Impeller comprising at least one blade

The impeller design with a foundation layer and WAAM-built blades addresses manufacturing inefficiencies and repair challenges, providing a robust, efficient, and cost-effective solution for turbomachines with reduced downtime and improved mechanical properties.

WO2026238686A1PCT designated stage Publication Date: 2026-11-19HOWDEN TURBO GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-11
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional manufacturing methods for impellers in turbomachines are material-intensive, costly, and time-consuming, and the reuse and repair of worn impellers are challenging due to issues with gap dimensions, imbalances, and mechanical weaknesses, leading to potential turbomachine failure and lengthy downtimes.

Method used

The impeller design features a foundation layer applied directly to a hyperbolic or rotationally symmetric blank, with blade superstructure layers built using Wire Arc Additive Manufacturing (WAAM) to ensure a robust connection, optimized geometry, and uniform stress distribution, reducing material consumption and production time.

Benefits of technology

This approach results in a cost-effective, quickly manufactured impeller with precise dimensions and improved structural integrity, minimizing downtime and extending service life by ensuring a strong, balanced connection between the base and blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063691_19112026_PF_FP_ABST
    Figure EP2026063691_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to an impeller (1) for a continuously operating turbine engine, comprising a main body (2) and at least one blade (3), wherein the main body (2) comprises a blank (10) and at least one base layer (11). The blank (10) takes the form of an axially symmetrical rotational body having a hyperbolic contour. The blade (3) has a blade thickness (4), a blade length (5) and a blade height (6), wherein the blade (3) is built up from a plurality of blade build-up layers (12) based on the main body (2) and has a built-up height which corresponds to the blade height (6). The base layer (11) is arranged directly on the blank (10).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PCT patent application

[0002] Howden V744

[0003]

[0004] Wheel with at least one blade

[0005] Description

[0006] The invention relates to an impeller for a continuously operating turbomachine with a base body and at least one blade, wherein the base body comprises a blank and at least one foundation layer, wherein the blank is designed as an axially symmetric body of revolution with a hyperbolic contour, wherein the blade has a blade thickness, a blade length and a blade height, wherein the blade is constructed from a plurality of blade superstructure layers based on the base body and has a superstructure height that corresponds to the blade height.

[0007] Industrial compressors are essential machines for compressing gases and play a central role in numerous industries, such as the chemical, oil and gas, energy production, and aerospace sectors. They operate according to different principles, with positive displacement and flow compressors being the most common.

[0008] Flow compressors are essential components in industrial applications where large volumes of gas need to be compressed with high efficiency. Unlike positive displacement compressors, they operate on the principle of fluid mechanics, transferring the kinetic energy of a rotating impeller to the gas and converting it into pressure energy through diffusion.

[0009] Impellers of turbomachinery are subjected to extreme mechanical loads in industrial applications and must simultaneously guarantee high efficiency. Their complex geometry, especially the design of the impeller blades and hub, is the result of fluid dynamic optimization. PCT - Patent application

[0010] Howden

[0011] V744

[0012] 2

[0013]

[0014] Conventional manufacturing methods for impellers present significant challenges. Manufacturing blades from solid metal blocks through machining is material-intensive and costly, as a large portion of the raw material must be removed. Furthermore, this approach requires an enormous amount of time.

[0015] In previous practice, rotor blades were often formed from sheet metal by bending and then joined to the main body by multiple caterpillar welds. However, this method presents problems with regard to the blade attachment, especially at the blade root, where material fatigue and structural weaknesses can occur.

[0016] Disclosure WO 2019 / 226463 A1 describes methods, devices, systems and / or software for three-dimensional (3D) printing for the production of one or more three-dimensional objects, including: an improved printing speed, the use of an energy beam with targeted alignment, the use of an energy beam directed at a target surface and / or the respective alignment of several energy beams to each other and / or in relation to a target surface.

[0017] EP 3251 787 A1 discloses a method for manufacturing a component of a rotary machine, wherein the component has at least one internal channel extending from a center to a boundary surface of the component and is at least partially closed, wherein a blank is provided comprising the boundary surface and a cover surface, wherein a first subtractive machining step is carried out in which a part of the channel is produced by machining, which has at least one opening of the channel into the boundary surface. PCT - Patent Application

[0018] Howden

[0019] V744

[0020] 3

[0021]

[0022] The component includes a recess in the cover surface, and the channel is subsequently finished on the blank using a build-up manufacturing process. Furthermore, a component manufactured using this method is proposed.

[0023] DE 102022 123029 A1 relates to a method for manufacturing an impeller of a turbomachine, comprising a base body and at least one impeller blade, wherein the base body and the impeller blade are materially bonded and wherein at least the following steps are carried out, preferably in the specified order: machining a blank formed from solid material to generate a first subsection of the base body, applying at least one layer of material to the first subsection of the base body to generate at least a second subsection of the base body in sections by applying an additive manufacturing process, applying at least one layer of material to the first subsection and / or the second subsection to generate at least one impeller blade on the base body in sections by applying an additive manufacturing process.

[0024] A promising approach for maintenance and repair is the reuse of old impeller bodies for continuously operating turbomachines using modern additive manufacturing processes. While conventional manufacturing processes involve long lead times for spare parts, this repair process enables significantly faster availability.

[0025] Until now, the reuse and repair of wheels that have already been in use and show signs of wear and tear represented a significant PCT patent application.

[0026] Howden

[0027] V744

[0028] 4

[0029]

[0030] This presents a technical challenge, particularly due to the problematic gap dimensions and the potential for imbalances.

[0031] The gap between the impeller and the housing of the turbomachine is crucial for the turbomachine's energy efficiency. If the gap is too large, short-circuit flows and undesirable turbulence occur. If the gap is too small, contact can occur between rotating and stationary components, potentially leading to total turbomachine failure.

[0032] Since an impeller in a turbomachine rotates at high speeds, even slight deviations in geometry lead to uneven mass distributions, which can cause unwanted vibrations, increased wear and in the worst case to premature failure of the component.

[0033] Particularly problematic is the combination with conventional caterpillar welding, which is used for reattaching or repairing buckets. This method not only creates additional heat distortions, which further complicate precise dimensional accuracy, but also results in mechanically weaker bucket connections that often cannot withstand the enormous centrifugal forces encountered during operation.

[0034] Due to these technical limitations, impeller replacement was generally avoided, even when it would have been economically advantageous. Instead, operators of turbomachinery often have to accept waiting times of several months for completely new impellers, which is not only costly but also results in significant downtime for the affected systems. PCT - Patent Application

[0035] Howden

[0036] V744

[0037] 5

[0038]

[0039] The object of the invention is to provide an impeller for a continuously operating turbomachine in which a robust connection between the base and the blades can be ensured. The impeller should be available with very precise dimensions, even in the event of repairs. Furthermore, the impeller should be manufactured as quickly as possible to avoid lengthy downtimes of systems using continuously operating turbomachines. The impeller should be characterized by cost-effective manufacturing and a long service life.

[0040] This problem is solved according to the invention by an impeller for a continuously operating turbomachine according to the features of claim 1 and a method and use according to the dependent main claims. Preferred embodiments can be found in the dependent claims, the description and the figures.

[0041] According to the invention, the foundation layer is arranged directly on the blank.

[0042] If the blades of impellers for continuously operating turbomachinery are worn or damaged, the impeller can be repaired according to the invention by removing the damaged blades from the base body and mounting new blades with optimized connection and defined transition layers in the form of a foundation layer and blade superstructure layers directly onto the existing base body. This not only improves the structural integrity of the connection but also significantly reduces material consumption and production time. PCT - Patent Application

[0043] Howden

[0044] V744

[0045] 6

[0046]

[0047] After the blades are removed, the base body has smaller dimensions than before and is then called a blank. This smaller size is achieved by grinding down the old blade tips.

[0048] Alternatively, the blank can also be used as a newly forged component, for example if the old base body can no longer be used.

[0049] In the present invention, the blank is designed as an axially symmetric body of revolution with a hyperbolic contour.

[0050] An axially symmetric shape means that the component can be mirrored around a central axis, so that the geometry is identical on both sides of the axis.

[0051] A hyperbolic contour refers to a shape that follows a hyperbola, enabling optimized flow guidance. This geometry is used in particular to reduce pressure losses in the flow and maximize the efficiency of the turbomachine.

[0052] As an alternative to the hyperbolic contour, the blank can also be designed as a rotationally symmetric body with a parabolic or conical contour, depending on the specific requirements of the respective application.

[0053] The foundation layer is a layer of material applied directly to the blank, serving as a transition zone between the solid base body and the additively manufactured blades. This layer ensures an improved mechanical connection between the blank and the blades. - PCT patent application

[0054] Howden

[0055] V744

[0056] 7

[0057]

[0058] applied blade structure layers and enables a uniform stress distribution.

[0059] The foundation layer acts as a metallurgically and mechanically coordinated transition layer between the blank and the blade superstructure layers, providing both a graded structural transition and an adapted distribution of mechanical properties.

[0060] The foundation layer can be applied, for example, using Wire Arc Additive Manufacturing (WAAM), a process also known as arc wire cladding. In this process, a wire is melted layer by layer and applied to the blank, creating a metallurgical bond.

[0061] Alternatively, other additive manufacturing processes such as laser cladding or electron beam cladding can be used to create the foundation layer with high precision and material homogeneity.

[0062] In one design variant, the foundation layer is at least twice as wide as the blade thickness. This foundation layer ensures a wide transition of the blades into the contour of the blank.

[0063] In another variant, the foundation layer covers more than 25%, preferably more than 50%, and in particular more than 75% of the blank surface on which at least one blade is arranged.

[0064] In an advantageous embodiment, the entire blank is covered with a foundation layer. PCT - Patent application

[0065] Howden

[0066] V744

[0067] 8

[0068]

[0069] The foundation layer is applied to the blank, for example, using concentric circles, to form the basic body.

[0070] For example, the foundation layer has a material-bonded connection to the blank.

[0071] For example, the foundation layer is applied to the blank by means of arc wire cladding with a layer thickness of more than 0.5 mm, preferably with a layer thickness of more than 1.5 mm, in particular with a layer thickness of more than 2 mm.

[0072] In a further processing step, the excess material is then removed by a chip-removing process, for example by milling, to the previous dimension or to the target dimension of the base body.

[0073] Surprisingly, it was found that the bonding of the blade assembly layers can be significantly improved by the foundation layer applied to the blank. This is particularly true compared to directly building the blade assembly layers onto the blank or to conventionally manufactured blades that are attached to a base body using caterpillar welds.

[0074] In one embodiment, a defined mixing zone and / or heat-affected zone forms between the blank and the foundation layer. This zone is created by applying the foundation layer to the blank and results in a metallurgically optimized transition between the blank material and the foundation layer material. PCT - Patent application

[0075] Howden

[0076] V744

[0077] 9

[0078]

[0079] For example, the mixing zone and / or heat-affected zone on the substrate side, i.e., extending from the original surface of the blank towards the blank, has a maximum depth of no more than 5 mm. The depth is preferably measured from the original substrate surface of the blank.

[0080] For example, a first area of ​​the mixing zone, preferably an area with a depth of no more than 3 mm extending from the original substrate surface, exhibits a mixed structure. This mixed structure comprises structural components of the blank, in particular a forged blank, and structural components of the foundation layer or the applied welding material.

[0081] In one design variant, the microstructure fraction of the blank and / or a forged structure in this first area of ​​the dilution zone is at least 20%. This ensures sufficient metallurgical integration of the blank into the foundation layer without excessively deep melting or thermal degradation of the blank.

[0082] In a further embodiment, a heat-affected second region adjoins the first region, extending inwards from the surface of the blank, and in this second region there is essentially no mixed microstructure. This second region preferably exhibits a microstructure of the blank, in particular a forged microstructure, without weld components.

[0083] Preferably, the second region extends within the maximum depth of the mixing zone and / or heat-affected zone. For example, the second region may have a depth of up to 2 mm or a differential PCT patent application.

[0084] Howden

[0085] V744

[0086] 10

[0087]

[0088] between the maximum depth of 5 mm and the depth of the first area.

[0089] In another embodiment, the former austenite grain size of the blank changes in the second region. Preferably, the former austenite grain size is at least one size unit smaller than the original austenite grain size of the blank. This further improves the mechanical strength in the transition region.

[0090] In another embodiment, precipitates form in the weld structure of the foundation layer after heat treatment, particularly after a final heat treatment. Preferably, these precipitates comprise carbides, especially precipitates of the Cr structure type. 23 C6 and / or Cr7C3.

[0091] The precipitates can form at grain boundaries and / or within the grain. This allows for improved structural stability of the base layer and targeted adjustment of mechanical properties, particularly hardness, strength, and toughness.

[0092] The blade assembly layers are attached to the foundation layer, built up layer by layer on the foundation layer and together forming the blade body.

[0093] In one embodiment, the blade assembly layers form a homogeneous welded structure among themselves, which differs deliberately from the structure of the blank. PCT - Patent application

[0094] Howden

[0095] V744

[0096] 11

[0097]

[0098] In one variant of the invention, the weld structure of the blade assembly layers has a former austenite grain size that preferably corresponds substantially to the former austenite grain size of the blank.

[0099] Alternatively, the former austenite grain size of the blade structure layers may be reduced compared to the former austenite grain size of the blank, with the grain size being at most two orders of magnitude smaller.

[0100] This targeted adjustment of the grain size creates a microstructure adapted to the mechanical requirements, ensuring both sufficient strength and high toughness of the shovel.

[0101] In another design variant, precipitates form within the blade assembly layers even before a final heat treatment.

[0102] For example, these deposits occur at least in the first blade assembly layers following the foundation layer, especially within the first ten layers.

[0103] The precipitates preferably comprise carbides, in particular precipitates of the Cr structure type 23 C6 and / or Cr7C3.

[0104] The precipitates can form both at the grain boundaries and within the grain interior and contribute to a targeted influence on the mechanical properties, especially strength and wear resistance. PCT - Patent application

[0105] Howden

[0106] V744

[0107] 12

[0108]

[0109] This early formation of precipitates in the weld structure allows a stabilized microstructure to be achieved even before the final heat treatment, thereby improving process reliability and the reproducibility of mechanical properties.

[0110] In addition, it has been found that the properties of the foundation layer and the subsequent blade structure layers are significantly influenced by the chemical composition.

[0111] In one design variant, the foundation layer and / or the blade assembly layers have a higher silicon content compared to the blank.

[0112] For example, the silicon content of the foundation layer and / or the blade assembly layers is increased by a factor of 1.5 to a maximum of 2.0 compared to the silicon content of the blank.

[0113] Surprisingly, it has been found that this targeted adjustment of the silicon content can achieve an improved formation of the metallurgical transition zone as well as the microstructure within the foundation layer and the blade superstructure layers.

[0114] In particular, the increased silicon content promotes the formation of a homogeneous microstructure as well as the targeted adjustment of microstructure parameters, such as grain size and precipitation formation.

[0115] In another embodiment, the increased silicon content contributes to improving the properties of the foundation layer and the blade assembly layers at PCT - Patent application

[0116] Howden

[0117] V744

[0118] 13

[0119]

[0120] to approximate the properties of the blank, so that a graduated transition with improved mechanical properties is created.

[0121] This chemical fine-tuning can further improve, in particular, the structural integrity of the transition area and the long-term stability of the impeller under dynamic load.

[0122] In addition, it has been found that the quality of the foundation layer and the bucket structure layers is significantly influenced by the porosity of the applied material.

[0123] In one design variant, the foundation layer has a porosity of at most 1%.

[0124] For example, the porosity is limited to a maximum of 0.5%, and in particular to a maximum of 0.2%.

[0125] In one design variant, the maximum pore size within the foundation layer is at most 0.1 mm.

[0126] Surprisingly, the special design of the WAAM made it possible to adjust the porosity and pore size so low that a significant improvement in the mechanical properties and structural integrity of the foundation layer can be achieved.

[0127] In another embodiment, the layered composite of the blade assembly layers also exhibits a porosity of no more than 1%. PCT - Patent application

[0128] Howden

[0129] V744

[0130] 14

[0131]

[0132] For example, the porosity within the blade structure layers is limited to a maximum of 0.5%, and in particular to a maximum of 0.2%.

[0133] In another design variant, the maximum pore size within the blade structure layers is at most 0.1 mm.

[0134] Preferably, after machining the surface of the blade assembly layers, there are essentially no pores present.

[0135] This targeted limitation of porosity ensures that no local weak points arise within the foundation layer or the blade assembly layers, thereby improving in particular the fatigue strength and operational reliability of the impeller.

[0136] The impeller blade has a blade thickness, a blade length, and a blade height. The blade thickness refers to the material thickness of the blade in a plane perpendicular to the flow direction. The blade length is the extent of the blade along the flow direction, while the blade height describes the maximum elevation of the blade from the base or body to the blade tip.

[0137] The blade base forms the transition from the blank to a blade of the impeller.

[0138] Thus, for example, the foundation layer can form at least the blade root after machining. PCT - Patent application

[0139] Howden

[0140] V744

[0141] 15

[0142]

[0143] In a further variant of the invention, the three blade assembly layers, preferably the first four blade assembly layers, in particular the first five blade assembly layers which are based directly on the foundation layer, together with the foundation layer form the blade root.

[0144] The blade, for example, consists of several or even numerous blade structure layers, which are built up layer by layer. The total height of the applied layers corresponds to the final blade height plus a small excess, which is then removed to the desired dimension using a chip-removing process.

[0145] One or more blades are built onto the base body, each consisting of a multitude of blade superstructure layers that are applied layer by layer and reach a superstructure height that corresponds to the blade height.

[0146] The blade superstructure layers are built up continuously above the foundation layer to ensure a uniform and homogeneous structure. In one embodiment, the individual layers are applied in a zigzag pattern by arc wire cladding to achieve improved material distribution and increased mechanical strength.

[0147] Alternatively, the layers can also be applied in uniform parallel paths or in a concentric circular pattern, depending on the specific requirements of the blade structure. PCT - Patent application

[0148] Howden

[0149] V744

[0150] 16

[0151]

[0152] For example, the blade assembly layers above the foundation layer are built up continuously on top of each other.

[0153] Advantageously, the blade assembly layers have a material-bonded connection to each other and / or to the foundation layer.

[0154] The blank, which serves as the base body for the impeller, exhibits a forged microstructure with a specifically controlled fiber orientation. The forging process is designed to achieve pronounced anisotropy in the direction of the main operational load. This directed forming process results in a targeted fiber orientation that improves fatigue strength, particularly in areas of high mechanical stress, and contributes to crack prevention.

[0155] The resulting microstructure is characterized by a fine-grained microstructure with an average grain size of ASTM grade 5 or finer, corresponding to a maximum grain size of approximately 65 pm. A homogeneous grain distribution exists throughout the entire component volume, ensuring uniform mechanical strength. The degree of deformation during the forging process is greater than 2, resulting in sufficient compaction and grain refinement.

[0156] The foundation layer and the blade superstructure layers are applied layer by layer to the blank using the WAAM process, forming a typical welded structure with a directional microstructure. Due to the local heat input from the electric arc and the relatively rapid solidification, dendritic structures oriented in the build-up direction form, growing perpendicular to the application surface. The resulting grain structure is different compared to the PCT patent application.

[0157] Howden

[0158] V744

[0159] 17

[0160]

[0161] The fine forged structure of the blank is significantly coarser, which is typical for welded-on structures.

[0162] At the beginning of the layer buildup, i.e., in the foundation layer or the first blade buildup layer, the temperature gradient to the underlying solid matrix is ​​particularly pronounced. This leads to a high solidification rate, directional grain orientation, and strong thermally induced gradation of the microstructure. Due to this interaction, the foundation layer exhibits the strongest metallurgical transition—both in terms of grain growth and chemical precipitation.

[0163] As the layer thickness increases, this effect diminishes because each new layer no longer primarily acts thermally on the solid base material, but rather on previously applied WAAM layers. The resulting thermal cycles lead to a thermal post-treatment of the underlying layer, which can result in precipitation formation (e.g., carbides, nitrides, or intermetallic phases) and local recrystallization.

[0164] The layer thickness of individual layers is a maximum of twice the wire diameter used, typically achieving a thickness in the range of 0.5–2.0 mm per layer. The precise grain structure within each layer therefore depends on the heat input, the wire feed rate, the number of layers, and the geometry of the component.

[0165] Overall, this results in a graduated structure in which the mechanical properties change continuously from the foundation layer to the uppermost blade assembly layer. This graduated transition is described in the PCT patent application.

[0166] Howden

[0167] V744

[0168] 18

[0169]

[0170] This enables optimized stress distribution and increases the structural integrity of the connection between the base body and the blade, so that the impeller is particularly advantageous for the special loads caused by vibrations and can offer an enormous service life compared to known impellers due to the special manufacturing process.

[0171] In the context of the present invention, the term radius or radii refers to the transition areas between different geometric elements of the impeller, particularly at the connection between the foundation layer and the blade in the form of a plurality of blade superstructure layers. These transition radii are crucial for the mechanical strength of the component and the prevention of vibration damage.

[0172] An increased radius design results in a more uniform stress distribution, thereby reducing notch effects and preventing potential cracking. Vibrations generated during operation by aerodynamic and mechanical loads can lead to material fatigue and structural damage. Optimizing the transition radii helps to mitigate these critical stress peaks and extend the service life of the impeller.

[0173] A particularly relevant area is the transition radius between the foundation layer and the blade, which, within the scope of the invention, is designed with a value greater than % of the blade root. This radius can be variably adjusted according to specific operating requirements to ensure an optimal balance between structural strength and aerodynamic efficiency. The targeted adjustment of the radii enables, PCT - Patent Application

[0174] Howden

[0175] V744

[0176] 19

[0177]

[0178] to significantly reduce vibration stresses and thus improve the operational reliability and long-term stability of the impeller.

[0179] In one embodiment of the invention, the transition radius between the foundation layer and the blade assembly layers is designed with a value of more than 1 / 3, preferably with a value of more than 1 / 2, in particular with a value equal to the blade thickness at the blade root.

[0180] This geometry prevents the formation of notch stresses that could otherwise lead to cracking and material failure. Alternatively, the transition area can be designed with a stepped geometry that combines several small radii to allow for a smooth load distribution.

[0181] For example, the foundation layer and / or the blade superstructure layers are applied to the blank using wire arc additive manufacturing / wire arc welding.

[0182] The diffusion homogeneity factor (DHF) is an essential parameter for evaluating the metallurgical quality of the bond between the WAAM-deposited material and the impeller base. It describes the uniform diffusion of alloying elements across the fusion boundary and ensures that no abrupt chemical gradient occurs. Homogeneous diffusion is crucial for mechanical stability, as sudden differences in chemical composition can promote brittle phases, microcracks, or other failure mechanisms.

[0183] Insufficient diffusion, characterized by a DHF value of less than 90%, can lead to structural weaknesses. In this PCT patent application...

[0184] Howden

[0185] V744

[0186] 20

[0187]

[0188] In certain areas, microcracks, undesirable brittle phases, or an uneven grain structure can form, ultimately leading to premature material fatigue or blade separation from the base body. By precisely controlling the heat input and process parameters in the WAAM process, the diffusion homogeneity factor can be optimized and high material integrity ensured.

[0189] To ensure maximum mechanical strength and long-term stability, the diffusion homogeneity factor between the base body and the foundation layer is greater than 92%, preferably greater than 95%, and particularly greater than 98%. These values ​​demonstrate that virtually complete homogeneity of the material transitions is achieved, resulting in a high load-bearing capacity for the connection between the base body and the foundation layer and preventing the formation of critical stress concentrations.

[0190] The diffusion homogeneity factor between the base body or foundation layer and the blade superstructure layers is greater than 90%, preferably greater than 94%, and particularly greater than 98%. This ensures that insufficient alloy mixing or microstructural inhomogeneities, which could impair the service life of the component, do not occur in the subsequently applied layers.

[0191] Surprisingly, it has been found that a diffusion homogeneity factor of more than 92%, preferably more than 95%, and particularly more than 98%, results in no abrupt changes in mechanical properties occurring in the transition area between the blank and the foundation layer (PCT patent application).

[0192] Howden

[0193] V744

[0194] 21

[0195]

[0196] which significantly reduces the formation of cracks and local stress peaks.

[0197] The verification of DHF is carried out using microstructural testing methods, in which the chemical composition and microstructure transitions between the material zones are examined in detail. These include scanning electron microscopy (SEM) with energy-dispersive X-ray spectroscopy (EDX) to analyze the diffusion profiles of the alloying elements, as well as microstructural cross-sections to evaluate the grain structure and microstructure homogeneity.

[0198] Additionally, hardness measurements can be performed in the fusion zone to identify any potential hardness gradients and brittle areas. These comprehensive testing procedures ensure that the diffusion process is fully controlled and that the mechanical properties of the blade joint meet the highest quality standards.

[0199] In addition to high material homogeneity, the foundation layer and the blade superstructure layers exhibit a bond depth of more than 80% of an average grain size, ensuring optimal mechanical bonding. This means that the structural elements of the applied layers penetrate deep into the base material, resulting in a particularly stable connection.

[0200] The Wire Arc Additive Manufacturing (WAAM) process enables the layer-by-layer construction of the foundation layer and blade superstructure layers using an arc welding technique in which a welding wire is used as filler material. PCT - Patent application

[0201] Howden

[0202] V744

[0203] 22

[0204]

[0205] In the present invention, for example, a forged material is used as the base material, while the superimposed blades are made of stainless steel 1.4313 (X3CrNiMo13-4). The metallurgical differences between these materials, as well as the characteristics of the transition zone, are crucial for the mechanical properties and long-term stability of the component.

[0206] In one embodiment, the blank, the foundation layer and the blade assembly layers are made of the same material or of materials of the same or similar type, in particular of a martensitic stainless steel, preferably of material 1.4313 (X3CrNiMo13-4).

[0207] In an alternative design variant, the foundation layer and / or the blade superstructure layers are made of duplex stainless steel with the material number 1.4462 (X2CrNiMoN22-5-3). This material has a two-phase microstructure of austenite and ferrite, which enables a combination of high strength, excellent corrosion resistance, and good weldability. The balanced phase distribution (approximately 50% ferrite, 50% austenite) ensures outstanding resistance to intergranular corrosion, pitting, and stress corrosion cracking – even under demanding operating conditions such as in the chemical industry or in seawater applications.

[0208] The alternative use of 1.4462 in the WAAM process requires controlled heat input to ensure the formation of a balanced duplex structure and to minimize the risk of phase transformations or brittle intermetallic phases. Through targeted process control, a fine lamellar microstructure can be created, resulting in high toughness (PCT - patent application).

[0209] Howden

[0210] V744

[0211] 23

[0212]

[0213] Simultaneously, a high yield strength is guaranteed. Due to its high strength, 1.4462 is particularly suitable for highly stressed blade structures subjected to high centrifugal forces, while also offering excellent corrosion resistance to chloride-containing media. With appropriate post-treatment, the WAAM-welded layers exhibit a homogeneous grain structure and good bond depth to the base material.

[0214] Another advantageous material choice for the foundation layer and / or the blade superstructure layers is the martensitic-hardenable steel 1.4542 or 1.4542.

[0215] 1.4548 (17-4 PH / X5CrNiCuNb16-4). This high-strength, stainless steel offers an excellent combination of high mechanical strength, good corrosion resistance, and hardenability through precipitation hardening. Its high tensile strength of up to 1100 MPa, combined with good machinability, makes 17-4 PH particularly suitable for heavily loaded impeller blades.

[0216] In the WAAM process, 17-4 PH exhibits a martensitic weld microstructure that can be further strengthened by targeted heat treatment (e.g., H900 or H1025 condition). The precipitation of copper phases during the aging process leads to a significant increase in strength while maintaining good dimensional stability. A stable microstructure transition to the base layer can be achieved through precise control of the process parameters. With appropriate process parameters, good weldability with controlled porosity and homogeneous bond depth between the layers is ensured. Corrosion resistance exceeds that of standard martensitic steels.

[0217] The microstructure of the forged cast material typically exhibits a dendritic solidification structure, especially if it is a PCT - patent application

[0218] Howden

[0219] V744

[0220] 24

[0221]

[0222] This is a martensitic or ferritic-pearlitic casting material. This structure can lead to segregation, where certain elements are unevenly distributed, which can negatively affect the mechanical properties. Subsequent forging refines and homogenizes the grain structure, resulting in improved strength and toughness. Heat treatment by tempering or annealing can also reduce internal stresses and optimize the material behavior.

[0223] In contrast, the WAAM weld metal exhibits a martensitic-ferritic microstructure resulting from the layered deposition of the welding wire. The material used, 1.4313, typically contains a low carbon content of approximately 0.03 to 0.05%, which enables high weldability. The alloy is characterized by 12 to 14% chromium, which improves corrosion resistance, while 3 to 4.5% nickel contributes to increased toughness and influences austenite stabilization. The molybdenum content, between 0.4 and 1%, further improves the material's strength and wear resistance.

[0224] During solidification in the WAAM process, for example, a primarily dendritic microstructure forms, which can be modified by the heat input and repeated heat application during the multilayer build-up. Subsequent heat treatment may be necessary to relieve stresses and further optimize the mechanical properties. The interaction between the layers presents a particular challenge, as repeated melting can lead to grain coarsening or local changes in hardness. PCT - Patent application

[0225] Howden

[0226] V744

[0227] 25

[0228]

[0229] The transition zone between the forged casting and the WAAM weld metal is a critical area where metallurgical changes occur. The heat from the welding process causes partial dissolution of the base material, altering its microstructure. Carbon can diffuse into the weld metal, while nickel and chromium from the alloy can migrate into the adjacent area of ​​the base material. This can lead to changes in hardness, especially if the base material has a higher carbon content than the weld metal. In this case, martensitic structures with increased hardness can form in the transition zone, potentially resulting in reduced toughness and increased brittleness.

[0230] Another characteristic of the transition zone is the presence of a microstructure gradient, where the microstructure changes continuously from the martensitic base structure through a mixed microstructure to the fully ferritic-martensitic WAAM weld metal. If the filler metal has a higher nickel concentration than the base material, residual austenite may remain in the transition zone, affecting the mechanical properties. The heat-affected zone (HAZ) is also an important area where microstructure changes can occur due to thermal effects. This zone can be optimized through targeted process control and heat treatments to avoid undesirable hardness gradients or stress concentrations.

[0231] The quality of the bond between the foundation layer and the blade superstructure layers of the impeller is crucial for the mechanical strength and long-term operational stability of the turbomachine. Metallurgical interface quality plays a particularly important role when using the Wire Arc Additive Manufacturing (WAAM) process. PCT - Patent Application

[0232] Howden

[0233] V744

[0234] 26

[0235]

[0236] One of the most important parameters for assessing WAAM quality is the bond depth, which determines how well each new blade is bonded to the base body. Insufficient bond depth can lead to inadequate adhesion between the material layers, significantly increasing the risk of microcracks or brittle fracture. An optimal metallurgical bond must ensure a homogeneous transition zone to distribute mechanical stresses evenly and prevent material fatigue.

[0237] The bond depth, also known as the fusion zone, describes the area in which the applied WAAM material fuses with the substrate. It is a crucial parameter for the mechanical stability of the bond and must penetrate sufficiently deep into the substrate to ensure high bond strength. Bond depth is assessed metallographically by analyzing cross-sections under a scanning electron microscope (SEM), evaluating the depth of the fused zone and the homogeneity of the microstructure.

[0238] The invention significantly improves WAAM quality by ensuring that the foundation layer and blade superstructure layers not only meet but exceed the mechanical requirements. Optimal quality is defined by a bond depth of at least 80% of the grain size of the base structure. This ensures that the metallurgical bond occurs over a sufficiently large contact area to minimize load peaks and guarantee optimal force transmission.

[0239] At the same time, for example, the maximum permissible porosity in the fusion zone is limited to a maximum area fraction of 0.2%. This ensures that no significant voids or inclusions are present in the PCT patent application.

[0240] Howden

[0241] V744

[0242] 27

[0243]

[0244] Weld structures may occur that could impair the mechanical properties.

[0245] For example, another crucial parameter is the hardness gradient in the heat-affected zone (HAZ), which must not exceed a maximum difference of AHV < 30 HV. This prevents abrupt changes in hardness in the transition zone between the base material and the WAAM coating layer, which could lead to stress cracks or a brittle structure.

[0246] Porosity is a measure of the proportion of trapped gas bubbles or voids within the weld zone, which can negatively affect the weld strength. High porosity leads to weak points in the material that can cause cracking or premature failure under load. Porosity testing is performed using ultrasonic testing (UT) or X-ray non-destructive testing (X-ray DDT), which visualizes internal defects to ensure that the permissible porosity limit of < 0.2% is met.

[0247] To ensure the high quality of the WAAM coatings, comprehensive testing procedures are employed. Metallographic analysis using scanning electron microscopy (SEM) allows for the examination of weld cross-sections and reveals whether microcracks or grain coarsening have formed in the fusion zone. Direct comparison with the microstructure of the original steel verifies whether the weld meets the desired quality requirements.

[0248] In addition, the hardness distribution within the foundation layer is determined by means of a hardness test, in particular according to the Vickers HV10 method. PCT - Patent application

[0249] Howden

[0250] V744

[0251] 28

[0252]

[0253] Here, the microhardness is measured along the bonding zone between the blank and the foundation layer.

[0254] In one design variant, the foundation layer immediately after application, i.e. before final heat treatment, exhibits a microhardness that is increased by a maximum of 30% compared to the original microhardness of the blank.

[0255] Preferably, the microhardness of the foundation layer in this state is at most 350 HV, in particular at most 35.5 HRC.

[0256] In another variant, after a final heat treatment, the foundation layer has a microhardness that differs from the original microhardness of the blank by a maximum of 10%.

[0257] Preferably, the microhardness of the foundation layer after the final heat treatment is at most 300 HV, in particular at most 29.8 HRC.

[0258] This coordinated hardness development ensures that no critical hardness gradients arise in the transition area between the blank and the foundation layer, thus preventing stress cracks and embrittlement while simultaneously guaranteeing sufficient strength.

[0259] In addition, the hardness distribution within the blade assembly layers is determined by means of a hardness test, in particular according to the Vickers HV10 method. Here, the microhardness within individual layers as well as across the entire layer assembly is determined. PCT - Patent application

[0260] Howden

[0261] V744

[0262] 29

[0263]

[0264] In one design variant, the individual blade assembly layers exhibit a microhardness immediately after application, i.e., before a final heat treatment, whereby the microhardness differs between individual layers by a maximum of 10%.

[0265] Preferably, the microhardness of the individual blade assembly layers in this state is at most 350 HV, in particular at most 35.5 HRC.

[0266] In another variant, the blade assembly layers exhibit microhardness after a final heat treatment, with the microhardness differing by a maximum of 10% between individual layers.

[0267] Preferably, the microhardness of the blade assembly layers after the final heat treatment is at most 300 HV, in particular at most 29.8 HRC.

[0268] This coordinated hardness distribution within the individual layers and across the entire layer composite ensures that no local hardness jumps occur, thus preventing stress cracks and embrittlement and simultaneously guaranteeing a homogeneous mechanical load-bearing capacity of the blade.

[0269] In one embodiment of the invention, the foundation layer has a yield strength ratio of at most 90% after a final heat treatment.

[0270] In a further embodiment of the invention, the foundation layer exhibits a yield strength ratio of at most 85% after the final heat treatment. PCT - Patent application

[0271] Howden

[0272] V744

[0273] 30

[0274]

[0275] In a particularly preferred embodiment of the invention, the foundation layer has a yield strength ratio of at most 80% after the final heat treatment.

[0276] The yield strength ratio refers specifically to the relationship between the yield strength and the tensile strength. It has been shown that a limited yield strength ratio can provide sufficient plastic deformation reserve for the foundation layer. This reduces stress peaks in the transition zone between the blank and the foundation layer and prevents brittle fracture failure.

[0277] In one embodiment of the invention, the layered composite of the blade structure layers exhibits a yield strength ratio of at most 90% after a final heat treatment.

[0278] In a further embodiment of the invention, the layered composite of the blade structure layers exhibits a yield strength ratio of at most 85% after the final heat treatment.

[0279] In a particularly preferred embodiment of the invention, the layered composite of the blade structure layers exhibits a yield strength ratio of at most 80% after the final heat treatment.

[0280] The yield strength ratio refers specifically to the relationship between the yield strength and the tensile strength. It has been shown that a limited yield strength ratio within the layered composite results in increased plastic deformation capacity of the blade assembly layers. (PCT patent application)

[0281] Howden

[0282] V744

[0283] 31

[0284]

[0285] This can reduce local stress peaks within the blade and achieve improved resistance to dynamic loads, especially those resulting from vibrations and centrifugal forces.

[0286] Another essential testing method is non-destructive ultrasonic testing (UT) or an alternative X-ray analysis (X-ray non-destructive testing), which verifies that porosity is less than 0.2%. This method ensures that there are no unwanted air inclusions, material inclusions, or unfilled areas in the weld structure that could compromise the mechanical strength of the foundation layer and blade superstructure layers.

[0287] To assess the toughness of the bonding zone, an impact test, particularly using the Charpy V method, is performed. This determines the impact energy of the respective material areas.

[0288] In one design variant, the foundation layer, after a final heat treatment, exhibits an impact strength that is at least 50% of the impact strength of the blank.

[0289] This design ensures that the foundation layer, as a bonding layer, has sufficient toughness to withstand sudden loads and thermally induced stresses without brittle failure.

[0290] In another embodiment, a layered composite of the blade structure layers exhibits a PCT patent application after a final heat treatment.

[0291] Howden

[0292] V744

[0293] 32

[0294]

[0295] Impact work that is at least 50% of the impact work of the blank.

[0296] Preferably, this coordinated toughness within the layered composite achieves a homogeneous mechanical load-bearing capacity of the blade, so that local failure mechanisms, in particular brittle fracture-related cracking, can be avoided.

[0297] It has been shown that the interaction of the described parameters, in particular the increased silicon content, the limited porosity, the high diffusion homogeneity factor and the matched hardness and toughness properties, leads to a significant improvement in mechanical load-bearing capacity and long-term stability.

[0298] In addition to mechanical strength, the corrosion resistance of the foundation layer and blade superstructure layers plays a crucial role, especially when the impeller is operated under less demanding environmental conditions. To ensure that the foundation layer and blade superstructure layers exhibit corrosion resistance equivalent to or better than the original material, a corrosion test according to ASTM G48 or a salt spray test according to DIN EN ISO 9227 is performed. In this test, the layer is exposed to an aggressive environment for at least 72 hours to check for intergranular corrosion or pitting. The acceptance criteria stipulate that no significant corrosion phenomena occur, thus ensuring the component's longevity.

[0299] Corrosion resistance describes a material's ability to withstand environmental influences such as moisture, chemicals, or salt solutions. PCT - Patent Application

[0300] Howden

[0301] V744

[0302] 33

[0303]

[0304] withstand corrosion without compromising mechanical stability or surface quality. Insufficient corrosion resistance can lead to pitting, intergranular corrosion, or stress corrosion cracking.

[0305] The combination of these comprehensive testing methods ensures that the foundation and blade superstructure layers produced by WAAM not only meet the required mechanical parameters but even exceed them. The optimized metallurgical bonding, the targeted reduction of porosity, and the controlled hardness distribution lead to a significant improvement in mechanical properties. This guarantees greater operational reliability, as stress cracks, premature material fatigue, and corrosion damage are avoided. The invention thus represents a crucial advancement of the WAAM process, raising quality assurance to a new level and revolutionizing the use of this additive manufacturing technology for high-performance components, such as impellers in turbomachinery according to the invention.

[0306] The foundation layer and the blade superstructure layers, for example, consist of a high-alloy, soft martensitic steel, specifically optimized for applications with high mechanical loads and stringent corrosion resistance requirements. Through targeted alloying with chromium, nickel, and copper, the steel's properties are tailored to ensure high strength, toughness, and resistance to environmental influences.

[0307] The chromium content, for example, ranges from 10% to 20%, resulting in pronounced corrosion resistance. Nickel is present in the alloy at a proportion of 1% to 7% to increase the material's toughness (PCT patent application).

[0308] Howden

[0309] V744

[0310] 34

[0311]

[0312] to improve and support the formation of a homogeneous microstructure. Additionally, the steel can contain 1% to 7% copper, which contributes to increased strength and improved mechanical properties under fatigue behavior. This alloy combination ensures that the applied layers withstand both high static and dynamic loads without premature material failure.

[0313] In addition to the main alloying elements, the chemical composition of the foundation layer and the blade superstructure layers is further optimized by targeted adjustments to the sulfur content, particularly to improve the weldability of the wire material in WAAM. For example, the sulfur content is at least 1.05 times higher, preferably 1.10 times higher, and especially 1.15 times higher, than the sulfur content of the blank, resulting in improved machinability of the material. This targeted increase contributes to improving the machining properties of the WAAM-welded layers, which is particularly important for final machining operations. At the same time, the mechanical integrity of the layers is maintained, so the strength and toughness of the component are not negatively affected.

[0314] In addition to increasing the sulfur content, the phosphorus content of the foundation layer and blade superstructure layers is also specifically adjusted, particularly to improve weldability. The phosphorus content is at least 1.05 times, preferably 1.10 times, and especially 1.15 times higher than the phosphorus content of the blank, thereby specifically influencing the grain size distribution and the material's strength. Small amounts of phosphorus can contribute to improving the mechanical properties by increasing hardness and wear resistance. At the same time, care is taken to ensure compliance with the PCT patent application.

[0315] Howden

[0316] V744

[0317] 35

[0318]

[0319] Increasing the phosphorus content has no adverse effects on the toughness or brittle fracture tendency of the material. These targeted chemical modifications ensure that the foundation layer and blade superstructure layers are optimally suited to the requirements of the WAAM process and the mechanical stresses encountered during operation.

[0320] In one variant of the invention, the blade assembly layers are aligned at an angle α to the foundation layer, wherein the angle α is greater than 5° and less than 45°.

[0321] In an advantageous embodiment of the invention, the angle a is greater than 15° and less than 30°.

[0322] The blade buildup layer, for example, is dimensioned to have a height of more than 400 pm and less than 1500 pm. The height of the buildup layer can be adjusted via the wire thickness and welding speed.

[0323] The selected height range also enables efficient load distribution along the blade structure and reduces local stress peaks that can occur, particularly in the blade root area. The ability to flexibly adjust the height of the blade superstructure layer within this range allows the impeller design to be adapted to specific operating conditions without compromising mechanical integrity or flow guidance.

[0324] The impeller has a diameter of more than 450 mm, for example more than 900 mm, making it optimized for use in large-scale turbomachinery with high throughput capacities. (See PCT patent application.)

[0325] Howden

[0326] V744

[0327] 36

[0328]

[0329] For this scale of production, the approach of not solely relying on machining to manufacture the impeller proves advantageous. Machining a rotor with a diameter exceeding 900 mm takes more than two weeks, whereas overhauling an existing impeller—by removing the existing blades, laser cladding the foundation and blade superstructure layers, and machining the excess material to create the finished impeller—can be accomplished in two working days. The robust construction achieved through WAAM ensures the impeller's structural integrity is maintained even at high speeds and dynamic loads, while simultaneously guaranteeing precise flow guidance.

[0330] In principle, the manufacturing process according to the invention is suitable for impellers of any size, so that the production can be carried out for both smaller and large-format compressor and turbine impellers.

[0331] Especially for large-dimensioned impellers, which were previously milled from a solid block of metal, resulting in material losses of several tons, additive manufacturing represents a significant improvement. Through layer-by-layer construction using wire arc additive manufacturing, the impeller can be produced with significantly reduced material costs and shorter production times, while simultaneously achieving high dimensional accuracy and an optimized microstructure.

[0332] The inventive method offers the advantage, particularly for large impellers with complex geometries, that flow optimizations can be directly integrated into the additive manufacturing process without being limited by the constraints of subtractive machining processes. PCT - Patent application

[0333] Howden

[0334] V744

[0335] 37

[0336]

[0337] According to the invention, the method for manufacturing an impeller for a continuously operating turbomachine comprises providing a base body that carries at least one blade, wherein the base body consists of a blank designed as an axially symmetric body of revolution with a hyperbolic contour. A foundation layer is applied directly to this blank using WAAM, which serves as the basis for the subsequent layer-by-layer construction of the blades. Subsequently, a plurality of blade superstructure layers are built up layer by layer on the foundation layer, so that the blade reaches a superstructure height corresponding to the final blade height.

[0338] Wire Arc Additive Manufacturing (WAAM), also known as arc wire additive manufacturing, is used to produce the foundation layer and the blade superstructure layers. The layers are initially applied in excess material to ensure secure adhesion and material homogeneity. The blade superstructure layers are aligned with a defined transition radius to the foundation layer to ensure uniform load distribution and optimized mechanical connection. In the final manufacturing step, the excess material is machined to the required dimensions. This ensures precise adherence to the specified geometry and a high surface quality, which is essential for the impeller's aerodynamic efficiency.

[0339] A significant advantage of the inventive method lies, for example, in the use of known CNC data for the initial production, thereby ensuring the production of high-precision impellers with reproducible properties. After the initial production, the PCT patent application

[0340] Howden

[0341] V744

[0342] 38

[0343]

[0344] Digital data sets are used for fast and efficient repairs. This makes it possible to repair damaged wheels in the shortest possible time without having to resort to a complete remanufacturing.

[0345] Furthermore, the process opens up the possibility not only of repairing newly manufactured impellers, but also of capturing existing impellers using a 3D scanning process and repairing them according to the same principle. By scanning the existing component, the geometric data can be digitized and used for targeted additive post-processing. This leads to a significant reduction in downtime and production costs, as impellers of various designs can be renewed quickly and efficiently without requiring a complete reconstruction.

[0346] Besides manufacturing new impellers, the process can also be used to refurbish existing ones. In this case, damaged blades are selectively removed and replaced with new blades that are built directly onto the existing base. Alternatively, damaged blades can be reinforced or reconstructed with an additional layer instead of being completely removed. This approach allows for fast and economical repair without requiring a complete replacement of the impeller.

[0347] Through the combination of optimized material selection, innovative manufacturing technology, and targeted geometry design, the invention offers a highly efficient solution for the production and refurbishment of impellers in turbomachinery. This leads to a significant improvement in mechanical strength, a reduction in flow losses, and a significant increase in the operational reliability and service life of the machine. PCT - Patent Application

[0348] Howden

[0349] V744

[0350] 39

[0351]

[0352] According to the invention, the method for renewing an impeller of a continuously operating turbomachine is used to create an impeller.

[0353] Further features and advantages of the invention will become apparent from the description of exemplary embodiments with reference to drawings and from the drawings themselves.

[0354] This shows:

[0355] Fig. 1 shows a perspective view of a running wheel,

[0356] Fig. 2 shows a perspective view of a basic body,

[0357] Fig. 3 shows a sectional view of a shovel,

[0358] Fig. 4 shows another sectional view of a shovel.

[0359] The perspective view of an impeller 1 for a continuously operating turbomachine shown in Fig. 1 comprises a base body 2 and, in this embodiment of the invention, eighteen blades 3.

[0360] The bucket 3 has a bucket thickness 4, a bucket length 5, and a bucket height 6. Each bucket 3 is constructed from a plurality of bucket superstructure layers 12 based on the base body 2, and the superstructure height of the bucket 3 corresponds to the bucket height 6.

[0361] The flow through the impeller 1 occurs along the blades 3 from the leading edge 8 of the blade towards the trailing edge 9. PCT - Patent application

[0362] Howden

[0363] V744

[0364] 40

[0365]

[0366] Fig. 2 shows a base body 2 comprising a blank 10. The blank 10 is completely covered with a foundation layer 11, which is applied by arc wire deposition welding in concentric circular paths, thereby bonding the foundation layer 11 to the blank 10. The blank 10 is designed as an axially symmetric body of revolution with a hyperbolic contour.

[0367] Figure 3 shows a cross-sectional view of a blade 3. A foundation layer 11 is arranged across the entire surface of the blank 10, from which the blade superstructure layers 12 extend.

[0368] In the illustrated embodiment, the blade 3 consists of twenty-five blade superstructure layers 12, which are built up layer by layer and bonded together by a material bond. The total height of the applied blade superstructure layers 12 corresponds to the blade height 6 plus a small excess, which is then removed to the desired dimension by a machining process.

[0369] The transition radius R is formed between the foundation layer 11 and the blade superstructure layers 12 of the blade 3. In the illustrated embodiment, the transition radius R has a value of 1 / 3. The transition radius R ensures advantageous structural strength and aerodynamic efficiency of the blade 3 by significantly reducing vibrational stress.

[0370] The design of the transition radius R results in a blade thickness 4 that decreases over the blade height 6. This design leads to an advantageous reduction in vibration stress. PCT - Patent application

[0371] Howden Patent V744 Hubble iOiWOOBwiil 41

[0372]

[0373] Figure 4 shows another sectional view of a blade 3, for example, a completely newly manufactured blade 3. In this embodiment, the foundation layer 11 is approximately twice as wide as the blade thickness 4 and, together with the first two blade superstructure layers 12, forms the blade root 13. As a result, the blade 3 has excellent adhesion to the blank 10 and is particularly resistant to stress cracking.

Claims

PCT patent application Howden V744 Wheel with at least one blade Patent claims 1. Impeller (1) for a continuously operating turbomachine with a base body (2) and at least one blade (3), wherein the base body (2) comprises a blank (10) and at least one foundation layer (11), wherein the blank (10) is designed as an axially symmetric body of revolution with a hyperbolic contour, wherein the shovel (3) has a shovel thickness (4), a shovel length (5), a shovel height (6) and a shovel foot (13), wherein the blade (3) is constructed from a plurality of blade assembly layers (12) based on the base body (2) and has an assembly height corresponding to the blade height (6), characterized by that the foundation layer (11) is arranged directly on the blank (10).

2. Impeller according to claim 1, characterized in that the foundation layer (11) is at least twice as wide as the blade thickness (4). PCT - Patent application Howden V744 2 3. Impeller according to claim 1 or 2, characterized in that the blade assembly layers (12) are continuously built up on top of each other above the foundation layer (11).

4. Impeller according to one of claims 1 to 3, characterized in that a transition radius R is formed between the foundation layer (11) and the blade (3), wherein the transition radius R is more than % of the blade thickness (4) and less than the blade thickness (4) at the blade root (13).

5. Impeller according to one of claims 1 to 4, characterized in that the foundation layer (11) and / or the blade assembly layers (12) are applied to the blank by means of wire arc additive manufacturing / arc wire cladding.

6. Impeller according to any one of claims 1 to 5, characterized in that the foundation layer (11) and / or the blade assembly layers (12) have a bond depth of more than 80% of an average grain size. PCT - Patent application Howden V744 3 7. Impeller according to one of claims 1 to 6, characterized in that the foundation layer (11) has a silicon content and the blank (10) has a silicon content, wherein the silicon content of the foundation layer (11) is at least 1.5 times and less than 2 times the silicon content of the blank (10).

8. Impeller according to one of claims 1 to 7, characterized in that the foundation layer (11) in an area adjacent to the blank (10) has a mixed structure of welded structure and forged structure, wherein the forged structure content is at least 20%.

9. Impeller according to one of claims 1 to 8, characterized in that in an area of ​​the blank (10) adjacent to the foundation layer (11) a former austenite grain size is formed which is at least one size unit finer than an original austenite grain size of the blank (10).

10. Impeller according to one of claims 1 to 9, characterized in that the yield strength ratio of the foundation layer (11) is less than 90%. PCT patent application Howden Patent V744 Hubble iOiWOOBwiil 4 11. Impeller according to one of claims 1 to 10, characterized in that the porosity of the foundation layer (11) is less than 1%, wherein the maximum pore size is less than 100 pm.

12. Impeller according to one of claims 1 to 11, characterized in that the foundation layer (11) has a microhardness, wherein the microhardness after a final heat treatment differs from the original microhardness of the blank (10) by a maximum of 10%.

13. Impeller according to any one of claims 1 to 12, characterized in that the foundation layer (11) and / or the blade assembly layers (12) are formed from a high-alloy, soft martensitic steel, wherein the steel contains at least 10% to 20% chromium and / or 1% to 7% nickel. PCT - Patent application Howden V744 5 14. Method for manufacturing an impeller (1) for a continuously operating turbomachine, comprising a base body (2) and at least one blade (3), characterized by the fact that A blank (10) is provided as an axially symmetric body of revolution with a hyperbolic contour, and a foundation layer (11) is applied directly to the blank (10). A plurality of blade superstructure layers (12) are applied layer by layer to the foundation layer (11) so that the blade (3) achieves a superstructure height corresponding to the blade height (6). The foundation layer (11) and the blade superstructure layers (12) are applied in excess by wire arc additive manufacturing. The blade superstructure layers (12) are applied with a transition radius R to the foundation layer (11), and the excess of the foundation layer (11) and the blade superstructure layers (12) is machined to the required dimension.

15. Use of a method according to claim 14 for renewing an impeller of a continuously operating turbomachine to an impeller (1) according to any one of claims 1 to 13.