OPTO-electronic device with silver-based electrode

A silver-based thin film electrode with a low loss composite material and seed layer improves the aperture ratio and reduces sheet resistance in opto-electronic devices, addressing the limitations of FMMs and enhancing device efficiency.

WO2026239264A1PCT designated stage Publication Date: 2026-11-19OTI LUMIONICS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054670
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-08-27
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing opto-electronic devices face challenges in achieving high aperture ratios and low sheet resistance in electrodes while maintaining transparency, often relying on fine metal masks (FMMs) that are costly and limit efficiency.

Method used

The use of a silver-based thin film electrode with a low loss composite material, combined with a seed material to enhance wetting and morphology, allows for selective deposition without FMMs, resulting in a low sheet resistance and high transmittance.

Benefits of technology

This approach enhances the aperture ratio and reduces current resistance losses, improving the efficiency and performance of opto-electronic devices by maintaining low absorption and thin film thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054670_19112026_PF_FP_ABST
    Figure IB2026054670_19112026_PF_FP_ABST
Patent Text Reader

Abstract

An opto-electronic device comprises a plurality of layers deposited on a substrate that extends in a lateral aspect defined by a lateral axis thereof. The plurality of layers defines an emissive region comprising a first electrode, a second electrode, and at least one semiconducting layer disposed between the first electrode and the second electrode. The first electrode is disposed between the substrate and the at least one semiconducting layer. The second electrode comprises a substantially low loss silver (Ag) (composite) thin film coating comprising a first deposited material and a substantially low loss Ag (composite) material. The second electrode exhibits a sheet resistance (Rs), while still exhibiting a transmittance (T) that is substantially high and an average layer thickness that is substantially thin, and absorption (Abs).
Need to check novelty before this filing date? Find Prior Art

Description

PATENT SPECIFICATION - PCTTitle: OPTO-ELECTRONIC DEVICE WITH SILVER-BASEDELECTRODEInventor(s): WANG, Zhibin (Canadian)ZHANG, Yingjie (Chinese)CHANG, Yi-Lu (Canadian)WANG, Qi (Chinese)All of: 3415 American Drive, Unit 1Mississauga, ON L4V 1T4 CanadaAssignee: OTI Lumionics Inc.3415 American Drive, Unit 1Mississauga, ON L4V 1T4CanadaPriority Claims: US 63 / 804,562 12 May 2025US 63 / 871,529 27 August 2025OTI File: 090-03 -WOOPTO-ELECTRONIC DEVICE WITH SILVER-BASED ELECTRODERELATED APPLICATIONS

[0001] The present application claims the benefit of priority to: United States Patent Application No. 63 / 804,562 filed 12 May 2025 and United States Patent Application No. 63 / 871,529 filed 27 August 2025, the contents of each of which are incorporated herein by reference in their entirety.TECHNICAL FIELD

[0002] The present disclosure relates to layered opto-electronic devices having a plurality of sub¬ pixel emissive regions, each sub-pixel comprising first and second electrodes separated by at least one semiconductor layer, in which at least one of: the electrodes, a conductive coating electrically coupled therewith, and transmissive regions therebetween, may be patterned by depositing a patterning coating that may at least one of: act, and be, a nucleation inhibiting coating for patterning at least one conductive deposited material such as may be deposited during a device fabrication process, to form such an electrode, and conductive coating, and to preclude deposition of such deposited material to form such transmissive region(s), including without limitation, by dispensing with the use of fine metal masks (FMM) in depositing one of the first and second electrode layer(s), including without limitation, to increase an aperture ratio corresponding to such emissive regions beyond the limitations of such FMMs.BACKGROUND

[0003] In an opto-electronic device such as an organic light emitting diode (OLED), at least one semiconducting layer, comprising an emissive layer, may be disposed between a pair of electrodes, such as an anode and a cathode. The anode and cathode may be electrically coupled with a power source, and respectively generate holes and electrons that migrate toward each other through the at least one semiconducting layer. When a pair of holes and electrons combine, light, in the form of a photon, may be emitted by the emissive layer.

[0004] OLED display panels, such as an active-matrix OLED (AMOLED) panel, may comprise a plurality of pixels, each pixel further comprising a plurality' of (including without limitation, one of: three, and four) sub-pixels. In some non-limiting examples, the various sub-pixels of a pixel may be characterized by a plurality of different colors, including without limitation, R(ed), G(reen), and B(lue). Each (sub-) pixel may have an associated emissive region, comprising a stack of: an associated pair of electrodes, and at least one semiconducting layer between them. In some non-limiting examples, each sub-pixel of a pixel may emit light, including withoutlimitation, photons, that have an associated wavelength spectrum characterized by a given color, including without limitation, one of, R(ed), G(reen), B(lue), and W(hite). In some non-limiting examples, the (sub-) pixels may be selectively driven by a driving circuit comprising at least one thin-film transistor (TFT) structure electrically coupled with conductive metal lines, in some non¬ limiting examples, within a substrate upon which the electrodes and the at least one semiconducting layer are deposited. Various coatings (layers) of such panels may, in some non¬ limiting examples, be formed by vacuum-based deposition processes.

[0005] In AMOLED panels, light may be emitted by a (sub-) pixel when a voltage is applied across an anode and a cathode thereof. By controlling the voltage applied across the anode and the cathode, it may be possible to control the emission of light from each (sub-) pixel of such panel. In cases where a common cathode is provided across multiple (sub-) pixels, the voltage across the anode and the cathode in each (sub-) pixel may be controlled by modulating the voltage of the anode. In some non-limiting examples, the adjacent anodes may be spaced apart in a lateral aspect, and at least one non-emissive region may be provided therebetween.

[0006] In some non-limiting examples, there may be an aim to provide a conductive deposited layer in a pattern for each (sub-) pixel of the panel across at least one of a: lateral, and cross- sectional, aspect thereof, by selective deposition of a closed coating of a conductive deposited material, to form one of a: device feature, including without limitation, an electrode, conductive element electrically coupled therewith, and region that is substantially devoid of the deposited material, including without limitation, to define a transparent region of the device, during the OLED manufacturing process.

[0007] In some non-limiting examples, the conductive deposited material used to form an electrode may comprise a substantially thin film layer so that the opto-electronic device may be substantially transmissive relative to light incident on an external surface thereof.

[0008] In some non-limiting examples, a reduced thickness of such an electrode may tend to increase a sheet resistance of such electrode, which may, in some non-limiting examples, reduce at least one of the: performance, and efficiency, of the device.

[0009] In some non-limiting examples, an electrode having a high sheet resistance may exhibit a substantially large current resistance (IR) drop in operation, resulting in substantially high current resistance losses. In some non-limiting examples, such an IR drop may be compensated for, to some extent, by increasing a voltage level of a power source thereof. In some non-limitingexamples, such voltage level increase may cause a concomitant increase in a level of a voltage to be suppled to other components to maintain effective operation of the device.

[0010] In some non-limiting examples, a deposited material that may be suitable for selective deposition employing an NIC may comprise silver (Ag). However, in some non-limiting examples, identifying a deposited material comprising Ag for use in an electrode that exhibits substantially low loss has proved challenging.

[0011] In United States Patent Application Publication No. 2011 / 0037062 entitled “Organic Electroluminescent Device” filed 27 February 2009 by FUKUMATSU, Takayuki, etal., and published 17 February 2011, there is disclosed an organic electroluminescent device (organic EL device) which can achieve high efficiency and long lifetime even when driven at low voltage. The organic EL device comprises at least a light-emitting layer and an electron-transporting layer between an anode and a cathode facing each other. The electron-transporting layer consists of two layers, namely, a first electron-transporting layer and a second electron-transporting layer and the first electron-transporting layer and the second electron-transporting layer are arranged sequentially in this order from the light-emitting layer side to the cathode side. The first electron-transporting layer contains an indole derivative in which the ring nitrogen atom is substituted with an aromatic group and an aromatic ring is fused to the indole ring.

[0012] In Taiwan Patent Application Publication No. 200731857 entitled “Cathode of Top Emission Inverted Organic Llight Emitting Diode Using Aluminum Metal Nitriding”, filed 6 February 2006 by JUANG, Fuh-Shyang, el al., and published 16 August 2007, there is disclosed using aluminum metal as the cathode of a top emission inverted device. Aluminum has high reflectivity and can be performed with a microwave plasma nitriding process to form a thin aluminum nitride insulation layer on the surface of the aluminum for increasing the capability of electrons to be injected into the cathode, thereby promoting the light emitting efficiency. In accordance with the manufacturing method of light emitting device, aluminum is used as device cathode, gold / silver dual-layer translucent metal is used as anode, and the structure includes aluminum / aluminum nitride / electron transmission and light emitting layer / electron injection layer / gold / silver, wherein the cathode uses aluminum structure which has a high reflectivity and lower power function. By using this cathode structure to manufacture active top emission inverted organic light emitting diode (TEIOLED) display, it is able to effectively increase the aspect ratio of each pixel, promote the light emitting efficiency, and prolong the lifetime of device.

[0013] In Korean Patent Application Publication No, 10-2013-0116750, entitled “Fabrication method of Top-Emission OLEDs by Using Semi-Transparent Electrode of Thin-Multi -Metal and OLEDs Using by the Method” filed 16 April 2012 by HYUNG, Gun Woo, et al., and published24 October 2013, there is disclosed [machine language translation] the multi layer the transparent film having the high conductivity. And the burden of the expensive manufacturing facility necessary' for the production process the production process is streamlined the damage of plasma is reduced according to the organic electroluminescence element manufacturing method in the oxide film sputtering including the ITO electrode or the IZO electrode etc. and the penetration of the metal electrode solves the problem of the top-emission method using the multimetal thin film formed is reduced The nickel (Ni) in the upper side of the step of forming the thickness the second upper electrode layer of 5nm to 15nm and the second upper electrode layer the step of forming the glass or plastic the substrate the problem according to the addition of the process is resolved and step of forming the thickness of 5nm to lOnm the first bottom electrode layer any one metal among the bottom electrode formed on the upper side of the substrate is the nickel (Ni), the aluminum (Al), the platinum (Pt), the Ti (titanium) and any one metal among the silver (Ag) in the upper side of the first bottom electrode layer, the gold (Au), and the copper (Cu) the step of forming the thickness of 50nm the second bottom electrode layer and any one metal among the nickel (Ni), the aluminum (Al), the platinum (Pt), the Ti (titanium) in the upper side of the second bottom electrode layer the step of forming the thickness the third bottom electrode layer of lOnm to 20nm and step of forming the organic emitting device layer of the multi layer in the upper side of the bottom electrode and any one metal among the upper electrode in the upper side of the organic layer is the nickel (Ni), the aluminum ( Al), the platinum (Pt), the Ti (titanium) the step of forming the thickness the phase 1 negative electrode layer of 2nm to 5nm and any one metal among the silver (Ag) in the upper side of the phase 1 negative electrode layer, the gold (Au), and the copper (Cu), the aluminum (Al), and the platinum (Pt). Any one metal among the Ti (titanium) may be referred to the organic electroluminescent device by the organic electroluminescence element manufacturing method of the top-emission method using the multimetal thin film imply ing and the method thereof the step of forming the thickness the third top electrode layer of 2nm to 5nm.

[0014] In United States Patent No. 7,768,210 entitled “Hybrid Electroluminescent Devices” filed25 May 2007 by SHIANG, Joseph John, et al., and published 3 August 2010, there is disclosed a, hybrid electroluminescent (EL) device that comprises at least one inorganic diode element and atI east one organic EL element that are electrically connected din series. The absolute value of the breakdown voltage of the inorganic diode element is greater than the absolute value of the maximum reverse bias voltage across the series. The inorganic diode element can be a power diode, a Schottky barrier diode, or a light-emiting diode.

[0015] In Schubert, Sylvio, el al... “Improvement of Transparent Metal Top Electrodes for Organic Solar Cells by Introducing a High Surface Energy Seed Layer”, Adv. Energy Mater. 2013, DOI: 10.1002 / aenm.201200903, pp. 1-6, the authors present highly transparent and conductive silver thin films in a thermally evaporated dielectric / metal / dielectric (DMD) multilayer architecture as top electrode for efficient small molecule organic solar cells. DMD electrodes are frequently used for optoelectronic devices and exhibit excellent optical and electrical properties. Here, the authors show that ultrathin seed layers such as calcium, aluminum, and gold of only 1 nm thickness strongly influence the morphology of the subsequently deposited silver layer used as electrode. The wetting of silver on the substrate is significantly improved with increasing surface energy of the seed material resulting in enhanced optical and electrical properties. Typically thermally evaporated silver on a dielectric material forms rough and granular layers which are not closed and not conductive below thicknesses of 10 nm. With gold acting as seed layer, the silver electrode forms a continuous, smooth, conductive layer down to a silver thickness of 3 nm. At 7 nm silver thickness such an electrode exhibits a sheet resistance of 19 Ω / □ and a peak transmittance of 83% at 580 nm wavelength, both superior compared to silver electrodes without seed layer and even to indium tin oxide (ITO). Top-illuminated solar cells using gold / silver double layer electrodes achieve power conversion efficiencies of 4.7%, which is equal to 4.6% observed in bottom-illuminated reference devices employing conventional ITO.The top electrodes investigated here exhibit promising properties for semitransparent olar cells or devices fabricated on opaque substrates.

[0016] In some non-limiting examples, there may be an aim to identify a mechanism to facilitate identification of Ag-based deposited materials that exhibit substantially low loss, including without limitation, for use in, and in some examples, as an electrode in an opto-electronic device.BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Examples of the present disclosure will now be described by reference to the following figures, in which identical reference numerals in different figures indicate at least one of: identical, and in some non-limiting examples, at least one of: analogous, and corresponding elements, and in which:

[0018] FIG. 1 is a simplified diagram, from a longitudinal aspect, of an exampie opto-eiectronic device, according to an example in the present disclosure;

[0019] FIGs. 2A-2E are SEM images of example samples of an opto-electronic device, according to an example in the present disclosure;

[0020] FIG. 3 is a simplified block diagram from a longitudinal aspect, of an example version of of an example device having a plurality of layers in a lateral aspect, formed by selective deposition of a patterning coating in a first portion of the lateral aspect, followed by deposition of a deposited material, to form a closed coating in a second portion thereof according to an example in the present disclosure;

[0021] FIG. 4 is a schematic diagram showing an example process for depositing a patterning coating in a pattern on an exposed layer surface 11 of an underlying layer in an example version of the device of FIG. 2, according to an example in the present disclosure;

[0022] FIG. 5 is a schematic diagram showing an example process for depositing a deposited material as a deposited layer in the second portion on an exposed layer surface that comprises the deposited pattern of the patterning coating of FIG. 4, where the patterning coating is an NIC;

[0023] FIG. 6 A is a schematic diagram illustrating an example version of the device of FIG. 3 in a cross-sectional view;

[0024] FIG. 6B is a schematic diagram illustrating the device of FIG. 6A in a complementary plan view,

[0025] FIGs. 7A-7B are schematic diagrams that show various potential behaviours of a patterning coating at a deposition interface with a deposited layer in an example version of the device of FIG. 1 according to various examples in the present disclosure;

[0026] FIGs. 8A-8H are simplified block diagrams from a cross-sectional aspect, of example versions of the device of FIG. 1, showing various examples of possible interactions between the particle structure patterning coating and the particle structures according to examples in the present disclosure;

[0027] FIG. 9 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 3 with additional example deposition steps according to an example in the present disclosure,

[0028] FIG. 10 is a schematic diagram that may show example stages of an example process for manufacturing an example version of an OLED device having sub-pixel regions having a second electrode of different thickness according to an example in the present disclosure,

[0029] FIG, 11 is a schematic diagram illustrating an example cross-sectional view of an example version of an OLED device in which a second electrode is coupled with an auxiliary electrode according to an example in the present disclosure;

[0030] FIG. 12 is a schematic diagram illustrating an example cross-sectional view of an example version of an OLED device having a partition and a sheltered region, such as a recess, in a non-emissive region thereof according to an example in the present disclosure;

[0031] FIGs. 13A-13B are schematic diagrams that show example cross-sectional views of an example OLED device having a partition and a sheltered region, such as an aperture, in a non- emissive region, according to various examples in the present disclosure;

[0032] FIG. 14 is a schematic diagram illustrating an example cross-sectional view of an example di splay panel having a plurality of layers, comprising at least one aperture therewithin, through which at least one electromagnetic signal may be exchanged according to an example in the present disclosure,

[0033] FIG. 15 is an example energy profile illustrating energy states of an adatom absorbed onto a surface according to an example in the present disclosure;

[0034] FIG. 16 is a schematic diagram illustrating the formation of a film nucleus according to an example in the present disclosure; and

[0035] FIG, 17 is a block diagram of an example computer device within a computing and communications environment that may be used for implementing devices and methods in accordance with representative examples of the present disclosure.

[0036] In the present disclosure, a reference numeral having at least one of: at least one numeric value (including without limitation, in at least, one of: superscript, and subscript), and at least one alphabetic character (including without limitation, in lower-case) appended thereto, may be considered to refer to a (subset of a) particular instance of the feature (element) described by the reference numeral. Reference to the reference numeral without reference to the at least one of the: appended value(s), and character(s), may, as the context dictates, refer generally to the feature! s) described by at least one of the: reference numeral, and set of all instances describedthereby. Similarly, a reference numeral may have the letter “x’ in the place of a numeric digit. Reference to such reference numeral may, as the context dictates, refer generally to feature(s) described by the reference numeral, where the character “x” is replaced by at least one of: a numeric digit, and the set of all instances described thereby.

[0037] In the present disclosure, for purposes of explanation and not limitation, specific details are set forth to provide a thorough understanding of the present disclosure, including without limitation, particular architectures, interfaces and techniques. In some instances, detailed descriptions of well-known systems, technologies, components, devices, circuits, methods, and applications are omitted to not obscure the description of the present disclosure with unnecessary' detail.

[0038] Further, it will be appreciated that block diagrams reproduced herein can represent conceptual view's of illustrative components embodying the principles of the technology.

[0039] Accordingly, the system and method components have been represented where appropriate by conventional symbols in the drawings, showing only those specific details that are pertinent to understanding the examples of the present disclosure, to not obscure the disclosure with details that will be readily apparent to those of ordinary skill in the art having the benefit of the description herein.

[0040] Any drawings provided herein may not be drawn to scale and may not be considered to limit the present disclosure in any way.

[0041] Any feature shown in dashed outline may in some examples be considered as optional.SUMMARY

[0042] The present disclosure discloses an opto-electronic device comprises a plurality of layers deposited on a substrate that extends in a lateral aspect defined by a lateral axis thereof. The plurality of layers defines an emissive region comprising a first electrode, a second electrode, and at least one semiconducting layer disposed between the substrate and the second electrode. The first electrode is disposed between the substrate and the at least one semiconducting layer. The second electrode comprises a substantially low loss silver (Ag) (composite) thin film coating comprising a first deposited material and a substantially low' loss Ag (composite) material that exhibits a sheet resistance (Rs), while still exhibiting a transmittance (T) that is substantially high and an average layer thickness that is substantially thin, and absorption (Abs).

[0043] According to a broad aspect of the present disclosure, there is disclosed An opto¬ electronic device comprising a plurality of layers deposited on a substrate and extending in a lateral aspect defined by a lateral axis thereof, the plurality of layers defining an emissive region comprising: a first electrode, a second electrode, at least one semiconducting layer disposed between the first electrode and the second electrode; wherein: the first electrode is disposed between the substrate and the at least one semiconducting layer; the second electrode comprises a substantially low loss silver (Ag) (composite) thin film coating comprising a first deposited material comprising a substantially low loss Ag (composite) material, and the second electrode exhibits a substantially low: sheet resistance (Rs), while still exhibiting a transmittance (T) that is substantially high and an average layer thickness that is substantially thin, and absorption (Abs).

[0044] In some non-limiting examples, the absorption may be defined by Abs = 1 -- T -- R, where R is a reflectance.

[0045] In some non-limiting examples, the absorption may be one of no more than substantially about: 2%, 3%, 5%, 10%, 15%, 20%, and 25%.

[0046] In some non-limiting examples, the absorption may be no more than substantially about 10%.

[0047] In some non-limiting examples, the substantially high transmittance may permit transmission of light therethrough.

[0048] In some non-limiting examples, the substantially low loss Ag (composite) thin film coating may exhibit a substantially small grain size.

[0049] In some non-limiting examples, a combination of the sheet resistance and transmittance may be one of substantially about: Rs< 10 Q / c, T > 50%; Rs< 9 £! / □, T > 50%; Rs< 8 Q / a, T > 50%; and Rs< 7!□ / □, T > 60%.

[0050] In some non-limiting examples, the average layer thickness may be one of no more than substantially about: 25, 20, 18, 15, 13, 10, 8, 7, and 5 nm.

[0051] In some non-limiting examples, the sheet resistance may be reduced by depositing a seed material prior to deposition of the substantially low loss Ag (composite) material for such materi l to coalesce therearound.

[0052] In some non-limiting examples, the seed material may change a morphology of the substantially low loss Ag (composite) material.

[0053] In some non-limiting examples, the seed material may exhibit a bond dissociation energy between it and Ag that is at least that of a bond dissociation energy of Ag-Ag.

[0054] In some non-limiting examples, the seed material may exhibit substantially low absorption and substantially increased wetting on organic materials.

[0055] In some non-limiting examples, the seed material may comprise at least one of: gold (Au), aluminum (Al), copper (Cu), germanium (Ge), indium (In), lithium (Li), cobalt (Co), nickel (Ni), palladium (Pd), and bismuth (Bi).

[0056] In some non-limiting examples, the seed material may comprise at least one of: Au, Al, Cu, Ge, In, Co, Ni, Pd, and Bi.

[0057] In some non-limiting examples, the seed material may comprise a second deposited material comprising Au.

[0058] In some non-limiting examples, the second deposited material may lie between the first deposited material and the at least one semiconducting layer.

[0059] In some non-limiting examples, the first electrode may be disposed between the substrate and at least one semiconducting layer.

[0060] In some non-limiting examples, when energized: the first electrode may be an anode adapted to generate holes; the second electrode may be a cathode adapted to generate electrons; and the at least one semiconducting layer may comprise an emissive layer adapted to combine a generated hole and a generated electron and emit a photon thereby.

[0061] In some non-limiting examples, the photon may be emitted through the second electrode.

[0062] In some non-limiting examples, the photon may have a wavelength that lies within one of the: visible, infrared (IR), near-IR, ultraviolet (UV), and extreme UV, spectrum.

[0063] In some non-limiting examples, the device may further comprise at least one patterning coating disposed on an exposed layer surface of an underlying layer of the device, in a first portion of the lateral aspect.

[0064] In some non-limiting examples, the at least one patterning coating may be adapted to impact a propensity of an evaporated flux of at least one of the: first, and second, deposited material to be deposited thereon.

[0065] In some non-limiting examples, the exposed layer surface of the at least one patterning coating may be substantially devoid of a closed coating of at least one of the: first, and second, deposited material.

[0066] In some non-limiting examples, the exposed layer surface of the at least one patterning coating may be substantially devoid of both a closed coating of the first deposited material, and a closed coating of the second deposited material.

[0067] In some non-limiting examples, the exposed layer surface of the at least one patterning coating may be substantially devoid of the first deposited material.

[0068] In some non-limiting examples, the second electrode may comprise a first deposited sub¬ layer comprising the first deposited material and a second deposited sub-layer comprising the second deposited material and the first deposited sub-layer may be disposed between the at least one semiconducting layer and the second deposited sub-layer.

[0069] In some non-limiting examples, the first deposited sub-layer and the second deposited sub-layer may both be disposed in a second portion of the lateral aspect.

[0070] In some non-limiting examples, the first deposited sub-layer may be a discontinuous layer of at least one particle structure of the first deposited material.

[0071] In some non-limiting examples, the second deposited sub-layer may be a closed coating of the second deposited material.

[0072] In some non-limiting examples, the at least one particle structure may be adapted to serve as a nucleation site for the second deposited material.

[0073] In some non-limiting examples, the second deposited material may be in physical contact with the at least one particle structure of the first deposited material.

[0074] In some non-limiting examples, the device may further comprise a layer comprising ytterbium ( Yb) disposed between the at least one semiconducting layer and the first deposited sub-layer.

[0075] In some non-limiting examples, the second electrode may comprise a mixture of the first deposited material and the second deposited material.

[0076] In some non-limiting examples, the first portion may exclude a lateral aspect of the emissive region.

[0077] In some non-limiting examples, the first portion may comprise a transmissive region adapted to allow light to pass therethrough.

[0078] In some non-limiting examples, the first portion may include a lateral aspect of the emissive region.

[0079] In some non-limiting examples, the average layer thickness of the second electrode may be one of no more than substantially about: 20, 18, 15, 12, 10, and 8, nm.

[0080] In some non-limiting examples, a sheet resistance of the second electrode may be one of no more than substantially about: 10, 15, 18, 20, and 30, Ω / □.

[0081] In some non-limiting examples, a light transmittance of the second electrode at a wavelength of 460 nm may be one of substantially at least about: 60%, 65%, and 70%.

[0082] In some non-limiting examples, a light transmittance of the second electrode at a wavelength of 940 nm may be one of substantially at least about: 40%, 50%, and 60%.

[0083] In some non-limiting examples, the at least one semiconducting layer may comprise an electron injection layer (EIL) comprising an electron injection material.

[0084] In some non-limiting examples, the electron injection material may comprise one of: Li, Yb, and Yb-doped Li.DESCRIPTIONOpto-Electronic Device

[0085] The present disclosure relates generally to opto-electronic devices 100. An opto-electronic device 100 may generally encompass any layered semiconductor device 100 that converts electrical signals 1431 (FIG. 14) into light in the form of photons and vice versa. In some non¬ limiting examples, the opto-electronic device 100 may be an organic light-emitting diode (OLED).

[0086] In some non-limiting examples, a lateral axis, identified as the X-axis, may be shown, together with a longitudinal axis, identified as the Z-axis. In some non-limiting examples, a second lateral axis, identified as the Y-axis, may be shown as being substantially transverse to both the X-axis and the Z-axis. In some non-limiting examples, at least one of the lateral axes may define a lateral aspect of the device 100. In some non-limiting examples, the longitudinal axis may define a longitudinal aspect of the device 100.

[0087] In some non-limiting examples, the layers of the device 100 may extend, in the lateral aspect, substantially parallel to a plane defined by the lateral axes. Those having ordinary skill inthe relevant art will appreciate that the substantially planar representation shown in FIG, 1 may be, in some non-limiting examples, an abstraction for purposes of illustration. In some non¬ limiting examples, there may be, across a lateral extent of the device 100, localized substantially planar strata of different thicknesses and dimension, including, in some non-limiting examples, the substantially complete absence of at least one layer, separated by non-planar transition areas (including lateral gaps and even discontinuities).

[0088] Thus, while for illustrative purposes, in some non-limiting examples, the device 100 may be shown in its longitudinal aspect as a substantially stratified structure of substantially parallel planar layers, such device 100 may illustrate, locally, a diverse topography, to define features, each of which may substantially exhibit the stratified profile discussed in the longitudinal aspect.

[0089] In some non-limiting examples, a lateral aspect of an exposed layer surface 11 of the device 100 may comprise a first portion 101 and a second portion 102. In some non-limiting examples, the second portion 102 may comprise that part of the exposed layer surface 11 of the device 100 that lies beyond the first portion 101.

[0090] FIG. 1 is a simplified block diagram in a cross-sectional view, of an example opto¬ electronic device 100, which may be, in some non-limiting examples, an electro-luminescent device 100, according to the present disclosure. In some non-limiting examples, the device 100 may be an OLED.

[0091] In some non-limiting examples, the device 100 may comprise a substrate 10, upon which a frontplane 103, comprising a plurality of layers, respectively, a first electrode 120, at least one semiconducting layer 130, and a second electrode 140, are disposed. In some non-limiting examples, the frontplane 103 may provide mechanisms for at least one of: emission of light, including without, limitation, photons, and manipulation of emitted light.

[0092] In some non-limiting examples, various coatings of such devices 100 may be formed by vacuum-based deposition processes.

[0093] In some non-limiting examples, the device 100 may be electrically coupled with a power source 104. When so coupled, the device 100 may emit light, including without limitation, photons, as described herein.Substrate

[0094] In some non-limiting examples, the substrate 10 may comprise a base substrate 115. In some non-limiting examples, the base substrate 115 may be formed of material suitable for usethereof, including without limitation, at least one of: an inorganic material, including without limitation, at least one of: silicon (Si), glass, metal (foil), sapphire, and other inorganic material, and an organic material, including without limitation, a polymer, including without limitation, at least one of: a polyimide, and an Si-based polymer. In some non-limiting examples, the base substrate 115 may be one of: rigid, and flexible. In some non-limiting examples, the substrate 10 may be defined by at least one planar surface. In some non-limiting examples, the substrate 10 may have at least one exposed layer surface 11 that supports the remaining frontplane 103 components of the device 100, including without limitation, at least one of the: first electrode 120, at least one semiconducting layer 130, and second electrode 140.

[0095] In some non-limiting examples, such surface may be at least one of an: organic, and inorganic, surface.

[0096] In some non-limiting examples, the substrate 10 may comprise, in addition to the base substrate 115, at least one additional (in)organic layer (not shown nor specifically described herein) supported on an exposed layer surface 11 of the base substrate 115.

[0097] In some non-limiting examples, such additional layers may comprise at least one organic layer, which may at least one of: comprise, replace, and supplement, at least one of the semiconducting layers 130.

[0098] In some non-limiting examples, such additional layers may comprise at least one inorganic layer, which may comprise at least one electrode 120, 140, 950, which in some non¬ limiting examples, may at least one of: comprise, replace, and supplement, at least one of the: first electrode 120, and second electrode 140.Backplane and TFT structure(s) embodied therein

[0099] In some non-limiting examples, such additional layers may comprise a backplane 105. In some non-limiting examples, the backplane 105 may comprise at least one of: power circuitry, and switching elements, for driving the device 100, including without limitation, at least one (component of an) electronic thin-film transistor (TFT) structure 106 that may be formed by a photolithography process.

[0100] In some non-limiting examples, the backplane 105 of the substrate 10 may comprise at least one electronic component, including without limitation, an opto-electronic component 1430, including without limitation, one of: transistors, resistors, and capacitors, which may support the device 100 acting as one of: an active-matrix, and a passive matrix, device 100.In some non-limiting examples, such structures may be a TFT structure 106, including without limitation, one of: top-gate, bottom-gate, n-type, and p-type, TFT structures 106. In some non¬ limiting examples, the TFT structure 106 may incorporate one of: amorphous Si (a-Si), indium gallium zinc oxide (IGZO), and low-temperature polycrystalline Si (LTPS).First Electrode

[0101] In some non-limiting examples, the first electrode 120 may be deposited over the substrate 10. In some non-limiting examples, the first electrode 120 may be electrically coupled with at least one of: a terminal of the power source 104, and ground. In some non-limiting examples, the first electrode 120 may be so coupled through at least one driving circuit that may, in some non-limiting examples, incorporate at least one TFT structure 106 in the backplane 105 of the substrate 10.

[0102] In some non-limiting examples, the first electrode 120 may comprise one of: an anode, and a cathode. In some non-limiting examples, the first electrode 120 may be an anode.

[0103] In some non-limiting examples, the first electrode 120 may be formed by depositing at least one thin conductive film, over (a part of; the substrate 10. In some non¬ limiting examples, there may be a plurality of first electrodes 120, disposed in a spatial arrangement over a lateral aspect of the substrate 10. In some non-limiting examples, at least one of such first electrodes 120 may be deposited over (a part of) a TFT insulating layer 107 disposed in a lateral aspect in a spatial arrangement. If so, in some non-limiting examples, at least one of such first electrodes 120 may extend through an opening of the corresponding TFT insulating layer 107 to be electrically coupled with an electrode of the TFT structures 106 in the backplane 105.

[0104] In some non-limiting examples, (at least one thin film of) the at least one first electrode 120 may comprise various materials, including without limitation, at least one metallic material, including without limitation, at least one of: magnesium (Mg), aluminum (Al), calcium (Ca), zinc (Zn), silver (Ag), cadmium (Cd), barium (Ba), and ytterbium (Yb), including without limitation, alloys comprising any of such materials, at least one metal oxide, including without limitation, a TCO, including without limitation, ternary compositions including without limitation, at least one of: fluorine-doped tin oxide (FTO), indium zinc oxide (IZO), and indium tin oxide (ITO), in varying proportions, including without limitation, combinations of any plurality thereof in at least one layer, any of which may be, without limitation, a thin film.Second Electrode

[0105] In some non-limiting examples, the second electrode 140 may be deposited over the at least one semiconducting layer 130. In some non-limiting examples, the second electrode 140 may be electrically coupled with at least one of: a terminal of the power source 104, and ground. In some non-limiting examples, the second electrode 140 may be so coupled through at least one driving circuit, that may, in some non-limiting examples, incorporate at least one TFT structure 106 in the backplane 105 of the substrate 10.

[0106] In some non-limiting examples, the second electrode 140 may comprise one of: an anode, and a cathode. In some non-limiting examples, the second electrode 140 may be a cathode.

[0107] In some non-limiting examples, the second electrode 140 may be formed by depositing a deposited layer 330 (FIG. 3), in some non-limiting examples, as at least one thin film, over (a part of) the at least one semiconducting layer 130.

[0108] In some non-limiting examples, there may be a plurality of second electrodes 140, disposed in a spatial arrangement over a lateral aspect of the at least one semiconducting layer 130.

[0109] In some non-limiting examples, (at least one thin film of) the at least one second electrode 140 may comprise various materials, including without limitation, at least one metallic material, including without limitation, at least one of: Li, Mg, Al, Ca, Zn, Ag, Cd, Ba, and Yb, including without limitation, alloys comprising at least one of: any of such materials, at least one metal oxide, including without limitation, a TCO, including without limitation, ternary compositions including without limitation, at least one of: FTO, IZO, and ITO, including without limitation, in varying proportions, zinc oxide (ZnO), and other oxides comprising at least one of: indium (In), and Zn, in at least one layer, and at least one non-metallic material, any of which may be, without limitation, a thin conductive film. In some non-limiting examples, for a Mg: Ag alloy, such alloy composition may range between about 1:9-9: 1 by volume.

[0110] In some non-limiting examples, the plurality of coatings of which the second electrode 140 may be comprised, may be distinct coatings disposed on top of one another.

[0111] In some non-limiting examples, the second electrode 140 may comprise a bi-layer coating, formed by depositing an evaporated flux 532 (FIG. 5) of a first deposited material, including without limitation, Au, to form a first coating thereof, followed by depositing anevaporated flux 532 of a second deposited material, including without limitation, Ag, to form a second coating thereof.

[0112] In some non-limiting examples, the second electrode 140 may comprise a Yb / Ag bi-layer coating. In some non-limiting examples, such bi-layer coating may be formed by depositing a Yb coating, followed by an Ag coating. In some non-limiting examples, a thickness of such Ag coating may be at least that of a thickness of the Yb coating.

[0113] In some non-limiting examples, the second electrode 140 may comprise an Au / Ag bi-layer coating. In some non-limiting examples, such bi-layer coating may be formed by depositing an Au coating, followed by an Ag coating. In some non-limiting examples, a thickness of such Ag coating mav be at least that of a thickness of the Au coating.

[0114] In some non-limiting examples, the second electrode 140 may be a multi-coating electrode 140 comprising a plurality of at least one of: a metallic, and an oxide, coating.

[0115] In some non-limiting examples, such multi-coating may comprise a Yb / Au / Ag coating. In some non-limiting examples, such multi -coating may be formed by depositing a Yb coating, followed by an Au coating, followed by an Ag coating. In some non-limiting examples, a thickness of such Ag coating may be at least that of a thickness of at least one of the Yb coating and the Au coating. In some non-limiting examples, a thickness of such Yb coating may be at least that of a thickness of the Au coating.

[0116] In some non-limiting examples, the Au coating may lie between the EIL 139 and the Ag coating.

[0117] In some non-limiting examples, the Au coating may be disposed in, including without limitation, on an exposed layer surface 11 of, the EIL 139.

[0118] In some non-limiting examples, the second electrode 140 may comprise a fullerene and Mg.

[0119] In some non-limiting examples, such coating may be formed by depositing a fullerene coating followed by an Mg coating. In some non-limiting examples, a fullerene may be dispersed within the Mg coating to form a fullerene-containing Mg alloy coating. In some non¬ limiting examples, such coatings may be described in at least one of: United States Patent Application Publication No. 2015 / 0287846 published 8 October 2015, and in PCT International Application No. PCT / IB2017 / 054970 filed 15 August 2017 and published as WO2018 / 033860 on 22 February^ 2018.

[0120] In some non-limiting examples, the second electrode 140 may be formed by co-depositing an evaporated flux 532 of Au, and Ag.

[0121] In some non-limiting examples, the second electrode 140 may comprise a substantially low loss Ag (composite) material, including without limitation, disposed in a substantially low loss Ag (composite) thin film coating.

[0122] In some non-limiting examples, a substantially low loss Ag (composite) thin film coating may tend to exhibit a substantially small grain size such that, in some non-limiting examples, it may appear, in a scanning electron microscope (SEM) image, as a substantially amorphous film.

[0123] As used herein, a substantially low loss Ag (composite) thin film coating may be one which exhibits both a substantially low:* sheet resistance ( Rs), while still exhibiting:o a transmittance (T) that is substantially high so as to permit transmission of light therethrough), ando an average layer thickness that is substantially thin, and® absorption (Abs), as defined by Equation 1:Abs = 1 – T – R where R is a reflectance.

[0124] In some non-limiting examples, a combination of sheet resistance that may be substantially low, and transmittance that may be substantially high so as to permit transmission of light therethrough, such as that exhibited by a substantially low loss Ag (composite) thin film coating suitable for use in, and in some non-limiting examples, as, a second electrode 140, may be one of about: Rs< 10 £& / □, T > 50%; Rs< 9 Q / n, T > 50%; Rs < 8 £! / □, T > 50%; and Rs < 7 Q / n, T > 60%.

[0125] In some non-limiting examples, an average layer thickness that may be substantially thin, such as that exhibited by a substantially low loss Ag (composite) thin film coating suitable for use in, and in some non-limiting examples, as, a second electrode 140, may be one of no more than about: 25, 20, 18, 15, 13, 10, 8, 7, and 5, nm.

[0126] In some non-limiting examples, an absorption that may be substantially low, such as that exhibited by a substantially low loss Ag (composite) thin film coating suitable for use in.and in some non-limiting examples, as, a second electrode 140, may be one of no more than about: 2%, 3%, 5%, 10%, 15%, 20%, and 25%. In some non-limiting examples, an absorption that, may be substantially low, such as that exhibited by a substantially low loss Ag (composite) thin film coating suitable for use in, and in some non-limiting examples, as, a second electrode 140, may be no more than about 10%.

[0127] In some non-limiting examples, a sheet resistance of a substantially low loss Ag (composite) thin film coating suitable for use in, and in some non-limiting examples, as, a second electrode 140, may be reduced, by depositing a seed material, in a templating layer, at at least one of appropriate: locations, density, and stage of deposition, to act as a seed / heterogeneity 351 (FIG. 3), to act as a nucleation site prior to the deposition of the substantially low loss Ag (composite) material, such that the substantially low loss Ag (composite) material may tend to coalesce around each such seed 351.

[0128] In some non-limiting examples, the seeds 351 may change a morphology of the substantially low loss Ag (composite) material surrounding them.

[0129] In some non-limiting examples, a seed material that may be suitable for use as a seed / heterogeneity 351, to act as a nucleation site prior to the deposition of the substantially low' loss Ag (composite) material, may be one that exhibits a bond dissociation energy between the seed material and Ag that is at least that of a bond dissociation energy of Ag-Ag, which in some non-limiting examples, has been measured at 162.9 ± 2.9.

[0130] Without wishing to be limited to any particular theory', it may be postulated that a bond dissociation energy between a seed material and Ag that is at least that of a bond dissociation energy of Ag-Ag may lead to substantially increased wetting of Ag onto the seed / heterogeneity 351 comprising such seed material,

[0131] In some non-limiting examples, a seed material that may be suitable for use as a seed / heterogeneity 351, to act as a nucleation site prior to the deposition of the substantially low loss Ag (composite) material, may exhibit substantially low absorption and substantially increased wetting on organic materials.

[0132] In some non-limiting examples, the seed material may comprise at least one of: gold (Au), Al, copper (Cu), germanium (Ge), In, lithium (Li), cobalt (Co), nickel (Ni), palladium (Pd), and bismuth (Bi). In some non-limiting examples, the seed material (one example measurement of bond dissociation energy between such materi al and Ag being indicated inparentheses, when available) may comprise at least one of: Au (202.5 ± 9.6), Al (183.7 ± 9.2), Ge(174.5 ± 21), In (166.5 ± 4.9), Co, Ni, Pd, and Bi (192 ± 42). In some non-limiting examples, the seed material may comprise Au,

[0133] In some non-limiting examples, the second electrode 140 may comprise Au. In some non-limiting examples, the second electrode 140 may comprise Ag.

[0134] In some non-limiting examples, the second electrode 140 may comprise both Au and Ag.

[0135] In some non-limiting examples, the second electrode 140 may comprise a layer of Au between an exposed layer surface 11 of the at least one semiconducting layer 130 and a layer of Ag.Performance Characteristics of Opto-Electronic Device with Second Electrode Comprising Substantially Low Loss Ag (Composite) Thin Film Coating

[0136] A series of sample devices 100 was fabricated to measure certain performance characteristics of opto-electronic devices 100 with a second electrode 140 comprising a substantially low loss Ag (composite) thin film coating.

[0137] Each sample was prepared by subjecting an exposed layer surface 11 of a glass substrate 10 to an evaporated flux 532 of Yb until a reference layer thickness of about 2 nm was reached.

[0138] In Sample 1, which corresponded to a scenario in which a second electrode 140 of an opto-electronic device 100 comprised a discontinuous layer 360 (FIG. 3) of seeds 351 comprising Au, to serve as nucleation sites for the deposition of Ag, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of Au until a reference layer thickness of about 1 nm was reached. Thereafter, the exposed layer surface 11 of the device 100 was subjected to an evaporated flux 532 of Ag until a reference layer thickness of about 11 nm was reached.

[0139] In Sample 2, which corresponded to a scenario in which a second electrode 140 of an opto-electronic device 100 comprised LiAg, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of LiAg (7% concentration of Li) until a reference layer thickness of about 11 nm was reached.

[0140] In Sample 3, which corresponded to a scenario in which a second electrode 140 of an opto-electronic device 100 comprised MgAg, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of MgAg (10% concentration of Mg) until a reference layer thickness of about 11 nm was reached.

[0141] Samples 4 through 6 correspond to Samples 1 through 3, but with a reduced reference layer thickness. Those having ordinary skill in the relevant art will appreciate that as a general rule, a substantially thin second electrode 140 may correlate positively with a substantially low microcavity and concomitantly to a substantially high angular dependence of the associated opto-electronic device 100.

[0142] In Sample 4, which corresponded to the same scenario as sample 1, but with a reduced reference layer thickness, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of Au until a reference layer thickness of about 1 nm was reached. Thereafter, the exposed layer surface 11 of the device 100 was subjected to an evaporated flux 532 of Ag until a reference layer thickness of about 7 nm was reached.

[0143] In Sample 5, which corresponded to the same scenario as sample 2, but with a reduced reference layer thickness, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of LiAg (7% concentration of Li) until a reference layer thickness of about 7 nm was reached.

[0144] In Sample 6, which corresponded to the same scenario as sample 3, but with a reduced reference layer thickness, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of MgAg (10% concentration of Mg) until a reference layer thickness of about 7 nm was reached.

[0145] In Sample 7, which corresponded to the same scenario as Sample 1, but with the order of deposition of the Yb layer and the Au layer reversed, an exposed layer surface 11 of the glass substrate 10 was subjected to an evaporated flux 532 of Au until a reference layer thickness of about 1 nm was reached before the deposition of the Yb layer. Thereafter, the exposed layer surface 11 of the Au layer of the device 100 was subjected to an evaporated flux of Yb until a reference layer thickness of about 2 nm was reached. Finally, the exposed layer surface 11 of the Yb layer was subjected to an evaporated flux of Ag until a reference layer thickness of about 11 nm was reached.Current Efficiency

[0146] Brightness, also known as luminous intensity, measures an amount of light emitted in a particular direction by a light source, and is typically expressed in units of candelas (cd).

[0147] Current efficiency refers to a ratio of collected light current to a maximum possible photon current, influencing brightness. A substantially high current efficiency is correlated to a ‘‘brighter” light source which may have applicability in applications calling for substantially high light emission. Current efficiency may be reflected as a quotient of brightness divided by current density (measured in amperes (A)).

[0148] Blue index refers to a ratio of current efficiency divided by the y-axis of the CIE 1931 color spaces that reflect mathematical models that attempt to define a relationship between the visible spectrum and human color vision as observed by a standard observer, a static idealization of the color vision of a normal human.

[0149] The blue index for each of Samples 1 through 7 was measured and summarized in Table 1 below:Table 1

[0150] Comparing Samples 1 through 3, it may be seen that Samples 1 and 2 exhibited substantially high and substantially identical current efficiency, while Sample 3 exhibited substantially reduced current efficiency compared to Samples 1 and 2.

[0151] Comparing Samples 4 through 6 against corresponding Samples 1 through 3, it may be seen that Sample 4 maintained substantially about 95% of the current efficiency of Sample 1, and Sample 6 maintained about. 93% of the current efficiency of Sample 3 (which was substantially reduced compared to Samples 1 and 2).

[0152] However, Sample 5 reflected a substantial reduction in current efficiency to about 72% of the current efficiency of Sample 2. This may reflect that the film morphology of Sample 5 may be deteriorated and may not even comprise a conformal film.

[0153] Sample 7 reflected a substantial reduction in current efficiency to about 75% of the current efficiency of Sample 1. This may suggest that the substantially high current efficiency of Sample 1 is due not simply to the presence of both Au and Ag in the second electrode 140 of the device 100, but to the interaction therebetween, including without limitation, the coalescence of the Ag about the Au seeds 351.Driving Voltage

[0154] Driving voltage refers to the voltage that is needed to achieve a given current density. A substantially low driving voltage may have applicability in applications calling for energy efficiency.

[0155] The driving voltage for each of Samples 1 through 7 was measured and summarized in Table 2 below:Table 2

[0156] Comparing Samples 1 through 3, it may be seen that Samples 1 and 2 exhibited substantially low and substantially identical driving voltage, while Sample 3 exhibited substantially increased driving voltage compared to Samples 1 and 2.

[0157] Comparing Samples 4 through 6 against corresponding Samples 4 through 6, it may be seen that Sample 4 maintained substantially about 103% of the driving voltage of Sample I, and Sample 6 maintained substantially about 102% of the driving voltage of Sample 3 (which was substantially increased compared to Samples 1 and 2).

[0158] However, Sample 5 reflected a substantial increase in driving voltage to about 169% of the driving voltage of Sample 2,

[0159] Sample 7 reflected a substantial increase in driving voltage to about 142% of the driving voltage of Sample 1. This may suggest that the substantially low driving voltage of Sample 1 is due not simply to the presence of both Au and Ag in the second electrode 140 of the device 100, but to the interaction therebetween, including without limitation, the coalescence of the Ag about the Au seeds 351.

[0160] A series of sample devices 100 was fabricated to measure certain performance characteristics of opto-electronic devices 100 with a second electrode 140 comprising a substantially low loss Ag (composite) thin film coating.

[0161] Each sample was prepared by subjecting an exposed layer surface 11 of a glass substrate 10 to an evaporated flux of an electron transport material until a reference electron transport layer (ETL) 237 layer thickness of about 20 nm was reached. Thereafter, the exposed layer surface 11 of the ETL 137 layer of the device 100 was subjected to an evaporated flux 532 of Yb until a reference layer thickness of about 2 nm was reached.

[0162] In Sample 8, which corresponded to a scenario, similar to that of Sample 1, in which a second electrode 140 of an opto-electronic device 100 compri sed a discontinuous layer 360 of seeds 351 comprising Au, to serve as nucleation sites for the deposition of Ag, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of Au until a reference layer thickness of about 1 nm was reached. Thereafter, the exposed layer surface 11 of the device 100 was subjected to an evaporated flux 532 of Ag until a reference layer thickness of about 11 nm was reached.

[0163] In Sample 9, which corresponded to a scenario, similar to that of Sample 2, in which a second electrode 140 of an opto-electronic device 100 comprised LiAg, the exposedlayer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of LiAg (7% concentration of Li) until a reference layer thickness of about 11 nm was reached.

[0164] In Sample 10, which corresponded to a scenario, similar to that of Sample 3, in which a second electrode 140 of an opto-electronic device 100 comprised MgAg, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of MgAg (10% concentration of Mg) until a reference layer thickness of about 11 nm was reached.

[0165] In Sample 11, which corresponded to a scenario, similar to that of Sample 7, which corresponded to the same scenario as Sample 1, but with the order of the deposition of the Yb layer and the Au layer reversed, an exposed layer surface of the ETL 137 layer of the device 100 was subjected to an evaporated flux 532 of Au until a reference layer thickness of about 1 nm was reached before the deposition of the Yb layer. Thereafter, the exposed layer surface 11 of the Au layer of the device 100 was subjected to an evaporated flux of Yb until a reference layer thickness of about 2 nm was reached. Finally, the exposed layer surface 11 of the Yb layer was subjected to an evaporated flux of Ag until a reference layer thickness of about 11 nm was reached.

[0166] In Sample 12, which corresponded to a scenario, similar to that of Sample 8, but without the deposition of a discontinuous layer 360 of seeds 351 comprising Au, to serve as nucleation sites for the deposition of Ag, the exposed layer surface 11 of the Yb layer of the device 100 was subjected to an evaporated flux 532 of Ag until a reference layer thickness of about 11 nm was reached.Sheet Resistance

[0167] In some non-limiting examples, a device 100 having at least one electrode 120, 140, with a high sheet resistance, may create a substantially large current resistance (IR) drop in operation, when coupled with the power source 104.

[0168] In some non-limiting examples, such an IR drop may be compensated for, to some extent, by increasing a voltage level of the power source 104. However, in some non-limiting examples, increasing a voltage level of the power source 104 to compensate for the IR drop due to high sheet resistance, for at least one (sub-) pixel 915 / 216 may call for increasing the level of a voltage to be supplied to other components to maintain effective operation of the device 100.

[0169] In some non-limiting examples, as discussed elsewhere, a reduced thickness of the second electrode 140, may generally increase a sheet resistance of the second electrode 140,which may, in some non-limiting examples, reduce at least one of the: performance, and efficiency, of the device 100.

[0170] In some non-limiting examples, to reduce power supply demands for a device 100 without substantially impacting an ability to make an electrode 120, 140 substantially thin, an auxiliary electrode 950 may be formed on the device 100 to allow current to be carried substantially efficiently to various emissive region(s) 110 of the device 100, while at the same time, reducing a sheet resistance and its associated IR drop of the transmissive electrode 120, 140.

[0171] In some non-limiting examples, the auxiliary electrode 950 may be electrically coupled with the second electrode 140, so that a sheet resistance and thus, an IR drop associated with the second electrode 140, may, in some non-limiting examples, be decreased.

[0172] In some non-limiting examples, a sheet resistance specification may be used to derive an example thickness of the auxiliary electrode 950 to comply with such specification for various panel sizes.

[0173] In some non-limiting examples, a sheet resistance specification, for a common electrode 120, 140 of a display device 100, may vary according to several parameters, including without limitation, at least one of a: (panel) size of the device 100, and tolerance for voltage variation across the device 100. In some non-limiting examples, a sheet resistance specification may increase (that is, a lower sheet resistance is specified) as a panel size increases. In some non-limiting examples, a sheet resistance specification may increase as a tolerance for voltage variation decreases.

[0174] The sheet resistance of each of Samples 8 through 12 was measured and summarized in Table 3 below:Table 3

[0175] Comparing Samples 8 through 10, it may be seen that Samples 8 and 9 exhibited substantially: low, and identical, sheet resistance, while Sample 10 exhibited substantially increased sheet resistance compared to Samples 8 and 9.

[0176] Sample 11 exhibited a substantial increase in sheet resistance of, on the order of 6 times the sheet resistance of Sample 8, This may suggest that the substantially low sheet resistance of Sample 8 is due not simply to the presence of both Au and Ag in the second electrode 140 of the devi ce 100, but to the interaction therebetween, including without limitation, the coalescence of the Ag about the Au seeds 351.

[0177] Sample 12 exhibited a substantially high sheet resistance of at least about 100 Q / L’J. This may suggest that the presence of the Au seeds 351 in the second electrode 140 of the device 100 may facilitate allowing the Ag in the second electrode 140 of the device 100 to act as a low loss Ag (composite) material.

[0178] In some non-limiting examples, the second electrode 140 may have a sheet resistance that is one of at least about: 10, 15, 18, 20, and 30 Ω / □.Morphology

[0179] In some non-limiting examples, a substantially low loss Ag (composite) thin film coating may tend to exhibit a substantially small grain size such that, in some non-limiting examples, it may appear, in an SEM image, as a substantially amorphous film.

[0180] Turning now to FIGs. 2A-2E, there are shown SEM images of Samples 8 through 12 respectively.

[0181] It may be seen that the SEM images corresponding to Samples 8 through 10 (respectively, FIGs. 2A-2C) exhibit a substantially small grain size, suggesting that they reflect a substantially low loss Ag (composite) thin film coating, while the SEM images corresponding to Samples 11 and 12 (respectively, FIGs. 2D-2E) exhibit a large grain size.Semiconducting layer

[0182] In some non-limiting examples, the at least one semiconducting layer 130 may comprise a plurality of layers 131, 133, 135, 137, 139, any of which may be disposed, in somenon-limiting examples, in a thin film, in a stacked configuration, which may include, without limitation, at least one of: a hole injection layer (HIL) 131, a hole transport layer (HTL) 133, an emissive layer (EML) 135, an ETL 137, and an electron injection layer (EIL) 139.

[0183] In some non-limiting examples, the at least one semiconducting layer 130 may form a “tandem” structure comprising a plurality of EMLs 135. In some non-limiting examples, such tandem structure may also comprise at least one charge generation layer (CGL).

[0184] Those having ordinary skill in the relevant art will readily appreciate that the structure of the device 100 may be varied by one of: omitting, and combining, at least one of the semiconductor layers 131, 133, 135, 137, 139.

[0185] In some non-limiting examples, any of the layers 131, 133, 135, 137, 139 of the at least one semiconducting layer 130 may comprise any number of sub-layers. In some non¬ limiting examples, any of such layers 131, 133, 135, 137, 139, including without limitation, sub¬ layers) thereof may comprise various ones of a: mixture, and composition gradient. In some non-limiting examples, although not shown, the device 100 may comprise at least one layer comprising one of an: inorganic, and organometallic, material, and may not be necessarily limited to devices 200 comprised solely of organic materials. In some non-limiting examples, the device 100 may comprise at least one quantum dot (QD).

[0186] In some non-limiting examples, the HIL 131 may be formed using a hole injection material, which may, in some non-limiting examples, facilitate injection of holes by the anode.

[0187] In some non-limiting examples, the HTL 133 may be formed using a hole transport material, which may, in some non-limiting examples, exhibit high hole mobility.

[0188] In some non-limiting examples, the ETL 137 may be formed using an electron transport material, which may, in some non-limiting examples, exhibit high electron mobility.

[0189] In some non-limiting examples, the EIL 139 may be formed using an electron injection material, which may, in some non-limiting examples, facilitate injection of electrons by the cathode.

[0190] In some non-limiting examples, the electron injection material may comprise one of: Li, Yb, and Yb-doped Li.

[0191] In some non-limiting examples, the at least one EML 135 may be formed, in some non-limiting examples, by doping a host material with at least one emitter material. In some non-limiting examples, the emitter material may be at least one of a: fluorescent, phosphorescent, and thermally activated delayed fluorescence (TADF), emitter material.

[0192] In some non-limiting examples, the emitter material may be one of: a R(ed), G(reen), and B(lue), emitter material, that is, an emitter material that facilitates the emission of respectively, R(ed), G(reen), and B(lue), light.

[0193] In some non-limiting examples, the device 100 may be an OLED in which the at least one semiconducting layer 130 may comprise at least one EML 135 interposed between conductive thin film electrodes 120, 140, whereby, when a potential difference is applied across them, holes may be injected into the at least one semiconducting layer 130 through the anode, and electrons may be injected into the at least one semiconducting layer 130 through the cathode, to migrate toward the at least one EML 135, and there combine to emit light in the form of photons.

[0194] In some non-limiting examples, the device 100 may be an electro-luminescent QD device 100 in which the at least one semiconducting layer 130 may comprise an active layer comprising at least one QD. When current is provided by the power source 104 to the first electrode 120 and second electrode 140, light, including without limitation, in the form of photons, may be emitted from the active layer comprising the at least one semiconducting layer 130 between them.

[0195] In some non-limiting examples, including where the device 100 comprises a lighting panel, an entire lateral aspect of the device 100 may correspond to a single emissive element. As such, the substantially planar cross-sectional profile shown in FIG. 1 may extend substantially along the entire lateral aspect of the device 100, such that light is emitted from the device 100 substantially along the entirety of the lateral extent thereof. In some non-limiting examples, such single emissive element may be driven by a single driving circuit of the device 100.

[0196] In some non-limiting examples, including where the device 100 comprises a display module, the lateral aspect of the device 100 may be sub-divided into a plurality of emissive regions 110 of the device 100, in which the longitudinal aspect of the device 100 structure, within each of the emissive region(s) 110, may cause light to be emitted therefrom when energized.

[0197] Those having ordinary skill in the relevant art will readily appreciate that the structure of the device 100 may be varied by the introduction of at least one additional layer (not shown) at appropriate position(s) within the at least one semiconducting layer 130 stack, including without limitation, at least one of: a hole blocking layer (HBL) (not shown), an electron blocking layer (EBL) (not shown), a charge transport layer (CTL) (not shown), and a charge injection layer (CIL) (not shown).

[0198] In some non-limiting examples, a patterning coating 112 (FIG. 1) may be formed concurrently with the at least one semiconducting layer(s) 130. In some non-limiting examples, at least one material used to form the patterning coating 112 may also be used to form the at least one semiconducting layer(s) 130, In some non-limiting examples, the ETL 137 of the at least one semiconducting layer 130 may be a patterning coating 112 that may be deposited in the first portion 101 and the second portion 102 during the deposition of the at least one semiconducting layer 130. The EIL 139 may then be selectively deposited in the emissive region 110 of the second portion 102 over the ETL 137, such that the exposed layer surface 11 of the ETL 137 in the first portion 101 may be substantially devoid of the EIL 139. The exposed layer surface 11 of the EIL 139 in the emissive region 110 and the exposed layer surface 11 of the ETL 137, which may act as the patterning coating 112, may then be exposed to an evaporated flux 532 of the deposited material 531 (FIG. 5) to form a closed coating 340 (FIG. 3) of the deposited layer 330 on the EIL 139 in the second portion 102, and a discontinuous layer 360 of the deposited material 531 on the ETL 137 in the first portion 101. In such non-limiting example, several stages for fabricating the device 100 may be reduced.Layered Device

[0199] Those having ordinary skill in the relevant art will appreciate that, while the present disclosure is directed to opto-electronic devices 100, the principles thereof may, in some non-limiting examples, be applicable to any panel having a plurality of layers, including without limitation, at least one layer of conductive deposited material 531, including as a thin film, and in some non-limiting examples, through which electromagnetic (EM) signals may pass, including without limitation, one of partially, and entirely, at a non-zero angle relative to a plane of at least one of the layers.

[0200] Turning now to FIG. 3, there may be shown a cross-sectional view of an example layered semiconductor device 300.

[0201] As shown in FIG. 3, the layers of the device 100 may comprise a substrate 10, and a patterning coating 112 disposed on an exposed layer surface 11 of at least a portion of the lateral aspect thereof. In some non-limiting examples, the patterning coating 112 may be limited in its lateral extent to the first portion 101 and a deposited layer 330 may be disposed as a closed coating 340 on an exposed layer surface 11 of the device 300 in a second portion 102 of its lateral aspect.

[0202] In some non-limiting examples, the deposition of the deposited layer 330 may be performed using one of: an open mask, and a mask-free, deposition process.

[0203] In some non-limiting examples, as shown in FIG. 1, the deposited layer 330, including without limitation, as (a layer of) the second electrode 140, may extend partially over the patterning coating 112 in a transition region 145.

[0204] In some non-limiting examples, at least one particle structure 350 (FIG. 3) may be disposed as a discontinuous layer 360 on (a part of) the exposed layer surface 11 of the patterning coating 112.

[0205] In some non-limiting examples, the at least one particle structure 350 may comprise a particle material that may, in some non-limiting examples, tend to coalesce about a seed / heterogeneity 351 that may comprise a seed material.

[0206] Thus, as shown in the inset region shown in dashed outline in FIG. 3, the particle material may be in physical contact with the seed material, including without limitation fully surrounding / encapsulating it.

[0207] In some non-limiting examples, the seeds 351 may be deposited in the templating layer, across the exposed layer surface 11 of a layer (underlying layer 410 (FIG. 4)), including without limitation, the substrate 10, an intervening layer between the substrate 10 and at least one of the: patterning coating 112, deposited layer 330, and the at least one particle structure 350, f of the device 300, in some non-limiting examples, using one of: an open mask, and mask-free, deposition process, of the seed material.

[0208] In some non-limiting examples, the particle material may comprise a substantially low loss Ag (composite) material.

[0209] In some non-limiting examples, the particle material may be the same as a material (deposited material 531 including without limitation, a substantially low loss Ag (composite) material) of which the deposited layer 330 may be comprised.

[0210] In some non-limiting examples, although not shown, at least one particle structure 350d of a discontinuous layer 360 may extend partially over the patterning coating 112, which may act as a particle structure patterning coating 112pin the transition region 145. In some non¬ limiting examples, such discontinuous layer 360 may form (a part of) the second electrode 140.

[0211] In some non-limiting examples, although not shown, at least one of: the patterning coating 112, the deposited layer 330, and at least one particle structure 350, may be deposited on a layer (underlying layer 410) other than the substrate 10, including without limitation, an intervening layer between the substrate 10 and at least one of the: patterning coating 112, deposited layer 330, and at least one particle structure 350. In some non-limiting examples, the underlying layer 410 may comprise at least one of an: orientation, and organic supporting, layer.

[0212] In some non-limiting examples, at least one of the: patterning coating 112, deposited layer 330, and at least one particle structure 350, may be covered by at least one overlying layer 370.

[0213] In some non-limiting examples, such overlying layer 370 may comprise at least one of an: encapsulation layer, and optical coating. In some non-limiting examples, the encapsulation layer may comprise at least one of: a glass cap, a barrier film, a barrier adhesive, a barrier coating, an encapsulation layer, and a thin film encapsulation (TFE) layer, provided to encapsulate the device 300. In some non-limiting examples, the optical coating may comprise (at least one component of) at least one of an: optical, and structural, coating, including without limitation, a polarizer, a color filter, an anti -refl ection coating, an anti-glare coating, cover glass, and an optically clear adhesive (OCA).

[0214] In some non-limiting examples, at least one of a: substantially thin patterning coating 112 in the first portion 101, and deposited layer 330 in the second portion 102, may provide a substantially planar surface on which the overlying layer 370 may be deposited. In some non-limiting examples, providing such a substantially planar surface for application of such overlying layer 370 may increase adhesion thereof to such surface.

[0215] In some non-limiting examples, the optical coating may be used to modulate optical properties of light being at least one of: transmitted, emitted, and absorbed, by the device 300, including without limitation, plasmon modes. In some non-limiting examples, the optical coating may be used as at least one of (a part of): an optical filter, an index-matching coating, an optical outcoupling coating, a scattering layer, and a diffraction grating.

[0216] In some non-limiting examples, the optical coating may be used to modulate at least one optical microcavity effect in the device 300 by, without limitation, tuning at least one of the: total optical path length, and refractive index thereof. At least one optical property of the device 300 may be affected by modulating at least one optical microcavity effect including without limitation, the output light, including without limitation, at least one of: an angular dependence of an intensity thereof, and a wavelength shift thereof. In some non-limiting examples, the optical coating may be a non-electrical component, that is, the optical coating may be configured not to at least one of: conduct, and transmit, electrical current during normal device operations.

[0217] In some non-limiting examples, the optical coating may be formed of any deposited material 531 including without limitation, a substantially low loss Ag (composite) material, and in some non-limiting examples, may employ any mechanism of depositing a deposited layer 330 as described herein.Patterning

[0218] In some non-limiting examples, with reference to FIG. 3, a patterning coating 112, comprising a patterning material 411 (FIG. 4), including without limitation, a nucleation inhibiting coating (NIC) material, may be disposed, in some non-limiting examples, as a closed coating 340, on an exposed layer surface 11 of an underlying layer 410, including without limitation, a substrate 10, of the device 300, in some non-limiting examples, restricted in lateral extent by selective deposition, including without limitation, using a shadow mask 415 (FIG. 4) including without limitation, a fine metal mask (FMM), including without limitation, to the first portion 101.

[0219] Thus, in some non-limiting examples, in the second portion 102 of the device 300, the exposed layer surface 11 of the underlying layer 410 of the device 300, may be substantially devoid of a closed coating 340 of the patterning coating 112,Patterning Coating

[0220] In some non-limiting examples, the patterning coating 112 may comprise a patterning material 411. In some non-limiting examples, the patterning coating 112 may comprise a closed coating 340 of the patterning material 411.

[0221] In some non-limiting examples, the patterning coating 112 may be adapted to impact a propensity against deposition of a deposited material 531, including without limitation,a substantially low loss Ag (composite) material, to be deposited thereon. In some non-limiting examples, the patterning coating 112 may provide an exposed layer surface 11 thereof with a substantially low propensity (including without limitation, a substantially low initial sticking probability) (in some non-limiting examples, under the conditions identified in the dual QCM technique described by Walker et al.) against deposition of a deposited material 531 to be deposited thereon upon exposing such surface to an evaporated flux 532 of the deposited material 531, which, in some non-limiting examples, may be substantially no more than a propensity' against deposition of the deposited material 531 to be deposited on the exposed layer surface 11 of the underlying layer 410 of the device 300, upon which the patterning coating 112 has been deposited.

[0222] Because of the attributes, including without limitation, a low initial sticking probability, of at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, against deposition of the deposited material 531, the exposed layer surface 11 of the first portion 101 comprising the patterning coating 112 may be substantially devoid of a closed coating 340 of the deposited material 531.

[0223] In some non-limiting examples, exposure of the device 300 to an evaporated flux 532 of the deposited material 531 including without limitation, a substantially low loss Ag (composite) material, may, in some non-limiting examples, result in the formation of a closed coating 340 of a deposited layer 330 of the deposited material 531 in the second portion 102, where the exposed layer surface 11 of the underlying layer 410 may be substantially devoid of the patterning coating 112.

[0224] In some non-limiting examples, the patterning coating 112 may be an NIC that provides high deposition (patterning) contrast against subsequent deposition of the deposited material 531, such that the deposited material 531 tends not to be deposited, in some non-limiting examples, as a closed coating 340, where the patterning coating 112 has been deposited.

[0225] In some non-limiting examples, there may be scenarios calling for providing a patterning coating 112 for causing formation of a discontinuous layer 360 of at least one particle structure 350, upon (a part of) the patterning coating 112 in the first portion 101 being subjected to an evaporated flux 532 of a deposited material 531. In at least some applications, the attributes of the patterning coating 112 may be such that a closed coating 340 of the depositedmaterial 531 including without limitation, a substantially low loss Ag (composite) material, may be formed in the second portion 102, which may be substantially devoid of the patterning coating 112, while only a discontinuous layer 360 of at least one particle structure 350 having at least one characteristic may be formed in the first portion 101 on the patterning coating 112.

[0226] For purposes of simplicity of discussion, in the present disclosure, to the extent that a patterning coating 112 is deposited to act as a base for the deposition of at least one particle structure 350 thereon, such patterning coating 112 may be designated as a particle structure patterning coating 112P. By contrast, to the extent that a patterning coating 112 is deposited in a first portion 101 to substantially preclude formation in such first portion 101 of a closed coating 340 of the deposited layer 330, thus restricting the deposition of a closed coating 340 of the deposited layer 330 to a second portion 102, such patterning coating 112 may be designated as a non-particle structure patterning coating 112n. Those having ordinary skill in the relevant art will appreciate that in some non-limiting examples, a patterning coating 112 may act as both a particle structure patterning coating 112pand a non-particle structure patterning coating 112n.

[0227] In some non-limiting examples, there may be scenarios calling for formation of a discontinuous layer 360 of at least one particle structure 350 of a deposited material 531, which may be, in some non-limiting examples, a metal (alloy), including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, in the first portion 101, while depositing, in the second portion 102, a closed coating 340 of the deposited material 531 having a thickness of, without limitation, one of no more than about: 100, 75, 50, 25, and 15, nm. In some non-limiting examples, an amount of the deposited material 531 deposited as a discontinuous layer 360 of at least one particle structure 350 in the first portion 101 may correspond to one of between about: 1-50%, 2-25%, 5-20%, and 7-10% of the amount of the deposited material 531 deposited as a closed coating 340 in the second portion 102, which, in some non-limiting examples may correspond to a thickness of one of no more than about: 100, 75, 50, 25, and 15, nm.

[0228] In some non-limiting examples, the patterning coating 112 may be disposed in a pattern that may be defined by at least one region therein that may be substantially devoid of a closed coating 340 of the patterning coating 112.

[0229] In some non-limiting examples, the at least one region may separate the patterning coating 112 into a plurality of discrete fragments thereof. In some non-limiting examples, the plurality of discrete fragments of the patterning coating 112 may be physically spaced apart fromone another in the lateral aspect thereof. In some non-limiting examples, the plurality of the discrete fragments of the patterning coating 112 may be arranged in a regular structure, including without limitation, an array (matrix), such that in some non-limiting examples, the discrete fragments of the patterning coating 112 may be configured in a repeating pattern.

[0230] In some non-limiting examples, at least one of the discrete fragments of the patterning coating 112 may each correspond to an emissive region 110. In some non-limiting examples, an aperture ratio of the emissive regions 410 may be one of no more than about: 50%, 40%, 30%, and 20%.

[0231] In some non-limiting examples, the patterning coating 112 may be formed as a single monolithic coating.Deposited Layer

[0232] In some non-limiting examples, where the patterning coating 112 is restricted in its lateral extent to the first portion 101, a deposited layer 330 comprising a deposited material 531 including without limitation, a substantially low loss Ag (composite) material, may be disposed as a closed coating 340 on an exposed layer surface 11 of the underlying layer 410 in the second portion 102 of the lateral aspect of the device 100.

[0233] In some non-limiting examples, the deposited material 531 may comprise an element selected from at least one of potassium (K), sodium (Na), lithium (Li), Ba, cesium (Cs), Yb, Ag, gold (Au), Cu, Al, Mg, Zn, Cd, tin (Sn), Bi and yttrium (Y). In some non-limiting examples, the element may comprise at least one of: K, Na, Li, Ba, Cs, Yb, Ag, Au, Cu, Al, and Mg. In some non-limiting examples, the element may comprise at least one of: Cu, Ag, and Au. In some non-limiting examples, the element may be Cu. In some non-limiting examples, the element may be Al. In some non-limiting examples, the element may comprise at least one of: Mg, Zn, Cd, and Yb. In some non-limiting examples, the element may comprise at least one of: Mg, Ag, Al, Yb, and Li. In some non-limiting examples, the element may comprise at least one of: Mg, Ag, Yb, and Li. In some non-limiting examples, the element may be Li and Ag.

[0234] In some non-limiting examples, the deposited material 531 may comprise a substantially low loss Ag (composite) material such that, the deposited layer 330 may form the substantially low loss Ag (composite) thin film coating.

[0235] In some non-limiting examples, the deposited material 531 may comprise additional materials. In some non-limiting examples, such additional materials may compriseelemental metals, including without limitation, Mg, Yb, and Au. In some non-limiting examples, such additional materials may comprise metal fluorides, including without limitation, LiF and NaF. In some non-limiting examples, such additional materials may comprise metal oxides.

[0236] In some non-limiting examples, the deposited material 531 may comprise a pure metal. In some non-limiting examples, the deposited material 531 may be (substantially) pure Ag. In some non-limiting examples, the substantially pure Ag may have a purity of one of at least about: 95%, 99%, 99.9%, 99.99%, 99.999%, and 99.9995%. In some non-limiting examples, the deposited material 531 may be (substantially) pure Mg. In some non-limiting examples, the substantially pure Mg may have a purity of one of at least about: 95%, 99%, 99.9%, 99.99%, 99.999%, and 99.9995%.

[0237] In some non-limiting examples, the deposited material 531 may comprise an alloy. In some non-limiting examples, the alloy may be one of an: Ag-containing, Mg- containing, Li-containing, LiAg-containing, and AgMg-containing, alloy. In some non-limiting examples, the LiAg-containing alloy may have an alloy composition that may range from about 1:10 (Li: Ag) to about 1: 1 by volume.

[0238] In some non-limiting examples, the deposited material 531 may comprise other metals in one of: in place of, and in combination with, Ag. In some non-limiting examples, the deposited material 531 may comprise an alloy of Ag with at least one other metal, including without limitation, at least one of: Mg, and Yb. In some non-limiting examples, such alloy may be a binary alloy having a composition between about 5-95 vol.% Ag, with the remainder being the other metal. In some non-limiting examples, the deposited material 531 may comprise Ag and Mg, including without limitation, in an Ag: Mg alloy having a composition between about 1:10-10:1 by volume. In some non-limiting examples, the deposited material 531 may comprise Ag and Yb, including without limitation, in a Yb: Ag alloy having a composition between about 1:20-l 0: 1 by volume. In some non-limiting examples, the deposited material 531 may comprise Mg and Yb, including without limitation, in an Mg: Yb alloy. In some non-limiting examples, the deposited material 531 may comprise Ag, Mg, and Yb, including without limitation, in an Ag: Mg: Yb alloy.

[0239] In some non-limiting examples, the deposited layer 330 may comprise at least one additional element, including without limitation, a non-metallic element, including without limitation, at least one of: O, S, N, and C. It will be appreciated by those having ordinary skill in the relevant art that., in some non-limiting examples, such additional element(s) may beincorporated into the deposited layer 330 as a contaminant, due to the presence of such additional element(s) in at least one of the: source material, equipment used for deposition, and vacuum chamber environment. In some non-limiting examples, the concentration of such additional element(s) may be limited to be no more than a threshold concentration. In some non-limiting examples, such additional element(s) may form a compound together with other element(s) of the deposited layer 330. In some non-limiting examples, a concentration of the non-metallic element in the deposited material 531 may be one of no more than about: 1%, 0.1%, 0.01%, 0.001%, 0.0001%, 0.00001%, 0.000001%, and 0.0000001%. In some non-limiting examples, the deposited layer 330 may have a composition in which a combined amount of O and C therein may be one of no more than about: 10%, 5%, 1%, 0.1%, 0.01%, 0.001%, 0.0001%, 0.00001%, 0.000001%, and 0.0000001%.

[0240] It has now been found that, reducing a concentration of certain non-metallic elements in the deposited layer 330, particularly in cases wherein the deposited layer 330 may be substantially comprised of metal (alloy)(s) may facilitate selective deposition of the deposited layer 330. Without wishing to be bound by any particular theory, it may be postulated that certain non-metallic elements, including without limitation, at least one of: O, and C, when present in the evaporated flux 532 of at least one of the: deposited layer 330, deposition chamber, and environment, may be deposited onto an exposed layer surface 11 of the patterning coating 112 to act as nucleation sites for the metallic element(s) of the deposited layer 330. It may be postulated that reducing a concentration of such non-metallic elements that could act as nucleation sites may facilitate reducing an amount of deposited material 531 deposited on the exposed layer surface 11 of the patterning coating 112.

[0241] In some non-limiting examples, the deposited material 531 may be deposited on a metal-containing underlying layer 410. In some non-limiting examples, the deposited material 531 and the underlying layer 410 thereunder may comprise a metal in common.

[0242] In some non-limiting examples, the deposited layer 330 may comprise a plurality of layers of the deposited material 531. In some non-limiting examples, the deposited material 531 of a first one of the plurality of layers may be different from the deposited material 531 of a second one of the plurality of layers. In some non-limiting examples, the deposited layer 330 may comprise a multilayer coating. In some non-limiting examples, such multilayer coating may be one of: Li / Ag, Yb / Mg, Li: Yb / Mg: Ag, Yb / Yb: Ag, Yb / Ag / Mg, and Yb / Mg / Ag.

[0243] In some non-limiting examples, the deposited material 531 may comprise a metal having a bond dissociation energy, of one of no more than about: 300, 200, 165, 150, 100, 50, and 20, kJ / mol.

[0244] In some non-limiting examples, the deposited material 531 may comprise a metal having an electronegativity that is one of no more than about: 1.4, 1.3, and 1.2.

[0245] In some non-limiting examples, a sheet resistance of the deposited layer 330 may generally correspond to a sheet resistance of the deposited layer 330, measured in isolation from other components, layers, and parts of the device 300. In some non-limiting examples, the deposited layer 330 may be formed as a thin film. Accordingly, in some non-limiting examples, the characteristic sheet resistance for the deposited layer 330 may be determined based on at least one of the: composition, thickness, and morphology, of such thin film. In some non-limiting examples, the sheet resistance may be one of no more than about: 10, 5, 1, 0.5, 0.2, and 0.1, Q / □.

[0246] In some non-limiting examples, the deposited layer 330 may be disposed in a pattern that may be defined by at least one region therein that is substantially devoid of a closed coating 340 of the deposited layer 330. In some non-limiting examples, the at least one region may separate the deposited layer 330 into a plurality of discrete fragments thereof. In some non¬ limiting examples, each discrete fragment of the deposited layer 330 may be a distinct second portion 102. In some non-limiting examples, the plurality of discrete fragments of the deposited layer 330 may be physically spaced apart from one another in the lateral aspect thereof. In some non-limiting examples, at least two of such plurality of discrete fragments of the deposited layer 330 may be electrically coupled. In some non-limiting examples, at least two of such plurality of discrete fragments of the deposited layer 330 may be each electrically coupled with a common conductive coating, including without limitation, the underlying layer 410, to allow the flow of electrical current between them. In some non-limiting examples, at least two of such plurality of discrete fragments of the deposited layer 330 may be electrically insulated from one another.Selective Deposition Using Patterning Coatings

[0247] FIG. 4 is an example schematic diagram illustrating a non-limiting example of an evaporative deposition process, shown generally at 400, in a chamber 420, for selectively depositing a patterning coating 112 onto a first portion 101 of an exposed layer surface 11 of the underlying layer 410.

[0248] In the process 400, a quantity of a patterning material 411 may be heated under vacuum, to evaporate (sublime) the patterning material 411. In some non-limiting examples, the patterning material 411 may comprise substantially (entirely), a material used to form the patterning coating 112. In some non-limiting examples, such material may comprise an organic material.

[0249] In some non-limiting examples, an evaporated flux 412 of the patterning material 411 may flow through the chamber 420, including in a direction indicated by arrow 41, toward the exposed layer surface 11 of the underlying layer 410. When the evaporated flux 412 is incident on the exposed layer surface 11 of the underlying layer 410, the patterning coating 112 may be formed thereon.

[0250] In some non-limiting examples, as shown in the figure for the process 400, the patterning coating 112 may be selectively deposited only onto a portion, in the example illustrated, the first portion 101, of the exposed layer surface 11 of the underlying layer 410, by the interposition, between the evaporated flux 412 and the exposed layer surface 11 of the underlying layer 410, of a shadow mask 415, including without limitation, an FMM. In some non-limiting examples, such a shadow mask 415 may, in some non-limiting examples, be used to form substantially small features, with a feature size on the order of (smaller than) tens of microns.

[0251] In some non-limiting examples, the shadow mask 415 may have at least one aperture 416 extending therethrough such that a part of the evaporated flux 412 passes through the aperture 416 and may be incident on the exposed layer surface 11 of the underlying layer 410 to form the patterning coating 112. Where the evaporated flux 412 does not pass through the aperture 416 but is incident on a surface 417 of the shadow mask 415, it is precluded from being disposed on the exposed layer surface 11 of the underlying layer 410 to form the patterning coating 112. In some non-limiting examples, the shadow mask 415 may be configured such that the evaporated flux 412 that passes through the aperture 416 may be incident on the first portion 101 but not the second portion 102. The second portion 102 of the exposed layer surface 11 of the underlying layer 410 may thus be substantially devoid of (a closed coating 340 of) the patterning coating 112. In some non-limiting examples (not shown), the patterning material 411 that is incident on the shadow mask 415 may be deposited on the surface 417 thereof.

[0252] Accordingly, a patterned surface may be produced on the exposed layer surface 11 of the underlying layer 410 upon completion of the deposition of the patterning coating 112.

[0253] While the present disclosure contemplates the patterned deposition of the patterning coating 112 by an evaporative deposition process involving a shadow mask 415, those having ordinary skill in the relevant art will appreciate that, in some non-limiting examples, this may be achieved by any applicable deposition process, including without limitation, a micro¬ contact printing process.Deposition of Deposited Layer

[0254] FIG. 5 is an example schematic diagram illustrating a non-limiting example of a result of an evaporative process, shown generally at 500, in the chamber 420, for selectively depositing a closed coating 340 of a deposited layer 330 onto the second portion 102 of an exposed layer surface 11 of the underlying layer 410 that is substantially devoid of a patterning coating 112 that was selectively deposited onto the first portion 101, including without limitation, by the evaporative process 400 of FIG. 4.

[0255] In some non-limiting examples, the deposited layer 330 may be comprised of a deposited material 531, in some non-limiting examples, comprising at least one metal including without limitation, a substantially low loss Ag (composite) material. It will be appreciated by those having ordinary skill in the relevant art that, in some non-limiting examples, a vaporization temperature of an organic material may be substantially low relative to a vaporization temperature of metals, such as may be employed as a deposited material 531.

[0256] Thus, in some non-limiting examples, there may be substantially few' constraints in employing a shadow' mask 415 to selectively deposit the patterning coating 112 in a pattern, relative to directly patterning the deposited layer 330 using such shadow mask 415.

[0257] Once the patterning coating 112 has been deposited on the first portion 101 of the exposed layer surface 11 of the underlying layer 410, a closed coating 340 of the deposited material 531 may be deposited, on the second portion 102 of the exposed layer surface 11 that is substantially devoid of the patterning coating 112, as the deposited layer 330.

[0258] In the process 500, a quantity of the deposited material 531 may be heated under vacuum, to sublime the deposited material 531. In some non-limiting examples, the deposited material 531 may be comprised of substantially (entirely) a material used to form the deposited layer 330.

[0259] In some non-limiting examples, an evaporated flux 532 of the deposited material 531 may be directed inside the chamber 420, including in a direction indicated by arrow' 51,toward the exposed layer surface 11 of both the patterning coating 112 in the first portion 101, and the underlying layer 410 in the second portion 102. When the evaporated flux 532 is incident on the exposed layer surface 11 of the underlying layer 410 in the second portion 102, a closed coating 340 of the deposited material 531 may be formed thereon as the deposited layer 330.

[0260] In some non-limiting examples, deposition of the deposited material 531 may be performed using one of: an open mask, and a mask-free, deposition process.

[0261] It will be appreciated by those having ordinary skill in the relevant art that, contrary' to that of a shadow mask 415, a feature size of an open mask may be generally comparable to the size of a device 410 being manufactured.

[0262] It will be appreci ted by those having ordinary skill in the relevant art that, in some non-limiting examples, the use of an open mask may be omitted. In some non-limiting examples, an open mask deposition process described herein may alternatively be conducted without the use of an open mask, such that an entire target exposed layer surface 11 may be exposed.

[0263] Indeed, as shown in FIG, 5, the evaporated flux 532 may be incident on an exposed layer surface 11 of both the patterning coating 112 across the first portion 101, as well as the underlying layer 410 across the second portion 102 that is substantially devoid of the patterning coating 112.

[0264] Since the exposed layer surface 11 of the patterning coating 112 in the first portion 101 may exhibit a substantially low initial sticking probability against deposition of the deposited material 531 relative to an exposed layer surface 11 of the underlying layer 410 in the second portion 102, the deposited layer 330 may be selectively deposited substantially only on the exposed layer surface 11 of the underlying layer 410 in the second portion 102, that is substantially devoid of the patterning coating 112. By contrast, the evaporated flux 532 incident on the exposed layer surface 11 of the patterning coating 112 across the first porti on 101 may tend not to be deposited (as shown 533), and the exposed layer surface 11 of the patterning coating 112 across the first portion 101 may be substantially devoid of a closed coating 340 of the deposited layer 330.

[0265] In some non-limiting examples, an initial deposition rate, of the evaporated flux 532 on the exposed layer surface 11 of the underlying layer 410 in the second portion 102, maybe one of at least about: 200, 550, 900, 1,000, 1,500, 1,900, and 2,000, times an initial deposition rate of the evaporated flux 532 on the exposed layer surface 11 of the patterning coating 112 in the first portion 101.

[0266] Thus, the combination of the selective deposition of the patterning coating 112 in FIG. 4 using a shadow mask 415 and one of: the open mask, and a mask-free, deposition of the deposited material 531, may result in a version 510 shown in FIG. 5, of the device 300,

[0267] After selective deposition of the patterning coating 112 across the first portion 101, a closed coating 340 of the deposited material 531 may be deposited over the device 300 as the deposited layer 330, in some non-limiting examples, using one of: an open mask, and a mask- free, deposition process, but may remain substantially only within the second portion 102, which is substantially devoid of the patterning coating 112.

[0268] The patterning coating 112 may provide, within the first portion 101, an exposed layer surface 11 with a substantially low initial sticking probability, against deposition of the deposited material 531, and that is substantially no more than an initial sticking probability, against deposition of the deposited material 531, of the exposed layer surface 11 of the underlying layer 410 of the device 510 within the second portion 102.

[0269] Thus, the first portion 101 may be substantially devoid of a closed coating 340 of the deposited material 531.

[0270] While the present disclosure contemplates the patterned deposition of the patterning coating 112 by an evaporative deposition process, involving a shadow mask 415, those having ordinary skill in the relevant art will appreciate that, in some non-limiting examples, this may be achieved by any applicable deposition process, including without limitation, a micro¬ contact printing process.

[0271] While the present disclosure contemplates the patterning coating 112 being an NIC, those having ordinary skill in the relevant art wall appreciate that, in some non-limiting examples, the patterning coating 112 may be a nucleating promoting coating (NPC) 720. In such examples, the portion (including without limitation, the first portion 101) in which the NPC 720 has been deposited may, in some non-limiting examples, have a closed coating 340 of the deposited material 531, while the other portion (including without limitation, the second portion 102) may be substantially devoid of a closed coating 340 of the deposited material 531.

[0272] In some non-limiting examples, an average layer thickness of the: patterning coating 112, and deposited layer 330 deposited thereafter, may be varied according to a variety of parameters, including without limitation, a given application, and given performance characteristics. In some non-limiting examples, an average layer thickness of the patterning coating 112 may be comparable to, including without limitation, substantially no more than, an average layer thickness of the deposited layer 330 deposited thereafter. Use of a substantially thin patterning coating 112 to achieve selective patterning of a deposited layer 330 may have applicability to provide flexible layered semiconductor devices 410.

[0273] In some non-limiting examples, although not shown, the device 410 may comprise an NPC 720 disposed between the patterning coating 112 and the second electrode 140.

[0274] In some non-limiting examples, the patterning coating 112 may be formed concurrently with the at least one semiconducting layer 130. In some non-limiting examples, at least one material used to form the patterning coating 112 may also be used to form the at least one semiconducting layer 130 to reduce a number of stages for fabricating the device 410.Edge EffectsPatterning Coating Transition Region

[0275] Turning to FIG. 6A, there may be shown a version 600aof the devi ce 300 of FIG.3 that may show in exaggerated form, an interface between the patterning coating 112 in the first portion 101 and the deposited layer 330 in the second portion 102. FIG. 6B may show the device 600ain plan.

[0276] As may be better seen in FIG. 6B, in some non-limiting examples, the patterning coating 112 in the first portion 101 may be surrounded on all sides by the deposited layer 330 in the second portion 102, such that the first portion 101 may have a boundary' that is defined by the further edge 615 of the patterning coating 112 in the lateral aspect along each lateral axis. In some non-limiting examples, the patterning coating edge 615 in the lateral aspect may be defined by a perimeter of the first portion 101 in such aspect.

[0277] In some non-limiting examples, the first portion 101 may comprise at least one patterning coating transition region 101t, in the lateral aspect, in which a thickness of the patterning coating 112 may transition from a maximum, to a reduced, thickness. The extent of the first portion 101 that does not exhibit such a transition may be identified as a patterning coating non-transition part 10 lnof the first portion 101. In some non-limiting examples, thepatterning coating 112 may form a substantially closed coating 340 in the patterning coating non¬ transition part 10 In of the first portion 101.

[0278] In some non-limiting examples, the patterning coating transition region 10 It may extend, in the lateral aspect, between the patterning coating non-transition part 101nof the first portion 101 and the patterning coating edge 615.

[0279] In some non-limiting examples, in plan, the patterning coating transition region 10 It may extend along a perimeter of the patterning coating non-transition part 10% of the first portion 101.

[0280] In some non-limiting examples, along at least one lateral axis, the patterning coating non-transition part 10 In may occupy the entirety' of the first portion 101, such that there is no patterning coating transition region 1011 between it and the second portion 102.

[0281] As illustrated in FIG. 6A, in some non-limiting examples, the patterning coating 112 may have an average film thickness d? in the patterning coating non-transition part 101nof the first portion 101 that may be in a range of one of between about: 1-100, 2-50, 3-30, 4-20, 5-15, 5-10, and 1-10, nm. In some non-limiting examples, the average film thickness d?. of the patterning coating 112 in the patterning coating non-transition part 101 n of the first portion 101 may be substantially the same (constant) thereacross. In some non-limiting examples, an average film thickness eh of the patterning coating 112 may remain, within the patterning coating nontransition part 101n, within one of about: 95%, and 90%, of the average film thickness d2 of the patterning coating 112.

[0282] In some non-limiting examples, the average film thickness d may be between about 1-100 nm. In some non-limiting examples, the average film thickness ch may be one of no more than about: 80, 60, 50, 40, 30, 20, 15, and 10, nm. In some non-limiting examples, the average film thickness d2 of the patterning coating 112 may be one of at least about: 3, 5, and 8, nm.

[0283] In some non-limiting examples, the average film thickness d of the patterning coating 112 in the patterning coating non -transition part 101nof the first portion 101 may be no more than about 10 nm. Without wishing to be bound by any particular theory, it has been found that, a non-zero average film thickness tfo of the patterning coating 112 that is no more than about 10 nm may, in some non-limiting examples, provide certain advantages for achieving, in some non-limiting examples, enhanced patterning contrast of the deposited layer 330, relative to apatterning coating 112 having an average film thickness cb in the patterning coating non¬ transition part 10 In of the first portion 101 of at least about 10 nm.

[0284] In some non-limiting examples, the patterning coating 112 may have a patterning coating thickness that decreases from a maximum to a minimum within the patterning coating transition region 10 It. In some non-limiting examples, the maximum may be proximate to a boundary between the patterning coating transition region 10ft and the patterning coating non¬ transition part 101n of the first portion 101. In some non-limiting examples, the minimum may be proximate to the patterning coating edge 615. In some non-limiting examples, the maximum may be the average film thickness d in the patterning coating non-transition part 10 In of the first portion 101. In some non-limiting examples, the maximum may be one of no more than about: 95%, and 90%, of the average film thickness dz in the patterning coating non-transition part 101« of the first portion 101. In some non-limiting examples, the minimum may be in a range of between about 0-0.1 nm.

[0285] In some non-limiting examples, a profile of the patterning coating thickness in the patterning coating transition region 10 It may be sloped. In some non-limiting examples, such profile may be tapered. In some non-limiting examples, the taper may follow one of a: linear, non-linear, parabolic, and exponentially decaying, profile.

[0286] In some non-limiting examples, the patterning coating 112 may completely cover the underlying layer 410 in the patterning coating transition region 10 It. In some non-limiting examples, (a part, of) the underlying layer 410 may be left uncovered by the patterning coating 112 in the patterning coating transition region 101 t. In some non-limiting examples, the patterning coating 112 may comprise a substantially closed coating 340 in at least one of: (a part of) the patterning coating transition region 1011, and (a part of) the patterning coating non¬ transition part 10 In.

[0287] In some non-limiting examples, the patterning coating 112 may comprise a discontinuous layer 360 in at least one of: (a part of) the patterning coating transition region 1011, and (a part of) patterning coating non-transition part 10%.

[0288] In some non-limiting examples, (a part of) the patterning coating 112 in the first portion 101 may be substantially devoid of a closed coating 340 of the deposited layer 330. In some non-limiting examples, at least, a part of an exposed layer surface 11 of the first portion 101may be substantially devoid of a closed coating 340 of one of the: deposited layer 330, and deposited material 531.

[0289] In some non-limiting examples, along at least one lateral axis, including without limitation, the X-axis, the patterning coating non-transition part 101 n may have a width of wi, and the patterning coating transition region 10 It may have a width of wz In some non-limiting examples, the patterning coating non-transition part 101n may have a cross-sectional area that, in some non-limiting examples, may be approximated by multiplying the average film thickness dz by the width wy. In some non-limiting examples, the patterning coating transition region 1011 may have a cross-sectional area that, in some non-limiting examples, may be approximated by multiplying an average film thickness across the patterning coating transition region lOltby the width i.

[0290] In some non-limiting examples, w i may be at least that of wz. In some non¬ limiting examples, a quotient of wi / wz may be one of at least about: 5, 10, 20, 50, 100, 500, 1,000, 1,500, 5,000, 10,000, 50,000, and 100,000.

[0291] In some non-limiting examples, at least one of wl and 2 may be at least that of an average film thickness di of the underlying layer 410.

[0292] In some non-limiting examples, at least one of wy and wz may be at least that of dz. In some non-limiting examples, both wy and wz may be at least that of dz. In some non¬ limiting examples, wi and wz both may be at least that of di, and di may be at least that of dz.

[0293] In some non-limiting examples, along at least one lateral axis, the patterning coating non-transition part 10 lnmay occupy the entirety of the first portion 101, such that there is no patterning coating transition region 1011 between it and the second portion 102.Deposited Layer Transition Region

[0294] As may be better seen in FIG. 6B, in some non-limiting examples, the patterning coating 112 in the first portion 101 may be surrounded by the deposited layer 330 in the second portion 102 such that the second portion 102 has a boundary that is defined by a further edge 635 of the deposited layer 330 in the lateral aspect along each lateral axis. In some non-limiting examples, the deposited layer edge 635 in the lateral aspect may be defined by a perimeter of the second portion 102 in such aspect.

[0295] In some non-limiting examples, the second portion 102 may comprise at least one deposited layer transition region 102t, in the lateral aspect, in which a thickness of the deposited layer 330 may transition from a maximum, to a reduced, thickness. An extent of the second portion 102 that does not exhibit such a transition may be identified as a deposited layer non¬ transition part 102n of the second porti on 102. In some non-limiting examples, the deposited layer 330 may form a substantially closed coating 340 in the deposited layer non -transit! on part 10211 of the second portion 102.

[0296] In some non-limiting examples, in plan, the deposited layer transition region 102t may extend, in the lateral aspect, between the deposited layer non-transition part IO2n of the second portion 102 and the deposited layer edge 635.

[0297] In some non-limiting examples, in plan, the deposited layer transition region 102t may extend along a perimeter of the deposited layer non-transition part 102nof the second portion 102.

[0298] In some non-limiting examples, along at least one lateral axis, the deposited layer non-transition part 102nof the second portion 102 may occupy the entirety of the second portion 102, such that there is no deposited layer transition region 102t between it and the first portion 101.

[0299] As illustrated in FIG. 6A, in some non-limiting examples, the deposited layer 330 may have an average film thickness ds in the deposited layer non-transition part 102nof the second portion 102 that may be in a range of one of between about: 1-500, 5-200, 5-40, 10-30, and 10-100, nm. In some non-limiting examples, ds may be one of at least about: 10, 50, and 100, nm. In some non-limiting examples, the average film thickness ds of the deposited layer 330 in the deposited layer non-transition part 102t of the second portion 102 may be substantially the same (constant) thereacross.

[0300] In some non-limiting examples, ds may be at least that of an average film thickness di of the underlying layer 410.

[0301] In some non-limiting examples, a quotient dsidi may be one of at least about: 1.5, 2, 5, 10, 20, 50, and 100. In some non-limiting examples, the quotient dsidi may be in a range of one of between about: 0.1-10, and 0.2-40.

[0302] In some non-limiting examples, ds may be at least that of an average film thickness ds of the patterning coating 112.

[0303] In some non-limiting examples, a quotient dsid.2 may be one of at least about: 1.5, 2, 5, 10, 20, 50, and 100. In some non-limiting examples, the quotient dsid. may be in a range of one of between about: 0.2-10, and 0.5-40.

[0304] In some non-limiting examples, ds may be at least that of d> and ds may be at least that of di. In some non-limiting examples, ds may be at least that of di and di may be at least that of ds.

[0305] In some non-limiting examples, a quotient dsldi may be between one of about: 0.2-3, and 0.1-5.

[0306] In some non-limiting examples, along at least one lateral axis, including without limitation, the X-axis, the deposited layer non-transition part 102nof the second portion 102 may have a width of w. In some non-limiting examples, the deposited layer non-transition part 102aof the second portion 102 may have a cross-sectional area as that, in some non-limiting examples, may be approximated by multiplying the average film thickness ds by the width ms.

[0307] In some non-limiting examples, ws may be at least that of the width wi of the patterning coating non-transition part 101B. In some non-limiting examples, wi may be at least that of ws.

[0308] In some non-limiting examples, a quotient wiiws may be in a range of one of between about: 0.1-10, 0.2-5, 0.3-3, and 0.4-2. In some non-limiting examples, a quotient ws!w i may be one of at least about: 1, 2, 3, and 4.

[0309] In some non-limiting examples, ws may be at least that of an average film thickness ds of the deposited layer 330.

[0310] In some non-limiting examples, a quotient wsids may be one of at least about: 10, 50, 100, and 500. In some non-limiting examples, the quotient wslds may be no more than about 100,000.

[0311] In some non-limiting examples, the deposited layer 330 may have a thickness that decreases from a maximum to a minimum within the deposited layer transition region 102t. In some non-limiting examples, the maximum may be proximate to a boundary between the deposited layer transition region 102t and the deposited layer non-transition part 102n of the second portion 102. In some non-limiting examples, the minimum may be proximate to the deposited layer edge 635. In some non-limiting examples, the maximum may be an average filmthickness ds in the deposited layer non-transition part 102n of the second portion 102. In some non-limiting examples, the minimum may be in a range of between about 0-0.1 nm. In some non-limiting examples, the minimum may be the average film thickness ds in the deposited layer non-transition part 102nof the second portion 102.

[0312] In some non-limiting examples, a profile of the thickness in the deposited layer transition region 102t may be sloped. In some non-limiting examples, such profile may be tapered. In some non-limiting examples, the taper may follow one of a: linear, non-linear, parabolic, and exponentially decaying, profile.

[0313] In some non-limiting examples, although not shown, the deposited layer 330 may completely cover the underlying layer 410 in the deposited layer transition region 102t. In some non-limiting examples, the deposited layer 330 may comprise a. substantially closed coating 340 in (a part of) the deposited layer transition region I02t. In some non-limiting examples, (a part of) the underlying layer 410 may be uncovered by the deposited layer 330 in the deposited layer transition region 102t.

[0314] In some non-limiting examples, the deposited layer 330 may comprise a discontinuous layer 360 in (a part of) the deposited layer transition region 102t.

[0315] Those having ordinary skill in the relevant art will appreciate that, although not shown, the patterning material 411 may be present to some extent at an interface between the deposited layer 330 and an underlying layer 410. Such material may be deposited as a result of a shadowing effect, in which a deposited pattern is not identical to a pattern of a mask and may, in some non-limiting examples, result in some evaporated patterning material 411 being deposited on a masked part of a target exposed layer surface 11. In some non-limiting examples, such material may form as at. least, one of: particle structures 350, and as a thin film having a thickness that may be substantially no more than an average thickness of the patterning coating 112.

[0316] In some non-limiting examples, along at least one lateral axis, the deposited layer non-transition part 102nof the second portion 102 may occupy the entirety of the second portion 102, such that there is no deposited layer transition region 102t between it and the first portion 101.Overlap

[0317] In some non-limiting examples, although not shown, the deposited layer edge 635 may be spaced apart, in the lateral aspect, from the patterning coating transition region 10 It ofthe first portion 101, such that there is no overlap between the first portion 101 and the second portion 102 in the lateral aspect.

[0318] In some non-limiting examples, (a part of) the first portion 101, and (a part of) the second portion 102, may overlap in the lateral aspect. Such overlap may be identified by an overlap portion 603, such as may be shown in some non-limiting examples in FIG. 7A, in which (a part of) the second portion 102 overlaps (a part of) the first portion 101.

[0319] In some non-limiting examples, although not shown, (a part of) the deposited layer transition region 102t may be disposed over (a part of) the patterning coating transition region 101t. In some non-limiting examples, (a part of) the patterning coating transition region 101t may be substantially devoid of at least one of the: deposited layer 330, and deposited material 531. In some non-limiting examples, the deposited material 531 may form a discontinuous layer 360 on an exposed layer surface 11 of (a part of) the patterning coating transition region 101t.

[0320] In some non-limiting examples, although not shown, (a part of) the deposited layer transition region 102t may be disposed over (a part of) the patterning coating non-transition part. 101n of the first portion 101.

[0321] Although not shown, those having ordinary skill in the relevant art will appreciate that, in some non-limiting examples, the overlap portion 603 may reflect a scenario in which (a part of) the first portion 101 overlaps (a part of) the second portion 102.

[0322] Thus, in some non-limiting examples, (a part of) the patterning coating transition region 101t may be disposed over (a part of) the deposited layer transition region 102t. In some non-limiting examples, (a part of) the deposited layer transition region 102t may be substantially devoid of at least one of the: patterning coating 112, and patterning material 411. In some non¬ limiting examples, the patterning material 411 may form a discontinuous layer 360 on an exposed layer surface 11 of (a part of) the deposited layer transition region 102t.

[0323] In some non-limiting examples, (a part of) the patterning coating transition region 101t may be disposed over (a part of) the deposited layer non-transition part 102nof the second portion 102.

[0324] In some non-limiting examples, the patterning coating edge 615 may be spaced apart, in the lateral aspect, from the deposited layer non-transition part 102nof the second portion 102.

[0325] In some non-limiting examples, the deposited layer 330 may be formed as a single monolithic coating across both the deposited layer non-transition part 102nand the deposited layer transition region 102t of the second portion 102.

[0326] In some non-limiting examples, at least one deposited layer 330, including without limitation, an initial deposited layer 330, may provide, at least in part, the functionality of an EIL 139, in the emissive region 110. In some non-limiting examples, the deposited material 531 for forming such initial deposited layer 330 may comprise Yb, which may, in some non-limiting examples, be substantially about 1-3 nm in thickness.Edge Effects of Patterning Coatings and Deposited Layers

[0327] FIGs. 7A-7B describe various potential behaviours of patterning coatings 130 at a deposition interface with deposited layers 140.

[0328] Turning to FIG. 7 A, there may be shown a first example of a part of an example version 700aof the device 300 at a patterning coating deposition boundary. The device 700amay comprise a substrate 10 having an exposed layer surface 11. A patterning coating 112 may be deposited over a first portion 101 of the exposed layer surface 11 of the underlying layer 410. A deposited layer 330 may be deposited over a second portion 102 of the exposed layer surface 11 of the underlying layer 410. As shown, in some non-limiting examples, the first portion 101 and the second portion 102 may be distinct and non-overlapping parts of the exposed layer surface 11.

[0329] In some non-limiting examples, the deposited layer 330 may comprise a first part 330i and a second part 330?. As shown, in some non-limiting examples, the first part 330i of the deposited layer 330 may substantially cover the second portion 102 and the second part 3302 of the deposited layer 330 may partially overlap (project over) a first part of the patterning coating 112.

[0330] In some non-limiting examples, since the patterning coating 112 may be formed such that its exposed layer surface 11 exhibits a substantially low initial sticking probability against deposition of the deposited material 531, there may be a gap 729 formed between the projecting second part 3302 of the deposited layer 330 and the exposed layer surface 11 of the patterning coating 112. As a result, the second part 330 may not be in physical contact with the patterning coating 112 but may be spaced-apart therefrom by the gap 729, in a cross-sectional aspect. In some non-limiting examples, the first part 3301 of the deposited layer 330 may be inphysical contact with the patterning coating 112 at an interface (boundary) between the first portion 101 and the second portion 102.

[0331] In some non-limiting examples, the projecting second part 3302 of the deposited layer 330 may extend laterally over the patterning coating 112 by an extent that may be comparable to an average layer thickness da of the first part 330i of the deposited layer 330. As shown, in some non-limiting examples, a width m of the second part. 3302 may be comparable to the average layer thickness da of the first part 330]. In some non-limiting examples, a ratio of a width My of the second part 3302 by an average layer thi ckness da of the first part 3301 may be in a range of one of between about: 1:1-1:3, 1:1-1:1 5, and1:1-1:2. While the average layer thickness ^may, in some non-limiting examples, be substantially uniform across the first part 330i, in some non-limiting examples, an extent to which the second part 3302 may project over the patterning coating 112 (namely wb), may vary to some extent across different parts of the exposed layer surface 11.

[0332] In some non-limiting examples, the deposited layer 330 may be shown to include a third part 330? disposed between the second part 3302 and the patterning coating 112. As shown, the second part 330? of the deposited layer 330 may extend laterally over, and may be longitudinally spaced apart from, the third part 3303 of the deposited layer 330, and the third part 330? may be in physical contact with the exposed layer surface 11 of the patterning coating 112. An average layer thickness dcof the third part 330j of the deposited layer 330 may be (substantially) no more than an average layer thickness daof the first part 330i thereof. In some non-limiting examples, a width wcof the third part 330? may be at least that of a width wi, of the second part 3302. In some non-limiting examples, the third part 330i may extend laterally to overlap the patterning coating 112 to an extent that is at least that of the second part 3302. In some non-limiting examples, a ratio of a width wcof the third part 330?, by an average layer thickness da of the first part 330i, may be in a range of one of between about: 1:2-3: 1, and 1: 1.2- 2.5:1. While the average layer thickness damay, in some non-limiting examples, be substantially uniform across the first part 330i, in some non-limiting examples, an extent to which the third part 330s may project (overlap) with the patterning coating 112 (iw) may vary' to some extent across different parts of the exposed layer surface 11.

[0333] In some non-limiting examples, an average layer thickness dc of the third part 3301 may be no more than substantially about 5% of an average layer thickness da of the first part 330i. In some non-limiting examples, dcmay be one of no more than about: 4%, 3%, 2%, 1%,and 0,5% of da. In some non-limiting examples, instead of (including without limitation, in addition to) the third part 3303 being formed as a thin film, as shown, the deposited material 531 of the deposited layer 330 may form as particle structures 350 (not shown) on a part of the patterning coating 112. In some non-limiting examples, such particle structures 350 may comprise features that are physically separated from one another, such that, they do not form a continuous layer.

[0334] In some non-limiting examples, as shown, an NPC 720 may be disposed between the substrate 10 and the deposited layer 330. In some non-limiting examples, the NPC 720 may be disposed between the first part 330i of the deposited layer 330 and the second portion 102 of the exposed layer surface 11 of the underlying layer 410. The NPC 720 is illustrated as being disposed on the second portion 102 and not on the first portion 101, where the patterning coating 112 has been deposited. In some non-limiting examples, the NPC 720 may be formed such that, at an interface (boundary) between the NPC 720 and the deposited layer 330, a surface of the NPC 720 may exhibit a substantially high initial sticking probability against deposition of the deposited material 531. As such, the presence of the NPC 720 may promote the formation (growth) of the deposited layer 330 during deposition.

[0335] In some non-limiting examples, although not shown, the NPC 720 may be disposed on both the first portion 101 and the second portion 102 of the substrate 10, and the underlying layer 410 may cover a part of the NPC 720 disposed on the first portion 101, and another part of the NPC 720 may be substantially devoid of the underlying layer 410 and of the patterning coating 112, and the deposited layer 330 may cover such part of the NPC 720.

[0336] Turning now to FIG. 7B, in some non-limiting examples, the first portion 101 of the substrate 10 may be coated with the patterning coating 112 and the second portion may be coated with the deposited layer 330. In some non-limiting examples, the deposited layer 330 may partially overlap a part of the patterning coating 112 in a third portion 703 of the substrate 10. In some non-limiting examples, although not shown, in addition to the first part 330i (and, if present, at least one of the: second part 3302, and third part 330j), the deposited layer 330 may comprise a fourth part 3304 that may be disposed between the first part 330i and the second part 3302 of the deposited layer 330, and in physical contact with an exposed layer surface 11 of the patterning coating 112. In some non-limiting examples, the fourth part. 3304 of the deposited layer 330 overlapping a subset of the patterning coating 1120in the third portion 703 may be in physical contact with an exposed layer surface 11 thereof. In some non-limiting examples, theoverlap in the third portion 703 may be formed as a result of lateral growth of the deposited layer 330 during one of: an open mask, and a mask-free, deposition process. In some non-limiting examples, while the exposed layer surface 11 of the patterning coating 112 may exhibit a substantially low initial sticking probability against deposition of the deposited material 531, and thus a probability of the material nucleating on the exposed layer surface 11 may be substantially low, as the deposited layer 330 grows in thickness, the deposited layer 330 may also grow laterally and may cover a subset of the patterning coating 112 as shown.

[0337] In some non-limiting examples, it has been observed that conducting one of: an open mask, and a mask-free, deposition of the deposited layer 330 may result in the deposited layer 330 exhibiting a tapered cross-sectional profile proximate to an interface between the deposited layer 330 and the patterning coating 112.

[0338] In some non-limiting examples, an average layer thickness of the deposited layer 330 proximate to the interface may be no more than an average film thickness ds of the deposited layer 330. While such tapered profde may be shown as being at least one of: curved, and arched, in some non-limiting examples, the profile may, in some non-limiting examples, be substantially one of: linear, and non-linear. In some non-limiting examples, an average film thickness ds of the deposited layer 330 may decrease, without limitation, in a fashion that is substantially at least one of: linear, exponential, and quadratic, in a region proximate to the interface.

[0339] It has been observed that a (thin film) contact angle 0c (FIG. 17) of the deposited layer 330 proximate to an interface between the deposited layer 330 and the patterning coating 112 may vary', depending on properties of the patterning coating 112, including without limitation, an initial sticking probability. It may be postulated that a contact angle 0Cof the nuclei may, in some non-limiting examples, dictate what a contact angle of the deposited layer 330 formed by deposition will be. Referring to FIG. 7B in some non-limiting examples, the contact angle 0cmay be determined by measuring a slope of a tangent of the deposited layer 330 proximate to an interface between the deposited layer 330 and the patterning coating 112. In some non-limiting examples, where the cross-sectional taper profile of the deposited layer 330 is substantially linear, the contact angle 0Cmay be determined by measuring a slope of the deposited layer 330 proximate to the interface. As will be appreciated by those having ordinary skill in the relevant art, the contact angle 0c may be generally measured relative to a non-zero angle of the underlying layer 410. In the present disclosure, for purposes of simplicity of illustration, the patterning coating 112 and the deposited layer 330 may be shown deposited on aplanar surface. However, those having ordinary skill in the relevant art will appreciate that the patterning coating 112 and the deposited layer 330 may be deposited on non-planar surfaces.

[0340] In some non-limiting examples, as shown in FIG. 7A, the contact angle 6'cof the deposited layer 330 may be at least about 90° and, in some non-limiting examples, the deposited layer 330 may be shown as including a part 330? extending past an interface between the patterning coating 112 and the deposited layer 330, and may be spaced apart from the patterning coating 112 (and, in some non-limiting examples, the third part 330? of the deposited layer 330), by the gap 729. In such non-limiting scenario, the contact angle 0c may, in some non-limiting examples, be at least 90°.

[0341] In some non-limiting examples, there may be scenarios calling for a deposited layer 130 exhibiting a substantially high contact angleIn some non-limiting examples, the contact angle 0cmay be one of at least about: 10°, 15°, 20°, 25°, 30°, 35°, 40°, 50°, 70°, 75°, and 80°. In some non-limiting examples, a deposited layer 330 having a substantially high contact angle 0cmay allow for creation of finely patterned features while maintaining a substantially high aspect ratio. In some non-limiting examples, there may be scenarios calling for a deposited layer 330 exhibiting a contact angle 0cthat may be at least about 90°. In some non-limiting examples, the contact angle 0cmay be one of at least about: 90°, 95°, 100°, 105°, 110° 120°, 130°, 135°, 140°, 145°, 150°, and 170°.

[0342] In some non-limiting examples, the contact angle 0c of the deposited layer 330 may be measured at an edge thereof near an interface between it and the patterning coating 112, as shown. In FIG. 7A, the contact angle 0cmay be at least about 90°, which may in some non¬ limiting examples result in a subset, namely the second part 3302, of the deposited layer 330 being spaced apart from the patterning coating 112 (and, in some non-limiting examples, the third part 330r of the deposited layer 330) by the gap 729.Particle Structure

[0343] An NP is a particle of matter whose predominant characteristic size is of nanometer (nm) scale, generally understood to be between about: 1-300 nm. At nm scale, NPs of a given material may possess unique properties (including without limitation, optical, chemical, physical, and electrical) relative to the same material in bulk form, including without limitation, an amount of absorption of light exhibited by such NPs at different wavelengths (ranges).

[0344] These properties may be exploited when a plurality of NPs is formed into a layer of a layered semiconductor device 300, including without limitation, an opto-electronic device 100, to improve its performance.

[0345] Current mechanisms for introducing such a layer of NPs into such a device 300 have some drawbacks.

[0346] First, in some non-limiting examples, such NPs may be formed into at least one of: a close-packed layer, and dispersed into a matrix material, of such device 300. Consequently, in some non-limiting examples, a thickness of such an NP layer may be substantially at least that of a characteristic size of the NPs themselves. A thickness of such NP layer may impart characteristics in terms of at least one of substantially poor device: performance, stability, reliability, and lifetime, that may reduce, including without limitation, obviate, any perceived advantages provided by the unique properties of NPs.

[0347] Second, techniques to synthesize NPs, in and for use in such devices, may introduce large amounts of at least one of: C, O, and S, through various mechanisms.

[0348] In some non-limiting examples, wet chemical methods may be used to introduce NPs that have a precisely controlled characteristic at least one of: size, length, width, diameter, height, size distribution, shape, surface coverage, configuration, deposited density, dispersity, and composition, into an opto-electronic device 100. Such methods may, in some non-limiting examples, employ an organic capping group (including without limitation, synthesis of citrate- capped Ag NPs) to stabilize the NPs, but such organic capping groups may introduce at least one of: C, O, and S, into the synthesized NPs.

[0349] In some non-limiting examples, an NP layer deposited from solution may comprise at least one of: C, O, and S, because of the solvents used in deposition.

[0350] In some non-limiting examples, these elements may be introduced as contaminants during at least one of the: wet chemical process, and deposition of the NP layer.

[0351] However introduced, the presence of a substantially high amount of at least one of: C, O, and S, in the NP layer of such a device 100, may erode at least one of the: performance, stability, reliability, and lifetime, of such device 100.

[0352] Third, when depositing an NP layer from solution, as the employed solvents dry,, the NP layer(s) may tend to have non-uniform properties at least one of: across the NP layer, andbetween different patterned regions of such layer. In some non-limiting examples, an edge of a given layer may be considerably at least one of: thicker and thinner, than an internal region of such layer, which disparities may adversely impact at least one of the device: performance, stability, reliability, and lifetime.

[0353] Fourth, while there are other methods (and processes) beyond wet chemical synthesis and solution deposition processes, of at least one of: synthesizing and depositing, NPs, including without limitation, a vacuum-based process including without limitation, PVD, such methods tend to provi de substantially little control of the characteristic at least one of: size, length, width, diameter, height, size distribution, shape, surface coverage, configuration, deposited density, dispersity, and composition, of the NPs deposited thereby. In some non¬ limiting examples, in a PVD process, the NPs tend to form a close-packed fdm as their size increases. As a result, methods such as PVD may not generally be well-suited to form a layer of large disperse NPs with low surface coverage. Rather, the substantially little control of at least one of the: characteristic size, length, width, diameter, height, size distribution, shape, surface coverage, configuration, deposited density, dispersity, and composition, imparted by such methods may result in at least one of substantially reduced device: performance, stability, reliability, and lifetime.

[0354] In some non-limiting examples, such as may be shown in FIG. 6A, there may be at least one particle, including without limitation, at least one of an NP, an island, a plate, a disconnected cluster, and a network (collectively particle structure 350) disposed on an exposed layer surface 11 of an underlying layer 410. In some non-limiting examples, the underlying layer 410 may be the patterning coating 112 in the first portion 101. In some non-limiting examples, the at least one particle structure 350 may be disposed on an exposed layer surface 11 of the patterning coating 112. In some non-limiting examples, there may be a plurality of such particle structures 350.

[0355] In some non-limiting examples, the at least one particle structure 350 may comprise a particle material. In some non-limiting examples, the particle material may be the same as the deposited material 531 including without limitation, a substantially low loss Ag (composite) material, in the deposited layer 330.

[0356] In some non-limiting examples, the particle material in the discontinuous layer 360 in the first portion 101, at least one of: the deposited material 531 in the deposited layer 330,and a material of which the underlying layer 410 thereunder may be comprised, may comprise a metal in common.

[0357] In some non-limiting examples, although not shown, at least one particle structure 350d of a discontinuous layer 360 of a particle material may extend partially over the patterning coating 112, which may act. as a particle structure patterning coating 112pin the transition region 145. In some non-limiting examples, such discontinuous layer 360 may form (a part of) the second electrode 140. In some non-limiting examples, the particle material may be the same as a material of which the deposited layer 130 may be comprised (deposited material 531).

[0358] In some non-limiting examples, the particle material may comprise an element selected from at least one of: K, Na, Li, Ba, Cs, Yb, Ag, Au, Cu, Al, Mg, Zn, Cd, Sn, and Y. In some non-limiting examples, the element may comprise at least one of: K, Na, Li, Ba, Cs, Yb, Ag, Au, Cu, Al, and Mg. In some non-limiting examples, the element may comprise at least one of: Cu, Ag, and Au. In some non-limiting examples, the element may be Cu. In some non¬ limiting examples, the element may be Al. In some non-limiting examples, the element may comprise at least one of: Mg, Zn, Cd, and Yb. In some non-limiting examples, the element may comprise at least one of: Mg, Ag, Al, Yb, and Li. In some non-limiting examples, the element may comprise at least one of: Mg, Ag, and Yb. In some non-limiting examples, the element may comprise at least one of: Mg, and Ag. In some non-limiting examples, the element may be Ag. In some non-limiting examples, the element may be A.u.

[0359] In some non-limiting examples, the particle material may comprise a pure metal. In some non-limiting examples, the at least one particle structure 350 may be a pure metal. In some non-limiting examples, the at least one particle structure 350 may be (substantially) pure Ag. In some non-limiting examples, the substantially pure Ag may have a purity of one of about: 95%, 99%, 99.9%, 99.99%, 99.999%, and 99.9995%. In some non-limiting examples, the at least one particle structure 350 may be (substantially) pure Mg. In some non-limiting examples, the substantially pure Mg may have a purity of one of at least about: 95%, 99%, 99.9%, 99.99%, 99.999%, and 99.9995%.

[0360] In some non-limiting examples, the at least one particle structure 350 may comprise an alloy. In some non-limiting examples, the alloy may be one of an: Ag-containing, Mg-containing, Au-containing, and AgMg-containing, alloy. In some non-limiting examples, the AgMg-containing alloy may have an alloy composition that may range from about 1:10 (Ag: Mg) to about 10:1 by volume.

[0361] In some non-limiting examples, the particle material may comprise other metals one of: in place of, and in combination with, Ag. In some non-limiting examples, the particle material may comprise an alloy of Ag with at least one other metal, including without limitation, at least one of: Mg, and Yb. In some non-limiting examples, such alloy may be a binary alloy having a composition of between about: 5-95 vol,% Ag, with the remainder being the other metal. In some non-limiting examples, the particle material may comprise Ag and Mg. In some non-limiting examples, the particle material may comprise an Ag: Mg alloy having a composition of between about 1: 10-10:1 by volume. In some non-limiting examples, the particle material may comprise Ag and Yb. In some non-limiting examples, the particle material may comprise a Yb: Ag alloy having a composition of between about 1:20-10:1 by volume. In some non-limiting examples, the particle material may comprise Mg and Yb. In some non-limiting examples, the particle material may comprise an Mg: Yb alloy. In some non-limiting examples, the particle material may comprise an Ag: Mg: Yb alloy.

[0362] In some non-limiting examples, the particle material may comprise other metals one of: in place of, and in combination with, Au. In some non-limiting examples, the particle material may comprise an alloy of Au with at least one other metal.

[0363] In some non-limiting examples, the at least one particle structure 350 may comprise at least one additional element. In some non-limiting examples, such additional element may be a non-metallic element. In some non-limiting examples, the non-metallic element may be one of O, S, N, and C. It will be appreci ted by those having ordinary skill in the relevant art that, in some non-limiting examples, such additional element(s) may be incorporated into the at least one particle structure 350 as a contaminant, due to the presence of such additional element(s) in at least one of the: source material, equipment used for deposition, and vacuum chamber environment. In some non-limiting examples, such additional element(s) may form a compound together with other element(s) of the at least one particle structure 350. In some non-limiting examples, a concentration of the non-metallic element in the particle material may be one of no more than about: 1%, 0.1%, 0.01%, 0.001%, 0.0001%, 0.00001%, 0.000001%, and 0.0000001%. In some non-limiting examples, the at least one particle structure 350 may have a composition, in which a. combined amount of O and C therein, is one of no more than about: 10%, 5%, 1%, 0.1%, 0.01%, 0.001%, 0.0001%, 0.00001%, 0.000001%, and 0.0000001%.

[0364] The at least one particle structure 350 takes advantage of plasmonics, a branch of nanophotonics, which studies the resonant interaction of light with metals. Those havingordinary skill in the relevant art will appreciate that metal NPs may exhibit at least one of: localized surface plasmon (LSP) excitations, and coherent oscillations of free electrons, whose optical response may be tailored by varying at least one of a characteristic: size, size distribution, shape, surface coverage, configuration, deposited density, and composition, of the nanostructures. Such optical response, in respect of particle structures 350, may include absorption of light incident thereon, thereby reducing at least one of: reflection thereof, and shifting to one of a: lower, and higher, wavelength ((sub-) range) of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum.

[0365] It has also been reported that arranging certain metal NPs near a medium having substantially low refractive index, may shift the absorption spectrum of such NPs to a lower wavelength (sub-) range (blue-shifted).

[0366] Accordingly, it may be postulated that disposing particle material, in some non¬ limiting examples, as a discontinuous layer 360 of at least one particle structure 350 on an exposed layer surface 11 of an underlying layer 410, such that the at least one particle structure 350 is in physical contact with the underlying layer 410, may, in some non-limiting examples, shift the absorption spectrum of the particle material, including without limitation, blue-shift, such that it does not substantially overlap with a wavelength range of the EM spectrum of light being at least one of: emitted by, and transmitted at least partially through, the device 300.

[0367] In some non-limiting examples, a peak absorption wavelength of the at least one particle structure 350 may be no more than a peak wavelength of the light being at least one of: emitted by, and transmitted, at least partially through the device 300. In some non-limiting examples, the particle material may exhibit a peak absorption at a wavelength (range) that is one of no more than about: 470, 460, 455, 450, 445, 440, 430, 420, and 400, nm.

[0368] It has now been found that, providing particle material, including without limitation, in the form of at least one particle structure 350, including without: limitation, those comprised of a metal, proximate to, including without limitation, within, at least one lo (er )- index coating, may further impact at least one of the: absorption, and transmittance, of light passing through the device 300, including without limitation, in a first direction, in at least a wavelength (sub-) range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum, passing in the first direction from, including without limitation, through, the at least one low(er)-index layer(s) and the at least one particle structure(s) 350.

[0369] In some non-limiting examples, at least one of: absorption may be reduced, and transmittance may be facilitated, in at least a wavelength (sub-) range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum.

[0370] In some non-limiting examples, absorption may be concentrated in an absorption spectrum that is a wavelength (sub-) range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum.

[0371] In some non-limiting examples, the absorption spectrum may be one of: blue- shifted, and shifted to a higher wavelength (sub-) range (red-shifted), including without limitation, to a wavelength (sub-) range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum, and to a wavelength (sub-) range of the EM spectrum that lies, at least in part, beyond the visible spectrum.

[0372] Those having ordinary skill in the relevant art will appreci te that in some non¬ limiting examples, a plurality of layers of at least one particle structure 350, may be disposed on one another, whether separated by additional layers, with varying lateral aspects and having different absorption spectra. In this fashion, absorption of certain regions of the device 300 may be tuned according to at least one desired absorption spectra.

[0373] In some non-limiting examples, the presence of the at least one particle structure 350, including without limitation, NPs, including without limitation, in a discontinuous layer 360, on an exposed layer surface 11 of the patterning coating 112 may affect some optical properties of the device 300.

[0374] In some non-limiting examples, such plurality of particle structures 350 may form a discontinuous layer 360.

[0375] Without wishing to be limited to any particular theory, it may be postulated that, while the formation of a closed coating 340 of the particle material may be substantially inhibited by the patterning coating 112, in some non-limiting examples, when the patterning coating 112 is exposed to deposition of the particle material thereon, some vapor monomers of the particle material may ultimately form at least one particle structure 350 of the particle material thereon.

[0376] In some non-limiting examples, at least some of the particle structures 350 may be disconnected from one another. In some non-limiting examples, the discontinuous layer 360 may comprise features, including particle structures 350, that may be physically separated from one another, such that the particle structures 350 do not form a closed coating 340. Accordingly,such discontinuous layer 360 may, in some non-limiting examples, thus comprise a thin disperse layer of deposited material 531 formed as particle structures 350, inserted at, including without limitation, substantially across, a lateral extent of, an interface between the patterning coating 112 and at least one overlying layer 370 in the device 300.

[0377] In some non-limiting examples, at least one (including without limitation, substantially all) of the particle structures 350 of particle material may be in physical contact with an exposed l yer surface 11 of the patterning coating 112.

[0378] Without wishing to be bound by any particular theory, it has been found that, the presence of such a thin, disperse discontinuous layer 360 of particle material, including without limitation, at least one (metal) particle structure 350, on an exposed layer surface 11 of the patterning coating 112, may exhibit at least one varied characteristic and concomitantly, varied behaviour, including without limitation, optical effects and properties of the device 300, as discussed herein. In some non-limiting examples, such effects and properties may be controlled to some extent by judicious selection of a characteristic at least one of a: size, size distribution, shape, surface coverage, configuration, deposited density, and dispersity, of the particle structures 350 on the patterning coating 112.

[0379] In some non-limiting examples, the particle structures 350 may be controllably selected so as to have a characteristic at least one of a: size, length, width, diameter, height, size distribution, shape, surface coverage, configuration, deposited density, dispersity, and composition, to achieve an effect related to an optical response exhibited by the particle structures 350.

[0380] Those having ordinary skill in the relevant art will appreciate that, having regard to the mechanism by which materials are deposited, due to possible stacking, including without limitation, clustering, of at least one of: monomers, and atoms, at least one of an actual: size, height, weight, thickness, shape, profile, and spacing, of the at least one particle structure 350 may be, in some non-limiting examples, substantially non-uniform. In some non-limiting examples, although the at least one particle structure 350 are illustrated as having a given profile, this is intended to be illustrative only, and not determinative of at least one of a: size, height, weight, thickness, shape, profile, and spacing, thereof.

[0381] In some non-limiting examples, the at least one particle structure 350 may have a characteristic dimension of no more than about 200 nm. In some non-limiting examples, the atI east one particle structure 350 may have a characteristic diameter that may be one of between about: 1-200, 1-160, 1-100, 1-50, and 1-30, nm.

[0382] In some non-limiting examples, the at least one particle structure 350 may comprise discrete metal plasmonic islands (clusters).

[0383] In some non-limiting examples, the at least one particle structure 350 may comprise a particle material.

[0384] In some non-limiting examples, such particle structures 350 may be formed by depositing a scant amount, in some non-limiting examples, having an average layer thickness that may be on the order of one of a: few, and fraction of one, angstrom(s), of a particle material on an exposed layer surface 11 of the underlying layer 410. In some non-limiting examples, the exposed layer surface 11 may be of an NPC 720.

[0385] In some non-limiting examples, the particle material may comprise at least one of: Ag, Yb, and Mg.

[0386] In some non-limiting examples, the formation of a characteristic at least one of a: size, size distribution, shape, surface coverage, configuration, deposited density, and dispersity, of particle structures 350 of such discontinuous layer 360 may be controlled, in some non¬ limiting examples, by judicious selection of at least one of a characteristic of the patterning material 411, an average film thickness (h of the patterning coating 112, and introduction of heterogeneities in at least one of: the patterning coating 112, and a deposition environment, including without limitation, a temperature, pressure, duration, deposition rate, and deposition process, for the patterning coating 11.

[0387] In some non-limiting examples, the formation of at least one of a characteristic: size, size distribution, shape, surface coverage, configuration, deposited density, and dispersity, of such discontinuous layer 360 may be controlled, in some non-limiting examples, by judicious selection of at least one of: at least one characteristic of the particle material (which may be the deposited material 531), an extent to which the patterning coating 112 may be exposed to deposition of the particle material (which, in some non-limiting examples may be specified in terms of a thickness of the corresponding discontinuous layer 360), and a deposition environment, including without limitation, at least one of a: temperature, pressure, duration, deposition rate, and method of deposition, of the particle material.

[0388] In some non-limiting examples, the discontinuous layer 360 may be deposited in a pattern across the lateral extent of the patterning coating 112.

[0389] In some non-limiting examples, the discontinuous layer 360 may be disposed in a pattern that may be defined by at least one region therein that is substantially devoid of the at least one particle structure 350.

[0390] In some non-limiting examples, the characteristics of such discontinuous layer 360 may be assessed, in some non-limiting examples, somewhat arbitrarily, according to at least one of several criteria, including without limitation, at least one of a characteristic: size, size distribution, shape, configuration, surface coverage, deposited distribution, dispersity, and a presence, and an extent of aggregation instances, of the particle material, formed on a part of the exposed layer surface 11 of the underlying layer 410.

[0391] In some non-limiting examples, an assessment of the discontinuous layer 360 according to such at least one criterion, may be performed on, including without limitation, by at least one of: measuring, and calculating, at least one attribute of the discontinuous layer 360, using a variety of imaging techniques, including without limitation, at least one of: transmission electron microscopy (TEM), atomic force microscopy (AFM), and SEM.

[0392] Those having ordinary skill in the relevant art will appreciate that such an assessment of the discontinuous layer 360 may depend, to at least one of a: greater, and lesser, extent, by the extent, of the exposed layer surface 11 under consideration, which in some non¬ limiting examples may comprise an area, including without limitation, a region thereof. In some non-limiting examples, the discontinuous layer 360 may be assessed across the entire extent, in at least one of a: first, and second, lateral aspect that is substantially transverse thereto, of the exposed layer surface 11. In some non-limiting examples, the discontinuous layer 360 may be assessed across an extent that comprises at least one observation window applied against (a part of) the discontinuous layer 360,

[0393] In some non-limiting examples, the at least one observation window may be located at at least one of a: perimeter, interior location, and grid coordinate, of the lateral aspect of the exposed layer surface 11. In some non-limiting examples, a plurality of the observation windows may be used in assessing the discontinuous layer 360.

[0394] In some non-limiting examples, the observation window may correspond to a field of view of an imaging technique applied to assess the discontinuous layer 360, includingwithout limitation, at least one of: TEM, AFM, and SEM. In some non-limiting examples, the observation window may correspond to a given level of magnification, including without limitation, one of: 2.00, and 1,00, pm, and 500, and 200, nm.

[0395] In some non-limiting examples, an assessment of the discontinuous layer 360, including without limitation, at least one observation window used, of an exposed layer surface 11 thereof, may involve at least one of calculating, and measuring, by any number of mechanisms, including without limitation, at least one of: manual counting, and known estimation techniques, which may, in some non-limiting examples, may comprise at least one of: curve, polygon, and shape, fitting techniques.

[0396] In some non-limiting examples, an assessment of the discontinuous layer 360, including without limitation, at least one observation window used, of the exposed layer surface 11 thereof, may involve at least one of: calculating, and measuring, at least one of: an average, median, mode, maximum, minimum, and other at least one of: probabilistic, statistical, and data, manipulation, of a value of the at least one of: calculation, and measurement.

[0397] In some non-limiting examples, one of the at least one criterion by which such discontinuous layer 360 may be assessed, may be a surface coverage of the particle material on such (part of the) discontinuous layer 360. In some non-limiting examples, a surface coverage may be represented by a (non-zero) percentage coverage by such particle material of such (part of the) discontinuous layer 360. In some non-limiting examples, the percentage coverage may be compared to a maximum threshold percentage coverage.

[0398] In some non-limiting examples, a (part of a) discontinuous layer 360 having a surface coverage that may be substantially no more than the maximum threshold percentage coverage, may result in a manifestation of different optical characteristics that may be imparted by such part of the discontinuous layer 360, to light passing therethrough, whether at least one of: transmitted entirely through the device 100, and emitted thereby, relative to light passing through a part of the discontinuous layer 360 having a surface coverage that may be substantially at keast that of the maximum threshold percentage coverage.

[0399] In some non-limiting examples, one measure of a surface coverage of an amount of an electrically conductive material on a surface may be a (light) transmittance, since in some non-limiting examples, electrically conductive materials, including without limitation, metals, including without limitation: Ag, Mg, and Yb, may at least one of: attenuate, and absorb, light.

[0400] Those having ordinary skill in the relevant art will appreci te that in some non¬ limiting examples, a surface coverage may be understood to encompass at least one of: particle size, and deposited density. In some non-limiting examples, a plurality of these criteria may be positively correlated. Indeed, in some non-limiting examples, a criterion of low surface coverage may comprise some combination of a criterion of low deposited density with a criterion of low particle size.

[0401] In some non-limiting examples, one of the at least one criterion by which such discontinuous layer 360 may be assessed, may be a characteristic size of the constituent particle structures 350.

[0402] In some non-limiting examples, the at least one particle structure 350 of the discontinuous layer 360, may have a ch racteristic size that is no more than a maximum threshold size. In some non-limiting examples, a characteristic size may be at least one of: height, width, length, and diameter.

[0403] In some non-limiting examples, substantially all of the particle structures 350 of the discontinuous layer 360 may have a characteristic size that lies within a specified range.

[0404] In some non-limiting examples, a characteristic size may be characterized by a characteristic length, including without limitation, a maximum value of the characteristic size. In some non-limiting examples, such maximum value may extend along a major axis of the particle structure 350. In some non-limiting examples, the major axis may be understood to be a first dimension extending in a plane defined by a plurality of lateral axes. In some non-limiting examples, a characteristic width may be identified as a value of the characteristic size of the particle structure 350 that may extend along a minor axis of the particle structure 350. In some non-limiting examples, the minor axis may be understood to be a second dimension extending in the same plane but substantially transverse to the major axis.

[0405] In some non-limiting examples, a characteristic length of the at least one particle structure 350, along the first dimension, may be substantially no more than the maximum threshold size.

[0406] In some non-limiting examples, a characteristic width of the at least one particle structure 350, along the second dimension, may be substantially no more than the maximum threshold size.

[0407] In some non-limiting examples, a size of the constituent particle structures 350, in the (part of the) discontinuous layer 360, may be assessed by at least one of: calculating, and measuring, a characteristic si e of such at least one particle structure 350, including without limitation, at least one of a: mass, volume, length of a diameter, perimeter, major, and minor axis, thereof.

[0408] In some non-limiting examples, one of the at least one criterion by which such discontinuous layer 360 may be assessed, may be a deposited density thereof

[0409] In some non-limiting examples, a characteristic size of the particle structure 350 may be compared to a maximum threshold size.

[0410] In some non-limiting examples, a deposited density of the particle structures 350 may be compared to a maximum threshold deposited density.

[0411] In some non-limiting examples, at least one of such criteria may be quantified by a numerical metric, including without limitation, a calculation of a dispersity D that describes a distribution of particle (area) sizes in a deposited layer 330 of particle structures 350, in which, according to Equation (2):n is the number of particle structures 350 in a sample area,is a(n) (area) size of an zthparticle structure 350,is a number average of the particle (area) sizes and& is a(n) (area) size average of the particle (area) sizes.

[0412] Those having ordinary skill in the relevant art will appreciate that the dispersity may be roughly analogous to a polydispersity index (PDI) and that these averages are roughly analogous to the concepts of number average molecular weight and weight average molecular weight familiar in organic chemistry, but applied to a(n area) size, as opposed to a molecular weight of a sample particle structure 350.

[0413] Those having ordinary skill in the relevant will also appreciate that while the concept of dispersity may, in some non-limiting examples, be considered a three-dimensional volumetric concept, in some non-limiting examples, the dispersity may be considered to be a two-dimensional concept. As such, the concept of dispersity may be used in connection with viewing and analyzing two-dimensional images of the deposited layer 330, such as may be obtained by using a variety of imaging techniques, including without limitation, at least one of: TEM, AFM, and SEM. It is in such a two-dimensional context, that the equations set out above are defined.

[0414] In some non-limiting examples, at least one of the: dispersity, and number average, of a particle (area) size and a(n) (area) size average of the particle (area) size, may involve a calculation of at least one of the: number average of the particle diameters, and (area) size average of the particle diameters, according to the Equations in (4):

[0415] In some non-limiting examples, the particle material, including without limitation, as particle structures 350, of the at least one deposited layer 330, may be deposited by one of: an open mask, and a mask-free, deposition process.

[0416] In some non-limiting examples, the particle structures 350 may have a substantially round, including without limitation, spherical, shape.

[0417] For purposes of simplification, in some non-limiting examples, it may be assumed that, a longitudinal extent of each particle structure 350 may be substantially the same (and, in any event, may not be directly measured from a plan view SEM image), so that a(n) (area) size of the particle structure 350 may be represented as a two-dimensional area coverage along a pair of lateral axes. In the present disclosure, a reference to a(n) (area) size may be understood to refer to such two-dimensional concept, and to be differentiated from a si e (without the prefix “area”) that may be understood to refer to a one-dimensional concept, such as a linear dimension.

[0418] Indeed, in some early investigations, it appears that, in some non-limiting examples, a longitudinal extent, along a longitudinal axis, of such particle structures 350, may tend to be substantially small relative to a lateral extent (along at least one of the lateral axes), such that, a volumetric contribution of the longitudinal extent thereof may be no more than that, of such lateral extent. In some non-limiting examples, this may be expressed by an aspect ratio (aratio of a longitudinal extent to a lateral extent) that may be no more than 1. In some non¬ limiting examples, such aspect ratio may be one of about: 1:10, 1:20, 1:50, 1:75, and 1:300.

[0419] In this regard, the assumption (that the longitudinal extent is substantially the same and can be ignored) set out above, to represent the particle structure 350 as a two- dimensional area coverage may be appropriate.

[0420] Those having ordinary skill in the relevant art. will appreciate, having regard to the non-determinative nature of the deposition process, especially in the presence of at least one of: defects, and anomalies, on the exposed layer surface 11 of the underlying layer 410, including without limitation, heterogeneities, including without limitation, at least one of a: step edge, chemical impurity, bonding site, kink, and contaminant, thereon, and consequently the formation of particle structures 350 thereon, the non-uniform nature of coalescence thereof as the deposition process continues, and in view of the uncertainty in the at least one of: size, and position, of observation windows, as well as the intricacies and variability inherent in at least one of the: calculation, and measurement, of their characteristic size, spacing, deposited density, degree of aggregation, and the like, there may be considerable variability in terms of the features (topology) within observation windows.

[0421] In the present disclosure, for purposes of simplicity of illustration, certain details of particle materials, including without limitation, at least one of: thickness, and edge, profiles, of layer(s) have been omitted.

[0422] Those having ordinary skill in the relevant art will appreciate that certain metal NPs, whether as part of a discontinuous layer 360 of particle material, including without limitation, at least one particle structure 350, may exhibit at least one of: surface plasmon (SP) excitations, and coherent oscillations of free electrons, with the result that such NPs may one of: absorb, and scatter, light in a range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum. An optical response, including without limitation, at least one of: a (sub-) range of the EM spectrum over which absorption may be concentrated (absorption spectrum), refractive index, and extinction coefficient, of such one of: LSP excitations, and coherent oscillations, may be tailored by varying properties of such NPs, including without limitation, at least one of a characteristic: size, size distribution, shape, surface coverage, configuration, deposition density, dispersity, and property, including without limitation, at least one of: material, and degree of aggregation, of at least one of: the nanostructures, and a medium proximate thereto.

[0423] Such optical response, in respect of photon-absorbing coatings, may include absorption of photons incident thereon, thereby reducing reflection. In some non-limiting examples, the absorption may be concentrated in a (sub-) range of the EM spectrum, including without limitation, (a (sub-) range of) the visible spectrum. While the at least one particle structure 350 may absorb light incident thereon from beyond the layered semiconductor device 100, thus reducing reflection, those having ordinary’ skill in the relevant art will appreciate that, in some non-limiting examples, the at least one particle structure 350 may absorb light incident thereon that is emitted by the device 100. In some non-limiting examples, employing a photon¬ absorbing layer as part of an opto-electronic device 100 may reduce reliance on a polarizer therein.

[0424] It has been reported in Fusella et al., “Plasmonic enhancement of stability and brightness in organic light-emitting devices”, Nature 2020, 585, at 379-382, that the stability of an OLED device may be enhanced by incorporating an NP -based outcoupling layer above the cathode layer to extract energy from the plasmon modes. The NP -based outcoupling layer was fabricated by spin-casting cubic Ag NPs on top of an organic layer on top of a cathode.However, since most commercial OLED devices are fabricated using vacuum-based processing, spin-casting from solution may not constitute an appropriate mechanism for forming such an NP- based outcoupling layer above the cathode.

[0425] It has been discovered that such an NP-based outcoupling layer above the cathode may be fabricated in vacuum (and thus, may have applicability for use in a commercial OLED fabrication process), by depositing a metal particle material in a discontinuous layer 360 onto a patterning coating 112, that may, in some non-limiting examples, be (deposited on) the cathode. Such process may avoid the use of one of solvents, and other wet chemicals, that may at least one of: cause damage to, and adversely impact device reliability of, the OLED device 100.

[0426] In some non-limiting examples, the presence of such a discontinuous layer 360 of particle material, including without limitation, at least one particle structure 350, may contribute to enhanced extraction of at least one of: light, and at least one of device: performance, stability, reliability, and lifetime.

[0427] In some non-limiting examples, the existence, in a layered device 300, of at least one discontinuous layer 360, proximate to at least one of an: exposed layer surface 11 of a patterning coating 112, and, in some non-limiting examples, interface of such patterning coating112 with at least one overlying layer 370, may impart optical effects to light, including without limitation, photons, that is one of: emitted by the device 300, and transmitted therethrough.

[0428] Those having ordinary skill in the relevant art will appreciate that, while a simplified model of the optical effects is presented herein, at least one of other: models, and explanations, may be applicable.

[0429] In some non-limiting examples, the presence of such a discontinuous layer 360 of the particle material, including without limitation, at least one particle structure 350, may reduce (mitigate) crystallization of thin film coatings disposed adjacent in a longitudinal aspect, including without limitation, at least one of: the patterning coating 112, and at least one overlying layer 370, thereby stabilizing the property of the thin film(s) disposed adjacent thereto, and, in some non-limiting examples, reducing scattering. In some non-limiting examples, such thin film may comprise at least one layer of at least one of an: outcoupling, and encapsulating coating (not shown) of the device 100, including without limitation, a capping layer (CPI.).

[0430] In some non-limiting examples, the presence of such a discontinuous layer 360 of particle material, including without limitation, at least one particle structure 350, may provide an enhanced absorption in (a part of) the UV spectrum. In some non-limiting examples, controlling the characteristics of such particle structures 350, including without limitation, at least one of a characteristic: size, size distribution, shape, surface coverage, configuration, deposited density, dispersity7, particle material, and refractive index, of the particle structures 350, may facilitate controlling at least one of a: degree of absorption, wavelength range, and peak wavelength, of the absorption spectrum, including in the UV spectrum. Enhanced absorption of light in (a part of) the UV spectrum may have applicability in some scenarios, for improving at least one of device: performance, stability, reliability, and lifetime.

[0431] In some non-limiting examples, the optical effects may be described in terms of its impact on at least one of the: transmission, and absorption, wavelength spectrum, including at least one of a: wavelength range, and peak intensity thereof

[0432] Additionally, while the model presented may suggest certain effects imparted on at least one of the: transmission, and absorption, of photons passing through such discontinuous layer 360, in some non-limiting examples, such effects may reflect local effects that may not be reflected on a broad, observable basis.

[0433] FIGs. 8A-8H illustrate non-limiting examples of possible interactions between the particle structure patterning coating 112pand the at least one particle structure 350t in contact therewith.

[0434] Thus, as shown in FIGs. 8A-8H, the particle material may be in physical contact with the patterning material 411, including without limitation, as shown in the various figures, being one of: deposited thereon, and being substantially surrounded thereby.

[0435] In FIG. 8A, the particle material may be in physical contact with the particle structure patterning coating 112pin that it is deposited thereon.

[0436] In FIG. 8B, the particle material may be substantially surrounded by the particle structure patterning coating 112p. In some non-limiting examples, the at least one particle structure 350 may be distributed throughout at least one of a: lateral, and longitudinal, extent of the particle structure patterning coating 112P.

[0437] In some non-limiting examples, a distribution of the at least one particle structure 350 throughout the particle structure patterning coating 112Pmay be achieved by causing the particle structure patterning coating 112pto be at least one of: deposited, and to remain, in a substantially viscous state at the time of deposition of the particle material thereon, such that the at least one particle structure 350t may tend to penetrate (settle) within the particle structure patterning coating 112p.

[0438] In some non-limiting examples, a viscous state of the particle structure patterning coating 112pmay be achieved in various manners, including without limitation, conditions during deposition of the patterning material 411, including without limitation, at least one of: time, temperature, and pressure, of the deposition environment thereof, a composition of the patterning material 411, a characteristic of the particle material 411, including without limitation, at least one of a: melting point, freezing temperature, sublimation temperature, viscosity, and surface energy thereof, conditions during deposition of the particle material, including without limitation, at least one of: time, temperature, and pressure, of the deposition environment thereof, a composition of the particle material, and a characteristic of the patterning material 411, including without limitation, at least one of a: melting point, freezing temperature, sublimation temperature, viscosity, and surface energy, thereof.

[0439] In some non-limiting examples, a distribution of the at least one particle structure 350 throughout the particle structure patterning coating 112pmay be achieved through the / 4presence of small apertures, including without limitation, at least one of: pin-holes, tears, and cracks, therein. Those having ordinary skill in the relevant art will appreciate that such apertures may be formed during the deposition of a thin film of the patterning structure patterning coating 112p, using various techniques and processes, including without limitation, those described herein, due to inherent variability in the deposition process, and in some non-limiting examples, to the existence of impurities in at least one of the: particle material, and exposed layer surface 11 of the patterning material 411.

[0440] In FIG, 8C, a particle material of which the at least one particle structure 350 may be comprised may settle at a bottom of the particle structure patterning coating 112psuch that it may effectively be disposed on an exposed layer surface 11 of the underlying layer 410.

[0441] In some non-limiting examples, a distribution of the at least one particle structure 350 at a bottom of the particle structure patterning coating 112pmay be achieved by causing the particle structure patterning coating 112p to be at least one of: deposited, and to remain, in a substantially viscous state at the time of deposition of the particle material thereon, such that the at least one particle structure 350 may tend to settle to the bottom of the particle structure patterning coating 112p. In some non-limiting examples, a viscosity of the patterning material 411 used in FIG. 8C may be no more than a viscosity of the patterning material 411 used in FIG. 8B, allowing the at least one particle structure 350 to settle further within the particle structure patterning coating 112p, eventually descending to the bottom thereof.

[0442] In FIGs, 8D-8F, a shape of the at least one particle structure 350 is shown as being longitudinally elongated relative to a shape of the at least one particle structure 350 of FIG. SB.

[0443] In some non-limiting examples, a longitudinally elongated shape of the at least one particle structure 350 may be achieved in a number of manners, including without limitation, conditions during deposition of the patterning material 411, including without limitation, at least one of a: time, temperature, and pressure, of the deposition environment thereof, a composition of the patterning material 411, a characteristic of the patterning material 411, including without limitation, at least one of a: melting point, freezing temperature, sublimation temperature, viscosity, and surface energy, thereof, conditions during deposition of the particle material, including without limitation, at least one of a: time, temperature, and pressure, of the deposition environment thereof, a composition of the particle material, and a characteristic of the particle material, including without limitation, at least one of a: melting point, freezing temperature,sublimation temperature, viscosity, and surface energy, thereof, that may tend to facilitate the deposition of such longitudinally elongated particle structures 350.

[0444] In FIG. 8D, the longitudinally elongated particle structures 350 are shown to remain substantially entirely within the particle structure patterning coating 112P. By contrast, in FIG. 8E, at least one of the longitudinally elongated particle structures 350 may be shown to protrude at least partially beyond an exposed layer surface 11 of the particle structure patterning coating 112P. Further, in FIG. 8F, at least one of the longitudinally elongated particle structures 350 may be shown to protrude substantially beyond the exposed layer surface 11 of the particle structure patterning coating 112p, to the extent that such protruding particle structures 350 may begin to be considered to be substantially deposited on an exposed layer surface 11 of the particle structure patterning coating 112p.

[0445] Thus, as shown in FIG. 8G, there may be a scenario in which at least one particle structure 350 may be deposited on an exposed layer surface 11 of the particle structure patterning coating 112p, and at least one particle structure 350 may settle within the particle structure patterning coating 112p. Although the at least one particle structure 350 is shown in FIG. 8B within the particle structure patterning coating 112pas having a substantially spherical shape, those having ordinary skill in the relevant art will appreciate that, although not shown, such particle structures 350 may have a longitudinally elongated shape such as is shown in FIGs. 8D- 8F.

[0446] FIG. 8H shows a scenario in which at least one particle structure 350 may be deposited on an exposed layer surface 11 of the particle structure patterning coating 112p, at least one particle structure 350 may penetrate (settle within) the particle structure patterning coating 112p, and at least one particle structure 350 may settle to the bottom of the particle structure patterning coating 112p.Auxiliary Electrode

[0447] Those having ordinary skill in the relevant art will appreciate that the process of depositing a deposited layer 330 to form the second electrode 140 may, in some non-limiting examples, be used in similar fashion to form an auxiliary electrode 950 for the device 100.

[0448] In some non-limiting examples, particularly in a top-emission device 100, the second electrode 140 may be formed by depositing a substantially thin conductive film layer in order, in some non-limiting examples, to reduce optical interference (including, withoutlimitation, at least one of: attenuation, reflections, and diffusion) related to the presence of the second electrode 140.

[0449] In some non-limiting examples, particularly in at least one of: a bottom-emission, and double-sided emission, device 100, the second electrode 140 may be formed as a substantially thick conductive layer without substantially affecting optical characteristics of such a device 100. Nevertheless, even in such scenarios, the second electrode 140 may nevertheless be formed as a substantially thin conductive film layer, in some non-limiting examples, so that the device 100 may be substantially transmissive relative to light incident on an external surface thereof, such that a substantial part of such extemally-incident light may be transmitted through the device 100, in addition to the emission of light generated internally within the device 100 as disclosed herein.

[0450] Those having ordinary skill in the relevant art will appreciate that the process of depositing a (second electrode) deposited layer 330 to form the second electrode 140 of the device 100, including without limitation, by, in the process shown schematically in FIGs. 4-5:« the deposition, using a (second electrode) shadow mask 415, of a (second electrode) patterning coating 112, followed by:« exposure of a(n) (second electrode) exposed layer surface 11 of the device 100 to a(n) (second electrode) evaporated flux 532 of a (second electrode) deposited material 531 of which the second electrode 140 may be comprised, in one of: an open mask, and mask- free, deposition process,may, in some non-limiting examples, be used in similar fashion to thereafter form an auxiliary electrode 950 of the device 100, including without limitation, by, in the process shown schematically in FIGs, 4~5:* the deposition, using a(n auxiliary electrode) shadow mask 415, of a(n auxiliary electrode) patterning coating 112, followed by:* exposure of a(n auxiliary electrode) exposed layer surface 11 of the device 100 to a(n auxiliary electrode) evaporated flux 532 of a (n auxiliary electrode) deposited material 531 of which the auxiliary' electrode 950 may be comprised, in one of: an open mask, and mask-free, deposition process.

[0451] Those having ordinary skill in the relevant art. will appreciate that, in some non¬ limiting examples, the auxiliary'' electrode 950 of the device 100 may be deposited beforedeposition of the second electrode 140 of the device 100, including without limitation, by, in the process shown schematically in FIGs. 4-5:® the deposition, using a(n auxiliary electrode) shadow mask 415, of a(n auxiliary electrode) patterning coating 112, followed by:® exposure of a(n auxiliary' electrode) exposed layer surface 11 of the device 100 to a(n auxiliary electrode) evaporated flux 532 of a(n auxiliary electrode) deposited material 531 of which the auxiliary / electrode 950 may be comprised, in one of: an open mask, and mask-free, deposition process, followed by,in the process shown schematically in FIGs. 4-5:• the deposition, using a(n) (second electrode) shadow mask 415, of a(n) (second electrode) patterning coating 112, followed by:« exposure of a(n) (second electrode) exposed layer surface 11 of the device 100 to a(n) (second electrode) evaporated flux 532 of a(n) (second electrode) deposited material 531 of the auxiliary electrode 950 may be comprised.

[0452] In some non-limiting examples, the auxiliary electrode 950 may be electrically coupled with the second electrode 140 to reduce a sheet resistance thereof.

[0453] In some non-limiting examples, the auxiliary electrode 950 may be in physical contact, including without limitation, being deposited over at least a part thereof, with the second electrode 140 to reduce a sheet resistance thereof.

[0454] In some non-limiting examples, the auxiliary electrode 950 may not be in physical contact with the second electrode 140 but may be electrically coupled with the second electrode 140 by several well -understood mechanisms. In some non-limiting examples, the presence of a substantially thin film (in some non-limiting examples, of up to about 50 nm) of a patterning coating 112 extending between and separating the auxiliary' electrode 950 and the second electrode 140, may still allow a current to pass therethrough, thus allowing a sheet resistance of the second electrode 140 to be reduced.

[0455] In some non-limiting examples, the auxiliary electrode 950 may' be electrically' conductive. In some non-limiting examples, the auxiliary electrode 950 may be formed by a metal (oxide). In some non-limiting examples, such metals may be at least one of: Cu, Al, molybdenum (Mo), and Ag. In some non-limiting examples, the auxiliary' electrode 950 may comprise a multi-layer metallic structure, including without limitation, one formed byMo / Al / Mo. In some non-limiting examples, such metal oxides may be at least one of: ITO, ZnO, IZO, and other oxides comprising In, and Zn. In some non-limiting examples, the auxiliary electrode 950 may comprise a multi-layer structure formed by a combination of at least one metal and at least one metal oxide, including without limitation, Ag / ITO, Mo / ITO, ITO / Ag / ITO, and ITO / Mo / ITO. In some non-limiting examples, the auxiliary electrode 950 may comprise a plurality' of such electrically conductive materials.

[0456] Because of the nucleation-inhibiting properties of those (auxiliary electrode) first portions 101 where the (auxiliary electrode) patterning coating 112 was disposed, the deposited material 531 disposed in the (auxiliary electrode) first portion 101 may tend to not remain, resulting in a pattern of selective deposition of the (auxiliary electrode) deposited layer 330, that may correspond substantially to at least one (auxiliary' electrode) second portion 102, leaving the (auxiliary' electrode) first portion 101 substantially devoid of a closed coating 340 of the (auxiliary electrode) deposited layer 330 that may form (part of) (a layer of) the auxiliary¬ electrode 950.

[0457] In other words, the (auxiliary electrode) deposited layer 330 that may form the auxiliary' electrode 950 may be selectively deposited substantially only on a (auxiliary electrode) second portion 102 comprising those regions of the at least one semiconducting layer 130, that surround but do not occupy the (auxiliary electrode) first portion 101.

[0458] In some non-limiting examples, selectively depositing the auxiliary' electrode 950 to cover only certain (auxiliary electrode) second portions 102 of the lateral aspect of the device 100, while other (auxiliary electrode) first portions 101 thereof remain uncovered, may one of: control, and reduce, optical interference related to the presence of the auxiliary electrode 950.

[0459] In some non-limiting examples, an auxiliary electrode 950 may be selectively deposited in a pattern that may not be readily detected by the naked eye from a typical viewing distance.

[0460] In some non-limiting examples, the auxiliary electrode 950 may be formed in devices 100 other than OLED devices 200, including for decreasing an effective resistance of the electrodes of such devices 100.

[0461] Turning now to FIG. 9, there may be shown an example version 900 of the device 100, which may encompass the device 100 shown in cross-sectional view in FIG. 1, but with additional deposition steps that are described herein.

[0462] The device 900 may show a(n auxiliary' electrode) patterning coating 112adeposited over the exposed layer surface 11 of an underlying layer 410, in the figure, the second electrode 140.

[0463] The (auxiliary electrode) patterning coating 112amay provide an exposed layer surface 11 with a substantially low initial sticking probability against deposition of a(n auxiliary' electrode) deposited material 53 lato be thereafter deposited as a(n auxiliary / electrode) deposited layer 330ato form an auxiliary / electrode 950.

[0464] In some non-limiting examples, after deposition of the (auxiliary electrode) patterning coating 112a, an NPC 720 may be selectively deposited over the exposed layer surface 11 of the underlying layer 410, in the figure, the (auxiliary / electrode) patterning coating 112a.

[0465] In some non-limiting examples, the NPC 720 may be disposed between the auxiliary / electrode 950 and the second electrode 140.

[0466] In some non-limiting examples, the NPC 720 may be selectively deposited using a shadow mask 415, in a(n auxiliary electrode) second portion 102aof the lateral aspect of the device 500.

[0467] In some non-limiting examples, the NPC 720 may provide an exposed layer surface 11 with a substantially high initial sticking probability against deposition of a(n auxiliary electrode) deposited material 53 lato be thereafter deposited as a(n auxiliary' electrode) deposited layer 330ato form an auxiliary electrode 950.

[0468] After selective deposition of the NPC 720, the (auxiliary / electrode) deposited material 53 lamay be deposited over the device 900 but may remain substantially where the (auxiliary / electrode) patterning coating 112ahas been overlaid with the NPC 720, to form the auxiliary' electrode 950, that is, substantially only the (auxiliary' electrode) second portion 102a.

[0469] In some non-limiting examples, the (auxiliary' electrode) deposited layer 330amay be deposited using at least one of: an open mask, and a mask-free, deposition process.Attributes of Patterning Coating / ' MaterialComposition

[0470] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, may comprise at least one of: a fluorine (F) atom, and a Si atom. Insome non-limiting examples, the patterning material 411 for forming the patterning coating 112 may be a compound that comprises at least one of: F and Si.

[0471] In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F and a carbon (C) atom. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 0.5, 0.7, 1, 1.5, 2, and 2.5.

[0472] In some non-limiting examples, an atomic ratio of F to C may be determined by counting the F atoms present in the compound structure, and for C atoms, only counting the sp3hybridized C atoms present in the compound structure. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises, as part of its molecular sub¬ structure, a moiety comprising F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 1, 1.5, and 2.

[0473] In some non-limiting examples, the patterning material 411 may comprise an organic-inorganic hybrid material.

[0474] In some non-limiting examples, the patterning material 411 may comprise an oligomer.

[0475] In some non-limiting examples, the patterning material 411 may comprise a compound having a molecular structure comprising a backbone and at least one functional group bonded to the backbone. In some non-limiting examples, the backbone may be an inorganic moiety, and the at least one functional group may be an organic moiety.

[0476] In some non-limiting examples, such compound may have a molecular structure comprising a siloxane group. In some non-limiting examples, the siloxane group may be one of a: linear, branched, and cyclic, siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group, and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group. In some non-limiting examples, such compound may comprise a fluoro- siloxane, including without limitation, Example Material 6 and Example Material 9 (discussed herein).

[0477] In some non-limiting examples, the compound may have a molecular structure comprising a silsesquioxane group. In some non-limiting examples, the silsesquioxane group may be a polyhedral oligomeric silsesquioxane (POSS). In some non-limiting examples, thebackbone may comprise a silsesquioxane group. In some non-limiting examples, the backbone may comprise a silsesquioxane group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group. In some non-limiting examples, such compound may comprise a fluoro-silsesquioxane and a fluoro-POSS, including without limitation, Example Material 8 (discussed herein).

[0478] In some non-limiting examples, the compound may have a molecular structure comprising at least one of: a substituted and, an unsubstituted aryl, a substituted heteroaryl, and an unsubstituted heteroaryl, group. In some non-limiting examples, the aryl group may be at least one of: phenyl, and naphthyl. In some non-limiting examples, at least one C atom of an aryl group may be substituted by a heteroatom, including without limitation, at least one of: oxygen (O), nitrogen (N), and sulfur (S), to derive a heteroaryl group. In some non-limiting examples, the backbone may comprise at least one of: a substituted aryl, an unsubstituted aryl, a substituted heteroaryl, and an unsubstituted heteroaryl, group. In some non-limiting examples, the backbone may comprise at least one of: a substituted aryl, an unsubstituted aryl, a substituted heteroaryl, and an unsubstituted heteroaryl, group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group.

[0479] In some non-limiting examples, the compound may have a molecular structure comprising at least one of: a substituted, an unsubstituted, a linear, a branched, and a cyclic, hydrocarbon group. In some non-limiting examples, at least one C atom of the hydrocarbon group may be substituted by a heteroatom, including without limitation, at least one of: O, N, and S.

[0480] In some non-limiting examples, the compound may have a molecular structure comprising a phosphazene group. In some non-limiting examples, the phosphazene group may be at least one of a: linear, branched, and cyclic, phosphazene group. In some non-limiting examples, the backbone may comprise a phosphazene group. In some non-limiting examples, the backbone may comprise a phosphazene group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group may comprise at least one of: F, chlorine (Cl), a hydroxy group, a substituted alkyl group, an unsubstituted alkyl group, a substituted fluoroalkyl group, an unsubstituted fluoroalkyl group, a substituted cycloalkyl group, an unsubstituted cycloalkyl group, a substituted fluorocycloalkyl group, an unsubstituted fluorocycloalkyl group, a substituted heterocycloalkyl group, an unsubstituted heterocycloalkyl group, a substituted fluoroheterocycloalkyl group, an unsubstituted fluoroheterocycloalkyl group,a substituted alkoxy group, an unsubstituted alkoxy group, a substituted fluoroalkoxy group, an unsubstituted fluoroalkoxy group, a substituted aryloxy group, an unsubstituted aryloxy group, a substituted fluoroaryloxy group, an unsubstituted fluoroaryloxy group, a substituted heteroaryloxy group, a unsubstituted heteroaryloxy group, a substituted fluoroheteroaryloxy group, a unsubstituted fluoroheteroaryloxy group, a substituted aryl group, an unsubstituted aryl group, a substituted fluoroaryl group, an unsubstituted fluoroaryl group, a substituted alkylsilyl group, an unsubstituted alkylsilyl group, a substituted alkylsiloxy group, an unsubstituted alkylsiloxy group, an amino group, an amine group, an alkylamine group, an arylamine group, a cyano group, a phosphazo group, a sulfanyl group, a pentafluorosulfanyl group, a sulfide group, a sulfonyl group, a thiol group, an alkylthio group, a trifluoromethylthio group, a carbonyl group, a siloxane group, a silane group, and an organosilicon group. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group, including without limitation, fluoro-phosphazenes, including without limitation, Example Material 4 (discussed herein),

[0481] In some non-limiting examples, the compound may be a fluoropolymer. In some non-limiting examples, the compound may be a block copolymer comprising F. In some non¬ limiting examples, the compound may be an oligomer. In some non-limiting examples, the oligomer may be a fluorooligomer. In some non-limiting examples, the compound may be a block oligomer comprising F. In some non-limiting examples, at least one of: fluoropolymers, and fluorooligomers, may have a molecular structure of at least one of: Example Material 3, Example Material 5, and Example Material 7 (discussed herein).

[0482] In some non-limiting examples, the compound may be a metal complex. In some non-limiting examples, the metal complex may be an organo-metal complex. In some nonlimiting examples, the organo-metal complex may comprise F. In some non-limiting examples, the organo-metal complex may comprise at least one ligand comprising F. In some non-limiting examples, the at least one ligand comprising F may comprise a fluoroalkyl group.

[0483] In some non-limiting examples, the patterning material 411 may comprise a plurality of different materials.Initial Sticking Probability

[0484] In some non-limiting examples, the initial sticking probability of the patterning material 411 may be determined by depositing such material as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating112 within the device 300, having sufficient thickness so as to mitigate I reduce any effects on the degree of inter-molecular interaction with the underlying layer 410 upon deposition on a surface thereof. In some non-limiting examples, the initial sticking probability may be measured on a film / coating having a thickness of one of at least about: 20, 25, 30, 50, 60, and 100, nm.

[0485] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an initial sticking probability against the deposition of the deposited material 531, that is one of no more than about: 0.3, 0.2, 0.15, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, 0.001, 0.0008, 0.0005, 0.0003, and 0.0001.

[0486] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an initial sticking probability against the deposition of at least one of: Ag, and Mg that is one of no more than about: 0.3, 0.2, 0.15, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, 0.001, 0.0008, 0.0005, 0.0003, and 0.0001.

[0487] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an initial sticking probability against the deposition of a deposited material 531 of one of between about: 0.15-0.0001, 0.1-0.0003, 0.08-0.0005, 0.08- 0.0008, 0.05-0.001, 0.03-0.0001, 0.03-0.0003, 0.03-0.0005, 0.03-0.0008, 0.03-0.001, 0.03-0.005, 0.03-0.008, 0.03-0.01, 0.02-0.0001, 0.02-0.0003, 0.02-0.0005, 0.02-0.0008, 0.02-0.001, 0.02-0.005, 0.02-0.008, 0.02-0.01, 0.01-0.0001, 0.01-0.0003, 0.01-0.0005, 0.01-0.0008, 0.01-0.001, 0.01-0.005, 0.01-0.008, 0.008-0.0001, 0.008-0.0003, 0.008-0.0005, 0.008-0.0008, 0.008-0.001, 0.008-0.005, 0.005-0.0001, 0.005-0.0003, 0.005-0.0005, 0.005-0.0008, and 0.005-0.001.

[0488] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an initial sticking probability against the deposition of a plurality of deposited materials 531 that is no more than a threshold value. In some non-limiting examples, such threshold value may be one of about: 0.3, 0.2, 0.18, 0.15, 0.13, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, and 0.001.

[0489] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an initial sticking probability that is no more than such threshold value against the deposition of a plurality of deposited materials 531 selected from at least one of: Li, Ag, Mg, Yb, Cd, and Zn. In some non-limiting examples, the patterning coating 112 may exhibit an initial sticking probability of no more than such threshold value against the deposition of a plurality of deposited materials 531 selected from at least one of: Li, Ag, Mg, and Yb.

[0490] In some non-limiting examples, at least one of the: patterning coating 300, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may exhibit an initial sticking probability against the deposition of a first deposited material 531 of, including without limitation, below, a first threshold value, and an initial sticking probability against the deposition of a second deposited material 531 of, including without limitation, below, a second threshold value. In some non¬ limiting examples, the first deposited material 531 may be Ag, and the second deposited material 531 may be Mg. In some non-limiting examples, the first deposited material 531 may be Ag, and the second deposited material may be Yb. In some non-limiting examples, the first deposited material 531 may be Yb, and the second deposited material 531 may be Mg. In some non¬ limiting examples, the first threshold value may be at least that of the second threshold value.

[0491] In some non-limiting examples, there may be scenarios calling for providing a patterning coating 112 for causing formation of a discontinuous layer 360 of at least one particle structure 350, upon the patterning coating 112 being subjected to an evaporated flux 532 of a deposited material 531. In some non-limiting examples, the patterning coating 112 may exhibit a substantially low initial sticking probability such that a closed coating 340 of the deposited material 531 may be formed in the second portion 102, which may be substantially devoid of the patterning coating 112, while the discontinuous layer 360 of at least one particle structure 350 having at least one characteristic may be formed in the first portion 101 on the patterning coating 112. In some non-limiting examples, there may be scenarios calling for formation of adiscontinuous layer 360 of at least one particle structure 350 of a deposited material 531, which may be, in some non-limiting examples, of a metal (alloy), in the second portion 102, while depositing a closed coating 340 of the deposited material 531 having a thickness of, including without limitation, one of no more than about: 100, 50, 25, and 15, nm. In some non-limiting examples, an amount of the deposited material 531 deposited as a discontinuous layer 360 of at least one particle structure 350 in the first portion 101 may correspond to one of between about: 1-50%, 2-25%, 5-20%, and 7-10% of the amount of the deposited material 531 deposited as a closed coating 340 in the second portion 102, which in some non-limiting examples may correspond to a thickness of one of no more than about: 100, 75, 50, 25, and 15, nm.

[0492] In some non-limiting examples, there may be a positive correlation between the initial sticking probability of at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 100, against the deposition of the deposited material 531, and an average layer thickness of the deposited material 531 thereon.Transmittance

[0493] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have a transmittance for light of at least a threshold transmittance value, after being subjected to an evaporated flux 532 of the deposited material 531, including without limitation, Ag.

[0494] In some non-limiting examples, such transmittance may be measured after exposing the exposed layer surface 11 of at least one of: the patterning coating 112 and the patterning material 411, formed as a thin film, to an evaporated flux 532 of the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, under typical conditions that may be used for depositing an electrode of an opto-electronic device 100, which in some non-limiting examples, may be a cathode of an organic light-emitting diode (OLED) device 100.

[0495] In some non-limiting examples, the conditions for subjecting the exposed layer surface 11 to the evaporated flux 532 of the deposited material 531, including without limitation,a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may comprise: maintaining a vacuum pressure at a reference pressure, including without limitation, of one of about: I0‘4, and IO’5, Ton; the evaporated flux 532 of the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, being substantially consistent with a reference deposition rate, including without limitation, of about 1 angstrom (A) / sec, which in some non-limiting examples, may be monitored using a QCM; the evaporated flux 532 of the deposited material 531 being directed toward the exposed layer surface 11 at an angle that is substantially close to normal to a plane of the exposed layer surface 11; the exposed layer surface 11 being subjected to the evaporated flux 532 of the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, until a reference average layer thickness, including without limitation, of about 15 nm, is reached, and upon such reference average layer thickness being attained, the exposed layer surface 11 not being further subjected to the evaporated flux of the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg.

[0496] In some non-limiting examples, the exposed layer surface 11 being subjected to the evaporated flux 532 of the deposited material 531, including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may be substantially at room temperature (e.g. about 25°C). In some non-limiting examples, the exposed layer surface 11 being subjected to the evaporated flux 532 of the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may be positioned about 65 cm away from an evaporation source by which the deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, is evaporated.

[0497] In some non-limiting examples, a threshold transmittance value may be measured at a wavelength in the visible spectrum, which may be one of at least about: 460, 500, 550, and 600, nm. In some non-limiting examples, the threshold transmittance value may be measured at a wavelength in the (N)IR spectrum. In some non-limiting examples, the threshold transmittance value may be measured at a wavelength of one of about: 700, 900, and 1,000, nm. In some non-limiting examples, the threshold transmittance value may be expressed as a percentage of incident EM power that may be transmitted through a sample. In some non-limiting examples, the threshold transmittance value may be one of at least about: 60%, 65%, 70%, 75%, 80%, 85%, and 90%.

[0498] It would be appreciated by a person having ordinary skill in the relevant art that high transmittance may generally indicate an absence of a closed coating 340 of the deposited material 531, including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg. On the other hand, low transmittance may generally indicate presence of a closed coating 340 of the deposited material 531, including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, since metallic thin films, particularly when formed as a closed coating 340, may exhibit a high degree of absorption of light.

[0499] A series of samples was fabricated to measure the transmittance of an example material, as well as to visually observe whether a closed coating 340 of Ag was formed on the exposed layer surface 11 of such example material. Each sample was prepared by depositing, on a glass substrate 10, an approximately 50 nm thick coating of an example material, then subjecting the exposed layer surface 11 of the coating to an evaporated flux 532 of Ag at a rate of about 1 A / sec until a reference layer thickness of about 15 nm was reached. Each sample was then visually analyzed and the transmittance through each sample was measured.

[0500] The molecular structures of the example materials used in the samples herein are set out in Table 4 below:Table 4

[0501] Those having ordinary skill in the relevant art will appreciate that samples having little to no deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, present thereon may be substantially transparent, while samples with substantial amounts of a metal (alloy) deposited thereon, including without limitation, as a closed coating 340, may in some non-limiting examples, exhibit a substantially reduced transmittance. Accordingly, the performance of various example coatings as a patterning coating 112 may be assessed by measuring transmission through the samples, which may be inversely correlated to at least one of an: amount and average layer thickness, of the deposited material 531, including without limitation, a metal (alloy) including without limitation, in the form of at least one of Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, being depositedthereon, since metallic thin films, including without limitation, when formed as a closed coating340, may exhibit a high degree of absorption of light.

[0502] The samples in which a substantially closed coating 340 of a deposited material 531, in the form of Ag, had formed were visually identified, and the presence of such closed coating 340 in these samples was further confirmed by measurement of transmittance therethrough, which showed transmittance of no more than about 50% at a wavelength of about 460 nm.

[0503] In addition, for samples in which the absence of formation of a closed coating 340 of a deposited material 531, in the form of Ag, was identified, the absence of such closed coating 340 in these samples was further confirmed by measurement of EM transmittance therethrough, which showed transmittance (of light at a wavelength of about 460 nm) of at least about 70%.

[0504] The results are summarized in Table 5 below:Table 5

[0505] Based on the foregoing, it was found that the materials used in the first 7 samples (HT211 to Example Material 2) and Example Material 9 in Tables 1 and 2 may have reduced applicability in some scenarios for inhibiting the deposition of the deposited material 531 thereon, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg.

[0506] On the other hand, it was found that Example Material 3 to Example Material 8 may have applicability in some scenarios, to act as a patterning coating 112 for inhibiting the deposition of the deposited material 531 including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, thereon.

[0507] In some non-limiting examples, the second electrode 140 may have a transmittance at a wavelength of 460 nm that is one of at least about: 60%, 65%, and 70%.

[0508] In some non-limiting examples, the second electrode 140 may have a transmittance at a wavelength of 940 nm that is one of at least about: 40%, 50%, and 60%.Deposition Contrast

[0509] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a given a metal (alloy) including without limitation, at least one of: Mg, Ag, and MgAg, may have a substantially high deposition contrast when deposited on a substrate 10.

[0510] In some non-limiting examples, if a substrate 10 tends to act as an NPC 720 and a portion thereof is coated with a material, including without limitation, a patterning material 411, that, may tend to function as an NIC against deposition of a deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, a coated portion (first portion 101) and an uncoated portion (second portion 102) may tend to have different at least one of: initial sticking probabilities, and nucleation rates, such that the deposited material 531 deposited thereon may tend to have different average film thicknesses.

[0511] As used herein, a quotient of an average film thickness of the deposited material 531 deposited in the second portion 102 divided by the average film thickness of the deposited material in the first portion 101 in such scenario may be generally referred to as a depositioncontrast. Thus, if the deposition contrast is substantially high, the average film thickness of the deposited material 531 in the second portion 102 may be substantially greater than the average film thickness of the deposited material 531 in the first portion 101.

[0512] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a given deposited material 531, may have a substantially high deposition contrast when deposited on a substrate 10.

[0513] In some non-limiting examples, there may be a negative correlation between the initial sticking probability of at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 100, against the deposition of the deposited material 531 and a deposition contrast thereof, that, is, a low initial sticking probability may be highly correlated with a high deposition contrast.

[0514] In some non-limiting examples, if the deposition contrast is substantially high, there may be little to no deposited material 531 deposited in the first portion 101, when there is sufficient deposition of the deposited material 531 to form a closed coating 340 thereof in the second portion 102.

[0515] In some non-limiting examples, if the deposition contrast is substantially low, there may be a discontinuous layer 360 of at least one particle structure 350 of the deposited material 531 deposited in the first portion 101, when there is sufficient deposition of the deposited material 531 to form a closed coating 340 in the second portion 102.

[0516] In some non-limiting examples, there may be scenarios calling for the formation of a discontinuous layer 360 of at least one particle structure 350 of the deposited material 531, in the first portion 101, when an average layer thickness of a closed coating 340 of the deposited material 531 in the second portion 102 is substantially small, including without limitation, one of no more than about: 100, 50, 25, and 15, nm, including without limitation, the formation of nanoparticles (NPs) in the first portion 101, where absorption of light by such NPs is called for, including without limitation, to protect an underlying layer 410 from light having a wavelength of no more than substantially about 460 nm,

[0517] In some non-limiting examples, in such scenarios, there may be applicability for a deposition contrast of one of between about: 2-100, 4-50, 5-20, and 10-15.

[0518] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against deposition of adeposited material 531, may have reduced applicability in some scenarios calling for substantially high deposition contrast, including without limitation, where the average layer thickness of the deposited material 531 in the first portion 101 is substantially large, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0519] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against deposition of a deposited material 531, may have reduced applicability in some scenarios calling for substantially high deposition contrast, including without limitation, scenarios calling for at least one of: the substantial absence of a closed coating 340, and a substantially high density of, particle structures 350 in the first portion 101, including without limitation, when an average layer thickness of the deposited material 531 in the second portion 102 is substantially large, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm, including without limitation, in some scenarios calling for the substantial absence of absorption of light in at least one of the: visible, and NIR, spectrum, including without limitation, scenarios calling for an increased transparency to light having a wavelength that is at least about 460 nm,

[0520] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against the deposition of a deposited material 531, may have applicability in some scenarios calling for at least one of a: discontinuous layer 360, and low density, of particle structures 350 of the deposited material 531 in the first portion 101, when an average layer thickness of a closed coating 340 of the deposited material 531 in the second portion 102 is substantially large, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm. In some non-limiting examples, a deposition contrast of one of between about: 2-100, 4-50, 5-20, and 10-15, may have applicability in some scenarios when an average layer thickness of the deposited material 531 in the second portion 102 is substantially large, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0521] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to have a substantially low deposition contrast if the initial sticking probability of such material against deposition of a metal (alloy) including without limitation, at least one of: Mg, Ag, and MgAg, is substantially high.Surface Energy

[0522] A characteristic surface energy, as used herein, in some non-limiting examples, with respect to a material, may generally refer to a surface energy determined from such material.

[0523] In some non-limiting examples, a characteristic surface energy may be measured from a surface formed by the material deposited (coated) in a thin film form.

[0524] Various methods and theories for determining the surface energy of a solid are known.

[0525] In some non-limiting examples, a surface energy may be calculated (derived) based on a series of contact angle measurements, in which various liquids may be brought into contact with a surface of a solid to measure the contact angle between the liquid-vapor interface and the surface. In some non-limiting examples, a surface energy of a solid surface may be equal to the surface tension of a liquid with the highest surface tension that completely wets the surface.

[0526] In some non-limiting examples, a critical surface tension of a surface may be determined according to the Zisman method, as further detailed in W. A. Zisman, Advances in Chemistry 43 (1964), pp. 1-51.

[0527] In some non-limiting examples, a characteristic surface energy of a material, including without limitation, a patterning material 411, in a coating, including without limitation, a patterning coating 112, may be determined by depositing the material as a substantially pure coating (e.g. a coating formed by a substantially pure material) on a substrate 10 and measuring a contact angle thereof with an applicable series of probe liquids.

[0528] In some non-limiting examples, a Zisman plot may be used to determine a maximum value of surface tension that would result in complete wetting (i.e. a contact angle (k of 0°) of the surface.

[0529] A material that has applicability for use in providing the patterning coating 112 may generally have a low surface energy when deposited as a thin film (coating) on a surface. In some non-limiting examples, a material with a low surface energy may exhibit low intermolecular forces.

[0530] Without wishing to be bound by any particular theory, it may be postulated that a material with a substantially high surface energy may have applicability at least in some applications that call for a high temperature reliability.

[0531] Without wishing to be bound by any particular theory', it has now been found that a patterning coating 112 comprising a material which, when deposited as a thin film, exhibits a substantially high surface energy, may, in some non-limiting examples, form a discontinuouslayer 360 of at least one particle structure 350 of a deposited material 531 in the first portion 101, and a closed coating 340 of the deposited material 531 in the second portion 102, including without limitation, in cases where the thickness of the closed coating is, in some non-limiting examples, one of no more than about: 100, 75, 50, 25, and 15, nm.

[0532] In some non-limiting examples, a series of samples was fabricated to measure the critical surface tension of the surfaces formed by the various materials. The results of the measurement are summarized in Table 6:Table 6

[0533] Based on the foregoing measurement of the critical surface tension in Table 6, and the previous observation regarding one of the: presence, and absence, of a substantially closed coating 340 of a deposited material 531, including without limitation, in the form of Ag, it wasfound that materials that form substantially low surface energy surfaces when deposited as a coating, including without limitation, a patterning coating 112, which in some non-limiting examples, may be those having a critical surface tension of one of substantially between about: 13-20, and 13-19, dynes / cm, may have applicability for forming the patterning coating 112 to inhibit deposition of a deposited material 531 thereon, including without limitation, at least one of Li, Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg.

[0534] Without wishing to be bound by any particular theory, it may be postulated that materials that form a surface having a surface energy lower than, in some non-limiting examples, substantially about 13 dynes / cm, may have reduced applicability as a patterning material 411 in some scenarios, as such materials may exhibit at least one of substantially: poor adhesion to layer / s) surrounding such materials, low melting point, and low sublimation temperature.

[0535] In some non-limiting examples, a material, including without limitation, a patterning material 411 that may tend to function as an NIC for a deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Mg, Ag, and Ag-containing materials, including without limitation, MgAg, may tend to exhibit a substantially low surface energy when deposited as a thin film (coating) on an exposed layer surface 11.

[0536] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to exhibit a substantially low surface energy when deposited as a thin film (coating) on an exposed layer surface 11.

[0537] In some non-limiting examples, a material, including without limitation, a patterning material 411, with a substantially low surface energy may tend to exhibit substantially low inter-molecular forces.

[0538] In some non-limiting examples, there may be scenarios calling for a patterning material 411 that has a substantially low surface energy that is not unduly low.

[0539] In some non-limiting examples, a material, including without limitation, a patterning material 411, with a substantially high surface energy may have applicability for some scenarios to detect a film of such material using optical techniques.

[0540] Without wishing to be bound by any particular theory, it may be postulated that, in some non-limiting examples, a material, including without limitation, a patterning material 411,having a substantially high surface energy may have applicability for some scenarios that call for substantially high temperature reliability'.

[0541] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a metal (alloy) including without limitation, at least one of Mg, Ag, and Ag-containing materials, including without limitation, MgAg, having a substantially high surface energy may have applicability in some scenarios calling for a discontinuous layer 360 of particle structures 350 of the metal (alloy) in the first portion 101, when an average layer thickness of a continuous coating 340 of the metal (alloy) in the second portion 102 is substantially low, including without limitation, one of no more than substantially about: 100, 50, 25, and 15, nm.

[0542] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a deposited material 531, including without limitation, a metal (alloy) including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, having a substantially low surface energy may have applicability in some scenarios calling for one of: a discontinuous layer 360 of, and a substantially low density of, particle structures 350 of the deposited material 531 in the first portion 101, when an average layer thickness of a closed coating 340 of the deposited material 531 in the second portion 102 is substantially high, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0543] In some non-limiting examples, the surface of at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, comprising the compounds described herein, may exhibit a surface energy of one of substantially no more than about: 24, 22, 20, 18, 16, 15, 13, 12, and 11, dynes / cm.

[0544] In some non-limiting examples, the surface values in various non-limiting examples herein may correspond to such values measured at around normal temperature and pressure (NTP), which may correspond to a temperature of 20°C, and an absolute pressure of 1 atm.

[0545] In some non-limiting examples, the surface energy may be one of at least about: 6, 7, and 8, dynes / cm.

[0546] In some non-limiting examples, the surface energy may be one of between about: 10-20, and 13-19, dynes / cm.TemperatureGlass Transition Temperature

[0547] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have a glass transition temperature that is one of: one of at least about: 300°C, 150°C, and 130°C, and one of no more than about: 30°C, 0°C, -30°C, and -50°C.Sublimation Temperature

[0548] In some non-limiting examples, a material, including without limitation, a patterning material 411, having substantially low inter-molecular forces may tend to exhibit a substantially low sublimation temperature.

[0549] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness in a deposited film of the material.

[0550] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a sublimation temperature that is one of no more than about: 140°C, 120°C, 110°C, 100°C and 90°C, may tend to encounter constraints on at least one of the: deposition rate and average layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0551] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0552] In some non-limiting examples, the patterning material may have a sublimation temperature of one of between about: 100-320°C, 120-300°C, 140-280°C, and 150-250°C. In some non-limiting examples, such sublimation temperature may allow the patterning material 411 to be substantially readily deposited as a coating using PVD.

[0553] In some non-limiting examples, a material with substantially low intermolecular forces may exhibit a substantially low sublimation temperature.

[0554] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness of a closed coating 340 of the deposited material 531.

[0555] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a sublimation temperature that is one of no more than about: 140°C, 120°C, 110°C, 100°C, and 90°C, may tend to encounter constraints on at least one of the: deposition rate and average layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0556] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0557] The sublimation temperature of a material, including without limitation, a patterning material 411, may be determined using various methods apparent to those having ordinary skill in the relevant art, including without limitation, by heating the material in an evaporation source under a substantially high vacuum environment, in some non-limiting examples, about 10-4Torr, and including without limitation, in a crucible and by determining a temperature that may be attained, to at least one of:« observe commencement of the deposition of the material onto an exposed layer surface11 on a QCM mounted a fixed distance from the crucible;• observe a specific deposition rate, in some non-limiting examples, 0.1 A / sec, onto an exposed layer surface 11 on a QCM mounted a fixed distance from the crucible; and« reach a threshold vapor pressure of the material, in some non-limiting examples, one of about: 10-4, and 10-5, Torr.

[0558] In some non-limiting examples, the QCM may be mounted about 65 cm away from the crucible for the purpose of determining the sublimation temperature.

[0559] In some non-limiting examples, the patterning material 411 may have a sublimation temperature of one of between about: 100-320°C, 100-300°C, 120-300°C, 100-250°C, 140-280°C, 120-230°C, 130-220°C, 140-210°C, 140- 200°C, 150-250°C, and 140-190°C.Melting Point

[0560] In some non-limiting examples, a material, including without limitation, a patterning material 411, with substantially low inter-molecular forces may tend to exhibit a substantially low melting point.

[0561] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low melting point may have reduced applicability in some scenarios calling for substantial temperature reliability for temperatures of one of no more than about: 60°C, 80°C, and 100°C, in some non-limiting examples, because of changes in physical properties of such material at operating temperatures that approach the melting point.

[0562] In some non-limiting examples, a material with a melting point of about 120°C may have reduced applicability in some scenarios calling for substantially high temperature reliability, including without limitation, of at least about: 100 °C.

[0563] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high melting point may have applicability in some scenarios calling for substantially high temperature reliability.

[0564] In some non-limiting examples, a (compound of a) patterning coating 112 may have a melting temperature that is one of at least about: 90°C, 100°C, 110°C, 120°C, 140°C, 150°C, and 180°C.Cohesion Energy

[0565] According to Young’s equation (Equation 14), a cohesion energy (fracture toughness / cohesion strength) of a material may tend to be proportional to its surface energy (cf Young, Thomas (1805) “An essay on the cohesion of fluids”, Philosophical Transactions of the Royal Society of London, 95: 65-87).

[0566] According to Lindemann’s criterion, a cohesion energy of a material may tend to be proportional to its melting temperature (cf Nanda, K. K., Sahu, S. N, and Behera, S. N (2002), “Liquid-drop model for the size-dependent melting of low-dimensional systems” Phys. Rev. A.66 (1): 013208).

[0567] In some non-limiting examples, a material, including without limitation, a patterning material 411, having substantially low inter-molecular forces may tend to exhibit a substantially low cohesion energy.

[0568] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low cohesion energy may have reduced applicability in some scenarios that call for substantial fracture toughness, including without limitation, in a device 100 that may tend to undergo at least one of: sheer, and bending, stress during at least one of: manufacture, and use, as such material may tend to crack (fracture) in such scenarios. In some non-limiting examples, a material, including without limitation, a patterning material 411, having a cohesion energy of no more than about 30 dynes / cm may have reduced applicability in some scenarios in a device 300 manufactured on a flexible substrate 10.

[0569] In some non-limiting examples, a material, including without limitation, a patterning material 411, that has a substantially high cohesion energy, may have applicability in some scenarios calling for substantially high reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.

[0570] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a surface energy that is substantially low but is not unduly low, may have applicability in some scenarios that call for substantial reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.Optical / Band Gap

[0571] In the present disclosure, a semiconductor material may be described as a material that, generally exhibits a band gap. In some non-limiting examples, a band gap may be formed between a highest occupied molecular orbital (HOMO) and a lowest unoccupied molecular orbital (LUMO) of the semiconductor material. Semiconductor materials may thus tend to exhibit electrical conductivity that is substantially no more than that of a conductive material (including without limitation, a metal (alloy)), but that is substantially at least that of an insulating material (including without limitation, glass). In some non-limiting examples, the semiconductor material may comprise an organic semiconductor material. In some non-limiting examples, the semiconductor material may comprise an inorganic semiconductor material.

[0572] In some non-limiting examples, an optical gap of a material, including without limitation, a patterning material 411, may tend to correspond to a HOMO-LUMO gap of the material.

[0573] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially large / wide optical (HOMO-LUMO) gap may tend to exhibit substantially weak, including without limitation, no, photoluminescence in at least one of the: deep B(lue) region of the visible, near UV, visible, and NIR, spectrum.

[0574] In some non-limiting examples, a material having a substantially small HOMO-LUMO gap, may have applicability in some scenarios to detect a film of the material using optical techniques.

[0575] In some non-limiting examples, an optical gap of the patterning material 411 may be wider than a photon energy of light emitted by the source, such that the patterning material 411 does not undergo photoexcitation when subjected to such light.Refractive Index and Extinction Coefficient

[0576] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 100, may have a substantially low refractive index.

[0577] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have a refractive index for light at a wavelength of 550 nm that may be one of no more than substantially about: 1.55, 1.5, 1.45, 1.43, 1.4, 1.39, 1.37, 1.35, 1.32, and 1.3.

[0578] In some non-limiting examples, a refractive index of the patterning coating 112 may be no more than substantially about 1.7. In some non-limiting examples, the refractive index of the patterning coating 112 may be one of no more than substantially about: 1.6, 1.5, 1.4, and 1.3. In some non-limiting examples, the refractive index of the patterning coating 112 may be one of substantially between about: 1.2-1.6, 1.2-1.5, and 1.25-1.45. In some non-limiting examples, a patterning coating 112 exhibiting a substantially low refractive index may have application in some scenarios, to enhance at least one of the optical: properties, and performance.of the device 100, including without limitation, by enhancing outcoupling of light emitted by the opto-electronic device 100.

[0579] Without wishing to be bound by any particular theory, it has been observed that providing a patterning coating 112 having a substantially low refractive index may, at least in some devices 100, enhance transmission of external light through the second portion 102 thereof. In some non-limiting examples, devices 300 including an air gap therein, which may be arranged near to the patterning coating 112, may exhibit a substantially high transmittance when the patterning coating 112 has a substantially low refractive index relative to a similarly configured device 100 in which such low-index patterning coating 112 was not provided.

[0580] In some non-limiting examples, a series of samples was fabricated to measure the refractive index at a wavelength of 550 nm for the coatings formed by some of the various example materials. The results of the measurement are summarized in Table 7 below':Table 7

[0581] Based on the foregoing measurement of refractive index in Table 7, and the previous observation regarding one of the: presence, and absence, of a substantially closed coating 340 of Ag in Table 5, it was found that materials that form a low refractive index coating.which in some non-limiting examples, may be those having a refractive index of one of no more than about: 1.4 and 1.38, may have applicability in some scenarios for forming the patterning coating 112 to substantially inhibit deposition of a deposited material 531 thereon, including without limitation, a metal (alloy) including without limitation, at least one of: Yb, Ag, Mg, and an Ag-containing material, including without limitation, MgAg.

[0582] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have a substantially low refractive index.

[0583] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have a refractive index for light at a wavelength of 550 nm that may be one of no more than substantially about: 1.55, 1.5, 1.45, 1.43, 1.4, 1.39, 1.37, 1.35, 1.32, and 1.3.

[0584] In some non-limiting examples, the patterning coating 112 may be at least one of substantially: transparent, and light-transmissive.

[0585] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 112 within the device 300, may have an extinction coefficient that may be no more than about 0.01 for light at a wavelength that is one of at least about: 600, 500, 460, 420, and 410, nm.

[0586] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may have an extinction coefficient that may be one of at least about: 0.05, 0.1, 0.2, and 0.5 for light at a wavelength that is one of no more than about: 400, 390, 380, and 370, nm.

[0587] In this way, at least one of the: patterning coating 112, and patterning material 411, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may absorb light in the UVA spectrum incident upon the device 300, thereby reducing a likelihood that, light in theUVA spectrum may impart constraints in terms of at least one of device: performance, stability, reliability, and lifetime.

[0588] In some non-limiting examples, the patterning coating 112 may exhibit an extinction coefficient of one of no more than about: 0.1, 0.08, 0.05, 0.03, and 0.01 in the visible spectrum.Photoluminescence, Absorption and Other Optical Effects

[0589] In some non-limiting examples, photoluminescence of at least one of a: coating, and material may be observed through a photoexcitation process. In a photoexcitation process, at least one of the: coating, and material, may be subjected to light emitted by a source, including without limitation, a UV lamp.

[0590] When the emitted light is absorbed by at least one of the: coating, and material, electrons thereof may be temporarily excited. Following excitation, at least one relaxation process may occur, including without limitation, at least one of: fluorescence and phosphorescence, in which light may be emitted from at least one of the: coating, and material.

[0591] The light emitted from at least one of the: coating, and material, during such process may be detected, including without limitation, by a photodetector, to characterize the photoluminescence properties of at least one of: the coating, and the material.

[0592] As used herein, a wavelength of photoluminescence, in relation to at least one of the: coating, and material, may generally refer to a wavelength of light emitted by such at least one of the: coating, and material, as a result of relaxation of electrons from an excited state. As would be appreciated by a person having ordinary skill in the relevant art, a wavelength of light emitted by at least one of the: coating, and material, as a result of the photoexcitation process may, in some non-limiting examples, be longer than a wavelength of radiation used to initiate photoexcitation. Photoluminescence may be detected using various techniques known in the art, including, without limitation, fluorescence microscopy.

[0593] In some non-limiting examples, an optical gap of the various coatings / materials may correspond to an energy gap of the coating / material from which light, is one of: absorbed, and emitted, during the photoexcitation process.

[0594] In some non-limiting examples, photoluminescence may be detected by subjecting the coating / material to light having a. wavelength corresponding to the UV spectrum, includingwithout limitation, one of: UVA, and UVB. In some non-limiting examples, light for causing photoexcitation may have a wavelength of about 365 nm.

[0595] In some non-limiting examples, the patterning material 411 may not substantially exhibit photoluminescence at any wavelength corresponding to the visible spectrum.

[0596] In some non-limiting examples, the patterning material 411 may not exhibit photoluminescence upon being subjected to light having a wavelength of one of at least about: 300, 320, 350, and 365.

[0597] As used herein, at least one of a: coating, and material, that is photoluminescent, may be one that exhibits photoluminescence at a wavelength when irradiated with an excitation radiation at a certain wavelength. In some non-limiting examples, at least one of a: coating, and material, that is photoluminescent, may exhibit photoluminescence at a wavelength that may be at least about 365 nm, which is a wavelength of the radiation source frequently used in fluorescence microscopy, upon being irradiated with an excitation radiation having a wavelength of 365 nm.

[0598] At least one of a: coating, and material, that is photoluminescent, may be detected on a substrate 10 using standard optical techniques, including without limitation, fluorescence microscopy, which may establish the presence of such at least one of the: coating, and material.

[0599] In some non-limiting examples, a coating, including without limitation, a patterning coating 112, may exhibit photoluminescence, including without limitation, by comprising a material that exhibits photoluminescence.

[0600] In some non-limiting examples, the presence of such patterning coating 112 may be detected (observed) using routine characterization techniques, including without limitation, fluorescence microscopy upon deposition of the patterning coating 112.

[0601] In some non-limiting examples, a coating, including without limitation, a patterning coating 112, may exhibit photoluminescence at a wavelength corresponding to at least one of the: UV, and visible, spectrum, including without limitation, by comprising a material that exhibits photoluminescence. In some non-limiting examples, photoluminescence may occur at a wavelength (range) corresponding to the UV spectrum, including, without limitation, one of the: UVA, and UVB, spectrum. In some non-limiting examples, photoluminescence may occur at a wavelength (range) corresponding to the visible spectrum. In some non-limiting examples,photoluminescence may occur at a wavelength (range) corresponding to one of: deep B(lue) and near UV.

[0602] In some non-limiting examples, at least one of the materials of the patterning coating 112 that may exhibit photoluminescence may comprise at least one of: a conjugated bond, an aryl moiety, a donor-acceptor group, and a heavy metal complex.

[0603] In some non-limiting examples, a coating, including without limitation, a patterning coating 112, comprised of a material, including without limitation, a patterning material 411, having substantially weak to no photoluminescence (absorption) in a wavelength range of one of at least about: 365, and 460, nm, may tend to not act as one of a photoluminescent, and an absorbing, coating and may have applicability in some scenarios calling for substantially high transparency in at least one of the: visible, and NIR, spectrum.

[0604] In some non-limiting examples, such material may tend to exhibit substantially low photoluminescence upon being subjected to light having a wavelength of about 365 nm, which is a wavelength of the radiation source frequently used in fluorescence microscopy. The presence of such materials, including without limitation, a patterning material 411, especially when deposited, in some non-limiting examples, as a thin film, may have reduced applicability in some scenarios calling for typical optical detection techniques, including without limitation, fluorescence microscopy. This may impose constraints in some scenarios in which such material may be selectively deposited, including without limitation through an FMM, over part(s) of a substrate 10, as there may be some scenarios for determining, following the deposition of the material, the part(s) in which such materials are present.

[0605] In some non-limiting examples, a material with substantially low, to no, absorption at a wavelength that is one of at least about: 365, and 460, nm, may have applicability in some scenarios calling for substantially high transparency in at least one of the: visible, and NIR, spectrum.

[0606] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may not substantially attenuate light passing therethrough, in at least the visible spectrum.

[0607] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, when deposited as at least one of a: film, and coating, in a form, andunder circumstances similar to the deposition of the patterning coating 112 within the device 300, may not substantially attenuate light passing therethrough, in the (N)IR spectrum.

[0608] In this way, at least one of the: patterning coating 112, and patterning material 411, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 112 within the device 300, may absorb light in the UVA spectrum incident upon the device 100, thereby reducing a likelihood that light in the UVA spectrum may impart constraints in terms of at least one of: performance, stability, reliability, and lifetime of the device 300.

[0609] In some non-limiting examples, the patterning coating 112 may act as an optical coating.

[0610] In some non-limiting examples, the patterning coating 112 may modify at least one of: at least one property, and at least one characteristic, of light (including without limitation, in the form of photons) emitted by the device 300. In some non-limiting examples, the patterning coating 112 may exhibit a degree of haze, causing emitted light to be scattered. In some non¬ limiting examples, the patterning coating 112 may comprise a crystalline material for causing light transmitted therethrough to be scattered. In some non-limiting examples, such scattering of light may facilitate enhancement of the outcoupling of light from the device 300. In some non¬ limiting examples, the patterning coating 112 may initially be deposited as a substantially non¬ crystalline, including without limitation, substantially amorphous, coating, whereupon, after deposition thereof, the patterning coating 112 may become crystallized and thereafter serve as an optical coupling.

[0611] In some non-limiting examples, the patterning material 411 may exhibit insignificant, including without limitation, no, detectable absorption when subjected to light having a wavelength of one of at least about: 300, 320, 350, and 365, nm.

[0612] In some non-limiting examples, the patterning coating 112 may not exhibit any substantial light absorption at any wavelength corresponding to the visible spectrum.Average Layer Thickness

[0613] In some non-limiting examples, an average layer thickness of the patterning coating 112 may be one of no more than about: 10, 8, 7, 6, and 5, nm.Weight

[0614] Without wishing to be bound by any particular theory, it may be postulated that, for compounds that are adapted to form surfaces with substantially low7surface energy, there may be scenarios calling for, in at least some applications, a molecular weight of such compounds to be one of between about: 800-3,000, 900-2,000, 900-1,800, and 900-1,600, g / mol.

[0615] In some non-limiting examples, the molecular weight of the compound of the at least one patterning material 411 may be no more than about 5,000 g / mol. In some non-limiting examples, the molecular weight of the compound may be one of no more than about: 4,500, 4,000, 3,800, and 3,500, g / mol.

[0616] In some non-limiting examples, a molecular weight of the compound of the at least one patterning material 411 may be at least about 800 g / mol. In some non-limiting examples, a molecular weight of the compound may be one of at least about: 1,500, 1,700, 2,000, 2,200, and 2,500, g / mol.

[0617] In some non-limiting examples, a molecular weight of the compound may be one of between about: 800-3,000, 900-2,000, 900-1,800, and 900-1,600, g / mol.

[0618] In some non-limiting examples, a percentage of a molar weight of such compound that may be attributable to the presence of F atoms, may be one of between about: 40-90%, 45-85%, 50-80%, 55-75%, and 60-75%. In some non-limiting examples, F atoms may constitute a majority of the molar weight of such compound.Inter-Relationships Between Patterning Coating Attributes

[0619] Without wishing to be bound by any particular theory, it may be postulated that exposed layer surfaces 11 exhibiting low7initial sticking probability with respect to the deposited material 531, including without limitation, a metal (alloy) including without limitation, Yb, Ag, Mg, and an Ag-containing material, including without limitation, MgAg, may exhibit high transmittance. Without wishing to be bound by any particular theory, it may be postulated that exposed layer surfaces 11 exhibiting high sticking probability with respect to the deposited material 531, including without limitation, a metal (alloy) including without limitation, Yb, Ag, Mg, and an Ag-containing material, including without limitation, MgAg, may exhibit low7transmittance.

[0620] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to have a substantially high initial sticking probability against deposition of a deposited material, including without limitation, a. metal (alloy) including withoutlimitation, at least one of: Yb, Ag, Mg, and an Ag-containing material, including without limitation, MgAg, if the material has a substantially high surface energy.

[0621] In some non-limiting examples, a patterning material 411 that has a substantially low surface tension, that is not unduly low, may have applicability in some scenarios calling for a substantially high melting point, including without limitation, between about 15-22 dynes / cm.

[0622] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a surface tension that is substantially low, but not unduly low, may have applicability in some scenarios that call for a substantially high sublimation temperature.

[0623] In some non-limiting examples, a coating, including without limitation, a patterning coating 112, comprised of a material, including without limitation, a patterning material 411, having a substantially low surface energy and a substantially high sublimation temperature, may have application in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0624] Without wishing to be bound by any particular theory, it may be postulated that materials that form an exposed layer surface 11 having a surface energy, in some non-limiting examples, of no more than about 13 dynes / cm, may have reduced applicability as a patterning material 411 in some scenarios, as such materials may exhibit at least one of: substantially low adhesion to layer / s) surrounding such materials, a substantially low7melting point, and a substantially low sublimation temperature.

[0625] In some non-limiting examples, a patterning coating 112 having a substantially low surface energy and a substantially high melting point may have applicability in some scenarios calling for high temperature reliability. In some non-limiting examples, there may be challenges in achieving such a combination from a single material given that in some non¬ limiting examples, a single material having a low surface energy may tend to exhibit a low melting point.

[0626] Without wishing to be bound by any particular theory, it may be postulated that such compounds, including without limitation, of at least one patterning material 411, may exhibit at least one property that may have applicability in some scenarios for forming at least one of a: coating, and layer, having at least one of a substantially: high melting point, in some non-limiting examples, of at least 100°C, low surface energy, and amorphous structure, when deposited, in some non-limiting examples, using vacuum-based thermal evaporation processes.

[0627] In some non-limiting examples, a coating, including without limitation, a patterning coating 112, having a substantially: low7surface energy, high cohesion energy, and high melting point, may have applicability in some scenarios that call for substantially high reliability under various conditions. In some non-limiting examples, there may be challenges in achieving such a combination from a single material, given that., in some non-limiting examples, a unitary’ material having a substantially low surface energy may tend to exhibit a substantially low: cohesion energy, and melting point.

[0628] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially: low surface energy, and high cohesion energy, may have applicability in some scenarios that call for substantially high reliability under at least one of: sheer, and bending, stress. In some non-limiting examples, there may be challenges in achieving such a combination from a single material, given that, in some non-limiting examples, a thin film formed substantially of a single material having a substantially low surface energy may tend to exhibit a substantially low cohesion energy.

[0629] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low surface energy may tend to exhibit at least one of a substantially: large, and wide, optical gap. In some non-limiting examples, an optical gap of a material, including without limitation, a patterning material 411, may tend to correspond to a HOMO-LUMO gap of the material.

[0630] In general, a material with a low surface energy may exhibit at least one of a substantially: large, and wide, optical gap which, in some non-limiting examples, may correspond to a HOMO-LUMO gap of the material.

[0631] It has now been found that a patterning coating 112 formed by a compound exhibiting a substantially low surface energy may exhibit a substantially low refractive index.

[0632] In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, may exhibit a: surface energy of no more than about 25 dynes / cm, and refractive index of no more than about 1.45. In some non-limiting examples, at least one of the: patterning coating 112, and patterning material 411, may comprise a material exhibiting a: surface energy of no more than about 20 dynes / cm, and refractive index of no more than about 1.4.

[0633] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low surface energy may have applicability in some scenarios calling for substantially weak to no, at least one of: photoluminescence, and absorption, in a wavelength range that is one of at least about: 365 and 460, nm.

[0634] In some non-limiting examples, a material, including without limitation, a patterning material 411, having at least one of a substantially: large, and wide, optical gap (and H0M0-LUM0 gap) may tend to exhibit a substantially weak to no photoluminescence in at least one of the: deep B(lue) region of the visible, near UV, visible, and NIR, spectrum,

[0635] Without wishing to be bound by any particular theory', it may be postulated that, for compounds that are adapted to form surfaces with substantially low surface energy, there may be an aim, in at least some applications, for a molecular weight of such compounds to be one of between about: 1,500-5,000, 1,500-4,500, 1,700-4,500, 2,000-4,000, 2,200-4,000, and 2,500- 3,800, g / mol.

[0636] At least some materials with at least one of a substantially: large, and wide, optical (and H0M0-LUM0) gap, may exhibit substantially weak, to substantially no, photoluminescence in at least one of the: visible, deep B(lue) region thereof, and near UV, spectrum. In some non-limiting examples, a material with a substantially small H0M0-LUM0 gap may have applicability in applications to detect a film of the material using optical techniques. In some non-limiting examples, a material with a substantially high surface energy may have applicability for applications to detect a film of the material using optical techniques.

[0637] In some non-limiting examples, a material having a substantially large H0M0- LUMO gap may have applicability in some scenarios calling for substantially weak to no at least one of: photoluminescence, and absorption, in a wavelength range of one of at least about: 365, and 460, nm.Doping

[0638] In some non-limiting examples, the patterning coating 112 may exhibit, including without limitation, because of at least one of the: patterning material 411 used, and deposition environment, at least one nucleation site for the deposited material 531.

[0639] In some non-limiting examples, the patterning coating 112 may be doped, including without limitation, by at least one of: covering, and supplementing, with another material that may act as at least one of a: seed, and heterogeneity, to act as such a nucleation sitefor the deposited material 531, including without limitation, to provide, in some non-limiting examples, because of at least one of the: patterning material 411 used, and the deposition environment, at least one nucleation site for the deposited material 531 to form at least one NP thereon.

[0640] In some non-limiting examples, such other material may comprise a material comprising a metallic element, including without limitation, Au.

[0641] In some non-limiting examples, such other material may comprise an NPC 720 material.

[0642] In some non-limiting examples, such other material may comprise: an organic material, in some non-limiting examples, at least one of a: polycyclic aromatic compound, and material comprising a non-metallic element, including without limitation, at least one of: O, S, N, and C, whose presence might otherwise be a contaminant in at least one of the: source material, equipment used for deposition, and vacuum chamber environment.

[0643] In some non-limiting examples, such other material, including without limitation, an elemental material, may be considered to be a dopant, where the patterning coating 112, with which it has been doped, may be considered to be the host.

[0644] In some non-limiting examples, such other material may be deposited in a layer thickness that is a fraction of a monolayer, to avoid forming a closed coating 340 thereof.Rather, the monomers of such other material may tend to be spaced apart in the lateral aspect so as form discrete nucleation sites for the deposited material.

[0645] In some non-limiting examples, such other material may comprise an NPC 720 material.Plurality of Patterning Materials

[0646] In some non-limiting examples, forming a patterning coating 112 of a single patterning material 411 against the deposition of a deposited material 531, including without limitation, of a given metal (alloy), including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, that satisfied constraints of at least one material property selected from at least one of: initial sticking probability, transmittance, deposition contrast, surface energy, glass transition temperature, melting point, sublimation temperature, evaporation temperature, cohesion energy, optical gap, photoluminescence, refractive index, extinction coefficient, absorption, other optical effect, average layer thickness,molecular weight, and composition, for a given scenario, may impose challenges, given the substantially complex inter-relationships between the various material properties.

[0647] In some non-limiting examples, the patterning coating 112 may comprise a plurality of materials. In some non-limiting examples, the patterning coating 112 may comprise a: first, and second, material.

[0648] In some non-limiting examples, at least one of the plurality of materials of the patterning coating 112 may serve as an NIC when deposited as a thin film.

[0649] In some non-limiting examples, at least one of the plurality of materials of the patterning coating 112 may serve as an NIC when deposited as a thin film, and another material thereof may serve as an NPC 720 when deposited as a thin film. In some non-limiting examples, the first material may serve as an NPC 720 when deposited as a thin film, and the second material may serve as an NIC when deposited as a thin film. In some non-limiting examples, the presence of the first material in the patterning coating 112 may result in an increased initial sticking probability thereof compared to cases in which the patterning coating 112 is formed of the second material and is substantially devoid of the first material.

[0650] In some non-limiting examples, at least one of the materials of the patterning coating 112 may be adapted to form a surface having a low surface energy when deposited as a thin film. In some non-limiting examples, the first material, when deposited as a thin film, may be adapted to form a surface having a surface energy that may be no more than that of a surface provided by a thin film comprising the second material.

[0651] In some non-limiting examples, the patterning coating 112 may exhibit photoluminescence, including without limitation, by comprising a material which exhibits photoluminescence.

[0652] In some non-limiting examples, the first material may exhibit photoluminescence at a wavelength corresponding to the visible spectrum, and the second material may not exhibit substantial photoluminescence at any wavelength corresponding to the visible spectrum.

[0653] In some non-limiting examples, the second material may not substantially exhibit photoluminescence at any wavelength corresponding to the visible spectrum. In some non¬ limiting examples, the second material may not exhibit photoluminescence upon being subjected to light having a wavelength of one of at least about: 300, 320, 350, and 365, nm. In some non-limiting examples, the second material may exhibit insignificant to no detectable absorption when subjected to such light.

[0654] In some non-limiting examples, a second optical gap of the second material may be wider than a photon energy of the light emitted by the source, such that the second material does not undergo photoexcitation when subjected to such light. In some non-limiting examples, the patterning coating 112 comprising such second material may nevertheless exhibit photoluminescence upon being subjected to light due to the first material exhibiting photoluminescence. In some non-limiting examples, the presence of the patterning coating 112 may be detected using routine characterization techniques, including without limitation, fluorescence microscopy upon deposition of the patterning coating 112.

[0655] In some non-limiting examples, the first material may have a first optical gap, and the second material may have a second optical gap. In some non-limiting examples, the second optical gap may be at least that, of the first optical gap. In some non-limiting examples, a difference between the first optical gap and the second optical gap may be one of at least about: 0.3, 0.5, 0.7, 1, 1.3, 1.5, 1.7, 2, 2.5, and 3, eV.

[0656] In some non-limiting examples, the first optical gap may be one of no more than about: 4.1, 3.5, and 3.4, eV. In some non-limiting examples, the second optical gap may be one of at least about: 3.4, 3.5, 4.1, 5, and 6.2, eV.

[0657] In some non-limiting examples, at least one of the: first, and second, optical gap, may correspond to the H0M0-LUM0 gap.

[0658] In some non-limiting examples, an optical gap of at least one of the various: coatings, and materials, including without limitation, at least one of the: first, and second, optical gap, may correspond to an energy gap of at least one of the: coating, and material, from which light is at least one of: absorbed, and emitted, during the photoexcitation process.

[0659] In some non-limiting examples, a concentration, including without limitation by weight, of the first material in the patterning coating 112 may be no more than that of the second material in the patterning coating 112. In some non-limiting examples, the patterning coating 112 may comprise one of at least about: 0.1, 0.2, 0.5, 0.8, 1, 3, 5, 8, 10, 15, and 20, wt.%, of the first material. In some non-limiting examples, the patterning coating 112 may comprise one of no more than about: 50, 40, 30, 25, 20, 15, 10, 8, 5, 3, and 1, wt.%, of the first material. In some non-limiting examples, a remainder of the patterning coating 112 may be substantially comprisedof the second material. In some non-limiting examples, the patterning coating 112 may comprise additional materials, including without limitation, at least one of a: third, and fourth, material.

[0660] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, the first material and the second material, may comprise at least one of: F, and Si. In some non-limiting examples, at least one of the: first, and second, material, may comprise at least one of: F, and Si. In some non-limiting examples, the first material may comprise at least one of: F, and Si, and the second material may comprise at least one of: F, and Si. In some non-limiting examples, the first material and the second material both may comprise F. In some non-limiting examples, the first material and the second material both may comprise Si. In some non-limiting examples, each of the first material and the second material may comprise at least one: F, and Si.

[0661] In some non-limiting examples, at least one of the: first, and second, material, may comprise both F and Si, In some non-limiting examples, one of the: first., and second, material may not comprise at least one of: F, and Si. In some non-limiting examples, the second material may comprise at least one of: F, and Si, and the first material may not comprise at least one of: F, and Si.

[0662] In some non-limiting examples, at least one of the materials of the patterning coating 112, which in some non-limiting examples, may be at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 112 may comprise a sp2C. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 112 may comprise a sp3C. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C, and at least one of the other materials of the patterning coating 112 may comprise an sp2C. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C, wherein all F bonded to a C may be bonded to an sp3C, and at least one of the other materials of the patterning coating 112 may comprise an sp2C. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C,wherein all F bonded to C may be bonded to an sp3C, and at least one of the other materials of the patterning coating 112 may comprise an sp2C and mmay not comprise F.

[0663] In some non-limiting examples, in any of the foregoing non-limiting examples, the term “at least one of the materials of the patterning coating 112” may, in some non-limiting examples, as the context dictates, correspond to the second material, and the term “at least one of the other materials of the patterning coating 112” may, in some non-limiting examples, as the context dictates, correspond to the first material.

[0664] As would be appreciated by those having ordinary skill in the relevant art, the presence of materials in a coating that comprises at least one of F, sp2C, sp3C, an aromatic hydrocarbon moiety, other functional groups, and other moieties, may be detected using various methods known in the art, including without limitation. X-ray Photoelectron Spectroscopy (XPS).

[0665] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 112 may comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the materials of the patterning coating 112 may not comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise an aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 112 may comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise an aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 112 may comprise an aromatic hydrocarbon moiety and may not comprise F, In some non-limiting examples, the aromatic hydrocarbon moiety may comprise at least one of: a substituted polycyclic aromatic hydrocarbon, an unsubstituted polycyclic aromatic hydrocarbon, a substituted phenyl, and an unsubstituted phenyl, moiety.

[0666] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, maycomprise F, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first., and second, material, may comprise F, and at least one of the materials of the patterning coating 112 may not comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety7and mmay not comprise F.

[0667] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and at least one of the materials of the patterning coating 112 may not comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and may not comprise a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and may not comprise a polycyclic aromatic hydrocarbon moiety7, and at least one of the other materials of the patterning coating 112 may comprise a polycyclic aromatic hydrocarbon moiety and may not comprise at least one of a: fluorocarbon, and siloxane, moiety.

[0668] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the materials of the patterning coating 112 may not comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety and may not comprise F.

[0669] In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety, and at least one of the materials of the patterning coating 112 may not comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may comprise at least one of a: fluorocarbon, and siloxane, moiety and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 112 may comprise a phenyl moiety and may not comprise either of a: fluorocarbon, and siloxane, moiety.

[0670] In general, at least, one of the molecular: structures, and compositions, of the materials of the patterning coating 112, including without limitation, at least one of the: first, andsecond, material, may be different. In some non-limiting examples, the materials may be selected such that they possess at least one property which is one of substantially: similar to, and different from, one another, including without limitation, at least one of: at least one of a: molecular structure of a monomer, monomer backbone, and functional group; a presence of a element in common; a similarity in molecular structure; a characteristic surface energy; a refractive index; a molecular weight; and a thermal property, including without limitation, at least one of a: melting, sublimation, glass transition, and thermal decomposition, temperature.

[0671] A characteristic surface energy, as used herein, in some non-limiting examples, with respect to a material, may generally refer to a surface energy determined from such material. In some non-limiting examples, a characteristic surface energy may be measured from a surface formed by the material deposited in a thin film form. Various methods and theories for determining the surface energy of a solid are known. In some non-limiting examples, a surface energy may be determined based on a series of contact angle measurements, in which various liquids may be brought into contact with a surface of a solid to measure a contact angle between the liquid-vapor interface and the surface. In some non-limiting examples, a surface energy of a solid surface may be equal to the surface tension of a liquid with the highest surface tension that completely wets the surface. In some non-limiting examples, a Zisman plot may be used to determine a highest surface tension value that would result in complete wetting i.e. contact angle of 0°) of the surface.

[0672] In some non-limiting examples, at least one of the: first, and second, material, of the patterning coating 112 may be an oligomer.

[0673] In some non-limiting examples, the first material may comprise a first oligomer, and the second material may comprise a second oligomer. In some non-limiting examples, each of the first, and second, oligomer may comprise a plurality of monomers.

[0674] In some non-limiting examples, at least a fragment of the molecular structure of the at least one of the materials of the patterning coating 112, including without limitation, at least one of the: first, and second, material, may be represented by Formula (I):Q where:Mon represents a monomer, andn is an integer of at least 2.

[0675] In some non-limiting examples, n may be an integer of one of between about: 2- 100, 2-50, 3-20, 3-15, 3-10, and 3-7.

[0676] In some non-limiting examples, the molecular structure of the first material and the second material of the patterning coating 112 may each be independently represented by Formula (I). In some non-limiting examples, at least one of: the monomer, and n, of the first material may be different from that of the second material. In some non-limiting examples, n of the first material may be the same as n of the second material. In some non-limiting examples, n of the first material may be different from n of the second material. In some non-limiting examples, the first material and the second material may be oligomers.

[0677] In some non-limiting examples, the monomer may comprise at least one of: F, and Si.

[0678] In some non-limiting examples, the monomer may comprise a functional group. In some non-limiting examples, at least one functional group of the monomer may have a low surface tension. In some non-limiting examples, at least one functional group of the monomer may comprise at least one of: F, and Si, including without limitation, at least one of a: fluorocarbon, and siloxane, group. In some non-limiting examples, the monomer may comprise a silsesquioxane group.

[0679] While some non-limiting examples have been described herein with reference to a first material and a second material, it will be appreciated that the patterning coating may further comprise at least one additional material, and descriptions regarding at least one of the molecular: structures, and properties, of at least one of the: first material, second material, first oligomer, and second oligomer, may be applicable with respect to additional materials which may be contained in the patterning coating 112.

[0680] The surface tension attributable to a fragment of a molecular structure, including without limitation, at least one of a: monomer, monomer backbone unit, linker, and a functional group, may be determined using various known methods in the art, including without limitation, the use of a Parachor, such as may be further described, in some non-limiting examples, in “Conception and Significance of the Parachor”, Nature 196: 890-891. In some non-limiting examples, at least one functional group of the monomer may have a surface tension of one of no more than about: 25, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, and 10, dynes / cm.

[0681] In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF2H, moiety. In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF3, moiety. In some non-limiting examples, the monomer may comprise a CH2CF3 moiety. In some non-limiting examples, the monomer may comprise at least one of: C, and O. In some non-limiting examples, the monomer may comprise a fluorocarbon monomer. In some non-limiting examples, the monomer may comprise at least one of a: vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, and fluorinated 1,3-di oxole, moiety.

[0682] In some non-limiting examples, the monomer may comprise a monomer backbone and a functional group. In some non-limiting examples, the functional group may be bonded, one of: directly, and via a linker group, to the monomer backbone. In some non-limiting examples, the monomer may comprise the linker group, and the linker group may be bonded to the monomer backbone and to the functional group. In some non-limiting examples, the monomer may comprise a plurality of functional groups, which may be one of: the same, and different, from one another. In such examples, each functional group may be bonded, one of: directly, and via a linker group, to the monomer backbone. In some non-limiting examples, where a plurality of functional groups is present, a plurality of linker groups may also be present.

[0683] In some non-limiting examples, the molecular structure of at least one of the materials of the patterning coating 112, wh...

Claims

1. WHAT IS CLAIMED IS:

1. An opto-electronic device comprising a plurality of layers deposited on a substrate and extending in a lateral aspect defined by a lateral axis thereof, the plurality of layers defining an emissive region comprising:a first electrode,a second electrode,at least one semiconducting layer disposed between the first electrode and the second electrode;wherein:the first electrode is disposed between the substrate and the at least one semiconducting layer;the second electrode comprises a substantially low loss silver (Ag) (composite) thin film coating comprising a first deposited material comprising a substantially low loss Ag (composite) material, andthe second electrode exhibits a substantially low:sheet resistance (Rs), while still exhibiting a transmittance (T) that is substantially high and an average layer thickness that is substantially thin, andabsorption (Abs).

2. The device of claim 1, wherein the absorption is defined by Abs = 1 - T - R, where R is a reflectance.

3. The device of claim 1 or 2, wherein the absorption is one of no more than substantially about: 2%, 3%, 5%, 10%, 15%, 20%, and 25%.

4. The device of any one of claims 1 through 3, wherein the absorption is no more than substantially about 10%.

5. The device of any one of claims 1 through 4, wherein the substantially high transmittance may permit transmission of light therethrough.

6. The device of any one of claims 1 through 5, wherein the substantially low loss Ag (composite) thin film coating exhibits a substantially small grain size.

7. The device of any one of claims 1 through 6, wherein a combination of the sheet resistance and transmittance is one of substantially about: Rs < 10 £! / □, T > 50%; Rs< 9 & / □, T > 50%, Rs< 8! Q / n, T > 50%; and Rs< 7 £} / □, T > 60%.

8. The device of any one of claims 1 through 7, wherein the average layer thickness is one of no more than substantially about: 25, 20, 18, 15, 13, 10, 8, 7, and 5 nm,9. The device of any one of claims 1 through 8, wherein the sheet resistance is reduced by depositing a seed material prior to deposition of the substantially low loss Ag (composite) material for such material to coalesce therearound.

10. The device of claim 9, wherein the seed material changes a morphology of the substantially low loss Ag (composite) material.

11. The device of claim 9 or 10, wherein the seed material exhibits a bond dissociation energy between it and Ag that is at least that of a bond dissociation energy of Ag-Ag.

12. The device of any one of claims 9 through 11, wherein the seed material exhibits substantially low absorption and substantially increased wetting on organic materials.

13. The device of any one of claims 9 through 12, wherein the seed material comprises at least one of: gold (Au), aluminum (Al), copper (Cu), germanium (Ge), indium (In), lithium (Li), cobalt (Co), nickel (Ni), palladium (Pd), and bismuth (Bi).

14. The device of any one of claims 9 through 13, wherein the seed material comprises at least one of: Au, Al, Cu, Ge, In, Co, Ni, Pd, and Bi.

15. The device of any one of claims 9 through 14, wherein the seed material comprises a second deposited material comprising Au.

16. The device of claim 15, wherein the second deposited material lies between the first deposited material and the at least one semiconducting layer.

17. The device of any one of claims 1 through 16, wherein the first electrode is disposed between the substrate and the at least one semiconducting layer.

18. The device of any one of claims 1 through 17, wherein, when energized:the first electrode is an anode adapted to generate holes,the second electrode is a cathode adapted to generate electrons; andthe at least one semiconducting layer comprises an emissive layer adapted to combine a generated hole and a generated electron and emit a photon thereby.

19. The device of claim 18, wherein the photon is emitted through the second electrode.

20. The device of claim 18 or 19, wherein the photon has a wavelength that lies within one of the: visible, infrared (IR), near-IR, ultraviolet (UV), and extreme UV, spectrum.

21. The device of any one of claims 1 through 20, further comprising at least one patterning coating disposed on an exposed layer surface of an underlying layer of the device, in a first portion of the lateral aspect.

22. The device of claim 21, wherein the at least one patterning coating is adapted to impact a propensity of an evaporated flux of at least one of the: first, and second, deposited material to be deposited thereon.

23. The device of claim 21 or 22, wherein an exposed layer surface of the at least one patterning coating is substantially devoid of a closed coating of at least one of the: first, and second, deposited material.

24. The device of any one of claims 21 through 23, wherein an exposed layer surface of the at least one patterning coating is substantially devoid of both a closed coating of the first deposited material, and a closed coating of the second deposited material.

25. The device of claim 24, wherein the exposed layer surface of the at least one patterning coating is substantially devoid of the first deposited material.

26. The device of any one of claims 1 through 25, wherein the second electrode comprises a first deposited sub-layer comprising the first deposited material and a second deposited sub-layer comprising the second deposited material and the first deposited sub-layer is disposed between the at least one semiconducting layer and the second deposited sub-layer.

27. The device of claim 26, wherein the first deposited sub-layer and the second deposited sub-layer are both disposed in a second portion of the lateral aspect.

28. The device of claim 26 or 27, wherein the first deposited sub-layer is a discontinuous layer of at least one particle structure of the first deposited material.

29. The device of any one of claims 26 through 28, wherein the second deposited sub-layer is a closed coating of the second deposited material.

30. The device of any one of claims 26 through 29, wherein the at least one particle structure is adapted to serve as a nucleation site for the second deposited material.

31. The device of any one of claims 26 through 30, wherein the second deposited material is in physical contact with the at least one particle structure of the first deposited material.

32. The device of any one of claims 26 through 31, further comprising a layer comprising ytterbium (Yb) disposed between the at least one semiconducting layer and the first deposited sub-layer.

33. The device of claims 26 through 32, wherein the second electrode comprises a mixture of the first deposited material and the second deposited material.

34. The device of any one of claims 1 through 33, wherein the first portion excludes a lateral aspect of the emissive region.

35. The device of any one of claims 1 through 34, wherein the first portion comprises a transmissive region adapted to allow light to pass therethrough.

36. The device of any one of claims 1 through 35, wherein the first portion includes a lateral aspect of the emissive region.

37. The device of any one of claims 1 through 36, wherein an average layer thickness of the second electrode is one of no more than substantially about: 20, 18, 15, 12, 10, and 8, nm.

38. The device of any one of claims 1 through 37, wherein a sheet resistance of the second electrode is one of no more than substantially about: 10, 15, 18, 20, and 30, Ω / □.

39. The device of any one of claims 1 through 38, wherein a light transmittance of the second electrode at a wavelength of 460 nm is one of substantially at least about: 60%, 65%, and 70%.

40. The device of any one of claims 1 through 39, wherein a light transmittance of the second electrode at a wavelength of 940 nm is one of substantially at least about: 40%, 50%, and 60%.

41. The device of any one of claims 1 through 40, wherein the at least one semiconducting layer comprises an electron injection layer (EIL) comprising an electron injection material.

42. The device of any one of claims 1 through 41, wherein the electron injection material comprises one of: Li, Yb, and Yb-doped Li.