Bitumen / plastomer composition incorporating a thermal plastic conversion residue
A bitumen/polymer composition with a distillation residue from plastic thermal conversion reduces fossil reliance and carbon footprint, enhancing cold pliability and flexibility for sealing and soundproofing materials.
Patent Information
- Application Number
- PCT/EP2026/063646
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Existing bituminous compositions for sealing and soundproofing materials are heavily dependent on fossil resources, leading to high oil consumption and significant greenhouse gas emissions, with a need for compositions that reduce fossil-based materials and improve sustainability while maintaining performance.
A bitumen/polymer composition incorporating a distillation residue from the thermal conversion of plastics, including 5% to 40% plastomer, which reduces the content of bitumen, polymer, and fluxing agents of petroleum origin, while maintaining or improving cold pliability and flexibility.
The composition achieves reduced reliance on fossil resources, lower carbon footprint, and improved cold pliability without compromising performance, making it suitable for sealing and soundproofing applications.
Smart Images

Figure IMGF000026_0001_TABLE 
Figure IMGF000027_0001_TABLE 
Figure IMGF000027_0002_TABLE
Abstract
Description
[0001] BITUMEN / PLASTOMER COMPOSITION INCORPORATING A PLASTIC THERMAL CONVERSION RESIDUE
[0002] The present invention relates to a bituminous composition modified by plastomers and incorporating a distillation residue of a hydrocarbon product obtained by thermal conversion of plastics, particularly plastic waste. The composition of the invention is particularly suitable for the manufacture of sealing and / or soundproofing materials. The invention also relates to a process for preparing a bitumen / plastomer composition according to the invention, as well as its use for the manufacture of various sealing and / or soundproofing materials.
[0003] Various waterproofing and soundproofing materials based on polymer-modified bitumen, particularly SBS (styrene-butadiene-styrene) elastomers, have been known for many years. Examples include waterproofing membranes, which have been widely developed since the 1970s for flat roof waterproofing, as well as adhesives, primers, and soundproofing membranes. It is also common practice to incorporate one or more fluxing agents into these products to lower their viscosity at the application temperature.
[0004] Bitumen is generally obtained from residues resulting from the atmospheric and / or vacuum distillation of crude oil. Furthermore, in the vast majority of cases, polymers are synthesized from petroleum. Finally, fluxing agents generally consist of oils of fossil or synthetic origin, derived from petroleum. The technical field of sealing and soundproofing products is therefore currently highly dependent on the availability of petroleum.
[0005] Oil resources are, however, limited. Indeed, "proven oil reserves" reached over 200 billion tons of oil equivalent (TOE) worldwide in 2018, according to experts at British Petroleum (who have been tracking the resource since 1980). Although substantial, these reserves could only cover 50.2 years of annual consumption at the 2017 rate. These figures are confirmed by the French Alternative Energies and Atomic Energy Commission (CEA) and the International Energy Agency (IEA).
[0006] It is therefore necessary to limit oil consumption but also the dependence of this industry on oil resources. In particular, and from a sustainable development perspective, it would be useful to have bituminous compositions for sealing and / or soundproofing materials with a reduced content of fossil-based compounds, in particular bitumen and / or polymer(s) and / or fluxing agent(s).
[0007] To reduce oil consumption, the plan here is to incorporate recycled compounds / materials, particularly recycled plastic waste, into bituminous compositions. This approach aims to promote the circular economy by limiting the use of fossil resources, especially bitumen, through the incorporation of waste from various sources into the composition.
[0008] In this respect, it is known that plastic waste can be valorized by using it as a feedstock in chemical processes (gasification, pyrolysis, depolymerization, dissolution) or in mechanical processes (shredding). In the feedstock, plastic waste can also be combined with waste derived from biomass.
[0009] High-temperature pyrolysis processes make it possible to transform plastic waste into several products in varying proportions depending on the nature of the waste used: an oil, a gaseous mixture, coke.
[0010] The oil resulting from the pyrolysis of plastic can then be separated into several fractions by all types of separation processes known per se:
[0011] • The light naphtha cut with a distillation range between 50°C and 200°C and a density between 720 kg / m³ 3 and 750 kg / m 3 ;
[0012] • The average diesel cut with a distillation range between 200°C and 300°C and a density between 750 kg / m³ 3 and 800 kg / m 3 ;
[0013] • Heavy cut type VGO (Vacuum Gasoil) with a distillation range between 300°C and 450°C and a density between 800 kg / m³ 3 and 840 kg / m 3 ;
[0014] • A very heavy VR (Visco-Reduced) type cut with an initial boiling point of at least 450 °C and a density between 840 kg / m³ 3 and 870 kg / m 3 .
[0015] Only light fractions such as naphtha can be used as petrochemical feedstock in a steam cracker. Heavy fractions such as VGO and very heavy fractions such as VR are not usable as steam cracker feedstocks. Therefore, there is an alternative need to utilize heavy and very heavy fractions.
[0016] EP 4 124638 A1 describes bitumen-based compositions comprising up to 5% by mass of at least one plastic pyrolysis oil having an initial boiling point of at least 300°C. The resulting compositions exhibit improved softening temperature variation properties compared to bitumen alone.
[0017] However, this document does not specifically address bituminous compositions suitable for waterproofing and / or soundproofing applications. In particular, it does not specifically address polymer-modified bitumen compositions. Furthermore, the pyrolysis oil content is limited to a maximum of 5% by mass.
[0018] Therefore, there remains a need to provide bituminous compositions whose dependence on fossil resources is significantly reduced compared to compositions already known.
[0019] In particular, there remains a need for compositions incorporating a larger proportion of recycled components compared to existing compositions. In other words, there remains a need for bituminous compositions with a significantly reduced content of fossil-based material(s), particularly bitumen and / or fluxing agent and / or polymer, compared to existing compositions.
[0020] Thus, there remains on the one hand the need for compositions whose bitumen content is significantly reduced compared to compositions already known.
[0021] On the other hand, there remains a need for compositions with significantly reduced polymer content compared to already known compositions.
[0022] Furthermore, there remains a need for compositions whose content of fluxing agents, particularly of petroleum or synthetic origin, is significantly reduced compared to compositions already known.
[0023] Furthermore, oil extraction is currently responsible for releasing significant quantities of greenhouse gases into the atmosphere, which have a substantial impact on global warming. The carbon footprint associated with bitumen / polymer compositions is even greater. Indeed, the carbon footprint of pure bitumen is estimated at 0.417 kg of CO2 equivalent per kg of bitumen (estimate by the Ecoinvent association). The carbon footprint of a polymer, particularly a styrene-butadiene elastomer, is currently estimated at between 2.2 and 4.7 kg of CO2 equivalent per kg of polymer, depending on the process used and the optimization of the plants.
[0024] Therefore, there remains a need for bituminous compositions, particularly those intended for use as waterproofing and / or soundproofing materials, with a reduced carbon footprint compared to existing compositions. Furthermore, it is essential that these bituminous compositions offer equivalent, or even improved, properties compared to existing compositions.
[0025] Thus, the present invention relates to a bitumen / polymer composition comprising:
[0026] - at least one bitumen base,
[0027] - at least one distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics,
[0028] - 5% to 40% by mass of at least one plastomer, and
[0029] compared to the total mass of plastomer(s), bitumen base(s) and distillation residue(s).
[0030] Preferably, the residue is an atmospheric distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by pyrolysis of plastic waste.
[0031] "Atmospheric distillation" refers to an operation that separates the different components of a liquid mixture according to their evaporation temperature at atmospheric pressure.
[0032] Advantageously, the residue has a boiling point at 10% by mass, measured according to ASTM D7169:20, greater than or equal to 350°C, preferably from 400°C to 600°C, typically from 410°C to 550°C.
[0033] According to one embodiment, the residue has a ball and ring softening temperature (BRT), measured according to EN 1427, greater than or equal to 60°C, more preferably ranging from 60°C to 120°C, typically ranging from 65°C to 100°C.
[0034] Preferably, the plastomer is chosen from polymers or copolymers comprising at least one ethylene motif, preferably chosen from the group consisting of isotactic polypropylene (IPP), atactic polypropylene (APP), poly alpha olefin polymers (APAO), thermoplastic polyolefins (TPO) and / or ethylene-vinyl acetate (EVAC).
[0035] In particular, the plastomer is selected from the group consisting of isotactic polypropylene, atactic polypropylene, and / or amorphous poly-alpha-olefins. According to one embodiment, the bitumen / polymer composition according to the invention comprises:
[0036] - from 10% to 90% bitumen by mass,
[0037] - from 0.1% to 30% by mass of said at least one distillation residue,
[0038] - 5% to 40% by mass of plastomer(s),
[0039] - from 0% to 70% fillers / or additives, and
[0040] - from 0% to 20% by mass of fluxing agent(s),
[0041] relative to the total mass of the composition.
[0042] The invention also relates to the use of a bitumen / polymer composition according to the invention, for the manufacture of a sealing and / or soundproofing material, preferably chosen from: a sealing membrane, a liquid coating, an adhesive, a primer and a soundproofing membrane.
[0043] The invention also relates to a prefabricated waterproofing membrane comprising:
[0044] - a support or reinforcement, in particular one or more fibrous reinforcements, - a bitumen / polymer composition according to the invention,
[0045] said support or reinforcement being coated on at least one side, preferably impregnated throughout, with said bituminous composition.
[0046] The invention also relates to a method for manufacturing a sealing membrane according to the invention, said method comprising the following successive steps:
[0047] 1) the supply of a bitumen / polymer composition according to the invention;
[0048] 2) the application of the composition obtained in step 1) on at least one face of a support or reinforcement.
[0049] The inventors have surprisingly discovered that it is possible to reduce the content of material(s) of fossil origin, in particular bitumen and / or plastomer(s) and / or fluxing agent(s) of petroleum or synthetic origin, in a bitumen / polymer composition intended for the preparation of a sealing and / or soundproofing product, by the integration into said bitumen / polymer composition of a particular residue, obtained by distillation of a hydrocarbon product, itself obtained by thermal conversion of (waste) plastics.
[0050] In particular, the inventors discovered that it was possible to reduce the content of non-renewable material(s), notably bitumen and / or plastomer and / or petroleum- or synthetic-derived fluxing agent, in the bitumen / polymer composition by incorporating such a residue, without significantly affecting the properties of the final product. The final product exhibits substantially equivalent, or even improved, properties compared to products free of said residue.
[0051] Furthermore, the inventors made a surprising discovery: incorporating this type of residue into a bitumen / polymer composition improves the composition's cold pliability or flexibility, while maintaining a constant polymer content. Consequently, the compositions, as well as the materials derived from them, are less susceptible to cold cracking.
[0052] More specifically, the inventors discovered that incorporating such a residue into a bitumen / polymer composition intended for the preparation of a waterproofing and / or soundproofing product allows:
[0053] - at a constant polymer content, to improve the properties of the composition, particularly in terms of cold pliability, or
[0054] - with equivalent performance, in particular with equivalent cold pliability, to reduce the polymer content in the composition.
[0055] The invention is thus advantageous in that it makes it possible to reduce the content of material(s) of fossil origin, in particular bitumen and / or fluxing agent and / or polymer, of the bitumen / polymer compositions classically used for the manufacture of sealing and soundproofing materials.
[0056] In the following description, and unless explicitly stated otherwise, the quantities of the different components present in a bituminous composition according to the invention are given as % mass, relative to the total mass of the composition (hereinafter referred to as % w / w).
[0057] Similarly, and unless explicitly stated otherwise, the standards mentioned later in the description correspond to the standard in force on the date of 1 er July 2023.
[0058] The term "boiling point" refers to the boiling point commonly used in the oil and gas industry. Boiling points are measured at atmospheric pressure. The initial boiling point is defined as the temperature at which the first vapor bubble forms. The final boiling point is the highest temperature achievable during standard distillation. At this temperature, no more vapor can be drawn into the condensing units. The determination of the initial and final boiling points is known in itself. Depending on the boiling range of the mixture, they can be determined using various standardized methods, such as ASTM D2887:2019, which relates to the distribution of the boiling range of petroleum fractions by gas chromatography.
[0059] For compositions containing heavier hydrocarbons, ASTM D7169:2020 or D2892-20:2020 can also be used. The boiling ranges of distillates can also be advantageously measured using ASTM D7500:2019.
[0060] As mentioned previously, the invention relates to a bitumen / polymer composition comprising:
[0061] - at least one bitumen base,
[0062] - at least one distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, in particular plastic waste, and
[0063] - at least one plastomer in a content ranging from 5% to 40% by mass relative to the total mass of plastomer(s), bitumen base(s) and distillation residue(s).
[0064] Bitumen base
[0065] The bitumen or bitumens used to prepare a bitumen / polymer composition according to the invention are called "bitumen base".
[0066] Among the bitumens usable according to the invention, we can first mention bitumens of natural origin, those contained in deposits of natural bitumen, natural asphalt, or oil sands, and bitumens obtained from crude oil refining. Within the scope of the invention, the bitumen(s) used are advantageously chosen from among bitumens obtained from crude oil refining, in particular bitumens containing asphaltenes or pitches. The bitumens can be obtained by conventional bitumen manufacturing processes in refineries, in particular by direct distillation and / or vacuum distillation of petroleum. These bitumens can optionally be viscoreduced and / or deasphalted and / or air rectified. It is common practice to perform vacuum distillation of atmospheric residues from the atmospheric distillation of crude oil.This manufacturing process therefore consists of a succession of atmospheric distillation and vacuum distillation, with the feedstock for the vacuum distillation being atmospheric residues. These vacuum residues from the vacuum distillation tower can also be used as bitumen. It is also common to inject air into a feedstock typically composed of distillates and heavy products from the vacuum distillation of atmospheric residues from petroleum distillation. This process yields blown, semi-blown, oxidized, air-rectified, or partially air-rectified bitumen.
[0067] Different bitumens obtained by refining processes can be combined in the compositions according to the invention to achieve the best compromise in terms of technical performance. In conventional processes for blending different bitumens, the mixture is blended at temperatures between 100°C and 200°C, preferably between 140°C and 200°C, and with agitation for a period of at least 10 minutes, preferably between 30 minutes and 10 hours, and more preferably between 1 and 6 hours. The temperature and duration of heating vary according to the quantity of bitumen used and are defined by standard NF EN 12594. Blown bitumens can be manufactured in a blowing unit by passing a flow of air and / or oxygen through a starting bitumen or mixture of bitumens. This operation can be carried out in the presence of an oxidation catalyst, for example, phosphoric acid.
[0068] Generally, blowing is carried out at high temperatures, in the range of 200 to 300°C, for relatively long periods typically between 30 minutes and 2 hours, either continuously or in batches. The duration and temperature of blowing are adjusted according to the desired properties of the blown bitumen and the quality of the starting bitumen.
[0069] Among the bitumens that can be used according to the invention, recycled bitumens can also be mentioned.
[0070] Bitumens can be hard grade bitumens (such as grades 10 / 20 and 20 / 30) or soft grade bitumens (such as grade 160 / 220) as defined by standard EN 12591.
[0071] The invention is particularly suitable for cases where the bitumen base consists of a hard grade bitumen or a mixture of hard grade bitumens, in particular chosen from grade 70 / 100, 35 / 50, 20 / 30 and 10 / 20 bitumens.
[0072] The bitumen bases usable within the scope of the invention preferably have a penetrability, measured at 25°C according to standard EN 1426, of 5 to 330 1 / 10 mm, preferably between 10 and 220 1 / 10 mm, and more preferably between 10 and 120 1 / 10 mm. As is well known, the measurement known as "needle penetration" is carried out using a standardized test NF EN 1426 at 25°C (P25). This penetrability characteristic is expressed in tenths of a millimeter (dmm or 1 / 10 mm). The needle penetration, measured at 25°C according to the standardized test NF EN 1426, represents the measurement of the penetration, after 5 seconds, of a needle whose weight, including its support, is 100 g into a sample of bitumen.Preferably, the composition according to the invention comprises at least 50% by mass of bitumen, relative to the total mass of bitumen base(s), residue(s) and plastomer(s) present in the composition of the invention, preferably at least 60% by mass, more preferably at least 65% by mass, typically at least 70% by mass.
[0073] Advantageously, the composition according to the invention comprises from 50% to 94% by mass of bitumen, relative to the total mass of bitumen base(s), residue(s), and plastomer(s) present in the composition of the invention, preferably from 60% to 90% by mass, and more preferably from 70% to 85% by mass. Any fillers, additives, and fluxing agents are not included in these ranges.
[0074] Distillation residue
[0075] The bitumen / polymer composition of the invention further comprises at least one distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, in particular plastic waste.
[0076] Common industrial methods of recycling hydrocarbons from plastic include thermal conversion liquefaction of plastic waste that might otherwise have ended up in a landfill or incinerator, followed by a purification step including hydrotreatment and the removal of contaminants using a variety of purification processes such as distillation.
[0077] The liquefaction of plastic waste can be achieved through pyrolysis or hydrothermal treatment. The thermal conversion stage transforms plastics and most of their additives and contaminants into gaseous chemicals, while most non-volatile contaminants or additives end up in the solid by-product, such as charcoal or ash. In principle, all types of plastic waste can be converted. However, a preliminary step of sorting non-organic waste is advisable. Purification of the output material can also be beneficial, as several heteroatoms (i.e., elements other than carbon, hydrogen, or oxygen) can be volatilized.
[0078] Plastic waste is a complex and heterogeneous material due to several factors. First, the term "plastic" refers to many different polymers with varying chemical properties that can be separated before recycling or recycled as a complex mixture. The main polymers found in plastic from municipal solid waste are polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), and polystyrene (PS). Other polymers include polyurethanes, polyamides (PA), polycarbonates, polyethers, and polyesters other than PET. Furthermore, many different additives to the base polymers are introduced during the production phase to adjust or improve the plastic's properties or to meet specific requirements.These include functional additives (stabilizers, antistatic agents, flame retardants, plasticizers, lubricants, sliding agents, curing agents, foaming agents, biocides, antioxidants, etc.), colorants and pigments, fillers (e.g., glass fibers, talc, carbon fibers, carbon nanotubes), commonly used in plastic packaging, as well as additives such as flame retardants, frequently used in plastics for electronics. In addition, several metallic compounds are intentionally added during plastic production (often in the form of oxides, carbonates, acids, etc.). Additives containing heteroatoms other than metals are also used in plastics manufacturing, for example, halogens such as bromine in flame retardants, plasticizers, stabilizers, etc.
[0079] Silicone polymers, which are organic materials containing silicon, are often used in plastic formulations. Thanks to their surface characteristics, silicone applications range from silicone rubbers, used as sealants for joints, to silicone surfactants for cosmetic products, while they are increasingly used in the plastics sector as process-enhancing additives (manufacturing auxiliaries) and for polymer modification.
[0080] In addition to these heteroelements, used plastic waste may have been contaminated during its lifetime by traces of liquids it has come into contact with (beverages, personal care products, etc.) and food, which can also contaminate the plastic. Finally, some plastic waste may be present in the form of partially decomposed material, such as partially burned plastic.
[0081] Finally, since plastics are contaminated by oxygenated compounds, plastic oils resulting from pyrolysis liquefaction may also contain oxygenated compounds such as aldehydes or ketones.
[0082] The term "hydrocarbon product obtained by thermal conversion of waste" or simply "hydrocarbon product" refers, for the purposes of this invention, to liquid products obtained after thermal conversion, particularly after thermal pyrolysis, of plastic waste or plastic waste. The thermal conversion process, especially pyrolysis, should be understood as a non-selective thermal cracking process.
[0083] According to a preferred embodiment, the hydrocarbon product used for the preparation of the residue of the invention is obtained by pyrolysis of waste, in particular by pyrolysis of plastic waste.
[0084] The residue incorporated into the bituminous composition of the invention corresponds to the residue obtained from the distillation of the hydrocarbon product obtained by thermal conversion of plastic waste.
[0085] The residue incorporated into the bituminous composition of the invention can be obtained by direct distillation and / or by vacuum distillation of said hydrocarbon product. When obtained by atmospheric distillation, the residue of the invention simply corresponds to the residue of the distillation carried out at atmospheric temperature and pressure. A vacuum manufacturing process, on the other hand, consists of successive atmospheric distillations followed by vacuum distillations, the feedstock for the vacuum distillation corresponding to the residues obtained after the atmospheric distillation. Thus, when obtained by vacuum distillation, the residue of the invention corresponds to the residue obtained after the vacuum distillation process.
[0086] Preferably, the residue incorporated into the composition of the invention is a residue obtained by vacuum distillation of the hydrocarbon product defined above.
[0087] The residue of the invention typically exhibits a penetrability at 25°C, measured according to standard EN 1426, less than or equal to 200 1 / 10 mm.
[0088] Preferably, the residue of the invention has a penetrability at 25°C, measured according to standard EN 1426, greater than or equal to 20 1 / 10 mm, more preferably greater than or equal to 30 1 / 10 mm, even more preferably greater than or equal to 35 1 / 10 mm.
[0089] More preferably, the residue of the invention has a penetrability at 25°C, measured according to standard EN 1426, ranging from 20 to 200 1 / 10 mm, preferably from 25 to 150 1 / 10 mm, even more preferably from 30 to 120 1 / 10 mm.
[0090] Preferably, the residue of the invention has a ball and ring softening temperature (BRT), measured according to EN 1427, greater than or equal to 60°C, more preferably from 60°C to 120°C, typically from 65°C to 100°C. Preferably, the residue of the invention has a Cleveland flash point, measured according to ASTM D 92, greater than or equal to 150°C, more preferably greater than or equal to 200°C, typically from 200°C to 350°C, for example from 230°C to 340°C.
[0091] As is well known, distillation is carried out by gradually heating a substance. In the case of a pure compound, the entire product is distilled at a constant temperature. Conversely, in the case of a mixture, fractions with different boiling points are evaporated sequentially. These boiling points increase during the distillation process.
[0092] Preferably, the residue of the invention has an initial boiling temperature, measured according to ASTM D7169:20, less than or equal to 500°C, more preferably from 100°C to 500°C, more preferably from 200°C to 480°C.
[0093] Preferably, the residue of the invention has a distillation endpoint, measured according to ASTM D7169:20, of less than or equal to 1000°C, more preferably less than or equal to 900°C.
[0094] More preferably, the residue of the invention has a final boiling point, measured according to ASTM D7169:20, ranging from 150°C to 1000°C, more preferably from 200°C to 900°C.
[0095] For the purposes of this invention, "boiling point at X% of product Y" means the boiling point of the remaining portion of product Y once X% by mass of the starting product has been evaporated.
[0096] Preferably, the residue of the invention has a boiling point at 5% by mass, measured according to ASTM D7169:20, greater than or equal to 300°C, more preferably greater than or equal to 350°C, typically greater than or equal to 400°C.
[0097] Preferably, the residue of the invention has a boiling point at 5% by mass, measured according to ASTM D7169:20, less than or equal to 550°C, more preferably less than or equal to 500°C.
[0098] Preferably, the residue of the invention has a boiling point at 10% by mass, measured according to ASTM D7169:20, greater than or equal to 350°C, more preferably greater than or equal to 400°C, typically greater than or equal to 410°C.
[0099] Preferably, the residue of the invention has a boiling point at 10% by mass, measured according to ASTM D7169:20, less than or equal to 600°C, more preferably less than or equal to 550°C. Preferably, the residue of the invention has a boiling point at 15% by mass, measured according to ASTM D7169:20, greater than or equal to 380°C, more preferably greater than or equal to 400°C, typically greater than or equal to 430°C.
[0100] Preferably, the residue of the invention has a boiling point at 15% by mass, measured according to ASTM D7169:20, less than or equal to 600°C, more preferably less than or equal to 550°C.
[0101] Preferably, the residue of the invention has a boiling point at 30% by mass, measured according to ASTM D7169:20, greater than or equal to 400°C, more preferably greater than or equal to 430°C, typically greater than or equal to 450°C.
[0102] Preferably, the residue of the invention has a boiling point at 30% by mass, measured according to ASTM D7169:20, less than or equal to 650°C, more preferably less than or equal to 600°C.
[0103] Preferably, the residue of the invention has a boiling point at 50% by mass, measured according to ASTM D7169:20, greater than or equal to 450°C, more preferably greater than or equal to 460°C, typically greater than or equal to 470°C.
[0104] Preferably, the residue of the invention has a boiling point at 50% by mass, measured according to ASTM D7169:20, less than or equal to 700°C, more preferably less than or equal to 650°C.
[0105] Preferably, the residue of the invention has a boiling point at 70% by mass, measured according to ASTM D7169:20, greater than or equal to 450°C, more preferably greater than or equal to 500°C, typically greater than or equal to 510°C.
[0106] Preferably, the residue of the invention has a boiling point at 70% by mass, measured according to ASTM D7169:20, less than or equal to 750°C, more preferably less than or equal to 730°C.
[0107] Preferably, the residue of the invention has a boiling point at 80% by mass, measured according to ASTM D7169:20, greater than or equal to 475°C, more preferably greater than or equal to 500°C, typically greater than or equal to 510°C.
[0108] Preferably, the residue of the invention has a boiling point at 80% by mass, measured according to ASTM D7169:20, less than or equal to 775°C, more preferably less than or equal to 750°C. Preferably, the residue of the invention has a final boiling point (i.e. boiling point at 100% by mass), measured according to ASTM D7169:20, greater than or equal to 500°C, more preferably greater than or equal to 550°C, typically greater than or equal to 600°C.
[0109] According to one embodiment, the residue of the invention has a calcium (Ca) content greater than or equal to 1 ppm, more preferably greater than or equal to 1.5 ppm, typically ranging from 1 to 1000 ppm. The calcium content is typically determined by calcination of the material, followed by acidification of the resulting ash and analysis of the solutions by ICP-OES.
[0110] According to one embodiment, the residue of the invention has a phosphorus (P) content greater than or equal to 10 ppm, more preferably greater than or equal to 15 ppm, typically ranging from 10 to 200 ppm. The phosphorus content is typically determined by acid digestion in a closed microwave instrument due to its volatility. The resulting solution is then analyzed by ICP-OES under conventional acidic conditions.
[0111] According to one embodiment, the residue of the invention has a silicon (Si) content greater than or equal to 5 ppm, more preferably greater than or equal to 10 ppm, typically ranging from 10 to 750 ppm. The silicon content is typically determined by X-ray fluorescence (XRF) after homogenization of the material and appropriate calibration.
[0112] According to one embodiment, the residue of the invention has a chlorine (Cl) content greater than or equal to 10 ppm, more preferably greater than or equal to 20 ppm, typically ranging from 10 to 1500 ppm. The chlorine content is typically determined by ion chromatography coupled to a combustion system (C-IC) after appropriate calibration.
[0113] According to one embodiment, the residue of the invention has an initial melting temperature, measured by thermal analysis (DSC), during a second heating ramp between -80°C and 180°C at 10°C / min, greater than or equal to -40°C, preferably ranging from -35 to -5°C, even more preferably ranging from -25 to -10°C.
[0114] According to one embodiment, the residue of the invention has a final melting temperature, measured by thermal analysis (DSC), during a second heating ramp between -80°C and 180°C at 10°C / min, less than or equal to 110°C, preferably from 75 to 110°C, even more preferably from 80 to 110°C.
[0115] Advantageously, the composition of the invention has a hydrocarbon product distillation residue content, said hydrocarbon product having been obtained by thermal conversion of plastics, ranging from 0.1% by mass to 30% by mass, relative to the total mass of bitumen base(s), residue(s), and plastomer(s) present in the composition of the invention, preferably ranging from 1% to 25% by mass, more preferably from 5% to 20% by mass. Any fillers, additives, and fluxing agents are not included in these ranges.
[0116] Plastomer
[0117] The composition according to the invention further comprises at least one plastomer. Thus, the composition of the invention is a bitumen / polymer composition, in which the polymer is selected from among the plastomers. It may be crosslinked or non-crosslinked.
[0118] The use of plastomers is not particularly limited, provided they possess the required qualities for the final waterproofing membranes. Such plastomers are well-known in the field and are generally plastic polymers. They are notably described in the article "Polymer modification of bitumen: Advantages and challenges" by Jiqing Zhu et al., European Polymer Journal, 54 (2014) 18-38. Plastomers are therefore distinct from elastomers and do not include polymers such as SBS, SIS, or SEBS.
[0119] Preferably, the plastomer is chosen from polymers or copolymers comprising at least one ethylene motif, preferably chosen from the group consisting of isotactic polypropylene (IPP), atactic polypropylene (APP), amorphous poly-alpha-olefin polymers (APAO), thermoplastic polyolefins (TPO) and / or ethylene-vinyl acetate (EVAC).
[0120] Examples of plastomers include the following polymers: chlorosulfonyl polyethylene (CSM), ethylene ethyl acrylate (EEA), ethylene butyl acrylate (EBA), ethylene-ethylene-vinyl acetate copolymer (EVAC), flexible polyolefin (FPO or PO-F), flexible polypropylene (FPP or PP-F), polyethylene (PE), chlorinated polyethylene (PE-C), polyisobutylene (PIB), polypropylene (PP) and / or polyvinyl chloride (PVC), or polyolefin copolymers. Preferably, isotactic polypropylene (IPP), atactic polypropylene (APP), and / or thermoplastic polyolefins (TPO) are examples.
[0121] Preferably, the plastomer is chosen from olefinic plastic polymers, preferably comprising at least one propylene and / or ethylene motif.
[0122] In particular, the plastomer is chosen from polymers or copolymers comprising at least one ethylene unit, preferably chosen from the group consisting of isotactic polypropylene (IPP), atactic polypropylene (APP) and / or thermoplastic polyolefins (TPO). According to one embodiment, the plastomer is chosen from the group consisting of isotactic polypropylene, polyethylene / polypropylene copolymers and their mixtures.
[0123] According to one embodiment, the plastomer according to the invention is chosen from the group consisting of isotactic polypropylene, atactic polypropylene and / or amorphous poly-alpha-olefins.
[0124] According to one embodiment, the bitumen / polymer composition of the invention comprises isotactic polypropylene.
[0125] According to one embodiment, the bitumen / polymer composition of the invention comprises atactic polypropylene.
[0126] According to one embodiment, the bitumen / polymer composition of the invention comprises an amorphous poly-alpha-olefin.
[0127] According to one embodiment, the bitumen / polymer composition of the invention comprises isotactic polypropylene and at least one polyethylene / polypropylene copolymer.
[0128] The waterproofing membrane composition (optionally cross-linked) according to the invention preferably comprises from 5% to 40% by mass of plastomer(s), in particular isotactic polypropylene or polyethylene / polypropylene copolymer, relative to the total mass of bitumen base(s), residue(s), and plastomer(s) present in the composition of the invention. Any fillers, additives, and fluxing agents are not included in these ranges.
[0129] More preferably, the composition (optionally crosslinked) according to the invention comprises from 6% to 35% by mass of plastomer(s), relative to the total mass of bitumen base(s), residue(s), and plastomer(s) present in the composition of the invention, more preferably from 7% to 20% by mass, advantageously from 10% to 15% by mass. Any fillers, additives, and fluxing agents are not considered in these ranges.
[0130] Charges (optional)
[0131] According to one embodiment, the composition of the invention may further include fillers.
[0132] The fillers used in the composition of the present invention are typically mineral and / or organic fillers. Preferably, the fillers are chosen from calcium carbonate, volcanic rocks, silica, talc, dolomite, kaolin, carbon black, titanium dioxide, and mixtures thereof.
[0133] Recycled fillers can also be used (lignin, recycled fibers, polymer shreds, coke, cement shreds).
[0134] Preferably, when present, the sealing membrane composition (possibly cross-linked) according to the invention comprises 20% to 70% by mass of fillers, relative to the mass of the composition more preferably 40% to 55% by mass, even more preferably 45% to 55% by mass.
[0135] Additives
[0136] The composition of the present invention may optionally include one or more additive(s).
[0137] Examples of additives that can be added to said composition according to the invention are flame retardants such as borates or halogens, root inhibitors such as Preventol® B5, antioxidants, and rheological agents.
[0138] Preferably, the composition (possibly crosslinked) according to the invention comprises from 0% to 40% by mass of additives, relative to the mass of the (crosslinked) composition, more preferably from 1% to 30% by mass, even more preferably from 2.5% to 20% by mass.
[0139] Fluxing agent
[0140] The composition of the invention may further include at least one fluxing agent.
[0141] For the purposes of this invention, "fluxing agent" means a product introduced into the composition of the invention in order to lower its viscosity at the processing temperature.
[0142] A fluxing agent suitable for the invention is typically chosen from oils of natural, petroleum or synthetic origin, possibly recycled.
[0143] By "recycled fluxing agent" is meant of the invention a fluxing agent obtained by recycling used mineral oils, typically recycled motor oils.
[0144] Preferably, the fluxing agent is chosen from petroleum or synthetic oils, more preferably from aromatic oils.
[0145] Preferably, the composition of the invention (optionally crosslinked) comprises from 0% to 20% by mass of fluxing agent(s), relative to the mass of the (crosslinked) composition, more preferably from 1% to 15% by mass, and even more preferably from 2% to 8% by mass. Any fillers, additives, and fluxing agents are not considered in these ranges.
[0146] According to one embodiment, the composition according to the invention comprises, preferably consists essentially of, or even more preferably consists exclusively of:
[0147] - from 50% to 94% by mass of bitumen, preferably from 60% to 90% by mass, more preferably from 70% to 85% by mass;
[0148] - from 0.1% to 30% by mass of distillation residue(s) of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, preferably from 1% to 25% by mass, more preferably from 5% to 20% by mass; and
[0149] - from 5% to 40% by mass of plastomer(s), preferably from 6% to 35% by mass, more preferably from 7% to 20% by mass;
[0150] compared to the total mass of bitumen base(s), residue(s) and plastomer(s) present in the composition of the invention.
[0151] According to one embodiment, the composition according to the invention comprises, preferably consists essentially of, or even more preferably consists exclusively of:
[0152] - from 10% to 60% bitumen by mass,
[0153] - 0.1% to 30% by mass of distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, - 0.1% to 30% by mass of plastomer,
[0154] - from 0% to 70% fillers and / or additives, and
[0155] - from 0% to 20% by mass of a fluxing agent,
[0156] relative to the total mass of the composition.
[0157] Advantageously, the composition according to the invention comprises, preferably consists essentially of, or even more preferably consists exclusively of:
[0158] - 20% to 50% bitumen by mass,
[0159] - 1% to 25% by mass of distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, - 0.5% to 20% by mass of polymer,
[0160] - 10% to 55% fillers and / or additives,
[0161] - from 1% to 15% by mass of a fluxing agent,
[0162] relative to the total mass of the composition. More advantageously, the composition according to the invention comprises, preferably consists essentially of, or even more preferably consists exclusively of:
[0163] - 30% to 40% bitumen by mass,
[0164] - 5% to 20% by mass of distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, - 1% to 10% by mass of polymer,
[0165] - from 2% to 55% fillers and / or additives, and
[0166] - 2% to 8% by mass of a fluxing agent,
[0167] relative to the total mass of the composition.
[0168] Even more advantageously, the composition according to the invention comprises, preferably consists essentially of, or even more preferably consists exclusively of:
[0169] - 30% to 40% bitumen by mass,
[0170] - 5% to 20% by mass of distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, - 3% to 10% by mass of polymer,
[0171] - 45% to 55% fillers and / or additives, and
[0172] - from 2.5% to 7.5% by mass of a fluxing agent,
[0173] relative to the total mass of the composition.
[0174] The waterproofing membrane composition according to the invention is homogeneous. By "homogeneous," it is understood, for the purposes of the invention, that the various components of the composition, namely the residue from the pyrolysis distillation of plastic and any polymers and / or additives, are distributed uniformly in the bituminous matrix.
[0175] According to one embodiment, the sealing membrane composition according to the invention has a penetration at 50°C, measured according to standard EN 1426, ranging from 50 to 200 1 / 10 mm, more preferably from 75 to 150 1 / 10 mm, typically 80 to 120 1 / 10 mm.
[0176] According to one embodiment, the sealing membrane composition according to the invention has a ball and ring softening temperature, measured according to standard EN 1427, greater than 80°C, more preferably greater than or equal to 100°C, advantageously ranging from 90°C to 150°C, typically ranging from 100°C to 130°C.
[0177] According to one embodiment, the composition according to the invention exhibits a dynamic viscosity at 170°C and at 10 s -1, measured on an AntonPaar type rheometer (MCR102) equipped with a peltier furnace and a plan / plane geometry, less than or equal to 25 Pa.s, more preferably less than or equal to 20 Pa.s, advantageously ranging from 1 Pa.s to 15 Pa.s, typically ranging from 4 Pa.s to 17 Pa.s.
[0178] According to one embodiment, the composition according to the invention exhibits improved cold pliability or flexibility, measured according to the UEAtc guide, in particular a lower cracking temperature, compared to the same composition free of distillation residue.
[0179] Preferably, the composition according to the invention has a cold pliability or flexibility, measured according to the UEAtc guide, of less than or equal to 0°C, more preferably less than or equal to -10°C, even more preferably less than or equal to -20°C, typically ranging from -30°C to -15°C, advantageously from -25°C to -20°C.
[0180] According to one embodiment, the composition of the invention comprises a significant proportion of recycled or waste-derived materials. It can therefore exhibit a high eco-material index. The eco-material index is defined by the following equation:
[0181] Eco-material index = 100% - [% of non-bio-based, non-biodegradable, non-recycled or non-waste-derived materials].
[0182] According to one embodiment, the composition has an eco-material content of at least 1% by mass, preferably at least 5% by mass, preferably at least 10% by mass, and more preferably at least 15% by mass, relative to the total mass of the composition of the invention.
[0183] Applications
[0184] The invention also relates to a method for preparing a bitumen / polymer composition as defined above, said method comprising mixing at least:
[0185] - a bitumen base,
[0186] - a distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics,
[0187] - a plastomer,
[0188] - possibly, fillers and / or additives, and
[0189] - possibly, a fluxing agent.
[0190] Preferably, the mixing step is carried out at a temperature ranging from 90°C to 230°C, more preferably from 120°C to 200°C, even more preferably from 150°C to 190°C. The invention also relates to the use of a bitumen / polymer composition according to the invention for the preparation of a sealing and / or soundproofing material.
[0191] Preferably, the sealing and / or soundproofing material is chosen from: a sealing membrane, a liquid coating, an adhesive, a primer and a soundproofing membrane.
[0192] In particular, the invention relates to the use of a composition according to the invention for the manufacture of a waterproofing membrane. The invention also relates to a waterproofing membrane prepared from a composition according to the invention.
[0193] More particularly, the invention relates to a prefabricated waterproofing membrane comprising a support (or reinforcement) coated on at least one face with a composition according to the invention.
[0194] According to one embodiment, the support or reinforcement consists of one or more fibrous or non-fibrous reinforcements.
[0195] Preferably, according to this embodiment, the fibrous or non-fibrous reinforcement(s) are impregnated throughout with said composition.
[0196] The invention also relates to a method for manufacturing a sealing membrane, said method comprising the following successive steps:
[0197] 1) the preparation of a composition according to the invention, preferably according to the preparation process defined above,
[0198] 2) the application of said composition on at least one face of a support or reinforcement, in particular on one or more fibrous reinforcement(s).
[0199] Preferably, step 2) of applying the composition to the support or reinforcement is carried out under heating and agitation, preferably at a temperature ranging from 90°C to 230°C, more preferably from 120°C to 200°C, even more preferably from 150°C to 190°C.
[0200] According to one embodiment, the support or reinforcement consists of fibrous or non-fibrous reinforcement(s).
[0201] Preferably, according to this embodiment, step 2) consists of a step of impregnating said reinforcements throughout with said composition.
[0202] The invention also relates to the use of a composition according to the invention for the manufacture of a liquid coating. The invention also relates to a liquid coating prepared from a composition according to the invention.
[0203] The invention also relates to a method for preparing a liquid coating according to the invention, the method comprising the following successive steps: a) mixing a composition according to the invention with a solvent, so as to obtain a diluted composition; and
[0204] b) the addition to the diluted composition obtained in a), preferably under stirring, of a polyurethane precursor.
[0205] Preferably, step b) is carried out in a vacuum disperser.
[0206] The invention also relates to the use of a composition according to the invention for the manufacture of an adhesive. The invention also relates to an adhesive prepared from a composition according to the invention.
[0207] The invention also relates to a method for preparing an adhesive according to the invention, the method comprising the following successive steps:
[0208] 1. Mixing at least one plastomer and at least one solvent in a vat; 2. Adding a bituminous composition according to the invention to the mixture obtained in 1); and
[0209] 3. the addition to the mixture obtained in 2) of at least one thixotropic filler. Preferably, steps 1) and / or 2) and / or 3), more preferably steps 1), 2) and 3), are carried out in a paddle mixer at temperatures between 50°C and 110°C.
[0210] The invention also relates to the use of a composition according to the invention for the manufacture of a primer. The invention also relates to a primer prepared from a composition according to the invention.
[0211] The invention also relates to a method for preparing a primer according to the invention, the method comprising the following successive steps:
[0212] 1. Mixing in a vat at least one plastomer and at least one solvent; 2. Adding to the mixture obtained in 1) a bituminous composition according to the invention.
[0213] Preferably, step 1) and / or step 2, more preferably steps 1) and 2), are carried out in a disperser at temperatures between 50 and 110°C.
[0214] The invention also relates to the use of a composition according to the invention for the manufacture of a soundproofing membrane. The invention also relates to a soundproofing membrane prepared from a composition according to the invention.
[0215] More particularly, the invention relates to a prefabricated soundproofing membrane comprising a support (or reinforcement) coated on at least one side with a composition according to the invention.
[0216] According to one embodiment, the support or reinforcement consists of one or more fibrous or non-fibrous reinforcements. The invention also relates to a method for manufacturing a soundproofing membrane, said method comprising the following successive steps:
[0217] 1) the preparation of a composition according to the invention, preferably according to the preparation process defined above,
[0218] 2) the application of said composition on at least one face of a support or reinforcement, in particular on one or more fibrous reinforcement(s).
[0219] Preferably, step 2) of applying the composition to the support or reinforcement is carried out under heating and agitation, preferably at a temperature ranging from 90°C to 230°C, more preferably from 120°C to 200°C, even more preferably from 150°C to 190°C.
[0220] According to one embodiment, the support or reinforcement consists of fibrous or non-fibrous reinforcement(s).
[0221] The invention also relates to the use of a distillation residue of a hydrocarbon product as defined above, in a bitumen / polymer composition intended for use in the preparation of sealing and / or soundproofing materials, to reduce the content of fossil-based compounds in said bituminous composition, the polymer being selected from plastomers. In particular, the invention relates to the use of a distillation residue of a hydrocarbon product as defined above, in a bitumen / polymer composition to reduce the content of bitumen and / or plastomer and / or petroleum- or synthetic-derived fluxing agent in said composition.
[0222] More particularly, the invention relates to the use of a distillation residue of a hydrocarbon product as defined above, in a bitumen / polymer composition in order to reduce the bitumen content in said composition by at least 5%, preferably from 8% to 20%, even more preferably from 9% to 15%.
[0223] More particularly, the invention relates to the use of a distillation residue of a hydrocarbon product as defined above, in a bitumen / polymer composition in order to reduce the plastomer(s) content in said composition by at least 5%, preferably from 8% to 12%, even more preferably from 9% to 11%.
[0224] In the case where the composition of the invention includes one or more fluxing agent(s) of petroleum or synthetic origin, the invention also relates to the use of a distillation residue of a hydrocarbon product as defined above, in a bitumen / polymer composition in order to reduce by at least 10% the content of fluxing agent(s) of petroleum or synthetic origin in said composition, preferably by at least 30%, more preferably by at least 50%, typically by 30% to 70%, even more preferably by 40% to 60%.
[0225] The invention further relates to the use in a bitumen / polymer composition intended for use in the preparation of sealing and / or soundproofing materials of at least one distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, in order to reduce the carbon footprint of said composition.
[0226] The "carbon footprint" of a product, as defined in this invention, refers to the amount of carbon (generally expressed in kg of CO2 equivalent per kg of product) required to produce said product. This amount of carbon equivalent takes into account both energy consumption, particularly related to heating, and the consumption of raw materials. A product's carbon footprint is typically determined according to either ISO 14040 or ISO 14044.
[0227] The invention is advantageous in that it enables the supply of sealing and / or soundproofing materials, particularly sealing membranes, with a reduced carbon footprint. The invention is also advantageous in that the binder composition used to prepare the various materials exhibits improved resistance to aging: the variation in pliability during aging is significantly reduced compared to a residue-free composition. Furthermore, this stability of pliability during aging is achieved without degrading the softening temperature of the composition. The invention is also advantageous in that it allows, at a constant plastomer content, the preparation of bituminous compositions with increased pliability. The invention is further advantageous in that it allows, at constant mechanical properties, a reduction in the plastomer content in the composition.
[0228] The invention is illustrated by the following examples, which are given by way of non-limiting example. EXAMPLES
[0229] In the examples below, and unless explicitly instructed otherwise, percentages are expressed by mass, relative to the total mass of the compositions.
[0230] 1. Materials and methods
[0231] 1.1. Measurement Methods
[0232] In the description and examples below, the following methods were used.
[0233] Ball-and-Ring Temperature (BRT) or Softening Temperature. The BRT (or softening temperature) is measured according to standard NF EN 1427, June 2007. The material to be tested is placed in brass rings. The rings are placed in a BRT measuring apparatus (ball-and-ring type apparatus). A metal ball is placed on the surface of the rings, which are heated until the ball passes through the ring. The temperature at which the ball passes through is the BRT.
[0234] Needle penetration at 50°C (Penetration)
[0235] Penetration is measured according to standard NF EN 1426, 20 December 1999. The material to be tested is stored at 50°C for 2 hours and the penetration into the sample is measured, after a time of 5 seconds, using a needle penetrometer, of a needle with a tip diameter of 0.14 to 0.16 mm and a weight including its holder of 100 g. Penetration is expressed in tenths of a mm.
[0236] Cold flexibility or flexibility
[0237] Bendability is measured according to the UEAtc guide. A 2 mm thick specimen is formed using a film puller. The specimen's susceptibility to cracking under bending at low temperatures is determined. The lowest temperature at which the specimen can be bent around a 30 mm diameter mandrel is thus found.
[0238] Viscosity at 170°C
[0239] The viscosity at 170°C (V170) is measured on an Anton-Paar MCR102 rheometer equipped with a Peltier oven and a planar / planar geometry. The bituminous composition is first placed in an oven at 170°C for 30 minutes and then deposited between the rheometer platform and the upper 25 mm diameter planar geometry. A viscosity measurement is performed over a shear range of 0.1 to 100 s⁻¹. 1The overall shape of the curve is taken into consideration, but the viscosity value at 10s -1 is taken as the reference value.
[0240] 1.2. Raw materials
[0241] Bituminous compositions were prepared from the following raw materials:
[0242] - Bitumen base B1 exhibiting a penetration at 25°C, measured according to standard NF EN 1426, equal to 86 1 / 10 mm, and a ball and ring softening temperature (BRT), measured according to standard NF EN 1427, equal to 45.8°C; commercially available from TotalEnergies under the reference AZALT® 70-100;
[0243] - Distillation residue R1;
[0244] - Plastomer P1: Isotactic polypropylene type polymer, name SlIMPOL IPP MF-10, from the supplier POLYMER TEAM;
[0245] - P2 Plastomer: Propylene-based olefinic elastomer polymer of the polyethylene / polypropylene copolymer type, comprising 15% by mass of ethylene (name Vistamaxx 6202, from supplier EXXON MOBIL);
[0246] - Fluxant: oil derived from the recycling of used petroleum oils and obtained by vacuum distillation thereof, commercially available under the name 700SR from the company ECO HUILE;
[0247] - Fillers: mixture consisting of at least 90% by mass of calcium carbonate and of which at least 90% by mass of particles have a particle size of less than 100pm, commercially available from Omya under the name Etanchcarb® P2.
[0248] The physical characteristics of the distillation residue R1 are given in the following table 1:
[0249] [Table 1]
[0250] P25 (in 1 / 10 mm) 61
[0251] TBA (in °C) 82.7
[0252] Flashpoint 278
[0253] T eb (ini) 288.0
[0254] T e b (5%) 378.0
[0255] Teb (10%) 432.0
[0256] Teb (15%) 458.0
[0257] Teb (30%) 503.0
[0258]
[0259] Teb (50%) 549.0
[0260] Teb (70%) 605.0
[0261] Teb (80%) 667.0
[0262] Teb (final) >738.0
[0263] Ca content 669
[0264] P content 56
[0265] Silicon content 286
[0266] Cl content 377
[0267] Broadcast -18
[0268] TFfusion 94
[0269]
[0270] 2. Preparation of bituminous membrane compositions
[0271] Bituminous compositions C1 and C2 were prepared according to the protocol defined below:
[0272] The bitumen or the previously prepared bitumen / residue mixture is placed in an oven at 185°C for approximately one hour, then placed on a hot plate at 190-200°C. The fluxing agent is then added. Under constant stirring with a propeller blade, the plastomer(s) are gradually added, and stirring is maintained for approximately 40-45 minutes, with the rate of stirring gradually increased. Once the plastomers are mixed with the bitumen, the heating is stopped, and the compositions are then characterized.
[0273] An additional step of adding fluxing agent and fillers under stirring was also carried out, after the introduction of the plastomers.
[0274] [Table 2]
[0275] C1 C2
[0276] (invention) (comparative)
[0277] Bitumen B1 (in %) 43.2 48
[0278] Residue R1 (in %) 4.8 - Plastomer P1 (in %) 7 7
[0279] Plastomer P2 (in %) 8 8
[0280] Fluxant (in %) 7 7
[0281] Charges (in %) 30 30
[0282]
[0283] The physicochemical properties of the C1 and C2 sealing membrane compositions were evaluated according to the protocols detailed above. The results are reported in Table 3 below.
[0284] [Table 3]
[0285] C1 C2
[0286] (invention) (comparative)
[0287] TBA (°C) 156 158
[0288] P60 (1 / 10 mm) 78 67
[0289] Foldableness (°C) -10 -2
[0290] Foldable, 28 days, 80°C -6 8
[0291] V180 (Pa.s) 77 8.3
[0292]
[0293] Comparing the composition according to the invention C1 (with residue) to the comparative composition C2 (without residue), it is observed that the presence of residue R1, replacing a portion of the bitumen, significantly improves the cold pliability of the bituminous mixture in its new state while maintaining all its properties. The viscosity is also slightly reduced, which is advantageous for the application. Furthermore, the presence of the residue ensures very good stability of the material during aging.
[0294] Here we see that the delta of loss of flexibility at cold for the composition according to the invention between new state and aging is only 4 degrees and remains below 0°C, while the comparative composition breaks at positive temperature (delta of 10°C)
Claims
DEMANDS 1. Bitumen / polymer composition comprising: - at least one bitumen base, - at least one distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by thermal conversion of plastics, - 5% to 40% by mass of at least one plastomer, and compared to the total mass of plastomer(s), bitumen base(s) and distillation residue(s).
2. Composition according to claim 1, wherein said residue is an atmospheric distillation residue of a hydrocarbon product, said hydrocarbon product having been obtained by pyrolysis of plastic waste.
3. Composition according to claim 1 or according to claim 2, wherein said residue has a boiling point at 10% by mass, measured according to ASTM D7169:20, greater than or equal to 350°C, preferably from 400°C to 600°C, typically from 410°C to 550°C.
4. Composition according to any one of the preceding claims, wherein said residue has a ball and ring softening temperature (BRT), measured according to EN 1427, greater than or equal to 60°C, more preferably from 60°C to 120°C, typically from 65°C to 100°C.
5. Composition according to any one of the preceding claims, wherein the plastomer is selected from polymers or copolymers comprising at least one ethylene motif, preferably selected from the group consisting of isotactic polypropylene (IPP), atactic polypropylene (APP), poly alpha olefin polymers (APAO), thermoplastic polyolefins (TPO) and / or ethylene-vinyl acetate (EVAC).
6. A composition according to any one of the preceding claims, wherein the plastomer is selected from the group consisting of isotactic polypropylene, atactic polypropylene, and / or amorphous poly-alpha-olefins.
7. A composition according to any one of the preceding claims, comprising: - from 10% to 90% bitumen by mass, - from 0.1% to 30% by mass of said at least one distillation residue, - 5% to 40% by mass of plastomer(s), - from 0% to 70% fillers / or additives, and - from 0% to 20% by mass of fluxing agent(s), relative to the total mass of the composition.
8. Use of a bitumen / polymer composition according to any one of claims 1 to 7, for the manufacture of a sealing and / or soundproofing material, preferably selected from: a sealing membrane, a liquid coating, an adhesive, a primer and a soundproofing membrane.
9. Prefabricated waterproofing membrane comprising: - a support or reinforcement, in particular one or more fibrous reinforcements, - a bitumen / polymer composition according to any one of claims 1 to 7, said support or reinforcement being coated on at least one side, preferably impregnated throughout, with said bituminous composition.
10. A method for manufacturing a sealing membrane according to claim 9, said method comprising the following successive steps: 1) the supply of a bitumen / polymer composition according to any one of claims 1 to 7, 2) the application of the composition obtained in step 1) on at least one face of a support or reinforcement.