A process for wet-ETCH patterning of mxene thin-films
The ambient condition MXene patterning process addresses the challenges of harsh conditions and equipment costs in current methods by achieving precise and scalable MXene patterning with 200 nm resolution, facilitating integration into microelectronic devices.
Patent Information
- Application Number
- PCT/IL2026/050390
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-11
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Current methods for micropatterning MXene thin-films require harsh conditions and expensive equipment, leading to inconsistent film thickness and poor lateral resolution, making it challenging to integrate MXenes into microelectronic devices effectively.
A process involving the deposition of a MXene layer on a substrate, application of a protecting material, selective etching with an aqueous medium containing an oxidant and acid, and removal of the protecting material, all performed at ambient conditions using conventional non-hazardous chemicals, achieving lateral resolution down to 200 nm.
The process provides highly precise and scalable MXene patterning that preserves electrical and structural properties, enabling integration into next-generation microelectronic technologies with superior uniformity and resolution.
Smart Images

Figure IL2026050390_19112026_PF_FP_ABST
Abstract
Description
[0001] A PROCESS FOR WET-ETCH PATTERNING OF MXENE THIN-FILMS FIELD OF THE INVENTION
[0002] The present invention relates to a process for micropatterning MXene thin-films at ambient conditions. The process features the wet etching approach for highly precise MXene patterning suitable for integration in next-generation 2D-based microelectronic technologies.
[0003] BACKGROUND OF THE INVENTION
[0004] Materials development is typically the bottleneck for device miniaturization in the microelectronics industry. As dimensions approach the few-nanometer scale, the conductivity of common metallic interconnects and electrodes becomes limited due to surface scattering and electromigration therefore shifting the focus towards alternative lower-dimensional materials. Materials such as graphene, carbon nanotubes, and transition metal dichalcogenides are explored as alternative interconnects, electrodes, and transistor channels due to their superior physical properties. However, integrating these 2D materials into modern technologies is challenging, involving arduous fabrication processes.
[0005] MXenes, a recent class of 2D materials, combine outstanding physical properties with promising synthesis scalability (Shuck, C. E. et al. Adv Eng Mater 22, 1901241 (2020)). These 2D transition metal carbides, nitrides, or carbonitrides exhibit excellent metallic conductivity, high breakdown current density, chemical stability, hydrophilicity, and mechanical strength (Mohammadi, A. V. et al. Science 372, 6547 (2021)).
[0006] MXenes are typically synthesized by etching precursor layered MAX phases to remove the A layer, using an HF-based solution or Lewis acid molten salt (Lim, K. R. G. et al. Nature Synthesis 1, 601-614 (2022)). They are converted into their 2D form by intercalation and exfoliation into a colloidal solution. Their general formula is Mn+iXnTz (n = 1-4), where M is an early transition metal, X is carbon and / or nitrogen, and Tzrepresents surface termination groups, often -O, -OH, -Cl, or -F (Schultz, T. et al. Chemistry of Materials 31, 6590-6597 (2019); Natu, V. et al. The Journal of Physical Chemistry C 06, 18 (2023)). These surface terminations, determined by the etchingprocess, significantly influence electronic properties, enabling a tunable work function from 1.6 to 6.2 eV (Liu, Y., et al. JACS 138, 15853-15856 (2016)).
[0007] EP 3957602 describes a method for the synthesis of MXenes comprising the etching of A layers from a MAX phase in non-aqueous solvents comprising iodine, the MXene nanosheets and the use of the MXenes nanosheets in electronic devices, sensors, reinforcement for composites, electrocatalysts or energy storage materials.
[0008] One of the key advantages of MXene is their synthesis and processability in colloidal solutions, enabling deposition at low temperatures and in ambient conditions.
[0009] US 2021 / 0262121 describes a method of manufacturing MXene fibers and MXene fibers manufactured therefrom, wherein the method includes a) preparing a dispersion including MXenes; and b) spinning the dispersion in a coagulation solution to obtain MXene fibers.
[0010] US 2021 / 0139379 describes a method of making a layered MXene material comprising a) introducing dried MAX phase powder into a vessel under anhydrous, inert conditions, the MAX phase powder comprising a general formula of Mn+iAXn(n=l, 2, 3, or 4), wherein M is a transition metal or p-block metalloid selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Re, Cu, Ni, Ag, Zn, Cd, In, Sn, and Pb; interlayer A is a Group III, IV, or V metalloid selected from the group consisting of Al, Si, Ga, Ge, In, Sn, Pb, As, Bi, Sb, and X is one of C (carbon) and N (nitrogen); b) introducing a halogen and solvent to the dried MAX phase to create a halogen solution having a predetermined concentration; and c) allowing a reaction to proceed for about 24 hours between 30-90 °C. to create a reaction slurry comprising a MXene material.
[0011] CN114368780 describes a method for preparing MXene material by wet etching under the mild conditions of fluorine-free low toxicity, which comprises two strategies. One strategy is to etch the MAX raw material in a solution containing chloride and alkali and then strip the MAX raw material; another strategy is to add a stripper to the etching solution or use a stripper as a solvent to synchronize the etching and stripping.
[0012] Etching by oxidation leading to perforation of MXenes in colloidal solutions has been reported in several studies (Jiang, Y. et al. PNAS USA 120, e2210211120 (2023);Zhang, H. et al. Small 20, 2403518 (2024); Cheng, Y. et al. Sci Bull (Beijing) 67, 2216-2224 (2022); and Li, S., et al. Ceram Int 47, 29930-29940 (2021)). The etching was typically performed by mixing diluted H2O2 with MXene colloidal solutions. MXene is known to be resistant to most acids but reacts with H2O2 to form TiOxnanoparticles and amorphous carbon. The flake edges are the most vulnerable areas in the MXene flakes and react rapidly with the H2O2 solution (Natu, V. et al. Journal of Physical Chemistry C 122, 27745-27753 (2018)). Concurrently, pinholes form at surface defects, such as vacancies, creating more exposed edges being dissolved and accelerating the etching rate.
[0013] Traditional ambient-conditions micropatterning of sub-20 nm MXene thin-film features relies on lift-off methods, where MXene is first deposited onto a photoresist layer using techniques like spray coating, dip coating, or spin coating (Xu, X., et al. Matter 6, 800-837 (2023); Favelukis, B., et al. Nanoscale Adv 7, 2329-2337 (2025)). Excess MXene is then removed by dissolving the underlying photoresist, leaving the desired pattern. While effective, this approach often leads to vertically oriented, folded flakes along pattern edges, resulting in inconsistent film thickness and poor lateral resolution. To date, the most reliable alternative at this scale is reactive ion etching (RIE), whereby the desired pattern is protected by photoresist while excess MXene is etched with CF4 plasma (Xu, X. et al. Advanced Materials 36, 2405214 (2024)). The main disadvantage of MXene patterning by RIE is the need for expensive dedicated equipment, the use of hazardous gases, and the lack of etching selectivity for different substrates.
[0014] Mim, M. et al. (ACS Omega 9, 32350-32393 (2024)) reviewed the synthesis of MXenes through different etching routes involving acids, such as hydrochloric acid, hydrofluoric acid, and lithium fluoride, and non-acidic alkaline solution, electrochemical, and molten salt methods. Furthermore, a concise overview of the different structural, optical, electronic, and magnetic properties of MXenes was provided corresponding to their role in supporting high thermal, chemical, mechanical, environmental, and electrochemical stability.
[0015] There remains an unmet need for cost-effective MXene patterning that does not require harsh conditions and reagents and can be implemented on a large scale to afford the integration of MXenes into microelectronic devices.SUMMARY OF THE INVENTION
[0016] The present invention provides a process for preparing micropatterned MXene at ambient conditions. The process comprises the deposition of a MXene thin-film on a substrate, patterning of a protecting material on predetermined regions of the MXene thin-film, wet etching of the unpatterned regions using a mixture of an oxidant and an acid, and removal of the protecting material. The process may further comprise the removal of salt residues on the MXene thin-films.
[0017] The present invention is based, in part, on the unexpected finding that selective etching and patterning of MXene thin-films with a lateral resolution down to 200 nm and a calibrated undercut etching rate, can be easily performed with relatively simple tools, using conventional non-hazardous chemicals, and at ambient conditions. Unlike graphene and transition metal dichalcogenides, the hitherto common MXene fabrication involves aggressive chemical conditions, such as HF or molten salt Lewis acids and mechanical exfoliation, leading to a relatively high concentration of defects. It was not previously realized that MXene fabrication can be performed by wet etching that avoids the use of aggressive chemicals and conditions while preserving the MXene intrinsic electrical and structural properties. Contrary to the wet etching of other 2D materials like graphene and transition metal dichalcogenides, disclosed herein for the first time is the wet etching of functional full-sized MXene features on a wafer scale. The present invention provides a highly precise MXene patterning that affords a scalable solution for next-generation MXene -based microelectronic technologies.
[0018] According to a first aspect, the present invention provides a process for preparing micropatterned MXene comprising the steps of: (i) depositing a MXene layer on a substrate, wherein the MXene is characterized by the general formula of Mn+iXnTz, wherein M is selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W; X is selected from the group consisting of C, N, and a combination thereof, n is an integer from 1 to 4, and Tzis a surface termination group; (ii) applying a protecting material onto a first region of the MXene layer; (iii) selectively etching a second region of the MXene layer using an aqueous medium comprising an oxidant and an acid; and (iv) removing the protecting material from the first region thereby obtaining micropatterned MXene.
[0019] In one embodiment, M is Ti. In another embodiment, X is C. In yet another embodiment, n is 2. In some embodiments, Tzis selected from the group consisting ofhydroxyl, oxo (oxide), halogen, chalcogen, hydride, alkoxide, carboxylate, sub-oxide, nitride, sub-nitride, sulfide, thiol, and a combination thereof. Each possibility represents a separate embodiment. In particular embodiments, Tzis selected from the group consisting of hydroxyl, oxo (oxide), halogen, chalcogen, and a combination thereof. Each possibility represents a separate embodiment. In further embodiments, Tzis a halogen selected from the group consisting of chloride, fluoride, and a combination thereof. Each possibility represents a separate embodiment.
[0020] In certain embodiments, the substrate comprises an organic substance. In other embodiments, the substrate comprises an inorganic substance. In further embodiments, the substrate comprises a semiconductor or a dielectric substrate. In particular embodiments, the substrate comprises at least one of a carbide, a nitride, or an oxide. Each possibility represents a separate embodiment. In further embodiments, the substrate comprises a III-V group compound. In specific embodiments, the III-V group compound is selected from the group consisting of AIN, A1P, AlAs, AlSb, AlBi, BN, BP, BAs, BSb, BBi, GaN, GaP, GaAs, GaSb, GaB, InN, InP, InAs, InSb, InBi, TIN, TIP, TlAs, TISb, TIBi, AlGaAs, InGaAs, GalnP, AlGaN, InGaN, and InGaAsP. Each possibility represents a separate embodiment. In additional embodiments, the substrate comprises silicon (including n-type p-doped silicon), silicon oxide, fused silica, sapphire, glass, or mica. Each possibility represents a separate embodiment. In one embodiment, the substrate comprises a modified surface. In another embodiment, the substrate has two opposing surfaces and is in the form of a wafer, a chip, or a disk. Each possibility represents a separate embodiment. In yet another embodiment, the substrate has sizes ranging from 1 mm to 30 cm or more, including each value within the specified range.
[0021] In various embodiments, depositing a MXene layer on a substrate is performed by a thin-film deposition method. In certain embodiments, depositing a MXene layer on a substrate is performed by at least one of spray coating, dip coating, spin coating, screen printing, blade casting, inkjet printing, Langmuir-Blodgett, and chemical vapor deposition. Each possibility represents a separate embodiment. In one embodiment, depositing a MXene layer on a substrate is performed by spin coating. In specific embodiments, the spin coating is performed at a spinning rate ranging from about 100 to about 5,000 rpm, including each value within the specified range. In certain embodiments,the spin coating is performed at a spinning rate ranging from about 1,000 to about 3,000 rpm, including each value within the specified range. In several embodiments, depositing a MXene layer on a substrate is performed using a MXene dispersion (e.g., a colloidal dispersion) at a concentration ranging from about 0.01 to about 100 g / L, including each value within the specified range. In other embodiments, depositing a MXene layer on a substrate is performed using a MXene dispersion at a concentration ranging from about 0.1 to about 50 g / L, including each value within the specified range. In additional embodiments, depositing a MXene layer on a substrate is performed at a temperature of about 10°C to about 60 °C, including each value within the specified range. In further embodiments, the deposited MXene layer is characterized by a thickness ranging from about 1 nm to about 20 pm, including each value within the specified range.
[0022] According to the principles of the present invention, a protecting material is applied onto a first region of the MXene layer in a pattern corresponding to the desired design, to protect said region from being etched in the subsequent step. In some embodiments, the protecting material comprises a metal or polymer. In other embodiments, the protecting material comprises a photoresist material. In further embodiments, the photoresist material is selected from the group consisting of hexamethyldisilazane (HMDS), SU-8 (epoxy -based negative photoresist), polyvinylcinnamate (PVCN), diazonaphthoquinone (DNQ)-novolac resists, poly(methyl methacrylate) (PMMA) and other acrylate-based resists, phenolic resin-based resists, chemically amplified photoresists (CARs), and a combination thereof. Each possibility represents a separate embodiment. In one embodiment, applying a protecting material onto a first region of the MXene layer comprises applying a dispersion comprising the photoresist material onto the MXene layer and patterning the first and second regions via UV exposure and subsequent development.
[0023] According to the principles disclosed herein, selective etching of a second region of the MXene layer which is not protected by the protecting material, is performed using an aqueous medium comprising an oxidant and an acid. In certain embodiments, the oxidant is selected from the group consisting of hydrogen peroxide, a metal peroxide, a metal superoxide, carbamide peroxide, benzoyl peroxide, and a combination thereof. Each possibility represents a separate embodiment. In one embodiment, the oxidant ishydrogen peroxide. In other embodiments, the acid is selected from the group consisting of hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, and a combination thereof. Each possibility represents a separate embodiment. In one embodiment, the acid is hydrochloric acid. In particular embodiments, the aqueous medium comprises an oxidant and an acid at a volume ratio of about 5: 1 to about 1: 10, including all iterations of ratios within the specified range. In one embodiment, the aqueous medium comprises an oxidant and an acid at a volume ratio of about 3:1 to about 1:8, including all iterations of ratios within the specified range. In another embodiment, the aqueous medium comprises an oxidant and an acid at a volume ratio of about 1: 1 to about 1:5, including all iterations of ratios within the specified range.
[0024] In certain embodiments, selective etching of a second region of the MXene layer using an aqueous medium comprising an oxidant and an acid is performed at a temperature of about 10 °C to about 60 °C, including each value within the specified range. In further embodiments, selective etching of a second region of the MXene layer using an aqueous medium comprising an oxidant and an acid is performed for a time duration ranging from about 1 s to about 15 min, including each value within the specified range. In particular embodiments, selective etching of a second region of the MXene layer using an aqueous medium comprising an oxidant and an acid is performed for a time duration ranging from about 1 min to about 10 min, including each value within the specified range.
[0025] In some embodiments, the aqueous medium comprising an oxidant and an acid further comprises a surfactant. In one embodiment, the surfactant is a non-ionic surfactant, an anionic surfactant, or a cationic surfactant. Each possibility represents a separate embodiment. In certain embodiments, the surfactant comprises at least one of polyethylene glycol, polysorbate, stearyltriethanolamine, sodium lauryl sulfate, sodium taurocholate, laurylaminopropionic acid, lecithin, benzalkonium chloride, benzethonium chloride, glycerin monostearate, polyvinyl alcohol, polyvinylpyrrolidone, carboxymethylcellulose sodium, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose. Each possibility represents a separate embodiment. In one embodiment, the surfactant is a non-ionic surfactant. In another embodiment, the surfactant is a polyethylene glycol, preferably polyethyleneglycol p-(l,l,3,3-tetramethylbutyl)-phenyl ether (i.e., Triton X-100).
[0026] In certain embodiments, removing the protecting material from the first region is performed by dissolving the protecting material. In some embodiments, dissolving the protecting material comprises the use of an organic solvent. In other embodiments, dissolving the protecting material comprises the use of at least one of acetone, acetonitrile, ethanol, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, water, and combinations thereof. Each possibility represents a separate embodiment.
[0027] In various embodiments, the process further comprises a step of removing salt residues from the MXene layer. In one embodiment, the step of removing salt residues from the MXene layer is performed following step (i) and prior to step (ii). In another embodiment, the step of removing salt residues from the MXene layer is performed following step (iv). In some embodiments, the salt residues are selected from the group consisting of lithium fluoride, lithium chloride, tetramethylammonium hydroxide, and a combination thereof. In further embodiments, removing salt residues from the MXene layer is performed by dissolving the salt residues in an acid. In other embodiments, the acid is selected from the group consisting of hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, and a combination thereof. Each possibility represents a separate embodiment. In yet other embodiments, the acid is at a concentration range of about 0.01M and about IM, including each value within the specified range. In additional embodiments, removing salt residues from the MXene layer is performed by dissolving the salt residues in an acid while spinning at a speed of about 500 to about 5,000 rpm for a time duration ranging from 1 s to 10 min, including each value within the specified ranges.
[0028] According to the principles of the present invention, the patterned MXene obtained by the process disclosed herein is characterized by superior uniformity including superior thickness uniformity and surface uniformity as compared to the patterned MXene obtained by currently available techniques such as the lift-off technique. In some embodiments, the difference in height of the patterned MXene edges to MXene center obtained by the process of the present invention is less than 10%, preferably less than 5%, more preferably less than 3%, and most preferably less than 1%. Each possibility represents a separate embodiment. In other embodiments, the lateral resolution of thepatterned MXene obtained by the process disclosed herein is only restricted by the photolithography resolution with values of lateral resolution being 200 nm or less.
[0029] The patterned MXene obtained by the process disclosed herein can be incorporated into microelectronic products such as, but not limited to, target devices, integrated circuits, flexible / transparent devices, etc.
[0030] In another aspect, the present invention provides a process for preparing micropatterned MXene comprising the steps of: (i) depositing a MXene layer on a patterned substrate comprising a protecting material, wherein the MXene is characterized by the general formula of Mn+iXnTz, wherein M is selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W; X is selected from the group consisting of C, N, and a combination thereof, n is an integer from 1 to 4, and Tzis a surface termination group; (ii) removing salt residues from the MXene layer; and (iii) removing the protecting material from the substrate thereby obtaining micropatterned MXene.
[0031] Other objects, features and advantages of the present invention will become clear from the following descriptions, examples and drawings.
[0032] BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 depicts a schematic illustration of a MXene thin-film patterning process using wet etching according to embodiments of the present invention.
[0034] Figures 2A-2C depict AFM measurements of (2A) MXene-depo sited thin-film, (2B) 10 pm electrodes, and (2C) 5 pm electrodes.
[0035] Figures 3A-3C depict (3A) XRD pattern of a TisCiTz freestanding film, inset shows a photograph of the film, (3B) XRD pattern of TiOx / C colloids after dissolving TisCiTz in H2O2 and HC1, inset shows a photograph of the solution, and (3C) SEM micrograph of dried TiOx / C residues.
[0036] Figures 4A-4C depict MXene free-standing film (4A) before, (4B) during, and (4C) after etching with H2O2 and different acids (sulfuric, left; nitric, middle; and hydrochloric, right) in a 1:3 ratio.
[0037] Figures 5A-5C depict SEM micrographs of MXene thin-film (5A) before, (5B) during, and (5C) after etching. Inset graphs show the respective Ti 2p XPS spectra.
[0038] Figure 6 depicts a photograph of MXene electrodes being etched with (right) andwithout (left) Triton X-100.
[0039] Figures 7A-7C depict SEM micrographs of (7 A) initial MXene thin-film, (7B) MXene thin-film after partial etching, and (7C) MXene thin-film at the end of the etching process (after removal of the photoresist).
[0040] Figures 8A-8D depict SEM micrographs of a MXene thin-film electrode patterned by 4-min wet etching. (8A) a low magnification of the electrode and (8B-8D) high-magnifications of certain locations in 8A showcasing the high-quality MXene thin-films, patterning precision, and undamaged Si substrate.
[0041] Figures 9A-9H depict MXene electrodes patterned by wet etching at different etching times of (9 A) 1 min, (9B) 2 min, (9C) 3 min, (9D) 4 min, (9E) 5 min, (9F) 6 min, (9G) 7 min, and (9H) 8 min. The effect of undercutting below the photoresist with extended durations of etching is evident.
[0042] Figures 10A-10D depict SEM micrographs of MXene wet etching stages before and after completion. (10A) complete etching after 3 min, (10B) incomplete etching after 2 min, (10C) high magnification of MXene residues with incomplete etching, and (10D) high magnification of electrode edge with incomplete etching.
[0043] Figure 11 depicts an optical micrograph showing non-heat-treated MXene degassing under developed photoresist.
[0044] Figure 12 depicts an optical micrograph showing adhesion problem of developed photoresist on MXene without HMDS.
[0045] Figures 13A-13H depict XPS spectra of HMDS-treated MXene thin-film. (13A) Ti 2p, (13B) C Is, (13C) O Is, (13D) N Is, (13E) F Is, (13F) Si 2p, (13G) Al 2p, and (13H) survey spectrum.
[0046] Figure 14 depicts a 4-inch MXene-coated wafer patterned by the wet etching process according to embodiments of the present invention.
[0047] Figure 15 depicts a SEM micrograph of MXene-patterned electrodes.
[0048] Figures 16A-16B depict MXene electrode patterned by wet etching on a 4-inch wafer: (16A) fused silica, and (16B) 100 nm SiOi.
[0049] Figure 17 depicts high-resolution STEM micrograph of a MXene thin-film crosssection.
[0050] Figures 18A-18I depict AFM analysis of patterned MXene electrodes. (18A) AFM average height profile of MXene electrodes patterned by lift-off and wet etching.Corresponding SEM micrographs of the entire MXene electrodes patterned by (18B) liftoff and (18C) wet etching, (18D-18F) AFM average height profiles of MXene electrodes with different widths, and (18G-18I) corresponding AFM scans.
[0051] Figures 19A-19C depict MXene electrodes patterned by wet etching for (19A) 4 min, (19B) 6 min, and (19C) 8 min.
[0052] Figure 20 depicts undercut etching rates, with the inset showing a SEM micrograph of an over-etched electrode (scale bar 1 pm). The arrow represents the undercut etching length.
[0053] Figure 21 depicts four-point probe measurement of MXene features at different etching times. The upper left inset shows a SEM micrograph of the MXene four-point electrode (scale bar 100 pm), and the bottom right graph shows the features height.
[0054] Figure 22 depicts IV measurement of a MXene-Si-MXene photodetector, with the inset displaying photocurrent at ±2 V versus illumination power density.
[0055] DETAILED DESCRIPTION OF THE INVENTION
[0056] The present invention provides a process for preparing thin-films of MXene by wet etching. In particular, the process employs a calibrated HiO HCl-based solution to achieve controlled MXene patterning down to -200 nm resolution with excellent reproducibility and minimal substrate damage. The process can be integrated with standard fabrication processes for the production of microelectronics, integrated circuits and the like.
[0057] Contrary to the hitherto micropatteming methods such as dry etching, lift-off, and micro-contact printing that require expensive equipment, specialized environments, or suffer from limited resolution and reproducibility, the process disclosed herein offers a facile, clean, cost-effective, and highly controllable technique that preserves the MXene intrinsic electrical and structural properties. The process avoids the use of high temperatures and harmful reagents and can be easily performed with relatively simple tools and chemicals on various substrates to afford functional MXene electrodes on a full-sized wafer scale.
[0058] Disclosed herein for the first time is a novel patterning method for MXene electrodes, using a wet etching process. The method requires common nanofabricationtools and reagents operating at ambient conditions, simplifying the integration of MXene into the microelectronics industry. Highly controllable patterning of TisCiTz MXene sub-10-nm thin-films on a variety of common substrates are demonstrated and MXene micropatterning is achievable with an excellent lateral resolution of -200 nm. The selective wet etching process creates sharp edge features without damaging the substrate and enables utilization of the undercut etching rate to fine tune the final electrode width for desired applications. The patterned MXene electrodes exhibit high electrical conductivity when deposited on a dielectric substrate and function as a highly sensitive photodetector when deposited on Si. This wet etching approach paves the way for the large-scale integration of MXenes into next-generation microelectronic nanoscale or 2D devices.
[0059] Reference is now made to Figure 1 demonstrating certain features according to embodiments of the present invention. A substrate is coated (e.g., by spin-coating) with MXene to form a MXene thin-film. The substrate may be an organic substance, for example an organic polymer such as, but not limited to, a (meth)acrylate, polyvinyl alcohol, an epoxy, a polysaccharide or a polyurethane; or an inorganic substance such as a carbide, a nitride, an oxide, any III-V group compound or a silicon-based substance such as, but not limited to, a silicon wafer (including n-type p-doped silicon wafer), a silicon oxide wafer, a fused silica wafer, a sapphire wafer (e.g., c-plane sapphire), a glass wafer (including a microscope glass slide), or a mica wafer. The substrate can be treated to modify its surface characteristics prior to depositing a MXene thin-film onto it. Typically, the deposited MXene thin-film includes salt by-products (for example, halide salts) resulting in from the synthesis of the MXene. The salt by-products can optionally be removed from the MXene layer e.g., by HC1 spin-cleaning as described in Favelukis, B., et al. Nanoscale Adv 7, 2329-2337 (2025).
[0060] MXene electrodes are then patterned as is known in the art. For example, photolithography using a photoresist material can be performed by applying the photoresist material onto the MXene thin-film followed by patterning through means of applying a mask and light exposure. Following photolithography, wet etching is performed using a solution of an oxidant such as hydrogen peroxide (H2O2), an acid such as hydrochloric acid (HC1), and optionally a surfactant such as octylphenol ethoxylate toafford the selective etching of the unpatterned regions of the MXene while the patterned regions are protected from etching by the photoresist. In this manner, controlled, selective etching at room temperature is obtained. Finally, the photoresist is removed thereby providing micropatterned MXene.
[0061] According to certain aspects and embodiments, provided herein are processes for preparing MXene architectures. As used herein, the term “MXene” refers to a class of inorganic materials comprising one or more layers derived from a precursor comprising a MAX-phase material having a general formula Mn+iAXnwherein “M” is a transition metal; “A” is an element from groups 12-16 of the periodic table including, but not limited to, Al, Si, P, S, C, B, Ga, Ge, As, Cd, In, Sn, Sb, Tl, Bi and Pb; “X” is carbon and / or nitrogen which may also contain O, and n is an integer from 1 to 4. The MXene is obtained by the selective removal or extraction of at least a portion of the A element from the MAX-phase precursor. The resulting MXene is characterized by a general formula Mn+iXnTz, where n is an integer from 1 to 4. In one embodiment, n is 2.
[0062] According to the principles of the present invention, “M” in general formula Mn+iXnTz represents a transition metal element. Typically, “M” comprises an early transition metal capable of forming stable layered compounds with carbon and / or nitrogen. Non-limiting examples of suitable “M” elements include titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), and combinations or alloys thereof. In one embodiment, “M” represents titanium (Ti). While “M” may comprise a single transition metal species, in some embodiments, “M” comprises two or more different transition metals within the same MXene structure. “M” as used herein encompasses all oxidation states, isotopic forms, and structural and crystallographic configurations that are compatible with MXene architectures prepared by the processes disclosed herein.
[0063] “X” in general formula Mn+iXnTz represents carbon (C) and / or nitrogen (N). In some embodiments, “X” represents carbon only, nitrogen only, or a combination of carbon and nitrogen. In one embodiment, “X” represents carbon (C). In certain embodiments, “X” may further comprise oxygen (O), such that the MXene material includes oxycarbide and / or oxynitride MXene structures, including mixed C / N / O compositions. The presence of oxygen may arise from partial substitution of C and / or Nwith O within the sublattice that occurs during synthesis or post- treatment, surface oxidation (including partial oxidation) or a combination thereof. “X” as used herein encompasses all compositional variations, bonding states, and structural configurations of C, N, and / or O that are compatible with MXene architectures prepared by the processes disclosed herein, including materials commonly referred to as carbide, nitride, carbonitride, oxycarbide, or oxynitride MXenes.
[0064] “Tz” in general formula Mn+iXnTz represents a surface termination and / or functional group bound to exposed surfaces of the MXene layer(s). In some embodiments, “Tz” represents one or more chemical species introduced during synthesis, post- treatment, or environmental exposure. Without being bound by any theory or mechanism of action, it is contemplated that “Tz” may stabilize the MXene structure and / or affect its physicochemical properties. “Tz” includes, but is not limited to, hydroxyl, oxo (oxide), halide, chalcogen, hydride, alkoxide, carboxylate, sub-oxide, nitride, sub-nitride, sulfide, thiol species, and combinations thereof. In some embodiments, “Tz” comprises hydroxyl (-OH), oxygen (-0), halide species including fluorine (-F) and chlorine (-C1), chalcogenide or sulfur-containing species, hydrogen, or combinations thereof. “Tz” as used herein encompasses all compositional variations, bonding states, surface coverages, and structural configurations of such terminations that are compatible with MXene architectures prepared by the processes disclosed herein.
[0065] MXenes as defined herein are typically two-dimensional materials and may exist as single layers, few-layer structures, or as multilayer stacks. MXenes encompassed by the present invention may be in the form of thin films, coatings, laminates, or assembled structures thereof. As used herein, the term “two-dimensional (2D) material” refers to a material having at least one lateral dimension that is substantially greater than the material thickness, such that a ratio of the thickness to the lateral dimension is sufficiently small for the material to exhibit electronic, optical, mechanical, chemical, and / or structural properties associated with minimized dimensionality in one direction. For example, the ratio of the material thickness to at least one lateral dimension is less than about 1: 10, less than about 1:100, less than about 1:500, or less than about 1:1,000. The MXene obtained by the processes disclosed herein may have a thickness in the nanometer to micrometer range or greater, and lateral dimensions ranging from nanometer scale to micrometerscale, centimeter scale or larger, depending on the preparation parameters and intended application. MXenes may be crystalline, polycrystalline, partially ordered, or disordered (amorphous), and may be electrically conductive, semiconductive, or insulating depending on their composition, surface terminations, and structural configuration. The term “MXene” further includes materials that are chemically modified, physically treated, doped, intercalated, functionalized, etched, annealed, oxidized, reduced, stacked, laminated, or combined with one or more additional materials, including polymers, metals, metal oxides, semiconductors, carbon-based materials, or other two-dimensional materials, to form composite films or heterostructures.
[0066] As used herein, the term “MXene” further encompasses MXene materials in any physical or morphological form, including but not limited to flakes, sheets, powders, films, coatings, dispersions, composites, heterostructures, and chemically or physically modified variants thereof. In some embodiments, MXene obtained by the processes disclosed herein is a thin-film MXene material which may comprise a single-layer, a few-layers, or multilayer structures. The MXene thin-films may be uniform or non-uniform in thickness, may exhibit controlled or uncontrolled in-plane orientation, and may be continuous or discontinuous across the substrate surface.
[0067] In further embodiments, the thin-film MXene materials are in the form of patterned layers disposed on a substrate or on an underlying layer. In accordance with these embodiments, the MXene materials are micropatterned MXene. The term “micropatterned MXene” refers to a MXene material which is spatially defined on the substrate in the form of discrete features, regions, or motifs having lateral dimensions on the micrometer scale, typically from about 1 pm to several hundred pm, although smaller or larger feature sizes are also contemplated. The micropatterned MXene may comprise any suitable pattern or geometry, including but not limited to arrays of lines, dots, grids, meshes, islands, and interdigitated structures arranged either periodically or non-periodically, as well as freeform, irregular, or otherwise unconstrained geometries. The micropatterning encompasses spatial variations of the MXene relative to the substrate and may involve modulation of MXene presence and thickness on the substrate as well as modulations in composition, surface termination, orientation, conductivity, or functional properties across the substrate surface. In certain embodiments, themicropatterned MXene forms electrically isolated regions, electrically interconnected networks, or functional device elements such as electrodes, sensing regions, active layers etc.
[0068] According to the principles of the present invention, the process disclosed herein encompasses the deposition of a layer or a plurality of layers of MXene material onto a substrate. Within the scope of the present invention are a wide variety of substrates, including, but not limited to metals, semiconductors, dielectrics, polymers, ceramics, glasses, paper-based substrates, and multilayer electronic device structures. Suitable substrates may be composed of organic materials or inorganic materials. Both electrically conductive and electrically insulating substrates may be employed, depending on the intended function of the MXene layer.
[0069] Semiconductor and dielectric substrates are particularly well suited for supporting MXene thin films and micropatterned MXene structures. Such substrates may be formed from carbide-, nitride-, or oxide-based materials, and / or may include semiconductor materials formed from two or more elements, including binary, ternary, and quaternary compounds, as well as their alloys, solid solutions, and lattice-matched combinations commonly used in thin-film and device fabrication. For example, substrates comprising Group III-V materials may be used, including binary, ternary, or quaternary compounds such as AIN, A1P, AlAs, AlSb, AlBi, BN, BP, BAs, BSb, BBi, GaN, GaP, GaAs, GaSb, GaB, InN, InP, InAs, InSb, InBi, TIN, TIP, TlAs, TISb, TIBi, as well as mixed compositions such as AlGaAs, InGaAs, GalnP, AlGaN, InGaN, and InGaAsP.
[0070] Elemental and oxide-based substrates may also be employed. For example, substrates may comprise silicon, including n-type, p-type, or doped silicon, as well as silicon oxide, fused silica, sapphire, glass, or mica. Such substrates are well established in thin-film processing and microfabrication and are particularly compatible with the formation, patterning, and integration of MXene films in device architectures.
[0071] The substrate surface may be unmodified or modified prior to MXene deposition. Surface modification may include chemical treatment, functionalization, oxidation, nitridation, texturing, roughening, planarization, or other conditioning steps that promote MXene deposition, adhesion, and / or nucleation. Depending on the application, the substrate may be provided as a wafer, chip, disk, sheet, or panel, typically having twoopposing major surfaces that support thin-film fabrication.
[0072] Substrates suitable for use herein may span a wide range of sizes, from millimeter-scale samples to larger scale samples on the order of tens of centimeters or more. The substrates may be rigid or flexible. This versatility of substrates enables MXene fabrication and integration suitable for laboratory-scale studies, pilot-scale processing, and large-scale commercial manufacturing for coating, sensing, or electronic applications.
[0073] Depositing a MXene layer(s) on a substrate may be carried out using a thin-film deposition method. Suitable thin-film deposition methods within the scope of the present invention include, but are not limited to spray coating, dip coating, spin coating, screen printing, blade casting, inkjet printing, Langmuir-Blodgett deposition, and chemical vapor deposition, as well as combinations thereof. Such deposition methods may be implemented using laboratory-scale, pilot-scale, or industrial-scale coating systems configured for planar, rigid, or flexible substrates.
[0074] Spin coating represents one suitable deposition technique for forming MXene thin films. Spin coating may be performed using a rotational coating apparatus comprising a substrate holder, a motor configured to control rotational speed, and a dispensing unit for delivering a MXene dispersion onto the substrate surface. When spin coating is employed, the spinning rate may be in a range of about 100 rpm to about 5,000 rpm, including each value within the specified range. Spinning rates within the scope of the present invention include, but are not limited to, about 500 rpm to about 4,000 rpm, about 1,000 rpm to about 3,500 rpm, or about 1,000 rpm to about 3,000 rpm, including each value within the specified ranges. Exemplary spinning rates include 100 rpm, 250 rpm, 500 rpm, 750 rpm, 1,000 rpm, 1,500 rpm, 2,000 rpm, 2,500 rpm, 3,000 rpm, 3,500 rpm, 4,000 rpm, 4,500 rpm, or 5,000 rpm.
[0075] The spin coating duration may be controlled to regulate film thickness and uniformity. Spin coating durations may range from about 1 second to about 300 seconds, including each value within the specified range. For example, spin durations may include, but are not limited to about 5 seconds to about 150 seconds or about 10 seconds to about 120 seconds, including each value within the specified ranges. Representative spin durations include 5 s, 10 s, 20 s, 30 s, 60 s, 120 s, 150 s, 180 s, 210 s, 250 s, 280 s, or 300s.
[0076] Deposition of the MXene layer(s) may be performed using a MXene dispersion, such as a colloidal MXene dispersion, which may be prepared in water or an aqueous or non-aqueous solvent system. The MXene dispersion may have a MXene concentration in a range of about 0.01 g / L to about 100 g / L, including each value within the specified range. Concentration ranges within the scope of the present invention include, but are not limited to, about 0.05 g / L to about 75 g / L, about 0.1 g / L to about 50 g / L, or about 0.5 g / L to about 25 g / L, including each value within the specified ranges. Representative MXene dispersion concentrations include 0.01 g / L, 0.05 g / L, 0.1 g / L, 0.5 g / L, 1 g / L, 5 g / L, 10 g / L, 25 g / L, 50 g / L, 75 g / L, or 100 g / L.
[0077] The MXene dispersion may be filtered, sonicated, stirred, or shear-mixed prior to deposition to control flake size distribution, dispersion stability, and film homogeneity. Sonication times may range from about 1 minute to about 120 minutes, including each value within the specified range. Stirring or mixing times may range from about 5 minutes to about 24 hours, including each value within the specified range.
[0078] Depositing the MXene layer(s) on the substrate may be performed at a temperature in a range of about 10 °C to about 60 °C, including each value within the specified range. Deposition temperatures within the scope of the present invention include, but are not limited to, about 15 °C to about 50 °C, about 20 °C to about 40 °C, or about 20 °C to about 30 °C, including each value within the specified ranges. Exemplary deposition temperatures include 10 °C, 15 °C, 20 °C, 25 °C, 30 °C, 35 °C, 40 °C, 45 °C, 50 °C, 55 °C, or 60 °C. Deposition may be carried out under ambient atmosphere or under a controlled atmosphere, including inert or reduced-oxygen environments.
[0079] Spray coating represents another suitable technique for depositing the MXene layer(s) on a substrate. Spray coating may be performed using a spraying apparatus comprising a nozzle, an atomization source, and a carrier gas supply configured to deliver a MXene dispersion toward a substrate surface. The spray flow rate may be in a range of about 0.1 mL / min to about 50 mL / min, including each value within the specified range, such as about 0.5 mL / min to about 40 mL / min or about 1 mL / min to about 30 mL / min. Representative non-limiting spray flow rates include 0.1 mL / min, 0.5 mL / min, 1 mL / min, 5 mL / min, 10 mL / min, 20 mL / min, 30 mL / min, 40 mL / min, or 50 mL / min.Dip coating may also be employed for forming MXene films. Dip coating may be carried out by immersing a substrate into a MXene dispersion followed by controlled withdrawal. The withdrawal speed may be in a range of about 0.1 mm / s to about 100 mm / s, including each value within the specified range, such as about 0.5 mm / s to about 50 mm / s or about 1 mm / s to about 20 mm / s. Representative withdrawal speeds include 0.1 mm / s, 0.5 mm / s, 1 mm / s, 5 mm / s, 10 mm / s, 20 mm / s, 30 mm / s, 40 mm / s, 50 mm / s, 60 mm / s, 70 mm / s, 80 mm / s, 90 mm / s, or 100 mm / s.
[0080] Blade casting represents a further suitable deposition method. Blade casting may be carried out using a blade assembly positioned at a controlled gap above the substrate surface. The blade gap may be in a range of about 0.1 pm to about 1,000 pm, including each value within the specified range, such as about 1 pm to about 800 pm or about 5 pm to about 500 pm. Representative blade gaps include 0.1 pm, 0.5 pm, 1 pm, 5 pm, 10 pm, 25 pm, 50 pm, 75 pm, 100 pm, 250 pm, 500 pm, 750 pm, or 1,000 pm.
[0081] Inkjet printing represents another suitable technique for localized or patterned deposition of MXene layer(s). Inkjet printing may be performed using a drop-on-demand or continuous inkjet system configured to dispense a MXene dispersion through one or more nozzles. Droplet volumes may range from about 1 pL to about 1,000 pL, including each value within the specified range, such as about 5 pL to about 800 pL or about 10 pL to about 500 pL. Representative droplet volumes include 1 pL, 5 pL, 10 pL, 20 pL, 50 pL, 100 pL, 250 pL, 500 pL, 750 pL, or 1,000 pL.
[0082] Langmuir-Blodgett deposition may also be used to form MXene layer(s), particularly for controlling layer packing and alignment. In such processes, MXene flakes may be assembled at a liquid-air interface and transferred onto a substrate by controlled immersion or withdrawal. The surface pressure during transfer may be in a range of about 1 mN / m to about 50 mN / m, including each value within the specified range, such as about 5 mN / m to about 30 mN / m or about 10 mN / m to about 25 mN / m.
[0083] Chemical vapor deposition-based approaches may additionally be employed for forming MXene layers or MXene-derived layers on a substrate. Such processes may be carried out in a reaction chamber configured for gas delivery and thermal control, at pressures ranging from about 0.01 Torr to about 1,000 Torr and at temperatures selected to enable MXene formation or conversion while preserving the layered structure.The deposited MXene layer(s) may be characterized by a thickness in a range of about 1 nm to about 20 pm, including each value within the specified range. Exemplary thickness ranges include, but are not limited to, about 5 nm to about 10 pm, about 10 nm to about 1 pm, or about 50 nm to about 500 nm, including each value within the specified ranges. Representative non-limiting MXene layer thicknesses include 1 nm, 5 nm, 10 nm, 25 nm, 50 nm, 100 nm, 250 nm, 500 nm, 1 pm, 5 pm, 10 pm, 15 pm, or 20 pm.
[0084] Following deposition, and where applicable, the MXene layer(s) may be subjected to a drying or solvent-removal step. Drying temperatures may range from about 20 °C to about 150 °C, including each value within the specified range, such as about 40 °C to about 120 °C or about 60 °C to about 100 °C. Drying times may range from about 1 minute to about 24 hours, including each value within the specified range.
[0085] Prior to application of the protecting material to form patterned MXene, the MXene surface may optionally be subjected to surface preparation steps, such as cleaning, mild plasma treatment, chemical activation, or application of an adhesion-promoting layer, to improve adhesion and pattern integrity. In some embodiments, the MXene layer may be subjected to a thermal treatment following deposition. Such treatment may be performed at a temperature at or above a subsequent processing or baking temperature, and may substantially prevent occurrence of defects, discontinuities, or other artifacts in the material.
[0086] In some implementations, the process further includes a salt-residue removal step, carried out to reduce or eliminate residual salts present at the surface of the MXene layer(s). Typically, these salt-residues are present as a result of the synthesis or deposition of the MXene layer(s) onto the substrate. Salt-residue removal may be performed prior to the application of the protecting material, thereby improving surface cleanliness, adhesion, and pattern definition of the subsequently applied protecting layer. Alternatively, salt-residue removal may be performed after one or more downstream processing steps, including after the patterning, depending on the process integration requirements.
[0087] Salt residues that may be removed include, but are not limited to, lithium fluoride, lithium chloride, tetramethylammonium hydroxide, and combinations thereof. Removal of the salt residues may be achieved by dissolving the residues using an acidic treatment,wherein the acid is selected to effectively solubilize the residual salt species while preserving the structural and chemical integrity of the MXene layer(s).
[0088] Suitable acids include, but are not limited to, hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, and combinations thereof. The acid concentration may be selected over a wide range, for example, from about 0.01 M to about 1 M, including each value within the specified range. Exemplary concentrations include, but are not limited to, about 0.01 M, about 0.02 M, about 0.03 M, about 0.04 M, about 0.05 M, about 0.06 M, about 0.07 M, about 0.08 M, about 0.09 M, about 0.1 M, about 0.2 M, about 0.3 M, about 0.4 M, about 0.5 M, about 0.6 M, about 0.7 M, about 0.8 M, about 0.9 M, and about 1 M.
[0089] Salt residue removal may further be carried out under dynamic conditions to enhance dissolution efficiency and uniformity across the MXene surface. Without being bound by any theory or mechanism of action, it is contemplated that combined chemical and mechanical action facilitates effective dissolution and removal of salt residues while maintaining thickness uniformity, surface continuity, and structural integrity of the MXene layer(s). For example, dissolution may be performed while the substrate is subjected to spinning, wherein the spinning speed may range from about 500 rpm to about 5,000 rpm, including each value within the specified range. Spinning speeds within the scope of the present invention include, but are not limited to, about 750 rpm to about 4,000 rpm, about 1,000 rpm to about 3,500 rpm, or about 1,500 rpm to about 3,000 rpm, including each value within the specified ranges. Exemplary non-limiting spinning speeds include 500 rpm, 750 rpm, 1,000 rpm, 1,500 rpm, 2,000 rpm, 2,500 rpm, 3,000 rpm, 3,500 rpm, 4,000 rpm, 4,500 rpm, or 5,000 rpm.
[0090] The treatment duration of the spinning may range from about 1 second to about 10 minutes, including each value within the specified range. Treatment durations that may be employed include, but are not limited to, about 5 seconds to about 5 minutes, about 10 seconds to about 2 minutes, or about 30 seconds to about 1 minute, including each value within the specified ranges. Representative treatment durations include 1 s, 5 s, 10 s, 30 s, 1 min, 2 min, 5 min, or 10 min.
[0091] According to the principles of the present invention, a protecting material is then applied onto a first region of the MXene layer, wherein the first region corresponds to aspatially defined portion of the MXene surface that is intended to remain after etching and to form part of the final micropattemed structure. The protecting material is arranged in a pattern that represents the desired MXene design, such that the first region is substantially resistant to etching, while one or more second regions of the MXene layer that remain unprotected are selectively removed or modified during the etching process.
[0092] The first region and the second region are defined laterally across the surface of the MXene layer and may form discrete features, continuous features, or combinations thereof. The first region may correspond to lines, islands, grids, interdigitated structures, or other geometric features having lateral dimensions on the micrometer scale or smaller, depending on the resolution of the patterning process. In this manner, the protecting material functions as an etch mask, enabling controlled spatial modulation of MXene presence, thickness, or continuity across the substrate surface.
[0093] The protecting material may comprise any material capable of adhering to the MXene surface and acting as an effective barrier to the subsequent etching while maintaining the patterned features. Suitable protecting materials include inorganic materials, organic materials, or hybrid materials. By way of example, the protecting material may comprise a metal, a polymeric material, a carbon-based material, or a radiation-sensitive material. Inorganic protecting materials may include metal oxides, metal nitrides, carbides, or mixed oxide-nitride compounds. Carbon-based protecting materials may include amorphous carbon, graphitic carbon, diamond-like carbon, or spin-on carbon films. Polymeric protecting materials may include chemically inert polymers, sacrificial polymers, or water-soluble polymers selected to allow subsequent removal without degrading the underlying MXene layer. Hybrid or multilayer protecting materials comprising combinations of polymeric and inorganic materials may also be employed, particularly where increased etch resistance or pattern stability is desired.
[0094] In particular, the protecting material may comprise a photoresist material, allowing spatial definition of the first and second regions of the MXene layer(s) using lithographic techniques. Suitable photoresist materials include, but are not limited to, hexamethyldisilazane (HMDS), epoxy-based negative photoresists such as SU-8, polyvinylcinnamate (PVCN), diazonaphthoquinone (DNQ)-novolac resists, poly(methyl methacrylate) (PMMA) and other acrylate-based resists, phenolic resin-based resists,chemically amplified photoresists (CARs), and combinations thereof. The photoresist may be selected based on desired resolution, resistance to the etching material, compatibility with the surface chemistry of MXene materials, and ease of subsequent removal.
[0095] Application of the protecting material onto the MXene layer may comprise depositing a composition comprising the protecting material onto the MXene surface, followed by selective exposure to radiation, such as ultraviolet radiation, electron beam radiation, or laser radiation, and subsequent development. Exposure may be performed through a photomask or by direct-write patterning. Development removes the protecting material from the second region while retaining the protecting material on the first region, thereby producing a patterned protecting layer. The thickness of the protecting material may be selected to provide sufficient etch resistance and may range, for example, from nanometer-scale thicknesses to micrometer-scale thicknesses, depending on the etching conditions and desired pattern definition.
[0096] When the protecting material is a photoresist material, it may be selectively exposed to ultraviolet (UV) radiation through a photomask to form a desired pattern which defines the first and second regions of the MXene layer(s). The photomask may comprise a quartz or glass substrate having opaque and transparent regions defining the pattern to be transferred, and may be positioned in proximity to or in contact with the photoresist layer during exposure.
[0097] The UV radiation may be provided by a UV light source operating at one or more wavelengths suitable for the selected photoresist, such as deep ultraviolet (DUV) or near-ultraviolet wavelengths. Representative exposure wavelengths include, but are not limited to, about 365 nm (i-line), about 248 nm (KrF excimer), or about 193 nm (ArF excimer), although other wavelengths may be employed depending on the photoresist chemistry. The exposure dose and duration may be selected to cause a chemical change in the exposed regions of the photoresist sufficient to enable subsequent development.
[0098] Following UV exposure, the photoresist may be developed using an appropriate developer solution to selectively remove either the exposed portions or the unexposed portions of the photoresist, depending on whether a positive or negative photoresist is used. Suitable developer solutions include, but are not limited to, aqueous alkalinedevelopers such as tetramethylammonium hydroxide (TMAH)-based solutions, organic solvent-based developers, or other developer chemistries compatible with the selected photoresist and the underlying MXene material. In some embodiments, the development process may be followed by a rinsing step and optional drying, resulting in the formation of a patterned photoresist layer that exposes selected regions of the underlying MXene layer(s) while protecting other regions.
[0099] Following patterning by application of the protecting material, the protected MXene regions are preserved during selective etching of the exposed regions, resulting in a micropatterned MXene structure that corresponds to the predefined design while retaining the intrinsic electrical and / or structural properties of the protected MXene regions. As used herein, the term “selective etching” refers to removal of MXene material from an exposed region of the MXene such that the region protected by the protecting material remains substantially intact.
[0100] According to the principles of the present invention, the selective etching of the non-protected regions of the MXene layer(s) is performed using an aqueous medium comprising a combination of an oxidant and an acid. Without being bound by any theory or mechanism of action, it is contemplated that the combination of an oxidant and an acid promotes concurrent oxidation and dissolution of MXene material in regions not covered by the protecting material.
[0101] The oxidant may include hydrogen peroxide, metal peroxides, metal superoxides, carbamide peroxide, benzoyl peroxide, or combinations thereof, with hydrogen peroxide being particularly suitable due to its availability, controllable reactivity, and compatibility with aqueous processing. The acid component may include hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, or combinations thereof, with hydrochloric acid being particularly suitable for providing effective etching while maintaining compatibility with the protecting material and underlying substrate. Preparation of the aqueous etching medium may be carried out by combining an aqueous medium such as water with the oxidant and acid in any suitable order. The oxidant and acid may be added sequentially or simultaneously, and the resulting mixture may be stirred, mixed, or otherwise agitated to form a substantially homogeneous etching composition prior to contacting the MXene layer(s). Theconcentration and relative proportions of the oxidant and acid may be selected to provide a desired balance between etch rate, etch uniformity, and selectivity. Typically, the oxidant and acid are combined at a volume ratio of from about 5:1 to about 1:10, for example about 3:1 to about 1:8 or about 1:1 to about 1:5, including each value within the specified ranges. Exemplary ratios of oxidant to acid include, but are not limited to about 5:1, about 4:1, about 3:1, about 2:1, about 1:1, about 1:2, about 1:3, about 1:4, about 1:5, about 1:6, about 1:7, about 1:8, about 1:9, or about 1:10.
[0102] The etching medium may be brought into contact with the MXene layer(s) using a variety of application techniques. For example, the substrate may be immersed in the etching medium, or the etching medium may be applied to the surface of the substrate by, for example, dispensing, puddle coating, spraying, or flowing the solution across the surface. In some cases, the etching medium may be continuously refreshed or flowed to maintain a substantially constant etchant composition at the MXene surface. The selected contact method may depend on factors such as substrate size, MXene thickness, pattern geometry, and desired throughput.
[0103] During the etching process, mass transport of the etching medium to the exposed MXene regions may be enhanced by agitation or movement. Agitation may be provided by, for example, stirring the etching medium, by moving or rotating the substrate, or by inducing fluid flow across the substrate surface. Such agitation can promote uniform exposure of the exposed MXene regions to the oxidant and acid, reduce local concentration gradients, and improve etch uniformity across patterned features.
[0104] The selective etching is typically carried out under controlled thermal conditions to balance etch uniformity, resolution, and process throughput. The aqueous etching medium may be maintained at a temperature from about 10 °C to about 60 °C, with lower temperatures generally reducing etch rate and higher temperatures increasing reaction kinetics. Suitable temperatures at which selective etching can be performed include, but are not limited to, about 10 °C, about 15 °C, about 20 °C, about 25 °C, about 30 °C, about 35 °C, about 40 °C, about 45 °C, about 50 °C, about 55 °C, or about 60 °C.
[0105] Exposure of the MXene layer(s) to the etching medium is typically performed for a duration sufficient to remove the unprotected region, with suitable etch times ranging from about 1 second to about 15 minutes, including each value within the specified range.In many implementations, exposure times from approximately 1 minute to approximately 10 minutes enable sufficient removal of the exposed MXene while avoiding under-etching of the protected region or degradation of the protecting material. Exemplary etching durations include, but are not limited to, 1 s, 5 s, 10 s, 20 s, 30 s, 1 m, l.5 m, 2 m, 2.5 m, 3 m, 3.5 m, 4 m, 4.5 m, 5 m, 5.5 m, 6 m, 6.5 m, 7 m, 7.5 m, 8 m, 8.5 m, 9 m, 9.5 m, 10 m, 10.5 m, 11 m, 11.5 m, 12 m, 12.5 m, 13 m, 13.5 m, 14 m, 14.5 m, or 15 m.
[0106] To improve wetting, etch uniformity, and penetration of the etching medium into exposed MXene regions, the aqueous medium may additionally include a surfactant. The surfactant may be non-ionic, anionic, or cationic in nature, and may be selected to reduce surface tension without adversely interacting with the protecting material or the MXene surface. Suitable surfactants within the scope of the present invention include, but are not limited to, polyethylene glycol, polysorbates, stearyltriethanolamine, sodium lauryl sulfate, sodium taurocholate, laurylaminopropionic acid, lecithin, benzalkonium chloride, benzethonium chloride, glycerin monostearate, polyvinyl alcohol, polyvinylpyrrolidone, carboxymethylcellulose sodium, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose, as well as combinations thereof. Non-ionic surfactants are particularly suitable for maintaining compatibility across a wide range of MXene chemistries. Polyethylene glycol-based surfactants, including polyethylene glycol p-(l,l,3,3-tetramethylbutyl)-phenyl ether (Triton X- 100), may be employed to facilitate uniform exposure of the exposed MXene regions to the etching medium while minimizing bubble formation and local etch non-uniformities.
[0107] Additional surfactants suitable for use in the aqueous etching medium include alcohol ethoxylates, alkyl polyglucosides, polyethylene oxide-polypropylene oxide block copolymers, alkylbenzene sulfonates, alkyl sulfates, alkyl sulfonates, quaternary ammonium surfactants, and polymeric dispersants, as well as combinations thereof. Alcohol ethoxylates may include Cs-Ci6 linear or branched alcohol ethoxylates, which can reduce surface tension and improve wetting of exposed MXene regions. Alkyl polyglucosides, such as decyl glucoside or lauryl glucoside, may also be employed. Polyethylene oxide-polypropylene oxide block copolymers, including triblock copolymers of the PEO-PPO-PEO type (e.g., Pluronic® surfactants), may be used toenhance etching uniformity and suppress bubble formation at the MXene surface.
[0108] Alkylbenzene sulfonates, including sodium dodecylbenzenesulfonate, as well as alkyl sulfates and alkyl sulfonates, may be employed to enhance dispersion and mass transport of the etching medium across exposed regions of the MXene layer(s). Quaternary ammonium surfactants may include alkyltrimethylammonium salts, such as cetyltrimethylammonium bromide or cetyltrimethylammonium chloride, which can be used to modify interfacial interactions between the etching medium and the MXene surface. Polymeric dispersants may include polyacrylic acid, polystyrene sulfonate, polyethyleneimine, or amphiphilic copolymers, which may assist in stabilizing the etching medium and promoting uniform contact with exposed MXene features. The surfactant or combination of surfactants may be selected based on compatibility with the oxidant and acid, stability under etching conditions, and the desired degree of wetting and etch uniformity.
[0109] Upon completion of the etching step, the etching reaction may be terminated by removing the substrate from the etching medium and optionally rinsing the substrate with deionized water, a buffered solution, or another compatible liquid to remove residual oxidant, acid, surfactant, and reaction by-products. The substrate may then be dried using ambient drying, nitrogen blow-drying, or other suitable drying techniques prior to subsequent processing.
[0110] Removal of the protecting material from the first region of the MXene layer is then performed. The protecting material may be removed using any process capable of removing the protecting material without affecting the integrity and structure of the micropatterned MXene. Such removal may be carried out by a stripping process in which the protecting material is dissolved, swollen, or otherwise disintegrated and separated from the underlying surface, while leaving the micropatterned MXene and underlying substrate substantially intact.
[0111] For polymer-based protecting materials, including photoresists, the removal process may be implemented using solvent-based stripping techniques commonly employed in lithographic processing. The stripping composition may comprise one or more solvents selected based on the chemical nature, crosslinking density, and thickness of the protecting material. Suitable solvents include organic solvents and aqueoussolvents such as, but not limited to, acetone, acetonitrile, ethanol, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, water, and combinations thereof. By way of example, acetone, tetrahydrofuran, or combinations thereof may be used to dissolve or lift-off acrylate-based or epoxy-based photoresists, while dimethyl sulfoxide or dimethylformamide may be employed for more chemically resistant or partially crosslinked materials. Water or water-containing solvent mixtures may be used to remove protecting materials that are water-soluble or water-swellable.
[0112] The stripping process may be carried out by immersing the substrate in the stripping composition, by dispensing or flowing the stripping composition over the substrate surface, or by a combination thereof. Removal may be conducted at ambient temperature or at an elevated temperature selected to accelerate dissolution of the protecting material, provided the temperature remains below levels that would degrade the MXene layer(s) or the substrate. Agitation may be employed to facilitate removal, including stirring of the stripping composition, movement or rotation of the substrate, and / or application of ultrasonic energy. Ultrasonic assistance, in particular, may promote lift-off of the protecting material from patterned features without mechanical abrasion.
[0113] In the case of photoresist materials, removal of the protecting material may be regarded as a photoresist stripping or resist-stripping step, with the duration of stripping selected to achieve substantially complete removal from the first region without adversely affecting the patterned MXene layer(s) or the substrate. Following removal, the substrate may be rinsed with a compatible liquid to remove residual dissolved material and then dried, thereby leaving the patterned MXene layer(s) exposed for subsequent processing or use.
[0114] The patterned MXene structures obtained by the processes disclosed herein exhibit high uniformity across patterned features, including improved thickness uniformity and surface uniformity relative to patterned MXene produced using previously available techniques, such as conventional lift-off processes. In particular, the transition between patterned edges and interior regions of the MXene features is substantially uniform, resulting in reduced edge thickness accumulation and improved surface planarity. In some implementations, the difference in height between edges of the patterned MXene features and corresponding central regions is less than about 10%, optionally less than about 5%,less than about 3%, or less than about 1%, thereby providing MXene patterns with highly uniform thickness profiles.
[0115] The patterning approaches described herein further enable formation of MXene features with fine lateral resolution. The achievable lateral resolution of the patterned MXene may be governed primarily by the resolution of the lithographic pattern used to define the protecting material, rather than by limitations of the MXene processing itself. Accordingly, lateral resolutions of about 200 nm or less may be obtained, allowing formation of micron-scale and sub-micron MXene patterns suitable for use in advanced device architectures.
[0116] While the process described herein may be carried out in various sequences, an alternative approach is provided in which micropatterned MXene is formed by depositing the MXene layer onto a substrate that is already patterned with a protecting material. In this sequence, a MXene layer is first deposited over a patterned substrate comprising regions covered by the protecting material and regions left exposed. The deposited MXene conforms to the surface topography of the patterned substrate, covering both the protecting material and the exposed substrate regions.
[0117] Following deposition, salt residues remaining from MXene synthesis, processing, or deposition are removed from the MXene layer(s). Salt removal may be carried out as described hereinabove subjecting the formed MXene layer(s) to acidic treatment, in order to dissolve the residual salt species. This step improves the electrical, chemical, and structural properties of the MXene layer(s) and prepares the material for subsequent processing.
[0118] After removal of the salt residues, the protecting material is removed from the substrate, thereby lifting-off MXene portions that were deposited on the protecting material. Removal of the protecting material may be performed using the stripping or dissolution techniques described herein, resulting in selective retention of the MXene pattern in regions corresponding to portions of the substrate that were not covered by the protecting material, while MXene deposited over the protecting material is removed. In this manner, a micropatterned MXene structure is obtained that reflects the pattern defined by the protecting material, without requiring etching of the MXene layer itself.
[0119] The patterned MXene structures produced by the disclosed processes may beincorporated into a wide range of microelectronic and related products. Such products may include, without limitation, microelectronic target devices, integrated circuits, flexible or transparent electronic devices, and other systems requiring spatially defined conductive or functional materials.
[0120] In these applications, the MXene thin film may serve as a functional layer within a device stack, coating, or structure. For example, the MXene thin-film may function as a membrane, electrode, interconnect, barrier layer, sensing layer, or as an electromagnetic, optical, thermal, or electrochemical functional film, depending on device requirements and MXene composition. The uniformity and pattern definition achieved by the processes disclosed herein facilitate reliable integration of MXene materials into such devices while maintaining desired functional performance.
[0121] The term “about” as used herein refers to ±10% of a specified value. The term “ambient temperatures” as used herein refers to 25°C±5°C.
[0122] Throughout the description and claims, the words “comprise” and “contain” and variations of the words, for example “comprising” and “comprises”, mean “including but not limited to”, and are not intended to (and do not) exclude other moieties, additives, components, integers or steps.
[0123] As used herein, the singular forms “a”, “an”, and “the” include plural forms unless the context clearly dictates otherwise. Thus, it is to be understood that reference to “a MXene layer” also includes a plurality of MXene layers as is known to those skilled in the art. In another example, reference to “a surfactant” also includes a plurality of surfactants.
[0124] As used herein, the term “and” or the term “or” include “and / or” unless the context clearly dictates otherwise.
[0125] Various embodiments and aspects of the present invention as delineated hereinabove and as claimed in the claims section below find experimental support in the following examples.EXAMPLES
[0126] Methods
[0127] MAX phase synthesis
[0128] Titanium carbide (TiC, 99.5%, Alfa Aesar), titanium (Ti, 99.7%, Strem), and aluminum (Al, 99.7%, Strem) powders were mixed in a 2: 1:1.1 ratio and tumbler-mixed with stainless steel balls at 200 rpm for 18 h. The blended powders were compacted into a pellet under a pressure of 5 MPa at room temperature. The green body pellet was heat-treated under an argon atmosphere in a tube furnace at 1,450 °C for 3 h, with a heating / cooling rate of 5 °C / min. The obtained TisAICi MAX phase pellet was ground and sieved to obtain a powder with a particle size of <20 pm.
[0129] MXene synthesis
[0130] TisCiTz MXene was synthesized by selectively etching TisAICi. 1 g of MAX powder was slowly added to 20 ml of 10.2 M HC1 (32%, Bio-Lab) with 1.6 g of lithium fluoride (LiF, 99%, Strem) at 45 °C and stirred for 24 h. After etching, the mixture was centrifuged at 3,500 rpm several times with DI water until the pH reached 6. To exfoliate the MXene, the suspension was sonicated in an ultrasonic bath for 30 min while being kept at 5 °C. After sonication, the suspension was centrifuged at 3,500 rpm for 30 min to separate any unexfoliated sediment. The MXene colloidal solution was bubbled with N2 for 15 min and stored at 4 °C. 5 ml of the colloid was dried and weighed to determine the MXene concentration, which was approximately 14 g / L.
[0131] MXene thin film deposition
[0132] MXene deposition was performed as detailed in Favelukis, B., et al. Nanoscale Adv 7, 2329-2337 (2025), the contents of which are hereby incorporated in their entirety. Multiple wafer substrates were piranha-treated using a 1:3 H2O2 / H2SO4 solution, respectively, (H2SO498%, SDFCL; H2O2 35%, ThermoFisher Scientific) to increase hydrophilicity. Si (4”, n-type, p-doped, 1-100 Q-cm, University Wafers), SiCL (4”, n-type, 100 nm wet thermal oxide, University Wafers), and fused silica (4”, University Wafers) wafers were spin-coated with MXene diluted to 7 g / L at 2,000 rpm for 1 min, followed by spin-cleaning with 0.5 M HC1 at 2,000 rpm for 1 min, resulting in an 8 nm-thick MXene film.
[0133] MXene wet etching
[0134] First, the MXene-coated wafers were heated to 200 °C for 5 min to remove residual water from the MXene. They were then spin-coated with HMDS (99%, Sigma-Aldrich) at 3,000 rpm for 40 s and heated again to 200 °C for 5 min. The MXene electrode was patterned by photolithography; the substrate was spin-coated with Futurrex NR-1500PY negative photoresist at 3,000 rpm for 40 s, baked at 150 °C for 1 min, exposed with 285 mJ / cm2using SUSS MA6 as a mask aligner, post-baked at 100 °C for 1 min, and developed in RD6 solution for 17 s. For process calibration, some of the wafers were diced using a Disco DAD300 dicing saw.
[0135] MXene removal by wet etching was performed using a 1:3 H2O2 / HCI solution with 0.5% vol of Triton X-100 for different etching times. After etching, the photoresist was removed using acetone, IPA, and water.
[0136] Characterization
[0137] X-ray diffraction (XRD) measurements of the freestanding MXene film and the etched by-products were performed over a 29 range of 3-85° with 0.02° steps using a Malvern Panalytical Aeris diffractometer.
[0138] X-ray photoelectron spectroscopy (XPS) analysis was carried out with an ESCALAB QXi (Thermo Scientific).
[0139] The morphology of the MXene electrode was examined via high-resolution scanning electron microscopy (SEM) using a ZEISS Gemini 300.
[0140] Atomic force microscopy (AFM) measurements were performed using the MFP-3D-Bio system (Asylum Research / Oxford Instruments) with an Olympus AC160TS probe (nominal o = 300 kHz, k = 26 N / m). The scans were taken in AC mode with a free amplitude (Ao) set to 2.34 V (200 nm) and a setpoint amplitude (As) of 1.423 V (125 nm), approximately 63% of Ao.
[0141] Scanning transmission electron microscopy (STEM) imaging of the MXene thin-film cross-section was performed with a probe Cs-corrected (S-CORR) Thermo Fisher Spectra 200 operating at 200 kV (Figures 2A-2C). The lamella for STEM analysis wasprepared using a dual-beam focused ion beam (FIB; FEI Helios G4 UC). Electrical measurements were carried out with a Keithley 4200A I-V / C-V probe system. Electrical conductivity was measured using a 4-point probe configuration by applying currents of 1-10 pA and recording the induced voltage. The performance of the MSM photodiode was analyzed with a 2-point probe configuration, using 0.04 V step increments under varying white LED illuminations ranging from 0.08 to 1.38 mW / cm2. The undercut etching rate was calculated through image analysis using ImageJ software.
[0142] EXAMPLE 1
[0143] Wet etching of MXene thin films using several mixtures of H2O2 and different acids (sulfuric, nitric, and hydrochloric) at a ratio of 1:3 was performed demonstrating highly controllable etching of MXene freestanding films. The oxyhalide by-products dissolved and only TiOxnanoparticles remained (Figures 3A-3C), which impart an orange color to the solution (Figures 4A-4C). The H2O2-HCI solution was chosen for patterning the MXene film due to the stability of common commercial photoresists in HC1, allowing to etch at high concentrations. Figures 5A-5C show SEM micrographs of an 8 nm-thick MXene thin-film deposited by spin coating on a silicon wafer before etching, after 2 min, and after 5 min of etching, respectively. The XPS measurements, shown in the upper right inserts of Figures 5A-5C, reveal that during the etching of the MXene flakes, most of the Ti in the MXene is not oxidized but removed into the solution. After 5 min of etching, small areas of unetched MXene still remained and did not completely disappear by increasing the etching time. This was attributed to bubbles that adhered to the MXene surface (Figure 6), blocking the etchant. The addition of a surfactant was performed to increase the surface tension and reduce the gas bubble size thereby affording complete etching.
[0144] Controlled patterning of the MXene thin-film was achieved using photolithography, as illustrated in Figure 1. The photoresist covering the flake surface significantly decreased the etching rate of the film, thus allowing regulation primarily through single-edge etching. The MXene flake morphology after 0, 2, and 5 min of etching (Figures 7A-7C) illustrates the etching mechanism: etching of uncovered MXene progresses through the flake edges coupled with pinholes forming new edges in the basalplanes. The flake basal planes covered by additional flakes etch gradually (Figure 7B), while after complete etching of all layers, the etching progresses homogeneously by the flake edges under the photoresist-protected area (Figure 7C). The resulting features exhibit an edge roughness of less than 100 nm, as shown in Figures 7C, 8A-8D, 9A-9H, and 10A-10D.
[0145] After MXene deposition, residual water remains between the flakes, which desorbs during heating. Therefore, the MXene were heated above the photoresist baking temperature to prevent bubble formation under the photoresist caused by water degassing (Figure 11). TisCiTz can withstand heating in an ambient atmosphere up to 245 °C without oxidation. Photoresist adhesion was ensured by spin coating with hexamethyldisilazane (HMDS) followed by heating at 200 °C. The MXene surface is highly hydrophilic due to -O and -OH terminations, causing photoresist adhesion issues and uneven etching (Figure 12). HMDS reacts with the MXene terminations, adding imido and amido silicate complexes to the MXene terminations, as measured by XPS (Figures 13A-13H), improving photoresist adhesion.
[0146] A major advantage of the wet etching approach is that it is readily adaptable to wafer scale. Figure 14 shows a 4-inch silicon oxide wafer with a high yield of 1x1 cm2dies with well-defined, sharp electrodes (Figure 15). The process was also demonstrated on 4-inch fused silica, as shown in Figures 16A-16B. By the end of the process, the electrode surface remains undamaged, as shown in the SEM micrographs (Figures 7A-7C and 8A-8D), and in the cross-sectional TEM micrograph (Figure 17) thus exhibiting the straightforward scalability potential of MXene patterning by wet etching using common techniques and materials in the microelectronics industry.
[0147] EXAMPLE 2
[0148] MXene electrodes are hitherto commonly patterned by a lift-off process due to its simplicity. A comparison of the wet etching according to some embodiments of the present invention to the state-of-the-art patterning by lift-off was performed on the same type of deposited MXene thin-film and electrode design. A clear advantage of the wet etching process was seen in comparative thickness profiles obtained by AFM cross-sectional scans (Figure 18A). This was also evident by the SEM micrographs ofelectrodes patterned by lift-off (Figure 18B) vs. wet etching (Figure 18C). It can be clearly seen that the wet-etched electrodes exhibit dramatic improvement in lateral resolution and thickness uniformity. AFM thickness profiles (Figures 18D-18F) and their corresponding area scans (Figures 18G-18I) are shown for different- sized electrodes, and average height profile in an over-etched sample is shown in Figures 18D-18I. The average edge profile reveals a stepped structure corresponding to the number of MXene flakes at the smallest electrode marked by arrows (in Figure 18D), which becomes less prominent in the wider electrodes, leading to nearly vertical edges.
[0149] The comparative characteristics of different MXene thin-film micropatterning methods are presented in Table 1. The wet etching process offers several advantages, combining excellent lateral resolution with high selectivity, throughput and scalability, as well as short processing time and low cost (both in reagents and equipment) under ambient conditions. Notably, it yields precise MXene patterning with lateral resolution on par with RIE, while using much simpler and cost-effective means.
[0150] Table 1. Comparison of MXene micropatterning method and their properties.
[0151] .s S £ -a 5 2 | £ £ 2 o 2 2P ~ £ S J S H § % £ £ § S* U
[0152]
[0153] Wet
[0154] 200 nm High High High Low Low etching
[0155] RIE 100-200 nm High Low High High High Lift-off 1.5-25 pm Medium Low Medium Low Low Contact
[0156] 5-300 pm Low Low Low Low Low printing
[0157] EXAMPLE 3
[0158] The undercut etching rate of MXene films is critical in integrated circuit fabrication processes, where etching must be controlled to maintain feature dimensions and prevent excessive undercutting beneath other structures (Konstantinova, T. G. el al.Scientific Reports 13, 1-9 (2023)). The MXene undercut etching rate was calculated by etching different samples for 1-8 min (Figures 9A-9H) and measuring the electrode dimensions. The dimensions after etching for 4, 6, and 8 min can be seen in the SEM micrographs in Figures 19A-19C. As with conventional isotropic etching, the electrode size decreases beneath the photoresist, rounding the corners of the features. This occurs due to the cumulative effect of multidirectional etching, which removes more material from the corners than from straight edges or flat surfaces, gradually rounding them over time. The undercut etching rate graph shown in Figure 20 starts after the electrodes are completely disconnected at 2 min of etching time. Complete removal of MXene residue from the uncovered surfaces is observed at 3 min (Figures 9A-9H and 10A-10D), contemplated as the limit for -200 nm features under the employed etching conditions (i.e., 1:3 IFC HCI 0.5 vol.% Triton X-100 at room temperature).
[0159] Without being bound by any theory or mechanism of action, improving the lateral resolution below -200 nm would require enhancing the surface (basal plane) etching while minimizing the flake edges etching. This could be achieved by fine-tuning the etching parameters, conceivably by adjusting the FhCh / acid solution concentration and etching temperature, or finding an alternative etchant with basal plane selectivity. Additionally, control over the etching rate can vary between MXene synthesis types, flake sizes, and stoichiometries.
[0160] EXAMPLE 4
[0161] Electrical properties were measured to assess the performance of the wet-etched MXene electrodes. The IV curve presented in Figure 21 shows the electrical conductivity of patterned MXene electrodes etched at 4, 6 and 8 min on SiOi. measured using a four-point probe configuration with an initial width of 20 pm, as shown in the upper insert of Figure 21. The MXene electrode shows conductivity of 1100-1746 S-cm'1typical to multi-flaked MXene films. The profile measurement shown in the bottom insert of Figure 21 illustrates that although the electrode width decreases by approximately 20% between 4 and 8 min of etching, the electrical conductivity decreases by 37% S-cm'1. Without being bound by any theory or mechanism of action, this non-linear relationship is likely due to an inhomogeneous etching effect that becomes more apparent with extendedetching times (as shown in the AFM scan in Figure 18G). MXene comb-shaped electrodes were patterned by 4 min etching on n-type Si to create MXene-Si-MXene (MSM) Schottky junction, which were tested as photodetectors. The IV curve shown in Figure 22 demonstrates that the MSM junctions exhibit high sensitivity to light across various illumination intensities, even under relatively low photon flux, with a responsivity of 11.03 AAV.
[0162] The foregoing description of the specific embodiments will so fully reveal the general nature of the invention that others can, by applying current knowledge, readily modify and / or adapt for various applications such specific embodiments without undue experimentation and without departing from the generic concept, and, therefore, such adaptations and modifications should and are intended to be comprehended within the meaning and range of equivalents of the disclosed embodiments. It is to be understood that the phraseology or terminology employed herein is for the purpose of description and not of limitation. The means, materials, and steps for carrying out various disclosed functions may take a variety of alternative forms without departing from the invention.
Claims
CLAIMS1. A process for preparing micropatterned MXene comprising the steps of:(i) depositing a MXene layer on a substrate, wherein the MXene is characterized by the general formula of Mn+iXnTz, wherein M is selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W; X is selected from the group consisting of C, N, and a combination thereof, n is an integer from 1 to 4, and Tzis a surface termination group;(ii) applying a protecting material onto a first region of the MXene layer;(iii) selectively etching a second region of the MXene layer using an aqueous medium comprising an oxidant and an acid; and(iv) removing the protecting material from the first region thereby obtaining micropatterned MXene.
2. The process of claim 1, wherein M is Ti.
3. The process of claim 1 or 2, wherein X is C.
4. The process of any one of claims 1 to 3, wherein n is 2.
5. The process of any one of claims 1 to 4, wherein Tzis selected from the group consisting of hydroxyl, oxo (oxide), halogen, chalcogen, hydride, alkoxide, carboxylate, sub-oxide, nitride, sub-nitride, sulfide, thiol, and a combination thereof.
6. The process of any one of claims 1 to 5, wherein the substrate comprises a carbide, a nitride, or an oxide.
7. The process of any one of claims 1 to 5, wherein the substrate comprises a III- V group compound.
8. The process of any one of claims 1 to 5, wherein the substrate comprises silicon, silicon oxide, fused silica, sapphire, glass, or mica.
9. The process of any one of claims 1 to 8, wherein the substrate has two opposing surfaces and is in the form of a wafer, a chip, or a disk.
10. The process of any one of claims 1 to 9, wherein step (i) is performed by at least one of spray coating, dip coating, spin coating, screen printing, blade casting, inkjet printing, Langmuir-Blodgett, and chemical vapor deposition.
11. The process of any one of claims 1 to 10, wherein the deposited MXene layer is characterized by a thickness ranging from about 1 nm to about 20 pm.
12. The process of any one of claims 1 to 11, wherein the protecting material comprises a photoresist material.
13. The process of claim 12, wherein the photoresist material is selected from the group consisting of hexamethyldisilazane (HMDS), SU-8 (epoxy-based negative photoresist), polyvinylcinnamate (PVCN), diazonaphthoquinone (DNQ)-novolac resists, poly(methyl methacrylate) (PMMA) and other acrylate- based resists, phenolic resin-based resists, chemically amplified photoresists (CARs), and a combination thereof.
14. The process of claim 12 or 13, wherein step (ii) comprises applying a dispersion comprising the photoresist material onto the MXene layer and patterning the first and second regions via UV exposure and subsequent development.
15. The process of any one of claims 1 to 14, wherein the oxidant is selected from the group consisting of hydrogen peroxide, a metal peroxide, a metal superoxide, carbamide peroxide, benzoyl peroxide, and a combination thereof.
16. The process of claim 15, wherein the oxidant is hydrogen peroxide.
17. The process of any one of claims 1 to 16, wherein the acid is selected from the group consisting of hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, and a combination thereof.
18. The process of claim 17, wherein the acid is hydrochloric acid.
19. The process of any one of claims 1 to 18, wherein the aqueous medium in step (iii) comprises an oxidant and an acid at a volume ratio of about 5:1 to about 1:10.
20. The process of any one of claims 1 to 19, wherein step (iii) is performed at a temperature of about 10°C to about 60 °C.
21. The process of any one of claims 1 to 20, wherein step (iii) is performed for a time duration ranging from about 1 s to about 15 min.
22. The process of any one of claims 1 to 21, wherein the aqueous medium in step (iii) further comprises a surfactant.
23. The process of claim 22, wherein the surfactant is a non-ionic surfactant, an anionic surfactant, or a cationic surfactant.
24. The process of claim 22 or 23, wherein the surfactant comprises at least one of polyethylene glycol, polysorbate, stearyltriethanolamine, sodium lauryl sulfate, sodium taurocholate, laurylaminopropionic acid, lecithin, benzalkonium chloride, benzethonium chloride, glycerin monostearate, polyvinyl alcohol, polyvinylpyrrolidone, carboxymethylcellulose sodium, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose.
25. The process of claim 24, wherein the surfactant is a polyethylene glycol, preferably polyethylene glycol p-(l,l,3,3-tetramethylbutyl)-phenyl ether.
26. The process of any one of claims 1 to 25, wherein step (iv) is performed by dissolving the protecting material.
27. The process of claim 26, wherein dissolving the protecting material comprises the use of at least one of acetone, acetonitrile, ethanol, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, tetrahydrofuran, water, and combinations thereof.
28. The process of any one of claims 1 to 27, further comprising a step of removing salt residues from the MXene layer.
29. The process of claim 28, wherein the step of removing salt residues from the MXene layer is performed following step (i) and prior to step (ii).
30. The process of claim 28, wherein the step of removing salt residues from the MXene layer is performed following step (iv).
31. The process of any one of claims 28 to 30, wherein the salt residues are selected from the group consisting of lithium fluoride, lithium chloride, tetramethylammonium hydroxide, and a combination thereof.
32. The process of any one of claims 28 to 31, wherein removing salt residues from the MXene layer is performed by dissolving the salt residues in an acid.
33. The process of claim 32, wherein the acid is selected from the group consisting of hydrochloric acid, hydrobromic acid, sulfuric acid, phosphoric acid, nitric acid, carbonic acid, and a combination thereof.
34. The process of claim 32 or 33, wherein dissolving the salt residues in an acid is performed while spinning at a rate about 500 to about 5,000 rpm for a time duration ranging from 1 s to 10 min.