Pipe with a polymer surface and a protective fibre reinforced cladding

By increasing the surface free energy of polymer surfaces using flame, plasma, or chemical treatments, and embedding fibres in a thermoset resin matrix, the bonding between polymer surfaces and fibre-reinforced claddings is enhanced, addressing mechanical strength issues and ensuring durable pipe performance.

WO2026238896A1PCT designated stage Publication Date: 2026-11-19RFD INNOVATIONS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064091
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Plastic materials used for pipe corrosion protection have low mechanical strength, leading to damage from physical forces during installation or operation, and existing methods fail to address inadequate bonding between polymer surfaces and fibre-reinforced claddings.

Method used

Increase the surface free energy of polymer surfaces through flame treatment, plasma treatment, or chemical treatment to enhance bonding with fibre-reinforced claddings, and optionally embed fibres in a thermoset resin matrix to create a durable, bonded system.

Benefits of technology

The treated polymer surfaces provide improved bonding with fibre-reinforced claddings, enabling pipes to withstand mechanical forces and maintain a tight bond during pipeline preparation and installation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026064091_19112026_PF_FP_ABST
    Figure EP2026064091_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention refers to a pipe for a pipeline. The pipe comprises a tube (12) either of plastic of enclosed by a plastic sheathing with a polymer surface, which is enclosed by a fibre reinforced cladding (16). According to the invention, the bonding to the fibre reinforced cladding to the polymer surface of the plastic is increased by increasing the free surface energy (FSE) of the polymer surface by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Eisenfiihr Speiser

[0002] Berlin, 13 May 2026

[0003] Our Ref.: TB 1278-02WO JVO / nes

[0004] Applicant: RFD Innovations AG

[0005] Serial Number: New Application

[0006] RFD Innovations AG

[0007] Alpenstrasse 6, 6004 LUZERN, SCHWEIZ

[0008] Pipe with a polymer surface and a protective fibre reinforced cladding

[0009] The invention relates to a pipe for a pipeline comprising a tube enclosed by a fibre reinforced cladding. The invention further relates to a method of producing such a pipe.

[0010] The invention concerns in particular a pipe with a fibre-reinforced cladding enclosing a polymer pipe surface. Such pipe can comprise a tube made of plastic, for example polyolefins, 5 or of metal, for example steel, or of a combination thereof, for example a metal pipe with an outer surface of plastic materials, for example fusion-bonded epoxy, polyethylene, polypropylene and / or polyurethane or hybrid pipes for example with a combination of layers such as steel pipes with a sheathing of polyurethane-foam and polyolefin-based casing materials for temperature insulation.

[0011] 0 Pipes for the transport of liquid or gaseous media are used in a wide range of applications, including buried onshore pipelines and subsea pipelines laid on the sea-bed. Such pipes can be made of plastic, such as for example polyethylene or polypropylene or comprise a metal tube, for example a steel tube covered with one or more plastic layers for corrosion protection. Plastic materials for corrosion protection include fusion-bonded epoxy, polyeth-5 ylene, polypropylene and / or polyurethane. Hybrid pipes are also known, for example metal pipes with temperature-insulating layers such as polyurethane foam enclosed by a thermoplastic casing.

[0012] While such plastic materials provide good corrosion protection on the one hand, as the moisture of the surrounding environment and / or electrolytes cannot cause corrosion of the

[0013] R7R*pipe (in the case of plastic pipes) respectively cannot come into contact with the metallic pipe materials (in the case of metallic pipes). On the other hand, plastic materials commonly used for such corrosion prevention or protection, such as fusion-bonded epoxy, polyethylene, polypropylene and / or polyurethane have only a relatively low mechanical strength. This means that physical forces acting on the plastic materials of the pipe during installation or operation of the pipeline can lead to damages of such plastic materials. Such forces could be static compression or pulling forces in axial as well as radial direction of the pipe (static forces) as well as abrasion, impact, indentation or gouging or similar forces (mechanical forces).

[0014] To protect pipes against mechanical forces, it is known to additionally provide the pipe with a fibre-cement coating, a concrete-weight coating or a fibre reinforced plastic (FRP) cladding, in particular a glass-fibre reinforced plastic (GRP) cladding.

[0015] Metal pipes with a glass-fibre reinforced plastic cladding are disclosed inter alia in WO 01 / 05580 A1 and WO 2020 / 002660 A1. The glass-fibre reinforced plastic cladding protects the pipe during various installation methods, such as trenchless pipe-laying, open trench pipe-laying or subsea pipe-laying. Various reinforced pipe structures are known from the prior art. US 9,243,727 B2 discloses a high temperature flexible pipe comprising an inner tubular layer of a high temperature thermoplastic, reinforcing layers of helically wound fibres, and an outer sheath. The reinforcing fibres are wound directly around the thermoplastic inner layer without surface activation of the polymer surface. US 2003 / 0127147 A1 discloses a reinforced pipe for transporting aggressive fluids, comprising a plastic inner pipe, a barrier layer and a reinforcing layer with fibres. The barrier layer is arranged between the inner pipe and the reinforcing layer to prevent aggressive substances from attacking the reinforcing layer. US 4,850,395 A discloses a flexible composite pipe with aramid fibre layers, tape layers and steel armour wire layers wound around a thermoplastic core tube. In none of these prior art documents is the problem of inadequate bonding between a polymer surface and a fibre reinforced cladding addressed.

[0016] For producing a fibre reinforced plastic cladding on a pipe, resin-impregnated or resin-soaked fibre fabrics can be wound around the pipe. Different types of fibres, such as glass fibres, basalt fibres, carbon fibres, polyamide fibres and others, in different fabric forms can be applied to the pipe with different fibre orientations and various winding / application angles.Plastic pipes are commonly not protected with a fibre-reinforced plastic cladding. Instead they can be directly reinforced by integration of fibres, such as glass fibres, into the plastic material of the pipe, for example during the extrusion process.

[0017] Hybrid pipes, such as metal pipes with temperature-insulation layers are disclosed in WO 2023 / 198902 A1 as a system with glass-fibre reinforced cladding for strengthening and protection of the pipe.

[0018] It is an object of the invention to provide an improved pipe with a polymer surface and a fibre-reinforced cladding applied thereon.

[0019] According to a first aspect, the object is achieved by a pipe comprising a plastic tube with a polymer surface or a metal tube enclosed by a plastic sheath with a polymer surface. A fibre-reinforced protective cladding is applied to the polymer surface and thus encloses the plastic tube or the intermediate plastic layer that encloses the metal tube. The polymer surface, in particular if made of Polyethylene (PE) or Polypropylene (PP) commonly has a very low surface energy and hence does not readily bond with thermoset plastic materials. It is one aspect of the invention to increase the surface free energy (SFE) of the polymer surface by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment. A polymer surface having an increased free surface energy herein is also called an activated polymer surface. According to the first aspect, the polymer surface of the plastic tube or plastic layer is activated by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment and thus provides an increased surface energy compared to an untreated polymer surface. Alternatively or additionally, fibres may be embedded in a surface layer of the thermoplastic tube or the thermoplastic sheath of the metal tube.

[0020] The term "tube" as used herein can refer to a plastic tube or a metal tube, such as a steel tube. In the case of a metal tube, the plastic layer enclosing the metal tube can be applied directly to the metal tube or indirectly via one or more intermediate layers, for example an anti-corrosion coating such as a fusion-bonded epoxy layer and / or an adhesive layer. The plastic layer can be a thermoplastic sheath, for instance made of polyethylene, polypropylene or polyurethane. In the case of hybrid pipes, the metal tube can be provided with temperature-insulating layers, such as polyurethane foam, enclosed by a thermoplastic casing.The term "polymer surface" as used herein refers to the outermost surface of the plastic tube or the plastic layer that is to receive the fibre reinforced protective cladding. The polymer surface can comprise or consist of a thermoplastic polymer, such as polyethylene or polypropylene. A polymer surface having an increased free surface energy as a result of surface treatment is also referred to herein as an activated polymer surface. According to the first aspect of the invention, the polymer surface of the plastic tube or plastic layer is activated.

[0021] The term "fibre reinforced cladding" as used herein refers to a composite layer comprising reinforcing fibres embedded in a matrix of a thermoset plastic material. The thermoset plastic material can be provided in a liquid state during application and can subsequently be cured or can cure to form a hardened matrix.

[0022] The term "increased free surface energy" means that the surface free energy (SFE) of the polymer surface is higher than the surface free energy of an untreated polymer surface of the same material. The increased surface free energy can enhance physicochemical bonding between the polymer surface and the thermoset plastic material of the fibre reinforced cladding. In particular, the increased surface free energy can improve the spreading coefficient, the adhesion work and / or the interfacial tension between the polymer surface and the liquid thermoset resin during application of the fibre reinforced cladding.

[0023] Flame treatment means briefly exposing the polymer surface to a flame to thus oxidize the polymer surface. Thus, flame treatment induces an increase in oxygen at the surface of polymers. The term "flame treatment" as used herein refers to a gas-phase surface pretreatment method in which a combustion flame is applied to the polymer surface to modify its surface chemistry without substantially affecting the bulk properties of the underlying polymer material. In flame treatment, a hydrocarbon fuel and an oxidiser are mixed, preferably in an oxygen-rich ratio, and combusted to generate a flame plasma. The flame is moved closely over the polymer surface to be treated. The oxidation of the polymer surface as a result of flame treatment can occur through multiple physical processes, including homogeneous combustion of the premixed reactants, transport of the products of combustion to the polymer surface and heterogeneous reaction of the flame products with the polymer surface. The adiabatic flame temperature can be approximately 1800°C. Flame treatment can introduce oxygen-containing functional groups, such as hydroxyl groups, carbonyl groups and / or carboxyl groups, onto the polymer surface, thereby increasing the surface free energy and improving the wettability of the surface for the subsequently applied thermoset resin. Flame treatment can be carried out without a precursor material, resultingin direct oxidative modification of the polymer surface, or with a precursor material for flame-pyrolytical deposition of an oxide layer on the polymer surface. The use of a precursor material in the flame treatment constitutes a process known as combustion chemical vapour deposition (CCVD).

[0024] The term "plasma treatment" as used herein refers to a surface treatment method in which the polymer surface is exposed to a plasma generated by ionisation of a process gas, such as oxygen, nitrogen, air or a noble gas. Plasma treatment can modify the surface chemistry by introducing functional groups onto the polymer surface.

[0025] The term "corona treatment" as used herein refers to a surface treatment method in which the polymer surface is exposed to a corona discharge generated by applying a high voltage between electrodes in the presence of air or another gas. The corona discharge can oxidise the polymer surface and introduce polar functional groups.

[0026] The term "surface-activating chemical treatment" as used herein refers to a surface treatment method in which the polymer surface is treated with a chemical agent to modify the surface chemistry to thus increase the free surface energy. Surface-activating chemical treatment can include treatment with oxidising agents, such as acids or oxidising solutions, or treatment with coupling agents.

[0027] Flame treatment, plasma treatment, corona treatment or chemical treatment result in an “activated” surface of the polymer surface, i.e. the polymer surface is in an activated state after the surface treatment by flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment.

[0028] Surface activation of a polymer surface by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment can increase the surface free energy compared to an untreated polymer surface temporarily. Various environmental factors, such as dust, humidity and other contaminants, can subsequently reduce the surface activation over time. It can therefore be advantageous to apply the fibre reinforced cladding to the activated polymer surface within a defined time window after the surface activation. Alternatively, flame-pyrolytical deposition of an oxide layer by CCVD can provide a more durable surface activation that is less susceptible to degradation by environmental factors.

[0029] By providing the polymer surface with an increased free surface energy, the bonding between the polymer surface and the fibre reinforced cladding can be significantly improved.This can enable a reliable bonded system between the polymer surface and the fibre reinforced protective cladding that can withstand bending of the pipe during preparation or installation of a pipeline while maintaining a tight bond.

[0030] The effect of the activated polymer surface is an improved bonding between the polymer surface and the fibre reinforced layer applied on the polymer surface.

[0031] This effect can be achieved or improved by heat treating the polymer surface so as to make the polymer material plastically deformable. For instance, a thermoplastic polymer material can be heat treated to make the polymer material plastically deformable. When in its plastically deformable state, fibres can be applied to a surface layer of the plastically deformable polymer to thus achieve a surface layer of the polymer wherein fibres are at least partially embedded in the surface layer of the polymer material.

[0032] Thus, according to a second aspect, a pipe for a pipeline is provided, wherein the pipe comprises a tube being enclosed by a fibre reinforced protective cladding that comprises reinforcing fibres embedded in a matrix made from a thermoset plastic material.

[0033] The tube is a plastic tube with a thermoplastic surface layer or a metal tube directly or indirectly enclosed by a plastic layer (for instance a plastic sheath) with a thermoplastic surface layer. The thermoplastic surface layer comprises fibres that are applied to the thermoplastic surface layer by heating the thermoplastic surface layer and thus temporarily making the thermoplastic surface layer plastically deformable and applying the fibres while the thermoplastic surface layer is in its plastically deformable state. The fibre-reinforced protective cladding is applied to the thermoplastic surface after the fibres have been applied to the thermoplastic surface layer to thus enclose the thermoplastic surface layer with a fibre reinforced protective layer comprising fibre embedded in a matrix made from a thermoset plastic material.

[0034] Instead of or in addition to flame treatment of the thermoplastic sheath surface, the surface layer of the plastic sheath 14 may be heat treated to temporarily make the surface layer 34 plastically deformable. When in its plastically deformable, for instance partially molten state, fibres may be applied to the plastically deformable surface layer such that the fibres are at least partially embedded in the surface layer. Such fibres may extend beyond the surface of the plastic sheath and can this improve bonding with a fibre reinforced cladding 16.The tube according to the second aspect can be produced by a method comprising the steps of:

[0035] providing a tube with a thermoplastic polymer surface layer or a metal tube enclosed by a thermoplastic sheath having a thermoplastic surface layer,

[0036] heating the thermoplastic surface layer to make the surface layer plastically deformable,

[0037] applying fibres to the surface layer in its plastically deformable state, such that the fibres are partially embedded in the surface layer,

[0038] applying a fibre reinforced cladding to the surface layer with embedded fibres,

[0039] wherein applying of the fibre reinforced cladding comprises applying a noncured thermoset resin matrix to the surface layer optionally with additional layer(s) of fibres embedded in such matrix and thus enclosing the plastic tube or the intermediate plastic sheath that encloses the metal tube, and

[0040] curing or letting the thermosetting resin cure and thus hardening it.

[0041] The application of fibres to the thermoplastic polymer surface layer occurs after producing a plastic tube of providing a metal tube with a plastic sheath made of thermoplastic material.

[0042] The heating of the surface layer for making the surface layer plastically deformable may include heating the surface layer to about 120°C to 200°C. The material of the plastic sheath can be polyethylene. For making a surface layer of a polyethylene plastic sheath plastically deformable, temperatures between 120°C and 160° are preferred.

[0043] The fibre to be embedded in the surface layer can be glass fibres, for instance short glass fibres such as cut rovings. Instead or in addition to short fibres, long fibres, for instance a fibre cloth or long rovings can be applied to the heated, plastically deformable surface layer of the plastic sheath. Long fibres can be wound around the surface layer in its heated, plastically deformable, for instance molten state. The fibres can be glass fibres. Alternatively or in addition to glass fibres, aramid, basalt or carbon fibres may be used for being embedded in the thermoplastic surface layer. After applying the fibres, the surface layer can cool down and thus harden.Accordingly, the pipe comprises a plastic tube with a polymer surface or a metal tube enclosed by a plastic layer with a polymer surface. The polymer surface is activated by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment. A fibre-reinforced cladding is applied to the activated polymer surface and thus encloses the plastic tube or the intermediate plastic layer that encloses the metal tube. In addition or as an alternative to flame treatment, plasma treatment, corona treatment or chemical treatment, a surface layer of the plastic sheath with embedded fibres may be provided.

[0044] According to a third aspect, the object is achieved by a method of producing a pipe with a fibre reinforced protective layer, said method comprising the steps of

[0045] providing a tube with a polymer surface or a metal tube enclosed by a plastic layer with a polymer,

[0046] increasing the surface free energy of the polymer surface by means of flame treatment, plasma treatment, corona treatment or chemical treatment, and

[0047] applying a fibre reinforced cladding to the polymer surface having an increased surface free energy,

[0048] wherein applying of the fibre reinforced cladding comprises applying a layer of fibres embedded in a non-cured thermoset resin matrix to the activated polymer surface and thus encloses the plastic tube or the intermediate plastic layer that encloses the metal tube, and

[0049] curing or letting the thermosetting resin cure and thus hardening it.

[0050] Applying of the fibre reinforced cladding may comprise

[0051] providing a mixture comprising randomly orientated short fibres embedded in a noncured, liquid thermoset plastic material, and

[0052] spraying or extruding the mixture of non-cured thermoset plastic material and short fibres on the activated polymer surface of the pipe.The step of increasing the surface free energy of the polymer surface by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment may comprise deposition of a flame-pyrolytically deposited layer on the polymer surface. The flame-pyrolytically deposited layer has an increased surface free energy compared to the polymer surface without a flame-pyrolytically deposited layer. The flame-pyrolytically deposited layer may comprise silicon dioxide (SiOa). Accordingly, a silicon-containing precursor material such as tetramethysilane Si(CH3)4 can be used as a precursor.

[0053] Preferably, the polymer surface is flame treated and provides a flame activated interface to which the fibre reinforced cladding is applied.

[0054] Surface activation of a polymer surface with otherwise low surface energy by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment only has a time-limited effect, as various environmental factors, such as dust, humidity, etc. can subsequently significantly reduce the surface activation. Therefore, it is another alternative aspect of the invention to activate the polymer surface by increasing the surface free energy by flame-pyrolytical deposition of certain oxides, for example silicon dioxide (SiOa). Thus, flame-pyrolytically deposited oxide layers, such as SiCk can be generated on the polymer surface.

[0055] The process used for flame-pyrolytical deposition of, for instance, SiCk is known as combustion chemical vapour deposition (CCVD). In the CCVD process, a precursor compound, for instance a metal-organic compound or a metal salt, is added to a burning gas. The flame of the burning gas is moved closely to the polymer surface to be activated by flame-pyro-lytical deposition of, for instance, SiCk. The high energy within the flame converts the precursors into highly reactive intermediates, which readily react with the plastic layer's polymer surface, forming a firmly adhering deposit. The microstructure and thickness of the flame-pyrolytically deposited layer can be controlled by varying process parameters such as speed of the passing of the flame over the pipe, number of passes, temperature of the plastic layer and distance between flame and the polymer surface. These parameters are determined in consideration of the required bonding with the fibre-reinforced protective cladding layer for the specific application, while ensuring that the temperature control during the flame treatment process causes no structural damages to the plastic tube or intermediate plastic layer. CCVD can produce coatings with orientation from amorphous to epitaxial, and can produce conformal flame-pyrolytically deposited layers less than 10 nm thick. Typically, CCVD produced coatings can be 5 to 500 nm thick, preferably 5 to 200 nm. Thus, CCVD technique is a vapour deposition process for making thin film coatings. TheCCVD coating process has the ability to deposit thin films in the open atmosphere using inexpensive precursor chemicals in solution allowing for continuous, production-line production of pipes to be provided with a fibre reinforced cladding on a polymer surface of a plastic layer. US 6,013,318 discloses a method for the Combustion Chemical Vapour Deposition of films and coatings.

[0056] The plastic layer may comprise a thermoplastic polymer such as Polypropylene or Polyethylene, for instance.

[0057] According to the preferred embodiment, the flame activated surface has an increased surface free energy (SFE) resulting from the flame treatment. The increased surface free energy of the flame activated surface increases a physicochemical bond between solid and liquid compared to a non-treated polymer surface. A low surface free energy (SFE) of polymers prevents the spreading of liquid coatings. Prior to application of the fibre reinforced cladding, the intermediate polymer surface is activated and the SFE is thus increased. In this way, physical effects that determine the adhesion behaviour of cladding and bonds (e.g. spreading coefficient, adhesion work, interfacial tension) are optimized. In general, techniques such as flame treatment, plasma treatment, corona treatment or chemical treatment are available for the activation of polymer surfaces.

[0058] The fibre-reinforced protective cladding comprises reinforcing fibres embedded in a thermoset plastic material. The thermoset plastic material embedding the fibres of the fibre-reinforced protective cladding preferably is a polyester-, a vinylester- or an epoxy resin. Accordingly, the tube is a metal tube, for instance a steel tube, or a plastic tube. If the tube is a metal tube, the pipe may comprise a thermoplastic sheath applied to the metal tube or other layers, for instance temperature insulating foams applied to the metal tube enclosed by a thermoplastic sheath. The pipe further comprises a fibre reinforced protective cladding that encloses the plastic tube or the metal tube with the thermoplastic sheath.

[0059] In an embodiment, the pipe with the fibre-reinforced cladding requires bending during preparation of or during pipeline installation. In this instance, a continuous connection between the polymer surface and the fibre-reinforced cladding maybe required of the pipe respectively a string of pipes forming a pipeline to ensure a continued performance of the fibre-reinforced cladding either for protection and / or for strengthening of the pipeline system. It is one aspect of the invention to create a bonded system between the polymer surface and the fibre-reinforced cladding to ensure a bending of the pipe assembly can be achievedwhile maintaining a tight bond between the polymer surface and the fibre reinforced cladding.

[0060] The reinforcing fibres preferably comprise glass fibres, aramid fibres, carbon fibres and / or basalt fibres that may be provided as a mat, a cloth - for instance textile glass - or rovings. In further embodiments, the fibre-reinforced cladding may comprise randomly orientated, short fibres, in particular short glass, basalt, aramid or carbon fibres. Short fibres may be fibres wherein at least 90% of the fibre have a length of less than 250 mm or less than 100 mm, preferably less than 50 mm or less than 20 mm. Short fibres may be cut rovings.

[0061] The fibre reinforced protective cladding may comprise more than one layer of reinforcing fibres. Preferably, the layers of reinforcing fibres are applied in a wet-in-wet process wherein a further layer of fibre reinforced plastic material is plied on another layer of fibre reinforced plastic material while the resin of the other layer of fibre reinforced plastic material is not fully cured.

[0062] Further details of the invention shall now be described by way of example with respect to the attached drawing.

[0063] Fig. 1 of the drawing is a longitudinal cross-sectional view of a first embodiment of plastic cover pipe assembly;

[0064] Fig. 2 illustrates application of a first layer of the fibre-reinforced cladding onto an activated polymer surface of a thermoplastic layer;

[0065] Fig. 3 illustrates application of a second layer of the fibre-reinforced cladding onto the first layer of the fibre-reinforced cladding;

[0066] Fig. 4 illustrates a method of producing a pipe with a fibre reinforced layer;

[0067] Fig. 5: illustrates an embodiment wherein a thermoplastic polymer material has a surface layer with fibres partially embedded therein;

[0068] Fig. 6: illustrates an embodiment wherein a thermoplastic polymer material has a surface layer with fibres partially embedded therein and a flame-pyrolytically deposited layer;Fig. 7: illustrates another method of producing a pipe with a fibre reinforced protective layer; and

[0069] Fig. 8 to 12: illustrate steps of applying a fibre-reinforced cladding to a tube with a polymer surface.

[0070] Figure 1 illustrates a pipe assembly 10 with metal pipe 12 that is enclosed by a plastic sheath 14 that in turn is enclosed by the fibre reinforced cladding 16.

[0071] The pipe assembly 10 shown in figure 2 comprises a metal pipe 12 that is enclosed by a plastic sheath 14. The plastic sheath 14 preferably is a thermoplastic sheath, for instance a thermoplastic sheath made of Polyethylene (PE), Polypropylene (PP) or Polyurethane (PU). If a fusion bonded epoxy (FBE) coating is used in combination with a thermoplastic sheath, an adhesive layer (not shown) may be provided between the fusion bonded epoxy (FBE) coating and thermoplastic sheath 14 enclosing the fusion bonded epoxy (FBE) coating. The thermoplastic sheath 14 has a polymer surface 30 that is activated by flame treating or combustion chemical vapour deposition (CCVD) to increase the surface free energy before applying a fibre reinforced cladding 16.

[0072] Accordingly, the polymer surface 30 has an increased surface free energy (SFE) that improves bonding of the fibre reinforced cladding 16 to the polymer surface. The increased surface free energy (SFE) can be achieved by way of flame treatment of the polymer surface with or without using a precursor material such as tetramethysilane Si(CH3)4. The use of a precursor material such as tetramethysilane Si(CH3)4 results in a deposition of a flame-pyrolytically deposited layer 32 on the polymer surface 30. The flame-pyrolytically deposited layer 32 may comprise silicon dioxide (SiOa) if tetramethysilane Si(CH3)4 is used as a precursor material.

[0073] The plastic sheath 14 with its activated polymer surface 30 is enclosed by the fibre reinforced cladding 16. As already known from the prior art, the fibre reinforced cladding preferably is made from a thermoset resin, for instance vinylester-, polyester- or epoxy resin, and reinforcing fibres embedded therein. The reinforcing fibres preferably are glass-fibres, basalt fibres, aramid fibres or carbon fibres. The fibres may be provided as fibre mat, fibre cloth (textile) or fibre rovings.A pipe 10 may have a nominal diameter Dnbetween 50 mm and 1400 mm or more. The fibre reinforced cladding 16 preferably has a thickness of between 1.5 mm and 75 mm, or even more, preferred of between 2.5 mm and 50 mm.

[0074] Preferably, the fibres are provided as an elongate fibre fabric 24 that can be wound around the plastic sheath 14 in two different winding directions, thus forming at least one right-handed helix and one left-handed helix as illustrated in figures 2 and 3. The fibre reinforced cladding 16 may comprise several layers of reinforcing fibres as, for instance, described in WO 2020 / 002660 A1 or US 2023 / 0052636 A1. In particular, one layer fibre reinforced protective cladding 16 may be produced by winding a fibre fabric 24.1 in a helical manner around a pipe 10' with a first winding sense and a further layer fibre reinforced protective cladding 16 may be produced by winding a further fibre fabric 24.2 in a helical manner around a pipe 10' with a second, opposite winding sense; see figure 3.

[0075] In the preferred embodiment illustrated in figures 2 and 3, the fibres of one layer of the fibre-reinforced cladding 16 are arranged at a first angle a with respect to the longitudinal axis of the pipe (see figure 2), while the fibres of another - for instance second - layer of the fibre-reinforced cladding 16 are arranged at a second angle p with respect to the longitudinal axis of the pipe; see figure 3. The first layer of the fibre-reinforced cladding 16 can be directly applied on the activated polymer surface 30 of the plastic sheath 14 while the second layer of the fibre-reinforced cladding 16 is applied on the first layer in a wet-in-wet process, i.e. the second layer of the fibre-reinforced cladding 16 is applied before the resin of the first layer is fully cured. Thus, a good bonding between the polymer surface 30 and the first layer and between the first layer and the second layer is achieved.

[0076] In alternative embodiments, fibre reinforced plastic layers comprising short fibres with a length of less than 250 mm, or less than 100 mm, for instance between 5 mm and 50 mm may be provided as the fibre reinforced cladding or as a part thereof. The fibre reinforced cladding 16 may comprise only short fibre in random orientation or a combination of layers comprising short fibres in random orientation and long, orientated fibres. Long fibres typically have length of more than 250 mm and are combined to form fibre threads that may have a length of several meters. While short fibres typically have a random orientation in the matrix of the fibre reinforced plastic layer, long fibres have defined orientation in a respective matrix of the fibre reinforced plastic layer. The fibre reinforced plastic cladding 16 may comprise only long fibres that are orientated in a defined way. Since the fibre reinforced plastic cladding 16 may comprise more than one layer, different kinds of layers maybe provided, i.e. layers with randomly orientated short fibres and layers with long fibres extending in defined directions.

[0077] A method 100 of producing a pipe with a fibre reinforced protective layer is illustrated in figure 4. The method 100 comprises providing a tube with a polymer surface 30; method step 102. The tube may be a plastic tube or a metal tube with a plastic layer. The surface free energy (SFE) of the polymer surface 30 is increased by means of flame treatment, plasma treatment, corona treatment or chemical treatment; method step 104. On the polymer surface 30 having an increased surface free energy the fibre reinforced cladding 16 is applied; method step 106. The application 106 of the fibre reinforced cladding 16 comprises applying a layer of fibres embedded in a non-cured thermoset resin matrix wherein the thermosetting resin is in a liquid state. Once the layer of fibres embedded in a non-cured thermoset resin matrix is applied to the polymer surface 30, the thermosetting resin cures or is cured and thus hardens; step 108.

[0078] Flame treatment is a gas-phase pretreatment method in which the combustion of a hydrocarbon fuel, generates the flame plasma that modifies the polymer surface without affecting the bulk properties of the polymer. The oxidation of the polymer surface as a result of flame treatment occurs through multiple physical processes, including homogeneous combustion of the premixed reactants, transport of the products of combustion to the polymer surface and heterogeneous reaction of flame products with the polymer. The adiabatic flame temperature is approximately 1800°C. For flame treatment, a hydrocarbon fuel and an oxidizer are mixed preferably in an oxygen-rich ratio and then combusted.

[0079] The step of increasing 104 the surface free energy of the polymer surface 30 by means of flame treatment may comprise depositing a flame-pyrolytically deposited layer 32 on the polymer surface 30 by way of combustion chemical vapour deposition (CCVD). The flame-pyrolytically deposited layer 32 has an increased surface free energy compared to the polymer surface without a flame-pyrolytically deposited layer.

[0080] The difference between mere flame treatment (without a precursor material) and combustion chemical vapour deposition that uses a precursor material is the use of a precursor material such as tetramethysilane Si(CH3)4.

[0081] According to a preferred embodiment of the method, applying of the fibre reinforced cladding (method step 106) comprises providing a mixture comprising randomly orientated short fibres embedded in a non-cured, liquid thermoset plastic material and spraying orextruding or otherwise applying the mixture comprising non-cured thermoset plastic material and short fibres on the activated polymer surface of the pipe.

[0082] Instead of or in addition to flame treatment of the thermoplastic sheath surface, the surface layer of the plastic sheath 14 may be heat treated to temporarily make the surface layer 34 plastically deformable. When in its plastically deformable, for instance partially molten state, fibres may be applied to the plastically deformable surface layer such that the fibres are at least partially embedded in the surface layer. Such fibres may extend beyond the surface of the plastic sheath and can this improve bonding with a fibre reinforced protective cladding 16.

[0083] Accordingly, a pipe assembly 10 with metal pipe 12 that is enclosed by a plastic sheath 14 that in turn is enclosed by the fibre reinforced cladding 16 maybe achieved, wherein a surface layer 34 of the plastic sheath 14 comprises fibres, for instance glass fibres, that extend beyond the plastic surface; see figure 5.

[0084] After partially embedding fibres in the surface layer 34 of the plastic sheath 14 and after flame treating the surface or applying a flame-pyrolytically deposited layer (not shown in figure 5), the fibre reinforced cladding 16 may be applied. Embedding fibres in the surface layer 34 of the plastic sheath 14 and activating the surface of the plastic sheath 14 can be combined. In particular, embedding fibres in the surface layer 34 of the plastic sheath 14 may be followed by flame treatment of the surface. Alternatively, flame treatment and heating the surface layer 34 for rendering the surface layer plastically deformable may be a single process step, because the surface layer can be heated and the surface can be flame treated by the same flame in one step.

[0085] As illustrated in figure 7, the tube 10’ of figure 5 can be produced by a method 200 comprising the steps of:

[0086] 202 providing a tube with a thermoplastic polymer surface layer or a metal tube enclosed by a thermoplastic sheath having a thermoplastic surface layer,

[0087] 204 heating the thermoplastic surface layer to make the surface layer plastically deformable,

[0088] 206 applying fibres to the surface layer in its plastically deformable state, such that the fibres are partially embedded in the surface layer,210 applying a fibre reinforced cladding to the surface layer with embedded fibres,

[0089] wherein applying of the fibre reinforced cladding comprises applying a a noncured thermoset resin matrix to the surface layer optionally with additional layer(s) of fibres embedded in such matrix and thus enclosing the plastic tube or the intermediate plastic sheath that encloses the tube, and

[0090] 212 curing or letting the thermosetting resin cure and thus hardening it.

[0091] Optionally, in a step 208, the surface layer 34 with fibres embedded therein may be flame treated or a flame-pyrolytically deposited layer 32 may be applied to the surface layer 34 with fibres 36 embedded therein as shown in figure 6.

[0092] The steps of producing a tube with a fibre reinforced cladding 16 are illustrated in figures 8 to 12.

[0093] Initially, as illustrated in figure 8, a metal tube 12 with a polymer plastic sheath 14 is provided. The metal tube 12 can be a steel tube and the plastic sheath 14 can be a corrosion protection sheath made from a polymer such as Polypropylene (PP), Polyurethane (PU) or Polyethylene (PE). Alternatively, the tube may be made of plastic material only, i.e. no metal tube but a plastic tube. In Any case, the plastic tube or the plastic sheath 14 has a polymer surface 30. The polymer surface typically has a low surface free energy (SFE). In Particular, Polyethylene has a very low surface free energy. A low surface free energy results in a weak bonding to other materials. This can affect the bonding between the polymer surface 14.2 and the fibre reinforced protective cladding 16 to be applied thereon.

[0094] To improve the bonding, a modification of the polymer surface 30, in particular a flame treatment of the polymer surface 30 and / or an embedding of fibres 36 in a surface layer 34 is provided.

[0095] For modifying the polymer surface 30 and a surface layer 34, the surface can be heated in order to make the surface layer 34 soft, i.e. plastically deformable. This is illustrated in figure 9. Heating can be achieved with a flame that also results in a flame treatment of the polymer surface 30. If the plastic sheath 14 is made from Polyethylene, the surface layer 34 is heated to between 120°C and 160°C.In the heated, plastically deformable surface layer 34, fibres 36, for instance glass fibres, are embedded. Embedding can be achieved by winding fibres 36 around the heated surface layer 34. The fibres 36 can be provided as fibre cloth, as UD-cloth or as rovings or the like. Figure 10 illustrated the surface layer 34 with fibres 36 embedded therein.

[0096] Optionally, as shown in figure 11 , the surface layer 34 with fibres 36 embedded therein may be flame treated or a flame-pyrolytically deposited layer 32 may be applied to the surface layer 34 with fibres embedded therein.

[0097] Finally, as shown in figure 12, a fibre reinforced protective cladding 16 may be applied to the modified surface layer 30. As illustrated above, the fibre reinforced protective cladding 16 may comprise at least two layers 20 and 22 that are wound around the tube with different pitches, resulting in a cross-wound structure.List of reference numerals:

[0098] 10 plastic covered protected metal pipe assembly

[0099] 12 metal pipe

[0100] 14 plastic sheath, thermoplastic sheath

[0101] 16 fibre reinforced protective cladding

[0102] 20 inner layer of the fibre reinforced protective cladding

[0103] 22 outer layer of the fibre reinforced protective cladding

[0104] 24 fibre fabric

[0105] 30 polymer (outer) surface of the plastic sheath

[0106] 32 flame-pyrolytically deposited layer

[0107] 34 thermoplastic surface layer of the thermoplastic sheath

[0108] 36 fibres in the surface layer of the thermoplastic sheath

[0109] 100 Method of producing a pipe with a fibre reinforced protective layer

[0110] 102 providing a tube with a polymer surface

[0111] 104 increasing the surface free energy (SFE) of the polymer surface

[0112] 106 application of a fibre reinforced cladding to the polymer surface having an increased the surface free energy

[0113] 108 curing or letting the thermosetting resin cure and thus hardening it

[0114] 200 Method of producing a pipe with a fibre reinforced protective layer

[0115] 202 providing a tube with a polymer surface

[0116] 204 heating the thermoplastic surface layer

[0117] 206 applying fibres to the heated surface layer

[0118] 208 optional flame treatment

[0119] 210 application of a fibre reinforced cladding to the polymer surface having an increased the surface free energy

[0120] 212 curing or letting the thermosetting resin cure and thus hardening ita, p angle between fibres and longitudinal axis of pipe Dnnominal outer diameter of the thermoplastic sheathing

Claims

Claims:

1. Pipe for a pipeline, the pipe comprising a tube (12) being enclosed by a fibre reinforced cladding (16) that comprises reinforcing fibres embedded in a matrix made from a thermoset plastic material,wherein the tube (12) is a plastic tube with a polymer surface (30) or a metal tube (12) directly or indirectly enclosed by a plastic sheath (14) with a polymer surface (30),wherein the fibre-reinforced cladding (16) is applied to the polymer surface (30) and thus encloses the plastic tube or the intermediate plastic layer (14) that encloses the metal tube (12) andwherein the polymer surface (30) is modified so as to havefibres embedded in a surface layer (34)and / oran increased free surface energy (FSE) achieved by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment.

2. Pipe according to claim 1 , wherein polymer surface (30) is flame treated and provides a flame activated interface to which the fibre reinforced cladding is applied.

3. Pipe according to claim 1 or 2, wherein a flame-pyrolytically deposited layer (32) is deposited on the polymer surface.

4. Pipe according to claim 3, wherein the flame-pyrolytically deposited layer (32) comprises silicon dioxide (SiOa):

5. Pipe according to at least one of claims 1 to 4, wherein the thermoset plastic material of the matrix of the fibre reinforced cladding comprises a thermoset resin, such as a vinylester resin, polyester resin or epoxy resin6. Pipe according to at least one of claims 1 to 5, wherein the reinforcing fibres are provided as rovings or fibre webs, said rovings or fibre webs being wound around the plastic tube or the plastic sheath (14) in a helical manner.

7. Pipe according to claim 6, wherein said rovings or fibre webs of the fibre reinforced protective cladding (16) are wound around the plastic tube (12') or the plastic sheath (14) in two different winding directions, thus forming at least one right-handed helix and one left-handed helix.

8. Pipe according to at least one of claims 1 to 7, wherein the reinforcing fibres comprise glass fibres, aramid fibres, carbon fibres and / or basalt fibres.

9. Pipe according to at least one of claims 1 to 8 wherein the fibre reinforced cladding (16) comprises more than one layer of reinforcing fibres that preferably are applied in a wet-in-wet process.

10. Pipe according to at least one of claims 1 to 9, wherein the fibre reinforced protective cladding (16) comprises at least one layer composed of short fibres embedded in the matrix made from a thermoset plastic material.

11. Pipe according to at least one of claims 1 to 10, wherein the pipe is bent after applying the fibre reinforced protective cladding (16).

12. Method (100) of producing a pipe with a fibre reinforced protective layer, said method comprising the steps of:providing (102) a tube with a polymer surface; (30),increasing (104) the surface free energy of the polymer surface (30) by means of flame treatment, plasma treatment, corona treatment or surface-activating chemical treatment;applying (106) a fibre reinforced cladding (16) to the polymer surface having an increased surface free energy,wherein applying of the fibre reinforced cladding comprisesapplying a layer of fibres embedded in a non-cured thermoset resin matrix wherein the thermosetting resin is in a liquid state andcuring or letting (108) the thermosetting resin cure and thus hardening it.

13. The method of claim 12, wherein increasing (104) the surface free energy of the polymer surface (30) by means of flame treatment comprises depositing a flame- pyrolytically deposited layer (32) on the polymer surface, said flame-pyrolytically deposited layer (32) having an increased surface free energy compared to the polymer surface (30) without a flame-pyrolytically deposited layer.

14. The method of claim 12 or 13, wherein applying (106) of the fibre reinforced cladding comprisesproviding a mixture comprising randomly orientated short fibres embedded in a non-cured, liquid thermoset plastic material, andspraying, extruding or moulding the mixture comprising non-cured thermoset plastic material and short fibres on the activated polymer surface of the pipe.

15. Pipe for a pipeline, the pipe comprising a tube (12) being enclosed by a fibre reinforced protective cladding (16) that comprises reinforcing fibres embedded in a matrix made from a thermoset plastic material,wherein the tube (12) is a plastic tube with a thermoplastic surface layer or a metal tube (12) directly or indirectly enclosed by a plastic layer with a thermoplastic surface layer,wherein the thermoplastic surface layer comprises fibres that are applied to the thermoplastic surface layer by heating the thermoplastic surface layer and thus temporarily making the thermoplastic surface layer plastically deformable and applying the fibres while the thermoplastic surface layer is in its plastically deformable state.wherein the fibre-reinforced protective cladding (16) is applied to the thermoplastic surface after the fibres have been applied to the thermoplastic surface layer to thusenclose the thermoplastic surface layer with a fibre reinforced protective layer comprising fibres embedded in a matrix made from a thermoset plastic material.