Furfural-based compounds
Patent Information
- Application Number
- PCT/FI2026/050253
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-15
- Publication Date
- 2026-11-19
Abstract
Description
[0001] Furfural-based compounds
[0002] BACKGROUND
[0003] Vinyl ester resins (VERs) and epoxies are widely utilized thermosets that mostly consist of oligomerized bisphenol A-glycidyl methacrylate (BisGMA) and bisphenol A diglycidyl ether (DGEBA), respectively. Typically, VERs show excellent mechanical and thermal properties, fast curing along with low volume shrinkage, corrosion resistance, low weight, and relatively low cost.1-4For those reasons, VERs are utilized in various applications from dental materials to corrosion resistant coatings. Epoxies, on the other hand, are utilized as strong adhesives and other applications which need ultimate strength.56
[0004] Utilization of bisphenol A-based resins brings several challenges. Being highly viscous liquids, BisGMA and DGEBA may require the addition of reactive diluents to achieve the low viscosity needed for liquid molding resin applications. Furthermore, reactive diluents act as chain extenders improving polymer performance. Styrene is the most preferred and widely used reactive diluent for VERs.4,7In addition to the challenges associated to volatile and hazardous styrene, there are concerns about the raw material of these resins, bisphenol A (BPA). It is an endocrine disruptor that can lead to several health problems.8In addition, BisGMA and DGEBA are currently produced from fossil-based chemicals received from oil refining. Utilization of fossil resources causes several problems including their negative effect on environment.9Since VERs and epoxies have excellent properties and are used in many applications, biobased alternatives should be developed to overcome the above-mentioned issues.
[0005] Biomass is continuously produced in nature - global estimation of the amount of biomass generated annually is 170 billion metric tons.10Recent studies have shown that increasing the bioplastic production, especially utilizing various residual biomasses as raw material sources, has a positive climate effect constraining the CO2 emissions and raise of global mean temperature.11Non-edible lignocellulosic biomass has shown to be the most promising and abundant renewable source of carbon.12 13
[0006] Furfural, also known as 2-furaldehyde, is a versatile furan-derivative and an important platform compound as it can be used as a starting material for several other biochemicals.14It can be produced from hemicellulose-rich lignocellulosic side streams and leftovers of agriculture or forestry, such as corncobs, sugarcane bagasse, wood chips, etc.15Furfural acts as a precursor for other furan derivatives, such as furfuryl alcohol, levulinic acid, andtetrahydrofuran.13’14 16The aldehyde functional group allows furfural to participate in reactions leading to thermosets, such as phenol-furfural resins which resemble traditional phenol-formaldehyde resins.17
[0007] In this disclosure, synthetic methods for two sulfur-bridged dimethacrylate monomers and one sulfur-bridged epoxy monomer derived from furfural are reported. Furfural-based dimethacrylates were thermally cured using tert-butyl peroxybenzoate as a curing agent to form cross-linked vinyl esters. Furfural-based epoxy resin was cured with 4,4-diaminodiphenyl sulfone, and with methylhexahydrophthalic anhydride and 2-ethyl-4-methylimidazole. The results suggest that these furfural -based materials have great potential as alternatives to their petroleum-based counterparts.
[0008] SUMMARY
[0009] The environmental impact of utilizing fossil-based resources in polymer production has raised serious concerns in recent decades. As a response, the development of renewable alternatives has garnered significant interest. Addressing the issue, the syntheses of two renewable sulfur-bridged dimethacrylates and one renewable sulfur-bridged diepoxy via three-step routes starting from commercial 5-bromofurfural are demonstrated. The dialdehyde and aldehyde intermediates were obtained using sodium sulfide and 2-mercaptoethanol, respectively, followed by reduction to diols and subsequent methacrylation using methacrylic anhydride or epoxidation using epichlorohydrin. The properties of the biobased dimethacrylates were compared to those of a commercially available petroleum-based vinyl ester resin and its neat monomer, BisGMA. The difuran-based dimethacrylate monomer was a waxy solid at room temperature but exhibited relatively low viscosity in its liquid state at elevated temperature, while the unsymmetrical vinyl ester and epoxy monomers, containing a single furan ring, showed low viscosity at room temperature - highlighting their favorable processing characteristics. Both cured biobased vinyl ester resins showed highly cross-linked networks, with high glass transition temperatures (183 and 162 °C), while thermal decomposition took place at 251 and 285 °C. The biobased epoxy resins cured with two different methods showed 7gvalues of 64 and 28 °C measured with DSC. The values determined from peak of tan 3 were 76 and 59 °C. Furthermore, both vinyl ester materials demonstrated chemical and water resistance comparable to their fossil-based counterpart. The results support the potential of thesedimethacrylates as renewable alternatives to unsustainable vinyl ester resins in various applications.
[0010] The invention is defined by the features of the independent claims. Some specific embodiments are defined in the dependent claims.
[0011] According to a first aspect of the present invention, there is provided a sulfur-bridged dimethacrylate compound comprising or consisting of a structure of formula
[0012]
[0013] According to a second aspect of the present invention, there is provided a sulfur-bridged diepoxy compound comprising or consisting of a structure of formula
[0014]
[0015] According to a third aspect of the present invention, there is provided a curable resin composition comprising the sulfur-bridged dimethacrylate compound of Formula I or II and / or the sulfur-bridged diepoxy compound of Formula III.
[0016] According to a fourth aspect of the present invention, there is provided a composite, an adhesive, or a coating comprising the sulfur-bridged dimethacrylate compound of Formula I and / or II or the sulfur-bridged diepoxy compound of Formula III.
[0017] According to a fifth aspect of the present invention, there is provided a use of the sulfur-bridged dimethacrylate compound of Formula I and / or II or the sulfur-bridged diepoxy compound of Formula III as a reactive diluent in a curable resin mixture.
[0018] According to a sixth aspect of the present invention, there is provided a method for preparing sulfur-bridged dimethacrylate compound of Formula I, the method comprising the steps ofa) reacting halogenated furfurals according to Formula IV
[0019] O
[0020]
[0021] wherein X is independently Cl, Br or I;
[0022] with sulfur donor
[0023] HS^^OH(V)
[0024] in order to produce a sulfur-bridged compound having Formula VI
[0025]
[0026] b) incubating compound VI obtained in step a) in methanol and subsequently in methanol with added NaBF in order to produce a compound having Formula VII
[0027]
[0028] H° OH (VII);
[0029] c) reacting compound VII obtained in step b) with methacrylic anhydride having formula O O
[0030]
[0031] (VIII)
[0032] in order to produce a compound having Formula (I)
[0033]
[0034] According to a seventh aspect of the present invention, there is provided a method for preparing sulfur-bridged dimethacrylate compound of Formula II, the method comprising the steps of:
[0035] a) reacting halogenated furfurals according to Formula IV
[0036] O
[0037]
[0038] wherein X is independently Cl, Br or I;
[0039] with sulfur donor Na2S in order to produce a sulfur-bridged compound having Formula IX
[0040]
[0041] b) incubating compound IX obtained in step a) in methanol and subsequently in methanol with added NaBFU in order to produce a compound having Formula X
[0042]
[0043] HO OH(X);
[0044] c) reacting compound VII obtained in step b) with methacrylic anhydride having formula O O
[0045]
[0046] According to an eighth aspect of the present invention, there is provided a method for preparing a sulfur-bridged diepoxy compound of Formula III, the method comprising the steps of:
[0047] a) reacting halogenated furfurals according to Formula IV
[0048] O
[0049]
[0050] wherein X is independently Cl, Br or I;
[0051] with sulfur donor
[0052] HS / X^0H(V)
[0053] in order to produce a sulfur-bridged compound having Formula VIO
[0054] S,
[0055] H
[0056]
[0057] OH (VI);
[0058] b) incubating compound VI obtained in step a) in methanol and subsequently in methanol with added NaBHj in order to produce a compound having Formula VII
[0059]
[0060] H0OH (VII);
[0061] c) reacting compound VII obtained in step b) with compound
[0062] Cl
[0063]
[0064] °(XI)
[0065] in order to produce a compound having Formula III
[0066]
[0067] ° ° (in).
[0068] According to a ninth aspect of the present invention, there is provided a sulfur-bridged compound comprising or consisting of a structure of formula
[0069]
[0070] H0\L_7 OH (vii).
[0071] BRIEF DESCRIPTION OF THE DRAWINGS FIGURE 1. Dynamic viscosities of (a) neat BisGMAand dimethacrylate 3 at 55 °C, and (b) commercial VER and neat dimethacrylate 6 at 25 °C.
[0072] FIGURE 2. DSC heat flow vs temperature thermograms of biobased resins (a) 3 and (b) 6, with heating rates of 5, 10, 15, and 20 °C / min.
[0073] FIGURE 3. Activation energies calculated using the Ozawa-Flynn-Wall Method.
[0074] FIGURE 4. (a) First heating and cooling cycles, and (b) second heating and cooling for 3, 6, and commercial VER. Arrows indicate the direction of the temperature change.
[0075] FIGURE 5. Thermogravimetric analysis of cured 3, 6, and commercial VER.
[0076] FIGURE 6. (a) Storage modulus E’, (b) loss modulus E", and (c) tan 3 of cured resins as functions of temperature.FIGURE 7. Stress vs strain curves of (a) 3, (b) 6, and (c) commercial VER.
[0077] FIGURE 8. Weight gain of cured resin samples during water immersion test.
[0078] FIGURE 9 illustrates the methods for synthesis of the sulfur-bridged dimethacrylate compound of Formula I or II and the sulfur-bridged diepoxy compound of Formula III as defined in the claims.
[0079] FIGURE 10. A furfural-based diepoxy according to Formula III and a blend thereof with diglycidyl ether of bisphenol A (DGEB A) were subjected to adhesion studies with DGEBA, 1,6-hexanediol diglycidyl ether (HDDGE) and a blend thereof with DGEB A. Although HDDGE exhibited better compatibility with DGEBA, the neat biobased diepoxy (7) showed 50% higher adhesive strength compared to DGEBA. These results indicate that the synthesized diepoxy (7) can be applied as an adhesive in high-performance applications.
[0080] DEFINITIONS
[0081] “Curable” refers to material that is obtained by irreversibly hardening a soft solid or viscous liquid prepolymer by cross-linking of individual chains of the polymeric substance of the resin under the influence of heat or suitable radiation, often under increased pressure. Preferably, the curable composition is cured by heating, or by UV radiation.
[0082] The invention is further directed to a composite, an adhesive, or a coating comprising at least one said curable sulfur-bridged difuran compounds.
[0083] Composite refers to composite material that comprises at least two components. These components may have notably dissimilar chemical or physical properties and are merged to create a material with properties unlike the individual elements. Within the finished structure, the individual elements remain separate and distinct, distinguishing composites from mixtures and solid solutions.
[0084] Adhesive refers to any composition that is capable of holding materials together by surface attachment that resists separation.
[0085] Unless otherwise clear from context, percentages referred to herein are expressed as percent by weight based on the total composition weight.Unless otherwise stated, properties that have been experimentally measured or determined herein have been measured or determined at room temperature. Unless otherwise indicated, room temperature is 25 °C.
[0086] Unless otherwise stated, properties that have been experimentally measured or determined herein have been measured or determined at atmospheric pressure.
[0087] As used herein, the term “glass transition temperature (Tg)” refers to a temperature range where a polymer changes from a hard, rigid or “glassy” state to a more pliable, compliant or “rubbery” state.
[0088] It must also be noted that, as used in the specification and the appended claims, the singular forms “a,” “an” and “the” include plural referents unless otherwise specified.
[0089] EXPERIMENTAL SECTION
[0090] Materials
[0091] 5 -Bromofurfural (>99%), methacrylic anhydride (MAA, >97%), sodium sulfide hydrate (Na2S, >60%), 2-mercaptoethanol (ME, >98%), diglycidyl ether of bisphenol A (DGEB A, >85%), methacrylic acid (>99.5%), epichlorohydrin (>99%), tetrabutylammonium bromide (>98%), and other commercially available chemicals were used as received. Triethylamine was dried over 4 A molecular sieves and distilled prior to use. 5,5'-Sulfanediyldi(furan-2-carbaldehyde) (1) and [sulfanediyldi(furan-5,2-diyl)]dimethanol (2) were prepared by following previously published methods.18 194-(Dimethylamino)pyridine (DMAP, >99%) was used as a catalyst for methacrylation reactions. Thin-layer chromatography (TLC) was used for monitoring reactions using a mixture of ethyl acetate and hexane (1 : 1) as an eluent.
[0092] Commercial vinyl ester resin (VER) was used as a reference material. It comprised oligomerized bisphenol A epoxy -based dimethacrylate with an average of 3 BPA units and ca. 40 wt% styrene. Methyl ethyl ketone peroxide (MEKP, ~32 wt%) and / c / V-butyl peroxybenzoate served as initiators for curing VER and synthesized biobased dimethacrylate resins, respectively. 4,4’-Diaminodiphenyl sulfone (4,4’-DDS), methylhexahydrophthalic anhydride (MHHPA), and 2-ethyl-4-methylimidazole (EMI) were used as curing agents for the diepoxy resin.Methods
[0093] Synthesis of dimethacrylate 3
[0094] Diol 2 (25.45 g, 112 mmol) and DMAP (0.67 g, 5.4 mmol, 4.8 mol%) were dissolved in MAA (42 mL, 272 mmol, 2.4 equiv) in a 1000 mL round-bottom flask equipped with a magnetic stirring bar and a reflux condenser. The reaction mixture was stirred at 60 °C for 22 h. After cooling, saturated NaHCO3solution (460 mL) was added slowly into the reaction system to prevent excessive foaming, and stirring was continued for 24 h. The reaction mixture was extracted with ethyl acetate (4 x 100 mL), the separated organic phase was dried over anhydrous Na2SO4 and filtered through a silica gel layer. Solvent evaporation yielded a brown waxy solid (41 g, >99%). Mp 45 °C.3H NMR (400 MHz, (CD3)2SO): 3 ppm 1.86 (s, 6H), 5.11 (s, 4H), 5.70 (t, J= 1.5 Hz, 2H), 6.01 (s, 1H), 6.60 (d, J= 3.3 Hz, 2H), 6.80 (d, J= 3.3 Hz, 2H).13C NMR (101 MHz, (CD3)2SO): 3 ppm 18.43, 58.39, 113.43, 118.94, 126.95, 135.88, 142.45, 153.51, 166.46. HRMS (ESI+, TOF) m / z [M + Na]+calculated for Ci8Hi8NaO6S 385.0716, found 385.0720.
[0095] Synthesis of aldehyde 4
[0096] 5 -Bromofurfural (25 g, 141 mmol) and deionized water (130 mL) were mixed in a 1000 mL three-necked flask equipped with a magnetic stirring bar, a reflux condenser, a dropping funnel, and a septum. The reaction mixture was heated to 70 °C under argon. Diethyl ether (10 mL) was added to the reaction flask through the septum using a needle and a syringe. Sodium hydroxide (5.94 g, 149 mmol, 1.05 equiv) was dissolved in deionized water (150 mL), and ME (10.6 mL, 149 mmol, 1.05 equiv) was added to the solution. The reagent solution was transferred to the dropping funnel and added to the heated reaction mixture over 20 min. The reaction mixture was stirred at 70 °C for 1.5 h. After cooling down, the reaction mixture was extracted with ethyl acetate (6 X 80 mL). The separated organic phase was dried over anhydrous Na2SO4 and filtered through a silica gel layer. After solvent evaporation, a brown liquid was obtained as a product (24 g, >99%). ’H NMR (400 MHz, (CD3)2SO): 3 ppm 3.12 (t, J = 6.3 Hz, 2H), 3.62 (dd, J= 6.3, 5.5 Hz, 2H), 5.06 (t, J= 5.5 Hz, 1H), 6.79 (d, J= 3.7 Hz, 1H), 7.57 (d, J= 3.7 Hz, 1H), 9.46 (s, 1H).13C NMR (101 MHz, (CD3)2SO): 3 ppm 36.29, 60.31, 113.98, 153.78, 156.26, 177.10. HRMS (ESI+, TOF) m / z: [M + H]+calculated for C7H8O3S 173.0267, found 173.0265.Synthesis of diol 5
[0097] Aldehyde 4 (24.30 g, 141 mmol) was dissolved in methanol (280 mL) in a 1000 mL roundbottom flask and placed in an ice bath. NaBHj (5.62 g, 141 mmol, 1 equiv) was added to the reaction flask over 25 min. After 1.5 h, methanol was recovered by distillation under reduced pressure and replaced with deionized water (100 mL). The mixture was stirred for 15 min and extracted with ethyl acetate (5 X 50 mL). The organic layer was dried over anhydrous Na2SO4 and filtered through a silica gel layer. Solvent evaporation yielded a dark yellow liquid (23 g, 95%). ’H NMR (400 MHz, (CD3)2SO): d ppm 2.80 (t, J= 6.9 Hz, 2H), 3.53 (dd, J= 6.9, 5.8 Hz, 2H), 4.36 (d, J= 5.8 Hz, 2H), 4.89 (t, J= 5.8 Hz, 1H), 5.27 (t, .7= 5.8 Hz, 1H), 6.30 (d, J= 3.1 Hz, 1H), 6.55 (d, J= 3.1 Hz, 1H).13C NMR (101 MHz, (CD3)2SO): <5 ppm 38.19, 56.26, 60.63, 109.22, 117.74, 144.42, 158.92. HRMS (ESI+, TOF) m / z [M + Na]+calculated for C7Hi0NaO3S+197.0243, found 197.0239.
[0098] Synthesis of dimethacrylate 6
[0099] Diol 5 (23.45 g, 135 mmol) was mixed with MAA (50 mL, 324 mmol, 2.4 equiv) and DMAP (0.80 g, 6.5 mmol, 4.8 mol%) in a 1000 mL round-bottom flask equipped with a magnetic stirring bar and a reflux condenser. The mixture was stirred at 60 °C for 22 h. After cooling to rt, saturated NaHCO3-solution (500 mL) was added slowly in the reaction mixture and stirring was continued for 24 h. The reaction mixture was extracted with ethyl acetate (3 x 100 mL). The separated organic phase was dried over anhydrous Na2SO4, filtered through a silica gel layer, and evaporated to dryness. The product was obtained as a brown liquid (41 g, 97%).XH NMR (400 MHz, (CD3)2SO): d ppm 1.85 (s, 3H), 1.88 (s, 3H), 3.09 (t, J= 6.3 Hz, 2H), 4.24 (t, J= 6.3 Hz, 2H), 5.12 (s, 2H), 5.65-5.70 (m, 2H), 5.69-5.74 (m, 2H), 5.99 (s, 1H), 6.04 (s, 1H), 6.58 (d, J= 3.2 Hz, 1H), 6.65 (d, J= 3.2 Hz, 1H).13C NMR (101 MHZ, (CD3)2SO): 3 ppm 18.36, 18.43, 34.05, 58.41, 63.61, 113.19, 117.97, 126.54, 126.87, 135.95, 136.02, 145.61, 152.81, 166.52, 166.73. HRMS (ESI+, TOF) m / z: [M + Na]+calculated for Ci5Hi8NaO5S+333.0767, found 333.0760.
[0100] Synthesis of epoxy 7
[0101] Diol 5 (7.41 g, 42.5 mmol) was dissolved in epichlorohydrin (47 mL, 503 mmol, 14 equiv) in a 250 mL round-bottom flask equipped with a magnetic stirring bar. TBAB (1.38 g, 4.25 mmol, 0.1 equiv) and KOH (7.16 g, 128 mmol, 3 equiv) were added to the solution, which was then stirred at room temperature for 1 h. The reaction mixture was diluted with ethyl acetate (100 mL) and washed with water and brine. The organic phase was dried overanhydrous Na2SO4 and filtered through a silica gel layer. Solvent evaporation yielded the product as a light brown liquid (11 g, 87%).
[0102] Synthesis ofBisGMA
[0103] DGEBA (38.43 g, 96 mmol), methacrylic acid (24.5 mL, 287 mmol, 3 equiv), and triethylamine (8 mL, 57.4 mmol, 0.6 equiv) were dissolved in DCM (60 mL) in a 250 mL round-bottom pressure flask equipped with magnetic stirring bar. The reaction solution was stirred at 70 °C for 45 h. After cooling, DCM was evaporated from the reaction mixture which was then left to stand at 4 °C overnight. The reaction mixture was dissolved in EtOAc (400 mL) and washed with water (200 mL), saturated NaHCCf-solution (50 mL), and brine (50 mL). The separated organic phase was dried over anhydrous Na2SO4 and filtered through a silica gel layer. After solvent evaporation, a light brown viscous liquid was obtained as a product (49.50 g, >99%).
[0104] Nuclear Magnetic Resonance (NMR) Spectroscopy
[0105] ’H and13CNMR spectra were measured with Bruker Avance 400 spectrometer at ambient temperature using the standard parameters PROTON and C13CPD, respectively. The samples were prepared by dissolving ca. 5 mg of compounds in approximately 0.5 mL of (CDa)2SO, which was then transferred into a 5 mm NMR tube.
[0106] High-Resolution Mass Spectrometry (HRMS)
[0107] The electrospray ionization mass spectrometric measurements were performed using Thermo Scientific Q Exactive Plus Hybrid Quadrupole-Orbitrap high-resolution mass spectrometer. Compound samples (ca. 1 mg / mL in HFIP) were diluted 20-fold with H2O / acetonitrile 1:3 (v / v) mixture, and 30-40 mL of the prepared dilutions were then injected into the mass spectrometer. Compounds 3, 5, and 6 were detected in positive mode as [M + Na]+, whereas compound 4 was detected as positive ion [M + H]+. Solvent system: Solvent A: 0.1% formic acid in H2O, solvent B: 1% formic acid in acetonitrile, A:B 40:60. Flow rate: 0.02 mL / min.
[0108] Dynamic viscosity
[0109] Measurements were done on a Discovery HR-1 rheometer (TA Instruments) with 1.999° cone plate (40 mm diameter) with shear rates between 0.01 and 150 s'1at temperature 25 °C for neat resin 6 and VER, and at 55 °C for neat resin 3 and BisGMA.Curing
[0110] Dimethacrylate 3 was melted at 55 °C in a water bath, blended with 2 wt% tert-butyl peroxybenzoate, and then stirred at 55 °C for 30 min and under vacuum for 15 min. The warm liquid resin was transferred to a silicone mold treated with a releasing agent. The resin in the mold was degassed under vacuum at 70 °C. The vacuum was replaced with argon gas, and the curing reaction was performed at 100 °C for 1 h, 130 °C for 3 h, followed by 150 °C for another 1 h in an oven.
[0111] Dimethacrylate 6 was blended with 2 wt% te / 7-butyl peroxybenzoate, stirred for 30 min and under vacuum for 15 min. The liquid resin was transferred to a silicone mold. Resin was degassed under vacuum, which was then replaced by argon gas. The curing reaction was performed at 100 °C for 1 h, 130 °C for 3 h, and 150 °C for 1 h in an oven. After cooling to room temperature, the samples were removed from the mold for testing.
[0112] For curing, the commercial VER was blended with 1.5 wt% MEKP and stirred for 5 min. The mixture was transferred to a silicone mold and left to cure at room temperature overnight. Samples were then post cured at 130 °C for 2 h.
[0113] Epoxy resin 7 was cured using two different curing methods. Method 1: 4,4’-diaminodiphenyl sulfone (4,4’-DDS) was mixed with monomer 7 in molar ratio 1 : 1 at elevated temperatures. The liquid resin mixture was transferred to a silicone mold. The curing reaction was performed at 110 °C for 2 h, 130 °C for 2 h, and 150 °C for 1 h in an oven. After cooling to room temperature, the samples were removed from the mold for testing. Method 2: Methylhexahydrophthalic anhydride (MHHPA) was mixed with monomer 7 in molar ratio 1 : 1 in the presence of 2-ethyl-4-methylimidazole (1 wt% of the resin mixture). The curing reaction was performed at 110 °C for 2 h, 130 °C for 2 h, and 150 °C for 1 h in an oven. After cooling to room temperature, the samples were removed from the mold for testing.
[0114] Differential Scanning Calorimetry (DSC)
[0115] The curing kinetics of biobased resins were evaluated from the uncured samples containing 2 wt% tert-butyl peroxybenzoate. The samples (ca. 5 mg) were placed in 40 u aluminium pans with a pierced lid and scanned from 25 to 250 °C under N2 flow (50 cm min) with heating rates of 5, 10, 15, and 20 °C / min using a DSC 82 le instrument (Mettler-Toledo). This instrument was also used to determine a melting point for compound 3. The curedresins (ca. 5 mg) were studied with DSC 25 (TA Instruments). The samples were placed in aluminium pans and scanned at 20-250 °C with heating and cooling rates of 10 °C / min under a 50 cm3 / min N2 flow.
[0116] Thermogravimetric Analysis (TGA)
[0117] Thermogravimetry was performed on the cured samples that were crushed into small grains (ca. 15 mg) and placed into AI2O3 crucibles. Measurements were done with a heating rate of 10 °C / min under 40 mL / min N2 flow (Netzsch STA 409 PC / PG). The temperature range of the measurements was 38-700 °C.
[0118] Dynamic Mechanical Analysis (DMA)
[0119] Storage modulus E loss modulus E ”, and tan d were evaluated from rectangular-shaped resin samples (20 x 5 x 1 mm3) using a DMA Q800 (TA Instruments). All runs were performed in a “multifrequency - strain” mode at 1 Hz frequency, 0.08% strain at 28-200 °C or 28-220 °C with a heating rate of 3 °C / min.
[0120] Tensile Testing
[0121] Samples of cured resins were tested with a tensile tester (ZwickRoell, 10 kN load cell). The dogbone-shaped specimens (total length 115 mm, gage length 30 mm, width of narrow section 6 mm, thickness 3 mm) were prepared according to the ASTM D638 Type IV standard.20The reported mechanical results were obtained from three to eight measurements.
[0122] Soxhlet extraction
[0123] A cellulose thimble with a cured resin sample (500-800 mg) inside was placed in a jacketed Soxhlet apparatus, which was then fitted to a 250 mL round-bottom flask, containing dichloromethane (150 mL), and a reflux condenser. The flask was heated using an Al heating block held at 70 °C. After 24 h, the solution was evaporated to dryness, and the remaining extract was weighed and analyzed by1H NMR. The sample that remained in the thimble was dried under vacuum at 100-140 °C, and the weight was compared to the initial weight of the sample.
[0124] Chemical resistance to hot alkali
[0125] Alkali resistance of cured resin specimens (ca. 3 x 3 x 3 mm3, altogether 150-190 mg) was evaluated by immersing them in a 1 M NaOH-solution (2 mL) in a 10 mL reaction tubeequipped with a magnetic stirring bar. The solution was heated to 100 °C and stirred for at least one day. After the exposure, reaction mixture was allowed to cool down, filtered in a Buchner funnel and washed with deionized water (8 mL). The filtrate was extracted with ethyl acetate (5 x 10 mL), and the organic phase was dried over anhydrous Na2SO4 and filtered through a silica gel layer. After solvent evaporation, the product was weighed and analyzed by 'HN R.
[0126] Water absorption
[0127] Cured resin samples (500-800 mg) were immersed in deionized water at room temperature inside sealed glass bottles. After certain time periods, the samples were wiped dry with a paper towel, weighed, and immersed in water again. The results of two to three samples were averaged for each material.
[0128] Results & Discussion
[0129] The synthesis of dimethacrylate 3 was carried out starting from commercial 5-bromofurfural (Figure 9). First, dialdehyde 1 was synthesized using our previously published method with high purity.19The reduction of dialdehyde 1 using our previously published method afforded diol 2 in excellent purity and yield.18The final step, methacrylation of diol 2 was carried out using MAA in the presence of DMAP.
[0130] Dimethacrylate 6 was synthesized through a route similar that of compound 3 (Figure 9). In this case, ME was utilized to produce the sulfur bridge between the furan ring and the aliphatic chain, resulting in monomer 4 in >99% yield. The reduction of aldehyde group of 4 with sodium borohydride afforded diol 5 in excellent yield. And finally, methacrylation of diol 5 afforded compound 6 in excellent yield. In addition, diol 5 could be utilized as a starting material for epoxy synthesis. Reaction of diol 5 with epichlorohydrin resulted in the desired epoxy 7 in high yield.
[0131] Dynamic Viscosity
[0132] The viscosity of dimethacrylate monomers 3 and 6 is important for real-world applications. BisGMAis highly viscous liquid, with reported viscosities of 1200 Pa s at 20 °C22and 593 Pa s at 25 °C23. Difuran-based dimethacrylate 3 is a waxy solid at room temperature.
[0133] However, 3 has a low melting point (DSC: 45 °C), and it melts into a thin oil at ca. 50 °C, making it convenient to handle. According to viscosities measured at 55 °C (Figure la), both 3 and BisGMA showed shear thinning, meaning these materials are non-Newtonianfluids. At higher shear rates, dimethacrylate 3 settled to a dynamic viscosity value of ca.
[0134] 0.1 Pa s, with BisGMA being 40 times more viscous. In contrast, monomer 6 remains as a liquid even at -18 °C. The viscosity of 6 was compared with that of commercial VER containing 40 wt% styrene as a diluent. Both resins exhibited prominent shear thinning (Figure lb), making them non-Newtonian fluids as well. The viscosities of VER and monomer 6 at higher shear rates were around 2.5 and 0.2 Pa s at 25 °C, respectively.
[0135] Resin curing
[0136] Due to the presence of the two terminal reactive double bonds, vinyl ester resins readily undergo free-radical polymerization, forming cross-linked network structures that result in cured thermosets.24Solid resin specimens were prepared by mixing the peroxide initiator tert-butyl peroxybenzoate (2 wt%) with each biobased monomer 3 and 6. The homogeneous mixtures were transferred into silicone molds followed by 5 h thermal curing cycle under an inert atmosphere. The commercial VER was cured in typical fashion at room temperature using MEKP as an initiator, followed by 2 h thermal post curing at 130 °C.
[0137] Differential Scanning Calorimetry
[0138] Non-isothermal DSC was used at four heating rates to study the curing kinetics of the biobased vinyl ester resin systems with tert-butyl peroxybenzoate. The DSC thermograms for curing of resins 3 and 6 at different heating rates are illustrated in Figure 2a-b. In thermogram of resin 3, the endothermic peaks at 50 °C indicate melting, which occurs due to the samples solidifying during transfer into the DSC. To determine the activation energy (Ea), the experimental data was plotted as -In ? vs 1000 / 7p, where represents the heating rate, following the Ozawa-Flynn-Wall method. The resulting linear fits are shown in Figure 3, with the slope of the line considered as m = -1.052 IffR. From this relation, the activation energy can be calculated using eq I25:
[0139]
[0140] where R = 8.314 J mol1K1.
[0141] By this method, the activation energies of resin 3 and 6 were determined to be 88 kJ / mol and 117.2 kJ / mol, respectively. Comparison with literature shows that the results are withinthe same range as the activation energy (108.49 kJ / mol) of an epoxy bisphenol A vinyl ester, dissolved in styrene, reported by Y Nasonov et al.26
[0142] The DSC heating and cooling curves of cured resins are shown in Figure 4. The glass transition temperature (7g) is one of the most important properties of thermosets considering their possible applications. 7gis the temperature or temperature range at which a material transitions from a rigid, glassy state to a more flexible, rubbery state.27It was not possible to determine glass transition temperature of resins 3 and 6 by DSC, indicating high cross-linking density. However, the 7gvalue detected for commercial VER was 113 °C. This aligns with the literature, which generally reports glass transition temperatures for vinyl esters in the range of 110-150 °C.28
[0143] Thermogravimetric analysis
[0144] TGA was used to examine the thermal stability of cured resins under a nitrogen atmosphere. The TGA curves are represented in Figure 5, and the weight loss temperatures Zd5% and Td5o% and residual weight percentage 76oo are shown in Table 1. The commercial VER showed higher thermal stability than biobased resins 3 and 6, as an earlier onset of decomposition (Zd5%) was observed in both cases. The observed 7d5% range from 251 to 285 °C for biobased dimethacrylates is higher than operating temperatures of any practical application thus indicating good thermal stability. The 7d5o% values were above 420 °C for all studied resin systems. Noteworthily, resins 3 and 6 demonstrated a higher residual weight percentage than commercial VER.
[0145] Table 1. TGA of cured resin systems.
[0146] Resin 7
[0147]
[0148] ds% (°C) 7dso% (°C) Rioo (%)
[0149] 3 251 439 34.3
[0150] 6 285 422 25.4
[0151] VER 373 429 9.4
[0152] Dynamic mechanical analysis
[0153] DMA measurements gave the storage modulus (E ’), loss modulus (E ”) and loss factor (tan <5) of the cured networks which are plotted as functions of temperature (Figure 6a-c). Thecross-linking densities were estimated using eq 229
[0154] Er
[0155] Ve =(2) 3RT
[0156] where Errepresents the storage modulus at temperature T, R is the universal gas constant (8.314 J mol'1K'1), and T= Tg+ 30 K. The vecalculated for cured resins are listed in Table 2. The Tgof cured 3 and 6 were 183 °C and 162 °C, respectively, which are significantly higher than that of commercial VER (126 °C). The Tgvalue determined by DSC was 113 °C for VER. Usually DMA gives higher Tgvalues than DSC, as it is more sensitive to glass transition.30,31The storage modulus at 30 °C was approximately same for all samples, but E’ of 3 and 6 decreased much more slowly towards the end temperature than that of VER. At 100 °C, the storage modulus of 3 remained nearly equivalent to that of VER. However, at 150 °C, it was significantly higher due to a considerable decrease in VER’s modulus over this temperature range. In contrast, E ’ of 6 was slightly lower than that of 3 and VER at 100 °C, but at 150 °C, it showed an almost 45-fold increase compared to VER.
[0157] Especially, 3 showed good results maintaining strength without notable deformation until 160 °C, whereas VER began to lose its strength at 110 °C. The cross-linking densities of 3 and 6 are about 6 and 17 times higher, respectively, than that of VER, which contains styrene as a reactive diluent. The tan 3 peak of 6 is very weak and broad, which indicates a very high degree of cross-linking and heterogeneous structure.
[0158] Table 2. DMA of cured vinyl resin systems.
[0159] E’ (GPa)
[0160] Resin Tg(°C) at 30 °C at 100 °C at 150 °C w (mol / m3) 3 183 2.6 1.8 1.1 8.77
[0161] 6 162 2.5 1.4 0.7 23.0 VER 129 2.6 1.8 0.01 1.36Table 3. DSC and DMA of cured epoxy resin 7.
[0162] Curing method 7« from DSC Tgfrom peak of tan 8 Storage modulus (GPa) (°C)
[0163] (°C) ' at 30 °C at 100 °C 1 64 76 1.8 0.0007 2 28 59 1.9 0.01
[0164] Tensile Testing
[0165] Table 4. Tensile test results of cured dogbones.
[0166] Resin Tensile strength (MPa) Elongation at break (%) 3 45.6 4.3 6 15.7 2.3 VER 41.3 4.6
[0167] Tensile test results of the cured 3, 6 and commercial VER are presented in Table 4 and depicted in Figure 7a-c. The test specimens prepared from biobased resin 3 exhibited analogous or slightly higher tensile strength (~46 MPa) compared to VER (~41 MPa). Additionally, their elongation at break values were within a same range, suggesting that these materials offer comparable mechanical performance.
[0168] Chemical resistance
[0169] VERs are well known for their excellent resistance to alkalis, acids, and various solvents, which is a critical property, as VERs are commonly utilized in applications such as chemical storage tanks, where exceptional corrosion resistance is essential. The chemical resistance of the cured resin samples was evaluated using Soxhlet extraction with hot DCM as a solvent. Cured resin sample from 3 partially broke apart but did not discolor the solvent. The mass of the extract after evaporation of the solvent was 0.8% of the original sample mass and the mass loss indicated by the dried resin sample was 1.3%, indicating high gel content. In contrast, cured resin sample from 6 remained intact, with the extraction solvent showing no discoloration and leaving no residue upon evaporation. After prolonged drying, the mass of the resin sample indicated a slight weight gain of 0.3%, most likely due to the resin containing trapped solvent. The commercial VER fractured and cracked duringthe extraction, although the solvent remained colorless. It showed the highest extraction (3.1%) and mass loss (3.8%), indicating inferior chemical resistance compared to the biobased samples.
[0170] To further evaluate chemical stability, samples were immersed in a hot 1 M aqueous NaOH-solution under an argon atmosphere for at least one day. After one day of exposure for cured resin 3, diol 2 was detected from the light brown solution by TLC. After 2 days the specimens had partly disintegrated. After work-up, diol 2 was recovered at 0.8 wt% of the original resin sample 3. Cured resin 6 degraded into small granulates after 2 days, yielding diol 5 at 1.6 wt% of the resin sample.
[0171] Water absorption
[0172] Water absorption in polymeric materials is influenced by both the free volume and the water affinity of the polymer. The free volume depends on the cross-linking density and physical aging, while polymer- water affinity is affected by the presence of hydrogenbonding sites, such as hydroxyl groups. If water is absorbed without causing swelling, it probably remains unbound to the polymer and occupies the voids within the material. On the contrary, when water molecules form hydrogen bonds with polymer chains, they disrupt the interchain hydrogen bonds, leading to swelling and a decline in the physical and mechanical properties of the material.32
[0173] The percent weight change during immersion was calculated using eq 3 :
[0174] z smt- m.
[0175] I(t) = — -l-x100%
[0176]
[0177] rHj
[0178] where I is the absorption intake at time t, mtis the mass of the specimen at time t, and mi is the initial mass of the sample. The results are shown in Figure 8. Within the first week, resins 3, 6, and commercial VER exhibited weight gains of 0.4, 0.5, and 0.8%, respectively. The water uptake of VER leveled off at 1.1% after 4 weeks, while resin 3 took 9 weeks to settle at 0.9%. Resin 6 absorbed water the longest and leveled off at 1.9% after 18 weeks. Overall, the absorption remained very minor across all resin systems, with biobased resins not showing significant deviation from petroleum-based VER.Conclusions
[0179] Two novel furfural-derived sulfur-bridged dimethacrylates and one furfural-derived sulfur-bridged epoxy were successfully prepared in high yields and purity. Difuran-based monomer 3 was a waxy solid at room temperature, but in its liquid state at elevated temperature it showed non-Newtonian behavior with very low viscosity. The unsymmetrical monomer 6, also a non-Newtonian fluid, exhibited a low viscosity already at room temperature, and maintained a liquid state even at sub-ambient temperatures. The epoxy monomer 7 also showed a low viscosity at room temperature. Both dimethacrylates were thermally cured into highly cross-linked solid specimens with excellent 7gvalues of 183 and 162 °C. Similarly, solid specimens were obtained from di epoxy resin through thermal curing using two different methods. The glass transition temperatures for the 7 / 4,4’ -DDS system were found to be 64 (from DSC) and 76 °C (from peak of tan d). For the 7 / MHHPA / EMI system the corresponding values were 28 and 59 °C, respectively. TGA showed lower thermal stabilities for cured biobased vinyl ester resins compared to commercial VER. However, the operational temperatures of typical applications are far lower than observed Tgand 7d5% of biobased dimethacrylates. According to tensile tests, 3 demonstrated comparable or slightly improved mechanical performance compared to VER. In contrast, 6 showed lower tensile strength. Results of chemical stability indicated that both furfural-derived resins offer equal solvent resistance to VER. Water absorption tests showed overall minor water intake (<2 wt%), with bioresins practically not differing from petroleum-based VER. Based on the results, the characterized dimethacrylates are promising alternatives to commercial petrochemical vinyl ester resins.
[0180] FURTHER EXAMPLE
[0181] Adhesion Testing
[0182] Adhesive test specimens were prepared from steel plates (3 mm thick, 20 mm wide). Two plates were glued together with an adhesive-coated area of 10 * 20 mm2. The adhesive contact surfaces were abraded using 80-grit sandpaper at crosswise diagonal (±45°) directions. The plates were washed with liquid detergent, rinsed with deionized water and acetone, and thoroughly dried. The adhesive layer thickness was controlled to 0.15 mm using thin aluminum shims coated with a release agent. The degassed resin adhesive mixture was applied to both steel surfaces, which were then gently pressed together. The total length of the assembled specimen was approximately 18 cm. Curing was performed ina hot press machine under a constant force of 20 kN at 110 °C for 1 h, 130 °C for 2 h, 150 °C for 1 h, and 180 °C for 2 h. Lap shear strength tests on adhesive test specimens were performed similarly to the tensile tests, with three to six replicate samples.
[0183] Results
[0184] As shown in Figure 10, HDDGE as a reactive diluent in the MHHPA-cured DGEBA systems (DGEBA / HDDGE20) gave adhesive strength of 35.8 MPa showing a 40% improvement compared to DGEBA without a diluent (25.4 MPa), whereas di epoxy 7 (DGEBA / 720) had little effect (23.4 MPa). In contrast, the neat diluents cured with MHHPA exhibited markedly different behavior: Diepoxy 7 gave adhesive strength of 38.5 MPa, over 50% higher than DGEBA alone, whereas HDDGE showed a very low adhesive strength of less than 5 MPa.
[0185] While HDDGE improved adhesive strength in DGEBA formulation, neat MHHPA-cured resin 7 showed substantially higher adhesive strength than DGEBA demonstrating the strong potential of diepoxy 7 to act as a biobased, low-viscosity adhesive. These results show that furfural -based diepoxy 7 is a promising biobased reactive diluent for epoxy systems.REFERENCES
[0186] (1) Yadav, S. K.; Schmalbach, K. M.; Kinaci, E.; Stanzione, J. F.; Palmese, G. R. Recent Advances in Plant-Based Vinyl Ester Resins and Reactive Diluents. EurPolym J 2018, 98, 199-215. https: / / doi.Org / 10.1016 / J.EURPGLYMJ.2017.11.002.
[0187] (2) Zhang, X.; Wu, J.; Wei, J.; Qin, Z.; Pan, Y. T.; Wu, X.; Zhang, W.; Yang, R. High- Performance Biobased Vinyl Ester Resin and Its Fiberglass-Reinforced Composite with High Glass Transition Temperature (Tg), Excellent Flame Retardancy and Mechanical Properties. Polym Degrad Stab 2023, 207, 110209. https: / / doi.Org / 10.1016 / J.PGLYMDEGRADSTAB.2022.110209.
[0188] (3) Zhao, Y. Z.; Chu, Y.; Xu, Y. J.; Zhu, P.; Wang, Y. Z. Highly Flame-Retardant Vinyl Ester Resins with Well-Balanced Comprehensive Performance. Chemical Engineering Journal 2023,464, 142659. https: / / doi.Org / 10.1016 / J.CEJ.2023.142659.
[0189] (4) Bednarczyk, P.; Irska, L; Gziut, K.; Ossowicz-Rupniewska, P. Synthesis of Epoxy Methacrylate Resin and Coatings Preparation by Cationic and Radical Photocrosslinking. Molecules 2021, Vol. 26, Page 76632021,26 (24), 7663. https: / / doi.org / 10.3390 / MOLECULES26247663.
[0190] (5) Can, E.; Kinaci, E.; Palmese, G. R. Preparation and Characterization of Novel Vinyl Ester Formulations Derived from Cardanol. EurPolym J 2015, 72, 129-147. https: / / doi.Org / 10.1016 / J.EURPGLYMJ.2015.09.010.
[0191] (6) Zhang, N.; Cui, X.; Wang, C.; Wu, S.; Zhao, Y; Qi, Y.; Hou, X.; Jin, H.; Deng, T.
[0192] Degradation of Vinyl Ester Resin and Its Composites via Cleavage of Ester Bonds to Recycle Valuable Chemicals and Produce Polyurethane, l / l / aste Management 2023, 755, 260-268. https: / / doi.Org / 10.1016 / J.WASMAN.2022.11.010.
[0193] (7) Bassett, A. W.; La Scala, J. J.; Stanzione III, J. F.; Appl Polym Sci, J.; Baroncini, E. A.;
[0194] Kumar Yadav, S.; Palmese, G. R.; Ogale, A. A.; Zhang, M.; Jin, J.; Appl, J.; DeBolt, M.; Kiziltas, A.; Mielewski, D.; Waddington, S.; Nagridge, M. J.; Rostagno, M.; Price, E. J.; Pemba, A. G.; Ghiriviga, L; Abboud, K. A.; Miller, S. A.; Rowe, M. D.; Eyiler, E.; Walters, K. B.; Rogers, D. P.; Sadler, J. M.; Wool, R. P.; ChengTeo, S.; Ngoc Uy Lan, D.; LengTeh, R; Quan Ngoc Tran, L.; Zhan, M.; Maiorana, A.; Yue, L.; Manas-Zloczower, L; Gross, R.; Garrison, M. D.; Harvey, B. G.; Masser, K. A.; Knorr Jr, D. B.; Yu, J. H.; Hindenlang, M. D.; Lenhart, J. L. The Effect of Impurities in Reactive Diluents Prepared from Lignin Model Compounds on the Properties of Vinyl Ester Resins. J Appl Polym Sci 2016, 133 (45). https: / / doi.Org / 10.1002 / APP.43817.
[0195] (8) Perez-Mondragon, A. A.; Cuevas-Suarez, C. E.; Gonzalez-Lopez, J. A.; Trejo-Carbajal, N.; Melendez-Rod riguez, M.; Herrera-Gonzalez, A. M. Preparation and Evaluation of a BisGMA-Free Dental Composite Resin Based on a Novel Trimethacrylate Monomer. Dental Materials 2020, 36 (4), 542-550. https: / / doi.Org / 10.1016 / J.DENTAL.2020.02.005.
[0196] (9) Cappelli, F.; Carnazza, G.; Vellucci, P. Crude Oil, International Trade and Political Stability: Do Network Relations Matter? Energy Policy 2023, 176, 113479. https: / / doi.Org / 10.1016 / J.ENPOL.2023.113479.(10) Amidon, T. E.; Liu, S. Water-Based Woody Biorefinery. Biotechnol Adi / 2009, 27(5), 542-550. https: / / doi.Org / 10.1016 / J.BIOTECHADV.2009.04.012.
[0197] (11 ) Mattlar, T.; Ekholm, T. The Impact of Bioplastics Production on Climate Change Mitigation, Fossil Fuels and Land-Use. Renewable and Sustainable Energy Reviews 2025,272, 115234. https: / / doi.Org / 10.1016 / J.RSER.2024.115234.
[0198] (12) Catrinck, M. N.; Barbosa, P. S.; Filho, H. R. O.; Monteiro, R. S.; Barbosa, M. H. P.; Ribas, R. M.; Teofilo, R. F. One-Step Process to Produce Furfural from Sugarcane Bagasse over Niobium-Based Solid Acid Catalysts in a Water Medium. Fuel Processing Technology 2020, 207, 106482. https: / / doi.Org / 10.1016 / J.FUPROC.2020.106482.
[0199] (13) Bao, Y.; Du, Z.; Liu, X.; Liu, H.; Tang, J.; Qin, C.; Liang, C.; Huang, C.; Yao, S. Furfural Production from Lignocellulosic Biomass: One-Step and Two-Step Strategies and Techno-Economic Evaluation. Green Chemistry 2024, 26 (11), 6318-6338. https: / / doi.Org / 10.1039 / D4GC00883A.
[0200] (14) Gandini, A.; Belgacem, M. N. Furans. Handbook of Thermoset Plastics 2014, 93-110.
[0201] https: / / doi.Org / 10.1016 / B978-1 -4557-3107-7.00005-1.
[0202] (15) Gandini, A.; Belgacem, M. N. Furans in Polymer Chemistry. Prog Polym Sci 1997, 22 (6), 1203-1379. https: / / doi.Org / 10.1016 / S0079-6700(97)00004-X.
[0203] (16) Bouzidi, K.; Chaussy, D.; Gandini, A.; Bongiovanni, R.; Beneventi, D. Development of Biomass-Based Slurry for the Manufacture of Furan / Cellulose Composite by Cast Moldingand 3D Printing. Journal of Polymer Science 2023, 67 (17), 2060-2075. https: / / doi.org / 10.1002 / PGL.20230074.
[0204] (17) Rivero, G.; Fasce, L. A.; Cere, S. M.; Manfredi, L. B. Furan Resins as Replacement of Phenolic Protective Coatings: Structural, Mechanical and Functional Characterization. Prog OrgCoat 2014, 77(1), 247-256.
[0205] https: / / doi.Org / 10.1016 / J.PORGCOAT.2013.09.015.
[0206] (18) Terho, R. A.; Kainulainen, T. P.; Salonen, M. A.; Sirvib, J. A.; Heiskanen, J. P. Renewable Furfural-Based Sulfur-Bridged Epoxy Resins with Excellent Adhesive Properties.
[0207] Macromolecules 2024, 57 (22), 10735-10744.
[0208] https: / / d0i.0rg / l 0.1021 / acs.macromol.4c01000.
[0209] (19) Ahmed, A. M.; Kainulainen, T. P.; Sirvib, J. A.; Heiskanen, J. P. Renewable Furfural- Based Polyesters Bearing Sulfur-Bridged Difuran Moietieswith High Oxygen Barrier Properties. Biomacromolecules 2022, 23 (4), 1803-1811. https: / / doi.org / 10.1021 / acs.biomac.2c00097.
[0210] (20) ASTM International. Standard Test Method forTensile Properties of Plastics; ASTM D638-22; West Conshohocken, PA, 2022.
[0211] (21) Pereira, S. G.; Nunes, T. G.; Kalachandra, S. Low Viscosity Dimethacrylate Comonomer Compositions [Bis-GMA and CH3Bis-GMA] for Novel Dental Composites; Analysis of the Network by Stray-Field MRI, Solid-State NMR and DSC & FTIR. Biomaterials 2002, 23 (18), 3799-3806. https: / / doi.Org / 10.1016 / S0142-9612(02)00094-7.(22) Zhang, Y.; Li, Y.; Thakur, V. K.; Gao, Z.; Gu, J.; Kessler, M. R. High-Performance Thermosets with Tailored Properties Derived from Methacrylated Eugenol and Epoxy- Based Vinyl Ester. Polym / nt2018, 67 (5), 544-549. https: / / doi.org / 10.1002 / PI.5542. (23) Sultania, M.; Rai, J. S. P.; Srivastava, D. Studies on the Synthesis and Curing of Epoxidized Novolac Vinyl Ester Resin from Renewable Resource Material. Eur PolymJ 2010,46(10), 2019-2032. https: / / doi.Org / 10.1016 / J.EURPGLYMJ.2010.07.014.
[0212] (24) Arhangel'skii, IgorV., Dunaev, Alexander V., Makarenko, Irina V., Tikhonov, Nikolay A.
[0213] and Tarasov, Andrey V. (2013). Non-lsothermal Kinetic Methods: Workbookand Laboratory Manual. Berlin: Max-Planck-Gesellschaft zur Fbrderungder Wissenschaften.
[0214] (25) Nasonov, Y.; Safonov, A.; Gusev, S.; Akhatov, I. Effect of Additives on Cure Kinetics of Pultrusion Resins. Procedia Manuf 2020, 47, 920-924. https: / / doi.Org / 10.1016 / J.PRGMFG.2020.04.283.
[0215] (26) Ebnesajjad, S. Introduction to Plastics. Chemical Resistance of Engineering Thermoplastics 2016, xiii-xxv. https: / / doi.org / 10.1016 / B978-0-323-47357-6.00021-0. (27) Sadler, J. M.; Nguyen, A. P. T.; Toulan, F. R.; Szabo, J. P.; Palmese, G. R.; Scheck, C.;
[0216] Lutgen, S.; La Scala, J. J. Isosorbide-Methacrylate as a Bio-Based Low Viscosity Resin forHigh Performance ThermosettingApplications. J Mater Chem A Mater 2013, 1 (40), 12579-12586. https: / / doi.Org / 10.1039 / C3TA12918G.
[0217] (28) Zhao, Y. Z.; Chu, Y.; Xu, Y. J.; Zhu, P.; Wang, Y. Z. Highly Flame-Retardant Vinyl Ester Resins with Well-Balanced Comprehensive Performance. Chemical Engineering Journal 2023,464, 142659. https: / / doi.Org / 10.1016 / J.CEJ.2023.142659.
[0218] (29) Foreman, J.; Sauerbrunn, S. R.; Marcozzi, C. L. Exploring the Sensitivity of Thermal Analysis Techniques to the Glass Transition; TA Instruments, Inc.: New Castle, DE, USA; Available online: http: / / tainstruments.com / pdf / literature / TA082.pdf (accessed on 16 May 2025)
[0219] (30) Whitcomb, K. Measurement of Glass Transition Temperatures by Dynamic Mechanical Analysis and Rheology; TA Instruments, Inc.: New Castle, DE, USA; Available online: https: / / www.tainstruments.com / pdf / literature / RH100.pdf (accessed on 16 May 2025) (31) Abdelkader, A. F.; White, J. R. Water Absorption in Epoxy Resins: The Effects of the Crosslinking Agent and Curing Temperature.2005. https: / / doi.org / 10.1002 / app.22400.
Claims
CLAIMS1. A sulfur-bridged dimethacrylate compound comprising or consisting of a structure of formula2. A sulfur-bridged diepoxy compound comprising or consisting of a structure of formula3. A curable resin composition comprising the sulfur-bridged dimethacrylate compound according to claim 1 or the sulfur-bridged diepoxy compound according to claim 2.
4. The curable resin composition according to claim 3, wherein the composition comprises the sulfur-bridged dimethacrylate compound according to claim 1 and the composition is cured by heating, by peroxide initiators, or by UV radiation.
5. The curable resin composition according to claim 3, wherein the composition comprises the sulfur-bridged diepoxy compound according to claim 2 and the composition is cured by heating, by anhydrides, by carboxylic acids, or by amine curing agents.
6. A composite, an adhesive, or a coating comprising the sulfur-bridged dimethacrylate compound according to claim 1 or the sulfur-bridged diepoxy compound according to claim 2.
7. Use of the sulfur-bridged dimethacrylate compound according to claim 1 or the sulfur-bridged diepoxy compound according to claim 2 as a reactive diluent in a curable resin mixture.
8. Method for preparing sulfur-bridged dimethacrylate compound of Formula I, the method comprising the steps of:a) reacting halogenated furfurals according to Formula IVA ,oxH(IV)wherein X is independently Cl, Br or I;with sulfur donorin order to produce a sulfur-bridged compound having Formula VIOH (VI);b) incubating compound VI obtained in step a) in methanol and subsequently in methanol with added NaBFU in order to produce a compound having Formula VII■Sc) reacting compound VII obtained in step b) with methacrylic anhydride having formula o Qin order to produce a compound having Formula (I)S9. Method for preparing sulfur-bridged dimethacrylate compound of Formula II, the method comprising the steps of:a) reacting halogenated furfurals according to Formula IVowherein X is independently Cl, Br or I;with sulfur donor Na2S in order to produce a sulfur-bridged compound having Formula IXb) incubating compound IX obtained in step a) in methanol and subsequently in methanol with added NaBFU in order to produce a compound having Formula XHO' 'L_yOH(X);c) reacting compound VII obtained in step b) with methacrylic anhydride having formula O O10. Method for preparing a sulfur-bridged diepoxy compound of Formula III, the method comprising the steps of:a) reacting halogenated furfurals according to Formula IVOwherein X is independently Cl, Br or I;with sulfur donorin order to produce a sulfur-bridged compound having Formula VIz°\^Sw / T OH (VI);b) incubating compound VI obtained in step a) in methanol and subsequently in methanol with added NaBFU in order to produce a compound having Formula VIIOH (VII);c) reacting compound VII obtained in step b) with compoundCl° (XI)in order to produce a compound having Formula IIIs0(HI).
11. A sulfur-bridged compound comprising or consisting of a structure of formulaOH (VII).