Battery anode and current collector materials and batteries containing such materials
A copper-nickel alloy current collector with a controlled nickel content and porous graphene interphase layer addresses dendrite issues in lithium-metal batteries, enhancing stability and energy density, and enabling fast charging.
Patent Information
- Application Number
- PCT/EP2026/063960
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional lithium-ion batteries face limitations in energy density, safety issues due to dendrite formation, and slow charging rates, while anode-free lithium-metal batteries suffer from manufacturing challenges and dendrite-induced performance degradation.
Employing a copper-nickel alloy current collector with a specific nickel content range (0.010 to 1.900% by weight) and a porous graphene interphase layer, optionally with a contiguous silver layer, to enhance stability, Coulombic efficiency, and prevent dendrite formation.
The copper-nickel alloy with a controlled nickel content and porous graphene interphase layer improves battery performance by preventing dendrite formation, enabling fast charging and high energy density, with enhanced stability and cyclic performance.
Smart Images

Figure EP2026063960_19112026_PF_FP_ABST
Abstract
Description
[0001] F07537 13.5.2026
[0002] 1
[0003] TITLE BATTERY ANODE AND CURRENT COLLECTOR MATERIALS AND BATTERIES CONTAINING SUCH MATERIALS
[0004] TECHNICAL FIELD
[0005] The present invention relates to the field of materials for elements of batteries, in particular electrode (current collector) materials e.g. for lithium-metal and sodium-metal batteries, including e.g. lithium solid-state batteries and anode-free batteries. It relates in particular to anode materials for batteries as well as uses of such anodes and methods for making such anodes and / or lithium-metal or sodium-metal batteries using such anodes.
[0006] PRIOR ART
[0007] With the advent of portable electronic devices, and even more so with increasing electric mobility there is an increasing need for high-capacity and long-lasting electric energy storage devices.
[0008] At present, the vast majority of high-capacity rechargeable batteries are provided as first-generation lithium-ion batteries having a liquid electrolyte. The problem of these conventional rechargeable batteries is that the graphite carbon anode limits the available energy density. Some liquid electrolyte systems in conventional batteries can also present safety challenges. Furthermore, the conventional Li-ion batteries show slow charging properties due to rate-limiting diffusion properties.
[0009] Some enhancements could be achieved by using a graphite-silicon composite anode to increase energy density, but still there is the problem with the increased volume required due to the addition of silicon and the resulting slow charging due to decreased diffusion rates.
[0010] The solution to this problem is seen in the provision of so-called lithium-metal batteries, where the graphite and / or graphite-silicon composite is replaced by a lithium metal due to its high specific capacity (3860 mAh g-1). Lithium-metal batteries are anticipated to show a higher energy density, faster charging and a longer lifespan. The anode material of such lithium-metal batteries can be provided in the form of an elemental metal, for example in the form of a lithium layer or foil, allowing for a high energy density, fast charging, low costs and long lifespan. The cathode can be provided in the form of transition metal oxide, sulphur or air. The electrolytes can for example take the form of either non-aqueous solutions or solid-state materials showing appropriate ion diffusion properties.
[0011] One problem of using lithium-metal battery technology is the progressive formation of lithium dendrite structures causing rapid degradation of capacity and performance. In theF07537 13.5.2026
[0012] 2
[0013] charging process deposition of elemental lithium on the anode, whether this is an elemental lithium anode or anode made of a different material acting as current collector, typically leads to the formation of dendritic structures which either lead to safety issues because the dendrites can penetrate a separator and even contact the cathode leading to short circuit situations, charging and discharging cycles can lead to disconnection of fractions of the dendritic structures leading to so-called “dead” or “stranded” lithium zones which are not available for future cycles reducing lifespan, and dendrite formation may lead to increasing surface area and / or volume expansion. These problems also appear if so called anode-free battery technology is used, wherein there is no elemental lithium anode, but the anode includes another metal layer as a current collector, for example a copper layer. For these anode-free constructions there is no excess lithium, and together with corresponding lower costs, offer simplified manufacturing processes in particular through adaptation of conventional Li-ion battery production systems.
[0014] Several approaches have been tried to avoid dendrite formation in lithium-metal (and anode-free) systems. Approaches can be grouped into electrolyte engineering, use of a 3D host, separator modification, and artificial solid-electrolyte interphase (SEI) optimisation. Artificial solid-electrolyte interphase systems should have a high mechanical stability to suppress dendritic lithium growth, they should show electrochemical stability and preferably themselves should be non-conducting, and they should have a high and spatially uniform ionic conductivity not only at room temperature but also under typical operating temperatures of the final battery.
[0015] In the past for such artificial solid-electrolyte interphase layers inorganic materials deposited on the anode (e.g., lithium) or the current collector have been proposed in the form of lithium fluoride, lithium phosphate, boron nitride systems or aluminium oxide. Also polymer deposition has been tried, inorganic and organic compound layers, as well as metal nano wire networks. However, the systems tried so far show rather low ionic conductivity under typical operation conditions (temperatures), they show a large interfacial impedance and the layers need to be rather thick.
[0016] US-A-2021057751 provides an electrode having a carbon-based structure with a plurality of localized reaction sites. An open porous scaffold is defined by the carbon-based structure and can confine an active material in the localized reaction sites. A plurality of engineered failure points is formed throughout the carbon-based structure and can expand in a presence of volumetric expansion associated with polysulfide shuttle. The open porous scaffold can inhibit a formation of interconnecting solid networks of the active material between the localized reaction sites. The plurality of engineered failure points can relax or collapse during an initial activation of the electrode. The open porous scaffold can define aF07537 13.5.2026
[0017] 3
[0018] hierarchical porous compliant cellular architecture formed of a plurality of interconnected graphene platelets fused together at substantially orthogonal angles. The hierarchical porous compliant cellular architecture can be expansion-tolerant and can expand in a presence of Li ion insertion or de-insertion.
[0019] US-A-2016301075 discloses a dendrite penetration-resistant layer for a rechargeable alkali metal battery, comprising multiple graphene sheets or platelets or exfoliated graphite flakes that are chemically bonded by a lithium- or sodium-containing species to form an integral layer that prevents dendrite penetration through the integral layer, wherein the lithium-containing species is selected from a specific group of compounds. Also provided is a process for producing a dendrite penetration-resistant layer based on the principle of electrochemical decomposition of an electrolyte in the presence of multiple graphene sheets.
[0020] US-A-2020328404 discloses electrochemical systems and related methods of making and using electrochemical systems. Electrochemical systems of the invention implement novel cell geometries and composite carbon nanomaterials based design strategies useful for achieving enhanced electrical power source performance, particularly high specific energies, useful discharge rate capabilities and good cycle life. Electrochemical systems of the invention are versatile and include secondary lithium ion cells, useful for a range of important applications including use in portable electronic devices.
[0021] CN-A-107871868 provides a graphene-enhanced integrated electrode, which comprises a conductive material linear structural body, an active material linear structural body, and a graphene layer growing in situ on the surface of the conductive material linear structural body and / or active material linear structural body, wherein the conductive material linear structural body and active material linear structural body interpenetrate in a three-dimensional space to form a linear network structure, and the graphene layer connects the two linear structural bodies to form an integrated three-dimensional linear network integral body, which has network gaps. The conductive material linear structural body is made from a current collector having an electron collection function, and the active material linear structural body is made from a material for energy storage via ion de-intercalation. The integrated electrode can efficiently improve the stress interface formed between an electrode active material and the current collector, and is high in energy density and circulation stability. The invention further provides a preparation method of the integrated electrode and a battery comprising the integrated electrode.
[0022] CN-A-103794791 provides a continuous-phase spongy graphene material. The core part of the material is provided with a foamed nickel substrate; the outer surface of the foamed nickel substrate is coated with graphene obtained by a CH4 gas via CVD (chemical vaporF07537 13.5.2026
[0023] 4
[0024] deposition); the graphene material is integrated continuous-phase spongy block graphene. The invention also provides two preparation methods of the continuous-phase spongy graphene material, wherein one preparation method provided by the invention is characterized in that the preparation material is the continuous-phase spongy graphene material two end surfaces of which are not provided with graphene, and can serve as the positive electrode or the negative electrode material of a lithium ion battery, and the advantages of maximum current carrier, favorable cycle stability, good heat conduction, rapid electric conduction, increase of electrolyte contact surface, and volume conservation can be realized; the other preparation method provided by the invention is characterized in that the preparation material is an integral continuous-phase spongy graphene heat radiation material, serves as a heat radiation material of heat radiation devices of a computer CPU, an LED light source, a tablet personal computer, a mobile phone and the like, and has better heat conduction and heat radiation effects compared with a traditional heat radiation material.
[0025] US-A-2017352869 discloses a lithium or sodium metal battery having an anode, a cathode, and a porous separator and / or an electrolyte, wherein the anode contains a graphene-metal hybrid foam composed of multiple pores, pore walls, and a lithium- or sodium-attracting metal residing in the pores; wherein the metal is selected from Au, Ag, Mg, Zn, Ti, Na (or Li), K, Al, Fe, Mn, Co, Ni, Sn, V, Cr, or an alloy thereof and is in an amount of 0.1% to 90% of the total hybrid foam weight or volume, and the pore walls contain single-layer or fewlayergraphene sheets, wherein graphene sheets contain a pristine graphene ornon-pristine graphene selected from graphene oxide, reduced graphene oxide, graphene fluoride, graphene chloride, graphene bromide, graphene iodide, hydrogenated graphene, nitrogenated graphene, doped graphene, chemically functionalized graphene, or a combination thereof.
[0026] Kumar et al. in NanoResearch, 2019, 12(11): 2655-2694 (https: / / doi.org / 10.10Q7 / s12274- 019-2467-1 report that the significance of graphene and its two-dimensional (2D) analogous inorganic layered materials especially as hexagonal boron nitride (h-BN) and molybdenum disulphide (MoS2) for "clean energy" applications became apparent over the last few years due to their extraordinary properties. In this review article the progress and selected challenges in the syntheses of graphene, h-BN and MoS2 including energy storage applications as supercapacitors and batteries is studied. Various substrates / catalysts (metals / insulator / semiconducting) have been used to obtain graphene, h-BN and MoS2 using different kinds of precursors. The most widespread methods for synthesis of graphene, h-BN and MoS2 layers are reported to be chemical vapor deposition (CVD), plasma-enhanced CVD, hydro / solvothermal methods, liquid phase exfoliation, physicalF07537 13.5.2026
[0027] 5
[0028] methods etc. Current research has shown that graphene, h-BN and MoS2 layered materials modified with metal oxide can have an insightful influence on the performance of energy storage devices as supercapacitors and batteries. This review article also contains the discussion on the opportunities and perspectives of these materials (graphene, h-BN and MoS2) in the energy storage fields.
[0029] US-A-2019168485 discloses a method for making a porous graphene layer of a thickness of less than 100 nm with pores having an average size in the range of 5-900 nm, includes the following steps: providing a catalytically active substrate catalyzing graphene formation under chemical vapor deposition conditions, the catalytically active substrate in or on its surface being provided with a plurality of catalytically inactive domains having a size essentially corresponding to the size of the pores in the resultant porous graphene layer; chemical vapor deposition using a carbon source in the gas phase and formation of the porous graphene layer on the surface of the catalytically active substrate. The pores in the graphene layer are in situ formed due to the presence of the catalytically inactive domains. CN-A-107293754 belongs to the technical field of lithium metal batteries, and particularly relates to preparing an anode porous copper current collector used for a lithium metal battery. The method at least comprises a first step of cleaning the surface of a Cu-X alloy sheet with a solvent to remove impurities on the surface of the Cu-X alloy sheet; a second step of preparing an acid solution; and a third step of preparing the porous copper current collector by scanning different numbers of turns from -1 V to different cut-off voltages by adopting linear scanning cyclic voltammetry in an electrochemical workstation, with a three-electrode system being utilized, platinum or nickel being adopted as a counter electrode, a saturated calomel electrode being adopted as a reference electrode, the Cu-X alloy sheet being adopted as a working electrode, and the acid solution prepared in the second step being adopted as an electrolyte. Compared with the prior art, the porous copper current collector having different pore diameters are etched through an electrochemical process by utilizing the Cu-X alloy sheet as a substrate and adopting acids having different concentrations as media. The current collector is used as a lithium metal battery anode current collector, and has functions of providing deposition space for lithium metal and limiting growth of lithium dendrites.
[0030] WO-A-2018098249 describes primary electrochemical cells having a stable operating voltage of 0.3 V to 2.0 V that include a Li anode coupled to a cathode that is formed of one or more Group 4A, 3A, or 5A elements provided alone or as an alloy with a second, third or other Group 4A, 3A, or 5A element or one or more transition metals. The cells further include a non-aqueous electrolyte optionally with low volatility such as having a vapor pressure of 5 mm Hg or lower at STP, and optionally a lithium-ion conductive and electrically insulatingF07537 13.5.2026
[0031] 6
[0032] separator inserted between the anode and the cathode. The cells provide stable operating voltage that in some aspects can serve to power ultra-low power devices for 10 or more years without the need for expensive or inefficient circuitry to alter the cell voltage.
[0033] US-A-2020381705 describes a method for preparing a lithium alloy as an anode material which includes the following steps: heating lithium metal into a molten state in an environment with a dew point not higher than -50°C. and an oxygen content not higher than 10 ppm; adding a transition metal to the molten lithium metal, maintaining the temperature for 5-15 minutes, and uniformly mixing to form a molten alloy; cooling the molten alloy to room temperature to obtain the lithium alloy as the anode material. The preparation method of the present invention is simple and feasible with less cost. The prepared lithium alloy as the anode material can effectively improve the coulombic efficiency and cycle lifespan of the lithium battery.
[0034] US-A-2021296641 describes a supporter of lithium metal, a material of the supporter of lithium metal is at least one of copper, an alloy of the copper, nickel, or an alloy of the nickel, and a surface of the supporter of lithium metal comprises a lithiophilic layer.
[0035] US-A-2013011734 describes a copper foil for a negative electrode current collector of secondary battery, wherein: roughening treatment is performed to both front and rear surfaces of a rolled copper alloy foil; an average surface roughness Ra of both the front and rear surfaces based on laser microscope measurement is 0.04 to 0.20 pm; and the ratio of surface area factor is within a range of 1.0<(C) / (C')<1.1, when a three-dimensional surface area upon measuring the roughened surfaces with a laser microscope is (A), a two-dimensional area as a projected area upon measuring the three-dimensional surface area is (B), and a calculated value of (A) / (B) is expressed in (C), and when a three-dimensional surface area upon measuring the surfaces of a non-roughened rolled copper or copper alloy foil with a laser microscope is (A'), a two-dimensional area as a projected area upon measuring the three-dimensional surface area is (B'), and a calculated value of (A') / (B') is expressed in (C'). This invention aims to provide a copper foil for a negative electrode current collector of a secondary battery in which the adhesiveness of the secondary battery active material is superior, and which can reduce the variation in the area weight of the secondary battery active material, and has superior weather resistance and thermal resistance.
[0036] WO-A-2022184807 discloses a Li or Na based battery having an anode (or current collector) at least partially covered on its side facing the electrolyte by at least one artificial solid-electrolyte interphase layer with at least one layer of porous graphene of a thickness of less than 25 nm with pores having an average characteristic width as defined in the specification in the range of 1 - 1000 nm.F07537 13.5.2026
[0037] 7
[0038] CN-A-118668261 provides an alloy foil and a preparation method thereof, a current collector, an electrode, a secondary battery and an electric device, the alloy foil comprises a copper element and a nickel element, the mass ratio of the nickel element in the alloy foil is 0.1-15%, and the thickness of the alloy foil is 0.7-6 pm. The alloy foil provided by the invention has relatively good structural integrity and uniformity, and is beneficial to improving the structural stability of the current collector, so that the cycling stability of the secondary battery can be improved.
[0039] CN-A-111321437 relates to a copper-nickel alloy foil and a preparation method thereof. A copper-nickel composite electrolyte system is adopted, and a specific complexing agent combination and an additive are selected according to electrodeposition characteristics of copper-nickel ions to form the copper-nickel alloy foil with the thickness of 3-10 pm, wherein the mass fraction of nickel is 5.0-15.0%. Through testing, nickel crystal grains are uniformly doped in copper crystal grains, the maximum value of the surface roughness Rz of a rough surface is 2 pm, the tensile strength is high and reaches 500 MPa or above, the elongation percentage is moderate, the wettability is suitable for a lithium battery current collector, the thickness is uniform, and edge tearing and belt breaking are avoided. The defects that a traditional pure copper double-sided plain foil is low in tensile strength, and edge tearing and belt breaking are extremely prone to occurring under the condition of thin thickness are overcome, and meanwhile, the problems that in a preparation process of the copper-nickel alloy foil, copper-nickel deposition is uneven, components of metal elements are difficult to control, the performance stability is poor, and the like are solved.
[0040] Yu et al in "Ag-Cu alloy induces uniform lithium nucleation and growth in anode-free lithium metal batteries" (Electrochimica Acta, Volume 535, 20 September 2025, 146623) disclose anode-free lithium metal batteries (AFLMBs), characterized by ultrahigh theoretical capacity, superior energy density, and cost-effectiveness, have emerged as a promising candidate for next-generation high-energy-density battery systems. However, the lithiophobic nature of copper foil and the high reactivity of metallic lithium lead to interfacial side reactions during lithium deposition / stripping on copper substrates, triggering lithium dendrite growth and irreversible “dead lithium” formation. These issues accelerate lithium inventory depletion and severely degrade cycling longevity. The poor electrochemical reversibility originates from heterogeneous lithium nucleation / growth on the current collector, resulting in massive accumulation of “dead lithium” and aggravated parasitic reactions, ultimately causing battery failure. To address these challenges, this study introduces a vacuum thermal evaporation strategy to deposit a nanoscale silver layer on copper foil, enhancing the lithiophilicity of the current collector surface and reducing nucleation overpotential. Subsequent high-temperature heat treatment facilitates theF07537 13.5.2026
[0041] 8
[0042] formation of Ag-Cu alloys, tailoring the structural configuration of Ag and Cu to guide spatially homogeneous lithium-ion deposition and optimize lithium plating morphology. The resultant uniform lithium deposition mitigates volume expansion-induced solid electrolyte interphase (SEI) fracture, fostering a stable lithium anode interface. When integrated into LiFePC>4 full cells, the modified Ag-Cu alloy current collector achieves stable cycling over 100 cycles, significantly outperforming bare copper counterparts. Furthermore, exceptional rate capability is demonstrated: upon reverting to 0.1 C after high-rate cycling (5 C), the discharge capacity recovers to 152.61 mAh g-1, approaching the initial capacity of 158.3 mAh g-1.
[0043] SUMMARY OF THE INVENTION
[0044] It is an object of the present invention to provide an improved battery in particular in terms of the material used for the anode (negative current collector, but also generally for a current collector).
[0045] The improvement is in at least one of the following properties: stability, Coulombic efficiency (CE), voltage profile, discharge capacity, cyclic performance and stability, electrical resistivity, manufacturing properties.
[0046] In particular, it was found that if a copper nickel alloy current collector (in particular anode) material is used, at least one of these properties can be improved.
[0047] A specific window of nickel content in such a copper nickel alloy turned out to be optimum. In particular, since an accepted threshold value for electric resistivity to deviate from the electric resistivity of elemental pure copper is to be below a factor of five in these constructions, the upper limit value for the nickel content in a copper nickel alloy is given by 1.9% by weight.
[0048] The lower limit value for the Nickel content is given by the possibility to produce a corresponding foil of such an alloy using the below described annealing process. Going lower than 0.01 percent by weight nickel content requires the generation of a very thin layer on top of the elemental copper, which cannot be achieved as a homogenous layer. So if a thinner layer than leads to 0.01% by weight nickel content is applied, no homogenous alloy can be produced with the method.
[0049] In particular in terms of Coulombic efficiency, it was further found that within this broad range an optimum nickel percentage is in the range of 0.1-1%, with an optimum in the range of 0.2-0.5% or 0.2 - 0.4 % by weight nickel, in each case complemented to 100% of the total weight of the anode by copper.
[0050] Since the starting materials, so copper and nickel, may, as is well known, contain minor amounts of impurities, this wording shall not exclude if next to the mentioned copper andF07537 13.5.2026
[0051] 9
[0052] nickel additional constituents are present in the current collector material in minor amounts. Minor amounts means that the material of the current collector contains less than 2%, preferably less than 1%, most preferably less than 0.5% or less than 0.2 or 0.1% or 0.01% (in each time by weight relative to the total weight of the material of the current collector) of constituents different from copper and / or nickel, in particular other metals.
[0053] The above-mentioned and below-mentioned percentage proportions given for pure Cu and pure Ni in case of the presence of such impurities are then the proportions of pure Cu and pure Ni present next to these impurities. So, if for example the material of the current collector contains 1% impurities in the form of metals different from copper and nickel, the below-mentioned lower limit value of 0.010% by weight for the nickel content scales to become 0.0099% by weight.
[0054] According to a first aspect of the present invention, it relates to a Li or Na based battery (alkali-metal battery) having an current collector, in particular an anode, which consists of a copper-nickel alloy with a copper content in the range of 98.100 to 99.990 % by weight and a nickel content in the range 0.010 to 1.900% by weight, the copper and nickel contents complementing to 100% by weight of the current collector (anode).
[0055] If in the following the more specific anode is mentioned, this also more generally includes a current collector.
[0056] Preferably, the anode is made from a copper-nickel alloy with a copper content in the range of 98.200 to 99.925 % by weight, preferably 99.000 to 99.900 % or 99.250 - 99.850 % by weight and a nickel content in the range 0.075 to 1.800% by weight, preferably 0.100 to 1.000% or 0.150 - 0.750 % by weight, in each case the copper and nickel contents complementing to 100% by weight of the anode.
[0057] The anode can at least partially be covered on its side facing the electrolyte by at least one artificial solid-electrolyte interphase layer with at least one layer of porous graphene of a thickness of less than 25 nm with pores having an average characteristic width in the range of 1 - 1000 nm.
[0058] The porous graphene layer according to this aspect of the present invention is to be understood as a contiguous layer having passage openings in the form of the mentioned pores. It is not to be equated with a graphene layer comprising or consisting of a number of platelets, flakes and / or grains of graphene forming a coherent structure and between which there are interstitial spaces, since in this case the graphene layer is not a contiguous layer but actually an assembly of individual graphene elements.
[0059] Also the porous graphene layer according to this aspect the present invention is not to be equated with a sponge or spongy structure, as the latter is not only porous but actually comprises a three-dimensional skeleton and correspondingly is also absorbent in the senseF07537 13.5.2026
[0060] 10
[0061] that it actually takes up and absorbs material in internal cavities of the porosity formed by the skeleton. The porous graphene layer according to the present invention is essentially a two-dimensional planar structure with pores within the planar layer which is not absorbing and is not a three-dimensional skeleton. Furthermore, the topology of the planar layer of the present invention is such that it may be separated from the supporting substrate as a single contiguous layer in contrast to a graphene layer supported on a spongy structure where the graphene layer cannot be separated from the substrate as a single contiguous layer due to topological interpenetration of the sponge network within the graphene structure.
[0062] The through openings forming the pores can have variable shape; normally they take the form of oval, round, but also of elongate shapes which can be linear or branched.
[0063] Using such an interphase layer fast charging is possible and a high energy density can be achieved. Typically, it is sufficient to have one such porous graphene layer in that artificial solid-electrolyte interphase layer, which can be supplemented by an additional non-porous graphene layer as will be detailed further below.
[0064] According to a preferred embodiment of such an artificial solid-electrolyte interphase layer, preferably a porous graphene layer, has a thickness in the range of 1-15 nm, preferably in the range of 5-10 nm.
[0065] The porous graphene layer preferably has an areal porosity in the range of at least 10%, preferably at least 15%, more preferably of at least 20% or at least 25% or at least 30% or at least 40%.
[0066] Further preferably, said porous graphene has pores having an average characteristic width in the range of 5 - 900 nm.
[0067] The average characteristic width of the pores is defined and measured as follows:
[0068] As the shape of the pores are generally elongated and uneven it is challenging to obtain the pore diameter. The characteristic width was, therefore, chosen and defined as the widest width of pore rather than the diameter of the pore. The characteristic width of the pores was extracted by using image analysis software (Imaged) on scanning electron microscope (SEM) images. Porous graphene was transferred onto SiNx chip including hole with 4 pm in diameter to make a free-standing section suitable for clear image interpretation. Five representative SEM images of porous graphene were then, taken over 1.14 urn2to visualize the clear difference in the contrast between pore and surrounding graphene (e.g., black for pore and grey for graphene). As the characteristic width of pore is few tens of nm, high magnification SEM images were required. Afterward, based on the SEM image, the widest width of each pore opening was measured and the average of the measured widths subsequently calculated.
[0069] Preferably the graphene has an areal porosity (defined as the ratio of total area of pores toF07537 13.5.2026
[0070] 11
[0071] total projected area of the layer) of more than 2.5%, preferably of more than 5%, preferably in the range of 10-70%, and at the same time a thickness in the range of more than 1 nm, preferably of more than 2 nm, preferably in the range of 2-15 nm. The areal porosity is, generally in this document, calculated in detail as following; first, five representative SEM images of transferred highly porous graphene on the substrate were collected and a pore region was extracted using Imaged program, typically said measurement pore region having an area of 4.6 pm2.
[0072] The artificial solid-electrolyte interphase layer preferably comprises or consists of said at least one porous graphene layer and at least one additional selective graphene layer ("selective graphene layer" in this context meaning a porous graphene layer as defined above, i.e. at least one layer of porous graphene of a thickness of less than 25 nm preferably with pores having an average characteristic width as defined in the specification in the range of 1 - 1000 nm), wherein preferably said at least one porous graphene layer is facing said anode or current collector and the at least one additional selective graphene layer is facing said liquid state or solid-state electrolyte. Such a selective graphene layer ensures no direct contact between metallic lithium deposits and electrolyte which can prevent a formation of natural solid-electrolyte interphase, reducing a consumption of a Li or Na salt in electrolyte. According to a preferred embodiment, such a selective graphene layer is provided in the form of a defective graphene layer, where the defects can be point defects or line defects. The defects are preferably provided in the form of atomic or grain boundary defects.
[0073] Preferably this selective graphene layer is a non-porous layer.
[0074] According to a preferred embodiment, said selective graphene layer has a thickness in the range of 0.34-5 nm, most preferably in the range of 0.34-1 nm.
[0075] Preferably the anode is a foil with a thickness in the range of 0.001 - 0.1 mm or 0.005-0.10mm, preferably in the range of 0.01-0.04 mm.
[0076] The at least one layer of porous graphene can be a layer grown directly on the metal layer forming the anode (or current collector), providing for a particularly simple manufacturing process and a particularly stable structure.
[0077] According to another aspect of the present invention, it relates to an anode (or current collector) in particular for such a Li or Na based battery (alkali-metal battery), wherein the anode which is made from a copper-nickel alloy with a copper content in the range of 98.100 to 99.990 % by weight and a nickel content in the range 0.010 to 1.900% by weight, the copper and nickel contents complementing to 100% by weight of the anode. Preferably the anode takes the form of a foil with the above-mentioned specifications.
[0078] The current collector, in particular the anode, is preferably at least partially, preferably fully, covered on its side facing the electrolyte by at least one contiguous Ag layer, preferablyF07537 13.5.2026
[0079] 12
[0080] having a thickness in the range of of 1-110 nm, or in the range 10 - 80 nm or 30 - 60 nm, preferably in the range of 20-50 nm. Preferably this contiguous Ag layer is annealed such that it has grain features (grains in the sense of crystalline domains, typically showing as domains with angular contours), wherein these grain features have characteristic lengths (average grain size, equivalent diameter according to SEM imaging) of at least 100 nm or at least 150 nm.
[0081] This provides a further improvement over CuNi alloy current collectors through provision of a thin contiguous Ag film surface layer on a CuNi alloy. There is improved performance of anode-free lithium-metal batteries through improved capacity retention over longer cycles and improved stability of battery cycling. Such a contiguous film of Ag proves beneficial for presenting a uniform interface to the battery chemistry, the thin layer of Ag improves lithium interaction (lithiophilicity) of current collector. Excessively thick Ag layers that would add to costs and would excessively sequester Li during battery operation should be avoided. Annealing temperature and time controls or rather limits extent of silver migration into CuNi alloy and final thickness of Ag layer.
[0082] It was surprisingly found that the formation of a contiguous annealed silver layer on top of the substrate is only possible under particular processing conditions as given further below and if the substrate is not a pure copper substrate, but a Cu-Ni substrate as defined above, preferably a Cu-Ni substrate which already has been annealed at a temperature in the range of 600-900°C before the Ag deposition. If the substrate is a pure copper substrate and annealing is carried out at a temperature below 400°C, a contiguous film is formed but it is insufficiently annealed leading to insufficient battery properties. If annealing is carried out at a temperature of about 400°C on a pure copper substrate, there is no formation of a contiguous annealed silver layer anymore, the silver layer becomes porous and granular, at even higher annealing temperatures there is no true Ag layer anymore but rather islands or dots of silver, and battery properties deteriorate as well.
[0083] Surprisingly the formation of a contiguous silver layer is possible on copper-nickel substrates of the above composition with appropriate annealing leading to surprisingly improved battery properties as detailed further below. Surprisingly, there is, if at all, on a Cu-Ni substrate only very limited reduction in Ag thickness in this annealing process with a tendency towards even slightly increased thickness after the annealing. This, without being bound to any explanation, is thought to be due to consolidation of crystallization in the silver layer on the Cu-Ni substrate - which is consistent with the observation of increased size of grain features in the contiguous silver layer as discussed above in SEM image after heat treatment (see also Fig 11 below). So preferably the silver layer on Cu-Ni substrate is such a contiguous layer with grain features, wherein these grain features have characteristicF07537 13.5.2026
[0084] 13
[0085] lengths (average grain size, equivalent diameter according to SEM imaging) of at least 100 nm or at least 150 nm, and which the size of grain features on the Cu-Ni substrate increase during the annealing. This crystallization consolidation effect while maintaining the contiguous layer after heat treatment contributes to further improve the lithiophilicity (e.g. lithium wetting phenomena) of the contiguous silver layer.
[0086] Yu et al teach that Ag on pure copper will have tendency to form clusters and then migrate into Cu with thermal treatment. In contrast, under the conditions described here, so on a Cu-Ni substrate, the system unexpectedly shows little (if any) migration of silver into the CuNi alloy substrate - this presents an advantageous opportunity to thermally anneal and consolidate the silver layer to form larger crystalline grain features and with confidence of maintaining a contiguous film layer and the thermal treatment consolidates the layer to have improved surface properties (e.g. lithiophilicity) compared to the non-annealed silver layer. According to yet another aspect of the present invention, it relates to a method for making such an anode (or current collector) or for making an anode (or current collector) for such a battery, wherein a nickel film is applied to a pure copper foil followed by annealing to generate the anode in the form of a copper-nickel alloy.
[0087] Said nickel film is preferably applied by using electrochemical plating, e-beam evaporation, physical vapor deposition (PVD), electroplating or (magnetron) sputtering, to form a nickel film of a thickness in the range of 1 nm to 2200 nm, preferably in the range of 10-1000 or 15-500 nm, preferably in the range of 20-300 nm on a pure copper foil.
[0088] Said nickel film is preferably applied to a pure copper foil having a thickness in the range of 0.005-0.10mm, preferably in the range of 0.01-0.06 mm, preferably having a purity of more than 99.5% or more than 99.8%.
[0089] Said annealing is preferably carried out at a temperature in the range of 500-1000°C, preferably in the range of 500 - 950°C or in the range of 500 - 900°C or 800-900°C, in particular during a time span of 10 minutes-300 minutes. Ramping up the temperature to the final value preferably takes place within a time span in the range of 10 minutes-200 minutes followed by annealing at the targe temperature for a time span of 10 minutes-100 minutes. Experimental evidence shows that heat treatment of the copper nickel foil having the above-mentioned proportions in a temperature window of 600-900°C or even as low as 600-700°C for a time span in the range of 10-200 minutes, preferably in the range of 10-30 minutes, unexpectedly leads to an improved battery performance, in particular over large number of cycles. This thermal step promotes interdiffusion of Cu and Ni, uniformly converting the Cu / Ni template into the Cu-Ni alloy while e.g. additionally promoting the surface smoothness.
[0090] Said annealing can be carried out during a time span in the range of 10 minutes-300 minutesF07537 13.5.2026
[0091] 14
[0092] or 120 - 240 minutes.
[0093] Preferably said annealing is carried out under hydrogen and / or argon atmosphere and / or under a pressure in the range of 10-10,000 Pa or 100-5,000 Pa.
[0094] Preferably at least one side of said copper-nickel alloy is covered, preferably by vapour deposition, preferably after the annealing of the Cu-Ni substrate, by at least one contiguous Ag layer, preferably having a thickness in the range of 1 -100 nm or in the range 10 - 70 nm or 25 - 50 nm, preferably in the range of 20-40 nm, followed by annealing carried out at a temperature in the range of 250 - 600°C, in the range of 275 - 550°C or in the range of 300 - 500°C during a time span of 10 minutes-80 minutes or in the range of 15-30 minutes. So formation of such a Ag layer is possible by:
[0095] • Start with CuNi alloy current collector as substrate
[0096] • Anneal the CuNi alloy current collector substrate
[0097] • Deposition of Ag layer to controlled thickness (between 1 nm to 100 nm) e.g using physical vapor deposition (deposition may be to one or both surfaces of the current collector substrate)
[0098] • Heat treatment (annealing) of substrate with deposited Ag layer. Temperature and time are managed so that treatment retains a contiguous Ag film with grain features as defined above on the surface of the substrate, and the structure does NOT progress to a ternary alloy where the silver layer fully migrates into the bulk of the substrate but rather a contiguous film layer of Ag grain features are formed. Normally during this annealing the layer thickness of the silver layer, if at all, only very little reduces in thickness, typically less than 10% or less than 5% thickness reduction compared with 100% before annealing are observed, in some cases thickness increases are observed due to the formation of the grain features.
[0099] Last but not least, the present invention relates to the use of such an anode for making such a battery.
[0100] Materials for such a battery or electrochemical cell can be chosen as follows:
[0101] Cathode materials may be selected, but are not limited to one or a combination of
[0102] ■ lithium-iron-phosphate (LFP) (e.g. 2.4 mAh / cm2);
[0103] ■ nickel-cobalt-manganese (NCM 811) (> 4 mAh / cm2);
[0104] Liquid electrolyte materials may be selected, but are not limited to one or a combination of ■ solution (e.g. a 1 mol L-1) of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) dissolved in a mixture (e.g. a 1:1 (v / v)) of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) and if needed containing 0.5 mol lithium nitrate (LiNO3) as a stabilizing additive;
[0105] ■ a localized high-concentration electrolyte comprising or consisting of (1 mol L-1) LiFSI dissolved in a mixed solvent of DME and 1,1,2,2-tetrafluoroethyl-2,2,3,3-F07537 13.5.2026
[0106] 15
[0107] tetrafluoropropyl ether (TTE), the latter serving as a non-solvating diluent.
[0108] Separator materials may be selected, but are not limited to one or a combination of
[0109] ■ graphene interposed between the cathode and anode (or current collector)
[0110] ■ microporous polypropylene separator (e.g. Celgard 2400), interposed between the cathode and anode (or current collector).
[0111] The battery configuration may take the form of coin, pouch, rolled and other forms commonly deployed in battery state-of-the-art.
[0112] Further embodiments of the invention are laid down in the dependent claims.
[0113] BRIEF DESCRIPTION OF THE DRAWINGS
[0114] Preferred embodiments of the invention are described in the following with reference to the drawings, which are for the purpose of illustrating the present preferred embodiments of the invention and not for the purpose of limiting the same. In the drawings,
[0115] Fig. 1 shows a schematic representation of a battery according to the invention Fig. 2 shows a schematic representation of the procedure to prepare an anode based on Cu-Ni alloy;
[0116] Fig. 3 shows schematic representations of rechargeable lithium metal batteries, wherein in a) a schematic representation of a rechargeable anode-free lithium metal battery according to one embodiment of the present invention is given and in b) a schematic representation of a rechargeable lithium metal battery; Fig. 4 shows a plot of Coulombic efficiency of anode-free half-cell as a function of Ni concentration in the current collector;
[0117] Fig. 5 shows voltage-capacity profiles of LilICu anode-free half cells using bare Cu and Cu-Ni alloys with a varied Ni concentration after 100 cycles;
[0118] Fig. 6 shows in a) a charge / discharge graph of an anode-free lithium metal battery including a bare Cu current collector and in b) a charge / discharge graph of an anode-free lithium metal battery according to one embodiment of the present invention;
[0119] Fig. 7 in a) shows a graph of the average voltage versus cycle number of an anode- free lithium metal battery including bare Cu current collector and in b) shows a graph of the average voltage versus cycle number of an anode-free lithium metal battery according to one embodiment of the present invention; Fig. 8 in a) shows a graph of the relative discharge capacity versus cycle number of an anode-free lithium metal battery including bare Cu current collector and according to one embodiment of the present invention and in b) shows a graph of the Coulombic efficiency versus cycle number of an anode-free lithium metalF07537 13.5.2026
[0120] 16
[0121] battery including bare Cu current collector and according to one embodiment of the present invention;
[0122] Fig. 9 shows a graph of the discharge capacity, charged C / 5 and discharged C / 5, versus cycle number of 520 mAh of an anode-free lithium metal battery (multilayer pouch cell) according to one embodiment of the present invention;
[0123] Fig. 10 shows, for heat treated Ag on Cu-Ni alloy, capacity in the lower line of black circles and black squares (left axis) and coulombic efficiency in the upper line of grey half circles (right axis) as a function of cycle number;
[0124] Fig. 11 shows Scanning Electron Microscope (SEM) images illustrating the difference between Ag film on CuNi alloy before (a) and after mild annealing heat treatment (b);
[0125] Fig. 12 shows the summary of data for the LFP (Lithium Iron Phosphate) cathode &
[0126] LiTFSI electrolyte;
[0127] Fig. 13 shows the summary of data for the NCM (lithium nickel cobalt manganese oxide) cathode & LiFSI electrolyte.
[0128] DESCRIPTION OF PREFERRED EMBODIMENTS
[0129] Fig. 1 shows a schematic representation of an anode-free battery 1 according to the invention. The cathode 2, which for example can be, but not limited to, a lithium sulphide (Li2S)y, an air, a lithium iron phosphate (LiFePO4), a lithium nickel cobalt aluminum oxide (LiNiCoAIO2), a lithium nickel manganese cobalt oxide (LiNixMnyCozO2), is followed by the electrolyte 3.
[0130] This electrolyte 3 may be a liquid electrolyte comprising or consisting of lithium salt such as, but not limited to, a lithium hexafluorophosphate (LiPFe) or a lithium tetrafluoroborate (LiBF4), in an organic solvent, such as, but not limited to, ethylene carbonate, dimethyl carbonate, or diethyl carbonate, or it may be a solid electrolyte, which for example can be a polymer, a oxide-based, or sulphide-based solid electrolyte material.
[0131] On the bottom there is provided the actual anode or current collector 5 in the form of a metal layer, in this case a CuNi alloy layer according to the invention. Between the current collector 5 and the electrolyte layer 3 having either liquid electrolyte (inclusive separator membrane), or solid-state electrolyte, there can be provided an artificial solid-electrolyte interphase layer 4 in the form of a graphene layer having the desired properties, in particular the porosity as discussed above. So, in this graphene layer 4 there can be provided pores 9.
[0132] The invention provides a catalyst structure that includes a copper (Cu) foil substrate having a purity of at least 99.9 %.F07537 13.5.2026
[0133] 17
[0134] Preparation of Cu-Ni alloy anode material:
[0135] Fig. 2 schematically illustrates the preparation method.
[0136] A thin film of nickel (Ni) is deposited directly onto the pure Cu substrate foil in a thickness of about 1 nm to about 1000 nm, and more preferably from about 20 nm to 300 nm. The Ni layer is formed by magnetron sputtering, for example in an FHR Pentaco 100 system using a Ni target of at least 99.95% purity, at a working pressure of approximately 0.003 mbar with an argon (Ar) flow rate of 200 seem while sustaining a direct-current plasma of about 0.25 kW, thereby achieving the desired film thickness.
[0137] Alternatively, the Ni layer may be deposited by electron-beam evaporation under conditions selected to deliver the same thickness range.
[0138] Following deposition, the Cu / Ni template is subjected to an annealing treatment intended to alloy the metals into a binary Cu-Ni current collector. The as-deposited structure is heated within a chemical vapor deposition (CVD, Graphene Square. Inc, TCVD-RF100CA) chamber operated at a pressure of about 8 Torr while a process gas stream consisting of 50 seem of hydrogen (H2) and 800 seem of Ar are introduced. The temperature is raised to between 600 and 900°C or in other experiments to between 800 and 900 °C by a ramp lasting roughly 2-3 hours and held for about 15 minutes. This thermal step promotes interdiffusion of Cu and Ni, uniformly converting the Cu / Ni template into the Cu-Ni alloy while additionally promoting the surface smoothness.
[0139] The resulting current collector exhibits a continuous alloy layer whose composition is governed by the controlled Ni content and annealing process.
[0140] Fig. 3 in a) shows an anode free lithium metal battery: the cathode 2 is top covered by an aluminium foil 7, followed downwards by a polymer separator 6 and on the bottom there is provided a copper nickel anode (or current collector) 5. b) illustrates a lithium metal battery, in this case between the polymer separator 6 and the copper nickel alloy anode (or current collector) 5 there is provided an elemental lithium metal layer 10.
[0141] Example 1 - Half-cell assembly:
[0142] LillCu-Ni alloy asymmetric half-cells (coin cell, diameter 12 mm) were assembled, consisting of lithium metal as a reference and counter electrode and Cu-Ni alloys as a working electrode.
[0143] The electrolyte can vary depending on the battery systems, but for the experiments discussed herein, 1 mol LiFSI in DME diluted with TTE was used.
[0144] A separator (Celgard 2325, 25-pm thick, polypropylene / polyethylene / polypropylene) thatF07537 13.5.2026
[0145] 18
[0146] was soaked with the liquid electrolyte was employed between the working electrode and the counter electrode.
[0147] As a reference test, LillCu asymmetric cells were prepared with bare Cu foil as a working electrode, instead of Cu-Ni alloy, and the rest of the conditions were identical. Li plating / stripping experiments were carried out on test cells constructed with either Cu or Cu-Ni alloys with varied Ni concentrations. Li was plated on the corresponding working electrode at a rate of 0.5 mAh / cm2.
[0148] Fig. 4 shows a plot of the Coulombic efficiency (CE) of half cells with bare Cu and Cu-Ni alloy current collectors as a function of Ni concentration in Cu. The bare Cu-based half-cell (0% Ni concentration) shows a very low CE (ca.72%) over 20 cycles. However, the Cu-Ni alloy-based half-cells exhibit stable and high CE (above 95%). In particular, 40 nm Ni (corresponding to 0.33% of Ni concentration) achieves the highest CE (96.0% at 15 cycles and 96.4% on average over 100 cycles).
[0149] Fig. 5 shows the corresponding voltage profiles of half-cells implementing bare Cu and Cu-Ni alloys cycled at the current density of 0.5 mA cm-2with the plating / stripping capacity of 0.5 mA cm-2 for 1st, 2nd, 10th, and 100th cycles. As shown, the cells implementing Cu-Ni alloys accomplish stable cycling for 100 cycles along with a tendency to increase a capacity which is considerably superior to that using the bare Cu with no Ni demonstrating bigger voltage polarization and decreased capacity.
[0150] Example 2 - Cell assembly:
[0151] The invention also provides an anode-free lithium-metal coin cell in which the negative electrode is a disk of a Cu-Ni alloy, the positive electrode is a lithium iron phosphate (LFP) layer coated on aluminium foil, and a microporous polypropylene separator is interposed between the two electrodes (see also Fig. 3). Disks of the Cu-Ni alloy having a diameter of approximately 13 mm were punched from foil stock, dried under vacuum at about 120 °C for not less than 12 hours, and transferred into an argon-filled glovebox maintained at oxygen and moisture levels below 0.1 ppm. Each Cu-Ni disk was then placed in the base of a stainless-steel 2032 coin-cell housing to serve as the anode (current collector).
[0152] A separator, preferably a 25 pm-thick Celgard 2400 polypropylene membrane of approximately 17 mm in diameter, was laid directly on the Cu-Ni disk. An electrolyte solution consisting of 1 mol LiTFSI in a mixture of DOL and DME and containing 0.5 mol LiNO3as a stabilizing additive was dispensed onto the separator in an amount of about 100 pL, thereby fully wetting the separator membrane.F07537 13.5.2026
[0153] 19
[0154] A 13 mm disk of LFP-coated aluminum foil was then positioned on the wetted separator to function as the cathode, after which the coin-cell assembly was completed by installing the spacer, spring, and lid and crimp-sealing the housing. The resulting cell architecture contains no pre-deposited lithium on the negative electrode. Upon initial charging, lithium is plated directly onto the Cu-Ni alloy surface, thereby establishing an anode-free configuration.
[0155] In a comparative example, a coin-type electrochemical cell was fabricated in which the negative electrode consisted of an untreated pure Cu current collector rather than the Cu-Ni alloy of the embodiment above. Cu foil of 13 mm diameter (> 99.9 wt % purity) was punched into disks, vacuum-dried at approximately 120 °C for at least 12 hours, and transferred into an argon-filled glovebox having oxygen and moisture levels below 0.1 ppm. Cell assembly then proceeded identically to the primary embodiment: the Cu disk was placed in the base of a 2032 coin-cell housing, a 25 pm Celgard 2400 separator of approximately 17 mm in diameter was laid upon the disk, and about 100 pL of an electrolyte comprising 1 mol LiTFSI in a mixture of DOL and DME and 0.5 mol LiNO3was dispensed to wet the separator. A 13 mm disk of LFP-coated aluminium foil was positioned on the wetted separator to serve as the cathode, after which the spacer, spring, and lid were installed and the cell housing was crimp-sealed.
[0156] Galvanostatic charge-discharge cycling was performed at 0.2 C using two otherwise identical anode-free lithium-metal coin cells that differed only in the material of the negative current collector (inventive Cu-Ni alloy or untreated Cu foil control).
[0157] The control cell employed an untreated Cu disc, prepared as described in the comparative example, while the inventive cell employed a binary Cu-Ni alloy disc fabricated according to the preceding embodiment.
[0158] Voltage profiles obtained over 100 cycles are presented in Fig. 6 a) and b) and reveal that while the bare-Cu cell delivered the higher initial specific discharge capacity, capacity retention diverged sharply thereafter.
[0159] Fig. 6 shows that the Cu control cell declined to 80% of its initial capacity after only 20 cycles, whereas the alloy-based cell required 63 cycles to reach 80% of its initial capacity, demonstrating substantially improved (>3x) resistance to lithium inventory loss. The endurance advantage persisted throughout extended cycling: after 100 cycles the Cu-Ni cell (0.17% by weight Ni) still retained 78 mAh / g milliampere-hours per gram, comfortably exceeding the 68 mAh / g remaining in the bare-Cu analogue. Expressed differently, the Cu-F07537 13.5.2026
[0160] 20
[0161] Ni alloy current collector maintained cumulative capacity retention to roughly 65% compared with nearly 44% for pure Cu over 100 cycles.
[0162] Because both cells shared identical LFP cathode, electrolyte formulation, separator, and assembly configuration, the enhanced stability can be attributed to the synergistic interfacial chemistry imparted by Ni incorporation (forming the Cu-Ni alloy) and improved surface smoothness.
[0163] As shown in Fig. 7, the coin cell that employs the Cu-Ni alloy current collector (0.17% by weight Ni) displays a slightly higher initial overpotential (both on charge and discharge) than the counterpart equipped with a bare-Cu collector, a trend that is consistent with the modest reduction in first-cycle discharge capacity observed for the Cu-Ni alloy system.
[0164] After repeated cycling, however, the voltage behaviour of the two cells diverges markedly. In the Cu-Ni alloy cell the average charge / discharge voltage converges to a stable plateau by approximately the 20th cycle (Fig. 7b). By contrast, the cell incorporating the bare-Cu collector exhibits a continually drifting average voltage throughout the same test window (Fig. 7a), indicating progressive interfacial degradation and loss of electrochemical efficiency.
[0165] The data therefore demonstrates that, despite a minor penalty in initial overpotential, the Cu-Ni alloy current collector delivers superior voltage stability and more durable energy efficiency over extended cycling compared to the bare Cu control.
[0166] Fig. 8 in a) illustrates the evolution of specific discharge capacity for anode-free lithium-metal coin cells that employ either a bare-Cu current collector or the Cu-Ni-alloy current collector described above.
[0167] Consistent with the capacity-retention behaviour already documented in Fig. 4, the Cu-Ni alloy-based (0.17% by weight Ni) cell preserves a substantially larger fraction of its initial capacity throughout prolonged cycling than does its bare-Cu analogue, confirming the superior lithium-inventory retention conferred by Ni incorporation (forming the Cu-Ni alloy) and surface smoothness.
[0168] Fig. 8 b) shows the Coulombic efficiency of the same two cells. The bare-Cu cell shows a marginally higher first-cycle efficiency, attributable to its lower nucleation over-potential; nevertheless, its average efficiency over the 100-cycle test window stabilises at only 98.88 %. In contrast, the Cu-Ni-collector cell, though beginning with a slightly lower initial value, rapidly converges to a steady plateau and achieves an average Coulombic efficiency of 98.97 %.
[0169] These data indicate that the Cu-Ni alloy current collector not only improves capacityF07537 13.5.2026
[0170] 21
[0171] retention but also reduces irreversible lithium losses over long-term cycling, as reflected by the higher sustained Coulombic efficiency.
[0172] Example 3 - Cell assembly:
[0173] In a further embodiment an anode-free lithium-metal pouch cell was fabricated by first thermoforming a multilayer aluminium-laminate film in a matched metal casting at elevated temperature and pressure to produce a rectangular cavity that serves as the pouch casing. A LFP composite cathode sheet was then cut with a high-precision steel die into electrodes measuring about 17 mm X 38.2 mm. Separately, the Cu-Ni-alloy current collector prepared according to the foregoing disclosure was cut into foils of approximately 18 mm X 39.2 mm, the slight oversizing ensuring complete lateral coverage when stacked.
[0174] The cell was assembled in a cathode | separator | anode sequence (inside an inertatmosphere dry-room): a microporous polymer separator was first placed in the formed pouch cavity, each LFP cathode was placed on the separator, another microporous polymer separator was laid over the cathode, and the Cu-Ni foil was positioned on the separator to act as the negative current collector. The stack sequence was repeated to the desired layer count (in this example 20 layers of Cu-Ni alloy), after which three of the four pouch edges are heat-sealed, leaving one short edge temporarily open.
[0175] An electrolyte of 1 mol LiFSI in DME diluted with 1,1,2,2-tetrafluoroethyl 2, 2,3,3-tetrafluoropropylether (TTE) — was injected through the open edge. Finally, the partially sealed pouch was evacuated to remove entrained gas and then heat-sealed along the remaining edge, thereby completing the hermetic cell enclosure.
[0176] All dimensions, solvent ratios, and sealing conditions may be adjusted within the ranges described herein without departing from the scope of the invention.
[0177] Fig. 9 depicts the cycling performance of a multilayer anode-free lithium-metal pouch cell incorporating the Cu-Ni-alloy current collector and LFP-based cathodes prepared and assembled as set forth above. Cell used electrolyte above
[0178] When charged and discharged at 0.2 C, the cell delivers an initial discharge capacity of about 500 mAh and sustains more than 85 % of that capacity after 45 cycles, thereby demonstrating robust capacity retention.
[0179] Preparation of Cu-Ni alloy anode material with silver layer:
[0180] A thin film of nickel (Ni) is deposited directly onto the Cu substrate to a thickness of about 10 nm to about 1000 nm, and more preferably from about 20 nm to 300 nm. The Ni layer may be formed by magnetron sputtering, for examples in an FHR Pentaco 100 system suingF07537 13.5.2026
[0181] 22
[0182] a Ni target of at least 99.95% purity, at a working pressure of approximately 0.003 mbar with an argon (Ar) flow rate of 200 seem while sustaining a direct-current plasma of about 0.25 kW, thereby achieving the desired film thickness. Alternatively, the Ni layer may be deposited by electron-beam evaporation under conditions selected to deliver the same thickness range.
[0183] Following deposition, the Cu / Ni template is subjected to an annealing treatment intended to alloy the metals into a binary Cu-Ni current collector. The as-deposited structure is heated within a chemical vapor deposition (CVD; Graphene Square Inc.; TCVD-RF100CA) chamber operated at a pressure of about 8 Torr while a process gas stream consisting of 50 seem of hydrogen (H2) and 800 seem of Ar are introduced. The temperature is raised to between 600 and 900 °C by a ramp lasting roughly 2-3 hours and held for about 15 minutes. This thermal step promotes interdiffusion of Cu and Ni, uniformly converting the Cu / Ni template into the Cu-Ni alloy with promoting the surface smoothness.
[0184] The resulting current collector exhibits a continuous alloy layer whose composition is governed by the controlled Ni content and annealing process.
[0185] Preparation of Ag thin film on said Cu-Ni alloy: A thin film layer of silver (Ag) is deposited directly onto the (pre-prepared, already annealed e.g. @ 600 or 900°C) Cu-Ni alloy substrate to a thickness of about 10 nm to about 200 nm, and more preferably from about 20 nm to 100 nm. The Ag layer may be formed by E-beam evaporator using Ag pellets of at least 99.99% purity. Deposition is carried out under a pressure of about 10'6Torr at an evaporation rate of around 0.3-0.4 A / s. Alternatively, the Ag layer may be deposited by magnetron sputter under conditions selected to deliver the same thickness range.
[0186] Following deposition, the Ag / Cu-Ni template is subjected to a mild annealing treatment. The as-deposited structure is heated within a chemical vapor deposition chamber operated at a pressure of about 1 Torr while a process gas stream consisting of 10 seem of hydrogen (H2) and 200 seem of Ar are introduced. The temperature is raised to between 400 and 600 °C by a ramp lasting roughly 30 minutes and held for about 20 minutes. This thermal step promotes enlargement of Ag grain size at 400 °C.
[0187] The resulting current collector exhibits a contiguous Ag layer on the surface of the Cu-Ni alloy.
[0188] It is noted that annealing under the conditions given in Yu, et.al. (2025. Ag-Cu alloy induces uniform lithium nucleation and growth in anode-free lithium metal batteries. Electrochimica Acta, 535, p.146623) on Cu substrates leads to an Ag-Cu alloy formation or non-contiguous silver layers at temperatures above 400 °C, and does not lead to a remaining contiguous Ag film on top of the Cu layer. Also, using the approach described in the paper leads to aF07537 13.5.2026
[0189] 23
[0190] significant drop in the initial specific capacity compared with pure copper, going down to about 10% compared with copper. Capacity retention at 100 cycles is only about 35%.
[0191] Furthermore, if Cu substrates are subsequently nickel and silver coated and then heat treated so that a ternary alloy Cu-Ni-Ag is formed and there is no remaining silver film, the normalized capacity retention at 100 cycles is significantly worse (48%) than for the uncoated copper nickel alloy, which is 64%. For the annealing, the temperature is raised to 900 °C by a ramp lasting roughly 2-3 hours and held for about 15 minutes.
[0192] As one can see from Fig. 10, showing the data for an Ag film on Cu-Ni alloy current collector. The data for a 60-nm-thick Ag film deposited onto Cu-Ni alloy (vapor deposition) followed by mild annealing treatment (400°C for 20 minutes) are given. It is the combination of temperature and time that yields a contiguous thin film on the surface of the Cu-Ni alloy and is insufficient duration to complete a full transformation to AgCuNi ternary alloy (SEM images see Fig. 11). The Ag film on Cu-Ni alloy shows high stability and long-term capacity retention of ca.60% after 100 cycles @ 1C and improvement over Cu-Ni alloy capacity retention ca.55% after 100 cycles @ 1C.
[0193] Fig. 11 shows in a) a SEM image of Ag film on surface of Cu-Ni alloy before heat treatment and in b) a SEM image of Ag film on surface of Cu-Ni alloy after mild annealing heat treatment @ 400 °C for 20 mins after ramping up from room temperature to 400 °C for 20 mins with the Ag layer.
[0194] C: Preparation of LFP batteries & testing method:
[0195] An anode-free lithium-metal coin cell in which the negative electrode is a disk of a Cu-Ni alloy, the positive electrode is a lithium iron phosphate (LFP) layer coated on aluminum foil, and a microporous polypropylene separator is interposed between the two electrodes (see also Fig. 3). Negative electrode disks (either Cu-Ni alloy annealed at 600 or 900 °C, or of the Ag-Cu-Ni alloy annealed at 900 °C) having a diameter of approximately 13 mm were punched from foil stock, dried under vacuum at about 120 °C for not less than 12 hours, and transferred into an argon-filled glovebox maintained at oxygen and moisture levels below 0.1 ppm. Each negative electrode disk material was then placed in the base of a stainless-steel 2032 coin-cell housing to serve as the anode (current collector).
[0196] D: Preparation of NCM batteries & testing method, Example 4
[0197] In a further embodiment an anode-free lithium-metal pouch cell was fabricated by firstF07537 13.5.2026
[0198] 24
[0199] thermoforming a multilayer aluminium-laminate film in a matched metal casting at elevated temperature and pressure to produce a rectangular cavity that serves as the pouch casing. A NCM composite cathode sheet was then cut with a high-precision steel die into electrodes measuring about 17 mm X 38.2 mm. Separately, the Cu-Ni-alloy current collector with or without Ag layer prepared according to the foregoing was cut into foils of approximately 18 mm X 39.2 mm, the slight oversizing ensuring complete lateral coverage when stacked. Each cell was assembled in a cathode | separator | anode sequence (inside an inertatmosphere dry-room): a microporous polymer separator was first placed in the formed pouch cavity, each NCM cathode was placed on the separator, another microporous polymer separator was laid over the cathode, and the negative electrode (e.g. Cu-Ni alloy foil) was positioned on the separator to act as the negative current collector. The stack sequence was repeated to the desired layer count (in this example 20 layers of Cu-Ni alloy), after which three of the four pouch edges are heat-sealed, leaving one short edge temporarily open.
[0200] An electrolyte of 1 mol LiFSI in DME diluted with 1,1,2,2-tetrafluoroethyl 2, 2,3,3-tetrafluoropropylether (TTE) was issued through the open edge. Finally, the partially sealed pouch was evacuated to remove entrained gas and then heat-sealed along the remaining edge, thereby completing the hermetic cell enclosure.
[0201] All dimensions, solvent ratios, and sealing conditions may be adjusted within the ranges described herein without departing from the scope of the invention.
[0202] In a further embodiment, the electrochemical performance of the anode-free lithium-metal cell prepared according to the foregoing disclosure was evaluated by means of a capacity retention metric, which was calculated as follows.
[0203] As-assembled cells were first subjected to a formation protocol comprising three (3) consecutive charge-discharge cycles at 0.1 C rate, the purpose of which is to establish a stable solid-electrolyte interphase and to condition the cell prior to long-term cycling. C-rate is the charge (or discharge) current normalized to a battery’s rated capacity. 1C corresponds to charging (or discharging) the full nominal capacity in 1 hour (e.g. a 10 Ah cell at 1C » 10 A, while at 0.1 C (C / 10) corresponds to a 10-hour charge or discharge at 1 A).
[0204] Upon completion of the formation step, each cell was transitioned to standard cycling at 1.0 C, and the discharge capacity recorded during the first post-formation cycle (i.e., the first cycle following the three formation cycles) was designated as the reference discharge capacity, Ci, and used as the denominator in all subsequent retention calculations.
[0205] The discharge capacity measured during any later cycle of interest, denoted Cnwhere nF07537 13.5.2026
[0206] 25
[0207] represents the cycle number, was used as the numerator. The capacity retention (%) at cycle n was thereby defined according to the relation:
[0208] Capacity Retention (%) = (Cn / C * 100
[0209] wherein Cnis the discharge capacity at the n-th cycle following formation and Ci is the discharge capacity of the first cycle following formation.
[0210] It is to be understood that the number of formation cycles, the current densities employed during formation and standard cycling, and the upper and lower cutoff voltages may be adjusted within the ranges described herein without departing from the scope of the invention.
[0211] The performance of the proposed approaches can be summarized as follows (summary of anode-free lithium metal battery capacity retention after 100 cycles):
[0212] Battery data based on LFP cathode & LiTFSI electrolyte (see above C for preparation, illustration in Fig. 12):
[0213] [1] Conventional Cu current collector n / a (cell not stable to 100 cycles)
[0214] [1] Ag-Cu current collector ca. 35% at 100 cycles
[0215] Cu current collector ca. 44% at 100 cycles
[0216] Ag-Cu-Ni ternary alloy current collector (annealed @ 900°C)
[0217] ca.48% at 100 cycles (9% #)
[0218] Cu-Ni alloy current collector (annealed @ 900°C)
[0219] ca.64% at 100 cycles (45% #)
[0220] Cu-Ni alloy current collector (annealed @ 600°C)
[0221] ca.66% at 100 cycles (50% #)
[0222] [1]: Yu, et.al., 2025. Ag-Cu alloy induces uniform lithium nucleation and growth in anode-free lithium metal batteries. Electrochimica Acta, 535, p.146623.
[0223] #: Improvement of capacity retention above Cu current collector
[0224] Battery data based on NCM cathode & LiTFSI electrolyte (see above D for preparation, illustration in Fig. 13):
[0225] Cu-Ni alloy current collector (annealed @ 900°C)
[0226] ca.55% at 100 cycles
[0227] Ag film on Cu-Ni alloy * ca.60% at 100 cycles
[0228] : Cu-Ni alloy pre-annealed @ 900°C. Deposition of Ag then mild annealing (400°C for 20F07537 13.5.2026
[0229] 26
[0230] minutes) but not to completion of ternary alloy formation. Contiguous Ag film is retained on surface.
[0231] LIST OF REFERENCE SIGNS
[0232] 1 battery, e.g. solid-state battery or anode-free battery
[0233] 2 cathode material
[0234] 3 electrolyte; liquid electrolyte (with separator membrane), or solid-state electrolyte
[0235] 4 artificial solid electrolyte interphase layer, porous graphene layer
[0236] 5 anode (or current collector) material
[0237] 6 polymer separator
[0238] 7 aluminium foil
[0239] 8 selective graphene layer with defects
[0240] 9 pores in 4
[0241] 10 lithium layer
Claims
F07537 13.5.202627CLAIMS1. Li or Na based battery (1) having a current collector, in particular an anode (5), which consists of a copper-nickel alloy with a copper content in the range of 98.100 to 99.990 % by weight and a nickel content in the range 0.010 to 1.900% by weight, the copper and nickel contents complementing to 100% by weight of the current collector.
2. Battery (1) according to claim 1, wherein the current collector, in particular the anode (5), is made from a copper-nickel alloy with a copper content in the range of 98.200 to 99.925 % by weight, preferably 99.000 to 99.900 % or 99.250 - 99.850 % by weight and a nickel content in the range 0.075 to 1.800% by weight, preferably 0.100 to 1.000% or 0.150 - 0.750 % by weight, in each case the copper and nickel contents complementing to 100% by weight of the current collector.
3. Battery (1) according to any of the preceding claims, wherein the current collector, in particular the anode (5), is at least partially covered on its side facing the electrolyte (3) by at least one artificial solid-electrolyte interphase layer (4) with at least one layer of porous graphene of a thickness of less than 25 nm with pores (9) having an average characteristic width as defined in the specification in the range of 1 - 1000 nm, wherein preferably the artificial solid-electrolyte interphase layer (4), preferably the porous graphene layer, has a thickness in the range of 1-15 nm, preferably in the range of 5-10 nm.and / or wherein the porous graphene layer has an areal porosity in the range of at least 10%, preferably at least 15%, more preferably of at least 20% or at least 25% or at least 30% or at least 40%,and / or said porous graphene has pores having an average characteristic width in the range of 5 - 900 nmand / or wherein it is a solid-state battery and the electrolyte (3) is a solid electrolyte.
4. Battery (1) according to any of the preceding claims, wherein the current collector, in particular the anode (5), is at least partially, preferably fully, covered on its side facing the electrolyte (3) by at least one contiguous, preferably annealed, Ag layer, preferably having a thickness in the range of 1-110 nm, or in the range 10 - 80 nm or 30 -60 nm, preferably in the range of 20-50nm.
5. Battery (1) according to any of the preceding claims, wherein the currentF07537 13.5.202628collector, in particular the anode (5), takes the form of a porous mesh, grid, woven or nonwoven fibre based structure or a foil, preferably a foil with a thickness in the range of 0.001-0.10mm, preferably in the range of 0.01-0.04 mm.
6. Battery (1) according to any of the preceding claims, wherein the anode (5) consists of a copper-nickel alloy with a copper content in the range of 98.100 to 99.990 % by weight and a nickel content in the range 0.010 to 1.900% by weight, the copper and nickel contents complementing to 100% by weight of the anode (5).
7. Current collector, in particular anode (5), for a Li or Na based battery (1) according to any of claims 1-6, wherein the current collector, in particular the anode (5), which is made from a copper-nickel alloy with a copper content in the range of 98.100 to 99.990 % by weight and a nickel content in the range 0.010 to 1.900% by weight, the copper and nickel contents complementing to 100% by weight of the current collector.
8. Method form making a current collector, in particular an anode (5), according to claim 7 or for making a current collector, in particular an anode (5), for a battery (1) according to any of claims 1-6, whereina nickel film is applied to a pure copper foil followed by annealing to generate the current collector, in particular the anode (5), in the form of a copper-nickel alloy.
9. Method according to claim 8, wherein said nickel film is applied by using electrochemical plating, e-beam evaporation, physical vapor deposition (PVD), electroplating, or (magnetron) sputtering, to form a nickel film of a thickness in the range of 1 nm to 2200nm, preferably in the range of 10-1000 or 15-500 nm, preferably in the range of 20-300 nm or 20 - 60 nm on a pure copper foil.
10. Method according to claim 8 or 9, wherein said nickel film is applied to a pure copper foil having a thickness in the range of 0.005-0.10mm, preferably in the range of 0.01-0.06 mm, preferably having a purity of more than 99.5% or more than 99.8%.
11. Method according to any of claims 8 - 10, wherein said annealing is carried out at a temperature in the range of 500-1000°C, in the range of 500 - 950°C or in the range of 500 - 900°C or preferably in the range of 800-900°C, in particular during a time span of 10 minutes-300 minutes.F07537 13.5.20262912. Method according to any of claims 8 - 11, wherein said annealing is carried out during a time span in the range of 10 minutes-300 minutes or 120 - 240 minutes, and / or wherein said annealing is carried out under hydrogen and / or argon atmosphere and / or under a pressure in the range of 10-10,000 Pa.
13. Method according to any of claims 8 - 12, wherein at least one side of said copper-nickel alloy is covered, preferably by vapour deposition, by at least one contiguous Ag layer, preferably having a thickness in the range of 1-100 nm or in the range 10-70 nm or 25 - 50 nm, preferably in the range of 20-40 nm, followed by annealing carried out at a temperature in the range of 250 - 600°C, in the range of 275 - 550°C or in the range of 300 - 500°C during a time span of 10 minutes-80 minutes or in the range of 15-30 minutes.
14. Use of a current collector, in particular an anode (5), according to claim 7 for making a Li or Na based battery (1) according to any of claim 1-6.
15. Use according to claim 14, wherein an anode (5) according to claim 7 is used for making the anode (5) of a Li or Na based battery (1) according to any of claims 1-6.