Process for preparing water-based polyimides

A novel process for producing water-based polyimides through controlled addition of monomeric salts in an aqueous solution with adjusted surface tension and latent conditions addresses energy inefficiencies, enabling efficient and stable polyimide production for coatings and films.

WO2026238728A1PCT designated stage Publication Date: 2026-11-19ASTA ENERGY SOLUTIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063782
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing polyimide synthesis processes require high energy input and are limited by high viscosities at low concentrations, making them inefficient and costly.

Method used

A method involving the stepwise addition of a monomeric salt to an aqueous solution with controlled surface tension and temperature, followed by latent conditions, to produce a water-based polyimide without the need for high temperatures or dehydrating agents.

Benefits of technology

This method reduces energy consumption and enables the production of water-based polyimides with improved stability and applicability in coating applications, such as enameled wires and films, while minimizing the use of hazardous solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000003_0001
    Figure IMGF000003_0001
  • Figure IMGF000003_0002
    Figure IMGF000003_0002
  • Figure IMGF000004_0001
    Figure IMGF000004_0001
Patent Text Reader

Abstract

The present invention relates to a novel process for preparing water-based polyimides from a tetracarboxylic acid or its anhydride compound and a diamine compound.
Need to check novelty before this filing date? Find Prior Art

Description

PROCESS FOR PREPARING WATER-BASED POLYIMIDES Field of the Invention

[0001] The present invention relates to a novel process for preparing water-based polyimides.Background Art

[0002] Polyimides are valuable materials for a wide range of applications. They are usually synthesized by polycondensation of diamines with tetracarboxylic acids or dianhydrides thereof in solution or in the molten or even in the solid state.

[0003] For polyimide synthesis dianhydrides and diamines as monomers are typically used, which then react at room temperature to form a soluble polyamic acid intermediate (see Fig. 1). / V-Methylpyrrolidone (NMP), for example, may be used as a solvent.

[0004] The final polyimide is obtained by a condensation reaction of polyamic acid intermediates, which can be carried out either thermally, wherein high temperatures are required, or chemically by using dehydrating agents which will release water as a byproduct.

[0005] Polyimide processing can only be carried out at relatively low concentrations, since high viscosities occur even at low concentrations of the starting compounds.

[0006] WO2021258120A and US20190177483A1 disclose a process for preparing polyimide films, wherein an aqueous solution of the monomeric salts (MS) of a tetracarboxylic acid and a diamine are subjected to a processing step and to a subsequent heating step for polycondensation and simultaneously evaporating the water, wherein the polycondensation step is carried out at temperatures of 3750C or higher.

[0007] US2019 / 177483A discloses a method for producing polyimides by polycondensation of previously produced stoichiometric salts from polycarboxylic acids or their polyanhydrides and polyamines by heating the salts for dehydration.

[0008] US4217389 discloses a coating composition of a highly aqueous resin system. The composition comprises of water soluble polyester, water soluble orthoamic acid diamine, and small amounts of water soluble polymeric coating materials.

[0009] Therefore, there is still the need for an energy efficient process for preparing polyimides which may be used as wire varnish.Summary of invention

[0010] It is the objective of the present invention to provide a process for preparing polyimides with low energy consumption. The objective is solved by the subject matter of the present invention.

[0011] According to one embodiment of the invention, there is provided a method for producing a water-based polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied.

[0012] In one embodiment the surface tension of the solution is determined using pendant-drop method.

[0013] In another embodiment, the molar ratio of the tetracarboxylic acid or the anhydride thereof and the diamine compound of step a) is in the range of 0.5 to 1.5, specifically 0.8 to 1.2, more specifically about 1.0.

[0014] According to one embodiment, the polar protic solvent is water, a CpCg shortchain alcohol, or a mixture thereof.

[0015] In one embodiment, the monomeric salt is comprised in the aqueous solution in the range of 20 - 80 wt.%, specifically of 55 - 65 wt.%.

[0016] In another embodiment, the aqueous solution comprises between 1 - 4 wt.% of a co-solvent. In a specific embodiment, the co-solvent is a CpCg short-chain alcohol or a glycolether, specifically the CpCg short-chain alcohol is n-butanol and the glycolether is butylglycol or butyldiglycol.

[0017] In one embodiment, the clear solution of step d) is a solution with no visible turbidity.

[0018] According to the invention, described herein is a method for producing a waterbased polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied; andwherein said anhydride is a compound of formula (I)o othe diamine compound is a compound of formula (II)+ H2N - Y - NH2(H)to yield the monomeric salt of general formula (III)o o° o(IV)whereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether;Y denotes Cr^alkyl or an optionally substituted C3-C7cycloalkyl; andn is >2.

[0019] According to the invention, described herein is a coating composition obtained by the method for producing a water-based polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied.

[0020] According to one embodiment of the invention, described herein is a coating composition obtained by the method for producing a water-based polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; and e) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied; and wherein said anhydride is a compound of formula (I)the diamine compound is a compound of formula (II)+ H2N - Y - NH2(II)to yield the monomeric salt of general formula (III)(Illi)and the polyimide is a compound of formula (IV)o o° o(IV)whereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether; Y denotes C ^alkyl or an optionally substituted C3-C7cycloalkyl; andn is >2.

[0021] In one embodiment, described herein is the use of the coating composition for coating a wire to obtain an enameled wire.

[0022] In another embodiment, described herein is the use for obtaining a water-based polyimide film or a water-based polyimide surface.

[0023] According to the invention, described herein is a method for coating and insulating a wire comprising the following steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained;e) coating the wire by applying the coating composition of step d); andf) curing the coated wire to provide an enameled wire,wherein latent conditions are conditions where energy is applied.

[0024] According to one embodiment, the steps a) to f) of the method for coating and insulating a wire are repeated until the desired enamel thickness is achieved.

[0025] In one embodiment, described herein is an enameled wire obtained by the method for coating and insulating a wire, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained;e) coating the wire by applying the coating composition of step d); andf) curing the coated wire to provide an enameled wire,wherein latent conditions are conditions where energy is applied.Brief description of drawings

[0026] Fig. 1 depicts a comparative process scheme according to the state of the art.

[0027] Fig. 2 depicts a scheme of a process according to the present invention.Description of Embodiments

[0028] The present invention provides a method for producing a water-based polyimide, comprising the steps of mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt; isolating the monomeric salt; adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m; stirring the resulting solution until a clear solution is obtained; and treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied.

[0029] In one embodiment, the amount of monomeric salt in the solution is in the range of 20-80 wt.%, the amount of water in solution is in the range of 10-70 wt.%, and the amount of co-solvent in solution is in the range of 1-10 wt.%.

[0030] In one embodiment, described herein is a method for producing a water-based polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m, the amount of monomeric salt in solution is in the range of 20-80 wt.%, the amount of water in solution is in the range of 10-70 wt.%, and the amount of cosolvent in solution is in the range of 1-10 wt.%;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied.

[0031] One embodiment of the invention relates to a method for producing a waterbased polyimide of general formula (IV), comprising the steps of:a) mixing a compound of formula (I) with a compound of formula (II)o op + H2N - Y - NH2(H)(I)in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt of general formula (III)o o++H3N Y - NH3b) isolating the monomeric salt of general formula (III);c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide of general formula (IV) is obtained,o oN(IV)wherein latent conditions refer to conditions where energy is applied; andwhereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R3and R2are independently from one another aryl, or heterocyclic ether;Y denotes C^^alkyl or an optionally substituted C3-C7cycloalkyl; andn is >2.

[0032] The term “polycarboxylic acid” refers to compounds containing more than one carboxylic acid. Unless specified otherwise, the term herein refers to compounds with four or more carboxylic acid functional groups present. According to one embodiment, the polycarboxylic acid is a tetracarboxylic acid or pentacarboxylic acid.

[0033] According to one embodiment, the polycarboxylic acid is a compound of formula (V), (VI) , or (VII) 0 1-0 HO--,,(V) (VI) wherein R denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)- R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether, andX denotes carbonyl, methylene, or a heteroatom selected from the list consisting of nitrogen, oxygen, sulfur, and phosphor.

[0034] According to one embodiment, the anhydride of the polycarboxylic acid is a compound of formula (I)(I)whereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether.

[0035] Unless specified otherwise, the term “cycloalkyl” refers to monocyclic hydrocarbon rings such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and bicyclohexyl.

[0036] The term “heterocycloalkyl” refers to groups which are derived from cycloalkyl as hereinbefore defined and wherein in the hydrocarbon rings one or more of the groups -CH2- are replaced independently of one another by -O-, -S- or -NH-.Representatives of heterocycloalkyl compounds are oxiranyl, thiiranyl, aziridinyl, oxetanyl, thietanyl, azetidinyl, oxolanyl, thiolanyl, pyrrolidinyl, oxanyl, thianyl, piperidinyl, piperazinyl, morpholinyl, thiomorpholinyl, and 1,4-oxathianyl.

[0037] A diaromatic ketone has the structure of R1-C(=O)-R2, where R2and R2are independently from one another aryl or heterocyclic ether.

[0038] The term “aryl” refers to an aromatic radical that is composed exclusively of carbon and hydrogen. Exemplary aryl groups include phenyl, naphthyl, and biphenyl.

[0039] Suitable heterocyclic ethers include tetrahydrofuran and dioxane for example.

[0040] Suitable polycarboxylic acid compounds are, for example, depicted in Table 1.Table 1: Suitable polycarboxylic acid and anhydride thereof.HO2C ^y°^^CO2H HO2C HO2C ^^^CO2H HO2C^^Lr^^co2HHO2C CO2H HO2C CO2Hc :O2Htetrahydrofuran tetracarboxylic butane-l,2,3,4-tetracarboxylic cyclopentane tetracarboxylic acid acid acidCO2CH3HO2C , CO2H CO2H CH3O2C^Xxy^ CO2H HO2C ^ ^ C02H HO2C / \Z T^O2HCO2H HO2C CO2H cyclopenta ne-la, 2a, 3a, 4a- cyclohexane-1, 2, 4, 5- cyclopenta ne-1, 2,3, 4,5- tetracarboxylic acid, 1,2- tetracarboxylic acid (mixture of pentacarbocylic acid dimethyl ester isomers)HO2C CO2H HO2CC°2HHO2C CO2HxHO2C — — CO2H HO2C — ' ' — CO2H HO2C — H < ' — CO2HH3Ccyclohexane-1, 2,3,4- butane-l,2,3,4-tetracarboxylic hexane-l,2,3,4-tetracarboxylic tetracarboxylic acid (mixture of acid (mixture of isomers) acidisomers)CO2Hcyclohexa ne-1, 2, 4,5-tetracarboxy lie anhydride 4,4'-carbonyldi(benzene-l,2-dihydroanthracene-2,3,6,7- tetracarboxylic dianhydride cyclopentanetetracarboxylic tetracarboxylic acid dianhydride1,2, 4, 5- tetra hydro-4,8-etha no di cycloh exy I -3,4,3' ,4'- cyclohexanetetracarboxylic benzo[l,2-c:4,5-c']difuran- tetracarboxylic dianhydride dianhydride l,3,5,7(3aH,7aH)-tetraone3-[(2,4-dioxocyclopentyl) 4, 4'-carbonyldi phthalic anhydrideoxy]oxolane-2,5-dionetetra hydro [3, 3'- Bifuran] -2, 2', 5, 5'- tetrahydrodifuro[3,4-Z?:3',4'-c / ]furan-l,3,5,7-tetrone tetrone

[0041] According to one embodiment, the diamine compound is a compound of formula (ID+ H2N - Y - NH2(II)wherein Y denotes C ^alkyl or an optionally substituted C3-C7cycloalkyl.

[0042] The diamine compound may be an aliphatic or cycloaliphatic diamine.Representatives of such diamines are for example, propane-1, 3-diamine, butane-1,4-diamine, pentane-l,2-diamine, 2, 2-dimethylpropane-l, 3-diamine, hexane-l,6-diamine, 2-methylpentane-l,5-diamine, heptane-l,7-diamine, octane-1, 8-diamine, nonane-1,9-diamine, decane-1, 10-diamine, undecane-l,ll-diamine, dodecane-l,12-diamine, tridecane-1, 13-diamine, tetradecane-1, 14-diamine, pentadecane-1, 15-diamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexane-diamine, 1,3-bis (a mi nomethyl) cyclohexane, 1,4- bis (a mi nomethyl) cyclohexane, bis(aminomethyl)-norbornane, 4, 4’- methylenebis (cyclohexylamine), 4,4’-methylenebis(2-methyl-cyclohexylamine), and isophoronediamine.

[0043] Suitable diamine compounds are, for example, depicted in Table 2.Table 2: Suitable diamine compounds.H3C CH3CH3CH3CH3H2N.H2hk / \ / NH22,2-dimethyl-l,5- 2-mehtyl-l,5-di a min pentane / 7?eso-2,4-dimethylcadaverine diaminopentane, .NH, H3C CH3• r -i ‘H2NX / ^ X ,NH2V / 51,9-diaminononane 4, 4-di methyl no nane-l,9-dia mine 1,4- bis (a mi no methyl) cyclo hexane H2N^ ^NH2rj N rdN- (9-a mi nononyl) no nan e- 1,9- 1,3- 4-a mi no methylcyclo hexylamine diamine bis (a mi no methyl) cyclo hexane (mixture of isomers)(mixture of isomers)

[0044] The term “about” as used herein refers to the same value or a value differing by + / -5 % of the given value.

[0045] The term “solvent” as used herein refers to a liquid that dissolves a solid, liquid, or gaseous solute resulting in a solution. “Co-solvent” refers to a second solvent used with a primary solvent.

[0046] Polar protic solvents have a high dielectric constant ( ar> 5) and large dipole moments (p > 1.0) in comparison to nonpolar solvents such as alkanes. They possess O-H or N-H bonds and can participate in hydrogen bonding due to the polar nature of the bonds caused by a difference in electronegativity ( EN > 0.8). These solvents can also serve as acids (sources of protons) and weak nucleophiles (forming bonds with strong electrophiles). Examples of suitable polar protic solvents include alcohols such as methanol, ethanol, n-propanol, isopropanol or / -propanol, n-butanol, isobutanol or i-butanol, tert-butanol or Abutanol, and Aamyl alcohol.

[0047] Typical co-solvents include short-chain alcohols or tensides such as for example butanol, butylglycol, or butyldiglycol.

[0048] According to one embodiment of the invention, there is provided a method for producing a water-based polyimide resin wherein a polycarboxylic acid or an anhydride thereof is suspended in a polar protic solvent. According to another embodiment, the method for producing a water-based polyimide resin comprises the suspension of a tetracarboxylic acid or an anhydride thereof in a polar protic solvent. Isopropanol may be used as polar protic solvent. Upon vigorous stirring and heating under reflux, a clear solution of the mixture is obtained. This solution is cooled down to room temperature, and a diamine compound is added to the clear solution and stirred vigorously to obtain a monomeric salt (MS). The resulting monomeric salt is insoluble in the polar protic solvent and precipitates.

[0049] In one embodiment, the monomeric salt is obtained by mixing a compound of formula (V), (VI), or (VII) with a compound of formula (II). In another embodiment, the monomeric salt is obtained by mixing a compound of formula (I) with a compound of formula (II).

[0050] According to one embodiment, the molar ratio of the tetracarboxylic acid or the anhydride thereof and the diamine compound is in the range of 0.5 to 1.5, specifically 0.8 to 1.2, more specifically about 1.0. Specifically, the molar ratio is about 0.7, about 0.8, about 0.9, about 0.95, about 0.98, about 1.0, about 1.02, about 1.05, about 1.1,about 1.2, or about 1.3. According to another embodiment, the molar ratio of a compound of formula (V), (VI), or (VII) to a compound of formula (II) is in the range of 0.5 to 1.5, specifically 0.8 to 1.2, more specifically about 1.0. According to another embodiment, the molar ratio of a compound of formula (I) to a compound of formula (II) is in the range of 0.5 to 1.5, specifically 0.8 to 1.2, more specifically about 1.0.

[0051] According to one embodiment, the monomeric salt is a compound of general formula (III)(Illi)whereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether; and Y denotes C ^alkyl or an optionally substituted C3-C7cycloalkyl.

[0052] The term “clear solution” as described herein refers to a solution with no visible turbidity.

[0053] The term “stirred vigorously” as described herein refers to a reaction mixture or solution being in constant motion with high agitation to ensure suitable heat distribution, mass transfer and diffusion of molecules, and maximize the homogeneity within the reaction mixture. Thus, the chances of overheating, aggregation of added starting material molecules, aggregation of the formed product molecules, or increase in viscosity is minimized. Inadequate stirring may be referred to as stirring or agitation done in a speed that results in the formation of heat pockets, and / or an inhomogeneous or heterogenous reaction mixture.

[0054] The precipitate comprising of the monomeric salt formed is isolated from the suspension. To remove traces of unreacted co-monomers, additional polar protic solvent is added to redisperse the unreacted co-monomers. The centrifugation and decantation procedure are repeated. Subsequently, the supernatant is discarded, and the isolated monomeric salt powder is dried until a constant weight is achieved.Specifically, the drying of the isolated monomeric salt may occur under ambient atmosphere (1 bar, 220C), at elevated temperatures (temperatures above 400C andup to 2000C), in vacuo (pressures in the range of 0.1 mbar to 800 mbar), ventilation and circulation, or a combination thereof.

[0055] In one embodiment, the suspension comprising the monomeric salt is centrifuged and decanted once. In another embodiment, the suspension comprising the monomeric salt is dried, specifically the dried monomeric salt is the crude monomeric salt.

[0056] According to one embodiment, the obtained monomeric salt is a water soluble powder. According to another embodiment, the obtained monomeric salt is insoluble in certain solvents or co-solvents, specifically / -propanol or n-butanol.

[0057] In one embodiment, the obtained monomeric salt is washed once, twice, or several times with a suitable solvent. Specifically, the washing is done with a suitable solvent which is not a diluent of the monomeric salt or a solvent which partially dissolves the monomeric salt. In another embodiment, the washed monomeric salt is the isolated or purified monomeric salt.

[0058] In order to minimize the environmental aspects of the previously employed solvents used, such as NMP or other solvents which are known to be a hazardous compound when used in excess, water has been identified as a suitable alternative (see Fig. 2). The obtained monomeric salt are soluble in water or an aqueous solution comprising a further co-solvent. Additionally, the use of water in large parts for producing a water-based coating system may lead to a financial benefit by avoiding expensive solvents. These solvents typically require higher levels of safety due to their hazardous characteristics, higher energy input and higher temperatures to be removed from the solution, and potentially the need for incineration and other types of waste management.

[0059] The surface tension is a parameter observable on the surface of liquids caused by the intermolecular interactions of the molecules of a substance resulting in the possible formation of droplets and influencing the coating ability of the substance to a solid surface. In one embodiment, the surface tension of the monomeric salt mixture in solution may be determined using any one of the common detection methods such as pendant-drop method, sessile-drop method, Du Nouy ring method, Wilhelmy plate method, capillary rise method, drop weight or drop volume method, bubble pressure method, or the like.

[0060] The pendant-drop method refers to a method as described herein for the determination of the surface tension of a liquid by suspending a drop of the liquid beinganalyzed from the end of a tube, needle, or capillary. Due to gravitational forces being present, the pendant drop is deformed to not be a spherical shape. The degree of deformation is dependent on the weight of the drop and the surface tension of the molecules. Thus, the surface tension may be calculated based on the image of the resulting shape of the drop.

[0061] The sessile-drop method refers to a method as described herein for the determination of the surface tension of a liquid by measuring the contact angle of a drop of the liquid being analyzed on a solid surface. The resulting image of the drop is analyzed using software programs and the measured contact angles directly correlate to the surface tension of the sample.

[0062] According to one embodiment, the surface tension of water is 72.75 mN / m (at 20° C). However, for coating systems the surface tension should be in the range of 28 and 40 mN / m. Therefore, the water-based coating systems may be adjusted accordingly. Surprisingly, the surface tension of the solution could be easily adjusted by providing a co-solvent to the aqueous solution, by slowly adding or stepwise adding the obtained monomeric salt to the aqueous solution whilst vigorously stirring, controlling the temperature of the aqueous solution during addition, and by controlling the quantity of monomeric salt present in solution. Thus, the resulting solution may be a desired water-based coating system for the production of enameled wires and polyimide films.

[0063] The terms “stepwise addition” and “slow addition” are used herein synonymously. According to one embodiment, stepwise adding is the addition of the monomeric salt to the aqueous solution comprising water and 1 - 10 wt.% of a cosolvent in a time span of about 1 min, about 5 min, about 10 min, about 20 min, about 30 min, about 45 min, about 1 hour, or even longer.

[0064] A further embodiment relates to the method as described herein, wherein the monomeric salt is present in an amount in the range of 20 to 80%, or in the range of 30 to 75%, or in the range of 40 to 70 %, or in the range of 50 to 65%, or in the range of 55 to 65%.

[0065] According to one embodiment, the surface tension of the water-based coating systems for producing a water-based polyimide is adjusted by the addition of a cosolvent in the range of 1 % to 10 %.

[0066] The co-solvent may be present in an amount in the range of 1 to 10%, or in the range of 1 to 9%, or in the range of 1 to 8%, or in the range of 1 to 7%, or in the range of 1 to 6%, or in the range of 1 to 5%, or in the range of 1 to 4%.

[0067] According to one embodiment of the invention, n-butanol is used as a cosolvent resulting in a reduced surface tension in the range of 28 and 36 mN / m, which is suitable for copper winding wire coating.

[0068] The addition of the co-solvent further improves the rheological properties, e.g, through edge coverage or through shear stability of the coating solution (pumping).

[0069] According to one embodiment of the invention, the clear solution is treated under latent conditions until the polyimide is obtained.

[0070] “Latent conditions” refer to conditions wherein energy is applied, e.g., heat or thermal energy. According to a specific embodiment, the latent conditions refer to the solution or the composition being heated to temperatures above 500C for a suitable amount of time. Specifically, the temperatures are in the range of 1500C to 3500C and the suitable amount of time is in the range of 1 sec up to 10 min. According to one embodiment, the latent conditions are conditions during which polymerization of the monomers to the polyimide resin occurs, and / or during which the solvent and cosolvent evaporate.

[0071] In one embodiment, the obtained monomeric salt has good storage stability. In another embodiment, the obtained water-base polyimide resin has good storage stability. The term “storage stability” described herein refers to the ability of a compound to be stored for an extended period of time, specifically more than 7 days, 15 days, 1 month, or even longer, at room temperature or elevated temperatures, specifically about 220C, about 300C, about 400C, or about 500C, with no or minimal signs of degradation.

[0072] According to one embodiment, described herein is the method for producing a water-based polyimide without the need for an accelerator.

[0073] According to one embodiment, described herein is the method for producing a water-based polyimide without the need for a nitrogen-based base, a volatile base, or a base.

[0074] One embodiment of the invention relates to a coating composition obtained by the method for producing a water-based polyimide, comprising the steps of mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt; isolating the monomeric salt; adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution isadjusted to be in the range of 28 to 40 mN / m; stirring the solution of step c) until a clear solution is obtained; and treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions refer to conditions where energy is applied. In another embodiment, the amount of monomeric salt in the solution is in the range of 20-80 wt.%, the amount of water in solution is in the range of 10-70 wt.%, and the amount of co-solvent in solution is in the range of 1-10 wt.%.

[0075] In one embodiment, described herein is the use of the coating composition obtained by the method for producing a water-based polyimide for coating a wire to obtain an enameled wire or for obtaining a water-based polyimide film or a waterbased polyimide surface.

[0076] One embodiment of the invention relates to a method for coating and insulating a wire comprising the following steps of mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt; isolating the monomeric salt; adding the monomeric salt stepwise to an aqueous solution comprising water and a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m, the amount of monomeric salt in solution is in the range of 20-80 wt.%, the amount of water in solution is in the range of 10-70 wt.%, and the amount of co-solvent in solution is in the range of 1-10 wt.%; stirring the solution until a clear solution is obtained; coating the wire by applying the coating composition; and curing the coated wire to provide an enameled wire, wherein latent conditions are conditions where energy is applied.

[0077] In one embodiment, the steps of the method for coating and insulating a wire are repeated at least 2 times, at least 5 times, at least 10 times, at least 15 times, at least 20 times, at least 30 times, at least 40 times, or at least 50 times.

[0078] One embodiment of the invention relates to an enameled wire obtained by the method for coating and insulating a wire comprising the following steps of mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt; isolating the monomeric salt; adding the monomeric salt stepwise to an aqueous solution comprising water and a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m, the amount of monomeric salt in solution is in the range of 20-80 wt.%, the amount of water in solution is in the range of 10-70 wt.%, andthe amount of co-solvent in solution is in the range of 1-10 wt.%; stirring the solution until a clear solution is obtained; coating the wire by applying the coating composition; and curing the coated wire to provide an enameled wire, wherein latent conditions are conditions where energy is applied.Examples

[0079] The Examples which follow are set forth to aid in the understanding of the invention but are not intended to and should not be construed to limit the invention in any way. The Examples do not include detailed descriptions of conventional methods. Such methods are well known to those of ordinary skill in the art.Example 1 - Synthesis guidelines

[0080] 1 Equiv. tetrahydrofuran-2,3,4,5-tetracarboxylic acid [6 g, 24 mmol] is suspended in 200 mL isopropanol ( / PrOH). Upon vigorous stirring and heating to 800C under reflux a clear solution is obtained. This solution is cooled down in air to room temperature (r.t.).

[0081] 1 Equiv. of ± l,4-bis(aminomethyl)cyclohexane [3.4 g, 3.6 mL, 24 mmol] is added directly to the clear solution of the acid using a micropipette whilst vigorous stirring for 1 hour under standard conditions (1 atm. 250C).

[0082] The resulting pale-yellow monomeric salt precipitate is isolated from the suspension via centrifugation at 11.500 rpm for 10 minutes. The supernatant solution is decanted. The wet monomeric salt precipitate still contains traces of unreacted comonomers. To remove these, further / PrOH is added to the wet monomeric saltprecipitate in the centrifuge tubes, and a redispersion is generated by stirring. The centrifugation and decantation procedure are repeated. Subsequently, the supernatant is discarded, and the isolated monomeric salt powder is dried under high vacuum until a constant weight is achieved.

[0083] Table 3 provides an overview of the chemicals employed in the synthesis of the water-soluble monomeric salt powder.Table 3. L ist of chemicals used for the synthesis of the monomeric saltItem CAS Mw [g.mol1] Density [g.mL1] Tetra hydrofuran-2,3,4,5-tetracarboxy lie 26106-63-8 248.14 - acid± 1,4- Bis (amino methyl) cyclo hexane 2549-93-1 142.25 0.95p.a. Isopropanol 67-63-0 60.10 0.79Distilled water 7732-18-5 18.02 1.00

[0084] The monomeric salt is added stepwise to an aqueous solution comprising water and up to 8 wt.% of a co-solvent, specifically n-butanol. The solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m. The solution is kept stirring until the solution shows no visible turbidity.

[0085] The obtained solution is treated under latent conditions, specifically inserted in an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the solution is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enamel consisting of the desired polyimide resin.

[0086] Additionally, the obtained solution is used for coating a copper wire to obtain an enameled wire. The wire is treated by inserting the coated wire into an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the wire is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enameled wire coated with the desired polyimide resin.Example 2 -Synthesis guidelines

[0087] 1 Equiv. cyclopentane-l,2,3,4-tetracarboxylic acid [6 g, 24 mmol] is suspended in 200 mL isopropanol ( / PrOH). Upon vigorous stirring and heating to 800C under reflux a clear solution is obtained. This solution is cooled down in air to room temperature (r.t.).

[0088] 1 equiv. of 2-methyl-l,5-diaminopentane [2.8 g, 3.2 mL, 24 mmol] is added directly to the clear solution of the acid using a micropipette whilst vigorous stirring for 1 hour under standard conditions (1 atm and 25° C).

[0089] The resulting white monomeric salt precipitate is isolated from the suspension via centrifugation at 11.500 rpm for 10 minutes, the supernatant solution is decanted. The wet monomeric salt precipitate still contains traces of unreacted co-monomers. To remove these, further / PrOH is added to the wet MS precipitate in the centrifuge tubes, and a redispersion is generated by stirring. The centrifugation and decantation procedure is repeated. Subsequently, the supernatant is discarded, and the isolated monomeric salt powder is dried under high vacuum until a constant weight is achieved.

[0090] Table 4 provides an overview of the chemicals employed in the synthesis of the water-soluble monomeric salt powder.Table 4. L ist of chemicals used for the synthesis of the monomeric saltItem CAS Mw [g.mol1] Density [g.mL1] Cy Io penta ne-l,2,3,4-tetra carboxy lie acid 3724-52-5 246.17 - 2-Methyl-l,5-diaminopentane 15520-10-2 116.21 0.87p.a. Isopropanol 67-63-0 60.10 0.79Distilled water 7732-18-5 18.02 1.00

[0091] The monomeric salt is added stepwise to an aqueous solution comprising water and up to 6 wt.% of a co-solvent, specifically n-butanol. The solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m. The solution is kept stirring until the solution shows no visible turbidity.

[0092] The obtained solution is treated under latent conditions, specifically inserted in an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the solution is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enamel consisting of the desired polyimide resin.

[0093] Additionally, the obtained solution is used for coating a copper wire to obtain an enameled wire. The wire is treated by inserting the coated wire into an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the wire is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enameled wire coated with the desired polyimide resin.Example 3 - Synthesis guidelines

[0094] 1 Equiv. tetrahydrofuran-2,3,4,5-tetracarboxylic acid [6 g, 24 mmol] is suspended in 200 ml_ isopropanol ( / PrOH). Upon vigorous stirring and heating to 800C under reflux a clear solution is obtained. This solution is cooled down in air to room temperature (r.t.).

[0095] 1 Equiv. of 2-methyl-l,5-diaminopentane [2.8 g, 3.25 mL, 24 mmol] is added directly to the clear solution of the acid using a micropipette whilst vigorously stirring for 1 hour under standard conditions (1 atm and 25° C).

[0096] The resulting pale-yellow MS precipitate is isolated from the suspension via centrifugation at 11.500 rpm for 10 minutes, the supernatant solution is decanted. The wet MS precipitate still contains traces of unreacted co-monomers. To remove these, further / PrOH is added to the wet MS precipitate in the centrifuge tubes, and a redispersion is generated by stirring. The centrifugation and decantation procedure arerepeated. Subsequently, the supernatant is discarded, and the isolated MS powder is dried under high vacuum until a constant weight is achieved.

[0097] Table 5 provides an overview of the chemicals employed in the synthesis of the water-soluble monomeric salt powder.Table 5. L ist of chemicals used for the synthesis of the monomeric saltItem CAS Mw [g.mol1] Density [g.mL1] Tetra hydrofuran-2,3,4,5-tetracarboxy lie 26106-63-8 248.14 - acid2-Methyl-l,5-diaminopentane 15520-10-2 116.21 0.86p.a. Isopropanol 67-63-0 60.10 0.79Distilled water 7732-18-5 18.02 1.00

[0098] The monomeric salt is added stepwise to an aqueous solution comprising water and up to 6 wt.% of a co-solvent, specifically n-butanol. The solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m. The solution is kept stirring until the solution shows no visible turbidity.

[0099] The solution obtained is treated under latent conditions, specifically inserted in an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the solution is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enamel consisting of the desired polyimide resin.

[0100] Additionally, the obtained solution is used for coating a copper wire to obtain an enameled wire. The wire is treated by inserting the coated wire into an oven heated to 3500C in the range of 20 to 60 seconds. Thus, the wire is only heated to temperatures of max. 2500C for a short period of time resulting in a cured enameled wire coated with the desired polyimide resin.Example 4 - Enameling oven process

[0101] The conductor is guided via diverting wheels to the enameling tank, where the copper wire is coated with enamel, wherein the enamel comprises at least one polyimide as described herein in Example 1 to 3 for the production of an enameled wire. The enamel is applied by using dies or application felts. These enamels are processed continuously in a vertically or horizontally positioned oven. The coated wire is exposed to temperatures between 300-5500C in the enameling oven. As the dwell time of the wires to be coated in the coating oven is between 20 and 60 seconds, the wires are only heated to temperatures of max. 2500C for a short period of time.

[0102] A number of chemical and / or physical processes take place during the transfer of the coating into the end product. In the oven itself, physical processes of solvent evaporation (in this case water and co-solvents) overlapped on the chemical cross-linking processes. The energy required for this is provided as heat radiation and / or circulating air heat. The temperatures and dwell times, i.e. extraction speeds, depend on the type of coating, the wire diameter and the coating machine.

[0103] The rheological behavior during application and film formation of the insulating coating systems is mainly determined by the evaporation behavior of the solvent (water). After coating, the wire is returned via deflection rollers to the coating unit outside the oven and is thus brought to the desired insulation wall thickness (20 and 180 pm) in several layers (up to 30).

[0104] Modern ovens are equipped with a circulating air circuit that runs with or against the direction of the wire and absorbs the solvents (in this case co-solvents) released during burning. With the addition of small quantities of fresh air, these solvents (co-solvents) are burned thermally or catalytically. The energy resulting from the combustion can be added to the drying process and used to heat the circulating air.

Claims

Claims1. A method for producing a water-based polyimide, comprising the steps of:a) mixing at least a tetracarboxylic acid or an anhydride thereof with a diamine compound in a polar protic solvent having a dielectric constant greater than 5 to yield a monomeric salt;b) isolating the monomeric salt;c) adding the monomeric salt stepwise to an aqueous solution comprising water and 1 - 10 wt.% of a co-solvent, wherein the solution is kept at a temperature in the range of 20 to 40° C, and the surface tension of the solution is adjusted to be in the range of 28 to 40 mN / m;d) stirring the solution of step c) until a clear solution is obtained; ande) treating the solution under latent conditions until the polyimide is obtained, wherein latent conditions are conditions where energy is applied.

2. The method of claim 1, wherein the surface tension of the solution is determined using pendant-drop method.

3. The method of claim 1, wherein a molar ratio of the tetracarboxylic acid or the anhydride thereof and the diamine compound is in the range of 0.5 to 1.5, specifically 0.8 to 1.2, more specifically about 1.0.

4. The method of claim 1, wherein the polar protic solvent is water, a CpCg short-chain alcohol, or a mixture thereof.

5. The method of any one of claims 1 to 4, wherein the monomeric salt is comprised in the aqueous solution in the range of 20 - 80 wt.%, specifically of 55 - 65 wt.%.

6. The method of any one of claims 1 to 5, wherein the aqueous solution comprises between 1 - 4 wt.% of a co-solvent.

7. The method of any one of claims 1 to 6, wherein the co-solvent is a CpCg shortchain alcohol or a glycolether.

8. The method of claim 7, wherein the CpCg short-chain alcohol is n-butanol.

9. The method of claim 7, wherein the glycolether is butylglycol, or butyldiglycol.

10. The method of claim 1, wherein the clear solution is a solution with no visible turbidity.

11. A method for producing a water-based polyimide of any one of claims 1 to 10, wherein said anhydride is a compound of formula (I)(I)the diamine compound is a compound of formula (II)+ H2N - Y - NH2(II)the monomeric salt is a compound of formula (III)(HI)and the polyimide is a compound of formula (IV)(IV)whereinR denotes C3-C7cycloalkyl, C3-C6heterocycloalkyl, diaromatic ketone R1-C(=O)-R2, wherein R2and R2are independently from one another aryl, or heterocyclic ether; Y denotes (^-^alkyl or an optionally substituted C3-C7cycloalkyl; andn is >2.