Three-way catalyst with improved light-off performance for close-coupled engine applications
The optimized palladium and rhodium coating ratios on a three-way conversion catalyst enhance catalytic activities for HC, CO, and NOx conversion, addressing the challenge of low-temperature performance in exhaust gas treatment systems.
Patent Information
- Application Number
- PCT/EP2026/063711
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing three-way conversion catalysts face challenges in achieving improved catalytic performance, particularly at lower temperatures during cold start-ups, for treating exhaust gases from internal combustion engines.
A three-way conversion catalyst design with specific ratios of palladium loadings and coatings on a substrate, including a first coating extending over 20-70% of the substrate length with a lower total loading but higher palladium content, and a second coating extending over 20-70% of the substrate length with a complementary palladium loading ratio, supported on various support materials like alumina, ceria, and zirconia, with a third coating of rhodium and palladium, optimized to enhance light-off temperature.
The catalyst exhibits enhanced catalytic activities for HC, CO, and NOx conversion, improving overall performance by carefully adjusting the palladium loadings and coatings, resulting in better catalytic performance at lower temperatures.
Smart Images

Figure 00000043_0000 
Figure 00000044_0000 
Figure 00000045_0000
Abstract
Description
[0001] Three-way Catalyst with Improved Light-Off Performance for Close-Coupled Engine Applications
[0002] TECHNICAL FIELD
[0003] The present invention relates to a three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC and to a process for preparing said catalyst. The present invention further relates to an exhaust gas treatment system comprising an internal combustion engine and the three-way conversion catalyst of the present invention, a method for the treatment of an exhaust gas of an internal combustion engine and to a use of said three-way conversion catalyst for the treatment of an exhaust gas of an internal combustion engine.
[0004] INTRODUCTION
[0005] Catalytic converters are widely used as exhaust emission control devices for the conversion of toxic gases and pollutants in exhaust gas originating from the combustion of gasoline fuels and the like into less toxic and more environmentally friendly compounds, which becomes ever more important in view of the increasingly stringent emission regulations. Three-way catalytic conversion catalysts are a special type of such catalytic converters that were developed to enable the oxidation of carbon monoxide and hydrocarbons while simultaneously reducing nitrogen oxides, wherein the oxidation and reduction catalyst are usually located in a common housing.
[0006] US 2022 / 161236 A1 relates to a tri-metallic layered catalytic article comprising a top layer comprising platinum supported on at least one of an oxygen storage component, zirconia component and an alumina component, and rhodium supported on an oxygen storage component; a bottom layer comprising a front zone and a rear zone, said front zone comprising palladium supported on an oxygen storage component and an alumina component, and the rear zone comprises platinum supported on at least one of an alumina component, a ceria component, and an oxygen storage component; and a substrate.
[0007] US 7922988 B2 relates to a three-way conversion catalyst having the capability of simultaneously catalyzing the oxidation of hydrocarbons and carbon monoxide and the reduction of nitrogen oxides. Engine exhaust treatment system and methods of using the same are also provided.US 8394348 B1 relates to a three-way conversion catalyst having the capability of simultaneously catalyzing the oxidation of hydrocarbons and carbon monoxide and the reduction of nitrogen oxides being separated in a front and rear portion is disclosed, wherein all layers comprise a platinum group metal component, and the rear bottom layer is substantially free of a ceriacontaining oxygen storage component (OSC).
[0008] WO 2022 / 090689 A1 relates to a three-way catalyst article, and its use in an exhaust system for internal combustion engines, is disclosed. The catalyst article for treating exhaust gas comprising a substrate comprising an inlet end and an outlet end with an axial length L; a first catalytic region comprising a first platinum group metal (PGM) component, wherein the first PGM component comprises Rh and Pt; a second catalytic region comprising a second PGM component, wherein the second PGM component comprises Pd; and wherein the first PGM component has a Pt to Rh ratio of at least 1 : 20.
[0009] US 2021 / 348534 A1 relates to a catalytic article comprising a first layer and a second layer. The first layer comprises a platinum group metal component impregnated on a porous support mate¬ rial; and the second layer comprises a rhodium component impregnated on a support material, wherein the support material is a composite material including zirconia doped with baria, alu¬ mina, or combinations thereof, wherein the zirconia-based support material includes zirconia in an amount from about 80 to about 99 wt. %.
[0010] Despite the significant progress made in developing effective three-way conversion catalysts, there remains the need for further improvements with regard to the catalytic performance at lower temperatures, especially for very cold start-ups, independently of the engine type and size or the catalyst position in the exhaust gas system.
[0011] DETAILED DESCRIPTION
[0012] Therefore, it was an object of the present invention to provide a three-way conversion catalyst for treating an exhaust gas comprising HC, CO and NO from a gasoline engine which exhibits improved catalytic activities, such as improved HC conversion, CO conversion and NOx conversion. Surprisingly, it was found that the three-way conversion catalyst for the treatment of an exhaust gas comprising HC, CO and NO according to the present invention permits to achieve improved catalytic activities, such as improved HC conversion, CO conversion and NOx conversion. In particular, it was surprisingly found that by carefully adjusting the ratio of the total loading of an inlet bottom coating to an outlet bottom coating as well as the ratio of the palladium loading of the inlet bottom coating to the outlet bottom coating such that the inlet bottom coatinghas a lower total loading but a higher palladium loading leads to an enhancement of the light-off temperature which results in an overall improved catalytic performance.
[0013] Thus, the present invention relates to a three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, preferably for the treatment of an exhaust gas from an internal combustion engine, more preferably a gasoline engine, the catalyst comprising:
[0014] (i) a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end, and a plurality of passages defined by internal walls of the substrate extending therethrough;
[0015] (ii) a first coating, preferably a first washcoat coating, comprising palladium supported on a first support material;
[0016] (iii) a second coating, preferably a second washcoat coating, comprising palladium supported on a second support material;
[0017] (iv) a third coating, preferably a third washcoat coating, comprising one or more of rhodium and palladium supported on a third support material;
[0018] wherein the first coating extends over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70;
[0019] wherein the second coating extends over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70;
[0020] wherein the ratio of the loading of the first coating to the loading of the second coating, preferably the ratio of the loading of the first washcoat coating to the loading of the second washcoat coating, is in the range of from 0.3:1 to 0.9:1;
[0021] wherein the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 1.5:1 to 5:1,
[0022] wherein the third coating is disposed on the first and the second coatings over z% of the substrate axial length, preferably from the inlet end, wherein z is in the range of from 80 to 100; and wherein the third coating is substantially free of platinum.
[0023] It is preferred that x is in the range of from 30 to 65, more preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0024] It is preferred that y is in the range of from 30 to 65, more preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0025] It is preferred that z is in the range of from 85 to 100, more preferably in the range of from 90 to 100, more preferably in the range of from 95 to 100, more preferably in the range of from 98 to 100, more preferably in the range of from 99 to 100.It is preferred that the substrate is a ceramic substrate, more preferably the substrate is a ceramic honeycomb flow-through substrate.
[0026] It is preferred that the first coating comprises palladium, calculated as elemental palladium, at a loading in the range of from 50 to 250 g / ft3, more preferably in the range of from 100 to 220 g / ft3, more preferably in the range of from 140 to 200 g / ft3, more preferably in the range of from 150 to 190 g / ft3, more preferably in the range of from 160 to 180 g / ft3.
[0027] It is preferred that the first support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the first support material is alumina.
[0028] In the case where the first support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, it is preferred that the first support material comprises one or more rare earth metals, wherein the one or more rare earth metals are more preferably selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.
[0029] It is preferred that the first coating further comprises an oxygen storage compound, the oxygen storage compound more preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprising cerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0030] In the case where the first coating further comprises an oxygen storage compound, it is preferred that the first coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, more preferably in the range of from 0.5 to 2 g / in3, more preferably in the range of from 0.6 to 1.5 g / in3, more preferably in the range of from 0.7 to 1.3 g / in3, more preferably in the range of from 0.8 to 1.2 g / in3, more preferably in the range of from 0.9 to 1.1 g / in3.In the case where the oxygen storage compound comprises cerium, it is preferred that the cerium content, calculated as CeC>2, of the mixed oxide comprising cerium is in the range of from 5 to 50 weight-%, more preferably in the range of from 10 to 40 weight-%, more preferably in the range of from 20 to 30 weight-%.
[0031] It is preferred that the first coating further comprises a non-zeolitic oxidic material, the non-zeo-litic oxidic material more preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0032] In the case where the first coating further comprises a non-zeolitic oxidic material, it is preferred that the first coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.-%, more preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the first coating.
[0033] Further in the case where the first coating further comprises a non-zeolitic oxidic material, it is preferred that the non-zeolitic oxidic material is zirconia and wherein more preferably the first coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-%, more preferably in the range of from 1 to 2 weight-%, based on the weight of the first coating.
[0034] Further in the case where the first coating further comprises a non-zeolitic oxidic material, it is alternatively preferred that the non-zeolitic oxidic material is lanthana and wherein more preferably the first coating comprises lanthana, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-% based on the weight of the first coating.
[0035] It is preferred that the first coating further comprises an NOx storage component, more preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, more preferably consists of, barium oxide.In the case where the first coating further comprises an NOx storage component, it is preferred that the first coating comprises the NOx storage component in an amount in the range of from 1 to 20 weight-%, more preferably of from 5 to 17 weight-%, more preferably of from 10 to 15 weight-%, based on the weight of the first coating.
[0036] It is preferred that the first coating is substantially free of platinum, wherein the platinum content of the second coating is more preferably 0.01 weight-% or less, calculated as the element, more preferably 0.001 weight-% or less, more preferably 0.0001 weight-% or less, wherein the first coating is more preferably free of platinum.
[0037] It is preferred that the loading of the first coating, preferably the loading of the first washcoat coating, is in the range of from 1 to 5 g / in3, more preferably in the range of from 1.5 to 2.5 g / in3, more preferably in the range of from 1.7 to 2.4 g / in3, more preferably in the range of from 1.9 to 2.2 g / in3, more preferably in the range of from 2 to 2.1 g / in3.
[0038] It is preferred that the second coating comprises palladium, calculated as elemental palladium, at a loading in the range of from 1 to 150 g / ft3, more preferably in the range of from 20 to 120 g / ft3, more preferably in the range of from 40 to 100 g / ft3, more preferably in the range of from 50 to 90 g / ft3, more preferably in the range of from 60 to 80 g / ft3.
[0039] It is preferred that the second support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the second support material is alumina.
[0040] In the case where the second support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, it is preferred that the second support material comprises one or more rare earth metals, wherein more preferably the one or more rare earth metals are selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.
[0041] It is preferred that the second coating further comprises an oxygen storage compound, the oxygen storage compound more preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprisingcerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0042] In the case where that the second coating further comprises an oxygen storage compound, it is preferred that the second coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, more preferably in the range of from 0.5 to 2.5 g / in3, more preferably in the range of from 1 to 2 g / in3, more preferably in the range of from 1.2 to 1.8 g / in3, more preferably in the range of from 1.3 to 1.7 g / in3, more preferably in the range of from 1.4 to 1.6 g / in3.
[0043] In the case where the oxygen storage compound comprises cerium, it is preferred that the cerium content, calculated as CeC>2, of the mixed oxide comprising cerium is in the range of from 20 to 60 weight-%, preferably in the range of from 30 to 50 weight-%, more preferably in the range of from 35 to 45 weight-%.
[0044] It is preferred that the second coating further comprises a non-zeolitic oxidic material, the non-zeolitic oxidic material more preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0045] In the case where the second coating further comprises a non-zeolitic oxidic material, it is preferred that the second coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.-%, more preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the second coating.
[0046] Further in the case where the second coating further comprises a non-zeolitic oxidic material, it is preferred that the non-zeolitic oxidic material is zirconia and wherein preferably the second coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-%, more preferably in the range of from 0.5 to 2 weight-%, based on the weight of the second coating.
[0047] Further in the case where the second coating further comprises a non-zeolitic oxidic material, it is alternatively preferred that the non-zeolitic oxidic material is lanthana and wherein more preferably the second coating comprises lanthana, calculated as the oxide, in the range of from 0.1to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-% based on the weight of the second coating.
[0048] It is preferred that the second coating further comprises an NOx storage component, more preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, preferably consists of, barium oxide.
[0049] In the case where the second coating further comprises an NOx storage component, it is preferred that the second coating comprises the NOx storage component in an amount in the range of from 1 to 15 weight-%, more preferably of from 5 to 12 weight-%, more preferably of from 8 to 10 weight-%, based on the weight of the second coating.
[0050] It is preferred that the second coating is substantially free of platinum, wherein the platinum content of the second coating is more preferably 0.01 weight-% or less, calculated as the element, more preferably 0.001 weight-% or less, more preferably 0.0001 weight-% or less, wherein the second coating is more preferably free of platinum.
[0051] It is preferred that the loading of the second coating, preferably the loading of the second washcoat coating, is in the range of from 1.5 to 5 g / in3, more preferably in the range of from 2 to 3 g / in3, more preferably in the range of from 2.3 to 2.8 g / in3, more preferably in the range of from 2.5 to 2.7 g / in3, more preferably in the range of from 2.55 to 2.65 g / in3.
[0052] It is preferred that the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 2:1 to 3:1, more preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3:1 to 2.5:1.
[0053] Further in the case where that the second coating further comprises an oxygen storage compound, it is preferred that the ratio of the oxygen storage compound loading of the first coating to the oxygen storage compound loading of the second coating is in the range of from 1 :1 to 1:4, more preferably in the range of from 1:1.1 to 1:3.5, more preferably in the range of from 1:1.1 to 1:3, more preferably in the range of from 1:1.1 to 1:2.5, more preferably in the range of from 1:1.1 to 1:2, more preferably in the range of from 1:1.2 to 1:1.9, more preferably in the range of from 1:1.3 to 1:1.7, more preferably in the range of from 1:1.4 to 1:1.6.It is preferred that the ratio of the loading of the first coating to the loading of the second coating, preferably the ratio of the loading of the first washcoat to the loading of the second washcoat, is in the range of from 0.4:1 to 0.89:1, more preferably in the range of from 0.5:1 to 0.88:1, more preferably in the range of from 0.6:1 to 0.87:1, more preferably in the range of from 0.7:1 to 0.86:1, more preferably in the range of from 0.75:1 to 0.85:1.
[0054] It is preferred that the third coating comprises rhodium, more preferably at a loading, calculated as elemental rhodium, in the range of from 1 to 100 g / ft3, more preferably in the range of from 2 to 70 g / ft3, more preferably in the range of from 3 to 50 g / ft3, more preferably in the range of from 4 to 20 g / ft3, more preferably in the range of from 6 to 15 g / ft3, more preferably in the range of from 8 to 12 g / ft3.
[0055] It is preferred that the third coating comprises palladium, more preferably at a loading, calculated as elemental palladium, in the range of from 1 to 100 g / ft3, more preferably in the range of from 2 to 70 g / ft3, more preferably in the range of from 3 to 50 g / ft3, more preferably in the range of from 4 to 20 g / ft3, more preferably in the range of from 6 to 15 g / ft3, more preferably in the range of from 8 to 12 g / ft3.
[0056] It is preferred that the Rh loading to the Pd loading of the third coating is in the range of from 0.5:1 to 5:1, more preferably in the range of from 0.6:1 to 2:1, more preferably in the range of from 0.7:1 to 1.5:1, more preferably in the range of from 0.8:1 to 1.3:1, more preferably in the range of from 0.9: 1 to 1.1 : 1.
[0057] It is preferred that the platinum content, calculated as elemental platinum, of the third coating is 0.01 wt.-% or less, more preferably 0.001 wt.-% or less, more preferably wherein the third coating is free of platinum.
[0058] It is preferred that the third support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the third support material is alumina.
[0059] In the case where the third support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, it is preferred that the third support material comprises one or more rare earth metals,wherein more preferably the one or more rare earth metals are selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.
[0060] It is preferred that the third coating further comprises an oxygen storage compound, the oxygen storage compound more preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprising cerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0061] In the case where the third coating further comprises an oxygen storage compound, it is preferred that the third coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, more preferably in the range of from 0.3 to 2 g / in3, more preferably in the range of from 0.5 to 1.5 g / in3, more preferably in the range of from 0.6 to 1.1 g / in3, more preferably in the range of from 0.7 to 1 g / in3, more preferably in the range of from 0.8 to 0.9 g / in3.
[0062] It is preferred that the third coating further comprises a non-zeolitic oxidic material, the non-zeo-litic oxidic material more preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0063] In the case where the third coating further comprises a non-zeolitic oxidic material, it is preferred that the third coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.-%, preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the third coating.
[0064] Further in the case where the third coating further comprises a non-zeolitic oxidic material, it is preferred that the non-zeolitic oxidic material is zirconia and wherein more preferably the third coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 5 weight-%, more preferably in the range of from 0.3 to 3 weight-%, more preferably in the range of from 0.5 to 2 weight-%, based on the weight of the third coating.Further in the case where the third coating further comprises a non-zeolitic oxidic material, it is alternatively preferred that the non-zeolitic oxidic material is lanthana and wherein more preferably the third coating comprises lanthana, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-% based on the weight of the third coating.
[0065] It is preferred that the coating of the third catalyst further comprises an NOx storage component, more preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, more preferably consists of, barium oxide.
[0066] In the case where the coating of the third catalyst further comprises an NOx storage component, it is preferred that the third coating comprises the NOx storage component in an amount in the range of from 0.1 to 10 weight-%, more preferably of from 0.5 to 7 weight-%, more preferably of from 1 to 5 weight-%, based on the weight of the third coating.
[0067] Further, the present invention relates to a process for preparing a three-way conversion catalyst, preferably the three-way conversion catalyst according to the embodiments of the present invention, the process comprising:
[0068] (a) providing a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end and a plurality of passages defined by internal walls of the substrate extending therethrough;
[0069] (b) preparing a slurry A comprising palladium supported on a first support material, disposing slurry A on the surface of the internal walls of the substrate over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with a first washcoat coating;
[0070] (c) preparing a slurry B comprising palladium supported on a second support material, disposing slurry B on the surface of the internal walls of the substrate over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating and a second washcoat coating;
[0071] (d) preparing a slurry C comprising one or more of rhodium and palladium supported on a third support material, disposing slurry C on the first and second coating over z% of the substrate length, preferably from the inlet end, wherein z is in the range of from 80 to 100, and calciningthe obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating, the second washcoat coating and a third washcoat coating;
[0072] wherein the ratio of the loading of the first washcoat coating disposed on the substrate according to (b) to the loading of the second washcoat coating disposed on the substrate according to (c) is in the range of from 0.3:1 to 0.9:1, wherein the loading is preferably the loading of the washcoat coating after calcining;
[0073] wherein the ratio of the palladium loading of the first washcoat coating to the palladium loading of the second washcoat coating is in the range of from 1.5:1 to 5:1,
[0074] wherein the third washcoat coating is substantially free of platinum.
[0075] It is preferred that (b) comprises
[0076] (b.1) impregnating the palladium on the first support material, preferably on the first support material and an oxygen storage compound, and calcining the palladium on the first support material, more preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, more preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0077] (b.2) mixing the calcined palladium on the first support material obtained according to (b.1) with water, more preferably one or more of alcohols, more preferably a baria precursor, and more preferably a zirconia precursor, obtaining a slurry A;
[0078] (b.3) optionally milling the slurry A obtained according to (b.2);
[0079] (b.4) disposing the slurry A obtained according to (b.2), preferably the milled slurry A obtained according to (b.3), on the surface of the internal walls of the substrate over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70;
[0080] (b.5) optionally drying the slurry-treated substrate obtained according to (b.4);
[0081] (b.6) calcining the slurry-treated substrate obtained according to (b.4), more preferably the dried slurry-treated substrate obtained according to (b.5), obtaining a substrate coated with the first washcoat coating.
[0082] In the case where (b) comprises (b.1), (b.2), (b.3), (b.4), (b.5) and / or (b.6), it is preferred that the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols more preferably comprise, more preferably consist of, n-octanol.
[0083] Further in the case where (b) comprises (b.1), (b.2), (b.3), (b.4), (b.5) and / or (b.6), it is preferred that (b.3) further comprises
[0084] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, more preferably in the range of from 3 to 5, preferably by adding an inorganic acid, more preferably an inorganicacid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.
[0085] Further in the case where (b) comprises (b.1 ), (b.2), (b.3), (b.4), (b.5) and / or (b.6), it is preferred that drying according to (b.5) is performed at a temperature in the range of from 90 to 200 °C, more preferably in the range of from 130 to 170 °C.
[0086] Further in the case where (b) comprises (b.1 ), (b.2), (b.3), (b.4), (b.5) and (b.6), it is preferred that calcining according to (b.6) is performed at a temperature in the range of from 300 to 700°C, more preferably in the range of from 400 to 600 °C.
[0087] Further in the case where (b) comprises (b.1), (b.2), (b.3), (b.4), (b.5) and / or (b.6), it is preferred that the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0088] Further in the case where (b) comprises (b.1 ), (b.2), (b.3), (b.4), (b.5) and / or (b.6), it is preferred that the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.
[0089] It is preferred that (c) comprises
[0090] (c.1) impregnating the palladium on the second support material, preferably on the second support material and an oxygen storage compound, and calcining the palladium on the second support material, more preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, more preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0091] (c.2) mixing the calcined palladium on the second support material obtained according to (c.1) with water, more preferably one or more of alcohols, more preferably a baria precursor, and more preferably a zirconia precursor, obtaining a slurry B;
[0092] (c.3) optionally milling the slurry B obtained according to (c.2);
[0093] (c.4) disposing the slurry B obtained according to (c.2), preferably the milled slurry B obtained according to (c.3), on the surface of the internal walls of the substrate over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70;;
[0094] (c.5) optionally drying the slurry-treated substrate obtained according to (c.4);
[0095] (c.6) calcining the slurry-treated substrate obtained according to (c.4), more preferably the dried slurry-treated substrate obtained according to (c.5), obtaining a substrate coated with the first washcoat coating and the second washcoat coating.Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols more preferably comprise, more preferably consist of, n-octanol.
[0096] Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that (c.3) further comprises
[0097] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, more preferably in the range of from 3 to 5, preferably by adding an inorganic acid, more preferably an inorganic acid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.
[0098] Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that drying according to (c.5) is performed at a temperature in the range of from 90 to 200 °C, more preferably in the range of from 130 to 170 °C.
[0099] Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that calcining according to (c.6) is performed at a temperature in the range of from 300 to 700°C, more preferably in the range of from 400 to 600 °C.
[0100] Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0101] Further in the case where (c) comprises (c.1), (c.2), (c.3), (c.4), (c.5) and / or (c.6), it is preferred that the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.
[0102] It is preferred that (d) comprises
[0103] (d.1) impregnating one or more of rhodium and palladium on the third support material, preferably on the third support material and an oxygen storage compound, and calcining one or more of rhodium and palladium on the third support material, more preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, more preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0104] (d.2) mixing the calcined one or more of rhodium and palladium on the third support material obtained according to (d.1) with water, more preferably one or more of alcohols, more preferably a baria precursor, and more preferably a zirconia precursor, obtaining a slurry C;
[0105] (d.3) optionally milling the slurry C obtained according to (d.2);(d.4) disposing the slurry C obtained according to (d.2), preferably the milled slurry C obtained according to (d.3), on the first and the second coating over z% of the substrate axial length, wherein z is in the range of from 80 to 100;
[0106] (d.5) optionally drying the slurry-treated substrate obtained according to (d.4);
[0107] (d.6) calcining the slurry-treated substrate obtained according to (d.4), more preferably the dried slurry-treated substrate obtained according to (d.5), obtaining a substrate coated with the first washcoat coating, the second washcoat coating, and the third washcoat coating.
[0108] In the case where (d) comprises (d.1), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols more preferably comprise, more preferably consist of, n-octanol.
[0109] Further in the case where (d) comprises (d.1 ), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that (d.3) further comprises
[0110] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, preferably in the range of from 3 to 5, more preferably by adding an inorganic acid, more preferably an inorganic acid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.
[0111] Further in the case where (d) comprises (d.1 ), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that drying according to (d.5) is performed at a temperature in the range of from 90 to 200 °C, more preferably in the range of from 130 to 170 °C.
[0112] Further in the case where (d) comprises (d.1 ), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that calcining according to (d.6) is performed at a temperature in the range of from 300 to 700°C, more preferably in the range of from 400 to 600 °C.
[0113] Further in the case where (d) comprises (d.1 ), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0114] Further in the case where (d) comprises (d.1 ), (d.2), (d.3), (d.4), (d.5) and / or (d.6), it is preferred that the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.It is preferred that z is in the range of from 90 to 100, more preferably in the range of from 95 to 100, more preferably in the range of from 98 to 100, more preferably in the range of from 99 to 100.
[0115] It is preferred that y is in the range of from 30 to 65, more preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0116] It is preferred that z is in the range of from 30 to 65, more preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0117] It is preferred that the slurry C is substantially free of Pt, more preferably wherein the platinum content, calculated as elemental platinum, of the slurry C is 0.01 wt.-% or less, preferably 0.001 wt.-% or less, more preferably wherein the slurry C is free of platinum.
[0118] It is preferred that the ratio of the palladium loading of the first washcoat coating to the palladium loading of the second washcoat coating is in the range of from 2:1 to 3:1, more preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3:1 to 2.5:1.
[0119] It is preferred that the weight-% ratio of palladium comprised in slurry A to palladium comprised in slurry B is in the range of from 2:1 to 3:1, more preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3:1 to 2.5:1.
[0120] It is preferred that the ratio of the loading of the first washcoat coating to the loading of the second washcoat coating is in the range of from 0.4:1 to 0.89:1, more preferably in the range of from 0.5:1 to 0.88:1, more preferably in the range of from 0.6:1 to 0.87:1, more preferably in the range of from 0.7:1 to 0.86:1, more preferably in the range of from 0.75:1 to 0.85:1, wherein the loading is preferably the loading of the washcoat coating after calcining.
[0121] Yet further, the present invention relates to a three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, the three-way conversion catalyst being obtainable or obtained by a process according to the embodiments of the present invention.
[0122] Yet further, the present invention relates an exhaust gas treatment system comprising an internal combustion engine and a three-way conversion catalyst according to the embodiments of the present invention located downstream of the internal combustion engine.
[0123] It is preferred that the internal combustion engine is a spark ignition internal combustion engine, preferably a gasoline internal combustion engine.Yet further, the present invention relates to a method for the treatment of an exhaust gas of an internal combustion engine, comprising providing an exhaust gas from an internal combustion engine and passing said exhaust gas through a catalyst according to the embodiments of the present invention.
[0124] It is preferred that the internal combustion engine is a spark ignition internal combustion engine, preferably a gasoline internal combustion engine
[0125] Yet further, the present invention relates to an use of a catalyst according to the embodiments of the present invention for the treatment of an exhaust gas of an internal combustion engine, preferably of a spark ignition internal combustion engine, more preferably of a gasoline internal combustion engine.
[0126] The present invention is further illustrated by the following set of embodiments and combinations of embodiments resulting from the dependencies and back-references as indicated. In particular, it is noted that in each instance where a range of embodiments is mentioned, for example in the context of a term such as “The three-way conversion catalyst of any one of embodiments 1 to 4”, every embodiment in this range is meant to be explicitly disclosed for the skilled person, i.e. the wording of this term is to be understood by the skilled person as being synonymous to “The three-way conversion catalyst of any one of embodiments 1, 2, 3, and 4”. Further, it is explicitly noted that the following set of embodiments represents a suitable structured part of the general description directed to preferred aspects of the present invention, and, thus, suitably supports, but does not represent the claims of the present invention.
[0127] 1. A three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, preferably for the treatment of an exhaust gas from an internal combustion engine, more preferably a gasoline engine, the catalyst comprising:
[0128] (i) a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end, and a plurality of passages defined by internal walls of the substrate extending therethrough;
[0129] (ii) a first coating, preferably a first washcoat coating, comprising palladium supported on a first support material;
[0130] (iii) a second coating, preferably a second washcoat coating, comprising palladium supported on a second support material;
[0131] (iv) a third coating, preferably a third washcoat coating, comprising one or more of rhodium and palladium supported on a third support material;wherein the first coating extends over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70;
[0132] wherein the second coating extends over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70;
[0133] wherein the ratio of the loading of the first coating to the loading of the second coating, preferably the ratio of the loading of the first washcoat coating to the loading of the second washcoat coating, is in the range of from 0.3:1 to 0.9:1;
[0134] wherein the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 1.5:1 to 5:1,
[0135] wherein the third coating is disposed on the first and the second coatings over z% of the substrate axial length, preferably from the inlet end, wherein z is in the range of from 80 to 100; and
[0136] wherein the third coating is substantially free of platinum.
[0137] 2. The three-way conversion catalyst of embodiment 1 , wherein x is in the range of from 30 to 65, preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0138] 3. The three-way conversion catalyst of embodiment 1 or 2, wherein y is in the range of from 30 to 65, preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0139] 4. The three-way conversion catalyst of any one of embodiments 1 to 3, wherein z is in the range of from 85 to 100, preferably in the range of from 90 to 100, more preferably in the range of from 95 to 100, more preferably in the range of from 98 to 100, more preferably in the range of from 99 to 100.
[0140] 5. The three-way conversion catalyst of any one of embodiments 1 to 4, wherein the first coating comprises palladium, calculated as elemental palladium, at a loading in the range of from 50 to 250 g / ft3, preferably in the range of from 100 to 220 g / ft3, more preferably in the range of from 140 to 200 g / ft3, more preferably in the range of from 150 to 190 g / ft3, more preferably in the range of from 160 to 180 g / ft3.
[0141] 6. The three-way conversion catalyst of any one of embodiments 1 to 5, wherein the first support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from thegroup consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the first support material is alumina.
[0142] 7. The three-way conversion catalyst of embodiment 6, wherein the first support material comprises one or more rare earth metals, wherein the one or more rare earth metals are preferably selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.
[0143] 8. The three-way conversion catalyst of any one of embodiments 1 to 7, wherein the first coating further comprises an oxygen storage compound, the oxygen storage compound preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprising cerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0144] 9. The three-way conversion catalyst of embodiment 8, wherein the first coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, preferably in the range of from 0.5 to 2 g / in3, more preferably in the range of from 0.6 to 1.5 g / in3, more preferably in the range of from 0.7 to 1.3 g / in3, more preferably in the range of from 0.8 to 1.2 g / in3, more preferably in the range of from 0.9 to 1.1 g / in3.
[0145] 10. The three way conversion catalyst of embodiment 8 or 9, wherein the cerium content, calculated as CeC>2, of the mixed oxide comprising cerium is in the range of from 5 to 50 weight-%, preferably in the range of from 10 to 40 weight-%, more preferably in the range of from 20 to 30 weight-%.
[0146] 11. The three-way conversion catalyst of any one of embodiments 1 to 10, wherein the first coating further comprises a non-zeolitic oxidic material, the non-zeolitic oxidic material preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0147] 12. The three-way conversion catalyst of embodiment 11, wherein the first coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.-%, preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the first coating.
[0148] 13. The three-way conversion catalyst of embodiment 11 or 12, wherein the non-zeolitic oxidic material is zirconia and wherein preferably the first coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-%, more preferably in the range of from 1 to 2 weight-%, based on the weight of the first coating.
[0149] 14. The three-way conversion catalyst of any one of embodiments 11 to 13, wherein the non- zeolitic oxidic material is lanthana and wherein preferably the first coating comprises lanthana, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight- % based on the weight of the first coating.
[0150] 15. The three-way conversion catalyst of any one of embodiments 1 to 14, wherein the first coating further comprises an NOx storage component, preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, preferably consists of, barium oxide.
[0151] 16. The three-way conversion catalyst of embodiment 15, wherein the first coating comprises the NOx storage component in an amount in the range of from 1 to 20 weight-%, preferably of from 5 to 17 weight-%, more preferably of from 10 to 15 weight-%, based on the weight of the first coating.
[0152] 17. The three-way conversion catalyst of any one of embodiments 1 to 16, wherein the first coating is substantially free of platinum, wherein the platinum content of the second coating is preferably 0.01 weight-% or less, calculated as the element, more preferably 0.001 weight-% or less, more preferably 0.0001 weight-% or less, wherein the first coating is more preferably free of platinum.
[0153] 18. The three-way conversion catalyst of any one of embodiments 1 to 17, wherein the loading of the first coating, preferably the loading of the first washcoat coating, is in the range of from 1 to 5 g / in3, preferably in the range of from 1.5 to 2.5 g / in3, more preferably in therange of from 1.7 to 2.4 g / in3, more preferably in the range of from 1.9 to 2.2 g / in3, more preferably in the range of from 2 to 2.1 g / in3.
[0154] The three-way conversion catalyst of any one of embodiments 1 to 18, wherein the second coating comprises palladium, calculated as elemental palladium, at a loading in the range of from 1 to 150 g / ft3, preferably in the range of from 20 to 120 g / ft3, more preferably in the range of from 40 to 100 g / ft3, more preferably in the range of from 50 to 90 g / ft3, more preferably in the range of from 60 to 80 g / ft3.
[0155] The three-way conversion catalyst of any one of embodiments 1 to 19, wherein the second support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the second support material is alumina.
[0156] The three-way conversion catalyst of embodiment 20, wherein the second support material comprises one or more rare earth metals, wherein preferably the one or more rare earth metals are selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.
[0157] The three-way conversion catalyst of any one of embodiments 1 to 21 , wherein the second coating further comprises an oxygen storage compound, the oxygen storage compound preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprising cerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0158] The three-way conversion catalyst of embodiment 22, wherein the second coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, preferably in the range of from 0.5 to 2.5 g / in3, more preferably in the range of from 1 to 2 g / in3, more preferably in the range of from 1.2 to 1.8 g / in3, more preferably in the range of from 1.3 to 1.7 g / in3, more preferably in the range of from 1.4 to 1.6 g / in3.The three way conversion catalyst of embodiment 22 or 23, wherein the cerium content, calculated as CeC>2, of the mixed oxide comprising cerium is in the range of from 20 to 60 weight-%, preferably in the range of from 30 to 50 weight-%, more preferably in the range of from 35 to 45 weight-%.
[0159] The three-way conversion catalyst of any one of embodiments 1 to 24, wherein the second coating further comprises a non-zeolitic oxidic material, the non-zeolitic oxidic material preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0160] The three-way conversion catalyst of embodiment 25, wherein the second coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.-%, preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the second coating.
[0161] The three-way conversion catalyst of embodiment 25 or 26, wherein the non-zeolitic oxidic material is zirconia and wherein preferably the second coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-%, more preferably in the range of from 0.5 to 2 weight-%, based on the weight of the second coating.
[0162] The three-way conversion catalyst of any one of embodiments 25 to 27, wherein the non-zeolitic oxidic material is lanthana and wherein preferably the second coating comprises lanthana, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably in the range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-% based on the weight of the second coating.
[0163] The three-way conversion catalyst of any one of embodiments 1 to 28, wherein the second coating further comprises an NOx storage component, preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, preferably consists of, barium oxide.The three-way conversion catalyst of embodiment 29, wherein the second coating comprises the NOx storage component in an amount in the range of from 1 to 15 weight-%, preferably of from 5 to 12 weight-%, more preferably of from 8 to 10 weight-%, based on the weight of the second coating.
[0164] The three-way conversion catalyst of any one of embodiments 1 to 30, wherein the second coating is substantially free of platinum, wherein the platinum content of the second coating is preferably 0.01 weight-% or less, calculated as the element, more preferably 0.001 weight-% or less, more preferably 0.0001 weight-% or less, wherein the second coating is more preferably free of platinum.
[0165] The three-way conversion catalyst of any one of embodiments 1 to 31 , wherein the loading of the second coating, preferably the loading of the second washcoat coating, is in the range of from 1.5 to 5 g / in3, preferably in the range of from 2 to 3 g / in3, more preferably in the range of from 2.3 to 2.8 g / in3, more preferably in the range of from 2.5 to 2.7 g / in3, more preferably in the range of from 2.55 to 2.65 g / in3.
[0166] The three-way conversion catalyst of any one of embodiments 1 to 32, wherein the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 2:1 to 3:1, preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3:1 to 2.5:1.
[0167] The three-way conversion catalyst of any one of embodiments 22 to 33, wherein the ratio of the oxygen storage compound loading of the first coating to the oxygen storage compound loading of the second coating is in the range of from 1:1 to 1:4, preferably in the range of from 1:1.1 to 1:4, more preferably in the range of from 1:1.1 to 1:3.5, more preferably in the range of from 1:1.1 to 1:3, more preferably in the range of from 1:1.1 to 1:2.5, more preferably in the range of from 1:1.1 to 1:2, more preferably in the range of from 1:1.2 to 1:1.9, more preferably in the range of from 1:1.3 to 1:1.7, more preferably in the range of from 1:1.4 to 1:1.6.
[0168] The three way conversion catalyst of any one of embodiments 1 to 34, wherein the ratio of the loading of the first coating to the loading of the second coating, preferably the ratio of the loading of the first washcoat to the loading of the second washcoat, is in the range of from 0.4:1 to 0.89:1, preferably in the range of from 0.5:1 to 0.88:1, more preferably in the range of from 0.6:1 to 0.87:1, more preferably in the range of from 0.7:1 to 0.86:1, more preferably in the range of from 0.75:1 to 0.85:1.The three-way conversion catalyst of any one of embodiments 1 to 35, wherein the third coating comprises rhodium, preferably at a loading, calculated as elemental rhodium, in the range of from 1 to 100 g / ft3, more preferably in the range of from 2 to 70 g / ft3, more preferably in the range of from 3 to 50 g / ft3, more preferably in the range of from 4 to 20 g / ft3, more preferably in the range of from 6 to 15 g / ft3, more preferably in the range of from 8 to 12 g / ft3.
[0169] The three-way conversion catalyst of any one of embodiments 1 to 36, wherein the third coating comprises palladium, preferably at a loading, calculated as elemental palladium, in the range of from 1 to 100 g / ft3, more preferably in the range of from 2 to 70 g / ft3, more preferably in the range of from 3 to 50 g / ft3, more preferably in the range of from 4 to 20 g / ft3, more preferably in the range of from 6 to 15 g / ft3, more preferably in the range of from 8 to 12 g / ft3.
[0170] The three-way conversion catalyst of any one of embodiments 1 to 37, wherein the ratio of the Rh loading to the Pd loading of the third coating is in the range of from 0.5:1 to 5:1, preferably in the range of from 0.6:1 to 2:1, more preferably in the range of from 0.7:1 to 1.5:1, more preferably in the range of from 0.8:1 to 1.3:1, more preferably in the range of from 0.9:1 to 1.1:1.
[0171] The three-way conversion catalyst of any one of embodiments 1 to 38, wherein the platinum content, calculated as elemental platinum, of the third coating is 0.01 wt.-% or less, preferably 0.001 wt.-% or less, more preferably wherein the third coating is free of platinum.
[0172] The three-way conversion catalyst of any one of embodiments 1 to 39, wherein the third support material is selected from the group consisting of alumina, ceria, silica, zirconia, titania, a mixture of two or more thereof, and a mixed oxide of two or more thereof, preferably selected from the group consisting of alumina, ceria, zirconia, a mixture of two or more thereof, and a mixed oxide of two or more thereof, more preferably selected from the group consisting of alumina, zirconia, a mixture thereof, and a mixed oxide thereof, more preferably wherein the third support material is alumina.
[0173] The three-way conversion catalyst of embodiment 40, wherein the third support material comprises one or more rare earth metals, wherein preferably the one or more rare earth metals are selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, and mixtures of two or more thereof, more preferably from the group consisting of La, Ce, and mixtures thereof, more preferably wherein the one or more rare earth metal is lanthanum.42. The three-way conversion catalyst of any one of embodiments 1 to 41 , wherein the third coating further comprises an oxygen storage compound, the oxygen storage compound preferably comprises cerium, more preferably comprises one or more of a cerium oxide, a mixture of oxides comprising cerium and a mixed oxide comprising cerium, wherein the mixed oxide comprising cerium more preferably further comprises one or more of zirconium, yttrium, neodymium, lanthanum, hafnium, samarium, and praseodymium, more preferably one or more of zirconium, yttrium, neodymium, lanthanum, and praseodymium, more preferably zirconium.
[0174] 43. The three-way conversion catalyst of embodiment 42, wherein the third coating comprises the oxygen storage compound at a loading in the range of from 0.1 to 3 g / in3, preferably in the range of from 0.3 to 2 g / in3, more preferably in the range of from 0.5 to 1.5 g / in3, more preferably in the range of from 0.6 to 1.1 g / in3, more preferably in the range of from 0.7 to 1 g / in3, more preferably in the range of from 0.8 to 0.9 g / in3.
[0175] 44. The three-way conversion catalyst of any one of embodiments 1 to 43, wherein the third coating further comprises a non-zeolitic oxidic material, the non-zeolitic oxidic material preferably comprises one or more of zirconia, alumina, ceria, titania, silica, lanthana, and a mixed oxide comprising one or more of zirconia, alumina, lanthana, and silica, more preferably comprises one or more of zirconia and lanthana, more preferably comprises zirconia and lanthana.
[0176] 45. The three-way conversion catalyst of embodiment 44, wherein the third coating comprises the non-zeolitic oxidic material, calculated as the oxide, in the range of from 0.1 to 10 wt.- %, preferably of from 0.3 to 7 weight-%, more preferably of from 0.5 to 5 weight-%, based on the weight of the third coating.
[0177] 46. The three-way conversion catalyst of embodiment 44 or 45, wherein the non-zeolitic oxidic material is zirconia and wherein preferably the third coating comprises zirconia, calculated as the oxide, in the range of from 0.1 to 5 weight-%, more preferably in the range of from 0.3 to 3 weight-%, more preferably in the range of from 0.5 to 2 weight-%, based on the weight of the third coating.
[0178] 47. The three-way conversion catalyst of any one of embodiments 44 to 46, wherein the non- zeolitic oxidic material is lanthana and wherein preferably the third coating comprises lanthana, calculated as the oxide, in the range of from 0.1 to 7 weight-%, more preferably inthe range of from 0.3 to 5 weight-%, more preferably in the range of from 0.5 to 3 weight-% based on the weight of the third coating.
[0179] The three-way conversion catalyst of any one of embodiments 1 to 47, wherein the coating of the third catalyst further comprises an NOx storage component, preferably wherein the NOx storage component comprises one or more of an oxide of an alkali earth metal and an oxide of an alkali metal, more preferably wherein the NOx storage component comprises an oxide selected from the group consisting of Mg, Ca, Sr, Ba, Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably an oxide selected from the group consisting of Mg, Ca, Sr, and Ba, more preferably wherein the NOx storage component comprises, preferably consists of, barium oxide.
[0180] The three-way conversion catalyst of embodiment 48, wherein the third coating comprises the NOx storage component in an amount in the range of from 0.1 to 10 weight-%, preferably of from 0.5 to 7 weight-%, more preferably of from 1 to 5 weight-%, based on the weight of the third coating.
[0181] A process for preparing a three-way conversion catalyst, preferably the three-way conversion catalyst according to any one of embodiments 1 to 49, the process comprising:
[0182] (a) providing a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end and a plurality of passages defined by internal walls of the substrate extending therethrough;
[0183] (b) preparing a slurry A comprising palladium supported on a first support material, disposing slurry A on the surface of the internal walls of the substrate over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with a first washcoat coating;
[0184] (c) preparing a slurry B comprising palladium supported on a second support material, disposing slurry B on the surface of the internal walls of the substrate over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating and a second washcoat coating;
[0185] (d) preparing a slurry C comprising one or more of rhodium and palladium supported on a third support material, disposing slurry C on the first and second coating over z% of the substrate length, preferably from the inlet end, wherein z is in the range of from 80 to 100, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating, the second washcoat coating and a third washcoat coating;wherein the ratio of the loading of the first washcoat coating disposed on the substrate according to (b) to the loading of the second washcoat coating disposed on the substrate according to (c) is in the range of from 0.3:1 to 0.9:1, wherein the loading is preferably the loading of the washcoat coating after calcining;
[0186] wherein the ratio of the palladium loading of the first washcoat coating to the palladium loading of the second washcoat coating is in the range of from 1.5:1 to 5:1,
[0187] wherein the third washcoat coating is substantially free of platinum.
[0188] The process of embodiment 50, wherein (b) comprises
[0189] (b.1) impregnating the palladium on the first support material, preferably on the first support material and an oxygen storage compound, and calcining the palladium on the first support material, preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0190] (b.2) mixing the calcined palladium on the first support material obtained according to (b.1) with water, preferably one or more of alcohols, preferably a baria precursor, and preferably a zirconia precursor, obtaining a slurry A;
[0191] (b.3) optionally milling the slurry A obtained according to (b.2);
[0192] (b.4) disposing the slurry A obtained according to (b.2), preferably the milled slurry A obtained according to (b.3), on the surface of the internal walls of the substrate over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70;
[0193] (b.5) optionally drying the slurry-treated substrate obtained according to (b.4);
[0194] (b.6) calcining the slurry-treated substrate obtained according to (b.4), preferably the dried slurry-treated substrate obtained according to (b.5), obtaining a substrate coated with the first washcoat coating.
[0195] The process of embodiment 51 , wherein the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols preferably comprise, more preferably consist of, n-octanol.
[0196] The process of embodiment 51 or 52, wherein (b.3) further comprises
[0197] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, preferably in the range of from 3 to 5, preferably by adding an inorganic acid, more preferably an inorganic acid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.54. The process of any one of embodiments 51 to 53, wherein drying according to (b.5) is performed at a temperature in the range of from 90 to 200 °C, preferably in the range of from 130 to 170 °C.
[0198] 55. The process of any one of embodiments 51 to 54, wherein calcining according to (b.6) is performed at a temperature in the range of from 300 to 700°C, preferably in the range of from 400 to 600 °C.
[0199] 56. The process of any one of embodiments 51 to 55, wherein the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0200] 57. The process of any one of embodiments 51 to 56, wherein the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.
[0201] 58. The process of any one of embodiments 50 to 57, wherein (c) comprises
[0202] (c.1) impregnating the palladium on the second support material, preferably on the second support material and an oxygen storage compound, and calcining the palladium on the second support material, preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0203] (c.2) mixing the calcined palladium on the second support material obtained according to (c.1) with water, preferably one or more of alcohols, preferably a baria precursor, and preferably a zirconia precursor, obtaining a slurry B;
[0204] (c.3) optionally milling the slurry B obtained according to (c.2);
[0205] (c.4) disposing the slurry B obtained according to (c.2), preferably the milled slurry B obtained according to (c.3), on the surface of the internal walls of the substrate over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70;;
[0206] (c.5) optionally drying the slurry-treated substrate obtained according to (c.4);
[0207] (c.6) calcining the slurry-treated substrate obtained according to (c.4), preferably the dried slurry-treated substrate obtained according to (c.5), obtaining a substrate coated with the first washcoat coating and the second washcoat coating.
[0208] 59. The process of embodiment 58, wherein the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols preferably comprise, more preferably consist of, n-octanol.60. The process of embodiment 58 or 59, wherein (c.3) further comprises
[0209] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, preferably in the range of from 3 to 5, preferably by adding an inorganic acid, more preferably an inorganic acid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.
[0210] 61. The process of any one of embodiments 58 to 60, wherein drying according to (c.5) is performed at a temperature in the range of from 90 to 200 °C, preferably in the range of from 130 to 170 °C.
[0211] 62. The process of any one of embodiments 58 to 61, wherein calcining according to (c.6) is performed at a temperature in the range of from 300 to 700°C, preferably in the range of from 400 to 600 °C.
[0212] 63. The process of any one of embodiments 58 to 62, wherein the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0213] 64. The process of any one of embodiments 58 to 63, wherein the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.
[0214] 65. The process of any one of embodiments 50 to 64, wherein (d) comprises
[0215] (d.1) impregnating one or more of rhodium and palladium on the third support material, preferably on the third support material and an oxygen storage compound, and calcining one or more of rhodium and palladium on the third support material, preferably in a gas atmosphere having a temperature in the range of from 300 to 800 °C, preferably in the range of from 400 to 700 °C, more preferably in the range of from 450 to 600 °C;
[0216] (d.2) mixing the calcined one or more of rhodium and palladium on the third support material obtained according to (d.1) with water, preferably one or more of alcohols, preferably a baria precursor, and preferably a zirconia precursor, obtaining a slurry C;
[0217] (d.3) optionally milling the slurry C obtained according to (d.2);
[0218] (d.4) disposing the slurry C obtained according to (d.2), preferably the milled slurry C obtained according to (d.3), on the first and the second coating over z% of the substrate axial length, wherein z is in the range of from 80 to 100;
[0219] (d.5) optionally drying the slurry-treated substrate obtained according to (d.4);
[0220] (d.6) calcining the slurry-treated substrate obtained according to (d.4), preferably the driedslurry-treated substrate obtained according to (d.5), obtaining a substrate coated with the first washcoat coating, the second washcoat coating, and the third washcoat coating.
[0221] The process of embodiment 65, wherein the one or more alcohols is selected from the group consisting of pentanol, hexanol, heptanol, octanol and nonanol, wherein the one or more alcohols preferably comprise, more preferably consist of, n-octanol.
[0222] The process of embodiment 65 or 66, wherein (d.3) further comprises
[0223] (i) adjusting the pH of the milled slurry to a value in the range of from 2 to 7, preferably in the range of from 3 to 5, preferably by adding an inorganic acid, more preferably an inorganic acid selected from the group consisting of HCI, H2SO4, HNO3 and H2CO3, wherein the inorganic acid preferably comprises, more preferably consists of, HNO3.
[0224] The process of any one of embodiments 65 to 67, wherein drying according to (d.5) is performed at a temperature in the range of from 90 to 200 °C, preferably in the range of from 130 to 170 °C.
[0225] The process of any one of embodiments 65 to 68, wherein calcining according to (d.6) is performed at a temperature in the range of from 300 to 700°C, preferably in the range of from 400 to 600 °C.
[0226] The process of any one of embodiments 65 to 69, wherein the baria precursor is selected from the group consisting of barium acetate, barium sulfate, barium nitrate, and mixtures of two or more thereof.
[0227] The process of any one of embodiments 65 to 70, wherein the zirconia precursor is selected from the group consisting of zirconium acetate, zirconium sulfate, zirconium nitrate, and mixtures of two or more thereof.
[0228] The process of any one of embodiments 50 to 71, wherein z is in the range of from 90 to 100, preferably in the range of from 95 to 100, more preferably in the range of from 98 to 100, more preferably in the range of from 99 to 100.
[0229] The process of any one of embodiments 50 to 72, wherein y is in the range of from 30 to 65, preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.
[0230] The process of any one of embodiments 50 to 73, wherein z is in the range of from 30 to 65, preferably in the range of from 40 to 60, more preferably in the range of from 45 to 55.The process of any one of embodiments 50 to 74, wherein the slurry C is substantially free of Pt, preferably wherein the platinum content, calculated as elemental platinum, of the slurry C is 0.01 wt.-% or less, preferably 0.001 wt.-% or less, more preferably wherein the slurry C is free of platinum.
[0231] The process of any one of embodiments 50 to 75, wherein the ratio of the palladium loading of the first washcoat coating to the palladium loading of the second washcoat coating is in the range of from 2:1 to 3:1, preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3: 1 to 2.5: 1.
[0232] The process of any one of embodiments 50 to 76, wherein the weight-% ratio of palladium comprised in slurry A to palladium comprised in slurry B is in the range of from 2:1 to 3:1, preferably in the range of from 2.1:1 to 2.7:1, more preferably in the range of from 2.3:1 to 2.5:1.
[0233] The process any one of embodiments 50 to 77 wherein the ratio of the loading of the first washcoat coating to the loading of the second washcoat coating is in the range of from 0.4:1 to 0.89:1, preferably in the range of from 0.5:1 to 0.88:1, more preferably in the range of from 0.6:1 to 0.87:1, more preferably in the range of from 0.7:1 to 0.86:1, more preferably in the range of from 0.75:1 to 0.85:1, wherein the loading is preferably the loading of the washcoat coating after calcining.
[0234] A three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, the three-way conversion catalyst being obtainable or obtained by a process according to any one of embodiments 50 to 78.
[0235] An exhaust gas treatment system comprising an internal combustion engine and a three-way conversion catalyst according to any one of embodiments 1 to 49 and 79 located downstream of the internal combustion engine.
[0236] The exhaust gas treatment system of embodiment 80, wherein the internal combustion engine is a spark ignition internal combustion engine, preferably a gasoline internal combustion engine.
[0237] A method for the treatment of an exhaust gas of an internal combustion engine, comprising providing an exhaust gas from an internal combustion engine and passing said exhaust gas through a catalyst according to any one of embodiments 1 to 49 and 79.83. The method of embodiment 82, wherein the internal combustion engine is a spark ignition internal combustion engine, preferably a gasoline internal combustion engine
[0238] 84. Use of a catalyst according to any one of embodiments 1 to 49 and 79 for the treatment of an exhaust gas of an internal combustion engine, preferably of a spark ignition internal combustion engine, more preferably of a gasoline internal combustion engine.
[0239] The present invention is further illustrated by the following examples.
[0240] EXAMPLES
[0241] Comparative Example 1 : Preparation of a three-way conversion catalyst not according to the present invention
[0242] Bottom inlet coating
[0243] An aqueous mixture of palladium salt precursors was impregnated on high porosity alumina and ceria-zirconia. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0244] A second mixture was prepared by mixing water, n-octanol and a precursor of baria was added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 5-8 wt.-% based on the weight of the coating. The obtained calcined Pd on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0245] The obtained slurry was disposed over half of a non-coated ceramic honeycomb flow-through substrate from the inlet (diameter: 4.66 inches x length: 4.5 inches, cylindrical shaped substrate with 750 cells per square inch and 0.0635 millimeter (2.5 mil) wall thickness), dried at 150 °C and further calcined at 500 °C in air. The final inlet coating comprises high porosity alumina, ceria-zirconia, Pd (final loading of Pd in the catalyst was 1-3 wt.-% based on the weight of the coating) and baria. The loading of the inlet coating is about 2.0 to 2.5 g / in3.
[0246] Bottom outlet coatingAn aqueous mixture of palladium salt precursors were impregnated on high porosity alumina and ceria-zirconia. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0247] A second mixture was prepared by mixing water, n-octanol and a precursor of baria was added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 5-8 wt.-% based on the weight of the coating. The obtained calcined Pd on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0248] The obtained slurry was disposed over half of the inlet-coated ceramic honeycomb flow-through substrate from the outlet, dried at 150 °C and further calcined at 500 °C in air. The final inlet coating comprises high porosity alumina, ceria-zirconia, Pd (final loading of Pd in the catalyst was 1-3 wt.-% based on the weight of the coating) and baria. The loading of the outlet coating was about 2.0 to 2.5 g / in3.
[0249] The ratio of Pd of the inlet coating to Pd of the outlet coating was 2:1
[0250] Top coating
[0251] An aqueous mixture of palladium and rhodium salt precursors (weight ratio of Pd:Rh: 1:1) were impregnated on high porosity La-doped alumina and ceria-zirconia. The obtained mixture of Pd / Rh on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0252] A second mixture was prepared by mixing water, n-octanol and a precursor of baria and zirconia were added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 3-6 wt.-% based on the weight of the coating and the amount of zirconia precursor was calculated such that the final loading of ZrO2 in the catalyst after calcination was 0.5-2 wt.-% based on the weight of the coating. The obtained calcined Pd / Rh on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0253] The obtained slurry was disposed over the bottom inlet and bottom outlet coating, dried at 150 °C and further calcined at 500 °C in air. The final coating comprises high porosity La-doped alumina, ceria-zirconia, Pd, Rh, zirconia and baria. The loading of the top coating is about 1.25 to 1.7 g / in3.Example 1 : Preparation of a three-way conversion catalyst according to the present invention
[0254] Bottom inlet coating
[0255] An aqueous mixture of palladium salt precursors were impregnated on high porosity La-doped alumina and ceria-zirconia. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0256] A second mixture was prepared by mixing water, n-octanol and a precursor of baria and zirconia were added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 3-6 wt.-% based on the weight of the coating and the amount of zirconia precursor was calculated such that the final loading of ZrC>2 in the catalyst after calcination was 1-2 wt.-% based on the weight of the coating. The obtained calcined Pd on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0257] The obtained slurry was disposed over half of a non-coated ceramic honeycomb flow-through substrate from the inlet (diameter: 4.66 inches x length: 4.5 inches, cylindrical shaped substrate with 750 cells per square inch (CPSI) and 0.0635 millimeter (2.5 mil) wall thickness), dried at 150 °C and further calcined at 500 °C in air. The final inlet coating comprises high porosity La-doped alumina, ceria-zirconia (final loading of Ce2O in the catalyst was 8-12 wt.-% based on the weight of the coating), Pd (final loading of Pd in the catalyst was 3-6 wt.-% based on the weight of the coating), zirconia and baria. The loading of the inlet coating is about 1.8 to 2.2 g / in3.
[0258] Bottom outlet coating
[0259] An aqueous mixture of palladium salt precursors was impregnated on high porosity La-doped alumina and ceria-zirconia. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0260] A second mixture was prepared by mixing water, n-octanol and a precursor of baria and zirconia were added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 8-10 wt.-% based on the weight of the coating and the amount of zirconia precursor was calculated such that the final loading of ZrO2 in the catalyst after calcination was 0.5-2 wt.-% based on the weight of the coating. The obtained calcined Pdon alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0261] The obtained slurry was disposed over half of the inlet-coated ceramic honeycomb flow-through substrate from the outlet, dried at 150 °C and further calcined at 500 °C in air. The final outlet coating comprises high porosity La-doped alumina, ceria-zirconia (final loading of Ce2O in the catalyst was 18-24 wt.-% based on the weight of the coating), Pd (final loading of Pd in the catalyst was 1-2 wt.-% based on the weight of the coating), zirconia and baria. The loading of the outlet coating was about 2.35 to 2.65 g / in3.
[0262] The ratio of Pd of the inlet coating to Pd of the outlet coating was 2.4:1.
[0263] Top coating
[0264] An aqueous mixture of palladium and rhodium salt precursors (weight ratio of Pd:Rh: 1:1) were impregnated on high porosity alumina and ceria-zirconia. The obtained mixture of Pd / Rh on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0265] A second mixture was prepared by mixing water, n-octanol and a precursor of zirconia was added. The amount of the zirconia precursor was calculated such that the final loading of ZrC>2 in the catalyst after calcination was 0.5-2 wt.-% based on the weight of the coating. The obtained calcined Pd / Rh on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0266] The obtained slurry was disposed over the bottom inlet and bottom outlet coating, dried at 150 °C and further calcined at 500 °C in air. The final coating comprises high porosity alumina, ceria-zirconia, Pd, Rh, and zirconia. The loading of the top coating is about 1.75 to 1.95 g / in3.
[0267] Example 2: Preparation of a three-way conversion catalyst according to the present invention
[0268] Bottom inlet coating
[0269] An aqueous mixture of palladium salt precursors were impregnated on high porosity La-doped alumina and ceria-zirconia. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.A second mixture was prepared by mixing water, n-octanol and a precursor of baria and zirconia were added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 10-15 wt.-% based on the weight of the coating and the amount of zirconia precursor was calculated such that the final loading of ZrC>2 in the catalyst after calcination was 1-3 wt.-% based on the weight of the coating. The obtained calcined Pd on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0270] The obtained slurry was disposed over half of a non-coated ceramic honeycomb flow-through substrate from the inlet (diameter: 4.66 inches x length: 4.5 inches, cylindrical shaped substrate with 750 cells per square inch and 0.0635 millimeter (2.5 mil) wall thickness), dried at 150 °C and further calcined at 500 °C in air. The final inlet coating comprises high porosity La-doped alumina, ceria-zirconia (final loading of Ce2O in the catalyst was 8-12 wt.-% based on the weight of the coating), Pd (final loading of Pd in the catalyst was 4-6 wt.-% based on the weight of the coating), zirconia and baria. The loading of the inlet coating is about 1.85 to 2.15 g / in3.
[0271] Bottom outlet coating
[0272] An aqueous mixture of palladium salt precursors were impregnated on high porosity La-doped alumina and a different ceria-zirconia compared to Example 1. The obtained mixture of Pd on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0273] A second mixture was prepared by mixing water, n-octanol and a precursor of baria and zirconia were added. The amount of the baria precursor was calculated such that the final loading of BaO in the catalyst after calcination was 8-10 wt.-% based on the weight of the coating and the amount of zirconia precursor was calculated such that the final loading of ZrO2 in the catalyst after calcination was 0.5-2 wt.-% based on the weight of the coating. The obtained calcined Pd on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0274] The obtained slurry was disposed over half of the inlet-coated ceramic honeycomb flow-through substrate from the outlet, dried at 150 °C and further calcined at 500 °C in air. The final outlet coating comprises high porosity La-doped alumina, ceria-zirconia (final loading of Ce2O in thecatalyst was 18-24 wt.-% based on the weight of the coating), Pd (final loading of Pd in the catalyst was 1-2 wt.-% based on the weight of the coating), zirconia and baria. The loading of the outlet coating was about 2.55 to 2.65 g / in3.
[0275] The ratio of Pd of the inlet coating to Pd of the outlet coating was 2.4:1.
[0276] Top coating
[0277] An aqueous mixture of palladium and rhodium salt precursors (weight ratio of Pd:Rh: 1:1) were impregnated on high porosity alumina and ceria-zirconia. The obtained mixture of Pd / Rh on alumina and ceria-zirconia was calcined at 500 °C for 2 hours.
[0278] A second mixture was prepared by mixing water, n-octanol and a precursor of zirconia was added. The amount of the zirconia precursor was calculated such that the final loading of ZrC>2 in the catalyst after calcination was 0.5-2 wt.-% based on the weight of the coating. The obtained calcined Pd / Rh on alumina and ceria-zirconia was added to the second mixture obtaining a slurry. The slurry content was adjusted to 35-45 weight-% and wet milled. After milling, the pH of the slurry was adjusted by adding nitric acid to have a pH of 3-5.
[0279] The obtained slurry was disposed over the bottom inlet and bottom outlet coating, dried at 150 °C and further calcined at 500 °C in air. The final coating comprises high porosity alumina, ceria-zirconia, Pd, Rh, and zirconia. The loading of the top coating is about 1.85 to 1.95 g / in3.
[0280] Example 3: Testing the three-way conversion catalysts according to Examples 1, 2, and comparative Example 1
[0281] The system and consequently component evaluation (WLTC) was carried out on a 2I Euro 6 GTDI engine bench test cell. The latter is fitted with thermos-elements and FT-IR units at the engine out / catalyst inlet, catalyst bed and outlet positions, allowing for accurate recording of temperatures and gaseous emissions along the exhaust line.
[0282] Figures 1-3 present the cumulated HC (hydrocarbon), CO and NOXemissions for each tested system using the WLTC cycle collected on the engine described above. As may be taken from Figure 1 , the cumulated HC emissions obtained with the comparative system are significantly higher compared to those of the inventive systems comprising the catalysts according to inventive examples 1 and 2 during cold start and high speed / temperatures. The best tailpipe results were obtained with the inventive example 1. As may be taken from Figure 2, the cumu-lated CO emissions obtained with the comparative system are much higher than for the inventive systems. The best tailpipe results were obtained with the system comprising the catalyst according to example 1. Furthermore, as may be taken from Figure 3, the cumulated NOx emissions obtained with the comparative system are higher than the inventive systems comprising the catalyst according to Example 1 and 2; from cold start until end of test cycle. In particular, from figure 3, the cumulated NOXtailpipe emissions of the comparative catalyst show significant NOx breakthroughs during high speed and space velocities which seem to set off from 1500 s in the WLTC cycle. This behaviour may indicate degeneration of the Rh-function of the comparative catalyst after high temperature aging. The best results were obtained with the system comprising the catalyst of Example 1.
[0283] Further, Figure 4 shows the Tso light-off temperatures of the tested catalysts, which refer to the temperature at which 50% of the respective pollutant (CO, HCs and NO) is converted. As may be taken from the Figure, the Tso(HC) light-off temperatures of the inventive catalysts are lower than the Tso(HC) of the comparative catalyst. Furthermore, the Tso(CO) and Tso(NO) are also lower for the inventive catalysts according to Examples 1 and 2 compared to the comparative catalyst. Without wanting to be bound by any theory, the combination of the Pd gradient of the bottom coating - with a higher Pd-content at the inlet and a lower Pd-content at the outlet end -with the washcoat gradient of the bottom coating - with a lower inlet washcoat loading compared to the higher outlet washcoat loading - allows lower Tso temperatures, because the inlet bottom layer, and thus the portion of the bottom layer containing the greater amount of catalytically active metal, heats up faster due to the reduced thermal mass and high precious metal concentration, respectively, compared to the comparative catalyst. Additionally, the back pressure of the inventive and comparative examples is similar to the inventive catalysts due to the overall similar washcoat load.
[0284] Description of the figures
[0285] Figure 1 shows the cumulated HC obtained with the three-way conversion catalyst according to Example 1 and 2, and comparative Example 1.
[0286] Figure 2 shows the cumulated CO obtained with the three-way conversion catalyst according to Example 1 and 2, and comparative Example 1.
[0287] Figure 3 shows the cumulated NOx obtained with the three-way conversion catalyst according to Example 1 and 2, and comparative Example 1.Figure 4 shows the Tso light-off temperature of the evaluated three-way conversion catalyst according to Example 1 and 2, and comparative Example 1.
[0288] CITED LITERATURE
[0289] - US 2022 / 161236 A1
[0290] - US 7922988 B2
[0291] - US 8394348 B1
[0292] - WO 2022 / 090689 A 1
[0293] US 2021 / 348534 A1
Claims
Claims1. A three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, the catalyst comprising:(i) a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end, and a plurality of passages defined by internal walls of the substrate extending therethrough;(ii) a first coating comprising palladium supported on a first support material;(iii) a second coating comprising palladium supported on a second support material; (iv) a third coating comprising one or more of rhodium and palladium supported on a third support material;wherein the first coating extends over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70;wherein the second coating extends over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70;wherein the ratio of the loading of the first coating to the loading of the second coating, is in the range of from 0.3:1 to 0.9:1;wherein the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 1.5:1 to 5:1,wherein the third coating is disposed on the first and the second coatings over z% of the substrate axial length, wherein z is in the range of from 80 to 100; andwherein the third coating is substantially free of platinum.
2. The three-way conversion catalyst of claim 1 , wherein x is in the range of from 30 to 65.
3. The three-way conversion catalyst of claim 1 or 2, wherein y is in the range of from 30 to 65.
4. The three-way conversion catalyst of any one of claims 1 to 3, wherein z is in the range of from 85 to 100.
5. The three-way conversion catalyst of any one of claims 1 to 4, wherein the first coating further comprises an oxygen storage compound.
6. The three-way conversion catalyst of any one of claims 1 to 5, wherein the second coating further comprises an oxygen storage compound.
7. The three-way conversion catalyst of any one of claims 1 to 6, wherein the ratio of the palladium loading of the first coating to the palladium loading of the second coating is in the range of from 2:1 to 3: 1.
8. The three-way conversion catalyst of embodiments 6 or 7, wherein the ratio of the oxygen storage compound loading of the first coating to the oxygen storage compound loading of the second coating is in the range of from 1:1 to 1:4.
9. The three way conversion catalyst of any one of claims 1 to 8, wherein the ratio of the loading of the first coating to the loading of the second coating is in the range of from 0.4:1 to 0.89:1.
10. The three-way conversion catalyst of any one of claims 1 to 9, wherein the ratio of the Rh loading to the Pd loading of the third coating is in the range of from 0.5:1 to 5:1.
11. A process for preparing a three-way conversion catalyst, the process comprising:(a) providing a substrate comprising an inlet end, an outlet end, a substrate axial length extending from the inlet end to the outlet end and a plurality of passages defined by internal walls of the substrate extending therethrough;(b) preparing a slurry A comprising palladium supported on a first support material, disposing slurry A on the surface of the internal walls of the substrate over x% of the substrate length from the inlet end, wherein x is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with a first washcoat coating;(c) preparing a slurry B comprising palladium supported on a second support material, disposing slurry B on the surface of the internal walls of the substrate over y% of the substrate length from the outlet end, wherein y is in the range of from 20 to 70, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating and a second washcoat coating;(d) preparing a slurry C comprising one or more of rhodium and palladium supported on a third support material, disposing slurry C on the first and second coating over z% of the substrate length, preferably from the inlet end, wherein z is in the range of from 80 to 100, and calcining the obtained slurry-treated substrate, obtaining a substrate coated with the first washcoat coating, the second washcoat coating and a third washcoat coating; wherein the ratio of the loading of the first washcoat coating disposed on the substrate according to (b) to the loading of the second washcoat coating disposed on the substrate according to (c) is in the range of from 0.3:1 to 0.9:1;wherein the ratio of the palladium loading of the first washcoat coating to the palladiumloading of the second washcoat coating is in the range of from 1.5:1 to 5:1, wherein the third washcoat coating is substantially free of platinum.
12. A three-way conversion catalyst for the treatment of an exhaust gas comprising NO, CO and HC, the three-way conversion catalyst being obtainable or obtained by a process according to claim 11.
13. An exhaust gas treatment system comprising an internal combustion engine and a three- way conversion catalyst according to any one of claims 1 to 10 and 12 located down- stream of the internal combustion engine.
14. A method for the treatment of an exhaust gas of an internal combustion engine, comprising providing an exhaust gas from an internal combustion engine and passing said exhaust gas through a catalyst according to any one of claims 1 to 10 and 12.
15. Use of a catalyst according to any one of claims 1 to 10 and 12 for the treatment of an exhaust gas of an internal combustion engine, preferably of a spark ignition internal combustion engine, more preferably of a gasoline internal combustion engine.