Process for making a brake disc provided with a protective layer and brake disc made directly

The laser deposition of a ferritic steel intermediate layer with embedded hard material particles addresses the wear and oxidation issues of brake discs, improving adhesion and corrosion resistance through a novel manufacturing process.

WO2026239216A1PCT designated stage Publication Date: 2026-11-19BREMBO NV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054526
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing brake discs made of grey cast iron or steel suffer from excessive wear and surface oxidation, leading to rust formation, which affects performance and aesthetics, while traditional protective coatings face issues with dispersion and adhesion of fine hard material particles during deposition.

Method used

A process involving laser deposition of an intermediate layer made of ferritic steel with embedded hard material particles less than 30 μm, using metal binders with lower melting temperatures to form pristine particles, followed by an anti-wear layer, enhances adhesion and corrosion resistance.

Benefits of technology

The process optimizes the adhesion of the anti-wear layer and improves mechanical strength and corrosion resistance, reducing particle dispersion and enhancing the durability of brake discs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054526_19112026_PF_FP_ABST
    Figure IB2026054526_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A process for making a brake disc (1) is described, comprising the following operational steps: a) preparing a brake disc (1), comprising a braking band (2) equipped with two side braking surfaces (4), said braking band (2) being made of grey cast iron or steel; b) after step a), depositing an intermediate layer (6) constituted by a metal alloy on at least one of the two side braking surfaces (4); c) after step b), depositing an anti-wear layer (5) made from a particle composition comprising a metal alloy and from particles (7) of hard material having an average size less than 30 μm, which are aggregated by metal binders so as to form pristine particles; said metal binders having melting temperature lower than the melting temperature of said particles (7) of hard material; said depositing step being implemented by laser deposition technique. A brake disc (1) made by the process according to the present invention is also described.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] “PROCESS FOR MAKING A BRAKE DISC PROVIDED WITH A

[0002] PROTECTIVE LAYER AND BRAKE DISC MADE DIRECTLY”

[0003] Field of the invention

[0004] The present invention relates to a process for making a brake disc for disc braking systems, which is equipped with a protective layer, and to a brake disc made directly. In particular, the invention relates to a process for making brake discs for vehicles equipped with a braking band whose braking surfaces, that is, adapted to come into contact with a brake caliper, are coated with at least one protective layer and the brake disc obtained directly.

[0005] Known art

[0006] The following documents describe some examples of braking systems equipped with protective coatings: US4715486, WO2014 / 097187.

[0007] Summary of the invention

[0008] As it is well known, the so-called brake discs may comprise a braking band equipped with braking surfaces adapted for cooperating with friction elements (brake pads), which are housed in at least one caliper body straddling such braking band and integral with a non-rotating component of the vehicle suspension.

[0009] Generally, the brake disc is made of grey cast iron or steel. Indeed, this material allows to achieve good braking performance (especially in terms of wear control) at relatively low cost. Furthermore, brake discs made of carbon or carbon-ceramic materials which offer significantly higher performances, but at much higher costs, are known.

[0010] The limitations of traditional cast iron or steel brake discs are related to excessive wear. Regarding grey cast iron discs, another major drawback is related to excessive surface oxidation, resulting in rust formation. This aspect affects both the performance of the brake disc and its appearance, as rust on the brake disc is aesthetically unacceptable to the user. Efforts have been made to address these problems by making grey cast iron or steel discs with a protective coating. The protective coating serves, on the one hand, to reduce disc wear and, on the other hand, to protect the grey cast ironbase from surface oxidation, thus preventing the formation of a rust layer.

[0011] The Applicant noted that a particularly important aspect in the design of this type of disc brake is the choice of materials to create the anti-wear layer.

[0012] The Applicant noted that, to reduce wear, hard metal- or carbide-based anti-wear layers are known to be applied. Furthermore, providing an intermediate layer between the anti-wear layer and the main element so as to serve, in particular, as a bonding agent and anti-corrosion layer between the anti-wear layer and the main element is known.

[0013] The Applicant further noted that some particles of hard material, which are particularly suitable for ensuring corrosion resistance, have a very fine particle size that is not suitable for deposition by standard deposition processes used in this field, in particular laser or thermal processes.

[0014] In these cases, as a matter of fact, the average particle size of hard material, typically in the order of 20 pm, results in very high dispersion during deposition. In other terms, a portion significantly higher than 50% of the particles of hard material ends up being dispersed rather than embedded in the protective layer by the end of the deposition step.

[0015] The Applicant therefore faced the problem of a process for making a brake disc that would allow optimizing the adhesion of the anti-wear layer to the intermediate layer as well as the corrosion resistance of the friction braking element by depositing hard material particles characterized by fine particle size, that is, by reduced average particle size, thereby significantly reducing particle dispersion during the deposition step.

[0016] Therefore, in a first aspect, the invention relates to a process for making a brake disc, comprising the following operational steps:

[0017] a) preparing a brake disc, comprising a braking band equipped with two side braking surfaces, said braking band being made of grey cast iron or steel;

[0018] b) after step a), depositing an intermediate layer constituted by a metal alloy on at least one of the two side braking surfaces;

[0019] c) after step b), depositing an anti-wear layer made from a particle composition comprising a metal alloy and particles of hard material having an average size less than 30 pm, which are agglomerated by metal binders so as to form pristine particles; saidmetal binders having melting temperature lower than the melting temperature of said particles of hard material; said depositing step being implemented by laser deposition technique.

[0020] Thus, the Applicant has achieved a novel optimization of the process for making a brake disc equipped with a protective layer which allows providing adequate mechanical strength and wear resistance, thanks to the presence of hard particles in the protective layer, and also improving the yield of the deposition process by reducing the amount of particles of hard material dispersed during their laser deposition.

[0021] For the purposes of the present invention, the following definitions apply:

[0022] "Particles of hard material" means particles with an average size of less than 30 pm and hardness of at least 700 HV, measured according to the Vickers hardness scale (HV).

[0023] “Pristine particle” means a mass constituted by heterogeneous metal-based elements, the pristine particle for descriptive purposes can be regarded as a spherical element having a radius equal to its average size, although it may take various forms.

[0024] “Freely contained”, referred to particles of hard material in a layer, means that these particles are not wholly or partially embedded in the initial metal binder.

[0025] "Ferritic steel" means a stainless steel that contains a large proportion of Chromium (typically ranging between 11% and 19 %), but without the content of other materials capable of forming austenite, for example, nickel, being in a sufficient percentage to make austenite a relevant phase in the micro- structure. In particular, this refers to stainless steel that should it contain a percentage of Nickel, that percentage would be negligible, by way of example less than or equal to 3% by weight, preferably less than 0.5% by weight, more preferably less than 0.1% by weight.

[0026] The present invention, in one or more preferred aspects, may comprise one or more of the following features.

[0027] Advantageously, the melting temperature of the metal binders is less than 85% of the melting temperature of the particles of hard material.

[0028] Conveniently, the hard material of said particles of hard material is selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0029] Preferably, the metal binders consist of a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof.

[0030] Advantageously, the pristine particles have an average size greater than or equal to 30 pm and less than or equal to 250 pm.

[0031] Preferably, during step c), said deposition is implemented by using a laser beam, with a technique selected from LMD (Laser Metal Deposition) technique, HSLC - high speed laser cladding - technique, EHLA - Extreme High Speed Laser Application -technique.

[0032] Conveniently, the intermediate layer is deposited so that its final thickness on the finished disc is greater than or equal to 30 pm and less than or equal to 1000 pm.

[0033] The term "thickness" of the outer anti-wear layer means the average thickness of said layer.

[0034] Preferably, the anti-wear layer is deposited so that its final thickness on the finished disc is greater than or equal to 30 pm and less than or equal to 1500 pm.

[0035] Advantageously, the intermediate layer comprises a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof.

[0036] Even more preferably, the intermediate layer comprises a ferritic steel alloy.

[0037] Advantageously, the aforementioned ferritic steel has a percentage of chromium Cr greater than or equal to 15% by weight.

[0038] Conveniently, the intermediate layer is made from a particle composition comprising a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof, and from particles of hard material having an average size less than 30 pm agglomerated by metal binders so as to form pristine particles; the metal binders having melting temperature lower than the melting temperature of said hard particles.

[0039] Preferably, the material of the particles of hard material is selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0040] Advantageously, the intermediate layer is deposited by laser deposition technique.

[0041] According to another aspect, the invention relates to a brake disc comprising a braking band extending around an axis of rotation; said braking band having two side braking surfaces adapted to cooperate with a respective brake caliper to exert braking action against the vehicle on which said brake disc is installed;

[0042] an anti-wear layer applied to the side surfaces; and

[0043] an intermediate layer arranged between said anti-wear layer and said side braking surfaces;

[0044] said anti-wear layer comprises a ferritic steel layer and is made from a particle composition comprising particles of hard material selected from carbides, oxides, nitrides, borides, silicides, oxides, carbonitrides or a combination thereof;

[0045] the aforementioned intermediate layer consists of a metal alloy, characterized in that the brake disc is made by a process as described above.

[0046] Further characteristics and advantages of the invention will become clearer from the detailed description of some preferred, but not exclusive, embodiments of a process for making a brake disc and the brake disc obtained directly according to the present invention.

[0047] Brief description of the drawings

[0048] This description will be set forth hereinafter with reference to the attached drawings provided for illustration purposes only and without limitation, in which:

[0049] - Figure 1 shows a schematic sectional view of a first embodiment of the brake disc according to the invention;

[0050] - Figure 2 is an enlarged view of a portion of the brake disc of Figure 1;

[0051] - Figure 3 is a schematic view of some steps of the process for making the brake disc according to the present invention.

[0052] Detailed description of embodiments of the invention

[0053] With reference to the attached figures, a brake disc according to the present invention is generally denoted by 1.

[0054] The brake disc 1 comprises a braking band 3 extending around a central axis of rotation denoted by X-X.

[0055] The braking band 2 is equipped with two side braking surfaces denoted by 4, adapted to be engaged by a brake caliper (not shown) of a disc braking system so as to exert a braking action against the vehicle on which said brake disc 1 is installed, if necessary.

[0056] The braking band 2 is made of grey cast iron or steel.

[0057] Preferably, the braking band 2 is made of grey cast iron. In particular, the entire disc is made of grey cast iron. Thus, in the description that follows, reference will be made to a disc made of grey cast iron, anyway without ruling out the possibility that it may be made of steel.

[0058] The disc 1 is equipped with at least one anti-wear layer 5 covering at least one, preferably both, the braking surfaces 4 of the braking band 2 and at least one intermediate layer 6 arranged between said at least one anti-wear layer 5 and the side braking surfaces 4.

[0059] Preferably, as in the embodiment shown in the figures, the brake disc 1 is equipped with an anti-wear layer 5 covering the two side braking surfaces 4 of the braking band 2 and an intermediate layer 6 arranged between the anti-wear layer 5 and the side braking surfaces 4.

[0060] The intermediate layer 6, arranged between the anti-wear layer 5 and the braking surfaces 4, serves in particular as a bonding agent and an anti-corrosion layer between the anti-wear layer and the braking surfaces 4.

[0061] According to an aspect of the present invention, the aforesaid at least one antiwear layer 5 is made from a particle composition comprising ferritic steel embedding particles of hard material.

[0062] In the embodiment shown in the figures, the anti-wear layer 5 has a thickness D greater than or equal to 30 pm and less than 1500 pm.

[0063] Preferably, the anti-wear layer 5 has a thickness D greater than or equal to 80 pm and less than 1000 pm.

[0064] The intermediate layer 6 has a thickness d greater than or equal to 30 pm and less than or equal to 1000 pm. Preferably, the intermediate layer 6 has a thickness d greater than or equal to 60 pm and less than or equal to 300 pm.

[0065] Preferably, but not necessarily, the anti-wear layer 5 has a thickness D greater than or equal to 1.2 times the thickness d of the intermediate layer 6.

[0066] According to a first embodiment, the intermediate layer 6 consists of a metal alloy selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof.

[0067] Preferably, the metal alloy is an iron-based alloy, even more preferably it is a ferritic steel alloy having a Nickel content of less than or at most 3% by weight.

[0068] Even more preferably, this intermediate layer 6 has a Nickel content of less than or at most 0.5% by weight.

[0069] Preferably, that intermediate layer 6 is totally nickel-free, that is, the Nickel content is not detectable by standard analytical methods. In particular, suitable methods of analysis are ASTM E1473-22. In other words, ferritic steel as defined here has a Nickel content that is undetectable according to the ASTM E1473-22 standard.

[0070] To allow for greater corrosion resistance, the ferritic steel used for the intermediate layer 6 has an amount of chromium Cr in a percentage greater than or equal to 15% by weight.

[0071] According to a further embodiment, the intermediate layer 6 is constituted by a metal alloy, as in the previously described case, and particles of hard material (Fig. 2).

[0072] Preferably, the particles 7 of hard material are selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0073] The particles 7 of hard material present in the intermediate layer 6 are predominantly “freely” embedded in the metal alloy the intermediate layer 6 is constituted by; in this case, they have an average size of less than 30 pm.

[0074] However, specifically depending on the process according to the present invention, some particles 7 of hard material may also be present in the intermediate layer 6, either fully embedded in a metal binder or only partially embedded in a metal binder that has been partially dissolved / broken up from the original pristine particles 9 (that is, as provided at the beginning of the process).

[0075] Indeed, the intermediate layer 6 is obtained by deposition using a laser technique, starting with at least one layer of a metal alloy onto which pristine particles, comprising hard particles aggregated by a metal binder, are deposited.

[0076] The initial metal binder used to make the intermediate layer 6 comprises a metal alloy selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof. The metal binder is adapted to aggregate the particles 7 of hard material so as to form pristine particles.

[0077] Preferably, the initial pristine particles 9 have an average size greater than or equal to 30 pm and less than or equal to 250 pm.

[0078] The metal binder has a melting temperature that is lower than that of the hard particles 7 it contains.

[0079] Preferably, the melting temperature of the metal binder is less than 85% of the melting temperature of the particles 7 of hard material contained therein.

[0080] As previously mentioned, the anti-wear layer 5 is constituted by a metal alloy and particles of hard material having an average size of less than 30 pm.

[0081] The metal alloy is selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof.

[0082] Preferably, the metal alloy is an iron-based alloy, even more preferably it is ferritic steel.

[0083] The ferritic steel used is the same as that used for the anti-wear layer 5, that is, ferritic steel having a Nickel content of less than or at most 3% by weight.

[0084] Even more preferably, the anti -wear layer 5 has a Nickel content of less than or at most 0.5% by weight.

[0085] Preferably, this anti-wear layer 5 is completely nickel-free, that is, that the Nickel content cannot be detected by standard analytical methods. In particular, suitable methods of analysis are ASTM E1473-22. In other words, ferritic steel as defined here has a Nickel content that is undetectable according to the ASTM E1473-22 standard.

[0086] This allows to limit, if not even to avoid, dispersion of nickel particles throughout the lifetime of the brake disc 1.

[0087] Even in this case, to allow for a greater corrosion resistance, the ferritic steel used for the anti-wear layer 5 has a relatively high amount of chromium Cr, that is, a percentage greater than or equal to 15% by weight.

[0088] The particles 7 of hard material are embedded in the anti-wear layer 5 and in particular in the ferritic steel, in an amount greater than or equal to 10% by volume and less than or equal to 90% by volume.

[0089] Preferably, the particles 7 of hard material are embedded in the anti -wear layer 5 and in particular in the ferritic steel, in an amount greater than or equal to 15% by volume and less than or equal to 85% by volume.

[0090] Preferably, the particles 7 of hard material are selected from particles of carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0091] In the case of carbides in particle form, the latter are selected from tungsten carbide (WC), chromium carbide, niobium carbide (NbC), titanium carbide (TiC) and / or mixtures thereof.

[0092] Preferably, the carbides in particulate form are selected from tungsten carbide (WC), titanium carbide (TiC) and / or mixtures thereof.

[0093] The particles 7 of hard material used for the anti-wear layer 5 may be the same as those used for the intermediate layer, if present in the latter.

[0094] The particles 7 of hard material preferably have an average size of less than 30 pm.

[0095] The particles 7 of hard material present in the anti-wear layer 5 are predominantly “freely” embedded in the metal alloy the anti-wear layer 5 is constituted by; in this case, they have an average size of less than 30 pm, as mentioned above.

[0096] However, specifically depending on the process according to the present invention, some particles 7 of hard material may also be present in the anti-wear layer 5, either fully embedded in a metal binder or only partially embedded in a metal binder that has been partially dissolved / broken up from the original, pristine particles.

[0097] Indeed, the anti-wear layer 5 is obtained by deposition using a laser technique involving the deposition of a particle composition comprising metal alloy powders and pristine particles comprising particles of hard material aggregated by a metal binder.

[0098] The initial metal binder used to make the anti-wear layer 5 comprises a metal alloy selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof.

[0099] The metal binder is adapted to aggregate the particles 7 of hard material so as to form pristine particles 9. Preferably, the original or initial pristine particles 9 have an average size greater than or equal to 30 pm and less than or equal to 250 pm.

[0100] The metal binder has a melting temperature that is lower than that of the hard particles 7 it contains.

[0101] Preferably, the melting temperature of the metal binder is less than 85% of the melting temperature of the particles 7 of hard material contained therein.

[0102] The brake disc 1 is made by the process according to the invention that will now be described.

[0103] In a first step, a brake disc 1 comprising a braking band 2 equipped with two side braking surfaces 4 is prepared. The braking band 2 is made of grey cast iron or steel, preferably the braking band 2 is made of grey cast iron.

[0104] Next, at least one side braking surface 4 of the braking band 2, preferably both, is pre-machined or pre-treated mechanically or thermally, in particular to roughen or geometrically adapt the surface onto which the intermediate layer 6 has to be applied.

[0105] In the next step, the intermediate layer 6 is then applied directly onto the braking side surfaces 2 by laser welding, for example, Laser Metal Deposition or Extreme High-Speed Laser Material Deposition.

[0106] The deposited intermediate layer 6 is a layer consisting of a metal alloy.

[0107] The metal alloy is a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof.

[0108] Preferably, the metal alloy is an iron-based alloy, even more preferably it is ferritic steel.

[0109] To allow for greater corrosion resistance, the ferritic steel used for the intermediate layer 6 has an amount of chromium Cr in a percentage greater than or equal to 15% by weight.

[0110] The intermediate layer 6, which is deposited, is therefore deposited so that its final thickness d is greater than or equal to 30 pm and less than or equal to 1000 pm.

[0111] According to an alternative embodiment, the intermediate layer 6 consists of a metal alloy of the type described above but embedding particles 7 of hard material that may be found freely embedded in the metal alloy or, as better described below, in their turn agglomerated by metal binders to form pristine particles 9 or in what remains from the disintegration of such metal binders due to their melting during the laser deposition itself.

[0112] The material of the hard material particles is selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0113] The particles 7 of hard material selected for this deposition step have an average size less than or equal to 30 pm and are aggregated to form pristine particles 9 by metal binders that have a melting temperature lower than that of the particles 7 of hard material contained therein.

[0114] Preferably, the melting temperature of said metal binders is less than 85% of the melting temperature of the particles of hard material.

[0115] The intermediate layer 6 is formed by deposition using a laser technique involving the deposition of a particulate composition comprising metal alloy powders and pristine particles 9 comprising particles of hard material aggregated by a metal binder.

[0116] The metal binder, having a melting temperature that is lower than that of the hard particles 7 it contains, when struck by the laser beam, fuses earlier than the particles 7 of hard material.

[0117] The latter are thus released into the metal alloy, which is in turn struck and fused by the laser beam 8.

[0118] During this deposition step, it is anyway possible that not all of the metal binder of the pristine particles 9 will fuse completely; instead, some pristine particles may remain intact or fuse only partially, causing them to break up only partially. In these cases, their presence will be detectable under microscopic analysis in the cooled intermediate layer 6.

[0119] The bond resulting from laser welding ensures that the intermediate layer 6 adheres well to the side braking surfaces 2. The resulting intermediate layer 6 preferably covers the side braking surfaces 2 entirely.

[0120] The resulting intermediate layer 6 is constituted by ferritic steel having a Nickel content of less than or at most 3% by weight.

[0121] Preferably, this intermediate layer 6 has a Nickel content of less than or at most 0.5% by weight.

[0122] The intermediate layer 6, which is deposited, has a thickness d greater than or equal to 30 pm and less than or equal to 1000 pm. Preferably, the intermediate layer 6 has a thickness d greater than or equal to 60 pm and less than or equal to 300 pm.

[0123] Then, after the intermediate layer 6 has solidified or cooled down, the anti-wear layer 5 is deposited directly onto the intermediate layer 6, also in this case using a laser technique.

[0124] The anti-wear layer 5 is obtained by deposition technique using a laser beam, for example, LMD (Laser Metal Deposition) technique, or HSLC - high speed laser cladding technique, or EHLA - Extreme High Speed Laser Application technique.

[0125] The anti-wear layer 5 that is formed may have indeed a thickness D greater than or equal to 30 pm and less than 1500 pm.

[0126] Preferably, the anti-wear layer 5 may have a thickness D greater than or equal to 80 pm and less than 1000 pm.

[0127] Preferably, even if not necessarily, the anti-wear layer 5 is deposited so that the thickness of the anti-wear layer 5 that is formed on the finished brake disc 1 is greater than that of the intermediate layer 6.

[0128] Preferably, the anti-wear layer 5 is deposited so that the thickness of anti-wear layer 5 that is formed on the finished brake disc 1 is greater than or equal to 1.2 times the thickness d of the intermediate layer 6.

[0129] The anti-wear layer 5 that is formed is constituted by ferritic steel embedding particles 7 of hard material.

[0130] The particles 7 of hard material that are embedded in the anti-wear layer 5, and in particular in ferritic steel, are embedded in an amount greater than or equal to 10% by volume and less than or equal to 40% by volume.

[0131] Preferably, the particles 7 of hard material are selected from particles of carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

[0132] The particles of hard material preferably have an average size of less than 30 pm.

[0133] At the end of the process, the particles 7 of hard material in the anti -wear layer 5 are found to be predominantly freely embedded in the metal alloy the anti-wear layer 5 is constituted by.

[0134] However, precisely depending on the laser deposition step, some particles 7 of hard material may also be present in the anti-wear layer 5, either aggregated by a metal binder of an original pristine particle or only partially aggregated by a metal binder of an original pristine particle that has partially broken up.

[0135] Indeed, the anti-wear layer 5 is obtained by deposition using a laser technique involving the deposition of a particle composition comprising metal alloy powders and pristine particles comprising particles of hard material aggregated by a metal binder.

[0136] The metal alloy powders and the pristine particles are struck and fused together by the laser beam 8.

[0137] However, the metal binder of the pristine particles, having a melting temperature that is lower than that of the hard particles 7 it contains, when struck by the laser beam, fuses earlier than the particles 7 of hard material.

[0138] The latter are thus released into the metal alloy, which is in turn struck and fused by the laser beam 8.

[0139] During this deposition step, it is anyway possible that not all of the metal binder of the pristine particles 9 will fuse completely; instead, some pristine particles may remain intact or their metal binder may fuse only partially, causing them to break up only partially. In such cases, their presence will be visually detectable under microscopic analysis in the cooled anti-wear layer 5.

[0140] Preferably, the initial metal alloy for the anti-wear layer 5 is an iron-based alloy and in particular ferritic steel.

[0141] The ferritic steel of the anti-wear layer 5 that is formed has a Nickel content of less than or at most 3%. Preferably, less than or at most 0.5%.

[0142] This allows to limit, if not even to avoid, dispersion of nickel particles throughout the lifetime of the brake disc 1.

[0143] The initial metal binder used to make the anti-wear layer 5 comprises a metal alloy selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof, embedding the particles 7 of hard material.

[0144] Preferably, the initial pristine particles 9 have an average size greater than or equal to 40 pm and less than or equal to 250 pm.

[0145] The metal binder has a melting temperature that is lower than that of the hard particles 7 it contains.

[0146] Preferably, the melting temperature of the metal binder is less than 85% of the melting temperature of the particles 7 of hard material contained therein.

[0147] The anti -wear layer 5 may be subjected to mechanical or thermal postprocessing, in particular grinding, to ensure the desired surface roughness for interaction with the friction brake pad.

[0148] Various modifications may be made to the embodiments described in detail, all anyhow remaining within the scope of protection of the invention, as defined by the following claims.

Claims

CLAIMS1. Process for making a brake disc (1), comprising the following operational steps:a) preparing a brake disc (1), comprising a braking band (2) equipped with two side braking surfaces (4), said braking band (2) being made of grey cast iron or steel;b) after step a), depositing an intermediate layer (6) constituted by a metal alloy on at least one of the two side braking surfaces (4);c) after step b), depositing an anti-wear layer (5) made from a particle composition comprising a metal alloy and from particles (7) of hard material having an average size less than 30 pm, which are aggregated by metal binders so as to form pristine particles (9); said metal binders having melting temperature lower than the melting temperature of said particles (7) of hard material; said depositing step being implemented by laser deposition technique.

2. Process for making a brake disc (1) according to claim 1, characterized in that the melting temperature of said metal binders is less than 85% of the melting temperature of said particles (7) of hard material.

3. Process for making a brake disc (1) according to claim 1, characterized in that the material of said particles (7) of hard material is selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

4. Process for making a brake disc (1) according to any one of claims 1 to3, characterized in that said metal binders consist of a metal alloy selected from an ironbased alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof.

5. Process for making a brake disc (1) according to any one of claims 1 to4, characterized in that said pristine particles (9) have an average size greater than or equal to 40 pm and less than or equal to 250 pm.

6. Process for making a brake disc (1) according to any one of claims 1 to 5, characterized in that during step c) said laser deposition is implemented with a technique selected from LMD (Laser Metal Deposition) technique, HSLC - high speed laser cladding technique, EHLA - Extreme High Speed Laser Application technique.

7. Process for making a brake disc (1) according to any one of claims 1 to 6, characterized in that said intermediate layer (6) is deposited so that its final thickness (d), on the finished disc, is greater than or equal to 30 pm and less than or equal to 1000 pm.

8. Process for making a brake disc (1) according to any one of claims 1 to 7, characterized in that said anti-wear layer (5) has a final thickness (D), on the finished disc, greater than or equal to 30 pm and less than or equal to 1500 pm.

9. Process for making a brake disc (1) according to any one of claims 1 to 8, characterized in that said intermediate layer (6) comprises a metal alloy selected from an iron-based alloy, a titanium-based alloy, an aluminum-based alloy or a combination thereof.

10. Process for making a brake disc (1) according to claim 9, characterized in that said intermediate layer (6) consists of a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof.

11. Process for making a brake disc (1) according to claim 10, characterized in that said intermediate layer (6) comprises a ferritic steel alloy.

12. Process for making a brake disc (1) according to claim 11, characterized in that said ferritic steel has a percentage of chromium Cr greater than or equal to 15% by weight.

13. Process for making a brake disc (1) according to claim 9, characterized in that said intermediate layer (6) is made from a particle composition comprising a metal alloy selected from an iron-based alloy, a titanium-based alloy or an aluminum-based alloy or a combination thereof, and from particles (7) of hard material having an average size less than 30 pm aggregated by metal binders so as to form pristine particles (9); said metal binders having melting temperature lower than the melting temperature of said hard particles.

14. Process for making a brake disc (1) according to claim 13, characterized in that the material of said particles of hard material is selected from carbides, oxides, nitrides, borides, silicides, carbonitrides or a combination thereof.

15. Process for making a brake disc (1) according to any one of claims 1 to 13,characterized in that said intermediate layer (6) is deposited by laser deposition technique.

16. Brake disc (1) comprising a braking band (2) extending around an axis of rotation (X-X); said braking band (2) having two side braking surfaces (4) adapted to cooperate with a respective brake caliper to exert braking action against the vehicle on which said brake disc (1) is installed;- an anti-wear layer (5) applied to said side surfaces (4); and- at least one intermediate layer (6) arranged between said anti-wear layer (5) and said side braking surfaces (4);- said anti-wear layer (5) comprises a ferritic steel layer and is made from a particle composition comprising particles of hard material selected from carbides, oxides, nitrides, borides, silicides, oxides, carbonitrides or a combination thereof; said intermediate layer (6) consists of a metal alloy,characterized in that said brake disc is made by a process according to any one of claims 1 to 15.