100°C.
[0013] In one embodiment, the granulating is a spray granulating to obtain a spray-dried granulate.
[0014] In one embodiment, the conversion of the granulate into the glass microspheres comprises subjecting the granulate to a temperature in a range of 800 to 1400°C for a period of time of less than 1 sec.
[0015] In one embodiment, the glass microspheres are solid glass microspheres, optionally having a a top cut particle size d98 of less than 200 pm. In an alternative embodiment, the glass microspheres are hollow glass microspheres, optionally having a density of less than 1.8 g / cm3.
[0016] In one embodiment, the glass microspheres have a chemical composition comprising: 40 to 70 wt.% of SiC>2; 12 to 50 wt.% of CaO; 1 to 20 wt.% of AI2O3, and 0.1 to 15 wt.% of a combined amount of Na2O and K2O.FIGURES
[0017] Fig. 1 shows a scanning electron microscopy (SEM) image of crystalline minerals in mining tailings of a calcium carbonate mining process (mining tailings 1).
[0018] Fig. 2 shows SEM images of ground mining tailings 1 as described in the examples section in two different magnifications.
[0019] Fig. 3 shows SEM images of spray dried granulate 1 as described in the examples section made from ground mining tailings 1 in two different magnifications.
[0020] Fig. 4 shows SEM images of spray dried granulate 2 as described in the examples section made from ground mining tailings 1 in two different magnifications.
[0021] Fig. 5 shows a SEM image of the solid glass microspheres of example 1 as described in the examples section.
[0022] Fig. 6 shows a SEM image of the solid glass microspheres of example 2 as described in the examples section.
[0023] Fig. 7 shows a x-ray diffraction (XRD) spectrum of the solid glass microspheres of example 2 as described in the examples section.
[0024] Fig. 8 shows a SEM image of the hollow glass microspheres as described in the examples section.
[0025] Fig. 9 shows another SEM image of the hollow glass microspheres as described in the examples section.
[0026] Fig. 10 shows another SEM image of hollow microspheres as described in the examples section at a high magnification.
[0027] Fig. 11 shows a SEM image of a comparative example, for which non-granulated, ground mining tailings were subjected to a glass microsphere formation process. The SEM image shows that, although a few glass microspheres were obtained, a major fraction of crystalline, mineral particles remained.DEFINITIONS
[0028] The term “glass” microsphere as used herein defines a microsphere which comprises a glassy phase as its major component, optionally in combination with a minor amount of a crystalline phase, e.g., less than 10 wt.%, less than 5 wt.% or less than 2 wt.% of a crystalline phase. In one preferred embodiment, the glass microspheres are substantially composed of an amorphous glass phase. In one embodiment, the glass microspheres are essentially free of a crystalline phase.
[0029] The term glass “microsphere” as used herein refers to a glass particle which is substantially spherical in shape and has a size which is less than 1000 pm.
[0030] The term “mining tailings” as used herein refers to the by-products of a mining process which are generated after extracting valuable minerals or metals from an ore. The extraction process typically involves crushing and grinding the ore, followed by various separation techniques such as flotation, filtration, particle size classification, leaching, or magnetic separation. The valuable minerals are isolated and the remaining material are tailings which are typically disposed or stored near a mining site, for example, in a pond. Mining tailings are distinct from an overburden which refers to the material that lies above an area which is exploited in the mining process, such as the rock, soil, and ecosystem that lies above an ore body.
[0031] The term “mineral blend” as used herein refers to a composition of two or more different minerals, and typically more than two minerals, like four or more, six or more, eight or more different minerals, or an even higher number of different minerals.
[0032] As will be understood by those skilled in the art, XRF analysis and ICP-MS analysis can be used to determine the concentration of metallic elements and selected non-metallic elements (e.g., P, S) of a composition. The results of the analysis are typically reported as weight percentage (wt.%) of the corresponding oxide of the measured element, based on the total weight of all the measured elements expressed as their oxides. For example, the element Fe is expressed as a wt.% of Fe2Os, the element Si as a wt.% of SiC>2, etc.. When a chemical composition is defined herein as being“determined by X-ray fluorescence (XRF) analysis or inductively coupled plasma mass spectrometry (ICP-MS) analysis", the element as determined by XRF analysis and / or ICP-MS analysis is expressed as its corresponding oxide and the indicated weight percentage (wt.%) of the specified oxide is based on the total weight of all the measured elements of the composition expressed as their oxides. The indicated weight percentages (wt.%) are values which are preferably normalized as described herein in the section "Measuring methods", i.e., taking into account the weight proportion of the composition to the overall weight of the XRF sample and its loss on ignition. When a chemical composition is defined herein by a specific weight amount of one or more specific elements expressed as their corresponding oxides, the remainder of the chemical composition may be balanced to 100 wt.% by other (measured, but not specifically defined) elements expressed as their corresponding oxides.
[0033] The “calculated viscosity” as used herein refers to a viscosity which may be calculated on the basis of a chemical (oxide) composition of a material, as determined by XRF analysis and / or ICP-MS analysis. The “calculated viscosity” may be expressed as logio(viscosity [in poise]) at a given temperature. Based on a chemical (oxide) composition of a material, as determined by XRF analysis and / or ICP-MS analysis, the “calculated viscosity” may be obtained using the calculations and tables described in A. Fluegel, Eur. J. Glass Sci, Technol. A, February 2007, 48 (1), 13-30, which is incorporated herein be reference. In particular, the prediction may be made using equation (2) as described in A. Fluegel, Eur. J. Glass Sci, Technol. A, February 2007, 48 (1), 13-30. Additionally or alternatively, the “calculated viscosity” may be calculated using the method as described in Q. Zheng, J. C. Mauro, and Y. Yue, “Reconciling calorimetric and kinetic fragilities of glass-forming liquids", Journal of Non-Crystalline Solids, Volume 456, 15 January 2017, pages 95-100, which is incorporated herein by reference. In particular, the calculation may be made using the Mauro-Yue-Ellison-Gupta-Allan (MYEGA) model as described in Q. Zheng, J. C. Mauro, and Y. Yue, Journal of Non-Crystalline Solids, Volume 456, 15 January 2017, pages 95-100. The method by Zheng et al may be carried out using differential scanning calorimetry (DSC) on a glass test specimen, e.g., a glass test specimen made from the mining tailings.
[0034] The "particle size dx" represents the diameter relative to which x % by weight or volume of the particles have diameters less than dx. This means that the particle size d20 value is the particle size at which 20 % by a weight or volume of all particles are smaller than the indicated size, and the d98 value is the (top cut) particle size at which 98 % by a weight or volume of all particles are smaller than the indicated size. The particle size d50 value is thus the median particle size, i.e., 50 % by weight or volume of all particles are smaller than the indicated particle size. Accordingly, the particle size dx is defined herein may be a weight-based particle size dx or a volume-based particle size dx. The "weight-based particle size dx" represents the diameter relative to which x % by weight of the particles have diameters less than dx. This means that the particle size d20 value is the particle size at which 20 % by weight of all particles are smaller than the indicated size, and the d98 value is the (top cut) particle size at which 98 % by weight of all particles are smaller than the indicated size. The weightbased median particle size is thus the particle size at which 50 % by weight of all particles are smaller than the indicated particle size. The weight-based particle size distribution can be measured as known in the art, e.g., by sedimentation analysis of a dispersed sample (based on the application of Stoke’s law) as known in the art, for example, using a Sedigraph device as supplied by MicrometicsInstruments Corporation. The "volume-based particle size dx" represents the diameter relative to which x % by volume have a size less than dx. Accordingly, in that case, the particle size d50 value is the volume-based median particle size, i.e., 50 % by volume of all particles are smaller than the indicated particle size. The volume-based particle size distribution can be measured as known in the art, e.g., by laser diffraction (based on the application of Mie theory) as known in the art, for example, using a Helos device the company Sympatec GmbH or a Mastersizer device of Malvern Instruments Ltd.
[0035] Where the term “comprising” is used herein, it does not exclude that further non-specified elements are present. For the purposes of the present invention, the terms “essentially consisting of’ and “consisting of’ are considered to be specific embodiments of the term “comprising of’. Whenever the terms “including” or “having” are used, these terms are meant to be equivalent to “comprising” as defined above.
[0036] Where an indefinite or definite article is used when referring to a singular noun, e.g., “a”, “an” or “the”, this includes a plural of that noun unless anything else is specifically stated.DETAILED DESCRIPTIONI. The method for making glass microspheres
[0037] In one aspect, the present invention provides a method for preparing glass microspheres, the method comprising:- providing mining tailings;- grinding the mining tailings to obtain ground mining tailings;- granulating the ground mining tailings with a binder to obtain a granulate;- converting the granulate into glass microspheres.The mining tailings
[0038] The method comprises a step of providing mining tailings. The mining tailings are not particularly limited as long as it is suitable for making a glass. The mining tailings may be calcium carbonate mining tailings and / or copper mining tailings. The mining of calcium carbonate minerals and copper ore and / or copper minerals may result in tailings with a comparatively high amount of silicate minerals. The tailings may be derived from one or more specific waste streams of a mining process. For example, the tailings may be derived from a separation process, like a flotation process and / or a filtration process, and particularly from a flotation process. It is also possible that the mining tailings are derived from two or more different mining tailings.
[0039] In one embodiment, the mining tailings are calcium carbonate mining tailings and / or copper mining tailings. In one embodiment, the mining tailings are obtained from calcium carbonate mining tailings. In one embodiment, the mining tailings are by-products from a flotation process of mining calcium carbonate mineral and / or copper ore, and particularly calcium carbonate mineral. The byproducts from flotation processes of calcium carbonate mines and copper mines may be rich in silicate minerals which may be preferred for the method described herein.
[0040] The mining tailings are typically in a form which does not require a specific pre-treating step previous to the grinding. However, if needed, the mining tailings may be pre-treated (e.g., dewatered, dried, sorted, or coarse ground).
[0041] The particle size distribution of the mining tailings is not particularly limited as long as the material is suitable for a grinding step as defined herein. The mining tailings typically have a rather coarse particle size. The mining tailings may have a median particle size d50 in a range of 10 to 100 pm, like in a range of 15 to 80 pm or 15 to 50 pm. The mining tailings may have a top cut particle size d98 in a range of 60 to 800 pm, like in a range of 80 to 600 pm or 100 to 400 pm. The mining tailings may have a volume-based median particle size d50 in a range of 10 to 100 pm, like in a range of 15 to 80 pm or 15 to 50 pm. The mining tailings may have a volume-based top cut particle size d98 in a range of 60 to 800 pm, like in a range of 80 to 600 pm or 100 to 400 pm.
[0042] The mining tailings typically comprise silicate minerals, usually in combination with calcium carbonate-containing minerals. The silicate minerals may be, but are not limited to, silica, mica, feldspar, chlorite, clay minerals, and talc. The calcium carbonate-containing minerals may be, but are not limited to, marble, limestone, and dolomite. The mining tailings may comprise further minerals, like iron-containing minerals. Iron-containing minerals may be, but are not limited to, iron sulphates, iron sulphides, and iron oxides. The minerals in the mining tailings may be determined as is known in the art, for example, by XRD analysis.
[0043] The mining tailings may be further characterized by a loss on ignition (LOI). The LOI may be determined using thermogravimetric analysis (TGA) up to a temperature of 1000°C. The mining tailings may have in a range of 4 to 27 wt.%, like in a range of 4 to 22 wt.%, in a range of 8 to 22 wt.% or in a range of 10 to 20 wt.%.
[0044] The mining tailings may further be defined by its chemical composition. The chemical composition may be determined as is known in the art. For example, the chemical composition may be determined by XRF analysis or ICP-MS analysis. In one embodiment, the chemical composition as defined herein is determined by XRF analysis. The chemical composition as determined by XRF analysis or ICP-MS analysis may be used to predict a viscosity of the mining tailings in relation to a temperature (i.e., a viscosity / temperature plot).
[0045] The mining tailings may have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(6) poise at a temperature of less than 1100°C, like in a range of 800 to 1050°C, in a range of 850 to 1050°C, or in a range of 900 to 1025°C. Additionally or alternatively, the mining tailings may have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(2) poise at a temperature of less than 1500°C, like in a range of 1000 to 1450°C, in a range of 1100 to 1400°C, or in a range of 1150 to 1350°C.
[0046] In one embodiment, the mining tailings have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of:log(6) poise at a temperature of less than 1100°C, like in a range of 800 to 1050°C, in a range of 850 to 1050°C, or in a range of 900 to 1025°C; andIog(2) poise at a temperature of less than 1500°C, like in a range of 1000 to 1450°C, in a range of 1100 to 1400°C, or in a range of 1150 to 1350°C.
[0047] The mining tailings may have a temperature difference between the calculated viscosity of log(6) poise and the calculated viscosity of log(2) poise in a range of 200 to 500°C, like in a range of 250 to 400°C or 250 to 350°C.
[0048] The mining tailings may be characterized by a chemical composition having a specific weight amount of one or more specific elements expressed as their corresponding oxides, as determined by XRF analysis or ICP-MS analysis. The mining tailings may have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising at least 40 wt.%, like in a range of 40 to 70 wt.%, 40 to 65 wt.% or 45 to 60 wt.%, of SiC>2.
[0049] The mining tailings may have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising:40 to 70 wt.% of SiC>2; and19 to 55 wt.% of a combined amount of Me1O and Me22O, wherein Me1O is selected from MgO, CaO, SrO and BaO, and Me22O is selected from IJ2O, Na2O, K2O and Rb2O.3 to 25 wt.% of Me32C>3, wherein Me32C>3 is selected from AI2O3 and Fe2C>3.
[0050] The mining tailings may have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising:40 to 70 wt.%, like 40 to 65 wt.%, 45 to 60 wt.% or 48 to 55 wt.%, of SiC>2;12 to 50 wt.%, like 15 to 40 wt.%, 20 to 35 wt.% or 23 to 30 wt.%, of CaO, optionally in combination with 1 to 9 wt.%, like 2 to 6 wt.% or 2 to 4 wt.%, of MgO;1 to 22 wt.%, like 3 to 18 wt.%, 6 to 15 wt.% or 8 to 12 wt.%, of AI2O3, optionally in combination with 0.1 to 8 wt.%, like 0.5 to 6 wt.% or 1 to 4 wt.% of Fe2O3; and0.1 to 15 wt.%, like 0.5 to 10 wt.%, 1 to 8 wt.%, or 2 to 6 wt.%, of a combined amount of Na2O and K2O, andoptionally 0.1 to 5 wt.%, like 0.5 to 3 wt.%, of SO3.
[0051] The mining tailings may have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising:40 to 70 wt.%, like 40 to 65 wt.%, 45 to 60 wt.% or 48 to 55 wt.%, of SiC>2;12 to 50 wt.%, like 15 to 40 wt.%, 20 to 35 wt.% or 23 to 30 wt.%, of CaO;1 to 9 wt.%, like 2 to 6 wt.% or 2 to 4 wt.%, of MgO;1 to 22 wt.%, like 3 to 18 wt.%, 6 to 15 wt.% or 8 to 12 wt.%, of AI2O3;0.1 to 8 wt.%, like 0.5 to 6 wt.% or 1 to 4 wt.% of Fe2O3; and0.1 to 15 wt.%, like 0.5 to 10 wt.%, 1 to 8 wt.%, or 2 to 6 wt.%, of a combined amount of Na2O and K2O, andoptionally 0.1 to 5 wt.%, like 0.5 to 3 wt.%, of SO3.
[0052] In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 40 to 65 wt.% of SiC>2; 20 to 50 wt.% of CaO; 1 to 9 wt.% of MgO; 1 to 15 wt.% of AI2O3; 0.1 to 6 wt.% of Fe2O3; 0.5 to 8 wt.% of a combined amount of Na2O and K2O; and 0.1 to 5 wt.% of SO3.
[0053] In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 40 to 65 wt.% of SiC>2; 15 to 40 wt.% of CaO; 2 to 6 wt.% of MgO; 3 to 18 wt.% of AI2O3; 0.5 to 6 wt.% of Fe2Os; 0.5 to 10 wt.% of a combined amount of Na2O and K2O; and 0.1 to 5 wt.% of SO3.
[0054] In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 45 to 60 wt.% of SiC>2; 20 to 35 wt.% of CaO; 2 to 6 wt.% of MgO; 6 to 15 wt.% of AI2O3; 0.5 to 6 wt.% of Fe2O3; 1 to 8 wt.% of a combined amount of Na2O and K2O, and 0.1 to 5 wt.% of SO3.In one embodiment, the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising: 48 to 55 wt.%, of SiO2; 23 to 30 wt.% of CaO; 2 to 4 wt.% of MgO; 8 to 12 wt.% of AI2O3; 1 to 4 wt.% of Fe2O3; 2 to 6 wt.% of a combined amount of Na2O and K2O, and 0.5 to 3 wt.% of SO3.
[0055] The specified oxide components of the chemical composition may be selected to add up to at least 95 wt.% or at least 98 wt.%, with an optional remainder being other (measured, but not specifically defined) elements expressed as their corresponding oxides (such as, but not limited to, TiC>2, P2O5, MnO, ZnO, SrO, Cr2Os, NiO, and / or BaO).Grinding the mining tailings to obtain ground mining tailings
[0056] The method comprises the step of grinding the mining tailings to obtain ground mining tailings.
[0057] In general, the grinding of the mining tailings may be a dry or wet grinding and may be carried out with any conventional grinding device, for example, under conditions such that comminution predominantly results from impacts with a secondary body, i.e. in one or more of: an agitator bead mill (e.g., a Dyno Mill), a ball mill, a rod mill, a vibrating mill, a roll crusher, a centrifugal impact mill, a vertical bead mill, an attrition mill, a pin mill, a hammer mill, a pulveriser, a shredder, a declumper, a knife cutter, or other such eguipment known to the skilled person. In case the mining tailings are wet ground, the grinding step may be performed under conditions such that autogenous grinding takes place and / or by horizontal ball milling, and / or other such processes known to the skilled man. The wet ground mining tailings thus obtained may be washed, dewatered, and / or dried by well-known processes, e.g. by flocculation, filtration, forced evaporation, spray drying. The wet grinding may provide an aqueous composition comprising the ground mining tailings. The aqueous composition may have a solids content of 30 to 80 wt.%, like 50 to 70 wt.%.
[0058] The ground mining tailings typically have a median particle size d50 in a range of 0.2 to 15 pm, like in a range of 0.2 to 10 pm, 0.5 to 7.5 pm, 0.5 to 5.0 pm, or 1 .0 to 3.0 pm. The mining tailings may have a top cut particle size d98 in a range of 3.0 to 50 pm, like in a range of 3.0 to 40 pm, 4.0 to 25 pm, 5.0 to 18 pm, or 6.0 to 12 pm. The ground mining tailings typically have a volume-based median particle size d50 in a range of 0.2 to 15 pm, like in a range of 0.2 to 10 pm, 0.5 to 7.5 pm, 0.5 to 5.0 pm, or 1.0 to 3.0 pm. The mining tailings may have a volume-based top cut particle size d98 in a range of 3.0 to 50 pm, like in a range of 3.0 to 40 pm, 4.0 to 25 pm, 5.0 to 18 pm, or6.0 to 12 pm.
[0059] In one embodiment, the ground mining tailings have a median particle size distribution d50 in a range of 0.5 to 7.5 pm and a top cut particle size d98 in a range of 4.0 to 25 pm. In one embodiment, the ground mining tailings have a median particle size distribution d50 in a range of 0.5 to 5.0 pm anda top cut particle size d98 in a range of 5.0 to 18 pm. In one embodiment, the ground mining tailings have a median particle size d50 in a range of 1.0 to 3.0 pm and a top cut particle size d98 in a range of 6.0 to 12 pm. In one embodiment, the ground mining tailings have a volume-based median particle size distribution d50 in a range of 0.5 to 7.5 pm and a volume-based top cut particle size d98 in a range of 4.0 to 25 pm. In one embodiment, the ground mining tailings have a volume-based median particle size distribution d50 in a range of 0.5 to 5.0 pm and a volume-based top cut particle size d98 in a range of 5.0 to 18 pm. In one embodiment, the ground mining tailings have a volume-based median particle size d50 in a range of 1.0 to 3.0 pm and a volume-based top cut particle size d98 in a range of 6.0 to 12 pm.
[0060] The ground mining tailings may be characterized by a specific surface area. The specific surface area may be determined according to the BET method using nitrogen as adsorbing gas. The ground mining tailings may have a specific surface area (BET method using nitrogen) in a range of 2.0 to 50 m2 / g, like in a range of 5.0 to 30 m2 / g or 10 to 20 m2 / g. The ground mining tailings may be characterized by its optical properties, like ISO brightness R457. The ground mining tailings may have an ISO brightness R457 of less than 80%, like in a range of 40 to 75% or 45 to 65%.
[0061] In one embodiment, the ground mining tailings have a volume-based median particle size d50 in a range of 0.5 to 5.0 pm, a volume-based top cut particle size d98 in a range of 5.0 to 18 pm, a specific surface area (BET method using nitrogen) in a range of 5.0 to 30 m2 / g, and optionally an ISO brightness R457 in a range of 30 to 75%. In one embodiment, the ground mining tailings have a volume-based median particle size d50 in a range of 1.0 to 3.0 pm, a volume-based top cut particle size d98 in a range of 6.0 to 12 pm, a specific surface area (BET method using nitrogen) in a range of 10 to 20 m2 / g, and optionally an ISO brightness R457 of in a range of 40 to 70%.Granulating the ground mining tailings to obtain a granulate
[0062] The method comprises a step of granulating the ground mining tailings with a binder to obtain a granulate. The granulating may be carried out by any suitable means. The granulating may be a spray granulating. Accordingly, the granulate may be a spray dried granulate.
[0063] Before and / or during granulation the ground mining tailings may be mixed with one or more components in addition to the binder. For example, the ground mining tailings may be mixed with one or more additional components before and / or during granulation to provide a mixture comprising the ground mining tailings and the one or more additional components. The composition of the mixture is not particularly limited as long as the mixture is suitable for forming a glass. The one or more additional components may be, but are not limited to, blowing agents, additives, glass, and / or glassforming components. The mixture is granulated with the binder to obtain the granulate.
[0064] The granulate may comprise the ground mining tailings in a comparatively low amount, e.g., when the granulate is made from a mixture comprising substantial amounts of other glass-forming components. For example, the granulate may comprise the ground mining tailings in an amount of at least 10 wt.% or at least 20 wt.%, based on the total weight of the granulate.
[0065] It is however typically preferred to incorporate the ground mining tailings into the granulate in a comparatively high amount to increase the overall amount of recycled mineral from mining tailing in the granulate. Accordingly, it is preferred that the granulate comprises the ground mining tailings in anamount of at least 80 wt.%, at least 90 wt.%, or at least 95 wt.%, based on the total weight of the granulate. A suitable upper limit for the weight amount of the ground mineral material may be, for example, 96 wt.%, 98 wt.%, or 99 wt.%, based on the total weight of the granulate. The granulate may essentially be composed of the ground mining tailings and the binder.
[0066] The binder is not particularly limited as long as it is suitable to bind (mineral) particles of mining tailings. The binder may be a binder for spray granulation. The binder is typically used as part of a liquid composition, like an aqueous composition. The binder may be, but is not necessarily limited to, a polyol, a starch-based binder, a cellulose-based binder, a polyvinylpyrrolidone, a polyvinyl alcohol, boric acid, or water glass. In one embodiment, the binder is a polyvinyl alcohol, boric acid or water glass. In one specific embodiment, the binder is a polyvinyl alcohol. The polyvinyl alcohol may be a homopolymer or a copolymer, like a vinyl acetate-vinyl alcohol copolymer. The polyvinyl alcohol may by a (essentially) fully hydrolyzed polyvinyl alcohol or partially hydrolyzed polyvinyl alcohol. For example, the partially hydrolyzed polyvinyl alcohol may be hydrolyzed in a range of 60 to 95 mol-%, like about 88 mol-%. Suitable polyvinyl alcohols are the commercial product Polyviol® solution LL 2850 or the commercial product Selvol™ Polyvinyl Alcohol 24-203 Solution.
[0067] The granulate may comprise the binder in an amount of 0.2 to 8 wt.%, like 0.5 to 6 wt.% or 1 to 5 wt.%, based on the total weight of the granulate. A suitable amount of binder may be about 2 wt.% or about 4 wt.%, based on the total weight of the granulate.
[0068] The granulate may comprise a blowing agent such as, but not limited to, sulfur-containing compounds, nitrates, carbonates or urea. In one embodiment, the granulation is a spray granulation to obtain a spray dried granulate comprising the ground mining tailings, the binder, and a blowing agent. It is however not absolutely necessary that the granulate comprises a blowing agent. This includes methods for making hollow glass microspheres. It may be that the mining tailings contain gasreleasing components (e.g., carbonate-containing components and / or sulfur-containing components) which provide sufficient gas to expand the glass spheres during formation, thereby providing hollow glass microspheres without the need for an external blowing agent. During formation of hollow glass microspheres, it is also possible that a residual amount of binder decomposes inside a forming sphere, thereby releasing gas which promotes the expansion of a hollow sphere. Accordingly, a binder as defined herein is not considered an additional blowing agent in the meaning of the present disclosure. In one embodiment, the granulate does not contain an additional blowing agent.
[0069] The granulate may have a particle size of less than 250 pm, less than 200 pm, less than 150 pm, less than 100 pm (e.g., in a range of 5 to 50 pm).
[0070] The granulate may have a specific surface area (BET method using nitrogen) in a range of 2.0 to 50 m2 / g, like in a range of 5.0 to 30 m2 / g or 8.0 to 18 m2 / g. The granulate may have an ISO brightness R457 of less than 60%, like in a range of 15 to 50% or 20 to 40%.
[0071] In one embodiment, the granulate has a particle size d50 of in a range of 5 to 100 pm, like 5 to 75 pm or 5 to 50 pm and a specific surface area (BET method using nitrogen) in a range of 2.0 to 50 m2 / g, like in a range of 5.0 to 30 m2 / g or 8.0 to 18 m2 / g.
[0072] The granulate may be defined by its moisture content. The moisture content may be determined by thermogravimetric analysis (TGA) as known in the art, for example, at a moisture desorption temperature of 105°C. The granulate may have a moisture content of less than 1 wt.%(e.g., in a range of 0.1 to 1 wt.%) or less than 0.7 wt.% (e.g., in a range of 0.1 to 0.5 wt.% or in a range of 0.4 to 0.7 wt.%), based on the total weight of the granulate.
[0073] The granulate may be classified by conventional means to remove non-granulated material and / or too coarse material.Converting the granulate into glass microspheres
[0074] The method further comprises the step of converting the granulate into glass microspheres. The conversion may be carried out according to a known process for making glass microspheres.
[0075] The conversion of the granulate into the glass microspheres typically comprises subjecting the granulate to a temperature in a range of 800 to 1400°C. The granulate is typically subjected to the heat for a relatively short period of time, like less than 1 sec, less than 500 msec, or less than 100 msec. The period of time may be in a range of microseconds.
[0076] The temperature for making the glass microspheres is an effective variable to control the density of the glass microspheres, i.e., to control whether solid glass microspheres or hollow microspheres are formed. Fora given granulate, solid glass microspheres may be obtained by subjecting the granulate to a lower temperature, whereas hollow glass microspheres may be obtained at a higher temperature. Without wishing to be bound by theory, it is believed that subjecting a given granulate to a higher temperature quickly converts the surface of the granules into a glass coating (“glazing”). Thereby, gas which forms upon heating of the granule may be substantially retained within the glass coating which ultimately may result in an expansion of the glass microspheres. On the other hand, when the granulate is subjected to a lower temperature, only a minor part of the surface may be quickly converted into a glass coating (“partial glazing”). The partial glass coating may not be sufficient to effectively seal large parts of the surface, thereby resulting in a loss of gas which is formed upon heating.
[0077] In one embodiment, the granulate is converted into solid glass microspheres. The solid glass microspheres may have a density of above 2.4 g / cm3, like in a range of 2.5 to 2.9 g / cm3or in a range of 2.6 to 2.8 g / cm3. The solid glass microspheres may have a median particle size d50 in a range of 2 to 50 pm, like in a range of 2 to 30 pm, in a range of 2 to 20 pm or in a range of 2 to 10 pm. The solid glass microspheres may have a volume-based median particle size d50 in a range of 2 to 50 pm, like in a range of 2 to 30 pm, in a range of 2 to 20 pm or in a range of 2 to 10 pm. The solid glass microspheres may have a top cut particle size d98 of less than 300 pm or less than 200 pm, like in a range of 50 to 150 pm or in a range of 50 to 100 pm. The solid glass microspheres may have a volume-based top cut particle size d98 of less than 300 pm or less than 200 pm, like in a range of 50 to 150 pm or in a range of 50 to 100 pm. The solid glass microspheres may have a refractive index in a range of 1.40 to 1.65, like in a range of 1.45 to 1.60 or 1.48 to 1.58. In one embodiment, the solid glass microspheres have a density of above 2.4 g / cm3, like in a range of 2.5 to 2.9 g / cm3or in a range of 2.6 to 2.8 g / cm3, and a (volume-based) top cut particle size d98 of less than less than 300 pm or less than 200 pm, like in a range of 50 to 150 pm or in a range of 50 to 100 pm.
[0078] In another embodiment, the granulate is converted into hollow glass microspheres. The hollow glass microspheres typically comprise a glass shell which encompasses a hollow core.
[0079] The hollow glass microspheres may have a density of less than 1.8 g / cm3, like in a range of 0.5 to 1.7 g / cm3, in a range of 0.5 to 1.5 g / cm3, or in a range of 0.5 to 1.05 g / cm3. The hollow glass microspheres may have a top cut particle size d98 of less than 500 pm, like less than 300 pm, less than 200 pm, or less than 100 pm. The hollow glass microspheres may have a volume-based top cut particle size d98 of less than 500 pm, like less than 300 pm, less than 200 pm, or less than 100 pm. In one embodiment, the hollow glass microspheres have a density of less than 1.8 g / cm3, like in a range of 0.5 to 1.7 g / cm3or in range of 0.5 to 1.5 g / cm3, and a (volume-based) top cut particle size d98 of less than 500 pm, like less than 300 pm.
[0080] The glass microspheres may have a chemical composition and / or a calculated viscosity as defined herein in the following section for the glass microspheres. The glass microspheres obtained by the method may be glass microspheres according to the invention which are further defined in the following section.II. The glass microspheres
[0081] One aspect of the present invention provides glass microspheres which are composed of a material which is at least partially made from mining tailings. The mining tailings may be characterized as defined in the sections above.
[0082] It is possible that a relatively small portion of the material of the glass microspheres is made from mining tailings. For example, at least 10 wt.% or at least 20 wt.% of the material may be made from the mining tailings, based on the total weight of the material making up the glass microspheres. Typically, the amount of the material which is made from the mining tailings is however higher, like at least 80 wt.%, at least 90 wt.%, at least 95 wt.%, or at least 98 wt.%, based on the total weight of the material making up the glass microspheres. The glass microspheres may essentially be composed of material which is made from mining tailings.
[0083] An indicator that the glass microspheres are at least partially made from mining tailings may be residual amounts (ppm) of contamination, like contamination with a series of (heavy) metals (below 500 ppm) such as, but not limited to, Zn, Ni, Cr, As, Cd, Hg or Pb. Said contamination is typically avoided or not present in glass microspheres produced from new raw materials.
[0084] The glass microspheres may be solid glass microspheres or hollow glass microspheres.
[0085] In one embodiment, the granulate is converted into solid glass microspheres. The solid glass microspheres may have a density of above 2.4 g / cm3, like in a range of 2.5 to 2.9 g / cm3or in a range of 2.6 to 2.8 g / cm3. The solid glass microspheres may have a median particle size d50 of in a range of 2 to 50 pm, like in a range of 2 to 30 pm, in a range of 2 to 20 pm or in a range of 2 to 10 pm. The solid glass microspheres may have a volume-based median particle size d50 of in a range of 2 to 50 pm, like in a range of 2 to 30 pm, in a range of 2 to 20 pm or in a range of 2 to 10 pm. The solid glass microspheres may have a top cut particle size d98 of less than 200 pm, like in a range of 50 to 150 pm. The solid glass microspheres may have a volume-based top cut particle size d98 of less than 300 pm or less than 200 pm, like in a range of 50 to 150 pm or in a range of 50 to 100 pm. The solid glass microspheres may have a refractive index in a range of 1.40 to 1.65, like in a range of 1.45 to 1.60 or 1.48 to 1.58. In one embodiment, the solid glass microspheres have a density of above 2.4 g / cm3, like in a range of 2.5 to 2.9 g / cm3or in a range of 2.6 to 2.8 g / cm3, and a (volume-based)top cut particle size d98 of less than 300 pm or less than 200 pm, like in a range of 50 to 150 pm or in a range of 50 to 100 pm.
[0086] In another embodiment, the granulate is converted into hollow glass microspheres. The hollow glass microspheres typically comprise a glass shell which encompasses a hollow core. The hollow glass microspheres may have a density of less than 1.8 g / cm3, like in a range of 0.5 to 1.7 g / cm3or in range of 0.5 to 1.5 g / cm3or in a range of 0.5 to 1.05 g / cm3. The hollow glass microspheres may have a top cut particle size d98 of less than 500 pm, like less than 300 pm, less than 200 pm, or less than 100 pm. The hollow glass microspheres may have a volume-based top cut particle size d98 of less than 500 pm, like less than 300 pm, less than 200 pm, or less than 100 pm. In one embodiment, the hollow glass microspheres have a density of less than 1.8 g / cm3, like in a range of 0.5 to 1 .7 g / cm3or in range of 0.5 to 1.5 g / cm3, and a (volume-based) top cut particle size d98 of less than 500 pm, like less than 300 pm.
[0087] The glass microspheres may be defined by its chemical composition. The chemical composition of the glass microspheres may be determined as known in the art, for example, by XRF analysis or by ICP-MS analysis. In one embodiment, the chemical composition is determined by XRF analysis, e.g., as described herein.
[0088] The glass microspheres may have a chemical composition comprising:40 to 70 wt.% of SiC>2;19 to 55 wt.% of a combined amount of Me1O and Me22O, wherein Me1O is selected from MgO, CaO, SrO and BaO, and Me22O is selected from IJ2O, Na2O, K2O and Rb2O;3 to 25 wt.% of Me32C>3, wherein Me32C>3 is selected from AI2O3 and Fe2Os.
[0089] The glass microspheres may have a chemical composition comprising:40 to 70 wt.%, like 40 to 65 wt.%, 45 to 60 wt.% or 48 to 55 wt.%, of SiC>2;12 to 50 wt.%, like 15 to 40 wt.%, 20 to 35 wt.% or 23 to 30 wt.%, of CaO,optionally in combination with 1 to 9 wt.%, like 2 to 6 wt.% or 2 to 4 wt.%, of MgO;1 to 22 wt.%, like 3 to 18 wt.%, 6 to 15 wt.% or 8 to 12 wt.%, of AI2O3,optionally in combination with 0.1 to 8 wt.%, like 0.5 to 6 wt.% or 1 to 4 wt.% of Fe2Os; and 0.1 to 15 wt.%, like 0.5 to 10 wt.%, 1 to 8 wt.%, or 2 to 6 wt.%, of a combined amount of Na2O, and K2O, andoptionally up to 2 wt.%, like up to 1 wt.%, like in a range of 0.1 to 1 wt.%, of SO3.
[0090] The glass microspheres may have a chemical composition comprising:40 to 70 wt.%, like 40 to 65 wt.%, 45 to 60 wt.% or 48 to 55 wt.%, of SiC>2;12 to 50 wt.%, like 15 to 40 wt.%, 20 to 35 wt.% or 23 to 30 wt.%, of CaO,1 to 9 wt.%, like 2 to 6 wt.% or 2 to 4 wt.%, of MgO;1 to 22 wt.%, like 3 to 18 wt.%, 6 to 15 wt.% or 8 to 12 wt.%, of AI2O3,0.1 to 8 wt.%, like 0.5 to 6 wt.% or 1 to 4 wt.% of Fe2Os; and0.1 to 15 wt.%, like 0.5 to 10 wt.%, 1 to 8 wt.%, or 2 to 6 wt.%, of a combined amount of Na2O, and K2O, andoptionally up to 2 wt.%, like up to 1 wt.%, like in a range of 0.1 to 1 wt.%, of SO3.
[0091] In one embodiment, the glass microspheres have a chemical composition comprising: 45 to 65 wt.% of SiC>2, 20 to 35 wt.% of CaO, 1 to 9 wt.% of MgO, 1 to 15 wt.% of AI2O3, 0.1 to 6 wt.% ofFe2C>3, 0.1 to 8 wt.% of a combined amount of Na2O, and K2O, and up to 1 wt.%, like in a range of 0.1 to 1 wt.%, of SO3.
[0092] In one embodiment, the glass microspheres have a chemical composition comprising: 40 to 65 wt.% of SiC>2; 15 to 40 wt.% of CaO, 2 to 6 wt.% of MgO; 3 to 18 wt.% of AI2O3; 0.5 to 6 wt.% of Fe2Os; and 0.5 to 10 wt.%, of a combined amount of Na2O, and K2O, and optionally up to 1 wt.%, like in a range of 0.1 to 1 wt.%, of SO3.
[0093] In one embodiment, the glass microspheres have a chemical composition comprising: 45 to 60 wt.% of SiC>2; 20 to 35 wt.% of CaO, 2 to 6 wt.% of MgO; 6 to 15 wt.% of AI2O3, 0.5 to 6 wt.% of Fe2Os; and 1 to 8 wt.% of a combined amount of Na2O, and K2O, and optionally up to 1 wt.%, like in a range of 0.1 to 1 wt.%, of SO3.
[0094] In one embodiment, the glass microspheres have a chemical composition comprising: 48 to 55 wt.% of SiC>2; 23 to 30 wt.% of CaO, 2 to 4 wt.%, of MgO; 8 to 12 wt.%, of AI2O3; 1 to 4 wt.% of Fe2Os; and 2 to 6 wt.%, of a combined amount of Na2O, and K2O, and 0.1 to 1 wt.%, of SO3.
[0095] The specified oxide components of the chemical composition of the glass microspheres may be selected to add up to at least 95 wt.% or at least 98 wt.%, with an optional remainder being other (measured, but not specifically defined) elements expressed as their corresponding oxides (such as, but not limited to, TiC>2, P2O5, ZnO, SrO, Cr2Os, NiO, and / or BaO).
[0096] The glass of the glass microspheres may have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(6) poise at a temperature of less than 1100°C, like in a range of 800 to 1050°C, in a range of 850 to 1050°C, or in a range of 900 to 1025°C. Additionally or alternatively, the glass of the glass microspheres may have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(2) poise at a temperature of less than 1500°C, like in a range of 1000 to 1450°C, in a range of 1100 to 1400°C, or in a range of 1150 to 1350°C.
[0097] In one embodiment, the glass of the glass microparticles has a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of:log(6) poise at a temperature of less than 1100°C, like in a range of 800 to 1050°C, in a range of 850 to 1050°C, or in a range of 900 to 1025°C; andlog(2) poise at a temperature of less than 1500°C, like in a range of 1000 to 1450°C, in a range of 1100 to 1400°C, or in a range of 1150 to 1350°C.
[0098] The glass of the glass microparticles may have a temperature difference between the calculated viscosity of log(6) poise and the calculated viscosity of log(2) poise in a range of 200 to 500°C, like in a range of 250 to 450°C or 250 to 400°C or 250 to 350°C.
[0099] In one embodiment, the calculated viscosity of the glass of the glass microspheres is calculated on the basis of its chemical composition determined by XRF analysis.
[0100] The glass microspheres may be obtained by the method according to the present invention.
[0101] Another aspect of the present invention provides a product comprising the glass microspheres according to the present invention. The product may be, but is not limited to, a paint, a coating, a polymer composite, a cement, a clay-based material, an adhesive, or a sealant.
[0102] The invention is further illustrated in the following by specific examples which are however not to be construed as limiting the invention in any way.III. Examples section1. Measuring methodsX-ray fluorescence (XRF) analysis
[0103] One gram of the sample material was fused with ten grams of lithium borate flux to create samples for XRF testing. Next, the composition of the fused sample, in terms of oxides, was determined using XRF spectroscopy. Normalizing the composition of the fused bead sample to the proportion of the sample material and the loss on ignition yielded the sample material composition.X-ray diffraction (XRD) analysis
[0104] Eight hundred milligrams of the sample material is micronized in 7 mL of water for 5 minutes using zirconia grinding elements. The contents are filtered and the filtrate is dried before mounting in the X-ray diffractometer. The XRD data is analyzed using Rietveld refinement to identify crystalline components in the sample.Particle size distribution
[0105] Weight-median particle size distribution was measured by sedimentation analysis of a fully dispersed sample using a Sedigraph device from the company Micrometrics Instruments Corporation. Volume-based particle size distribution was measured by laser diffraction using a HELOS device from the company Sympatec GmbH or Mastersizer device of Malvern Instruments Ltd.Specific surface area
[0106] The specific surface area (in m2 / g) was determined using the BET method (using nitrogen as adsorbing gas) according to ISO 9277:2010.Moisture content
[0107] Moisture content was measured by TGA at a desorption temperature of 105°C using a HB43 device from the company Mettler Toledo.Density
[0108] A dry, powder sample of known mass is introduced to the pycnometer sample chamber. The sample chamber is closed and the system is purged with Helium gas. The expansion valve is opened, and the helium fills the reference chamber of known volume. Since the pressure is known before and after the expansion valve is opened, the volume excluded by the sample may be calculated via Boyle’s Law. Dividing the sample mass by the sample volume yields the true density.Refractive index
[0109] Glass samples were cast into molds and a piece of glass with a 1 cm2cross-section is cut. This piece of glass is embedded in epoxy resin and polished to 1 micron roughness. The embedded glass sample is then measured using a refractometer (jeweler's refractometer).2. MaterialsMining tailings
[0110] Mining tailings 1: mining tailings were obtained from a calcium carbonate mining process. A sample of the mining tailings had the following volume-based particle size distribution: d10 = 4.9 pm; d25 = 10.6 pm; d50 = 26.9 pm; d75 = 64.9 pm; d90 = 120.6 pm; d98 = 206.8 pm. A representative SEM image of a sample of the mining tailings is shown in Fig. 1.
[0111] A sample of the mining tailings was analyzed by XRF. Based on the oxide composition determined by XRF, a viscosity-temperature plot was calculated. The results are provided in table 1.
[0112] Table 1: XRF analysis of mining tailings 1 and calculated viscosityXRF data Calculated viscosity Oxide [wt.%] [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO243.2 52.52 1262AI2O3 8.4 10.2 2.5 1215Na2O 0.2 0.2 3 1171K2O 3.8 4.6 4 1094MgO 2.5 3.0 5 1029CaO 20.7 25.1 6 972TiO20.3 0.4 7 922Fe2Os 1.6 2.0 7.6 895P2O50.1 0.1 8 878SO31.5 1.8 9 839Other oxides <0.1 <0.1 10 80411 77211.5 758loss on ignition 17.6 (excluding LOI)(LOI) 12 74413 718Total 100 100 13.3 71014 69414.5 683
[0113] Mining tailings 2: mining tailings were obtained from a calcium carbonate mining process. A sample of the mining tailings had the following volume-based particle size distribution: d10 = 1.5 pm; d25 = 8.6 pm; d50 = 45.4 pm; d75 = 141.8 pm; d90 = 141.8 pm; d98 = 210.9 pm.
[0114] A sample of the mining tailings was analyzed by XRF and, based on the oxide composition determined by XRF, a viscosity-temperature plot was calculated. The results are provided in table 2.
[0115] Table 2: XRF analysis of mining tailings 2 and calculated viscosityXRF data Calculated viscosity Oxide [wt.%] [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO234.1 45.3 2 1163AI2O3 0.8 1.0 2.5 1102Na2O 0.3 0.3 3 1049K2O 0.2 0.2 4 965MgO 6.0 8.0 5 900CaO 33.4 44.3 6 848TiO20.1 0.1 7 806Fe2Os 0.3 0.4 7.6 784P2O50.1 0.1 8 771SO30.1 0.2 9 742Other oxides <0.1 <0.1 10 71711 69511.5 685loss on ignition 24.4 (excluding LOI)(LOI) 12 67613 660Total 100 100 13.3 65514 64514.5 638
[0116] Mining tailings 3: mining tailings were obtained from a calcium carbonate mining process. A sample of the mining tailings had the following volume-based particle size distribution: d10 = 5.1 pm; d25 = 12.4 pm; d50 = 26.3 pm; d75 = 49.1 pm; d90 = 79.7 pm; d98 = 125.1 pm.
[0117] A sample of the mining tailings was analyzed by XRF and, based on the oxide composition determined by XRF, a viscosity-temperature plot was calculated. The results are provided in table 3.
[0118] Table 3: XRF analysis of mining tailings 3 and calculated viscosityXRF data Calculated viscosity Oxide [wt.%] [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO246.5 57.0 2 1427AI2O3 5.4 6.6 2.5 1331Na2O 0.1 0.1 3 1251 K2O 1.5 1.9 4 1128MgO 2.5 3.1 5 1037CaO 22.5 27.6 6 967TiO20.1 0.2 7 911Fe2O3 1.2 1.5 7.6 8838 866SO31.5 1.9 9 829Other oxides <0.1 <0.1 10 79711 77111.5 759loss on ignition 18.6 (excluding LOI)(LOI) 12 74713 727Total 100 100 13.3 72214 70914.5 701Binding agent
[0119] Binding agent 1: commercial product Polyviol® LL2850 which is a 25% agueous solution of a polyvinyl alcohol with a density (20°C) of 1.06 g / cm3 and a viscosity of 1300 to 1900 mPa*s (23°C).
[0120] Binding agent 2: commercial product SELVOL™ Polyvinyl alcohol 24-203 solution which is a solution (24 wt.% solids) of vinyl acetate-vinyl alcohol copolymer (about 88 mol-% hydrolyzed) with a solution viscosity of 775 ± 525 cP and a solution pH of 5.5 ± 1.0.3. Glass made from the mining tailings
[0121] A glass made from each one of the mining tailings 1 to 3 was analyzed for its chemical composition by XRF as well as its calculated viscosity. The results are provided in tables 4 to 6.
[0122] Table 4: XRF analysis of glass made from the mining tailings 1 and its calculated viscosity XRF data Calculated viscosity Oxide [wt.%] (raw) [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO249.0 51.0 2 1244AhOs 9.7 10.1 2.5 1197Na2O 0.5 0.5 3 1154K2O 4.3 4.5 4 1078MgO 3.0 3.1 5 1014CaO 26.2 27.3 6 958TiO20.4 0.4 7 910Fe2O3 1.9 2.0 7.6 883P2O5 0.1 0.1 8 867 so30.9 0.9 9 829Other oxides <0.1 <0.1 10 79511 765Total 96.1 100 11.5 75112 73813 71313.3 70614 69014.5 680
[0123] Table 5: XRF analysis of glass made from the mining tailings 2 and its calculated viscosity XRF data Calculated viscosity Oxide [wt.%] (raw) [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO258.8 59.8 2 1361AI2O3 1.5 1.5 2.5 1267Na2O 0.4 0.4 3 1190K2O 0.3 0.3 4 1071MgO 6.7 6.8 5 985CaO 29.8 30.4 6 919TiO20.1 0.1 7 866Fe2O3 0.4 0.5 7.6 840P2O5 0.1 0.1 8 8249 790Other oxides <0.1 <0.1 10 76011 736Total 98.2 100 11.5 72412 71413 69613.3 69014 67914.5 672
[0124] Table 6: XRF analysis of glass made from the mining tailings 3 and its calculated viscosity XRF data Calculated viscosity Oxide [wt.%] (raw) [wt.%] (normalized) Viscosity in Temperature in [°C] logio(visc. [poise])SiO257.7 58.2 2 1362.8AI2O3 7.7 7.8 2.5 1285.6Na2O 0.3 0.3 3 1219.8K2O 1.7 1.7 4 1113.4MgO 2.5 2.6 5 1031.1CaO 26.6 27.0 6 965.6TiO20.2 0.2 7 912.2Fe2O3 1.5 1.6 7.6 884.68 867.8SO3 0.5 0.5 9 830.4Other oxides <0.1 <0.1 10 798.411 770.7Total 98.8 100 11.5 758.212 746.513 725.113.3 719.214 706.214.5 697.54. Processing steps for making glass microspheresGranules
[0125] Mining tailings 1 were subjected to a wet grinding as follows: mining tailings 1 were mixed with water and the resulting slurry was continuously pumped into a ceramic jar / media (agitator bead mill) and pumped back into the slurry. The exiting slurry was sampled and measured for its particle size distribution. When the desired particle size distribution was achieved, the process is stopped. An aqueous suspension (slurry) of ground tailings was obtained having a solids content of about 65%. The ground tailings had a volume-based median particle size d50 of about 1.75 pm, a BET specific surface area of about 15.3 m2 / g, and an ISO brightness R457 of about 51.9%. Representative SEM images of the ground tailings are shown in Fig. 2.
[0126] The ground tailings were subjected to spray dry granulation using 2% dry weight of polyvinyl alcohol of binding agent 1 (25% solution) to provide spray dried granules 1. The spray dried granules 1 had a moisture content (determined at a desorption temperature of 105°C) of 0.35 wt.%; a BET specific surface area of 13.2 m2 / g, and an ISO brightness R457 of 29.8%. Representative SEM images of the spray dried granules 1 are shown in Fig. 3.
[0127] The ground tailings were subjected to spray dry granulation using 4% dry weight of polyvinyl alcohol of binding agent 1 (25% solution) to provide spray dried granules 2. The spray dried granules 2 had a moisture content (determined at a desorption temperature of 105°C) of 0.6 wt.% and a BET specific surface area of 10.6 m2 / g. Representative SEM images of the spray dried granules 2 are shown in Fig. 4.
[0128] In each case, the spray drying was carried out on a Biichi Mini Spray Dryer B-290 (adjusted with 2-fluid nozzle 0.7 mm). The aqueous suspension of the ground tailings was diluted to a BF100 viscosity of 130 mPa*s (about 48% solids). The spray dryer was run with the following parametersettings: inlet temperature max. 220°C; outlet temperature targeting to 80 - 90°C; aspirator gas flow rate fixed to 75% (equal to about 30 m3 / h); spray gas flow rate approx. 600 l / h (indicated height 35 - 40 mm on flow meter / rotameter); pump rate 25%, feed flow 7 - 8 ml / min.Solid glass microspheres
[0129] Example 1: Spray-dried granules were obtained as described herein above for spray-dried granules 1 with the exception that binding agent 2 was used instead of binding agent 1. The spray-dried granules were subjected to a temperature of 1300°C for a very short time, thereby providing solid glass microspheres. The solid glass microspheres had a density of 2.66 g / cm3. A representative SEM image of the sold glass microspheres is shown in Fig. 5.
[0130] Example 2: Spray-dried granules were obtained as described herein above for spray-dried granules 1 with the exception that binding agent 2 was used instead of binding agent 1. A burner was run with the following parameters: propane (psig) = 9; air (psig) = 6; oxygen (psig) = 6. The spray-dried granules were fed to a close proximity of a torch of the burner, thereby providing solid glass microspheres. The solid glass microspheres had a volume-based particle size distribution of: d10 = 1.8 pm; d25 = 3.0 pm; d50 = 4.8 pm; d75 = 7.5 pm; d90 = 12.3 pm; d98 = 71.3 pm. The solid glass microspheres had a density of 2.74 g / cm3and a refractive index n = 1.50-1.55. A representative SEM image of the sold glass microspheres is shown in Fig. 5. An XRD spectrum of the solid glass microspheres is shown in Fig. 7 indicating a substantially amorphous material (glass).Hollow glass microspheres
[0131] Spray-dried granules were obtained as described herein above for spray-dried granules 2 with the exception that binding agent 2 was used instead of binding agent 1. A burner was run with the following parameters: propane (psig) = 20; air (psig) = 7; oxygen (psig) = 13.5. The spray-dried granules 2 were fed to a torch of the burner at a position having a temperature of about 1100°C, thereby providing hollow glass microspheres. The hollow glass microspheres had a density of 1.33 g / cm3. Representative SEM images of the hollow glass microspheres are shown in Figs. 8 to 10.
Claims
CLAIMS1. A method for preparing glass microspheres, the method comprising:- providing mining tailings;- grinding the mining tailings to obtain ground mining tailings;- granulating the ground mining tailings with a binder to obtain a granulate;- converting the granulate into glass microspheres.
2. The method of claim 1 , wherein the mining tailings are calcium carbonate mining tailings or copper mining tailings.
3. The method of claim 1 or 2, wherein the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising:40 to 70 wt.% of SiC>2;19 to 55 wt.% of a combined amount of Me1O and Me22O, wherein Me1O is selected from MgO, CaO, SrO and BaO, and Me22O is selected from Li2O, Na2O, K2O and Rb2O;3 to 25 wt.% of Me32C>3, wherein Me32C>3 is selected from AI2O3 and Fe2Os.
4. The method of any one of claims 1 to 3, wherein the mining tailings have a chemical composition, as determined by XRF analysis or ICP-MS analysis, comprising:40 to 70 wt.% of SiC>2;15 to 50 wt.% of CaO;1 to 20 wt.% of AI2O3; and0.1 to 15 wt.% of a combined amount of Na2O and K2O.
5. The method of any one of claims 1 to 4, wherein the ground mining tailings have a median particle size d50 in a range of 0.2 to 15 pm.
6. The method of any one of claims 1 to 5, wherein the mining tailings have a calculated viscosity, calculated on the basis of its chemical composition determined by XRF analysis or ICP-MS analysis and expressed as logio(viscosity in [Poise]), of log(6) poise at a temperature of less than 1100°C .
7. The method of any one of claims 1 to 6, wherein the granulating is a spray granulating to obtain a spray-dried granulate.
8. The method of any one of claims 1 to 7, wherein the conversion of the granulate into the glass microspheres comprises subjecting the granulate to a temperature in a range of 800 to 1400°C for a period of time of less than 1 sec.
9. The method of any one of claims 1 to 8, wherein the glass microspheres are solid glass microspheres.
10. The method of any one of claims 1 to 8, wherein the glass microspheres are hollow glass microspheres.
11. Glass microspheres, being composed of a material which is at least partially made from mining tailings.
12. The glass microspheres of claim 11, having a chemical composition comprising: 40 to 70 wt.% of SiC>2;12 to 50 wt.% of CaO;1 to 20 wt.% of AI2O3, and0.1 to 15 wt.% of a combined amount of Na2O and K2O.
13. The glass microspheres of claim 11 or claim 12, being solid glass microspheres having a top cut particle size d98 of less than 200 pm.
14. The glass microspheres of claim 11 or claim 12, being hollow glass microspheres having a density of less than 1.8 g / cm3.