Composite material

Composite materials with renewable phenolic resin binders for metal smelting address slag generation and CO2 emissions, enhancing process efficiency and environmental sustainability.

WO2026238979A1PCT designated stage Publication Date: 2026-11-19PROCARBON BIO AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/064233
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing metal smelting, extraction, and refining processes using powdered feed materials with inorganic binders generate excessive slag and release CO2 due to the use of fossil-derived organic binders, posing environmental and handling challenges.

Method used

Development of composite materials comprising metal-containing materials and renewable phenolic resin binders, which are cured and compressed to form briquettes, providing structural integrity and reducing CO2 emissions.

Benefits of technology

The composite materials exhibit high compression strength, enabling efficient handling and processing while minimizing CO2 emissions, thus addressing environmental concerns and improving process efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026064233_19112026_PF_FP_ABST
    Figure EP2026064233_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure a composite material formed from about 1%-99% by weight of at least one metal-containing material; and about 1% to about 40% by weight of at least one binder comprising a phenol based polymer. The phenol based polymer may be formed from phenols, such as those derived from Cashew Nut Shell Liquid and optionally an accelerator. The metal-containing material may comprise a metal ore, such as iron ore. The composite material may additionally contain a carbon material such as charcoal. The invention also provides methods for making materials of the invention.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] 95.177.175845 / 01

[0002] Composite Material

[0003] FIELD OF USE

[0004] The present disclosure relates generally to composite materials, particularly to composite materials containing a metal-containing material and a binder. The materials are useful as a feed material for metalogical processes, such as metal smelting, extraction, purification, and / or refining.

[0005] BACKGROUND

[0006] Feed materials for metal smelting, extraction or refining are most effectively used as a powder, in order to maximise the surface area for reaction, and thus optimise the smelting and the rate at which the material can be processed. However, powders are difficult to handle and can cause dust which can clog machinery, be hazardous to workers and even be explosive if suspended in the air in the correct proportions.

[0007] Attempts have been made to overcome this limitation by taking powdered feed materials (e.g. ores) and binding these together with a binder, such as lime, in order to generate a pellet or briquette of feed material and binder. However, such binders are typically inorganic materials, which typically do not contain the same metal ions as the desired feed materials and thus generate a greater quantity of biproduct (slag) when the feed material is processed.

[0008] Organic binders formed from carbon-based materials are an option of binding powdered materials but these must form a composite material that is robust enough to survive handling within and automated production line. Most organic materials are also ultimately derived from fossil fuels such as crude oil or natural gas. Since the binder will typically be burned off or oxidised in the anaerobic metal processing, this releases CO2 into the atmosphere. Since iron ore is processed at a rate of around 2.5 billion metric tons per year globally, even a small proportion of fossil-derived95.177.175845 / 01

[0009] organic materials processed with this ore will result in a significant release of fossil carbon in the form of CO2 into the atmosphere from non-renewable resources.

[0010] Climate change is an increasing concern to governments and individuals and increasing efforts are being made and proposed to use less fossil-fuel based carbon sources and more “CO2 Neutral” carbon sources. A significant way of reducing CO2 build up in the atmosphere is to use carbon from renewable resources. These include solid materials such as wood or processed wood materials (e.g. charcoal / biochar) as well as liquid carbon sources such as bio-ethanol or biomethanol. Carbon dioxide neutral carbon sources rely on carbon previously captured from the atmosphere and so do not contribute to atmospheric carbon, even if that carbon is subsequently released. This allows carbon-dioxide generating processes to be used without any net increase in atmospheric carbon.

[0011] SUMMARY

[0012] To address the limitations in the state of the art, the present specification discloses composite materials, and methods for creating these materials, that comprise at least one metal-containing material and at least one binder material.

[0013] In a preferred embodiment, the at least one metal-containing material is at least one metal ore. In a first aspect, the present disclosure thus provides a composite material comprising:

[0014] a) about 1% to about 99% by weight of at least one metal-containing material; and about 1% to about 40% by weight of at least one binder comprising a phenol based polymer (e.g. phenolic resin), preferably a renewable phenolic resin.

[0015] In a preferred embodiment, the “phenol based polymer” in any aspect of the invention is a phenolic resin (e.g. a resin formed by polymerisation of at least one phenol (e.g. as disclosed95.177.175845 / 01

[0016] herein) and at least one aldehyde (e.g. formaldehyde), formyl carbon source, or equivalent material (such as an alkanoyl carbon source - all, for example, as disclosed herein)).

[0017] The term “renewable” as used in any aspect herein refers to the origin of the material being a natural resource which can be replenished or replaced through natural processes within a human timeframe (e.g. within 1 to 50 years).

[0018] In one embodiment, the phenol based polymer (e.g. renewable phenolic resin) may be formed or formable from at least one phenol compound of formula I:

[0019]

[0020] wherein X is H or OH and R is H or an optionally substituted, saturated or unsaturated, hydrocarbon moiety of 1 to 24 carbons, which may be straight-chain or branched. One or two independent R groups may be present and may independently be in the position ortho-, meta- or para- to the -OH group shown. One meta- R group is preferred. In one embodiment, the at least one phenol of formula I comprises at least one phenol wherein R is not hydrogen.

[0021] The at least one phenol of formula I may comprise, consist essentially of or consist of phenols of formula I wherein at least one non-hydrogen R group is present, preferably meta- to the -OH moiety.95.177.175845 / 01

[0022] In one embodiment, the at least one phenol of formula I may partially comprise phenols of formula I wherein at least one non-hydrogen R group is present, preferably meta- to the -OH moiety and partially comprise phenol and / or resorcinol.

[0023] In one embodiment, the phenol based polymer may be a polymer of at least one phenol of formula I optionally with other components (such as those described herein, for example a formyl carbon source such as hexamine).

[0024] In one embodiment, the phenol based polymer may be formed or formable from at least one phenol of formula I where the at least one phenol comprises cardol and / or cardanol.

[0025] In one embodiment, the phenol based polymer may be formed or formable from at least one phenol of formula I by reaction with at least one aldehyde, urea or a formyl-carbon source such as hexamine.

[0026] In one embodiment, the composite material additionally includes at least one carbon material, such as coke and / or charcoal (biochar). In one preferred combination, a carbon material may be included when the metal-containing material comprises metal ore. This allows the composite material to include some or all of the carbon needed in heating and / or reducing the ore to provide purified metal from the ore.

[0027] In a second aspect, the present disclosure provides a composition comprising:

[0028] cardanol; iron ore powder; charcoal powder; and optionally an accelerator such as hexamine; wherein said cardanol, said charcoal powder, said iron ore powder and optionally said accelerator are mixed together to form a mixture;95.177.175845 / 01

[0029] wherein said mixture is cured at a range of approximately 100°C to 250°C;

[0030] wherein said mixture is pressurized at a range of approximately 3 to 50 MPa;

[0031] wherein said cardanol is in a range of approximately 2% to 12% by weight of said mixture;

[0032] wherein said iron ore is in a range of approximately 50 to 80% by weight of said mixture;

[0033] wherein said charcoal powder is in a range of approximately 10% to 30% by weight of said mixture; and wherein said hexamine is in a range of 0.01% to 1% by weight of said mixture where present.

[0034] In one embodiment, the composition may additionally comprise an epoxy, preferably an epoxy from renewable resource e.g. soy epoxy. In a further embodiment, the composition may additionally or alternatively contain inorganic materials e.g. waterglass, bentonite, kaolin, metakaolin, wollastonite and / or lime. Typically, when these materials are added, they are added to the smelter which is at a temperature of 300 to 2000 °C. Without being bound by theory, the addition of such materials is believed to increase the hot strength of the composition and allows the composition to self-cure or cure at a lower temperature.

[0035] In one embodiment, the composite material has a compression strength of at least 5 MPa (e.g. 5 to 150 MPa, preferably at least 20MPa, such as at least 30 MPa or at least 40MPa) when tested in accordance with the method described below (as described herein below with reference to the examples). In one particular embodiment, the composite based material has a compression strength of at least 40MPa (e.g. 40 to 120 MPa), preferably at least 50MPa and more preferably at least 60 MPa (e.g. 60 to 100 MPa). One appropriate test for measuring the compressive strength of the composite material is the American Society for Testing Materials ASTM C39 / C39M95.177.175845 / 01

[0036] method. This provides a Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens. This method for testing compressive strength is intended herein unless otherwise specified.

[0037] In a further aspect, the present disclosure provides a method of preparing a composite material, comprising the steps:

[0038] providing at least one phenol such as cardanol;

[0039] providing at least one metal-containing material (e.g. metal ore powder);

[0040] optionally providing charcoal powder;

[0041] mixing at least one said phenol with said metal-containing material and with said charcoal powder if present, such that a composition comprising phenol and metal-containing material is created; compressing and optionally vibrating said composition; and

[0042] curing said composition.

[0043] The resulting products may be used in any manner, including, but not limited to: the metallurgical industry, particularly for smelting, extracting purifying and / or refining at least one metal.

[0044] Brief Description of Figures

[0045] Figure 1 illustrates a briquette formed according to IE1 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 500°C (bottom).95.177.175845 / 01

[0046] Figure 2 illustrates a briquette formed according to IE2 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 500°C (bottom).

[0047] Figure 3 illustrates a briquette formed according to IE1 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 750°C (bottom).

[0048] Figure 4 illustrates a briquette formed according to IE2 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 750°C (bottom).

[0049] Figure 5 illustrates a briquette formed according to IE1 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 900°C (bottom).

[0050] Figure 6 illustrates a briquette formed according to IE2 of Example 2 (top), and the material having a particle size greater than 6.30 mm, less than 3.15 mm, less than 0.50 mm and the fines following reduction at 900°C (bottom).

[0051] Detailed Description of the Invention

[0052] In the various aspects and embodiments of the present invention, the composite materials comprise at least one metal-containing material. In a preferred embodiment, the at least one metalcontaining material comprises, consists essentially of, or consists of at least one metal ore (also referred to herein as “metal ore material”, “ore material” or “ore”). Typically, suitable metal ores will be ores of industrially valuable metal elements such as iron, copper, zinc, tin, manganese,95.177.175845 / 01

[0053] nickel but not limited thereto. Preferred ores for use in the various aspects of the present invention are iron ores. Iron ores useful in the aspects of the present invention include any rock or mineral material with a substantial iron content, as well as mixtures of such ores. Evidently, the ore material may also comprise other rock and mineral materials and so the overall iron content of the ore material may be lower than the individual ores themselves. An iron content of at least about 30% (e.g. about 30 to about 75%) is desirable, such as at least about 40% or at least about 45%. Most preferred is an iron content of at least 55% or at least 60% (e.g. 65 to 71% iron). An iron content of 55 to 60% is preferable in some embodiments. Magnetite (FesCE, 72.4% Fe), hematite (Fe2O3, 69.9% Fe), goethite (FeO(OH), 62.9% Fe), limonite (FeO(OH) n(H20), 55% Fe), and / or siderite (FeCCh, 48.2% Fe) are typical examples of suitable iron ores and the ore of any aspect or embodiment of the invention may comprise any of these, or any mixture thereof. Preferably, the iron ore will comprise at least about 50% (e.g. 50 to 99%), preferably at least 70% or at least 80% of at least one of these ores, or any mixture thereof. In one embodiment, the iron ore may consist of, or consist essentially of at least one of these ores, or any mixture thereof.

[0054] Metal ores will typically comprise at least one mineral salt of the relevant metal. Oxides, hydroxides, carbonates, sulphides, silicates and mixtures thereof are examples of suitable mineral salts of appropriate metals (e.g. as indicated herein). Suitable ores are well known to the skilled worker.

[0055] The composite materials of the present invention comprise about 1% to 99% by weight, particularly 20% to 99% or 10% to 98% by weight, such as 40% to about 98% by weight metalcontaining material (e.g. metal ore, especially iron ore, as described herein). This may be up to 96% or up to 95%, such as up to 92% or up to 90% by weight. An amount of at least 50%, preferably at least 60% or at least 70% is preferred. Where a carbon material (such as coke or95.177.175845 / 01

[0056] charcoal) is also present, an amount of 60 to 95% by weight metal-containing material (e.g. metal ore, especially iron ore) may be most suitable, such as 75 to 92% or 70 to 90%. Alternatively, where a carbon material (such as charcoal or coke) is present, the metal-containing material (e.g. metal ore) may be present in an amount of 1 to 50% by weight of the composite material, and the carbon material may be present in an amount of 1 to 50% by weight of the composite material. In various embodiments, the amount of metal-containing material in the composite material is preferably in the range of 70% to 99%, such as 80% to 98%, preferably 85% to 95%, especially 90% to 95% by weight of the composite material.

[0057] In various embodiments, the metal-containing material comprises, consists of or consists essentially of metal powder and / or metal fines. Suitable metal powder and / or metal fines may be of any suitable metal, such as those discussed herein above. In particular iron / steel powder / fines may form at least a part of the metal-containing material. Such iron / steel powder / fines may be generated as a waste product from industrial processes (e.g. from metal smelting or metal working / machining) or may be formed from recycled iron / steel materials (e.g. scrap iron / steel). Recycled materials may be physically divided into pieces (e.g. shredded, milled etc.) prior to use in any appropriate embodiment of the present invention.

[0058] In various embodiments, the composite material of the present disclosure may comprise a carbon material, preferably obtained from a renewable resource. Such carbon materials will comprise, consist of, or consist essentially of, elemental carbon from any appropriate source. Suitable carbon materials may comprise, consists essentially of or consists of charcoal (also referred to as “biochar”). Alternatively or in addition, the carbon material may comprise, consist essentially of or consist of coal, carbon black, coke and / or any other suitable carbon material. Generally, coal95.177.175845 / 01

[0059] will preferably have an elemental carbon content of at least 70%, preferably at least 80%, more preferably at least 90% (e.g. anthracite). Coke as referred to herein may include any of biocoke, semicoke, metallurgical coke and / or petcoke (e.g. anode grade petcoke). Alternatively, or additionally, the carbon material may comprise carbon black and / or artificial graphite. The carbon material may additionally comprise any of the following materials: lignite, anthracite and / or wood chips. The most preferably source of carbon material will be carbon that has been removed from the atmosphere, such as by biological processes (e.g. tree growth). In charcoal / biochar and similar materials “fixed carbon" is the percentage of non-volatile carbon by weight and will preferably be in the range of 2 to 99%. Preferably, the fixed carbon is at least 60% or at least 75% by weight. This will vary depending upon the nature of the charcoal. Similarly, the composite materials (when a carbon material is present) will have a certain % of fixed carbon depending on the carbon material and binder. For charcoal / biochar, the conditions under which the charcoal is made and / or treated will have an effect, as will and the curing of the binder.

[0060] A carbon material (e.g. charcoal) having a fixed carbon content of at least 70% (e.g. 75 to 98%) may be used. In one embodiment, the charcoal used in the materials of the present disclosure has a fixed carbon content of at least 80%. Such charcoal may, for example, be generated by heat treatment in the absence of oxygen to 300-900°C. In a further embodiment, the charcoal used may be at least 80%, at least 90% or at least 95% fixed carbon. Such charcoal may, for example, be generated by heat treatment to at least 700°C (e.g. 800-1200°C) in an inert atmosphere.

[0061] The composition may include a catalyst and / or accelerator to improve the curing time, lower the curing temperatures and / or control the nature of the binder.

[0062] In one embodiment, the accelerator or catalyst may be hexamine, which may start the polymerization process when mixed with the other binder components (e.g. phenols of formula I)95.177.175845 / 01

[0063] and charcoal powder. Aldehydes such as formaldehyde and their precursors such as polymethylene glycol and the like are also suitable accelerators or catalysts. Further accelerators and catalysts are discussed below and may be used in any appropriate embodiment of the invention. In some embodiments, the accelerator and / or catalyst may comprise, consist or consist essentially of epoxidized oil (e.g. epoxidized soybean oil), polycarboxylic acids (e.g. citric acid and adipic acid), isocyanates, anhydrides (e.g. methyl nadic anhydride), tannin and / or lignin. In some cases, an acid catalyst is used. Suitable acid catalysts include p-toluenesulfonic acid, Lewis acid catalysts (e.g. zinc acetate, zinc oxide) and polyacids (e.g. citric acid). In some embodiments, it is preferred if the accelerator and / or catalyst does not comprise hexamine.

[0064] In one embodiment, the composite material (e.g. briquettes) may be cured in the range of 95 to 400 degrees Celsius (“°C”). Preferably this will be 110 to 300°C, or 180 to 250°C such as 190 to 220°C. The curing period will depend upon the binder, the optional accelerator / catalyst and the treatment temperature. However, typical curing periods will be from 5 minutes to 12 hours, preferably from 20 minutes to 3 hours, such as 30 minutes to 2 hours or 1 to 4 hours.

[0065] Curing may be monitored by any appropriate technique in the art, such as optical sensing (e.g. absorption or reflection of light), ultrasound or acoustic sensing (e.g. reflection of sound), conductivity sensing (e.g. electrical impedance spectroscopy), moisture sensing (e.g. dielectric measurement), thermal imaging (e.g. infrared thermography), weight calculations, spectroscopy (e.g. Raman or Fourier Transform infrared spectroscopy), mass spectrometry and / or gas chromatography. Weight calculations are particularly preferred.

[0066] In one embodiment, the pressure used in forming the composite material into pieces (e.g. into briquettes, blocks, rods or any appropriate shape, including those discussed herein) may be at least95.177.175845 / 01

[0067] 5 kN / cm2(i.e. at least 50 MPa) such as 5 to 500 kN / cm2(50 to 5000 MPa). Suitable compression forces may be, for example, at least 8 kN / cm2, such as around 10 kN / cm2. However, greater compression such as at least 20 N / cm2(200 MPa) or at least 50 N / cm2may be used. Vibration may alternatively or additionally be used to compress and / or compact the products of the disclosure prior to curing. In one embodiment, vibration is used in combination with the compression forces indicated above.

[0068] Typically, higher compression forces (preferably in combination with vibration) are associated with final materials having a greater density, lower surface area, lower water adsorption and / or a stronger compressive strength. Repeated compression, optionally in combination with vibration, may also be used. Compression may be carried out once, twice, three times or a larger number of times (e.g. 1 to 10 times). Vibration may be used or not used during each compression step independently.

[0069] Where the composite material of the present invention is in the form of briquettes, these may be used for any appropriate purpose including smelting, refining, purifying and extracting. Where a carbon material is present in the composite material comprising metal ore (e.g. briquettes) then this may act as a fuel for heating the ore and / or may act as reductant in the metallurgical process. In one embodiment the carbon present in the composite material comprising metal ore is sufficient reductant for the processing (e.g. metal extraction) of the ore. Alternatively, the composite material of the present invention may be used with additional reductant. Such an additional reductant may be another solid material comprising carbon (e.g. formed to comprise charcoal and / or coke (e.g. as described herein)).

[0070] In one embodiment, the metal-containing material (optionally with carbon material such as charcoal) and binder mixture may be pressurized by a hydraulic press, a mechanical press, an95.177.175845 / 01

[0071] extruder, and / or a roller press, and may have a pillow, prismatic (e.g. cuboidal or cylindrical), or other uniform shape. Formation by extrusion is a preferred method.

[0072] In addition to the nature of the binder, by adding charcoal to the compositions of the present disclosure, the carbon dioxide footprint of the metal extraction / smelting process can be controlled, shrinking the carbon dioxide footprint, or making the process carbon dioxide neutral, at least in the metal extraction step.

[0073] In one embodiment, the binder may be approximately 1-50%, 1-30%, or 2-50% weight of the final mixture (and thus of the final composite material). This will preferably be 2 to 35% or 5 to 30% by weight. The amount of binder may vary depending upon the application with higher compression strength generally requiring higher amounts of binder. For briquettes in some metallurgical processes, the amount of binder may typically be 1 to 20%, 2 to 15%, 4 to 15%, or 5 to 10% by weight of the composite material. Where strength is of greater importance, higher levels of binder, such as 15 to 25% or 20 to 30% by weight.

[0074] In some cases, the preferred amount of binder is no less than 3.5 wt%, such as no less than 3.0 wt%, no less than 2.5 wt%, especially no less than 2.0 wt% or 1.5 wt% of the weight of the composite material. In certain cases, the preferred amount of binder is 2.0 - 40 wt%, 2.5 -40 wt%, 3.0 - 40 wt% or 3.5 - 40 wt% of the composite material.

[0075] In some cases, the preferred amount of binder is 2.0 - 23 wt%, 2.2-23 wt%, 2.5 -23 wt%, 3.0 -23 wt% or 3.5 - 40 wt% of the composite material. Especially preferred amounts of binder (e.g. phenol based polymer binder) include 5 to 15 wt% and 4 to 12 wt% of the composite material, which advantageously allows for a composite material with good performance and which maintains its structural integrity, even when subjected to high temperatures (e.g. up to 900 °C). In some cases, it is preferred that the amount 4 to 10 wt%, especially 5 to 9 wt%. It is desirable95.177.175845 / 01

[0076] for briquettes to demonstrate good thermal resistance and structural integrity at high temperatures when used in smelting applications, to avoid valuable materials from being lost prematurely, and also to allow for more efficient and uniform smelting, which is more economical and environmentally friendly.

[0077] The “binder” as indicated herein may comprise at least one phenol component (such as those described herein, especially of formula I) but may also comprise at least one accelerant and / or catalyst. Accelerants such as hexamine (and others described herein and known in the art) preferably may be present at approximately 2 to 15% or 4 to 10% (e.g. 6-8%) by weight of the binder component. In one embodiment, the accelerant is a source of formyl carbons and is present in an amount equivalent to at least one mole of formyl carbon per mole of phenol present in the binder. In an alternative or additional embodiment, the accelerant may comprise an acid accelerant (as described herein or as known in the art).

[0078] In addition to the optional accelerator / catalyst, the binder component may comprise at least one oil component such as a renewable epoxy component. Such an oil forms an optional part of the binder and my thus be absent or may be present as up to 50% of the total weight of binder (i.e. up to approximately the same content by weight as the phenol component). Suitable oils include “drying oils”. Drying oils typically comprise glycerol triesters of highly unsaturated fatty acids, especially alpha-linolenic acid. The “iodine number” is an indicator of the number of double bonds in an oil and thus its tendency to be a drying oil. Oils with an iodine number greater than 130 are considered drying and are preferred as the oil component in the present invention. Those with an iodine number of 115-130 are semi-drying and may be used, preferably in combination with a drying oil. One preferred drying oil is linseed oil. Such oils dry by oxidative cross-linking and without being bound by theory, may cure with unsaturated phenolic components by such a process.95.177.175845 / 01

[0079] In one embodiment, an oil component is used in combination with at least one phenol of formula I having an unsaturated “R” group. Examples include cardanol and cardol.

[0080] One embodiment may be a composition comprising: cardanol (and optionally cardol); and metalcontaining material (e.g. metal ore powder); wherein the cardanol and the metal-containing material (e.g. metal ore powder) are mixed together to form a mixture; and wherein the mixture is cured to form a composite material. The composition may additional comprise a carbon material such as charcoal or coke. The composition may further comprise an accelerant or catalyst, wherein the accelerant / catalyst is mixed together with the cardanol and the metal-containing material (and optionally charcoal powder) as part of the mixture. The mixture may be compressed, and if compressed, it may be compressed with a pressure in a range of approximately 5 to 500 kN / cm2(50 to 5000 MPa) such as 5 to 100 kN / cm2. Suitable pressures are described herein such as in the range of 10 to 50 kN / cm2. The mixture may preferably be cured at less than 450 °C. Suitable curing temperatures may be in the range of approximately 100 to 300°C, such as 120 °C to 250°C. The curing time can vary, but may be for as little as 1 minute, approximately 2 hours, or longer. Suitable curing times are described herein but may be, for example, 5 minutes to 2 hours, such as 15 minutes to 1 hour.

[0081] In any embodiment of the disclosure, the mixture may be cured via a curing mechanism selected from the group of curing or heating mechanisms consisting of one or more of: indirect heat; direct heat; radiant heat; ultraviolet light; infrared rays; microwaves; ultrasound; inductive power; and combinations thereof. Direct heating, such as electrical heating, forms a preferred curing method. The compressed mixture may be cured directly into its final shape (e.g. formed into briquettes, cylinders, rods, blocks, cubes, balls or prisms before curing). Alternatively, the mixture may be formed into its final shape after curing by any appropriate means, such as cutting, grinding or95.177.175845 / 01

[0082] crushing. Briquetes may be a suitable shape for use in metallurgical processes. Alternatively, the composite material may be formed and / or further processed into any appropriate form. Further processing may include shaping the composite material such as by cutting and / or crushing, or by subsequent treatment such as further curing, coating or heat treatment.

[0083] In general, for the composite material of the disclosure, the binder (e.g. cardanol and / or cardol optionally including an accelerator) in the mixture may be in a range of approximately 1% to 50% or 2% to 40% by weight of the final material / mixture. Typically, this may be 5% to 30%, such as 8% to 24% by weight. An especially preferred range of binder is 4% to 12% of the composite material.

[0084] It is generally preferred that the primary binder does not form a hydrogel. The term “hydrogel” is known in the art, and is a gel which is typically formed from a hydrophilic polymer forming an interconnected crosslinked network. It is therefore preferred that the primary component of the binder is free from, or substantially free from, any material which promotes the formation of hydrogels. Such materials include, but are not limited to: carboxymethyl cellulose (CMC), polysaccharides, guar gum and mixtures thereof. The primary component of the binder is that component of the binder which forms the largest component by weight (e.g. a phenol component in some embodiment). In one aspect, the secondary binder (as disclosed herein) may form a hydrogel. In an alternative aspect, the secondary binder (as disclosed herein) does not form a hydrogel.

[0085] The catalyst / accelerator, which is preferably hexamine, in the mixture may be in a range of 0.1% to 15% by weight of the binder. Suitable amounts are described herein.

[0086] In one embodiment, the metal-containing material (e.g. metal ore powder), charcoal powder and binder may be the only, or substantially the only components, such that the composite material95.177.175845 / 01

[0087] consists of, or consists essentially of, metal-containing material (e.g. metal ore powder), optional carbon material (e.g. charcoal) and binder (optionally including accelerator). The metalcontaining material may be any suitable metal-containing material (e.g. as described herein) and the carbon material may be any suitable material described herein, including charcoal with reduced volatiles as described herein. In an alternative embodiment, at least one additional mineral may be present in the composite material. Minerals, such as CaCCh (chalk / limestone) are well known additives in the metal smelting process and may, for example, help in removing silica materials as slag. Preferably the composite material will be free of mineral materials or may contain (e.g. be formed from) not more than 30% mineral material by weight. This may be 0 to 30% or 1 to 30% such as 10 to 25% or 15 to 25% filler by weight. The mineral material may serve to increase the compressive strength of the composite material and / or may be used to control the density of the material and / or be included as part of the smelting / extraction / purification process. Suitable mineral materials include those disclosed herein below and may include materials such as limestone or chalk. Preferred mineral particle sizes may be in the range 50 nm to 500 pm diameter, such as 100 nm to 200 pm, such as 3 pm to 100 pm. Very fine mineral materials, such as those having average particle diameters below 100 pm (e.g. 100 nm to 80 pm or 1 pm to 50 pm) may also be used.

[0088] One specific embodiment may be a composition comprising: cardanol (optionally including up to 12% cardol); metal-containing material powder (e.g. iron ore powder), and an activator (e.g. hexamine or an acid activator). Generally, the metal-containing material, the cardanol, and the activator are mixed together to form a mixture; wherein the mixture is cured at a range of approximately 100 °C to 250 °C for a period of 5 mins to 2 hours; wherein the mixture is compressed in a range of approximately 3 to 50 kN / cm2(prior to and / or during curing); wherein95.177.175845 / 01

[0089] the cardanol is in a range of approximately 2% to 35% (e.g. 5 to 20%) by weight of the mixture; wherein the metal-containing material is in the range of approximately 60% to 98% by weight of the mixture; and wherein the catalyst / accelerator (e.g. hexamine) is in a range of 0.1% to 20% (e.g.

[0090] 0.1% to 15%) by weight of the cardano 1 / cardol component.

[0091] Another specific embodiment may be a composition comprising: cardanol (optionally including up to 12% cardo 1); metal-containing material (e.g. iron ore powder), charcoal powder; and an activator (e.g. hexamine or an acid activator). Generally, the metal-containing material, the cardanol, the charcoal powder, and the activator are mixed together to form a mixture; wherein the mixture is cured at a range of approximately 100 °C to 250 °C for a period of 5 mins to 2 hours; wherein the mixture is compressed in a range of approximately 3 to 50 kN / cm2(prior to and / or during curing); wherein the cardanol is in a range of approximately 2% to 35% (e.g. 5 to 20%) by weight of the mixture; wherein the metal-containing material is in the range of approximately 60% to 80% by weight of the mixture; charcoal powder is in a range of approximately 5% to 30% by weight of the mixture; and wherein the catalyst / accelerator (e.g. hexamine) is in a range of 0.1% to 20% (e.g. 0.1 to 15%) by weight of the cardanol / cardol component. All descriptions herein appropriate to the various features of this embodiment may be employed and combined with this embodiment, where technically viable.

[0092] Another embodiment may be a method of preparing metal-containing material(and optionally charcoal powder) and cardanol products, comprising the steps: providing cardanol; providing metal-containing material; and optionally providing charcoal powder; mixing the cardanol with the metal-containing material (and optionally the charcoal powder), such that a composition is created comprising cardanol and metal-containing material (and optionally charcoal powder); pressurizing the composition; and curing the composition. The method may include the step of95.177.175845 / 01

[0093] providing a catalyst; / activator wherein the catalyst / activator is mixed with the cardanol and the metal-containing material, such that the composition comprises the catalyst. The components may be in a range indicated herein; wherein the composition may be pressurized (optionally with vibration) at a range of approximately 3 to 100 kN / cm2; wherein the composition may be cured at a range of approximately 180 °C to 250 °C for 5 minutes to 2 hours.

[0094] Other features and advantages will become apparent to those skilled in the art from the following detailed description.

[0095] DETAILED DESCRIPTION OF THE EMBODIMENTS

[0096] In the following detailed description of various embodiments, numerous specific details are set forth in order to provide a thorough understanding of various aspects of the embodiments. However, the embodiments may be practiced without some or all of these specific details. In other instances, well-known procedures and / or components have not been described in detail so as not to unnecessarily obscure aspects of the embodiments.

[0097] While some embodiments are disclosed here, other embodiments will become obvious to those skilled in the art as a result of the following detailed description. These embodiments are capable of modifications of various obvious aspects, all without departing from the spirit and scope of protection. Also, the reference or non-reference to a particular embodiment shall not be interpreted to limit the scope of protection.

[0098] In the following description, certain terminology is used to describe certain features of one or more embodiments. For purposes of the specification, unless otherwise specified, the term “substantially” refers to the complete or nearly complete extent or degree of an action, characteristic, property, state, structure, item, group of items, or result. For example, in one95.177.175845 / 01

[0099] embodiment, an object that is “substantially” located within a housing would mean that the object is either completely within a housing or nearly completely within a housing. The exact allowable degree of deviation from absolute completeness may in some cases depend on the specific context. However, generally speaking, the nearness of completion will be so as to have the same overall result as if absolute and total completion were obtained. The use of “substantially” is also equally applicable when used in a negative connotation to refer to the complete or near complete lack of an action, characteristic, property, state, structure, item, group of items, or result. In another example, substantially all of a group of items, may include all of the items of that group, or at least all of the items of that group that re generally within the normal parameters for the items. To the extent that the group of items might include members that far exceed the normal parameters, this abnormal item might not be expected to be part of substantially all the group of items.

[0100] As used herein, the terms “approximately” and “about” generally refer to a deviance of within 5% of the indicated number or range of numbers. Correspondingly, “substantially pure” or “consisting substantially of’ will indicate that something is effectively pure but allows for a certain degree of impurity, such as less than 12%, less than 10%, less than 5% or less than 1% other material(s). In one embodiment, the term “approximately” and “about”, may refer to a deviance of between 0.0001-39% from the indicated number or range of numbers, such as a deviance of less than 10%, less than 5% or less than 1% from the number or range given.

[0101] As used herein, the term “charcoal” (sometimes referred to in the art as “biochar” and used herein equivalently such that “charcoal” herein may be read as “biochar”) may be produced from any organic material undergoing carbonisation. Generally, charcoal / biochar is a solid, carbon-rich, material obtained from the thermochemical conversion of biomass in an oxygen-limited environment. Preferably the charcoal may be derived from any biomass, including, but not limited95.177.175845 / 01

[0102] to, sugar cane, bagasse, straw, bamboo, nut shells and other nut by-products (e.g. coconut shell or cashew nut shells and / or solid residues), rice husk, agricultural residues (e.g. agricultural waste), municipal waste, hard and softwoods. Any such materials, or any other organic material, may be the basis for the charcoal. An advantageous aspect of the present invention is the facility to use carbon captured from the atmosphere in order to reduce the net carbon released in producing the product and / or using the product in industry. In one embodiment, the charcoal (biochar) and / or the binder is therefore formed of biomass that was recently living (growing). This may be biomass which was growing (and thus taking carbon from the atmosphere) within the last 100 years (e.g. 1 week to 100 years before use) or within the last 50 years. For some forms of biomass (especially, for example, bamboo or crop residues such as straw or rice husk), the biomass may have been growing within the last 5 years (e.g. within the last 3 years or the last 1 year).

[0103] Preferably the charcoal used in the composition of the present disclosure is in the form of charcoal powder. “Charcoal powder” as used herein will typically have a weight average particle size of no more than 20 mm, such as no more than 8 mm in the largest dimension (e.g. 1 nm to 20 mm, 1 nm to 8 mm, such as 100 nm to 8 mm or 1 pm to 8 mm). Preferably the charcoal powder will have a weight average particle size of no more than 2 mm (e.g. 3 pm to 1 mm or 10 pm to 1 mm). The present inventors have found that smaller charcoal particles typically result in a stronger composite material and thus preferred charcoal powder sizes are no larger than 200 pm (e.g. 10 pm to 200 pm), preferably no more than 100 pm in largest dimension.

[0104] As used herein, the term “charcoal powder” refers to crushed or grinded charcoal, preferably of sizes indicated above. “Charcoal fines” is a waste product comprised of charcoal dust and small pieces created when processing charcoal for barbecue, the metallurgical industry, or any other application where charcoal is commonly used and may be used as the starting material for charcoal95.177.175845 / 01

[0105] powder. Charcoal powder may be found as a residue from charcoal that is a soot black powdery substance normally found at the bottom of charcoal sacks or at charcoal production and / or packing sites. Charcoal fines are generally pieces of charcoal that are normally less than 40 millimetres in diameter. These are then crushed and / or ground into charcoal powder. Preferably, the charcoal powder used may have a diameter of less than 2 millimetre (as described herein).

[0106] The charcoal powder in the various embodiments of the present invention should be approximately 60% to 100% or 70% to 100% pure charcoal, with not more than approximately 40% or 30% carbon-based filler (by weight of the charcoal component). As used herein, the term “carbonbased filler” refers to, for example, coal, coke, anthracite, graphite, wood dust, lignite, semicoke, petcoke, metallurgical coke, carbon fiber, and the like. This is in contrast to the optional “mineral filler” described herein. In one embodiment the charcoal component is pure charcoal or substantially pure charcoal.

[0107] The ratio of charcoal (where present) to metal-containing material (e.g. iron ore) in the composite material of the invention may depend on the purity of the metal-containing material. For example, the ratio may vary depending on the metal content (e.g. iron content) of the metal-containing material (e.g. iron ore). In one embodiment, sufficient carbon content is present in the composite material to reduce the metal ore to elemental metal under blast furnace conditions. In preferred embodiments, the ratio (by weight) between the metal-containing material and the charcoal is in the range of 50: 1 to 1:1, especially 10:1 to 1:1 or 5:1 to 1:1. For composite materials which contain both metal-containing material and charcoal, the preferred ratio (by weight) of metal-containing material to charcoal is in the range of 7:1 to 2:1, such as 5.5:1 to 2.5:1. Ideally the ratio (by weight) of the metal content of the metal-containing material to charcoal is in the range of 25: 1 to 1:2, such as 5:1 to 1:2 or 3:1 to 1:1.95.177.175845 / 01

[0108] All embodiments described above and elsewhere herein with respect to charcoal may also be implemented with and other elemental carbon material such as, for example, coal, coke, anthracite, graphite, lignite, semicoke, petcoke, metallurgical coke, carbon fiber, and the like.

[0109] Charcoal has significant advantages in metal processing (e.g. smelting or purification) because it typically contains much lower levels of certain undesirable impurities such as sulphur. For some metal producers, charcoal's high CO2 reactivity is an advantage compared to coke with a low CO2 reactivity of 0, 1 (AC-method)

[0110] Additionally, since charcoal contains low levels of ash (typically 1-3% by wt) compared to coke with an ash content 10-12 %, this is an advantage for biocoke made from charcoal.

[0111] In addition, the CO2 reactivity will be reduced by adding metal-containing material (e.g. metal powder) to the biocoke briquettes.

[0112] In the various aspects and embodiments of the present invention, the composite materials comprise at least one metal-containing material. It is generally preferred that the at least one metal-containing material is, comprises, consists of or consists essentially of at least one metal ore. In various embodiments, the metal-containing material (e.g. metal ore) comprises, consists or consists essentially of metal powder and / or metal fines. As used in aspect herein, “metal fines” refers to a waste product comprised of metal dust and small pieces generated when processing metal ore.

[0113] Typically, suitable metal ores will be ores of industrially valuable metal elements such as iron, copper, zinc, tin, manganese and / or nickel. Preferred ores for use in the various aspects of the present invention are iron ores (e.g. as described herein). Magnetite (FesO-i, 72.4% Fe), hematite (Fe2O3, 69.9% Fe), goethite (FeO(OH), 62.9% Fe), limonite (FeO(OH) n(H20), 55% Fe), and / or siderite (FeCCh, 48.2% Fe) are typical examples of suitable iron ores and the ore of any aspect or95.177.175845 / 01

[0114] embodiment of the invention may comprise any of these, or any mixture thereof. In one embodiment, the iron ore may consist of, or consist essentially of at least one of these ores, or any mixture thereof.

[0115] The metal-containing material (e.g. metal ore powder, especially iron ore powder) as used herein will typically have a weight average particle size of no more than 20mm, such as no more than 8mm in the largest dimension (e.g. 1 nm to 20 mm, 1 nm to 8 mm, such as 100 nm to 8 mm or 1 pm to 8 mm). Preferably when the metal-containing material comprises metal powder and / or metal fines, the metal powder and / or metal ore fine have an average particle size (largest dimension) of 10 pm to 2 mm. Preferably, the charcoal powder will have a weight average particle size of no more than 2 mm (e.g. 3 pm to 1 mm or 10 pm to 1 mm). The present inventors have found that smaller charcoal particles typically result in a stronger composite material and thus preferred charcoal powder sizes are no larger than 2000 pm (e.g. 10 pm to 200 pm), preferably no more than 1000 pm in the largest dimension.

[0116] The “metal ore” referred to herein may be purified ore obtained from mining or other suitable processes. Alternatively, or in addition, the metal ore may at least partially comprise metal ore tailings. Use of tailings may help reduce the waste generated by metal extraction processes. When filtered tailings are used, typically metals are extracted from the tailings and are formed into briquettes for re-entering the furnace, making metals. These ‘tailing’ materials typically comprise, consist or consist essentially of metal-containing material, along with finely ground rock and process water from the extraction process. Managing tailings properly is crucial to prevent environmental contamination as they may contain heavy metals, sulphides, and other hazardous substances.

[0117] The compositions of the present invention may additionally comprise waste or recycled metal95.177.175845 / 01

[0118] material and slag which is to be re-processed in a metal extraction and / or purification process. Such materials may substitute for some or all of the “metal-containing material” indicated herein such that the total amount of “metal-containing material” and recycled metal material and / or slag may be in the ranges indicated herein for metal-containing material.

[0119] Certain minerals (e.g. as described herein) have specific beneficial uses in metal smelting, extraction or purification. For example, calcium-containing materials (e.g. calcium carbonate, such as from chalk or limestone, or calcium oxide - quicklime) may be added to help generate a slag that prevents unwanted impurities from alkali metals and other unwanted metals in the final product. Preferred mineral material particle sizes may be in the range 1 nm to 100 pm, such as 1 pm to 20 pm or 3 pm to 1 pm.

[0120] As used herein, “captured carbon” indicates carbon which has been removed from the atmosphere within the last 100 years or the last 50 years. This is typically by the growth of plants such as trees, bamboo or agricultural crops but may be by other means such as chemical methods. Captured carbon may be contrasted with “fossil carbon” which is derived from fossil fuels. If captured carbon is utilized in a way that releases that carbon as CO2 into the atmosphere, the net effect is simply to replace carbon that was previously in the atmosphere (e.g. was previously removed from the atmosphere by plant growth). This has an overall zero effect on the carbon content of the atmosphere and is known as “carbon neutral”.

[0121] As used herein, “carbon neutral” or “CO2 neutral” is the property of having net-zero carbon dioxide emissions. A product or process can be carbon neutral by balancing emissions of carbon dioxide associated with a process with the capture of a corresponding amount of carbon from the atmosphere. An imbalance of no more than ±20% or ±10%, preferably no more than ±5% in the weight of carbon released and absorbed is considered “carbon neutral” herein since exact95.177.175845 / 01

[0122] measurements can be difficult.

[0123] In some embodiments, the carbon content of the composite material consists essentially of or consists of captured carbon as described herein. The use of captured carbon is significant because it avoids the release or risk of release of fossil carbon (in the form of CO2) into the atmosphere. Captured carbon (which is also referred to as “bio-carbon”) is also measurably different from fossil carbon at least in isotopic profile and can be distinguished from fossil carbon by radiocarbon methods. For example, the ratio of14C in the atmosphere is around 1 atom of14C in 1012atoms of12C and is similar for the terrestrial biosphere. Captured carbon may thus have an atom ratio of14C :12C of around 1 : 1012, such as between l:1012and l:1013or between l:1012and 1 : 1014. Carbon with an atom ratio of14C :12C of less than around 1 : 1015is likely to comprise a high level of carbon which has not been in the atmosphere or biosphere for at least 50,000 years and so would not be considered “captured carbon” or composite herein.

[0124] The carbon material, as described herein will preferably comprise at least 50% (e.g. 50 to 100%), preferably at least 70% and more preferably at least 95% captured carbon (e.g. in the form of charcoal). Similarly, the binder material as described herein will preferably comprise at least 50% (e.g. 50 to 100%), preferably at least 70% and more preferably at least 95% captured carbon. In one embodiment, the binder is formed of phenols which are of biological origin and thus consist of captured carbon. Phenols from Cashew Nut Shell Liquid are a preferred example. Where the binder comprises an accelerator (e.g. hexamine or a formyl carbon source) then this may comprise captured carbon (e.g. if the accelerator is formed form bio-methanol) or may comprise fossil carbon (e.g. if the accelerator is formed from a fossil carbon source such as oil or natural gas). In various embodiments of the present disclosure, at least one binder is utilized. Preferred binders include at least one phenol based polymer (e.g. phenolic resin). Phenol based polymers may be95.177.175845 / 01

[0125] any polymer formed or formable from phenolic materials (e.g. formed or formable from at least 50% (such as 50% to 100% or 75% to 100%) by weight of starting materials having at least one phenol moiety, such as those discussed herein including those of formula I) by any polymerisation method. Examples include by formation of phenol / aldehyde phenolic resins (addition / alkylolation, alkylene bridge formation etc.) and / or by oxidative cross-linking of unsaturated carbon-carbon bonds (e.g. under acid catalysis). Phenolic resins are typically generated by the polymerization of at least one phenol, typically with or utilizing at least one aldehyde or alkanoyl (esp. formyl) carbon source such as hexamine.

[0126] Phenols suitable for the formation of phenol based polymers (e.g. phenolic resins) for use as a binder include those of formula I below:

[0127]

[0128] In formula I, X is H or OH and R is H or an optionally substituted, saturated or unsaturated, hydrocarbon moiety of 1 to 24 carbons, which may be straight-chain or branched. In one embodiment, the at least one phenol of formula I comprises at least one phenol wherein R is not hydrogen. R will typically be at the position meta to the phenolic OH group. Generally, unsubstituted phenol does not form the sole phenol for generating the phenol based polymer as described herein.

[0129] Thus, generally, the phenol based polymer (e.g. phenolic resin) will be formed from (i.e. be95.177.175845 / 01

[0130] polymers of) at least one phenol wherein at least a portion of the phenols of formula I will have R as a moiety other than hydrogen. Preferably, not more than 60% (e.g. 1 to 50%) or not more than 30% by weight of the phenols of formula I will have R=H, preferably not more than 10% and more preferably not more than 1%. In one embodiment, the phenol(s) of formula I do not have hydrogen as moiety R. Typical examples of R include Cl to C24 hydrocarbons, such as C6 to C20 (e.g. C8 to Cl 8 or CIO to Cl 7) saturated or unsaturated hydrocarbons having straight or branched chains. Such hydrocarbon moieties may be saturated or unsaturated. Such unsaturation may be in the form of at least one double and / or triple bond within the hydrocarbon moiety, such as 1, 2, 3, 4 or 5 double bonds. Double bonds, where present, may be cis- or trans- double bonds. Preferably at least one cis double bond may be present in at least a portion of the phenols of Formula I. In one embodiment, 0, 1, 2 or 3 double bonds may be present and mixtures of two or more may be present in the phenols of formula I. Where the R moiety is a substituted hydrocarbyl moiety, this may be substituted with any appropriate group, such as Cl, F, OH, NH2 epoxy or other substituents. Amine and hydroxyl substituted compounds of formula I are particularly suitable. Epoxy substitution may also be used. In one embodiment, R is CisHsi-n where n is 0, 2, 4 and / or 6.

[0131] In one embodiment, the phenolic binder may be a polymer of (e.g. formed or formable from) phenols of formula I comprising, consisting essentially of or consisting of cardanol and / or cardol. In one embodiment, the phenolic binder is formed or formable from phenols comprising at least 50% (e.g. 50% to 100%) cardol and / or cardanol (e.g. at least 70% or at least 80%, such as at least 90%).

[0132] As an alternative or partial alternative to pure phenol based polymer binders, epoxy resins may be utilized. In particular, the phenols of formula I may be epoxidised using known methods such as epichlohydrin. For example, cardanol may be epoxidised as below:95.177.175845 / 01

[0133] Cardanol Monoepoxidized cardanol

[0134]

[0135] Diepoxidized cardanol

[0136] Furthermore, the phenols of formula I may be formed into novalac-type phenolic resins by use of a formyl carbon source such as hexamine, as disclosed herein, and may subsequently be epoxidised and then further crosslinked by reaction of the epoxidised prepolymer:

[0137] OH

[0138] Acid nHCHO

[0139] novolac-type phenolic resins

[0140] n

[0141]

[0142] novolac-type phenolic resins epoxy novolac resin

[0143] In an alternative embodiment, the phenol based polymer (e.g. phenolic resin) does not comprise any epoxy groups and does not include any epoxidation step in the synthesis of the phenol based polymer.95.177.175845 / 01

[0144] As used herein, the term “cashew nutshell liquid” or “CNSL” refers to the liquid that is a natural resin with a yellowish sheen found in the honeycomb structure of the cashew nutshell and is a byproduct of processing cashew nuts. Naturally occurring CNSL contains mainly four components: anacardic acid, cardanol, cardol, and 2-methyl cardol. These four components are monohydric or dihydric phenols or phenolic acids with a hydrocarbon sidechain at the metaposition. CNSL may be heat treated to decarboxylate the anacardic acids, producing a technical grade of CNSL that is rich in cardanol. Distillation of this material gives distilled, technical CNSL containing 78% cardanol and 8% cardol. In one embodiment, the phenols of formula I are around 78% cardanol and around 8% cardol (e.g. 75-85% cardanol and 5 to 15% cardol). In one embodiment, the phenol based polymers (e.g. phenolic resins) referred to herein may be polymers of phenols comprising, consisting essentially of, or consisting of phenols derived from CNSL. In a preferred embodiment, the binder used herein is derived from CNSL (e.g. comprises CNSL or a component derived therefrom (e.g. cardol and / or cardanol) as at least 50% by weight (e.g. 60 to 99%) of the binder / polymer starting material).

[0145] As used herein, the term “cardanol” or “cardanol oil” refers to the component of CNSL that has the molecular formula of C21H30O, C21H32O, C21H34O and / or C21H36O and the following structure:

[0146]

[0147] Where n is 0, 2, 4 or 6. Typically a mixture containing at least some n=6 is present.

[0148] Cardanol is a phenolic lipid obtained from anacardic acid, the main component of cashew nutshell liquid.95.177.175845 / 01

[0149] OH O

[0150] Anarcardic Acid Cardol

[0151]

[0152] Some anarcardic acid (e.g. 0 to 20% such as 1 to 15% or 1 to 10% by weight) may be present in the binder.

[0153] Cardanol as a mixture of long-chain alkyl phenols having the Cl 5 chains shown above (which correspond to group “R” in formula I and the structures herein) has CAS number 37330-39-5. Purified cardanol having R-group C15H25 as above is also available under the same CAS number. Either grade may be used in the various aspects of the present invention as all or a part of the phenols of formula I. In one embodiment, at least 50%, preferably at least 75% of the phenols of formula I consist of cardanol CAS 37330-39-5, such as the cardanol mixture indicated above. In the composite materials of the present disclosure, the amount of binder component will typically be 1% to 30% by weight (as discussed herein). A maximum of around 25-30% binder is preferred as the material can lose binder when compressed if a greater amount is employed. However, as the particle size of the metal-containing material (and optionally charcoal and / or optional mineral material) may affect the maximum amount of binder, the upper limit will be readily determined for any specific composition by the skilled worker.

[0154] In some embodiments, the binder is a phenol based polymer comprising, consisting or consisting95.177.175845 / 01

[0155] essentially of functionalised cardanol, preferably epoxidized cardanol, formylated cardanol, and / or a cardanol based epoxy resin.

[0156] The binder component in the various embodiments of the present invention may comprise, consist essentially of, or consist of a phenolic binder. Such a binder may comprise or consist of polymers of phenols such as the phenols of Formula I as described herein. The method of forming the composite material of the disclosure may comprise mixing metal-containing material (e.g. metal ore powder) with the phenol(s) and other materials such as the optional accelerator (as described herein) and / or optional carbon materials, forming the mixture into the desired shape, optionally compressing the material (as described herein) and curing the material (as described herein). The binder component may alternatively be in the form of a pre-polymer such as a “novalac” type resin (as known in the art and described above). This pre-polymer may be mixed with the other components including metal-containing material (e.g. metal ore powder) and optionally including additional phenol(s) and optional components such as accelerator(s), drying oils and / or carbon and / or mineral materials. These various components are described herein. The pre-polymer mixture may then be cured by crosslinking such as by reaction with aldehydes or formyl carbon sources, by epoxy modification and crosslinking (see above) and / or by oxidative crosslinking (as is known for drying oils).

[0157] In one embodiment, at least 50% of the carbon present in the binder is captured carbon. This may be 50 to 100% or 50 to 98% or 70 to 99% by weight. Using binders comprising materials from natural sources (such as cardanol with or without cardol) increases the amount of captured carbon in the composite material and improves the carbon-neutral properties. Binders utilising fossil carbon may be used as a full or partial alternative.

[0158] In one embodiment, the binder does not comprise lignin or comprises lignin in an amount of less95.177.175845 / 01

[0159] than 1% by weight of the binder component.

[0160] As used herein, the term “pressurized” or “compressed” refers to the act of subjecting a mixture or composition to pressure. The pressure applied may be via a pneumatic press, mechanical press, electric press, extruder, roller press, and the like. Compression may take place once or may be carried out multiple times (e.g. 2, 3, 5 or 10 times). Multiple compression may provide a stronger product once cured. Whenever pressurizing or compression is referred to herein, this may optionally be accompanied by vibration, either sequentially or simultaneously.

[0161] CNSL and cardanol may be extracted and purified, using many different methods, including mechanical extraction, thermal extraction, solvent extraction (static, Soxhlet, ultrasonic, carbon dioxide), and pyrolysis. Mechanical and thermal extractions are favorable and are the most commonly used and commercially practiced. In one embodiment, CNSL is typically treated with high temperatures, which decarboxylates anacardic acid, yielding cardanol. Additional distillation of CNSL removes at least some of the cardol leaving the cardanol in pure or at least purer form. Such “technical grades” of cardanol are suitable as sources of phenols for the binders of the present invention.

[0162] As used herein the term “hexamine”, which is also called urotropine, methenamine, hexamethylenetetramine, refers to a heterocyclic organic compound with the formula (CILje Hexamine is a white crystalline compound that is highly soluble in water and polar organic solvents. It is useful in the synthesis of other organic compounds, including plastics, pharmaceuticals, and rubber additives. It may also be used as an accelerator or catalyst. Other sources of formyl carbon may be used as accelerator, including those described herein.

[0163] Other catalysts & accelerators that may be used are cationic, ionic, and oxidizing agents that may accelerate the polymerization of the cardanol when it is heated. Other alkalis may also be used as95.177.175845 / 01

[0164] a catalyst. The terms accelerator, accelerant and catalyst may be used interchangeably herein. Hexamine is a useful source of formyl carbons but other formyl sources may be used. These include formaldehyde and oligomers of polymethylene glycol such as formalin or paraformaldehyde. Other aldehydes may also be used.

[0165] Urea and / or urea derivatives (such as methylolurea) may also be used as accelerator alone or in combination with a formyl carbon source. Metal oxides such as magnesium oxide may be of value as a catalyst where urea or urea derivatives are included.

[0166] Acids may also be used as accelerants in the materials of the present invention (either alone or in combination with accelerants such as alkanoyl carbon (esp. formyl carbon) sources). Suitable acids include mineral acids, such as hydrochloric acid, sulphuric acid, nitric acid and / or phosphoric acid. Organic acids such as acetic acid, citric acid, oxalic acid etc may also be used as accelerators. Examples of suitable acid accelerators include p-toluenesulfonic acid, Lewis acid catalysts (e.g. zinc acetate, zinc oxide) and polyacids (e.g. citric acid).

[0167] In general, bio-based catalysts are preferred to avoid formaldehyde emissions using hexamine as a catalyst.

[0168] Phenol based polymer binders (particularly those formed at least partially from cardanol) form one preferred embodiment of the present disclosure. Such phenolic binders may be formed by reaction of phenols, such as those of formula I herein with themselves (e.g. by oxidative cross-linking) or with accelerators such as hexamine or other formyl carbon sources. They may additionally be epoxidised either as monomers or as pre-polymers and cured with conventional epoxy curing agents such as amines (e.g. phenalkamines). In one particular embodiment, epoxidised phenols and / or phenol pre-polymers such as those indicated herein may be cured by or with the addition of ionic liquids. In particularly, phosphonium based ionic liquids may be used. In one95.177.175845 / 01

[0169] embodiment, the phenol based polymer is not an epoxy resin. For example, in one embodiment, the phenol based polymer does not comprise any epoxy component (e.g. is not formed by epoxidation of the phenol or any pre-polymer). In one embodiment, the binder component may comprise, consist essentially (e.g. contain 90% to 100% by weight) of or consist of at least one phenol based polymer (e.g. phenolic resin), optionally with an additional binder such as those described herein.

[0170] As whole or partial replacement for the phenol based polymer binder described herein, any appropriate binder may be utilized in all proportions and embodiments described herein where technically viable. Such alternative binders include other polymers such as melamine or epoxy resins or inorganic binders. Suitable inorganic binders, such as polysilicates, include water glass (e.g. sodium silicate) modified with nanoparticles of metal oxides. Such materials are described in EP3524372A1 which is incorporated herein by reference. Inorganic binder may be used in combination with organic binders such as the phenol based polymer binders described herein. In one preferred embodiment, the materials of the present invention do not comprise any inorganic binder (although they may comprise mineral material(s) such as CaCCF, as described herein). In some embodiments, the phenol based polymer binder may be wholly or partially replaced with non-ionic polyacrylamide (NPAM) and / or anionic polyacrylamide (APAM). In preferred embodiments, the phenol based polymer binder may be partially replaced with NPAM and / or APAM. The presence of NPAM and / or APAM may enhance the green strength of the material. In preferred embodiments, NPAM and / or APAM is present in an amount of 0.1 to 5 wt% of the total composite material, preferably 0.1 to 2.0 wt%, especially 0.25 to 1.0 wt%. of the total composite material.

[0171] In some embodiments, the phenol based polymer binder may be wholly or partially replaced with95.177.175845 / 01

[0172] polyvinyl alcohol (PVA). In some embodiments PVA is used in combination with APAM and / or NPAM. The presence of PVA, particularly in combination with APAM and / or NPAM may enhance the green strength of the material. The presence of PVA may also improve the water resistance and elasticity of the composite material. In preferred embodiments, PVA is present in an amount of 0.1 to 5 wt% of the total composite material, preferably 0.1 to 2.0 wt%, especially around 1 wt% of the total composite material. In preferred embodiments, a combination of PVA and APAM is used. In preferred embodiments, PVA and APAM are used as partial replacements of the phenol based polymer binder and are present at a weight ratio of 5:1 to 1:5 PVA / APAM, such as 3:1 to 1:2, especially 2.5:1 to 1:1 PVA / APAM.

[0173] In some embodiments, the phenol based polymer binder may be wholly or partially replaced with hydrated lime (i.e. calcium hydroxide). In preferred embodiments, the phenol based polymer binder may be partially replaced with hydrated lime. For example, hydrated lime may be used as a partial replacement of the phenol based polymer binder, particularly when the ratio (by weight) of phenol based polymer (e.g. cardanol) binder to hydrated lime binder is in the range of 1:1 to 1:5, especially 1:1 to 1:3, such as around 1:2.

[0174] In some embodiments, the phenol based polymer binder may be wholly or partially replaced with melamine formaldehyde resin. In preferred embodiments, melamine formaldehyde is used as a partial replacement for the phenol based polymer binder. Any melamine formaldehyde may be used, for example, as an accelerator since it is a formyl carbon source. In some embodiments therefore, melamine formaldehyde may be used wholly (or partially) in place of hexamine. In especially preferred embodiments, melamine formaldehyde is present in amount of up to 50 wt% of the phenol based polymer (e.g. phenolic resin) binder, such as 10 to 50 wt% or 20 to 40 wt%, especially 25 to 35 wt% of the phenol based polymer binder. Advantageously, when melamine95.177.175845 / 01

[0175] formaldehyde is used as a secondary binder, hexamine accelerator may be avoided.

[0176] In addition to the main (especially phenolic) binder, the composite materials and all corresponding aspects of the invention may also comprise an optional secondary binder. In one embodiment, the secondary binder serves to increase the “green strength” of the material, which is the strength after forming but before curing. The secondary binder may be any binder which serves to increase “green strength” of the mixture without compromising the strength of the cured product.

[0177] Examples of typical “secondary binders” include “drying oils” such as those discussed herein above including linseed oil, and polysaccharide binders such as alginate, guar gum or starch-based binders. Starch binders may comprise any form of starch such as corn starch, wheat starch, potato starch, rice starch and any combination thereof. “Starch” in all examples includes “modified starch” such as modified corn starch, modified wheat starch, modified potato starch, modified rice starch and any combination thereof. “Modified starch” is a well understood term in the art and includes physically, enzymatically, and / or chemically treated starch from any suitable source. Particularly useful starch modifications include those which make starch soluble in cold water. These may include extrusion, drum drying, spray drying or dextrinization (roasting with HC1). In one embodiment, the secondary binder comprises cold-water soluble modified starch (e.g. from potato).

[0178] The whole or partial replacements for phenol based resin binder discussed herein, such as NPAM, APAM, PVA, hydrated lime and melamine formaldehyde may serve as secondary binders. Therefore the term “secondary binder” includes components which partially replace the phenolic resin binder content.

[0179] The secondary binder may be present in an amount of up to 50% (e.g. 1 to 50%) by weight of the binder component or around 15% of the total composite material. This will preferably be 5 to 40%95.177.175845 / 01

[0180] of the binder component or 10 to 35% (e.g. 15 to 30%).

[0181] In some cases, the secondary binder may be present in an amount of up to 5 wt% of the total composite material, such as 0.1 to 5 wt%.

[0182] In some cases, the secondary binder may be present in an amount of 3 to 15 wt% of the total binder component, preferably 5 to 14 wt% of that component.

[0183] In the methods described herein, water may be used as a processing aid. This is particularly to serve as a lubricant in formation (e.g. extrusion, briquetting or peletisation) and may also assist in the incorporation of secondary binders such as polysaccharide binders (such as starch or modified starch). Where water is added to the mixture, this will typically be prior to the shaping of the product and will typically be removed by drying prior to curing of the binder. In one embodiment, the shaped “green” product (i.e. prior to curing) is dried at a temperature of 50 to 120°C (e.g. 80 to 105°C or 60 to 98°C) for 10 minutes to 2 hours prior to the curing step. This drying step may be to reduce the water content of the green product to less than 10% by weight, preferably less than 8% or less than 5% by weight prior to curing. If high levels of water remain in the product at the curing step, the binder may not cure effectively and the properties of the final product may be inferior. Water used as a processing aid is not taken into account in the calculation of the wt% of components herein since this water is generally not present at a high level in the final product. In one embodiment, the composite material (e.g. briquette) as described herein may be waterproof or substantially weatherproof and can be stored outside in the elements. In one embodiment, the composite material (e.g. briquette) as described herein may be waterproof to the extent that the material will not crumble or lose its structure after immersion in water at 20°C for 24 hours, preferably 48 hours, more preferably 7 days. Preferably, the composite material (e.g. briquette) as95.177.175845 / 01

[0184] described herein may take on 5-10% by weight of water and may be exposed to immersion in water for corresponding periods without there being any structural weaknesses of the material.

[0185] In one embodiment, the composite material (e.g. briquette) as described herein is sufficiently strong that it can be loaded, transported, unloaded and stored in bulk with similar equipment and practices commonly used today in the manipulation and storage of coal, petcoke, metcoke and gravel.

[0186] In preferred embodiments, the composite material maintains structural integrity when heated to 500°C or higher, such as 750°C or higher, especially up to and including 900°C. The term “maintains structural integrity” herein refers to the composite material being robust to manual handling. For example, the composite material undergoes no collapse in structure when subjected to a force of at least 50 dN, preferably at least 100 dN.

[0187] Prior to the compositions and methods of the present disclosure, the volatile organic compounds and gasses within charcoal are in the range of approximately 0-30% weight by volume. Cardanol is a preferred binder for use in the various aspects of the present invention. Cardanol has approximately less than 1% volatile organic compounds after purification and distillation of the CNSL. Accordingly, Cardanol is not only environmentally friendly, but it is non-volatile and essentially harmless.

[0188] In one embodiment, the pressurization (compression) may be done at standard pressure (approximately 1 bar or approximately 0.1 MPa).

[0189] In one embodiment, curing may take place in an inert, standard atmosphere.

[0190] When cured in an oxygen rich atmosphere with no added pressure, the curing temperature may be lowered to approximately 400°C and below (as described herein) below 300 °C or below 200 °C are preferred.95.177.175845 / 01

[0191] Other embodiments may be used in addition to or instead of the illustrative embodiments. Details that may be apparent or unnecessary may be omitted for the purpose of saving space or for more effective illustrations. Some embodiments may be practiced with additional components or steps and / or without some or all components or steps provided in the illustrations.

[0192] Unless otherwise stated, all measurements, values, ratings, positions, magnitudes, sizes, locations, and other specifications that are set forth in this specification, including in the claims that follow, are approximate, not exact. They are intended to have a reasonable range that is consistent with the functions to which they relate and with what is customary in the art to which they pertain. All percentages are by weight unless indicated otherwise, or unless context requires another meaning. Where a quantity or range is indicated as “about”, approximately, substantially or similar, the stated value will be most preferred but may be varied as understood in the art without departing from the substance or effectiveness of the invention. Typically, values of ±10%, preferably ±5%, ±1% or ±0.5% of the stated value will be appropriate where such qualifiers are given. Components that “consist essentially of’ a material will have a corresponding interpretation, while all components which “comprise” or “consist essentially of’ some material(s) may consist of the stated material(s) as a preferred embodiment.

[0193] The foregoing description of the preferred embodiment has been presented for the purposes of illustration and description. While multiple embodiments are disclosed, still other embodiments will become apparent to those skilled in the art from the above detailed description. These embodiments are capable of modifications in various obvious aspects, all without departing from the spirit and scope of protection. Accordingly, the detailed description is to be regarded as illustrative in nature and not restrictive. Also, although not explicitly recited, one or more embodiments may be practiced in combination or conjunction with one another. Furthermore, the95.177.175845 / 01

[0194] reference or non-reference to a particular embodiment shall not be interpreted to limit the scope of protection. It is intended that the scope of protection not be limited by this detailed description, but by the claims and the equivalents to the claims that are appended hereto.

[0195] Except as stated immediately above, nothing that has been stated or illustrated is intended or should be interpreted to cause a dedication of any component, step, feature, object, benefit, advantage, or equivalent, to the public, regardless of whether it is or is not recited in the claims.

[0196] The invention will be illustrated further below by reference to the following non-limiting examples:

[0197] Example 1 - Formation of metal ore briquettes with phenolic binder

[0198] Iron ore particles were passed through a sieve of 1 mm in width and 2 mm in length mesh size (the holes in the sieve is oblong in shape) to provide particles no larger than 100 pm.

[0199] The iron ore powder particle sizes were measured by laser using a Mastersizer 3000E laser size analyzer. The particles were found to have a distribution from 10 pm to 100 pm. A summary of the properties of the iron ore particle size is provided in the below Table 1. The chemical composition of the iron ore particles is additionally summarised in Table 2, where the composition was determined using X-Ray diffraction (XRD). The iron ore concentrate comprises hematite (45.0 %), goethite (34.8 %), quartz low (9.6 %), kaolinite (7.9 %) and magnetite (2.6 %).

[0200] Table 1

[0201] Top-Size (mm) 0.029

[0202] D50 (mm) 0.006

[0203] D90 (mm) 0.022

[0204]

[0205] 95.177.175845 / 01

[0206] Average Diameter (mm) 0.023

[0207] Specific Area (cm2 / g) 2800

[0208]

[0209] Table 2

[0210] Fraction Fe FeO S1O2 AI2O3 P (%) Mn CaO MgO T1O2 PPC (mm) (%) (%) (%) (%) (%) (%) (%) (%) (%) Total 57.32 8.94 2.53 0.097 0.138 0.126 0.042 0.100 5.01 > 0.045 mm 37.05 39.78 0.990 0.097 0.114 1.536 0.093 0.119 3.90 < 0.045 mm 58.51 8.32 2.320 0.087 0.133 0.099 0.044 0.102 4.86

[0211]

[0212] Technical grade cardanol was mixed with iron ore in the amounts indicated in table 3 below. The mixture was stirred for around 1-10 minutes until moist but not wet. The mixture was then kneaded and_20.5g of the moist mixture was transferred to a die with more than 10 holes with diameter 3-10 mm where the mixture was sheared. Bentonite clay was added in an amount of 1-10%, which is thought to increase homogeneity, plasticity and green strength of the briquette

[0213] After kneading and shearing the extruded mixture was pressed with hydraulic press with vibration with a force of 1-500 kN / cm2to form green tablet blocks / briquettes ready for curing. A repeated pressing was found to improve the strength of the final product.

[0214] The green tablet blocks / briquettes were cured in an oven at 200°C for up to 5 hours before cooling in ambient air.

[0215] Iron ore briquettes:

[0216] Table 395.177.175845 / 01

[0217] Mixture Ore (g) Ore (%) Cardanol (g) Cardanol (%) 1 950 95% 50 5%

[0218] 2 4700 94% 300 6%

[0219] 3 5880 98% 120 2%

[0220]

[0221] Example 2 - Formation of extruded composite material with iron ore and binder

[0222] Iron ore (as defined in Example 1), modified starch (secondary binder) and hexamine were thoroughly mixed as dry powders in a high-speed industrial mixer. Once the powders were mixed, cardanol (which had been pre-activated at 130 °C for 2 hours) and water 18% were added and the mixture introduced to an extruder.

[0223] 15mm rods were extruded and cut to a length of around 200mm. The rods were found immediately to have sufficient “green” strength for manual and automated handling without loss of shape. The extruded rods were then dried and cured as indicated in Table 4 below.

[0224] Table 4

[0225] Mixture IE1 IE2

[0226] Iron Ore (%) 93.00 91.00

[0227] Modified Starch (%) 1.00 1.00

[0228] Cardanol (+10% hexamine*) 6.00 8.00

[0229] Extrusion

[0230] Pellet Diameter (mm) 19 19

[0231]

[0232] 95.177.175845 / 01

[0233] Extruder pressure (bar) 50 11

[0234] Throughput (g / min) 2077 2183

[0235] Pellet Temperature (‘C) 50 50

[0236] Curing

[0237] Cure time (h) 3 3

[0238] Cure Temp (‘C) 135 135

[0239]

[0240] *with respect to the total cardanol content.

[0241] The degree of size degradation of IE1 and IE2 was tested following method ISO 13930-2015 and compared to a commercial iron-ore containing briquette as a comparison. When heated to 500 °C, both IE1 and IE2 showed a thermal resistance which was similar to the commercial standard. When heated to 750 °C and 900 °C, the highest thermal resistance was evident for IE1, and the pellets of the commercial standard demonstrated the lowest thermal resistance.

[0242] The resistance after reduction (RAR) was then measured on each sample, and the results for all fractions were similar, with the structure remaining intact after exposure to high temperatures and being subjected to forces of at least 100 dN, with no collapse observed.

[0243] The results therefore demonstrate that briquettes based on iron ore and cardanol based binder have an impressive performance, wherein the agglomerate could maintain structural integrity, even when subjected to temperatures up to 900 °C. The performance of the briquette was just as good, if not better than the commercial standard.95.177.175845 / 01

[0244] Example 3 - Composite Materials with Alternative Secondary Binders

[0245] Iron ore (as defined in Example 1), secondary binder (as set out in Table 5) and hexamine were thoroughly mixed as dry powders in a high-speed industrial mixer. Once the powders were mixed, cardanol (which had been pre-activated at 130 °C for 2 hours) and water (18%) were added and the mixture introduced to an extruder.

[0246] 15mm rods were extruded and cut to a length of around 200mm. The rods were found immediately to have sufficient “green” strength for manual and automated handling without loss of shape. The extruded rods were then dried and cured as indicated in Table 5 below.

[0247] Table 5

[0248] Mixture IE3 IE4

[0249] Iron Ore (%) 95 93.5

[0250] Anionic Polyacrylamide (APAM) (%) 1 0.5

[0251] Polyvinyl alcohol (PVA) (%) 1

[0252] Cardanol (+8% hexamine*) 4 5

[0253] Extrusion

[0254] Pellet Diameter (mm) 19 19

[0255] Extruder pressure (bar) 50 11

[0256] Throughput (g / min) 2077 2183

[0257] Pellet Temperature (‘C) 50 50

[0258]

[0259] 95.177.175845 / 01

[0260] Curing

[0261] Cure time (h) 3 3

[0262] Cure Temp (‘C) 135 135

[0263]

[0264] *with respect to the total cardanol content.

[0265] Example 4 - Formation of extruded composite material with ore, binder and carbon Iron ore particles were passed through a sieve of 1 mm in width and 2 mm in length mesh size (the holes in the sieve is oblong in shape) to provide particles no larger than 100 pm.

[0266] The iron ore powder particle sizes were measured by laser using a Mastersizer 3000E laser size analyzer. The particles were found to have a distribution from 10 pm to 100 pm.

[0267] Charcoal pieces were crushed and the resulting particles passed through a sieve of 1mm in width and 2mm in length mesh size (the holes in the sieve is oblong in shape) to provide particles no larger than 100 pm.

[0268] Carbon powder particle sizes were measured by laser using a Mastersizer 3000E laser size analyzer. The particles were found to have a distribution from 10 pm to 100 pm.

[0269] Iron ore, charcoal powder, modified starch (secondary binder) and hexamine were thoroughly mixed as dry powders in a high-speed industrial mixer. Once the powders were mixed, cardanol and water 18% were added and the mixture introduced to an extruder.

[0270] 15mm rods were extruded and cut to a length of around 200mm. The rods were found immediately to have sufficient “green” strength for manual and automated handling without loss of shape. The extruded rods were then dried and cured as indicated in Table 6 below.95.177.175845 / 01

[0271] Table 6

[0272] Mixture 1 2 3

[0273] Iron Ore (%) 70.7 70.7 76.2

[0274] Charcoal (%) 22.3 22.3 16.3

[0275] Modified Starch (%) 1.00 1.00 1.50

[0276] Cardanol (+10% hexamine*) 6.00 6.00 6.00

[0277] Extrusion

[0278] Pellet Diameter (mm) 19 19 19

[0279] Extruder pressure 100 75 35

[0280] Throughput (g / min) 2077 2183 2580

[0281] Pellet Temperature (‘C) 50 50 35

[0282] Curing

[0283] Cure time (h) 3 3 3

[0284] Cure Temp (‘C) 135 135 135

[0285] Analysis

[0286] Green Pellet Density (g / cm3) 2.14 2.18 2.43

[0287] Dry Pellet Density (g / cm3) 1.88 1.94 2.06

[0288]

[0289] 95.177.175845 / 01

[0290] *with respect to the total cardanol content.

[0291] Example 5 - water resistance testing.

[0292] 10 briquettes of composite material were each weighed and placed in a closed bottle of water. The briquettes were each soaked for 12, 24, 48 and 72 hours before removal and re- weighing. No briquette exceeded 5% increase in mass after soaking in water. Furthermore, when the briquettes were placed in a tumbler and tumbled for 30 minutes following immersion, no weakness in the briquettes was found.

Claims

95.177.175845 / 01Claims:1) A composite material comprising:a) about 1% to about 99% by weight of at least one metal-containing material; and about 1% to about 40% by weight of at least one binder comprising a phenol based polymer.2) The composite material of claim 1 further comprising at least one carbon material.3) The composite material of claim 1 or claim 2 wherein the metal-containing material is a metal ore, preferably comprising at least one iron ore.4) The composite material of any of claims 1 to 3 wherein the binder is present in an amount of 2% to 32% by weight.5) The composite material of any preceding claim wherein the phenol based polymer is a polymer of at least one phenol of formula I and optionally an accelerator:Iwherein X is H or OH and R is one or more groups selected from H or an optionally substituted, saturated or unsaturated, hydrocarbon moiety of 1 to 24 carbons, which may be straight-chain or branched.95.177.175845 / 016) The composite material of claim 5 wherein the at least one phenol of formula I comprises at least one phenol wherein at least one R is not hydrogen.7) The composite material of claim 5 wherein the at least one phenol of formula I comprises at least one phenol wherein one R is a C6 to C20 unsaturated hydrocarbyl moiety optionally substituted with at least one amine, hydroxyl and / or epoxy moiety.8) The composite material of claim 5 wherein the at least one phenol of formula I comprises, consists essentially of or consists of anacardic acid, cardol, methyl cardol and / or cardanol.9) The composite material of any preceding claim wherein the phenol based polymer is a phenolic resin polymer of at least one phenol of formula I and at least one accelerator selected from at least one aldehyde or formyl-carbon source such as hexamine, formaldehyde or a polyformaldehyde.10) The composite material of any preceding claim wherein the binder consists of or consists essentially of at least one phenol based polymer, such as the polymer of claim 5.11) The composite material of any preceding claim wherein the phenol based polymer is a polymer of at least one phenol consisting of or consisting essentially of anacardic acid, cardol and / or cardanol, particularly cardol and / or cardanol.12) The composite material of any preceding claim wherein an accelerator is present in a range of 0.1% to 15% by weight of the binder.95.177.175845 / 0113) The composite material of claim 5 or 12 where the accelerator is at least one source of formyl carbons such as hexamine, formaldehyde and / or oligomers of polymethylene glycol such as formalin or paraformaldehyde.14) The composite material of claim 5 or 12 where the accelerator is at least one acid, such as a mineral acid.15) The composite material of any preceding claim, wherein said binder is present in a range of approximately 2.2% to 30% by weight of said mixture.16) The composite material of any of claims 2 to 15 wherein the carbon material is present in an amount of 1 to 50 wt%, such as 5 to 40 wt%, preferably 10 to 30 wt%.17) The composite material of any of claims 2 to 16 wherein the carbon material comprises, consists essentially of or consists of at least one material selected from coke, charcoal and mixtures thereof.18) The composite material of any preceding claim wherein said material is formed by mixing said metal-containing material and said binder and curing said binder.19) The composite material of claim 18 wherein said mixture is compressed and optionally vibrated.20) The composite material of claim 19, wherein said mixture is compressed at a range of approximately 1 to 50 MPa for between one and ten repetitions.21) The composite material of any preceding claim wherein said material is cured at less than 450° C.95.177.175845 / 0122) The composite material of any preceding claim wherein said material is cured at a range of approximately 90°C to 250° C for approximately 1 hour to 8 hours.23) The composite material of any preceding claim for use as a feedstock for metal smelting.24) The composite material of any preceding claim wherein the binder additionally comprises 1 to 50% by weight of the binder component of a secondary binder which increases the uncured (green) strength of the material.25) The composite material of claim 24 wherein the secondary binder is at least one “drying oil” such as linseed oil, and / or at least one polysaccharide such as alginate, guar gum or starch.26) The composite material of claim 25 wherein the starch is corn starch, wheat starch, potato starch, rice starch, modified corn starch, modified wheat starch, modified potato starch, modified rice starch and any combination thereof.27) A composition comprising:cardanol;iron ore powder;charcoal powder; and optionallyhexamine;wherein said cardanol, said charcoal powder, said iron ore power, and optionally said hexamine are mixed together to form a mixture;wherein said mixture is cured at a range of approximately 100°C to 250°C;95.177.175845 / 01wherein said mixture is pressurized at a range of approximately 3 to 50 MPa;wherein said cardanol is in a range of approximately 2% to 12% by weight of said mixture; wherein said iron ore powder is in a range of approximately 50 to 80% by weight of said mixture;wherein said charcoal powder is in a range of approximately 10% to 30% by weight of said mixture; andwherein said hexamine is in a range of 0.01% to 1% by weight of said mixture where present. 28) A method of preparing a composite material, comprising the steps:providing at least one phenol such as cardanol;providing at least one metal-containing material (e.g. metal ore powder);optionally providing charcoal powder;mixing at least one said phenol with said metal-containing material and with said charcoal powder if present, such that a composition comprising phenol and metal ore (and optionally charcoal) is created;compressing and optionally vibrating said composition; andcuring said composition.29) The method of claim 28, further comprising the step:providing a catalyst and / or accelerator;wherein said catalyst and / or accelerator is mixed with said phenol and said metal-containing material (and optionally charcoal material), such that said composition comprises said catalyst95.177.175845 / 01and / or accelerator.30) The method of claim 29, wherein said phenols are present in a range of approximately 1% to 40% by weight of said composition;wherein said metal-containing material is present in a rage of approximately 58% to 95% by weight of said composition;wherein said catalyst and / or accelerator is in a range of 0.1% to 15% by weight of said composition;wherein said composition is pressurized at a range of approximately 3 to 50 MPa; and wherein said composition is cured at a range of approximately 100 °C to 250 °C.31) The method of claim 29, wherein charcoal is present and said phenols are present in a range of approximately 1% to 40% by weight of said composition;wherein said metal-containing material is present in a rage of approximately 50% to 80% by weight of said composition;wherein said charcoal powder is in a range of approximately 10% to 30% by weight of said composition; andwherein said catalyst and / or accelerator is in a range of 0.1% to 15% by weight of said composition;wherein said composition is pressurized at a range of approximately 3 to 50 MPa; and wherein said composition is cured at a range of approximately 100 °C to 250 °C.32) A briquette comprising a composite material as claimed in any of claims 1 to 26.33) The briquette of claim 32 which is waterproof.