A composite for cooling a photovoltaic (PV) device, and method of forming the composite
A cross-linked polyacrylate-hygroscopic salt composite addresses inefficiencies in passive PV cooling by enhancing moisture absorption and evaporative cooling, ensuring stable and efficient temperature reduction across different climates.
Patent Information
- Application Number
- PCT/IB2026/054732
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional materials for passive cooling of photovoltaic (PV) devices face challenges such as low moisture release rates, structural integrity issues, and reduced porosity leading to inefficient evaporative cooling, along with the need for frequent material replacement and complex fabrication techniques.
A composite comprising a cross-linked network of polyacrylate and hygroscopic salt, which absorbs moisture effectively, maintains mechanical stability, and provides efficient evaporative cooling without the need for additional cross-linkers or catalysts, with a balanced ratio of polyacrylate and hygroscopic salt for optimal performance.
The composite achieves high water uptake and thermal conductivity, maintaining effective cooling power and temperature reduction of PV devices, even under varying humidity conditions, with long-term stability and durability.
Smart Images

Figure IB2026054732_19112026_PF_FP_ABST
Abstract
Description
[0001] A composite for cooling a photovoltaic (PV) device, and method of forming the composite
[0002] Technical Field
[0003] The present invention relates to an improved composite for cooling a photovoltaic (PV) device, and method of forming the composite.
[0004]
[0005] Photovoltaic (PV) technology is a key player in harnessing clean and renewable energy. PV systems are valued for their efficiency, low operating costs, and long lifespan. When exposed to sunlight, PV devices absorb solar radiation and convert it into electricity. However, one downside is that heat is generated during the process, which raises devices temperatures, and in turn cause hotspots, thermal stress, efficiency loss, which ultimately reduces energy output of a PV system.
[0006] Strategies for cooling PV devices are broadly categorised into active and passive methods. Conventional active cooling employs powered systems, such as water or air circulation, to remove heat. However, active cooling is costly, energy-intensive, and reguires complex maintenance.
[0007] Passive cooling relies on natural processes for heat dissipation. However, conventional materials used for evaporative cooling of solar panels reguire freguent replacement of the materials during daytime operation, which is highly impractical for long-term use. Other conventional materials aiming to enhance water uptake involves complicated fabrication technigues, such as freeze drying, to increase the hydrogel porosity and provide a larger moisture absorption area. However, the porous structure of the hydrogel collapses during water evaporation due to the loss of structural integrity, leading to a decrease in surface area available for water absorption in subseguent cycles, and lower sorption rates in the long term. Additionally, the reduced porosity limits the rate of water evaporation, as there is less surface area for the water to escape from the hydrogel, and thus reduces cooling power.
[0008] Conventional materials also face challenges in achieving a desirable rate of moisture release. Captured water cannot be released easily for efficient evaporative cooling, since the strong hydrogen bonds between ions and water and between polymer chains andwater, which contribute to ease of water uptake, results in the water being strongly bound and preventing evaporative cooling from occurring.
[0009] There is therefore a need for an improved composite for cooling of a PV device.
[0010] Summary of the invention
[0011] The present invention seeks to address these problems, and / or to provide an improved composite particularly suitable for, but not limited to, passive cooling of a PV device, and a method of forming the composite.
[0012] According to a first aspect, there is provided a composite for cooling a photovoltaic (PV) device, wherein the composite comprises a cross-linked network comprising a polyacrylate and a hygroscopic salt.
[0013] According to a particular aspect, the polyacrylate may have an average molecular weight of 4-11 million g / mol. The cross-linked network may not comprise a cross-linker.
[0014] According to a particular aspect, a weight ratio of the polyacrylate and the hygroscopic salt may be 1.5: 1-3: 1.
[0015] The polyacrylate may comprise sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, ammonium polyacrylate, or a combination thereof. The hygroscopic salt may comprise lithium chloride, sodium chloride, calcium chloride, magnesium chloride, or a combination thereof.
[0016] According to a particular aspect, the composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30%.
[0017] The composite may have a thermal conductivity of > 0.435 W / (m K). The composite may have a cooling power of > 140 W / m2.
[0018] According to a particular aspect, in use, the composite may provide a rate of liquid water mass loss of > 0.5 kg / (m2h). In use, the composite may be capable of reducing temperature of the PV device by > 9 °C.
[0019] The composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 3 weeks of use. The composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 12 months of use.According to a second aspect, there is provided a method of forming the composite according to the first aspect, the method comprising:
[0020] mixing a polyacrylate and a solution of a hygroscopic salt, to form a mixture; and
[0021] curing the mixture to form the composite.
[0022] According to a particular aspect, the curing may be for 3-60 minutes. The curing may be at a temperature of 20-25 °C.
[0023] The method may not comprise adding a cross-linker. According to a particular aspect, the mixture may comprise the polyacrylate and the hygroscopic salt at a weight ratio of 1.5:1-3:1.
[0024] Brief Description of the Drawings
[0025] In order that the invention may be fully understood and readily put into practical effect there shall now be described by way of non-limitative example only exemplary embodiments, the description being with reference to the accompanying illustrative drawings. In the drawings:
[0026] Figure 1 shows an illustration of an embodiment of a composite with a crosslink network of PAAS matrix and LiCI as the hygroscopic agent;
[0027] Figure 2 shows scanning electron microscopy (SEM) images of PAAS-LiCI composite prepared using PAAS with an average molecular weight of (a) 0.15 million; (b) 5-7 million; and (c) 12 million;
[0028] Figure 3 shows an SEM image of LiCI crystals distributed and anchored within the PAAS framework, in which the composite was prepared using PAAS with an average molecular weight of 5-7 million;
[0029] Figure 4 shows an X-ray diffraction (XRD) analysis of the PAAS-LiCI composite;
[0030] Figure 5 shows (a) stress-strain curve of the PAAS-LiCI hydrogel before and after moisture absorption; (b) tensile test showing the force required to separate the hydrogel from the solar cell in a direction perpendicular to the panel; (c) tensile test showing the force required to separate the hydrogel from the solar cell in a direction parallel to the panel;Figure 6 shows (a) water uptake of PAAS, PAAS-LiCI, and LiCI particles at 30%, 60%, and 90% relative humidity (RH), over 12 hours; (b) water uptake and corresponding water collected by PAAS-LiCI composites with different thicknesses (here ‘w.u.’ stands for water uptake, and ‘w.c.’ denotes weight change); (c) water uptake of PAAS-LiCI composites coated on a PV panel, under different relative humidity for 12 h at 25°C; (d) 72-hour sorption test of a pre-dried composite; (e) the impact of wind and relative humidity on the water uptake of PAAS-LiCI composite at 30 °C; (f) thermal conductivity of composite after exposed to different relative humidity for 12 hours;
[0031] Figure 7 shows (a) actual (line) solar irradiation and applied (shaded bar) solar irradiation intensity for indoor tests; (b) the temperatures of the PV panels with and without hydrogel under applied solar intensity; (c) weight loss rate and weight change of the cooling layer during the test in hours; (d) a schematic of thermal analysis for the solar cell with composite under the sun; (e) maximum power output point of PV panels with and without composite;
[0032] Figure 8 shows results of indoor experiments of PV modules with (w / ) and without (w / o) hydrogel for cooling from 7:00 to 18:00; (a) temperature of PV modules with / without cooling layer under 0.8, 1.0, and 1.2 times (left to right) of simulated outdoor solar irradiation; (b) weight loss and weight change trend of PV modules with a cooling layer under 0.8, 1.0, and 1.2 times (left to right) of simulated outdoor solar irradiation; (c) Pmax of PV modules with / without cooling layer under 0.8, 1.0, and 1.2 times (left to right) of simulated outdoor solar irradiation;
[0033] Figure 9 shows evaporative cooling power of the composite for a 12-hour indoor experiments of PV module as a function of the hour; (a) cooling power of the composite under 0.8 kW / m2solar irradiation; (b) cooling power of hydrogel under 1.0 kW / m2solar irradiation; (c) cooling power of composite under 1.2 kW / m2solar irradiation;
[0034] Figure 10 shows results of indoor experiments of PV modules with (w / ) and without (w / o) composites over 12 hours of cooling; (a) temperature of PV modules with / without cooling layer under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2(left to right) solar irradiation; (b) weight loss and weight change trend of PV modules with a cooling layer under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2(left to right) solar irradiation; (c) Pmax of PV moduleswith / without cooling layer under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2(left to right) solar irradiation;
[0035] Figure 11 shows results of indoor experiments of PV modules with / without composites over 12 hours of cooling, the open-circuit voltage under (a) 0.8 kW / m2, (b) 1.0 kW / m2, and (c) 1.2 kW / m2solar irradiation; the short-circuit current under (d) 0.8 kW / m2, (e) 1.0 kW / m2, and (f) 1.2 kW / m2solar irradiation; the fill factor of PV modules with / without cooling layer under (g) 0.8 kW / m2, (h) 1.0 kW / m2, and (i) 1.2 kW / m2solar irradiation; (j) vapour pressure of lithium chloride (LiCI) at different mass concentrations;
[0036] Figure 12 shows results of outdoor experiments of continuous cooling cycle from 12 July to 19 July (a) temperature; (b) weight variation; (c) weather conditions (RH and wind speed); (d-f) cooling performance on 16 July, (d) temperature of the PV panel without composite, PV panel with composite, and ambient weather in 24 hours; (e) the Pmax (shaded area) of PV panel with / without cooling layer measured by a PV analyzer; (f) power conversion efficiency (shaded area) and fill factor (line) of PV panel with / without cooling layer; and
[0037] Figure 13 shows additional outdoor experimental results of a continuous cooling cycle over 20 July to 2 August 2022; (a) 13-day temperature trends showing the average noon temperature difference between PV panels with and without the composite cooling layer; (b) weight variation of the cooling layer over 13 days (the values indicated are daily changes in moisture content); (c) weather conditions from 20 July to 28 July, including relative humidity and wind speed.
[0038] Detailed Description
[0039] As explained above, there is a need for an improved composite particularly suitable for, but not limited to, cooling of a PV device, and a method of forming the composite.
[0040] In general terms, the invention relates to an improved composite and a method of forming the same. In particular, the composite may be for, but not limited to, passive cooling of a PV device. Further, the composite of the present invention overcomes the problem of low rate of moisture release for evaporative cooling and has superior mechanical properties.In the present disclosure, the use of the singular includes the plural unless specifically stated otherwise. It should be noted that, as used in the specification and the appended claims, the singular forms “a”, “an” and “the” include plural referents unless the context clearly dictates otherwise. Further, the use of the term “including”, “comprising”, and “having” as well as other forms, such as “include”, “comprise”, “have” are not considered limiting.
[0041] According to a first aspect, there is provided a composite for cooling a photovoltaic (PV) device, wherein the composite comprises a cross-linked network comprising a polyacrylate and a hygroscopic salt. The polyacrylate may comprise any porous crosslinkable acrylic hydrogels and / or superabsorbent polyacrylate networks.
[0042] In the present disclosure, references to a cross-linked network comprising a polyacrylate and a hygroscopic salt refers to a matrix of physical cross-links formed between carboxylate groups of the polyacrylate and cations of the hygroscopic salt. The polymer backbone of the polyacrylate may be composed of saturated carbon chains and carboxylate side groups and thus lacks UV-labile or oxidizable functionalities such as aromatic rings, amides, or esters, and advantageously offers resistance to photodegradation and thermal aging during prolonged exposure.
[0043] The composite of the present aspect allows increase in water storage via the highly hydrophilic carboxylate groups in the polyacrylate polymer backbone, and the hygroscopic salt within the cross-linked network actively absorbs moisture from the environment. Upon water absorption, the composite becomes more adhesive, thus enabling it to be anchored to a PV device for use.
[0044] The polyacrylate may have any suitable average molecular weight to enable formation of the composite and confer water absorption capability. If the average molecular weight is too low, the composite cannot be formed through stirring due to its short molecular chains. Conversely, if the average molecular weight is too high, the water absorption capability of the formed composite is significantly reduced. According to a particular aspect, the polyacrylate may have an average molecular weight of 4-11 million g / mol. In particular, the polyacrylate may have an average molecular weight of 4.5-10.5 million, 5-10 million, 5.5-9.5 million, 6-9 million, 6.5-8.5 million, 7-8 million g / mol. Even more in particular, the polyacrylate may have an average molecular weight of 5-7 million g / mol.The cross-linked network may not comprise a cross-linker. For example, the cross-linked network may contain only physical cross-links between the polyacrylate and the hygroscopic salt, and may not comprise additional covalent cross-linkers, radical initiators, or the like. In this way, the composite advantageously does not contain chemical agents that demand precise handling and pose potential toxicity risks, do not require catalysts or initiators to form the cross-linked network, and is environmentally friendly.
[0045] The polyacrylate and the hygroscopic salt may be present in the composite in any suitable weight ratio. According to a particular aspect, a weight ratio of the polyacrylate and the hygroscopic salt may be 1.5: 1-3: 1. In particular, aweight ratio of the polyacrylate and the hygroscopic salt may be 1.6:1-2.9:1, 1.7:1-2.8:1, 1.8:1-2.7:1, 1.9:1-2.6:1, 2:1-2.5:1, 2.1:1-2.4:1, 2.2:1-2.3:1. Even more in particular, a weight ratio of the polyacrylate and the hygroscopic salt may be 2:1. A higher concentration of hygroscopic salt increases water uptake, however, rate of liquid water mass loss and efficiency of evaporative cooling becomes adversely affected, and because the hygroscopic salt reduces the saturation concentration of the polyacrylate, this in turn affects the stability of the sample and increases the risk of deliquescence. Thus, the present composite advantageously balances water uptake with cooling performance and stability.
[0046] The polyacrylate may be any suitable polyacrylate. For example, the polyacrylate may be, but is not limited to, any porous cross-linkable acrylic hydrogels. For example, the polyacrylate may comprise sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, ammonium polyacrylate, or a combination thereof. In particular, the polyacrylate may comprise sodium polyacrylate. The hygroscopic salt may be any suitable hygroscopic salt. For example, the hygroscopic salt may be, but is not limited to, a lithium salt, a chloride salt, or a combination thereof. The hygroscopic salt may comprise lithium chloride, lithium bromide, lithium nitrate, sodium chloride, calcium chloride, magnesium chloride, or a combination thereof. In particular, the hygroscopic salt may comprise lithium chloride.
[0047] The composite may have any suitable thickness. For example, the composite may have a thickness of 1-10 mm. In particular, the composite may have a thickness of 2-9, 3-8, 4-7, 5-6 mm. Even more in particular, the composite may have a thickness of 7 mm.The composite may have superior water uptake at different relative humidity levels. According to a particular aspect, the composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30%. In particular, the composite may have a water uptake of > 0.55, > 0.60, > 0.65 g / g at a relative humidity of > 30%. Even more in particular, the composite may have a water uptake of > 0.65 g / g at a relative humidity of > 30%. Thus, the composite advantageously retains substantial moisture absorption capability even under relatively low-humidity conditions.
[0048] At a relative humidity of > 60%, the composite may have a water uptake of > 1.0 g / g. In particular, the composite may have a water uptake of > 1.05, > 1.10, > 1.15, > 1.20, > 1.25 g / g at a relative humidity of > 60%. Even more in particular, the composite may have a water uptake of > 1.25 g / g at a relative humidity of > 60%.
[0049] At a relative humidity of > 90%, the composite may have a water uptake of > 2.0 g / g. In particular, the composite may have a water uptake of > 2.05, > 2.10, > 2.15, > 2.20, > 2.25, > 2.30, > 2.35 g / g at a relative humidity of > 90%. Even more in particular, the composite may have a water uptake of > 2.35 g / g at a relative humidity of > 90%.
[0050] Thus, the present composite advantageously increases water uptake across different humidity levels, for effective evaporative cooling in different climates.
[0051] The composite may have superior thermal conductivity. For example, the composite may have a thermal conductivity of > 0.435 W / (m K). In particular, the composite may have a thermal conductivity of > 0.440, > 0.445, > 0.450, > 0.455, > 0.460, > 0.465, > 0.470 W / (m K). Even more in particular, the composite may have a thermal conductivity of > 0.470 W / (m K).
[0052] The composite may have an improved cooling power. The composite may have a cooling power of > 140 W / m2. In particular, the composite may have a cooling power of > 145, > 155, > 165, > 175, > 185, > 195, > 205, > 215, > 225, > 235, > 245, > 255, > 265, > 275, > 285, > 295, > 305, > 315, > 325, > 335, > 345, > 355, > 365, > 375 W / m2. Even more in particular, the composite may have a cooling power of > 375 W / m2.
[0053] To ensure optimal cooling of PVs when the composite is in use, maintaining a consistent evaporation rate to release moisture throughout the daytime period is crucial. Thus, according to a particular aspect, in use, the composite may provide a rate of liquid watermass loss of > 0.5 kg / (m2h). In particular, the composite may have a rate of liquid water mass loss of 0.6-0.85 kg / (m2h). Even more in particular, the composite may have a rate of liquid water mass loss of 0.7-0.8 kg / (m2h). The composite may have a liquid water mass loss of 6-8 g during daytime, and moisture absorption of 6.5-8.5g during nighttime.
[0054] The greater the liquid water mass loss rate, the greater the temperature reduction. In use, the composite may be capable of reducing temperature of the PV device by > 9 °C. In particular, the composite may be capable of reducing temperature of the PV device by > 10, > 11, > 12, > 13, > 14, > 15 °C when in use. Even more in particular, the composite may be capable of reducing temperature of the PV device by > 15 °C when in use.
[0055] The composite may have long-term stability and durability and maintain superior performance over long-term use, in all types of climate conditions. For example, the composite may maintain water uptake, cooling power, size and weight, over prolonged periods of use in various weather.
[0056] The composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 3 weeks of use. In particular, the composite may have a water uptake of > 0.55, > 0.60, > 0.65 g / g at a relative humidity of > 30% after > 3 weeks of use. Even more in particular, the composite may have a water uptake of > 0.65 g / g at a relative humidity of > 30% after > 3 weeks of use.
[0057] Further, the composite may have a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 12 months of use. In particular, the composite may have a water uptake of > 0.55, > 0.60, > 0.65 g / g at a relative humidity of > 30% after > 12 months of use. Even more in particular, the composite may have a water uptake of > 0.65 g / g at a relative humidity of > 30% after > 12 months of use. Thus, the composite advantageously maintains maintain superior performance over long-term use.
[0058] According to a second aspect, there is provided a method of forming the composite according to the first aspect, the method comprising:
[0059] mixing a polyacrylate and a solution of a hygroscopic salt, to form a mixture; and
[0060] curing the mixture to form the composite.
[0061] The composite may be as described above.The method may further comprise pouring the mixture into a suitable vessel for the curing to occur. The vessel may be selected based on suitability of dimensions (length, breadth, and height) for the composite to be formed.
[0062] According to a particular aspect, the curing may be for 3-60 minutes. In particular, the curing may be for 5-55, 10-50, 15-45, 20-40, 25-35 minutes. Even more in particular, the curing may be for 60 minutes. The curing may be at a temperature of 20-25 °C. In particular, the curing may be at a temperature of 21-24, 22-23 °C. Even more in particular, the curing may be at a temperature of 25 °C. Thus, the method is advantageously quick and may be performed at room temperature without requiring external energy sources for heating.
[0063] The method may not comprise adding a cross-linker. In this way, the method is advantageously simple, without the need for adding catalysts, initiators, nor UV and thermal curing steps.
[0064] According to a particular aspect, the mixture may comprise the polyacrylate and the hygroscopic salt at a weight ratio of 1.5: 1-3:1. In particular, the mixture may comprise the polyacrylate and the hygroscopic salt at a weight ratio of 1.6: 1-2.9:1, 1.7: 1-2.8:1, 1.8:1-2.7:1, 1.9:1-2.6:1, 2:1-2.5:1, 2.1:1-2.4:1, 2.2:1-2.3:1. Even more in particular, a weight ratio of the polyacrylate and the hygroscopic salt may be 2:1.
[0065] Having now generally described the invention, the same will be more readily understood through reference to the following embodiment which is provided by way of illustration, and is not intended to be limiting.
[0066] Examples
[0067] Materials and methods
[0068] Synthesis of PAA S-LiCI composite
[0069] A schematic of the composite used in this Example is shown in Figure 1, in which LiCI was used as the hygroscopic agent, and a crosslink network of PAAS was used as the matrix for the holding of LiCI and water.Lithium chloride (LiCI) was dissolved in deionized water at a weight ratio of 1:1.5. The solution was stirred until fully homogenized. Thereafter, sodium polyacrylate (PAAS) powder was added, in a PAAS: LiCI mass ratio of 2:1. The resulting mixture was gently stirred for approximately 3 minutes. The hydrogel was then cast into a mold and compressed to achieve a flat shape and left to cure naturally for one hour.
[0070] Three sets of composites were formed using the same method as described above, with different average molecular weights of PAAS at 0.15 million, 5-7 million, or 12 million g / mol.
[0071] For comparison, another set of composite was formed using the same method as described above, with PAAS at an average molecular weight of 5-7 million g / mol and PAAS: LiCI mass ratio of 1:1.
[0072] Further, three additional sets of composites were formed with thicknesses varied at 1.5 mm, 3 mm, and 7 mm. The average molecular weight of the PAAS was 5-7 million g / mol, and the PAAS: LiCI mass ratio was 2:1.
[0073] PAAS-LiCI composite coated on a PV panel
[0074] A polycrystalline silicon PV panel measuring 54 mm x 54 mm (AOSHIKE® 2V 130mA Solar Panels) was used, and a PAAS-LiCI composite material was formed matching these dimensions, featuring a thickness of 7 mm before moisture absorption. The weight of the composite was recorded at approximately 24 g, with a variance of ± 1.7 g. the composite-coated PV panel was used for water uptake tests, indoor cooling performance tests, and outdoor long-term cooling performance tests.
[0075] Characterisation and results
[0076] Scanning electron microscopy (SEM)
[0077] The PAAS-LiCI composite samples were dried at 80°C for 12 hours prior to imaging, to remove absorbed moisture and to preserve the porous morphology. Imaging was performed using a field-emission scanning electron microscope. The dry composite was mounted on aluminium stubs and sputter-coated with a thin layer of gold / palladium to prevent charging. Secondary electron imaging was used to visualize the pore structure and LiCI crystal distribution. Representative images were captured at magnificationsspanning 500x to 5000x to characterise the overall pore network and the individual LiCI crystallite morphology.
[0078] As shown in Figure 2(a), the composite material prepared using PAAS with an average molecular weight of 0.15 million comprised many independent particles and did not have a defined shape. The composite material prepared using PAAS with an average molecular weight of 5-7 million was well-formed and had a defined porosity (Figure 2(b)). As shown in Figure 2(c), although the composite material prepared using PAAS with an average molecular weight of 12 million molecular weight was successfully formed, the surface voids were largely blocked, which was not conducive to water absorption.
[0079] PAAS with an average molecular weight between 5-7 million entangled with each other to form a three-dimensional network in the solution, which improved the stability of the complexes, and at the same time synergistically endowed the gels with good mechanical properties due to the presence of hydrogen and ionic bonds in the PAAS macromolecules. Meanwhile, when the average molecular weight is too low, such as 0.15 million, the prepared complexes cannot even be successfully prepared, and when the average molecular weight is too high, an excess of entanglement nodes were formed, which decreases the porosity of hydrogel and limits the moisture absorption efficiency of LiCI. Thus, PAAS with an average molecular weight between 5-7 million g / mol was used for further experiments.
[0080] As seen in Figure 3, a porous structure densely populated with clusters of LiCI crystals intricately distributed and securely anchored within the PAAS framework was formed. The crystalline particles exhibited an average diameter spanning from hundreds of nanometers to several micrometers, while the pore diameters varied from a few micrometers to more than ten micrometers.
[0081] X-ray diffraction (XRD) analysis
[0082] X-ray diffraction analysis was conducted on dry composite samples and reference materials (PAAS powder, LiCI powder, and PAAS-LiCI composite) using a powder X-ray diffractometer with Cu Ka radiation (A = 0.15406 nm), scanning from 20 = 10° to 80° at a scan rate of 27min.As seen in Figure 4, XRD analysis shows characteristic LiCI diffraction peaks identified and confirmed in the composite pattern, verifying the integration of LiCI crystals within the PAAS matrix.
[0083] The PAAS-only XRD pattern (not shown) had broad amorphous scattering as expected for a high-molecular-weight polymer.
[0084] Mechanical tests
[0085] A series of mechanical and adhesion tests were performed, including strength-strain tests before and after moisture absorption, and adhesion tests in two directions (perpendicular to the panel, and parallel to the panel).
[0086] Dumbbell-shaped specimens were cut from the respective dry and moisture-saturated PAAS-LiCI composites using a standard tensile test die. Tests were performed on a universal testing machine (UTM) at a constant crosshead speed of 50 mm / min at room temperature. Load-displacement data were converted to stress-strain curves. Tests were repeated in triplicate.
[0087] As shown in Figure 5(a), when the PAAS-LiCI hydrogel was tested both before and after moisture absorption, due to strong cross-linking within the hydrogel, excellent mechanical integrity was maintained under operational conditions, thus ensuring longterm shape retention.
[0088] To demonstrate the adhesive force between the hydrogel and the solar panel, tensile tests were further conducted, in two directions:
[0089] (i) Perpendicular to the panel: As shown in Figure 5(b), a force of 14.2 N was required to separate the hydrogel, which weighed around 26.8 g. This force is hundreds of times greater than the gravitational weight of the hydrogel, ensuring that there is strong adhesion to the rear surface of the PV panel.
[0090] (ii) Parallel to the panel: As shown in Figure 5(c), the force required to separate the hydrogel in the parallel direction was at least 12.1 N. To provide context, even in hurricane conditions with wind speeds exceeding 118 km / h, the calculated wind force on the hydrogel was only 0.353 N. This force is tens of times lower than the tolerated force.These results confirm that the hydrogel exhibited exceptional mechanical stability and strong adhesion, attributed to mechanisms such as hydrogen bonding and capillary forces from water molecules. Thus, durability and reliable attachment to solar panels in outdoor environments is ensured.
[0091] Optimal ratio of PAAS:LiCI
[0092] Increasing the ratio of LiCI to PAAS enhanced the moisture collection property of the PAAS-LiCI composite. When the weight ratio of PAAS: LiCI was varied, from 2:1 to 1:1, the 12-hour water uptake of the composite increased from 0.53 g / g to 0.74 g / g. However, a higher concentration of LiCI in the composite also increased the likelihood of deliquescence. This deliquescence phenomenon was detected in an environment even with lower relative humidity (-60% RH). Thus, to balance between water uptake performance and longevity of the composite, the optimal ratio of PAAS: LiCI was determined to be 2:1, and composites with this weight ratio were used for further experiments.
[0093] Water uptake test
[0094] A sequence of water vapor absorption performance tests was conducted within a regulated indoor setting to measure the water uptake of 1 gram of PAAS, PAAS-LiCI (weight ratio of 2:1), and LiCI particles, at 30%, 60%, and 90% relative humidity (RH), over 12 hours (Figure 6(a)). While pure LiCI salt had the best performance in moisture absorption capability, LiCI dissolved upon moisture uptake even at lower humidity levels, resulting in a solution with low viscosity that lacked the ability to adhere to the rear surface of solar panels directly. On the other hand, while pure PAAS exhibited robust water retention capabilities, the ability for direct moisture absorption from the air is comparatively limited. Thus, the introduction of LiCI into PAAS at a weight ratio of 1:2 significantly increased the 12-hour water uptake of PAAS from 0.11, 0.22, and 0.94 g / g to 0.68, 1.28, and 2.34 g / g at relative humidity of 30%, 60%, and 90%, respectively. The PAAS-LiCI composite therefore leveraged the advantages of both materials and overcome the weakness (i.e. , no solution leakage under high humidity environment).
[0095] Additional experiments were conducted to test the water absorption of PAAS-LiCI composites of varying thicknesses, under different humidity levels, as shown in Figure 6(b). The composites with reduced thickness demonstrated higher water uptake,whereas those with increased thickness showed a faster rate of water absorption. Specifically, a composite of 7 mm thickness absorbed 3.85 g of water, escalating its mass from 12.72 g to 16.55 g and thickness from 7 mm to 10 mm, which translates to a water uptake ratio of 0.30 g / g.
[0096] Sorption dynamics of the composite-coated PV panel were analyzed at a stable temperature of 25 °C, as depicted in Figure 6(c), revealing a pronounced relationship between the RH levels and the pace of moisture absorption. The maximal water uptake was noted at 100% RH, amounting to about 0.23 g / g, which is equivalent to a water collection capacity of roughly 5.8 g.
[0097] In a separate test, the PAAS-LiCI composite was pre-dried in an oven at 80°C for 12 hours to determine its maximum water uptake capacity, as shown in Figure 6(d). The absorption test was conducted at 25°C with 90% RH. The pre-dried composite exhibited a water uptake of approximately 0.53 g / g and the corresponding accumulative water uptake was 8.28 g. Extending the observation period from 12 to 72 hours showed that the initial absorption rates were notably high but tapered off over time, culminating in a water uptake ratio of 1.77 g / g, equivalent to a total water collection of around 27.7 g.
[0098] Testing was also done to examine the impact of wind in outdoor environments and the typically higher RH levels during the night, based on the outdoor environment conditions during the night in hot and arid climates like Saudi Arabia. A controlled airflow was introduced near the sample, with a velocity of approximately 1 m / s, which brought more humid air into contact with the sample, thereby improving the efficiency of moisture absorption. The temperature of the experimental environment was raised to 30 °C, which is similar to that of Saudi Arabia at night (29.9 °C, as measured in July 2022). The water uptake of PAAS-LiCI composites under different weather conditions was measured, the results of which are shown in Figure 6(e). There was a significant enhancement in the water absorption rates of the composite with increasing RH and the introduction of wind. At 60% RH, the introduction of wind raised the water uptake from 0.08 g / g to 0.15 g / g, resulting in a total moisture absorption of 3.5 g. When the RH was elevated to 75%, the water uptake surged from 0.14 g / g to 0.27 g / g, with the composite absorbing 6.1 g of water. At the highest tested humidity level of 90% RH, the water uptake jumped from 0.22 g / g to 0.42 g / g, leading to a significant increase in water absorption to 10.8 g.To ascertain that the incorporation of water does not adversely affect the thermal efficiency of the composites, a detailed investigation of the thermal conductivity was measured using a Hot Disk® Thermal Constants Analyzer. As shown in Figure 6(f), the baseline thermal conductivity of the composite was 0.455 W / (m K). After subjecting the samples to RH levels of 20%, 60%, 75%, and 90% for 12 hours, the thermal conductivities were observed to be 0.438, 0.463, 0.468, and 0.470 W / (nr K), respectively. This suggests a gradual increase in thermal conductivity corresponding with the rise in moisture content. Thus, environmental factors such as wind and humidity are critical in optimising the water absorption capabilities of the composite material, presenting a significant advancement in the application of such materials for PV cooling.
[0099] Indoor cooling performance
[0100] The cooling performance of the composite-coated PV panel was first assessed in a controlled indoor setting. A commercial solar simulator was used to replicate sunlight exposure. First, the composite was conditioned under environmental parameters of 90% RH, a room temperature of 25°C, and an airflow of 1 m / s for 12 hours. The composite had a thickness of 1 cm post-moisture absorption, and dimensions of 54 mm x 54 mm. The experimental setup contains a single PV panel without the composite coating, and one with the PAAS-LiCI composite coating (i.e. , the cooling layer) attached at the rear surface. The solar panel was mounted on a fixed bracket and placed on a high-precision electronic scale, with the entire setup situated beneath the solar simulator. A thermocouple was positioned at the center of the panel's rear side to monitor temperature variations, while a solar analyzer was connected to the panel to record output changes, such as Pmax. To mimic the outdoor solar illumination condition, the solar irradiance curve was recorded on 17 July 2022, on the campus of KALIST, and mapped in Figure 7(a). This averaged light intensity was then utilised as the baseline for the solar simulator, to better evaluate the performance of the cooling layer on the temperature of the solar panel throughout the day under simulated outdoor conditions. Infrared (IR) images captured (not shown) the temperature of the operational solar panel near noon, with the average surface temperature of the panel equipped with the cooling layer being 10.3°C lower than that of the panel without cooling layer (reduced from an average of 65.3°C to 55.0°C).
[0101] Figure 7(b) shows a comparison of the hourly temperatures of a PV panel without composite coating and the same PV panel equipped with the composite as cooling layer.The introduction of the cooling layer markedly improved the temperature regulation of the PV panel. At the beginning of the experiment, which simulated morning solar radiation, the cooling layer led to a temperature decrease of about 4.7°C. As the light intensity increased, so did the temperature of the panel. Notably, during peak solar radiation between 10:00 AM and 11 :00 AM, the panel with the cooling layer experienced a significant temperature reduction of approximately 11 ,8°C, from 53.3°C to 41 ,5°C. The performance of the cooling layer varied throughout the day. In the early morning (8:00 AM to 9:00 AM) with an average light intensity of 364 W / m2, the temperature decreased by about 9.6°C. This cooling effect ranged between 8.3°C and 11.7°C under peak sunlight conditions (800 to 1000 W / m2). However, in the late afternoon (16:00 to 17:00), with light intensity at 485 W / m2, the effect diminished to around 5.9°C, correlating with reduced water content in the composite.
[0102] This trend mirrors the changes in weight of the cooling layer, depicted in Figure 7(c). Early in the morning (8:00 AM to 9:00 AM), 0.91 g of water evaporated from the cooling layer, whereas in the afternoon (15:00 to 16:00), the evaporation decreased to 0.40 g, despite higher light intensity and temperature. The highest evaporation rate of 1.06 g / h occurred between 10:00 and 11:00. The cooling process relies on enthalpy of vaporization of water, described by the equation:
[0103] p ^HvapXLm LHvap Lm
[0104] r — — X — ( J )
[0105]
[0106] AtxA A Lt '
[0107] where AHvaprepresents the enthalpy of vaporization of water at room temperature, specifically 2,450 J / g, A is the surface area of the composite material connected to the PV panel, and is the rate of mass loss.
[0108]
[0109] Throughout the experiment, the average cooling power was around 160 W / m2, peaking at approximately 247 W / m2between 10:00 AM and 11:00 AM. To validate the thermal experimental findings, a comprehensive thermal analysis of the solar cell was conducted using COMSOL Multiphysics, incorporating both radiative and non-radiative heat transfer processes (Figure 7(d)). Simulations were performed under solar irradiation conditions from 10:00 AM to 11:00 AM (725 W / m2), with an evaporative cooling power of 247 W / m2. The simulated results demonstrate a temperature reduction of 11.2°C (54.5°C vs.
[0110] 43.3°C) due to the presence of the cooling layer, aligning closely with the experimentalmeasurements, which showed a temperature reduction of 11.8°C (53.3°C vs. 41.5°C). This consistency between experimental and simulated results validates the accuracy of the thermal experimental results.
[0111] The evaporative cooling effect significantly boosted the performance of the PV panel, as shown in Figure 7(e). The addition of the cooling layer resulted in a substantial increase in power output during the morning hours (8:00 AM to 9:00 AM), with an enhancement from 96.1 mW to 104.8 mW, marking a 9.1% improvement. Moreover, in the critical midday period under peak solar intensity (11:00 to 15:00), the maximum output power (Pmax) increased significantly by 10.0%, averaging from 145.4 mW to 160 mW. This improvement demonstrates effectiveness of the composite in significantly boosting the cooling effect and thus the operational efficiency of the PV panel during periods of high solar irradiance.
[0112] To further evaluate the effectiveness of the composite under different irradiation conditions, additional experiments were conducted, demonstrating that the composite provides effective cooling performance suitable for global deployment across regions with varying irradiation conditions.
[0113] Considering the solar irradiation difference in various latitudes, simulation results under 0.8 times, 1.0 times, and 1.2 times of the actual solar irradiation were investigated. The overall results under all conditions are shown in Figure 8, in which the results under 0.8 times, 1.0 times, and 1.2 times solar irradiation are shown from left to right. The corresponding peak temperature reduction of the cooling layer in one hour was 11.75 °C (46.44 °C for the control PV module and 34.69 °C for the PV module with composite), 11.79 °C (53.28 °C for the control PV module and 41.48 °C for the PV module with composite), and 12.64 °C (58.14 °C for the control PV module and 45.5 °C for the PV module with composite), all of which were located in the period between 10:00 and 11:00 (Figure 8(a)). The corresponding weight loss during that period is 1.06g, 1.06g, and 1.19g, and the overall weight loss during the simulated daytime test is 7.43g, 7.52g, and 8.36g (Figure 8(b)). The maximum cooling powers observed under solar radiance conditions of 0.8 times, 1 time, and 1.2 times of the applied solar irradiation between 10:00 and 11:00 were 247 W / m2, 247 W / m2, and 278 W / m2, respectively. The corresponding average cooling powers during the test were approximately 158 W / m2, 160 W / m2, and 177 W / m2, respectively. Thus, it can be seen that the increase of solarirradiation on the PV module increased the temperature of PV modules, which, on the other hand, resulted in an increasing evaporation rate and temperature reduction. Figure 8(c) shows the maximum power output (Pmax) for each pair of tests. Between 10:00 and 11:00, the average Pmax values of the PV modules with the samples were 117 mW, 153 mW, and 182 mW, corresponding to enhancements of 4%, 10%, and 5%, respectively, compared to the control modules without cooling (112 mW, 139 mW, and 173 mW). A portion of the results is summarized in Table 1. The results of the cooling power under 0.8 times, 1.0 times, and 1.2 times solar irradiation are shown in Figure 9(a), Figure 9(b), and Figure 9(c), respectively.
[0114] The simulation results under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2constant solar irradiation was investigated and the experiments above repeated. The overall results of all conditions are shown in Figure 10. In the experiment conducted under 1.0 kW / m2constant solar radiation, the cooling layer supported a cooling power of 373 W / m2during the first 3 hours, which decreased to 187 W / m2after extending the working period to 12 hours. This resulted in an average temperature reduction of 12.8 °C and 8.7 °C, respectively. Similar to Figure 8, the results of Figure 10 under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2constant solar irradiation are shown from left to right. Considering that the curves of temperature started to stabilize after two hours, the results in the first 2 hours were not included in the calculation. During these experiments, where solar irradiation remains constant, the cooling powers observed under different levels of sun radiance (0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2) after 2 hours were estimated to be 124 W / m2, 136 W / m2, and 131 W / m2, respectively. To facilitate comparison, a summary of all results from Figures 8 and 10 is provided in Table 1 below.Time-varying solar irradiation, Constant solar irradiation,
[0115] 10:C 10-11:00 2h~12h
[0116] Design &
[0117] Temperature Weight P max Temperature Weight P max Times of Solar
[0118] (°C) loss (g) (mW) (°C) loss (g) (mW) Irradiation
[0119] w / o hydrogel,
[0120] 46.44 - 112 63.56 - 161 0.8
[0121] w / hydrogel, 34.69 117 56.26 170
[0122] 1.06 5.312
[0123] 0.8 (-11.75) (+5%) (-7.3) (+6%) w / o hydrogel,
[0124] 53.28 - 139 70.31 - 182 1.0
[0125] w / hydrogel, 41.48 153 62.7 191
[0126] 1.06 5.845
[0127] 1.0 (-11.8) (+10%) (-7.61) (+5%) w / o hydrogel,
[0128] 58.14 - 173 77.95 - 203 1.2
[0129] w / hydrogel, 45.5 182 64.85 219
[0130] 1.19 5.63
[0131]
[0132] 1.2 (-12.64) (+5%) (-13.1) (8%) * The values in parentheses are the difference from the data in the corresponding variable above.
[0133] Table 1 : Cooling performance of indoor experiments
[0134] Other characteristics used to rate the output performance of PV modules were investigated, and the results are shown in Figure 11. Figures 11(a)-(c) show the opencircuit voltage of PV modules under 0.8 kW / m2, 1.0 kW / m2, and 1.2 kW / m2constant solar irradiation, and Figures 11 (d)-(f) and (g)-(i) show the corresponding short-circuit current and fill factor, respectively. Thus, it can be seen that the impact on performance of PV modules with or without a cooling sample on lscis comparable. The FF was slightly higher, and Vocvaried significantly. The results aligned with the conclusion that reduced operating temperatures contributed to higher output voltage values. The power conversion efficiency (PCE) was calculated using the Pmaxfrorn Table 1, and the results are summarised in Table 2.
[0135] Design & Times of
[0136] Voc(V) lsc (A) FF(%) PCE (%) Solar Irradiation
[0137] w / o hydrogel, 0.8 2.11 0.106 71.8 10.0 w / hydrogel, 0.8 2.18 (+0.07) 0.108 72.3 (+0.5) 10.5 w / o hydrogel, 1.0 2.08 0.129 67.5 9.0 w / hydrogel, 1.0 2.13 (+0.05) 0.132 67.7 (+0.2) 9.4 w / o hydrogel, 1.2 2.05 0.160 62.0 8.4
[0138]
[0139] w / hydrogel, 1.2 2.15 (+0.10) 0.159 64.2 (+2.2) 9.0 *The values in parentheses are the difference from the data in the corresponding variable above.
[0140] Table 2: Additional output performance results of indoor experimentsAdditional cooling power tests were conducted, under a solar simulator set at an irradiance of 1000 W / m2for 3 hours. The composite showed an evaporative rate of 0.55 kg / (m2h). The effectiveness of evaporative cooling was directly correlated with the rate of liquid water mass loss, as described in Equation (1), and in brief, the faster the evaporative rate, the greater the temperature reduction. Thus, moisture capture capacity, while being a common parameter used to assess the potential of evaporative cooling, does not provide a complete picture. The moisture capture capacity may be enhanced by incorporating hygroscopic agents like LiCI or CaCh into the composite, however, higher content of hygroscopic agents led to a lower evaporative rate, as indicated by the lower vapor pressure (Figure 11(j)). This lower vapour pressure meant that fewer molecules had sufficient energy to undergo the transition from liquid to gas phase, thus diminishing the evaporation rate and leading to lower efficiency in temperature reduction. In addition, a higher concentration of hygroscopic agent introduces more ions like Li+and Ca2+, which replaced part of the Na+in sodium polyacrylate, and reduced the saturation concentration of sodium polyacrylate. This, in turn, affected the stability of the sample and increased the risk of deliquescence. Therefore, the present composite was finely tuned in terms of the ratio of PAAS: LiCI to balance the trade-off between water uptake and evaporative rate.
[0141] Long-term outdoor cooling performance (3 weeks)
[0142] To evaluate the effectiveness of the PAAS-LiCI composite in real-world conditions, an outdoor experiment was conducted at the KALIST campus (Thuwal, 37°C and 53% relative humidity during daytime). The experiment was conducted using two similar PV panels, one with the cooling layer applied, and the other without, and situated in Saudi Arabia at the coordinates 22°19’06.1”N, 39°06’15.0”E. From 12 July to 2 August 2022, a 21-day trial was conducted under ambient temperatures ranging from 25 °C to 41 °C, with the attached solar cells reaching an operating temperature of 51 °C. The results showed continuous cooling of the solar cells without requiring maintenance.
[0143] As shown in Figure 12(a), over the first week, the temperature differences between these panels and the ambient environment confirmed the autonomous cooling capability of the composite. A notable temperature reduction of 14.1 °C was achieved on 16 July, with an average decrease of 7.8°C observed daily from 7:30 to 17:30 throughout the entire experiment period. The daily water evaporation averaged at approximately 6.1 g with apeak value of 7.5 g on 16 July, translating to a cooling power of 141 W / m2and 175 W / m2as per Equation (1). The weight fluctuations of the cooling layer, outlined in Figure 12(b), indicated the ability of the composite to absorb water at night and evaporate it during the day, a process crucial for its cooling function. Throughout this 7-day period, the weight loss occurred nearly linearly as a function of time each day, indicating stable and sustained daily water evaporation. This confirms that the water stored in the composite was gradually released over the entire daytime. Notably, the maximum evaporation in the daytime during this period reached 7.5 g, while the maximum moisture absorption overnight was 7.6 g. This ability of the composite to rehydrate ensures the sustainability of the cooling effect, validating the practical applicability and effectiveness of the composite in real-world solar panel installations. The composite was capable of undergoing a reversible water absorption-evaporation cycle. Throughout the outdoor test, the cooling layer remained intact, showing no evidence of wear, separation, or damage, affirming its durability and potential for prolonged, low maintenance usage. The visual comparisons in Figure 12(b) (with insets showing days 1 and 7) show the consistent hydration and dehydration states of the cooling film, further attesting to the reliability and effectiveness of the composite. Further, as the composite was applied to the rear surface of the solar panel, which faces away from the sun, direct light exposure is significantly reduced. This minimised potential impact on the composite.
[0144] As shown in Figure 12(c), with nighttime relative humidity frequently exceeding 85% (averaging about 75%), there was ample atmospheric moisture available for the composite to replenish water content overnight, allowing effective evaporative cooling the following day. The average wind speed was 1.0 m / s, promoting efficient heat and moisture dissipation. The airflow at this rate was sufficient to transport over 900 g of moisture per day to the composite surface, enhancing the rehydration capability of the composite.
[0145] To elucidate the advantages brought forth by the cooling effect, an in-depth characterization of the PV panel performance was performed, focusing on the period between 6:00 AM on 16 July and 6:00 AM on 17 July, which had the daily highest evaporative cooling power. As depicted in Figure 12(d), the PV panel equipped with a cooling layer demonstrated a significant average temperature reduction of 9.4°C over the 10-hour period, compared to a similar PV panel lacking the cooling composite. The most pronounced temperature drop was recorded between 12:00 PM and 1:00 PM, withan average decrease of 12.5°C (from 54.9°C down to 42.4°C, with peaks reaching a 14.1 °C reduction) amidst an ambient temperature of 38.0°C. Further analysis revealed enhancements in PV panel performance due to the cooling layer, as illustrated in Figures 12(e) and 12(f). The greatest disparity in performance occurred during midday and early afternoon, especially between 12:00 PM and 1:00 PM. Figure 12(e) shows that the maximum power output (Pmax) of the PV panel without a cooling layer stood at 140 mW around midday. Conversely, the inclusion of a cooling layer increased the Pmax to 158 mW during the same period, marking a noteworthy enhancement of 12.9%. This trend of improvement was consistent across other performance metrics such as power conversion efficiency and fill factor, as detailed in Figure 12(f). The PV panels without and with the cooling layer reached peak efficiencies of 13.1% and 14.7%, respectively, reflecting a 12.2% improvement (with an average daytime increase of 10.2%). The fill factor (FF) during daylight was 0.74 for the control panel, compared to 0.78 for the panel incorporating the cooling layer.
[0146] This outdoor experiment results demonstrate the efficacy of the evaporative process enabled by the PAAS-LiCI composite cooling layer in reducing peak daytime temperatures. The dynamic absorption and desorption cycles within the cooling layer play a crucial role in providing consistent and effective cooling to the photovoltaic system, thereby enhancing its operational efficiency over the long term. Such improvements translate into significant mitigation of performance degradation typically induced by excessive heat in PV panels.
[0147] During this 21-day test in Thuwal, Saudi Arabia, where solar radiation exceeded 1000 W / m2at noon, the hydrogel consistently demonstrated continuous cooling performance (Figure 13). The effects of light exposure on the hydrogel were negligible. As seen in Figure 13(a), the average noon temperature of PV panels with the composite cooling layer consistently remained lower than those without the composite. Figure 13(b) shows daily changes in moisture content, with a consistent trend over the entire period. These results were consistent with the molecular-level design of the PAAS-LiCI hydrogel, which confers excellent long-term stability under harsh environmental conditions. Specifically, LiCI forms stable hydration shells (e.g., [Li(H2O)x]+) that reduce water vapor pressure and enable persistent moisture retention even in hot and arid climates. In parallel, dynamic ionic coordination between Li+ions and the carboxylate groups of PAAS leads to a physically cross-linked yet reconfigurable network that maintains mechanicalintegrity under environmental fluctuations. Furthermore, the PAAS backbone, which is composed of saturated carbon chains and carboxylate side groups, lacks UV-labile or oxidizable functionalities such as aromatic rings, amides, or esters, offering inherent resistance to photodegradation and thermal aging during prolonged exposure. Figure 13(c) shows the weather conditions from 20 July to 28 July, including relative humidity and wind speed.
[0148] Long-term outdoor cooling performance ( 1 year)
[0149] To evaluate long-term stability, the composite-coated solar panel was tested over a one-year period (July 2023 to July 2024) in Buffalo, USA. The testing included one month of outdoor exposure, during which it withstood two weeks of intense rainfall, followed by eleven months of indoor testing. Even after a series of intense rainfall events, the sample remained firmly attached to the rear surface of the solar panel with no visible signs of detachment. After 12 months, the sample continued to function effectively and remained securely attached to the solar cell. Due to the sticky surface of the composite following moisture absorption, dust or grass particles may be attached to the surface. However, since these particles are considerably larger than moisture, their presence did not significantly impact the moisture absorption performance of the composite. In particular, water uptake was 0.53 g / g for the unused sample, and 0.50 g / g for the sample used for the one-year testing. Additionally, after one year, the composite retained over 90% of its original material (dry weight reduced from 18.0 g to 16.8 g), demonstrating excellent durability over prolonged use. Further investigations revealed that even if the sample is immersed in water at room temperature for 72 hours, its structure can remain relatively stable.
[0150] To further mitigate the effect of dust or rain, a superhydrophobic yet breathable membrane may be integrated, which would allow moisture to pass through while blocking dust and rain droplets, ensuring the hydrogel remains clean and functional. Furthermore, the composite may be recycled, further enhancing its overall sustainability. As the composite was physically cross-linked without relying on cross-linking agents, the used samples were successfully recycled and reshaped at elevated temperature (80 °C), significantly extending the material lifespan and reducing associated costs. When immersed in water and heated above 80 °C for a sufficient duration, the compositegradually dissolved (especially when subjected to stirring), thereby facilitating its recycling and reuse.
[0151] Whilst the foregoing description has described exemplary embodiments, it will be understood by those skilled in the technology concerned that many variations may be made without departing from the present invention.
Claims
Claims1. A composite for cooling a photovoltaic (PV) device, wherein the composite comprises a cross-linked network comprising a polyacrylate and a hygroscopic salt.
2. The composite according to claim 1, wherein average molecular weight of the polyacrylate is 4-11 million g / mol.
3. The composite according to claim 1 or 2, wherein the cross-linked network does not comprise a cross-linker.
4. The composite according to any preceding claim, wherein a weight ratio of the polyacrylate and the hygroscopic salt is 1.5: 1-3:1.
5. The composite according to any preceding claim, wherein the polyacrylate comprises sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, ammonium polyacrylate, or a combination thereof.
6. The composite according to any preceding claim, wherein the hygroscopic salt comprises lithium chloride, lithium bromide, lithium nitrate, sodium chloride, calcium chloride, magnesium chloride, or a combination thereof.
7. The composite according to any preceding claim, wherein the composite has a water uptake of > 0.5 g / g at a relative humidity of > 30%.
8. The composite according to any preceding claim, wherein the composite has a thermal conductivity of > 0.435 W / (m K).
9. The composite according to any preceding claim, wherein the composite has a cooling power of > 140 W / m2.
10. The composite according to any preceding claim, wherein in use, the composite provides a rate of liquid water mass loss of > 0.5 kg / (m2h).
11. The composite according to any preceding claim, wherein in use, the composite is capable of reducing temperature of the PV device by > 9 °C.
12. The composite according to any preceding claim, wherein the composite has a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 3 weeks of use13. The composite according to any preceding claim, wherein the composite has a water uptake of > 0.5 g / g at a relative humidity of > 30% after > 12 months of use14. A method of forming the composite according to any of claims 1-13, the method comprising:mixing a polyacrylate and a solution of a hygroscopic salt, to form a mixture; andcuring the mixture to form the composite.
15. The method according to claim 14, wherein the curing is for 3-60 minutes.
16. The method according to claim 14 or 15, wherein the curing is at a temperature of 20-25 °C.
17. The method according to any of claims 14 to 16, wherein the method does not comprise adding a cross-linker.
18. The method according to any of claims 14 to 17, wherein mixture comprises the polyacrylate and the hygroscopic salt at a weight ratio of is 1.5: 1-3:1.