Compostable polymer blend

A compostable polymer blend with PLA, talc, and optional additives addresses thermal and biodegradability issues in bioplastics, achieving high thermal resistance and gas barrier properties, suitable for food packaging like coffee capsules.

WO2026239243A1PCT designated stage Publication Date: 2026-11-19PLANET BIOPLASTICS SRL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054631
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-11
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing bioplastics used in food packaging, such as coffee capsules, face challenges in achieving high thermal resistance, gas barrier properties, and biodegradability, with issues like slow crystallization, hydrolysis, and potential toxicity, making them unsuitable for large-scale commercial use.

Method used

A compostable polymer blend comprising poly-lactic acid (PLA), polylactone, talc as a nucleating agent, and optional additives like organic fibers, polyprotic acids, and inorganic substances to accelerate crystallization and enhance mechanical and barrier properties, without using 1,4-butanediol polyesters or polyhydroxyalkanoates.

Benefits of technology

The blend achieves a heat deflection temperature above 90°C, high gas barrier properties, and rapid biodegradability, meeting industrial compostability standards and ensuring safety for food contact, while reducing production costs and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000013_0001_TABLE
    Figure IMGF000013_0001_TABLE
  • Figure IMGF000014_0001_TABLE
    Figure IMGF000014_0001_TABLE
  • Figure IMGF000014_0002_TABLE
    Figure IMGF000014_0002_TABLE
Patent Text Reader

Abstract

The present invention relates to a compostable polymer blend, process for preparing the blend and its use as a compostable polymer in the food sector.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] COMPOSTABLE POLYMER BLEND

[0002] * * *

[0003] Technical field of the invention

[0004] The present invention relates to a compostable polymer blend. Such a compostable polymer blend can be used in the food sector as a compostable polymer.

[0005] State of the art

[0006] At present, capsules intended for the infusion of granular powder or leaf products (such as coffee, barley, powdered milk, tea, chamomile, etc.) have become an essential element of daily life for millions of consumers around the world. With the evolution of technologies and the growing focus on sustainability, the capsule market has transformed significantly. Traditional plastic and aluminium capsules are giving way to more eco-friendly solutions, such as compostable and biodegradable ones, designed to reduce environmental impact.

[0007] Usually, the capsule for infusion consists of a container, made of plastic or paper material, in which the product to be infused is inserted, and a lid consisting of a film of polymeric or paper material, responsible for ensuring optimal storage conditions for the granular product.

[0008] Currently, coffee capsules are mainly made of polypropylene (PP) and aluminium, but they are no longer sustainable, as aluminium is not easily recoverable and petroleum-derived plastic capsules end up predominantly incinerated or in landfill, while compostable capsules represent only a small share of this market.

[0009] The European Commission's Packaging and Packaging Waste Regulation (PPWR) highlights the importance of compostability for coffee capsules, stressing that coffee grounds contain valuable nutrients such as potassium, phosphorus and nitrogen, which can enrich the soil if composted.

[0010] Bioplastics represent a new class of bio-based and biodegradable plastics and are considered the most promising material to replace traditional plastics in many applications. Currently, the most produced bioplastics are poly(lactic acid) (PLA), polyhydroxyalkanoate (PHA), poly(butylene succinate) (PBS), starch-based plastics and those derived from cellulose such as, for example, cellulose acetate.

[0011] However, polyhydroxyalkanoate (PHA), polybutylene succinate (PBS), starch-based plastics and those derived from cellulose have problems which severely limit the application thereof on a large scale, such as different processing methods, impacts on food production, poor mechanical properties and slowness in their industrialisation, making them therefore not yet able to respond to the growing demand for bioplastics on a large scale. In particular, starch-based plastics and those derived from cellulose, to be processable with normal polymer

[0012] processing techniques, require the addition of plasticizers which can migrate to the surface of the products and contaminate the food with which they are put in contact. Furthermore, PHA is still too expensive to be used in large production volumes.

[0013] In addition to PHA and PBS, other common bioplastics which can be used in compounds for the production of coffee capsules are poly(butylene succinate adipate) (PBSA), poly(butylene succinate sebacate) (PBSe), and poly(butylene succinate terephthalate) (PBAT). The problem in using these materials lies in being copolymers of the monomer 1,4-butanediol, and in that during the operations of mixing in the melt and subsequent forming by injection or compression moulding or during extrusion into sheets by thermoforming, their degradation by hydrolysis can give rise to tetrahydrofuran (THF), or a substance classified as a suspected carcinogen in category A3.

[0014] PLA is a polyester which has gained popularity thanks to its economic production from renewable resources, being derived from the dextrose extracted from biomass, and is best suited to replace petroleum-derived materials thanks to its availability, biodegradability and lower cost with respect to other bioplastics. PLA products can be composted in industrial composting plants, where temperature (>60°C) and humidity (min 60% RH) can be controlled, according to the standard EN13432. The material is hygroscopic and in most cases requires pre-drying before processing to avoid hydrolysis during the process. Below 60°C, the temperature corresponding to its glass transition (Tg), the PLA degrades very slowly, as the diffusion of water in the glassy amorphous regions is limited, and this slows down hydrolysis, which is the key step of the biodegradation process.

[0015] Therefore, objects in PLA do not degrade in the time required for biodegradation in seawater (pelagic zone, according to ASTM D6691 and ISO 23977) or for domestic composting according to European standard EN 17427.

[0016] The technical specifications required for a polymeric material suitable in the food sector, in particular in infusion capsules, are very strict. In addition to suitability for food contact and compression and injection moulding, as well as extrusion into sheets for thermoforming, the material must have a high thermal resistance, i.e. with a temperature resistance value (thermal deformation temperature or heat deflection temperature or HDT), according to the standard ISO 75- IB, higher than 90°C. It must also be industrially compostable (OK Compost Industrial) according to the standard EN 13432 for thicknesses up to 1.2 mm. Another important aspect for a material suitable for food packaging is to provide an effective gas barrier, keeping the aroma of the contained products, especially that of coffee, unchanged. These specifications are not easily reached with normal PLA, as it is a material that tends to crystallise very slowly and,in common moulding or compression and extrusion processes, does not reach a crystallinity percentage such as to develop the required thermal resistance. Furthermore, PLA is characterized by low barrier properties.

[0017] Currently, to obtain the necessary crystallinity and thermal resistance, the state of the art envisages a subsequent annealing treatment, typically at temperatures above 80°C, in ovens or by means of infrared lamps.

[0018] A further difficulty in achieving the technical specifications required for a polymeric material suitable for food contact, for example for infusion capsules, is the fact that the biodegradation rate depends on the thickness: the thicker the product, the longer the time required for its biodegradability, and even longer for a semi-crystalline material.

[0019] Therefore, at the state of the art, developing a PLA-based material, free of potentially toxic substances, suitable for food contact, industrially compostable for thicknesses up to 1.2 mm, with a high gas barrier and with HDT above 90°C, is a particularly demanding challenge.

[0020] In view of the above, the need is still felt to provide an alternative, environmentally friendly, non-toxic material with excellent thermal and mechanical and gas barrier properties, responding to the growing need for biodegradable materials in different applications, in particular in the field of moulded products, including in the food sector, for example for infusion capsules.

[0021] Shikha et al. in Macromolecular Materials and Engineering, 2010, 295, 750-762 describe PLA / PCL blends with -40% PCL and low talc content (<5%) employed to obtain biodegradable flexible films. The compositions described therein do not provide guarantees of compostability at 1200 pm and do not guarantee EN13432 compliance on typical capsule thicknesses. The amounts of talc used (5%) are not able to raise the HDT to ~130°C and the high amount of PCL determines unsuitable mechanical properties for compostable capsules (flexibility and poor rigidity).

[0022] Biodegradable PLA-based polymer compositions are described in Arrieta et al., Carbohydrate Polymers, vol 107, 2024, 16-24, US 2024 / 132716, WO 2023 / 194663, WO 2024 / 074561, Chen Li. et al., J. of Thermal Analysis and Calorimetry Vol. 139 82), 2029, 1069-1090, EP 4 624529.

[0023] These compositions, in addition to the use of components with potential toxicity such as aliphatic polyesters (PBS, PBSA, PBAT or PBSeT), do not have satisfactory thermal stability and mechanical, barrier and compostability properties.

[0024] Summary of the invention

[0025] The present invention relates to a compostable polymer blend free of 1,4-butanediol polyesters and polyhydroxyalkanoates, comprising or consisting of:

[0026] - poly-lactic acid (PLA);

[0027] - at least one polylactone in percentage by weight from 10 to 20% ;

[0028] - 5 to 40 % w / w talc as a nucleating agent accelerating PLA crystallisation; and

[0029] - optionally a further additive selected from:

[0030] - organic, vegetable and / or animal fibres;

[0031] - polyprotic organic acids and salts thereof;

[0032] - inorganic additives; and combinations thereof.

[0033] - secondary organic nucleants accelerating the cold crystallisation of PLA.

[0034] The invention further relates to a compostable polymeric product, preferably a capsule, having a body comprising the compostable polymer blend of the invention.

[0035] The invention further relates to a process for preparing a compostable polymer product comprising or consisting of the steps of:

[0036] 1) providing the compostable polymer blend of the invention;

[0037] 2) injecting or compression moulding the final product or extrusion into sheets for subsequent thermoforming.

[0038] The invention further relates to a compostable polymeric product obtainable or obtained by the aforesaid process and finally the use of the blend of the invention, as a compostable polymer employable, for example, for moulding compostable products, preferably in the food sector, more specifically in the body of compostable capsules, for example of coffee.

[0039] Brief description of the Figures

[0040] Figure 1: depicts an FT-IR spectrum of the blend according to Example 1.

[0041] Figures 2A-H: photographs of the samples used in the test of Example 12.

[0042] Detailed description of the invention

[0043] It has surprisingly been found that it was possible to overcome the existing disadvantages by means of novel polymer blends based on poly-lactic acid (PLA), which do not develop THF during extrusion, their moulding and subsequent use in the food sector, for example in the body of compostable capsules for coffee, having accelerated degradation thanks to the use of additives which reduce the induction time of PLA biodegradation.

[0044] Furthermore, after injection or compression moulding or extrusion into sheets for thermoforming, these new PLA-based polymer blends demonstrate a temperature resistance (heat deflection temperature or HDT) greater than 90°C, without the need for an additionalannealing treatment with a clear advantage in terms of production time and costs. Finally, these new polymer blends based on poly-lactic acid (PLA) have very high barrier property values, i.e. very low permeability values, with respect to oxygen and water vapour.

[0045] In the present invention, the term

[0046] "compostable" means compliant with the certification criteria of the standard UNI EN 13432:2002: "Packaging - Requirements for packaging recoverable through composting and biodegradation — Test scheme and evaluation criteria for the final acceptance of packaging” ; Therefore, the present invention relates to a compostable polymer blend free of 1,4-butanediol polyesters comprising or consisting of:

[0047] - poly-lactic acid (PLA);

[0048] - at least one polylactone in percentage by weight from 10 to 20% ;

[0049] - 10 to 40 % w / w talc as a nucleating agent accelerating PLA crystallisation; and

[0050] - optionally a further additive selected from:

[0051] - organic, vegetable and / or animal fibres;

[0052] - polyprotic organic acids and salts thereof;

[0053] - inorganic additives; and combinations thereof.

[0054] - secondary organic nucleants accelerating the cold crystallisation of PLA; and combinations thereof.

[0055] Preferably, the poly-lactic acid (PLA) is comprised in the compostable polymer blend of the invention in an amount from 50% to 75%, preferably about 58.3% w / w with respect to the total polymer blend.

[0056] Poly-lactic acid (PLA) is a polymer of lactic acid, obtained from the ring-opening polymerisation (ROP) of two optical isomers: L-lactide (predominant) and D-lactide.

[0057] Preferably, the D-lactide content is between 0.1 and 1.4% w / w with respect to the total weight of the polymer, more preferably it is 0.3%.

[0058] Also preferably, the weight- average molecular weight (Mw) of the poly-lactic acid (PLA) is between 50 - 300 KDa, more preferably between 100 - 200 KDa, even more preferably 140 - 180 KDa.

[0059] The PLA Melt Flow Index (MFI) value (tested at about 210 °C under a 2.16 kg load according to the standard ISO 1133 or ASTM D1238) is preferably between 10 and 40 g / 10 min, more preferably 24 g / 10 min.

[0060] Talc, in the form of small solid particles in molten PLA, during the cooling process, allows the molecular chain of the PLA to adsorb and create an ordered arrangement with

[0061] formation of nuclei, reducing the energy barrier for nucleation, promoting the formation of smaller and more uniformly dispersed crystalline structures in the PLA.

[0062] Talc has the function of both reinforcing filler, that is, it is capable of determining an increase in the elastic modulus of the final polymer blend, and of nucleating agent and inorganic additive. Furthermore, it has a low cost and has been included by the EFSA (European Food Safety Authority) in the positive list of substances suitable for food contact (Food Contact Materials - FCMs), i.e. plastic additives which can be used in polymers in food contact applications.

[0063] Preferably, the talc has a particle diameter of less than 3 pm, more preferably in a range from 2 pm to 0.2 pm, even more preferably from 1 pm to 0.5 pm.

[0064] Particle sizes of less than 3 pm ensure its uniform distribution within the polymer blend.

[0065] Examples of talc usable in the present invention are Imifabi HTP ultra 5c® with dimensions of 0.5 pm.

[0066] Talc is preferably comprised in the compostable polymer blend of the invention in an amount most preferably from 20 to 40%, even more preferably from 30 to 40%, in particular 30% w / w with respect to the total of the polymer blend.

[0067] Examples of polylactones include polycaprolactone (PCL), polybutyrolactone (PBL), poly valerolactone (PVL), preferably polycaprolactone (PCL

[0068] Preferably, the polycaprolactone (PCL) is comprised in the compostable polymer blend of the invention in an amount from 10% to 20% w / w, preferably from 15 to 30%, more preferably about 11.7% w / w with respect to the total polymer blend.

[0069] The optional further additive is selected from

[0070] - organic, vegetable and / or animal fibres;

[0071] - polyprotic organic acids and salts thereof;

[0072] - inorganic additives; and combinations thereof.

[0073] - secondary organic nucleants accelerating the cold crystallisation of PLA; and combinations thereof.

[0074] These further additives are intended to promote the biodegradation of the PLA in the blend, through mechanical or catalytic action, thereby improving the environmental impact of the PLA-based materials used for the production of injection moulded and thermoformed products.

[0075] Preferably, when the optional additive is organic fibres, they are selected from vegetable fibres, for example cellulose, cotton, flax, ramie, sisal, and / or animal fibres, for example wool, silk, cashmere. More preferably they are vegetable fibres, even more preferably it is cellulose.

[0076] Organic, vegetable and / or animal fibres predominantly have a physical-mechanical function in that, by absorbing water, they increase in volume and cause the formation of internal stresses to the material which cause microcracks and subsequent breaks in the product during the composting phase, accelerating the process of fragmentation and disintegration.

[0077] When present, the optional additives in the form of organic fibres are comprised in the compostable polymer blend of the invention in an amount from 5 to 20% w / w, preferably 10% w / w with respect to the total polymer blend.

[0078] When present in the form of organic fibres, the optional additives have the advantage of accelerating the degradation of the PLA, since they swell when in contact with an aqueous environment, causing internal cracks to the moulded material and thus facilitating the fragmentation and subsequent degradation of the polymer, thereby improving the compostability of the product using the blend of the invention.

[0079] Preferably, when the optional additive is polyprotic organic acids and salts thereof, they are selected from citric acid, malic acid and salts thereof, more preferably they are selected from citric acid, malic acid, even more preferably citric acid.

[0080] The polyprotic organic acids and the salts thereof catalyse the hydrolysis reaction resulting in a significant reduction in the incubation phase due to the cleavage of the polymer chains, i.e. the crucial phase of the entire biodegradation process.

[0081] When present, optional additives in the form of polyprotic organic acids are comprised in the compostable polymer blend of the invention in an amount from 0.5 to 5% w / w, preferably 2% w / w with respect to the total polymer blend.

[0082] When present in the form of polyprotic acids, the optional additives have the advantage of dissociating in an aqueous environment, releasing hydrogen ions, capable of activating and accelerating the biodegradation process of the polymer.

[0083] Preferably, when the optional additives are inorganic additives, they are selected from wollastonite, bentonite, hydrotalcite, such as for example hydrotalcite MgAl citrate, hydrotalcite MgAl azelate and hydrotalcite MgAl stearate, nanoclay, such as for example montmorillonite, halloysite nanotubes, carbon nanotubes and possibly functionalised graphene, preferably from wollastonite and hydrotalcite, such as for example hydrotalcite MgAl citrate, hydrotalcite MgAl azelate and hydrotalcite MgAl stearate.

[0084] They are generally intended to accelerate and / or catalyse the cleavage of polymer chains in biodegradable materials, and / or introduce defects in the polymer network, such as microfractures or porosity, increasing the hydrophilicity and therefore the surface exposed to water, thus promoting the hydrolysis of PLA.

[0085] Furthermore, the release of metal ions contributes to the possible increase in pH, which favours a faster degradation with respect to neutral or acidic environments, since the basic conditions favour the breakage of the PLA ester bonds.

[0086] When present, the optional additives in the form of inorganic additives are comprised in the compostable polymer blend of the invention in an amount from 5 to 15% w / w, preferably 10% w / w with respect to the total polymer blend.

[0087] When present in the form of inorganic additives, the optional additives also have the advantage of acting as reinforcing fillers, capable of acting as fillers within the polymer blend of the invention and thus improving the final mechanical properties thereof, and at the same time accelerating the biodegradation process by means of either mechanical stresses (e.g. bentonite) or catalysis of the hydrolysis reaction (e.g. wollastonite).

[0088] Preferably, when the optional additive is a secondary organic nucleant, it is selected from aliphatic amides and aromatic amides, in particular from ethylene bis-stearamide (EBS), ethylenebis(12-hydroxystearamide) (EBH), N,N’-ethylenebis (10-undecenamide) (EBU), N,N’,N” -tricyclohexyl-l,3,5-benzenetricarboxylamide (TMC-328), potassium dimethyl 5- sulfonateisophthalate (LAK-301), and combinations thereof, more preferably ethylene bis-stearamide (EBS).

[0089] The secondary organic nucleants have the function of promoting the cold crystallisation of the PLA during the thermoforming process. In this process, the extruded film is heated above the glass transition temperature (Tg, about 60°C) of the PLA, but below its melting temperature (Tm, about 150-180°C), making it deformable. Under these conditions, the secondary organic nucleants provide nucleation sites which lower the energy barrier to crystallisation, allowing the PLA chains to organise into crystalline structures more quickly with respect to PLA devoid of such additives. Thereby, the material develops a crystallinity of more than 50% during thermoforming, sufficient to give the final product a heat deflection temperature (HDT) greater than 100°C, without the need for an additional annealing treatment.

[0090] When present, optional additives in the form of secondary organic nucleants are comprised in the compostable polymer blend of the invention in an amount from 0.5 to 5% w / w, preferably 1 to 3% w / w with respect to the total polymer blend.

[0091] The use of secondary organic nucleants allows, in particular in the sheet extrusion process and subsequent thermoforming, to reduce the talc content with respect to formulations optimised for injection or compression moulding. While for injection or compression moulding a talc content of 20 to 40% w / w is preferred to ensure the required HDT (PLA crystallisation is limited by the short residence time in the mould), in the extrusion / thermoforming process, thepre-thermoforming heating phase occurring above the Tg and in longer times activates cold crystallisation and allows to reach HDT above 100°C even with lower talc contents, between 5 and 20% w / w, preferably around 10% w / w, as long as a secondary organic nucleant is present. This reduction in talc content reduces the brittleness of the film during thermoforming, improving industrial processability.

[0092] A composition free of 1,4-butanediol polyesters means a composition free of polyesters such as PBS, PBSA, PBAT or PBSeT. The compositions of the invention are also free of poly hydroxy alkanoates (PHA).

[0093] The compostable polymer blend of the invention preferably has a maximum tensile stress value, measured according to the ISO 527-1 A standard, in a range from 30 to 70 MPa, preferably from 50-53 MPa.

[0094] The compostable polymer blend of the invention preferably has a maximum deformation value, measured according to the ISO 527- 1 A standard, in a range from 0.5% to 10%, preferably from 0.9 to 1%.

[0095] The compostable polymer blend of the invention preferably has a tensile modulus value, measured according to the ISO 527-1 A standard, in a range from 5 GPa to 10 GPa, preferably from 7.6 to 8.5 GPa.

[0096] The compostable polymer blend of the invention preferably has a Charpy impact strength value, measured according to the ISO 179-1 standard, in a range from 2 kJ / m2to 5 kJ / m2preferably from 3.5 to 3.7 kJ / m2.

[0097] The compostable polymer blend of the invention preferably has a Melt Flow Index (MFI) value, measured according to ISO 1133 D, in a range from 2 g / 10 min to 10 g / 10 min, preferably from 4-5 g / 10 min.

[0098] All the values listed above are, as will be evident in the experimental part below, significantly higher than the pure material, thus making it an improved material in terms of mechanical performance, in particular the improved tensile modulus value allows the blend of the invention to be more easily treated with tips or water pressures.

[0099] The compostable polymer blend of the invention preferably has a Melt Flow Index of 2 g / 10 min, preferably greater than 3.5 g / 10 min, as measured in accordance with ASTM D1238.

[0100] The viscosity is therefore preferably sufficiently low to make the blend of the invention easily usable in moulding processes, preferably injection moulding, i.e. able to flow easily within the mould.

[0101] The compostable polymer blend of the invention has a heat deflection temperature (HDT) above 90°C, preferably above 100°C, more preferably above 129°C, measured according toASTM D 648 (0.45 MPa at 120°C / h) and ISO 75- IB, thus making it suitable for use as a material in the food sector, for example in the body of coffee capsules, and at the same time suitable for use in moulding processes, preferably injection moulding and / or extrusion into sheets for thermoforming.

[0102] In fact, the water used in the production of coffee has a temperature of about 90°C, and therefore the capsule (and the material forming it) should preferably not change its dimensions during the process.

[0103] Furthermore, the melting temperature in the range described above guarantees a lower probability that the material will negatively affect the coffee aromas which develop during the process, thus being usable in the food sector, for example in coffee capsules.

[0104] The same range lastly ensures that the blend of the invention can be easily melted without subsequent deterioration during, for example, moulding processes.

[0105] The compostable polymer blend of the invention is preferably insoluble in water and preferably has a flammability temperature greater than 388eC, a decomposition temperature preferably greater than 350eC, and a specific weight preferably of 1.3 kg / m3, as per CFR directives: 1910.1200: 2012, ANSI Z400.1-2010 and ISO1101-1: 2009.

[0106] The polymer blend of the invention preferably has an O2 permeability value of less than 0.10 cm3 / m224h and a water permeability value of less than 0.9 cm3 / m2-24h. Therefore, these new polymer blends based on poly-lactic acid (PLA) have very high barrier property values, i.e. very low permeability values, with respect to oxygen and water vapour.

[0107] Furthermore, the polymer blend of the invention is composed of at least 50% raw materials from a biological source, and is biodegradable under industrial composting conditions, and non-toxic, since there are no effects noted after ingestion or contact with the skin.

[0108] Due to its composition, therefore, the compostable polymer blend of the invention and the products derived therefrom are considered practically non-harmful for ingestion and nonirritating in contact with the skin and eyes and non-hazardous according to the following regulations: ADR / RID, IMO, IATA.

[0109] In fact, the blend of the invention and the products derived therefrom are biologically inert and therefore do not present genotoxicity, carcinogenic effects and toxicity for reproduction.

[0110] The invention further relates to a compostable polymeric product, preferably a capsule, having a body comprising the compostable polymer blend of the invention.

[0111] Preferably, the capsule body has a thickness of 1.2 mm or less.

[0112] The aforesaid capsule, obtained from the compostable polymer blend of the invention, can be classified as packaging according to the Packaging and Packaging Waste Regulation (PPWR) approved on 16 December 2024 by the EU Council and officially published in the Official Journal of the EU on 22 January 2025, and was found, also thanks to the composition of the compostable polymer blend of the invention, to comply with the certification criteria of the standard UNI EN 13432:2002: "Packaging — Requirements for packaging recoverable through composting and biodegradation — Test scheme and evaluation criteria for the final acceptance of packaging" .

[0113] The invention further relates to a process for preparing a compostable polymer product comprising or consisting of the steps of:

[0114] 1) providing the compostable polymer blend of the invention;

[0115] 2) injecting or compression moulding the final product or extrusion into sheets for subsequent thermoforming.

[0116] Preferably, the final product has a thickness of 1.2 mm or less. Preferably, step 1) occurs in an extruder, for example a twin-screw extruder, more preferably having a temperature profile with eleven zones, even more preferably as follows: 165°C, 175°C, 185°C, 185°C, 185°C, 175°C, 175°C, 175°C, 170°C, 160°C and 155°C, in which the die zone is at 155°C.

[0117] Preferably, step 2) occurs by injection moulding, for example in a Megatech H10 / 18 press.

[0118] Alternatively, when step 2) envisages extrusion into sheets for subsequent thermoforming, the process comprises the following sub-steps: (a) extrusion of the polymer blend into sheets or plates, preferably of thickness between 400 and 800 pm, more preferably about 600 pm, on cooling and calendering rollers, with collection in coils; (b) heating the extruded sheet to a temperature between the glass transition temperature (Tg) and the melting temperature (Tm) of the PLA, preferably between 80°C and 140°C, so as to make it deformable and promote the cold crystallisation of the PLA; and (c) thermoforming the sheet to shape the final product, preferably capsules or containers for food. In this process path, the presence of a secondary organic nucleant in the blend promotes cold crystallisation during step (b), allowing the PLA to achieve a crystallinity greater than 50% and an HDT greater than 100°C in the final product.

[0119] More preferably, the moulding conditions were:

[0120] temperature profile: 180°C, 185°C, 190°C;

[0121] mould temperature: 60°C;

[0122] injection holding time: 5 s

[0123] cooling time: 15s; and

[0124] injection pressure: 90 bar.

[0125] A further object of the invention is a compostable polymeric product obtainable or obtained by the aforesaid process.

[0126] Finally, a further object of the invention is the use of the blend as a compostable polymer employable, for example, for moulding compostable products, preferably in the food sector, more specifically in the body of compostable capsules, for example of coffee.

[0127] All the embodiments according to the present invention may be combined with one another. The following examples further illustrate the invention.

[0128] EXAMPLES

[0129] Example 1 - Preparation of the compostable polymer blend of the invention

[0130] 2915 g of Ingeo 3100HP PLA fromNatureworks in granules and 585 g of CAPA 6500D PCL from Ingevity in granules and 1500 g of HiTalc Premium HTP 05c talc from IMI - FABI S.p.A. in powder were provided and extruded in a Comae EBC 25HT extruder (L / D = 44) (Comae, Cerro Maggiore, Italy) with a temperature profile between 155°C and 185°C. In particular, the temperature profile of the extruder (11 zones) used for the preparation of the blends was: 165°C, 175°C, 185°C, 185°C, 185°C, 175°C, 175°C, 175°C, 170°C, 160°C and 155°C, in which the die zone is at 155°C. The PLA and PCL granules, after having optionally been dried with dry air at a temperature lower than 55 °C for at least 8 h, with a Piovan DP 604-615 dryer (Piovan S.p.A., Verona, Italy), were pre-blended and loaded into the main loader while the talc was distributed between the two side loaders. The molten blend after extrusion was collected in the form of filaments and cooled with a cold water bath and these filaments, after being dried, were transformed into granules by means of a cutter and subsequently dried before bagging, again with the Piovan dryer. The blend was injection moulded with a Megatech H10 / 18 press (TECNICA DUEBI s.r.l., Fabriano, Italy), to obtain three types of samples: samples for tensile tests according to ISO 527-1A (width: 10 mm, thickness: 4 mm, length: 80 mm) and Charpy parallelepiped samples for the Charpy impact test according to ISO 179 (width: 10 mm, thickness: 4 mm, length 80 mm) and 50x50x1.2 mm square sheets for composting tests. After injection moulding, the Charpy samples were cut with a hand cutter to produce a V-notch in the centre (V-notch: 2 mm at 45°). The moulding conditions were: temperature profile: 180 / 185 / 190 °C; mould temperature: 60°C; injection holding time: 5 s; cooling time: 15 s; injection pressure: 90 bar.

[0131] Example 2 - FT-IR qualitative and thickness analysis of the blend of the invention according to Example 1

[0132] An FT-IR analysis was carried out on the compostable polymer blend of the invention in order to identify the polymer which constitutes the sample. The analysis was performed considering the homogeneous sample and composed of a single material. The sample was subjected to FT-IR scans in the range from 4000 to 400 cm1by means of the p-ATR technique with diamond crystal.

[0133] The spectrum obtained is shown in Figure 1. The infrared spectrum is characterised by a main peak at 1004 cm'1attributable to the Si-0 bond stretching of talc; another important peak attributable to talc is that at 670 cm'1, due to -OH bending in the MgO / MgOH system. The second peak in the spectrum is at 1748 cm'1and is attributable to the stretching of the C=O bonds in the ester groups, attributable to polylactic acid (PLA). From 1200 cm'1up to 1085 cm'1there are peaks attributable to the stretching vibrations of the C-0 bond of the polyester. There are other signals due to hydrocarbon parts: at 2925 cm'1there are peaks attributable to the asymmetric stretching of CH2 and CH3 and at 2852 cm'1peaks attributable to the symmetric stretching of the CH2 and CH3 bonds. At 1452 cm'1there is a peak attributable to the asymmetric folding of CH2 and CH3 while at 1362 cm'1to the folding of CH2 and CH3. At 754 cm'1the rocking of the CH2 occurs.

[0134] This spectrum thus demonstrates that the blend of the invention therefore consists mainly of PLA and talc. The thickness of a sample of the blend of the invention was subsequently measured by Digital Micrometer - Flat surface - Resolution 0.001 mm and the results are reported in Table 1.

[0135] Table 1

[0136]

[0137] Example 3 - Analysis of the mechanical characteristics of the compostable polymer blend according to Example 1 with respect to a polymer of the known art and analysis of the barrier properties

[0138] The compostable polymer blend of the invention, according to Example 1, was analysed in the form of white granules with a cylindrical shape (diameter and length of about 3 mm). The mechanical properties of the compostable polymer blend were evaluated under the conditions reported in Table 2.

[0139] Table 2

[0140]

[0141] The values analysed and compared with a PLA-based polymer (Ingeo 3100 HP from Natureworks) known in the art are shown in Table 3.

[0142] Table 3

[0143]

[0144] From Table 3 it can be seen that the blend of the invention is characterized by a heat deflection temperature (HDT) which is not only greater than 90°C, without the need for an additional annealing treatment with evident advantage in production time and cost, but even greater than twice the value of the temperature of the polymer of the prior art. Furthermore, the impact strength value is also greater with respect to the polymer of the prior art.

[0145] The compostable polymer blend of the invention according to Example 1 was provided in the form of sheets of dimensions 50 mm x 50 mm and 1200 pm in thickness. The sheets were analysed to determine water vapour (WVTr) and oxygen (OiTr) permeability values.

[0146] The values were measured with the ExtraSolution PermeH2O and ExtraSolution PermeO

[0147] 2 instruments of Permtech S.r.l., Pieve Fosciana (LU) Italy, respectively, according to the standards ASTM F1249 (WVTr) and ASTM F1927 (O2Tr).

[0148] The results are reported in Tables 4 and 5.

[0149] Table 4

[0150]

[0151] Table 5

[0152]

[0153] Tables 4 and 5 demonstrate that the blend of the invention according to Example 1 possesses a high barrier to oxygen and water vapour, i.e. an O2 permeability value of less than 0.10 cm3 / m2-24h and a water permeability value of less than 0.9 cm3 / m224h.

[0154] Example 4 - Preparation of compostable polymer blends of the invention

[0155] Different blends were obtained following the protocol of Example 1 but varying the percentages of the reagents. The samples are shown in Table 6.

[0156] Table 6

[0157]

[0158] Example 5 - Analysis of the mechanical characteristics of the compostable polymer blends of the invention according to Example 4

[0159] The compostable polymer blends of the invention, according to Example 4, were analysed in the form of white granules with a cylindrical shape (diameter and length of about 3 mm). The mechanical properties of the compostable polymer blend were evaluated under the conditions reported in Table 2 in Example 3, and the results are reported in Table 7.

[0160] Table 7

[0161]

[0162] All samples were found to be suitable and characterised by a heat deflection temperature (HDT) far greater than 90°C.

[0163] Example 6 - Preparation of compostable polymer blends of the invention with addition of further additives in the form of polyprotic acids

[0164] Different blends were obtained following the protocol of Example 1 but varying the percentages of the reagents and adding as a further additive a polyprotic acid, i.e. citric acid. The purpose was to optimise the polymer blend of the invention, obtaining a blend with high HDT and therefore resistant to operating temperatures, but with a higher degradation rate during composting, thanks to the presence of polyprotic acid, a degradation catalyst in the aqueous environment.

[0165] The samples are shown in Table 8.

[0166] Table 8

[0167]

[0168]

[0169] Example 7 - Mechanical tests of compostable polymer blends of the invention according to Example 6

[0170] The compostable polymer blends of the invention, according to Example 6, were analysed in the form of white granules with a cylindrical shape (diameter and length of about 3 mm). The mechanical properties of the compostable polymer blends were evaluated under the conditions reported in Table 2 in Example 3, and the results are reported in Table 9.

[0171] Table 9

[0172]

[0173] The analyses of Table 9 show that a polymer blend of the invention was obtained with a high HDT (always greater than 90°C) and therefore resistant to operating temperatures, but with a higher degradation rate during composting, thanks to the presence of polyprotic acid, a degradation catalyst in an aqueous environment.

[0174] Example 8 - Preparation of compostable polymer blends of the invention with addition of further additives in the form of inorganic additives

[0175] Different blends were obtained following the protocol of Example 1 but varying the percentages of the reagents and adding as a further additive an inorganic additive, namely wollastonite, specifically Wollastonite Tremin 939 from HPF Minerals Italia S.r.l. with a

[0176] needle-shaped structure coated with an organosilicon compound with a 6-7 / 1 needle length / diameter ratio (wolla-939) and Wollastonite Tremin 283 (wolla-283) with coarser particle size, hydrotalcite MgAl citrate, hydrotalcite MgAl azelate and hydrotalcite MgAl stearate. The purpose was to optimise the polymer blend of the invention, obtaining a blend with high HDT and therefore resistant to operating temperatures, but with a higher degradation rate during composting, thanks to the presence of inorganic additives, catalysts for the cleavage of polymer chains in biodegradable materials.

[0177] The samples are shown in Table 10.

[0178] Table 10

[0179]

[0180] Example 9 - Mechanical tests of compostable polymer blends of the invention according to Example 8

[0181] The compostable polymer blends of the invention, according to Example 8, were analysed in the form of white granules with a cylindrical shape (diameter and length of about 3 mm). The mechanical properties of the compostable polymer blends were evaluated under the conditions reported in Table 2 in Example 3, and the results are reported in Table 11.

[0182] Table 11

[0183]

[0184] The analyses in Table 1 show that a polymer blend of the invention was obtained with high HDT (always greater than 90°C) and therefore resistant to operating temperatures, but with a higher degradation rate during composting, thanks to the presence of inorganic additives,capable of promoting the degradation of PLA.

[0185] Example 10 - Migration test of the compostable polymer blend of the invention according to Example 1

[0186] On specimens of the compostable polymer blend of the invention, analyses were carried out to verify compliance with current legislation on plastic objects, i.e. Italian Ministerial Decree 21.3.73 and subsequent updates and amendments, Reg. (EU) No. 10 / 2011 and subsequent updates and amendments, Reg. (EC) No. 1935 / 2004, with application by contact with high temperature coffee (ARCHA code No. 22304434 / 1) relating to global migrations in food simulants. The determination of the total migration was carried out with the non-specific weight quantification of the substances which are released from the packaging during contact with the simulants. The legislation relating to plastic materials provides for a maximum limit of 10 mg / dm2.

[0187] The simulants to be used were selected based on the characteristics of the food for which it is intended, in particular the simulant liquids shown in Table 12 were used.

[0188] The test conditions, i.e., duration and temperature, were selected according to the actual use, i.e. the tests were conducted at 100°C, for 5 minutes and included the complete immersion of 1 sample for each glass container with lid.

[0189] The specimens were prepared in the form of a paddle, having a contact surface of 0.224 dm2. 40 ml of simulat liquid were used and the surface area / volume ratio was 5.6 dm2 / !. Table 12 below describes the conditions used.

[0190] Table 12

[0191]

[0192] The tests were repeated in triplicate for each specimen and the mean values of the results of the measurements are shown in Table 13.

[0193] Table 13

[0194]

[0195] Based on the results of the checks carried out, the compostable polymer blend samples of the invention comply with national and European legislation relating to contact with food, i.e. Italian Ministerial Decree 21.3.73 and subsequent updates and amendments, REG. (EU) No. 10 / 2011 and subsequent updates and amendments as well as REG. (EC) No. 1935 / 2004 with the simulants water, acetic acid and ethanol under the test conditions used.

[0196] Example 11 - Analysis of the heavy metal content of the compostable polymer blend of the invention according to Example 1

[0197] The granular samples of the blend of the invention were analysed to detect the content of any heavy metals, which would render the product toxic according to the standards EN 13432 for metals and ISO 17088 for Cobalt.

[0198] The values detected are reported in Table 14.

[0199] Table 14

[0200]

[0201] The values detected in the analysed sample and reported in Table 14 are therefore in compliance with the limits set forth in EN 13432. The value of Cobalt is compliant with the standard ISO 17088.

[0202] Example 12 - Determination of the degree of disintegration of the compostable ir blend of the invention according to Example 1 under composting conditions according to ISO 16929:2021

[0203] Disintegration testing under defined conditions of pilot scale composting is a standardised composting process. The analysis is carried out in composting containers of sufficiently high volume to allow the natural self-heating process. The bins are made of non-biodegradable and heat-resistant material so as not to affect the composting process or the quality of the compost and have a grille on the bottom to facilitate air flow. The reactors are equipped with a humid forced air system. The set-up of the test consists of two steps:

[0204] - the preparation of the test sample; and

[0205] filling the composting reactors.

[0206] The test material is used in a shape (thickness and weight) identical to that of the intended end use. Plates of compostable polymer blend were prepared according to Example 1, of size 5 cm x 5 cm and thickness 1225 ± 25 pm, and having a total solids content of 99.95 ± 0.78 w / w according to EN13432 and a moisture content of 0.05% w / w according to EN13432.

[0207] The reactors are then prepared by filling them in precise proportions with a standard recipe, containing fresh compost, fresh organic waste with a ubiquitous natural microbial population, and structural material, and mixing everything with the test sample.

[0208] For all reactors or reactor networks with organic waste and the blend of organic waste and test material, the following conditions are used:

[0209] the samples are studied for 12 weeks;

[0210] between the 2nd and 7th day of testing the temperature is between 60°C and 75°C; between the 8th and the 28th day of testing the temperature is between 55±5°C and 65±5°C;

[0211] between the 29th and 56th day of testing the temperature is between 50±5°C and 60±5°C;

[0212] between the 57th and 70th day of testing, the temperature is below 45°C; between the 71st and 84th day of testing, the temperature is below 45°C;

[0213] the pH during the test rises above 7 but never falls below 5; and

[0214] the control compost shows a maturity (Rottegrad) of IV or V on the scale after 12 weeks.

[0215] The organic compost waste used derives from an industrial composting plant which mainly treats the organic fraction of municipal solid waste, or alternatively from domestic waste or from the union of both. Before starting the composting process, in order to obtain a product with the desired characteristics, it is necessary to mix the different matrices intended as freshcompost and organic waste in appropriate proportions. The compost used for the analysis complies with the parameters of the standard ISO 16929, namely:

[0216] - it was sieved at 50 mm;

[0217] - it consists of 25% pruning residues and 5% wood flakes, to which a 1:5 solution of inoculum (i.e. mature compost) in water with a pH of 5.10 ± 0.20 has been added;

[0218] - it has a C / N value (ratio between the amount of carbon (C) and the amount of nitrogen (N) present in the organic material) of 22.1;

[0219] - it has a moisture content, measured according to the standard EN13432 at 105eC, of 64.7 ± 0.78;

[0220] - a volatile solids content, measured according to the standard EN13432 of 77.1% w / w.

[0221] 20 kg wet weight of the compost was used in a total reactor volume of 50 L (isolated, having a reactor aeration system, regulating the incoming air humidity and the incoming air flow) and in a useful volume of 42 L, and 202 g of compostable polymer blend plates of the invention were added, with a mixing ratio of the wet organic waste and sample of 1%.

[0222] The temperature was checked once a day, the oxygen concentration (%) in the outgoing air was measured every day for the first 30 days and once a week thereafter, the pH was checked at each stirring, the humidity (%) was measured at each stirring (> 40% w / w), the stirring took place weekly for the first 4 weeks and followed every 2 weeks until the end of the test and the photos shown in Figures 2A-H, were taken with each stirring. The plates were tested for 12 weeks and the w / w % (dry weight) disintegration of the test material (< 2 mm) was calculated. The test threshold value, according to EN13432 is > 90 w / w %.

[0223] The test showed that a sample of the blend of the invention according to Example 1, after 84 days (12 weeks) from the start of the test according to the standard ISO 16929:2021, reported a disintegrated fraction of 94.6 ± 14.2 % w / w on dry weight, and a non-disintegrated fraction of 5.4 % w / w on dry weight. The test is considered as passed according to the standard EN 13432 if the threshold value of 90% w / w is reached. The average of the values obtained in duplicate was 94.6% w / w, thus resulting in a suitable material for disintegration in the composting process. The organic substance, analysed according to the standard UNI EN 13432:2002, was composed of a dry residue of 99.95 ± 0.78 g / 100 g, ash at 550°C of 28.95 ± 0.18 g / 100 g and volatile solids of 71.00 ± 0.80 g / 100.

[0224] Table 15 shows the measurements taken in duplicate and the photographs of the samples.

[0225] Table 15

[0226]

[0227] The temperature monitored corresponded to that desired, the concentration of oxygen inside the composting material was always greater than 10% and the control compost has a maturity (Rottegrad) equal to IV of the scale after 12 weeks.

Claims

CLAIMS1. A compostable polymer blend free of 1,4-butanediol polyesters comprising or consisting of:- poly-lactic acid (PLA);- at least one polylactone in percentage by weight from 10 to 20% ;- 5 to 40 % w / w talc as a nucleating agent accelerating PLA crystallization;- optionally a further additive selected from:- natural, vegetable and / or animal fibres;- polyprotic organic acids and salts thereof;- inorganic additives; and combinations thereof;- secondary organic nucleants accelerating the cold crystallisation of PLA; and combinations thereof.

2. The compostable polymer blend according to claim 1, wherein the polylactone is polycaprolactone.

3. The compostable polymer blend according to claim 1 or 2, wherein the fibres are selected from cellulose, cotton, linen, ramie, sisal, wool, silk, cashmere, preferably cellulose.

4. The compostable polymer blend according to any one of claims 1-3, wherein the polyprotic organic acids are selected from citric acid, malic acid preferably citric acid.

5. The compostable polymer blend according to any one of claims 1-4, wherein the optional inorganic additive is selected from wollastonite, hydrotalcite MgAl citrate, hydrotalcite MgAl azelate, hydrotalcite MgAl stearate, nanoclays, such as for example montmorillonite, halloysite nanotubes, carbon nanotubes and possibly functionalised graphene, preferably from wollastonite, hydrotalcite MgAl citrate, hydrotalcite MgAl azelate and hydrotalcite MgAl stearate.

6. The compostable polymer blend according to any one of claims 1-5, having a heat deflection temperature (HDT) greater than 90°C, preferably greater than 100°C, more preferably 129°C, measured according to ASTM D 648 and ISO 75- IB.

7. The compostable polymer blend according to any one of claims 1-6, having a Melt Flow Index (MFI) value, measured according to the standard ISO 1133 D, in a range from 2 g / 10 min to 10 g / 10 min, preferably from 4-5 g / 10 min.

8. The compostable polymer blend according to any one of claims 1-7, having an O2 permeability value of less than 0.10 cm3 / m2-24h and a water permeability value of less than 0.9 cm3 / m2-24h.

9. The compostable polymer blend according to any one of claims 1-8, wherein theoptional further additive comprises a secondary organic nucleant selected from ethylene bisstearamide (EBS), ethylene bis(12-hydroxystearamide) (EBHSA), N,N’,N”-tricyclohexyl- I,3,5-benzenetricarboxylamide (TMC-328), potassium dimethyl 5-sulfonate isophthalate (LAK-301), and combinations thereof.

10. The compostable polymer blend according to claim 9, wherein the secondary nucleant is present in an amount from 0.5 to 5% w / w with respect to the total polymer blend, and wherein the talc is present in an amount from 5 to 20% w / w with respect to the total polymer blend.II. A compostable polymer product, preferably a capsule, having a body comprising the compostable polymer blend according to any one of claims 1-10.

12. A process for preparing a compostable polymer product comprising or consisting of the steps of:1) providing the compostable polymer blend according to any one of claims 1-8;2) injecting or compression moulding the final product or extrusion into sheets for subsequent thermoforming.

13. Use of the compostable polymer blend according to any one of claims 1-10 as a compostable polymer employable for moulding compostable products, preferably in the food sector, more preferably in the body of compostable capsules.

14. A process for preparing a compostable polymeric product by means of extrusion and thermoforming, comprising or consisting of the steps of: (1) providing the compostable polymer blend according to claim 9 or 10; (2) extruding the blend into sheets or slabs of a thickness of 400 to 800 pm, with cooling on rollers and collection in coils; (3) heating the extruded sheet to a temperature between the Tg and Tm of the PLA, preferably between 80°C and 140°C, so as to promote the cold crystallisation of the PLA up to a crystallinity greater than 50%; and (4) thermoforming the sheet to obtain the final product with HDT greater than 100°C.

15. A product obtainable or obtained by the process according to claim 12 or 14.