Processes for polymerising olefins

By treating a settled bed of polymer particles in a high pressure separator with controlled volumes of separating gas, the process addresses carryover issues in multistage polymerization, ensuring optimal polymer production with desirable properties and reduced process complexity.

WO2026238923A1PCT designated stage Publication Date: 2026-11-19BOREALIS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064148
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing multistage polymerization processes face challenges in preventing the carryover of hydrogen and certain diluents or reactants from one reactor stage to another, which can negatively impact the molecular weight and properties of the polymer produced in downstream reactors.

Method used

A process involving a slurry loop reactor followed by a gas phase reactor, where a settled bed of polymer particles in a high pressure separator is treated with separating gas to separate hydrocarbon and hydrogen, controlling the gas volume to 25% to 800% of the void volume, thereby reducing carryover and maintaining optimal reactor conditions.

Benefits of technology

This method effectively minimizes the risk of hydrocarbon and hydrogen carryover, ensuring the production of polymers with desirable properties and multimodal capabilities, while optimizing separation efficiency and reducing process requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026064148_19112026_PF_FP_ABST
    Figure EP2026064148_19112026_PF_FP_ABST
Patent Text Reader

Abstract

This disclosure relates to a process for polymerising olefins, said process comprising: polymerising olefin monomer, optionally in the presence of comonomer, in a first reactor to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen; introducing the first product into a high pressure separator; allowing the particles of the first polymer component to settle as a settled bed in a lower region of the high pressure separator; passing separating gas through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed; wherein the volume of separating gas passed through the settled bed is equal to 25% to 800% of the void volume of the settled bed, said void volume being the total volume of the interstices between particles of the first polymer component in the settled bed; recovering the separated hydrocarbon and / or hydrogen in a gas recovery unit; transferring the particles of the first polymer component from the high pressure separator to a second reactor; and polymerising olefin monomer, optionally in the presence of comonomer, in the second reactor in the presence of the particles of the first polymer component to produce a second polymer component.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PROCESSES FOR POLYMERISING OLEFINS

[0002] FIELD OF THE DISCLOSURE

[0003] The present disclosure relates to a process for polymerising olefins in a multistage polymerisation process configuration.

[0004] BACKGROUND OF THE DISCLOSURE

[0005] Multistage polymerisation processes (e.g. Borstar PE or PP and Spheripol PP) employ multistage reactor configurations to provide the multimodal capability for achieving easy-to-process resins with desirable properties. In such processes, a combination of e.g. slurry loop reactors in series, followed by a gas phase reactors may be employed to produce a range of polyolefins.

[0006] When producing polyolefins in a multistage reactor configuration, it may be desirable to restrict or prevent the flow of certain diluents and / or reactants from one polymerisation stage to the next. For example, the carryover of hydrogen from an upstream polymerisation reactor to a downstream polymerisation reactor can reduce the molecular weight of the polymer produced in the downstream reactor and this may be undesirable in terms of the specifications of the final product. Similarly, the carryover of certain comonomer(s) from an upstream reactor to a downstream reactor may have a negative impact on the polymer produced in the downstream reactor.

[0007] Various methods have been developed to separate e.g., hydrogen and / or hydrocarbons between stages of a multistage polymerisation system. For example, WO 2004 / 039847 describes a process in which a polymer slurry containing polymer and a fluid mixture containing diluent, monomers and optionally hydrogen is withdrawn from an upstream slurry loop reactor. This slurry is optionally concentrated by removing part of the hydrocarbon diluent. The concentrated slurry is then passed to a high pressure flash unit, where essentially all of the remaining hydrocarbon diluent is removed to provide a product stream containing a mixture of polymer solids and gases. The product stream from the flash unit is preferably purged countercurrently in a gas-exchange zone with essentially hydrogen-free gas to reduce the amount of hydrogen carryover to the gas phase reactor.Nonetheless, there may be a risk of carryover of hydrocarbon (e.g., monomers and / or comonomers) and / or hydrogen that may compromise polymerisation in the downstream gas reactor. It is among the objects of embodiments of the present invention to further minimise the risk of such carryover.

[0008] BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 depicts a schematic view of a multistage polymerisation process configuration for carrying out a process according to an example of the present disclosure.

[0010] DESCRIPTION OF THE DISCLOSURE

[0011] According to a first aspect, there is provided a process for polymerising olefins in multistage polymerisation process configuration. The process comprises polymerising olefin monomer, optionally in the presence of comonomer, in a first reactor to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen, wherein preferably the first reactor is a slurry loop reactor. The first product is introduced into a high pressure separator, and the particles of the first polymer component are allowed to settle as a settled bed in a lower region of the high pressure separator. Separating gas is passed through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed. The volume of separating gas passed through the settled bed is equal to 25% to 800% of the void volume of the settled bed, wherein preferably the volume of separating gas passed through the settled bed is equal to 25% to 400%, more preferably 25% to 200%, more preferably 30% to 180%, more preferably 50 to 150%, more preferably 60 to 140%, yet more preferably 70 to 130%, even more preferably 80 to 120%, for example, 90 to 110% of the void volume of the settled bed.. In a certain aspect the volume of separating gas passed through the settled bed is equal to 25% to 200% of the void volume of the settled bed. The void volume is the total volume of the interstices between particles of the first polymer component in the settled bed. The separated hydrocarbon and / or hydrogen is recovered in a gas recovery unit. Advantageously, once treated with the separating gas, the particles of the first polymer component from the high pressure separator are transferred to a second reactor, preferably a gas phase reactor. Olefin monomer, optionally in the presence of comonomer, is then polymerised in the second reactor (preferably gas phase reactor) in the presence of the particles of the first polymer component to produce a second polymer component.

[0012] As set out above, the first reactor is preferably a slurry loop reactor.As set out above, the second reactor is preferably a gas phase reactor.

[0013] As set out above, the volume of separating gas passed through the settled bed is preferably equal to 25% to 200% of the void volume of the settled bed.

[0014] Therefore, according to a preferred aspect, there is provided a process for polymerising olefins in multistage polymerisation process configuration. The process comprises polymerising olefin monomer, optionally in the presence of comonomer, in a slurry loop reactor to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen. The first product is introduced into a high pressure separator, and the particles of the first polymer component are allowed to settle as a settled bed in a lower region of the high pressure separator. Separating gas is passed through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed. The volume of separating gas passed through the settled bed is equal to 25% to 200% of the void volume of the settled bed. The void volume is the total volume of the interstices between particles of the first polymer component in the settled bed. The separated hydrocarbon and / or hydrogen is recovered in a gas recovery unit. Advantageously, once treated with the separating gas, the particles of the first polymer component from the high pressure separator are transferred to a gas phase reactor. Olefin monomer, optionally in the presence of comonomer, is then polymerised in the gas phase reactor in the presence of the particles of the first polymer component to produce a second polymer component.

[0015] According to the first aspect, the concentration of first polymer component in the first product introduced into the second reactor (preferably high pressure gas phase reactor) is 20 to 65% by weight, preferably 30 to 60% by weight, more preferably 35-58% by weight.

[0016] Preferably, the volume of separating gas passed through the settled bed is equal to preferably 25% to 400%, more preferably 25% to 200%, more preferably 30% to 180%, more preferably 50 to 150%, yet more preferably 60 to 140%, even more preferably 70 to 130%, yet even more preferably 80 to 120%, for example, 90 to 110% of the void volume of the settled bed. In a certain aspect, the volume of separating gas passed through the settled bed is 25% to 200% of the void volume of the settled bed.

[0017] Void volume is a difference of total volume and volume of solids (first polymer). The void volume of the settled bed may be determined from the material density of the first polymer component, average size of first polymer and the density of the settled bed and may bedetermined from bulk density of the settled bed and density of the first polymer component. The density of the first polymer component may be determined by applicable standard method(s) The density of the settled bed may be determined from the bulk density of the settled bed. The material density (i.e. the density of the polymer material itself) can be determined by any suitable method, preferably determined according to ISO 1183-1.

[0018] By allowing the particles of the first polymer component to settle as a settled bed in a lower region of the high pressure separator and passing separating gas through the settled bed, it is possible to separate hydrocarbon and / or hydrogen from the settled bed. This is advantageous in producing polymer with desirable properties in reactor downstream of high pressure separator, i.e., multistage reactor configurations to provide the multimodal capability for achieving easy- to- process resins with desirable properties. This may be advantageous as it reduces the risk of carryover of hydrocarbon (e.g., monomers and / or comonomers) and / or hydrogen that may compromise polymerisation in the downstream gas reactor. In the present disclosure, the volume of separating gas relative to the void volume of the settled bed is controlled such that it is equal to 25% to 800% of the void volume of the settled bed, wherein preferably the volume of separating gas passed through the settled bed is equal to 25% to 200% of the void volume of the settled bed. Advantageously, this optimises the separation or removal of hydrocarbon and / or hydrogen from the interstices between the particles of the first polymer component in the settled bed, while, at the same time, reduces the apparatus and / or process requirements for recovering the separating gas downstream. Furthermore, by controlling the amount of separating gas flowing through the high pressure separator, it is possible to maintain the pressure of the high pressure separator above the pressure of operating pressure of the gas recovery unit. This can reduce the risk of backflow of e.g., hydrogen and / or hydrocarbon from the gas recovery unit to the high pressure separator, which may, in turn, reduce the risk of re-adsorption of the hydrogen and / or hydrocarbon to the particles of the first polymer component. Similarly, by controlling the amount of separating gas flowing through the high pressure separator, it is possible to maintain the pressure of the high pressure separator above the pressure of second reactor. This can reduce the risk of backflow from the second reactor to the high pressure reactor.

[0019] Another advantage may be that a polymer with desirable properties can be produced in a reactor downstream of high pressure separator, i.e., in a multistage reactor configuration to provide the multimodal capability for achieving easy- to- process resins with desirable properties.The high pressure separator is operated above the operating pressure of the second reactor. As set out above, the second reactor is preferably a gas phase reactor. By controlling the amount of separating gas flowing through the settled bed (25% to 800% of the void volume), a barrier is created between high pressure separator and second reactor and this reduces the risks of hydrogen and / or hydrocarbon passing from the first reactor (preferably slurry loop reactor) and / or gas recovery unit to the second reactor. By controlling the amount of separating gas flowing through the settled bed (25% to 800% of the void volume, preferably 25% to 200%), a barrier is created between high pressure separator and the second reactor, and this reduces the risks of backflow from the second reactor to the high pressure reactor. To flow separating gas into the settled bed, the separating gas may be introduced directly into a lower section of high pressure separator. Alternatively or additionally, the separating gas may be introduced above a valve positioned in the pipework between the high pressure separator and second reactor and / or below the valve positioned in the pipework between the high pressure separator and second reactor.

[0020] The high pressure separator may be operated at a pressure that is 0.2 to 2.0 bar higher than the operating pressure of the second reactor; and / or the high pressure separator may be operated at a pressure that is 0.1 to 2.0 bar higher than the operating pressure of the gas recovery unit., preferably 0.1 to 1.5 bar, more preferably 0.2 to 1.0 bar and more preferably 0.2 to 0.7 bar, more preferably 0.2 to 0.5 bar higher than the operating pressure of the gas recovery unit.

[0021] A valve may be positioned downstream of the high pressure separator. The valve may be a rotary valve and / or control valve(s). The valve may be heated e.g., with heating jackets to reduce the risk of any hydrocarbons from condensing.

[0022] The valve may be connected directly to high pressure separator or positioned in a conduit or pipe from the high pressure separator, for example, in a conduit or pipe connected to an outlet in the lower region of the high pressure separator. The whole high pressure separator or lower section of high pressure separator, conduit or pipe may be heated to reduce the risk of any hydrocarbons from condensing.

[0023] The separating gas may be passed through the settled bed using any suitable method. For example, the separating gas may be introduced into an inlet located in the lower region of the high pressure separator. The inlet may positioned to introduce separating gas directly into the region where the settled bed forms. Alternatively or additionally, the separating gas may be introduced downstream of the high pressure separator. This separating gasintroduced may be introduced into a conduit or pipe connected to the high pressure separator, and this separating gas may be directed upwards through the settled bed via the conduit or pipe. This separating gas may further be introduced above and below the valve positioned below the high pressure separator, valve may be connected directly or via a conduit or pipe connected to the high pressure separator.

[0024] A valve may be positioned downstream of the high pressure separator. The valve may be a rotary valve(s) and / or control valve(s). The valve may be heated e.g., with heating jackets to reduce the risk of hydrocarbons from condensing.

[0025] The valve may be opened to allow e.g. particles of the first polymer component to be transferred to the downstream gas reactor. However, when the valve is closed, the valve serves to retain the particles of the first polymer component in the high pressure separator, allowing the settled bed to form e.g., for a desired residence time. The settled bed may occupy the lower region of the high pressure separator, as well as the conduit or pipe section upstream of the valve. The valve may be kept in a closed position for sufficient time to allow for the particles to settle to form a settled bed and for the separating gas to be passed through the settled bed.

[0026] As discussed above, the separating gas may displace at least some of any hydrogen and / or hydrocarbon that may be present in the interstices between the particles of the first polymer component. The separating gas may displace at least 30 volume%, preferably at least 40 volume %, more preferably at least 50 volume %, yet more preferably at least 60 volume %, even more preferably at least 70 volume % of any hydrogen and / or hydrocarbon that may be present in the void volume in the settled bed. In a preferred embodiment, the separating gas may displace at least 80 volume %, preferably at least 90 volume %, more preferably at least 95 volume %, even more preferably at least 99 volume % of any hydrogen and / or hydrocarbon that may be present in the void volume in the settled bed.

[0027] When a valve is used, the separating gas may be introduced upstream and / or downstream of the valve. The separating gas introduced upstream of the valve may be passed upstream through the settled bed. The separating gas introduced downstream of the valve may help to reduce the risk of backflow from the downstream reactor, and further reduce the risk of any entrained hydrogen and / or hydrocarbon reaching the downstream gas reactor.

[0028] The particles of the first polymer component may be retained in the high pressure separator for a residence time of 5 seconds to 10 minutes, preferably 5 seconds to 8 minutes, morepreferably 5 seconds to 5 minutes, more preferably 10 seconds to 3 minutes, for example, 15 seconds to 2 minutes. The retention time can be controlled by the use of the valve, e.g., rotary valve. The retention time can allow for adequate settling, as well as treatment with the separating gas.

[0029] Once treated with the separating gas, the particles of the first polymer component may be transferred to the second reactor (preferably a gas phase reactor) by gravity and / or by using a conveying gas.

[0030] The high pressure separator is operated at a pressure of 18 to 22 barg. The high pressure separator is operated at a temperature of 60 to 75 degrees C. Selection of operating pressure of high pressure separator is linked to operating pressure of a second reactor (preferably a gas phase reactor). The high pressure separator may be operated at a pressure higher than the operating pressure of the second reactor (see paragraph on operating pressure of high pressure separator, row 21). Operating temperature of high pressure separator is selected to avoid risk any hydrocarbons from condensing and minimize the risk of further / continue polymerization of first polymer; temperature is high enough to avoid risk any hydrocarbons from condensing but also low enough to minimize the risk of (or reduces) polymerization of first polymer; at higher temperature polymerization reaction of first polymer will accelerate in the presence of monomer and / monomer.

[0031] Any suitable separating gas may be used. Preferably, the separating gas comprises propane.

[0032] Polymerisation

[0033] As mentioned above, the process of the present disclosure is a process for polymerising olefins preferably in multistage polymerisation process configuration. The process comprises polymerising, in a reactor, first olefin monomer, in the presence of a polymerisation catalyst to produce a first polymer component. Optionally, the first olefin monomer may also be co-polymerised with a comonomer to produce the first polymer component. The process also comprises polymerising, in a downstream second reactor (preferably gas phase reactor), second olefin monomer in the presence of the first polymer component to produce a second polymer component. The second olefin monomer may also be co-polymerised with a comonomer to produce the second polymer component. The first monomer may be the same or different, preferably the same as the second monomer. Thecomonomer used to form the first polymer component and the second polymer component may be the same or different.

[0034] To distinguish the reactor(s) in which the first polymer component is produced from the downstream second reactor in which the second polymer component is produced, the reactor(s) in which the first polymer component is produced can be referred to as the upstream reactor(s). Polymerisation in the upstream reactor(s) may be referred to upstream polymerisation, while polymerisation in the downstream second reactor(s) may be referred to as downstream polymerisation. Preferably, the downstream reactor is a gas phase reactor.

[0035] The first polymer component is transferred to the downstream reactor (preferably gas phase reactor) from the upstream reactor(s), such that the second olefin polymer component is produced in the presence of first polymer component. Additionally, the polymerisation catalyst may be transferred from the upstream reactor(s) to the downstream reactor (preferably gas phase reactor) so that the second olefin monomer is produced in the presence of both the first polymer component and the polymerisation catalyst from the upstream reactor(s).

[0036] Preferably, the same catalyst is used in each step and ideally, it is transferred from prepolymerisation (if employed) to subsequent polymerisation steps in sequence.

[0037] Prepolymerisation

[0038] The process may include a prepolymerisation step. The purpose of the prepolymerisation is to polymerise a small amount of polymer onto the catalyst at a low temperature and / or a low monomer concentration. By prepolymerisation, it may be possible to improve the performance of the catalyst in the subsequent polymerization process stages.

[0039] The catalyst components are preferably all introduced to the prepolymerisation step when a prepolymerisation step is present. Preferably, the reaction product of the prepolymerisation step is introduced to the polymerisation in which the first polymer component is produced.

[0040] In some instances, the solid catalyst component and the cocatalyst can be fed separately. Here, it is possible that only a part of the cocatalyst is introduced into the prepolymerisation stage and the remaining part into subsequent polymerisation stages. Also in such cases it may not be necessary to introduce as much cocatalyst into the prepolymerisation stage to achieve sufficient polymerisation therein.It is understood within the scope of the invention, that the amount or polymer produced in the prepolymerisation lies within 0.5% to 7 wt% in respect to the final multimodal (co)polymer.

[0041] Producing the first polymer component

[0042] As discussed above, the process of the present disclosure preferably comprises polymerising, in an upstream reactor, first olefin monomer, optionally in the presence of at least comonomer (an alpha olefin comonomer), in the presence of a polymerisation catalyst to produce a first polymer component.

[0043] Preferably, the first olefin monomer is propylene or ethylene, preferably ethylene.

[0044] The first olefin monomer may be polymerised to form a homopolymer as the first polymer component. Alternatively, the first olefin monomer may be polymerised to form a copolymer of the first olefin monomer and the at least one alpha olefin comonomer as the first polymer component.

[0045] For example, propylene may be polymerised in the upstream reactor to produce propylene homopolymer as the first polymer component. Alternatively, propylene may be copolymerised with at least one alpha olefin comonomer to produce a propylene copolymer as the first polymer component.

[0046] In one embodiment, ethylene is polymerised in the upstream reactor to produce ethylene homopolymer as the first polymer component. Alternatively, ethylene may be copolymerised with at least one alpha olefin comonomer to produce ethylene copolymer as the first polymer component.

[0047] Where an alpha olefin comonomer is used, the alpha olefin comonomer may be selected from a C2 to C10 alkene. For the avoidance of doubt, the alpha olefin comonomer is different from the first olefin monomer polymerised in the upstream reactor. Suitable alpha olefin comonomers include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-hexene, 1 -octene, 1 -nonene and 1 -decene. Preferably, the alpha olefin comonomer is selected from at least one of ethylene, propylene, 1-butene, 1-hexene, and 1 -octene. Where the first olefin monomer is propylene, the alpha olefin comonomer may be ethylene, 1-butene, 1-hexene and / or 1 -octene. Where the first olefin monomer is ethylene, the alpha olefin comonomer may be propylene, 1-butene and / or 1-hexene. Where an alpha olefincomonomer is used, one or more alpha comonomers may be employed. Preferably, one or two alpha comonomers are employed.

[0048] The alpha olefin comonomer content of the first polymer component may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the first polymer component is a polypropylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the first polymer component is a polyethylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%.

[0049] The upstream polymerisation may take place in any suitable type of reactor. Preferably, the upstream polymerisation may take place in any suitable slurry loop reactor or series of such reactors. The upstream polymerisation step may take place in one or more slurry polymerisation reactor(s) or in a gas phase polymerisation reactor, or a combination thereof.

[0050] The upstream polymerisation step may take place in one or more slurry polymerisation reactor(s), more preferably in at least two (e.g., two) or at least three (e.g. three) slurry phase reactors. Where, for example, at least three (e.g., three) slurry reactors are used, this does not include a slurry reactor for prepolymerisation.

[0051] Slurry ethylene polymerisation can take place in an inert diluent, typically a hydrocarbon diluent such as methane, ethane, propane, n-butane, isobutane, pentanes, hexanes, heptanes, octanes etc., or their mixtures. Preferably the diluent is a low-boiling hydrocarbon having from 1 to 4 carbon atoms or a mixture of such hydrocarbons. An especially preferred diluent is propane, possibly containing minor amount of methane, ethane and / or butane. In bulk propylene polymerization, propylene acts as monomer and diluent at the same time.

[0052] Polymer particles of the first polymer component formed by polymerisation, together with the catalyst fragmented and dispersed within the particles, may be suspended in the inert diluent. The slurry is agitated to enable the transfer of reactants from the fluid into the particles.

[0053] The olefin content in the fluid phase of the slurry may be from 2 to about 99 % by mole, preferably from about 3 to about 96% by mole and in particular from about 5 to about 90 % by mole. Where the first olefin monomer is propylene, the propylene content in the fluid phase of the slurry may be from 2 to about 99 % by mole, preferably from about 3 to about96 % by mole and in particular from about 5 to about 90 % by mole. Where the first olefin monomer is ethylene, the ethylene content in the fluid phase of the slurry may be from 2 to about 50 % by mole, preferably from about 3 to about 20 % by mole and in particular from about 5 to about 15 % by mole. The benefit of using higher olefin concentration is that the productivity of the catalyst can be increased.

[0054] The temperature in the upstream polymerisation may be from 20 to 115 °C, preferably from 25 to 110 °C and in particular from 30 to 100 °C. The pressure is from 1 to 150 bar, preferably from 10 to 100 bar.

[0055] The residence time in the upstream reactor (including any prepolymerisation reactor employed) may be typically from 0.15 h to 3.0 h, preferably from 0.20 h to 2.0 h and in particular from 0.30 to 1.5 h.

[0056] It is sometimes advantageous to conduct the slurry polymerisation above the critical temperature and pressure of the fluid mixture. Such operation is described in US-A-5391654. In such operation, the temperature is typically from 70 to 110 °C, preferably from 80 to 105 °C and the pressure is from 40 to 150 bar, preferably from 50 to 100 bar.

[0057] Where the upstream polymerisation is carried out by slurry polymerisation, the slurry polymerisation may be conducted in any known reactor used for slurry polymerisation. Such reactors include a continuous stirred tank reactor and a loop reactor. It is especially preferred to conduct the polymerisation in loop reactor. In such reactors the slurry is circulated with a high velocity along a closed pipe by using a circulation pump. Loop reactors are generally known in the art and examples are given, for instance, in USA-4582816, US-A-3405109, US-A-3324093, EP-A-479186, and US-A-5391654. The slurry may be withdrawn from the reactor either continuously or intermittently. A preferred way of intermittent withdrawal is the use of settling legs where slurry is allowed to concentrate before withdrawing a batch of the concentrated slurry from the reactor. The use of settling legs is disclosed, among others, in US-A-3374211 , US-A-3242150 and EP- A-1310295. Continuous withdrawal is disclosed, among others, in EP-A-891990, EP-A- 1415999, EP-A-1591460 and WO-A-2007 / 025640. The continuous withdrawal is advantageously combined with a suitable concentration method, as disclosed in EP-A- 1310295, EP-A-1591460, and EP3178853B1.

[0058] Hydrogen may be fed into the reactor to control the molecular weight of the polymer as known in the art. Furthermore, one or more alpha-olefin comonomers may be added into the reactor to control the density of the polymer product. The actual amount of such hydrogenand comonomer feeds depends on the catalyst that is used and the desired melt index (or molecular weight) and density (or comonomer content) of the resulting polymer.

[0059] Downstream polymerisation

[0060] As mentioned above, polymerisation in the second reactor involves polymerising an olefin monomer and optionally at least one alpha olefin comonomer. Where an upstream reactor is employed, polymerisation in the second reactor may take place in the presence of the first polymer component. The downstream polymerisation is preferably a gas phase polymerisation. The downstream polymerisation preferably employs a gas phase reactor.

[0061] Suitable olefin monomers include ethylene or propylene.

[0062] Where an alpha olefin comonomer is used, the alpha olefin comonomer may be selected from a C2 to C10 alkene. Suitable alpha olefin comonomers include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-hexene, 1-octene, 1-nonene and 1-decene. Preferably, the alpha olefin comonomer is selected from at least one of ethylene, propylene, 1 -butene, 1-hexene, and 1-octene. Where the olefin monomer polymerised in the second reactor (preferably gas phase reactor) is propylene, the alpha olefin comonomer may be ethylene, 1 -butene, 1-hexene and / or 1-octene. Where the olefin monomer is ethylene, the alpha olefin comonomer may be propylene, 1-butene and / or 1-hexene. Where an alpha olefin comonomer is used, one or more alpha comonomers may be employed. Preferably, one or two alpha comonomers are employed.

[0063] The alpha olefin comonomer content of the polymer component formed in the second reactor (preferably gas phase reactor) may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the polymer component is a polypropylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the polymer component is a polyethylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%.

[0064] The olefin monomer in the second reactor (preferably gas phase reactor) is preferably the same as the first olefin monomer. For example, the first and second olefin monomers may be propylene. Alternatively, the first and second olefin monomers may be ethylene.

[0065] The olefin polymerised in the second reactor (preferably gas phase reactor) may be termed a “second” olefin monomer. The second olefin monomer may be polymerised in thedownstream reactor to form a homopolymer as the second polymer component.

[0066] Alternatively, the second olefin monomer may be polymerised to form a copolymer of the second olefin monomer and the at least one alpha olefin comonomer as the second polymer component.

[0067] For example, propylene may be polymerised in the downstream reactor (preferably gas phase reactor) to produce propylene homopolymer as the second polymer component. Alternatively, propylene may be co-polymerised with at least one alpha olefin comonomer to produce a propylene copolymer as the second polymer component.

[0068] In one embodiment, ethylene is polymerised in the downstream reactor (preferably gas phase reactor) to produce ethylene homopolymer as the second polymer component.

[0069] Alternatively, ethylene may be co-polymerised with at least one alpha olefin comonomer to produce ethylene copolymer as the second polymer component.

[0070] Where an alpha olefin comonomer is used, the alpha olefin comonomer may be selected from a C2 to C10 alkene. For the avoidance of doubt, the alpha olefin comonomer is different from the second olefin monomer polymerised in the downstream reactor. Suitable alpha olefin comonomers include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-hexene, 1-octene, 1-nonene and 1-decene. Preferably, the alpha olefin comonomer is selected from at least one of ethylene, propylene, 1-butene, 1-hexene and 1-octene. Where the second olefin monomer is propylene, the alpha olefin comonomer may be ethylene, 1-butene, 1-hexene and / or 1-octene. Where the second olefin monomer is ethylene, the alpha olefin comonomer may be propylene, 1-butene, 1-hexene, and / or 1-octene. Where an alpha olefin comonomer is used, one or more alpha comonomers may be employed. Preferably, one or two alpha comonomers are employed.

[0071] The same of different alpha olefin comonomer may be used to form the first polymer component and second polymer component. Alternatively either or both of the first polymer component and second polymer components is a homopolymer.

[0072] The alpha olefin comonomer content of the second polymer component may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the second polymer component is a polypropylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%. Where the second polymer component is a polyethylene, the alpha olefin comonomer content may be 0 to 10 mol%, preferably 0 to 8 mol%, more preferably 0 to 6 mol%.As set out above, the downstream polymerisation is preferably gas phase polymerisation. The downstream gas phase polymerisation may take place in one or more gas phase polymerisation reactor(s) to produce the second polymer component.

[0073] The downstream polymerisation (preferably gas phase polymerisation) may be conducted in any suitable reactor. Preferably, the downstream polymerisation may be conducted in any known reactor used for gas phase polymerisation. Such reactors include a fluidized bed reactor and a fast fluidized bed reactor or in any combination of these. When a combination of reactors is used then the polymer is transferred from one polymerisation reactor to another. Furthermore, a part or whole of the polymer from a polymerisation stage may be returned into a prior polymerisation stage.

[0074] The temperature in the downstream polymerisation (preferably gas phase polymerisation) may be from 50 to 100 °C, preferably from 65 to 90 °C.

[0075] Generally, the operating pressure in the downstream polymerisation (preferably gas phase polymerisation) may be from 5 to 30 barg. For example, 5 to 29 barg. Preferably, the operating pressure may be 10 to 27 barg, yet more preferably 15 to 22 barg. Where the second olefin monomer is propylene, the operating pressure may be 5 to 30 barg, more preferably 10 to 27 barg, yet more preferably 15 to 22 barg.

[0076] The residence time in the downstream polymerisation (preferably gas phase polymerisation) is from 1.0 h to 4.5 h, preferably from 1.5 h to 4.0 h and in particular from 2.0 to 3.5 h. The residence time in the downstream polymerisation (preferably gas phase polymerisation) may be longer than the residence time in the upstream reactor(s) by at least 30%, preferably at least 40% or at least 50%.

[0077] The polymer production rate in the second reactor (preferably gas phase reactor) may be from 10 tn / h to 65 tn / h, preferably from 12 tn / h to 58 tn / h and in particular from 13 tn / h to 52.0 tn / h, and thus the total polymer withdrawal rate from the second reactor (preferably gas phase reactor) may be from 15 tn / h to 100 tn / h, preferably from 18 tn / h to 90 tn / h and in particular from 20 tn / h to 80.0 tn / h.

[0078] The downstream polymerisation (preferably gas phase polymerisation) is preferably conducted in a gas-solids fluidized bed(s).The product from the second reactor (preferably gas phase reactor) may be transferred to a separator (e.g., low pressure separator) to facilitate the separation of entrained gases from the polymer product. In some instances, it may be possible for a portion of the first product from the first reactor (preferably slurry loop reactor) to be passed directly to the separator located downstream of the second reactor (preferably gas phase reactor) bypassing the second reactor (preferably gas phase reactor).

[0079] Polymerization catalyst

[0080] The polymerization in the multi-stage olefin polymerization reactors is conducted in the presence of an olefin polymerization catalyst. The catalyst may be any catalyst which is capable of producing the desired olefin polymer. Suitable catalysts are, among others, Ziegler - Natta catalysts based on a transition metal, such as titanium, zirconium and / or vanadium catalysts. Especially Ziegler - Natta catalysts are useful as they can produce olefin polymers within a wide range of molecular weight with a high productivity.

[0081] Suitable Ziegler-Natta catalysts preferably contain a magnesium compound, an aluminium compound and a titanium compound supported on a particulate support.

[0082] The particulate support can be an inorganic oxide support, such as silica, alumina, titania, silica-alumina and silica-titania. Preferably, the support is silica.

[0083] The average particle size of the silica support can be typically from 6 to 100 pm. However, it has turned out that special advantages can be obtained if the support has median particle size from 6 to 90 pm, preferably from 10 to 70 pm.

[0084] The magnesium compound may be a reaction product of a magnesium dialkyl and an alcohol. The alcohol may be a linear or branched aliphatic monoalcohol. Preferably, the alcohol has from 6 to 16 carbon atoms. Branched alcohols are especially preferred, and 2-ethyl-1 -hexanol is one example of the preferred alcohols. The magnesium dialkyl may be any compound of magnesium bonding to two alkyl groups, which may be the same or different. Butyl-octyl magnesium is one example of the preferred magnesium dialkyls.

[0085] The aluminium compound may be chlorine containing aluminium alkyl. Especially preferred compounds are aluminium alkyl dichlorides and aluminium alkyl sesquichlorides.The titanium compound may be a halogen containing titanium compound, preferably chlorine containing titanium compound. Especially preferred titanium compound is titanium tetrachloride.

[0086] The catalyst can be prepared by sequentially contacting the carrier with the above mentioned compounds, as described in EP-A-688794 or WO-A-99 / 51646 . Alternatively, it can be prepared by first preparing a solution from the components and then contacting the solution with a carrier, as described in WO-A-01 / 55230.

[0087] Another group of suitable Ziegler-Natta catalysts contains a titanium compound together with a magnesium halide compound acting as a support. Thus, the catalyst contains a titanium compound on a magnesium dihalide, like magnesium dichloride. Such catalysts are disclosed, for instance, in WO-A-2005 / 118655 and EP-A-810235 .

[0088] Still a further type of Ziegler-Natta catalysts are catalysts prepared by a method, wherein an emulsion is formed, wherein the active components form a dispersed, i.e. a discontinuous phase in the emulsion of at least two liquid phases. The dispersed phase, in the form of droplets, is solidified from the emulsion, wherein catalyst in the form of solid particles is formed. The principles of preparation of these types of catalysts are given in WO-A-2003 / 106510 of Borealis.

[0089] The Ziegler-Natta catalyst is used together with an activator. Suitable activators are metal alkyl compounds and especially aluminium alkyl compounds. These compounds include alkyl aluminium halides, such as ethylaluminium dichloride, diethylaluminium chloride, ethylaluminium sesquichloride, dimethylaluminium chloride and the like. They also include trialkylaluminium compounds, such as trimethylaluminium, triethylaluminium, triisobutylaluminium, trihexylaluminium and tri-n-octylaluminium. Furthermore they include alkylaluminium oxy-compounds, such as methylaluminiumoxane (MAO), hexaisobutylaluminiumoxane (HIBAO) and tetraisobutylaluminiumoxane (TIBAO). Other aluminium alkyl compounds, such as isoprenylaluminium, may also be used. Especially preferred activators are trialkylaluminiums, of which triethylaluminium, trimethylaluminium and tri-isobutylaluminium are particularly used. If needed the activator may also include an external electron donor. Suitable electron donor compounds are disclosed in WO-A-95 / 32994 , US-A-4107414 , US-A-4186107 , US-A-4226963 , US-A-4347160 , US-A-4382019 , US-A-4435550 , US-A-4465782 , US 4472524 , US-A-4473660 , US-A-4522930 , US-A-4530912 , US-A-4532313 , US-A-4560671 and US-A-4657882 . Also electron donors consisting of organosilane compounds, containing Si-OCOR, Si-OR, and / or Si-NR2 bonds,having silicon as the central atom, and R is an alkyl, alkenyl, aryl, arylalkyl or cycloalkyl with 1-20 carbon atoms are known in the art. Such compounds are described in US-A-4472524 , US-A-4522930 , US-A-4560671 , US-A-4581342 , US-A-4657882 , EP-A-45976 , EP-A-45977 and EP-A-1538167 .

[0090] The amount in which the activator is used depends on the specific catalyst and activator.

[0091] Typically triethylaluminium is used in such amount that the molar ratio of aluminium to the transition metal, like Al / Ti, is from 1 to 1000, preferably from 3 to 100 and in particular from about 5 to about 30 mol / mol.

[0092] Metallocene catalysts may also be used. Metallocene catalysts comprise a transition metal compound which contains a cyclopentadienyl, indenyl or fluorenyl ligand. Preferably the catalyst contains two cyclopentadienyl, indenyl or fluorenyl ligands, which may be bridged by a group preferably containing silicon and / or carbon atom(s). Further, the ligands may have substituents, such as alkyl groups, aryl groups, arylalkyl groups, alkylaryl groups, silyl groups, siloxy groups, alkoxy groups or other heteroatom groups or the like. Suitable metallocene catalysts are known in the art and are disclosed, among others, in WO-A-95 / 12622 , WO-A-96 / 32423 , WO-A-97 / 28170 , WO-A-98 / 32776 , WO-A-99 / 61489 , WO-A-03 / 010208 , WO- A- 03 / 051934 , WO-A-03 / 051514 , WO-A-2004 / 085499 , EP-A-1752462 and EP-A- 1739103 .

[0093] These and other aspects of the present disclosure will now be described with reference to the accompanying drawings in which Figure 1 is a schematic drawing of a process scheme polymerising olefins in multistage polymerisation process configuration according to an example of the present disclosure.

[0094] Figure 1 is a schematic diagram of an apparatus for carrying out a process for polymerising olefins in multistage polymerisation process configuration in accordance with an example of the present disclosure.

[0095] The apparatus comprises a first reactor which is a slurry loop reactor 10 and a high pressure separator 12. The slurry loop reactor 10 is coupled to the high pressure separator 12 via a conduit that may optionally be heated. The high pressure separator 12 is coupled to a second reactor which is a gas phase reactor (not shown) via conduits 18, 24. Conduits 18, 24 may optionally be heated. Positioned downstream of the high pressure separator 12 is a control valve or rotary valve 20, which controls flow through the conduit 24 to the gas phasereactor. The high pressure separator 12 is coupled to a gas recovery and separation unit (not shown) via conduit 14.

[0096] In operation, the apparatus may be used to polymerise olefins in multistage configuration. The process comprises polymerising olefin monomer, optionally in the presence of comonomer, in the slurry loop reactor 10 to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen (not shown). This first product is introduced into a high pressure separator 12 via the conduit that may optionally be heated.

[0097] With the rotary valve 20 closed, the particles of the first polymer component are allowed to settle as a settled bed in a lower region 16 of the high pressure separator 12. The lower region may also include the frustoconical region that connects the lower region 16 and the cylindrical portion of the high pressure separator 12. The settled bed also occupies a portion 18 of the conduit 18 of the valve 20. The valve may be kept in a closed position for sufficient time to allow for the particles to settle to form a settled bed and for the separating gas to be passed through the settled bed.

[0098] Separating gas (e.g., propane) is passed through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed. The volume of separating gas passed through the settled bed is equal to 25% to 800% of the void volume of the settled bed (e.g. 25% to 200% of the void volume of the settled bed). The void volume is the total volume of the interstices between particles of the first polymer component in the settled bed. The separated hydrocarbon and / or hydrogen is passed via conduit 14 and recovered in a gas recovery unit (not shown). Advantageously, once treated with the separating gas, the particles of the first polymer component from the high pressure separator 12 are transferred to a gas phase reactor (not shown) via conduit 24 by opening the rotary valve 20. Olefin monomer, optionally in the presence of comonomer, is then polymerised in the gas phase reactor in the presence of the particles of the first polymer component to produce a second polymer component.

[0099] The separating gas may be introduced into an inlet located in the lower region 16 of the high pressure separator 12 via conduit 22a. The inlet may be positioned to introduce separating gas directly into the region where the settled bed forms. Alternatively or additionally, the separating gas may be introduced upstream and / or downstream of the valve 20 via conduits 22b and 22c, respectively. The separating gas introduced upstream of the valve via conduit 22b may be passed upstream through the settled bed. The separating gas introduceddownstream of the valve via conduit 22c may help to reduce the risk of backflow from the downstream gas reactor, and further reduce the risk of any entrained hydrogen and / or hydrocarbon reaching the downstream gas reactor.

[0100] Example

[0101] Polymerisation is performed using a system as depicted in Figure 1. A first polymer may be produced in the loop reactor and the polymer collected in the high pressure separator, such that the settled bed density in the lower region of the high pressure separator 16 and conduit 18 above the control or rotary valve 20 may be 250 - 450 kg / m3. The residence time in the lower region of the high pressure separator 16 and conduit 18 may be 5 seconds to 2 minutes.

[0102] Inert gas may be fed to the bottom of the high pressure separator via conduit 22a and above and below the valve 20 via conduits 22b and 22c, respectively, in an amount of amount to 25%-200% of void volume between the first polymer particles (settled bed void volume).

[0103] In this example, 50 m3 / h of polymer produced is in the loop reactor having a density of 950kg / m3This first polymer has settled bed density of 400kg / m3. The total void volume is ~ 58% and 42% as polymer volume, i.e., ~ 120m3 / h total volume moving through HP separator, out of which 50m3 / h is polymer and ~70m3 / h is gas in voids (70m3is void). The inert gas feed rate is set to 17m3 / h to 140m3 / h (25%-200% of void volume). The major part of this gas fed at the bottom of high pressure separator through conduit 22a and rest is divided between feed above and below the rotary valve via conduits 22b and 22c, respectively. It has been found that this rate of inert gas injection can be used to reduce the risk of carryover of hydrogen in the downstream gas reactor. At the same time, backflow of comonomer from the gas phase reactor to the loop reactor or high pressure separator is reduced.

[0104] Aspects of the invention are described by the following numbered clauses:

[0105] 1. A process for polymerising olefins in multistage polymerisation process configuration, said process comprising:

[0106] polymerising olefin monomer, optionally in the presence of comonomer, in a slurry loop reactor to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen;

[0107] introducing the first product into a high pressure separator;allowing the particles of the first polymer component to settle as a settled bed in a lower region of the high pressure separator;

[0108] passing separating gas through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed; wherein the volume of separating gas passed through the settled bed is equal to 25% to 200% of the void volume of the settled bed, said void volume being the total volume of the interstices between particles of the first polymer component in the settled bed;

[0109] recovering the separated hydrocarbon and / or hydrogen in a gas recovery unit; transferring the particles of the first polymer component from the high pressure separator to a gas phase reactor; and

[0110] polymerising olefin monomer, optionally in the presence of comonomer, in the gas phase reactor in the presence of the particles of the first polymer component to produce a second polymer component.

[0111] 2. A process as defined in clause 1 , wherein the volume of separating gas passed through the settled bed is equal to 30% to 180%, preferably 50 to 150%, more preferably 60 to 140%, yet more preferably 70 to 130%, even more preferably 80 to 120%, for example, 90 to 110% of the void volume of the settled bed.

[0112] 3. A process as defined in clause 1 or 2, wherein separating gas is introduced into an inlet located in the lower region of the high pressure separator; and / or downstream of the high pressure separator.

[0113] 4. A process as defined in any one of the preceding clauses, wherein a valve is positioned downstream of the high pressure separator.

[0114] 5. A process as defined in clause 4, wherein the valve is a rotary valve(s) and / or control valve(s).

[0115] 6. A process as defined in clause 4 or 5, wherein separating gas is introduced upstream and / or downstream of the valve.

[0116] 7. A process as defined in any one of clauses 4 to 6, wherein the particles of the first polymer component are allowed to settle as a settled bed in the lower region of the high pressure separator and in pipework connecting the high pressure separator and the valve.8. A process as defined any one of the preceding clauses, wherein the particles of the first polymer component are retained in the high pressure separator for a residence time of 5 to 500 seconds.

[0117] 9. A process as defined in any one of the preceding clauses, wherein the particles of the first polymer component are transferred to the gas phase reactor by gravity and / or by using a conveying gas.

[0118] 10. A process as defined in any one of the preceding clauses, wherein the high pressure separator is operated at a pressure of 18 to 22 barg.

[0119] 11. A process as defined in any one of the preceding clauses, wherein the high pressure separator is operated at a temperature of 60 to 75 degrees C.

[0120] 12. A process as defined in any one of the preceding clauses, wherein the high pressure separator is operated at a pressure that is 0.2 to 2.0 bar higher than the operating pressure of the gas phase reactor; and / or wherein the high pressure separator is operated at a pressure that is 0.2 to 2.0 bar higher than the operating pressure of the gas recovery unit.

[0121] 13. A process as defined in any one of the preceding clauses, wherein the separating gas comprises propane.

[0122] 14. A process as defined in any one of the preceding clauses, wherein olefin polymerised in at least the slurry loop reactor is ethylene and / or the hydrocarbon in the fluid phase of the first product comprises an olefin selected from 1-butene and / or 1-hexene.

[0123] 15. A process as defined in any one of the preceding clauses, wherein the concentration of first polymer component in the first product introduced into the high pressure gas phase reactor is 20 to 65% by weight.

Claims

CLAIMS1. A process for polymerising olefins, said process comprising:polymerising olefin monomer, optionally in the presence of comonomer, in a first reactor to produce a first product comprising particles of a first polymer component and a fluid phase comprising hydrocarbon and / or hydrogen;introducing the first product into a high pressure separator;allowing the particles of the first polymer component to settle as a settled bed in a lower region of the high pressure separator;passing separating gas through the settled bed to separate hydrocarbon and / or hydrogen from the settled bed; wherein the volume of separating gas passed through the settled bed is equal to 25% to 800% of the void volume of the settled bed, said void volume being the total volume of the interstices between particles of the first polymer component in the settled bed;recovering the separated hydrocarbon and / or hydrogen in a gas recovery unit; transferring the particles of the first polymer component from the high pressure separator to a second reactor; andpolymerising olefin monomer, optionally in the presence of comonomer, in the second reactor in the presence of the particles of the first polymer component to produce a second polymer component.

2. A process as claimed in claim 1 , wherein the first reactor is a slurry loop reactor and / or the second reactor is a gas phase reactor.

3. A process as claimed in claim 1 or 2, wherein the volume of separating gas passed through the settled bed is equal to 25% to 400%, preferably 25% to 200%, more preferably 30% to 180%, more preferably 50 to 150%, more preferably 60 to 140%, yet more preferably 70 to 130%, even more preferably 80 to 120%, for example, 90 to 110% of the void volume of the settled bed.

4. A process as claimed in any one of the preceding claims, wherein separating gas is introduced into an inlet located in the lower region of the high pressure separator; and / or downstream of the high pressure separator.

5. A process as claimed in any one of the preceding claims, wherein a valve is positioned downstream of the high pressure separator.

6. A process as claimed in claim 5, wherein the valve is a rotary valve(s) and / or control valve(s)and / orwherein separating gas is introduced upstream and / or downstream of the valve.

7. A process as claimed in claim 5 or 6, wherein the particles of the first polymer component are allowed to settle as a settled bed in the lower region of the high pressure separator and in pipework connecting the high pressure separator and the valve.

8. A process as claimed any one of the preceding claims, wherein the particles of the first polymer component are retained in the high pressure separator for a residence time of 5 to 500 seconds.

9. A process as claimed in any one of the preceding claims, wherein the particles of the first polymer component are transferred to the second reactor by gravity and / or by using a conveying gas.

10. A process as claimed in any one of the preceding claims, wherein the high pressure separator is operated at a pressure of 18 to 22 barg.

11. A process as claimed in any one of the preceding claims, wherein the high pressure separator is operated at a temperature of 60 to 75 degrees C.

12. A process as claimed in any one of the preceding claims, wherein the high pressure separator is operated at a pressure that is 0.2 to 2.0 bar higher than the operating pressure of the second reactor; and / or wherein the high pressure separator is operated at a pressure that is 0.2 to 2.0 bar higher than the operating pressure of the gas recovery unit.

13. A process as claimed in any one of the preceding claims, wherein the separating gas comprises propane.

14. A process as claimed in any one of the preceding claims, wherein olefin polymerised in at least the first reactor is ethylene and / or the hydrocarbon in the fluid phase of the first product comprises an olefin selected from 1-butene and / or 1-hexene.

15. A process as claimed in any one of the preceding claims, wherein the concentration of first polymer component in the first product introduced into the second reactor is 20 to 65% by weight.