Composition for the sealing and coating of edges and / or bevels of material panels

An aqueous silane-based sealant with hydrophobic and hydrophilic properties addresses water penetration issues in laminate flooring, ensuring effective protection and compatibility with high-speed production, reducing swelling and environmental impact.

WO2026238667A1PCT designated stage Publication Date: 2026-11-19FLOORING TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063647
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-11
Publication Date
2026-11-19

Smart Images

  • Figure EP2026063647_19112026_PF_FP_ABST
    Figure EP2026063647_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a composition for the sealing and coating of joining edges of support panels, comprising at least one compound of the general formula (I) R1SiX3, where X is alkoxy, aryloxy, or acyloxy and R1 is an organic moiety selected from the group comprising C5 - C25 alkyl, and at least one compound of the general formula (II) R2 2SiX2, where X is alkoxy, aryloxy, or acyloxy and R2 is a non-hydrolyzable organic moiety R2 selected from the group comprising C1-C4 alkyl.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Composition for sealing and coating edges and / or chamfers of material panels

[0002] The present invention relates to a composition for coating and sealing edges and / or chamfers of material panels, in particular wood-based panels, the production of this composition and wood-based panels with this composition.

[0003] Description

[0004] Floor panels with tongue-and-groove profiles on the sides, designed for installation in panel systems such as laminate flooring, are widely used and commonplace. The tongue-and-groove profiles allow for easy installation of the floor panels over the floor coverings. These floor coverings can be made of materials such as wood fiberboard, particleboard, or plastic panels. Most floor panels feature a decorative layer and an abrasion-resistant surface layer.

[0005] These tongue-and-groove profiles feature a tongue (or tongue) with a (first) joining surface located above the tongue on one side edge, and a groove with a lip and a (second) joining surface on a second side edge. When the panels are installed, the tongue and groove are inserted or clicked into place, resulting in contact between the first and second joining surfaces. However, this design creates a gap on the top side of the joined panels, particularly at the contact points of the joining surfaces on the two opposing side edges of two joined floor panels. This gap allows moisture and dirt to penetrate between the floor panels.

[0006] To reduce water penetration at the contact points of the tongue-and-groove profiles, modern click profiles also feature a rebate in the area of ​​the joining edge. A rebate is understood to be a step, an edge, or a fold.

[0007] Laminate flooring with so-called V-grooves has also proven very popular. A V-groove is created when the edges of the wood panels are chamfered or beveled. These chamfers are angled cuts on the side edges that, when the floor panels are joined, form a V-shaped joint. The joint serves to enhance the visual appearance of individual panels and create a visual separation between them. However, a problem with V-grooves is that moisture can accumulate in the joint and penetrate the gap between the panels.

[0008] Laminate flooring with so-called pressed joints has also become established. A pressed joint is created when the edges of the panels are shaped in the press during the coating process, resulting in a chamfer or radius with a continuous coating. These chamfers or radii are formed during the formatting process so that they create a V-shaped or arc-shaped joint on the side edges when the floor panels are joined. The joint formation serves to enhance the visual appearance of individual panels and create a visual separation between them. However, a problem with chamfered or rounded joints is that moisture can accumulate in the joint and penetrate the gap between the panels.

[0009] However, all these panel connection methods still offer insufficient protection against water penetration at the joint or contact point. This is because, in these products, water (e.g., during cleaning) is drawn into the profile area through the fine gaps or cracks between the floor panels via capillary action, causing swelling. To test for this problem, the so-called NALFA test was developed and is now standardized in DIN EN ISO 4760. In this test, a defined quantity of water is applied to the joint area of ​​three laid plank sections. After a defined test period (24 hours), it is analyzed whether water is still present on the surface, whether water has penetrated the profile, whether it has reached the underside through the profile, and whether there is clearly visible and measurable swelling of the planks.

[0010] To mitigate moisture damage, various strategies are currently employed, either individually or in combination. The simplest way to hinder moisture penetration into the profile is to achieve the tightest possible fit in the tongue and groove joint. However, this can lead to difficulties in joining the elements or to damage occurring during installation. This method also has the disadvantage that if water penetrates the tongue and groove area, the wood-based substrate will swell as usual. Another option is to seal the profile with water-repellent agents. For example, WO 2006 / 038867 describes the use of waxes for coating the edges, whereby at least partial penetration of the wax into the wood-based material is observed. EP 903451 A2 describes the use of diphenylmethane diisocyanate for treating the edges, which readily penetrates the wood-based material.In WO 2008 / 078181 A1, a fluorinated polymer, e.g., perfluoroalkyl methacrylate copolymer, is used as a coating agent, with the film-forming material being solid at room temperature. The disadvantage of these sealants is that they often migrate into the wood substrate during application, thus minimizing the hydrophobic effect. This can also occur subsequently, so the effect is gradually lost with use. Furthermore, perfluoro compounds are considered critical from an environmental perspective.

[0011] Other edge sealants are based on mixtures of various substituted silanes. For example, WO 2020 / 016176 A1 describes a composition of hydrophobic and hydrophilic silanes in combination with a polymer dispersion for sealing the edges of wood-based panels. The silane-containing composition described in WO 2024 / 121003 A1 additionally contains beveling compound suitable for sealing bevels and joints. The composition described in WO 2024 / 170287 A1 contains a swelling agent in addition to the silanes and the polymer dispersion. The aforementioned silane-containing compositions are aqueous systems whose viscosity and flowability can be specifically adjusted by adding polymer dispersion, swelling agent, and, if necessary, beveling compound. However, it has been shown that these compositions are only suitable for limited use in high-speed production lines.

[0012] The present invention was therefore based on the objective of overcoming the aforementioned disadvantages. In particular, the invention was based on the technical objective of providing an edge sealant that both seals the edge and chamfer area against water and simultaneously dries quickly, thus enabling application in high-speed production lines.

[0013] This problem is solved according to the invention by a composition with the features of claim 1. Accordingly, an aqueous composition for sealing and coating joint edges or joint surfaces of carrier boards, in particular for use in floor panels, is provided, wherein the composition comprises the following:

[0014] at least one compound of the general formula (I)

[0015] R 1 SiX3(I),

[0016] where

[0017] - X is alkoxy, aryloxy, acyloxy, and

[0018] - R 1 An organic residue is selected from the group comprising Cs-C25 alkyl, and

[0019] - at least one compound of the general formula (II)

[0020] R 2 2SiX2(II),

[0021] where

[0022] - X is alkoxy, aryloxy, acyloxy, and

[0023] - R 2 a non-hydrolyzable organic residue R 2 is selected from the group comprising C1-C4 alkyl.

[0024] A fast-drying, water-clear composition is thus provided as an edge sealant, with which laminate floors made from carrier boards edge-coated with this composition are reliably protected against the penetration of water (ISO 4760 or NALFA test); these floors are laid floating as so-called click laminate floors.

[0025] For the purposes of the present invention, an aqueous composition is understood to be one that is preferably in the form of an aqueous suspension. In one embodiment, the aqueous suspension contains, in addition to water, an organic solvent, in particular a water-miscible organic solvent. The organic solvent is preferably a solvent with a flash point below 30°C, more preferably below 25°C, and particularly preferably below 20°C. Suitable organic solvents are methanol, ethanol, propanol, such as isopropanol or n-propanol, with propanol being particularly preferred. It should be noted that the organic solvent is added during the preparation of the composition (ex-situ) or is formed in the reaction mixture during the preparation of the composition by hydrolysis of the starting materials (in situ).The weight percentage of propanol in the final composition can be between 5 and 20 wt%, preferably between 10 and 15 wt%. For example, it has been shown that using propanol results in rapid drying of the sealant after application to the joint edges of the substrate.

[0026] The use of solvents with a flash point above 30°C is therefore expressly prohibited. Thus, the use of higher alcohols or ethers, such as dipropylene glycol alkyl ethers, e.g., dipropylene glycol methyl ether, is not permitted.

[0027] A key advantage of this composition is that it contains no separable phases, meaning it is neither a dispersion nor an emulsion. This simplifies processing and application.

[0028] The effect of this composition can be achieved for a wide variety of locking profiles. This composition is applied in particular to the joint edges or surfaces of profile surfaces, chamfers of side edges and / or V-joints of carrier panels, especially for floor panels.

[0029] As described, the present composition is suitable for sealing joint surfaces or joint edges. For the purposes of the present invention, joint surfaces are understood to be the pair of surfaces on which the joined panels support each other in order to form a closed (flat) upper surface of the connected and locked panels. Accordingly, the technical term "joining surface" encompasses the section of the side edges that are actually pressed together. The joint surfaces lie directly against each other to close the surface. The first and second joint surfaces run parallel to each other simultaneously, so that in the assembled state of the floor panels, the joint surfaces lie against each other and are in contact with each other along their entire surface.

[0030] In a preferred embodiment, the present composition is suitable for sealing vertical joining edges, wherein the vertical joining edges can be part of a painted or unpainted V-joint. The compound of general formula (I) used in the present composition exhibits hydrophobic properties due to the longer-chain substituent, while the compound of general formula (II) has more hydrophilic properties due to the shorter-chain substituent.

[0031] The hydrophobic component of formula (I) - formed, for example, from the alkyl groups of the residue R 1- forms a water-repellent barrier. In this way, water cannot diffuse through the network of the formed coating. The hydrophilic component of formula (II) enables, firstly, the bonding of the compound to the wood fibers, particularly via the free -OH groups (existing or formed by hydrolysis of, for example, alkoxy groups), and secondly, the formation of a network.

[0032] Surprisingly, it has also been shown that the use of long-chain alkylated silanes of formula (I) eliminates the need for the (often common) use of phenyl-containing silanes as the hydrophobic component. While phenyl-containing silanes, such as phenyltrimethoxysilane (PTMS), exhibit significantly higher thermal stability and are cost-effective, their hydrophobic properties are considerably less pronounced than those of long-chain alkylated silanes of formula (I), such as hexadecyltrimethoxysilane. For example, contact angles in compositions with phenyltrimethoxysilane (PTMS) as the main component for hydrophobizing wood fiberboards can reach a maximum of 92°, whereas samples with solutions containing hexadecyltrimethoxysilane as the main component for hydrophobizing wood fiberboards achieve contact angles of over 125°.These results were particularly surprising when used with wood fiberboards, since, due to the lignin components of the wood, a stronger interaction of the aromatic rings in the lignin with a phenyl group (and thus an increased hydrophobic effect) would have been expected than with a long-chain alkyl group. Accordingly, the addition of phenyl-containing silanes, such as phenyltrimethoxysilane (PMTS), is avoided.

[0033] Preferably, the present composition is free of agents that increase viscosity. In particular, the composition is free of polymers (with the exception of polyorganosiloxanes) and / or swelling agents. The present composition is also free of dyes, e.g., free of chamfering dye, which can commonly contain color pigments such as carbon black, iron oxides, titanium dioxide, and / or organic pigments.

[0034] This composition can be used with any panel and adhesive system. It reduces swelling in wood fiberboards regardless of the adhesive system used, porosity, or panel thickness. The swelling-reducing effect of this composition has been demonstrated in HDF (high-density fiberboard) and particleboard bonded with urea-formaldehyde (UF) adhesive, melamine-urea-formaldehyde (MUF) adhesive, or polyurethane-based (PMDI) adhesive.

[0035] The composition according to the invention offers several advantages. It results in significantly less swelling of the edges, does not penetrate or migrate into the panels, can be used with any panel and adhesive system, and requires only relatively small application quantities. Furthermore, the composition can be applied to the joining edges of the narrow sides of the substrate panels in a high-speed system (up to 350 m / min).

[0036] In one embodiment, the present composition contains at least two compounds of general formula (I) and at least one compound of general formula (II); i.e., the composition comprises

[0037] at least two compounds of the general formula (I)

[0038] R 1 SiX3(I),

[0039] where

[0040] - X is alkoxy, aryloxy, acyloxy, and

[0041] - R 1 An organic residue is selected from the group comprising Cs-C25 alkyl, and

[0042] - at least one compound of the general formula (II)

[0043] R 2 2SIX2(II),

[0044] where

[0045] - X is alkoxy, aryloxy, acyloxy, and

[0046] - R 2 a non-hydrolyzable organic residue R 2 The residue X is selected from the group comprising C1-C4 alkyls. The residue X is advantageously selected from the group comprising Ci-6-alkoxy, in particular methoxy, ethoxy, n-propoxy and butoxy, Ce-w aryloxy, in particular phenoxy, C2-7-acyloxy, in particular acetoxy or propionoxy. The residue X methoxy or ethoxy is particularly preferred.

[0047] The non-hydrolyzable organic R 1The compound of general formula (I) is preferably selected from a group comprising C5-C2o-alkyl, in particular Ce-C -alkyl, in particular preferably C3-Ci6-alkyl, preferably Octyl, Nonyl, Decyl, Undecyl, Dodecyl Tridecyl, Tetradecyl, Pentadecyl, Hexadecyl, in particular preferably Octyl and Hexadecyl.

[0048] Furthermore, the remainder R 1 are present substituted with further hydrophobic residues.

[0049] In the context of the present invention, the term “non-hydrolyzable organic residue” means an organic residue which, in the presence of water, does not lead to the formation of an OH group or NH2 group linked to the Si atom.

[0050] In a preferred embodiment, the compound of formula (I) comprises one of the following variants:

[0051] - R 1 SiX3 with R 1as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, e.g. octyltriethoxysilane, or

[0052] - R 1 SiX3 with R 1 as C14-C18 alkyl group, preferably tetradecyl, pentadecyl, hexadecyl and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, e.g. hexadecyltrimethoxysilane.

[0053] In a preferred embodiment, the present composition comprises each

[0054] - a silane compound of formula R 1 SiX3 with R 1 as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, e.g. octyltriethoxysilane, and

[0055] - a silane compound of formula R 1 SiX3 with R 1as a C14-C18 alkyl group, preferably tetradecyl, pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, e.g. hexadecyltrimethoxysilane. The non-hydrolyzable organic R 2 The compound of general formula (II) is selected from a group comprising Ci-Cs-alkyl, preferably methyl, ethyl, n-propyl, isopropyl. These may be unsubstituted, like the residue R1, or substituted with a further, preferably hydrophilic, group.

[0056] In a preferred embodiment, the compound of formula (II) comprises one of the following variants:

[0057] - R 2 2SiX2 with R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, e.g. dimethyldimethoxysilane.

[0058] In one variant, the composition may contain octyltriethoxysilane and hexadecyltrimethoxysilane as compounds of formula (I) and dimethyldimethoxysilane as compounds of formula (II).

[0059] In a further embodiment, the compounds of general formula (I) are included in the composition in a molar amount between 0.08 - 0.2 mol, preferably 0.1 - 0.15 mol, particularly preferably 0.1-0.12 mol, and the compound of general formula (II) is included in a molar amount between 0.05 and 0.1 mol, preferably between 0.06 and 0.09 mol, particularly preferably between 0.07 and 0.08 mol.

[0060] The range of molar quantity specified for the compound of the general compound (I) can refer to a single compound or to the sum of two compounds of the general formula (I).

[0061] The ratio of the silane compounds of formula (I) to the silane compound of formula (II) is preferably between 1 : 0.5 and 1 : 2, particularly preferably between 1 : 0.75 and 1 : 1.5, most preferably between 1 : 1 and 1 : 1.2.

[0062] In a further embodiment, the present composition comprises at least one compound of general formula (III)

[0063] R 3 SiX3(III), wherein

[0064] - X as defined above, preferably methoxy and ethoxy, and - R 3 an organic residue is selected from the group comprising C1-C10 alkyls, which may be interrupted by -O- or -NH-, and

[0065] - where R 3 has at least one functional group Qi selected from a group containing an isocyanate, methacrylic, methacryloxy, vinyl, and epoxy group.

[0066] The silane compound of formula (III) has at least one functional group, such as an isocyanate or glycidyl group, for chemical bonding to free OH groups of the cellulose on the edge surface. This enables rapid crosslinking and setting of the sealant on the edge surface of the wood-based panel; penetration or displacement of the sealant into the side edge of the wood-based panel is reduced or prevented.

[0067] The organic R 3 The compound of general formula (III) is preferably selected from a group comprising methyl, ethyl, propyl, pentyl, hexyl, heptyl, octyl, which may be interrupted by -O- or -NH-. The organic R 3 The compound of general formula (III) preferably consists of methyl, ethyl, or propyl.

[0068] The functional group Q 1Advantageously, it comprises a residue with a double bond or an epoxy group that can be activated and polymerized by UV radiation. Isocyanate, vinyl, and epoxy groups are preferred as the functional group Q. 1 A particularly preferred functional group Q 1 is isocyanate.

[0069] In a preferred embodiment, the compound of formula (III) comprises one of the following variants:

[0070] R 3 SiXsmit R 3 as a C1-C3 alkyl group functionalized with Q1, wherein Q1 is an isocyanate, vinyl, and epoxide group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0071] In another preferred embodiment, the compound of formula (III) comprises one of the following variants:

[0072] R 3 SiXs with R 3as a C1-C3 alkyl group functionally fused with Q1, wherein Q1 is an isocyanate group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0073] Particularly preferred are the compounds trimethoxy(3-isocyanatopropyl)silane and triethoxy(3-isocyanatopropyl)silane as compounds of general formula (III).

[0074] In a further embodiment, the present composition comprises at least one alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and with R 3 = C1-C5 alkyl, especially C2, C3 or C4 alkyl. The alkyl metal compound serves as a condensation catalyst, which undergoes hydrolysis during the reaction, resulting in the release of the corresponding low molecular weight alcohol, such as ethanol or propanol.

[0075] In one embodiment, at least one alkyl titanium compound of the general formula Ti(OR) can be used. 3 )4 with R 3C1-C5 alkyl, in particular C2, C3 or C4 alkyl, may be used. The use of titanium tetrabutanoate (or titanium n-butoxide) is particularly preferred.

[0076] The use of at least one alkylzirconium compound of the general formula Zr(OR) is also preferred. 3 )4 with R 3 = C1-C5 alkyl, in particular C2, C3 or C4 alkyl. The use of zirconium tetraisopropylate (or tetrapropylzirconate) is particularly preferred.

[0077] The ratio of the alkyl metal compound to the silane compounds of formula (I), (II) and optionally (III) is 1 : 30, preferably 1 : 25.

[0078] In a further embodiment, the present composition can contain inorganic particles, in particular SiO₂, Al₂O₃, ZrO₂, and TiO₂ particles, and preferably SiC₂ particles, e.g., as nanoparticles. The particles preferably used have a size between 2 and 400 nm, preferably between 2 and 100 nm, and particularly preferably between 2 and 50 nm. The nanoscale SiO₂ particles are preferably used in the form of aerosils, in particular hydrophobically modified aerosils, such as Aerosil R 819 or Aerosil R 812.

[0079] The addition of inorganic particles increases the solids content of the composition, thereby improving its application properties. The addition of inorganic particles also prevents shrinkage and cracking. The inorganic particles can be used in a quantity range of 0.1 to 25 wt%, preferably 5 to 20 wt%, based on the solids content of the silane material (sol-gel material).

[0080] The present composition can thus exist in one embodiment in the following combination:

[0081] - R 1 SiX3 with R 1 as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and / or

[0082] - R 1 SiX3 with R 1 as a C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0083] - R 2 2SiX3mit R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0084] - at least one alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and R 3 = C1-C5 alkyl, especially C2, C3 or C4, and

[0085] - SiO2 particles.

[0086] A particularly preferred variant of the present composition comprises octyltriethoxysilane and hexadecyltrimethoxysilane as compound of formula (I) and dimethyldimethoxysilane as compound of formula (II) and SiO2 particles.

[0087] In another embodiment, the present composition may have the following combinations:

[0088] - R 1 SiX3 with R 1as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and / or

[0089] - R 1 SiX3 with R 1 as a C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0090] - R 2 2SiX2 with R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0091] R 3 SiX3 with R 3 as a C1-C3 alkyl group functionalized with Q1, wherein Q1 is an isocyanate, vinyl, and epoxide group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, at least an alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and R 3 = C1-C5 alkyl, especially C2, C3 or C4, and

[0092] - SiO2 particles.

[0093] Another particularly preferred variant of the present composition comprises octyltriethoxysilane and hexadecyltrimethoxysilane as compound of formula (I), dimethyldimethoxysilane as compound of formula (II), triethoxy(3-isocyanatopropyl)silane as compound of general formula (III) and SiO2 particles.

[0094] In another embodiment, the present composition may contain at least one polyorganosiloxane. Preferably, polydimethylsiloxane (PDMS) of the general formula (CH3)3SiO[(CH3)2SiO]nSi(CH3)3 is used, which is added to the composition as an aqueous silicone dispersion.

[0095] Therefore, the present composition can also have the following combinations:

[0096] - R 1 SiX3 with R 1as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and / or

[0097] - R 1 SiX3 with R 1 as a C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0098] - R 2 2SiX3mit R 2 as a C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0099] - at least one alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and R 3 = C1-C5 alkyl, especially C2, C3 or C4, and

[0100] - at least one polyorganosiloxane.

[0101] Another particularly preferred variant of the present composition comprises octyltriethoxysilane and hexadecyltrimethoxysilane as compound of formula (I) and dimethyldimethoxysilane as compound of formula (II) and at least one polyorganosiloxane.

[0102] In another embodiment, the present composition may have the following combinations:- R 1 SiX3 with R 1 as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and / or

[0103] - R 1 SiX3 with R 1 as a C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0104] - R 2 2SiX3mit R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0105] R 3 SiX3 with R 3 as a C1-C3 alkyl group functionalized with Q1, wherein Q1 is an isocyanate, vinyl, and epoxide group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0106] at least one alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and R 3 = C1-C5 alkyl, in particular C2, C3 or C4, and at least one polyorganosiloxane.

[0107] In a further particularly preferred embodiment, the present composition can have the following combinations:

[0108] - R 1 SiX3 with R 1 as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and / or

[0109] - R 1 SiX3 with R 1as a C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and

[0110] - R 2 2SiX2 with R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0111] R 3 SiX3 with R 3 as a C1-C3 alkyl group functionalized with Q1, wherein Q1 is an isocyanate group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy,

[0112] at least one alkyl metal compound of the general formula Ti(OR 3 )4 with R 3 = C1-C5 alkyl, especially C2, C3 or C4,

[0113] - at least one polyorganosiloxane, and

[0114] - SiO2 particles. A particularly preferred variant of the present composition comprises octyltriethoxysilane and hexadecyltrimethoxysilane as compound of formula (I), dimethyldimethoxysilane as compound of formula (II), triethoxy(3-isocyanatopropyl)silane as compound of general formula (III) and at least one polyorganosiloxane.

[0115] The present composition can be produced according to a first embodiment in a process comprising the following steps:

[0116] -Providing a mixture of at least one silane compound of general formula (I), preferably at least two silane compounds of general formula (I), and at least one silane compound of general formula (ii);

[0117] Addition of at least one catalyst, in particular an acid, to the mixture of at least one silane compound of formula (I) and at least one silane compound of formula (II) and heating of the mixture;

[0118] - optional addition of a water-isopropanol mixture to the mixture, - separation of the alcohols formed during the hydrolysis of the silane compounds, in particular methanol and / or ethanol,

[0119] - Addition of at least one alkyl metal compound of the general formula M(OR 3 )4ZU the mixture, and

[0120] - optional addition of at least one silane compound of general formula (III),

[0121] As already mentioned, the alkyl metal compound undergoes hydrolysis during the reaction, resulting in the in situ release of the corresponding low-molecular-weight alcohol, such as propanol. The weight fraction of propanol in the final composition can thus be between 5 and 20 wt%, preferably between 10 and 15 wt% (based on the total amount of the composition).

[0122] Due to their low boiling point and flash point, these alcohols released by hydrolysis evaporate quickly after the composition is applied to the joining edges of the substrate.

[0123] If a water-isopropanol mixture is added to the mixture, the ratio of water to isopropanol is 10:90, particularly 20:80, and most preferably 30:70. As also described above, inorganic particles, such as SiC>2 particles, and / or a polyorganosiloxane can be added to the mixture during the process. In a particularly preferred embodiment, inorganic particles, such as SiO2 particles, or a polyorganosiloxane are added.

[0124] In the case that inorganic particles are added to the composition, the inorganic particles are preferably used in an amount between 0.1 and 10 wt%, preferably 0.5 and 5 wt%, and particularly preferably between 1 and 3 wt%. In this embodiment, a water-isopropanol mixture can be added during the manufacturing process.

[0125] In the case that polyorganosiloxane is added to the composition, the polyorganosiloxane is preferably used in an amount between 5 and 30 wt%, preferably 10 to 30 wt%, and particularly preferably between 20 and 30 wt% (based on the total amount of the composition).

[0126] When polyorganosiloxane is added, the addition of isopropanol or a water-isopropanol mixture during production can be omitted. This is particularly possible when tetrapropyl zirconate is used as the alkyl metal compound.

[0127] Suitable inorganic and / or organic acids as catalysts are selected from a group containing phosphoric acid, acetic acid, p-toluenesulfonic acid, hydrochloric acid, formic acid, or sulfuric acid. Ammonium salts such as ammonium sulfate, which react as weak acids, are also suitable. p-Toluenesulfonic acid is particularly preferred.

[0128] As mentioned above, this composition can be used for coating or sealing the joint edges of substrate panels. The joint edges can be straight edges or sealed and / or already coated V-joints or chamfers.

[0129] The object of the present invention is therefore also achieved by a carrier board whose edges are coated with the present composition. Suitable carrier boards are wood-based panels, in particular WPC (wood-plastic composite), plywood, particleboard, OSB (oriented strand board), HDF (high-density fiberboard), or MDF (medium-density fiberboard). However, carrier boards made of plastic or mineral fiber, such as SPC (stone polymer composite), gypsum plasterboard, or cement fiberboard, can also be considered. Particleboard and HDF are particularly preferred wood-based panels.

[0130] Wood-based panels, such as particleboard and fiberboard (e.g., MDF and HDF), are manufactured from wood chips or fibers obtained by chipping wood in a chipper or by fiberizing wood chips in a refiner. The wood fibers used in fiberboard have a length between 1.5 mm and 20 mm and a thickness between 0.05 mm and 1 mm. The size of the wood chips used in particleboard depends on whether they are used in the face or core layer. In the core layer, the chips start at a particle size greater than 0.125 mm, while in the face layer, they start at 0.8–1.0 mm.

[0131] The wood-based panels in question can incorporate various binder systems, which are mixed and pressed together with the wood fibers. Preferred binder systems include: formaldehyde resins, such as urea-formaldehyde resins, melamine-formaldehyde resins, and melamine-urea-formaldehyde resins; polyurethanes, preferably based on polydiphenylmethane diisocyanate (PMDI), epoxy resin, or polyester resins.

[0132] The composition can be applied to the joint edges, profiles and / or chamfers of the wood-based panel, e.g. by spraying, rolling or using a vacuum device, and then dried (air drying or thermal drying).

[0133] The speed of a corresponding production unit, i.e., a unit for applying a sealing agent to a side edge, can be between 200 and 400 m / min, preferably between 250 and 380 m / min, and particularly preferably between 300 and 350 m / min. In a preferred embodiment, the speed of the unit is up to 350 m / min in the longitudinal direction and up to 50 m / min in the transverse direction.

[0134] The width of the side edge to be coated with the sealant is between 2.5 and 3.5 mm, preferably 3 mm. In one embodiment, the at least one sealant has a solids content between 30 and 100 wt%, preferably between 50 and 100 wt%, and particularly between 70 and 100 wt%. The sealant is preferably in the form of a suspension, particularly an aqueous suspension. In a preferred embodiment, aqueous suspensions with a solids content of 50–70 wt% and an aqueous component of 30–50 wt% are used. The aqueous component (or aqueous solvent component) can comprise water and isopropanol.

[0135] In a further embodiment, the at least one sealing agent is applied to the side edge in an amount between 0.5 g / lfm and 3.0 g fl / lfm (liquid / linear meter), preferably between 1.0 and 2.5 g fl / lfm, particularly preferably between 1.5 and 2.3 g fl / lfm, e.g. preferably 2.0 g fl / lfm.

[0136] The layer thickness of the composition on the plate edge and / or chamfer can be in a range between 10 and 50 pm, preferably between 20 and 40 pm.

[0137] When used as flooring panels, the carrier boards are fitted with a tongue-and-groove locking system and used for floating installation. Various locking systems can be used, allowing the panels to be installed using the following mechanisms:

[0138] • angle-snap (angle in lengthwise and horizontally, snap together crosswise)

[0139] • angle-angle (angles longitudinally and transversely)

[0140] • angle-fold down (angle in lengthwise and lower across)

[0141] Angle-fold down locking systems have proven to be the preferred choice, offering simple and secure installation. These systems are particularly well-known under the trade names 5G (Välinge) and UDX (Illinilin). Both systems feature a specific tongue-and-groove structure in the side edges, with the 5G system incorporating an additional plastic component inserted into the groove. The UDX system does not include this additional plastic component.

[0142] As shown in the exemplary embodiments, these locking systems (without additional sealing) do not provide protection against water ingress. The 5G system, in particular, is especially susceptible in this regard. If the sealant provided is applied to the side edges before locking, water ingress along the locking line is stopped, and effective protection against water penetration is achieved.

[0143] A corresponding installation method includes laying a first floor panel and attaching a second floor panel to the first floor panel, whereby the tongue of the second floor panel is inserted into the groove of the first floor panel.

[0144] The invention is explained in more detail below with reference to exemplary embodiments.

[0145] Exemplary embodiment 1: Production of a first variant of the composition V3 (S-1 3N) according to the invention

[0146] 12.4 g oxytriethoxysilane

[0147] 3.7 g dimethoxydimethylsilane

[0148] 6.9 g hexadecyltrimethoxysilane

[0149] The mixture is placed in a container and heated to 40 °C. Then, 4.57 g of H₂O and 1.3 g of H₂SO₄ (37%) are added, and the mixture is stirred for a further 60 minutes at 40 °C. Next, 14.48 g of a water-isopropanol mixture are added, and the alcohol (ethanol or methanol) produced during hydrolysis is removed using a rotary evaporator. Finally, 4.5 g of tetrapropyl zirconate and 1.2 g of nanoscale silicon dioxide (e.g., Aerosil R819) are added while stirring at room temperature.

[0150] Exemplary embodiment 2: Production of a second variant of the composition V5 (S-26) according to the invention

[0151] 12.4 g oxytriethoxysilane

[0152] 3.7 g dimethoxydimethylsilane

[0153] 6.9 g hexadecyltrimethoxysilane

[0154] The mixture is placed in a container and heated to 40 °C. Then, 4.57 g of H₂O and 1.3 g of H₂SO₄ (37%) are added, and the mixture is stirred for a further 60 minutes at 40 °C. Next, 28.49 g of an aqueous silicone dispersion (e.g., Korasilon TXP) are added, and the alcohol (ethanol or methanol) produced during hydrolysis is removed using a rotary evaporator. Finally, 4.5 g of tetrapropyl zirconate is added while stirring at room temperature.

[0155] Application example 3: Production of a third variant of the composition V6 (S26i) according to the invention

[0156] 12.4 g oxytriethoxysilane

[0157] 3.7 g dimethoxydimethylsilane

[0158] 6.9 g hexadecyltrimethoxysilane

[0159] The mixture is placed in a container and heated to 40 °C. Then, 4.57 g of H₂O and 1.3 g of H₂SO₄ (37%) are added, and the mixture is stirred for a further 60 minutes at 40 °C. Subsequently, 28.49 g of an aqueous silicone dispersion (e.g., Korasilon TXP) and 1.42 g of isopropanol are added, and the alcohol (ethanol or methanol) produced during hydrolysis is removed using a rotary evaporator.

[0160] In a further step, the following is added:

[0161] 3.2 g titanium n-butyrate

[0162] 2.27 g Aerosil 819

[0163] 1.67 g triethoxy(3-isocyanatopropyl)silane.

[0164] Example 4: HDF board

[0165] The joining edges of an 8 mm HDF with a density of approximately 850 kg / m³ 3, which had been produced with a urea-formaldehyde adhesive in a conventional quantity, are each coated with a composition according to the invention V3 (according to embodiment 1), V5 (according to embodiment 2) and V6 (according to embodiment 3) in a system with a coating speed of up to 350m / min longitudinally, up to 50m / min transversely by means of spraying, rolling, transfer, vacuum processes and an application quantity of up to 2g / linear meter edge and subsequently air-dried (thermal drying is also possible).

[0166] The edge-sealed HDF panels (V3, V5, V6) are then joined together and subjected to a NALFA test (DIN EN ISO 4760). Unsealed HDF panels are used as the control sample (V0). Ten test specimens of each variant were produced and tested. The results of the NALFA test are summarized in Table 1 below:

[0167] Water variant description

[0168] cycle

[0169] VO 10 10 of 10 completed, no source values

[0170] V3 0 10 out of 10 tight and below 0.1 mm

[0171] swelling

[0172] V5 0 10 out of 10 tight and below 0.2 mm

[0173] swelling

[0174] V6 0 10 out of 10 tight and below 0.1 mm

[0175] swelling

[0176]

[0177] Table 1

[0178] The tests show a clear difference between the untreated panels (VO) and those with edge-sealed panels (V3, V5, or V6). The treated panels passed the NALFA test 100%, both with the maximum required swelling values ​​of < 0.3 mm and without any water seeping through the joint. Each variant was tested with 10 specimens.

[0179] Example 5: Chipboard

[0180] The joining edges of an 8 mm chipboard were each coated with a composition according to the invention V3 (according to embodiment 1) and V6 (according to embodiment 3) in a system with a coating speed of up to 350m / min longitudinally, up to 50m / min transversely by means of spraying, rolling, transfer, vacuum processes and an application quantity of up to 2g / linear meter of edge and subsequently air-dried (thermal drying also possible).

[0181] Four samples of the edge-sealed particleboard (V3) were then joined together and subjected to a NALFA test (DIN EN ISO 4760). Unsealed HDF boards were used as the control sample (V0). The results of the NALFA test are summarized in Table 2 below:

[0182] Duration V0-1 V3-1 V3-2 V3-3 V3-4 V6-1 V6-2 Oh aborted dry dry dry dry dry dry 18.75h X dry dry dry dry dry dry 48h X dry dry dry dry dry dry dry 72h X dry dry dry dry dry dry 144h X dry dry dry dry dry dry 240h X dry dry dry dry dry

[0183]

[0184] The tests show a clear difference between the untreated panels (V0) and those with edge-sealed finishes (V3 and V6). The treated panels passed the NALFA test 100%, requiring that no water seep through the joint. Since the untreated sample emptied immediately after filling, only the treated version was tested with four test specimens. Swelling values ​​were not measured, but visual inspection revealed no abnormalities.

[0185] Example 6: HDF and chipboard, each with different locking systems

[0186] The joint edges of an 8 mm chipboard and an 8 mm HDF with a density of approximately 850 kg / m³ 3 , were each coated with the compositions V3 (according to embodiment 1) and V5 (according to embodiment 2) according to the invention. The coated panels were then joined together using the locking systems 5G (designed under license from Välinge) and UDX (designed under license from Unilin).

[0187] The test setup was then carried out in the SKDE laboratory in accordance with ISO 4760. Unsealed HDF boards and particleboard were used as control samples (V0). The results of the NALFA test are summarized in Table 3 below: Substrate | Interlock | Seal | Water | Swell value | Swell value after medium run-through | after 24 h | 48 h and re-drying | HDF 5G | VO (none) | Yes | 1.06 | 1.04

[0188] HDF 5G VO (none) Yes 0.97 0.90

[0189] HDF 5G V3 No 0.34 0.09

[0190] HDF 5G V3 No 0.32 0.15

[0191] HDF 5G V3 No 0.20 0.10

[0192] HDF 5G V5 No 0.16 0.05

[0193] HDF 5G V5 No 0.18 0.08

[0194] HDF 5G V5 No 0.18 0.11

[0195] HDF 5G V5 No 0.20 0.09

[0196] Chipboard 5G VO (none) Yes 0.93 0.79

[0197] Chipboard 5G V3 No 0.26 0.12

[0198] Chipboard 5G V3 No 0.27 0.01 Chipboard 5G V3 No 0.41 0.13

[0199] Chipboard 5G V5 No 0.32 0.22

[0200] Chipboard 5G V5 No 0.28 0.23

[0201] Chipboard 5G V5 No 0.38 0.23

[0202] Chipboard UDX VO (none) Low 0.40 0.17

[0203] Chipboard UDX V5 No 0.27 0.07

[0204] Chipboard UDX V5 No 0.28 0.11

[0205]

[0206] Table 3

[0207] As shown in the embodiments in Table 3, the 5G locking system, without additional sealing, provides no protection against water penetration in the case of HDFA and particleboard. If the sealant V3 or V5 is applied to the side edges of the HDFA or particleboard before locking, no water penetration along the locking line is detectable, thus providing effective protection against water ingress. In the case of the IIDX locking system, only a small amount of water penetration is observed; however, the application of the sealant V5 also improves edge swelling in this case.

[0208] The results listed in Table 3 are illustrated in the diagrams in Figures 1 and 2. The diagram in Figure 1 shows the source values ​​(and their mean) after 24 hours for the measured samples.

[0209] The diagram in Figure 2 shows the swelling values ​​(and their mean value) after 48 hours and drying for the measured samples. It can be seen that the swelling of all samples treated with the sealant is below the standard-required 0.3 mm.

Claims

Claims 1. Composition for sealing and coating joint edges of at least one carrier board comprising at least one compound of the general formula (I) R 1 SiX3(I), where - X is alkoxy, aryloxy, acyloxy, and - R 1 An organic residue is selected from the group comprising Cs-C25 alkyl, and - at least one compound of the general formula (II) R 2 2SiX2(II), where - X is alkoxy, aryloxy, acyloxy, - R 2 a non-hydrolyzable organic residue R 2 is selected from the group comprising C1-C4 alkyl.

2. Composition according to claim 1, characterized in that it contains at least two compounds of general formula (I) and at least one compound of general formula (II).

3. Composition according to one of the preceding claims, characterized in that X is selected from a group comprising Ci-6-alkoxy, in particular methoxy, ethoxy, n-propoxy and butoxy, Ce-w aryloxy, in particular phenoxy, C2-7-acyloxy, in particular acetoxy or propionoxy.

4. Composition according to one of the preceding claims, characterized in that the non-hydrolyzable organic R 1 The compound is selected from a group comprising C5-C2o-alkyl, in particular Ce-C alkyl, in particular preferably Cs-C alkyl, preferably octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, in particular preferably octyl and hexadecyl.

5. Composition according to one of the preceding claims, characterized in that the compound of formula (I) comprises one of the following formulas - R 1 SiX3 with R 1as a C6-C12 alkyl group, preferably hexyl, heptyl, octyl, nonyl, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, and -R 1 SiX3 with R 1 as C14-C18 alkyl group, preferably pentadecyl, hexadecyl and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy.

6. Composition according to one of the preceding claims, characterized in that the non-hydrolyzable organic R 2 selected from a group comprising Ci-C3-alkyl, preferably Methyl, Ethyl, n-Propyl, Isopropyl.

7. Composition according to one of the preceding claims, characterized in that the compound of formula (II) comprises one of the following formulas: - R 2 2SiX3mit R 2 as C1-C3 alkyl group, preferably methyl, ethyl, n-propyl, isopropyl, and with X as alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy.

8. Composition according to one of the preceding claims characterized by at least one compound of the general formula (III) R 3 SiX3(III), where - X as defined above, and - R 3 an organic residue is selected from the group comprising C1-C10 alkyls, which may be interrupted by -O- or -NH-, and - where R 3 has at least one functional group Qi selected from a group containing an isocyanate, methacrylic, methacryloxy, vinyl, and epoxy group.

9. Composition according to claim 8, characterized in that it contains at least two compounds of general formula (I), at least one compound of general formula (II) and at least one compound of general formula (III).

10. Composition according to one of claims 8-9, characterized in that the compound of formula (III) comprises one of the following formulas: R 3 SiXsmit R 3 as a C1-C3 alkyl group functionalized with Q1, wherein Q1 is an isocyanate, vinyl, and epoxide group, and with X as an alkoxy, in particular methoxy, ethoxy, n-propoxy or i-propoxy, 11. Composition according to one of the preceding claims, characterized by at least one alkyl metal compound of the general formula M(OR 3 )4 with M = Zr or Ti and with R3 = C1-C5 alkyl, in particular C2, C3 or C4 alkyl.

12. Composition according to one of the preceding claims, characterized in that it may contain inorganic particles, in particular SiC>2-, Al2O3-, ZrÜ2-, TiC>2- particles, preferably in particular SiO2 particles.

13. Composition according to one of the preceding claims, characterized in that it contains at least one polyorganosiloxane.

14. A method for producing a composition according to any of the preceding claims comprising the following steps: -Providing a mixture of at least one silane compound of general formula (I), preferably at least two silane compounds of general formula (I), and at least one silane compound of general formula (ii); Addition of at least one catalyst, in particular an acid, to the mixture of at least one silane compound of formula (I) and at least one silane compound of formula (II) and heating of the mixture; - optional addition of a water-isopropanol mixture to the mixture, - separation of the alcohols formed during the hydrolysis of the silane compounds, in particular methanol and / or ethanol, - Addition of at least one alkyl metal compound of the general formula M(OR 3 )4 TO the mixture, and-optionally adding at least one silane compound of formula (III).

15. The method according to claim 14, characterized by the addition of inorganic particles and / or a polyorganosiloxane.

16. Carrier plate comprising at least one composition applied to an edge and / or chamfer, in particular to a joining edge, according to one of claims 1 to 13.

17. Carrier board according to claim 16, characterized in that the carrier board is a wood-based panel, in particular WPC (Wood-Plastic-Composite), plywood, particleboard, OSB (Oriented Strand Board), HDF (High Density Fiber) or MDF (Middle Density Fiber) panel.