A process for preparing an active material and implementation thereof

Pulsation mixing of silicon and carbon-based materials at specific speeds addresses uneven distribution issues in lithium-ion batteries, enhancing mechanical stability and electrochemical performance.

WO2026239411A1PCT designated stage Publication Date: 2026-11-19OLA ELECTRIC MOBILITY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2026/050823
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges such as uneven distribution of silicon particles, lower material homogeneity, uneven current density, and varying particle shapes and sizes, leading to reduced packing efficiency, lower energy density, and safety issues due to localized heating and mechanical instability.

Method used

A process involving pulsation mixing of a silicon compound with a carbon-based material at alternating speeds (2500-3500 rpm and 1000-1500 rpm) for 7-20 minutes each, repeated twice, to achieve a uniform distribution of silicon particles in the active material.

Benefits of technology

The process results in a homogeneous active material with improved mechanical stability, enhanced electrochemical performance, and increased cycle life, ensuring efficient electron flow and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000019_0001_TABLE
    Figure IMGF000019_0001_TABLE
  • Figure IMGF000021_0001_TABLE
    Figure IMGF000021_0001_TABLE
  • Figure 00000028_0000
    Figure 00000028_0000
Patent Text Reader

Abstract

The present disclosure provides a process for preparing an active material, the process comprising: pulse mixing a mixture comprising a silicon compound / composite and a carbon based anode active material to obtain the diluted anode active material, wherein the pulse mixing comprises a) a first pulse mixing at a rotational speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes, followed by, b) a second pulse mixing at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice The present disclosure further provides an active material obtained by the process and an anode comprising the active material obtained by the process.
Need to check novelty before this filing date? Find Prior Art

Description

A PROCESS FOR PREPARING AN ACTIVE MATERIAL AND IMPLEMENTATION THEREOF FIELD OF INVENTION

[0001] The subject matter of the present disclosure broadly relates to the field of battery. Particularly, the present disclosure relates to a process of preparing an active material. Additionally, the present disclosure relates to an active material and anode comprising the active material.BACKGROUND OF THE INVENTION

[0002] The increasing fascination with lithium-ion batteries (LIBs) is primarily fuelled by their superior energy density, faster charging times, and extended lifespan compared to traditional batteries. These benefits make them well-suited for electric vehicles, portable electronics, and various other applications.

[0003] In LIBs, the anode is composed of an anode active material (AAM), which is crucial for achieving high energy density and directly influences the battery’s capacity. This development in the anode of LIBs is crucial for improving battery performance, providing high energy density, and contributing to the overall capacity of the battery. The AAM of electrode must ensure uniform distribution of active materials throughout and maintain mechanical stability to support high energy density and safety. This alignment underscores the criticality of optimizing electrode active materials and design to achieve the desired battery performance and safety standards.

[0004] Several researchers have developed LIBs using silicon (Si) blended with carbon-based materials as an active material for the anode. However, existing Li-Si batteries face challenges such as uneven / nonuniform distribution of Si particles, lower material homogeneity, uneven current density, localized n / p variations and varying particle shapes and sizes. These issues can lead to reduced packing efficiency, lower energy density, inherently lower electrical conductivity, localized heating and safety.

[0005] The inhomogeneous mixing of Si particles in the active material blend in LIBs leads to rapid capacity fading and reduced cycle life of the battery. To address these issues, advanced mixing techniques such as dry particle mixing and ball milling are employed to achieve a more regular distribution of silicon particles.However, the development of highly efficient Si based homogeneously mixed active material remains a challenging task.

[0006] Therefore, there is a dire need to develop a process for preparing a Si based active material blend that can overcome the above-mentioned drawbacks and provide an improved mechanical and electrochemically efficient active material.SUMMARY OF THE INVENTION

[0007] In an aspect of the present disclosure, there is provided a process for preparing an active material, the process comprising: pulse mixing a mixture comprising a silicon compound and a carbon based material to obtain the active material, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes, followed by, b) a second pulse mixing at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice.

[0008] In another aspect of the present disclosure, there is provided an active material obtained by the process as disclosed herein, wherein the active material has a particle size (D50) distribution in a range of 11 to 14 micron.

[0009] In one another aspect of the present disclosure, there is provided an anode comprising: a) the active material obtained by the process as disclosed herein; b) a conductive additive; and c) a binder.

[0010] In yet another aspect of the present disclosure, there is provided an electrochemical cell comprising: (a) the anode as disclosed herein; (b) a cathode, and (c) an electrolyte.

[0011] These and other features, aspects, and advantages of the present subject matter will be better understood with reference to the following detailed description and appended claims. This summary is provided to introduce a selection of concepts in a simplified form. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The following drawings form a part of the present specification and are included to further illustrate aspects of the present disclosure. The disclosure may be better understood by reference to the drawings in combination with the detailed description of the specific embodiments presented herein.

[0013] Figure 1 depicts energy dispersive X-ray spectroscopy (EDS) images of pulse mixed mixture of the active material Al (a) after 60 minutes of pulsation mixing, and (b) after 120 minutes of pulsation mixing, in accordance with an embodiment of the present disclosure.

[0014] Figure 2 depicts energy dispersive X-ray spectroscopy (EDS) images of the comparative active material AP2 (a) after 30 minutes of conventional continuous mixing, (b) after 60 minutes of conventional continuous mixing, (c) after 90 minutes of conventional continuous mixing, (d) after 120 minutes of conventional continuous mixing, (e) after 150 minutes of conventional continuous mixing, and (f) after 180 minutes of conventional continuous mixing, in accordance with an embodiment of the present disclosure.

[0015] Figure 3 depicts (a) energy dispersive X-ray spectroscopy (EDS) image of the active material Al, (b) energy dispersive X-ray spectroscopy (EDS) image of silicon (Si), (c) energy dispersive X-ray spectroscopy (EDS) image of graphite / carb on (C), (d) backscattered electron image of pulse mixed mixture of the comparative active material API, after 60 minutes of pulsation, (e) energy dispersive X-ray spectroscopy (EDS) image of the comparative active material API, after 60 minutes of pulsation, (f) backscattered electron image of pulse mixed mixture of the comparative active material API, after 120 minutes of pulsation, (g) energy dispersive X-ray spectroscopy (EDS) image of the comparative active material API, after 120 minutes of pulsation, in accordance with an embodiment of the present disclosure.

[0016] Figure 4 depicts particle size (D50) distribution (a) of silicon carbide used for preparation of active material Al, (b) of graphite used for preparation of active material Al, (c) pulse mixed mixture of the active material Al after 60 minutes of pulsation mixing, (d) pulse mixed mixture of the active material Al after 120minutes of pulsation mixing, (e) pulse mixed mixture of the comparative active material API after 60 minutes of pulsation mixing, (f) pulse mixed mixture of the comparative active material API after 120 minutes of pulsation mixing, (g) mixture of the comparative active material AP2 after 60 minutes of conventional continuous mixing, (h) mixture of the comparative active material AP2 after 120 minutes of conventional continuous mixing, and (i) mixture of the comparative active material AP2 after 180 minutes of conventional continuous mixing, in accordance with an embodiment of the present disclosure.

[0017] Figure 5 depicts peel strength, and resistance data of the active material Al and the comparative active material AP2, in accordance with an embodiment of the present disclosure.

[0018] Figure 6 depicts the discharge capacity, initial coulombic efficiency (ICE), coulombic efficiency of cycle 1 and cycle 2 of electrochemical cell prepared with the anode El and the comparative anode EP2, in accordance with an embodiment of the present disclosure.

[0019] Figure 7 depicts the discharge capacity, average discharge capacity, and standard deviation of electrochemical cells / comparative electrochemical cells i.e. EC1 / ECP2, EC2 / ECP3, EC3 / ECP4, and EC4 / ECP5, prepared with anode / comparative anode E1ZEP2, in accordance with an embodiment of the present disclosure.

[0020] Figure 8 depicts the capacity retention of the electrochemical cell ECI, and the comparative electrochemical cell ECP2, in accordance with an embodiment of the present disclosure.DETAILED DESCRIPTION OF THE INVENTION

[0021] Those skilled in the art will be aware that the present disclosure is subject to variations and modifications other than those specifically described. It is to be understood that the present disclosure includes all such variations and modifications. The disclosure also includes all such steps, features, compositions, and compounds referred to or indicated in this specification, individually orcollectively, and any and all combinations of any or more of such steps or features. Definitions

[0022] For convenience, before further description of the present disclosure, certain terms employed in the specification, and examples are delineated here. These definitions should be read in the light of the remainder of the disclosure and understood as by a person of skill in the art. The terms used herein have the meanings recognized and known to those of skill in the art, however, for convenience and completeness, particular terms and their meanings are set forth below.

[0023] The articles “a”, “an” and “the” are used to refer to one or to more than one (i.e., to at least one) of the grammatical object of the article.

[0024] The terms “comprise” and “comprising” are used in the inclusive, open sense, meaning that additional elements may be included. It is not intended to be construed as “consists of only”.

[0025] Throughout this specification, unless the context requires otherwise the word “comprise”, and variations such as “comprises” and “comprising”, will be understood to imply the inclusion of a stated element or step or group of elements or steps but not the exclusion of any other element or step or group of elements or steps.

[0026] The term “at least one” is used to mean one or more and thus includes individual components as well as mixtures / combinations.

[0027] The term “active material” refers to electrode active material.

[0028] The term “silicon compound” refers to the component within an active material that actively participate in the electrochemical reactions necessary for energy storage and release. For the purpose of present disclosure, the silicon compound is selected from silicon carbide (SiC), silicon oxide (SiOx, x<2), amorphous silicon (a-Si), silicon quantum dots, or combinations thereof.

[0029] The term “carbon based material” refers to carbon based compounds which aid with silicon compound in the preparation of active material. For the purpose of present disclosure, carbon based material is selected from artificial graphite, natural graphite, hard carbon, soft carbon, or combinations thereof.

[0030] The term “pulsation mixing” refers to a mixing technique where the mixture is subjected to periodic variations in speed and intensity. This method involves alternating between high-speed and low-speed pulses to enhance the mixing process. The high-speed pulses create strong turbulence, while the low-speed pulses allow for more thorough blending of the components. For the purpose of present disclosure, the mixture of a silicon compound and a carbon based material is subjected to pulsation mixing comprising a first pulse at a speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes followed by a second pulse at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes. The first pulse mixing and the second pulse mixing are sequentially repeated at least twice to obtain an active material.

[0031] The term “conductive additive” refers to a conducting substance and is useful for the preparation of electrode, particularly anode. For the purposes of the present disclosure, the conductive additive is selected from graphene, carbon black, carbon nanofiber, carbon nanotube, flaky carbon, or combinations thereof.

[0032] The term “binder” refers to a type of binding constituent of an electrode, particularly anode, which has the property to provide adhesion to the active material when loaded on a current collector to obtain anode. For the purposes of the present disclosure, the binder is selected from carboxymethyl cellulose (CMC), lithium modified carboxymethyl cellulose (Li-CMC), sodium modified carboxymethyl cellulose (Na-CMC), styrene-butadiene rubber (SBR), modified styrene-butadiene rubber, poly acrylic acid modified styrene-butadiene rubber (SBR-PAA), rubber based polymers, polyacrylic acid (PAA), modified polyacrylic acid, lithium modified polyacrylic acid (Li-PAA), acrylates, amides, imides based polymer, or combinations thereof.

[0033] The term “particle size distribution (PSD)” refers to the range and proportion of different-sized particles of a sample, such as powders, granular materials, or particles. Particularly, PSD is expressed by mass or volume, showing the relative amounts of particles according to their sizes. PSD provides a comprehensive overview of the range and proportion of different-sized particleswithin a sample, often represented through graphs or tables showing the percentage of particles at various sizes.

[0034] The term “D50” or “median particle size” refers to the median particle size of a sample, at a specific point within the PSD. It is a key metric derived from the PSD that summarizes the central tendency of particle sizes in a sample. It indicates the particle diameter at which 50% of the particles are smaller and 50% are larger. For the purposes of the present disclosure, the active material has a particle size (D50) distribution in a range of 11 to 14 micron.

[0035] The term “electrode density” refers to volumetric mass density of an electrode material, which includes the active material, conductive additive, and binder. It measures the mass of the electrode material packed in a given volume. The higher electrode density is indicative of improved energy and power density in batteries. For the purposes of the present disclosure, the anode exhibits an electrode density in the range of 1.0 to 2.0 g / cc.

[0036] The term “mass loading” refers to the amount of active material deposited per unit area of the anode. Higher mass loading indicates the presence of more active material, which enhances the energy storage capacity of the anode. For the purposes of the present disclosure, the anode has mass loading in the range of 6.5 to 12.0 mg / cm2.

[0037] The term “electrical resistance” refers to the opposition that a material presents towards the flow of electric current. The electrical resistance of an anode depends on the properties / amounts of the active material, conductive additive, and binder, along with the structure and morphology of the active material. Lower electrical resistance in anode allows for more efficient electron flow, which can enhance the overall performance of the battery by improving its energy and power density. For the purposes of the present disclosure, the anode exhibits an average electrical resistance in a range of 0.0078 to 0.0083 Q.

[0038] The term “peel strength” refers to the force required to separate the active material from current collector of anode. This is the measure of integrity and efficiency of the battery performance and durability. For the purpose of present disclosure, the anode has a peel strength in a range of 1.0 to 2.5 N / 25mm.

[0039] The term “charge-discharge capacity” refers to the ability of an electrochemical cell to store and release charge during the charging and discharging processes, respectively. This is an important parameter for evaluating the performance of electrochemical cells.

[0040] The term “initial coulombic efficiency” (ICE) refers to a measure of the efficiency of the first charge-discharge cycle of an electrochemical cell. Specifically, it is the ratio of the discharge capacity to the charge capacity during the first cycle, expressed as a percentage. A higher ICE indicates that a larger proportion of the charge stored during the first cycle can be recovered during discharge. It reflects longer battery life and better overall efficiency.

[0041] The term “capacity retention” refers to the percentage of the initial capacity that an electrochemical cell retains after a certain number of cycles. It is a measure of an electrochemical cell’s ability to maintain its charge capacity over time and through multiple charge-discharge cycles.

[0042] Ratios, concentrations, amounts, and other numerical data may be presented herein in a range format. It is to be understood that such range format is used merely for convenience and brevity and should be interpreted flexibly to include not only the numerical values explicitly recited as the limits of the range, but also to include all the individual numerical values or sub-ranges encompassed within that range as if each numerical value and sub-range is explicitly recited.

[0043] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. Although any methods and materials similar or equivalent to those described herein can be used in the practice or testing of the disclosure, the preferred methods, and materials are now described.

[0044] The present disclosure is not to be limited in scope by the specific embodiments described herein, which are intended for the purposes of exemplification only. Functionally equivalent products, and methods are clearly within the scope of the disclosure, as described herein.

[0045] As discussed in the background, there is a need in the art to develop an active material for the anode of lithium-ion batteries (LIBs) with improved mechanicalproperties, better electrochemical performance, and enhanced coulombic efficiency. Several approaches, such as advanced mixing techniques like ball milling and conventional dry particle mixing, are employed to achieve a more uniform distribution of silicon (Si) particles with carbon based materials. However, these techniques, result in uneven distribution of Si particles, leading to agglomeration and reduced uniformity. This uneven distribution decreases packing efficiency, reduces capacity retention, lowers electrical conductivity, and causes localized heating. Nevertheless, the development of highly efficient Si and carbon based homogeneously mixed active material remains a challenging task. There is still a need to develop a process for preparing a uniformly mixed Si with carbonbased active material. Hence, to overcome these challenges, the present disclosure focuses on improving the mixing process of Si particles with carbon based material by introducing a pulsation technique and optimizing the mixing time. The active material of the present disclosure possesses enhanced electrochemical performance.

[0046] The present process for the preparation of an active material involves pulsation mixing of Si compound with carbon based material, with first pulse mixing at 2500 to 3500 rpm for 7 to 20 minutes, followed by second pulse mixing at 1000 to 1500 rpm for 7 to 20 minutes, and repeating the first and second pulse mixing sequentially at least twice, completing a total process time of 90 to 180 minutes. Mixing the Si compound with carbon based material at 2500 to 3500 rpm, and 1000 to 1500 rpm optimizes the balance between intensity and particle integrity. Pulsating the mixture at 2500 to 3500 rpm provides high shear force to break agglomerates and ensures even dispersion, while pulsating the mixture at 1000 to 1500 rpm reduces mechanical stress and prevents excessive particle breakage. These two mixing with different pulses provide a balance between effective mixing with material integrity. The optimal duration for pulsation mixing is between 90 to 180 minutes, which ensures effective dispersion of Si compound in carbon based material while reducing overall processing time compared to conventional mixing time. Thus, the present process minimizes processing time without compromising homogeneity. Sequential mixing with two different pulses, alternating every 7 to 20 minutes between 2500 to 3500 rpm, and 1000 to 1500 rpm continuously maintainsuniformity of the active material, preventing Si compound from settling or clustering. This process results in a homogeneous and uniform distribution of Si particles in carbon based material, enhancing the anode’s performance. Electrochemical data confirms that the homogeneously dispersed active material prepared by the process of the present disclosure exhibits improved battery’s cycle life up to 50 cycles.

[0047] The active material has enhanced peel strength and good contact with current collectors. It also shows good electrical conductivity by creating efficient conductive pathways due to its homogeneous uniform feature. Further, high and increased mechanical stability, prevents structural failure during cycling. These features make the disclosed active material a commercially viable and effective anode material with extensive market potential. Hence, the pulsation mixing of Si compound and carbon based material in a specific sequential manner as disclosed in the present disclosure, provides highly unvarying homogenous active material with enhanced mechanical and electrochemical properties.

[0048] In an embodiment of the present disclosure, there is provided a process for preparing an active material, the process comprising: pulse mixing a mixture comprising a silicon compound and a carbon based material to obtain the active material, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes, followed by, b) a second pulse mixing at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice. In another embodiment of the present disclosure, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 2700 to 3300 rpm for a time period in the range of 8 to 18 minutes, followed by, b) a second pulse mixing at a speed in the range of 1100 to 1400 rpm for a time period in the range of 8 to 18 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice. In yet another embodiment of the present disclosure, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 2800 to 3100 rpm for a time period in the range of 8 to 15 minutes, followed by, b) a second pulse mixing at a speed in therange of 1100 to 1300 rpm for a time period in the range of 8 to 15 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least thrice to six times. In still another embodiment of the present disclosure, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 3000 rpm for a time period of 9 to 13 minutes, followed by, b) a second pulse mixing at a speed in the range of 1200 rpm for a time period in the range of 9 to 13 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated six times.

[0049] In an embodiment of the present disclosure, there is provided a process for preparing an active material as disclosed herein, wherein the first pulse mixing and the second pulse mixing are sequentially repeated two to eight times, for a total time period of 90 to 160 minutes. In another embodiment of the present disclosure, the first pulse mixing and the second pulse mixing are sequentially repeated three to seven times, for a total time period of 95 to 150 minutes. In yet another embodiment of the present disclosure, the first pulse mixing and the second pulse mixing are sequentially repeated four to seven times, for a total time period of 100 to 140 minutes.

[0050] In an embodiment of the present disclosure, there is provided a process for preparing an active material as disclosed herein, wherein the silicon compound is selected from silicon carbide (SiC), silicon oxide (SiOx,x<2), amorphous silicon (a-Si), silicon quantum dots, or combinations thereof; and the silicon precursor is in a weight range of 2 to 55% (w / w) , with respect to total weight of the active material. In another embodiment of the present disclosure, the silicon compound is selected from silicon carbide (SiC), silicon oxide (SiOx. x<2), amorphous silicon (a-Si), or combinations thereof; and the silicon precursor is in a weight range of 5 to 50% (w / w), with respect to total weight of the active material. In yet another embodiment of the present disclosure, the silicon compound is selected from silicon carbide (SiC), amorphous silicon (a-Si), or combinations thereof; and the silicon precursor is in a weight range of 10 to 50% (w / w), with respect to total weight of the active material.

[0051] In an embodiment of the present disclosure, there is provided a process for preparing an active material as disclosed herein, wherein the carbon based material is selected from artificial graphite, natural graphite, hard carbon, soft carbon, graphene-modified graphite, or combinations thereof; and the carbon based material is in a weight range of 45 to 95% (w / w), with respect to total weight of the active material. In another embodiment of the present disclosure, the carbon based material is selected from artificial graphite, natural graphite, hard carbon, soft carbon, or combinations thereof; and the carbon based material is in a weight range of 48 to 90% (w / w), with respect to total weight of the active material. In yet another embodiment of the present disclosure, the carbon based material is selected from artificial graphite, natural graphite, or combinations thereof; and the carbon based material is in a weight range of 50 to 90% (w / w), with respect to total weight of the active material.

[0052] In an embodiment of the present disclosure, there is provided a process for preparing an active material as disclosed herein, wherein the active material has a particle size (D50) distribution in a range of 6 to 9 micron for silicon compound and 12 to 15 micron for carbon based material. In another embodiment of the present disclosure, the active material has a particle size (D50) distribution in a range of 6 to 8.5 micron for silicon compound and 12.5 to 15 micron for carbon based material. In yet another embodiment of the present disclosure, the active material has a particle size (D50) distribution in a range of 6.5 to 8.5 micron for silicon compound and 13 to 15 micron for carbon based material.

[0053] In an embodiment of the present disclosure, there is provided an active material obtained by the process as disclosed herein, wherein the active material blend has a particle size (D50) distribution in a range of 11 to 14 micron. In another embodiment of the present disclosure, the active material blend has a particle size (D50) distribution in a range of 11 to 13.5 micron. In yet another embodiment of the present disclosure, the active material blend has a particle size (D50) distribution in a range of 11 to 13 micron.

[0054] In an embodiment of the present disclosure, there is provided an anode comprising: a. the active material obtained by the process as disclosed herein; b. a conductive additive; and c. a binder.

[0055] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the active material is in a weight range of 92 to 98%, with respect to the total weight of the anode. In another embodiment of the present disclosure, the active material is in a weight range of 93 to 98%, with respect to the total weight of the anode. In yet another embodiment of the present disclosure, the active material is in a weight range of 94 to 97%, with respect to the total weight of the anode.

[0056] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the conductive additive is selected from graphene, carbon black, carbon nanofiber, carbon nanotube, flaky carbon, or combinations thereof; and the conductive additive is in a weight range of 0.2 to 3.5%, with respect to total weight of the anode. In another embodiment of the present disclosure, the conductive additive is selected from graphene, carbon black, carbon nanofiber, carbon nanotube, or combinations thereof; and the conductive additive is in a weight range of 0.3 to 3.3%, with respect to total weight of the anode. In yet another embodiment of the present disclosure, the conductive additive is selected from graphene, carbon nanofiber, carbon nanotube, or combinations thereof; and the conductive additive is in a weight range of 0.4 to 3.0%, with respect to total weight of the anode.

[0057] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the binder is selected from carboxymethyl cellulose (CMC), lithium modified carboxymethyl cellulose (Li-CMC), sodium modified carboxymethyl cellulose (Na-CMC), styrene-butadiene rubber (SBR), modified styrene-butadiene rubber, poly acrylic acid modified styrene-butadiene rubber (SBR-PAA), rubber based polymers, polyacrylic acid (PAA), modified polyacrylic acid, lithium modified polyacrylic acid (Li-PAA), acrylates, amides, imides based polymer, or combinations thereof; and the binder is in a weight range of 1.8 to 5% (w / w), with respect to total weight of the anode. In another embodiment of thepresent disclosure, the binder is selected from carboxymethyl cellulose (CMC), lithium modified carboxymethyl cellulose (Li-CMC), sodium modified carboxymethyl cellulose (Na-CMC), styrene-butadiene rubber (SBR), modified styrene-butadiene rubber, poly acrylic acid modified styrene-butadiene rubber (SBR-PAA), rubber based polymers, polyacrylic acid (PAA), modified polyacrylic acid, acrylates, amides, or combinations thereof; and the binder is in a weight range of 1.8 to 4.5% (w / w), with respect to total weight of the anode. In yet another embodiment of the present disclosure, the binder is selected from carboxymethyl cellulose (CMC), lithium modified carboxymethyl cellulose (Li-CMC), sodium modified carboxymethyl cellulose (Na-CMC), styrene-butadiene rubber (SBR), modified styrene-butadiene rubber, poly acrylic acid modified styrene-butadiene rubber (SBR-PAA), rubber based polymers, polyacrylic acid (PAA), modified polyacrylic acid, or combinations thereof; and the binder is in a weight range of 2 to 4.0% (w / w), with respect to total weight of the anode.

[0058] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, further comprises a current collector. In another embodiment of the present disclosure, the current collector is selected from copper (Cu) foil, primer coated copper foil, graphene-coated foil.

[0059] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode has a peel strength in a range of 1.0 to 2.5 N / 25mm. In another embodiment of the present disclosure, the anode has a peel strength in a range of 1.0 to 2.2 N / 25mm. In yet another embodiment of the present disclosure, the anode has a peel strength in a range of 1.0 to 2.0 N / 25mm.

[0060] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode has a density in a range of 1.0 to 2.0 g / cc; and a mass loading in the range of 6.5 to 12.0 mg / cm2In another embodiment of the present disclosure, the anode has a density in a range of 1.2 to 1.7 g / cc; and a mass loading in the range of 6.7 to 11.0 mg / cm2. In yet another embodiment of the present disclosure, the anode has a density in a range of 1.4 to 1.7 g / cc; and a mass loading in the range of 7.0 to 10.0 mg / cm2.

[0061] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode exhibits an average electrical resistance in a range of 0.0078 to 0.0083 Q. In another embodiment of the present disclosure, the anode exhibits an average electrical resistance in a range of 0.0079 to 0.0083 Q. In yet another embodiment of the present disclosure, the anode exhibits an average electrical resistance in a range of 0.0079 to 0.0082 Q.

[0062] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode has a discharge capacity in a range of 530 to 540 mAh / g within a standard deviation range of 1.6 to 1.8%. In another embodiment of the present disclosure, the anode has a discharge capacity in a range of 532 to 539 mAh / g within a standard deviation range of 1.65 to 1.8%. In yet another embodiment of the present disclosure, the anode has a discharge capacity in a range of 533 to 539 mAh / g within a standard deviation range of 1.65 to 1.75%.

[0063] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode exhibits at least 96% capacity retention up to 50 cycles. In another embodiment of the present disclosure, the anode exhibits 98% capacity retention up to 50 cycles.

[0064] In an embodiment of the present disclosure, there is provided an anode as disclosed herein, wherein the anode has an initial coulombic efficiency of 88 to 99.7%. In another embodiment of the present disclosure, wherein the anode has an initial coulombic efficiency of 88.2 to 99.6%. In yet another embodiment of the present disclosure, wherein the anode has an initial coulombic efficiency of 88.5 to 99.5%.

[0065] In an embodiment of the present disclosure, there is provided an electrochemical cell comprising: (a) the anode as disclosed herein; (b) a cathode, and (c) an electrolyte.

[0066] Although the subject matter has been described in considerable detail with reference to certain examples and implementations thereof, other implementations are possible.EXAMPLES

[0067] The disclosure will now be illustrated with following examples, which is intended to illustrate the working of disclosure and not intended to take restrictively to imply any limitations on the scope of the present disclosure. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood to one of ordinary skill in the art to which this disclosure belongs. Although methods and materials similar or equivalent to those described herein can be used in the practice of the disclosed methods and compositions, the exemplary methods, devices and materials are described herein. It is to be understood that this disclosure is not limited to particular methods, and experimental conditions described, as such methods and conditions may apply.Materials and methods

[0068] For the purpose of the present disclosure, following raw materials with the specified grades / brands were used. Silicon carbide, graphite, carboxymethyl cellulose (CMC), carbon nano tube (CNT) and styrene-butadiene rubber (SBR) were procured from commercial sources.EXAMPLE 1Preparation of active material

[0069] The present example provides a process for preparing the active material Al.

[0070] 14.6% (w / w) of silicon carbide (SiC) (silicon compound) and 85.4% (w / w) of graphite (carbon based material) were mixed at 24°C by pulsation mixing. The pulse mixing of the mixture was carried out with a first pulse mixing at a speed of 3000 rpm for 10 minutes, followed by a second pulse mixing at a speed of 1200 rpm for 10 minutes. The first and second pulse mixing were sequentially repeated six times each, for a total time period of 120 minutes, to obtain the active material Al.

[0071] Comparative active material API was prepared, wherein a first pulse mixing of the mixture was carried out at a speed of 3000 rpm for 5 minutes, followed by a second pulse mixing at a speed of 1200 rpm for 5 minutes. The first and secondpulse mixing were sequentially repeated twelve times each, for a total time period of 120 minutes.

[0072] Comparative active material AP2 was prepared by conventional continuous mixing 14.6% (w / w) of silicon carbide (SiC) (silicon compound) and 85.4% (w / w) of graphite (carbon based material) at 3000 rpm for 180 minutes.EXAMPLE 2Analysis of active material

[0073] The active material Al (prepared in Example 1) was analysed for its morphological studies and particle size distribution.Morphological studiesEnergy dispersive X-ray spectroscopy (EDS) studies and Backscattered electron studies

[0074] The active material Al, was analysed by energy dispersive X-ray spectroscopy (EDS), at every 60 minutes interval of pulse mixing. Observations were recorded after 60 and 120 minutes, as illustrated in Figures 1(a) and 1(b), respectively. As depicted in Figure 1(b), a higher concentration of silicon carbide (SiC) particles was observed in Al. As shown in Figures 1(a) and 1(b), the pulsed mixed mixture at 60 and 120 minutes exhibited uniformity of silicon carbide within graphite. As the mixing time increased, the SiC particles were better dispersed in the graphite.

[0075] Similarly, the distribution of silicon carbide (SiC) in graphite in the comparative active material AP2 was analysed by energy dispersive X-ray spectroscopy (EDS), at 30 minutes intervals. Observations were recorded after 30, 60, 90, 120, 150, and 180 minutes, as illustrated in Figures 2(a), 2(b), 2(c), 2(d), 2(e), and 2(f), respectively. As depicted in Figures 2 (a), to 2 (f), the particle distribution was non-uniform.

[0076] To understand the uniform distribution of silicon carbide (SiC) in graphite, energy dispersive X-ray spectroscopy (EDS) studies (Figures 3(a) to (c)) of the active material Al, was carried out. Figure 3 (a) showed the area mapping analysisof the active material Al after pulse mixing. It was clearly observed in Figure 3(a) that the bright particles of silicon carbide (SiC) were uniformly distributed within the dark particles of graphite.

[0077] To study the uniform distribution of silicon carbide (SiC) in graphite, backscattered electron studies and energy dispersive X-ray spectroscopy (EDS) studies (Figures 3(d) and 3(e)) were carried out for the comparative active material API, after 60 minutes and after 120 minutes (Figures 3(f) and 3(g)) of mixing. It could be observed that the 5-minutes pulsed mixed silicon carbide (SiC) and graphite, exhibited higher concentration of silicon carbide (SiC) particles in some specific highlighted zones and did not provide homogenous mixture of the active material.

[0078] Hence, it was revealed that the pulse mixing carried out with the process of the present disclosure, facilitated a more uniform, steady and homogeneous dispersion of silicon carbide within the graphite.Particle size distribution

[0079] The particle size (D50) distribution of silicon carbide (SiC) (a silicon compound) and graphite (a carbon-based material) used in the preparation of Al is depicted in Figures 4(a) and 4(b), respectively. It was observed that the particle size D50 for silicon carbide was 7.9 micron, while for graphite, it was 14.5 micron.

[0080] The particle size (D50) distribution of the prepared active material Al was analysed. The particle size (D50) distribution data obtained after 60 minutes of pulse mixing and after 120 minutes of pulse mixing of Al are depicted in Figures 4(c) and 4(d), respectively. It was determined that the particle size D50 for Al obtained after 60 minutes of pulse mixing was 12.15 micron, and for Al obtained after 120 minutes of pulse mixing was in the range of 11.71 micron.

[0081] The particle size (D50) distribution of the comparative active material API was analyzed. The particle size (D50) distribution data obtained (Table 1) after 60 minutes of pulse mixing and after 120 minutes of pulse mixing of API are depicted in Figures 4(e) and 4(f), respectively. It could be determined that the particle size D50 of APlobtained after 60 minutes was 12.08 micron, and obtained after 120 minutes was 11.74 micron, respectively.

[0082] The particle size (D50) distribution data of the comparative active material AP2 after 60 minutes of mixing, 120 minutes of mixing, and 180 minutes of mixing as illustrated in Figures 4(g), 4(h), and 4(i), respectively. It was determined that the particle size (D50) of AP2 obtained after 60 minutes was 11.69 micron, after 120 minutes was 11.41 micron, and after 180 minutes was 11.38 micron.Table 1APIPulsed mixed blend Parameter Pulsed mixed blend(micron) after 60 minutes after 120 minutesDio 6.55 6.12Dso 12.08 11.75D90 21.62 22.31EXAMPLE 3Preparation of anode

[0083] For the analysis purposes, anode El (prepared in Example 1) was prepared by active material, Al, and analysed for its mechanical and electrochemical performance properties.

[0084] 0.5% (w / w) of carbon nanotube (conductive additive) and 0.7% (w / w) of carboxymethyl cellulose (Ashland CMC) (binder) was mixed at 2000rpm for 30 minutes. Subsequently, 96% (w / w) of Al (active material) was added in the prepared mixture and mixed again at 2000 rpm for another 30 minutes. This was followed by addition of a sufficient quantity of deionized water to obtain a slurry, which was further mixed for 30 minutes at 2000 rpm. Finally, 1.4% (w / w) of styrene-butadiene rubber (SBR) (binder), and 1.4% (w / w) of modified styrenebutadiene rubber (binder) were added and mixed for 30 minutes at lOOOrpm, resulting in the prepared anode El.

[0085] Similarly, comparative anode EP2 was prepared using comparative activematerial AP2.EXAMPLE 4Mechanical studies

[0086] The density and peel strength of the prepared anodes El, and EP2 were determined.Density measurement

[0087] The density measurements of the prepared anodes El and EP2 were conducted. As shown in Table 2, the anodes obtained from active material Al and comparative active material AP2 exhibited a similar density of 1.67 g / cc. This result indicated that the active materials had similar packing areas in the anodes, despite the different distribution of silicon (Si) particles.Peel strength

[0088] Peel strength analysis is a conventional method in battery industry for ranking the adhesion strength of sample. The peel strength of the prepared anodes El, and EP2 was measured using Scotch tape method with ASTM D3330D standards. A Scotch tape was pasted over the prepared anode in the dimension of 25 mm length and 25 mm width. The prepared anode was fixed with fixtures at top and bottom, followed by the application of a load at the front and back twice using a rubber roller. The lower side of the anode was placed in the lower fixed grips, and the upper movable grip was brought towards the lower and tightened firmly on both sides for position adjustment of the anode. It was ensured that the anode was placed in the centre of the grips, and the speed of the grip’s movement as 3 rpm. The rotary switch was turned in the upward direction, which led to the movement of upper grip in the upper direction. At this instance, the rotary switch was turned off, and peeled sample was obtained. The peel strength data of each of anode is provided in Table 2 and Figure 5.Mass loading

[0089] Mass loading analysis of the prepared anodes El and EP2 was conducted. As shown in Table 2, the El anode obtained from active material Al showed lowermass loading compared to EP2. This result indicated that the active material obtained from the process of the present disclosure, had uniformly distributed silicon (Si) particles in the graphite, resulting in compact packing areas in the anode El and was attributed to varying thicknesses.Table 2Anode Density (g / cc) Peel strength (N / 25mm) Mass loading (mg / cm2) El 1.67 1.21 7.13EP2 1.67 0.90 9.88

[0090] As shown in Table 2, the anode El prepared with the active material Al (prepared by the process of the present disclosure) showed greater peel strength than the anode EP2 comprising the comparative active material AP2. The homogenised blend of silicon carbide and graphite in the active material Al, exhibited more adhesive properties than the comparative active material AP2. The uniform distribution of both silicon carbide and graphite in Al lowered the surface tension leading to uniform spreading and adhesion.Electrochemical performance

[0091] The electrical resistance of the prepared anodes El, and EP2 was determined.

[0092] It was observed that anode EP2 exhibited lower average electrical resistance (0.0076 Q) compared to El (0.0081 Q) and might have better conductivity, but the uneven dispersion in EP2 could lead to localized over-lithiation, higher mechanical stress, and a risk of delamination (lower peel strength). It was also found that although anode El exhibited lower discharge capacity (536.3 mAh / g) compared to EP2 (559.5 mAh / g), and lower initial coulombic efficiency (89.01%) compared to EP2 (91.35%), the more uniform silicon (Si) dispersion and stronger electrode adhesion (higher peel strength) remarkably improved the long-term cycling stability compared to EP2, despite a marginally higher resistance.

[0093] The electrochemical performance of the electrochemical cell ECI, prepared using the anode El, comprising active material Al, was assessed as depicted herein.

[0094] To evaluate the efficiency of the charge-discharge cycle of the electrochemical cell (EC), the initial charge-discharge of ECI, prepared with anode El, and ECP2 prepared with comparative anode EP2, was measured. As shown in Figure 6, ECI prepared with El, exhibited a discharge capacity of 536.3 mAh / g during first discharging process. Its initial coulombic efficiency (ICE), coulombic efficiency at first and second cycle, was found to be 89.01%, 99.01%, and 99.4% respectively. The coulombic efficiency at first and second cycle of EC, indicated that the charge stored during the first cycle was recovered during discharge. It reflected a longer life and better overall efficiency of the electrochemical cell.

[0095] To assess the anode efficiency comparable to electrochemical cell ECI, similar cells EC2, EC3, and EC4 were also prepared, and their initial chargedischarge cycles were examined. As shown in Figure 7, cells with anode El, comprising active material Al, demonstrated more consistent discharge capacity, with values closely clustered between 534.0 and 537.9 mAh / g. The average discharge capacity was 536.3 mAh / g, with a minimal standard deviation of 1.7. However, the comparative electrochemical cell ECP2, prepared with a comparative anode EP2, and comparative active material AP2, exhibited significantly higher variability in the discharge capacity among the similarly prepared cells, ECP3, ECP4 and ECP5, ranging from 529.0 mAh / g to 580.1 mAh / g. The average discharge capacity was found to be 559.5 mAh / g, but individual cell values showed a greater standard deviation of 22.5.

[0096] These observations revealed that the active material AP2 prepared using conventional processes led to an inhomogeneous distribution of silicon (Si) in anodes, resulting in uneven lithiation, increased resistance, mechanical failure, and capacity fading. However, by optimizing material dispersion, electrode architecture, and processing conditions with a pulsation technique for the preparation of active material Al, a homogeneous distribution was achieved, leading to high-performance, long-cycle-life lithium-ion batteries.

[0097] Hence, greater variation in discharge capacity for comparative electrochemical cell ECP2, and similarly prepared electrochemical cell ECP3, ECP4, and ECP5 suggested non-uniform lithiation. ECP4 performed at 580.1 mAh / g, while ECP2 performed at 529 mAh / g, indicating localized stress due to higher or lower silicon distribution in the area. This in turn could lead to faster degradation and capacity fading over cycling. However, electrochemical cells ECI, EC2, EC3, and EC4 exhibited more consistent performance across all cells, suggesting improved silicon (Si) dispersion, leading to better electrical and ionic conductivity. The lower variability implied more stable lithiation / de-lithiation, which enhanced cycle life and overall battery reliability.

[0098] Therefore, it could be determined that the electrochemical cells ECI, EC2, EC3, and EC4, prepared with the active material Al, using the process of the present disclosure, were superior formulated due to better adhesion, stable conductivity, and lower variation in discharge capacity. However, comparative electrochemical cells might have short-term benefits in resistance but suffered from delamination risks and inhomogeneous performance, and potential long-term degradation. The optimized mixing process with sequential specific pulsation mixing provided homogeneous active material and critically exhibited improved Si-anode battery performance.Cycle life stability

[0099] The cycle life of an electrochemical cell is characterized by an initial period of stable performance, followed by gradual degradation, and finally, accelerated capacity loss leading to the end of life. The cycle life of electrochemical cell ECI was analysed in a capacity retention range of 90 to 100% and cycle range of 0 to 50 numbers. As shown in Figure 8, the cycle life of electrochemical cell ECI, comprising anode El, showed stable behaviour up to 50 charge discharge cycle and exhibited constant charge retention. These data revealed the higher electrochemical efficiency of the active material Al, over AP2.ADVANTAGES OF THE PRESENT DISCLOSURE

[0100] The present disclosure provides a process for preparing an active material, the process comprising: pulse mixing a mixture comprising a silicon compound and a carbon based material to obtain the active material, wherein the pulse mixing comprises a) a first pulse mixing at a speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes, followed by, b) a second pulse mixing at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice. The specific pattern of pulsation mixing ensures efficient and homogenous mixing of silicon compound with carbon based material, resulting in a highly uniformly packed, and consistent active material. The anode of the present disclosure exhibits a peel strength in a range of 0.1 to 2.5 N / 25mm, which implies increased mechanical stability. The anode of the present disclosure also exhibits a density in a range of 1.0 to 2.0 g / cc, a mass loading in the range of 6.5 to 8.5 mg / cm2, an average electrical resistance in a range of 0.0078 to 0.0083 Q and a discharge capacity in a range of 530 to 540 mAh / g within a standard deviation range of 1.6 to 1.8% which contributes to increased electrochemical performance. The anode described in the present disclosure further exhibits at least 96% capacity retention up to 50 cycles, thereby enhancing the electrochemical behavior of the cell. Moreover, the present disclosure provides a convenient and a facile process for preparing the active material.

Claims

I / We Claim:

1. A process for preparing an active material, the process comprising:pulse mixing a mixture comprising a silicon compound and a carbon based material to obtain the active material,wherein the pulse mixing comprisesa) a first pulse mixing at a speed in the range of 2500 to 3500 rpm for a time period in the range of 7 to 20 minutes, followed by, b) a second pulse mixing at a speed in the range of 1000 to 1500 rpm for a time period in the range of 7 to 20 minutes, and the first pulse mixing and the second pulse mixing are sequentially repeated at least twice.

2. The process as claimed in claim 1, wherein the first pulse mixing and the second pulse mixing are sequentially repeated two to eight times, for a total time period of 90 to 160 minutes.

3. The process as claimed in claim 1, wherein the silicon compound is selected from silicon carbide (SiC), silicon oxide (SiOx), amorphous silicon (a-Si), silicon quantum dots, or combinations thereof; and the silicon precursor is in a weight range of 2 to 55% (w / w) with respect to total weight of the active material.

4. The process as claimed in claim 1, wherein the carbon based material is selected from artificial graphite, natural graphite, hard carbon, soft carbon, graphene-modified graphite, or combinations thereof; and the carbon based material is in a weight range of 45 to 95% (w / w), with respect to total weight of the active material.

5. The process as claimed in claim 1, wherein the active material has a particle size (D50) distribution in a range of 6 to 9 micron for silicon compound and 12 to 15 micron for carbon based material.

6. An active material obtained by the process as claimed in claim 1, wherein the active material has a particle size (D50) distribution in a range of 11 to 14 micron.

7. An anode comprising:a. the active material obtained by the process as claimed in claim 1; b. a conductive additive; andc. a binder.

8. The anode as claimed in claim 7, wherein the active material is in a weight range of 92 to 98%, with respect to the total weight of the anode.

9. The anode as claimed in claim 7, wherein the conductive additive is selected from graphene, carbon black, carbon nanofiber, carbon nanotube, flaky carbon, or combinations thereof; and the conductive additive is in a weight range of 0.2 to 3.5%, with respect to total weight of the anode.

10. The anode as claimed in claim 7, wherein the binder is selected from carboxymethyl cellulose (CMC), lithium modified carboxymethyl cellulose (Li-CMC), sodium modified carboxymethyl cellulose (Na-CMC), styrenebutadiene rubber (SBR), modified styrene-butadiene rubber, poly acrylic acid modified styrene-butadiene rubber (SBR-PAA), rubber based polymers, polyacrylic acid (PAA), modified polyacrylic acid, lithium modified polyacrylic acid (Li-PAA), acrylates, amides, imides based polymer, or combinations thereof; and the binder is in a weight range of 1.8 to 5% (w / w), with respect to total weight of the anode.

11. The anode as claimed in claim 7, further comprises a current collector.

12. The anode as claimed in claim 7, wherein the anode has a peel strength in a range of 1.0 to 2.5 N / 25mm.

13. The anode as claimed in claim 7, wherein the anode has a density in a range of 1.0 to 2.0 g / cc; and a mass loading in the range of 6.5 to 12.0 mg / cm214. The anode as claimed in claim 7, wherein the anode exhibits an average electrical resistance in a range of 0.0078 to 0.0083 Q.

15. The anode as claimed in claim 7, wherein the anode has a discharge capacity in a range of 530 to 540 mAh / g within a standard deviation range of 1.6 to 1.8%.

16. The anode as claimed in claim 7, wherein the anode exhibits at least 96% capacity retention up to 50 cycles.

17. The anode as claimed in claim 7, wherein the anode has an initial coulombic efficiency of 88 to 99.7%.

18. An electrochemical cell comprising:(a) the anode as claimed in claim 7;(b) a cathode, and(c) an electrolyte.