Process for manufacturing cellulose microfibrils using a twin-screw extruder

The aldehyde-assisted fractionation pretreatment of lignocellulosic fibers in an acidic solvent, combined with twin-screw extrusion, addresses the inefficiencies of traditional methods by preserving cellulose structure and reducing environmental impact, resulting in high-quality cellulose microfibrils with enhanced mechanical properties.

WO2026238844A1PCT designated stage Publication Date: 2026-11-19INSTITUT NAT POLYTECHN DE GRENOBLE +4
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063995
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for manufacturing cellulose microfibrils are energy-intensive, environmentally harmful, and produce low-quality suspensions due to the use of harsh chemical treatments and bleaching processes, which degrade the cellulose structure and limit scalability.

Method used

A method involving aldehyde-assisted fractionation (AAF) pretreatment of lignocellulosic fibers in an acidic organic solvent to preserve the cellulose structure, followed by mechanical treatment with a twin-screw extruder, eliminating the need for bleaching and oxidative treatments, and enabling efficient fibrillation.

Benefits of technology

This process reduces environmental impact, lowers production costs, and enhances the quality and mechanical properties of cellulose microfibrils by maintaining their native structure, allowing for higher lignin content and improved barrier properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026063995_19112026_PF_FP_ABST
    Figure EP2026063995_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing cellulose microfibrils comprising: a) Providing a first composition derived from biomass and comprising lignocellulosic fibers, b) Conducting a chemical pretreatment step by reacting the lignocellulosic fibers of step a) with an aldehyde in the presence of an acid catalyst in an organic solvent to form a second composition comprising aldehyde treated cellulose, aldehyde protected lignin and hemicellulose, wherein the aldehyde protected lignin and the hemicellulose are dissolved in the organic solvent, c) Separating at least the aldehyde treated cellulose from the organic solvent, d) Mechanically treating the aldehyde treated cellulose obtained in step c) by a twin-screw extruder to form the cellulose microfibrils.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Process for manufacturing cellulose microfibrils using a twin-screw extruder

[0002] The present invention relates to the manufacture of cellulose microfibrils from lignocellulosic fibers. It has particularly advantageous applications in the fields of packaging, paper, membranes, and even cosmetics and paints as a rheology modifier.

[0003] The recovery of biomass is an extremely important aspect of the decarbonization of our daily lives, as it enables the generation of basic ingredients for the chemical and manufacturing industries. Traditional uses of biomass generally focus on the extraction of cellulose and the manufacture of paper or textiles from it, which represent 40 to 80% of the biomass by mass. This stage, known as biorefining, is typically carried out using bleaching processes.

[0004] A large proportion of packaging today is made from plastic materials, particularly non-biodegradable plastics. In general, these materials are produced from non-renewable resources, particularly petrochemical-based polymers. In the field of food packaging, there is considerable interest in finding biodegradable materials in order to limit the impact of packaging on the environment. Interest would be further enhanced if such biodegradable materials were also at least partly bio-based, in order to reduce the proportion of petrochemical-based polymers, or even replace them altogether.

[0005] Bio-based and / or biodegradable polymers are promising candidates for this purpose. However, these polymers are generally considered to be less effective than petrochemical-based polymers, particularly in terms of their mechanical properties and their barrier properties to gases (e.g., oxygen, water vapor) and liquids (e.g., oil and water).

[0006] Cellulose microfibrils (CNF for "cellulose nanofibers" or, equivalently, MFC for "microfibrillated cellulose" according to Anglo-Saxon terminology) have additional properties that make them very attractive. MFC films can be transparent and have high mechanical properties. MFCs also have barrier properties, such as barriers against grease, oxygen, aromas, and contaminants. Industrial production of MFCs began in 2011, but the quantities produced are still low due to manufacturing costs (high energy consumption, raw material costs, chemicals) and also due to transportation costs (due to the low dry matter concentration of the suspensions produced). Cellulose microfibril compositions are currently produced at a concentration of between 2% and 5% dry matter, i.e. , 98% to 95% water. The

[0007] A24555WO / 13. 05. 2026 / 2% compositions behave like a gel and it is very difficult to remove the water from them. As a result, most of the material transported is water, which also creates storage problems.

[0008] WO2020221934A1 describes a process for manufacturing a cellulose microfibril suspension from an aqueous suspension of cellulose fibers, comprising mechanical treatment of the suspension by a twin-screw extruder in order to fibrillate the cellulose fibers. This process produces a cellulose microfibril suspension with a much higher consistency than conventional solutions. However, this process starts with a pulp that has been bleached using standard papermaking processes (e.g., the Kraft process) and requires the cellulose fibers to undergo chemical oxidation treatment, for example with ozone, prior to extrusion. This affects the properties of the cellulose microfibrils obtained. The energy and environmental costs of this process also remain significant.

[0009] Saad et al. (2022, Cellulose 2022, 29:5593-5607) reported a process for producing lignin-containing micro- and nanofibrillated cellulose from lignocellulosic biomass, specifically Eucalyptus globulus bark, using steam explosion as a key pretreatment step. In their approach, the bark is first subjected to steam explosion under elevated temperature and pressure conditions, which disrupts the lignocellulosic structure and promotes the partial depolymerization of hemicelluloses as well as the weakening of the lignin-carbohydrate matrix. The pretreated material is subsequently subjected to alkaline treatment and mechanical refining and grinding in order to obtain lignin-containing micro- and nanofibrillated cellulose suspensions.

[0010] Talebi Amiri et al. (Nature Protocols, Vol. 14, 2019, 921-954) describe a method for the fractionation of lignocellulosic biomass that enables the isolation of lignin in a stabilized form while simultaneously allowing the separation of carbohydrate fractions. In their approach, lignin is extracted from biomass under acidic conditions in the presence of aldehydes, such as formaldehyde or propionaldehyde, which act as stabilizing agents during the depolymerization process. The aldehyde reacts with reactive lignin intermediates, preventing condensation reactions that would otherwise lead to the formation of recalcitrant C-C linkages and thereby preserving the native lignin structure.

[0011] The problem underlying the present invention is to provide a method for manufacturing cellulose microfibrils that achieves both a reduced environmental impact and a high quality of the resulting suspension.

[0012] A24555WO / 13. 05. 2026 / The problem is solved by the method and the cellulose microfibrils according to the present invention. Further preferred embodiments are set forth in the dependent claims.

[0013] It has been shown that the method according to the invention results in a reduced environmental impact and a high quality of the resulting microfibrils. The method for producing cellulose microfibrils comprises at least the following steps:

[0014] a) Providing a first composition derived from biomass and comprising lignocellulosic fibers,

[0015] b) Conducting a chemical pretreatment step by reacting the lignocellulosic fibers of step a) with an aldehyde in the presence of an acid catalyst in an organic solvent to form a composition comprising aldehyde treated cellulose, aldehyde protected lignin and hemicellulose, wherein the aldehyde protected lignin and the hemicellulose are dissolved in the organic solvent,

[0016] c) Separating at least the aldehyde treated cellulose from the organic solvent,

[0017] d) Mechanically treating the aldehyde treated cellulose obtained in step c) by a twin-screw extruder to form the cellulose microfibrils.

[0018] The chemical treatment described in step b) is an aldehyde-assisted fractionation (AAF) and enables the extraction of biomass components, namely lignin, cellulose, and, for example, hemicellulose. The use of an acidic medium promotes the isolation of these components while preserving their properties. AAF pretreatment is conducted in an organic solvent. Due to the combination of the AAF pretreatment and acidic conditions (using an acid catalyst) rather than basic conditions, the cellulose structure and fibers do not swell as they do in most conventional methods. As a result, the aldehyde treated cellulose (also called AAF cellulose) retains a structure similar to that of the original wood and does not resemble traditional cellulose pulp. This means that the cellulose remains more intact and wood-like, since the combination of the AAF pretreatment and acidic conditions preserves the original structure much better than alkaline treatments.

[0019] Before the mechanical treatment is carried out, the cellulose is separated from the organic solvent, so that it subsequently takes the form of a highly viscous composition, typically having a dry matter

[0020] A24555WO / 13. 05. 2026 / content of between 10% and 60% by weight, relative to the total weight of the composition. This can be done, for example, by filtration.

[0021] Surprisingly, it was found that the aldehyde treated cellulose (i.e. AAF cellulose) could be fibrillated, preferably directly, in a twin-screw extruder. Remarkably, AAF pretreatment makes it possible to weaken the lignocellulosic fibers sufficiently to allow them to pass through a twin-screw extruder for effective fibrillation, which is typically achieved after oxidation or biological pretreatment (enzymatic hydrolysis). One significant advantage of using AAF pretreatment is that the cellulose remains more intact and wood-like, preserving its native structure. This not only results in fibers with enhanced mechanical properties but also reduces the extent of chemical modification and degradation. As a result, the final material exhibits improved strength, durability, and a more natural appearance compared to fibers processed with harsher methods. Additionally, maintaining a more intact cellulose structure can lead to higher yields and better process efficiency, while potentially lowering the environmental impact due to reduced chemical usage and milder processing conditions.

[0022] The process according to the present invention reduces the number of steps and the energy cost of manufacturing cellulose microfibrils thanks to the synergy between AAF pretreatment and fibrillation by twin-screw extruder. This leads to higher efficiency and lower production costs compared to conventional methods. Additionally, the improved process enables easier scalability for industrial applications.

[0023] In addition, since AAF pretreatment sufficiently weakens the cellulose fibers for passage through the twin-screw extruder, it is not necessary to use pulp bleached by conventional papermaking processes or to carry out oxidative or enzymatic treatment prior to fibrillation. The microfibrils obtained can thus contain a higher proportion of lignin than cellulose microfibrils obtained from traditional pulps. This can be particularly advantageous because lignin gives cellulose microfibrils greater hydrophobicity and improved barrier properties. Furthermore, the retention of lignin can reduce processing costs and environmental impact by eliminating the need for harsh chemicals and energy-intensive bleaching steps. This approach also broadens the range of suitable raw materials, enabling the use of less refined or even waste lignocellulosic sources.

[0024] A24555WO / 13. 05. 2026 / Within the context of the present invention, “lignocellulosic fibers” refer to fibrous structures that are derived from plant-based materials containing lignin, cellulose, and hemicellulose as principal components.

[0025] A further aspect of the present invention relates to cellulose microfibrils that can be obtained by the process according to the present invention. The cellulose mibrofibrils have a lignin content between 1 % and 40% by weight relative to the total dry weight of cellulose microfibrils, and characterized in that said lignin has p-O-4 content of 50% to 80%, preferably of 70% to 80%. They are also called lignified cellulose microfibrils.

[0026] Another aspect concerns the use of the cellulose microfibrils according to the present invention to form a paper.

[0027] BRIEF DESCRIPTION OF THE FIGURES

[0028] Figure 1 shows the steps in the process of manufacturing the cellulose microfibrils and manufacturing paper from the cellulose microfibrils, according to a particular example of implementation. Variants are also indicated in dotted lines.

[0029] Figure 2 shows a front view of the two screws, juxtaposed with each other, of the twin-screw extruder used in one embodiment.

[0030] Figure 3 shows a front view of one of the two screws shown in Figure 2.

[0031] Figures 4Ato 4C show enlargements of the different fibrillation segments of the screw shown in Figure 3.

[0032] Figure 5 is a graph of the time in minutes taken to reach 80°SR for AAF-pretreated cellulose (AAF-cellulose), unbleached hardwood (UHW), and unbleached softwood (USW), according to one embodiment.

[0033] Figure 6 is a graph of torque (in Nm) as a function of time in minutes during twin-screw extrusion for AAF-pretreated cellulose (AAF-cellulose) and commercial unbleached Kraft pulp (UKP) according to

[0034] A24555WO / 13. 05. 2026 / an example implementation. The passages of AAF-cellulose through the extruder can be observed by the change in torque at 40, 60, 75, and 85 minutes.

[0035] Figures 7A and 7B are optical microscopy images of, respectively: 7A: lignified cellulose microfibrils obtained according to one example of the process and without enzymatic treatment prior to mechanical treatment in a twin-screw extruder; 7B: lignified cellulose microfibrils obtained according to an example of the process and with enzymatic treatment prior to mechanical treatment in a twin-screw extruder.

[0036] Figure 8 shows a schematic representation of the chemical pretreatment of the process according to the invention and possible processing steps prior to extrusion.

[0037] DETAILED DESCRIPTION

[0038] Before embarking on a detailed review of the embodiments of the invention, the following are optional features that may be used in combination or alternatively.

[0039] According to one example, the first composition has a lignin content of between 1 % and 40% by weight, relative to the total dry weight of the first composition. By adjusting the lignin content of the first composition to a range of 1 % to 40% by weight, relative to the total dry weight, particularly when using wood-based raw materials, an optimal balance between mechanical strength and processability is achieved. A moderate to high lignin content, for example 20 to 30%, especially enhances the structural integrity of the final cellulose microfibrils, while still allowing for efficient processing.

[0040] According to one example, the first composition comprises lignocellulosic fibers derived from wood, preferably the first composition comprises wood fragments. Within the context of the present invention, “wood fragments” refer to pieces of wood that have been mechanically processed or comminuted from natural wood sources. These fragments may include chips, particles, splinters, shavings, or other irregularly shaped pieces that retain the essential lignocellulosic structure of the original wood. The size, shape, and degree of comminution of the wood fragments can vary depending on the requirements of the specific application, but they are generally larger and less refined than isolated wood fibers or powders. Both hardwood and softwood can be used as biomass sources. Hardwood has a higher syringol content and a greater xylose content. A high xylose content ensures good fiber swelling, which contributes to high-quality paper production. It increases the contact area and

[0041] A24555WO / 13. 05. 2026 / strengthens the fiber-to-fiber bonds, resulting in higher tensile strength in the paper. The process according to the invention allows the use of both types of wood, which provides high flexibility, whereas this was not possible in the prior art.

[0042] Lignocellulosic fibers derived from wood are characterized by lignins and hemicelluloses that differ from those found in “alternative raw materials” not derived from wood, such as hemp, wheat, or flax. Typically, wood-derived fibers contain lignin in the range of 20% to 35% by weight and hemicelluloses in the range of 15% to 35% by weight, relative to the total dry weight. These “alternative raw materials” are typically easier to fibrillate. However, their availability remains limited for industrial-scale production. Wood is a widely available source for the industrial-scale production of cellulose microfibrils. Aldehyde-assisted fractionation pretreatment according to the present invention sufficiently weakens the lignocellulosic fibers in wood to enable the efficient formation of cellulose microfibrils using a twin-screw extruder. The pretreatment modifies the structure of the wood-derived fibers, disrupting the lignin-carbohydrate complex and loosening the fiber matrix, thereby facilitating the subsequent fibrillation process. Experimental evidence has shown that, in the absence of the aldehyde-assisted fractionation pretreatment, cellulose fibers obtained from wood, despite having a comparable lignin content, cannot be successfully fibrillated by means of twin-screw extrusion. This is due to the inherent rigidity and resistance of untreated lignocellulosic fibers, which prevents the mechanical forces within the extruder from separating the fibers into microfibrils. The aldehyde-assisted fractionation pretreatment thus represents a key enabling step that overcomes this technical barrier. As a result, the present invention allows for the use of wood -derived lignocellulosic fibers as a starting material for the production of cellulose microfibrils on an industrial scale. Wood is a cost-effective, readily available, and renewable resource, making it an attractive alternative to other, less abundant feedstocks. By enabling the efficient processing of these lignocellulosic fibers, the invention provides a pathway for the large-scale, economically viable manufacture of cellulose microfibrils.

[0043] In one example, the first composition is unbleached. Upstream of the process, the first composition has therefore not undergone a bleaching step according to the usual papermaking processes, for example by the Kraft process or by TEMPO oxidation. By omitting the bleaching step, the process becomes more environmentally friendly, as bleaching often involves the use of chemicals that can generate harmful byproducts and require additional energy and water consumption. Further, avoiding

[0044] A24555WO / 13. 05. 2026 / bleaching reduces overall production costs, since fewer chemicals and process steps are required. In addition, the mechanical and chemical integrity of the lignocellulosic fibers is better preserved, as bleaching can partially degrade the cellulose or alter its surface properties, which may negatively impact the efficiency of subsequent fibrillation or the performance of the final product.

[0045] The lignin content in AAF cellulose and in cellulose microfibrils can be controlled. AAF lignin and hemicellulose are soluble in organic solvents, whereas the aldehyde-treated cellulose that contains a residual lignin content remains as a solid in the composition.

[0046] In one embodiment of the present invention the aldehyde treated cellulose can be separated from the aldehyde-protected lignin. Filtration can be used to separate the dissolved hemicellulose and dissolved AAF-lignin, leaving the cellulose with only a residual lignin content (see Figure 8, option B).

[0047] Alternatively, according to another aspect of the present invention, before step c), the aldehyde-protected lignin in the second composition is precipitated by adding an acid (for example, sulfuric acid, preferably to a pH below 4) and / or by adding an anti-solvent. Within the context of the present invention an antisolvent is a liquid in which AAF lignin has low solubility and which, when added to the second composition, reduces the solubility of AAF lignin and thereby induces its precipitation. An example of an antisolvent is water, which can preferably be added in excess. In step c), the aldehyde-treated cellulose and the aldehyde-protected lignin are then separated from the hemicellulose and the organic solvent, preferably by filtration (see Figure 8, option A). This typically results in a lignin content that is about 10% higher than when the dissolved lignin is removed by. Preferably, the AAF cellulose and the cellulose microfibrils according to the present invention have a lignin content of between 1% and 40%, preferably between 5% and 30%, even more preferably between 10% and 25% by weight relative to the total dry weight of the second composition. There is no significant difference in the lignin content before and after fibrillation using twin-screw extrusion.

[0048] According to one example, the process does not include a delignification step for the second pretreated cellulose composition between the aldehyde-assisted fractionation pretreatment and the mechanical treatment. Within the context of the present invention, “delignification” means any process step specifically intended to reduce or remove lignin from the cellulose composition, such further chemical, treatments. The mere separation of already solubilized lignin from the AAF cellulose containing

[0049] A24555WO / 13. 05. 2026 / suspension by filtration, washing, or other physical means is not considered delignification, unless it is combined with an active process that further reduces the lignin content of the cellulose phase. Examples are a kinematic treatment or a treatment with an oxidizing agent, for example ozone. During the development of the invention, it was found that the aldehyde-assisted fractionation pretreatment sufficiently weakened the lignocellulosic fibers for the formation of cellulose microfibrils by twin-screw extrusion. It is therefore not necessary to delignify the pretreated cellulose before it passes through the extruder, even though it is, of course, possible to take such a step. The process is thus particularly advantageous for obtaining cellulose microfibrils with a higher lignin content than those that have undergone delignification. The cellulose microfibrils obtained has particularly advantageous hydrophobic and barrier properties.

[0050] According to one example, at the inlet of the twin-screw extruder, a composition comprising the aldehyde-treated cellulose (i.e. , the pretreated cellulose) has a lignin content of between 1 % and 40%, preferably between 5% and 30%, even more preferably 10% to 25% by weight relative to the total dry weight of the pretreated cellulose. During the development of the invention, it was found that pretreatment by aldehyde-assisted fractionation sufficiently weakened the lignocellulosic fibers to allow the formation of cellulose microfibrils by twin-screw extrusion, with significant lignin content. The lignin proportion can be substantially maintained between the start and end of the extrusion treatment. The cellulose microfibrils can therefore have a lignin proportion substantially between 1% and 40% by weight relative to the total dry mass of the suspension. The cellulose microfibrils have particularly advantageous hydrophobic and barrier properties. This means that such a material effectively repels water and provides an excellent barrier against gases and liquids, making it highly suitable for applications such as coatings and packaging materials. Furthermore, the presence of lignin makes the production process more resource-efficient and potentially more cost-effective compared to fully bleached cellulose products. By retaining lignin, the microfibrils also exhibits enhanced mechanical strength and durability.

[0051] According to one example, during pre-treatment by aldehyde-assisted fractionation, the first composition is maintained, preferably heated, at a temperature less than or equal to 100°C, preferably less than or equal to 80°C. This temperature control ensures a good yield.

[0052] A24555WO / 13. 05. 2026 / According to one example, during pre-treatment by aldehyde-assisted fractionation, the first composition is heated to a temperature greater than or equal to 50°C.

[0053] According to one example, during pretreatment by aldehyde-assisted fractionation, the first composition is heated for a period of substantially between one and five hours, preferably substantially equal to three hours.

[0054] Conventional methods for preparing cellulose pulp, for example by the Kraft process, are generally carried out at higher temperatures, typically 140°C, and for significantly longer periods of time, typically between 10 and 20 hours. The process according to the invention therefore significantly reduces the time and energy required to manufacture the cellulose microfibril suspension. The process is thus more compatible with industrial-scale manufacturing constraints.

[0055] In one example, the aldehyde is an aldehyde according to the formula R-CHO, wherein R is selected from the group consisting of hydrogen, an aliphatic chain comprising one to six carbon atoms, such as for example propionaldehyde, and (CH2)nCOOH, wherein n is an integer between 0 and 5, preferably 0. Preferably, the aldehyde is selected from the group consisting of formaldehyde, glyoxylic acid, and propionaldehyde.

[0056] According to one example, during pretreatment by aldehyde-assisted fractionation, the first composition comprises an organic solvent. The organic solvent may, for example, be an alcohol selected from alcohols having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, isopropanol, butanol, and polyethylene glycol, cyclic ethers, such as tetrahydrofuran, methyltetrahydrofuran, and dioxane; nitriles, such as acetonitrile; carboxylic acids, such as formic acid and acetic acid; carboxamides, such as dimethylformamide and dimethylacetamide; lactones, such as y-valerolactone, lactams, such as N-methyl-2-pyrrolidone and dimethyl sulfoxide. Preferably the organic solvent is an ether (such as dioxane), and more preferably an ether in a mixture in a proportion greater than or equal to 6% v / v with water.

[0057] After separation from the organic solvent, preferably by filtration, hemicellulose, and optionally the lignin (depending on whether it was precipitated or not), an optional drying step may be performed (see Figure 8). Prior to drying, the aldehyde treated cellulose is present as a highly viscous composition, whose moisture content is ideally reduced. Ideally, the dry content is controlled during

[0058] A24555WO / 13. 05. 2026 / filtration to achieve the targeted input dry content for the twin-screw extrusion, i.e., without drying in a vacuum oven or under temperature. According to one example, the pretreated cellulose is a solid composition comprising treated wood fragments.

[0059] Preferably, the composition comprising the aldehyde treated cellulose has a dry matter content of between 10% and 40% by weight, relative to the total weight of the composition. The cellulose microfibril composition obtained at the extruder outlet exhibits a high consistency, meaning it has a relatively high concentration of solid material and a thicker, more cohesive texture. This elevated consistency makes the suspension easier to handle during transport, as it is less prone to settling or phase separation, and reduces the risk of leakage or spillage. Additionally, the robust texture ensures that the suspension can be efficiently processed in subsequent industrial steps, such as shaping, coating, or forming into composite materials. Typically, the cellulose microfibril suspension obtained may have a cellulose proportion of between 10% and 40% by weight relative to the total weight of the suspension.

[0060] According to one example, during mechanical treatment by a twin-screw extruder, the aldehyde treated cellulose suspension passes through the twin-screw extruder a number N of times, N being an integer between one and ten, preferably between one and three. In synergy with the chemical pretreatment by aldehyde-assisted fractionation, the aldehyde treated cellulose- suspension is thus sufficiently weakened to reduce the number of passes through the twin-screw extruder and obtain the microfibril and cellulose suspension.

[0061] In one optional embodiment a further mechanical pretreatment step of the second composition takes place to form an aldehyde treated cellulose pulp. Said mechanical pretreatment step takes place after the chemical pretreatment b) and prior to mechanical treatment step d). Preferably, it takes place in a solution. In this optional step, the cellulose fibers are redispersed in water, enabling easy pumping and feeding into the extruder. This pretreatment step can also enhance the material’s fibrillation.

[0062] According to one example, before conducting the mechanical treatment in step d) the proportion of AAF cellulose by weight relative to the total weight of the composition has to be adjusted so as to obtain a cellulose proportion of between 10% and 40% by weight relative to the total weight of the suspension.

[0063] A24555WO / 13. 05. 2026 / It is known to form cellulose microfibrils (CMF), or nanofibrils, also known as cellulose nanofibrils (CNF) or cellulose nanofibers (NFC), or nanocellulose, from cellulose fibers, and in particular from cellulose fibers contained in wood pulp. Nanocellulose is a heterogeneous nanomaterial composed of micrometric elements, fragments of cellulose fibers, and at least 50% by number of nano-objects (i.e., objects with at least one dimension between 1 and 100 nanometers (nm). The nano objects of cellulose micro- or nanofibrils typically have a diameter between 5 and 70 nm and a length of 0.3 to 5 pm. It should be noted that, in the context of the present invention, the terms "microfibrillated cellulose" or "cellulose microfibrils" are used interchangeably to refer to nanocellulose.

[0064] Preferably, the cellulose microfibrils according to the present invention have a mean arithmetic length of 50 to 500 pm, preferably 100 to 250 pm and a mean arithmetic width of 1 to 30 pm, preferably 5 to 25 pm measured by optical microscopy using a MorFi laboratory analyser. The arithmetic mean is calculated by summing the measured values and dividing by the number of measurements for each parameter (length and width), wherein at least 100 individual microfibrils are measured for each parameter. The resulting mean values are reported as the mean arithmetic length and the mean arithmetic width of the cellulose microfibrils.

[0065] A further aspect of the present invention relates to cellulose microfibrils that can be obtained by the process according to the present invention. The cellulose mibrofibrils have a lignin content between 1 % and 40% by weight relative to the total dry weight of cellulose microfibrils, and characterized in that said lignin has p-O-4 content of 50% to 80%, preferably of 70% to 80%. The cellulose microfibrils according to the present invention comprise lignin that is preserved in a state that remains very close to its natural native structure, retaining a high p-O-4 linkage content and thereby maintaining the highly desirable inherent properties of natural lignin. As a result, the highly desirable inherent properties of natural lignin are largely retained, including its structural integrity, functional group richness, and favorable reactivity profile.

[0066] Preferably, the cellulose microfibrils according to the present invention have a lignin content between 5 and 30 % by weight relative to the total dry weight of cellulose microfibrils.

[0067] A24555WO / 13. 05. 2026 / The cellulose microfibrils according to the invention have an enhanced mechanical strength and durability. Preferably, the cellulose microfibrils display one or more of following characteristics, which further enhance their performance profile:

[0068] One such characteristic is the zeta potential, which reflects the surface charge of the cellulose microfibrils in a liquid medium and serves as an indicator of colloidal stability. Preferably, the zeta potential lies within a range from -18 to -20.

[0069] In addition, the cellulose microfibrils may exhibit a cationic demand representing the quantity of positively charged species required to neutralize the negatively charged sites present on the cellulose microfibrils surface. Typically, the cationic demand is in the range of 0 to 10.

[0070] The carbonyl content, expressed per anhydroglucose unit (AGU), may also be used to quantify the amount of carbonyl functional groups present along the cellulose chains. Preferably, the carbonyl content is more than 0.1 preferably more than 0.2.

[0071] Furthermore, the surface energy, which describes the energetic state of the cellulose microfibrils surface and encompasses interactions such as wettability, adhesion, and compatibility with other materials, is preferably below 50. The expression "A and / or B" means (A), (B), or (A and B). The expression "A, B, and / or C" means (A), (B), (C), (A and B), (A and C), (B and C), or (A, B, and C).

[0072] The word "bio-based" refers to materials of natural origin, and more specifically those that may be derived from plant-based biomass.

[0073] Unless explicitly stated otherwise, "% by mass" of a component refers to the mass percentage of that component relative to the total mass of a whole, for example a suspension or composition, or an object, such as a material or paper, containing that component.

[0074] A parameter "substantially equal to / greater than / less than" a given value means that this parameter is equal to / greater than / less than the given value, within plus or minus 10%, or even plus or minus 5%, of this value.

[0075] A "twin-screw extruder" is an extruder equipped with two co-penetrating or interpenetrating and corotating screws, typically mounted in parallel in a barrel. The extrusion process consists of continuously

[0076] A24555WO / 13. 05. 2026 / manufacturing finished or semi-finished products, or transforming materials, with-in a screw / barrel system. Single-screw extrusion refers to a single screw rotating within a cylindrical barrel, while twin-screw extrusion refers to two screws, usually parallel, rotating inside a barrel whose cross-section typically has the shape of an eight. There are two main families of twin-screw extruders: co-rotating extruders and counter-rotating extruders. In one particular example, the twin-screw extruder belongs to the family of co-rotating extruders, in which the screws rotate in the same direction. In the case of the present invention, the twin-screw extruder may more specifically comprise two intermeshing screws. This geometry de-fines quasi-independent "C" chambers on each screw and minimizes material exchange be-tween the different chambers.

[0077] The term "fibrillation segment" refers to a segment of a twin-screw extruder screw configured with mixing elements to continuously manufacture finished or semi-finished products, or to transform materials, within a screw / barrel system, by imposing shear forces on the material passing around this segment in the barrel.

[0078] A "conveying segment" is a segment of a twin-screw extruder screw configured with convey-ing elements to move the material through the barrel in a direction oriented from the inlet to the outlet of the twin-screw extruder.

[0079] A "direct screw pitch section or sub-section" refers to a section or sub-section of a fibrillation segment of a twin-screw extruder screw configured to favor the delivery of material transport-ed in the twin-screw extruder towards the outlet of the twin-screw extruder.

[0080] The term "reverse screw pitch portion or sub-segment" refers to a portion or sub-segment of a fibrillation segment of a screw of the twin-screw extruder configured to favor the delivery of material transported in the twin-screw extruder toward the inlet of the twin-screw extruder.

[0081] Each fibrillation segment, as well as each part or sub-segment of a fibrillation segment, may be composed of a plurality of elements, conveying elements or processing elements such as mixing discs, juxtaposed with each other along the longitudinal axis of the screw to which they belong. Among other things, the angular configuration of the discs relative to each other defines the shear rate induced on the material in transit within the segment, part of the segment, or sub-segment.

[0082] A24555WO / 13. 05. 2026 / The term "deformation" of the material in transit in the twin-screw extruder refers to a measurement consisting of multiplying the local shear rate of a disc or segment of the twin-screw extruder by the residence time of the material in that disc or segment.

[0083] The process for manufacturing the cellulose microfibril suspension 60 is now described according to several specific examples of implementation.

[0084] Figure 1 illustrates an example of the process for manufacturing the cellulose microfibril suspension 60. Variations of the process are also shown in dotted lines as examples.

[0085] The process comprises supplying a first composition 10 comprising lignocellulosic fibers. The lignocellulosic fibers comprise at least cellulose and lignin. The lignocellulosic fibers may further comprise hemicellulose. Equivalently, the term "lignocellulose" may be used to refer to lignocellulosic fibers.

[0086] In one example, the first composition 10 is derived from, and preferably is, a lignocellulosic biomass. The lignocellulosic biomass may be virgin lignocellulosic biomass, for example wood 1. The lignocellulosic biomass preferably comes from trees 1 such as birch, beech, poplar, cedar, Douglas fir, cypress, fir, juniper, kauri, larch, pine, hemlock, redwood, spruce, and yew. The preferred hardwood 1 is birch and / or beech as the primary lignocellulose-containing composition 10.

[0087] Lignocellulosic biomass may be derived from raw materials other than wood, such as plants such as hemp, wheat, bagasse, nut shells, apricot kernels, and / or flax.

[0088] It is preferable that the first composition 10 containing lignocellulose be solid at room temperature, for example between 20°C and 25°C. In one example, the first composition 10 containing lignocellulose is air-dried. For example, the first composition 10 containing lignocellulose is air-dried for storage in order to remove excess water.

[0089] The first composition 10 preferably comprises a proportion of less than or equal to 50% by weight, more preferably 30% by weight, in particular 0% to 20% by weight of water relative to the total weight of the first composition 10.

[0090] A24555WO / 13. 05. 2026 / In addition, the first composition 10 preferably has a lignin content of 1% to 40% by weight, more preferably 5% to 30% by weight, in particular 10% to 25% by weight relative to the total dry weight of the composition.

[0091] The following table illustrates, by way of example, the proportions of cellulose, hemicellulose, and lignin by weight (%wt) in a first composition 10 consisting of wood, pretreated cellulose 20 by aldehyde-assisted fractionation 2 (hereinafter referred to as AAF-cellulose), and in a sample of standard commercial cellulose.

[0092] Table 1:

[0093] Sample Cellulose (%wt) Hemicellulose (%wt) Lignin (%wt) Beech wood 47.7 19.4 29

[0094] AAF Cellulose example 62.4 10.2 19

[0095] 1 (after the AAF process

[0096] once filtered and dried)

[0097] AAF Cellulose example 61.0 5.92 12.7

[0098] 2 (after the AAF process

[0099] once filtered and dried)

[0100] Standard commercial 71-76 17-25 3

[0101]

[0102] cellulose

[0103] Lignin can be determined as Klason lignin. To determine Klason lignin, the Klason lignin test can be applied. To do this, wood particles (0.25 to 0.50 g) are loaded into 50 mL beakers with the addition of 7.5 mL of a 72% mass solution of H2SO4 solution relative to the total mass of the solution. The mixture is left at room temperature for 2 hours and stirred with a glass rod every 10 minutes.

[0104] The suspension is then transferred to a round-bottom flask and 290 mL of water is added to achieve a mass concentration of H2SO4 of 3%. The glass bottle is sealed with a screw cap and sterilized at 120°C for 1 hour in an autoclave. The resulting solution is filtered and the precipitate is washed with water, dried at 105°C, and weighed to determine the mass of Klason lignin.

[0105] The Klason lignin content can be determined using the following equation:

[0106] KL * 100

[0107] Klason lignin content [%] = — — — —

[0108]

[0109] A24555WO / 13. 05. 2026 / Where:

[0110] - KL is the mass of Klason lignin (in g),

[0111] - LCC is the mass of the lignocellulosic sample (in g).

[0112] According to one example, the first composition 10 is provided in a fractionated form, for example in the form of particles, such as chips, flakes, pellets, balls, splinters, granules, splinters, dust, and fragments. For example, trees 1 can be cut and sawn to obtain these particles. In addition, to obtain a smaller and more homogeneous particle size, the particles can preferably be crushed and then sieved.

[0113] The first composition 10 may be an "organosolv" pulp produced by a chemical process for treating biomass in one or more organic solvents, rather than aqueous solvents as is usually the case in conventional wood treatments.

[0114] The first composition 10 is subjected to an aldehyde-assisted fractionation pretreatment 2, also referred to by the acronym AAF. The AAF 2 pretreatment comprises the reaction of the first composition 10, preferably in an organic solvent, and in the presence of an aldehyde and an acid catalyst.

[0115] The AAF 2 pretreatment uses an aldehyde which, in the presence of an organic solvent and in the presence of the acid catalyst, acts as a stabilizing agent for the at least partial deconstruction (or fractionation) of the complex structures of the lignocellulosic fibers.

[0116] The bonds in the first composition 10 between the lignin fraction and the cellulose or hemicellulose fractions are at least partially cleaved. In addition, the bonds within the lignin are also cleaved. It is therefore understood that the lignocellulosic fibers are weakened, which allows subsequent fibrillation by mechanical treatment 6 in a twin-screw extruder 62.

[0117] The organic solvent may comprise a single organic solvent or a mixture of organic solvents. It is further preferable that the organic solvent has a boiling point of 60°C to 250°C, preferably at 1013 mbar. Furthermore, the boiling point is not linked to a single temperature but may also refer to a temperature range, for example when a mixture of organic solvents is used.

[0118] A24555WO / 13. 05. 2026 / The organic solvent may, for example, be an alcohol selected from alcohols having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, isopropanol, butanol, and polyethylene glycol, cyclic ethers, such as tetrahydrofuran, methyltetrahydrofuran, and dioxane; nitriles, such as acetonitrile; carboxylic acids, such as formic acid and acetic acid; carboxamides, such as dimethylformamide and dimethylacetamide; lactones, such as y-valerolactone, lactams, such as N-methyl-2-pyrrolidone and dimethyl sulfoxide. Preferred alcohols are alcohols such as methanol and ethanol, cyclic ethers such as tetrahydrofuran, methyltetrahydrofuran, and dioxane, and lactones such as y-valerolactone. Methyltetrahydrofuran and tetrahydrofuran, in particular methyltetrahydrofuran, are particularly preferred.

[0119] According to one example, the organic solvent may be mixed with water. It is preferable that the organic solvent be mixed with less than 50% by volume of water relative to the total volume of organic solvent(s) and water, preferably less than 30% by volume of water, in particular 0 to 10% by volume of water.

[0120] The use of an acidic compound prevents the swelling of lignocellulosic fibers and thus the formation of a cellulose pulp, as is usually the case under basic conditions. To obtain acidic conditions, one or more acidic compounds are added to the first composition 10, and preferably the first composition with the organic solvent. In AAF pretreatment, the acidic compound acts as a catalyst. It is therefore referred to as an "acid catalyst."

[0121] When added to water, an acidic compound lowers the pH value to below 7. Examples of acidic compounds are organic carboxylic acids, such as acetic acid, and mineral acids, with mineral acids being preferred. Mineral acids are considered to be acids that do not contain carbon atoms. Examples of mineral acids are hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, phosphoric acid, boric acid, and silicic acid. Hydrochloric, sulfuric, and phosphoric acids are preferred, and sulfuric acid in particular.

[0122] Preferably, the aldehyde is an aldehyde according to the formula R-CHO; wherein R is selected from the group consisting of hydrogen, a linear or branched aliphatic chain comprising one to six carbon atoms and (CH2)nCOOH, wherein is an integer between 0 and 5, and wherein the aldehyde is

[0123] A24555WO / 13. 05. 2026 / preferably selected from the group consisting of formaldehyde, glyoxylic acid, and propionaldehyde. These aldehydes are commercially available.

[0124] The reaction mixture formed by the first composition 10, the organic solvent, the acid catalyst, and the aldehyde may preferably be subjected to mechanical agitation, such as stirring.

[0125] During pretreatment AAF 2, the reaction medium may be maintained and preferably heated to a temperature between substantially 35°C and 140°C, preferably between 40°C and 130°C, in particular between 50°C and 120°C. It is particularly preferable to apply a temperature of substantially between 70°C and 100°C, in particular substantially equal to 80°C. Pretreatment AAF 2 does not require high temperatures to degrade the lignocellulosic fibers, which reduces the environmental footprint of the process.

[0126] According to one example, the AAF 2 pretreatment can be carried out over a period of substantially between 0.5 hours and 12 hours, preferably between 0.75 hours and 10 hours, more preferably between 1 hour and 8 hours, in particular between 1.5 hours and 5.5 hours. The reduced time makes the manufacturing process more compatible with industrial manufacturing constraints. The environmental footprint is further reduced by the decrease in pretreatment time compared to conventional solutions.

[0127] At the end of the AAF 2 pretreatment, the second composition 20 is obtained, as illustrated, for example, in Figure 1. The aldehyde-protected lignin is present in the solution, while the aldehyde treated cellulose is present as a solid. The aldehyde-treated cellulose can now be separated from the aldehyde-protected lignin by filtration, or the lignin can be deposited onto the cellulose by drying or precipitation. The aldehyde treated cellulose in the second composition 20 may have a wood-like structure, which therefore does not resemble the consistency of traditional cellulose pulps. The second composition may be in a fractionated form, for example in the form of particles, of AAF cellulose, as described above in relation to the first composition 10. This can be done by filtration to remove the organic solvent and dissolved AAF lignin and hemicellulose, or if a precipitation took place, to remove the organic solvent and hemicellulose. Typically, the filtration comprises two steps, namely a washing step with MeTHF and subsequent filtration and a washing step with water and subsequent filtration. Then drying, for example by air or by heating, can be performed but is not required.

[0128] A24555WO / 13. 05. 2026 / Compared to traditional cellulose pulps, AAF-cellulose 20, also known as pretreated cellulose or as aldehyde treated cellulose, may have a higher lignin content than commercial Kraft pulps (see, for example, Table 1 above). As lignin confers interesting properties, particularly in terms of hydrophobicity and barrier properties, pretreatment with AAF 2 allows the various constituents of the lignocellulosic fibers to be better preserved for subsequent fibrillation.

[0129] AAF-cellulose 20 obtained after filtration and / or drying is preferably suspended to form a pretreated cellulose 30, as illustrated, for example, in Figure 1. However, it is also possible to conduct this step in the extruder. In this case, filtered, but not dried AAF-cellulose 20 is added into the extruder and water is added to adjust to right solid content in-situ of fibrillation.

[0130] AAF-cellulose 20 can optionally be suspended in a solvent, preferably water. The proportion of AAF-cellulose 20 in the suspension may be less than or equal to 5% by weight relative to the total weight of the suspension. However, this step can also be omitted, for example if the AAF- cellulose is not dried after the AAF process and is directly fed into the extruder in a first pass in which adjustment of solid content can be performed as well as a first slight fibrillation.

[0131] When forming this composition 30, the AAF-cellulose 20 may be subjected to mechanical treatment 3 prior to its passage through the twin-screw extruder 62. This suspension may be mechanically pretreated 3 by conventional mechanical means such as a homogenizer, a ball mill, or other mechanical treatments.

[0132] The mechanical pretreatment 3 is preferably configured to achieve at least partial fibrillation of the pretreated cellulose 20. Preferably, the mechanical treatment 3 is carried out until 80° Shopper Riegler is reached, according to ISO 5267-1. The Shopper Riegler degree is a measure of a sample's ability to retain water, which is an indicator of the sample's degree of refinement. Conventional paper typically has a Shopper Riegler degree of between 15 and 30.

[0133] The process may include adjusting 4 the proportion of cellulose in the pulp obtained. This adjustment is specifically intended to increase the proportion of cellulose in the pretreated cellulose composition 30 in order to facilitate fibrillation 6 in the twin-screw extruder 62 and obtain a cellulose microfibril composition 60 with a higher consistency.

[0134] A24555WO / 13. 05. 2026 / The adjustment 4 of the proportion of cellulose may be configured so that the pretreated cellulose composition 30 has a dry matter proportion of between 10% and 50%, preferably between 10% and 40%, or even between 10% and 30%, or even between 10% and 20%, and even more preferably substantially equal to 20%, relative to the total mass of the suspension.

[0135] To this end, and according to one example, the pulp obtained after mechanical pretreatment 3 may be dried and / or centrifuged or diluted to achieve the desired consistency.

[0136] Mechanical treatment 6 is carried out by introducing the pretreated cellulose composition 30 into a twin-screw extruder 62. As illustrated, for example, in Figure 1, the pretreated cellulose composition 30 may be subjected to several passes 6a through the twin-screw extruder 62, typically between one and ten passes, and preferably between one and five passes.

[0137] With reference to Figures 2 and 3, each screw 61 of the twin-screw extruder 62 comprises at least two fibrillation segments 611, 612, 613, and preferably less than nine, or even six fibrillation segments. The mechanical treatment 6 may be carried out under controlled temperature conditions, for example using a water cooling circuit. More specifically, water circulation channels may be provided in the extruder barrel. Thus, the twin-screw extruder may be maintained at a temperature substantially less than or equal to 60°C, preferably between 0°C and 20°C, for example substantially equal to 10°C.

[0138] In addition, mechanical treatment 6 by twin-screw extruder 62 is carried out at a screw rotation speed of between 100 rpm and 500 rpm, for example substantially equal to 400 rpm. The use of a twin-screw extruder 62 with the pretreated cellulose 30 allows for a reduction in energy consumption for the production of cellulose microfibrils 60. This energy consumption can typically be between 5% and 70%, more particularly between 10% and 60%, compared to the mechanical treatments of conventional industrial processes.

[0139] Furthermore, although twin-screw extruders 62 allow and are generally used to mix the material in transit with at least one reagent injected through the barrel, mechanical treatment 6 is preferably advantageously free of any addition of chemical agents.

[0140] Preferably, in order to maintain the proportion obtained in the AAF cellulose, the process does not include any delignification treatment prior to mechanical treatment 6 in the twin-screw extruder 62. It

[0141] A24555WO / 13. 05. 2026 / is therefore understood that the proportion of lignin relative to the total dry mass can be substantially maintained between the AAF cellulose and the cellulose microfibril suspension 60 obtained at the end of treatment 6 in the twin-screw extruder 62.

[0142] Alternatively, the process may include a delignification treatment 5 configured to reduce the lignin content of the pretreated cellulose composition 30, preferably prior to its introduction into the twin-screw extruder 62. The delignification treatment may be at least one treatment selected from a kinematic treatment, a treatment with an oxidizing agent, for example ozone.

[0143] As indicated above, the pretreated cellulose composition 30 may have the aforementioned dry matter content. It is this composition with a controlled dry matter content by mass that can be fed into the twin-screw extruder 62. For these proportions, the passage of the material through the twin-screw extruder 62, from its inlet to its outlet, is satisfactory, in particular in that it causes only slight overheating of the material in transit and in that it presents no risk, or at least a limited risk, of the material becoming blocked. This produces a composition of cellulose microfibrils 60 at the outlet of the twin-screw extruder 62 with a dry matter content equivalent to, and more particularly substantially equal to, the concentration of the pretreated cellulose composition 30 introduced into the twin-screw extruder 62. At these concentrations, it appears that the process according to the invention has undeniable advantages in terms of production costs, storage costs, transport costs, and applications, and appears to be a good alternative for the industrialization of cellulose microfibril production.

[0144] In one example, each screw 61 of the extruder 62 comprises between 3 and 8, preferably 6, fibrillation segments. Figure 2 shows the two screws 61 of the twin-screw extruder 62 interpenetrating each other. The two screws are preferably at least complementary to each other, and for example identical to each other. For the sake of simplicity, only three fibrillation segments are shown in the figures for each screw 61.

[0145] As shown in Figures 2 and 3, the fibrillation segments 611 , 612, 613 are preferably different from each other. More specifically, they have different shear rates and cumulative deformations. For example, the shear rates may differ from one another by a factor greater than or equal to two. Alternatively, the fibrillation segments may be identical to one another.

[0146] A24555WO / 13. 05. 2026 / In addition, each fibrillation segment 611, 612, 613 may comprise a direct screw pitch sub-segment, followed by a reverse screw pitch sub-segment, arranged relative to each other upstream and downstream of the twin-screw extruder, so as to retain the material passing through the extruder at the fibrillation segment. The transit time of the material at each fibrillation segment is thus advantageously increased, for better fibrillation of the pretreated cellulose at the outlet of said segment.

[0147] The configuration of each screw, as illustrated for example in Figures 2 and 3, shows that the three fibrillation segments are different from each other. More specifically, with reference to Figures 4A to 4C:

[0148] the first fibrillation segment 611 may comprise a first sub-segment 611a comprising ten identical discs arranged successively so that two adjacent discs have an angular offset of substantially 30°. This first sub-segment 611a may be supplemented by a second sub-segment 611b comprising three additional discs, arranged so as to also have an angular offset of substantially 30° between each pair, but so as to generate a reverse screw pitch with respect to the direct screw pitch generated by the first sub-segment 611 a.

[0149] the second fibrillation segment 612 may comprise two sub-segments comprising a total of fifteen discs. The first sub-segment 612a comprises the first seven discs arranged in a direct screw pitch with an angular offset of substantially 30° between each pair, and the four intermediate discs arranged in a direct screw pitch with an angular offset of substantially 60° between each pair. The second sub-segment 612b comprises the last four discs arranged in reverse screw pitch with an angular offset of substantially 60° between each pair;

[0150] the third fibrillation segment 613 may comprise two sub-segments comprising a total of twenty discs. The first sub-segment 613a comprises the first four discs arranged in a direct screw pitch with an angular offset of substantially 60° between each pair, and the twelve intermediate discs arranged in a direct screw pitch with an angular offset of substantially 90° between each pair. The second sub-segment 613b comprises the last four discs arranged in reverse screw pitch with an angular offset of substantially 60° between each pair.

[0151] As shown in Figures 2 and 3, each fibrillation segment may comprise a conveyor segment 614, 615, 616, 617 on either side. The conveyor segments are configured to convey the material passing through the twin-screw extruder 62 respectively from the extruder inlet to the first fibrillation segment, from the

[0152] A24555WO / 13. 05. 2026 / first fibrillation segment to the second fibrillation segment, from the second fibrillation segment to the third fibrillation segment, and from the third fibrillation segment to the outlet of the twin-screw extruder. Each conveyor segment may, for example, be configured in the manner of a worm screw. In addition, each conveyor segment can be configured to induce, on the material in transit in the twin-screw extruder 62, a deformation that is substantially ten times less than the deformation induced by a fibrillation segment.

[0153] A nanopaper 70 can then be manufactured from the cellulose microfibrils 60, for example by filtration 7.

[0154] Specific examples

[0155] 20 kg of biomass (beech wood, approximately 5% moisture content) were added to a 250 L reactor equipped with a mechanical stirrer. 71.4 kg of solvent (2-methyltetrahydrofuran), 35.7 kg of stabilizing aldehyde (50% glyoxylic acid by mass in H2O) were added, as well as 5.1 kg of acid (96% H2SO4). The reactor was then heated to 90°C and stirred for 3 hours under reflux. The mixture was then cooled to room temperature and 7 kg of base (NaOH 30% by mass in H2O) was added for neutralization. The mixture was filtered to isolate the solid cellulose and a lignin liquor. The reactor and the substances retained by the filter were washed with 2-methyltetrahydrofuran (10 L) and a second time with water (20 L). The cellulose was left to dry at room temperature.

[0156] The cellulose obtained by AAF 2 pretreatment was refined 3 using a Valley beater at a concentration of 2% by mass in the presence of a non-foaming agent until 80° Shopper Riegler was reached, according to ISO 5267-1.

[0157] Figure 5 illustrates the time taken to reach 80° Shopper Riegler for AAF cellulose, compared with an unbleached, untreated softwood (USW) and hardwood (UHW) composition. This time, approximately 45 minutes for AAF cellulose, is significantly reduced, clearly indicating a weakening of the lignocellulosic fibers by AAF 2 pretreatment.

[0158] The table below summarizes the time and energy consumption during refining prior to extrusion for these samples.

[0159] Table 1:

[0160] A24555WO / 13. 05. 2026 / AAF cellulose UHW USW Time (in min) 45 59 110

[0161] Energy consumption (in 921.0 977.6 1799.6

[0162]

[0163] kWh / t)

[0164] The refined pulp was drained overnight on a 1 pm sieve, then centrifuged at 2800 rpm until a composition comprising pretreated cellulose 30 with a consistency of approximately 17-20% by weight of dry matter in water was obtained.

[0165] The refined AAF-cellulose 30 was fed into the HAAKE Rheomex OS (Thermo Scientific) twin-screw extruder 62 for fibrillation with one to five repeated passes through the twin-screw extruder 62 at . The screw speed 61 was 400 rpm. The screws used were Rheomex PTW with dimensions D: 16 mm and L / D: 40. No die was used at the end of the rheometer.

[0166] Screws 61 comprise a combination of fibrillation segments and fully oriented conveying segments. The six fibrillation segments are composed as shown in the table below.

[0167] Table 3:

[0168] Zone 1 2 3 4 5 6 Fibrillation Seven discs Nine discs Eleven discs Nine discs Nine discs Seven discs segment separated by separated by separated by separated by separated separated 0 = 30° 0 = 90° 0 = -30° 0 = -30° by 0 = -30° by 0 = -60°

[0169]

[0170] The temperature is regulated at 10°C by a cooling system to prevent overheating in the 62 twin-screw extruder. A feeder (Thermo Scientific, PolyLab OS 567-4002) was placed above the inlet of the twin-screw extruder 62 and was used to introduce the pretreated cellulose composition 30. The feed rate was 15% for the first pass and 20% for passes 2 to 5. A graph of torque versus time for the different passes is shown in Figure 6.

[0171] An alternative procedure was applied in which the AAF cellulose 20 was not dried after filtration but kept as a composition with solid content between 30-70 wt%, preferably between 50-60 wt%. The composition was directly fed into the twin screw extruder 62 and addition of water was done in the process to adjust to the desired dry content, between 10-40 wt%. An additional pass through the

[0172] A24555WO / 13. 05. 2026 / extruder has to be performed in this case, to ensure homogenisation of the material and the correct dry content.

[0173] An alternative procedure was applied with enzymatic pretreatment after refining the AAF cellulose, i.e., after the cellulose had been extracted from the wood by AAF pretreatment and refined, but before centrifugation and fibrillation in extruder 62. All other steps are identical to those described above. To do this, enzymatic hydrolysis at a mass content of 2% was carried out in a reaction flask under mechanical stir-ring at 350 rpm. A temperature of 50°C was set using an oil bath, and a stable pH of 5.0 was achieved with an acetate buffer composed of acetic acid and sodium acetate trihydrate. The enzyme solution (FiberCare R cellulase with an activity of 4770 ECU.g-1) at an enzyme concentration of 300 ECU.g-1of cellulose (6.29 *10-2g of enzyme solution / g of cellulose) was then poured into the reactor . After 2 hours of reaction, the enzymatic hydrolysis was stopped by increasing the temperature to 85°C and maintaining it at this temperature for 15 minutes before cooling. After the temperature had dropped, the pulp was filtered using a 1 pm nylon sieve. It was also washed with 30 liters of deionized water to remove the salts and sugars produced during the reaction.

[0174] It should be noted that hardwood fibers obtained by the Kraft process and bleached were used for a twin-screw extrusion test without any other chemical or biochemical (e.g., enzymatic) pretreatment. The pulp was first refined using a Valley beater as described above, but it took 60 minutes to achieve the correct Shopper Riegler degree (see Figure 5).

[0175] The materials obtained were then drained and centrifuged to achieve a consistency of 17-20% by mass in water of the total mass of the composition. The material was then fed into the twin-screw extruder under the same conditions as AAF cellulose, but the extruder quickly stopped due to excessive torque on the screw caused by the fiber winding around the screw in the shear zones (see UKP Figure 6). It was therefore impossible to produce LMFC with traditional hardwood cellulose using this process and these conditions.

[0176] Softwood fibers obtained by the Kraft process and bleached were used for LMFC production by twin-screw extrusion without any other pretreatment (e.g., enzymatic). The pulp was refined using a Valley beater as described above, but it took 110 minutes to reach the correct Shopper Riegler degree (see Figure 5).

[0177] The materials obtained were then drained and centrifuged to achieve a consistency of 17-20% by weight in water relative to the total mass of the composition. The material was then fed into the twin-

[0178] A24555WO / 13. 05. 2026 / screw extruder under exactly the same conditions as the AAF cellulose, but the extruder quickly stopped for the same reason that the hardwood material did not work.

[0179] For some of the properties, nanopapers were made from the MFCs, which were prepared by filtration using a Rapid Kothen sheet former. Suspensions at 0.5% by weight relative to the total weight of the suspension were prepared by diluting 2 g of MFC in 400 ml of deionized water and homogenized with an Ultra Turrax T-25 dis-perser at 8000 rpm for 2 minutes. The suspension was then filtered under a controlled vacuum of -500 mbar and the sheet former was equipped with an additional nylon screen with a mesh size of 1 pm. Once the water had been completely re-moved, the MFC sheets were dried between two nylon screens and hard paper un-der vacuum at 85°C for 20 minutes. Four nanopapers were prepared for each sample.

[0180] The lignified cellulose microfibrils (LMFC) were then analyzed according to various parameters that reflect their quality, morphology, physical properties, and barrier properties (see table below).

[0181] The final composition of LMFCs is determined using a composition analysis protocol described in Sluiter A., Hames B., Ruiz R., et al. Determination of Structural Carbohydrates and Lignin in Biomass Laboratory Analytical Procedure (LAP), 7 / 17 / 2005.; 2008. The cellulose, hemicellulose, lignin, and ash content was determined using this protocol. The cellulose, hemicellulose, and lignin content remained essentially unchanged from the initial AAF cellulose content, with the lignin content ranging from approximately 14% to 19%.

[0182] A comparison of LMFCs with commercial cellulose microfibrils (MFCs) was performed using the quality index ( determination described in Desmaisons, et al.. A new quality index for benchmarking of different cellulose nanofibrils. Carbohydrate Polymers, 174, 318-329, 2017 ), which combines several essential measurements for MFCs and provides a single figure for comparison.

[0183] LMFCs have a quality index of 61, which is comparable to other MFCs studied in the literature (index typically between 60 and 65), or MFCs prepared in-house using ultra-fine grinding processes (whose index is approximately equal to 70).

[0184] Table 4

[0185]

[0186] Composition Analysis technique Value Protocol

[0187] A24555WO / 13. 05. 2026 / Crystallinity index (%) X-ray diffraction (XRD) 80.0 Measurements were performed on dry, unbleached, and bleached AAF cellulose, and X-ray diffraction patterns were obtained using an X'Pert Pro MPD diffractometer (PANalytical, Netherlands) equipped with a Bragg-Brentano geometry. A copper anode (Ko, A = 1.5419 A) was used, with an angle of 20. The crystallinity index (Cl) of the samples was determined using the amorphous subtraction method. The area under the curve of an amorphous standard was subtracted from the area of the sample, and this difference was divided by the area of the sample. The amorphous sample used in this work was cryogenically ground bleached birch cellulose pulp for twenty minutes using a Cryomill (Retsch) apparatus.

[0188] Cellulose content (%) Sugar analysis (HPLC- 70-75 Protocol described in Sluiter A., Hames B., Ruiz PAD) R., et al. Determination of Structural Carbohydrates and Lignin in Biomass Laboratory Analytical Procedure (LAP), 7 / 17 / 2005.; 2008.

[0189] Lignin content (%) Acid-insoluble lignin 14 Protocol described in Sluiter A., Hames B., Ruiz (AIL) R., et al. Determination of Structural Carbohydrates and Lignin in Biomass Laboratory Analytical Procedure (LAP), 7 / 17 / 2005.; 2008.

[0190] Salts (%) Composition analysis < Protocol described in Sluiter A., Hames B., Ruiz R., et al. Determination of Structural Carbohydrates and Lignin in Biomass Laboratory Analytical Procedure (LAP), 7 / 17 / 2005.; 2008.

[0191] Turbidity (NTU) AL-250 turbidimeter 365 ± Samples were diluted to 0.1 % by mass with 5 deionized water (2 g of dry pulp or MFC material in 400 mL of water) and homogenized with an Ultra Turrax T-25 blender at 8000 rpm (initial materials: 2 minutes, MFCs produced by TSE: 2 minutes, MFCs produced by ultrafine grinding: 40 seconds). Turbidity values in nephelometric turbidity units (NTU) were measured using an AL-250 turbidimeter (Aqualytic, Germany). The test measures the light scattered at 90° from incident light (A = 860 nm), which is related to the size and shape of the cellulosic fiber elements in the suspension. At least 14 measurements were taken for each sample and the

[0192]

[0193] average value was calculated.

[0194] A24555WO / 13. 05. 2026 / Young's modulus Instron (NF Q03- 004 5.6 ± The tensile properties of the nanopapers were (GPa) standard) on nanopaper 0.3 measured using a 5965 double-column testing system with a maximum force of 50 kN (Instron, USA), in accordance with standard NF Q03- 004. The tests were carried out at a deformation speed of 10 mm / min and with a gauge length of 10 mm. The samples were in the form of strips 15 mm wide and 100 mm long. Three nanopapers were analyzed for each sample and four measurements were taken for each of them, and the average was calculated. The measurements were carried out in an air- conditioned room (23°C and 50% relative humidity).

[0195] Nanometric fraction Gravimetric method 53.4 The samples were diluted to 0.02% by mass (%) (Naderi et al., 2015) ± 0.5 with deionized water (0.12 g of dry MFC material in 600 mL of water) and homogenized with an Ultra Turrax T-25 grinder at 5000 rpm for 5 minutes. The mass of 80 mL of the suspension was determined before and after centrifugation, which was performed at 1000 g, 4 °C for 15 minutes. Two measurements were taken for each sample and the average value was calculated.

[0196] Average particle size Optical microscopy (x10 18.1 The optical microscopy images were obtained (pm? ) magnification, see ± 2.5 using an Axio Imager M1 microscope (Carl Figures 7A and 7B Zeiss, Germany) equipped with an AxioCam respectively t without MRc 5 digital camera. The suspensions were and with enzymatic diluted to 0.1% by mass and homogenized at treatment prior to 8000 rpm ( ) using an Ultra-Turrax T-25 fibrillation) homogenizer (initial materials: 2 minutes, MFC produced by TSE: 2 minutes). The slide was prepared by adding a drop of the diluted suspension. Magnifications of 50x and 100x were used. At least 10 images were taken at 10x magnification and the most representative ones were selected.

[0197] QI (Quality index) J. Desmaisons et al, The QI is a combination of numerous 2017 measurements, as described in J; Desmaisons et al., 2017

[0198] pH pH meter 7

[0199] Oxygen transmission Oxtran, 23°C 0% 1.01 OTR in a desiccator with silica gel at 23°C ± rate (OTR, in cm3relative humidity; on 1 °C, 0% RH for at least 24 hours prior to / (m2.day) nanopaper analysis.

[0200] Procedure according to ASTM F1927-14 Sample preparation

[0201] 1. 2. Cut a 4.5 x 4.5 cm sample from the circle

[0202]

[0203] of materials.

[0204] A24555WO / 13. 05. 2026 / Place the square between two aluminum adhesive masks to reduce the exchange surface area (5 cm2).

[0205] 3. Place the masked sample in Oxtran for analysis.

[0206] 4.2. Test conditions

[0207] Conditioning time: 24 hours

[0208] Individual zero: yes

[0209] Mode: standard; 40 cycles of 40 min Carrier gas: Nitrogen (98%), Hydrogen (2%) / Flow rate: N2: 10 mL / min

[0210] Test gas: Oxygen (10%) / Flow rate: O2: 20 mL / min

[0211] Climate conditions: 23°C±1°C / 0 ± 3% RH Number of series: 4

[0212] Number of samples / series: 1

[0213] 4.3. Equipment

[0214] Mocon OX-TRAN ML2 / 21; MH 2 / 20 and SH 2 / 20

[0215] Measurement range: 0.05 to 200 crn7(m2'day) Resolution: 0.01 cm3 / (m2'day)

[0216] Water vapor Permatran, 23°C, 50% 289 WVTR in laboratory at 23°C ± 1°C, 50% r.h. ± transmission rate relative humidity; on 5% r.h. for at least 24 hours prior to analysis (WVTR, in g / (m2'day)) nanopaper Operating mode according to the PERMATRAN W 3 / 33 user manual Sample preparation

[0217] 1. 2. Cut a 4.5 x 4.5 cm sample from the circle of material.

[0218] Place the square between two adhesive aluminum masks to reduce the exchange surface (5cm2).

[0219] 3. Insert the masked sample into the Permatran for analysis.

[0220] 5.2. Test conditions

[0221] No zero individual

[0222] Conditioning time: No

[0223] Test mode: continuous, 30-minute cycle Carrier gas: Dry nitrogen (100%) / Flow rate: N2: 100 mL / min

[0224] Climatic conditions: 323°C ± 1°C / 50 ± 3% RH

[0225] Number of series: 4

[0226] Number of samples / series: 1

[0227] 5.3. Equipment

[0228] MOCON PERMATRAN 3 / 33

[0229] Range for an exchange surface area of 50cm2:

[0230]

[0231] 0.035 to 120 g / (m7day)

[0232] A24555WO / 13. 05. 2026 / Table 5

[0233] Sample Contact angle; t = 0 Contact angle; References

[0234] min (in %) t = 2 min (in %)

[0235] MFC1: Bleached 39.1±2.5 Booregard Exilva, from Poothanari, M. A., & MFC, non- Leterrier, Y. (2024). Fluorine Free Surface fibrillated, using Modification of Microfibrillated Cellulose- twin-screw Clay Composite Films: Effect of extruder Hydrophobicity on Gas Barrier Performance.

[0236] Surfaces, 7(2), 283-295.

[0237] MFC2: Bleached n. n. Bleached birch fibers, purchased from Sbdra non-fibrillated (Sweden). Conventional fibrillation.

[0238] MFC produced by Highly hydrophilic: water absorbed directly twin-screw

[0239] extruder

[0240] ENZ-TSE-5P n. n. Commercially bleached birch fibers - water is absorbed directly and distributed over the surface.

[0241] LMFC - derived 64.7 LMFC derived from unbleached softwood and from softwood and hardwood, respectively, produced by Kraft non-fibrillated by pulping using ultra-fine grinding.

[0242] twin-screw

[0243] extruder

[0244] LMFC -made from 67.5 Li, H. et al., (2024). A comparative study of hardwood and lignin-containing microfibrillated cellulose non-fibrillated by fibers produced from softwood and hardwood twin-screw pulps. Cellulose, 31(2), 907-926. extruder

[0245] LMFC derived 69 ±0.07 76±0.07

[0246] from AAF

[0247] cellulose and

[0248] fibrillated by 5

[0249] passes through a

[0250] twin-screw

[0251] extruder, without

[0252] enzymatic

[0253] treatment

[0254] LMFC derived 54.2 ±0.5 n.m.

[0255] from cellulose

[0256] AAF and fibrillated

[0257] by 5 passes

[0258] through a twin- screw extruder,

[0259] with enzymatic

[0260] treatment prior to

[0261]

[0262] extrusion

[0263] A24555WO / 13. 05. 2026 / The contact angle was measured using a Kriiss Scientific DSA30 drop shape analyzer (Germany) with an integrated camera and opposite-side illumination in sessile drop mode. The samples were placed on the movable support. The drops were deposited using a 1 mL syringe filled with ultrapure water, and ADVANCE drop analysis software version 1.6.2.0 (Kriiss Scientific, Germany) was used to analyze the contact angles. The angles were measured using the same software five times during the deposition inter t one-second intervals and five more times after two minutes. Triplicates were performed each time.

[0264] The contact angles were measured on nanopapers. An increase in the contact angle can thus be observed between LMFCs and MFCs. The hydrophobic properties are further improved (as a larger contact angle is observed) for LMFCs obtained according to an example of implementation (with AAF pretreatment and twin-screw extrusion).

[0265] The table below shows the energy consumption associated with the fibrillation step. TSE-nP indicates n passes through the twin-screw extruder for MFCs produced by fibrillation in a twin-screw extruder.

[0266] Table 6

[0267] Starting material Pre-treatment Fibrillation Specific Reference

[0268] energy

[0269] consumption

[0270] (MWh / t)

[0271] Unbleached - TSE-4P 11.7 - cellulose AAF

[0272] AAF unbleached Enzymatic TSE-4P 13.8 - cellulose hydrolysis

[0273] Bleached birch Enzymatic TSE-4P 26.6 Banvillet, G., et al., kraft pulp hydrolysis (2021). Alkaline treatment combined with enzymatic hydrolysis for efficient cellulose nanofibrils production. Carbohydrate Polymers, 255, 117383.

[0274] Bleached birch NaOH 10 wt% TSE-4P+enzymes 14.3 Banvillet, G., et al., kraft pulp (2021). Alkaline treatment combined with enzymatic hydrolysis for efficient cellulose

[0275]

[0276] nanofibrils production.

[0277] A24555WO / 13. 05. 2026 / Carbohydrate Polymers,

[0278]

[0279] 255, 117383.

[0280] Characterization

[0281] A) Characterization of AAF cellulose

[0282] AAF cellulose was characterized using a set of physicochemical parameters to describe their surface charge and chemical functionality.

[0283] The zeta potential reflects the surface charge of the micronized nanofibrils in a liquid medium and is an important indicator of colloidal stability. The zeta potential of the fibers was determined using a SPZ 06.

[0284] The cationic demand represents the amount of positively charged species required to neutralize the negatively charged sites on the fiber surface. This parameter is determined by polyelectrolyte titration, where a cationic polymer is added and the endpoint is detected using streaming current or particle charge measurements.

[0285] The carbonyl content (expressed per anhydroglucose unit, AGU) quantifies the amount of carbonyl functional groups present on the cellulose chains. It can be measured using chemical titration methods, such as hydroxylamine hydrochloride titration (Hofreiter method).

[0286] The surface energy describes the energetic state of the fiber surface and includes interactions such as wetting, adhesion, and compatibility with other materials. It can be determined using contact angle measurements on Infra Reg pad made with micronized material using digidrop (GBX) equipment. Two solvents were used, drop of 4 l for water or 6 pl for ethanol onto the recto side.

[0287] Characteristics AAF cellulose fibres Cellulose fibres (Kraft fibres)

[0288] (Present invention) (Comparative example) Zeta potential in mV -19.6 -20 to -30

[0289]

[0290] Cationic demand in peg / g 3.9 20 to 30

[0291] A24555WO / 13. 05. 2026 / Carbonyl content in mmol / g 0.2 About 0.1

[0292] AGU

[0293]

[0294] Surface energy in mJ / m237 About 60

[0295] B) beta-0-4 content of the ligin in the cellulose microfibrils

[0296] The beta-O-4 content is a value which enables the comparison of lignin quality and tha nativity of the lignin structure. According to literature, the highest possible monomer yield possible is approximately 70-80% for hardwoods and 50-60% for softwood lignins (the literature values are based on Ralph et al, Lignin structure and its engineering, Current Opinion in Biotechnology, Volume 56, April 2019, Pages 240-249). The lignin in biomass is uncondensed in its structure and gives the reference point for maximum lignin quality.

[0297] Reductive catalytic fractionation (RCF) of lignin for beta-O-4 content determination RCF of the lignocellulosic materials was performed in a 50-mL Parr reactor with a bar-type, PTFE- coated stir bar (20-mm length x 10-mm diameter). The lignocellulosic material (1 g), ruthenium on carbon (5% (wt / wt), 200 mg), and ethanol (20 mL) were added, the Parr reactor sealed, and backfilled with H2 gas by filling it with 40 bar of H2 and slowly releasing the pressure. The backfill was repeated for a total of three times. The Parr reactor was filled with 40 bar of H2 gas and heated to 250 °C with stirring for 15 h. The reaction was cooled to room temperature, the pressure released and the Parr reactor opened. The solution was then analysed by GC-FID as described below.

[0298] GC-FID

[0299] Quantitative analysis of lignin monomer yield was performed with an Agilent 7890B series GC equipped with an HP5 column and a FID. N-Decane (0.2 mL) was added to the reaction mixture after RCF hydrogenolysis as the internal standard. 1 mL of this solution was filtered into a vial with a 0.2 m PTFE syringe filter and then injected into GC-FID for quantification. The GC-FID method was performed as follows: The injection temperature was 300 °C. 1 pL of the sample was injected with an autosampler in split mode (split ratio: 25:1). The column was initially kept at 40 °C for 3 min, then was heated at a rate of 30 °C-min-1 to 100 °C, followed by a heating rate of

[0300] A24555WO / 13. 05. 2026 / 40 °C-min-1 to 300 °C that was held for 5 min. The monomer yields were calculated based on the respective effective carbon number (ECN) in reference to the n-decane standard (ECN=10). The ECNs of lignin monomers are summarized in the work of Shuai et al. (L. Shuai et al., Science, 2016, 354, 329-333. DOI: 10.1126 / science.aaf7810).

[0301] Determination of B-O-4 linkages as an indicator for lignin quality

[0302] Determination of p-O-4 linkages is calculated by taking the square root of the monomer yield of the lignin contained in the fibres (wt% monomers per mass lignin).

[0303] For example, for AAF cellulose microfibrils (entry 2 table below), with a lignin content of 15 wt%, a monomer yield of 75.8 mg was determined for an RCF sample of 1 g using the above GC-FID method after RCF. The corrected mass of monomers takes into account the molecular weight of syringol and guaiacol units in the original biomass which are 196 and 226 g / mol respectively. For the monomer yield calculation, an average molecular weight of the lignin monomers (221 g / mol for hardwood and 196 g / mol for softwood) are used.

[0304] Monomer yield on dry feedstock basis [wt%] = (mass of monomer corrected) / (mass feedstock) = 75.8 mg / 1.002 g x 100 = 7.57

[0305] Monomer yield on dry lignin basis [mol%] = (mol yield of monomer) / ((mass of lignin) / (corrected by non-reduced lignin monomer mass) = 0.3527 mmol / (150.3 mg / 221 g / mol) * 100 = 51.9

[0306] P-O-4 on lignin polymer [%] = square root (monomer yield on dry lignin basis) = square root (0.519)= 72

[0307] The following results were found:

[0308] Name sample Lignin Monomer Monomer p-O-4 on quantity yield on dry yield on dry lignin [wt%] feedstock lignin basis polymer basis [wt%] [mol%]

[0309] Beech 6-8mm (used to calculate p-O-4

[0310] content) 21 14.29 69.5 83.4% AAF cellulose microfibrils 15 7.57 51.9 72.0% Kraft non-bleached softwood 4.6 0.28 6.06 24.6%

[0311]

[0312] Kraft non-bleached eucalyptus 7.4 0.44 6.7 25.9%

[0313] A24555WO / 13. 05. 2026 / The results highlight the remarkable lignin quality of the cellulose microfibrils according to the present invention, which retain native-like lignin having a p-O-4 content of at least 50%, in contrast to the Kraft lignin’s highly condensed structure having a p-O-4 content of less than 35% that leads to an extremely low monomer yield on a dry feedstock basis. This demonstrates the superior preservation of lignin within the fibers of the present invention.

[0314] A24555WO / 13. 05. 2026 /

Claims

Claims1. A method for producing cellulose microfibrils comprising:a) Providing a first composition derived from biomass and comprising lignocellulosic fibers,b) Conducting a chemical pretreatment step by reacting the lignocellulosic fibers of step a) with an aldehyde in the presence of an acid catalyst in an organic solvent to form a second composition comprising aldehyde treated cellulose, aldehyde protected lignin and hemicellulose, wherein the aldehyde protected lignin and the hemicellulose are dissolved in the organic solvent,c) Separating at least the aldehyde treated cellulose from the organic solvent,d) Mechanically treating the aldehyde treated cellulose obtained in step c) by a twin-screw extruder to form the cellulose microfibrils.

2. Process according to claim 1, wherein the first composition comprises lignocellulosic fibers derived from wood, preferably wood fragments.

3. Process according to any of the preceding claims, wherein in step c) the aldehyde treated cellulose is separated from the aldehyde-protected lignin, preferably by filtration.

4. Process according to any of claims 1 to 2, wherein prior to step c) the aldehyde protected lignin in the second composition is precipitated by adding an acid or an antisolvent, and separating the aldehyde treated cellulose and the aldehyde-protected lignin in step c) from the hemicellulose and the organic solvent.

5. Process according to any of the preceding claims, wherein aldehyde treated cellulose in step d) has a lignin content of between 1% and 40%, preferably 5 to 30% by weight relative to the total dry weight of the aldehyde treated lignocellulosic fibers.A24555WO / 13.

05. 2026 / 6. Process according to any of claims 2 to 5, wherein the composition obtained after the separation in step c) is essentially solid and preferably comprises aldehyde-protected lignin derived from wood.

7. Process according to any of the preceding claims, wherein the process is free of a delignification step of the aldehyde treated cellulose between the chemical pretreatment step b) and the mechanical treatment step d).

8. Process according to any of the preceding claims, wherein a composition comprising the aldehyde treated cellulose at the inlet of the twin-screw extruder has a lignin content of between 5% and 30% by weight relative to the total dry weight of the aldehyde treated cellulose.

9. Process according to any of the preceding claims, wherein the temperature in step b) is maintained at 100°C or lower, preferably 80°C or lower.

10. Process according to any of the preceding claims, wherein the aldehyde is an aldehyde of the formula R-CHO, wherein R is selected from the group consisting of hydrogen, a linear or branched aliphatic chain comprising one to six carbon atoms, and (CH2)nCOOH, wherein is an integer between 0 and 5, and wherein the aldehyde is preferably selected from the group consisting of formaldehyde, glyoxylic acid, and propionaldehyde.

11. Process according to any of the preceding claims, wherein, during mechanical treatment by twin-screw extruder (62), the pretreated cellulose suspension passes a number N of times through the twin-screw extruder, N being an integer between one and ten, preferably between one and three.

12. Process according to any of the preceding claims, further comprising mechanical pretreatment step of the second composition to form an aldehyde treated cellulose pulp, wherein said mechanical pretreatment step takes place after the chemical pretreatment b) and prior to mechanical treatment step d).A24555WO / 13.

05. 2026 / 13. Cellulose microfibrils having a lignin content between 1% and 40% by weight relative to the total dry weight of cellulose microfibrils, and characterized in that said lignin has p-O-4 content of 50% to 80%, preferably of 70% to 80%.

14. Cellulose microfibrils according to claim 13 having a lignin content between 5% and 30 % by weight relative to the total dry weight of cellulose microfibrils, preferably between 10 and 25% by weight.

15. Use of the cellulose microfibril suspension (60) according to any of claims 13 or 14 to form a paper based on lignified cellulose microfibrils.A24555WO / 13.