Arc discharge deposition system containing a double-anode configuration
The double-anode arc discharge system effectively filters byproducts and enhances plasma density, addressing the issues of sp3/sp2 ratio and deposition rate in DLC coatings, achieving high-quality coatings with improved mechanical properties and reduced complexity.
Patent Information
- Application Number
- PCT/IB2026/054479
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-19
AI Technical Summary
Existing arc discharge systems for depositing Diamond-like Carbon (DLC) coatings suffer from high byproduct generation, which affects the sp3/sp2 ratio and deposition rate, leading to poor coating quality and increased system complexity.
A double-anode configuration with a second anode connected to a capacitance, filtering byproducts and enhancing plasma density, combined with a synchronized charging and discharging system to maintain high deposition rates and sp3/sp2 ratio.
The system achieves high sp3/sp2 ratios and deposition rates with reduced byproduct generation, resulting in high-quality DLC coatings with enhanced mechanical properties and simplified system architecture.
Smart Images

Figure IB2026054479_19112026_PF_FP_ABST
Abstract
Description
Arc discharge deposition system containing a double-anode configurationTechnical domain
[0001] The invention relates to a method and system for the deposition of various coating materials, such as Diamond-like carbon (DLC), on target materials and / or parts. Specifically, the invention is in the technical field of arc discharge, where a laser pulse, a spark, or another ignition source triggers an electrical arc between a target (the cathode) and a nearby anode, and plasma is transported from cathode to substrate.Related art
[0002] Mechanical parts are often coated to enhance their properties. Several methods are known in the art for the deposition of coating material such as plasma-enhanced chemical vapor deposition (PECVD), magnetron sputtering, pulsed laser deposition (PLD), ion beam deposition, and cathodic arc deposition. The choice of the deposition method is typically guided by the desired film properties such as prioritizing ID / IG ratio and / or coating morphology and / or deposition rate and / or costs. Laser-induced arc discharge is already known and used for its high efficiency and quality of deposition.
[0003] Among different coating materials, DLC coatings are widely used across different industry sectors due to their exceptional mechanical, tribological and physical / chemical properties. Such coatings are used to enhance said properties of materials regularly used in large scale manufacturing such as metals, ceramics, glass and semiconductors, while maintaining manufacturing costs at a reasonable level.
[0004] Generally, coated parts exhibit higher hardness, lower friction coefficients, excellent wear resistance, a high degree of chemical inertness,SNANOC-9-PCTand higher thermal conductivity, making them suitable for applications in cutting and drilling tools, automotive components, medical implants and electronic devices.
[0005] DLC coatings consist of a mix between carbon atoms bonded in sp2 and sp3 hybridizations. In particular, the sp3 bonded atoms form a tetrahedral structure similar to the one observed in diamonds. Such sp3 hybridization is primarily responsible for the desirable properties of the coating material. In contrast, sp2 bonded atoms present a structure similar to graphite. When present in excess, sp2 bonded atoms may result in high electrical conductivity and poor mechanical performance of the coating material.
[0006] Therefore, the ratio of sp3 to sp2 material is a critical parameter to characterize the structural and functional quality of the DLC coating. Commonly, such ratio can be estimated by means of Raman spectroscopy according to known methods such as the one described by A. C. Ferrary and J. Robertson in https: / / doi.org / 10.1098 / rsta.2004.1452 (incorporated herein in its entirety as reference).
[0007] In a Raman spectrum of a DLC material using an excitation wavelength such as 480 nm, 514.5 nm or 532 nm, the relative intensities of the D and G bands Raman peaks (approximately at 1360 cm-1 and 1580 cm-1, respectively), and the position and broadening of the G band are used to extract information relevant to the ratio of sp2 to sp3 material, commonly referred to as ID / IG ratio, and structural information of the DLC coating material. Generally, higher values of the ID / IG ratio indicate DLC coating material containing a higher sp2-to-sp3 ratio.
[0008] Further characterization techniques such as electron energy loss spectroscopy (EELS) and X-ray photoelectron spectroscopy (XPS) may also be used to provide further insights into the sp2-to-sp3 ratio and morphology of the analyzed coating material such as grain sizes and film homogeneity.SNANOC-9-PCT
[0009] In recent years, arc discharge techniques have been employed to produce DLC coating materials with a high content of spa materials, that is, presenting a low ID / IG ratio, typically about 0.3. This technique further provides the advantages of high homogeneity and cost-effectiveness in the coating of a large volume of materials and / or parts. Recent advancements in DLC coating material properties with such low ID / IG ratio have enabled the mass production of precise machining parts such as PCB drill bits with diameters below 0.5 mm with exceptional mechanical properties and extended service life.
[0010] The quality of the DLC coating is heavily affected by the generation of byproducts such as macro- and nano-particles, debris, droplets and neutral species, all originating from the ablation of the graphite target material during the generation of a carbon rich plasma by the arc ignition and discharge. Such byproducts, if not filtered effectively, will affect negatively the properties of the resulting DLC coating material.
[0011] To mitigate this issue, the arc discharge system can further incorporate filtering mechanisms, such as magnetic and / or electrostatic filtering systems involving the use of magnetic and / or electric fields to change the direction of the desired carbon ion flow in a controlled way through a bending portion of said system. When passing through this filtering, byproducts will not follow the ion flow, thereby ensuring that a substantial portion of such byproducts does not reach the area where the DLC is deposited on a material and / or part. However, the use of any type of electromagnetic bending filters cause intensity and energy losses of carbon ion flux, resulting in lower deposition rate and lower spa ratio.
[0012] EP355338A1 discloses an apparatus and method for surface processing. It makes use of a plurality of coating equipment, one of which may be a laser ablation ion source. In this configuration, a bent duct that links said source to the deposition chamber is used to filter unwanted byproducts. It utilizes a combination of change in ion flow direction viaSNANOC-9-PCTmagnetic and electrostatic forces to reduce the concentration of unwanted byproducts that reach the region where the DLC is deposited on a target.
[0013] Although managing to produce DLC coating materials exhibiting ID / IG ratios as low as 0.33, as shown by X. Rao et. all., https: / / doi.Org / 10.1016 / j.bioactmat.2020.02.009 (incorporated herein in its entirety as reference), the use of curved ducts and magnetic / electric fields for filtering byproducts results in a system with high complexity.
[0014] Furthermore, due to the extended path length of the filtered carbon ions, a high bias voltage is typically required to maintain deposition efficiency and good adhesion of the DLC material. Such high bias voltage can lead to undesired electrical discharges or arcing near the materials and / or parts to be coated, which, in turn, can severely damage the deposited DLC film, resulting in poor coating properties and morphology.
[0015] While such systems generally result in DLC coating materials presenting a lower ID / IG rate, curved ducts are prompt to scattering, collisions, and energy dissipation of the generated carbon ions, resulting in reduced deposition rates. Such curved duct geometry also increases the ion path length, reducing significantly the plasma energy and generally resulting in lower deposition rates. Furthermore, contamination of the DLC can still occur by re-sputtered materials that accumulate on the surface of the curved duct and / or byproducts that collide with the surface of the duct elastically.Short disclosure of the invention
[0016] The inventors have found that, In DLC deposition, the production of unwanted byproducts is strongly related with the distance between anode and cathode and that this parameter has a profound influence on the sp3 ratio. At distances less that 150 mm carbon (graphite) clusters are undesirably abundant, while the flux of carbon ions becomes unpractically low at distances beyond 350 mm. The plasma flux intensity also plays anSNANOC-9-PCTimportant role, in that excess plasma flux may lead to an overheating of the sample which results in degradation of sp3 ratio.
[0017] The improved disposition of the invention provides a complete solution with a simple geometry that can be optimized to reduce energy losses and provide an optimal intensity of carbon ions at the sample avoiding overheating of the latter, which yields high sp3 ratios and deposition rates of the resulting DLC coatings.
[0018] Hence, the invention is suitable, among other purposes, for the creation of DLC coating specifically, hydrogen-free DLC with a very high fraction of sp3(diamond-like) bonds, also known under the denomination ta-C or Tetrahedral amorphous carbon coating. Such films behave closer to diamond than other DLC types, are extremely hard and wear-resistant, have low friction and withstand higher temperatures than hydrogenated DLC.
[0019] The inventive deposition system overcomes the shortcomings and limitations of the state of the art. More specifically, an aim of the invention is the provision of an effective and reliable technique of filtering unwanted by products generated during a laser-induced arc discharge, while maintaining a simplified and compact system architecture particularly suited for robust operation and manufacturing efficiency.
[0020] Another aim of the present invention is the provision of DLC deposition system that is configured to provide a DLC coat demonstrating an ID / IG ratio below 0.3, or better below 0.25 when measured by Raman spectroscopy, which is signature of high quality ta-C films.
[0021] According to the invention, these aims are attained by the object of the attached claims, and especially by the independent claims.
[0022] In particular, these aims are attained by the provision of a system for coating materials and / or parts with Diamond-like Carbon (DLC), theSNANOC-9-PCTsystem comprising a deposition chamber and an induced arc discharge coating equipment for depositing DLC on said materials and / or parts contained within said deposition chamber, wherein said system further comprises:a target serving as a cathode;a first anode spaced from the cathode to define an arc discharge path and connected to a first capacitance;one or more laser sources configured to initiate a plasma arc discharge along the arc discharge path;a second anode spaced from the first anode and connected to a second capacitance, wherein the first and second anode are arranged so that an ion propagation path is formed from said target material towards said deposition chamber, and wherein an electrical discharge of the second anode occurs when the plasma arc discharge between the cathode and first anode is present, and wherein the first and / or the second anode is configured to filter macro- and nanoparticles, debris, droplets and neutral species;a holder positioned within said deposition chamber configured to hold the materials and / or parts to be coated and connected to a third capacitance, wherein the holder is positioned within said ion propagation path.
[0023] These aims are further attained by the provision of a deposition method for the DLC coating of materials and / or parts using the system, the method comprising the steps of:A. placing materials and / or parts to be coated being held by a holder within said deposition chamber;SNANOC-9-PCTB. providing a target material as a cathode;C. providing a vacuum within the deposition chamber;D. providing a first, a second and a third capacitance to said first and second anodes, and said holder, respectively;E. irradiating said target material as a cathode with one or more laser pulses from one or more laser sources, or use another ignition device to initiate a plasma arc discharge between the cathode and first anode, thereby triggering a current discharge pulse from said first, second and third capacitances and creating a plasma;F. transporting said plasma to the deposition chamber, wherein a bias voltage between said first and second anodes and said holder accelerates ions towards said materials and / or parts to be coated;G. coating said materials and / or parts with Diamond-like Carbon (DLC);H. repeating the steps D. to G. until a Diamond-like Carbon (DLC) coating is formed on said materials and / or parts with a specified thickness.
[0024] The provision of a first and a second anode, each being connected to a first and second capacitance, provides for an extended region in which the arc discharge occurs and generates plasma containing carbon ions. The discharge of the second anode connected to a second capacitance is triggered whenever the first anode provides for an initial arc discharge between the first anode and the cathode, said initial arc discharge being triggered by one or more laser pulses from one or more laser sources.SNANOC-9-PCT
[0025] In comparison to a single anode configuration, such extended region in which the arc discharge occurs from the first and second anode contains a plasma with a higher density of carbon ions, a more uniform distribution of carbon ions, and a larger volume of plasma that contains said ions. Importantly, since the discharge of the second anode occurs in a region farther from the cathode, namely, farther from the source of carbon, the generation of the plasma with improved characteristics within the extended region is achieved without a corresponding increase in the production of the unwanted by products.
[0026] Remarkably, comparatively with a single anode configuration, the incorporation of the second anode has been shown to reduce the threshold in the laser power required to create the initial arc discharge between the first anode and the cathode.
[0027] In a possible embodiment, by providing the second anode, it becomes possible to create the initial arc discharge with a reduced laser power, for example a laser power reduced by at least a factor of two to three.
[0028] Furthermore, and remarkably, comparatively with a single anode configuration, the incorporation of the second anode has been shown in some embodiments to enhance the achievable DLC deposition rate by a factor larger than two, said enhanced DLC deposition rate being the result of the creation of the plasma with improved characteristics within the extended region.
[0029] In a possible embodiment, the second power supply is set to charge the second capacitance to a maximum voltage that is higher than the maximum voltage of the first capacitance. This voltage difference creates an electric potential between the first and second anodes that further facilitates the flux of ions away from the cathode region along the ion propagation path.SNANOC-9-PCT
[0030] In another possible embodiment, the first, second, and third power supplies provide for a synchronous pulsed cycle of charging and discharging of the first, second and third capacitances. This synchronous operation assures a high degree of precision and reproducibility in the generation of the plasma and conduction of the ion flow towards the materials and / or parts to be coated. This, in turn, results in a reliable growth rate of the DLC coating within individual cycles, as well as in a DLC coating with reliable properties such as sp3 content and optimum morphology.
[0031] The first and / or second anode is configured to filter by products such as macro- and nano-particles, debris, droplets and neutral species. This is achieved by the first and / or the second anode being provided with a specific geometry and shape, and with a specific spatial position and arrangement relative to the cathode and the holder, which results in the filtering of unwanted byproducts by trapping macro- and nano-particles, debris, droplets and neutral species whose trajectories deviate from the ion propagation path.
[0032] In a possible embodiment, the ion propagation path is straight. The straight ion propagation path is defined by the relative position and arrangement of the cathode, the first and second anodes, and the holder, said components being coaxially, and / or centrally, and / or symmetrically, and / or axially aligned depending on their specific geometries. This provides for further simplification of the deposition system architecture, enabling a more compact system configuration.
[0033] The system is configured to provide a Diamond-like Carbon (DLC) coating deposited on a substrate, wherein the coating, when analysed with Raman spectroscopy using an excitation wavelength such as 480 nm, 514.5nm or 532 nm, exhibits a D peak signal and a G peak signal, the ratio of the intensity of the D peak signal and a G peak signal being - < 0.25.SNANOC-9-PCT
[0034] The inventive system and method are highly suitable for the deposition of DLC layers, and in this case the target cathode will be preferably made of graphite or another carbon-rich material. However, the invention is not limited to his special coating and may be usefully employed in the deposition of other materials, for example using cathodes containing nitrides, such as TiN and CrN, to deposit a thin layer of a corresponding composition, on materials and / or parts. In all cases, the inventive disposition of two tandem anodes along the ion propagation path provides a high current, fast deposition rates, and limits unwanted byproducts.
[0035] Remarkably, controlled experiments have proven that the installation of the second anode downstream the first anode procured an increase in the deposition rate between 50% and 70%, and this was not combined with an increase of macro particles and droplets in the beam. This is in stark contrast with most known beam filtering systems, be they electromagnetic, magnetic or mechanical, that invariably reduce the deposition rate. This favourable effect is attributed, without being limited by the theory, to a superior potential distribution between cathode, first anode, and second anode.
[0036] The Laser ignition method has proved to be preferable for the realization of the invention, since it combines high repetition rates with a long cathode life, and the present disclosure will show an embodiment of this nature, as example. However, the invention is not so limited, and encompasses all possible ignition methods, including electric sparks.Short description of the drawings
[0037] Exemplar embodiments of the invention are disclosed in the description and illustrated by the drawings in which:Figure 1 illustrates schematically one possible implementation of the laser-induced arc discharge coating equipment according to the invention.SNANOC-9-PCTFigure 2 illustrates schematically one possible implementation of the system for coating materials and / or parts with Diamond-like Carbon (DLC) according to the invention, configured to coating said materials and / or parts with Diamond-like Carbon (DLC) according to the method of the invention.Figure 3 offers a schematic view of the first anode.Figure 4A and Figure 4B illustrate different schematic views of one possible implementation of the second anode.Figure 5 illustrates a schematic time diagram of the values of current, voltage, capacitance and laser irradiance of different components according to the system of the invention, said time diagram representing multiple / repeated deposition cycles according to the method of the invention.Figure 6 illustrates schematically one possible implementation of a holder that is rotatably positioned and shielded from the carbon ion flux.Examples of embodiments of the present invention
[0038] With reference to Figure 1, the schematic illustration of one preferable embodiment portraits the laser-induced arc discharge coating equipment 8 including a cathode 1, a first anode 33a, a second anode 33b, which are arranged so that an ion propagation path 6 is formed, and a laser source 2 configured to irradiate the cathode 1 with laser light 2a.
[0039] In this preferable embodiment, the cathode 1 and the first anode 33a are operatively connected to a first power supply 5a and a first capacitance 4a, said first capacitance 4a being configured to deliver a current discharge pulse between the cathode 1 and the first anode 33a.SNANOC-9-PCT
[0040] Further, in this preferable embodiment, the cathode 1 and the second anode 33b are operatively connected to a second power supply 5b and a second capacitance 4b, said second capacitance 4b being configured to deliver a current discharge pulse between the second anode 33b and the first anode 33a and / or the cathode 1 , thereby providing for an extended region in which the arc discharge occurs and generates plasma containing carbon ions.
[0041] In a typical embodiment, the first capacitance 4a is charged by the first power supply 5a to a minimum value of 100 V and a maximum value of 400 V, with the first capacitance 4a having a minimum value of 2000 pF, and the second capacitance 4b is charged by the second power supply 5b to a minimum value of 150 V and a maximum value of 450 V, with the second capacitance 4b having a minimum value of 600 pF.
[0042] Preferably, in a typical embodiment, the voltages to which the first 4a and second 4b capacitances are charged differ by at least 50 V, with the voltage of the second capacitance 4b being higher, which provides for a facilitated flux of ions away from the cathode 1 along the ion propagation path 6.
[0043] Advantageously, the first power supply 5a and the second power supply 5b provide for the charging of the first capacitance 4a and second capacitance 4b, respectively, only within the time where, during a deposition cycle of DLC according to the invention method, current discharge is absent within the coating equipment.
[0044] More advantageously, the first power supply 5a and the second power supply 5b each are equipped with switches and / or electronic protection mechanisms (not shown in Figure 1 for simplicity) that electrically disconnect and / or shield said first power supply 5a and said second power supply 5b from their corresponding electronic circuits during the time where, during a deposition cycle of DLC according to theSNANOC-9-PCTinvention method, current discharge is present within the coating equipment.
[0045] The provision of switches and / or electronic protection mechanisms assures that the current discharge is solely a capacitive current provided by the respective capacitances. Furthermore, this provision guarantees the safeguarding of the power supplies against strong fluctuations induced by the rapid and violent process of arc discharge, thereby extending its lifetime.
[0046] The cathode 1 acts as the source of material provided by the coating equipment for the coating of materials and / or parts. For DLC coating, a graphite or a carbon-rich target material is utilized. The cathode may be a fixed or movable source, such as a rotating bar or a rotating rod.
[0047] The coating equipment operates under a vacuum base pressure, preferably a high vacuum with a pressure of 10-5mbar or below.Consequently, the region between the cathode 1 and first 33a and second 33b anodes is electrically isolated. The laser source 2 may use one or more laser pulses 2a to irradiate the cathode 1 target material, which delivers a high energy density when focused on the surface of said cathode 1 target material.
[0048] Such irradiation results in the rapid local heating of the of the cathode 1 target material, lowering the breakdown voltage in the region between the cathode 1 and the first anode 33a, allowing for the formation of a high-current arc discharge. In a typical embodiment, the arc discharge current has a minimum value of 4000 A and a maximum value of 10000 A.
[0049] The laser source 2 may comprise one or more laser sources illuminating a single or multiple cathode 1 spots during one or more laser pulses. The laser source 2 may be fixed or movably scanned by means of mechanical stages and / or optical elements (not shown for simplicity) to avoid strong local erosion of the cathode 1 material during repeatedSNANOC-9-PCTirradiation cycles. Such a provision assures the homogeneous use and longevity of the cathode material.
[0050] In a typical embodiment, the capacitances present in the deposition system can be provided by a single capacitor, such as a pulse discharge capacitor, or a capacitor bank, or a distributed capacitance within the electronic circuit.
[0051] In an optional embodiment, the electronic circuit associated with the first 4a and second 4b capacitances, and the first 5a and second 5b power supplies may be connected to a system electrical ground 12. This provision further enhances the protection of these components during charging and discharging cycles.
[0052] With reference to Figure 2, the schematic illustration of one preferable embodiment portraits the overall arrangement of the system for coating materials and / or parts with DLC, including the laser-induced arc discharge coating equipment 8 described with reference to Figure 1.
[0053] The system for coating materials comprises a vacuum chamber 13 that is operatively connected to one or more vacuum pumps (not shown in the figure for simplicity), which enable the provision of a vacuum base pressure within said chamber. The one or more vacuum pumps also assure that unwanted byproducts dispersed within the chamber environment are efficiently removed from the vacuum chamber 13 to avoid the progressive degradation of the vacuum level with repeated deposition cycles according to the deposition method of the present invention.
[0054] It should be understood that the depiction of the laser-induced arc discharge coating equipment 8 as being embedded within the vacuum chamber 13 is merely illustrative of one possible embodiment. The specific positioning of the laser-induced arc discharge coating equipment 8 is not critical to the function of the system for coating materials, provided that an ion propagation path 6 is established. Alternative configurations, such asSNANOC-9-PCTthe attachment of the laser-induced arc discharge coating equipment 8 to a sidewall of the vacuum chamber 13 via a vacuum flange, may also be used and are intended to be covered by the scope of this invention.
[0055] In a preferred embodiment, a holder 9 provides for the secure holding of materials and / or parts 10 to be coated. The materials and / or parts 10 are held by the holder 9 within the ion propagation path 6 to expose them to the carbon ion flux generated by the laser-induced arc discharge coating equipment 8.
[0056] In an optional embodiment, for the coating of a plurality of materials and / or parts, the holder 9 may be a flat tray or a rack-type of holder configured to hold said plurality of materials and / or parts fixedly, or it may be a carousel system configured to hold said plurality of materials and / or parts movably, like rotatably around a fixed axis within the ion propagation path 6.
[0057] In a preferred embodiment, the holder 9 is operatively connected to a third power supply 5c and a third capacitance 4c, said third capacitance 4c being configured to provide for a negative bias voltage between the holder 9 and the first 33a and second 33b anodes. The bias voltage is responsible for controlling the energy with which ions will reach the holder 9. The bias voltage also plays a crucial role in the adhesion of the DLC to the material and / or parts 10 to be coated.
[0058] The presence of the second anode 33a allows for the use of lower bias voltages while achieving similar deposition rates in comparison to geometrically analogous single anode configurations. In a typical embodiment, the third capacitance 4c is charged by the third power supply 5c to a minimum value of -10 V and a maximum value of -60 V, and the third capacitance has a minimum value of 400 pF.SNANOC-9-PCT
[0059] In a typical embodiment, during a discharging cycle, the collected ion current has a minimum value of 1000 A and a maximum value of 3000 A.
[0060] Similarly, and advantageously, the third power supply 5c provides for the charging of the third capacitance 4c only within the time where, during a deposition cycle of DLC according to the invention method, current discharge is absent within the coating equipment.
[0061] Similarly, and more advantageously, the third power supply 5c is equipped with switches and / or electronic protection mechanisms (not shown in Figure 2 for simplicity) that electrically disconnect and / or shield said third power supply 5c from its corresponding electronic circuit during the time where, during a deposition cycle of DLC according to the invention method, current discharge is present within the coating equipment.
[0062] In a preferable embodiment, the provisions of independently charging of the first 4a, second 4b and third 4c capacitances by the first 5a, second 5b and third 5c power supplies, respectively, as well as of independently discharging of said capacitances, have the advantage of reducing the electrical interference between the electrical circuits associated to the first 4a, second 4b and third 4c capacitances.
[0063] As a result, during the charging cycle, a reliable charging of each individual capacitances is achieved by each individual power supply.Further, during the discharging cycle, a higher level of stability of the generated plasma is observed, as well as a higher stability of the resulting ion flow along the ion propagation path 6 towards the holder 9.
[0064] In a typical embodiment, the holder 9 is surrounded by a cage 11 formed by a grounded conductive shield. The cage 11 provides for the capturing of any remaining ion flow that does not reach the holder 9SNANOC-9-PCTduring a deposition cycle according to the deposition method of the present invention.
[0065] In a preferred embodiment, the first 5a, second 5b and third 5c power supplies are connected to synchronization channels 7a, 7b, which are, in turn, connected to a synchronization unit 14. The synchronization unit 14 provides for the synchronization of the charging and discharging cycles of the first 4a, second 4b and third 4c capacitances, resulting in a stable and controlled deposition of DLC by means of one or more deposition cycles according to the method of the present invention.
[0066] The provision of the synchronization channels 7a, 7b connected to the synchronization unit 14 ensures that the holder 9 is biased only when plasma is present, preventing spontaneous arc discharges at the surface of the materials and / or parts 10 and reducing unwanted ion bombardment during the charging cycles of the capacitances according to the method of the present invention.
[0067] Furthermore, and advantageously, the provision of the synchronization channels 7a, 7b connected to the synchronization unit 14 allows for a reduced arc discharge current rise time and the discharging of the first 4a and second 4b capacitances occurs simultaneously, resulting in the formation of a plasma-transporting waive from the arc discharge zone towards the holder region within the vacuum chamber 13.
[0068] It should be understood that the depiction of the capacitances, power supplies, synchronization unit 14 and grounding 12 as being embedded within the vacuum chamber 13 is merely illustrative of one possible embodiment. Alternative configurations, such as the placement of said capacitances, power supplies, synchronization unit 14 and grounding 12 outside of the vacuum chamber 13, may also be used and are intended to be covered by the scope of this invention.SNANOC-9-PCT
[0069] For an effective DLC coating, the control of the number of charging and discharging cycles plays a critical role. In an optional embodiment, the provision of monitoring of the values of the discharge currents and capacitance charge level by suitable electronic measurement devices is present (not show for simplicity). When combined with the provision of the synchronization channels 7a, 7b connected to the synchronization unit 14, a precise setting and reduced cycling time can be achieved, with a typical value of 300 ns per charge / discharge cycle.
[0070] In a typical embodiment, the system for coating materials and / or parts with DLC provides for the coating with a deposition rate of up to 0.5 |im / h. Furthermore, the DLC coating after deposition presents a thickness range between 100 nm to 300 nm, or between 1 nm and 2 nm. Such value ranges are particularly suited for the coating of cutting and drilling tools, automotive components, medical implants and electronic devices.
[0071] Figure 3 is a simplified schematic illustration of the first anode 33a, in a preferable embodiment. The first anode 33a, in this realization is configured as a hollow cage 15 traversed coaxially by the ion propagation path 6.
[0072] In this preferrable mode of realization, which is not however the only one, the first anode has a flange 15 for fastening to the deposition apparatus and a surface 18 that is placed vis-à-vis the cathode. This may be the surface from which the plasma arc discharge occurs between the fist anode 33a and the cathode 1 during the discharging of the first capacitance 4a.
[0073] The first anode 33a may comprises two or more parallel plates 16, preferably spaced by 10 mm to 20 mm in distance, which are configured to enhance the filtering by trapping unwanted byproducts such as macro- and nano-particles, debris, droplets and neutral species whose trajectories deviate from the ion propagation path. The flange 15 with the arcSNANOC-9-PCTdischarge surface 18 may be connected to subsequent parallel plates 16 by rods for mechanical stability purposes.
[0074] With reference to Figures 4A and 4B, the schematic illustrations of one preferable embodiment portraits the geometry of the second anode 33b.
[0075] In a possible embodiment, the second anode 33b comprises two or four plates presenting corrugations 19 on the surfaces that are directly exposed to the generated plasma within the ion propagation path 6. The corrugations 19 are configured to enhance the filtering by trapping unwanted byproducts such as macro- and nano-particles, debris, droplets and neutral species whose trajectories deviate from the ion propagation path.
[0076] In this possible embodiment, the corrugations 19 may be a series of baffles, a series of comb structures, a series of rib structures or a series of protrusions. These structures may be arranged in equidistant patterns or irregular patterns.
[0077] In a possible embodiment, the surfaces of the second anode 33b that present corrugations 19 are configured such that the distance between said surfaces is smaller at a region closer to the cathode 20 than at a region closer to the holder 21. Such configuration provides for the option of enhancing the deposition rate at the expense of less efficient filtering of the unwanted byproducts by the second anode 33b.
[0078] Preferably, the distances between said surfaces 20, 21 is adjustable with an angle with respect to the ion propagation path 6 between 0° and 80°, depending on the preferred function of the second anode 33b as an effective filter of the unwanted byproducts (smaller angles) or as a deposition rate enhancer (larger angles).SNANOC-9-PCT
[0079] With reference to Figure 5, the schematic illustration of one preferable embodiment portraits the time evolution of the values of current, capacitance, voltage and laser irradiation of the different components of the system for coating materials and / or parts with DLC.
[0080] In a preferred embodiment, the synchronization unit 14 controls the charging and discharging timing of the first 4a, second 4b and third 4c capacitances synchronously. Advantageously, the monitoring of the values of the charge and discharge currents 22, 24, 27 and capacitance charge levels 23, 25, 28 by suitable electronic measurement devices is performed, and a feedback loop is provided to adjust the charging and discharging cycle times according to pre-set values of capacitances and / or currents and / or voltages.
[0081] In a preferred embodiment, and according to the method of the present invention, a deposition cycle starts with the first 4a, second 4b and third 4c capacitances being charged synchronously by the first 5a, second 5b and third 5c power supplies, respectively 23, 25, 28. When one or more pre-set values of the voltage across one or more capacitors or capacitor banks (with reference to said capacitances), and / or one or more pre-set values of the capacitances across one or more capacitor or capacitor banks are achieved, the synchronization unit 14 sends a trigger signal to the laser source 2 for the generation of a laser pulse 26 configured to irradiate the cathode 1 with laser light 2a.
[0082] The laser pulse 26 serves as the trigger for the formation of a high-current arc initially driven by the discharging current of the first capacitance 27 and immediately extended by the discharging current of the second capacitance 24 synchronously, resulting in the creation of the plasma. Simultaneously, the discharging current of the third capacitance 22 provides for the bias voltage needed to transport the plasma along the ion path towards the holder 9.SNANOC-9-PCT
[0083] Consequently, it is only during the discharging period that the provision of coating DLC material on the materials and / or parts 10 held by the holder 9 is given.
[0084] After the discharge of all the capacitances, either fully or to preset values, the deposition cycle ends. In an optional embodiment, a waiting time may be added after said full discharge to allow for the cooling of any of the deposition system parts and components.
[0085] In a preferred embodiment, a series of deposition cycles is performed according to the method of the present invention until a Diamond-like Carbon (DLC) coating is formed on said materials and / or parts 10 with a specified thickness. In a preferred embodiment, the deposition cycles are repeated with frequency not higher than 120 Hz, preferably within a frequency from 60 Hz to 100 Hz.
[0086] In an optional embodiment, the thickness may be estimated based on pre-calibrated deposition rates or measured in-situ by a thickness measurement device such as an interferometer, an ellipsometer, a spectrometer, or a quartz crystal sensor.
[0087] With reference to Figure 6, the schematic illustration of one embodiment with a carousel holder that is in part shielded from the carbon ion flux.
[0088] In a possible embodiment, the holder 9 is rotatably positioned 31 in the vacuum chamber 13. This allows for the provision of coating multiple surfaces or portions of the material and / or parts 10 with DLC without requiring the interruption of the deposition process.
[0089] In a possible embodiment, the holder 9 is protected by mechanical shields 29a, 29b configured to block carbon ions that propagate along the ion propagation path 6.SNANOC-9-PCT
[0090] The provision of a first 33a and second 33b anodes results in the extended region in which the arc discharge occurs. This, in turn, would result in a higher density of carbon ions that would reach the holder region. The provision of mechanical shields 29a, 29b prevents that carbon ions reach the holder 9 by physically blocking their flow, therefore resulting into a lower temperature of the holder 9 during the deposition of DLC. This, in turn, results in a lower temperature also of the materials and / or parts 10 due to cooling effects by means of irradiation and / or conduction of heat.
[0091] In a possible embodiment, the temperature of any of the holder 9 and / or materials and / or parts 10 does not exceed 100°C during the deposition of DLC. It was found by the present invention that such temperature range results in the best possible sp3 ratio in the DLC coating, preferably presenting an — < 0.25 when measured by Raman spectroscopy.IG
[0092] In a possible embodiment, the mechanical shields 29a, 29b are held at the same electrical potential as the holder 9. This provision permits that the carbon ions that reach the vicinity of the holder region are not deviated from their original trajectory along the ion propagation path 6 as there is no electrical potential difference between the holder 9 and the mechanical shields 29a, 29b.
[0093] Furthermore, the provision of mechanical shields 29a, 29b result in a flux of carbon ions that propagate along the ion propagation path 6 reaching the materials and / or parts 10 with trajectories largely perpendicular to the rotation axis of the holder 9. This provision results in further control of the temperature, as carbon ions that would reach the materials and / or parts 10 at an angle substantially different than ninety degrees from the rotation axis of the holder 9 do not contribute to the growth of the DLC coating, but only for the generation of heat due to collisions with the materials and / or parts 10 at grazing angles.SNANOC-9-PCT
[0094] The provision of a flux of carbon ions that propagate along the ion propagation path 6 reaching the materials and / or parts 10 with trajectories largely perpendicular to the rotation axis of the holder 9 further allows for carbon ions to reach the material and / or parts with an optimum energy for the formation of DLC favouring a high sp3 content.
[0095] In a possible embodiment, the energy of carbon ions that reach the materials and / or parts 10 is higher than 120 eV. It was found by the present invention that such energy regime results in the necessary subsurface incorporation of carbon atoms at materials and / or parts 10 within the first deposition cycles, resulting in optimum adhesion of the DLC coating.SNANOC-9-PCT
Claims
Claims1. System for coating materials and / or parts (10) with Diamond-like Carbon (DLC), the system comprising a deposition chamber (13) and an arc discharge coating equipment (8) for depositing DLC on said materials and / or parts (10) contained within said deposition chamber (13), wherein said system further comprises:a cathode (1);a first anode (33a) spaced from the cathode (1) to define an arc discharge path and connected to a first capacitance (4a);one or more ignition devices (2) configured to initiate a plasma arc discharge along the arc discharge path;a second anode (33b) spaced from the first anode (33a) and connected to a second capacitance (4b), wherein the first (33a) and second (33b) anode are arranged so that an ion propagation path (6) is formed from said target material towards said deposition chamber, and wherein an electrical discharge of the second anode (24) occurs when the plasma arc discharge between the cathode and first anode (27) is present, and wherein the first (33a) and / or the second (33b) anode is configured to filter macro- and nano-particles, debris, droplets and neutral species;a holder (9) positioned within said deposition chamber configured to hold the materials and / or parts (10) to be coated and connected to a third capacitance (4c), wherein the holder (9) is positioned within said ion propagation path (6).
2. System according to claim 1, wherein the ignition device is a laser or a spark electrode.SNANOC-9-PCT3. System according to any one of the preceding claims, wherein the cathode (1) and first anode (33a) are operatively connected to a first power supply (5a) and the first capacitance (4a) is configured to deliver a current discharge pulse (27), and wherein the cathode (1) and second anode (33b) are operatively connected to a second power supply (5b) and a second capacitance (4b) is configured to deliver a current discharge pulse (24), and wherein the holder (9) is operatively connected to a third power supply (5c) and a third capacitance (4c) is configured to deliver a negative potential between the materials and / or parts (10) to be coated and the first (33a) and second (33b) anodes.
4. System according to claim 3, wherein the second power supply (5b) is set to charge the second capacitance (4b) to a maximum voltage (25) that is higher than the maximum voltage of the first capacitance (28).
5. System according to any of the preceding claims, wherein the cathode (1) contains graphite or a carbon-rich material or any one of nitrides, such as TiN and CrN.
6. System according to any of the preceding claims, wherein the first (5a), second (5b), and third (5c) power supplies provide for a synchronous pulsed cycle of charging and discharging of the first (4a, 28), second (4b, 25) and third (4c, 23) capacitances.
7. System according to any of the preceding claims, wherein the first capacitance (4a) is charged (28) by the first power supply (5a) to a minimum value of 100 V and a maximum value of 400V, and wherein the first capacitance (4a) has a minimum value of 2000 |iF.
8. System according to any of the preceding claims, wherein the second capacitance (4b) is charged (25) by the second power supply (5b) to a minimum value of 150 V and a maximum value of 450 V, and wherein the second capacitance (4b) has a minimum value of 600 |iF.SNANOC-9-PCT9. System according to any of the preceding claims, wherein the third capacitance (4c) is charged (23) by the third power supply (5c) to a minimum value of -10 V and a maximum value of -60 V, and wherein the third capacitance (4c) has a minimum value of 400|iF.
10. System according to any of the preceding claims, wherein during the discharging of said first (4a), second (4b) and third (4c) capacitances the arc discharge current (27, 24) has a minimum value of 4000 A and a maximum value of 10000 A, and wherein the collected ion current (22) has a minimum value of 1000 A and a maximum value of 3000 A.
11. System according to any of the preceding claims, wherein the ion propagation path (6) is straight.
12. System according to any of the preceding claims, wherein the first anode (33a) is a hollow cage (15) configured to be coaxial with the ion propagation path (6).
13. System according to any of the preceding claims, wherein the first anode (33a) further comprises two or more parallel plates (16) configured to enhance the filtering of unwanted byproducts such as macro- and nanoparticles, debris, droplets and neutral species.
14. System according to any of the preceding claims, wherein the second anode (33b) is formed by plates presenting corrugations (19) on the surfaces that are directly exposed to the generated plasma, said corrugations (19) being configured to enhance the filtering of unwanted byproducts such as macro- and nano-particles, debris, droplets and neutral species.
15. System according to claim 13, wherein the surfaces that present corrugations (19) are configured such that the distance between saidSNANOC-9-PCTTlsurfaces is smaller at a region closer to the cathode (20) than at a region closer to the holder (21).
16. System according to any of the proceeding claims, wherein the holder (9) is rotatably positioned (31) in the vacuum chamber (13).
17. System according to any of the proceeding claims, wherein the holder (9) is placed at distance between 100 mm and 350 mm from cathode (1).
18. System according to any of the proceeding claims, wherein the holder (9) is protected by mechanical shields (29a, 29b) configured to block carbon ions that propagate along the ion propagation path (6), and wherein the carbon ions that propagate along the ion propagation path (6) reach the materials and / or parts (10) with trajectories largely perpendicular to the rotation axis of the holder (9).
19. System according to the preceding claim, wherein the mechanical shields (29a, 29b) are held at the same electrical potential as the holder (9).
20. System according to any of claims 16 or 17, wherein the energy of carbon ions that reach the materials and / or parts (10) is higher than 120 eV.
21. System according to any of claims 15 to 18, wherein the temperature of any of the holder (9) or materials and / or parts (10) does not exceed 100°C during the deposition of DLC.
22. System according to any of the preceding claims, wherein the holder (9) includes a carousel.
23. A deposition method for the DLC coating of materials and / or parts (10) using the system of any of the proceeding claims, the method comprising the steps of:SNANOC-9-PCTA. placing materials and / or parts (10) to be coated being held by a holder (9) within said deposition chamber (13);B. providing a cathode (1);C. providing a vacuum within the deposition chamber (13);D. providing a first (4a), a second (4b) and a third (4c) capacitance to said first (33a) and second (33b) anodes, and said holder (9), respectively;E. triggering a current discharge pulse from said first (4a), second (4b) and third (4c) capacitances and creating a plasma;F. transporting said plasma to the deposition chamber (13), wherein a bias voltage between said first (33a) and second (33b) anodes and said holder (9) accelerates ions towards said materials and / or parts (10) to be coated;G. coating said materials and / or parts (10) with Diamond-like Carbon (DLC);H. repeating the steps D. to G. until a Diamond-like Carbon (DLC) coating is formed on said materials and / or parts (10) with a specified thickness.
24. Method according to claim 23, the triggering of the current discharge pulse involving irradiating said target material as a cathode (1) with one or more laser pulses (2a) from one or more laser sources (2) to initiate a plasma arc discharge between the cathode (1) and first anode (33a).SNANOC-9-PCT25. Method of claim 23, wherein a full cycle including steps D. to G. is performed within a frequency not higher than 120 Hz, preferably within a frequency from 60 Hz to 100 Hz.
26. Method according to any of claims 23-25, wherein the cathode (1) contains graphite or a carbon-rich material or any one of nitrides, such as TiN and CrN.
27. Diamond-like Carbon (DLC) coating deposited on a substrate, wherein the coating, when analysed with Raman spectroscopy using an excitation wavelength such as 480 nm, 514.5nm or 532 nm, exhibits a D peak signal and a G peak signal, the ratio of the intensity of the D peak signal and a G peak signal being — < 0.25.IG SNANOC-9-PCT