Method for recycling alkali metal battery production waste, and alkali metal battery production waste recovery system
Mechanical stripping and classification of alkali metal battery waste effectively separate coating material, achieving comparable battery performance and reducing environmental impact.
Patent Information
- Application Number
- PCT/EP2026/064245
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-19
Smart Images

Figure EP2026064245_19112026_PF_FP_ABST
Abstract
Description
[0001] G intreallemctumal pr Lopienrtsy Duesenfeld GmbH Lawyer's file:
[0002] Rothbergstraße 8 6110-0125 PCT-1 38176 Wendeburg
[0003] Germany Date:
[0004] May 15, 2026
[0005] Methods for recycling alkali metal battery production waste and alkali metal battery production waste recovery plant
[0006] The invention relates to a method for recycling alkali metal battery production waste in the form of scrap electrode foil, which (i) comprises a current collector foil and (ii) a coating of the current collector foil, wherein (iii) the coating contains active material and a binder.
[0007] According to a second aspect, the invention relates to an alkali metal battery production waste recovery plant comprising (A) a mixer for mixing and / or dispersing coating material, (B) a coating plant for coating current collector foil with the coating material coming from the mixer, so that electrode foil is formed, and optionally (C) a removal device for removing a part of the electrode foil as reject electrode foil.
[0008] In the manufacture of alkaline metal batteries, a current collector foil is coated with a coating material containing active material and a binder. The binder serves to hold the active material to the current collector foil. If the electrode foil produced in this way does not meet the specified quality, it is not used for the production of alkaline metal batteries but is disposed of as reject electrode foil.
[0009] The coating material is subject to stringent requirements regarding potential impurities. For example, it must generally be ensured that the content of metallic copper and / or aluminum is low.
[0010] It is known to chemically separate the rejected electrode foil from the current collector foil. This removes the aluminum and copper foils, thus preventing contamination with metallic copper and aluminum. The coating material is then treated using wet chemicals, particularly with dilute acid and / or oxidizing agents. This yields salts of the expensive metals involved in the electrochemical reaction, which can then be used to produce new active material.
[0011] When recycling alkaline metal battery production waste, it is desirable that the active material obtained at the end of the process has at least essentially the same properties as the active material produced from raw materials. In other words, it is desirable that alkaline metal batteries manufactured using recycled active material exhibit at least essentially the same properties with regard to cycle life and discharge capacity.
[0012] It is also desirable that the recycling of alkali metal battery production waste has the smallest possible CO2 footprint and / or is as cost-effective as possible.
[0013] From the article by Ahuis et al., "Direct recycling of lithium-ion battery production scrap - Solvent-based recovery and reuse of anode and cathode coating materials," Journal of Power Sources, Vol. 593, February 1, 2024 (2024-02-01), page 233995, XP093327719, Amsterdam, ISSN: 0378-7753, DOI: 10.1016 / j.jpowsour.2023.233995, a process is known in which active material is removed from scrap electrode foil both mechanically and, in comparison, by solvent. A solvent is then added to the active material thus obtained, and the resulting electrode suspension is used for coating electrode foil.
[0014] The article by Rajyaguru et al., "Greening the future: Pioneering lithium battery recycling and beyond in the E-mobility revolution", Vietnam Journal of Chemistry, Vien, Hoboken, USA, Vol. 62, No. 5, May 9, 2024 (2024-05-09), pages 704-716, XP072718255, ISSN: 0866-7144, DOI: 10.1002A / JCH.202300241, provides an overview of existing methods for recycling lithium batteries.
[0015] WO 2025 / 051627 A1 describes the use of a rotary die-cutting machine or a die-cutting press to prevent abrasion of the electrode current collector film during comminution by ensuring uniform cutting conditions. The active material is then removed using a solvent.
[0016] The invention is based on the objective of improving the recycling of alkali metal battery production waste. The invention solves this problem by a method comprising the steps of (a) stripping the rejected electrode foil, in particular by mechanical stripping, to obtain separatable material, (b) classifying the separatable material to obtain a coating material fraction and a foil fragment fraction, and (c) using the coating material fraction to coat current collector foil to obtain electrode foil, wherein preferably (d) the stripping and the classification are carried out such that the coating material fraction particle size distribution F52 corresponds to a primary particle particle size distribution F21.
[0017] According to a second aspect, the invention solves the problem by means of a generic alkali metal battery production waste recovery plant, comprising (D) a stripping plant for the, in particular mechanical and / or dry, stripping of electrode foil to produce separatible material, wherein the stripping plant is arranged in the material flow direction of the electrode foil downstream of the coating plant and optionally a removal device, and (E) a classifying device for classifying the separatible material to produce a coating material fraction and a foil fragment fraction, wherein (F) the classifying device is connected to the mixer for feeding at least parts of the coating material fraction to the mixer, and optionally (G) a production plant for manufacturing the alkali metal batteries from the electrode foil. The electrode foil is the one that comes from the coating plant.The alkali metal battery production waste recovery plant is also an alkali metal battery production plant.
[0018] An advantage of the invention is that a significantly shorter process chain is possible for recycling rejected electrode foil. It has been shown that the foil components can be separated so effectively from the coating material fraction that the coating material fraction contains so few pieces of the current collector foil, in particular so little metallic copper and / or aluminum, that alkaline metal batteries can be manufactured from the coating material of the coating material fraction whose electrical properties are essentially indistinguishable from those of alkaline metal batteries manufactured without recycled coating material. A further advantage is that recycling according to the invention generally produces significantly fewer residual materials than conventional wet-chemical recycling. This reduces the CO2 footprint of recycling rejected electrode foil.
[0019] In this description, the terms recycling and recovery are used synonymously. Both recycling and recovery refer to the process of restoring a material (here: the coating material) that is part of a component considered scrap to a state where it becomes part of that component without the component itself being considered scrap. The decision as to whether an electrode foil is scrap or not is made based on tests that measure at least one measurable parameter and determine whether that parameter falls within a predefined target range. If not, the electrode foil is considered scrap.
[0020] In the production of electrode foil, the current collector foil is typically unwound from a current collector foil coil, coated, and, after optional further processing such as drying, wound onto an electrode foil coil. The electrode foil is then unwound from this coil to manufacture the alkaline metal battery. It is possible, but not necessary, for the rejected electrode foil to be part of a coil. In particular, an entire coil can also be considered a rejected electrode foil.
[0021] A current collector foil is an electrically conductive foil, for example made of aluminum, copper or an alloy of at least one of these metals, which in the alkaline metal battery serves to remove or supply electrons generated during the electrochemical reaction.
[0022] The coating consists of coating material. In addition to the active material and the binder, the coating material may also contain additives, such as carbon black and / or carbon nanotubes.
[0023] The active material is understood to be the material that participates in the electrochemical reaction of the alkali metal battery, by which the alkali metal battery stores electrical energy. An alkali metal battery is understood to be a battery, in particular an accumulator, in which the usable electrical energy is provided by an electrochemical reaction of an alkali metal, in particular lithium or sodium. The alkali metal battery preferably contains (i) a liquid electrolyte containing a conducting salt solvent and dissolved conducting salt, or (ii) a solid electrolyte that is conductive for alkali metal ions. The alkali metal battery can have a liquid electrolyte or a solid electrolyte.
[0024] The term "coating removal" refers specifically to a process in which coating material is removed from the current collector foil to which the coating material is applied. Specifically, coating removal is a mechanical process. It involves acting upon the rejected electrode foil in such a way that the coating detaches from it. In other words, coating removal is the breaking of the bond between the coating and the current collector foil through mechanical action. Specifically, coating removal does not involve the destruction or chemical dissolution of the binder.
[0025] In particular, the stripping process does not involve the destruction of the binder and / or the bond between the coating and the current collector foil by, and especially not exclusively by, thermal action.
[0026] In other words, the stripping process is preferably carried out at least substantially solvent-free. If more than one stripping step is performed, at least one of these stripping steps is carried out at least substantially solvent-free. This means, in particular, that preferably no solvent is used to remove the coating material from the current collector foil. While it is possible that small amounts of solvent are used, these are so small that the absence of solvent results in a reduction of at most 15 percent by weight, and in particular at most 10 percent by weight, of the stripped coating material.
[0027] In particular, stripping includes separating particles bound by the binder. Stripping can be achieved, at least in part, by comminution and / or reduction in size. Comminution involves shifting the particle size distribution towards smaller particles by breaking up the material structure (and not by disassembly). If stripping also involves comminution, the resulting material is simultaneously the comminution material. Preferably, stripping is carried out such that at least 50%, in particular at least 60%, preferably at least 70%, more preferably at least 80%, most preferably at least 90%, and most preferably at least 95% of the coating detaches from the reject electrode foil. The percentages are given as weight percent.
[0028] Definition of a coating removal system: A coating removal system is understood to be, in particular, a device designed to remove coating material, i.e., active material and binder, as well as any additives, from the current conductor foil. For example, a coating removal system may include an impact mill, an impact classifier, a hammer crusher, a hammer mill, and / or an air jet mill. An impact mill is understood to be a device by which the coating is at least partially separated from the current conductor foil by applying an impact load. The term impact rotor mill could also be used instead of impact mill. The impact mill preferably has impact elements made of metal, for example, steel, preferably hardened steel.
[0029] Classification refers to the separation of a dispersed solid mixture into fractions, in particular the formation of at least two fractions based on a classification criterion. The classification criterion could be, for example, particle size, particle density, settling velocity, and / or specific drag. Classification can be performed in one, two, or more steps.
[0030] Classification is preferably carried out dry, i.e., without the addition of a liquid solvent. Powdered material is preferably classified. In particular, pastes, slurries, and / or suspensions are not classified. Classification is preferably performed according to particle size.
[0031] It is advantageous if the classification process involves or includes sieving. The classification criterion for sieving is particle size. Sieving can, for example, be acoustically assisted, and in particular, ultrasonically assisted.
[0032] Alternatively or additionally, classification can include or involve inspection. In inspection, the classification criterion is the weight-specific drag. The fact that the coating material fraction and the film fragment fraction can also be separated by inspection is surprisingly possible in this case because the two fractions to be separated consist of particles whose density differs between the fractions, but which are generally the same within each fraction. It is therefore possible and preferred to classify by inspection, at least predominantly, according to the particle size classification criterion.Although classification is also performed according to the density and shape of the particles during inspection, it has been shown that both the density and shape of the particles within the coating material fraction and the film fragment fraction are sufficiently homogeneous, so that classification by particle size can also be performed to a good approximation by inspection.
[0033] Preferably, the classification is carried out such that, to a good approximation, all particles of the coating material fraction are smaller than the size of the separating particles. This is achieved in particular by including sieving in the classification process.
[0034] The classification criterion is whether a particle has a particle size larger than a predetermined separation particle size. In other words, classification is preferably carried out such that the particle size in the coating material fraction, particularly at least 95% by weight, particularly at least 97.5% by weight, preferably at least 99% by weight, particularly at least 99.9% by weight, is smaller than the separation particle size and / or the particle size in the film fragment fraction, particularly at least 95% by weight, particularly at least 97.5% by weight, is larger than the separation particle size.
[0035] The invention is based, among other things, on the finding that separating based on particle size (measured as equivalent diameter according to ISO 13320: 2020) can separate the coating material from the film fragments so effectively that direct reuse of the coating material—i.e., the active material, the binder, and any additives—is possible, without alkaline metal batteries produced in this way having significantly inferior electrical properties compared to alkaline metal batteries manufactured without recycled material. This is because the stripping process can be carried out in such a way that the diameter of the film fragment components differs significantly from the particle diameter of the coating material.
[0036] The coating material fraction is defined as a fraction in which the amount of foil fragments is reduced by at least a factor of 10 compared to the rejected electrode foil. This means, in particular, that the proportion of current collector foil by weight in the rejected electrode foil is at least 10 times greater than the proportion of current collector foil or its components in the coating material fraction. Preferably, the amount of foil fragments in the coating material fraction is reduced by at least a factor of 20, 30, preferably 50, and most preferably 100 compared to the rejected electrode foil.
[0037] The use of the coating material fraction for coating current collector foil to obtain electrode foil is understood to mean, in particular, that the coating material fraction is not treated with wet chemicals and / or thermally, especially not pyrolytically, before being used again for coating current collector foil. The feature that the coating material fraction is not treated thermally, especially not pyrolytically, means, in particular, that the binder is not substantially (i.e., at least 95% by weight) decomposed, at least also by the action of heat. This specifically prevents the formation of gaseous fluorine compounds, such as hydrogen fluoride, which could damage the coating material. Preferably, the coating material fraction is not heated to a temperature of 80°C or higher.
[0038] Preferably, the coating material fraction is not treated, at least predominantly, preferably to at least 70% by weight, more preferably to at least 80% by weight, and particularly preferably to at least 90% by weight, before being used for coating current collector foil, in such a way as to change the oxidation number of components of the active material, for example the NMC crystals.
[0039] It is possible, but not necessary, for the use of the coating material fraction to take place at the same location as the stripping and / or classification. For example, as provided in a preferred embodiment, the stripping and / or classification can take place at a location at least 1 km, and in particular at least 10 km, away from the location where the coating material fraction is used for coating current collector foil. A stripping plant is understood to be, in particular, a plant that is not only capable of, but is designed to, remove the coating from the reject electrode foil. Preferably, the stripping plant is designed to strip the coating from the reject electrode foil by mechanical action. Preferably, the stripping plant is not designed to thermally act on the reject electrode foil.Although heating of the rejected electrode foil is unavoidable, the coating is not removed by thermal action. The stripping system is or preferably includes an impact mill, an impact classifier, a cutting mill, a classifier mill, a hammer mill, a mill with grinding media, and / or an air jet mill.
[0040] According to one embodiment, the method includes the step of separating a cathode from an anode, yielding two reject electrode foils. A method for manufacturing alkali metal batteries may include the step of joining a cathode to an anode, forming an electrode-separator assembly, for example, a rolled electrode-separator assembly (also known as a Swiss roll or jelly roll). To recover the coating material with high purity, it is advantageous to first procure this electrode assembly, yielding the cathode and anode, and then to recycle the cathode as a reject electrode foil according to the steps of claim 1 and / or to recycle the anode as a reject electrode foil according to the steps of claim 1, separately from the cathode in time and / or space.
[0041] Preferably, the steps mentioned in claim 1 are carried out in the specified order. However, other orders are also possible. For example, stripping and classification can be carried out simultaneously. This is done, for example, using an impact classifier and / or an air jet screen.
[0042] Preferably, the active material contains NMC crystals, i.e., lithium nickel manganese cobalt oxide crystals. NMC crystals are complex to produce; therefore, it is particularly advantageous if they can be recovered during recycling without having to be synthesized anew. Alternatively, the active material contains LiFePCk, NaFePCk, or lithium nickel manganese cobalt oxide (LiNii-x-). y Mn xCoyC), lithium titanium oxide, lithium manganese iron phosphate, graphite, graphite silicon, silicon, nickel cobalt aluminum oxide, Na₂MnFe(CN)e, hard (non-graphitized) carbon, and / or metallic lithium. According to one embodiment, the stripping process includes or is at least partially a comminution. The comminution is preferably a mechanical stress, in particular cutting, shearing, impact, and / or tearing. During comminution, the reject electrode foil is subjected to mechanical stress, causing coating material to detach. In this case, the comminution is preferably carried out with a cutting mill. The cutting mill is an embodiment of a comminution device. Preferably, the comminution is a shearing cut and / or tearing. Shearing is the division of a material by two cutting edges moving past each other, as defined in DIN 8588.
[0043] The term "comminuted processing" refers specifically to a shift in the particle size distribution of the current collector foil towards smaller particles by manipulating the particles, thus increasing their number. A process in which only coating material is removed from the current collector foil without cutting the foil itself is not considered comminution.
[0044] Alternatively or additionally, the rejected electrode foil can be shredded before stripping. Shredding is preferably done by cutting and / or tearing. In other words, shredding is optional, and this shredding can also involve stripping, but it doesn't have to.
[0045] The stripping process is preferably impact crushing. Impact crushing is understood to mean crushing by blunt force. Examples of impact crushing include crushing by impacting the material to be crushed against a solid, stationary object, by impacting the material to be crushed against a moving tool (impact crushing), and / or by causing collisions between particles of the material to be crushed.
[0046] Preferably, impact crushing is a type of impact crushing.
[0047] Preferably, the rejected electrode foil is present in the form of fragments before stripping, with a particle size, in the form of the outer sphere diameter, of no more than 100 mm, and in particular no more than 50 mm. The outer sphere diameter is the diameter of the smallest possible imaginary sphere that completely surrounds the particle. This can be achieved by comminution. Preferably, the rejected electrode foil is present in the form of fragments before stripping, with a particle size, in the form of the sieve size, of no more than 100 mm, and in particular no more than 50 mm.
[0048] If the process includes comminution of the rejected electrode foil, it is advantageous for the process to include a classification step after comminution and before stripping. Preferably, the classification is performed such that the particle size of the material to be separated, in the form of the outer sphere diameter, is at most 100 mm, and in particular at most 50 mm.
[0049] If the process includes comminution of the rejected electrode foil, it is advantageous for the process to include the classification step after comminution and before stripping. Preferably, classification is performed such that the particle size of the material to be separated, measured as a sieve size, is at most 100 mm, and in particular at most 50 mm. According to a preferred embodiment, the comminution is carried out such that at most 5% by weight of the comminution material has a fragment size, measured as a sieve size, of more than 100 mm, and in particular more than 50 mm, and / or has a maximum fragment size, measured as a spherical diameter, of at most 100 mm, and in particular at most 50 mm.
[0050] According to a preferred embodiment, the comminution is carried out such that at most 40% by weight, in particular at most 30% by weight, in particular at most 20% by weight, in particular at most 15% by weight of the comminution material has a fragment size, measured as sieve size, of less than 50 pm, in particular less than 100 pm.
[0051] Alternatively or additionally, the coating removal is preferably carried out in a coating removal plant by mechanical action on the comminution material. Alternatively or additionally, the material to be separated is dry during classification, whereby classification is in particular dry sieving. If the process has two or more coating removal steps, at least one of these restrictions applies to at least one coating removal step, and in particular to all coating removal steps.
[0052] Preferably, the stripping and / or comminution process does not substantially involve the use of a solvent or a binder of the active material. Alternatively or additionally, the stripping and / or comminution process does not involve thermal decomposition of the binder. Alternatively or additionally, the stripping and / or comminution process does not involve cryogenic treatment. This is understood to mean, in particular, that the rejected electrode foil is cooled to a maximum of -10°C. Typically, the rejected electrode foil is not cooled. Alternatively or additionally, the stripping and / or comminution process does not substantially involve the addition of water or an aqueous liquid. If the process has two or more stripping steps, at least one of these restrictions applies to at least one stripping step, and in particular to all stripping steps.
[0053] The coating material fraction has a coating material fraction particle size distribution that plots the volume of particles below an equivalent diameter over the equivalent diameter.
[0054] In other words, the equivalent diameter determined by a laser diffraction method according to ISO 13320:2020 is plotted on the x-axis of the coating material fraction particle size distribution. The y-axis represents the volume fraction, normalized to 1, of particles whose equivalent diameter is equal to or less than this equivalent diameter. The equivalent diameter is measured in a suspension where the liquid used is not a solvent for the binder and / or any of the additives.
[0055] According to one embodiment, the stripping and / or classification is carried out such that the coating material fraction particle size distribution corresponds to a primary particle particle size distribution. This means, in particular, that the medians of the two particle size distributions (xso value) differ from each other by no more than 100%, in particular no more than 50%, and in particular no more than 35%. The deviation is calculated by dividing the larger median value by the smaller value.
[0056] The primary particle size distribution is the particle size distribution of the particles in the active material of the coating. If the coating material fraction particle size distribution corresponds at least substantially to the primary particle size distribution, it can be achieved that an alkaline metal battery manufactured using recycled coating material does not differ significantly in its storage capacity and / or discharge capability from alkaline metal batteries manufactured without recycled coating material.
[0057] The particle size distribution, for example the primary particle-particle size distribution, is measured, for example, by laser diffraction according to ISO 13320, for example using the HELOS / KR device from Sympatec GmbH Clausthal-Zellerfeld.
[0058] Alternatively or additionally, the stripping and / or classification is carried out such that the median of the coating material particle size distribution is at most 50 pm, in particular at most 30 pm, preferably at most 25 pm, in particular at most 10 pm.
[0059] According to a preferred embodiment, the method comprises the steps (a) stripping the rejected electrode foil, such that
[0060] a first coating material detachment fraction of coating material is removed from the electrode foil,
[0061] a first coating material residue proportion of coating material remains on the electrode foil and
[0062] The first intermediate sorting material is created,
[0063] (b) Classifying the first intermediate separation material according to particle size, so that a first coating material fraction and
[0064] a residual faction will be preserved,
[0065] (c) Delamination of the residual fraction, so that
[0066] a second coating material removal fraction of coating material is removed from the electrode foil,
[0067] a second coating material residue remains on the electrode foil and
[0068] A second intermediate sorting material is created,
[0069] (d) Classifying the second intermediate separation material according to particle size, so that a second coating material fraction and
[0070] a second residual fraction, particularly in the form of the foil fragment fraction, is obtained, and
[0071] (e) Using the first coating material fraction to coat current collector foil, so that electrode foil is obtained. The first coating material removal fraction is preferably at least 5% by weight, in particular at least 10% by weight, in particular at least 15% by weight, in particular at least 20% by weight, in particular at least 25% by weight, in particular at least 30% by weight.
[0072] The second coating material detachment fraction is preferably at least 5% by weight, in particular at least 10% by weight, in particular at least 15% by weight, in particular at least 20% by weight, in particular at least 25% by weight, in particular at least 30% by weight.
[0073] An advantage of this approach is that the first stripping and the first classification – as provided for in a preferred embodiment – can be carried out such that the first intermediate separation material contains a lower percentage (by weight) of particles from the current collector film than the second intermediate separation material. The first stripping and the first classification can then – as provided for in a preferred embodiment – be carried out such that the first intermediate separation material falls below a predetermined contamination threshold concentration.The impurity threshold concentration is preferably chosen such that alkaline batteries manufactured using coated current collector foil, the coating of which was produced using first intermediate separating material, do not differ significantly in their properties from alkaline batteries manufactured without the use of recycled coating material.
[0074] The characteristic that the batteries are essentially identical means in particular that the capacities differ by no more than 10%, and in particular no more than 5%, after 300 charging and discharging cycles from 100% to 0% within 1 hour.
[0075] In a subsequent, particularly a second, stripping and classification process, intermediate material can be obtained whose impurities exceed the impurity threshold concentration. While this intermediate material cannot be used directly for battery production, it can be further processed, for example, using wet chemical methods. It is also possible for the second coating material fraction to be used for coating current collector foil, thus obtaining electrode foil.
[0076] Preliminary tests determine how the material must be stripped and classified so that the first intermediate separation product falls below the specified contamination threshold concentration.
[0077] It is possible, but not necessary, for the initial stripping and initial classification to be carried out simultaneously and / or in the same machine. It is generally advantageous for the initial stripping to take place before the initial classification.
[0078] It is possible, but not necessary, for the second stripping and the second classifying to be performed simultaneously and / or in the same machine. It is generally advantageous for the second stripping to occur before the second classifying. If the first stripping and the first classifying are performed simultaneously, the second stripping follows the first classifying and does not occur concurrently with it.
[0079] Preferably, the method includes the step of bunkering the first intermediate segregated material and / or - if present - the second intermediate segregated material and / or - if present - the third or further intermediate segregated material.
[0080] Preferably, the process comprises the step of storing the first coating material fraction and / or - if available - the second coating material fraction and / or - if available - the third or further coating material fraction.
[0081] Preferably, the process includes the step of storing the first residual fraction and / or - if present - the second residual fraction and / or - if present - the third or further residual fraction.
[0082] Preferably, at least two different stripping steps are carried out in the same stripping plant. For example, the first stripping and the second stripping are carried out in the same stripping plant. If there are more than three or more stripping steps, preferably at least two stripping steps are carried out in the same stripping plant.
[0083] For example, the first stripping and classification processes are carried out first, and the resulting coating material fraction and the residual fraction are stored separately. Then, the first coating material fraction from the same stripping unit is stripped a second time. It is possible, but not necessary, for the second stripping step to be performed with a higher stripping intensity than the first.
[0084] Preferably the procedure comprises the following steps:
[0085] (a) Shredding, in particular shearing, of the rejected electrode foil to produce first intermediate material, the shredding also being a stripping process,
[0086] (b) Classifying the first intermediate fraction according to particle size, so that the first coating material fraction and the residual fraction are obtained, and (c) second stripping of the residual fraction by impact crushing, so that a second intermediate fraction is produced,
[0087] (d) second classification of the second intermediate separation material according to particle size, so that the second coating material fraction and the residual fraction are obtained, and
[0088] optionally (e) repeating steps (c) and (d) at least once and preferably (f) carrying out all stripping and classifying such that at least the first coating material fraction particle size distribution corresponds to a primary particle particle size distribution.
[0089] According to a preferred embodiment, the stripping and classification steps are carried out at least twice, in particular at least three times, and in particular at least four times. Preferably, the stripping is carried out at least once by impact crushing and / or at least once by shearing.
[0090] In this way, coating material fractions with varying levels of impurities can be specifically generated, while simultaneously achieving a high degree of coating removal. Preferably, at least one coating material fraction is not used for coating current collector foil. In particular, at least one coating removal step, especially the last one, is carried out in such a way that the impurity threshold concentration is exceeded.
[0091] According to one embodiment, the stripping and classification steps are carried out in such a way that
[0092] (a) at least one, in particular the first, coating material fraction has a foil material content, in particular of aluminium and / or copper, which is less than a specified impurity threshold concentration and / or
[0093] (b) at least one coating material fraction has a film material content above the impurity threshold concentration and / or
[0094] (c) at least one coating material fraction, the foil material content of which is less than the specified impurity threshold concentration, is used for coating current collector foil and / or
[0095] (d) the at least one coating material fraction, the foil material content of which is not less than the specified impurity threshold concentration, is not used for coating current collector foil. According to one embodiment, the stripping intensity for at least one stripping step is greater than in at least one preceding stripping step.
[0096] The term "delamination intensity" refers to a parameter where a higher delamination intensity results in more delamination and a higher foil material content, particularly of aluminum and / or copper. Delamination intensity specifically relates to mechanical delamination.
[0097] The stripping intensity, for example, is a measure of the (average) impulse applied to the material during stripping.
[0098] Because the stripping intensity is lower in an early stripping step than in a later one, a coating material fraction with small impurities containing foil material is obtained. Such material is particularly valuable for direct reuse in the manufacture of alkaline metal batteries. A coating material fraction with more impurities, while unsuitable for direct recycling to produce coating material, is generally more useful than fragments of coated current collector foils.
[0099] The stripping intensity depends on the method used for stripping. For example, if an impact mill is used for stripping, the stripping intensity can be determined by factors such as the rotor speed, the mesh size of a bottom screen, or a value calculated from the rotor speed, mesh size, and possibly other parameters.
[0100] According to one embodiment, the method comprises the steps (a) stripping the rejected electrode foil with a first stripping intensity, (b) separating coating material and / or a coating material fraction, in particular during or after stripping, in particular by classifying, for example according to particle size, and (c) subsequently stripping the rejected electrode foil with a second, greater stripping intensity.
[0101] Separation during stripping is achieved, for example, by extracting air from the stripping system and separating, in particular filtering, particles from this air.
[0102] According to one embodiment, the method comprises the steps
[0103] (a) Stripping the rejected electrode foil by mechanical action, in particular such that (i) a first coating material detachment fraction of coating material is removed from the electrode foil and / or in particular (ii) a first coating material retention fraction of coating material remains on the electrode foil and (iii) first intermediate separation material is created, and
[0104] (b) Classifying the first intermediate material according to particle size, such that (i) a first coating material fraction and (ii) a residual fraction are obtained, wherein (iii) the film material content of the first coating material fraction is less than a predetermined impurity threshold concentration, (c) optionally repeating the stripping and classification at least once to obtain a residual fraction,
[0105] (d) Stripping the residual fraction using a binder solvent, such that (i) a second coating material removal fraction of coating material is removed from the electrode foil, (ii) a second coating material retention fraction of coating material remains on the electrode foil, and (iii) a second intermediate separation fraction is produced.
[0106] (e) Separation of the second coating material fraction from the intermediate separation material and
[0107] (f) Using the first coating material fraction and / or the second coating material fraction to coat current collector foil, so that electrode foil is obtained. Alternatively, only the first coating material fraction may be used to coat current collector foil, but not the second coating material fraction.
[0108] Mechanical stripping is generally less complex, so it is advantageous to first remove the coating material mechanically, particularly until further mechanical stripping would exceed the specified contamination threshold concentration. Subsequently, stripping is carried out using a binder solvent. This stripping process is more complex, but usually allows the recovery of coating material that also remains below the contamination threshold concentration. This increases the recycling rate for direct recycling.
[0109] The binder solvent is preferably water, acetone, γ-butyrolactone (GBL), diethyl carbonate (DEC), dimethylacetamide (DMA), N,N-dime-ethylformamide (DMF), dimethyl sulfoxide (DMSO), 3-heptanone, 3-hexanone, methyl ethyl ketone (MEK), methyl octanoate, N-methyl-2-pyrrolidone, supercritical carbon dioxide, or a mixture of two, three, four, or more of the aforementioned chemical compounds.
[0110] According to a preferred embodiment, the delamination intensities differ at at least two time points, in particular in the average over 10 seconds, by at least 50%, and in particular by at least 100%.
[0111] Alternatively or additionally, the film material contents of at least two coating material fractions differ by at least 50%, in particular at least 100%, preferably at least 150%, especially at least 100%, and most preferably at least 150%. For the calculation, the larger film material content is divided by the smaller film material content.
[0112] Preferably, the classification is carried out such that at most 0.1 wt. percent, in particular at most 0.01 wt. percent, of the coating material fraction particles are larger than a separating particle size xsepar, wherein the separating particle size is at most five times an active material particle size XAM in the form of the xgo particle size of the active material. The xgo particle size is that size determined by laser diffraction according to ISO 13320:2020 for which 90 volume percent of all particles have at most this size.
[0113] Preferably, the classification process comprises sieve classification, wherein the mesh size is at most 100 pm, in particular at most 80 pm, and in particular at most 65 pm. An advantage of sieve classification is that it largely prevents particles larger than the mesh size from passing through the sieve.
[0114] It is possible, but not necessary, for the classification process to include further classification steps besides sieve classification, such as screening.
[0115] According to one embodiment, the method comprises magnetic deposition after stripping and before using the coating material fraction to coat current collector foil. Magnetic deposition is used, for example, to remove magnetic debris generated during stripping.
[0116] According to one embodiment, the classification is carried out such that the metallic aluminum content in the coating material fraction is at most 1% by weight, preferably at most 0.5% by weight, and particularly preferably at most 0.25% by weight. It has been found that a low aluminum content improves the electrical properties of an alkaline metal battery manufactured using recycled coating material.
[0117] According to one embodiment, the classification is carried out such that the copper content of metallic copper in the coating material fraction is at most 1 percent by weight, and in particular at most 0.5 percent by weight. It has been found that a low copper content improves the electrical properties of an alkali metal battery manufactured using recycled coating material.
[0118] According to one embodiment, the classification is carried out such that the iron content (metallic or bound) in the coating material fraction is at most 0.1 percent by weight, and in particular at most 0.05 percent by weight. It has been found that a low iron content improves the electrical properties of an alkaline metal battery manufactured using recycled coating material. This is especially true when the active material does not contain an iron compound, such as lithium iron phosphate.
[0119] According to one embodiment, the classification is carried out such that the chromium content (metallic or bound) in the coating material fraction is at most 0.1 percent by weight, and in particular at most 0.05 percent by weight. It has been found that a low chromium content improves the electrical properties of an alkaline metal battery manufactured using recycled coating material. Chromium is a common alloying element in steels and can be present in the abrasion generated during stripping.
[0120] If the iron and / or chromium content is too high, the coating removal process is carried out with lower stress intensity. For example, the rotational speed of an impact mill is reduced.
[0121] According to one embodiment, the classification is carried out such that two or more coating material sub-fractions are obtained, wherein at least one of the coating material sub-fractions has the aluminum, copper, and / or iron content specified above. The at least one other coating material sub-fraction may have a higher aluminum, copper, and / or iron content.
[0122] For example, the at least two coating material sub-fractions are produced by sieving with sieves of different screen cuts. Alternatively or additionally, the classification can also include a screening step in which the coating material sub-fractions are produced from the coating material fraction. According to one embodiment, the process includes the step of drying the rejected electrode foil before stripping. If the process includes comminution, drying preferably also takes place before comminution. The drying is preferably carried out such that the solvent content is at most 20% by weight, in particular at most 5% by weight, and most preferably at most 1% by weight, in each case measured at 105°C according to DIN EN 14346.
[0123] According to one embodiment, the comminution, stripping, and / or classification are carried out under an inert gas atmosphere. This largely prevents degradation of the active material. Alternatively or additionally, the comminution takes place in an atmosphere with a relative humidity of at most 5%, preferably at most 1%, and particularly at most 0.5%, based on 20°C. This is referred to as dry room conditions.
[0124] It is advantageous if the stripping, classification, and / or, if applicable, comminution take place in an atmosphere containing no more than 0.1% water by weight. Water can impair the properties of the active material.
[0125] Preferably, the rejected electrode foil and / or the coating material, after stripping, particularly after any comminution, has at least substantially no contact with hydrogen fluoride. The same preferably applies to the at least one intermediate separation material and the at least one coating material fraction. This means, in particular, that at most 0.1 percent by weight, and especially at most 0.01 percent by weight, of the coating material reacts with hydrogen fluoride. Hydrogen fluoride can be formed when binders decompose due to temperature.
[0126] Alternatively or additionally, the coating material, after stripping, in particular after any crushing, has at least substantially no contact with air whose relative humidity is so low that the air at 20°C has a relative humidity of at most 5%, preferably at most 1%, in particular at most 0.5%, most preferably at most 0.01%.
[0127] Preferably, a portion of the film fragment fraction is recycled for re-delamination, particularly to the delamination unit. Delamination, especially by impact crushing, is a stochastic process in which not all particles are subjected to the same mechanical action. Particles that have not been sufficiently delaminated are larger and / or heavier than particles that have been sufficiently delaminated. Preferably, therefore, the portion of the film fragment fraction whose particle size (measured as mesh size (sieve size) or as aerodynamic diameter) is larger than a predetermined return separation particle size is fed back into the system. The return separation particle size is at least the separation particle size, for example, at least 100 pm.
[0128] Preferably, the method comprises the steps (a) coating current collector foil with coating material to form electrode foil, (b) removing a portion of the electrode foil as reject electrode foil, (c) subsequently carrying out steps (a) to (c), in particular also feature (d), of claim 1, and then manufacturing the alkali metal batteries using the coating material fraction. In this embodiment, the method is also a method for manufacturing alkali metal batteries.
[0129] An advantage of this process is that it produces less waste. It has been shown that, at least up to a recycled coating material content of 26 percent by weight, the electrical properties of the alkali metal battery are approximately indistinguishable from those of alkali metal batteries manufactured without recycled coating material.
[0130] Removing defective electrode foil can, for example, involve cutting out portions of the electrode foil. Preferably, the method includes the step of detecting, particularly with spatial resolution, at least one quality parameter of the electrode foil and removing areas of the electrode foil where the quality parameter lies outside a predetermined target range. The quality parameter can be, for example, a layer thickness, the basis weight, the specific electrical resistance, or the presence of defects such as cracks or waves.
[0131] Preferably, the method comprises the step, particularly prior to step (a) of coating the current collector foil, of mixing active material, binder, and optionally binder solvent. In this way, a pasty material can be obtained with which the current collector foil is coated. Preferably, the method comprises the following step: after coating and prior to removing the portion of the electrode foil, drying, calendering, and / or cutting and / or finishing the electrode foil.
[0132] Preferably, the process comprises mixing the coating material fraction with primary coating material to obtain the coating material with which the current collector foil is coated. Primary coating material is understood to be material synthesized from raw material. In other words, the primary coating material does not contain any material recycled within the described process.
[0133] The recycled content of the coating material, i.e., of the material that has undergone the steps according to claim 1, is preferably at least 1 percent by weight, more particularly at least 5 percent by weight, and more particularly at least 15 percent by weight. It has been shown that an alkaline metal battery with a recycled content of 26 percent by weight has essentially the same properties with regard to service life and storage capacity as an alkaline metal battery manufactured without recycled coating material.
[0134] The coating material used to manufacture alkaline metal batteries, which contains recycled coating material, has a coating material binder content. The coating material fraction immediately after separation from the film fragment fraction also contains recycled binder. With ideal stripping and classification, the recycled binder content is equal to the coating material binder content.
[0135] Preferably, the classification is carried out such that the recycled binder content is at least half, in particular at least two-thirds, preferably at least three-quarters, in particular at least 80%, and most preferably at least 85%, and in particular at least 90%, of the coating material binder content. Alternatively or additionally, the recycled binder content is preferably at most twice, in particular at most 1.25 times, in particular at most 1.15 times, and more preferably at most 1.1 times, of the coating material binder content. In other words, the binder content is essentially unchanged after stripping and classifying the separated material. It is particularly advantageous if the recycled binder content corresponds at least substantially to the binder content in the primary coating material.This means that both binder parts should be as similar as possible, whereby deviations of, for example, a maximum of 15%, in particular a maximum of 10%, preferably a maximum of 5% are tolerable.
[0136] In particular, the process does not include the substantial removal of binder from the coating material fraction. This is specifically understood to mean that no more than 15% by weight, in particular no more than 10% by weight, and in particular no more than 5% by weight, of the binder is removed from the coating material fraction before it is used to coat current collector foil. In particular, the process does not include the washing out of the binder and / or the binder with a solvent and / or the thermal decomposition of the binder and / or the binder.
[0137] The coating process for manufacturing alkali metal batteries is preferably carried out such that the coating thickness d27 of the electrode coating is at least 1.5 times, preferably twice, more preferably at least three times, more preferably at least four times, and particularly preferably at least five times, the size of the separating particles. The coating thickness d27 is the thickness of the coating after the current collector foil has been coated with the coating, particularly after calendering and optionally after drying the coating. Alternatively or additionally, the coating contains particles larger than the coating thickness, preferably less than 10⁻⁵. 4 Weight percent, preferably less than 10% 5 Percent by weight. Particles that are too large can puncture the current collector foil and / or the separator, which can lead to battery failure.
[0138] The alkali metal battery production waste recovery plant can also be called an alkali metal battery production plant. The alkali metal battery production plant can also include a coating unit for applying the coating material to the electrode foil. According to one embodiment, this alkali metal battery production plant has a dryer for drying the coated electrode foil and / or a calender for calendering the electrode foil to achieve a specific coating thickness. The alkali metal battery production plant can also include a cutter designed to cut the calendered electrode foil to a predetermined size. The cut electrode foils for the cathode and anode are then combined with a separator to form an electrode-separator assembly. This assembly is then packaged in a housing or casing and filled with electrolyte to create the alkali metal battery.The advantage of such an alkali metal production plant is that it produces less waste. This generally leads to more cost-effective and / or efficient production.
[0139] Preferably, the alkali metal battery production waste recovery plant has a primary coating material container connected to the mixer for feeding primary coating material and containing primary coating material. The primary coating material has a primary particle particle size distribution. Preferably, the classifying device is designed for classification such that the coating material fraction has a coating material fraction particle size distribution that corresponds to the primary particle particle size distribution.
[0140] Preferably, the alkali metal battery production device includes a comminution device for comminuting the rejected electrode foil to obtain comminution material. The comminution device is preferably connected to the stripping unit, preferably by means of a dust-tight conduit.
[0141] The comminution device is preferably arranged downstream of the coating unit – and optionally the removal unit – in the material flow direction of the rejected electrode foil. The comminution device in the material flow direction of the comminution material is preferably arranged upstream of the stripping unit. The comminution device is particularly designed for cutting or friction comminution. The comminution device preferably has a second stripping unit for stripping using a solvent. In the second stripping unit, coating material is removed from the current collector foil by at least partially dissolving or partially dissolving the binder using the solvent.
[0142] According to one embodiment, the alkali metal battery production waste recovery plant comprises at least one bunker for storing the first intermediate sorting material and / or – if present – the second intermediate sorting material and / or – if present – the third or further intermediate sorting material. The bunker is preferably connected to the stripping plant and / or the classifying device by means of a pipeline, preferably dust-tight, such that material produced by the stripping plant or classifying device can be stored in the bunker and / or the material can be fed to the stripping plant or classifying device.
[0143] According to a preferred embodiment, the alkali metal battery production waste recovery plant has a contaminant measuring device 65 for automatically, and in particular continuously, determining whether the film material content cs of the coating material fraction 52.i is below the contaminant threshold concentration C24. The contaminant measuring device 65 is preferably an X-ray fluorescence or LIBS (laser-induced plasma spectroscopy) device.
[0144] The invention will now be explained in more detail with reference to the accompanying drawings. These drawings show
[0145] Figure 1 shows a flowchart of a process and an alkali metal battery production waste recycling plant according to the invention.
[0146] Figure 2 shows a schematic view of an alkali metal battery production waste recovery plant or alkali metal battery production plant according to the invention for carrying out a process according to the invention.
[0147] Figure 3a shows an idealized coating material fraction particle size distribution of a coating material fraction from a method according to the invention.
[0148] Figure 3b shows the specific discharge capacity of each alkaline metal battery made exclusively from primary material and with 26% recycled coating material.
[0149] Figure 3c shows the specific discharge capacity (at 0.1C) during repeated charging and discharging at 1C, and Figure 4 shows a schematic of an alkali metal battery production waste recycling plant according to a further embodiment of the invention for carrying out a method according to the invention.
[0150] Figure 1 shows an alkali metal battery production waste recovery plant 10, which is referred to below simply as the recovery plant, but can also be called an alkali metal battery production plant. The recovery plant 10 has a mixer 12 for mixing and / or dispersing coating material 14, which contains active material 16, binder 18, and optionally additives 20. The active material 16, the binder 18, and optionally the additives 20 are primary coating materials 21, which consist of primary particles. A primary coating material 21 is understood to be a material that has not yet undergone a recycling process as defined in the procedure described here and was synthesized from raw materials. The active material 16, the binder 18, and optionally the additives 20 are contained in a coating material container 23, which has partial coating containers 21.1, 21.2, and 21.3.
[0151] The recovery unit 10 also includes a coating unit 22 for coating current collector foil 24 with the coating material 14 coming from the mixer 12, so that electrode foil 26 with a coating 27 is produced, as shown schematically in the partial diagram. The coating 27 has a coating thickness d2 of, for example, d27 = 0.2 mm.
[0152] The recovery unit 10 can include a dryer 28 for drying the coated electrode foil 26. Alternatively, the recovery unit 10 can also include a calender 30 for calendering the, optionally dried, electrode foil 26, so that the coating 27 has a coating thickness d27.
[0153] The recovery unit 10 can also include a cutter 32 designed to cut the calendered electrode foil 26 to a predetermined size. The cut electrode foil 26 is then combined with cut electrode foil from the other electrode and the separator to form an electrode-separator assembly. An optional cell manufacturer 34 then packages this assembly into a housing or casing and fills it with electrolyte 36 to produce the alkali metal battery 38. Areas of the electrode foil 26 that do not meet a predetermined specification are removed by a removal unit 39 as reject electrode foil 40 and can be fed into an optional comminution device 42 to obtain comminution material 43. The comminution device 42 is, for example, a cutting and comminution device. The comminution material 43 has a particle size (sieve size) of preferably no more than 100 mm, and in particular no more than 50 mm.For example, the comminution device 42 has a bottom screen that ensures that only comminution material with the specified particle size leaves the comminution device 42. The rejected electrode foil 40 is fed to a stripping unit 44, for example, an impact mill. In the stripping unit 44, the coating 27 is at least partially separated from the current collector foil, resulting in the separated material 46.
[0154] The removal device 39 includes, for example, a separating device by which the rejected electrode foil 40 is separated from the electrode foil 26. If an entire web of electrode foil 26 is considered reject, the removal device is the device that conveys the web, for example in the form of a coil, to the stripping unit 44. The removal device 39 can also include measuring devices by which it is determined whether an area of the electrode foil is classified as reject electrode foil or meets predefined quality criteria.
[0155] The impact mill contains, for example, rotating impact elements that apply an impact load to the material being crushed, thus separating the coating 27 from the fragmented current collector foil 24.
[0156] Optionally, a dryer 45 can be arranged upstream of the stripping unit 44 in the material flow direction M. The dryer 45 can also be arranged upstream of any shredding device 42 that may be present in the material flow direction M.
[0157] The material 46 enters a classifying device 48, which separates it into a film fragment fraction 50 and a coating material fraction 52. It is possible that at least one further fraction is formed, but this is not necessary. The classifying device 48 is preferably a screen classifier or comprises a screen classifier. A screen classifier has at least one screen with exactly one mesh size. The mesh size is the clear distance between the openings of the screen, also called the screen cut. The screen cut corresponds to the separation particle size xsepar. The classifying device 48 classifies the material 46 into two fractions. The fraction with particles smaller than the separation particle size xsepar is the coating material fraction 52. The fraction with particles of at least the separation particle size xsepar is the film fragment fraction 50.
[0158] Alternatively or additionally, the classifying device 48 includes a classifier. To ensure that the particles in the fraction with the smaller particle sizes are always smaller than the separation particle size x_separ, it is advantageous, but not necessary, to arrange a screen classifier downstream of the classifier in the material flow direction, the screen opening of which corresponds at most to the separation particle size.
[0159] Immediately after separation from the film fragment fraction 50, the coating material fraction 52 has a recycled binder content B52 of, for example, 3% by weight. The primary coating material 21 has a primary binder content B21 of, for example, 4% by weight. The coating material fraction used for coating, which contains the primary coating material 21 and the coating material fraction 52, also has a coating material binder content B14 of 4% by weight. To compensate for the lower binder content in the coating material fraction 52, additional binder is added. If the recycled binder content is greater than the coating material binder content B14, additional active material and, if necessary, additives are added.
[0160] The classifying device 48 is connected to the mixer 12 for feeding at least parts of the coating material fraction 52 to the mixer 12.
[0161] The mixer 12, the coating unit 22, optionally the dryer 28, the calender 30 and the cutter 32 are part of a production line 56 of the alkali metal battery production plant 54. The optional crushing device 42, the stripping unit 44 and the classifying device 48 are part of a recovery line 58 of the alkali metal battery production plant 10.
[0162] Figure 2 shows a flow diagram of an alkali metal battery production waste recovery plant 10 for carrying out a process according to the invention. A first, optional step S1 of comminution is carried out in the comminution device 42. The stripping step S1 takes place in the stripping unit 44. The classifying step S2 takes place in the classifying device 48, and the coating material fraction 52 is fed to the mixer 12 in step S3, where it is mixed with primary coating material 21. The primary coating material 21 is synthesized from raw materials and has not yet undergone a recycling process within the meaning of this invention.
[0163] According to an optional step S2.1, a portion of the film fragment fraction is recycled to the stripping unit 44. For example, the film fragment fraction 50 is classified, in particular sieved and / or screened, and the particles above a critical particle size Xcrit are recycled. The particle size Xcrit is, for example, greater than or equal to the separation particle size xtrenn.
[0164] It is possible that the comminution device 42 and / or the stripping unit 44 and / or the classifying device 48 is connected to an inert gas source 62. This allows the comminution, stripping and / or classifying to take place under inert gas 64, which reduces or even prevents undesirable chemical reactions of the coating material.
[0165] According to one variant, the comminution process in step SO is carried out in the comminution device 42 in such a way that it also involves stripping. The comminution can, for example, be a shearing process. This yields the first intermediate material 46.1, which is fed to the classifying device 48, so that the film fragment fraction 50 and the coating material fraction 52 are obtained.
[0166] According to a further variant of a method according to the invention, the separating material 46 is fed to the classifying device 48 either as first intermediate separating material 46.1 from the stripping unit 44 or as first intermediate separating material 46.1 from the comminution device 42, resulting in a first coating material fraction 52.1 and a first residual fraction 50.1. The residual fraction 50.1 is wholly or completely returned to the stripping unit 44 or fed to another stripping unit.
[0167] In the first stripping step, the rejected electrode foil 40 or the comminution material 43 is stripped with a first stripping intensity h, for example, with a first stripping and / or a first rotational frequency of a rotor of the stripping unit 44. The remaining fraction 50.1 is stripped with a second stripping intensity h, which can be equal to or greater than the first stripping intensity I1. While it is also possible for I2 to be less than I1, this often leads to poorer results.
[0168] The return of the resulting residual fraction 50.i (i = 1, 2, ...) can occur once, twice, three times, or more. If the residual fraction 50.i is returned, a second intermediate separation material (46.2) is produced during the second separation.
[0169] The alkali metal battery production waste recovery plant 10 optionally has at least one bunker 70.j (j = 1, 2, ...)), which is connected to the classifying device 48 or, if applicable, the stripping plant 44. The at least one bunker 70.i serves to receive one of the film fragment fractions 50.i or the separated material 46 or intermediate separated material 46.i.
[0170] For example, the first fraction of foil fragments, 50.1, coming from the classifying device 48, is stored in bunker 70.1. After the rejected electrode foil 40 has been processed, the first fraction of foil fragments, 50.1, is transferred from bunker 70.1 to the stripping unit 44, stripped a second time, and then classified in the classifying device 48, resulting in the second fraction of foil fragments, 50.2. This is stored in bunker 70.2 so that it can be stripped a third time.
[0171] The resulting coating material fraction 52.i is examined using an optional impurity measuring device 65 to determine whether the film material content cs is below the impurity threshold concentration C24. If so, the coating material fraction 50.i is fed to the mixer 12.
[0172] It is possible that the second stripping is carried out with the same device as the first stripping.
[0173] For all the variants mentioned, it is possible to determine the foil material content C24 of the current collector foil 24 before feeding the coating material fraction 50 to the mixer 12. If the foil material content C24 is above a predetermined impurity threshold concentration cs, the coating material fraction 50 is not fed to the mixer 12 and is therefore not used directly for the production of coating material. Instead, this coating material fraction 50 is fed, for example, to a wet-chemical recycling plant 63. The foil material content, in particular of aluminum and / or copper, is determined, for example, by wet chemical analysis.
[0174] Figure 3a shows an idealized coating material fraction particle size distribution F52 of coating material fraction 52. The coating material fraction particle size distribution F52 plots the volume of particles of coating material fraction 52 below an equivalent diameter x on the y-axis and above the equivalent diameter x on the x-axis. The coating material fraction particle size distribution F52 depends on the duration of the stripping process and the intensity of the mechanical action. Generally, the longer the stripping process and the greater the mechanical action, the smaller the particles become. The coating material fraction particle size distribution Fs2 is determined by laser diffraction according to ISO 13320:2020.
[0175] The median is the equivalence diameter xso for which particles with at most this equivalence diameter make up 50 percent of all particles by volume.
[0176] The primary coating material 21 has a primary particle particle size distribution F21, which is shown in an exemplary and idealized form in Figure 3. It can be seen that the two medians of the particle size distributions F52 and F52 differ only slightly from each other, so that they correspond.
[0177] Figure 3b shows the specific discharge capacity in milliampere-hours per gram of active material of an alkali metal battery consisting exclusively of primary material (square symbols) and containing 26% by weight of coating material recycled using the inventive method (round symbols). First, both types of alkali metal batteries were charged with a current one-tenth the current required to fully charge them in one hour (0.1 C / h, often denoted as 0.1C). They were then fully discharged with this current (0.1 C), and the discharge capacity of the alkali metal battery was determined. It can be seen that the two types of alkali metal batteries do not differ within the margin of error. The charge capacity is the electrical charge that the alkali metal battery can store (between the discharge cut-off voltage and the charge cut-off voltage).Figure 3c shows the specific discharge capacity after repeated charging and discharging at 0.1C. It can be seen that the specific discharge capacity of the alkaline metal battery with 26% recycled coating material by weight hardly differs within the margin of error.
[0178] Figure 4 shows a schematic diagram of an alkali metal battery production waste recycling plant 10 according to a further embodiment of the invention for carrying out a method according to the invention. In this variant, a coating material fraction 52.i, whose film material content C24 is above a second threshold concentration C2, is fed to a second stripping plant 44.2, in which the coating material fraction 52.i is mixed with a solvent 66. For example, the second stripping plant 44.2 has a device for introducing mechanical energy, such as a stirrer or an ultrasonic source. Furthermore, the stripping plant 44.2 has a separator for separating the dissolved binder from the active material, for example, a filter. The stripping plant 44.2 can also optionally include a dryer 68.The second threshold concentration C2 is chosen, for example, such that further mechanical stripping in the stripping plant 44 would lead to an exceedance of the impurity threshold concentration cs.
[0179] Figure 4 shows that the alkali metal battery production waste recovery plant may include an optional additional stripping unit 44.3 and / or an additional classifying device 48.i. In general, the alkali metal battery production waste recovery plant may include two or more stripping units 44.i and / or two or more classifying devices 48.i. The number of stripping units may differ from the number of classifying devices.
[0180] It is possible to use the contamination measuring device 65 to determine, based on the film material content C24, whether the film fragment fraction 50, 50.i is fed to the second stripping unit 44.2, the third stripping unit 44.3, or again to the (first) stripping unit 44. Alternatively, the film fragment fraction 50, 50.i can leave the process for further processing. Reference numeral list
[0181] 10 Alkali metal battery production 46.1 first intermediate sorting waste recovery plant, 46.2 second intermediate sorting alkali metal battery production 48 classifying device
[0182] attachment
[0183] 12 mixers, 50 foil fragment fraction
[0184] 14 Coating material 52 Coating material fraction 16 Active material 54 Alkaline metal battery production 18 Binder branch
[0185] 56 Production branch
[0186] 20 Additives 58 Recovery branch
[0187] 21 Primary coating material 62 Inert gas source
[0188] 22 Coating plant 63 Recycling plant
[0189] 23 primary coating materialbe64 inert gas
[0190] Holder 65 Contamination measuring device, 24 Current collector foil XRF, LIBS
[0191] 26 Electrode foil 66 Solvent
[0192] 27 coating 68 dryer
[0193] 28 dryers, 70 bunkers
[0194] 30 Calender B Binder content
[0195] 32 Schneider Bi4 coating material binder on 34 cell manufacturer part
[0196] 36 Electrolyte B21 Primary material binder content 38 Alkaline metal battery B52 Recycled binder content
[0197] 39 Removal device C24 film material content
[0198] cs Contamination threshold con40 Reject electrode foil centration
[0199] 42 Crushing device d27 Coating thickness
[0200] 43 Comminution material F51 Primary material particle size distribution 44 Stripping plant
[0201] 45 Dryer F52 Coating material fraction - 46 Separation material Particle size distribution i Flow index Stripping step M Material flow direction x Equivalent diameter Xcrit Critical particle size Xseparation Separation particle size
Claims
~ 5 i - v. Intel! ectua I property Duesenfeld GmbH Lawyer's file: Rothbergstraße 8 6110-0125 PCT-1 38176 Wendeburg Germany Date: May 15, 2026 Patent claims 1. Method for recycling alkali metal battery production waste in the form of reject electrode foil (40), which (i) a current collector foil (24) and (ii) has a coating (27) of the current collector foil (24), (iii) wherein the coating (27) contains active material (16) and a binder (18), comprising the steps (a) Stripping the coating from the rejected electrode foil (40) to produce separation material (46), (b) classifying the separation material (46), in particular according to particle size, to obtain a coating material fraction (52) and a foil fragment fraction (50), and (c) Using the coating material fraction (52) to coat current collector foil (24) to obtain electrode foil (26), (d) wherein the stripping and classification are carried out such that the coating material fraction particle size distribution (F52) corresponds to a primary particle particle size distribution (F21).
2. Method according to claim 1, characterized in that (a) the stripping is at least partly a crushing, in particular a shearing, and / or (b) the rejected electrode foil (40) is crushed, in particular cut or torn, before stripping.
3. Method according to claim 2, characterized in that (a) the crushing is carried out in such a way that (i) at most 5% by weight of the material to be crushed (43) a fragment size, measured as sieve size, of more than 100 mm, in particular more than 50 mm, and / or (ii) not more than 40% by weight, in particular not more than 20% by weight, of the comminution material (43) has a fragment size, measured as a sieve size, of less than 50 pm, in particular less than 100 pm; (b) the stripping in a stripping plant (44) is carried out by mechanical action on the comminution material (43) and / or (c) the material being separated (46) is dry during classification, where classification is in particular dry sieving.
4. Method according to one of the preceding claims, characterized in that the stripping of the rejected electrode foil (40) (a) is carried out at least substantially without the use of a solvent (66) of a binder (18) of the active material (16) and / or (b) does not include thermal decomposition of the binder (18) and / or (c) does not include cryotherapy and / or (d) without the addition of water or an aqueous liquid.
5. A method according to one of the preceding claims, characterized in that the coating material fraction (52) has a coating material fraction particle size distribution (F52) which applies the volume of particles below an equivalent diameter (x) over the equivalent diameter (x), and the stripping and classification are carried out such that the coating material fraction particle size distribution (F52) corresponds to a primary particle particle size distribution (F 2i ) corresponds.
6. Method according to one of the preceding claims, characterized by the steps (a) stripping the rejected electrode foil (40) such that first intermediate material (46.1) is formed, (b) Classifying the first intermediate separation material (46.1) according to particle size, so that a first coating material fraction (52.1) and a residual faction (50.1) will be obtained, (c) second separation of the residual fraction (50.1) so that a second intermediate separation material (46.2) is produced, (d) second classification of the second intermediate separation material (46.2) according to particle size, so that a second coating material fraction (52.1) and a second residual fraction (50.2), in particular in the form of the foil fragment fraction (50), are obtained, and (e) Using the first coating material fraction (52.1) to coat current collector foil (24) to obtain electrode foil (26).
7. Method according to claim 6, characterized in that (a) steps (c) and (d) are repeated at least once and (b) at least one coating material fraction (52) is not used for coating current collector foil (24).
8. Method according to one of claims 6 or 7, characterized in that (a) at least one, in particular the first coating material fraction (52) has a foil material content (C24) of foil material, in particular of aluminium and / or copper, which is less than a specified impurity threshold concentration (cs) and (b) at least one coating material fraction (52) has a foil material content (C24) above the impurity threshold concentration (cs) and (c) the at least one coating material fraction (52) whose foil material content (C24) is less than the specified impurity threshold concentration (cs) is used for coating current collector foil (24) and (d) that at least one coating material fraction (52) whose foil material content (C24) is not less than the specified impurity threshold concentration (cs) is not used for coating current collector foil (24).
9. Method according to one of the preceding claims, characterized in that for at least one stripping step the stripping intensity is greater than in at least one preceding stripping step.
10. Method according to one of the preceding claims, characterized by the steps (a) stripping the rejected electrode foil (40) with a first stripping intensity, (b) Separation of coating material (14), in particular during or after stripping, (c) then stripping the rejected electrode foil (40) with a second, greater stripping intensity.
11. Method according to one of claims 6 to 8, characterized by the steps (a) stripping the rejected electrode foil (40) by mechanical action, so that first intermediate separation material (46.1) is formed, (b) Classifying the first intermediate separation material (46.1) according to particle size, such that (i) a first coating material fraction (52.1) and (ii) a residual fraction (50.1) is obtained, (iii) wherein the film material content (C24) of the first coating material fraction (52.1) is less than a predetermined impurity threshold concentration (Cs), (c) Treating the residual fraction (50.1) with a binder solvent to produce a second intermediate separation material (46.2), (d) Separation of the second coating material fraction (52.2) from the intermediate separation material (46.2) and (e) Using the first coating material fraction (52.1) and / or the second coating material fraction (52.2) to coat current collector foil (24) to obtain electrode foil (26).
12. Method according to one of the preceding claims, characterized in that the classification (a) is carried out in such a way that the coating material fraction (52) is at most 0.1% by weight, in particular at most 0.01% by weight, of the particles larger than a separation particle size (x tre nn), where the separation particle size (x tre nn) is at most five times the active material particle size (XAM) in the form of the xgo particle size of the active material (16) and / or (b) the classification includes sieve classification, wherein the mesh size is at most 100 pm, in particular at most 80 pm, in particular at most 65 pm.
13. Method according to one of the preceding claims, characterized in that the classification is carried out such that (a) the aluminum content of metallic aluminum in the coating material fraction (52) is not more than 1 percent by weight, in particular not more than 0.5 percent by weight, and / or (b) the copper content of metallic copper in the coating material fraction (52) is not more than 1 percent by weight, in particular not more than 0.5 percent by weight, and / or (c) the iron content in the coating material fraction (52) is below 0.1 percent by weight, as long as iron is not a component of the active material (16).
14. Method according to one of the preceding claims, characterized by the step:
15. Method according to one of the preceding claims, characterized in that (a) the comminution, stripping and / or classification is carried out under inert gas (64) and / or dry room conditions and / or (b) the coating material (14) after stripping, in particular after any crushing, has at least substantially no contact with hydrogen fluoride and / or water.
16. Method according to one of the preceding claims, characterized by the step after classification of recycling at least a part of the film fragment fraction (50) for re-delamination, preferably a part whose particle size is larger than a predetermined recycling separation particle size, which is at least equal to the separation particle size (x tre nn) corresponds.
17. A method according to any of the preceding claims, in particular a method for producing alkali metal batteries (38), comprising the steps: (a) Coating current collector foil (24) with coating material (14) to form electrode foil (26), (b) Removing a portion of the electrode foil (26) as a reject electrode foil (40), (c) then performing steps (a) to (c) of claim 1, (d) then manufacture the alkali metal batteries (38) using the coating material fraction (52).
18. Method according to claim 17, characterized by the steps: Mixing the coating material fraction (52) with primary coating material (21) to obtain the coating material (14) with which the current collector foil (24) is coated.
19. Method according to claim 17 or 18, characterized in that (a) the coating material (14) has a coating material binder content (B) of binder (18) and (b) the coating material fraction (52) has a recycled binder content (B52) immediately after the coating material fraction (52) has been separated from the film fragment fraction (50) and (c) the recycled binder content (B52) is between half and twice the coating material binder content (B14).
20. Method according to one of the preceding claims, characterized in that the production of the alkali metal batteries (38) using the electrode foil (26) is carried out such that a coating thickness (d2?) of the coating (27) of the electrode is at least 1.5 times greater than the separating particle size (x tre nn).
21. Alkali metal battery production waste recovery plant (10) with (A) a mixer (12) for mixing and / or dispersing coating material (14), (B) a coating system (22) for coating current collector foil (24) with the coating material (14) coming from the mixer (12) so that electrode foil (26) is formed, (C) optionally a removal device (39) for removing part of the electrode foil (26) as a reject electrode foil (40), characterized by (D) a stripping unit (44) for, in particular purely mechanical, stripping of reject electrode foil (40) so that separation material (46) is produced, wherein the stripping unit (44) is arranged in the material flow direction (M) of the electrode foil (26) behind the coating unit, and (E) a classifying device (48) for classifying the separation material (46) to produce a coating material fraction (52) and a film fragment fraction (50), (F) wherein the classifying device (48) is connected to the mixer (12) for feeding at least parts of the coating material fraction (52) to the mixer (12).
22. Alkali metal battery production waste recovery plant (10) according to claim 21, characterized by (a) a primary coating material container (23) connected to the mixer (12) for feeding primary coating material (21), and containing primary coating material (21), (b) wherein the primary coating material (21) has a primary particle particle size distribution F2I, and (c) the classifying device (48) is designed to classify such that the coating material fraction (52) has a coating material fraction particle size distribution (F 52 ) which corresponds to the primary particle particle size distribution (F21).
23. Alkali metal battery production waste recovery plant (10) according to claim 21 or 22, characterized by a comminution device (42) for comminuting the reject electrode foil (40) so that comminution material (43) is obtained, wherein the comminution device (42) is arranged in the material flow direction (M) of the reject electrode foil (40) behind the coating system and wherein the comminution device (42) is arranged in the material flow direction (M) of the comminution material (43) upstream of the stripping unit (44).
24. Alkali metal battery production waste recovery plant (10) according to claim 21 or 22, characterized by a second coating removal system (44) for coating removal using solvent (66).