Composition comprising a fluorinated polymer and a hydrophilic polymer and use thereof as an electrode binder

A fluorinated and hydrophilic polymer combination addresses the bonding and gelation issues of lithium-ion battery binders, improving processability and stability of electrode compositions, particularly with phosphoolivine-type active materials, by reducing viscosity and enhancing manufacturing efficiency and electrode lifespan.

WO2026238811A1PCT designated stage Publication Date: 2026-11-19ARKEMA FRANCE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063939
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing lithium-ion battery binders, such as polyvinylidene fluoride (PVDF), face challenges in bonding to other materials and can cause rapid gelation in the presence of lithium iron phosphate-type active ingredients, hindering the processability and stability of electrode compositions.

Method used

A binding composition comprising a fluorinated polymer P1 and a hydrophilic polymer P2, with specific repeating units derived from vinylidene fluoride and functionalized monomers, improves the rheological properties of lithium ion cathode slurry, reducing viscosity and preventing gelation, thereby enhancing the processability and stability of electrode compositions containing phosphoolivine-type active materials.

Benefits of technology

The composition increases the dry extract content while maintaining low viscosity, facilitating manufacturing, reducing production costs, and ensuring consistent electrode performance and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000004_0001
    Figure IMGF000004_0001
  • Figure IMGF000004_0002
    Figure IMGF000004_0002
  • Figure IMGF000004_0003
    Figure IMGF000004_0003
Patent Text Reader

Abstract

The present invention relates to a binder composition for a lithium-ion battery, characterized in that it comprises a fluorinated polymer P1 and a hydrophilic polymer P2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Composition comprising a fluorinated polymer and a hydrophilic polymer, and its use as an electrode binder.

[0002] Technical field of the invention

[0003] The present invention relates generally to the field of electrical energy storage in rechargeable Li-ion secondary batteries. More specifically, the invention relates to a composition for electrode preparation.

[0004] Technological background of the invention

[0005] Lithium batteries are increasingly used due to their higher voltages and energy densities compared to conventional batteries (such as Ni-MH batteries). A basic cell of a Li-ion storage battery, or lithium battery, comprises an anode (discharge) and a cathode (also discharge), typically made of a metal oxide lithium interlayer compound, such as LiMn2O4, LiCoO2, or LiNiO2, between which an electrolyte that conducts lithium ions is inserted.

[0006] Rechargeable or secondary batteries are more advantageous than primary (non-rechargeable) batteries because the associated chemical reactions that occur at the positive and negative electrodes of the battery are reversible. The electrodes of secondary cells can be regenerated multiple times by applying an electrical charge. Numerous advanced electrode systems have been developed to store electrical charge. At the same time, considerable effort has been devoted to developing electrolytes capable of improving the performance of electrochemical cells.

[0007] For their part, electrodes generally comprise at least one current collector coated with a film of a composite material consisting of an active material (because it has electrochemical activity towards lithium), a polymer that acts as a binder, one or more electroconductive additives (usually carbon black or acetylene black), and possibly a surfactant. Binders are considered inactive components because they do not directly contribute to cell capacity. However, their key role in electrode processing and their considerable influence on the electrochemical performance of the electrodes have been extensively described. The main relevant physical and chemical properties of binders are thermal stability, chemical and electrochemical stability, tensile strength (strong adhesion and cohesion), and flexibility.The main purpose of using a binder is to form stable networks of the solid components of the electrodes, i.e., the active materials and conductive agents (cohesion). In addition, the binder must ensure close contact between the composite electrode and the current collector (adhesion).

[0008] Polyvinylidene fluoride (PVDF) is used as a binder in lithium-ion batteries due to its excellent electrochemical stability, good bonding capacity, and strong adhesion to electrode materials and current collectors. In wet suspension processes for electrode preparation, the active materials and binders are dispersed in a liquid solution. This liquid solution is typically based on organic solvents or water. The dispersion is poured onto a current collector and then dried in a high-temperature oven to produce an electrode. Unfortunately, the excellent properties provided by fluoropolymers such as PVDF can also limit their applications. For example, fluoropolymers are difficult to bond to other materials.Therefore, organic solvents and other organic additives are generally used in coating formulations to ensure good adhesion between PVDF-based polymers, a porous separator or electrode, and possibly added powder particles. Alternatively, fluoropolymer binders can carry functional groups to enhance the polymer's adhesive behavior. It has been observed that in the presence of a phosphoolivine-type active ingredient, electrode compositions tend to gel rapidly, hindering good processability of the electrode composition on the current collector. Consequently, the development of new binders is still needed to prepare electrode compositions that remain stable over time, even in the presence of a lithium iron phosphate-type active ingredient.

[0009] Summary of the invention

[0010] According to a first aspect, the present invention relates to a binding composition for a lithium-ion battery characterized in that it comprises a fluorinated polymer P1 and a hydrophilic polymer P2; said fluorinated polymer P1 comprises repeating units derived from vinylidene fluoride, repeating units derived from a monomer M1a of formula (la) R 1 R 2 C=C(R 3 )(C(O)OY 1 ) and repeating units derived from a monomer M1b of formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which

[0011] R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently selected from the group consisting of H, CO2H and C^Cs alkyl;

[0012] Y 1 is selected from the group consisting of H, C1-C5 alkyl substituted by an OH group;

[0013] Y 2is selected from the group consisting of CO2H, SO3H and PO3H2;

[0014] X 1 is an atomic group having a molecular weight less than or equal to 456 having a main chain composed of 1 to 18 atoms;

[0015] said hydrophilic polymer P2 comprises repeating units derived from a monomer M2a of formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CTCS alkyl; R d is -OR d 'with R d 'selected from the group consisting of Ci-Ci8alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -OC(O)R d ”, -C(O)OR d "or a nitrogenous heterocycle with 5 or 6 links; R d "being selected from the group consisting of alkyl CTCG and C6-C 12aryl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H.

[0016] The present invention makes it possible to improve the rheological properties of lithium ion cathode slurry by reducing the viscosity of the slurry at the same dry extract, making it possible to improve the dry extract at similar viscosity.

[0017] The binding composition according to the present invention improves the processability of electrode compositions, particularly those containing phosphoolivine-type active materials, by limiting gelation. This composition thus increases the dry extract content while maintaining low viscosity, facilitating the manufacturing process, reducing production costs, and ensuring consistent performance and an improved electrode lifespan.

[0018] According to a preferred embodiment, said hydrophilic polymer P2 also comprises repeating units derived from a monomer M2b or a monomer M2c; said monomer M2b being selected from the group consisting of monomers of formula (II), (III), (IV), (V), (VI), (VII) or (VIII)R 10 R 11 C=C(R 12 )C(O)OH (II)

[0019] R 13 R 14 C=C(R 15 )(OC(O)R 16 ) (III);

[0020] R 17 R 18 C=CR 19 C(O)OC(O)CR 20 =CR 21 R 22 (IV);

[0021] [Chem 1]

[0022]

[0023] (V)

[0024] [Chem 2]

[0025]

[0026] (VI)

[0027] R 33 R 34 C=CR 35 (CN) (VII);

[0028] R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0029] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;

[0030] R 13 , R 14 and R 15 are independently selected from the group consisting of H and C1-C5 alkyl;

[0031] R 16 is C1-C5 alkyl;

[0032] p22 p23 p24 p25 p26 p27 p28 p29 p30 p31 p32 p33 p34 p35 p36 p37

[0033]

[0034] and R 38 are independently selected from the group consisting of H and C1-C5alkyl;

[0035] R 39 and R 40 are independently selected from the group consisting of H and C 10 alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -OPO3H2, -C(O)OR 41 or -OC(O)R 41 R 41being selected from the group consisting of C1-C5 alkyl and C6-Ci2aryl optionally substituted by one or more CO2H functional groups;

[0036] said monomer M2c comprising at least two vinyl groups and selected from the group consisting of divinyl aryl, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers, and tetra- or tri-(meth)acrylate esters monomers. In a preferred embodiment, said hydrophilic polymer P2 comprises from 0.01 to 30 mole percent of repeating units derived from monomer M2b or monomer M2c. In a preferred embodiment, said hydrophilic polymer P2 comprises at least 50 mole percent of repeating units derived from monomer M2a.

[0037] According to a preferred embodiment, said monomer M2b is selected from the group consisting of monomers of formula (II), (VII) or (VIII)

[0038] R 10 R11 C=C(R 12 )C(O)OH (II)

[0039] R 33 R 34 C=CR 35 (CN) (VII);

[0040] R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0041] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;

[0042] R 33 , R 34 , R 35 , R 36 , R 37 and R 38 are independently selected from the group consisting of H and C1-C5 alkyl;

[0043] R 39 and R 40 are independently selected from the group consisting of H and Ci-C 10 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -C(O)OR 41 OR -OC(O)R 41 R 41 being selected from the group consisting of C^-Cs alkyl and C6-C 12aryl optionally substituted by one or more CO2H functional groups; and

[0044] said monomer M2c comprises at least two vinyl groups and is selected from the group consisting of divinyl aryl, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers and tetra or tri-(meth)acrylate esters.

[0045] According to a preferred embodiment, said monomer M2b is selected from the group consisting of monomers of formula (II) R 10 R 11 C=C(R 12 )C(O)OH (II) in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C3 alkyl; preferably R 10 , R 11 and R 12 are independently selected from the group consisting of H and CH3.

[0046] According to a preferred embodiment, the mass ratio P1 / P2 is from 50 / 50 to 99 / 1, preferably from 70 / 30 to 99 / 1.

[0047] According to a preferred embodiment, said monomer M1b is selected from the group consisting of 2-carboxyethyl (meth)acrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxypropyl succinate, and mixtures thereof. According to a preferred embodiment, said monomer M1a is selected from the group consisting of acrylic acid, methacrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxyethylhexyl (meth)acrylate, and mixtures thereof. According to a preferred embodiment, said polymer P1 comprises at least 60 mole percent of repeating units derived from vinylidene fluoride.

[0048] According to a preferred embodiment, said polymer P1 comprises less than 10% by moles of repeating units derived from monomer M1a.

[0049] According to a preferred embodiment, said polymer P1 comprises less than 10% by moles of repeating units derived from monomer M1b.

[0050] According to a preferred embodiment, said monomer M2a has the formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CH3; R d is -OR d 'with R d 'selected from the group consisting of C1-C5 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -OC(O)R d ”, -C(O)OR d R d " being selected from the group consisting of C^Ca alkyl and C6aryl optionally substituted by one or more -OH or -CO2H functional groups.

[0051] The present invention also relates to an electrode composition comprising said binding composition according to the present invention, an active material and optionally a conductive agent, an additive or a mixture of both.

[0052] According to a preferred embodiment, said electrode composition comprises a conductive agent composed of one or more materials selected from the group consisting of carbon black, graphite, carbon fibers, carbon nanotubes, carbon nanofibers, metal powders such as SUS powder and aluminum powder, or mixtures thereof.

[0053] According to a preferred embodiment, said active material is selected from the group consisting of phospho-olivine materials of formula LixAyDzPO4 in which A is selected from the group consisting of Mn, Fe, Co, Ni and Cu; D is selected from the group consisting of Mg, Ca, Sr and Ba; x, y and z being numbers satisfying the equation: 0.9 < x < 1.2, 0 < y < 1.5 and 0 < z < 1.5; or mixtures thereof.

[0054] According to a preferred embodiment, said active material is selected from the group consisting of lithium iron phosphate, lithium manganese iron phosphate and lithium manganese phosphate. The present invention also relates to an electrode comprising a current collector and a layer consisting of said electrode composition according to the present invention.

[0055] The present invention also relates to a Li-ion battery comprising a positive electrode, a negative electrode and a separator, characterized in that said positive electrode is an electrode according to the present invention.

[0056] Detailed description of the present invention

[0057] According to a first aspect, a composition comprising a fluorinated polymer P1 and a hydrophilic polymer P2 is provided. The specific combination between the fluorinated polymer P1 and said polymer P2 improves the stability of electrode compositions containing a phospho-olivine type active material. According to a preferred embodiment, the mass ratio P1 / P2 is 50 / 50 to 99 / 1, advantageously 55 / 45 to 98 / 2, preferably 60 / 40 to 97 / 3, more preferably 65 / 35 to 96 / 4, in particular 70 / 30 to 95 / 5, more particularly 80 / 20 to 95 / 5, and preferably 85 / 15 to 95 / 5.

[0058] Fluorinated polymer P1

[0059] The fluorinated polymer P1 according to the present invention comprises at least three types of repeating units derived from three different monomers: vinylidene fluoride, monomer M1a as defined below, and monomer M1b as defined below. Monomer M1a is different from monomer M1b. Thus, the fluorinated polymer P1 comprises repeating units derived from vinylidene fluoride, repeating units derived from monomer M1a of formula (la)R 1 R 2 C=C(R 3 )(C(O)OY 1 ) and repeating units derived from a monomer M1b of formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which

[0060] R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;

[0061] Y 1is selected from the group consisting of H, C1-C5 alkyl substituted by an OH group;

[0062] Y 2 is selected from the group consisting of CO2H, SO3H and PO3H2;

[0063] X 1 is an atomic group having a molecular weight less than or equal to 456 having a main chain composed of 1 to 18 atoms.

[0064] Preferably, said monomer M1a has the formula (la) R 1 R 2 C=C(R 3 )(C(O)OY 1 ) in which R 1 , R 2 and R 3 are independently selected from the group consisting of H, CO2H and C1-C3 alkyl; Y 1 is selected from the group consisting of H, CTCS alkyl substituted by an OH group. More preferably, said monomer M1a has the formula (la) R 1 R 2 C=C(R 3 )(C(O)OY 1 ) in which R 1 , R 2 and R 3are independently selected from the group consisting of H and C^-Cs alkyl; Y 1 is selected from the group consisting of H, C^-Cs alkyl substituted with an OH group. In particular, said monomer M1a is selected from the group consisting of acrylic acid, methacrylic acid, hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxyethylhexyl(meth)acrylate, and mixtures thereof. More specifically, said monomer M1a is selected from the group consisting of acrylic acid, hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, and mixtures thereof.

[0065] Preferably, said monomer M1b has the formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H, CO2H and Ci-C5alkyl; Y 2is selected from the group consisting of CO2H, SO3H and PO3H2; X 1 is an atomic group having a molecular weight less than or equal to 456 having a main chain composed of 1 to 18 atoms.

[0066] More preferably, said monomer M1b has the formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H, CO2H and C^-Cs alkyl; Y 2 is selected from the group consisting of CO2H, SO3H and PO3H2; X 1 is an atomic group having a molecular weight less than or equal to 456 and a main chain composed of 1 to 18 atoms. In particular, said monomer M1 b has the formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 4 , R 5 and R 6are independently selected from the group consisting of H and Ci-C3 alkyl; Y 2 is selected from the group consisting of CO2H; X 1 is an atomic group having a molecular weight less than or equal to 456 having a main chain composed of 1 to 18 atoms.

[0067] Preferably, said monomer M1b has the formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H and C^-Ca alkyl; Y 2 is selected from the group consisting of CO2H; X 1 is an atomic group having a molecular weight less than or equal to 256 and a main chain composed of 1 to 13 atoms. More preferably, said monomer M1b has the formula (Ib)R 4 R 5 C=C(R 6 )(C(O)-OX 3 -Y 2) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H and C1-C3 alkyl; Y 2 is selected from the group consisting of CO2H; X 3 is an atomic group having a molecular weight less than or equal to 240 having a main chain composed of 1 to 13 atoms.

[0068] In particular, said monomer M1b has the formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H and CT-C3 alkyl; Y 2 is selected from the group consisting of CO2H; X 1 is an atomic group having a molecular weight less than or equal to 156 and a main chain composed of 1 to 8 atoms. More specifically, said monomer M1b has the formula (Ib)R 4 R5 C=C(R 6 )(C(O)-OX 3 -Y 2 ) in which R 4 , R 5 and R 6 are independently selected from the group consisting of H and C1-C3 alkyl; Y 2 is selected from the group consisting of CO2H; X 3 is an atomic group having a molecular weight less than or equal to 140 having a main chain composed of 1 to 8 atoms.

[0069] In particular, said monomer M1b is selected from the group consisting of 2-carboxyethyl (meth)acrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxyethyl phthalate, (meth)acryloyloxypropyl succinate, and mixtures thereof. More specifically, said monomer M1b is selected from the group consisting of 2-carboxyethyl (meth)acrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxypropyl succinate, and mixtures thereof. More specifically, said monomer M1b is 2-carboxyethyl (meth)acrylate.

[0070] Preferably, the repeating units from monomers M1a and M1b are randomly distributed within the chain of the fluorinated polymer P1. In particular, at least 40%, preferably at least 50%, and in particular at least 70% of the repeating units from monomers M1a and M1b are randomly distributed within the chain of the fluorinated polymer P1. The random distribution of the repeating units from monomers M1a and M1b corresponds to the ratio of [(the number, in moles, of repeating units from monomers M1a and M1b arranged between two vinylidene fluoride units) / (the total number, in moles, of repeating units from monomers M1a and M1b in the fluorinated polymer P1)*100]. The random distribution of the repeating units from monomers M1a and M1b is determined by NMR. 1 H and 19 F (DMSO solvent d 6 ) by integrating the -CF2 signals at -18 ppm in 19 F (reference TFA) and -OH signals at 12.5 ppm in 1H. Said fluorinated polymer P1 preferably has a melt viscosity greater than 2000 Pa.s measured at 232°C and a shear stress of 100 s -1 according to ASTM D3835. Preferably, said fluorinated polymer P1 comprises at least 60 mole percent of repeating units derived from vinylidene fluoride, advantageously at least 70 mole percent, preferably at least 80 mole percent, more preferably at least 90 mole percent, in particular at least 95 mole percent.

[0071] Preferably, said fluorinated polymer P1 comprises less than 10% by mole of repeating units derived from monomer M1a, advantageously less than 8% by mole, preferably less than 5% by mole. Preferably, said fluorinated polymer P1 comprises from 0.01% to 10% by mole, advantageously from 0.05% to 8% by mole, preferably from 0.1% to 5% by mole of repeating units derived from monomer M1a.

[0072] Preferably, said fluorinated polymer P1 comprises less than 10% by mole of repeating units derived from monomer M1b, advantageously less than 8% by mole, preferably less than 5% by mole. Preferably, said fluorinated polymer P1 comprises from 0.01% to 10% by mole, advantageously from 0.01% to 8% by mole, preferably from 0.01% to 5% by mole, in particular from 0.05% to 5% by mole, more particularly from 0.1% to 5% by mole of repeating units derived from monomer M1b.

[0073] In one embodiment, the average particle size of polymer P1 is between 10 and 1000 nm. In another embodiment, the average particle size is between 1 µm and 200 µm, preferably from 1 µm to 100 µm. The average particle size is determined by laser diffraction. A Malvern INSITEC System particle size analyzer is used for the measurement. This measurement is performed using a dry method by laser diffraction on a powder with a focal length of 100 mm.

[0074] In certain embodiments, the vinylidene fluoride contained in said fluorinated polymer P1 is bio-based. The term "bio-based" means "derived from biomass." This improves the polymer's environmental footprint. Bio-based vinylidene fluoride can be characterized by a renewable carbon content, i.e., carbon of natural origin from a biomaterial or biomass, of at least 1 atomic percent as determined by the 14C content according to standard NF EN 16640. The term "renewable carbon" indicates that the carbon is of natural origin and comes from a biomaterial (or biomass), as described below.According to some embodiments, the bio-carbon content of VDF may be greater than 5%, preferably greater than 10%, preferably greater than 25%, preferably greater than or equal to 33%, preferably greater than 50%, preferably greater than or equal to 66%, preferably greater than 75%, preferably greater than 90%, preferably greater than 95%, preferably greater than 98%, preferably greater than 99%, advantageously equal to 100%.

[0075] According to a preferred embodiment, the fluorinated polymer P1 is prepared by a suspension or emulsion polymerization process forming a latex, which may optionally be dried to obtain a fluorinated polymer P1 in powder form. The polymerization step involves vinylidene fluoride, monomer M1a, and monomer M1b as defined above.

[0076] The polymerization step can be carried out at a temperature above 40°C, preferably at a temperature of 40°C to 120°C, in particular from 40°C to 90°C.

[0077] The polymerization step can be carried out at a pressure of 10 to 120 bara, advantageously at a pressure of 15 to 110 bara, preferably at a pressure of 20 to 110 bara, and particularly at 40 to 110 bara. During the polymerization reaction, the pressure applied is higher than the critical pressure of vinylidene fluoride. The pressure can be maintained by the continuous addition of monomer M1a, monomer M1b, or water or an aqueous solution thereof.

[0078] Preferably, said monomers M1a and M1b are added to said reactor in the form of an aqueous solution. According to a preferred embodiment, said monomers M1a and M1b are added continuously to said reactor in order to ensure a random (homogeneous) distribution of the latter in said polymer P1.

[0079] The process is preferably carried out in the presence of an initiator. The initiator may be one or a combination of several of the initiators known in the art to be useful in the dispersion polymerization of halogenated monomers. Suitable, non-limiting classes of initiators include persulfate salts, peroxides, and redox systems. Examples of persulfate salts are sodium persulfate, potassium persulfate, and ammonium persulfate. The amount of persulfate salt added to the reaction mixture, based on the total weight of monomer added to the reaction mixture, is typically about 0.005 to about 1.0% by weight. Useful organic peroxides include dialkyl peroxides, alkyl hydroperoxides, peroxyesters, and peroxydicarbonates. A suitable example of a dialkyl peroxide is di-tert-butyl peroxide.Examples of suitable peroxy esters include tert-amyl peroxypivalate, tert-butyl peroxypivalate, and succinic acid peroxide. Examples of suitable peroxydicarbonate initiators include di-n-propyl peroxydicarbonate and di-n-propyl peroxydicarbonate, which are typically added to the reaction mixture in an amount based on the total weight of monomer added to the reaction mixture, ranging from approximately 0.05 to approximately 2.5% by weight. The initiator may comprise a redox system. By "redox system," we mean a system comprising an oxidizing agent, a reducing agent, and possibly a promoter acting as an electron-transfer medium. The promoter is a component that, in different oxidation states, is capable of reacting with both the oxidizing and reducing agents, thereby accelerating the overall reaction.Oxidizing agents include, for example, persulfate salts; peroxides, such as hydrogen peroxide; hydroperoxides, such as tert-butyl hydroperoxide and cumene hydroperoxide; and oxidizing metal salts, such as ferric sulfate and potassium permanganate. Examples of reducing agents include sodium formaldehyde sulfoxylate; sodium or potassium sulfite, bisulfite, or metabisulfite; ascorbic acid; oxalic acid; and reduced metal salts. Typical promoters include transition metal salts, such as ferrous sulfate. In redox systems, the oxidizing and reducing agents are typically used in amounts of about 0.01 to about 0.5% by weight, based on the total weight of monomer added to the reaction mixture.The promoter, if used, is typically employed in an amount of about 0.005 to about 0.025% by weight based on the total weight of monomer added to the reaction mixture.

[0080] The process can be carried out in the presence of a phase-transfer agent. This agent can be a dispersant, preferably when the process is carried out in suspension. The dispersant can be polyvinyl alcohol (PVA) or a compound comprising a cellulose moiety such as cellulose ethers; for example, methylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, or ethylhydroxyethylcellulose. The phase-transfer agent can be a surfactant, preferably when the process is carried out in emulsion. For example, the surfactant comprises a polyethylene glycol segment and a polypropylene glycol segment. Preferably, the surfactant has an HLB value of 1 to 20, in particular an HLB value of 1 to 5 or 10 to 15. In particular, the surfactant comprising a polyethylene glycol segment and a polypropylene glycol segment has an HLB value of 1 to 5 and a weight-average molecular weight of 2500 to 10000 g·mol⁻¹.Alternatively, the surfactant, comprising a polyethylene glycol segment and a polypropylene glycol segment, has an HLB value of 10 to 15 and a weight-average molecular weight of 500 to 2500 g·mol⁻¹. A paraffin antifouling agent may optionally be used in the polymerization. Any long-chain saturated hydrocarbon wax or oil may be used. The oil or wax is added to the reactor before fluoropolymer formation, in sufficient quantity to minimize polymer adhesion to reactor components. This quantity is generally proportional to the reactor's internal surface area and may range from approximately 1 to approximately 40 mg / cm² of the reactor's internal surface area. If a paraffin wax or hydrocarbon oil is used as an antifouling agent, the quantity used is typically about 5 mg / cm² of the reactor's internal surface area.

[0081] The polymerization reaction mixture may optionally contain a buffering agent to maintain a controlled pH during the polymerization reaction. The pH is typically controlled within the range of 3 to 8. The buffering agent may be added at the beginning, at various points, or throughout the polymerization process. Suitable buffering agents include phosphate buffers and acetate buffers, which are well known to those skilled in the art.

[0082] Molecular weight regulators, also known as chain transfer agents, can be used to adjust the molecular weight profile of the product. They can be added in a single portion at the beginning of the reaction, gradually, or continuously throughout the reaction. The amount of molecular weight regulator added to the polymerization reaction is typically about 0.05 to about 5% by weight, more commonly about 0.1 to about 2% by weight, based on the total weight of the monomer added to the reaction mixture. Oxygenated compounds such as alcohols, carbonates, ketones, esters, and ethers can be used as molecular weight regulators. Examples of suitable oxygenated compounds include isopropyl alcohol, acetone, ethyl acetate, and diethyl carbonate.Other classes of molecular weight regulators include halogenated compounds such as chlorocarbons, hydrochlorocarbons, hydrofluorocarbons, chlorofluorocarbons, and hydrochlorofluorocarbons. Specific examples of halogenated molecular weight regulators include 1-fluoroethane, trichlorofluoromethane, and 1,1-dichloro-2,2,2-trifluoroethane. Certain hydrocarbons can be used as molecular weight regulators, such as hydrocarbons containing two to five carbon atoms, with ethane and propane being specific examples. The P1 polymer obtained at the end of the reaction can be washed and dried to form a powder. Alternatively, the P1 polymer obtained at the end of the reaction can be washed and used as a latex.

[0083] Hydrophilic polymer P2

[0084] Said hydrophilic polymer P2 comprises repeating units derived from a monomer M2a of formula (I) R aR b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and C1-C5 alkyl; R d is -OR d 'with R d 'selected from the group consisting of Ci-C alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -OC(O)R d ”, -C(O)OR d "or a nitrogenous heterocycle with 5 or 6 links; R d " being selected from the group consisting of Ci-C6alkyl and C6-Ci2aryl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H.

[0085] Preferably, said monomer M2a has the formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and C^-Ca alkyl; Rd is -OR d 'with R d 'selected from the group consisting of CTCTS alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -OC(O)R d ”, -C(O)OR d R d "being selected from the group consisting of alkyl CTCG and C6-C 12 aryl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H.

[0086] More preferably, said monomer M2a has the formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and Ci-C3alkyl; R d is -OR d 'with R d 'selected from the group consisting of C1-C10 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -OC(O)R d ”, -C(O)ORd R d " being selected from the group consisting of Ci-C3alkyl and C6aryl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H.

[0087] In particular, said monomer M2a has the formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CH3; R d is -OR d 'with R d 'selected from the group consisting of C-C8 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -OC(O)R d ”, -C(O)OR d R d " being selected from the group consisting of CTCSalkyl and C6aryl optionally substituted by one or more -OH or -CO2H functional groups.

[0088] More specifically, said monomer M2a has the formula (I) Ra R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CH3; R d is -OR d 'with R d 'selected from the group consisting of C-C5 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -OC(O)R d ”, -C(O)OR d R d " being selected from the group consisting of C1-C3 alkyl and C6 aryl optionally substituted by one or more -OH or -CO2H functional groups.

[0089] Preferably, said hydrophilic polymer P2 comprises at least 50%, advantageously at least 60%, preferably at least 70%, in particular at least 80%, more particularly at least 85% by moles of repeating units from a monomer M2a. As mentioned above, said hydrophilic polymer P2 also comprises repeating units from a monomer M2b or a monomer M2c; said monomer M2b being selected from the group consisting of monomers of formula (II), (III), (IV), (V), (VI), (VII) or (VIII).

[0090] R 10 R 11 C=C(R 12 )C(O)OH (II)

[0091] R 13 R 14 C=C(R 15 )(OC(O)R 16 ) (III);

[0092] R 17 R 18 C=CR 19 C(O)OC(O)CR 20 =CR 21 R 22 (IV);

[0093] [Chem 1]

[0094]

[0095] (V)[Chem 2]

[0096]

[0097] (VI)

[0098] R 33 R 34 C=CR 35 (CN) (VII);

[0099] R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0100] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;

[0101] R 13 , R 14 and R 15 are independently selected from the group consisting of H and C1-C5 alkyl;

[0102] R 16 is C1-C5 alkyl;

[0103] p17 p18 p19 p20 p21 p22 p23 p24 p25 p26 p27 p28 p29 p30 p31 p32 p33 p34 p35 p36 R

[0104]

[0105] 38 are independently selected from the group consisting of H and C1-C5 alkyl; R 39 and R 40are independently selected from the group consisting of H and C1-C10 alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -C(O)OR 41 or -OC(O)R 41 R 41 being selected from the group consisting of alkyl CTCS and C6-C 12 aryl optionally substituted by one or more CO2H functional groups;

[0106] said monomer M2c comprising at least two vinyl groups and being selected from the group consisting of divinyl aryl, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers and tetra or tri-(meth)acrylate esters.

[0107] Preferably, said monomer M2b being selected from the group consisting of monomers of formula (II), (III), (IV), (V), (VI), (VII) or (VIII)

[0108] R 10 R 11 C=C(R 12 )C(O)OH (II)

[0109] R13 R 14 C=C(R 15 )(OC(O)R 16 ) (III);

[0110] R 17 R 18 C=CR 19 C(O)OC(O)CR 20 =CR 21 R 22 (IV); [Chem 1]

[0111] o

[0112] (V)

[0113]

[0114] R 33 R 34 C=CR 35 (CN) (VII);

[0115] R36R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0116] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;

[0117] R 13 , R 14 and R 15 are independently selected from the group consisting of H and C1-C3 alkyl;

[0118] R 16 is C1-C3 alkyl;

[0119] p17 p18 p19 p20 p21 p22 p23 p24 p25 p26 p27 p28 p29 p30 p31 p32 p33 p34 p35 p36 R

[0120]

[0121] 38 are independently selected from the group consisting of H and C1-C3 alkyl; R 39 and R 40 are independently selected from the group consisting of H and C1-C5 alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -C(O)OR 41 or -OC(O)R 41 R 41 being selected from the group consisting of CTCS alkyl and C6-C8aryl optionally substituted by one or more CO2H functional groups.

[0122] More preferably, said monomer M2b is selected from the group consisting of monomers of formula (II), (VII) or (VIII)

[0123] R 10 R 11 C=C(R 12 )C(O)OH (II)

[0124] R 33 R 34 C=CR 35 (CN) (VII);

[0125] R 36 R 37 C=CR 38 (C(O)NR 39 R 40) (VIII);

[0126] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl;R 33 , R 34 , R 35 , R 36 , R 37 and R 38 are independently selected from the group consisting of H and CTCS alkyl;

[0127] R 39 and R 40 are independently selected from the group consisting of H and Ci-C alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -C(O)OR 41 OR -OC(O)R 41 R 41 being selected from the group consisting of alkyl CTCS and C6-C 12 aryl optionally substituted by one or more CO2H functional groups.

[0128] In particular, said monomer M2b is selected from the group consisting of monomers of formula (II), (VII) or (VIII)

[0129] R 10R 11 C=C(R 12 )C(O)OH (II)

[0130] R 33 R 34 C=CR 35 (CN) (VII);

[0131] R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0132] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C3 alkyl;

[0133] R 33 , R 34 , R 35 , R 36 , R 37 and R 38 are independently selected from the group consisting of H and CTC3alkyl;

[0134] R 39 and R 40 are independently selected from the group consisting of H and C^Cs alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -C(O)OR 41 OR -OC(O)R 41 R 41being selected from the group consisting of Ci-C3alkyl and C6-C8aryl optionally substituted by one or more CO2H functional groups.

[0135] More specifically, said monomer M2b is selected from the group consisting of monomers of formula (II), (VII) or (VIII)

[0136] R 10 R 11 C=C(R 12 )C(O)OH (II)

[0137] R 33 R 34 C=CR 35 (CN) (VII);

[0138] R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII);

[0139] in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and Ci-C3alkyl, preferably R 10 , R 11 and R 12 are independently selected from the group consisting of H and CH3;

[0140] R 33 , R 34 , R 35 , R 36 , R 37and R 38 are independently selected from the group consisting of H and CTC3alkyl;

[0141] R 39 and R 40 are independently selected from the group consisting of H and C^Cs alkyl optionally substituted by one or more functional groups -OH, -CO2H, -C(O)OR 41 or -OC(O)R 41 R 41 being selected from the group consisting of C1-C3 alkyl and C6aryl optionally substituted by one or more CO2H functional groups.

[0142] Preferably, said monomer M2c comprises at least two vinyl groups. Said monomer M2c is selected from the group consisting of divinyl aryl monomers, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers, and tetra- or tri-(meth)acrylate esters. Examples of divinyl aryl monomers include divinyl benzene. Examples of (meth)acrylate diester monomers include alkylene di(meth)acrylates such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, and 1,4-butylene glycol di(meth)acrylate. Examples of oligo alkylene glycol di(meth)acrylate monomers include tetraethylene glycol di(meth)acrylate, poly(ethylene glycol) di(meth)acrylate, and poly(propylene glycol) di(meth)acrylate. Among the divinyl (meth)acrylamide monomers, methylene bisacrylamide can be cited. Among the divinyl ether monomers, poly(ethylene glycol) divinyl ether can be cited.Among the tetra or tri-(meth)acrylate monomer esters, we can mention pentaerythritol tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate or glucose di- to penta-(meth)acrylate).

[0143] Preferably, said hydrophilic polymer P2 comprises from 0.01% to 30% by moles of repeating units derived from a monomer M2b. In particular, said hydrophilic polymer P2 comprises from 0.05% to 25%, advantageously from 0.1% to 20%, preferably from 0.5% to 15%, in particular from 1% to 15%, more particularly from 3% to 15% by moles of repeating units derived from a monomer M2b.

[0144] Preferably, said hydrophilic polymer P2 comprises from 0.01 to 30% by mole of repeating units derived from a monomer M2c. In particular, said hydrophilic polymer P2 comprises from 0.01% to 25%, advantageously from 0.05% to 20%, preferably from 0.05% to 15%, more preferably from 0.05% to 15%, in particular from 0.05% to 15%, more particularly from 0.05% to 10%, preferably from 0.1% to 5% by mole of repeating units derived from a monomer M2b.

[0145] Process of

[0146]

[0147] corn

[0148]

[0149] The composition can be prepared by various processes. The fluorinated polymer P1 and the hydrophilic polymer P2 can be mixed together in powder or latex form. Alternatively, the composition can be in the form of an interpenetrating polymer network (IPN) or a semi-interpenetrating polymer network (semi-IPN). An interpenetrating polymer network (IPN) is defined as a network in which the polymers are at least partially intertwined at the molecular level but not covalently bonded to each other and can only be separated if chemical bonds are broken. A semi-interpenetrating polymer network (semi-IPN) comprises one or more polymer networks and one or more linear or branched polymers and is characterized by the molecular penetration of at least one of the networks by at least some of the linear or branched macromolecules.A mixture of two or more preformed polymer networks is not an interpenetrating polymer network or a semi-interpenetrating polymer network. In this case, said composition may be prepared by a process comprising the steps of:

[0150] a) Supply of a reactor containing said fluorinated polymer P1,

[0151] b) Addition of at least one M2a monomer, and one M2b monomer or one M2c monomer as defined above;

[0152] c) Implementation of the polymerization of said at least one monomer M2a and one monomer M2b or one monomer M2c to obtain said composition according to the present invention;

[0153] d) Optionally drying and grinding of the product obtained in step c).

[0154] In step a), said fluorinated polymer P1 is preferably in the form of a latex.

[0155] In step b), the fluorinated polymer P1 and said monomers M2a and M2b or M2c are brought into contact for a sufficiently long period to allow said monomers to impregnate the particles of the fluorinated polymer P1 before its polymerization. This contact time may be at least 5 minutes, preferably 10 minutes, and in particular at least 15 minutes. The longer the contact time between the monomers and the fluorinated polymer P1, the more intimate the mixing between the fluorinated polymer P1 and the hydrophilic polymer P2; this can improve the adhesion properties of the composition.

[0156] Step c) is preferably carried out in the presence of water. The polymerization step c) is carried out in the presence of an initiator. Said initiator may be a persulfate type initiator such as sodium persulfate, potassium persulfate, barium persulfate, or ammonium persulfate; alkali metal bisulfites; peroxides such as benzoyl peroxide or dicumyl peroxide; hydroperoxides such as methyl hydroperoxide or tert-butyl hydroperoxide; acyloins such as benzoin; peracetates such as methyl peracetate or tert-butyl peracetate; perbenzoates such as tert-butyl perbenzoate; peroxalates such as dimethyl peroxalate or di(tert-butyl) peroxalate; azo-type compounds such as azo-bisisobutyronitrile or dimethyl azo-bisisobutyrate. The initiator is preferably added at a concentration of 0.005 to 1% by weight based on the weight of said M2a, M2b or M2c.Step c) can be carried out at a temperature of 20°C to 160°C. Step c) can be carried out at a pressure of 280 to 20,000 kPa. Preferably, steps b) and c) are carried out under stirring. The polymerization product obtained in step c) is optionally dried in step d) to obtain a powder. The drying step can be carried out by spray drying or co-spray drying, preferably at a temperature of 50°C to 220°C. If it is desired to obtain the composition in powder form, it can also be obtained by grinding techniques, such as cryo-milling, where the mixture is brought to a temperature below ambient temperature, for example by means of liquid nitrogen, before grinding.At the end of the powder manufacturing stage, i.e. after the drying stage, the particle size can be adjusted and optimized by selection or screening processes and / or by grinding to obtain the desired particle size distribution.

[0157] Use

[0158] The said binding composition can be used in the preparation of an electrode, preferably a positive electrode, i.e., a cathode. Thus, the present invention provides an electrode composition comprising the said binding composition according to the present invention, an active material, and optionally a conductive agent.

[0159] In a preferred embodiment, the electrode composition has the following mass composition:

[0160] a. 50% to 99.95% of active material, preferably 50% to 99%, b. 0% to 25% of conducting agent, preferably 0.5% to 25%, c. 0.05% to 25% of said binder according to the invention, preferably 0.5% to 25%, d. 0% to 5% of at least one additive selected from the group consisting of a plasticizer, an ionic liquid, a dispersing agent for conducting additive, and a flow-aiding auxiliary agent;

[0161] The sum of all these percentages is 100%. The conductive agents in the electrode are composed of one or more materials that can improve conductivity. Some examples include carbon blacks such as acetylene black and Ketjen black; carbon fibers, such as carbon nanotubes, carbon nanofibers, and vapor-growth carbon fibers; and metal powders such as SUS powder and aluminum powder. The active materials in electrode compositions are materials capable of storing and releasing lithium ions.

[0162] The said active material is selected from the group consisting of phospho-olivine materials of formula Li xAyDzPO4, in which A is selected from the group consisting of Mn, Fe, Co, Ni, and Cu; D is selected from the group consisting of Mg, Ca, Sr, and Ba; x, y, and z being numbers satisfying the equation: 0.9 < x < 1.2, 0 < y < 1.5, and 0 < y < 1.5, or mixtures thereof. Preferably, A is Fe, Mn, or Ni, more particularly Fe. Preferably, D is Mg or Ca. Examples of compounds having an olivine structure include lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), and lithium manganese phosphate. The surface of the active material may be partially or totally coated with carbon to improve conductivity. Said active material may be lithium iron phosphate or lithium manganese iron phosphate or a mixture of the two. Phospho-olivine materials have an average D50 size of 0.1 pm to 100 pm measured by laser granulometry.

[0163] The electrode composition can be deposited on at least one face of a current collector to form a positive electrode. This deposition can be carried out in the presence of an organic solvent, water, a mixture of the two, or by a solvent-free process, i.e., by a dry coated electrode production process. The organic solvent can be selected from the group consisting of n-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), triethylphosphite, triethylphosphate, acetone, cyclopentanone, tetrahydrofuran, methyl ethylketone (MEK), methyl isobutyl ketone (MiBK), ethyl acetate (EA), butyl acetate (BA), ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), gamma-butyrolactone, and N-butylpyrrolidone; and mixtures thereof.

[0164] The said process for preparing the dry-coated electrode comprises the following steps: - mixing the active material in powder form, said binder according to the present invention, and optionally the conductive agent in powder form, the additive in powder form, or both, to form said electrode composition according to the present invention.

[0165] - deposition of said electrode composition onto said current collector to manufacture an electrode, and

[0166] - Optionally, consolidation of said electrode by thermomechanical treatment. The dry-coated electrode is thus prepared using a "solvent-free" process, meaning that it does not require a residual solvent evaporation step after the deposition stage because all the constituents are mixed in a dry, powdered state, and the deposition is also carried out without solvent. Thermomechanical treatment refers to the application of mechanical pressure to the electrode at a given temperature. Such thermomechanical treatment can be performed, for example, by a calendering machine with heated rollers or a plate press that can also be heated.

[0167] Solvent-free mixing processes of the different constituents of the electrode composition before the deposition phase on the collector include, but are not limited to: stirring, air jet, high shear, V-mixer, screw mass mixer, double cone, drum, conical, double Z-arm, fluidized bed, planetary mixer, fusion, extrusion, calendering, and grinding.

[0168] According to one embodiment, after the powder mixing step, the electrode is manufactured by a solvent-free spraying process, by depositing the electrode composition onto the metallic substrate, by a pneumatic spraying process, by electrostatic spraying, by dipping in a fluidized powder bed, by sprinkling, by electrostatic screen printing, by deposition with rotary brushes, by deposition with rotary adding rollers, by calendering.

[0169] In one embodiment, the electrode consolidation after deposition onto the metallic substrate by solvent-free spraying (pneumatic spraying, electrostatic spraying, fluidized bed immersion, sputtering, electrostatic screen printing, deposition with rotary brushes, or deposition with rotary rollers) is carried out by a calendering process. This process consists of applying pressure to the electrode using two rollers, which may be heated. The consolidation step is optional. Its implementation depends on the technique used to deposit the components onto the electrode. Thus, when the deposition step has been carried out by calendering, this consolidation step is optional because calendering allows for the simultaneous deposition and consolidation of the electrode.

[0170] In one embodiment, after the powder mixing step, the electrode is manufactured by a solvent-free, two-step process. The first step consists of manufacturing a self-supporting film from the premixed formulation using a thermomechanical process such as extrusion, calendering, or thermocompression. In the second step, the self-supporting film is laminated onto the metallic substrate by a process combining temperature and pressure, such as calendering or thermocompression.

[0171] In one embodiment, after the powder mixing step, the electrode is manufactured using a solvent-free process involving calendering. This process allows for the film formation and transfer of the coating onto the current collector in a single step, i.e., without a separate step for manufacturing a self-supporting film. To achieve this, the calender used has several rollers (at least three). The powder obtained after the mixing step is introduced between the first two rollers, which are usually heated and have differential rotation speeds to shear the powder. The coating formed and remaining adhered to the fastest roller is then directly laminated onto the current collector by a third roller. The resulting electrode can then be passed through another calender to adjust its porosity or thickness if necessary.

[0172] According to another aspect of the present invention, a Li-ion battery is provided. Preferably, the Li-ion battery comprises a positive electrode according to the present invention, a negative electrode, and a separator. Preferably, said Li-ion battery also comprises a lithium salt selected from the group consisting of LiCF3SO3, LiPF6, LiClO4, LiBF4, LiB(C2O4)2, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F3)2, LiN(SO2C2F5)2, LiN(SO2F)(SO2CF3), LiN(SO2F)(SO2C2F5), LiN(SO2CF3)(SO2C2F5), LiAsF6, LiBF2C2O4, LiNO3, LiPF3(CF2CF3)3, LiBETI, LiTDI, or a mixture thereof.

[0173] Examples

[0174]

[0175] P1a: PVDF-AA-CEA

[0176] The polymerization was carried out in a 3-liter vertical reactor. The reactor was loaded with 1755 g of water, 25.9 g of a solution containing 23.6 g / L of hydroxypropyl methylcellulose, and 1 g of ethyl acetate. A vacuum was applied to the reactor before the introduction of 1020 g of vinylidene difluoride. The reactor was stirred at 750 rpm, and 1.53 g of n-propyl peroxydicarbonate initiator was added. The reactor temperature was raised to 50 °C, and the internal pressure increased to 90 bar. To maintain the pressure at 90 bar throughout the polymerization, an aqueous solution containing 12 g / L of acrylic acid and 8 g / L of carboxyethyl acrylate was continuously introduced into the reactor. The polymerization reaction was carried out for 7 hours, during which a total of 820 g of solution was injected. Once finished, the polymer was washed and dried, yielding 791 g of P1a polymer.The P1a polymer contains 0.75 mol% acrylic acid and 0.25 mol% carboxyethyl acrylate.

[0177]

[0178] P1b: PVDF-AAco

[0179] The polymerization was carried out in a 3-liter vertical reactor. The reactor was loaded with 1755 g of water, 25.9 g of a solution containing 23.6 g / L of hydroxypropyl methylcellulose, and 1 g of ethyl acetate. A vacuum was applied to the reactor before the introduction of 1020 g of vinylidene difluoride. The reactor was stirred at 750 rpm, and 1.53 g of n-propyl peroxydicarbonate initiator was added. The reactor temperature was set to 50 °C, and the internal pressure to 90 bar. To maintain the pressure at 90 bar throughout the polymerization, an aqueous solution containing 16 g / L of acrylic acid was continuously introduced into the reactor. The polymerization reaction was carried out for 7 hours, during which a total of 790 g of solution was injected. Once completed, the polymer was washed and dried, yielding 750 g of polymer P1 b. Polymer P1 a contains 1.0 mol% acrylic acid.

[0180]

[0181] roohile P2a:

[0182] The hydrophilic polymer is a copolymer containing 90% methyl methacrylate units and 10% methacrylic acid. The molecular weight of the hydrophilic polymer P2a is 64,900 g / mol. -1 .

[0183]

[0184] electrode horn

[0185] In the examples below, the binding compositions are composed of 90% by mass of copolymers or terpolymers of vinylidene fluoride, acrylic acid and optionally carboxyethyl acrylate (PA or PB) and 10% by mass of the hydrophilic polymer.

[0186] Table 1 presents the binding agent compositions used:

[0187] [Table 1]

[0188] Fluorinated polymer Hydrophilic polymer Ratio

[0189] P1 P2 P1 / P2 Binder composition P1a P2a 90 / 10

[0190] 1 (Inv.)

[0191] Binder composition P1b P2a 90 / 10

[0192] 2 (comp.)

[0193] Composition liante P1a - 100 / 0

[0194] 3 (comp.)

[0195] Composition liante P1b - 100 / 0

[0196]

[0197] 4 (comp.)

[0198] The electrode composition was manufactured according to the following steps: a 7% (wt) binder solution was prepared in N-methyl-2-pyrrolidone until completely dissolved. Super P C65 carbon black (supplier Timcal) was then added to this solution. The solution was mixed using a mechanical stirrer. Next, an active material of the LiFePO4 oxide type was added. N-methyl-2-pyrrolidone was then added to adjust the final dry extract. The resulting electrode composition had a final dry extract between 40% and 90%. The dry composition of the electrode composition was 96% (wt) active material, 2% (wt) binder, and 2% (wt) carbon black.

[0199] Table 2 summarizes the prepared electrodes.

[0200] [Table 2]

[0201] Binder composition Active material Ratio

[0202] Example 1 1 LFP 96 / 2 / 2

[0203] Example comp. 2 2 LFP 96 / 2 / 2

[0204] Example comp. 3 3 LFP 96 / 2 / 2

[0205]

[0206] Example comp. 4 4 LFP 96 / 2 / 2

[0207] Ratio = mass ratio of active material / carbon black / binder composition

[0208] Measurement of the viscosity of the electrode composition applied to a metallic substrate. The viscosity of the electrode compositions was measured at 23°C using a TA HR 10 rheometer. The ink was deposited between two parallel plates (40 mm diameter) separated by 500 Tl

[0209] pm (=gap of 500 pm). Viscosity values ​​are obtained at different shear rates ranging from 0.1 s-1 to 100 s-1. The value of 10 s-1 is mentioned in the table below.

[0210] Measurement of the Delta of Electrode Composition Applicable to a Metallic Substrate: The dynamic viscosity of the electrode formulations was measured at 23°C using a TA HR 10 rheometer. The ink was deposited between two parallel plates (40 mm diameter) separated by a 500 µm gap. Dynamic viscosity values ​​were obtained at various stress levels ranging from 0.1% to 100% at an oscillation frequency of 1 Hz. The delta was then calculated using a formula known to those skilled in the art. The delta value at 1% was used for comparison between the different compositions.

[0211] The rheological properties of the different electrode compositions are detailed in Table 3 below.

[0212] [Table 3]

[0213] Electrode composition Ex 1 Example Example Example Comp 2 Comp 3 Comp 4 Binder composition 1 2 3 4

[0214] %mol of functional groups 2.0 2.0 1.0 1.0 acid

[0215] Of which CEA 0.25 0 0.25 0

[0216] Viscosity t=0 (cp) 3050 4593 3752 4124

[0217] Dry extract (%) 58 55 50 51

[0218] Delta t=0 (°) 71 62 41 39

[0219]

[0220] Coating application (visual inspection)* 1 1 0 0

[0221] * When coating was not possible on the manifold, a score of 0 is assigned; when coating was possible on the manifold, a score of 1 is assigned

[0222] It has been observed that the presence of CEA in the binding composition, in combination with acrylic acid, results in an electrode slurry with more advantageous rheological properties. Indeed, the dry extract of the slurry in Example 1 is higher for a lower viscosity, thus requiring less NMP to be used in electrode preparation and subsequently evaporated.

Claims

Demands 1. Binder composition for lithium-ion battery characterized in that it comprises a fluorinated polymer P1 and a hydrophilic polymer P2; said fluorinated polymer P1 comprises repeating units derived from vinylidene fluoride, repeating units derived from a monomer M1a of formula (la) R 1 R 2 C=C(R 3 )(C(O)OY 1 ) and repeating units derived from a monomer M1b of formula (Ib) R 4 R 5 C=C(R 6 )(C(O)-X 1 -Y 2 ) in which R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl; Y 1 is selected from the group consisting of H, C1-C5 alkyl substituted by an OH group; Y 2 is selected from the group consisting of CO2H, SO3H and PO3H2; X 1 is an atomic group having a molecular weight less than or equal to 456 having a main chain composed of 1 to 18 atoms; said hydrophilic polymer P2 comprises repeating units derived from a monomer M2a of formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CTCS alkyl; R d is -OR d 'with R d 'selected from the group consisting of CTCTS alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -OC(O)R d ”, -C(O)OR d "or a nitrogenous heterocycle with 5 or 6 links; R d " being selected from the group consisting of Ci-C6alkyl and C6-Ci2aryl optionally substituted by one or more functional groups -OH, -CO2H OR -SO3H.

2. Binder composition according to the preceding claim characterized in that said hydrophilic polymer P2 also comprises repeating units derived from a monomer M2b or a monomer M2c; said monomer M2b being selected from the group consisting of monomers of formula (II), (III), (IV), (V), (VI), (VII) or (VIII) R 10 R 11 C=C(R 12 )C(O)OH (II) R 13 R 14 C=C(R 15 )(OC(O)R 16 ) (III); R 17 R 18 C=CR 19 C(O)OC(O)CR 20 =CR 21 R 22 (IV); [Chem 1] o (V) R33R34 C =CR 35 (CN) (VII); R 36 R 37 C=CR 38 (C(O)NR 39 R' ') (VIII); in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl; R 13 , R 14 and R 15 are independently selected from the group consisting of H and C1-C5 alkyl; R 16 is C1-C5 alkyl; and R 38 are independently selected from the group consisting of H and C1-C5alkyl; R 39 and R 40 are independently selected from the group consisting of H and Ci-C 10 alkyl optionally substituted by one or more functional groups -OH, -CO2H, -SO3H, -C(O)OR 41 or -OC(O)R 41 R 41 being selected from the group consisting of C^Cs alkyl and C6-C 12 aryl optionally substituted by one or more CO2H functional groups; said monomer M2c comprising at least two vinyl groups and being selected from the group consisting of divinyl aryl, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers and tetra or tri-(meth)acrylate esters monomers.

3. Binder composition according to the preceding claim characterized in that said hydrophilic polymer P2 comprises from 0.01 to 30 mole percent of repeating units from a monomer M2b or a monomer M2c.

4. Binder composition according to any one of the preceding claims characterized in that said hydrophilic polymer P2 comprises at least 50% by moles of repeating units derived from a monomer M2a.

5. Binder composition according to any one of the preceding claims 2 to 4 characterized in that said monomer M2b is selected from the group consisting of monomers of formula (II), (VII) or (VIII) R 10 R 11 C=C(R 12)C(O)OH (II) R 33 R 34 C=CR 35 (CN) (VII); R 36 R 37 C=CR 38 (C(O)NR 39 R 40 ) (VIII); in which R 10 , R 11 and R 12 are independently selected from the group consisting of H, CO2H and C1-C5 alkyl; R 33 , R 34 , R 35 , R 36 , R 37 and R 38 are independently selected from the group consisting of H and C^Cs alkyl; R 39 and R 40 are independently selected from the group consisting of H and C alkyl optionally substituted by one or more functional groups -OH, -CO2H, SO3H, -C(O)OR 41 OR -OC(O)R 41 R 41 being selected from the group consisting of C1-C5 alkyl and C6-Ci2aryl optionally substituted by one or more CO2H functional groups; said monomer M2c comprises at least two vinyl groups and is selected from the group consisting of divinyl aryl, (meth)acrylate diesters, oligo alkylene glycol di(meth)acrylates, divinyl (meth)acrylamides, divinyl ethers and tetra or tri-(meth)acrylate esters monomers.

6. Composition according to the preceding claim characterized in that said monomer M2b is selected from the group consisting of monomers of formula (II) R 10 R 11 C=C(R 12 )C(O)OH (II) in which R 10 , R 11 and R 12 are independently selected from the group consisting of H,CO2H and C1-C3 alkyl; preferably R 10 , R 11 and R 12 are independently selected from the group consisting of H and CH3.

7. Binder composition according to any one of the preceding claims characterized in that the mass ratio P1 / P2 is from 50 / 50 to 99 / 1, preferably from 70 / 30 to 99 / 1.

8. Binder composition according to any one of the preceding claims characterized in that said monomer M1b is selected from the group consisting of 2-carboxyethyl (meth)acrylate, (meth)acryloyloxyethyl succinate, (meth)acryloyloxypropyl succinate and mixtures thereof.

9. Binder composition according to any one of the preceding claims characterized in that said monomer M1a is selected from the group consisting of acrylic acid, methacrylic acid, hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxyethylhexyl(meth)acrylate and mixtures thereof.

10. Binder composition according to any one of the preceding claims characterized in that said polymer P1 comprises at least 60 mole percent of repeating units derived from vinylidene fluoride.

11. Binder composition according to any one of the preceding claims characterized in that said polymer P1 comprises less than 10% by moles of repeating units derived from monomer M1a.

12. Binder composition according to any one of the preceding claims characterized in that said polymer P1 comprises less than 10% by moles of repeating units derived from monomer M1b.

13. Binder composition according to any one of the preceding claims, characterized in that said monomer M2a has the formula (I) R a R b C=C(R c )HORN d (I) in which R a , R b and R c are independently selected from the group consisting of H and CH3; R dis -OR d 'with R d 'selected from the group consisting of CT-CS alkyl optionally substituted by one or more functional groups -OH, -CO2H, -OC(O)R d ”, -C(O)OR d "; R d " being selected from the group consisting of CTCS alkyl and C6aryl optionally substituted by one or more -OH or -CO2H functional groups.

14. Electrode composition comprising said binder composition according to any one of the preceding claims, an active material and optionally a conductive agent, an additive or a mixture of both.

15. Electrode composition according to the preceding claim characterized in that it comprises a conductive agent composed of one or more materials selected from the group consisting of carbon black, graphite, carbon fibers, carbon nanotubes, carbon nanofibers, metal powders such as SUS powder and aluminum powder, or mixtures thereof.

16. Electrode composition according to any one of the preceding claims 7 or 8, wherein said active material is selected from the group consisting of phosphoolivine materials of formula Li x HAS y D z PO4 in which A is selected from the group consisting of Mn, Fe, Co, Ni and Cu; D is selected from the group consisting of Mg, Ca, Sr and Ba; x, y and z being numbers satisfying the equation: 0.9 < x < 1.2, 0 < y < 1.5 and 0 < z < 1.5; or mixtures thereof.

17. Electrode composition according to the preceding claim characterized in that said active material is selected from the group consisting of lithium iron phosphate, lithium manganese iron phosphate and lithium manganese phosphate.

18. Electrode comprising a current collector and a layer consisting of said electrode composition according to any one of the preceding claims 14 to 17.

19. Li-ion battery comprising a positive electrode, a negative electrode and a separator, characterized in that said positive electrode is an electrode according to claim 18.