Laminated glazing with a textured internal surface

By using glass with refractive index-matched reliefs and optional reflective coatings, the clarity issues in laminated glass are resolved, achieving high transparency and reduced blur.

WO2026238864A1PCT designated stage Publication Date: 2026-11-19SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064031
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Standard textured glass laminated with polyvinyl butyral (PVB) exhibits clarity issues due to refractive index mismatch, leading to increased blur and loss of clarity, especially when texture slopes exceed 5°, resulting in a milky appearance.

Method used

Laminated glazing with a first sheet of glass having reliefs with a refractive index matching that of the lamination interlayer, such as borosilicate glass, and optionally a reflective coating to enhance clarity and reduce blur.

Benefits of technology

Achieves clarity exceeding 97% by matching the refractive index of glass reliefs with the interlayer, reducing blur and maintaining transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026064031_19112026_PF_FP_ABST
    Figure EP2026064031_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Laminated glazing comprising a first glazing sheet, a second glazing sheet and a laminating interlayer between the first glazing sheet and the second glazing sheet, the first glazing sheet having an internal surface in contact with the laminating interlayer, and the first glazing sheet comprising relief features forming a textured internal surface, characterised in that the relief features have a refractive index substantially identical to that of the laminating interlayer
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description

[0002] Title of the invention: Laminated glazing with a textured internal surface

[0003] [1]The present invention relates to the use of textured glass in laminated glazing (textured glass / adhesive interlayer / glass), preferably with additional coating (textured glass / coating / adhesive interlayer / glass); optical defects due to the structure of the glass may appear.

[0004] [2] The structure of textured glass can be defined by a random or ordered, symmetrical distribution of concave and convex surfaces. It can also be described as a distribution of negative and positive facets with a specific slope. Such textured glass can be manufactured by processes such as acid etching, dry or wet sandblasting, stamping (shaping by pressing), laser engraving, etc.

[0005] [3] Standard textured glass, usually made of standard composition glass, has a different refractive index than the most common interlayer adhesive, polyvinyl butyral (PVB): clear glass has a refractive index of 1.52–1.53, while PVB has a refractive index of 1.47–1.48. As a consequence, light rays passing through both textured glass and PVB are refracted, according to Snell's equation: msin ii = msin i². When textured glass has a variety of facet slopes, multiple refractions occur, resulting in a loss of clarity. Clarity is measured by the amount of diffuse light within a narrow area (angles less than 2.5°) around the normal to the surface (the main surface of the laminated glass); clarity is notably evaluated according to ASTM D1003 and ISO standards.A clarity of at least 98%, for example, characterizes the quality of visible light transmission, sharpness, and good definition of the transparency of laminated glass; it corresponds to a low amount of diffuse light in the defined narrow zone. When multiple deviations of visible light occur, the textured glass / PVB or textured glass / PVB / glass laminated structure exhibits increased blur. Blur, also defined by ASTM DI 003 and ISO standards, characterizes the amount of diffuse light at an angle greater than 2.5° relative to the normal to the surface of the laminated glass (wide-angle zone).

[0006] [4]The deposition of a coating is possible on any surface of the glass sheets (textured or not), but does not affect the problem related to the difference in refractive indices mentioned above.

[0007] [5] As the slope of the texture increases, the angle of deviation of the light rays increases, leading to an increase in the loss of clarity. If the clarity falls below 96–98%, direct vision is obstructed. Blurring is the deviation of beams above 2.5°, as mentioned previously; in terms of visual effect, this gives the glazing a milky appearance. This occurs with slope distributions exceeding 5°, the slopes being the angles formed by the texture (facets, etc.) with respect to the main surface of the laminated glazing.

[0008] [6] According to a first approach, one could consider filling the cavities in the glass texture with a transparent material having a refractive index substantially identical to that of the glass (1.52–1.53), forming a planarization layer whose surface in contact with the PVB is flat. Alternatively, one could imagine replacing all the PVB with an interlayer adhesive having a refractive index of 1.52–1.53. This type of solution is difficult to implement from the point of view of development and fine-tuning, as well as the implementation of the manufacturing process for laminated glass.

[0009] [7] Instead of employing a planarizing layer or a lamination interlayer adhesive with refractive indices almost equal to those of the standard mineral glass usually used, such as clear soda-lime float glass with a refractive index of 1.52 - 1.53, the inventors have instead envisaged a laminated glazing having a glazing sheet comprising reliefs which form a textured internal surface, in which it is the material constituting the reliefs whose refractive index is adapted, substantially identical to that of the lamination interlayer.It has indeed proven to be more advantageous and simple to implement using a sheet of glazing on which a texture can be easily formed, and whose refractive index is equal to that of the lamination interlayer, or to apply reliefs to any sheet of glazing whose material has a refractive index (in the visible) equal to that of the lamination interlayer.

[0010] [8] To this end, the invention relates to laminated glazing comprising a first sheet of glazing, a second sheet of glazing, and a lamination interlayer between the first and second sheets of glazing. The first sheet of glazing has an internal surface in contact with the lamination interlayer (or with a reflective coating between the textured internal surface and the lamination interlayer), and the first sheet of glazing comprises reliefs forming a textured internal surface. These reliefs have a refractive index substantially identical to that of the lamination interlayer. In particular, the laminated glazing of the invention readily achieves a clarity of over 97%.

[0011] [9]The first and second panes of glass can be made of clear or extra-clear glass, or conversely, of tinted glass, such as yellow, blue, green, or bronze glass. They typically each have a thickness of 2 to 20 mm, particularly 3 to 12 mm, for example 4, 6, 8, or 10 mm. They can be made of mineral glass or organic glass (transparent polymer material).

[0012]

[0010] The lamination interlayer is a sheet of thermoformable or pressure-sensitive polymer material. In particular, it may be a lamination interlayer based on polyvinyl butyral (PVB), ethylene vinyl acetate (EVA), thermoplastic polyurethane (TPU), poly(ethylene terephthalate) (PET), or polyvinyl chloride (PVC). The lamination interlayer generally has a thickness of approximately 0.2 to 1.5 mm, for example, around 0.76 mm.

[0013]

[0011] According to a first main embodiment, the first glazing sheet comprises a monolithic substrate having a textured internal surface, preferably selected from borosilicate glass, other mineral glass, or polycarbonate substrates. "Other mineral glass" means a glass whose composition is adjusted so that its refractive index is substantially equal to that of the chosen laminating interlayer, selected, for example, from polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), or thermoplastic polyurethane (TPU). For example, the textured substrate is a so-called "crown glass."

[0014]

[0012] Preferably, the first glazing sheet comprises a monolithic substrate having the internal surface textured, chosen a borosilicate glass, the internal textured surface being the atmospheric face and the lamination interlayer being preferably based on PVB.

[0015]

[0013] The texture of the inner surface of the first pane of glass can be obtained by any known texturing process, for example by stamping, embossing the inner surface of the pane of glass preheated to a temperature at which it can be deformed, in particular by calendering, rolling with a roller having on its surface a texture complementary to the texture to be formed on the inner surface of the pane of glass; by abrasion with abrasive particles or surfaces, in particular by sandblasting; by chemical treatment, in particular acid treatment; or by etching, possibly using masks to keep at least part of the substrate surface untextured (for decorative glazing in particular). The textured inner surface can be formed by a plurality of patterns recessed or raised relative to a general plane of the surface.The textured inner surface can feature randomly or periodically distributed patterns. Specifically, it can display several different patterns across various areas of the surface. The nature of these patterns is not limited and can include, for example, cones, pyramids, grooves, ribs, and wavelets. The textured surface of the first pane of glass typically has a roughness Ra greater than 0.5 µm, for example, from 1 µm to 2 mm. When the pane of glass is a patterned glass pane, the textured surface has, for example, a roughness Ra of 1 to 100 µm (microtexturing), from 0.3 to 1 mm (mini-texturing), or greater than 1 mm.Examples of directly usable textured glazing sheets include the glasses marketed by Saint-Gobain Glass in the SGG SATINOVO® range, which have on one of their surfaces a texture obtained by sandblasting or acid etching; the glasses marketed by Saint-Gobain Glass in the SGG DECORGLASS®, SGG MASTERGLASS® or SGG ALBARINO® ranges, which have on one of their surfaces a texture obtained by lamination.

[0014] According to a second main embodiment, the first glazing sheet comprises a substrate having a smooth internal surface on which are arranged reliefs of a material, different from that of the substrate, in particular forming a textured layer at least partially through its thickness (in particular a coating obtained by liquid means), preferably chosen from enamels, resins, or sol-gel materials.It is this relief material that then has a refractive index approximately equal to that of the laminate interlayer. Adjusting this refractive index is easily done by modifying the composition of enamels, resins, or sol-gel materials. The relief is preferably created using a printing process, examples of which include screen printing, digital printing such as inkjet printing, pad printing, etc. Masks can be used to create the relief on surfaces not covered by the mask.

[0016]

[0015] Preferably, the refractive index of the reliefs differs from that of the laminate interlayer by ±0.02, preferably by ±0.01 (in the visible), in particular at 550nm ±50nm and even ±100nm or even 450nm to 750nm or even throughout the visible.

[0017]

[0016] Preferably, the laminated glazing comprises a reflective coating between (and even in direct contact with) the textured inner surface of the first glazing sheet and the lamination interlayer. By "reflective coating" for the purposes of the present invention, we mean a coating having a visible light reflectance (light reflection) greater than 8%, or 10%, and in particular of at most 30% or even at most 20%, in particular at 550nm ±50nm and even ±100nm or even from 450nm to 750nm or throughout the visible spectrum. In particular for building glazing, the reflection of the reflective coating (and even the light transmission TL) is preferably measured according to ISO 9050:2003 with illuminant D65 and observer CIExy 2° and for automotive glazing is preferably measured according to ISO 13837 with illuminant A and observer CIExy 2°.More precisely, the reflection refers to that of the first pane of glass with the reflective coating, or even that of the laminated glass itself. It is preferable to measure the external light reflection (RExt), which corresponds to the fraction of the luminous flux reflected outwards from the incident surface of the glass. Ideally, the light transmission (TL) of the laminated glass is at least 20%, and even at least 30%, and / or at most 85%, and even at most 75%.

[0018]

[0017] Preferably, the reflective coating is a multilayer coating, preferably comprising (at least) one functional layer selected from metallic and nitrided layers, and even two to four metallic functional layers, particularly silver-based ones. A "multilayer coating" is understood to be a coating formed by a stack of thin films, obtained in particular by magnetron sputtering. The reflective coating is in direct contact with the textured inner surface of the first glazing sheet (textured substrate or smooth substrate and textured layer) and even forms a deposit conforming to the texture. The multilayer coating typically comprises two to fifteen thin layers, for example, three to seven.

[0019]

[0018] In the present invention, the term "functional layer" refers to a thin layer that imparts light-reflecting properties to the coating in the visible spectrum and even in the infrared (particularly the near-infrared). Each functional layer is preferably a nitride layer, in particular based on niobium nitride, titanium nitride, aluminum nitride, or silicon nitride; or a metallic layer, in particular based on silver, gold, titanium, chromium, nickel, copper, tungsten, zirconium, niobium, silicon, aluminum, stainless steel, or their alloys (particularly NiCr); or an oxide layer (simple or mixed), in particular titanium oxide or even a transparent conductive oxide such as indium tin oxide or fluorine-doped tin oxide. Each functional layer (in particular the metallic layer, preferably silver-based) is generally 3 to 50 nm thick, preferably 5 to 30 nm.

[0020]

[0019] The multilayer coating may also include one or more dielectric layers disposed below and / or above the (each) functional layer (in particular, a metallic layer, preferably silver-based). The dielectric layer may be an oxide-based layer, such as silicon dioxide (SiOx, in particular SiO2), titanium dioxide (TiOx, in particular TiO2), tin dioxide, or a mixed oxide, in particular tin and zinc or silica and zirconium; a nitride-based layer, such as aluminum nitride or silicon nitride (SiN, in particular Si3N4) or silica and zirconium nitride; or an oxynitride-based layer, such as silicon oxynitride (SiON). Disposed between the textured glazing sheet and the (each) functional layer, the dielectric layer may improve the adhesion of the functional layer.Positioned above the (last) functional layer (in particular, a metallic layer preferably silver-based), notably as the final dielectric layer of the coating, the dielectric layer can serve as a protective layer. Dielectric layers typically have a thickness of 5 to 150 nm, preferably 10 to 50 nm.

[0021]

[0020] The multilayer coating may also include a blocking layer below and / or above each functional layer, particularly when the functional layer is metallic and preferably silver-based. The blocking layers are generally in direct contact with the functional layer. The blocking layers protect the functional layer from potential degradation during the deposition of a dielectric layer above the functional layer and / or during any heat treatment such as bending or quenching. The blocking layers are generally metallic, such as gold, titanium, or NiCr-based layers, but may be partially oxidized and / or nitrided during the deposition of the dielectric layers or any heat treatments. The blocking layers are generally 0.5 to 2 nm thick.

[0021] The choice of the nature of the layers, their thicknesses and their combinations depends on the desired effect, particularly in terms of color, light reflection and light transmission.

[0022]

[0022] Preferably, the first sheet of glazing is intended to be the sheet facing outwards (for a building facade application in particular or automotive glazing)

[0023]

[0023] The reflective coating can form a solar control (for building or automotive glazing) and preferably the first sheet of glazing is intended to be the sheet facing outwards (for a building facade application in particular or automotive glazing) and / or a solar control layer.

[0024]

[0024] In the case of building glazing, laminated glazing can have a solar factor g of at least 0.1 and even of at least 0.2 and / or of at most 0.5 and even of at most 0.4.

[0025]

[0025] By way of example, reflective coatings (in particular solar control – by reflection and / or absorption –) can be formed by the following stacks, on the first pane of glazing (textured or smooth glass with a textured coating) starting from the first pane of glazing: SisN4 / NiCr / Ag / NiCr / SLN4

[0026] TiO2 / Si3N4 / NiCrN / Ag / NiCrN / Si3N4

[0027] SiN / SnZnO / ZnO / NiCr / Ag / NiCr / ZnO / SiN SiN / SnZnO / ZnO / Ag / ZnO / SiN / SiZrN / SiN / SnZnO / ZnO / Ag / ZnO / SiN

[0028] SiOx / TiOx / SiN

[0029] SiN / TiOx / SiOx / TiOx

[0030] Si3N4 / NbN / Si3N4

[0031] SiN / NbN / SiN

[0032] TiO2 / Si3N4 / NbN / Si3N4

[0033] Si3N4 / NiCu / Si3N4

[0034] Si3N4 / CrSi / Si3N4

[0035] Si3N4 / CrAl / Si3N4 / Ti

[0036] Si3N4 / Cr / Si3N4 / Ti

[0037] Si3N4 / NiCrW / Si3N4

[0038] Si3N4 / CrZr / TiZnO x / Si3N4

[0039]

[0026] In an advantageous embodiment of the invention, the reflective coating is present (deposited) on a portion of the internal textured surface of a determined orientation(s), but not on the entire internal textured surface. Particular reference is made to the deposition of the reflective coating (solar control or anti-solar) on the facets of the texture oriented, in the mounting position of the laminated glazing, towards the sky and not towards the ground.

[0040]

[0027] In an advantageous embodiment of the invention for corrosion protection purposes, the reflective coating (in particular with metallic functional layer(s), especially silver-based) is absent—or rather, demarcated—for at least 5 mm and even at most 2 cm or 1 cm from the periphery of the first pane of glass.

[0028] The functionality of laminated glass can be to limit the transmission of solar radiation into a building, for example, while limiting light reflection towards the ground. This limits ground-level heating, and in cities, the phenomenon known in English as "Urban Heat Island" (and in English, its mitigation: "Urban Heat Island Mitigation").

[0041]

[0029] More broadly, applications of the glazing according to the invention are found in the automotive industry (screen projection), in decorative glazing, exterior and / or building glazing, in particular facade glazing (attenuation of heat concentration in urban environments, at ground level / sidewalks - in English Urban Heat Island mitigation -, seasonal solar control (depending on the solar angle), "day lighting", English terms designating the reflection of solar radiation towards the ceiling, etc.).

[0042]

[0030] Laminated glazing can be part of double glazing.

[0043] [3 l] The invention will be better understood in the light of the embodiment examples described below with reference to the accompanying drawings in which

[0044] [Fig. 1] is the graph of the refractive index n as a function of wavelength in nm

[0045] - for face 1, called Sn (in contact with the molten tin bath in the "float" process), of a borosilicate glass sheet: upper curve formed by disks, and - for face 2, called atmosphere (opposite the molten tin bath in the "float" process), of this borosilicate glass sheet: lower curve formed by triangles [Fig. 1'] is the noise-free graph of the refractive index n as a function of wavelength in nm for these faces 1 and 2

[0046] [Fig. 2] is the graph of the refractive index n as a function of wavelength in nm

[0047] - for the atmospheric face of a sheet of clear soda-lime glass marketed by Société Saint-Gobain Glass under the registered trademark Planiclear®: upper curve formed by discs,

[0048] - for the atmospheric side of a borosilicate glass sheet: lower curve formed of triangles, and

[0049] - for a polyvinylbutyral sheet: lower curve formed of squares; and [Fig. 2'] is the noise-free graph of the refractive index n as a function of wavelength in nm for these atmospheric faces.

[0050] [Fig.3] is a comparative photograph of the transparency (clarity) of a Planiclear® textured borosilicate glass / PVB / soda-lime clear laminated glazing (right) and a Planiclear® textured borosilicate glass / PVB / soda-lime clear glazing (left).

[0051]

[0032] With reference to Figure 1, sandblasted borosilicate glass sheets are used, either in the presence of liquid (water) or dry, to create a textured surface on the transparent sheet, which has a refractive index similar to that of PVB. Ellipsometer measurements on the borosilicate glass sheet show that its refractive index at 580 nm is close to 1.47 for the atmospheric face; for the tin face, it is higher. Evaluation of the texture with an optical profilometer of the sandblasted borosilicate glass on the one hand, and of standard (soda-lime) glass on the other, shows a random concave / convex structure with a slope distribution here around 25°.

[0052]

[0033] With reference to Figure 2, the following refractive indices are measured in the visible spectrum:

[0053] - borosilicate atmosphere face: 1.48,

[0054] - clear soda-lime glass atmosphere face: 1.52, and

[0055] - PVB: 1.47.

[0056] The refractive index of borosilicate is almost equal to that of PVB, allowing for a clarity exceeding 97% for laminated glass, provided there is no planarization layer between the texture and the PVB before lamination. This significantly simplifies the manufacturing process of laminated glass. Furthermore, blurring, or the scattering of light at wide angles (greater than 3° relative to the normal), is also considerably reduced.

[0057]

[0034] Figures 1' and 2' are the noise-free graphs. Table 1 below shows the refractive index values ​​as a function of wavelength in the visible range.

[0058] [Table 1]

[0059] index of

[0060] refractive index

[0061] borosilicate refraction index

[0062] wavelength borosilicate face PLC face refraction

[0063] (nm) tin face atmosphere PVB atmosphere

[0064] 450 1.50 1.48 1.52 1.47

[0065] 455 1.50 1.48 1.52 1.47

[0066] 460 1.50 1.48 1.52 1.47

[0067] 465 1.50 1.48 1.52 1.47

[0068] 470 1.50 1.48 1.52 1.47

[0069] 475 1.50 1.48 1.51 1.47

[0070] 480 1.50 1.48 1.51 1.47

[0071] 485 1.50 1.48 1.51 1.47

[0072] 490 1.50 1.48 1.51 1.47

[0073] 495 1.50 1.48 1.51 1.47

[0074] 500 1.50 1.48 1.51 1.47

[0075] 505 1.50 1.48 1.51 1.47

[0076] 510 1.50 1.48 1.51 1.47

[0077] 515 1.50 1.48 1.51 1.47

[0078] 520 1.50 1.48 1.51 1.47

[0079]

[0080] 525 1.50 1.48 1.51 1.47 530 1.50 1.48 1.51 1.47

[0081] 535 1.50 1.48 1.51 1.47

[0082] 540 1.50 1.48 1.51 1.47

[0083] 545 1.50 1.48 1.51 1.47

[0084] 550 1.50 1.48 1.51 1.47

[0085] 555 1.50 1.48 1.51 1.47

[0086] 560 1.50 1.48 1.51 1.47

[0087] 565 1.50 1.48 1.51 1.47

[0088] 570 1.50 1.48 1.51 1.47

[0089] 575 1.50 1.48 1.51 1.47

[0090] 580 1.50 1.48 1.51 1.47

[0091] 585 1.50 1.48 1.51 1.47

[0092] 590 1.50 1.48 1.51 1.47

[0093] 595 1.50 1.48 1.51 1.47

[0094] 600 1.50 1.48 1.51 1.47

[0095]

[0096]

[0035] Figure 3 visually shows the improvement in clarity thanks to the use of borosilicate glass.

[0097]

[0036] The clarity and blur of laminated glass are measured using wet and dry sandblasting. The results are shown in Table 2 below. In the case of Figure 3 (wet sandblasting), the clarity is 77.6% with textured soda-lime glass and 98.3% with textured borosilicate glass.

[0098]

[0037] [Table 2]

[0099] Blurry Clarity

[0100] Clear soda-lime glass

[0101] wet sandblasting / PVB / glass 77.6 6.1

[0102] clear sodocalcic

[0103] Borosilicate sandblasting

[0104] moist / PVB / clear glass 98.3 1.9 soda-lime

[0105] Clear soda-lime glass

[0106] dry sandblasting / PVB / clear glass 71.8 7.7 Borosilicate sandblasting

[0107] dry / PVB / clear glass 97 2.2

[0108]

[0109] sodium calcium

[0110]

[0038] The improvement in clarity is maintained by interposing a stack of magnetron-deposited thin films.

[0111]

[0039] A first example of laminated glazing with a stack of thin films (silver functional layer) is described in the following Table 3.

[0040] [Table 3]

[0112] thickness

[0113] layer

[0114] (nm)

[0115] TiOx 12

[0116] SnZnO 8

[0117] ZnO 9

[0118] Ag 11

[0119] ZnO 6

[0120] SiN 60

[0121] SnZnO 7

[0122] ZnO 9

[0123] Ag 10

[0124] ZnO 5

[0125] SiN 22

[0126]

[0127]

[0041] The light transmission, external light reflection, and clarity of the laminated glazing comprising a sandblasted textured borosilicate glass coated with the above-mentioned bi-silver stack, a PVB interlayer, and a second standard soda-lime glass are measured. The results are recorded in Table 4 below.

[0128]

[0042] [Table 4]

[0129] TL (%) Rext (%) C (%)

[0130] 68.2 7.7 98.3

[0131]

[0132]

[0043] A second example of laminated glazing with a stack of thin films (NbN functional layer) is described in the following Table 5

[0133]

[0044] [Table 5]

[0134] thickness

[0135] layer

[0136] (nm)

[0137] SiN 10

[0138] NbN 6

[0139] SiN 30

[0140]

[0141]

[0045] The light transmission, external light reflection, and clarity of the laminated glazing comprising a sandblasted textured borosilicate glass coated with the NbN stack described above, a PVB interlayer, and a second standard soda-lime glass are measured. The results are shown in Table 6 below.

[0142]

[0046] [Table 6]

[0143] TL (%) Rext (%) C (%)

[0144] 54.0 15.0 98.3

[0145]

[0146]

[0047] A third example of laminated glazing with a stack of thin films (TiOx functional layer) is described in the following table 7.

[0147]

[0048] [Table 7]

[0148] thickness

[0149] layer

[0150] (nm)

[0151] SiN 25

[0152] TiOx 22

[0153] SiO2 7

[0154] TiOx 2

[0155]

[0156]

[0049] The light transmission, external light reflection, and clarity of the laminated glazing comprising a sandblasted textured borosilicate glass coated with the stack of TiOx described above, a PVB interlayer, and a second standard soda-lime glass are measured. The results are recorded in Table 8 below.

[0157]

[0050] [Table 8]

[0158] TL (%) Rext (%) C (%)

[0159] 76.0 21.0 98.3

[0160]

[0161]

[0051] The invention can be implemented using an EVA with a refractive index of 1.48 to 1.52 depending on the annealing temperature of the FDM, instead of PVB. Alternatively, an EVA with a suitable refractive index and a soda-lime clear glass can be chosen.

Claims

Demands

1. Laminated glazing comprising a first sheet of glazing, a second sheet of glazing and a lamination interlayer between the first sheet of glazing and the second sheet of glazing, the first sheet of glazing having an internal surface in contact with the lamination interlayer, and the first sheet of glazing comprising reliefs forming a textured internal surface, characterized in that the reliefs have a refractive index substantially identical to that of the lamination interlayer.

2. Glazing according to claim 1, characterized in that the first sheet of glazing comprises a monolithic substrate having a textured internal surface, preferably selected from substrates made of borosilicate glass, other mineral glass, or polycarbonate.

3. Glazing according to claim 1, characterized in that the first sheet of glazing comprises a substrate having a smooth internal surface on which are arranged reliefs of a material, different from that of the substrate, preferably chosen from enamels, resins, or sol-gel materials.

4. Glazing according to any one of claims 1 to 3, characterized in that the refractive index of the reliefs differs from that of the lamination interlayer by ±0.02, preferably by ±0.

01.

5. Glazing according to any one of claims 1 to 4, characterized in that the laminated glazing comprises a reflective coating between the textured inner surface of the first sheet of glazing and the lamination interlayer.

6. Glazing according to claim 5, characterized in that the reflective coating is a multilayer coating, preferably comprising at least one functional layer selected from metallic layers, nitrided layers, oxide layers.

7. Glazing according to any one of claims 5 or 6, characterized in that the reflective coating is deposited on a part of the internal textured surface of determined orientation(s), but not on all of this internal textured surface, preferably the reflective coating being only on the facets of the internal textured surface oriented, in the mounting position of the laminated glazing, towards the sky.