Aqueous dispersion of wax particles and method for increasing water and / or water vapour resistance of a moulded fibre article
An aqueous dispersion of plant or algal wax, stabilized with emulsifying and stabilizing agents, addresses the challenge of achieving effective water and vapor resistance in moulded fibre articles by reducing AKD usage and enhancing barrier properties in manufacturing and coating processes.
Patent Information
- Application Number
- PCT/FI2026/050251
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for enhancing the water and water vapor resistance of moulded fibre articles, such as those used in packaging and disposable products, face challenges in achieving desired barrier properties while adhering to regulatory limits, often requiring high amounts of petroleum-based chemicals like alkyl ketene dimer (AKD).
Aqueous dispersion of wax particles derived from plants or algae, stabilized with specific emulsifying and stabilizing agents, is applied in the wet end of the manufacturing process or as a coating, providing improved barrier properties with reduced amounts of AKD and other petroleum-based materials.
The dispersion achieves enhanced water and water vapor resistance in moulded fibre articles, meeting regulatory standards with improved stability and reduced chemical usage, suitable for both manufacturing and coating applications.
Smart Images

Figure IMGF000016_0001_TABLE 
Figure IMGF000017_0001_TABLE 
Figure IMGF000019_0001_TABLE
Abstract
Description
[0001] AQUEOUS DISPERSION OF WAX PARTICLES AND METHOD FOR INCREASING WATER AND / OR WATER VAPOUR RESISTANCE OF A MOULDED FIBRE ARTICLE
[0002] The present invention relates to an aqueous dispersion of wax particles comprising wax originating from plants and / or from algae as well as to a method for increasing water resistance and / or water vapour resistance of a moulded fibre article according to preambles of enclosed independent claims.
[0003] There is an overall interest to reduce the amount of petroleum-based materials, such as plastics, in manufacture of various goods. This includes manufacture of materials used for packaging applications as well as for single-use consumer products, such as disposable tableware. In these applications petroleum-based materials, such as plastics, increase challenges in recycling and reusing, especially when combined with other materials, such as cellulosic fibres. Furthermore, some consumers are concerned about the impact the plastics may have on the environment as well as human health, for example in form of microplastics.
[0004] Manufacture of fibre-based moulded pulp articles provides a versatile technique for producing complex 3D-shapes for a variety of different end-uses. Moulded pulp articles can be used for packaging of different products, such as foodstuffs, as well as for single-use products, such as disposable plates, cups, etc. Many of these enduses require a certain level of barrier performance. For example, moulded pulp articles used for packaging and / or serving food or liquids should show at least some water resistance and / or resistance against water vapour transmission.
[0005] In order to improve the barrier properties of fibre-based articles, different chemistries can be employed during the manufacturing process. Chemicals can be added to the fibre suspension from which the article is formed and / or a protective barrier coating can be formed on the surface of the produced article. A conventional way to provide water resistance properties for a fibre-based moulded pulp article is to add alkyl ketene dimer (AKD) sizing agent to the fibre suspension at the wet end of the manufacturing process. However, the amount of AKD needed for achieving thedesired barrier properties, especially in food contact applications, is often too high in view of regulatory limitations. Therefore, it can be difficult to achieve the required barrier properties, such as water resistance and / or water vapor transmission, while keeping within the allowable regulatory limits.
[0006] In view of above, there is a need for new composition, which can be used to improve the barrier properties of moulded pulp articles. These compositions should be safe to use, sustainable and be based on renewable sources.
[0007] An object of this invention is to minimise or possibly even eliminate the disadvantages existing in the prior art.
[0008] An object of this invention is also to provide a wax dispersion which is suitable for use both in the wet end of the manufacture of moulded pulp articles as well as in coating of produced moulded pulp articles.
[0009] A further object of this invention is to provide a wax dispersion which improves the barrier properties of moulded pulp articles.
[0010] These objects are attained with the invention having the characteristics presented below in the characterising parts of the independent claims. Some preferable embodiments are disclosed in the dependent claims.
[0011] The features recited in the dependent claims and the embodiments in the description are mutually freely combinable unless otherwise explicitly stated. The exemplary embodiments presented in this text and their advantages relate by applicable parts to all aspects of the invention, even though this is not always separately mentioned.
[0012] A typical aqueous dispersion of the present invention comprises wax particles dispersed in a continuous phase comprising water, wherein the wax particles comprise wax originating from a plant and / or from an alga and wherein the waxparticles have a mean particle size D50 of <15 pm, preferably <10 pm, more preferably <5 pm,
[0013] wherein the continuous phase of the aqueous dispersion comprises
[0014] - an emulsifying agent which is selected from sulphonated fatty alcohols and their salts, sulfonated hydrocarbons and their salts, ethoxylated alkyl phenols, polyethylene glycol esters and any combinations thereof, and
[0015] - a stabilizing agent which has a cationic charge, and is selected from synthetic wet strength polymers, cationized starches and cationized a-1 ,3-glucans.
[0016] A typical method according to the present invention for increasing water and / or water vapour resistance of a moulded fibre article, comprises
[0017] - obtaining a fibre suspension,
[0018] - forming the fibre suspension into a moulded fibre article in a mould,
[0019] - drying the moulded fibre article,
[0020] wherein the aqueous dispersion of wax particles according to the invention is added to the fibre suspension and / or applied on a surface of the moulded fibre article in form of a coating composition.
[0021] Now it has been surprisingly found that an aqueous dispersion of wax particles comprising wax originating from plants and / or algae is suitable both for a wet end addition in the manufacture of moulded pulp articles as well as for coating compositions applied on the produced moulded pulp articles. The aqueous dispersion of the present invention comprises a stabilization system comprising at least one emulsifying agent and at least one stabilizing agent. The stabilization system makes the dispersion of the wax particles suitable for both the wet end and coating applications, for example by providing the dispersion with low average particle size and dispersion stability.
[0022] In the present context “wet end application” means that the aqueous dispersion of wax particles is added to a fibre suspension comprising cellulosic fibres, where it is mixed with the cellulosic fibres and interacts with them. The fibre suspension may have a consistency of 0.1 - 4 weight-%, preferably 0.3 - 2 weight-%, at the time of addition of the dispersion of the wax particles.In the context of the present invention and in this text, all references to “wax particles” denotes wax particles comprising or consisting of wax originating from a plant and / or from an alga, if not explicitly stated otherwise.
[0023] In the aqueous dispersion of the present invention, the wax particles are dispersed in a continuous phase comprising water. The continuous phase may comprise >50 weight-%, preferably >75 weight-%, more preferably >90 weight-%, more preferably >95 weight-%, of water, calculated from total weight of the continuous phase. The continuous phase may comprise, for example, 50 - 100 weight-%, preferably 75 -99.9 weight-%, more preferably 90 - 99 weight-%, even more preferably 95 - 98 weight-%, of water, calculated from total weight of the continuous phase. In addition to water, the continuous phase may comprise an additional solvent, for example an alcohol, such as ethanol, isopropanol or butanol, or propylene glycol or glycerol. The additional solvent is preferably non-toxic and preferably approved for food contact by FDA (the US Food and Drug Administration). Preferably the continuous phase essentially consists of water. “Essentially consists of” means that the continuous phase comprises 0.5 weigh-% or less, preferably 0.25 weight-% or less, of an additional solvent other than water. According to one embodiment the continuous phase consists solely of water.
[0024] In the aqueous dispersion, the wax particles originating from a plant and / or from an alga may have a mean particle size D50 of <15 pm, preferably <10 pm, more preferably <5 pm, even more preferably <3 pm or <2.5 pm. The mean particle size D50 of the wax particles may be in a range of 0.05 - 15 pm, preferably 0.07 - 10 pm, more preferably 0.08 - 5 pm, even more preferably 0.1 - 3 pm or 0.1 - 2.5 pm. The particle size D50 can be determined by laser diffraction technique, by using Malvern Mastersizer. In the present context particle size D50 refers to the value for 50th percentile of a volume-based distribution. The combination of the emulsifying agent and the stabilizing agent, present in the continuous phase of the dispersion, makes it possible to provide a relatively low particle size for the wax particles originating from a plant and / or from an alga. This is beneficial not only for the stability of the dispersion, but also for its behaviour in the wet end and coating applications.Preferably the aqueous dispersion of the wax particles originating from a plant and / or from an alga is stable, which means that the wax particles are essentially uniformly dispersed in the continuous phase. Uniformly dispersed means that the difference in wax particle concentrations between any given two volumes within the aqueous dispersion is less than 20%, preferably less than 15%, more preferably less than 10%. Alternatively, the aqueous dispersion shows less than 5 %, preferably less than 3 %, change in turbidity over a specified period of 24 hours and / or less than 1 %, preferably less than 0.75 %, volume change over a specified period of 24 hours, which can be taken as indications of stable dispersion.
[0025] According to one preferable embodiment, the wax particles in the aqueous dispersion comprise or consist of wax originating from at least one plant. In the present context, the term “plant” encompasses land plants, such as vegetables, berries, trees, shrubs, grasses, etc, and aquatic plants, such as floating aquatic plants or submerged aquatic plants. The wax originating from a plant may be derived from various parts of plants, such as leaves, stems, fruits or any mixtures thereof. The aqueous dispersion may comprise wax particles originating from one type of plant or the aqueous dispersion may comprise wax particles originating from different plants, i.e. the dispersion may be a mixture of wax particles originating from different plants and / or from different parts of plant.
[0026] According to one preferable embodiment the wax particles comprise or consist of wax originating from sunflower, rapeseed, rice bran, coconut, canola, palm, palm kernel, soy, carnauba, ouricury, candelilla, sugarcane, linseed, cottonseed, jojoba, berry, castor, com, kokum, bayberry, peanut, esparto grass, kapok, sumac, laurel, olive, orange peel or any mixtures thereof. Preferably the wax originates from rapeseed, sunflower, rice bran, palm, palm kernel, sugarcane, or any mixtures thereof.
[0027] According to one embodiment of the invention the wax particles comprise wax originating from a plant material which is a by-product or surplus of food and / or energy production.According to one embodiment the wax particles comprise or consist of wax originating from at least one alga. For example, the wax particles may comprise wax originating from algae selected from Botryococcus braunii, Nannochloropsis, Isochrysis, Phaeodactylum tricornutum and Schizochytrium.
[0028] The wax originating from a plant and / or an alga may comprise a heterogenous mixture of esters of long-chain fatty acids, fatty alcohols, n-alkanes, fatty acids and sterol esters and / or esters of pentacyclic triterpenoids. The wax may comprise, for example, esters of long-chain fatty acids, e.g. esters of C14 - C36 fatty acids, esters of C16 - C30 fatty acids or esters of C18-C28 fatty acids.
[0029] The wax originating from a plant and / or an alga is preferably solid at room temperature of 20 °C or 25 °C. The wax may have a melting temperature >30 °C, preferably >40 °C or >50 °C, for example in a range of 30 - 95 °C, preferably 40 -90 °C or 50 - 90 °C. According to one embodiment the wax may have a melting temperature in a range of 40 - 90 °C, preferably 45 - 80 °C, more preferably 50 -75 °C.
[0030] The wax originating from a plant and / or an alga may be derived or obtained by any known method, for example, by solvent extraction followed by crystallization; supercritical fluid extraction; distillation, such as steam distillation, hydrodistillation or fractional distillation; enzymatic extraction; or by mechanical pressing, such as cold pressing. The wax may be purified by separating the wax from other lipid components, e.g. by using distillation, chromatography, or crystallization, or filtration. The wax may be further deodorized, bleached and / or hydrogenated. According to one embodiment the dispersion may comprise wax particles comprising wax originating from a plant and / or an alga, which wax has been hydrogenated or partially hydrogenated.
[0031] The aqueous dispersion of the present invention is preferably essentially free of wax particles comprising waxes of animal or microbiological origin, such as lanolin or beeswax. Further, the aqueous dispersion of the present invention is preferablyessentially free of wax particles comprising petroleum-based waxes of hydrocarbon origin.
[0032] According to one embodiment of the invention, the aqueous dispersion may comprise 1 - 50 weight-%, preferably 5 - 30 weight-%, more preferably 10 - 25 weight-% or 10 - 20 weight-%, of wax particles originating from a plant and / or an alga, calculated from the total weight of the aqueous dispersion. This means that the aqueous dispersion may comprise 1 - 50 weight-%, preferably 5 - 30 weight-%, more preferably 10 - 25 weight-% or 10 - 20 weight-%, of wax originating from a plant and / or from an alga, calculated from the total weight of the aqueous dispersion. The stabilization system comprising at least one emulsifying agent and at least one stabilizing agent, as described below, make it possible to obtain an aqueous dispersion having a high concentration of wax particles / wax while maintaining an appropriate dispersion stability and / or particle size.
[0033] The continuous phase of the aqueous dispersion comprises an emulsifying agent which is selected from sulphonated fatty alcohols and their salts, sulphonated hydrocarbons and their salts, ethoxylated alkyl phenols, polyethylene glycol (PEG) esters and any combinations thereof. The emulsifying agent may be or comprise a sulphonated fatty alcohol, including sulfonated aromatic fatty alcohols. The sulphonated fatty alcohol may be selected from sulphonated C12-C20 fatty alcohols, preferably C14-C20 or C12-C16 fatty alcohols and any of their salts, especially sodium or ammonium salts, for example lauryl sulphate, laureth sulphate sulphonate, olefin sulfonates and the corresponding sodium or ammonium salts. The sulphonated aromatic fatty alcohols may be selected from toluene sulphonates, xylene sulphonates, cumene sulphonates and naphthalene sulphonates and their sodium salts. The emulsifying agent may be or comprise a sulphonated hydrocarbon selected from synthetic and natural sulphonated hydrocarbons and aromatic hydrocarbons, and their salts. For example, the sulphonated hydrocarbon may be or comprise an aromatic hydrocarbon of natural origin, such as lignosulphonate. Alternatively, the sulphonated hydrocarbon may be or comprise synthetic aromatic hydrocarbon, such as xylene sulphonate. The emulsifying agent may further be or comprise a sulphonated hydrocarbon selected from dodecylbenzene sulphonateand alkyl sulphonates, such as C8-C18 alkyl sulphonates, and their salts. The emulsifying agent may be or comprise ethoxylated alkyl phenol selected from ethoxylated C4-C12 alkyl phenols, such as butylphenol ethoxylates, octylphenol ethoxylates, nonylphenol ethoxylates, dodecylphenol ethoxylates. The emulsifying agent may be or comprise polyethylene glycol (PEG) ester, such as PEG-400 monooleate or PEG-600 dilaureate, i.e. esters obtained by reacting polyoxyethylene glycol with a C10-C20 fatty acid, wherein the number in name indicates the number of ethylene oxide units in polyoxyethylene glycol.
[0034] According to one embodiment, the emulsifying agent is a sulphonated aromatic fatty alcohols and their sodium salts, such as naphthalene sulphonate.
[0035] The aqueous dispersion of wax particles may comprise 0.01 - 10 weight-%, preferably 0.02 - 5 weight-%, more preferably 0.05 - 3 weight-%, even more preferably 0.1 - 1 weight-% or still preferably 0.1 -0.95 weight-% , of the emulsifying agent, calculated from total weight of the dispersion. It was observed that these amounts of emulsifying agent could provide desired dispersion characteristics.
[0036] According to one embodiment, the aqueous dispersion of wax particles comprising wax originating from a plant and / or from an alga may comprise the emulsifying agent in a ratio from 1:50 to 1:55 (emulsifying agent:wax).
[0037] The continuous phase of the aqueous dispersion comprises a stabilizing agent which has a cationic charge. The stabilizing agent is selected from cationic synthetic wet strength polymers, cationized starches and / or cationized a-1 ,3-glucans. The stabilizing agent may be or comprise a synthetic wet strength polymer selected from polyamidoamine epihalohydrin, preferably polyamidoamine epichlorohydrin. Alternatively, the stabilizing agent may be or comprise a cationized polysaccharide, selected from cationized starches having a degree of cationic substitution DS in a range of 0.01 - 0.2. The stabilizing agent may comprise or be selected from cationized a-1 ,3-glucan polymers. Suitable a-1,3-glucan polymers may have a degree of polymerization in a range of 55 - 10 000, preferably 55 - 5000, more preferably 100 - 1000, and they may have a degree of cationic substitution degreein a range of 0.05 - 3, preferably 0.1 - 2.0, more preferably 0.2 - 1.5, even more preferably 0.2 - 1 or 0.2 - 0.8.
[0038] According to one preferable embodiment, the stabilizing agent is cationized starch.
[0039] The stabilizing agent may have a cationic charge in a range of 0.1 - 5 meq / g, for example 0.5 - 4 meq / g or 1 - 3.5 meq / g. The charge density may be measured by using Mutek at pH 4.0.
[0040] The aqueous dispersion of the wax particles originating from a plant and / or an alga may comprise 0.01 - 15 weight-%, preferably 0.03 - 12 weight-%, more preferably 0.05 - 10 weight-%, even more preferably 0.1 - 5 weight-%, of the stabilizing agent, calculated from total weight of the dispersion. Preferably the amount of the stabilizing agent is higher than the amount of the emulsifying agent in the aqueous dispersion.
[0041] According to one embodiment, the aqueous dispersion of wax particles comprising wax originating from a plant and / or from an alga may comprise the stabilizing agent in a ratio from 1:4 to 1:5 (stabilizing agent:wax).
[0042] The aqueous dispersion of the wax particles originating from a plant and / or an alga may have a solid content in a range of 10 - 30 weight-%, preferably 15 -25 weight-%.
[0043] The aqueous dispersion of the wax particles originating from a plant and / or from an alga is preferably free of solid material, such as solid particles or solid fibres.
[0044] According to one preferable embodiment the aqueous dispersion of the wax particles originating from a plant and / or from an alga may further comprise alkyl ketene dimer. It was unexpectedly found that when the aqueous dispersion comprising wax particles, comprising wax originating from a plant and / or an alga, is used together with alkyl ketene dimer, significantly improved barrier performance, such as resistance for water and / or resistance for water vapour transmission, canbe achieved. This means that better barrier properties can be obtained, even by using low amounts of alkyl ketene dimer and low amounts of wax particles. The aqueous dispersion preferably comprises alkyl ketene dimer in an amount of 0.1 -10 weight-%, preferably 0.3 - 5 weight-%, more preferably 0.5 - 3 weight-%, calculated from the total weight of the aqueous dispersion. If present, alkyl ketene dimer is present in the aqueous dispersion as discrete alkyl ketene dimer particles, dispersed in the continuous phase of the dispersion, preferably having a particle size D95 in a range of 1 - 100 pm , preferably 10 - 100 pm , more preferably 20 - 95 pm. Particle size D95 indicates that 95% of the total particles are smaller than the given value, and can be measured by using laser diffraction technique.
[0045] The aqueous dispersion comprising wax particles originating from a plant and / or an alga may further comprise one or more biocidal agent and / or fungicidal agent. The amount of biocidal agent and / or fungicidal agent may be <0.05 weight-%, more preferably <0.03 weight-%, calculated from the total weight of the dispersion. For example, the aqueous dispersion may comprise biocidal agent and / or fungicidal agent in amount of 0.001 - 0.05 weight-% or 0.005 - 0.03 weight-%.
[0046] The aqueous dispersion comprising wax particles originating from a plant and / or an alga is especially suitable for increasing water resistance and / or water vapour resistance of a moulded fibre article. The moulded pulp article may be an article that comes into a contact with food products, such as a food packaging product or a food serving product. The moulded fibre article can be a cup, bowl, plate, clamshell container, food service tray, food container, carryout food container, catering tray, food pot, food box, frozen food tub or the like. The formed moulded fibre article may have a grammage of 200 - 2000 g / m2, preferably 300 -1500 g / m2, more preferably 350 - 900 g / m2.
[0047] In the manufacturing process of fibre articles, a fibre suspension is obtained and formed into a moulded fibre article in a mould and dried. This kind of processes are known for a person skilled in the art and need not to be described in detail. For example, the moulded fibre articles can be formed by depositing a fibre layer on the surface of the mould, preferably by using vacuum. The pulp layer, i.e. the mouldedfibre article, is then compacted by pressing between the surface of the mould and the surface of a counter-mould, wherein at least one of the surfaces has a temperature of >100 °C. Preferably, the temperature of at least one of the surfaces may be in a range of 130 - 230 °C, preferably 140 -210 °C, more preferably 150 -200 °C, at the compacting of the formed moulded fibre article.
[0048] The moulded fibre articles may be formed from a fibre suspension comprising cellulosic fibres. The cellulosic fibres may comprise virgin fibres, recycled fibres or their mixtures. The cellulosic fibres may comprise non-wood fibres, wood fibres or any mixtures thereof. The non-wood fibres may comprise bamboo fibres; sugarcane fibres; bagasse fibres; sorghum fibres; straw or grass fibres, such as sabai grass fibres; seed hair fibres, such as cotton, kapok, coir or milkweed fibres; leaf fibres, such as sisal, abaca or pineapple fibres; bast fibres, such as flax, hemp, jute, ramie or kenaf fibres; or any mixtures thereof. The cellulosic fibres may comprise softwood fibres and / or hardwood fibres, for example fibres of pine, spruce, fir, poplar, eucalyptus, maple, birch, aspen, alder, acacia or any mixtures thereof.
[0049] The aqueous dispersion comprising wax particles originating from a plant and / or an alga can be added in the wet end, i.e. into the fibre suspension before formation of the moulded fibre article, or the aqueous dispersion comprising wax particles can be applied on a surface of the moulded fibre article, usually after drying of the moulded fibre article, in form of a coating composition. It is also possible to add the aqueous dispersion of wax particles both to the fibre suspension and on the surface of the moulded fibre article.
[0050] The aqueous dispersion of wax particles may be added to the fibre suspension within wide application limits, depending on the end-application of the moulded fibre article to be produced. If strong barrier properties against water and / or water vapour are required, and the formed article is not intended for food contact, the dispersion of wax particles can be added up to 200 kg / t dry article. For example, when the aqueous dispersion of wax particles is added in the wet end, i.e. to the fibre suspension before forming of the moulded fibre article, the aqueous dispersion of wax particles may be added to the fibre suspension in amount, which provides waxin a range of 5 - 150 kg / t dry fibre article, preferably 25 - 100 kg / t dry fibre article, more preferably 40 - 80 kg / t dry fibre article.
[0051] When the aqueous dispersion of wax particles originating from a plant and / or an alga is used in a combination with alkyl ketene dimer, the alkyl ketene dimer may be added to the fibre suspension in an amount of 0.5 - 60 kg / t dry fibre article, preferably 0.8 - 30 kg / t dry fibre article, more preferably 1 - 10 kg / t dry fibre article. Very good barrier properties against water and / or water vapour can thus be achieved.
[0052] If the moulded fibre article is intended for food contact, alkyl ketene dimer may be added to the fibre suspension in an amount of 0.1 - 4 kg / t dry fibre article, preferably 0.4 - 3.5 kg / t dry fibre article, more preferably 0.5 - 2 kg / t dry fibre article.
[0053] Alkyl ketene dimer may be added to the fibre suspension together with aqueous dispersion comprising the wax particles. The alkyl ketene dimer particles may be present in the aqueous dispersion of wax particles comprising wax originating from a plant and / or from an alga, i.e. the aqueous dispersion may be a mixture of wax particles and alkyl ketene dimer particles. Alternatively, alkyl ketene dimer may be added as an alkyl ketene dimer dispersion, separately from the aqueous wax dispersion, wherein the addition of the dispersions may be simultaneous or successive.
[0054] According to one embodiment the aqueous dispersion comprising wax particles originating from a plant and / or an alga may be added on the surface of the formed article in form of a coating composition. In addition to the aqueous dispersion of wax particles, the coating composition may comprise an acrylate copolymer. For example, the coating composition comprises 5 - 40 weight-%, preferably 10 - 35 weight-%, more preferably 15- 30 weight-%, of the dispersion of wax particles, and optional acrylate copolymer, preferably in amount of 60 - 95 weight-%, preferably 65 - 90 weight-%, more preferably 70 - 85 weight-% of the acrylate copolymer, calculated from total dry weight of the coating composition.The acrylate copolymer used in the coating composition together with the aqueous dispersion comprising wax particles may be in form of a dispersion comprising polymer particles suspended in a continuous aqueous phase. The polymer dispersion may comprise acrylate copolymer particles, which have a particle size D50 <800 nm. The particle size D50 for the acrylate copolymer particles may be, for example, in a range of 50 - 800 nm, preferably 60 - 500 nm, more preferably 80 -350 nm. Particle size is measured by using Zetasizer Nano ZS, Malvern. In the present context the particle size D50 refers to the value for 50th percentile of a volume-based distribution.
[0055] According to one embodiment, the coating composition may comprise an acrylate copolymer which is obtained by a radical polymerisation, preferably by a free radical polymerisation, of one or more vinyl monomers. The vinyl monomers comprise at least one alkyl (meth)acrylate. The acrylate copolymer may be obtained by a radical polymerisation of several, such as two, three or more, different vinyl monomers, of which at least one is alkyl (meth)acrylate. Preferably the acrylate copolymer is obtained by a radical polymerisation of two or three different vinyl monomers of which at least one is alkyl (meth)acrylate. The alkyl (meth)acrylate may be selected from as C1-C18 alkyl (meth)acrylates, preferably C1-C12 alkyl (meth)acrylates, more preferably C1-C4 alkyl (meth)acrylates, and any of their mixtures. Vinyl monomers may comprise methyl acrylate; methyl methacrylate; ethyl acrylate; ethyl methacrylate; n-propyl or iso-propyl acrylate and corresponding propyl methacrylates; n-butyl, iso-butyl, tert-butyl or2-butyl acrylate and the corresponding butyl methacrylates; n-pentyl or neopentyl acrylate and the corresponding pentyl methacrylates; 2-hexyl or 2-ethylhexyl acrylate and corresponding methacrylates; n-octyl or isooctyl acrylate and corresponding methacrylates; decyl acrylate; decyl methacrylate; dodecyl acrylate; dodecyl methacrylate; lauryl acrylate; lauryl methacrylate; stearyl acrylate; stearyl methacrylate. Preferably vinyl monomers may comprise C1 -C4-alkyl acrylates, C1 -C4-alkyl methacrylates or any of their mixtures, e.g. n-butyl, iso-butyl, tert-butyl or 2-butyl acrylate and the corresponding butyl methacrylates; methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate or propyl methacrylate. According to one preferable embodiment the vinyl monomers may comprise or consists of a mixture of at leasttwo isomeric butyl acrylates, e.g. a mixture of n-butyl acrylate and methyl methacrylate or a mixture of n-butyl acrylate and tert-butyl acrylate.
[0056] According to one embodiment, the acrylate copolymer may be obtained by a radical polymerisation of one or more alkyl (meth)acrylates, as listed above, and one or more styrene monomers selected from styrene, substituted styrenes, such as a-methylstyrene, vinyltoluene, ethylvinyltoluene, chloromethylstyrene, and any mixtures thereof.
[0057] According to one preferable embodiment the acrylate polymer be a styrene (meth)acrylate copolymer be obtained by free radical polymerisation of at least one styrene monomer, as listed above, and at least one C1-C4-alkyl (meth)acrylate monomer, in a presence of a stabiliser, as listed above. The C1-C4-alkyl (meth)acrylate monomer may be selected from a group consisting of C1-C4-alkyl acrylates; C1-C4-alkyl methacrylates; or their mixtures, e.g. n-butyl, iso-butyl, tertbutyl or2-butyl acrylate and the corresponding butyl methacrylates; methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate or propyl methacrylate. According to one preferred embodiment the C1-C4-alkyl (meth)acrylate monomer is selected from butyl (meth)acrylates, such as n-butyl acrylate, tert-butyl acrylate or their mixtures. The amount of the styrene monomer may be 0.1 - 75 weight-%, preferably 5 - 60 weight-%, more preferably 10 - 55 weight-%, and the amount of the C1-C4-alkyl (meth)acrylate monomer may be 25 -99.9 weight-%, preferably 30 - 95 weight-%, more preferably 35 - 90 weight-%, calculated from the total dry solids content of the monomers.
[0058] According to another embodiment, the acrylate copolymer is obtained by radical polymerisation of one or more alkyl (meth)acrylates, as listed above, in absence of styrene monomers, such as styrene and substituted styrenes. The acrylate copolymer may thus be free of structural units originating from monomers selected from styrene, substituted styrenes, such as a-methylstyrene, vinyltoluene, ethylvinyltoluene, chloromethylstyrene, and any of their mixtures.According to one embodiment, the acrylate copolymer may be obtained by a radical polymerisation of one or more alkyl (meth)acrylates, as listed above, and one or more charge-carrying monomers. The charge-carrying monomer may be anionic or cationic. For example, the charge-carrying monomer may be anionic and selected from carboxylic acid, such as acrylic acid, methacrylic acid, itaconic acid, maleic acid or styrene sulphonic acid. Acrylic acid and styrene sulphonic acid are preferable charge-carrying monomers. The amount of the charge-carrying may be 0.1 - 15 weight-%, preferably 0.1 - 10 weight-%, more preferably 1 -5 weight-%, calculated from the total dry solids content of the monomers.
[0059] The acrylate copolymer is preferably obtained by radical polymerisation in the presence of a polymerisation stabiliser, such as degraded starch or polyvinyl alcohol. Preferably the polymerisation stabiliser is degraded starch having a number average molecular weight Mn of 500 to 10000. Degraded starch may be obtained by subjecting starch to oxidative, thermal, acidic, hydrolytic or enzymatic degradation, the oxidative degradation presently being preferred. Hypochlorite, peroxodisulphate, hydrogen peroxide or their mixtures may be used as oxidising agents. Degraded starch, which is used as the polymerisation stabiliser in the radical polymerisation of the acrylate copolymer may be any suitable degraded natural starch, such as potato, rice, corn, waxy corn, wheat, barley or tapioca starch. Starches having an amylopectin content >80 %, preferably >95 %, are advantageous.
[0060] The acrylate copolymer used in the coating composition may have a glass transition temperature Tg in a range from -40 °C to +80 °C, preferably from -30 °C to +40 °C or from -25 °C to +20 °C, more preferably from -20 °C to +15 °C or from -15 °C to +10 °C. The glass transition temperatures are measured from freeze dried samples using a differential scanning calorimeter Mettler Toledo DSC 3+. The acrylate copolymers with a glass transition temperature within these ranges are able to provide coating compositions with the aqueous dispersion comprising wax particles which have an appropriate ductility, able to withstand cracking when the fibre article, such as fibrous sheet, is creased or folded.EXAMPLES
[0061] Some embodiments of the invention are described in the following non-limiting examples.
[0062] Wax dispersions 1 -6 used in the application examples 1 and 2 were prepared from RSPO certified palm oil and / or rapeseed oil. Cationized starch was used as a stabilizing agent and naphthalene sulphonate as an emulsifying agent in all wax dispersions 1 - 6. Given to the amount of wax, the stabilizing agent was present in the wax dispersions in a ratio from 1:4 to 1:5 (stabilizing agent:wax) and the emulsifying agent in a ratio from 1 :50 to1 :55 (emulsifying agent:wax).
[0063] Plant source for the wax and the mean particle size D50 for the wax dispersions used in the application examples 1 and 2 are given in Table 1.
[0064] Table 1 Wax dispersions used in the application examples.
[0065] Mean particle size D50
[0066] # Wax source
[0067] [pm]
[0068] Wax1 Palm oil 1.63
[0069] Wax2 Palm oil + rapeseed 1.78
[0070] Wax3 Rapeseed 2.6
[0071] Wax4 Rapeseed + coconut 11.9
[0072] Wax5 Vegetable* 2.16
[0073]
[0074] Wax6 Vegetable* - *palm oil free
[0075] Application example 1
[0076] Fibre stock comprised 70 weight-% of bleached hardwood Kraft fibres and 30 weight-% of bleached softwood Kraft fibres, calculated from total dry fibre weight. The fibre stock had a freeness of 25 °SR. Alkyl ketene dimer (AKD), wax dispersion and a retention additive (cationic polyacrylamide) were introduced to the fibre stock in amount and order shown in Table 2. All amounts are given per ton of dry fibre stock. Consistency of the fibre stock was adjusted to 0.35 - 0.4 weight-%. After the addition of each chemical, the fibre stock was mixed for 90 seconds.Table 2 Used chemicals, their amounts and application order, as well as results of application example 1.
[0077] Sample AKD Wax1 Wax2 Wax3 Retention Cobb 300
[0078] # [kg / t]* [kg / t] [kg / t] [kg / t] additive [g / m2]
[0079] 1
[0080] (reference) 2 - - - 0.15 43
[0081] 2 2 60 - - 0.15 33
[0082] 3 2 120 - - 0.15 33
[0083] 4 2 180 - - 0.15 34
[0084] 5 - 180 - - 0.15 38
[0085] 6 2 - 60 - 0.15 33
[0086] 7 2 - 120 - 0.15 33
[0087] 8 2 - 180 - 0.15 32
[0088] 9 - - 180 - 0.15 40
[0089] 10 2 - - 60 0.15 35
[0090] 11 2 - - 120 0.15 35
[0091] 12 2 - - 180 0.15 35
[0092]
[0093] 13 - - - 180 0.15 39 as active chemical
[0094] After introduction of the chemicals according to Table 2, the fibre stock was vacuum formed to dryness of 20 - 30 weight-% using Rapid Kothen method and forming wire with 200 - 400 micron openings. A wet 2D fibre article in form of a sheet with a gram mage of 200 - 800 g / m2(as dry) was first wet pressed to 28 - 33 weight-% dryness and then hot press dried and thermoformed to 0.2 - 1.2 mm thickness between 130 - 200 °C metal plates until dryness of 94 - 99 weight-% was reached.
[0095] Cobb300 test was performed for the formed fibre articles, by using a test method based on standard ISO 535. The procedure of the standard is followed except the used cylinder area was 10 cm2. Table 2 shows the Cobb300 results for the fibre articles. It can be seen from Table 2 that the use of wax dispersion significantly improve the Cobb300 results even if the AKD amount is kept constant.
[0096] It can be seen from Table 2 that dispersion of wax particles provided better Cobb300 values than AKD alone. The results were improved when wax dispersions were used together with AKD.Application Example 2: Wax dispersion applied on the surface in form of a coating composition
[0097] Coating formulations were prepared by mixing a styrene acrylate polymer dispersion SAP and various dispersions of wax particles in a weight ratio 80:20, as indicated in Table 3. The solid content of the coating formulations was about 38 weight-%.
[0098] The coating formulations were coated on uncoated cupstock board, grammage 215 g / m2.
[0099] Used substrate was 215 g / m2uncoated cupstock board. Coating formulation was applied on the uncoated substrate by using RK K Control Coater rod coating unit. The formulation was applied by using coating rod (3) with wire diameter of 24 pm. For triple-coated samples the first pre-coat layer was applied by using coating rod 3 or 4. Coat weights of the samples are given in Table 3. The drying of the coated samples was carried out using IR dryer, 60 seconds.
[0100] The coated samples were climatized for minimum of 18 hours before measuring the grammage and coat weight. The following parameters were then measured:
[0101] Cobb60 and Cobb300 (ISO 535)
[0102] KIT value (TAPPI method T-559 pm-96)
[0103] Olive oil resistance (ISO 16235-2 & TAPPI 507 cm-99), 40 °C, 5 bar, 170 h Standard water vapor transmission, SWVTR (ASTM E-96, D3985 & F1927, 23 °C 50% RH)
[0104] Tropical water vapor transmission, TWVTR (ASTM E-96, D3985 & F1927, 38 °C 90% RH)
[0105] Gurley porosity, ISO 5636-5:2013
[0106] Bendtsen roughness, ISO 5636-3
[0107] The obtained results are given in Table 3.Table 3 Results of application example 2.
[0108] 100%
[0109] SPA*
[0110] (reference)
[0111] Coat weight 15.3 16.9 16.8 16 16.6 16.1 16.7 [g / m2]
[0112] SWVTR 47 22 27 30 25 32 29 [g / m2 / day] 80% SPA*
[0113] TWVTR 488 3 20% W1ax06 352 398 323 420 339 [g / m2 / day]
[0114] Cobb60 25 13 15 16 11 14 14 [g / m2] 80% SPA*
[0115] Cobb300 20% W2ax
[0116] 56 38 40 41 39 39 39 [g / m2]
[0117] Bendtsen 0 0.45 0.12 80% SPA* 0 0.43 1.58 1.37
[0118]
[0119] Gurley >45000 28267 41167 >450 20% W3ax00 29133 9555 14553 *SPA denotes styrene acrylate polymer, % values are weight-%, given as dry.
[0120] 80% SPA*
[0121] It can be seen from Table 3 that addition of wax dispersion 20% W4ax according to the present invention to the coating formulation clearly improved the water resistance of the 80% SPA*
[0122] coated sample. 20% W5ax
[0123] Even if the invention was described with reference to what at present see 80% SPA*ms to be 20% W6ax the most practical and preferred embodiments, it is appreciated that the invention shall not be limited to the embodiments described above, but the invention is intended to cover also different modifications and equivalent technical solutions within the scope of the enclosed claims.
Claims
CLAIMS1. An aqueous dispersion of wax particles dispersed in a continuous phase comprising water, wherein the wax particles comprise wax originating from a plant and / or from an alga and wherein the wax particles have a mean particle size D50 of <15 pm, preferably <10 pm, more preferably <5 pm,wherein the continuous phase of the aqueous dispersion comprises- an emulsifying agent which is selected from sulphonated fatty alcohols and their salts, sulphonated hydrocarbons and their salts, ethoxylated alkyl phenols, polyethylene glycol esters and any combinations thereof, and- a stabilizing agent which has a cationic charge, and is selected from synthetic wet strength polymers, cationized starches and cationized a-1 ,3-glucans.
2. The aqueous dispersion according to claim 1 , characterised in that the wax particles comprise wax originating from sunflower, rapeseed, rice bran, coconut, canola, palm, palm kernel, soy, carnauba, ouricury, candelilla, sugarcane, linseed, cottonseed, jojoba, berry, castor, com, kokum, bayberry, peanut, esparto grass, kapok, sumac, laurel, olive, orange peel, or any mixture thereof.
3. The aqueous dispersion according to claim 1 or 2, characterised in that the wax originating from a plant and / or an alga has a melting temperature in a range of 40 -90 °C, preferably 45 - 80 °C, more preferably 50 - 75 °C.
4. The aqueous dispersion according to claim 1, 2 or 3, characterised in that the wax particles have the mean particle size D50 in a range of 0.05 - 15 pm, preferably 0.07 - 10 pm, more preferably 0.08 - 5 pm, even more preferably 0.1 - 3 pm.
5. The aqueous dispersion according to any of preceding claims 1 - 4, characterised in that the dispersion comprises 1 - 50 weight-%, preferably 5 - 30 weight-%, more preferably 10 - 20 weight-%, of the wax particles, calculated from the total weight of the dispersion.
6. The aqueous dispersion according to any of preceding claims 1 - 5, characterised in that the emulsifying agent comprises- a sulphonated fatty alcohol selected from sulphonated C12-C20, preferably C14-C20 fatty alcohols; and / or- a sulphonated hydrocarbon selected from synthetic and natural sulphonated hydrocarbons and aromatic hydrocarbons, and their salts, such as lignosulphonates, xylene sulphonate, dodecylbenzene sulphonate, alkyl sulphonates; and / or- ethoxylated alkyl phenols selected from ethoxylated C4-C12 alkyl phenols, such as butylphenol ethoxylates, octylphenol ethoxylates, nonylphenol ethoxylates, dodecylphenol ethoxylates; and / or- polyethylene glycol esters, such as PEG-400 monooleate and PEG-600 dilaurate.
7. The aqueous dispersion according to any of preceding claims 1 - 6, characterised in that the dispersion comprises 0.01 - 10 weight-%, preferably 0.05 -3weight-%, more preferably 0.1 - 1 weight-%, of the emulsifying agent, calculated from total weight of the dispersion.
8. The aqueous dispersion according to any of preceding claims 1 - 7, characterised in that the stabilizing agent comprises- a synthetic wet strength polymer selected from polyamidoamine epihalohydrin, and / or- cationized starch having a degree of substitution DS in a range of 0.01 - 0.2, and / or - a cationized a-1 ,3-glucan.
9. The aqueous dispersion according to any of preceding claims 1 - 8, characterised in that the dispersion comprises 0.01 - 15 weight-%, preferably 0.05 - 10 weight-%, more preferably 0.1 -5 weight-%, of the stabilizing agent, calculated from total weight of the dispersion.
10. The aqueous dispersion according to any of preceding claims 1 - 9, characterised in that the dispersion has a solid content in a range of 10 - 30 weight-%, preferably 15 - 25 weight-%.
11. The aqueous dispersion according to any of preceding claims 1 - 10, characterised in that the aqueous dispersion further comprises alkyl ketene dimer, preferably in amount of 0.1 - 10 weight-%, preferably 0.3 - 5 weight-%, more preferably 0.5 - 3 weight-%, calculated from the total weight of the aqueous dispersion.
12. The aqueous dispersion according to any of preceding claims 1 - 11, characterised in that the dispersion further comprises one or more biocidal agents and / or fungicidal agents, preferably in amount of <0.05 weight-%, more preferably <0.03 weight-%, calculated from the total weight of the aqueous dispersion.
13. Method for increasing water and / or water vapour resistance of a moulded fibre article, the method comprising- obtaining a fibre suspension,- forming the fibre suspension into a moulded fibre article in a mould,- drying the moulded fibre article,characterised in thatthe aqueous dispersion of wax particles according to any of claims 1 - 12 is added to the fibre suspension and / or applied on a surface of the moulded fibre article in form of a coating composition.
14. Method according to claim 13, characterised in that the aqueous dispersion of wax particles added to the fibre suspension in amount of 5 - 150 kg / t dry fibre article, preferably 25- 100 kg / t dry fibre article, more preferably 40 - 80 kg / t dry fibre article.
15. Method according to claim 13 or 14, characterised in that alkyl ketene dimer is added to the fibre suspension in an amount of 0.5 - 60 kg / t dry fibre article, preferably 0.8 - 30 kg / t dry fibre article, more preferably 1 - 10 kg / t dry fibre article.
16. Method according to claim 13 or 14, characterised in that alkyl ketene dimer is added to the fibre suspension in an amount of 0.1 - 4 kg / t dry fibre article, preferably 0.4 - 3.5 kg / t dry fibre article, more preferably 0.5 - 2 kg / t dry fibre article.
17. Method according to any of preceding claims 13 - 16, characterised in that the aqueous dispersion of wax particles is applied on the surface of the moulded fibre article in a form of a coating composition.
18. Method according to claim 17, characterised in that the coating composition comprises 5 - 40 weight-%, preferably 10 - 35 weight-%, more preferably 15 - 30 weight-%, of the dispersion of wax particles, and optionally an acrylate copolymer, preferably in amount of 60 - 95 weight-%, preferably 65 - 90 weight-%, more preferably 70 - 85 weight-%.