Process for forming hollow carbon spheres
A method for producing hollow carbon spheres using silver-cored carbon spheres and acidic treatment addresses the challenges of toxic chemicals and scalability, achieving controlled size and shell thickness while being safer and more efficient.
Patent Information
- Application Number
- PCT/EP2026/063884
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing hollow carbon spheres face challenges such as the use of toxic chemicals like hydrofluoric acid, lack of scalability, inefficiency, and poor control over sphere diameter and morphology, particularly in industrial settings.
A method involving a precursor solution of carbon-containing materials and silver salts is used to form silver-cored carbon spheres, which are then treated with an acidic solution to remove the silver core, producing hollow carbon spheres without the need for hydrofluoric acid, allowing for controlled size and shell thickness through adjustable parameters.
The method enables the production of hollow carbon spheres with controlled size and shell thickness, is safer at scale, more efficient, and recyclable, reducing environmental and economic risks associated with toxic chemicals.
Smart Images

Figure EP2026063884_19112026_PF_FP_ABST
Abstract
Description
[0001] Process for Forming Hollow Carbon Spheres Field
[0002] The present invention relates to a method of producing hollow carbon spheres at the nanometre and micrometre scale. In particular, the present invention relates to a method of producing hollow carbon spheres, such as nanospheres and / or microspheres, suitable for use in lithium-sulphur batteries.
[0003] Background of the Invention
[0004] Hollow carbon spheres, such as hollow carbon nanospheres and / or hollow carbon microspheres, exhibit unique properties such as high surface area to volume ratio, strong chemical stability, high-temperature resistance, facile modification and / or functionalisation of surface chemistry, and may be used to encapsulate other materials. There is a general need to develop methods of producing hollow carbon spheres, especially methods that may be applicable to industrial scalability.
[0005] Generally, methods of producing hollow carbon spheres can be divided into hard-templating and soft-templating approaches. Hard-templating methods employ rigid particles as “hard” core templates. A carbon shell is typically formed around the core template and then the core template is removed sacrificially. Silica is a commonly used hard template material because the diameter of silica particles can be easily tuned from the nanometre to micrometre scale, and it is well-known that hollow carbon spheres maintain the size of and shape of such templates. Typically, silica cores are removed sacrificially by etching using hydrofluoric acid, which dissolves I removes the silica particle without affecting the carbon shell. Hydrofluoric acid is a highly toxic substance and must be handled with extreme care. The use of hydrofluoric acid at an industrial scale presents severe health and safety concerns.
[0006] Soft-template methods address disadvantages of hard-templating approaches, such as the removal of the core template. Typically, soft templates are generally easier to remove than traditional hard templates. Examples of soft templates include colloidal systems, such as emulsion droplets, micelles, vesicles, gas bubbles, or combinations thereof. However, hollow carbon spheres produced by soft templating methods may suffer from less satisfactory morphology and monodispersity compared to hard templating because of the polydispersity and dynamics of soft templates.
[0007] Several techniques are suitable for producing hollow carbon materials, for example hollow carbon spheres, such as chemical vapor deposition, thermal plasma processing, laser ablation, arcdischarge, hydrothermal carbonization, amongst others.
[0008] However, there remains a need for an improved process for the formation of hollow carbon spheres that avoids the use of toxic chemicals, and which can provide hollow carbon spheres in a controllable and efficient manner, for example in terms of sphere diameter and product yield.Summary of the Invention
[0009] It is one aim of the present invention, amongst others, to provide a method of manufacturing hollow carbon spheres, such as hollow carbon nanospheres and / or hollow carbon microspheres, that addresses at least one disadvantage of the prior art, whether identified here or elsewhere, or to provide an alternative method of manufacture to existing methods. For example, it may be an aim of the present invention to provide a method of manufacturing hollow carbon spheres which is more efficient, less energy intensive and / or less costly than known methods.
[0010] It may be an aim of the present invention to provide a method wherein the design of nanosphere and / or microsphere materials may be tailored without the use of pre-formed templates.
[0011] It may be one aim of the present invention to provide a method which is safer at large scale than known methods of producing nanosphere and / or microsphere materials. For example, by avoiding the use of hydrofluoric acid.
[0012] It may be one aim of the present disclosure to provide a method of nanosphere and / or microsphere materials production which offers improved recyclability of chemicals which may be beneficial for health and economic reasons.
[0013] It may be one aim of the present invention to provide a material for use in a cathode for a lithiumsulphur battery which confines soluble polysulfide species during battery operation, suitably which improves sulphur utilisation and / or reduces polysulfide shuttle in said lithium-sulphur battery.
[0014] According to aspects of the present invention, there is provided a method, a material, an electrode and uses as forth in the appended claims. Other features of the invention will be apparent from the dependent claims, and from the description which follows.
[0015] According to a first aspect of the present invention, there is provided a method of producing hollow carbon spheres, the method comprising the steps:
[0016] (a) providing a precursor solution comprising a carbon-containing material and a silver salt, and arranging the precursor solution in a reaction vessel;
[0017] (b) heating the precursor solution in the reaction vessel to produce silver-cored carbon spheres; and
[0018] (c) treating the silver-cored carbon spheres produced in step (b) with an acidic solution to remove the silver core and provide the hollow carbon spheres.
[0019] According to a second aspect of the invention, there is provided hollow carbon spheres obtainable by the method of the first aspect of the invention.According to a third aspect of the invention, there is provided an electrode for a battery comprising hollow carbon spheres obtainable by the method of the first aspect of the invention.
[0020] According to a fourth aspect of the invention, there is provided a use of hollow carbon spheres obtainable by the method of the first aspect of the invention in batteries, such as in lithium-sulphur (Li-S) batteries.
[0021] According to a fifth aspect of the invention, there is provided a use of hollow carbon spheres obtainable by the method of the first aspect of the invention in water purification.
[0022] According to a sixth aspect of the invention, there is provided a use of hollow carbon spheres obtainable by the method of the first aspect of the invention as support materials for heterogenous catalysis.
[0023] According to a seventh aspect of the present invention, there is provided a lithium-sulphur battery comprising a cathode according to the third aspect.
[0024] Detailed Description of the Invention
[0025] The first aspect of the present invention provides method of producing hollow carbon spheres, the method comprising the steps:
[0026] (a) providing a precursor solution comprising a carbon-containing material and a silver salt, and arranging the precursor solution in a reaction vessel;
[0027] (b) heating the precursor solution in the reaction vessel to produce silver-cored carbon spheres; and
[0028] (c) treating the silver-cored carbon spheres produced in step (b) with an acidic solution to remove the silver core and provide the hollow carbon spheres.
[0029] The hollow carbon spheres produced in the present invention have a carbon shell surrounding a void. The inventors have found that the method of this first aspect can provide hollow carbon spheres with a desired size and shell thickness without the use of pre-formed templates, for example by tailoring parameters of the method. For example, the concentration of precursors and / or the annealing time may be tailored to produce a sphere material of a desired size, for example nanosphere and / or microsphere materials. Tailored properties may be particularly beneficial for specific applications where enhanced reliability and performance may be required.
[0030] Furthermore, the method of this first aspect may advantageously provide an efficient and reliable method for forming hollow carbon spheres which would be safer to run at a large scale than known methods, due to harsh chemicals, for example hydrofluoric acid, not being required in the method.Suitably, the present method is essentially free of hydrofluoric acid. In some embodiments, the present method is free of hydrofluoric acid. Suitably the amount of hydrofluoric acid is less than 1 wt%, such as less than 0.1 wt%, preferably less than 0.01 wt%, based on the total reaction mass. Suitably no hydrofluoric acid is used to form the hollow carbon spheres in the method of the present invention.
[0031] The inventors have also found that the present method may provide an improved recyclability of chemicals used, compared to known methods. For example, the silver species used to form the silver-cored carbon spheres may be recycled and / or regenerated from waste streams of the method. Silver is a relatively expensive reagent and therefore its recycling and / or regeneration may be beneficial for economic reasons. Said recycling of material from waste streams may also advantageously reduce the potential environmental impact of the method.
[0032] The hollow carbon spheres produced by the method are suitably hollow carbon nanospheres and / or hollow carbon microspheres.
[0033] Production of Silver-Cored Carbon Spheres
[0034] The method of this first aspect involves the step (a) of providing a precursor solution comprising a carbon-containing material and a silver salt, and arranging the precursor solution in a reaction vessel; and step (b) of heating the precursor solution in the reaction vessel to produce silver-cored carbon spheres, such as silver-cored carbon nanospheres and / or silver-cored carbon microspheres.
[0035] Advantageously, the present method may have high procedural economy because it may have fewer steps compared to typical methods of producing hollow carbon spheres. For example, the method as described herein does not require the use of pre-formed templates, such as pre-formed silica templates and / or does not require the use of organic templating agents such as organosilanes. Examples of organosilanes include but are not limited to alkylsilanes.
[0036] Suitably the present method is essentially free of silica and organosilanes. In some embodiments, the present method is free of silica and organosilanes. Suitably no silica or organosilanes is used to form the silver-cored carbon spheres or the hollow carbon spheres in the method of the present invention.
[0037] Suitably the present method is essentially free of silicon. In some embodiments, the present method is free of silicon. Suitably no silicon is used to form the silver-cored carbon spheres or the hollow carbon spheres in the method of the present invention.
[0038] Suitably the silver-cored spheres produced in step (b) are essentially free from silicon. Suitably the amount of silicon in the silver-cored spheres is less than 1 wt%, such as less than 0.1 wt%, preferably less than 0.01 wt% by weight.Suitably the hollow carbon spheres produced in step (c) are essentially free from silicon. Suitably the amount of silicon in the hollow carbon spheres is less than 1 wt%, such as less than 0.1 wt%, preferably less than 0.01 wt% by weight.
[0039] The precursor solution comprises a carbon-containing material and a silver salt.
[0040] The carbon-containing material may be a saccharide (such as a monosaccharide, a disaccharide, oligosaccharide, a polysaccharide, or mixtures thereof), a phenolic compound, or mixtures thereof. For example, the carbon-containing precursor may be selected from glucose (dextrose), fructose (levulose), galactose, sucrose, lactose, maltose, cellulose, starch, resorcinol, or mixtures thereof.
[0041] The silver salt may be a silver(l) salt selected from silver(l) nitrate, silver(l) nitrite, silver(l) oxide, silver(l) carbonate, silver(l) fluoride, silver(l) chloride, silver(l) bromide, silver(l) iodide, silver(l) sulphide, silver(l) tetrafluoroborate, silver(l) cyanide, silver(l) permanganate, silver(l) thiocyanate, silver(l) hexafluorophosphate, silver(l) acetate, silver(l) triflate, silver(l) acetylide, silver(l) oxalate, silver(l) chromate, silver(l) molybdate, silver(l) sulphite, silver(l) sulphate, silver(l) selenide, silver(l) selenite, or mixtures thereof. For example, the salt of silver may be silver(l) nitrate.
[0042] The precursor solution is suitably an aqueous solution of the carbon-containing material and the silver salt. Therefore, the precursor solution suitably comprises water. For example, the precursor solution may comprise deionised water. The precursor solution may comprise a solvent. For example, the precursor solution may comprise an organic solvent. The organic solvent may be a polar organic solvent, such as isopropanol, acetone, ethanol, or mixtures thereof. The precursor solution may comprise water and a single organic solvent or a mixture of organic solvents. The precursor solution may comprise water, an organic solvent, a mixture of water and an organic solvent or a mixture of organic solvents. The precursor solution may comprise water and an organic solvent or water and a mixture of organic solvents. The solvent(s) of the precursor solution are selected such that the silver salt is soluble in said solvent(s).
[0043] The concentration of the carbon-containing material in the precursor solution may be from 0.05 to 5 M, suitably from 0.1 to 2 M or from 0.2 to 1 M, for example approximately 0.5 M.
[0044] The concentration of the silver salt in the precursor solution may be from 0.05 to 100 pM, suitably from 0.1 to 50 pM or from 1 to 10 pM, for example approximately 5 pM.
[0045] The precursor solution may be formed from a solution of the carbon-containing material and a solution of the silver salt, suitably from an aqueous solution of the carbon-containing material and an aqueous solution of the silver salt. The concentration of the carbon-containing material in said solution of the carbon-containing material may be from 0.05 to 10 M, suitably from 0.1 to 5 M, suitably from 0.1 to 2 M or from 0.2 to 1 M, for example approximately 0.5 M.The concentration of the silver salt in said solution of the silver salt may be from 0.01 to 1 M, suitably from 0.02 to 0.5 M or from 0.05 to 0.2 M, for example approximately 0.1 M.
[0046] Suitably the precursor solution is formed by the addition of the solution of the silver salt to the solution of the carbon-containing material.
[0047] The ratio of the carbon-containing material to the silver salt affects the hollow carbon sphere particle size and the core:shell volume ratio. For example, the molar ratio of carbon-containing material to silver salt may be from 1 x 104: 1 to 1 x 106: 1 , suitably from 6 x 104: 1 to 4 x 105: 1. For example the molar ratio of carbon-containing material to silver salt may be approximately 1 x 105: 1.
[0048] In step (b) of the method, the precursor solution is arranged in a reaction vessel and heated. The reaction vessel is therefore suitable for heating the precursor solution to the required temperatures. The reaction vessel may be suitable for heating under pressure. For example, the reaction vessel may be an autoclave, such as a Teflon-lined autoclave.
[0049] The method of this first aspect includes heating the precursor solution in the reaction vessel to produce silver-cored carbon spheres. For example, the reaction vessel may be heated in an oven. The oven may be preheated to a specified temperature or may be initially at room temperature and be heated at a temperature ramp overtime to a specified temperature.
[0050] For example, the precursor solution may be heated in the reaction vessel at a temperature of at least 100°C, suitably at least 130°C or at least 150°C. The precursor solution may be heated at a temperature of up to 180°C, suitably up to 170°C or up to 160°C. The precursor solution is suitably heated at a temperature of from 100 to 180°C, suitably 130 to 170°C or from 150 to 160°C.
[0051] Said heating of step (b) is suitably carried out for a period of time sufficient to form the silver-cored carbon spheres. Said heating may be carried for at least 30 minutes, at least 1 hour or at least 2 hours. Said heating may be carried out for up to 10 hours, up to 8 hours or up to 6 hours. Said heating may be carried out for from 30 minutes to 10 hours, suitably from 1 hour to 8 hours or from 2 hours to 6 hours.
[0052] Step (b) may involve heating the precursor solution at a temperature of at least 100°C for a period of time of at least 1 hour. Step (b) suitably involves heating the precursor solution at a temperature of at least 150°C for a period of time of at least 2 hours.
[0053] Advantageously, the size of the hollow carbon spheres produced according to the method described herein may be tailored by controlling the concentration of components in the precursor solution, controlling the temperature of the reaction and / or controlling the duration of the reaction.The mean sphere diameter of hollow carbon spheres produced according to the method described herein may be determined by measurement methods including transmission electron microscopy according to ISO 21363:2020 and / or scanning electron microscopy imaging according to ISO 19749:2021. For example, the mean sphere diameter of hollow carbon spheres produced according to the method described herein may be from 50 to 5,000 nm, such as from 100 to 2,000 nm, such as 200 to 1 ,000 nm, as determined by the measurement methods discussed above.
[0054] Advantageously, the thickness of the carbon shell of the hollow carbon spheres produced according to the method described herein may be tailored by controlling the concentration of components in the precursor solution, controlling the temperature of the reaction and / or controlling the duration of the reaction.
[0055] The thickness of the carbon shell of the spheres may be determined by measurement methods including transmission electron microscopy according to ISO 21363:2020 and / or scanning electron microscopy imaging according to ISO 19749:2021. For example, the thickness of the carbon shell of the spheres may be from 10 to 300 nm, suitably 20 to 200 nm as determined by the measurement methods discussed above.
[0056] Step (b) of the method of this first aspect may be followed by a step (b2) of isolating the silver-cored spheres produced in step (b) from the precursor solution.
[0057] Step (b2) may involve washing the silver-cored spheres produced in step (b).
[0058] Such a washing step as defined herein may include preparing a suspension of the silver-cored spheres in a washing solution. The washing solution may comprise water. For example, the washing solution may comprise deionised water. The washing solution may comprise a solvent. For example, the washing solution may comprise an organic solvent. The washing solution may comprise water and a single solvent or a mixture of solvents. The washing solution may comprise water, an organic solvent, a mixture of water and an organic solvent or a mixture of organic solvents. The washing solution may comprise water and an organic solvent or water and a mixture of organic solvents.
[0059] Step (b2) may involve of centrifugation of the silver-cored spheres produced in step (b).
[0060] Therefore the suspension of silver-cored carbon spheres produced by heating the precursor solution in the reaction vessel in step (b) may be centrifuged. It is believed that larger spheres have a lower density and therefore centrifugation may result in a decrease in mean particle size, due to larger spheres being removed by the process. For example, should larger spheres be desired, it may not be advantageous to centrifuge the silver-cored carbon spheres produced from the reaction step. Alternatively, should smaller spheres be desired, it may be advantageous to centrifuge the silver-cored carbon spheres produced from the reaction step.In some embodiments, step (b2) involves a washing step and a centrifugation step.
[0061] Washing and / or centrifugation steps may improve the purity of the sphere materials described herein. The removal of impurities will be apparent to a person skilled in the art. For example, the washing solution appearance (e.g. colour) and / or properties (e.g. pH) may be relied upon as an indication of purity. Additionally and / or alternatively, other analytical methods may be performed on the sphere materials to inspect the purity and / or characteristics thereof.
[0062] Silver-Cored Carbon Sphere Annealing
[0063] Step (b) of the method of this first aspect may be followed by a step (b3) of annealing the silver-cored carbon spheres produced in step (b).
[0064] In embodiments wherein step (b2) is present, step (b3) suitably follows step (b2).
[0065] Annealing is a common technique known to the person skilled in the art involving heat treatment of a material to alter the physical and / or chemical properties of said material. Annealing as described herein may include heating the silver-cored carbon spheres at relatively high temperature. Annealing as described herein may include heating under inert conditions, such as under an atmosphere of an inert gas such as: nitrogen; a Nobel gas, such as argon; or mixtures thereof.
[0066] Step (b3) may involve annealing the silver-cored spheres at a temperature of at least 300°C, suitably at least 400°C or at least 500°C. Step (b3) may involve annealing the silver-cored carbon spheres at a temperature of up to 900 °C, suitably up to 800°C or up to 700°C. Step (b3) may involve annealing the silver-cored carbon spheres at a temperature of from 400 to 800°C, from 500 to 700°C or from 550 to 650°C.
[0067] Said heating of step (b3) is suitably carried out for a period of time sufficient to anneal the silver-cored carbon spheres. Said heating may be carried for at least 30 minutes, at least 1 hour or at least 1.5 hours. Said heating may be carried out for up to 6 hours, up to 4 hours or up to 3 hours. Said heating may be carried out for from 30 minutes to 6 hours, suitably from 1 hour to 4 hours or from 1.5 hours to 3 hours.
[0068] Step (b3) may involve annealing the silver-cored spheres at a temperature at of at least 300°C for a period of time of at least 30 minutes. Step (b3) suitably involves annealing the silver-cored spheres at a temperature of at least 400°C for a period of time of at least 1 hour.
[0069] Annealing as described herein can be performed in any suitable annealing furnace. For example, the annealing furnace may comprise a quartz glass tube furnace. For example, the annealing furnace may comprise an oven.Annealing as described herein may include heating from room temperature to a target temperature in a controlled manner. Alternatively, annealing may occur in a pre-heated annealing furnace. Additionally and / or alternatively, the annealing may include sustaining the silver-cored carbon spheres at a dwell temperature for a determined period of time.
[0070] For example, annealing may include heating the silver-cored carbon spheres from room temperature to a higher temperature as described above at a rate of 5°C per minute.
[0071] Removal of Silver Core
[0072] The method of the present invention involves step (c) of treating the silver-cored carbon spheres produced in step (b) with an acidic solution to remove the silver core and provide the hollow carbon spheres. This step may be referred to as a template removal step. In step (c), the acidic solution suitably penetrates the carbon spheres and reacts with the silver core to produce a silver salt which dissolves in the solution and is therefore removed from the carbon spheres.
[0073] The acidic solution may comprise any acid capable of reacting with silver to produce an aqueous salt of silver. For example, the acidic solution suitably comprises an acid selected from the group containing: nitric acid, hydrochloric acid, sulphuric acid, acetic acid, phosphoric acid, acetic acid, carbonic acid, citric acid, formic acid, perchloric acid, hydrobromic acid, hydroiodic acid, boric acid, nitrous acid, or mixtures thereof. The acidic solution suitably comprises nitric acid. The acidic solution used in step (c) is suitably a nitric acid solution.
[0074] The method according to the present disclosure may be essentially free of hydrofluoric acid. Specifically, step (c) preferably does not involve the use of hydrofluoric acid. Advantageously, the method described herein may be safer at large scale compared to known methods of producing hollow carbon spheres because the method can avoid the use of hydrofluoric acid.
[0075] The acidic solution is suitably an aqueous solution. The acidic solution suitably has a concentration of at least 0.5 M, suitably at least 1 M or at least 2 M. The acidic solution may have a concentration of up to 10 M, suitably up to 8 M or up to 6 M. The acidic solution suitably has a concentration of from 0.5 M to 10 M, suitably from 2 M to 8 M, for example approximately 5 M, suitably wherein the acidic solution is a nitric acid solution.
[0076] Step (c) may be carried out with continuous stirring of the silver-cored carbon spheres and the acidic solution.
[0077] The treatment of the silver-cored carbon spheres with an acidic solution of step (c) as described herein may be performed as elevated temperature. Step (c) may be carried out at a temperature of at least 30°C, suitably at least 40°C or at least 45°C. Step (c) may be carried out at a temperature ofup to 80°C, suitably up to 70°C or up to 60°C. Step (c) may be carried out at a temperature of from 30 to 80°C, from 40 to 70°C or from 45 to 60°C.
[0078] Step (c) may be carried out at said temperatures for a period of time sufficient to dissolve and remove substantially all of the silver cores from the carbon spheres. Step (c) may be carried for at least 1 hour, at least 6 hours or at least 12 hours. Step (c) may be carried out for up to 72 hours, up to 48 hours or up to 36 hours. Said heating may be carried out for from 6 hours to 48 hours, suitably from 12 hours to 36 hours.
[0079] Suitably, the hollow carbon spheres produced in step (c) are essentially free from silver. Suitably the amount of silver in the hollow carbon spheres is less than 1 wt%, such as less than 0.1 wt%, preferably less than 0.01 wt%.
[0080] In some embodiments, the hollow carbon spheres produced in step (c) are essentially free from metallic components. Suitably the amount of metallic components in the hollow carbon spheres is less than 1 wt%, such as less than 0.1 wt%, preferably less than 0.01 wt%.
[0081] Suitably, the hollow carbon spheres produced in step (c) consist essentially of carbon. Suitably, the hollow carbon spheres produced in step (c) consist of carbon.
[0082] Following treatment of the silver-cored carbon spheres with an acidic solution, the method of the present invention may include a step:
[0083] (d) isolating the hollow carbon spheres produced in step (c) from the acidic solution.
[0084] Therefore step (d) suitably produces a waste acidic solution. The waste acidic solution suitably comprises silver removed from the silver-cored carbon spheres. In embodiments wherein the acidic solution used in step (c) is nitric acid, the waste acidic solution suitably comprises silver nitrate.
[0085] Step (d) suitably involves centrifugation of the hollow carbon spheres produced in step (c), to separate the hollow carbon spheres from the acidic solution. Step (d) may involve washing the hollow carbon spheres until the washings are essentially neutral in pH, i.e. approximately pH 7.
[0086] Step (d) of the method may include drying the hollow carbon spheres. Therefore step (d) may comprise isolating and drying the hollow carbon spheres. For example, the drying of the hollow carbon spheres may involve drying the hollow carbon spheres at an elevated temperature such as a temperature of at least 40°C, at least 60°C or at least 80°C, for example for at least 1 hour, at least 6 hours or at least 10 hours.Suitably, the hollow carbon spheres are porous. Suitably, the hollow carbon spheres have a specific surface area of from 100 to 2,000 m2 / g, suitably from 200 to 1 ,500 m2 / g, suitably as measured according to ISO 9277:2022.
[0087] Regeneration of Silver
[0088] Advantageously, the method according to the present invention may offer improved recyclability of chemicals. For example, silver material from the waste stream from the acidic treatment step (c), which is suitably separated from the hollow carbon sphere product in step (d), may be recovered by known methods to regenerate and recycle the silver material. Therefore the method of the present invention may comprise a step (e) of treating waste streams from the method to recover silver. Suitably step (e) involves treating the waste acidic solution produced in step (d) to obtain silver material.
[0089] Therefore the method of this first aspect may comprise the steps:
[0090] (d) isolating the hollow carbon spheres from the acidic solution to provide a waste acidic solution;
[0091] and
[0092] (e) treating the waste acidic solution produced in step (d) to obtain recovered silver material;
[0093] suitably wherein the waste acidic solution comprises silver nitrate and suitably wherein the recovered silver material is silver nitrate.
[0094] For example, in step (e), silver may be precipitated out of waste solutions, which are suitably aqueous solutions, as silver chloride by the addition of sodium chloride to the waste solution. The silver chloride may then be separated by any appropriate means, such as centrifugation. The silver chloride may then be oxidised to silver oxide by any appropriate means, such as treatment with sodium hydroxide. Silver oxide may then be heated to form silver metal. The silver metal may then be dissolved in nitric acid and crystallised to form silver nitrate, which may then be re-used in a method of the present invention, which may advantageously reduce the waste produced by the method and may reduce costs due to the recovery and re-use of the silver species.
[0095] Suitably the silver material obtained in step (e) is silver nitrate. Said silver nitrate may be re-used in a method of the present invention, to provide the silver salt in the precursor solution of step (a) of the method.
[0096] Therefore the method of the present invention may comprise a step:
[0097] (f) repeating steps (a) to (c) using the recovered silver material from step (e) to provide the silver salt of the precursor solution.A similar process may be carried out on waste streams derived from step (b) and / or step (b2), for example waste streams produced after washing steps, which may contain unreacted silver nitrate.
[0098] The inclusion of step (e) to recover silver from the waste streams may advantageously avoid the discharge of silver nitrate, which may be harmful to the environment.
[0099] In some preferred embodiments, the method of this first aspect comprises the steps:
[0100] (a) providing a precursor solution comprising a carbon-containing material and a silver salt, and arranging the precursor solution in a reaction vessel;
[0101] (b) heating the precursor solution in the reaction vessel at a temperature of at least 100°C for a period of time of at least 1 hour to produce silver-cored carbon spheres;
[0102] (b3) annealing the silver-cored carbon spheres produced in step (b) at a temperature of at least 400°C fora period of time of at least 1 hour; and
[0103] (c) treating the silver-cored carbon spheres produced in step (b) with an acidic solution to remove the silver core and provide the hollow carbon spheres.
[0104] In some preferred embodiments, the method of this first aspect comprises the steps:
[0105] (a) providing a precursor solution comprising a carbon-containing material and silver nitrate, and arranging the precursor solution in a reaction vessel;
[0106] (b) heating the precursor solution in the reaction vessel at a temperature of at least 100°C for a period of time of at least 1 hour to produce silver-cored carbon spheres;
[0107] (b3) annealing the silver-cored carbon spheres produced in step (b) at a temperature of at least 400°C fora period of time of at least 1 hour; and
[0108] (c) treating the silver-cored carbon spheres produced in step (b) with a nitric acid solution to remove the silver core and provide the hollow carbon spheres;
[0109] suitably wherein the method further comprises the steps:
[0110] (d) isolating the hollow carbon spheres from the acidic solution to provide a waste acidic solution comprising silver nitrate; and
[0111] (e) treating the waste acidic solution produced in step (d) to obtain recovered silver nitrate.The second aspect of the present invention provides hollow carbon spheres obtainable by the method of the first aspect of the invention.
[0112] The hollow carbon spheres may have any of the suitable features and advantages described in relation to the first aspect. Suitably the hollow carbon spheres are obtained by the method of the first aspect.
[0113] The third aspect of the present invention provides an electrode for a battery, the electrode comprising hollow carbon spheres obtainable by the method of the first aspect of the invention.
[0114] The hollow carbon spheres may have any of the suitable features and advantages described in relation to the first aspect. Suitably the hollow carbon spheres are obtained by the method of the first aspect.
[0115] The electrode is suitably an electrode for use in a lithium-sulphur (Li-S) battery. The electrode may be an anode or a cathode for an Li-S battery. Suitably the electrode is a cathode. Such hollow carbon spheres may be particularly advantageous in such electrodes to provide a conductive structural support network for sulphur which can cope with the physical demands placed on such electrodes in use, particularly the significant volumetric expansion which occurs during cycling of said batteries.
[0116] In the electrode of this first aspect, the hollow carbon spheres are present in a carbon-sulphur composite with sulphur. The carbon-sulphur composite material comprising the hollow carbon spheres may be formed by first preparing a carbon-sulphur mixture by mixing the hollow carbon spheres with a material comprising sulphur, such as elemental sulphur; homogenising the carbonsulphur mixture by mechanical grinding or other suitable mixing; and heat-treating the carbon-sulphur mixture to produce the carbon-sulphur composite material.
[0117] The carbon-sulphur composite material suitably comprises from 10 to 60 wt% of the hollow carbon spheres and from 40 to 90 wt% of sulphur. Suitably the carbon-sulphur composite material comprises from 25 to 50 wt% of the hollow carbon spheres and from 50 to 75 wt% of sulphur.
[0118] Suitably the sulphur is provided within the hollow carbon spheres. Suitably the sulphur is provided within the void of the hollow carbon spheres and / or within pores of the carbon shell of the hollow carbon spheres.
[0119] The carbon-sulphur composite material may be incorporated into an electrode for a Li-S battery using known techniques.
[0120] The fourth aspect of the present invention provides a use of hollow carbon spheres obtainable by the method of the first aspect of the invention in batteries, such as in lithium-sulphur (Li-S) batteries,lithium-ion batteries, sodium-ion batteries, sodium-sulphur and / or magnesium-sulfur. Suitably the use of the hollow carbon spheres of this fourth aspect is in lithium-sulphur (Li-S) batteries.
[0121] The hollow carbon spheres may have any of the suitable features and advantages described in relation to the first aspect. Suitably the hollow carbon spheres are obtained by the method of the first aspect.
[0122] The use of this fourth aspect suitably involves incorporating the hollow carbon spheres into an electrode, suitably as part of a carbon-sulphur composite material, as described above in relation to the third aspect.
[0123] The fifth aspect of the present invention provides a use of hollow carbon spheres obtainable by the method of the first aspect of the invention in water purification.
[0124] The sixth aspect of the present invention provides a use of hollow carbon spheres obtainable by the method of the first aspect of the invention as support materials for heterogenous catalysis.
[0125] In said uses, the hollow carbon spheres may have any of the suitable features and advantages described in relation to the first aspect. Suitably the hollow carbon spheres are obtained by the method of the first aspect.
[0126] The seventh aspect of the present invention provides a lithium-sulphur battery comprising an electrode according to the third aspect.
[0127] The electrode may have any of the suitable features or advantages of the electrode described in relation to the third aspect or of the hollow carbon spheres described in relation to the first and second aspects.
[0128] The lithium-sulphur battery of this seventh aspect suitably comprises the electrode according to the third aspect as a cathode, an anode and an electrolyte. Suitable anodes and electrolytes for use with the cathode according to the third aspect will be known to those skilled in the art.
[0129] As used herein, unless otherwise expressly specified, all numbers such as those expressing values, ranges, amounts or percentages may be read as if prefaced by the word "about", even if the term does not expressly appear. Also, the recitation of numerical ranges by endpoints includes all integer numbers and, where appropriate, fractions subsumed within that range (e.g. 1 to 5 can include 1 , 2, 3, 4 when referring to, for example, a number of elements, and can also include 1.5, 2, 2.75 and 3.80, when referring to, for example, measurements). The recitation of end points also includes the end point values themselves (e.g. from 1.0 to 5.0 includes both 1.0 and 5.0). Any numerical range recited herein is intended to include all sub-ranges subsumed therein.Singular encompasses plural and vice versa. For example, although reference is made herein to "a" material, “an” acid, and the like, one or more of each of these and any other components can be used. For example, “a” washing step can include one or more washing steps.
[0130] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as is commonly understood by one of skill in the art. All publications referenced herein are incorporated by reference thereto.
[0131] The terms "comprising", "comprises" and "comprised of’ as used herein are synonymous with "including", "includes" or "containing", "contains", and are inclusive or open-ended and do not exclude additional, non-recited members, elements or method steps. Additionally, although the present disclosure has been described in terms of “comprising”, the coating compositions detailed herein may also be described as “consisting essentially of’ or “consisting of’.
[0132] As used herein, the term "and / or," when used in a list of two or more items, means that any one of the listed items can be employed by itself or any combination of two or more of the listed items can be employed. For example, if a list is described as comprising group A, B, and / or C, the list can comprise A alone; B alone; C alone; A and B in combination; A and C in combination, B and C in combination; or A, B, and C in combination.
[0133] All of the features contained herein may be combined with any of the above in any combination.
[0134] For a better understanding of the invention, and to show how embodiments of the same may be carried into effect, reference will now be made, by way of example, to the following examples.
[0135] Examples
[0136] Example 1 - Hollow Carbon Nanospheres
[0137] Synthesis of silver-cored carbon nanospheres
[0138] A 0.5 M solution of glucose in deionised water was prepared by dissolving 6.75 g of glucose in 75 mL of deionised water. To this solution was added dropwise 3.75 mL of a 0.1 M silver nitrate solution while under continuous stirring and the resultant mixture left to stir for a further 20 mins. The mixed solution was poured into a 125 mL Teflon-lined stainless-steel autoclave and placed into a preheated oven at 180°C for 4 h, producing silver-cored carbon nanospheres. The silver-cored carbon nanospheres were isolated via centrifugation above 8000 rpm for 5 mins. The isolated silver-cored carbon nanospheres were distributed in fresh deionized water and then collected by centrifugation above 8000 rpm for 5 mins. Further steps of washing and centrifugation were performed until the supernatant was colourless. The silver-cored carbon nanospheres were then dried in an oven at 100°C for 12 hours.Annealing of silver-cored carbon nanospheres
[0139] The silver-cored carbon nanospheres were then annealed as follows under an inert argon atmosphere. The dried silver-cored carbon nanospheres were placed into a ceramic crucible and transferred to a quartz glass tube furnace. The furnace was heated from room temperature to 600°C at a ramp rate of 5°C / min. The furnace was maintained at 600°C for a further 2 hours.
[0140] Removal of silver core
[0141] The annealed silver-cored carbon nanospheres were added to a solution of 5 M nitric acid and stirred at 50°C for 24 hours, resulting in the removal of the silver core. The resulting hollow carbon nanospheres were isolated from the waste acidic solution via centrifugation above 8000 rpm for 5 mins. The isolated hollow carbon nanospheres were distributed in fresh deionized water and then collected by centrifugation above 8000 rpm for 5 mins. Further steps of washing and centrifugation were performed until the supernatant had reached a neutral pH. The hollow carbon nanospheres were then dried in an oven at 100°C for 12 hours.
[0142] Structural characterisation
[0143] Imaging of the product materials was carried out using a Hitachi SU-70 scanning electron microscope with an accelerating voltage of 10 kV, in addition to a JEOL JEM-21 OOF transition electron microscope operating at 200 kV. Powder X-ray diffraction measurements were collected using a PANalytical Empyrean diffractometer in reflection mode, with a Cu Ka radiation source (A = 1.5406 A) and tube current and voltage of 40 kV and 40mA, respectively. Raman spectroscopy was conducted using a Horiba LabRAM 300 spectrometer system, with a 632.81 nm laser and 50 x objective lens. The groove density, slit, and hole, were set to 1800, 100, and 1000, respectively. The elemental composition and binding states of the HCS / S and Ag-CS / S was investigated with a Kratos AXIS ULTRA X-ray photoelectron spectrometer, with a mono Al K 1486.58 eV, 150 W X-ray gun. Construction and peak fitting of synthetic peaks in narrow region spectra used a Shirly type background and peaks were of a mixed Gaussian-Lorentzian type.
[0144] Figure 1 shows data of silver-cored carbon nanospheres produced using the above method using 0.5 M glucose and 0.1 M silver(l) nitrate. Figure 1 displays images acquired from scanning electron microscopy (SEM) and transition electron microscopy (TEM), and particle size distribution.
[0145] Figure 1 shows the imaging and particle size measurements of the silver-cored carbon nanospheres produced by the method described above, before removal of the core, as obtained by scanning electron microscopy (SEM) (according to ISO 19749:2021) and transition electron microscopy (TEM) (according to ISO 21363:2020). The silver-cored carbon nanospheres display a well-defined coreshell morphology with a mean sphere diameter of 643 nm ± 20% and an average silver core diameter of 196 nm ± 8%, indicating a carbon shell thickness of ~224 nm.Figure 2 shows the imaging and particle size measurements (obtained by the SEM and TEM methods referenced above) of the hollow carbon nanospheres after the removal of the silver core. The hollow carbon nanospheres maintain the core-shell structure but display a reduced sphere diameter of 582nm ± 20%, corresponding to a 61 nm decrease. The slight reduction in average sphere size after the acid treatment step may be an artifact of increased washing, as the larger spheres have a lower density, they have a higher chance of being washed away during centrifugation. The core diameter of the HCS did not significantly change after silver removal, resulting in hollow carbon nanospheres having a shell thickness of ~191 nm.
[0146] Figure 3 shows the X-ray diffraction (XRD) and Raman spectroscopy characterisation of the silver-cored carbon nanospheres (Ag-CS) and the hollow carbon nanospheres of Example 2 (HCS).
[0147] The XRD pattern for Ag-CS shows four diffraction peaks at ~38°, ~44°, ~64°, and ~77° — indexed to the (111), (200), (220), and (311) diffraction planes of silver (JCPDS No. 01-071-4613). The absence of these peaks in HCS further confirms the successful removal of silver via acid etching. The XRD pattern for the HCS show two broad reflection peaks at ~24° and ~45°, which can be indexed to the (002) and (100) diffraction planes of hexagonal graphite (JCPDS No. 00-41-1487) and suggests that HCS consist of an amorphous carbon structure. This is supported by the Raman spectra in Figure 3b, which shows the presence of two characteristic D and G bands at ~1330 and 1575 cm'1, respectively. The D band corresponds to the breathing mode ofsp2hybridised carbon rings, following Aigsymmetry. The G band corresponds to in-plane bond stretching of sp2hybridised carbon, in both rings and chains, and follows E2g symmetry 10. The ID / IG ratio of Ag-CS and HCS are 0.98 and 1.07 respectively, which is indicative of an amorphous disordered carbon structure.
[0148] Example 2 - Carbon-sulphur composite
[0149] Carbon-Sulphur Composite preparation
[0150] Carbon-sulphur composites were prepared by combining the silver-cored carbon nanospheres and the hollow carbon nanospheres of Example 1 with sulphur in a 3:8 ratio by weight and homogenised with a mortar and pestle. The composites were heat treated in a quartz glass tube furnace under the following protocol: the respective carbon I sulphur mixture was transferred to a glazed ceramic boat and heated from room temperature to 155°C at 2°C min-1with a 12 h dwell time, under an inert argon atmosphere. This method provided a carbon-sulphur composite of the silver-cored carbon nanospheres (Ag-CS / S) and a carbon-sulphur composite of the hollow carbon nanospheres (HCS / S) - Example 2.
[0151] The accurate weight percentage of sulphur remaining in the composite after melt infiltration was determined using a Perkin Elmer Thermogravimetric Analyser 4000, where ~10 mg of the composite was heated at a ramp rate of 5°C min-1to 500°C under nitrogen gas. The final sulphur content of thecarbon-sulphur composites was found to be 63 wt% and 64 wt% for Ag-CS / S and HCS / S respectively.
[0152] Electrochemical Characterisation
[0153] Cathodes were prepared through a traditional slurry casting process using the Ag-CS / S and the HCS / S materials. The slurry composition included 80 wt% of the carbon-sulphur composite, 10 wt% conductive additive (Super-P, Timcal, Switzerland), and 10 wt% binder (Polyethylene oxide, MW 4,000,000 g mol-1, Sigma-Aldrich), with acetonitrile as solvent. Slurries were mixed at 12,000 rpm for 5 mins and cast onto carbon-coated aluminium foil using a doctor blade adjusted to a wet thickness of 120 urn. After 24 h drying at room temperature, electrode discs were cut with a diameter of 12.7 mm and passed into an argon-filled glovebox for coin cell assembly. The mass loading of sulphur on each electrode was approximately ~1 mg. Li-S half cells were assembled by pairing the prepared cathodes with a pure Li metal anode (GELON, China) in stainless-steel coin cells (CR2032), an 18 mm diameter Celgard 2325 membrane was used as a separator. The electrolyte composition was 1 M lithium bis(trifluoromethane) sulfonimide LiTFSI in a 2:1 mixture by weight of dimethoxyethane (DME) and 1 ,3-dioxolane (DOL) (E-Lyte Innovations, Germany), including 0.5 M lithium nitrate (Thermo Scientific, Czech Republic) additive.
[0154] A BioLogic BCS-805 battery cycler was used for cyclic voltammetry measurements, with a voltage window of 2.7-1.8 V (vs. Li / Li+) and a scan rate of 0.05 mV s-1. Galvanostatic cycling and rate capability testing was performed using a Neware Battery Testing System from C / 10 - 2C, where 1C = 1672 mA g-1, in a voltage window of 2.7-1.8 V (vs. Li / Li+). All electrochemical tests were performed at least twice using working electrodes with approximately the same S mass loadings.
[0155] The operando X-ray diffraction measurements were conducted using an XRDynamic 500 powder diffractometer (Anton Paar).
[0156] The long-term galvanostatic cycling performance and selected voltage profiles of Ag-CS / S and HCS / S electrodes cycled at C / 5 are shown in Figure 4. The Ag-CS / S sample displayed an initial specific charge of 762 mAh g-1, corresponding to a 45.57% utilisation of available sulphur (theoretical specific charge = 1672mAh g-1). After an initial stabilisation period of ~50 cycles, the specific charge proceeded to steadily decrease until it reached 326 mAh g-1at the 500thcycle, resulting in a capacity retention of 42.78% and an average C.E of 99.83% per cycle. The HCS / S electrodes showed a substantial improvement in performance and stability, with an in initial specific charge of 922 mAh g-1, corresponding to a 55.14% sulphur utilisation. At the 500thcycle, HCS / S displayed a discharge specific charge of 510 mAh g-1, resulting in a capacity retention of 55.31% and an average C.E of 99.88% per cycle. The significant improvement in both active sulphur (+160 mAh g-1) and capacity retention (+12.5%) of HCS / S relative to Ag-CS / S shows the effectiveness of hollow-cored carbon spheres as sulphur host materials for Li-S batteries, as previously described. These resultsdemonstrate that the present facile, cost-effective, and renewably focused method may produce HCS with the desired properties of effective sulphur host materials.
[0157] This is further highlighted by the excellent capacity retention after the HCS / S cell was stopped for roughly 72 hours during the 354thcycle. Stopping a Li-S cell mid cycle typically leads to either significant capacity fading or complete cell failure due to the high level of self-discharge, where soluble polysulfides migrate to the anode and are reduced to form a passive Li2S2 / Li2S layer. The discharge specific charge delivered by HCS / S electrode before pausing was 547 mAh g-1and after being paused for three days was 532 mAh g-1, resulting in a capacity loss of ~3%. This is lower than the >25% capacity loss due to self-discharge over a three-day period previously reported for Li-S batteries.
[0158] Voltage profiles from various stages of the long-term galvanostatic cycling are displayed in Figure 4(b)-(g). Both Ag-CS / S and HCS / S profiles consist of three distinct discharge (lithiation) plateaux, which are characteristic of Li-S batteries. The three regions are centred at ~2.35, 2.20, and 2.1 V (vs Li / Li+) and correspond to different stages of the sulphur reduction reaction. Firstly, solid-phase sulphur is reduced to high-order lithium polysulfides (Sa —> Li2Sa —> Li2Se). Following this, high-order polysulfides are further reduced to low-order polysulfides OJ2S6 —> Li2S4), and finally low-order polysulfides are reduced to lithium sulphide (U2S4 —> Li2S2 —> Li2S)29. The voltage profiles during charge (delithiation) consist of two plateaux centred at ~2.25 and ~2.35 V vs (Li / Li+), corresponding to the stepwise oxidation of low-order polysulfides and high-order polysulfides, respectively. Across all stages of the long-term galvanostatic cycling, HCS / S cells displayed a consistently lower polarisation, especially in the lower discharge plateau region, which suggests both a heightened electrochemical reversibility and improved redox kinetics for the sluggish Li2S2 —> Li2S reaction. Further to this, the shape of the lower voltage profile is significantly different between Ag-CS / S and HCS / S samples. HCS / S has a longer, flatter plateau with a sharper voltage drop to 1.8 V (vs Li / Li+). On the other hand, Ag-CS / S has a shorter and more rounded lower voltage plateau. As the lower voltage profile is associated with a liquid-solid phase change as low order polysulfides are reduced to Lithium sulfide, the length and flatness of the plateau gives an insight into the level of soluble lithium polysulfides that remain available for further reduction. This indicates that HCS / S electrodes are better able to confine the soluble long-chain polysulfides, reducing the shuttle effect and maintaining a higher capacity for longer.
[0159] In summary, the present invention provides a method for preparing hollow carbon nanospheres through a hard templating route, suitably utilising glucose as an inexpensive carbon source and silver nitrate as an easily recoverable hard template precursor. In this reaction, the hard template and carbon shell are synthesised in a single hydrothermal process, preventing the necessity of template preparation prior to carbon sphere synthesis. This initial hydrothermal reaction produces carbon nanospheres with an internal silver core, which is easily removed through nitric acid digestion, leavinghollowed carbon nanospheres along with a silver nitrate solution which can be processed with established silver recovery procedures for use with further HCS production.
[0160] Attention is directed to all papers and documents which are filed concurrently with or previous to this specification in connection with this application and which are open to public inspection with this specification, and the contents of all such papers and documents are incorporated herein by reference.
[0161] All of the features disclosed in this specification (including any accompanying claims, abstract and drawings), and / or all of the steps of any method or process so disclosed, may be combined in any combination, except combinations where at least some of such features and / or steps are mutually exclusive.
[0162] Each feature disclosed in this specification (including any accompanying claims, abstract and drawings) may be replaced by alternative features serving the same, equivalent or similar purpose, unless expressly stated otherwise. Thus, unless expressly stated otherwise, each feature disclosed is one example only of a generic series of equivalent or similar features.
[0163] The invention is not restricted to the details of the foregoing embodiment(s). The invention extends to any novel one, or any novel combination, of the features disclosed in this specification (including any accompanying claims, abstract and drawings), or to any novel one, or any novel combination, of the steps of any method or process so disclosed.
Claims
Claims1. A method of producing hollow carbon spheres, the method comprising the steps:(a) providing a precursor solution comprising a carbon-containing material and a silver salt, and arranging the precursor solution in a reaction vessel;(b) heating the precursor solution in the reaction vessel to produce silver-cored carbon spheres; and(c) treating the silver-cored carbon spheres produced in step (b) with an acidic solution to remove the silver core and provide the hollow carbon spheres.
2. The method according to claim 1, wherein the carbon-containing material comprises a saccharide.
3. The method according to claim 2, wherein the saccharide is glucose.
4. The method according to any preceding claim, wherein the silver salt is silver(l) nitrate.
5. The method according to any preceding claim wherein step (b) involves heating the precursor solution at a temperature of at least 100 °C for a period of time of at least 1 hour.
6. The method according to any preceding claim, wherein step (b) is followed by a step (b2) of centrifugation of the silver cored spheres.
7. The method according to any preceding claim, wherein step (b) is followed by a step (b3) of annealing the silver-cored carbon spheres produced in step (b).
8. The method according to claim 7, wherein step (b3) involves annealing the silver-cored carbon spheres at a temperature of at least 400°C for a period of time of at least 1 hour.
9. The method according to any preceding claim, wherein step (c) further comprises one or more washing steps wherein the hollow carbon spheres are washed with an aqueous washing solution.
10. The method according to any preceding claim, wherein the acidic solution of step (c) comprises nitric acid.
11. The method according to any preceding claim wherein the silver-cored carbon spheres are essentially free of silicon.
12. The method according to any preceding claim wherein the method is essentially free of hydrofluoric acid.
13. The method according to any preceding claim wherein the hollow carbon spheres are essentially free of silver.
14. The method according to any preceding claim, wherein the method comprises the steps:(d) isolating the hollow carbon spheres from the acidic solution to provide a waste acidic solution; and(e) treating the waste acidic solution produced in step (d) to obtain recovered silver material.
15. The method according to any preceding claim, wherein the hollow carbon spheres are hollow carbon nanospheres.
16. Hollow carbon spheres obtainable by the method of any one of claims 1 to 15.
17. An electrode for a battery, the electrode comprising hollow carbon spheres obtainable by the method of any one of claims 1 to 15.
18. The electrode of claim 17, wherein the electrode is a cathode.
19. The electrode of claim 18, wherein sulphur is provided within the hollow carbon spheres.
20. Use of hollow carbon spheres obtainable by the method of any one of claims 1 to 15 in batteries, such as in lithium-sulphur (Li-S), lithium-ion batteries, sodium-ion batteries, sodiumsulphur and / or magnesium-sulphur batteries.
21. Use of hollow carbon spheres obtainable by the method of any one of claims 1 to 15 in water purification.
22. Use of hollow carbon spheres obtainable by the method of any one of claims 1 to 15 as support materials for heterogenous catalysis.
23. A lithium-sulphur battery comprising an electrode according to any one of claims 17 to 19.