Optical switches based on magnetic metal-organic frameworks

Magnetic MOFs with embedded nanoparticles allow controlled orientation and alignment, addressing the limitations of traditional MOFs by enabling reversible optical switching and advanced display technology.

WO2026239388A1PCT designated stage Publication Date: 2026-11-19YEDA RES & DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IL2026/050404
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies lack the ability to effectively control the orientation and position of metal-organic frameworks (MOFs) for enhanced optical properties and functionality, limiting their efficiency in devices.

Method used

The development of magnetic metal-organic frameworks (MOFs) with embedded magnetic nanoparticles allows for controlled orientation and alignment of these structures using external magnetic fields, enabling opto-magnetic switches and display technology applications.

Benefits of technology

This approach enables reversible optical switching and synchronized motion of MOFs under magnetic fields, providing a platform for advanced optical switches and display systems with enhanced functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IL2026050404_19112026_PF_FP_ABST
    Figure IL2026050404_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is directed to the field of opto-magnetic switches, devices and their related systems and methods. The devices and switches comprise porous anisotropic-shaped nanoparticles such as metal-organic frameworks (MOFs) with magnetic nanoparticles attached on the surface. These magnetic anisotropic nanoparticles are configured for particular orientations to enable a variety of electro-optic responses under the influence of external forces such as magnetic fields.
Need to check novelty before this filing date? Find Prior Art

Description

P-632909-PCOPTICAL SWITCHES BASED ON MAGNETIC METAL-ORGANIC FRAMEWORKS FIELD OF THE INVENTION

[0001] The presently disclosed subject matter relates to the field of opto-magnetic switches, devices and their related systems and methods. The devices and switches comprise porous anisotropic-shaped nanoparticles such as metal-organic frameworks (MOFs) with magnetic nanoparticles attached on the surface. These magnetic anisotropic nanoparticles are configured for particular orientations to enable a variety of electro-optic responses under the influence of external forces such as magnetic fields.BACKGROUND

[0002] Metal-organic frameworks (MOFs) constitute a class of crystalline porous materials composed of inorganic and organic groups, connected to form 3D structures. The high surface area of MOFs, together with the ability of capturing molecules inside the different pores and channels, makes such crystals ideal candidates for storage, separation and catalysis. The ability to control the position of MOFs is crucial for their use in devices, as their properties can be confined to a controlled location, therefore increasing the devices efficiency. MOFs position can be oriented by directed growth on functionalized surfaces or specific patterns using lithography or by fixing their orientation in cured polymer resins. MOF -based magnetic nanocomposites are of particular interest, due to the possibility of positioning and collecting them using an external magnetic field. Magnetic MOFs have several uses, among them the use as magnetic nano catalysts that can be recycled several times, as dye-adsorbents or as sustainable environment adsorbents of hazardous components from the environment.

[0003] In this present disclosure anisotropic micro-size structures whose orientation and position, and hence function, can be controlled. Properties are being introduced to molecularbased, monodisperse crystals that cannot be achieved solely by a predesigned crystallization process. Changing the orientation of such optically functionalized crystals with a magnetic field under polarized light will affect their optical properties. Motion is induced by a magnetic field using nano- and micron-sized crystals that are coated with magnetic nanoparticles. The magnetically responsive particles of the present disclosure, micro-size crystals having embedded and aligned chromophores can find applications as optical switches and in display technology.P-632909-PCSUMMARY

[0004] In one embodiment the invention provides an opto-magnetic switch comprising:a substrate;porous anisotropic-shaped nanoparticles with magnetic nanoparticles (MNPs) attached on the surface of the porous anisotropic-shaped nanoparticles, resulting in magnetic anisotropic nanoparticles;a solvent or gel within which the magnetic anisotropic nanoparticles are dispersed; andwherein the magnetic anisotropic nanoparticles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0005] In one embodiment the porous anisotropic-shaped nanoparticles comprise metal organic frameworks (MOFs). In one embodiment the anisotropic shape is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism. In one embodiment the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof. In one embodiment the MNPs are selected from: FesCU, y-Fe2O3, FeCo, FeCoFe2O4, NiFe2O4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao.sSro.sCoCh, or a combination thereof. In one embodiment the MNPs further comprise a capping layer. In one embodiment the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HDA), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochloride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinyl alcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof. In one embodiment the porous anisotropic-shaped nanoparticles further comprise at least one dye incorporated therein. In one embodiment the dye is selected from: optical, fluorescent, or a combination thereof. In one embodiment the dye comprises any of the following selected from: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5 -aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7,7,8, 8-tetracyanoquinodimethane (TCNQ). In one embodiment the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane,P-632909-PCcyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or a combination thereof. In one embodiment the opto-magnetic switch further comprises an encapsulation layer. In one embodiment the substrate and the encapsulation layer comprise any of the following selected from: glass, AI2O3, quartz, silicon oxide, fluorinedoped tin oxide (FTO), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), cyclo-olefin polymer (COP), cyclo-olefin copolymer (COC), polymethyl methacrylate (PMMA, acrylic), and polycarbonate (PC), or a combination thereof.

[0006] In one embodiment the invention provides a display system or interface comprising the opto-magnetic switch of the invention.

[0007] In one embodiment the invention provides an opto-magnetic system comprising:the opto-magnetic switch of the invention;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; anda magnetic-field inducing apparatus configured to generate a varying magnetic field, thereby controlling the position and / or orientation of the magnetic anisotropic nanoparticles within the opto-magnetic switch;wherein the position and / or orientation of the magnetic anisotropic nanoparticles relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.

[0008] In one embodiment the porous anisotropic-shaped nanoparticles are metal organic framework (MOF) particles, and wherein the magnetic anisotropic nanoparticles are magnetic MOF (mMOF) particles. In one embodiment the analyzer is positioned perpendicular to the polarizer. In one embodiment the polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer. In one embodiment the light source is selected from: laser, or light-emitting diode (LED). In one embodiment the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof.

[0009] In one embodiment the opto-magnetic system further comprises a controller configured to:implement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the magnetic anisotropic nanoparticles; orP-632909-PCimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.

[0010] In one embodiment the invention provides an opto-magnetic device comprising:a substrate;a film comprising porous anisotropic-shaped nanoparticles with magnetic nanoparticles (MNPs) attached on the surface of the porous anisotropic-shaped nanoparticles, resulting in a magnetic anisotropic nanoparticles; and wherein the magnetic anisotropic nanoparticles are permanently aligned in a predetermined direction.

[0011] In one embodiment the porous anisotropic-shaped nanoparticles comprise metal organic framework (MOF) particles. In one embodiment the anisotropic shape and / or structure is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism. In one embodiment the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof. In one embodiment the MNPs are selected from: FesC , y-Fe2O3, FeCo, FeCoFe2O4, NiFe2O4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao.sSro.sCoCh, or a combination thereof. In one embodiment the MNPs further comprise a capping layer. In one embodiment the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HDA), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochloride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinyl alcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof. In one embodiment the porous anisotropic-shaped nanoparticles further comprise at least one dye incorporated therein. In one embodiment the dye is selected from: optical, fluorescent, or a combination thereof. In one embodiment the dye comprises any of the following selected from: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5 -aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7, 7,8,8-tetracyanoquinodimethane (TCNQ). In one embodiment the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane, cyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or aP-632909-PCcombination thereof. In one embodiment the opto-magnetic device further comprises an encapsulation layer. In one embodiment the substrate and the encapsulation layer comprise any of the following selected from: glass, AI2O3, quartz, silicon oxide, fluorine-doped tin oxide (FTO), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), cyclo-olefin polymer (COP), cyclo-olefin copolymer (COC), polymethyl methacrylate (PMMA, acrylic), and polycarbonate (PC), or a combination thereof.

[0012] In one embodiment the invention provides an opto-magnetic device system comprising:the opto-magnetic device of the invention;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; andwherein the position and / or orientation of the magnetic anisotropic nanoparticles relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.

[0013] In one embodiment the magnetic anisotropic nanoparticles comprise metal organic framework (MOF) particles. In one embodiment the analyzer is positioned perpendicular to the polarizer. In one embodiment the polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer. In one embodiment the light source is selected from: laser, or light-emitting diode (LED). In one embodiment the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof.

[0014] In one embodiment the opto-magnetic system further comprises a controller configured to:implement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the magnetic anisotropic nanoparticles; orimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.

[0015] In one embodiment the invention provides a method of fabricating an opto-magnetic device, the method comprising:providing a substrate;P-632909-PCproviding a solvent or gel comprising magnetic anisotropic nanoparticles, resulting in a magnetic anisotropic nanoparticles;dispersing the magnetic anisotropic nanoparticles on the substrate; evaporating or curing the solvent or gel whilst the magnetic anisotropic nanoparticles are oriented in a predetermined direction by an external magnetic field thereby resulting in the magnetic anisotropic nanoparticles being permanently oriented in the predetermined direction on the substrate.

[0016] In one embodiment the evaporating comprises any of the following selected from: vacuum drying, gas flow drying, thermal drying, or a combination thereof. In one embodiment the curing is carried out at a temperature ranging between 100 to 200 °C.

[0017] In one embodiment the invention provides a method of producing magnetic metalorganic framework (mMOF) particles, the method comprising:providing metal-organic framework (MOF) particles dispersed in a first solvent, resulting in a first MOF dispersion;drying the first MOF dispersion until the first solvent is evaporated, resulting in dried MOF particles;dispersing the dried MOF particles in a second solvent, resulting in a second MOF dispersion;dispersing magnetic nanoparticles (mNPs) in a third solvent, resulting in a mNPs dispersion;adding the mNPs dispersion to the second MOF dispersion, resulting in a mNP / MOF dispersion;incubating the mNP / MOF dispersion, resulting in a mMOF particles dispersion.

[0018] In one embodiment the first solvent, second solvent, and third solvent comprise any of the following selected from: ethanol, methanol, isopropanol, dimethylformamide (DMF), toluene, and hexane, or a combination thereof. In one embodiment the magnetic nanoparticles comprise iron oxide nanoparticles (IONPS). In one embodiment the drying is carried out by: blowing gas, heating, and vacuum pumping, or a combination thereof. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 1 mg / mL to 20 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 1 mg / mL to 20 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.1 mg / mL to 1 mg / mL. In one embodiment the method further comprises adding a fourth solvent to theP-632909-PCmNP / MOF dispersion. In one embodiment the fourth solvent comprises any of the following selected from: ethanol, methanol, isopropanol, dimethylformamide (DMF), toluene, and hexane, or a combination thereof. In one embodiment the method further comprises centrifuging the mNP / MOF dispersion at least once, before the incubating step. In one embodiment the centrifuging is carried out at spinning rate ranging between 3000-5000 rpm and for a duration ranging between 30 seconds to 20 minutes.BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to better understand the subject matter that is disclosed herein and to exemplify how it may be carried out in practice, embodiments will now be described, by way of non-limiting example only, with reference to the accompanying drawings, in which:

[0020] Figure 1 shows an optical microscopy set-up for moving the mMOFs.

[0021] Figure 2A shows optical microscopy and Figure 2B shows SEM images of Ni-MOFs.

[0022] Figure 3 shows TEM images of the iron oxide nanoparticles (IONPS) dispersed in toluene (top-right) with a diameter of 9 ± 1 nm).

[0023] Figure 4A shows an experimental setup; comparison between magnetic metal-organic frameworks (mMOFs) and IONPs' behavior in a magnetic field. Figure 4B shows a photo of uncoated MOFs. Figure 4C shows a photo uncoated IONP. Figure 4D shows a photo uncoated mMOF. Figure 4E shows the mMOFs' location (rectangle) after vial rotation clockwise. Figure 4F shows the change in mMOFs' location (square), attracting to magnet.

[0024] Figure 5A shows a scheme for MOFs with magnetic nanoparticles. Figure 5B-5E shows SEM images of magnetic MOFs (Ni-mMOF). Images of Ni-mMOF were taken immediately after centrifugation, solvent removal and washing with DMF. Figure 5B (SE2 image) and Figure 5C (energy-selective backscattered (EsB)) show SEM images of Ni-mMOF s after 1 day reaction time. Figure 5D (SE2 image) and Figure 5E (EsB) show SEM images of Ni-mMOF after a reaction time of 3 days

[0025] Figure 6A shows SEM images of ‘ 1 day’ Ni-mMOF s, freshly synthesized, and Figure 6B shows 3 months after keeping Ni -mMOFs in 0.5 mL DMF.

[0026] Figure 7 shows EDS spectra and mapping of a Ni-mMOF after a reaction time of 3 days. The elements Fe and O can be seen on areas where carbon is masked by the IONP. Red frame: enlarged area of the mMOF.

[0027] Figures 8A-8D show optical microscopy and SEM images of Ni -mMOFs before (Figure 8A, 8C) and after (Figure 8B, 8D) centrifugation.P-632909-PC

[0028] Figures 9A-9E show SEM images of Cu-MOF (Figs. 9A, 9B) and Cu-mMOF (Figs.9C, 9D, 9E)

[0029] Figure 10A-10C show SEM images of a Cd-MOF after lONP-coating. Figure 10A shows SE2 detector and Figure 10B shows BSE detector. Figure 10C shows a zoom-out of the coated MOFs (Top right: Optical microscopy images of the MOF before and after coating).

[0030] Figures 11A-11D show representative SEM images of Ni-mMOFs before (left column) and after (right column) applied parameters. Figure 11A shows 5 months waiting time after drop-casting (solid state). Figure 11B shows magnetic exposure of vial containing Ni-mMOFs in DMF to a Nd magnet (0.33 T) for 30 min. Figure 11C shows drop-casting mMOFs while placing a Nd magnet below, and wait for solvent (DMF) evaporation. Figure 11D shows one-minute sonication in DMF.

[0031] Figure 12 shows Micro-Raman spectra of Ni-MOFs and Ni-mMOFs.

[0032] Figures 13A-13C show M-H SQUID graphs for: uncoated Ni-MOFs (Figure 13A), Ni-mMOFs (Figure 13B), IONP (Figure 13C); powder obtained from the purchased IONP solution.

[0033] Figure 14A shows AFM images of Ni-MOF. Figure 14B shows AFM images of Ni-mMOF.

[0034] Figure 15 shows FTIR spectra of magnetic NP (IONP) and oleic acid (OA). Each line represents an average of 3 measurements.

[0035] Figure 16 shows the combined FTIR spectra of magnetic NP (IONP), oleic acid (OA), AdDB, uncoated Ni-MOFs and Ni-mMOFs. Each line represents an average of 3 measurements.

[0036] Figure 17A shows XPS spectra for the oxygen atom (IS) for uncoated MOFs. Figure 17B shows XPS spectra for the oxygen atom (IS) for mMOFs. The “envelope” line is the sum of the fitting curves and identical of the O Is spectrum.

[0037] Figure 18A shows XPS spectra for the carbon atom (IS) for uncoated MOFs. Figure 18B shows XPS spectra for the carbon atom (IS) for mMOFs. The “envelope” line is the sum of the fitting curves and identical of the C Is spectrum.

[0038] Figure 19A shows XPS spectra for the iron atom (2p) for IONP. Figure 19B shows XPS spectra for the iron atom (2p) for mMOFs.

[0039] Figure 20A shows XPS spectra for the nickel atom (2p) for IONP. Figure 20B shows XPS spectra for the nickel atom (2p) for IONP mMOFs.

[0040] Figures 21A-21B shows dynamic alignment and rotational movement of mMOFs as seen in an optical microscope, under polarized light, transmittance, bright field mode, with polarizer parallel (21 A) and perpendicular (21B) to the analyzer. Scale bar: 10 / / m.P-632909-PC

[0041] Figures 22A-22D show dynamic alignment and rotational movement of mMOFs as observed with a optical microscope, under polarized light, transmittance, bright field mode, with polarizer perpendicular to the analyzer. (Figure 22A) t = 0 s, no external magnetic field, random orientation. (Figure 22B) t = 4 s, mMOFs alignment to an external magnetic field. (Figure 22C) t = 18 s, magnetic field removed, mMOFs are at random orientation. (Figure 22D) t = 19 s, mMOFs alignment to an external magnetic field. Scale bar: 10 / / m.

[0042] Figures 23A-23C show dynamic alignment and translocation of mMOFs as observed with an optical microscope under non-polarized light, using reflectance, dark field mode. The center of each MOF was marked with a yellow dot during the video from the start (Figures 23A) to end of video (Figures 23C), recording of the mMOFs’ movement. The dynamic alignment of the mMOFs together, position and orientation simultaneously change, is shown. Scale bar: 10 / m.

[0043] Figures 24A-24B show opptical (24A) and SEM (24B) images of dye-loaded mMOFs under polarized light.

[0044] Figures 25A-25B shows SEM image of magnetic dyed Ni-MOF, in different magnifications. Figure 25A shows the SE2 detector. Figure 25B shows the EsB detector.

[0045] Figures 26A-26B show Dynamic alignment of magnetic dyed MOFs as seen in an optical microscope, under polarized light, bright field mode. (Figure 26A) Polarizer parallel to analyzer. (Figure 26B) Polarizer nearly perpendicular to analyzer, to see the crystals orientation and color in the different modes. Scale bar: 10 / / m.

[0046] Figures 27A-27D show fluorescent images excited at 2exc= 560 nm, collected at 2 = 570-650 nm. Snapshots are taken from videos of fluorescent mMOFs before (Figure 27A) and after (Figures 27B-27D) applying a magnetic field.

[0047] Figures 28A-28C show fluorescent images of dyed mMOFs excited at 2exc= 350 nm, collected at 2 = 410-480 nm. Snapshots are taken from videos of fluorescent dyed-mMOFs before (Figure 28A) and after (Figures 28B-28C) applying a magnetic field.

[0048] Figures 29A-29D show polarized fluorescent images excited at 2exc= 561 nm, collected at 2 = 571-650 nm. Snapshots taken from videos of fluorescent dyed mMOFs before (Figure 29A) and after (Figure 29B-29D) applying a magnetic field. Top row: fluorescence channel. Bottom row: bright field channel.

[0049] Figure 30A shows Normalized intensity vs time of fluorescent mMOFs movement recording. Laser polarization: 90°. Excitation wavelength: 2 = 561 nm. The highest intensity was observed at MOF angle of 0°. Lower intensities were observed in MOF angle of 45°, 90°. FigureP-632909-PC30B shows screenshots of mMOF orientation during video recording are shown below the graphs.

[0050] Figure 31A shows Normalized intensity vs time of fluorescent mMOFs movement recording. Laser polarization: 0°. Excitation wavelength: A = 561 nm. The highest intensity was observed at MOF angle of 45°. Lower intensities were observed in MOF angle of 0°, 90°. Figure 31B shows screenshots of mMOF orientation during video recording are shown below the graphs.

[0051] Figures 32A-32G shows EDS characterization for uncoated Ni-MOFs, immediately after synthesis. Scale bar: 10 «m.

[0052] Figure 33 shows SEM images of Ni-mMOFs before (left) and after (right) 12 h in 110 °C. The Ni-mMOFs were drop-casted on a silicon wafer, examined in SEM, and the silicon wafer was inserted to an oven pre-heated to 110 °C for 12 h.

[0053] Figure 34A shows Dynamic Light Scattering (DLS) measurements of IONP in two solvents: toluene and DMF. Each sample was measured 3 times. Figures 34B-34C show the visual appearance of the tested solutions, TEM images of IONP in toluene and in DMF.

[0054] Figure 35A-35B show SEM images of mMOFs prepared in hexane. Scale bar: 1 um.

[0055] Figures 36A-36B show TEM-EDS images of mMOFs. Scale bar: 1 um. IONPS are bound to the surface of the MOF with retention of the morphology of the MOFs.

[0056] Figures 37A-37C show SEM images of mMOFs immediately after the reaction with IONP, and after 24 hours: before and 5 min after centrifugation re-arrangement.

[0057] Figures 38A-38C show SEM images of mMOFs using 100 uL of Ni Bn -MOFs and Figure 38A shows 5 uL IONP; Figure 38B shows 25 uL IONP; Figure 38C shows 50 uL IONP. Scale bar: 2 «m. The mMOFs were prepared in DMF and centrifuged after 3 days of IONP addition to the MOF solution.

[0058] Figures 39A-39F shows Cross-Nicols polarized images of SR-dyed Ni-MOFs at different angles: 0° (Figure 39A and Figure 39B), 45° (Figure 39C and Figure 39D) and 90° (Figure 39E and Figure 39F). Scale Bar: 10 / z. Left column: unpolarized light. Right column: cross-polarized light. The crystallinity of the MOF is apparent from the observed birefringence.

[0059] Figure 40 shows optical images of dyed Ni-mMOFs under non polarized and polarized light, one week after dye-inclusion (sample kept in solution avoiding light exposure). Scale bar: 10 m.

[0060] Figures 41A-41F show optical images of dyed Ni-MOFs under polarized light.Figures 41A-41C show 5 days after dye inclusion (sample kept in solution avoiding lightP-632909-PCexposure). Figures 41D-41F show 3 months after dye inclusion (sample kept in solution avoiding light exposure), Scale bar: 10 / / m.

[0061] Figures 42A-42B show XPS spectra for the nitrogen atom (IS) for Ni-MOFs (Figure 42A) and Ni-mMOFs (Figure 42B). The “envelope” line is the sum of the fitting curves and identical to the N Is spectrum.

[0062] Figures 43A-43D shows optical images of SR-dyed Ni-mMOFs, 7 months after dye incorporation inside the MOFs with unpolarized light (Figure 43A), and with polarization of 90° (Figure 43B), 45° (Figure 43C) and 0° (Figure 43A, crossed-polarized image).

[0063] Figures 44A-44B show dynamic alignment of SR-dyed mMOFs as seen in an optical microscope, under polarized light, when the polarizer is parallel to the analyzer, dark field mode. In this mode, there is an enhancement of the MOFs’ outer surface and no dichroism of the dye in the crystals is appearing. The (purple) color originates from the fluorophore. Scale bar: 10 / / m.

[0064] Figures 45A-45C show optical (45A) and fluorescence (45B) images of Ni-MOFs, excited at 350 nm, collected at = 410-480 nm. Scale bar: 10 / m. (45C) Fluorescence emission (orange line, excited at 350 nm) and excitation (blue line, emittion wavelength 430 nm) spectra of the ligand (AdDB).

[0065] Figures 46A-46C show fluorescent Ni-mMOFs (Figure 46A) and Fluorescent Ni-MOFs (Figure 46B) Polarized emission dependency graphs. Images shows each MOF under a laser polarization angle of 0° and 90°, in excitation wavelength of = 561 nm. Scale bar: 5 «m (A), 10 iim (B). (Figure 46C) Fluorescence emission (orange line, excited at 561 nm) and excitation (blue line, emittion wavelength 650 nm) spectra of the flourophor (SR).

[0066] Figure 47A shows the formation of nickel -based MOFs. Figure 47B-47C shows the coating of the MOFs with magnetic NPs and group-alignment using a magnetic field (47B).Under polarized light, the birefringent aligned crystals form “on” and “off’ states as they interact with light (47C). Figure 47D-47F shows the formation of fluorescent mMOFs, incorporating fluorophore, and dynamic movement under polarized light.

[0067] Figure 48 shows the synthesis and molecular structure of l,3,5,7-tetrakis{4-[(£)-2-pyridine-4-yl-vinyl]phenyl}admantane (AdDB): (1) Friedel -Crafts alkylation using 1-bromoadmantane and benzene to form 1,3,5,7-tetraphenyladmantane (80%-90% yield), (2) Bromination to form l,3,5,7-tetrakis(4-bromophenyl)admantane (60%-70% yield), (3) Heck coupling with 4-vinylpyridine, resulting in AdDB (50% yield).

[0068] Figure 49 shows MOFs preparation: 1) adding NiBn (dissolved in DMF) and AdDB (dissolved in chloroform) into a glass pressure tube. 2) placing the tube in an oven at 105 °C forP-632909-PC48 h. 3) separation of the crystals from the mother solution by centrifugation (4000 rpm, 5 min) with ethanol.

[0069] Figure 50 shows the MOFs magnetization process: 1) 100 «L solution of cleaned MOFs in ethanol was dried using pressurized air. 2) The MOFs were re-dispersed in DMF. 3) 5 «L IONP in toluene (25 / / g; used as purchased) was added to the MOFs. The Eppendorf was filled with DMF (2 mL) and centrifuged twice (4000 rpm, 5 min) and the solvent was reduced to 0.5 mL to obtain the mMOFs.

[0070] Figure 51 shows the moving of mMOFs: Drop-casting a solution of mMOFs onto a glass slide, adding a cover slide and placing above two Teflon blocks to allow a magnet to move below the sample. A Nd magnet is attached to a metal spatula, placed on top of a copper spatula holder jig and is moved below the sample manually, in several directions.

[0071] Figure 52A shows two preparation routes for dyed mMOFs. Figure 52B shows the Sodium Resorufin dye.

[0072] For simplicity and clarity of illustration, elements shown in the figures are not necessarily drawn to scale, and the dimensions of some elements may be exaggerated relative to other elements. In addition, reference numerals may be repeated among the figures to indicate corresponding or analogous elements.DETAILED DESCRIPTION

[0073] The present invention provides micro-sized anisotropic structures whose orientation and position, and hence function, can be controlled by a magnetic field. The unidirectional alignment of continuous channels in metallo-organic single crystals allows guest molecules (i.e., fluorophores) to align in the channels. Metal-organic frameworks (MOFs) are crystals that consist of metal cations, linked together with multidentate organic ligands by coordination bonds, connected to form 3D structures. A uniform-coating process of MOFs with magnetic iron-oxide nanoparticles, e.g., FesO4 (IONPS), is shown. In various embodiments, the acentric MOFs are based on bivalent nickel cations and a tetrahedral ligand having four pyridine groups for coordination. MOFs based on different bivalent metals (e.g., Cu, Cd) are also coated with the same magnetic nanoparticles. The coating, electrostatically bonded to the MOFs, showed good stability under various conditions, including exposure to an external magnetic field. The MOFs were optically functionalized with a fluorophore and their dynamic alignment to a magnetic field was observed under various polarization directions of light using both optical and fluorescent microscopy. Under polarized light, reversible synchronized switching of the optical appearanceP-632909-PCand properties was recorded for the magnetic MOFs. Thus, providing a platform for magnetically activated optical switches.Opto-magnetic switches of the invention

[0074] In one embodiment the invention provides an opto-magnetic switch comprising porous anisotropic-shaped nanoparticles. In one embodiment the invention provides an opto-magnetic switch comprising metal organic framework (MOF) particles that are magnetized.

[0075] In one embodiment the invention provides an opto-magnetic switch comprising:a substrate;porous anisotropic-shaped nanoparticles with magnetic nanoparticles (MNPs) attached on the surface of the porous anisotropic-shaped nanoparticles, resulting in magnetic anisotropic nanoparticles;a solvent or gel within which the magnetic anisotropic nanoparticles are dispersed; andwherein the magnetic anisotropic nanoparticles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0076] In one embodiment the opto-magnetic switch comprises:a substrate;metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles;a solvent or gel within which the mMOF particles are dispersed; and an encapsulation layer;wherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0077] In one embodiment the solvent or gel comprising the mMOF particles are disposed on the substrate. In one embodiment the solvent comprises an oligomer. In one embodiment the substrate comprises a flexible material.

[0078] In one embodiment the porous anisotropic-shaped nanoparticles comprise metal organic framework (MOF) particles. In one embodiment the porous anisotropic-shaped nanoparticles consist of metal organic framework (MOF) particles. In one embodiment the anisotropic shape is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism.P-632909-PC

[0079] In one embodiment the anisotropic-shaped nanoparticles are understood as MOFs, and can be understood interchangeably. In one embodiment the porous anisotropic-shaped nanoparticles further comprise at least one dye incorporated therein.

[0080] As understood herein metal-organic frameworks (MOFs) are crystalline materials composed of metal ions or metal clusters coordinated to organic ligands to form one-, two-, or three-dimensional porous structures. As used herein, an "opto-magnetic switch" refers to a device comprising magnetic particles that are configured to align, orient, or move (or any combination) in response to an external magnetic field, wherein such alignment, orientation, or movement (or any combination) produces a corresponding optical output. As used herein, the terms "align", "move", "orient" and the likes, are intended to broadly refer to any form of positional or directional change of the magnetic particles, including but not limited to alignment, translation, rotation, or combinations thereof, in response to an external force e.g., a magnetic field. As used herein, the term “attach” refers to any form of association between the MNPs and the MOFs, including but not limited to physical adsorption, chemical bonding, electrostatic interaction, van der Waals forces, covalent or non-covalent linkage, or encapsulation. In various embodiments, the motion of the mMOFs in the solvent or gel are synchronized.

[0081] As understood herein “predetermined direction” refers to a direction that is selected or established in advance by a user, system designer, or control mechanism, or other, based on the intended operation of the device or system. This direction may be defined by parameters such as the orientation or gradient of an externally applied magnetic field, the geometry of the surrounding environment, or programmed instructions within a control system. It represents a known or intended path or alignment along which the nanoparticles (e.g., mMOFs) are configured to orient or move when subjected to the magnetic field. Thus, the predetermined direction is selected to achieve particular output for whatever application the opto-magnetic device is being used.

[0082] As understood herein the term “collectively align” refers to the behavior of a population of nanoparticles (e.g., MOFs, mMOFs) wherein a substantial portion of the particles exhibit a coordinated or generally uniform orientation or arrangement in response to an external stimulus, such as a magnetic field. This may include, but is not limited to, alignment of dipole moments, axes of anisotropy, or translational motion along a common direction. The alignment need not be perfectly uniform or simultaneous, and may occur progressively, locally, or in clusters.P-632909-PC

[0083] In one embodiment size of the MNPs range between 2 to 20 nm. In one embodiment size of the MNPs range between 2 to 10 nm. In one embodiment size of the MNPs are about 10 nm. In one embodiment size of the MNPs are about 5 nm.

[0084] In one embodiment the substrate is transparent. In one embodiment the substrate comprises any of the following selected from: glass, polymer, crystalline, semiconductor, or a combination thereof. Other examples of substrates include, but are not limited to: borosilicate glass, fused silica, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), polyimide, sapphire, aluminum oxide, zinc celanide, gallium nitride, fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), indium-doped zinc oxide (IZO), indium tin oxide (ITO), graphene, carbon nanotubes, poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS), poly(3-hexylthiophene) (P3HT), metal, etc.

[0085] In one embodiment the substrate is a transparent conductive oxide. In one embodiment the substrate further comprises raised edges to contain the solvent or gel therein. The edges can be made of the same material as the substrate, or a different material.

[0086] In one embodiment the MNPs at least partially cover the surface of the MOF particles. In one embodiment the MNPs cover between 5-95% of the MOF particles. In one embodiment the MNPs cover between 50-95% of the MOF particles. In one embodiment the MNPs cover between 80-95% of the MOF particles.

[0087] In one embodiment the opto-magnetic switch comprises:a container;metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles;a solvent or gel within which the mMOF particles are dispersed within the container; andan encapsulation layer;wherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0088] The use of MOFs as the porous anisotropic-shaped nanoparticles is one embodiment of the present invention. As understood herein, a “container” is any vessel that holds the MOF particles which are dispersed in the solvent or gel. In various embodiments the ‘solvent or gel’ can be understood as ‘solvent and / or gel’ depending on the application. In one embodiment the mMOFs are dispersed in a solvent. In one embodiment the mMOFs are dispersed in a gel. AllP-632909-PCcombinations of solvents, gels, or a combination thereof, are considered for the dispersion of MOFs in the applications described herein.

[0089] In one embodiment the opto-magnetic switch comprises:a substrate;metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles;a solvent or gel within which the mMOF particles are dispersed; and wherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0090] In one embodiment the opto-magnetic switch comprises:metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles;a solvent or gel within which the mMOF particles are dispersed; and an encapsulation layer;wherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0091] In one embodiment the opto-magnetic switch comprises:metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles; andan encapsulation layer;wherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0092] In one embodiment the opto-magnetic switch comprises:metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles, resulting in magnetic MOF (mMOF) particles; andwherein the mMOF particles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

[0093] In one embodiment the opto-magnetic switch further comprises an encapsulation layer.

[0094] In one embodiment the opto-magnetic switch does not require a liquid for the mMOF particles to be configured or aligned. In one embodiment the MOF particles have an anisotropicP-632909-PCshape and / or structure. In one embodiment the anisotropic shape and / or structure is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism. In one embodiment the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof. In one embodiment the MNPs are selected from: FesC , y-Fe2O3, FeCo, FeCoFe2O4, NiFe2C>4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao.sSro.sCoCh, or a combination thereof. Examples of anisotropic structures are shown in the Cu(NOs)2 structures of Figures 9A-9E, the Cd(NOs)2 structures of Figure IOC, and the barrel shaped NiBn-AdDB MOF structures of Figures 8A-8B.

[0095] In one embodiment for FexNii-x, x ranges between 0 to 1. In one embodiment the MNPs further comprise a capping layer.

[0096] In one embodiment the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HD A), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochi oride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinyl alcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof.

[0097] In one embodiment the MOF particles are porous. The porosity of the MOF particles enable the incorporation of dyes within. As such, ‘porosity’ is understood to include any void and / or channel within the MOF particles that enables the incorporation of other materials (e.g., liquids, dyes) therein. In one embodiment the MOF particles further comprise at least one dye incorporated therein. In one embodiment the dye is selected from optical, and fluorescent dye, or a combination thereof. Examples of dyes include any of the following, but not limited to: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5 -aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7,7,8,8-tetracyanoquinodimethane (TCNQ) . In one embodiment the dye is sodium resorufin (SR).

[0098] In various embodiments the dye used is fluorescent and enters the channel of the MOF s where it aligns according to its dipole moment. When polarized light is incident on the MOFs, the interaction between the light and the dye depends on this orientation. If the dipole moment of a dye molecule aligns with the polarization direction of the light, it absorbs the light more effectively and fluoresces. If the orientation is misaligned, the dye interacts less strongly with the light, resulting in reduced fluorescence. This orientation-dependent response enables polarization-sensitive detection.P-632909-PC

[0099] In one embodiment the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane, cyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or a combination thereof. In one embodiment the solvent or gel comprise a polymer. In one embodiment the solvent or gel comprise an epoxy.mMOF particles as films in opto-magnetic devices[000100] The mMOF particles themselves can comprise a film on a substrate. The directionality (e.g., alignment, orientation, etc.) of the mMOF particles gives them certain opto-magnetic-electric properties. The alignment of the mMOF particles can be achieved by dispersing the mMOFs in a solvent or gel, orienting the mMOFs in a predetermined direction by an external magnetic field and then setting the mMOFs by evaporating away (or curing) the solvent or gel, leaving the mMOFs permanently oriented on a surface.[000101] In one embodiment the invention provides an opto-magnetic device comprising:a substrate;a film comprising metal organic framework (MOF) particles with magnetic nanoparticles (MNPs) attached on the surface of the MOF particles resulting in magnetic MOF (mMOF) particles; andwherein the mMOF particles are permanently aligned in a predetermined direction.[000102] In one embodiment the MOF particles have an anisotropic shape and / or structure. In one embodiment the anisotropic shape and / or structure is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism.[000103] In one embodiment the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof.[000104] In one embodiment the MNPs are selected from: FesC , y-Fe2O3, FeCo, FeCoFe2O4, NiFe2O4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao.sSro.sCoCh, or a combination thereof.[000105] In one embodiment the MNPs further comprise a capping layer. In one embodiment the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HDA), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochloride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinylP-632909-PCalcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof.[000106] In one embodiment the MOF particles are porous. In one embodiment the MOF particles further comprise at least one dye incorporated therein. In one embodiment the dye is further incorporated in the solvent, gel, or a combination thereof. In one embodiment the dye is selected from: optical, fluorescent, or a combination thereof. In one embodiment the dye comprises any of the following selected from: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5 -aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7, 7,8,8-tetracyanoquinodimethane (TCNQ). In one embodiment the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane, cyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or a combination thereof. In one embodiment the device further comprises an encapsulation layer. In one embodiment the substrate and the encapsulation layer comprise any of the following selected from: glass, AI2O3, quartz, silicon oxide, fluorine-doped tin oxide (FTO), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), cycloolefin polymer (COP), cyclo-olefin copolymer (COC), polymethyl methacrylate (PMMA, acrylic), and polycarbonate (PC), or a combination thereof.Various applications of the opto-magnetic switches and devices of the invention[000107] The opto-magnetic switch (and related devices) of the invention can be utilized in various display technologies, wherein its ability to modulate optical properties in response to an external magnetic field enables dynamic control of visual output. For example, the switch comprises magnetically responsive nanoparticles suspended or immobilized within a medium, such that upon application of a magnetic field, the nanoparticles align or reorient (e.g., collectively), producing a change in optical appearance - such as brightness, color, reflectivity, polarization, or transparency. In various embodiments this field-responsive optical behavior is harnessed for pixel modulation in display devices.[000108] Displays based on such opto-magnetic switches may be passive or active, reflective or emissive, and may be constructed using modular or scalable architectures. For instance, a matrix of individually addressable opto-magnetic elements can be arranged to form a display screen capable of presenting dynamic visual information.P-632909-PC[000109] In one embodiment the invention provides a display comprising the opto-magnetic switch of the invention. In one embodiment the invention provides a display system or interface comprising the opto-magnetic switch of the invention.[000110] As used herein, the term “display system” and “display” refers to any system, assembly, or device configured to present visual information to a viewer, typically by modulating light, color, brightness, contrast, or other optical properties in a controlled manner. Examples of display systems include, but are not limited to: electronic billboards, digital signage, televisions, computer monitors, handheld screens, e-readers, heads-up displays, and wearable displays.[000111] As used herein, the term “interface” refers to any medium, device, or component that provides a visual, optical, or interactive communication pathway between a user and a system. An interface may comprise a display or portion of a display, and may include means for presenting information (e.g., graphical, textual, symbolic) as well as, optionally, accepting input or feedback from a user. Examples of interfaces include, but are not limited to: dashboards, control panels, touchscreens, graphical user interfaces (GUIs), automotive instrument clusters, industrial machine readouts, or any surface or region designed to communicate information visually using the opto-magnetic switch of the invention.[000112] In various embodiments, the invention provides a display system or interface comprising the opto-magnetic switch of the invention. Such a system may include additional components configured to control, drive, power, or interface with the opto-magnetic device to enable practical use in a display environment. In one embodiment the display system further comprises a control unit or driver circuit configured to apply a magnetic field or sequence of magnetic field inputs to the opto-magnetic switch, either directly or indirectly. In one embodiment the display system further comprises a magnetic field generation system comprising at least one electromagnet, magnet arrays, field-generating coils, or a combination thereof. In one embodiment the display system further comprises a controller configured to manage image data, signal processing, timing control, and display modulation, or a combination thereof. In one embodiment the display system further comprises a power source configured to provide energy to the opto-magnetic switch and / or opto-magnetic device and systems. Examples of power sources include, but are not limited to: battery, capacitor, mains port, and photovoltaic element, or a combination thereof. In one embodiment the display system further comprises circuitry including, but not limited to: drivers, multiplexers, integrated circuits, for actuation of the display. In one embodiment the display system further comprises a support structure configured to hold the opto-magnetic switch and / or related opto-magnetic switches and related systems. In one embodiment the opto-magnetic switch further comprises a housing.P-632909-PC[000113] Other examples of the opto-magnetic switch (and related devices and systems) include, but are not limited to: electronic billboards, road signs, traffic signals, warning signs, emergency information panels, general display technology, screen panels, decorative surfaces, e-readers, low-power electronic paper.Opto-magnetic device systems of the invention[000114] An opto-magnetic device system comprising:the opto-magnetic device of the invention;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; andwherein the position and / or orientation of the mMOFs relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.[000115] An opto-magnetic device system comprising:the opto-magnetic device of the invention;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; andwherein the position and / or orientation of the magnetic anisotropic nanoparticles relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.[000116] In one embodiment the porous anisotropic-shaped nanoparticles are metal organic framework (MOF) particles, wherein the magnetic anisotropic nanoparticles are magnetic MOF (mMOF) particles. In one embodiment the analyzer is positioned perpendicular to the polarizer. In one embodiment the polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer. In one embodiment the light source is selected from: laser, or light-emitting diode (LED). In one embodiment the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof.[000117] In one embodiment the system further comprises a controller configured to:P-632909-PCimplement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the magnetic anisotropic nanoparticles; orimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.[000118] The mMOFs exhibit polarization-dependent intensity in both transmitted (optical) and emitted (fluorescent) light, as determined by their orientation relative to the polarizer and analyzer. In one embodiment the mMOFs are configured to exhibit polarization-dependent intensity and / or color in both optical and fluorescent emission, such that their position and / or orientation relative to the polarizer and analyzer alters the polarized light detected by the analyzer.Opto-magnetic systems of the invention[000119] In one embodiment the invention provides an opto-magnetic system comprising:the opto-magnetic switch of the invention;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; anda magnetic-field inducing apparatus configured to generate a varying magnetic field, thereby controlling the position and / or orientation of the magnetic MOFs (mMOFs) within the opto-magnetic switch;wherein the position and / or orientation of the mMOFs relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.[000120] In one embodiment the analyzer is positioned perpendicular to the polarizer. In one embodiment polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer. In one embodiment the light source is selected from: laser, or light-emitting diode (LED). In one embodiment the light is an LED. In one embodiment the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof. In one embodiment the system further comprises a fluorescent detector configured to detect the fluorescence of the mMOF particles.[000121] In one embodiment the opto-magnetic system further comprises a controller configured to:P-632909-PCimplement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the mMOFs; orimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.Methods of fabricating opto-magnetic devices[000122] In one embodiment the invention provides a method of fabricating an opto-magnetic device, the method comprising:providing a substrate;providing a solvent or gel comprising magnetic MOF (mMOF) particles, resulting in a mMOF particles dispersion;dispersing the mMOF particles dispersion on the substrate;evaporating or curing the solvent or gel whilst the mMOF particles are oriented in a predetermined direction by an external magnetic field thereby resulting in the mMOF particles being permanently oriented in the predetermined direction on the substrate.[000123] In one embodiment the evaporating comprises any of the following selected from: vacuum drying, gas flow drying, thermal drying, or a combination thereof.[000124] In one embodiment the curing is thermal curing. In one embodiment the curing is UV curing. In one embodiment the curing is chemical curing. In one embodiment the curing is light curing.[000125] In one embodiment the curing is carried out at about room temperature. In one embodiment the curing is carried out at a temperature ranging between 50 to 200 °C. In one embodiment the curing is carried out at a temperature ranging between 50 to 100 °C. In one embodiment the curing is carried out at a temperature ranging between 100 to 200 °C. In one embodiment the curing is carried out at a temperature ranging between 120 to 180 °C.EXAMPLES EXAMPLE 1Experimental: Materials and Methods[000126] For the preparation of ligand (AdDB): 1-bromoadmantane (99%), benzene (99.7%), AlCh, bromine, bis(triphenylphosphine)palladium(II) dichloride, 4-vinylpyridine (95%), and M methyl pyrroliodone (NMP) were purchased from Merck. The following compounds were also purchased: / -butylbromide (Apollo), tri ethylamine (Alfa Aesar), chloroform (CHCh, > 99.8%)P-632909-PC(Bio-Lab), and diethyl ether (Bio-Lab). For the preparation of the metal-organic frameworks (MOFs): NiBn (> 98.0%) and chloroform (CHCL, anhydrous > 99%) were purchased from Merck. Dimethylformamide (DMF, > 99.5% HPLC grade) was purchased from J. T. Baker. Ni-MOFs were synthesized using glass pressure tubes (Ace Glass, Inc., pressure tubes #15 with a plunger valve, PTFE Bushing and FETFE® O-Ring, volume 50 mL). The glass tubes were cleaned by immersion in a cone, sulfuric acid (98%) (Bio-Lab) for 2 days, then washed with water and dried at 110°C for 12 h. Iron oxide magnetic nanoparticles (IONP, 0 = 10 nm, in toluene) were purchased from Cytodiagnostics. Sodium resorufin (SR) was purchased from Sigma-Aldrich. All reagents were used without further purification.Methods[000127] l,3,5,7-Tetrakis{4-[(£)-2-pyridine-4-yl-vinyl]phenyl}admantane (AdDB) was prepared in 3 steps: 1) Friedel -Crafts alkylation: 1-Bromoadmantane (5.0 g, 23 mmol) was dissolved in benzene (50 mL). To this solution, Lbutylbromide (9.0 mL, 45 mmol) was added, followed by slow addition of A1CL (0.56 g, 4.2 mmol) at 0 °C. The reaction mixture was refluxed for 4 h at 90°C. After being cooled to room temperature, the reaction was quenched with deionized (DI) water. The product was collected by vacuum filtration and washed with chloroform, DCM, and diethyl ether. The final product, 1,3,5,7-tetraphenyladmantane, was isolated as a white powder by recrystallization in chloroform and drying under vacuum, Yield: 80% (8.1 g, 18 mmol). 2) Bromination: 1,3,5,7-tetraphenyladmantane (1.0 g, 2.3 mmol) was added portion-wise to bromine (7.3 g, 46 mmol) at 0 °C. The mixture was stirred at room temperature for 30 min and quenched with a large excess of ethanol (~50 mL). The product, l,3,5,7-tetrakis(4-bromophenyl)admantane, was vacuum dried after vacuum-filtration and washed with ethanol and diethyl ether and dried under vacuum to obtain white powder. Yield: 76% (1.34 g, 1.77 mmol) 3) Heck coupling: l,3,5,7-tetrakis(4-bromophenyl)admantane (1.0 g, 1.1 mmol) and bis(triphenylphosphine)palladium(II) dichloride (0.020 g, 0.028 mmol) were dissolved in A-m ethyl pyrroliodone (4.0 mL, 41 mmol), 4-vinylpyridine (1.0 mL, 9.0 mmol), and triethylamine (3.0 mL, 22 mmol) under N2. The mixture was heated to 110°C for 3 days; then it was allowed to cool to room temperature, filtered, and washed with methanol (until filtrate becomes clear) and diethyl ether. AdDB was purified by column chromatography using a 1:9 v / v mixture of methanol and DCM as an eluent. Thin-layer chromatography was used to identify the AdDB fractions and indicate its purity. The yield of AdDB was 50% and obtained as a white powder (470 mg, 0.55 mmol). ’H NMR (300 MHz, CDCh) 8.59 (8H, d, JHH= 5.9 Hz), 7.56 (16H, br s), 7.38 (8H, d, JHH= 5.9 Hz), 7.32 (4H, d, JHH= 16.3 Hz), 7.01 (4H, d, JHH=P-632909-PC16.2 Hz), 2.23 (12H, br s). ThisXH NMR spectrum matches literature data using 500MHzXH NMR.[000128] Ni-MOFs. In the present disclosure, several modifications were done to obtain larger (4-10 / / m) barrels (no sonication, chloroform only to dissolve ligand, different layering inside pressure tube): A solution of NiBn (1.54 mg, 7.04 / mol) in DMF (1.0 mL), DMF (2.0 mL) and a solution of AdDB (3.0 mg, 3.5 / / mol) in CHCL (1.0 mL) were added to a glass pressure tube (50 mL) and heated at 105 °C for 48 h. The tube was allowed to cool to room temperature, resulting in a light green precipitation. The MOFs are isolated by centrifugation (4000 rpm, 5 min). After the solvent is discarded, the MOFs are washed with. The yield, 92%, based on AdDB, was obtained by drying the MOFs under pressurized air. The Ni-MOFs were redispersed in 5 mL ethanol and stored in solution.[000129] Magnetic MOFs (mMOFs). 100 / / L (~2.0 mg) from the prepared Ni-MOF-ethanol solution was added to a 2 mL Eppendorf tube. The Eppendorf was filled with ethanol and centrifuged (4000 rpm, 5 min). The remaining solvent was discarded, and the MOFs were dried using pressurized air. The Eppendorf was filled with hexane and centrifuged (4000 rpm, 5 min). The remaining solvent was discarded, and the MOFs were dried using pressurized air. The hexane-washing was used to allow fast solvent evaporation. Next, the MOFs were dispersed in DMF (100 / / L), followed by the addition of a toluene solution of IONP (5 / / L, 25 / / g; used as purchased). The Eppendorf tube was gently shaken by hand. The light-green MOF solution darkens upon the addition of the IONPS. Light brown particles appeared, and the solution became clear. After 3 days, the Eppendorf containing mMOFs was filled with DMF (2 mL), centrifuged twice (4000 rpm, 5 min) and the volume of DMF was reduced to 0.5 mL using a pipette and. Finally, the Eppendorf was stored for further use. This procedure was done to the Cu-mMOFs and Cd-mMOFs as well. The MOFs are based on the same ligand (AdDB). Cu-MOFs (prepared at molar ratio of ligand-to-metal salt of 1:2) and Cd-MOFs were prepared according to known procedures.[000130] Magnetized sodium resorufin dyed Ni-mMOFs. 100 / / L (~2.0 mg) from the Ni-MOF solution was added to a 2 mL Eppendorf tube. The Eppendorf was filled with ethanol and centrifuged (4000 rpm, 5 min) twice. The solvent was removed, and Ni-MOF was redispersed in 1.0 mL ethanol. Next, 0.2 mg (8.5 / / mol) of sodium resorufin (in powder form) was added to the MOFs’ solution, gently shaken (manually) and reacted for 24 h without agitation without light exposure. To wash the dye excess, the Eppendorf was filled with ethanol and centrifuged (4000 rpm, 5 min) until the color of the ethanol solution was clear, and the dyed Ni-MOF appeared purple at the bottom of the Eppendorf. The solvent was removed, and the dyed MOFsP-632909-PCwere dried using pressurized air. Then, DMF (100 «L) and IONP (5 «L, 25 «g; used as purchased) were added to the vial with the dyed Ni-MOFs. The vial was briefly shaken and after 24 h without agitation, the reaction mixture was centrifuged with DMF (4000 rpm, 5 min) and the solvent was reduced to 0.5 mL to obtain the magnetized dyed Ni-mMOFs solution.[000131] Dyeing mMOFs with Sodium Resorufin (SR). 0.05 mL SR dye solution (0.1 mg, 4.2 / mol SR in 1.0 mL ethanol, 0.42 [mM]) in DMF was added to a 2 mL Eppendorf containing 0.5 mL mMOFs in DMF, followed by gentle manual shaking. After 24 h the excess dye was removed by introducing a magnet near the Eppendorf, causing the dyed mMOFs to move towards the magnet. Subsequently, the solution was replaced with 0.5 mL DMF using a pipette. After shaking the Eppendorf again and repeating the solvent exchange process twice using a magnet, a clear solution was obtained with dispersed purple mMOFs.[000132] NMR spectroscopy. A Bruker NMR spectrometer (300 MHz) was used for the ’H NMR measurements.[000133] Optical Light Microscopy. Samples were prepared by drop-casting 5 «L of the mMOFs in DMF solution onto a glass slide (thickness = 0.17 mm) and covering the sample with a cover slide with the same thickness. Optical images and videos were taken using a Nikon microscope Eclipse E600 Pol and DeltaPix Invenio 12EIII camera.[000134] Controlled movement of mMOFs using a magnetic field. A square (1 cm x 1 cm) neodymium magnet (Eclipse Magnetics, N861) was used to generate a magnetic field (0.33 T, tested using FW Bell 5180 Gauss Meter). The magnet was placed 1 cm below the sample and placed on top of a metal spatula, to allow accurate manual movement of the magnet. The sample was raised 1 cm using Teflon jigs to allow placement of the magnet below the sample (Figure 1). Figure 1 shows the sample placed between two thin glass slides (thickness = 0.17 mm) and raised 1 cm using Teflon jigs. A Nd magnet is attached to a metal spatula, placed on top of a copper spatula holder jig and is moved below the sample, without blocking the incoming light.[000135] Scanning Electron Microscope (SEM). Samples were prepared by drop-casting 5 / L of the tested solution on a silicon substrate and allowing the solvent to evaporate. Measurements were performed using a Gemini 500 Zeiss electron microscope at an EHT voltage of 0.8 kV and with an aperture size of 20 / m. Images were collected in secondary mode by using an Everhart-Thornley detector and in back scattering mode by using an EsB detector with a filtering grid.[000136] Energy-dispersive X-ray spectroscopy (EDS). EDS measurements were performed using a four-quadrant detector (Bruker QUANTAX FlatQUAD) installed on a Zeiss Ultra 55 electron microscope with a landing voltage of 3 kV. The secondary electrons were imaged with an Everhart-Thornley detector.P-632909-PC[000137] Dynamic light scattering (DLS). Solution of 25 «L IONP (as purchased) in DMF (3 mL) or toluene (3 mL) were analyzed in a quartz cuvette (Hellma, 104-10-40; 1 mL) using a Zetasizer Nano ZS from Malvern Panalytical instrument.[000138] Transmission electron microscopy (TEM) Samples were prepared by drop-casting 5 / L of the tested solution on 400-mesh carbon-coated copper grids (SPIGridsTM, 3 mm). Energy dispersive X-ray spectroscopy (EDS) maps were acquired using a double aberration-corrected Themis-Z microscope (Thermo Fisher Scientific Electron Microscopy Solutions, Hillsboro, USA (TFS)) at an accelerating voltage of 200 kV.[000139] Fluorescence spectroscopy. The mMOFs (in DMF) were drop-casted onto a glass slide (0.17 mm), and another cover slide (0.17 mm) was added on top. Imaging was conducted by using a galvometric scanner with a confocal system Leica TCS SP8, based on a motorized inverted microscope DMi8 and equipped with internal Hybrid (HyD) detectors and an Acusto Optical Tunable Filters (Leica microsystems CMS GmbH, Germany). Images were acquired using the 20* air objective (HC PL APO CS220* / 0.75). Excitation was performed using a white light laser (A = 561 nm). The emission signal was collected using an internal HyD SMD 4 detector at a range of A = 571-650 nm and 100 % gain. The rotatable polarizer was set to positions at 0 and 90 degrees. The DMi8 microscope was set to be in a “Scan-BF” state (analyzer out of the optical path), and a quarter wavelength retardation plate was removed from the optical path. A magnetic field was introduced to the samples using a square (1 cm x 1 cm) neodymium magnet (Eclipse Magnetics, N861) placed and moved ~1 cm away from the sample. The acquired images were visualized and analyzed using the LAS X Office program.[000140] Measuring magnetic properties using a Superconducting Quantum Interference Device (SQUID). The measurements were carried out with a SQUID magnetometer MPMS3 (LOT-Quantum Design, Inc.) in Vibrating Sample Magnetometry (VSM) mode, applying a peak amplitude of 5 mm with a frequency of 13 Hz, and an average time of 4 s. The samples were drop-casted from their solution onto a double-sided polished 4 mm x 4 mm undoped silicon wafer substrate. The weight of the substrate was reduced from the weight after sample loading, to obtain the mass of the sample. Polyethylene straws were used to hold the samples, with minimal impact on the magnetic moment background (~ IO-6emu at 1 T). The polyethylene straws were mounted so that the silicon wafer surface with the drop-casted sample was perpendicular to the direction of the applied magnetic field. The magnetic moments (emu) were measured while varying the magnetic field (H) over the range of -6 T < H < 6 T, at a constant temperature of 300K. The mass moment [emu / g] was calculated by the following formula: (M-MSi) / msampie where M is the measured moment [emu] of the silicon wafer with the sample loaded, MSiis the silicon waferP-632909-PCmoment [emu] and msampie is the sample’s mass [g]. To measure powder IONP, 0.5 mL from the as-purchased IONP solution was washed three times with 3 mL ethanol, and the top layer was magnetic decanted between each washing. Next, vacuum-drying under N2 atmosphere for 48 h was done to get IONP powder. The powder was placed in a gelatin capsule held by a polyethylene straw, measured in the same conditions for other samples, and the mass moment [emu / g] was calculated by the following formula: M / msampie where M is the measured moment [emu] and msampie is the sample’s mass [g], (The gelatin capsule has a minimal impact on the magnetic moment background: < 7* IO-7emu at 2 T).[000141] Attenuated total reflection (ATR) FT-IR spectroscopy. FT-IR Alpha (Bruker, UK) equipped with a Platinum ATR was used to measure each sample 3-5 times. The samples were drop-casted on a square Cu substrate ( I cm l cm). After every scan of a sample, a background of clean Cu substrate reference was performed, and the spectrum was obtained against the background of the clean Cu substrate.[000142] Raman scattering measurements were taken in a home-built back-scattering system. A 1.57 eV CW diode laser (T optica Inc., USA) was used, with a power of 16 mW. The beam was focused on the sample with a 50* objective (Zeiss, USA). The Rayleigh scattering was filtered by notch filters (Ondax Inc., USA). The scattered light was focused into a l m spectrometer (FHR 1000, Horiba) with a 600 g / mm grating and a CCD detector.[000143] X-ray photoelectron spectroscopy (XPS). XPS measurements were carried out with a Kratos AXIS ULTRA system using a monochromatic Al Ker X-ray source (hv = 1486.6 eV) at 75 W and detection pass energies ranging between 20 and 80 eV. A low-energy electron flood gun (eFG) was applied for charge neutralization for all tested samples, excluding the IONP. Curve fitting analysis was based on linear or Shirley background subtraction and application of Gaussian-Lorenzian line shapes. The samples were drop-casted on 1 cm x 1 cm silicon wafers.[000144] Atomic Force Microscopy (AFM). Atomic force microscope (AFM) imaging was performed with an AFSEM nano (Quantum Design. San Diego USA) system, with the AFM installed inside of a scanning electron microscope (SEM) (LEO-Supra 55 VP, Zeiss). The SEM allowed quick identification of suitable metal-organic framework (MOF) structures. Then the AFM scanned the 3D topography of such particles in AC mode to yield true 3D imaging, allowing determination of the roughness and size of the magnetic particle coating. The probe was a piezoresistive self-sensing AFM probe (PRS 70 «m x 30 «m Si-Tip, SCL-Sensor.Tech. Fabrication GmbH). Image analysis was performed using Gwyddion software.P-632909-PCEXAMPLE 2Preparation Methods[000145] 1 ,3,5,7-tetrakis {4- [(E)-2-pyridine-4-yl-vinyl] phenyl} admantane (Ad-DB)[000146] The ligand (AdDB) was synthesized as shown in Figure 48. Starting from the commercially available 1-bromoadmantane undergoing Friedel-Craft reaction with benzene (step 1), followed by bromination (step 2). The last reaction (step 3) was a Heck reaction with 4-vinyl pyridine, resulting in AdDB in 50% yield. 'H-NMR spectroscopy and thin-layer chromatography (TLC) was used to identify the structure and indicate the purity of AdDB.Ni-MOF[000147] Ni-MOFs were prepared using a solvothermal reaction between NiBn and AdDB in 2:1 mole ratio (Figure 49). A solution of NiBn (1.54 mg, 7.04 / mol) in DMF (1.0 mL), DMF (2.0 mL), and a solution of AdDB (3.0 mg, 3.5 / / mol) in CHCL (1.0 mL) were added to a glass pressure tube (50 mL) and heated at 105 °C for 48 h. The tube was allowed to cool to room temperature, resulting in a light green precipitation. The MOFs are separated by centrifugation (4000 rpm, 5 min). After the solvent is discarded, the MOFs are washed with ethanol and stored in ethanol.[000148] The Ni-MOFs were analyzed both by optical microscopy and Gemini 500 Zeiss SEM by drop-casting the MOFs on an optical glass slide or a silicon wafer, respectively (Figure 2).The optical microscopy shows uniform barrel-shaped MOFs. The SEM data is in good agreement with the optical measurements. The barrel-shaped crystals have a length of 5.0 ± 1.2 / / m and a width of 2.7 ± 0.48 / / m (avg. of 50 crystals). It is noted that the Ni-MOF crystals are hexagonal in shape and match the rare hexagonal space group P622. These MOFs have two types of chiral channels, hexagonal and triagonal with diameters of -7.0 and -10.2 A.[000149] Figure 48 shows the synthesis and molecular structure of l,3,5,7-tetrakis{4-[(E)-2-pyridine-4-yl-vinyl]phenyl} admantane (AdDB) where: (1) Friedel-Crafts alkylation using 1-bromoadmantane and benzene to form 1,3,5,7-tetraphenyladmantane (80%-90% yield), (2) Bromination to form 1, 3,5,7-tetrakis(4-bromophenyl)admantane (60%-70% yield), (3) Heck coupling with 4-vinylpyridine, resulting in AdDB (50% yield).[000150] Figure 49 shows MOFs preparation: (1) adding NiBn (dissolved in DMF) and AdDB (dissolved in chloroform) into a glass pressure tube, (2) placing the tube in an oven at 105 °C for 48 h, (3) separation of the crystals from the mother solution by centrifugation (4000 rpm, 5 min) with ethanol. Figure 2 shows the barrel-shaped crystals have a length of 5.0 ± 1.2 zm and a width of 2.7 ± 0.5 zm. Magnetic iron oxide nanoparticles (I0NP)P-632909-PC[000151] The magnetic iron oxide nanoparticles (magnetite, FesC ), capped with oleic acid (OA), were used as received from the supplier (Cytodiagnostics, 10 nm in toluene, 5 mg / mL). Transmission electron microscopy (TEM) images confirm their shape and diameter of 9 ± 1 nm (Figure 3). The average diameter was obtained by analyzing 50 particles using ImageJ software. The presence of the OA capping layer was confirmed by FTIR measurements using a drop-casted sample on a Cu substrate, compared with the FTIR spectrum for OA only. A distinct Fe-OA peak is observed at 600 cm'1(see ATR-FTIR measurements, Figure 17).Magnetized MOFs (mMOFs)[000152] The procedure for the MOFs magnetization is shown in Figure 50. 100 «L (~2.0 mg) Ni-MOF in ethanol was transferred into a 2 mL Eppendorf and centrifuged (4000 rpm, 5 min) to precipitate the MOFs. The remaining solvent was discarded, and the MOFs were dried using pressurized air. The Eppendorf was filled with hexane and centrifuged (4000 rpm, 5 min). The remaining solvent was discarded, and the MOFs were dried using pressurized air. The hexane-washing was used to allow fast solvent evaporation. Next, the MOFs were dispersed in DMF (100 «L), followed by the addition of a toluene solution of IONP (5 «L, 25 / / g; used as purchased). The Eppendorf tube was gently shaken by hand. After 3 days, the Eppendorf containing mMOFs was filled with DMF (2 mL), centrifuged twice (4000 rpm, 5 min) and the volume of DMF was reduced to 0.5 mL using a pipette. Finally, the Eppendorf was stored for further use.[000153] The MOF magnetization was visually demonstrated by placing 3 vials (2 mL) next to 4 round disc magnets (0out = 4.5 cm, 0jn= 2 cm) placed on top of each other (~0.8 kG measured magnetic strength, using FW Bell 5180 Gauss Meter) (Figure 4A). Each vial contained 200 «L DMF with one of the following: Ni-MOFs (~ 2 mg Ni-MOFs, vial 1), IONP (10 «L IONP, vial 2). The third vial initially contained -2 mg Ni-MOFs dispersed in 200 «L DMF, to which 10 «L IONP was subsequently added (vial 3). The Ni-MOFs (vial 1) (Figure 4B) are not attracted to the magnet. The IONPS (vial 2) (Figure 4C) diffuse slowly (several hours) towards the magnets. However, after adding the 10 / / L IONP to the uncoated MOFs in vial 3 (Figure 4D), immediately visible changes are observable: the solution becomes clear, and a light brown precipitate formed. The resulting precipitate, the Ni-mMOFs, moves relatively fast (< 5 min) and accumulates near the magnet. Rotating the vial with Ni-mMOFs while keeping it close to the magnet shows the rapid reposition (~ 2 sec) of the Ni-mMOFs due to the magnetic field (Figure 4E, 4F). From this experiment, it is concluded that the magnetic IONP interacts with the Ni-MOFs in solution to create a new functionality for the MOFs that react to a magnetic field.P-632909-PC[000154] The SEM images of the mMOFs show a uniform coating on all the facets (Figure 5B-5E). An energy-selective backscattered (EsB) detector showed the compositional contrast (Figure 5B, 5D). The brighter areas are correlated to the iron atoms. Larger atoms such as iron (atomic number Z = 26) have a higher probability for elastic collision and reaching the detector, resulting in higher brightness. The EDS spectra of the mMOFs exhibit the Fe and O peaks at 0.70 keV and 0.52 keV, respectively. The coating is composed of clusters of IONPS. The average cluster size (51 ± 21 nm) and distance (41 ± 19 nm) between two clusters was measured using image processing software (ImageJ) on 50 different areas in different crystals (SEM images, Figure 5C). The arrangement of the IONP coating depends on the reaction time. Specifically, the duration between the addition of IONP and the subsequent centrifugation with DMF (Figure 49, step 3). The longer reaction time (3 days versus 1 day) resulted in a coating with more aggregates and relatively larger uncoated areas. A shorter reaction time (1 day) resulted in the formation of less aggregates and a more homogeneous coating. Examining the stability of the coating of 1-day mMOFs with time (while kept in 0.5 mL DMF), showed a similar appearance to 3-day mMOFs after three months (Figures 6A-6B). In some batches, 1-day mMOFs kept a few days in solution formed aggregate which were similar to 3 -days mMOFs. Therefore, mMOFs were centrifuged after a reaction time of 3 days. The presence of the IONP on the surface of the MOFs was further confirmed by Energy Dispersive X-ray spectroscopy (EDS) measurements comparing to uncoated MOFs (Figure 7, Figure 32).[000155] The formation of surface-bound IONP aggregates indicates that the initially bound IONP can translocate on the MOFs’ surface at room temperature in solution. It is shown that thermally-induced movement and fusion of gold nanoparticles on the surface of inorganic nanotubes. The IONP coating is stable at high temperatures, as a dry drop-casted Ni-mMOF sample on a Si wafer was heated to 110 °C and kept for 12 h and examined on SEM (Figure 33).Nanoparticles fusion was not seen on top of the mMOFs. This is due to that the oleic acid desorption and evaporation from the IONP take place at the range of 200-360 °C. DLS measurements showed that the IONPs are better dispersed in toluene (relative polarity: 0.099; average NP size = 9 ± 2 nm) compared to DMF (relative polarity: 0.386; average NP size = 30 ± 7 nm) (Figure 34A). The hydrophobic oleic acid carbon chains surrounding each NP cause the IONP to form clusters due to dipolar interactions. The average NP cluster size is larger in DMF, however no precipitation is observed by adding IONP to DMF (Figure 34A-34C).Changing the solvent from toluene to DMF does not affect the binding of the oleic acid to the IONP in DMF.P-632909-PC[000156] To evaluate the solvent effect on the coating, mMOFs were prepared using hexane (relative polarity: 0.009; 100 «L) and Ni-MOF (~2 mg), followed by IONP (5 «L) addition. Centrifugation was not necessary here. These mMOFs, are readily dispersed in DMF, and do not tend to disperse in hexane. The SEM images (Figures 35A-35B, 36A-36B) show IONP coating on all the facets, indicating that the NP attachment is not solvent-dependent. However, the coating is more dispersed, and individual IONPS can be seen on the surface of the MOFs. In addition to the MOF’s dispersion issue, a less volatile solvent (DMF) for the dynamic movement of mMOFs in a magnetic field was used. The centrifugation done after IONP addition (Figure 49, step 3) is a crucial step, assisting the IONP distribute uniformly on top of the MOF surface (Figures 8A-8D) and reducing mMOFs aggregation (Figures 37A-37C). The centrifuge increases the collision between MOFs and un-bounded NP so more surface is coated, in addition to causing NP movement on top of the MOFs surface, resulting at fuller coating with less NP aggregations. In addition, the ideal MOFs to IONP ratio was found to be 5 «L NP solution (25 «g) to every 100 «L of MOFs in DMF (~2 mg); When using higher concentration of IONP, excess of IONP aggregates on top of the MOFs’ surface, and mMOFs aggregates are formed (Figures 38A-38C).[000157] Figures 8A-8D the optical microscopy and SEM images of Ni-mMOFs before (Figures 8A, 8C) and after (Figures 8B, 8D) centrifugation (stage 3 in Figure 49). The 2 mL Eppendorf tube containing Ni-mMOF was filled with DMF and centrifuged at 4000 rpm for 5 min. The solvent was reduced to a final volume of 0.5 mL. The centrifugation resulted in better dispersion of IONP over the surface of the MOF (image Figure 8B) and reduced mMOFs aggregation and IONP aggregation (marked squares in image Figure 8C)EXAMPLE 3Formation of Cu-mMOFs and Cd- mMOFs[000158] MOFs based on the same ligand (AdDB) and Cu(NOs)2 or Cd(NOs)2 were also used to prepare mMOFs according to procedures to form Cu-MOFs (prepared at molar ratio of ligand-to-metal salt of 1:2) and Cd-MOFs. The IONP coating was formed using the procedures for the Ni-mMOFs, with the centrifugation done after 3 days from IONP addition. The two MOFs are hexagonal prisms. Cd-MOF is larger than Cu-MOF (100 «m in length compared to 5 «m for Cu-MOF, length measured using optical microscope). The SEM images of Cu-MOF and Cd-MOF (Figures 9A-9E, 10A-10C) show a uniform coating on both MOFs, demonstrating the scope of the NP coating method.[000159] Figure 1 show SEM images of a Cd-MOF after lONP-coating: SE2 (Figure 10A) and BSE (Figure 10B) detectors. Figure 10C shows zoom-out of the coated MOFs. Top right: Optical microscopyP-632909-PCimages of the MOF before and after coating. Coating was done at the same way as for Ni-mMOF. The length of Cd-MOF is ~90 um (as seen in optical microscope), the IONP can be seen at higher magnifications of SEM, or as a surrounding brown area at the MOFs’ circumference in the optical microscope. Centrifugation was done after 3 days from IONP addition.mMOFs Stability[000160] The stability of the Ni-mMOFs coating was examined by assessing its temporal stability in both solution and solid state. The coating remains after 1 min sonication of Ni-mMOFs in DMF. Furthermore, the mMOFs were subjected to a magnetic field exposure of 0.33 T for 30 min while kept in DMF and during drop-casting, with the magnet positioned beneath the silicon wafer, aiming to investigate any potential migration of IONP from the MOFs' surface toward the magnet. The mMOFs were examined by SEM before and after each parameter. The results show a stable coating, without any noticeable change in IONP density or IONP migration.(Figures 11A-11D).Micro-Raman Spectroscopy[000161] Micro-Raman measurement were done to locate the functional groups that changed during the magnetization process. The spectrum of uncoated and coated MOFs was taken from samples that were drop-casted on Si wafer, and compared while both spectra were scaled to the intense band at v = 1600 cm'1(Figure 12). MOF magnetization resulted in a signal intensity increasement comparing to the uncoated MOFs, with no shifts. These changes appear in bands related to pyridine-moi eties coordinated to Ni2+(two bands at v = 1620 cm'1, one band at v= 960 cm'1). A change in relative intensity at v = 1620 cm'1between the two bands was observed too. Furthermore, additional intensity increasement are noticed in the vibrational pyridine mode at v = 1020 cm'1band, and in benzene mode at v = 1890 cm'1.[000162] In addition, a red shift observed at v= 1335 cm'1for uncoated MOFs to v= 1330 cm'1for mMOFs, bands that are indicative for the vibration of the C=C pyridine ring bond. These changes suggest an interaction between the pyridine moieties and the IONPS, however such interactions were not identified by XPS measurement for the nitrogen atoms (see XPS results in Figures 42A-42B). No new peaks were observed for mMOFs, as the characteristic band of magnetite nanoparticles at 700 cm'1, and oleic acid peaks could not be identified using micro Raman. Attempting to measure the spectra of IONP only resulted in sample burning and high noise. As the IONP could not be measured separately, this might be a reason for the absence of the indicative peak of magnetite in the mMOFs spectra.Superconducting quantum interference device (SQUID)P-632909-PC[000163] SQUID measurements were done to determine the magnetic strength of the Ni-mMOFs, comparing to the uncoated Ni-MOFs and the magnetic IONP (Figures 13A-13C). A SQUID magnetometer MPMS3 (LOT-Quantum Design, Inc.) was used in the VSM mode to measure the mass moment [emu / g], which is normalization of the magnetic moment by the weight of the sample. Samples were drop-casted on 4 mm x 4 mm undoped Si wafer for the measurement. The IONP measured in a powder form, after washing with ethanol. The Ni-MOFs (Figure 13A) have a mass moment (at saturation) of 0.2 [emu / g] and show a paramagnetic behavior (magnetism is linearly positive proportional to an external magnetic field). The Ni-mMOFs (Figure 13B) however resulted at 6 [emu / g] and a superparamagnetic behavior with stronger magnetism and no permanent magnetization in the absence of an external magnetic field. In its powder form, the IONP has a magnetism of 45 [emu / g] (Figure 13C), which corresponds to the literature value and the company (Cytodiagnostics) spec sheet. The major contribution to the mMOFs magnetism is from the IONP. However, the mass moment (emu / g) was calculated by dividing the magnetic moment (emu) with the total mass of the MOFs and the IONP. Thus, dividing the magnetic moment by the IONP mass coating the MOFs only, the total magnetism would be much higher as a result of the strong superparamagnetic IONP. In addition, magnetic aggregates of superparamagnetic nanoparticles have a higher magnetic dipole moment than single particles. In Ni-mMOFs, calculated the mass ratio between the MOFs and the NP to be 6.7:1, given the Ni-mMOFs sample is composed only from MOFs and NP, and having the emu\g of all the samples (MOFs, NP, mMOFs).[000164] As shown herein, the magnetism is dependent on the amount of the IONP in the MOFs surface, and can be ranged from 0.2 emu / g to 20 emu / g where all values were found to be sufficient to match the needed mobility applications. It was concludes that the mMOFs react strongly to an applied magnetic field, with a total magnetism of 6 emu / g (at saturation) showing superparamagnetic behavior.Atomic Force Microscope (AFM)[000165] Atomic force microscope (AFM) imaging was performed with an AFSEM nano (Quantum Design. San Diego USA) system, with the AFM installed inside of a scanning electron microscope (SEM) (LEO-Supra 55 VP, Zeiss). The SEM allowed readily identification of the mMOFs. The measurement was done to evaluate the roughness of the Ni-MOFs and the Ni-mMOFs' surface and to measure the height of the IONP coating on top of the MOFs’ surface. Image analysis was performed using Gwyddion software. The roughness was calculated as the root mean square (RMS) average of the profile height deviations from the mean line profile. For the Ni-MOFs, and the Ni-mMOFs, the roughness is calculated to be 3.6 nm and 9.1 nm,P-632909-PCaccordingly (Figures 14A-14B), as the iron oxide spheres increase the MOFs’ surface roughness. The roughness of 9.1 nm indicates that the average roughness is about the order of an individual IONP (purchased with diameter of 10 nm). The height of the NP coating was evaluated by plotting a line profile of 30 different coated areas, taking the height value as the difference between the lowest area (MOFs surface) and the coating highest area (top of the NP sphere). The resulting NP coating height was 30 nm ± 5 nm which match the DLS measurement done for the IONP in DMF solvent (Figures 34A-34C). This result indicate there is a partial fusion of NP, and this happens due to the solvent used (DMF).Attenuated total reflectance Fourier transform IR spectroscopy (ATR-FTIR)[000166] ATR-FTIR spectroscopy measurement was done to the IONP, OA, AdDB, uncoated Ni-MOFs and Ni-mMOFs. This was done to identify new peaks that could provide insights into the binding between IONP and MOFs. The samples measured were drop-casted on Cu substrate and each spectrum is an average of three single measurements, after reducing the Cu background for each measurement. For the uncoated MOFs and mMOFs, peaks were intensified (xl.5, x3 respectively) for better peak identification. Figure 15 shows the ATR-FTIR spectra of the pure OA (green line) and FesO4 NP coated with OA (orange line). Oleic acid can be seen in the spectrum of the IONP. An indicative Fe-0 stretching peak of the magnetite can be seen at the IONP spectrum at 600 cm'1. In both OA and IONP spectra, Two sharp bands at 2922 and 2582 cm'1were attributed to the asymmetric CH2 stretch and the symmetric CH2 stretch, respectively. The intense peak at 1710 cm'1was derived from C=O stretch and the O-H in-plane and out-of-plane bands appeared at 1464 and 943 cm'1, respectively. The appearance of O-H peaks for both IONP and OA can indicate excess OA in the IONP sample.[000167] Next, the AdDB, Ni-MOFs and Ni-mMOFs were compared to IONP and OA FTIR spectra (Figure 16). The indicative Fe-0 band at 600 cm'1was not observed for mMOFs. No other IONP / OA related peaks observed for mMOFs. As the IONP presence was confirmed by other methods (EDS, SQUID, XPS), in this method a change between the uncoated and coated MOFs was not identified. From this alone the nature of the binding of the mMOFs to the NP cannot be concluded. The lack of peaks can be due to masking of the IONP by the mMOFs in this. MethodX-ray photo spectroscopy (XPS)[000168] XPS measurements were performed to evaluate the chemical composition of the samples. For this measurement, the IONP, uncoated Ni-MOFs and Ni-mMOFs were measured, after drop-casting on 1 cm x 1 cm Si wafer. The XPS spectra for the oxygen atom (Is) for theP-632909-PCuncoated MOFs and mMOFs (Figures 17A-17B), shows an additional Fe-0 peak at 530 eV, for the iron oxide in the mMOFs. The high intensity of the SiO2 peak in the mMOFs related the Si wafer.[000169] The XPS spectrum for the nitrogen atom (Is) for the uncoated MOFs and mMOFs (Figures 42A-42B), shows additional peaks after MOF magnetization of oxidized forms of nitrogen. However, their intensity is very low, and nitrogen oxide presence was not found in other methods such as micro-Raman. Therefore, it is considered to be due to noise or impurities in the sample. The XPS spectrum for the carbon atom (Is) of the uncoated MOFs and mMOFs (Figures 18A-18B), indicates the presence of carbonyl groups of OA in the mMOFs. The coating procedure did not remove the oleic acid capping layer from the IONP.[000170] The spectrum of iron (2p) for both IONP and mMOFs remains the same with no additional peaks (Figures 19A-19B). The intensity is lower for the mMOFs due to the lower concentration of IONP in the sample comparing to pure IONP. The binding energy of the Fe 2ps / 2 is 710.8 eV for the IONP, and after binding to the MOFs, the binding energy of the Fe 2p3 / 2 is 711.1 eV. Comparing to measured oleic acid-capped nanoparticles values of Fe2O3 (710.9 eV) and of Fe3O4 (710.4 eV), it can be assumed that the Fe3O4 purchased nanoparticles (Cytodiagnostics) contain more iron in +3 oxidation state that fits Fe2O3 form.[000171] The spectrum of nickel (2p) for both uncoated MOFs and mMOFs remains the same with no additional peaks (Figures 20A-20B). The higher intensity of the Ni in the mMOFs spectrum might be due to shielding effect from the IONP. As no significant chemical change is noticed for the mMOFs, it can be concluded that the binding of the IONP to the MOFs is through electrostatic interactions between the positively charged MOFs’ and the negatively charged IONP.Dynamic alignment using magnetic field[000172] In the following experiments, the mMOF sample was prepared and placed under the microscope as shown in Figure 51. A square Nd magnet (1 cm x 1 cm, Eclipse Magnetics, N861) was placed ~1 cm below the sample, and manually moved in several directions, resulted in movement of the mMOFs. Figure 51 shows the drop-casting of a solution of mMOFs onto a glass slide, adding a cover slide and placing above two Teflon blocks to allow a magnet to move below the sample. A Nd magnet is attached to a metal spatula, placed on top of a copper spatula holder jig and is moved below the sample manually, in several directions.Polarized optical microscope[000173] The Ni-mMOFs were imaged using Nikon microscope (Eclipse E600 Pol), which allows rotation of a polarizer, whereas an analyzer position is fixed. First the transmittance modeP-632909-PC(bright field) when the incoming light came from below the sample was used. The sample, Ni-mMOFs, were drop-casted from their solution (kept in DMF) onto a thin (0.17 mm) glass slide and covered with a glass slide with the same thickness on the top. The sample was raised 1 cm by using Teflon jigs to allow placement of a square (1 cm x 1 cm) neodymium magnet below the sample (see methods, Figure 1). The crystalline Ni-MOFs show birefringence under polarized light. When the polarizer is placed in parallel to the analyzer (Figure 21A), the synchronized rotational alignment of the crystals as a result of the magnetic field is observed. Their appearance change at MOFs angle of 45° due to the birefringence that splits the incoming light into two components that are parallel to the crystal optical axes. This effect is better seen under crosspolarized light when the polarizer is perpendicular to the analyzer (Figure 21B). In this case, the crystals acts as a third polarizer that is located between two perpendicular polarizers, allowing a maximum intensity at 45° (“ON” mode) and minimum intensity at 0° (“OFF” mode). Using a magnetic field, the “ON” and “OFF” modes of a group of crystals was controlled, thus effectively engineering optical switches that function akin to liquid crystals that change their orientation under external stimuli (electric field, magnetic field, heat, light, mechanical force, etc.). The control of the crystal’s alignment can be done to a large group of mMOFs. Because of the superparamagnetic property of the IONP, this effect is reversible; the mMOFs orientation is randomized once the magnetic field is removed and can be re-aligned with another exposure (Figures 22A-22D).[000174] The magnetic field enables us to control both speed of alignment, and the translocation of the mMOFs. Using non-polarized light, reflectance mode and dark-field light, the mMOFs outer surface are enhanced with no birefringence effect, while keeping the black background. It is also demonstrated that simultaneous changes in mMOFs location by recording their dynamic movement with magnetic field manipulation. Figures 23A-23C show the mMOFs changing their location, by marking each mMOFs’ center during the movement recording. The movement of the mMOFs is in three dimensions, as the mMOFs can also lay on their bases as observed at t = 10 sec.Fluorophore inclusion - magnetic MOFs[000175] There are routes for the formation of fluorescent magnetic MOFs, as the fluorophore can be added before or after magnetizing the MOFs (Figure 52A).[000176] Embedding sodium resorufin (SR) dye (7 A x 9.5 A) resulted in functionalization of the MOFs (coloration, fluorescence) and polarized absorption and emission dependency on the angle of the incoming polarized light. The MOFs have two types of chiral channels, hexagonal and triagonal with diameters of ~7.0 and -10.2 A. This dye exhibits strong dichroism underP-632909-PCpolarized light when it is aligned. When the polarization direction is aligned parallel to the optical axis, the crystals exhibit a distinct purple color. Conversely, when the polarization direction is perpendicular to the optical axis, the crystals appear nearly colorless. This property is used in addition to the birefringence that are observed in the crystal (Figures 39A-39F). The two routes from Figure 52 A are:1) Coloring the magnetic MOFs (Figure 52A, top): The mMOFs were colored by adding 0.05 mL of 0.42mM SR dye solution in DMF into an Eppendorf contained 0.5 mL mMOFs in DMF. After 24 h, the excess dye was removed by placing a magnet to the Eppendorf s edge, and changing the solvent to clean DMF while the dyed mMOFs are attracted to the magnet. The solvent was changed 3 times until the solution was colorless with the dispersed purple mMOF. Optical microscopy images (Figure 24A) show the dyed mMOFs under 3 angles of polarized light: 0°, 45°, 90° (left to right). The dyed mMOFs showed a dichroism effect as a result of the SR orientation inside mMOFs. SEM images (Figure 24B) showed the coating stability after dye inclusion. By that, the MOFs were functionalized after their magnetization. In this route, the SR dye was not visible after about a week (Figure 40).2) Magnetizing the dyed MOFs - “fluorescent mMOFs” (Figure 52 A, bottom): Dyeing the MOFs before the magnetization process resulted in a pink color of the MOFs (Figures 41A-41F). This color is a result of the different solvent used (here, the MOFs were dyed while kept in ethanol, than the solvent was changed to DMF before adding the IONP). In addition, magnetizing the MOFs did not affect the coloration of the MOFs. The dye remained incorporated inside the MOFs longer time (few months) comparing to dyeing the mMOFs (one week) (Figures 40, 43A-43D). These magnetized, dyed MOFs, named fluorescent mMOFs, were used for the dynamic movement experiments. SEM images of the fluorescent mMOFs (Figure 25A) show a uniform coating with the IONP. The presence of the IONP was further confirmed by using the EsB detector of the SEM (Figure 25B).[000177] The dynamic movement of magnetic dyed Ni-MOFs (Figure 52A, bottom) was recorded too, in the same way as for the Ni -mMOFs. The incorporation of the fluorophore into the MOFs enables us to create another switching mechanism, using the dye transition dipole moment. When the polarizer is parallel to the analyzer, the color appears at 45° (“ON” mode) and is not visible when the MOFs is at 0° (“OFF” mode) (Figure 26, A). At 45°, the polarized light is double refracting into 2 components which are parallel the crystal optical axis, and parallelP-632909-PCto the linear configuration of the dye in the MOFs’ channels, resulting at color appearance. Note that the birefringence can still be used as a switching mechanism, however the dye is not visible in that mechanism (Figure 26B). Using reflectance, dark field mode, polarized light did not cause switching, as expected in dark-field mode, but dynamic orientation with a colored mMOFs surface (Figures 44A-44B).Fluorescence microscope[000178] Looking at (Figures 27A-27D), the SR dye is visible at an excitation wavelength of 560 nm. Videos were taken before and after exposing the fluorescent mMOFs to a magnetic field.[000179] In addition to the SR dye, the ligand itself also exhibits fluorescence (Figures 45A-45C) under excitation at 350 nm. This property can be used to switch mMOFs at two excitation wavelengths, for the ligand and for the fluorophore. In Figures 28A-28C, the fluorescence Ni-mMOFs were excited at zC\c = 350 nm, and emission collected at A = 410-480 nm.Polarized Fluorescence microscope[000180] Using STED-SP8 microscope, the fluorescent mMOFs were observed under polarized light. The fluorescent mMOFs were drop-casted onto a cover slide (0.17 mm), and another cover slide (0.17 mm) was added on top. For the fluorophore SR, the excitation was performed using a white light laser at A = 561 nm and the emission signal was collected at a range of A = 571-650 nm. The rotatable polarizer was set to 0° or 90° positions. As for all the fluorescent mMOFs, a magnetic field was introduced to the samples using a square (1 cm x 1 cm) neodymium magnet (Eclipse Magnetics, N861) that was placed and moved ~1 cm away from the sample. The mMOFs dynamic movement was recorded (Figures 29A-29D).[000181] The normalized intensity vs time graphs (Figures 30A-30B, 31A-31B) shows the dependence of the fluorescent mMOFs intensity on the orientation of fluorescent mMOFs, compared to a background area selected as the region of interest (ROI). The normalized intensity was calculated for each ROI by LAS X Office program. When the polarization angle of the laser is set to 90° (Figure 30A), the general intensity of the fluorescent mMOFs was at the maximum with low background noise. It was observed that the fluorescent mMOFs have the highest intensity at MOF angle of 0° (longitudinal axis of the MOF) whereas lower intensities were observed at 45°, 90°.[000182] When the polarization angle of the laser is set to 0° (Figure 31 A), the general intensity of the fluorescent mMOFs was at the minimum with more background noise, and it was observed that the MOF angle with the highest normalized intensity is 45, while the lowest intensitiesP-632909-PCobserved at MOF angles of 0°, 90°. The background here has higher intensity, at this polarization due to a lower signal-to-noise ratio.[000183] In both laser polarization, it was observed that a change in the intensity, that is solely dependent on the orientation of the MOF. At 90° polarization, MOFs appears with the highest intensity at MOF angle of 0° and at 0° polarization, MOFs appears with the highest intensity at MOF angle of 45°. This phenomenon was observed also by looking at SR-dyed MOFs (nonmagnetic) (Figures 46A-46C). Both polarizations show the same dichroism effect, polarized-dependent emission, due to the alignment of the linear SR dye in the MOFs’ channels. As the polarized light is parallel to the longitudinal MOF axis, the intensity is higher. In the STED-SP8 microscope, the intensity change is ~ 20% between the highest and lowest normalized intensities, and it is dependent only on mMOFs orientation in space. The ability of dynamic alignment of fluorescent mMOFs, together with polarized-dependent emission, is thus shown.Methods of producing magnetic metal-organic framework particles[000184] In one embodiment the invention provides a method of producing magnetic metalorganic framework (mMOF) particles, the method comprising:providing metal-organic framework (MOF) particles dispersed in a first solvent, resulting in a first MOF dispersion;drying the first MOF dispersion until the first solvent is evaporated, resulting in dried MOF particles;dispersing the dried MOF particles in a second solvent, resulting in a second MOF dispersion;dispersing magnetic nanoparticles (mNPs) in a third solvent, resulting in a mNPs dispersion;adding the mNPs dispersion to the second MOF dispersion, resulting in a mNP / MOF dispersion;incubating the mNP / MOF dispersion, resulting in a mMOF particles dispersion.[000185] In one embodiment the first solvent, second solvent, and third solvent comprise any of the following selected from: ethanol, methanol, isopropanol, dimethylformamide (DMF), toluene, and hexane, or a combination thereof. In one embodiment the magnetic nanoparticles comprise iron oxide nanoparticles (IONPS).[000186] In one embodiment the mNP / MOF dispersion is lightly shaken before the incubating step. For example lightly shaking the mNP / MOF dispersion can comprise any of the followingP-632909-PCselected from: manual inversion of the container holding the dispersion, vortex mixing, orbital shaking on a platform, tapping the container gently, etc. The lightly shaking can be carried out for anywhere between 1 to 120 seconds.[000187] In one embodiment the drying is carried out by: blowing gas, heating, and vacuum pumping, or a combination thereof.[000188] In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 1 mg / mL to 50 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 1 mg / mL to 20 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 1 mg / mL to 10 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 1 mg / mL to 5 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 10 mg / mL to 20 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration ranging between 20 mg / mL to 40 mg / mL. In one embodiment the first MOF dispersion has a MOF particles to first solvent concentration of about 1 mg / mL.[000189] In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 1 mg / mL to 50 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 1 mg / mL to 20 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 1 mg / mL to 10 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 1 mg / mL to 5 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 10 mg / mL to 20 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration ranging between 20 mg / mL to 40 mg / mL. In one embodiment the second MOF dispersion has a dried MOF particles to second solvent concentration of about 1 mg / mL.[000190] In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.01 mg / mL to 1 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.1 mg / mL to 5 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.1 mg / mL to 1 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.1 mg / mL to 0.5 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration ranging between 0.1 mg / mL to 1 mg / mL. In one embodiment theP-632909-PCmNPs dispersion has a mNPs to third solvent concentration of about to 0.2 mg / mL. In one embodiment the mNPs dispersion has a mNPs to third solvent concentration of about to 0.5 mg / mL.[000191] In one embodiment the method further comprises adding a fourth solvent to the mNP / MOF dispersion. In one embodiment the fourth solvent comprises any of the following selected from: ethanol, methanol, isopropanol, dimethylformamide (DMF), toluene, and hexane, or a combination thereof.[000192] In one embodiment the method further comprises centrifuging the mNP / MOF dispersion at least once before the incubating step.[000193] In one embodiment the centrifuging is carried out at spinning rate ranging between 3000-5000 rpm and for a duration ranging between 30 seconds to 20 minutes. In one embodiment the centrifuging is carried out at a spinning rate of about 4000 rpm and for a duration of about 1 min. In one embodiment the centrifuging is carried out at spinning rate of about 4000 rpm and for a duration of about 5 mins. In one embodiment the centrifuging is carried out at a spinning rate of about 4000 rpm and for a duration of about 30 mins.[000194] In one embodiment, the term “a” or “one” or “an” refers to at least one. In one embodiment the phrase “two or more” may be of any denomination, which will suit a particular purpose. In one embodiment, “about” or "approximately" may comprise a deviance from the indicated term of + 1 %, or in some embodiments, - 1 %, or in some embodiments, ± 2.5 %, or in some embodiments, ± 5 %, or in some embodiments, ± 7.5 %, or in some embodiments, ± 10 %, or in some embodiments, ± 15 %, or in some embodiments, ± 20 %, or in some embodiments, ± 25 %.[000195] Those skilled in the art to which this invention pertains will readily appreciate that numerous changes, variations, and modifications can be made without departing from the scope of the presently disclosed subject matter, mutatis mutandis.

Claims

P-632909-PCCLAIMS1. An opto-magnetic switch comprising:a substrate;porous anisotropic-shaped nanoparticles with magnetic nanoparticles (MNPs) attached on the surface of the porous anisotropic-shaped nanoparticles, resulting in magnetic anisotropic nanoparticles;wherein the porous anisotropic-shaped nanoparticles comprise metal organic frameworks (MOFs);a solvent or gel within which the magnetic anisotropic nanoparticles are dispersed; andwherein the magnetic anisotropic nanoparticles are configured to collectively align and / or move in a predetermined direction in response to an external magnetic field.

2. The opto-magnetic switch of claim 1 wherein the anisotropic shape is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism.

3. The opto-magnetic switch of claim 1 wherein the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof.

4. The opto-magnetic switch of claim 1 wherein the MNPs are selected from: FesC , y- FeiCh, FeCo, FeCoFe2O4, NiFe2O4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao sSro CoCh, or a combination thereof.

5. The opto-magnetic switch of claim 1 wherein the MNPs further comprise a capping layer.

6. The opto-magnetic switch of claim 5 wherein the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HD A), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochloride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinyl alcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof.P-632909-PC7. The opto-magnetic switch of claim 1 wherein the porous anisotropic-shaped nanoparticles further comprise at least one dye incorporated therein.

8. The opto-magnetic switch of claim 7 wherein the dye is selected from: optical, fluorescent, or a combination thereof.

9. The opto-magnetic switch of claim 7 wherein the dye comprises any of the following selected from: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5- aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7,7,8, 8-tetracyanoquinodimethane (TCNQ).

10. The opto-magnetic switch of claim 1 wherein the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane, cyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or a combination thereof.

11. The opto-magnetic switch of claim 1 further comprising an encapsulation layer.

12. The opto-magnetic switch of claim 11 wherein the substrate and the encapsulation layer comprise any of the following selected from: glass, AI2O3, quartz, silicon oxide, fluorine-doped tin oxide (FTO), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), cyclo-olefin polymer (COP), cycloolefin copolymer (COC), polymethyl methacrylate (PMMA, acrylic), and polycarbonate (PC), or a combination thereof.

13. A display system or interface comprising the opto-magnetic switch of claim 1.

14. An opto-magnetic system comprising:the opto-magnetic switch of claim 1;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; andP-632909-PCa magnetic-field inducing apparatus configured to generate a varying magnetic field, thereby controlling the position and / or orientation of the magnetic anisotropic nanoparticles within the opto-magnetic switch;wherein the position and / or orientation of the magnetic anisotropic nanoparticles relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.

15. The opto-magnetic system of claim 14 wherein the porous anisotropic-shaped nanoparticles are metal organic framework (MOF) particles, and wherein the magnetic anisotropic nanoparticles are magnetic MOF (mMOF) particles.

16. The opto-magnetic system of claim 14 wherein the analyzer is positioned perpendicular to the polarizer.

17. The opto-magnetic system of claim 15 wherein the polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer.

18. The opto-magnetic system of claim 14 wherein the light source is selected from: laser, or light-emitting diode (LED).

19. The opto-magnetic system of claim 14 wherein the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof.

20. The opto-magnetic system of claim 14 further comprising a controller configured to:implement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the magnetic anisotropic nanoparticles; orimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.

21. An opto-magnetic device comprising:a substrate;a film comprising porous anisotropic-shaped nanoparticles with magnetic nanoparticles (MNPs) attached on the surface of the porous anisotropic-shaped nanoparticles, resulting in a magnetic anisotropic nanoparticles; andP-632909-PCwherein the magnetic anisotropic nanoparticles are permanently aligned in a predetermined direction.

22. The opto-magnetic device of claim 21 wherein the porous anisotropic-shaped nanoparticles comprise metal organic framework (MOF) particles.

23. The opto-magnetic device of claim 21 wherein the anisotropic shape and / or structure is selected from: elongated shape, barrel, elongated cuboid, elongated ellipsoid, cylinder, rod, wire, tube, egg, hexagonal, stella-octangula, star, and prism.

24. The opto-magnetic device of claim 21 wherein the MNPs comprise any of the following selected from: Fe, Co, Ni, Nd, Gd, Dy, Tb, Sm, Mn, and Cr, or a combination thereof.

25. The opto-magnetic device of claim 21 wherein the MNPs are selected from: FesC , y- FeiCh, FeCo, FeCoFe2O4, NiFe2C>4, MnFe2O4, FePt, Co, Ni, NdFeB, FexNii-x, and Lao sSro CoCh, or a combination thereof.

26. The opto-magnetic device of claim 21 wherein the MNPs further comprise a capping layer.

27. The opto-magnetic device of claim 26 wherein the capping layer comprises any of the following selected from: chitosan (CS), ethylenediaminetetraacetic acid (EDTA), hexadecylamine (HD A), hexadecylthiol (HDT), oleic acid (OA), poly(allylamine hydrochloride) / poly(styrene sulfonate) (PAH / PSS), poly(amidoamine) dendrimer with amino groups (Generation 4) (PAMAM NH2, G4), polyvinyl alcohol (PVA), poly(vinylpyrrolidone) (PVP), and tetradecyltrimethylammonium bromide (TTAB), or a combination thereof.

28. The opto-magnetic device of claim 21 wherein the porous anisotropic-shaped nanoparticles further comprise at least one dye incorporated therein.

29. The opto-magnetic device of claim 28 wherein the dye is selected from: optical, fluorescent, or a combination thereof.

30. The opto-magnetic device of claim 28 wherein the dye comprises any of the following selected from: sodium resorufin (SR), methyl orange (MO), fluorescein (SF), 5- aminofluorescein (AF), fluorescein isothiocyanate isomer I (FITC), sulforhodamine B, brilliant blue R250 (BBR), and the lithium salt of 7,7,8, 8-tetracyanoquinodimethane (TCNQ).P-632909-PC31. The opto-magnetic device of claim 21 wherein the solvent or gel comprises any of the following selected from: toluene, acetone, methanol, ethyl acetate, isopropanol, ethanol, dimethylformamide (DMF), N,N-Dimethylacetamide (DMAc), chloroform, tetrahydrofuran (THF), N-Methyl-2 -pyrrolidone (NMP), hexane, cyclohexane, cyacetonitrile (ACN), dimethyl sulfoxide (DMSO), dichloromethane (DCM), water, salt, buffer, resin, and glycerol, or a combination thereof.

32. The opto-magnetic device of claim 21 further comprising an encapsulation layer.

33. The opto-magnetic device of claim 32 wherein the substrate and the encapsulation layer comprise any of the following selected from: glass, AI2O3, quartz, silicon oxide, fluorine-doped tin oxide (FTO), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polydimethylsiloxane (PDMS), cyclo-olefin polymer (COP), cycloolefin copolymer (COC), polymethyl methacrylate (PMMA, acrylic), and polycarbonate (PC), or a combination thereof.

34. An opto-magnetic device system comprising:the opto-magnetic device of claim 21;a light source configured to produce light;a polarizer positioned to receive the light and produce polarized light;an analyzer positioned to receive the polarized light that has passed through the opto-magnetic switch; andwherein the position and / or orientation of the magnetic anisotropic nanoparticles relative to the polarizer and analyzer alters the intensity and / or color of the polarized light detected by the analyzer.

35. The opto-magnetic device system of claim 34 wherein the magnetic anisotropic nanoparticles comprise metal organic framework (MOF) particles.

36. The opto-magnetic device system of claim 34 wherein the analyzer is positioned perpendicular to the polarizer.

37. The opto-magnetic device system of claim 36 wherein the polarizer is further configured to rotate relative to the analyzer thereby changing the intensity and / or color of the polarized light detected by the analyzer.

38. The opto-magnetic device system of claim 34 wherein the light source is selected from:laser, or light-emitting diode (LED).P-632909-PC39. The opto-magnetic device system of claim 34 wherein the analyzer comprises a photodetector, a camera, a photodiode, or a combination thereof.

40. The opto-magnetic device system of claim 34 further comprising a controller configured to:implement changes in the magnetic-field inducing apparatus to achieve a predetermined position and / or orientation of the magnetic anisotropic nanoparticles; orimplement a predetermined rotational change to the polarizer;thereby controlling the intensity, color, and / or polarization of the polarized light detected by the analyzer.

41. A method of fabricating an opto-magnetic device, the method comprising:providing a substrate;providing a solvent or gel comprising magnetic anisotropic nanoparticles, resulting in a magnetic anisotropic nanoparticles;dispersing the magnetic anisotropic nanoparticles on the substrate; evaporating or curing the solvent or gel whilst the magnetic anisotropic nanoparticles are oriented in a predetermined direction by an external magnetic field thereby resulting in the magnetic anisotropic nanoparticles being permanently oriented in the predetermined direction on the substrate.

42. The method of claim 41 wherein the evaporating comprises any of the following selected from: vacuum drying, gas flow drying, thermal drying, or a combination thereof.

43. The method of claim 41 wherein the curing is carried out at a temperature ranging between 100 to 200 °C.

44. A method of producing magnetic metal-organic framework (mMOF) particles, the method comprising:providing metal-organic framework (MOF) particles dispersed in a first solvent, resulting in a first MOF dispersion;drying the first MOF dispersion until the first solvent is evaporated, resulting in dried MOF particles;P-632909-PCdispersing the dried MOF particles in a second solvent, resulting in a second MOF dispersion;dispersing magnetic nanoparticles (mNPs) in a third solvent, resulting in a mNPs dispersion;adding the mNPs dispersion to the second MOF dispersion, resulting in a mNP / MOF dispersion;incubating the mNP / MOF dispersion, resulting in a mMOF particles dispersion.

45. The method of claim 44 wherein the first solvent, second solvent, and third solvent comprise any of the following selected from: ethanol, methanol, isopropanol, dimethylformamide (DMF), toluene, and hexane, or a combination thereof.

46. The method of claim 44 wherein the magnetic nanoparticles comprise iron oxide nanoparticles (IONPS).

47. The method of claim 44 wherein the drying is carried out by: blowing gas, heating, and vacuum pumping, or a combination thereof.

48. The method of claim 44 further comprising centrifuging the mNP / MOF dispersion at least once, before the incubating step.

49. The method of claim 48 wherein the centrifuging is carried out at spinning rate ranging between 3000-5000 rpm and for a duration ranging between 30 seconds to 20 minutes.