Dispersion comprising polyvinyl fluoride, composition for varnish, composite membrane, and methods for preparing the dispersion and the composition

A PFAS-free varnish composition using PVF and poly((meth)alkyl acrylate) in specific solvents addresses the need for durable and cleanable composite membranes, providing effective resistance to fouling and adherence.

WO2026238905A1PCT designated stage Publication Date: 2026-11-19SERGE FERRARI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064114
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing varnish compositions containing polymeric PFAS, such as polyvinylidene fluoride (PVDF), are being phased out due to health and environmental concerns, and there is a need for a PFAS-free alternative that maintains properties like resistance to soiling, good cleanability, and durability, especially for composite membranes.

Method used

A varnish composition is developed using poly(vinyl fluoride) (PVF) and poly((meth)alkyl acrylate) dispersed in specific solvents like 2-butoxyethyl acetate, with a controlled mass ratio and drying temperature, to create a composite membrane with a coating layer that adheres well and exhibits reduced fouling.

Benefits of technology

The PVF-based varnish composition achieves good resistance to soiling, cleanability, and durability, adhering effectively to composite membranes while minimizing fouling, thus addressing the need for PFAS-free alternatives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000014_0001_TABLE
    Figure IMGF000014_0001_TABLE
  • Figure IMGF000015_0001_TABLE
    Figure IMGF000015_0001_TABLE
  • Figure IMGF000015_0002_TABLE
    Figure IMGF000015_0002_TABLE
Patent Text Reader

Abstract

A dispersion obtained by the method comprising the following steps: a) preparing a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide, b) adding to the dispersion obtained in step a) a solution of poly(alkyl (meth)acrylate) in a solvent selected from the group consisting of N-butyl acetate and N,N-dimethylformamide, wherein the alkyl group consists of 1 to 4 carbon atoms, and the poly(vinyl fluoride):poly(alkyl (meth)acrylate) mass ratio is between 0.15 and 1.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] DISPERSION COMPRISING POLYVINYL FLUORIDE, VARNISH COMPOSITION, COMPOSITE MEMBRANE, AND METHODS FOR PREPARING THE DISPERSION AND THE COMPOSITION

[0002] TECHNICAL FIELD OF THE INVENTION

[0003] The present invention relates to the technical field of fouling-resistant varnish compositions. More specifically, the invention concerns a dispersion from which a varnish composition is derived, comprising poly(vinyl fluoride) (PVF), a composite membrane comprising a textile core and at least one coating layer covered at least partially by the varnish composition, as well as a method for preparing the dispersion and the composition.

[0004] PREVIOUS STATE OF TECHNOLOGY

[0005] Perfluoroalkyl substances (PFAS) are compounds comprising a carbon chain in which at least one carbon atom is entirely replaced by fluorine atoms, according to the OECD definition. Thus, any chemical substance containing at least one perfluorinated methyl group (-CF3) or a perfluorinated methylene group (-CF2-) is a PFAS. In the case of perfluoroalkyl substances, all hydrogen atoms are replaced by fluorine atoms. These perfluoroalkyl molecules have the general formula C n F2n+l.

[0006] PFAS can also be divided according to molecule size: a distinction is made between polymeric and non-polymeric PFAS, whose properties differ. Non-polymeric PFAS, such as perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS), are small molecules with molecular weights between 300 and 800 Da, which are often soluble and mobile. Polymeric PFAS, such as polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF), with molecular weights generally ranging from 100,000 to several million Da, are primarily stable and relatively immobile. However, their manufacture, use at high temperatures, or end-of-life can release non-polymeric PFAS.

[0007] PFAS comprise over 4,000 compounds, most of which are amphiphilic molecules with varying solubility depending on their functionalization. Furthermore, the electronegativity of fluorine generates a strong C-F bond, giving these molecules significant thermal and chemical stability. They are particularly resistant to hydrolysis and oxidation. Their flame-retardant, waterproofing, and non-stick properties have led to their use in diverse fields, such as fire-fighting foams, electrical wire insulation, non-stick cookware, lubricants, and food packaging.

[0008] However, due to their low reactivity, these substances, and in particular non-polymeric PFAS, remain persistent in the environment. Traces of PFOA and PFOS have been found in some rivers, and even in polar waters. Groundwater is also believed to contain them. Furthermore, non-polymeric PFAS are found in many consumer products, such as food and drinking water.

[0009] Finally, although they are not very volatile, some PFAS are vaporized into the air and can be inhaled. A study by the C8 Science Panel working group demonstrates that high blood concentrations of PFAS are likely to have detrimental health consequences, particularly affecting the liver, the immune system, and fertility. The study links PFAS levels to the incidence of diseases such as high cholesterol, ulcerative colitis, thyroid disease, and kidney cancer.

[0010] Although polymeric PFAS are less of concern due to their low mobility and lower risk of bioaccumulation, they remain under surveillance because of their persistence and potential for secondary contamination.

[0011] The demonstration of the toxicity of these compounds has led public authorities to legislate on the matter. In France, Law No. 2025-188 of February 27, 2025, adopted by the National Assembly and the Senate, provides for a ban, starting from January 1st... er January 2026 the manufacture, import, export and placing on the market of many products containing PFAS.

[0012] From the 1st erBy January 2030, all textile products containing PFAS, with a few exceptions, will be banned. However, in the field of technical textiles, polymeric PFAS are used in certain varnishes because they offer good resistance to soiling, easy cleaning, and significant durability. Some varnish compositions include a copolymer of vinylidene fluoride and hexafluoropropene (poly(VDF-co-HFP)) marketed under the name Kynar®, which is a polymeric PFAS classified as non-hazardous. However, as mentioned previously, PVDF will soon be prohibited, along with all PFAS.

[0013] Document JP 2006183165 describes a laminated material comprising a base fabric and a waterproof coating layer made of a polyvinyl chloride resin-based composition. The coating layer includes a soil-resistant layer consisting of a mixture of acrylic resin and PVDF-based resin.

[0014] US document 3524906 describes a transparent composition comprising an ethyl acrylate polymer, a methyl methacrylate polymer, and a PVDF polymer.

[0015] It is therefore necessary to use alternative compounds to PFAS, which have the same properties but do not present risks to health and the environment.

[0016] PVF is a satisfactory alternative to known PFAS.

[0017] Document KR 102172508 describes a paint composition comprising between 15 and 20%, by weight, of a PVDF or PVF copolymer, and between 2 and 8%, by weight, of a thermosetting acrylic resin prepared in particular from alkyl methacrylate monomers.

[0018] US patent 2025 / 0075093 describes a coating composition comprising PVF, an acrylic copolymer containing amine and / or hydroxyl groups, and an isocyanate or melamine crosslinking agent. The mass ratio of the acrylic copolymer to the PVF is between 0.05:1 and 0.25:1.

[0019] Document EP 2468833 describes a process for producing a polymeric substrate coated with a fluoropolymer composition. The fluoropolymer is selected from PVF homopolymers / copolymers and PVDF homopolymers / copolymers.

[0020] Document KR 102196133 describes a process for producing a membrane comprising a PVF film.

[0021] However, prior art does not allow the implementation of a varnish composition comprising PVF and which has a reduced propensity to fouling, good cleanability and significant durability, to allow in particular application on a composite membrane and, in particular, a flexible composite membrane.

[0022] DETAILED DESCRIPTION OF THE INVENTION

[0023] It is within this framework that the Applicant has developed a composition for varnish without PFAS, comprising poly(vinyl fluoride), and a poly((meth)alkyl acrylate) exhibiting properties at least as satisfactory as those of prior art varnishes.

[0024] In particular, a first object of the present invention relates to a dispersion obtained by the process comprising the following steps:

[0025] a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide,

[0026] b) addition to the dispersion obtained in step a) of a solution of poly(alkyl (meth)acrylate), in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms,

[0027] the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1.

[0028] A second object of the present invention relates to a varnish composition obtained by drying the dispersion according to the first object of the invention, at a temperature between 130°C and 170°C.

[0029] A third object of the invention relates to a composite membrane comprising a textile core and at least one coating layer, covered at least in part by the varnish composition according to the second object of the invention.

[0030] A third object of the invention relates to a method for preparing a dispersion according to the first object of the invention, the method comprising the following steps:

[0031] a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide,

[0032] b) addition to the dispersion obtained in step a) of a solution of poly((alkyl)methacrylate) in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms, the mass ratio poly(vinyl fluoride):poly((alkyl)methacrylate) being between 0.15 and 1.

[0033] Finally, a fourth object of the invention relates to a method for preparing a varnish composition according to the second object of the invention, the method comprising the following steps: a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide,

[0034] b) addition to the dispersion obtained in step a) of a solution of alkyl poly((meth)acrylate) in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms,

[0035] the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1,

[0036] c) drying of the dispersion obtained in step b) at a temperature between 130°C and 170°C.

[0037] Remarkably, the varnish composition according to the invention makes it possible to obtain a PFAS-free composite membrane that exhibits good resistance to soiling, good cleanability, and significant durability. Achieving all these properties is made possible by the combination of the PVF dispersion in one of the solvents described in the present invention, as well as the PVF:alkyl poly(meth)acrylate ratio in this dispersion.

[0038] In the context of the invention, "X and / or Y" means "X," or "Y," or "X and Y." Also included in the invention are all possible combinations of the various disclosed embodiments, whether preferred or given by way of example. Furthermore, where ranges of values ​​are indicated, the limits are included in those ranges. The invention also includes all combinations of the limits of those ranges of values. For example, the ranges of values ​​"1-20, preferably 5-15" imply the disclosure of the ranges "1-5," "1-15," "5-20," and "15-20," and the values ​​1, 5, 15, and 20.

[0039] All the specific and / or preferred embodiments described in the invention may be combined, provided they are not incompatible. In the present invention, percentages (%) correspond to mass (or weight) percentages, defined as the ratio of the mass of a compound to the total mass of the composition. Within the scope of the invention, the total mass of the compounds is equal to the total mass of the varnish composition.

[0040] In the context of the invention, "polymer" means a homopolymer or a copolymer. A homopolymer is a polymer composed of a single identical repeating unit, while a copolymer is composed of two or more different repeating units.

[0041] In the context of this invention, "alkyl (meth)acrylate" includes alkyl acrylates and alkyl methacrylates. Similarly, "poly(alkyl (meth)acrylate" includes poly(alkyl acrylates) and poly(alkyl methacrylates).

[0042] The term "varnish composition" refers to a composition that is a finishing product applied as the final layer to a coating. Generally, varnish compositions are designed to impart certain properties to the coating, such as protection against external elements, improved durability, ease of maintenance, or an aesthetic appearance. The varnish composition according to the invention is considered to be dry. Its thickness is preferably between 3 µm and 15 µm.

[0043] The term "varnish composition" refers to a dry varnish composition. In the context of this invention, "particle size" refers to the particle size distribution based on a number distribution. Regardless of its shape, particle size corresponds to the diameter of a sphere scattering in the same manner as the particle. For example, D50 means that 50% of the particles in the distribution have a size smaller than D50, while the remaining 50% have a size larger than D50. Particle size can be measured using conventional techniques, for example, with a laser measuring device such as the Malvem® Zetasizer® Nano.

[0044] The compounds described in the application are also designated by their CAS number (registration number with the "Chemical Abstracts Service").

[0045] Dispersion

[0046] The dispersion according to the invention is obtained by the process comprising the following steps: a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide,

[0047] b) addition to the dispersion obtained in step a) of a solution of poly(alkyl (meth)acrylate), in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms,

[0048] the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1.

[0049] Polyvinyl fluoride (PVF) (CAS: 24981-14-4) is a semi-crystalline thermoplastic fluoropolymer that possesses, among other things, flame-retardant properties. The repeating unit of this polymer is -CH2-CHF-. It is not considered a PFAS because none of its carbon atoms are entirely substituted by fluorine atoms. Due to its chemical inertness, it cannot be dissolved at room temperature, which makes its formulation very complex. It can, however, form a dispersion in solvents such as propylene carbonate, which has the disadvantage of being an allergenic substance. The polyvinyl fluoride according to the invention is advantageously a homopolymer.

[0050] According to one embodiment, the PVF according to the invention is the product marketed under the name Tedlar® by the company EI DU PONT DE NEMOURS AND COMPANY.

[0051] Preferably, PVF is not cross-linked.

[0052] The alkyl group of alkyl poly((meth)acrylate) consists of 1 to 4 carbon atoms. Preferably, the alkyl group consists of one carbon atom. Preferably, alkyl poly((meth)acrylate) is poly(methyl methacrylate) (also called PMMA (CAS: 9011-14-7)) or poly(methyl acrylate) (CAS: 9003-21-8). Preferably, alkyl poly((meth)acrylate) is poly(methyl methacrylate).

[0053] In the context of the invention, the poly((alkyl)acrylate) is preferably a homopolymer of poly(methyl methacrylate) or a copolymer of poly(methyl methacrylate) and poly(ethyl methacrylate).

[0054] Advantageously, the alkyl poly(meth)acrylate is not crosslinked in the invention.

[0055] Preferably, the alkyl poly((meth)acrylate) has a weight-average molecular weight between 50,000 Da and 700,000 Da, preferably between 60,000 Da and 600,000 Da, more preferably between 70,000 Da and 550,000 Da, even more preferably between 80,000 Da and 500,000 Da, and even more preferably between 90,000 Da and 450,000 Da. Advantageously, this molecular weight range helps to limit fouling of the composite membrane to which the composition is applied.

[0056] In the present invention, the weight-average molecular weight (Mw) is determined by gel permeation chromatography (GPC), which is a method known to the person skilled in the art.

[0057] Advantageously, poly((meth)alkyl acrylate) has a glass transition temperature (T g) between 60°C and 150°C, preferably between 70°C and 140°C, more preferably between 80°C and 130°C, more preferably between 85°C and 125°C, and even more preferably between 95°C and 125°C. Such a T g has the advantage of limiting the fouling of the composite membrane onto which the composition is applied.

[0058] The T gThe concentration is determined by differential scanning calorimetry (DSC), according to ISO 11357-2 (2013), using the TA Instruments® DSC Q2000 instrument. The analysis is performed using the standard method, with sealed aluminum crucibles. The scanning gas is U-grade nitrogen, with a flow rate of 50 mL / min. The temperature ramps used are as follows: isothermal at 0 °C for 5 minutes, from 0 to 200 °C at 10 °C / min; isothermal at 200 °C for 5 minutes, from 200 °C to 0 °C at 20 °C / min; isothermal at 0 °C for 5 minutes, from 0 to 200 °C at 10 °C / min; and finally, isothermal at 200 °C for 5 minutes.

[0059] The dispersion is achieved using a process that improves the dispersion of PVF and reduces its instability, notably by dispersion in 2-butoxyethyl acetate (CAS: 112-07-2) or BEA, N-butyl acetate (CAS: 123-86-4), dibasic esters (CAS: 95481-62-2), also known as DBE, N,N-dimethylformamide (CAS: 68-12-2), or dimethyl sulfoxide (CAS: 67-68-5). The dibasic esters are a mixture of dimethyl succinate, dimethyl glutarate, and dimethyl adipate.

[0060] Unlike propylene carbonate (CAS: 108-32-7), which is used in the prior art to disperse PVF, BEA is non-allergenic and can therefore be handled safely. Preferably, the dispersion in step a) is carried out by sonication, which improves the dispersion of PVF in the solvent, particularly in BEA. Indeed, the application of high shear forces and turbulence enhances PVF dispersion.

[0061] Step a)

[0062] Preferably, the PVF in solid form is introduced into a container as a powder. The PVF is dispersed in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide, preferably the solvent is 2-butoxyethyl acetate, preferably at a concentration of between 5% and 35% by weight, preferably between 10% and 30% by weight relative to the total weight of the dispersion.

[0063] The dispersion is advantageously carried out in step a) at a temperature between 15 °C and 80 °C, preferably between 20 °C and 75 °C, more preferably between 25 °C and 70 °C, and even more preferably between 30 °C and 65 °C. Preferably, the dispersion is carried out for a duration of between 5 and 50 minutes, preferably between 10 and 40 minutes, more preferably between 15 and 35 minutes.

[0064] According to a preferred embodiment, the dispersion is carried out by sonication in step a), preferably using a sonotrode. Preferably, the sonication is performed at a frequency between 5 kHz and 90 kHz, preferably between 10 kHz and 80 kHz, and even more preferably between 20 kHz and 35 kHz. The dispersion is preferably cooled to a temperature between 5°C and 60°C, preferably between 15°C and 55°C, more preferably between 20°C and 50°C, and even more preferably between 40°C and 45°C, for a duration between 5 minutes and 50 minutes, preferably between 10 minutes and 40 minutes, and more preferably between 15 minutes and 35 minutes.

[0065] The dispersion advantageously has a particle size D50 between 1 pm and 50 pm, preferably between 3 pm and 40 pm, preferably between 4 pm and 30 pm, and even more preferably between 5 pm and 10 pm.

[0066] In another embodiment, the dispersion is carried out using zirconia beads. In this embodiment, the dispersion is performed at ambient temperature, preferably between 10°C and 40°C, and preferably between 15°C and 35°C. The shear forces induced by the zirconia beads cause the dispersion to heat up. The dispersion is preferably cooled using a fluid with a temperature between 5°C and 25°C, and preferably between 12°C and 15°C. In this embodiment, the dispersion advantageously has a particle size D50 between 1 µm and 50 µm, preferably between 3 µm and 40 µm, and preferably between 7 µm and 10 µm.

[0067] According to another embodiment, the dispersion is achieved using a rotor-stator.

[0068] Step b)

[0069] A solution of alkyl poly((meth)acrylate), preferably poly(methyl methacrylate), in an N-butyl acetate or N,N-dimethylformamide solvent, preferably N-butyl acetate, is added to the dispersion from step a).

[0070] Preferably, the alkyl poly((meth)acrylate) solution has a mass concentration between 5% and 25%, preferably between 8% and 20%, even more preferably between 10% and 15%.

[0071] Advantageously, the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) is between 0.15 and 1, preferably between 0.25 and 0.8, more preferably between 0.3 and 0.7.

[0072] The resulting mixture is advantageously maintained at a temperature between 20°C and 70°C, preferably between 25°C and 60°C, more preferably between 30°C and 50°C, preferably for a period of between 5 and 50 minutes, preferably between 10 and 40 minutes, more preferably between 15 and 20 minutes. It is advantageously subjected to sonication during this period.

[0073] Optionally, a pigment, such as TiCl, may be added to the dispersion after the sonication step. Optionally, at least one additive, such as a dispersing agent, may be added to the dispersion after the sonication step. Examples of dispersing agents include EFKA® PX 4330 or Solsperse® 3000. Preferably, the pigment and additive content in the dispersion is between 0 and 12% by weight, relative to the total weight of the dispersion, or even between 0.5 and 10%. Composition for varnish

[0074] The varnish composition is obtained by drying the dispersion of the invention, at a temperature between 130°C and 170°C.

[0075] This drying is advantageously carried out during a step c), subsequent to the step b), previously described.

[0076] Preferably, the varnish composition is obtained by the process comprising the following steps:

[0077] a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide,

[0078] b) adding to the dispersion obtained in step a) a solution of alkyl poly((meth)acrylate in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms, the mass ratio poly(vinyl fluoride):alkyl poly((meth)acrylate) being between 0.15 and 1, c) drying the dispersion obtained in step b) at a temperature between 130°C and 170°C.

[0079] Step c)

[0080] The dispersion obtained at the end of step b) is dried at a temperature between 130°C and 180°C, preferably between 135°C and 170°C, or even between 140°C and 145°C. The drying step is advantageously carried out in an oven. It can last between 1 and 3 minutes.

[0081] After this drying stage, the varnish composition is obtained.

[0082] Preferably, the nail polish composition includes:

[0083] i) between 20% and 60% by weight of poly(vinyl fluoride),

[0084] ii) between 40% and 80% by weight of alkyl poly((meth)acrylate), the alkyl group consisting of 1 to 4 carbon atoms,

[0085] compared to the total weight of the varnish composition.

[0086] These proportions are evaluated in relation to the dry varnish composition. Preferably, the varnish composition according to the invention comprises:

[0087] i) between 25% and 55%, or even between 28% and 50%, or even between 30% and 40%, or even between 32% and 38%, by weight of poly (vinyl fluoride),

[0088] ii) between 45% and 75%, or even between 50% and 72%, or even between 60% and 70%, or even between 62% and 68%, by weight of poly((meth)alkyl acrylate), the alkyl group consisting of 1 to 4 carbon atoms, preferably of poly(methyl methacrylate),

[0089] compared to the total weight of the varnish composition.

[0090] Optionally, the varnish composition may include a pigment, for example, TiCh. Optionally, the varnish composition may include at least one additive, for example, a dispersing agent. Examples of dispersing agents include EFKA® PX 4330 or Solsperse® 3000. Preferably, the pigment and additive content in the varnish composition is between 0 and 7% by weight, or even between 0.1 and 6%, relative to the total weight of the varnish composition.

[0091] Advantageously, the varnish composition is intended to be applied to the composite membrane, which is the subject of the invention.

[0092] The respective proportions of PVF and poly(alkyl (meth)acrylate) help to limit fouling and improve the cleanability of the composite membrane.

[0093] Composite membrane

[0094] According to the invention, the composite membrane comprises a textile core and at least one coating layer. The varnish composition according to the invention is applied to the coating layer.

[0095] The composition of the textile core depends on the intended use of the composite membrane. A skilled professional will select the appropriate core composition based on the application of the composite membrane. Advantageously, the textile core is chosen from a group consisting of at least one fabric, woven material, non-woven material, grid, yarn, fiber, filament, or combination thereof. The materials composing the textile core are preferably chosen from a group consisting of polyester, polyamide, nylon, viscose, cotton, linen, and glass.

[0096] Advantageously, the textile core comprises at least two faces, at least one of which, advantageously both, is covered with the coating layer. Preferably, the coating layer consists of at least one polymer selected from the group consisting of polyvinyl chloride (CAS: 9002-86-2), poly(methyl methacrylate), and combinations thereof. The coating layer may further comprise at least one compound selected from the group consisting of: a plasticizer, a thermal stabilizer, a flame retardant, a UV inhibitor, a pigment, and combinations thereof.

[0097] Advantageously, the membrane is flexible, meaning it has a stiffness between 30 and 80 Taber units, determined using a Taber® stiffness meter, according to ISO 2493-2 (2011), ASTM D5342 and ASTM D5650 standards. The stiffness is determined using a Taber® Stiffness device, Model 150-E, with a 15° bending angle.

[0098] The membrane according to the invention can be used, for example, in the fields of construction, tensile architecture, or even in modular structures.

[0099] Among the possible application techniques for the varnish composition onto the coating layer, rotogravure can be mentioned. Preferably, the thickness of the varnish composition is between 3 µm and 15 µm, more preferably between 5 µm and 12 µm.

[0100] Dispersion preparation process

[0101] The section concerning dispersion above also applies to the process of preparing the dispersion.

[0102] Method for preparing the composition for varnish

[0103] The section concerning the varnish composition above also applies to the process of preparing the varnish composition.

[0104] DESCRIPTION OF THE FIGURES

[0105] Figure 1 is a graph representing the evolution of the resistance of a composite membrane, on which a varnish composition is deposited, according to the mass percentage of PVF in the varnish composition.

[0106] Figure 2 is a graph representing the evolution of fouling on a composite membrane, onto which a varnish composition is deposited, as a function of the glass transition temperature of PMMA. EXAMPLES OF IMPLEMENTATION OF THE INVENTION

[0107] Abbreviations:

[0108] PVF: polyvinyl fluoride

[0109] BEA: 2-Butoxyethyl acetate

[0110] DBE: dibasic esters

[0111] PMMA: poly(methyl methacrylate)

[0112] CP: propylene carbonate

[0113] PVC: polyvinyl chloride

[0114] Example 1: Preparation of dispersions and compositions for varnishes

[0115] The preparation of the dispersion El, according to the invention, is carried out according to the following protocol:

[0116] i) weighing of 79 mL of the BEA solvent,

[0117] ii) addition of 20 g of PVF homopolymer powder, at an ambient temperature of 23°C, iii) sonication (power: 40 W, amplitude: 30%, frequency: 24 kHz), then maintaining the temperature at 45°C for 15 to 20 minutes,

[0118] (iv) preparation of a PMMA homopolymer solution with a molecular weight greater than 400,000 Da characterized by GPC, in an N-butyl acetate solvent, at a mass concentration of 10%,

[0119] v) addition of the PMMA solution to the PVF dispersion, at an ambient temperature of 23°C, vi) sonication (power: 100 W, amplitude: 70%, frequency: 24 kHz), then maintaining the temperature at 55°C for 30 minutes,

[0120] vii) addition to the dispersion of TiCE at 58% by weight in a BEA solvent and 6.3% additive.

[0121] The process is repeated to prepare IEC to CE5 dispersions, by modifying the mass percentage of PVF during the process, the nature of the PVF solvent in the dispersions, and / or the molecular weight of PMMA. These parameters are summarized in Table 1.

[0122] Acetate Weight TiO2

[0123] Ratio PVF BEA DBE CP PMMA of N-molecular + Mass Dispersions (%) (%) (%) (%) (%) PMMA Butyl Additive PVF / PMMA (%) (Da) (%)

[0124] El 4.7 18.6 0 0 8 67.8 > 400000 0.9 0.59 CEI 29.3 0.7 0 45.5 3.3 0 14000 21.2 8.9 CE2 11.5 0 0 13.5 5.6 69.4 > 400000 0 2.05

[0125]

[0126] CE3 11.5 0 0 13.5 5.6 69.4 119000 0 2.05CE4 10.86 43.1 0 0 4.7 40.25 > 400000 1.09 2.3

[0127]

[0128] CE5 18.86 74.7 0 0 0.5 4.47 > 400000 1.47 35.72 Table 1: Dispersions El to CE5 (E=invention, CE=comparative example)

[0129] The El to CE5 dispersions are applied to the PVC coating layers covering both sides of a composite membrane with a PET textile core. The composite membrane is intended for use as a tensile architectural element. The membranes coated with the dispersions are then dried in an oven at a temperature of 140°C for 1 minute to obtain the El to CE5 varnish compositions.

[0130] The mass percentages of PVF and PMMA contained in the compositions for El to CE5 varnishes are indicated in Table 2.

[0131] Composition for PVF (%) PMMA (%) TiU2+ additive (%) varnish

[0132] El 35 59 6 IEC 64 7.2 28.8 CE2 67 33 0

[0133] CE3 67 33 0

[0134] CE4 65 29 6

[0135]

[0136] CE5 90.8 2.5 6.7 Table 2: Compositions for varnishes El to CE5 (E=invention, CE=comparative example)

[0137] Example 2: Evaluation of the properties of compositions for El to CE5 varnishes

[0138] Each El to CE5 varnish composition is considered compliant according to the invention if it meets the following requirements:

[0139] - Ability to adhere to the PVC coating layer: the protocol for evaluating this criterion consists of applying the varnish composition to the PVC coating layer of the composite membrane and performing a scrub or wrinkle test of 4000 cycles, according to standard NF EN ISO 5981. The number of dry scrub cycles performed before the composition loses its adhesion to the PVC is then determined. An adhesive tape test is then carried out according to standard ASTM D3359-23;

[0140] - Membrane resistance to fouling: The protocol for evaluating this criterion involves fouling the membrane by spraying it with a standardized fouling powder and measuring the color difference compared to the membrane in its initial state. The color difference (AD) is measured using the parameters of the L*a*b* system, which a person skilled in the art can define. The lower the value, the more resistant the membrane is to fouling. - Membrane cleanability: The protocol for evaluating this criterion involves cleaning the previously fouled area of ​​the membrane with a water-soaked sponge and measuring the color difference compared to the membrane in its initial state. The color difference (AD) is measured using the parameters of the L*a*b* system, which a person skilled in the art can define. The lower the value, the more cleanable the membrane.

[0141] The results are summarized in Table 3.

[0142] Composition for Resistance to

[0143] PVC adhesion, varnish cleanability, and resistance to soiling

[0144] El + + + IEC - + NA CE2 - + + CE3 - + + CE4 + - -

[0145]

[0146] CE5 - - - Table 3: Properties of compositions for El to CE5 varnishes

[0147] + : compliant

[0148] - : non-compliant

[0149] NA: Not applicable

[0150] It is thus shown that only composition E1, meeting the definition of the invention, satisfies the criteria of adhesion to PVC, fouling reduction, and cleanability. Composition CEI (obtained by dispersion in CP, with a PVF / PMMA ratio of 8.9) and compositions CE2 and CE3 (obtained by dispersion in CP, with a PVF / PMMA ratio of 2.05) do not adhere to the PVC membrane. Composition CE4 (obtained by dispersion in BEA, with a PVF / PMMA ratio of 2.3) is not resistant to fouling and is not cleanable. Composition CE5 (obtained by dispersion in BEA, with a PVF / PMMA ratio of 35.72) does not adhere to PVC, is not resistant to fouling, and is not cleanable.

[0151] Example 3: Evaluation of the influence of the proportion of PVF in the composition on the cleanability and fouling of the membrane

[0152] Varnish compositions 6 through 9 are prepared according to the same protocol as described in Example 1, varying the mass percentage of PVF in each composition. PMMA has a molecular weight greater than 400,000 Da. Compositions 6 through 9 are applied to a PVC coating layer of a composite membrane as described in Example 2. The ability of each membrane to resist fouling and its cleanability are evaluated. The results are summarized in Figure 1 and Table 4.

[0153] Composition of the fouling

[0154] PVF (%) PMMA (%) Cleanability (AE) for varnish (AE)

[0155] 6 20 80 7.4 9.5 7 30 70 7.4 7.8 8 35 65 9 6

[0156]

[0157] Table 4: Properties of compositions for varnishes 6 to 9

[0158] It appears that the membrane's resistance to fouling decreases with increasing PVF mass percentage in the varnish composition. Conversely, the membrane's cleanability increases with increasing PVF mass percentage. A satisfactory compromise is achieved with a PVF mass percentage between 30% and 40% by weight.

[0159] Example 4: Evaluation of the influence of the glass transition temperature of PMMA on membrane fouling

[0160] The compositions for varnishes 10 to 16 are prepared according to the same protocol as that described in Example 1, using PMMA with different T g Their composition is that of the varnish composition of Example 1 according to the invention, namely 35% PVF and 60% PMMA by weight, relative to the total weight of the varnish composition. PMMA has a molecular weight greater than 400,000 Da.

[0161] Compositions 10 to 16 are applied to a PVC coating layer of a composite membrane as described in Example 2. The fouling capacity of each membrane is evaluated. The results are summarized in Figure 2 and Table 5. Composition for

[0162] Tg PMM A (°C) Fouling ( \ E) varnish

[0163] 10 40 26.2 11 65 31.6 12 86 11.5 13 98 10.2 14 104 9.7 15 105 9.1

[0164]

[0165] 16 122 8.8 Table 5: Properties of compositions 10 to 16

[0166] It appears that membrane fouling decreases as a function of temperature. g PMMA. Plus the T g The higher the temperature of PMMA, particularly above or equal to 85°C, the more resistant the membrane is to fouling. Conversely, it is observed that for a glass transition temperature below 85°C, fouling is significant.

[0167] Example 5: Preparation of dispersions according to the prior art and evaluation of the properties of the resulting compositions

[0168] Dispersion CE6 to CE9 was performed according to the protocol described in US document 2025 / 0075093. PVF was dispersed in CP. Details of the dispersions are summarized in Table 6.

[0169] Dispersions PVF / PMMA mass ratio

[0170] CE6 (Example 1 of US 2025 / 0075093) 7

[0171] CE7 (Example 3 of US 2025 / 0075093) 4

[0172] CE8 (Example 5 of US 2025 / 0075093, PVF 10

[0173] (crosslinked without epoxy)

[0174] CE9 (Example 6 of US 2025 / 0075093) 5

[0175]

[0176] Table 6: Dispersions according to US 2025 / 0075093

[0177] The CE6 to CE9 dispersions are applied to layers of PVC coating covering both sides of a flexible composite membrane comprising a PET textile core, as described in Example 1, and then dried in an oven at 140°C for 1 min, to obtain the corresponding CE6 to CE9 varnish compositions.

[0178] The ability of compositions CE6 to CE9 to adhere to the PVC coating layer is evaluated according to the protocol described in Example 2.

[0179] None of the CE6 to CE9 compositions adhere to the PVC. In particular, CE6 and CE7 compositions detach from the membrane and exhibit a crazing appearance. Composition CE7 even causes the PVC to shrink. Compositions CE8 and CE9 detach completely from the PVC membrane and exhibit poor spreading and a very crazing appearance.

Claims

DEMANDS 1. Dispersion obtained by the process comprising the following steps: a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide, b) addition to the dispersion obtained in step a) of a solution of poly(alkyl (meth)acrylate) in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms, the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1.

2. Dispersion according to claim 1, characterized in that the poly(alkyl (meth)acrylate) has a weight average molecular weight between 50000 Da and 700000 Da, preferably between 60000 Da and 600000 Da.

3. Dispersion according to any one of the preceding claims, characterized in that the poly((meth)alkyl acrylate) has a glass transition temperature between 60°C and 150°C, preferably between 70°C and 140°C.

4. Dispersion according to any one of the preceding claims, characterized in that the poly((meth)alkyl acrylate) is the poly(methyl methacrylate).

5. Dispersion according to any one of the preceding claims, characterized in that the dispersion is carried out by sonication in step a).

6. Dispersion according to any one of the preceding claims, characterized in that the dispersion in step a) is carried out at a temperature between 15°C and 80°C.

7. Dispersion according to any one of the preceding claims, characterized in that the poly(alkyl (meth)acrylate) solution has a mass concentration of between 5% and 25%, preferably between 8% and 20%.

8. Varnish composition characterized in that the varnish composition is obtained by drying the dispersion according to any one of the preceding claims, at a temperature between 130°C and 170°C.

9. Varnish composition according to claim 8, characterized in that the varnish composition comprises: i) between 20% and 60% by weight of poly(vinyl fluoride), and ii) between 40% and 80% by weight of alkyl poly((meth)acrylate), the alkyl group consisting of 1 to 4 carbon atoms, compared to the total weight of the varnish composition.

10. Composite membrane comprising a textile core and at least one coating layer, characterized in that the varnish composition according to claim 8 or 9 covers at least part of said coating layer.

11. Composite membrane according to claim 10, characterized in that the coating layer is made up of at least one polymer selected from the group consisting of polyvinyl chloride, poly(methyl methacrylate) and their combination.

12. Composite membrane according to claim 10 or 11, characterized in that the textile core is selected from the group consisting of at least one fabric, woven material, non-woven material, grid, yarn, fiber, filament, and combinations thereof.

13. A method for preparing a dispersion according to any one of claims 1 to 7, characterized in that the method comprises the following steps: a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide, b) addition to the dispersion obtained in step a) of a solution of poly(alkyl (meth)acrylate) in a solvent chosen from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms, the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1.

14. A process for preparing a varnish composition according to claim 8 or 9, characterized in that the process comprises the following steps: a) preparation of a dispersion of poly(vinyl fluoride) in a solvent selected from the group consisting of 2-butoxyethyl acetate, N-butyl acetate, dibasic esters, N,N-dimethylformamide and dimethyl sulfoxide, b) addition to the dispersion obtained in step a) of a solution of poly(alkyl (meth)acrylate) in a solvent selected from the group consisting of N-butyl acetate and N,N-dimethylformamide, the alkyl group consisting of 1 to 4 carbon atoms, the mass ratio poly(vinyl fluoride):poly(alkyl (meth)acrylate) being between 0.15 and 1, c) drying of the dispersion obtained in step b) at a temperature between 130°C and 170°C.